betaFeedback

WorksPhysics and Astronomy

Vibrational and mechanical properties of the highly mismatched (Cd,Be)Te semiconductor alloy : Experiment and ab initio calculations

Abstract

The (Cd, Be)Te semiconductor alloy that exhibits a dramatic mismatch in bond covalency and stiffness clarifying its vibrational and mechanical properties is used as a benchmark to test the limits of the percolation model (PM) worked out to explain the complex Raman spectra of the related but less contrasted (Zn, Be) chalcogenides. The test is done by way of experiment (x smaller than 0.11) combining Raman scattering with X ray diffraction at high pressure and ab initio calculations (x around 0, 0.5 and 1). The (macroscopic) bulk modulus B drops below the CdTe value on minor Be incorporation, at variance with a linear B versus x increase predicted ab initio, thus hinting at large anharmonic effects in the real crystal. Yet, no anomaly occurs at the microscopic (bond) scale as the regular bimodal PM Raman signal predicted ab initio for the BeTe bond in minority (x around 0 and 0.5) is (barely) detected experimentally. Although at large Be content (x around 1) the same bimodal signal relaxes down to inversion, an unprecedented case, specific pressure dependencies of the regular (x around 0 and 0.5) and inverted (x around 1) BeTe Raman doublets are in line with PM predictions. Hence, the PM applies as such to (Cd, Be)Te albeit in a relaxed form, without further refinement. This enhances the scheme validity as a generic descriptor of phonons in alloys.

pressure / low-temperature experiment (x=0.11x = 0.11). However, at large Be content (x∼1x \sim1) the ab initio bimodal Be-Te Raman signal “relaxes” all the way down to (a slight) inversion – giving rise to an unprecedented crossing of percolation sub-branches in a “Raman frequency vs. xx” plot. The inverted doublet exhibits a remarkable intensity interplay under pressure, grasped within a linear dielectric approach. Altogether, the B0B_{0}-drop at x∼0x \sim0 and the inversion of the Raman signal at x∼1x \sim1 reflect a negative impact of the large bond mismatch on the Cd1−x_{1-x}Bex_{x}Te mechanical-vibrational properties at various length scales and compositions. Yet, the percolation scheme applies as such to Cd1−x_{1-x}Bex_{x}Te – albeit in a “relaxed” form, without further refinement. This enhances the scheme’s validity as a generic descriptor of phonons in alloys.

Due to its direct optical band gap of 1.5 eV and high optical absorption coefficient, the cubic-zincblende II-VI CdTe semiconductor compound is almost ideal for solar energy conversion. The CdTe-based technology, stimulated by high conversion rates achieved over the past decade (exceeding 22% in laboratory) together with the stability of the photovoltaic devices under operating conditions, has now developed up to the industrial scale [1]. As early as in 1960’s, the alloying of CdTe has been explored as a convenient means to finely tune its physical properties being of major interest as those of a semiconductor (the optical band gap E0E_0 and the lattice constant aa), in view of targeted applications. The current study of the prospective Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_x\mathrm{Te} II-VI semiconductor alloy is in this line – although it mainly concerns the mechanical-vibrational properties and not so much the optical (E0E_0) and structural (aa) ones.

One conventionally refers to II-VI and III-V pseudobinary A1−xBxC\mathrm{A}_{1-x}\mathrm{B}_x\mathrm{C} semiconductor alloys of first generation – still actively studied[2] – as those in which the A↔B substitution involves elements from the third to sixth rows of the periodic table. The A-C and B-C chemical bonds enter with physical properties (length ll and covalency αc\alpha_c; the values below – given cubed in the latter case – are cited from Refs.[3, 4] unless specified) close within a few percent[4], which facilitates alloying. The CdTe-based Cd1−xZnxTe\mathrm{Cd}_{1-x}\mathrm{Zn}_x\mathrm{Te}, CdSexTe1−x\mathrm{CdSe}_x\mathrm{Te}_{1-x} and CdSxTe1−x\mathrm{CdS}_x\mathrm{Te}_{1-x} systems are like this, forming “well-matched” alloys (WMA’s)[1]. In the exemplary III-V WMA, Al1−xGaxAs\mathrm{Al}_{1-x}\mathrm{Ga}_x\mathrm{As} (Δll∼8‰\frac{\Delta l}{l}\sim8\text{‰}, Δαc3αc3∼5%\frac{\Delta\alpha_c^3}{\alpha_c^3}\sim5\%), and the leading II-VI WMA, Cd1−xHgxTe\mathrm{Cd}_{1-x}\mathrm{Hg}_x\mathrm{Te} (Δll∼3‰\frac{\Delta l}{l}\sim3\text{‰}, Δαc3αc3∼2.5%\frac{\Delta\alpha_c^3}{\alpha_c^3}\sim2.5\%), the matching is nearly perfect[3].

In the 1990’s, the emergence of semiconductor alloys involving second-row elements in substitution –like N, Be and O, – e.g., N-dilute GaAs1−xNx\mathrm{GaAs}_{1-x}\mathrm{N}_x (Ref.[5]) and Zn1−xBex\mathrm{Zn}_{1-x}\mathrm{Be}_x-chalcogenides[6, 7] –created a disruption. In fact, light elements with small covalent radii form extremely short bonds which, moreover, exhibit odd features of the αc\alpha_c that governs the resistance of a bond to a distortion in shear (increasing with αc\alpha_c) and hence the stability of the lattice. So, with Be-bonding (BeS, BeSe, BeTe) the αc\alpha_c achieves maximum among II-VI’s, whereas, on the contrary, the αc\alpha_c of N-bonded compounds (InN, GaN, AlN) hits a minimum among III-V’s[4]. Consequently, in zincblende alloys such as Zn1−xBexSe\mathrm{Zn}_{1-x}\mathrm{Be}_x\mathrm{Se} and GaAs1−xNx\mathrm{GaAs}_{1-x}\mathrm{N}_x the bond properties do dramatically differ, by as much as (Δll∼9%\frac{\Delta l}{l}\sim9\%, Δαc3αc3∼33%\frac{\Delta\alpha_c^3}{\alpha_c^3}\sim33\%) and (∼20%\sim20\%, ∼23%\sim23\%), respectively. The discrepancy softens as N is replaced by next-row P – to form GaAs1−xPx\mathrm{GaAs}_{1-x}\mathrm{P}_x (∼3.5%\sim3.5\%, ∼1%\sim1\%). The “bond mismatch” is likewise large for ZnSe1−xOx\mathrm{ZnSe}_{1-x}\mathrm{O}_x (∼21%\sim21\% – Ref.[8], ∼16%\sim16\%) but small for ZnSe1−xSx\mathrm{ZnSe}_{1-x}\mathrm{S}_x (∼4.5%\sim4.5\%, ∼6.8%\sim6.8\%). Hence, the second-generation alloys involving (Be, N, O) in substitution were singled out as forming a new class of “highly-mismatched alloys” (HMA’s for short)[9].

HMA’s – to which belongs Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_x\mathrm{Te} studied in this work – attract attention because in certain cases their large bond mismatch dramatically impacts the electronic band structure. For instance, even slight N-incorporation into GaAs (anyway limited to a few percent[10]) induces a giant (negative) bowing of E0E_0 (of ∼100\sim100 meV per atomic percent of N)[10], due to a band anticrossing which results from coupling of the extended states forming the host conduction band with a quasi-resonant highly localized impurity state[10, 11, 12, 13, 14]. Oxygen likewise induces an intermediate band within the bandgap of O-dilute ZnTe1−xOx\mathrm{ZnTe}_{1-x}\mathrm{O}_{x}[15, 16] and CdTe1−xOx\mathrm{CdTe}_{1-x}\mathrm{O}_{x}[17]. No similar outstanding features were detected with Zn1−xBex\mathrm{Zn}_{1-x}\mathrm{Be}_{x}-chalcogenides, which therefore received less attention so far. E0E_0 varies linearly with xx in Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te}[18], or undergoes just a slight bowing in Zn1−xBexSe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Se}[19]. More generally, the (quasi) linearity with composition governs all studied critical points of the electronic band structure of Zn1−xBex\mathrm{Zn}_{1-x}\mathrm{Be}_{x}-chalcogenides (considering the direct gaps between the upper valence band and the lower conduction band at the Γ\Gamma, LL and XX points – namely E0E_0, E1E_1 and E2E_2, and the corresponding gaps involving the light hole valence band – notably E0+Δ0E_0 + \Delta_0 and E1+Δ1E_1 + \Delta_1, as assigned in Ref. 20), for both Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te}[21] and Zn1−xBexSe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Se}[22].

However, the Zn1−xBex\mathrm{Zn}_{1-x}\mathrm{Be}_{x}-chalcogenides have held a central place in what regards vibrational properties. In early 2000’s, pioneering Raman studies[23, 24, 25] revealed a bimodal signal per bond (1-bond→2-mode) that contested the classical view of a unique mode per bond (1-bond→1-mode) in random zincblende alloys[26]. This was explained in terms of sensitivity of the effective bond force constant (kk) – probed by Raman scattering – to local Be- and Zn-like environments, casted into the percolation model (PM, Ref. 27 and refs. therein). Subsequently, the PM enabled a unified understanding, hitherto missing, of the Raman spectra of II-VI, III-V and IV WMA’s with cubic (zincblende, diamond) and hexagonal (wurtzite) structures, suggesting the model’s universality [27].

The bond force constant (kk) and the bond length (ll) are related via a basic rule that the former decreases as the latter is stretched, and vice versa. Referring this to the Zn1−xBex\mathrm{Zn}_{1-x}\mathrm{Be}_{x}-HMA’s the variation in Be-related bond force constant (~10%) observed in Raman[25, 27] and far-infrared absorption[28] experiments is correlated with a predicted variation in Be-related bond length (~2%, from ab initio calculations[29]) depending on whether the Be-related bond is in a Be-like or Zn-like environment. Unfortunately, this bimodal distribution of the Be-related bond length could not be resolved in extended X-ray absorption fine structure (EXAFS) measurements on a synchrotron[30, 31], and is a priori hardly detectable via the pair distribution function in conventional total X-ray scattering experiments[32, 33]. The same applies a fortiori to the less contrasted WMA’s. For instance, the III-V (covalent) Ga1−xInxAs\mathrm{Ga}_{1-x}\mathrm{In}_{x}\mathrm{As} and II-VI (ionic) ZnSe1−xTex\mathrm{ZnSe}_{1-x}\mathrm{Te}_{x} alloys usually ranked among WMA’s despite their significant lattice mismatch (~7%, Ref. 3) likewise exhibit a unique bond length per species at a given xx value in EXAFS data[34, 35, 36]. Yet their Raman signal is bimodal per bond – of the percolation type[25, 37]. Hence, EXAFS does not resolve the splitting of the A-C or B-C bond lengths of A1−xBxC\mathrm{A}_{1-x}\mathrm{B}_{x}\mathrm{C} zincblende alloys – HMA’s included – due to A-like or B-like local environments and thus yields a basic 1-bond→1-length description[38], whereas the Raman signal diversifies into a (percolation-type) 1-bond→2-mode pattern. In a nutshell, the lattice dynamics zooms deeper into the alloy disorder than the lattice relaxation. This is interesting on the fundamental side.

Besides, the PM opens applications. In particular, the phonons being sensitive to the local environment – as formalized within the PM, they can be used to elucidate whether the atom substitution is ideally random or not[27], the central issue when dealing with alloys. Apart from vibrational spectroscopies, the nuclear magnetic resonance (NMR) seems to be the only one in-house technique capable of addressing such issue quantitatively[39] –an example is given below. Alternatively, one may resort to EXAFS measurements (using a synchrotron) of the second-neighbor distances for the common-atom sublattice (i.e., the Te-Cd-Te and Te-Be-Te ones for Cd1−x_{1-x}Bex_xTe) – which differ on account that each bond tends to preserve its natural length in an alloy[35, 38].

In this work, the PM is tested on the emerging Cd1−x_{1-x}Bex_xTe HMA that exhibits an even larger bond mismatch (Δll∼15%\frac{\Delta l}{l} \sim15\%, Δac3ac3∼36%\frac{\Delta a_c^3}{a_c^3} \sim36\%) than the Zn1−x_{1-x}Bex_x-chalcogenides. It is not a priori obvious whether the PM would apply to such special system. In the positive case, it will be instructive to elaborate on specific consequences from the PM, listed below from basic to more advanced ones[40]:

  1. Only Be-Te should exhibit a distinct Raman doublet. Being small, Be has more room than Cd to move around in the Te-cage to accommodate the local strain created by the bond mismatch, with concomitant impact on the Raman frequencies being more diversified for Be-Te than for Cd-Te.

  1. Out of the two sub-modes within the Be-Te doublet, the softer (harder) one would refer to Be (Cd)-like environments. Consider, e.g., an isolated Cd atom embedded in BeTe. In its vicinity, the short Be-Te bonds suffer a compressive strain due to a competition with the longer Cd-Te ones within the given lattice spacing, hence vibrate at a higher frequency than the bulk-like Be-Te bonds away from Cd. An inverse argumentation applies to CdTe doped with Be.

  1. The Be-Te doublet is expected to converge under pressure. This is due to a larger volume derivative of the bond ionicity ∂fi/∂ln⁡V\partial f_i/\partial\ln V (with fi=1−αcf_i = 1 - \alpha_c) for Be-Te (0.7453) than for Cd-Te (0.407)[3]. Hence, the Be-like environment hardens under pressure faster than the Cd-like environment does, so that thence stemming (softer) Be-Te Raman line within the percolation doublet drifts (upwards) under pressure faster. A classification of II-VI and III-V (WMA’s and HMA’s) alloys was accordingly suggested in Ref.[27].

  1. This convergence either ends up into a phonon exceptional point at the crossing-resonance (scenario 1), or freely develops into an inverted doublet post resonance (scenario 2), depending on whether the (Be-Te) bond responsible for the vibration doublet is dispersed (self-connects in chains) or matrix-like (self-connects in bulk), respectively. The Raman intensity of the minor mode within the doublet undergoes, correspondingly, an extinction (scenario 1) or enhancement (scenario 2).

More generally, the ambition of this work is an integrated and coherent fundamental study of mechanical properties of the Cd1−x_{1-x}Bex_xTe HMA at the macroscopic (via elasticity) and microscopic (sensitive to chemical bonds) scales, using Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_x\mathrm{Te}[40] as a suitable reference–based on proximity of Cd and Zn in the periodic table. Specifically, we combine high-pressure X-ray diffraction measurements on single crystals at the PSICHÉ and CRISTAL beamlines of SOLEIL synchrotron, in search for the macroscopic bulk modulus (B0B_0), with high-pressure Raman scattering measurements (on the same samples), probing the effective bond force constants in line with the above raised issues (1-to-4) around the PM. The discussion of Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_x\mathrm{Te} experimental data is supported by high-pressure ab initio snapshots of the lattice relaxation, notably to determine the equation of state from which B0B_0 is issued, and of the lattice dynamics, with special attention to the Raman frequencies and intensities. Additional ab initio calculations are implemented to cover xx values beyond the experimental range (currently limited to 11 at.% Be). Various ab initio codes are used, i.e., AIMPRO41,42{}^{41,42} (Ab Initio Modeling PROgram), SIESTA43,44{}^{43,44} and QE45{}^{45} (Quantum Expresso), depending on need – as specified in the course of the discussion.

Besides, we briefly test by ellipsometry and transmission if the E0E_0 vs. xx dependency is (quasi) linear, like with Zn1−xBex\mathrm{Zn}_{1-x}\mathrm{Be}_x-HMA’s, or significantly deviates from linearity, like with N/O-dilute HMA’s. It is a matter to appreciate on an experimental basis whether HMAlloying with second-row elements (Be, N, O) is virtuous for E0E_0 (in that it generates a smooth linear-like E0E_0 vs. xx variation) only in case of Zn↔Be substitution (as discussed above) – for whatever reason, or is a more general rule with Be.

Results and discussion

The studied samples consist of high-quality / purity Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_x\mathrm{Te} and Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_x\mathrm{Te} bulk single crystals grown by the Bridgman method with small Be content (x≤0.11x \leq0.11 and 0.21, as determined by chemical analysis – see methods – and via the aa vs. xx linearity$[46], correspondingly). The zincblende structure, common to end compounds, was confirmed by powder X-ray diffraction (Figure S1 and Figure S2; “S” stands for Supplementary Information) throughout intermediate compositions. The Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_x\mathrm{Te} lattice expands / shrinks homothetically as xx varies (reflected by a linear aa vs. xx variation between the CdTe – this work – and BeTe[47] values, Figure S1), that seems to be common in alloys, HMA’s included[2]. Further structural insight at the microscopic scale is gained via powder (x=0.07x=0.07) 125Te{}^{125}\mathrm{Te} solid-state nuclear magnetic resonance (NMR) measurements[39]. A bimodal NMR pattern (Figure 1a) distinguishes between two tetrahedral environments for Te among five possible ones depending on the number of Cd and Be nearest neighbors. The NMR peak intensities scale as the fractions of tetrahedral Te-clusters with 4×Cd and (3×Cd, 1×Be) atoms at the vertices, as suggested by the Bernoulli’s binomial distribution[39] at x=0.07x=0.07 (Figure 1a, inset). One notes a practical absence of Te-centered clusters with more Be atoms, consistently with experiment. Altogether the NMR data point towards an ideally random Cd↔Be substitution in Cd0.93Be0.07Te\mathrm{Cd}_{0.93}\mathrm{Be}_{0.07}\mathrm{Te}, presumably valid in all studied samples owing to the close Be contents.

Cd$_{1-x}$Be$_x$Te structural, optical and mechanical properties

Figure 1. Cd1−x_{1-x}Bex_xTe structural, optical and mechanical properties. (a) CPMG Cd0.93_{0.93}Be0.07_{0.07}Te 125^{125}Te NMR signal. The binomial distribution of Te-centered nearest-neighbor (NN) tetrahedron clusters depending on the number of Cd atoms at the vertices in case of a random Cd↔Be substitution is added for comparison (inset). The NMR peaks are labeled accordingly. (b) Composition dependence of the main Cd1−x_{1-x}Bex_xTe electronic transitions measured at room temperature by transmission (filled symbols, Figure S5) and ellipsometry (hollow symbols, Figure S5). CdTe (Ref. 48) and BeTe (Ref. 20) values taken from the literature are added, for reference purpose. Linear (dashed) trends between parent values are guidelines for the eye. Laser lines used to excite the Raman spectra are positioned to appreciate resonance conditions. Antagonist arrows help to appreciate the shift of electronic transitions by lowering temperature from ambient to liquid nitrogen, by referring to the E0E_0 gap of CdTe Ref. 49. (c) Pressure dependence of the zincblende (zb), rocksalt (rs) and Cmcm (cm) Cd0.89_{0.89}Be0.11_{0.11}Te lattice constant(s) measured by high-pressure X-ray diffraction (Figure S1). (d) The B0B_0 value derived for Cd0.89_{0.89}Be0.11_{0.11}Te in its native zb phase (filled circle) from the corresponding volume vs. pressure dependence (Figure S1) is compared with the parent values taken from the literature (filled triangles, Refs. 30,50) and with current ab initio data obtained with the AIMPRO (hollow diamonds) and SIESTA (hollow squares) codes. Corresponding linear xx-dependencies are shown (dashed lines), for reference purpose.

High-pressure Cd$_{1-x}$Be$_x$Te X-ray diffraction data

Figure S1. (High-pressure) Cd1−x_{1-x}Bex_xTe (x≤0.11x \le0.11) X-ray diffraction data. (a) Powder Cd1−x_{1-x}Bex_xTe X-ray diffractograms obtained at ambient pressure in laboratory. (b) Corresponding xx-dependence of the lattice parameter. The BeTe value, taken from the literature[47], is added to complete the trend. The linearity is emphasized (dotted line). (c) selection of Cd0.89_{0.89}Be0.11_{0.11}Te-powder X-ray diffractograms obtained at increasing pressure. The individual peaks are labelled via the (hkl) Miller indices of the corresponding diffraction planes in various (zincblende-zb, rocksalt-rs, Cmcm-cm) structural phases. Additional diffraction peaks originate from Au and Ne used for pressure calibration and as the pressure transmitting medium, respectively. (d) Corresponding pressure dependence of the unit cell volume fitted to the Birch-Murnaghan equation of state.

High-pressure Zn$_{1-x}$Be$_x$Te X-ray diffraction data at moderate Be content

Figure S2. High-pressure Zn1−x_{1-x}Bex_xTe X-ray diffraction data at moderate Be content. Selection of (a) Zn0.955_{0.955}Be0.045_{0.045}Te and (b) Zn0.79_{0.79}Be0.21_{0.21}Te powder X-ray diffractograms obtained at increasing pressure. The individual peaks are labelled via the (hkl) Miller indices of the corresponding diffraction planes in various (zincblende-zb, rocksalt-rs, Cmcm-cm) structural phases. Additional diffraction peaks originate from Au and Ne used for pressure calibration and as the pressure transmitting medium, respectively, and from the gasket, as specified.

Hence the discussed experimental trends hereafter are presumably intrinsic to random Cd1−x_{1-x}Bex_xTe-alloying. Additional (9^{9}Be and 117^{117}Cd) NMR experiment completing the current (125^{125}Te) NMR insight into Cd0.93_{0.93}Be0.07_{0.07}Te are reported as Supplementary Information (Figure S4).

Substituent-related Cd₀.₉₃Be₀.₀₇Te NMR spectra

Figure S4. Substituent-related Cd0.93Be0.07Te\mathrm{Cd}_{0.93}\mathrm{Be}_{0.07}\mathrm{Te} NMR spectra. (a) 9Be{}^{9}\mathrm{Be} and (b) 113Cd{}^{113}\mathrm{Cd} NMR standard direct acquisition spectra.

The Tauc plots of Cd1−x_{1-x}Bex_xTe transmission data (x≤0.11x \le0.11, Figure S5) reveal a quasi linear E0E_0 vs. xx trend between the CdTe[48, 49] and BeTe[20] values (Figure 1b). The linearity persists with E1E_1 and E1+Δ1E_1 + \Delta_1 (Figure 1b) accessed by ellipsometry (Figure S5) – and also with E2E_2 (not shown) notwithstanding a poor signal-to-noise ratio due to the lack of luminous flux at high energy with the light source used. This resembles the case of Zn1−x_{1-x}Bex_x-chalcogenides[18, 19, 20, 21, 22], contrasting that of dilute nitrides/oxydes[10, 11, 12, 13, 14, 15, 16, 17]. Hence, the E0E_0 vs. xx linearity seems to be the rule with Be substitution. The (Be, Zn, Cd) substituents involved in (Zn,Cd)1−x_{1-x}Bex_x-chalcogenides are nearly iso-electronegative (within few percent), in contrast with dilute nitrides / oxydes that exhibit a large contrast in electronegativity between alloying elements (in the range 25-40%) – the admitted cause[16] for their large (negative) E0E_0 vs. xx bowing[12, 13, 14, 15, 16]. This might be the reason why the (Zn,Cd)1−x_{1-x}Bex_x-HMA’s behave like WMA’s in what regards their optical properties.

Cd₁₋ₓBeₓTe transmission and ellipsometry data

Figure S5. Cd₁₋ₓBeₓTe transmission and ellipsometry data. (a) Cd₁₋ₓBeₓTe Tauc plot (curves) of transmission data (symbols) giving access to E0E_0. (b) Corresponding ellipsometry data obtained by direct (model free) wavelength-per-wavelength inversion of the sine and cosine of the depolarization angles measured by ellipsometry. The main electronic transitions are indicated.

We turn now to mechanical-vibrational properties, independently probed at the macroscopic scale at SOLEIL synchrotron (PSICHÉ beamline), searching for the bulk modulus B0B_0 by high-pressure X-ray diffraction (HP-XRD), and at the microscopic scale by high-pressure Raman scattering (HP-RS), sensitive to the bond force constants, in relation to the raised issues (1-to-4) around the PM. For the sake of consistency, both studies are performed at the same Be content (x=0.11x=0.11).

The sequence of pressure-induced structural transitions (Figure 1c) apparent in the Cd0.89_{0.89}Be0.11_{0.11}Te HP-XRD diffractograms (taken on the upstroke, Figure S1) repeats that of pure CdTe (0 GPa: zincblende/ZB-cubic; 4 GPa: Rocksalt/RS-cubic, 12 GPa: Cmcm-orthorhombic)[50], however shifted to higher pressures (ZB→RS: 5 GPa, RS→Cmcm: 16 GPa) due to a reinforcement of the soft (ionic) CdTe-lattice by the stiff (covalent) Be-bonding –coming about also in Zn1−x_{1-x}Bex_xSe[30] and Zn1−x_{1-x}Bex_xTe[40]. One disconcerting feature, though, is that B0B_0 derived for Cd0.89_{0.89}Be0.11_{0.11}Te (41.667 ± 0.243 GPa – the error bar is within the symbol size, Figure 1d) from best fitting of the experimental pressure vs. volume dependence via the Birch-Murnaghan equation[51] (Figure S1) drops below the B0B_0 value of CdTe[52] (43.7 ± 1.0 GPa, Figure 1d, symbol) – which in turn is well below the BeTe one[53] (~67 GPa).

The B0B_0-drop is not accidental, due to the quality of fit. The first-order pressure derivative of B0B_0 evaluated at 0 GPa, B0′B'_0, coming out in the fit is 4.00 ± 0.15 for Cd0.89_{0.89}Be0.11_{0.11}Te, nearly matching the CdTe[51] (3.8 ± 0.6) and BeTe (fixed to 4 in Ref. [53]) values. By adopting for B0′B'_0 the “optimized” AIMPRO (B0′B'_0=4.7, B0B_0=40.5 GPa) and SIESTA (B0′B'_0=5.1, B0B_0=39.7 GPa) values at ~10 at.% Be (see below), the B0B_0-drop for Cd0.89_{0.89}Be0.11_{0.11}Te is emphasized (and the quality of fit degraded – not shown). A similar B0B_0-drop is also evidenced by HP-XRD diffraction with Zn1−x_{1-x}Bex_xTe (Figure S3, x≤0.21x\leq0.21) – using B0′B'_0=4 (found relevant for both ZnTe[54] and BeTe[53] parents in experiment) for the fitting (Figure S3), hence apparently a common feature of BeTe-based alloys.

Zn1-xBexTe bulk modulus plots

Figure S3. Zn1−x_{1-x}Bex_xTe bulk modulus. (a) Pressure dependencies of the unit cell volume – as derived from the high-pressure Zn1−x_{1-x}Bex_xTe X-ray diffractograms (partially reported in Figure S2) – fitted to the Birch-Murnaghan equation of state, including similar data obtained with Zn0.86_{0.86}Be0.14_{0.14}Te in the same run of experiment. (b) Resulting B0B_0 vs. xx variations.

The B0B_0-drop deviates from the (quasi) linear B0B_0 vs. xx experimental trend observed with Zn1−x_{1-x}Bex_xSe – however, disrupted by a punctual lattice hardening on percolation of the stiff Be-Se bonds[30]. The reason why Cd1−x_{1-x}Bex_xTe and Zn1−x_{1-x}Bex_xTe, but not Zn1−x_{1-x}Bex_xSe, suffer a B0B_0-drop from minor Be incorporation, might relate to a much weaker ionicity of the Be-Te chemical bonding (fif_i=0.222) compared with Be-Se (fif_i=0.420)[3]. This gives rise to more dramatic Δfi/fi\Delta f_i/f_i-contrasts in the BeTe-based Cd1−x_{1-x}Bex_xTe (∼\sim70%) and Zn1−x_{1-x}Bex_xTe (∼\sim60%) alloys than in the BeSe-based Zn1−x_{1-x}Bex_xSe one (∼\sim43%)[3], resulting in more severe bond distortions eventually affecting the mechanical properties in bulk.

Remarkably, no such B0B_0-drop but a linear B0B_0 vs. xx trend is suggested by ab initio results (x≤0.3x \leq0.3, hollow symbols, Figure 1d). The linearity seems robust since it is verified by two independent sets of calculations, applying the SIESTA (64-atom supercells, squares) and AIMPRO (for 216-atom supercells, diamonds) codes to distinct sets of fully- and partially-relaxed quasirandom (see methods) pseudobinary atomic arrangements, correspondingly. The ab initio vs. experiment discrepancy around B0B_0 suggests large anharmonic effects in real Cd1−x_{1-x}Bex_xTe, developing on large length scales – involving the full variety of atom arrangements making up a real randomly-disordered alloy, i.e., beyond the finite supercell-sizes used for the current ab initio calculations.

Now we address microscopic / vibrational properties of Cd1−x_{1-x}Bex_xTe, in line with the PM-issues around the Be-Te Raman signal (1-to-4) raised in the introductory Sec. A. A comparison with the reference Be-Te Raman percolation doublet of Zn0.89_{0.89}Be0.11_{0.11}Te – recently studied in detail[40] – matched in Be content with Cd0.89_{0.89}Be0.11_{0.11}Te, helps to fix ideas. Two impurity modes are involved in this case, a lower / minor TOBe−TeBeTO_{\mathrm{Be-Te}}^{\mathrm{Be}} and an upper / dominant TOBe−TeZnTO_{\mathrm{Be-Te}}^{\mathrm{Zn}} – with subscript and superscript referring to the vibrating bond and to the local environment, respectively – separated by ΔBe−Te∼20\Delta_{\mathrm{Be-Te}}\sim20 cm−1^{-1}, the intensities of these modes differing by roughly an order of magnitude.

Figure 2a displays an overview of the Cd-Te and Be-Te Cd1−x_{1-x}Bex_xTe TO Raman signals across the composition domain with information on frequency (curves) and intensity (color code) – technical detail is given below – offering a convenient eye-support for the forecoming discussion of the xx-dependence of the Be-Te Raman doublet of Cd1−x_{1-x}Bex_xTe. Experimental TO and LO Raman frequencies of pure BeTe taken from the literature[55] are added, for reference purpose. The given overview unveils in advance the main result of this work, namely, an irregular crossing of the two Be-Te “percolation” sub-branches (x∼0.8x\sim0.8) contrasting with the regular parallelism of the Cd-Te ones.

Cd$_{1-x}$Be$_x$Te vibrational properties

Figure 2. Cd1−x_{1-x}Bex_xTe vibrational properties. Panels are arranged anti-clockwise – starting from an overview at the top-center (a) – in the sense of increasing xx values from left (x∼0x \sim0) to right (x∼1x \sim1) for direct vertical comparisons of the side panels, i.e., (b) vs. (c) and (f) vs. (e), with a snapshot at intermediary composition in-between (d). (a) Theoretical overview of the Cd1−x_{1-x}Bex_xTe TO Raman frequencies (curves) and intensities (color of curves) at 0 GPa within a four-mode {2×(Cd−Te),2×(Be−Te)}\{2 \times(Cd - Te), 2 \times(Be - Te)\} description in absence of mechanical coupling between oscillators (ω′=0\omega'=0). A sensitivity of bond vibrations to first neighbors is assumed by analogy with Zn1−x_{1-x}Bex_xTe[40]. The current TO and LO Raman frequencies (hollow symbols) are indicated. BeTe data taken from the literature[55] are added (filled symbols), for reference purpose. A schematic view of the prototypical parent-like supercell (216-atom) containing one isolated impurity-duo used to generate an ab initio insight into the end (x∼0,1x \sim0,1) TO Raman frequencies of Cd1−x_{1-x}Bex_xTe is inserted. Labels (i) to (iv) refer to in-chain, out-of-chain, near-chain and away-from-chain bond vibrations – in this order, as sketched out. The shape of the Be-Te doublet dictated by the sole effect of the local strain, i.e., in absence of dispersion, is schematically represented by straight-dashed parallel lines. The dispersion effect affecting the impurity modes is emphasized by vertical arrows at x∼0,1x \sim0,1. (b) High-pressure / low-temperature Cd0.89_{0.89}Be0.11_{0.11}Te Raman spectra taken in the upstroke. The Be-Te signal, modeled via Lorentzian functions (dotted lines) transiently exhibits a minor feature at ∼3.5\sim3.5 GPa (marked by an asterisk). (c, d, e) Ab initio (AIMPRO) insights into the pressure dependence of the Be-Te Raman signal in large (216-atom) supercells (c) due to the Be-duo (x∼0x \sim0), (d) at intermediary Be content (x=0.5x=0.5) and (e) in presence of the Cd-duo (x∼1x \sim1) – giving rise to various local modes (spotted by asterisks). (f) Raman cross section reflecting the pressure-dependence of the irregular-inverted (see text) Be-Te TO Raman doublet at minor Cd content (x∼0.81x \sim0.81) in case of a minor mechanical coupling (ω′=50\omega'=50 cm−1^{-1}). Straight and dotted lines represent the pressure-dependencies of the frequencies of the raw-uncoupled Be-Te modes behind the coupled ones. In panels (b, c), a color code is used to distinguish between the raw-uncoupled TO’s stemming from domestic (red) and foreign (blue) environments. Paired vertical – horizontal arrows (in panels (b–f)) emphasize pressure-induced changes in Raman intensity – frequency for a given mode.

Raman measurements at 0 GPa / 300 K with the red (632.8 nm) and blue (488.0 nm) laser lines (nearly resonant with the E0E_0 and / or E0+Δ0E_0+\Delta_0 electronic transitions of Be-dilute Cd1−x_{1-x}Bex_xTe, Figure 1b) fail to reveal the Be-Te doublet (Fig. S7). Only one Be-Te mode is visible, at ∼\sim390 cm−1^{-1}, consistent with the scarce experimental (far-infrared) data in the literature[56] and existing calculations using the Green’s function theory[57], far away from the (TO, LO) CdTe-lattice band (140–170 cm−1^{-1}). This line is assigned as the upper/main TOBe−TeCdTO^{Cd}_{Be-Te}, by analogy with TOBe−TeZnTO^{Zn}_{Be-Te} of Zn1−x_{1-x}Bex_xTe. The lower/minor TOBe−TeBeTO^{Be}_{Be-Te} band is not visible, presumably screened by the second-order CdTe-lattice signal (2LOCd−Te2LO_{Cd-Te}) that emerges as a strong feature nearby, being emphasized / reduced with the red / blue laser excitation.

The conditions for testing the PM are improved by keeping the blue laser line but working at high pressure and low temperature (80 K), that offers a number of benefits. First, the Be-Te signal sharpens due to the increased phonon lifetime. Second, the pressure domain of the native zincblende phase enlarges[58]. Third, the low temperature slows down the formation of Te aggregates under intense laser exposition such as achieved by focusing the laser beam onto a tiny sample placed in a diamond anvil cell—a notorious problem with CdTe-like crystals[59]. The Raman spectra taken in the upstroke up to 4.3 GPa in the native zincblende phase of Cd0.89_{0.89}Be0.11_{0.11}Te (Figure 2b) transiently reveal the target lower / minor TOBe−TeBeTO^{Be}_{Be-Te} (marked by an asterisk) on the low-frequency side of the main TOBe−TeCdTO^{Cd}_{Be-Te} at ∼\sim3.5 GPa, before its partial resorption at ∼\sim4.3 GPa. This is consistent with TOBe−TeBeTO^{Be}_{Be-Te} suffering a progressive collapse while converging towards TOBe−TeCdTO^{Cd}_{Be-Te} prior to its extinction at the crossing / resonance, as observed with the reference Be-Te doublet of Zn0.89_{0.89}Be0.11_{0.11}Te across a similar pressure range (2.3–7.9 GPa)[40]. This fits into scenario 1 of the convergence process (cf. the issue 4).

Although the analogy with Zn0.89_{0.89}Be0.11_{0.11}Te is enlightening, it remains limited to grasp the behaviour of Cd0.89_{0.89}Be0.11_{0.11}Te. Additional support is searched for by calculating the high-pressure ab initio (AIMPRO) Cd1−x_{1-x}Bex_xTe Raman spectra at small-to-moderate (x∼x\sim0, 0.5) Be content. However, a limit to pressure is set by the supercells becoming unstable from 10 GPa (x∼x\sim0, not shown) and 15 GPa (x∼x\sim0.5, Fig. S7) onwards. The stability improves at large Be content (x∼x\sim1), also considered to complete an ab initio Raman insight at well-spanned xx values across the composition domain (Figure 2c, Figure 2d and Figure 2e).

Paired impurities (forming a duo connected via Te, as schematized in Figure 2a) in large parent supercells represent the minimal impurity motif offering a clear distinction, in the context of the PM, between “impurity” and “host” vibrations in “domestic” and “foreign” environments (labels ii-to-iviv in Figure 2a), hence four situations in total at both ends of the composition domain (x∼x\sim0 – Figure 2c and x∼x\sim1 – Figure 2e). The duo-impurity modes are identified via their wavevectors, depending on whether they point along the duo (in-chain, noted iiii and symbolized by ↔\leftrightarrow) or perpendicular to it (out-of-chain, noted ii and marked ↔\leftrightarrow, yielding five possible variants[40]). For the host / dominant bond species, the distinction between “foreign” and “domestic” environments is established through the Raman intensity, being small next to the impurity-duo (close-duo, noted iviv, the “foreign” case) and large away from it (bulk, noted iiiiii, the “domestic” case). Additional insight at maximum alloy disorder (xx=0.5 – Figure 2d) using a nominally random Cd54_{54}Be54_{54}Te108_{108} supercell (see methods) completes the ab initio picture.

Ab initio results do reveal an actual Cd-Te percolation doublet for Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} at x∼0x \sim0 (Figure S6) and 1 (Figure S6), albeit a compact one (Figure 2a) – cf. the issue 1, with TOCd−TeBeTO_{\mathrm{Cd-Te}}^{\mathrm{Be}} set below TOCd−TeCdTO_{\mathrm{Cd-Te}}^{\mathrm{Cd}} – cf. the issue 2, as expected. The frequency gap ΔCd−Te\Delta_{\mathrm{Cd-Te}} hardly exceeds a few cm−1\mathrm{cm}^{-1} (that won’t be detectable in experiment) meaning that the Cd-Te vibration is almost blind to the local environment. At x∼1x \sim1 the upper TOCd−TeCdTO_{\mathrm{Cd-Te}}^{\mathrm{Cd}} is frozen (not Raman active, the frozen mode – identified by its wavevector – is spotted by an arrow in Figure S6) due to a phonon exceptional point being achieved already at 0 GPa – cf. the issue 4. At x∼0x \sim0 the Cd-Te doublet becomes inverted by increasing pressure to 5 GPa (Figure S6) – cf. the issues 3 and 4. Altogether, this offers a perfect analogy with the Zn-Te doublet of the reference Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te} case [40].

High-pressure ab initio (AIMPRO) CdTe-like Raman signals of Cd₁₋ₓBeₓTe generated by impurity-duos

Figure S6. High-pressure ab initio (AIMPRO) CdTe-like Raman signals of Cd1−x_{1-x}Bex_xTe generated by impurity-duos (x∼0,1x \sim0,1). (a) Cd106_{106}Be2_2Te108_{108}. (b) Cd2_2Be106_{106}Te108_{108}. Under pressure the CdTe-like branches either cross (as emphasized by a curved arrow) or freeze (the concerned submode is spotted by vertical arrows) at the resonance, as sketched out.

The analogy between Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} and Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te} is not as clear in their common Be-Te spectral range, successively addressed hereafter with Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} at small, intermediary and large Be contents.

At x∼0x \sim0 (Figure 2c), the Be-duo generates a nominal percolation-type (lower / in-chain TOBe−TeBeTO_{\mathrm{Be-Te}}^{\mathrm{Be}}, upper / out-of-chain TOBe−TeCdTO_{\mathrm{Be-Te}}^{\mathrm{Cd}}) Raman doublet at 0 GPa with a large separation (ΔBe−Te∼35 cm−1\Delta_{\mathrm{Be-Te}} \sim35\ \mathrm{cm}^{-1}) – conforming to the issue 2. Not surprisingly, the corresponding (TOBe−TeBeTO_{\mathrm{Be-Te}}^{\mathrm{Be}}, TOBe−TeZnTO_{\mathrm{Be-Te}}^{\mathrm{Zn}}) doublet in Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te} is less resolved (ΔBe−Te∼20 cm−1\Delta_{\mathrm{Be-Te}} \sim20\ \mathrm{cm}^{-1}) [40] due to the smaller bond (Δll,Δa3a3)(\frac{\Delta l}{l},\frac{\Delta a^{3}}{a^{3}})-contrast in Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te} (∼\sim9%, ∼\sim31%) than in Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} (∼\sim15%, ∼\sim36%). As pressure is increased TOBe−TeBeTO_{\mathrm{Be-Te}}^{\mathrm{Be}} gets closer to TOBe−TeCdTO_{\mathrm{Be-Te}}^{\mathrm{Cd}} – cf. the issue 3 – and suffers a major collapse, to such extent that both its Raman intensity and ΔBe−Te\Delta_{\mathrm{Be-Te}} are halved (Figure 2c), i.e., the early signs of a phonon exceptional point on the verge of being achieved, in line with scenario 1 – cf. the issue 4. Generally, this finds echo in experimental findings – even though TOBe−TeBeTO_{\mathrm{Be-Te}}^{\mathrm{Be}} shows up as a mere shoulder on TOBe−TeCdTO_{\mathrm{Be-Te}}^{\mathrm{Cd}} in experiment (marked by an asterisk in Figure 2b), whereas it emerges as a distinct feature in ab initio data (Figure 2c). This might relate to a basic difference at minor Be content that ab initio calculations run on an “ideal” lattice – verified by the B0B_{0} vs. xx linearity – whereas the real lattice suffers a massive B0B_{0}-drop in experiment (Figure 1d).

At x∼0.5x \sim0.5 (Figure 2d), scenario 1 still applies, as expected – cf. the issue 4. At 0 GPa, the Be-Te Raman signal of Cd54Be54Te108\mathrm{Cd}_{54}\mathrm{Be}_{54}\mathrm{Te}_{108} (x=0.5x=0.5) shows up as a unique broad TOBe−TeTO_{\mathrm{Be-Te}} band. At 5 GPa, this latter transforms into a compact percolation-type (TOBe−TeBeTO_{\mathrm{Be-Te}}^{\mathrm{Be}}, TOBe−TeCdTO_{\mathrm{Be-Te}}^{\mathrm{Cd}}) doublet subsided on its low-frequency side. At 10 GPa, the doublet further shrinks and the subsidence is emphasized to such extent that, apparently, only TOBe−TeCdTO_{\mathrm{Be-Te}}^{\mathrm{Cd}} survives, and TOBe−TeBeTO_{\mathrm{Be-Te}}^{\mathrm{Be}} is killed. This nicely recapitulates the sequence leading to the achievement of a phonon exceptional point – cf. the issue 4. The sequence is interrupted from 15 GPa on, due to the collapse of the zincblende structure in the supercell used, manifested by a departure of bond angles from the nominal tetrahedral value (109°, Fig. S7).

At x∼1x \sim1 (Figure 2e), the situation becomes irregular. While well separated when stemming from the Be-duo (x∼0x \sim0), the (TOBe−TeBeTO_{\mathrm{Be-Te}}^{\mathrm{Be}}, TOBe−TeCdTO_{\mathrm{Be-Te}}^{\mathrm{Cd}}) doublet of Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} becomes quasi degenerate (TOBe−TeBe≡TOBe−TeCdTO_{\mathrm{Be-Te}}^{\mathrm{Be}} \equiv TO_{\mathrm{Be-Te}}^{\mathrm{Cd}}) at 0 GPa when due to the Cd-duo (x∼1x \sim1). Indeed, various minor features composing TOBe−TeCdTO_{\mathrm{Be-Te}}^{\mathrm{Cd}} (marked by asterisks in Figure 2e) do overlap with the main TOBe−TeBeTO^{Be}_{Be-Te}. In contrast, the (TOBe−TeBeTO^{Be}_{Be-Te}, TOBe−TeZnTO^{Zn}_{Be-Te}) doublet of the reference Zn1−x_{1-x}Bex_xTe case is globally preserved across the composition domain[40].

The quasi degeneracy of the Be-Te Raman doublet of Cd1−x_{1-x}Bex_xTe at x∼1x \sim1 from 0 GPa undermines the possibility for scenario 2 to develop under pressure – cf. the issue 4 – offering a novel case study.

Under pressure, the TOBe−TeBeTO^{Be}_{Be-Te} and TOBe−TeCdTO^{Cd}_{Be-Te} lines, already close at 0 GPa, are forced to further proximity – because the local environment becomes less discriminatory between like bond vibrations under pressure[40] – and hence do couple mechanically. This mediates a transfer of the oscillator strength from the main to the minor mode, directly impacting the Raman intensities. Remarkably, the Be-Te oscillator strength is channeled from high to low frequency in the Cd1−x_{1-x}Bex_xTe case (x∼1x \sim1, as emphasized by a vertical arrow in Figure 2e), and not the other way around as observed in the reference Zn1−x_{1-x}Bex_xTe (x∼1x \sim1) case[40]. This can be explained only if the minor TOBe−TeCdTO^{Cd}_{Be-Te} (recipient of oscillator strength) lies below the main TOBe−TeBeTO^{Be}_{Be-Te} (donor of oscillator strength) at 0 GPa. Hence, at 0 GPa the Be-Te doublet of Cd1−x_{1-x}Bex_xTe (x∼1x \sim1) is inverted relative to its regular Zn1−x_{1-x}Bex_xTe counterpart (x∼1x \sim1) – and not only degenerated. Specifically, the vibration lines follow (upwards) in the (TOBe−TeCdTO^{Cd}_{Be-Te}, TOBe−TeBeTO^{Be}_{Be-Te}) order – pay attention to the superscripts, as opposed to the regular (TOBe−TeBeTO^{Be}_{Be-Te}, TOBe−TeZnTO^{Zn}_{Be-Te}) order with Zn1−x_{1-x}Bex_xTe[40] (x∼1x \sim1) – cf. the issue 2.

In earlier work[60] we have shown that the shape of the upper (best-resolved) TO percolation doublet in a “Raman frequency vs. xx” plot may vary a lot (parallel branches vs. trapezoidal / triangular distortions) depending on whether the parent TO is dispersive or not. The main arguments are briefly recalled hereafter by focusing on the lower parent–iviv and upper impurity–iiiiii modes forming the percolation doublet in the parent limit. Only the latter mode is subject to dispersion, not the former one, so that their comparison provides a straightforward insight into the dispersion effect.

In absence of dispersion (as, e.g., for GaP), the iiiiii–iviv frequency gap is governed by the local strain due to the bond mismatch (between, e.g., Ga-As and Ga-P in the case of GaAs1−x_{1-x}Px_x), resulting in parallel branches across the composition domain[60]. The TO mode of CdTe is nearly dispersionless[61], so that the Cd-Te doublet of Cd1−x_{1-x}Bex_xTe actually exhibits such parallelism (Figure 2a). In case of a positive (resp. negative) dispersion, iiiiii is upward (resp. downward) shifted with respect to iviv roughly by the magnitude of the dispersion, with concomitant on the iiiiii–iviv frequency gap being enlarged – trapezoidal distortion – (resp. squeezed – triangular distortion), as observed[60] with ZnSe1−x_{1-x}Sx_x (resp. Si1−x_{1-x}Gex_x).

We are mainly interested in the negative TO dispersion (with Cd1−x_{1-x}Bex_xTe, see below). In this case an inversion of the percolation doublet occurs if the dispersion effect outweighs the effect of the local strain (as observed, e.g., with the Si-Si doublet of Si1−x_{1-x}Gex_x at x∼0x \sim0 – Ref.[60]). Such an inversion does not occur in the dilute limit, because, being impurity modes, the ii and iiii forming the percolation doublet at this limit suffer a similar dispersion effect. Since the percolation doublet is inverted in the parent limit but regular in the dilute one, its two sub-branches should cross at a certain composition. Such crossing was not observed yet – not even with Si1−x_{1-x}Gex_x (due to the ii-iiii degeneracy[60] at x∼1x\sim1).

The TO mode of BeTe exhibits a large negative dispersion[62] (∼50\sim50 cm−1^{-1}). Accordingly, in both Zn1−x_{1-x}Bex_xTe[40] and Cd1−x_{1-x}Bex_xTe the Be-Te splitting is smaller in the parent limit (x∼1x\sim1, iiiiii-iv∼7iv\sim7 cm−1^{-1} – Ref.[40] and ∼0\sim0 cm−1^{-1} – Figure 2d, respectively) than in the dilute one (x∼0x\sim0, iiiiii-iv∼30iv\sim30 cm−1^{-1} – Ref.[60] and ∼45\sim45 cm−1^{-1} – Figure 2c, respectively). Based on ab initio (SIESTA) calculations done on the Be-Te impurity-ii mode of Cd1−x_{1-x}Bex_xTe (Sec. SII.1) – taken as representative for all (ii-to-iiiiii) Be-Te impurity modes – the Be-Te doublet at x∼0x\sim0 (ii-iiii) is downshifted by ∼11\sim11 cm−1^{-1} due to the dispersion effect (short vertical arrows in Figure 2a at x∼0x\sim0). A crude view of the (virtual) Be-Te doublet of Cd1−x_{1-x}Bex_xTe due to the sole effect of the local strain, i.e., deprived of dispersion, is reconstructed by drawing parallel Be-Te sub-branches (dashed lines, taken straight in a first approximation) – by analogy with the dispersionless Ga-P doublet of GaAs1−x_{1-x}Px_x (Ref.[60]) – between the (virtual) Be-Te doublet inferred at x∼0x\sim0 in absence of dispersion and the same doublet attached to the parent TO mode at x∼1x\sim1.

When confronted with ab initio data at x∼1x\sim1 – taking into account blindly the effects of strain and dispersion, the above-derived (virtual) strain-related Be-Te doublet appears to be seriously challenged by the TO dispersion, whether considering Cd1−x_{1-x}Bex_xTe or Zn1−x_{1-x}Bex_xTe. In the latter case, however, the effect of the local strain dominates so that the ordering of Be-Te branches is nicely preserved across the composition domain[40], even if the branches do not run exactly parallel (cf. the comparison between the ii-iiii and iiiiii-iviv frequency gaps). In Cd1−x_{1-x}Bex_xTe the effect of the dispersion achieves maximum at x∼1x\sim1 (long vertical arrow, Figure 2a) and overwhelms the effect of the local strain. This leads to an inversion of the Be-Te doublet (x∼1x\sim1), preceded by the crossing of Be-Te sub-branches (x∼0.8x\sim0.8) – an unprecedented case among all re-examined alloys within the PM so far.

Generally, the small / large Be-Te dispersion effect in Zn1−x_{1-x}Bex_xTe / Cd1−x_{1-x}Bex_xTe at x∼1x\sim1 reflects a small / large (negative) impact of the local lattice distortions due to the Zn / Cd ↔\leftrightarrow Be atom substitution on the Be-Te vibrations (the minimum / maximum Be-Te dispersion effect at x∼0x\sim0 / ∼1\sim1 in Cd1−x_{1-x}Bex_xTe – compare the lengths of arrows in Figure 2a – can be discussed on the same line). However, Cd1−x_{1-x}Bex_xTe is not so much remarkable than Zn1−x_{1-x}Bex_xTe with this respect, as the dispersion effect usually achieves maximum for the impurity modes of alloys, even in case of WMA’s. The distorted percolation doublets of ZnSe1−x_{1-x}Sx_x and Si1−x_{1-x}Gex_x were discussed on this basis[60]. The Ga-As impurity mode likewise experiences the same (maximal) dispersion effect whether taken in the lattice-matched Ga1−x_{1-x}Alx_xAs (Δl/l∼8%\Delta l/l\sim8\%) or lattice-mismatched Ga1−x_{1-x}Inx_xAs (Δl/l∼7%\Delta l/l\sim7\%) alloys[63].

At this stage, the inversion of the Be-Te Raman doublet at x≥0.8x \ge0.8 is (qualitatively) explained. Now we examine how the mechanical coupling develops between the inverted Be-Te submodes when forced to (further) proximity by pressure. The discussion is conducted in reference to the uncoupled case represented in Figure 2a.

The uncoupled modes of Figure 2a are modeled by assimilating the TO Raman cross section with the imaginary part of the relative dielectric function εr\varepsilon_r (that captures the εr→∞\varepsilon_r \to\infty divergence characteristic of a purely-mechanical TO)[64]. The adopted four-mode {2×(Cd−Te),2×(Be−Te)}\{2 \times(Cd-Te), 2 \times(Be-Te)\} description conforms with the current ab initio findings—referring to the end ii-to-iviv modes. A sensitivity of both bond vibrations to their local (CdTe- and BeTe-like) environments at the first-neighbor scale is assumed by analogy with Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_x\mathrm{Te}[40], impacting the Raman intensities. The mechanical bond force constants are linearly interpolated between the parent and impurity ab initio values, leading to quadratic xx-dependencies of the TO frequencies. A uniform broadening (1 cm−1^{-1}) is used, so that the Raman intensities (color code) can be directly compared. The remaining input parameters are determined ab initio (Sec. SIII.2); no adjustable parameters are used. The ab initio frequencies are slightly shifted upwards with respect to the experimental ones (symbols – Figure 2a) – by a few cm−1^{-1} for pure CdTe (hollow symbols) and by less than 15 cm−1^{-1} for pure BeTe (filled symbols) – due to a generally known bias of the local density approximation, innate to our ab initio calculations, to overbind and hence to overestimate the bond force constants – except for the Be-Te impurity-ii mode at x∼0x \sim0 (hollow symbols) for which a nearly perfect matching occurs.

Fair modeling of the pressure-induced interplay between the ab initio Raman intensities of the two Be-Te submodes forming the irregular-inverted (TOBe−TeCd,TOBe−TeBeTO^{Cd}_{Be-Te}, TO^{Be}_{Be-Te}) percolation doublet of Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_x\mathrm{Te} near the crossing of percolation branches (x∼1x \sim1, Figure 2e) can be achieved within a dielectric parametrization of two like (TOBe−Te−,TOBe−Te+TO^{-}_{Be-Te}, TO^{+}_{Be-Te}) mechanically-coupled harmonic oscillators (Figure 2f) – ranked in order of frequency, by slightly adapting the approach developed in Ref.[40] – notably using there a simplified form of eq:7 a – see Sec. SIII.2. The pressure dependence of the parent BeTe oscillator strength is taken into account as done in Ref.[40]. For better visualization of trends, the dielectric study has been moved from dilute (x∼1x \sim1) to minor (x=0.81x = 0.81) Cd content – further offering a direct comparison with the regular Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_x\mathrm{Te} case (referring to Fig. 1c of Ref.[40]). A small mechanical coupling is used (with characteristic frequency ω′=50\omega' = 50 cm−1^{-1}, similar to that used with ZnBeTe[40]) scaled down by (roughly) an order of magnitude with respect to the TO frequencies (∼480\sim480 cm−1^{-1}) of the raw-uncoupled (TOBe−TeCd,TOBe−TeBeTO^{Cd}_{Be-Te}, TO^{Be}_{Be-Te}) oscillators (whose pressure dependence are represented by straight and dotted lines in Figure 2f, correspondingly). The small coupling successfully mimics the minimal – but finite – ab initio splitting manifesting the anticrossing (∼3\sim3 cm−1^{-1}, emphasized by paired arrows in Figure 2f) of the coupled (TOBe−Te−,TOBe−Te+TO^{-}_{Be-Te}, TO^{+}_{Be-Te}) near the resonance – corresponding to frequency matching of the raw-uncoupled oscillators. At this limit, the mechanical coupling achieves maximum (∼20\sim20 GPa) and the two Be-Te TO submodes exhibit comparable Raman intensities. A further pressure increase eventually results in a proper doublet inversion (30 GPa, Figure 2f) – as the oscillators tend to decouple by shifting away from the resonance. Such inversion manifests, in fact, the free coupling of Be-Te oscillators at the resonance in Cd1−x_{1-x}Bex_xTe – cf. the issue 4.

The free Be-Te coupling is also observed with Zn1−x_{1-x}Bex_xTe[40] (x∼1x\sim1), only that the transfer of Be-Te oscillator strength mediated by the mechanical coupling is opposite (due to inversion of the native Be-Te Raman doublets with respect to Cd1−x_{1-x}Bex_xTe at 0 GPa – see above). A further difference relates to the Be-Te convergence rate under pressure at x∼1x\sim1, being fast for Zn1−x_{1-x}Bex_xTe (the inversion is completed already at ∼10\sim10 GPa, Ref. 40) and slow for Cd1−x_{1-x}Bex_xTe (the inversion is still in progress at the largest tested pressure of 20 GPa in our ab initio data – Figure 2e, being delayed to ∼30\sim30 GPa in view of our dielectric parametrization of Raman lineshapes – Figure 2f). This reflects different driving forces behind the pressure-induced Be-Te convergence processes, namely the regular ∂fi/∂ln⁡V\partial f_i/\partial\ln V-mechanism for Zn1−x_{1-x}Bex_xTe – cf. the issue 3, and for Cd1−x_{1-x}Bex_xTe just a basic trend for like bonds to behave uniformly under pressure (the local environment becoming less discriminatory at high pressure[40], as already mentioned). Anyway, the free coupling of the inverted / irregular Be-Te doublet of Cd1−x_{1-x}Bex_xTe at large Be content (Figure 2e and Figure 2f) opposes the phonon exceptional point achieved at minor-to-moderate Be content (Figure 2b, Figure 2c and Figure 2d), conforming to scenarii 2 and 1 in the main lines – cf. the issue 4.

Conclusion

Among Be-based highly mismatched alloys (HMA’s), Cd1−x_{1-x}Bex_xTe achieves maximum contrast in bond properties, exacerbating its vibrational-mechanical properties. As such, Cd1−x_{1-x}Bex_xTe is an appealing benchmark to test the limit of the percolation model (PM) that so far provided a unified understanding of the Raman spectra of semiconductor alloys – covering well matched alloys (WMA’s) as well as HMA’s.

The Cd1−x_{1-x}Bex_xTe mechanical-vibrational properties are studied experimentally (x≤0.11x \le0.11) by addressing the bulk modulus B0B_0 and the effective bond force constants, using high-pressure X-ray diffraction and high-pressure Raman scattering in combination. The discussion of experimental data is supported by high-pressure ab initio (SIESTA, AIMPRO) snapshots at moderate Be contents (x≤0.3x \le0.3), extended to intermediary (x∼0.5x\sim0.5) and large (x∼1x\sim1) Be contents situated beyond the experimental stage.

Cd1−x_{1-x}Bex_xTe exhibits degraded mechanical-vibrational properties across the composition domain, at both the macroscopic and microscopic scales. On minor Be incorporation (x∼0x\sim0), the bulk modulus suffers a counterintuitive drop below the CdTe value. At large Be content (x∼1x \sim1) and ambient pressure, the percolation-type Raman signal of the sensitive Be-Te bond is fully relaxed by the phonon dispersion, down to inversion – an unprecedented case among revisited alloys within the PM so far. Yet, the percolation scheme is not challenged for all that and basically applies as such to Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te}. In fact, the Be-Te bond exhibits a mere bimodal Raman pattern at any composition, and not a more complicated one. Further, the pressure-induced convergence of the Be-Te Raman doublet either ends up into a phonon exceptional point at minor-to-moderate Be content or develops into a free mechanical coupling at large Be content, in line with predictions. This reinforces the status of the PM as a robust (phenomenological) descriptor of phonons in semiconductor alloys.

Methods

This Section provides details on the samples and various experimental techniques and simulation (numerical and analytical) methods used to probe and / or to support the discussion on the structural, electronical and / or vibrational properties of Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te}, depending on pressure.

Samples. Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} (x=0x=0, 0.03, 0.05, 0.07, 0.11) and Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te} (x=0.04x=0.04, 0.21) free-standing single crystals required for high-pressure (Raman scattering and / or X-ray diffraction) measurements are grown from the melt by mixing high-purity CdTe and ZnTe (99.9995, i.e., 5N quality) with Be (99.5, i.e., 2N quality) using the Bridgman method[65]. The Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} composition is determined better than 1% by selective Cd and Be dosing via the inductively coupled plasma (ICP) method applied to powders. All samples crystallize in the native zincblende structure of CdTe and BeTe, verified by powder X-ray diffraction measurements at 0 GPa – Sec. S.I. The Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te} composition is derived from the linear composition dependence of the lattice constant[46] measured at 0 GPa by powder X-ray diffraction.

Solid-state nuclear magnetic resonance measurements. Solid-state nuclear magnetic resonance measurements of the chemical shift due to the invariant Te species of Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} are performed on a finely ground powder (∼20\sim20 ml) obtained from the largest crystal piece at hand (x=0.07x=0.07) to test whether the Cd↔\leftrightarrowBe atom substitution is ideally random, or not (i.e., subject to clustering or antic lustering). For all solid-state NMR spectra, Bruker 2.5 mm double resonance probes are used and the magic angle spinning frequency is set to 25 kHz. 125Te{}^{125}\mathrm{Te}, 113Cd{}^{113}\mathrm{Cd} and 9Be{}^{9}\mathrm{Be} longitudinal relaxation times (T1T_{1}), respectively 450 s, 840 s and 175 s, are measured using standard saturation recovery experiments. Recycle delays of 5 times T1T_{1} are then used to ensure quantitativity. 125Te{}^{125}\mathrm{Te} NMR spectrum is acquired on a Bruker Avance III spectrometer operating at 7 T (corresponding to 300 MHz 1H{}^{1}\mathrm{H} resonance frequency). The direct-acquisition Carr-Purcell-Meiboom-Gill (CPMG) experiment[66] enables to record, in each scan, 49 full echoes with 400 ms acquisition time. 256 scans are accumulated in 7 days and 9 hours. 113Cd{}^{113}\mathrm{Cd} and 9Be{}^{9}\mathrm{Be} NMR standard direct acquisition experiments are recorded on a Bruker Avance III 600 MHz spectrometer (14 T). Respectively 112 and 56 transients are recorded, for a total experimental time of 5 days 10 h for 113Cd{}^{113}\mathrm{Cd} and 15 h for 9Be{}^{9}\mathrm{Be}.

Ellipsometry measurements. Near the direct absorption edge, the square root of the deviation (E−E0E-E_{0}) from the fundamental band gap (E0E_{0}) scales linearly with the energy (EE) weighted by the absorption coefficient (α\alpha). E0E_{0} is obtained by measuring such so-called Tauc plots[67] in the visible using non-oriented crystal pieces with parallel faces polished to optical quality – both directly, in a transmission experiment at normal incidence, and indirectly, by ellipsometry at a near-Brewster incidence (using a HORIBA UVISEL phase modulated spectroscopic ellipsometer). Higher interband transitions (E1E_{1}, E1+E_{1}+ Δ1\Delta_{1}, E2E_{2}) on top of E0E_{0} are accessed via a direct (model-free) wavelength-per-wavelength inversion of spectrometric ellipsometry data (the sine and cosine of the depolarization angles).

(High-pressure) X-ray diffraction measurements. High-pressure powder X-ray diffractograms are recorded on the PSICHÉ (Cd0.89_{0.89}Be0.11_{0.11}Te) and CRISTAL (Zn1−x_{1-x}Bex_xTe, x=0.045x=0.045, 0.14 and 0.21) beamlines of SOLEIL synchrotron using radiation wavelengths of 0.3738 Å and 0.485 Å, respectively. The high-pressure data are recorded with a similar Chervin type diamond anvil cell[68] (with 300 μ\mum in diameter diamond culet) as for the Raman measurements (see below), using, in both cases, Ne and Au as the pressure transmitting medium and for pressure calibration, respectively. The high-pressure X-ray data are treated by using the DIOPTAS[69] software at PSICHÉ and the DATLAB software – kindly provided by K. Syassen (Max-Planck Institut für Festkörperphysik, Stuttgart, Germany) – at CRISTAL. The B0B_{0} value of the native zincblende phase at 0 GPa is obtained by fitting the Birch-Murnaghan’s equation of state to the pressure dependence of the unit cell volume[51]. The volume of the unit cell at 0 GPa coming into the cited equation is determined from powder X-ray diffraction measurement done at 0 GPa in laboratory conditions using the CuKα\alpha radiation.

(High-pressure) Raman scattering measurements. High-pressure / low-temperature Raman experiment on Cd0.89_{0.89}Be0.11_{0.11}Te is done in the backscattering geometry by focusing the laser beam through a ×50 microscope objective with a long working distance at normal incidence onto a 40 μ\mum in diameter spot at the (non-oriented) surface (polished to optical quality) of a tiny monocrystal inserted into a Chervin type diamond anvil cell (described above) set into a Helium flow cryostat system operated at liquid nitrogen temperature. CdTe-based crystals being notoriously poor Raman scatterers[59], near-resonant conditions are used to enhance the Raman signal, as best achieved at 300 K and 77 K by using the 632.8 nm line of a helium-neon laser, falling in between E0E_{0} and E0+Δ0E_{0}+\Delta_{0}, and the 488.0 nm line of an argon laser, near-resonant with E0+Δ0E_{0}+\Delta_{0}, respectively. Fair modeling of the Raman signal due to uncoupled or mechanically-coupled TO oscillators is achieved within a linear dielectric function approach, adapted from Ref.[40] (Sec. SIII).

(High-pressure) ab initio insights into the lattice relaxation/dynamics. Three ab initio codes operated within the density functional theory, using pseudopotentials and the local density approximation for the exchange-correlation, are employed, according to need. Reference B0B_{0} vs. xx curves for Cd1−x_{1-x}Bex_xTe at moderate Be content (x≤0.3x\leq0.3) are separately obtained by applying the SIESTA[43, 44] and AIMPRO (Ab Initio Modeling PROgram[41, 42]) codes to distinct series of large (64- and 216-atom, respectively) fully-relaxed (lattice constant, atom positions, supercell shape) and partially-relaxed (preventing any supercell distortion so as to maintain the cubic structure needed for a strict application of the Birch-Murnaghan[51] equation of state) disordered zincblende-type supercells, correspondingly. Each supercell represents a random Cd↔Be substitution, obtained by adjusting the fractions of individual Te-centred tetrahedra to the binomial Bernouilli distribution[39]. At each xx value, B0B_{0} is estimated by fitting the pressure dependence of the volume unit cell with the Birch-Murnaghan equation of state[51]. Further AIMPRO calculations are done on parent-like supercells containing Be- (x∼0x \sim0) or Cd-paired (x∼1x \sim1) impurity motifs, searching to imitate the limiting-cases Raman signals due to the non-polar (purely-mechanical) TO’s of the host and impurity species, using the formula given by de Gironcoli[70]. In their current versions, the AIMPRO and SIESTA codes do not take into account the long-range electric field accompanying the Raman-active polar LO’s. Further simulations thus resorted to QE code[45], giving access to ωT\omega_{T} (the frequency of the non-polar TO), ωL\omega_{L} (the frequency of the Raman-active polar LO) and ε∞\varepsilon_{\infty} (the high-frequency relative dielectric constant, i.e., as defined at ω≫ωT\omega\gg\omega_{T}) of BeTe and CdTe, calculated for (2×2×2)(2 \times2 \times2) cubic zincblende-type supercells (64 atoms). From these, the static relative dielectric constant εs\varepsilon_{s} (defined at ω≪ωT\omega\ll\omega_{T}) could have been extracted by force of the LST relation[71], to be further used to estimate the phonon oscillator strengths within the classical form of the relative Cd1−x_{1-x}Bex_{x}Te dielectric function εr\varepsilon_{r}, used in our simplified analytical expression of the Cd1−x_{1-x}Bex_{x}Te Raman cross section (Sec. SIII).

Data availability statement

The reported experimental (high-pressure Raman, high-pressure X-ray diffraction, nuclear magnetic resonance) and ab initio (AIMPRO, SIESTA and QE codes) data in this work are available upon request to the corresponding author.

Acknowledgements

We acknowledge assistance from the PSICHÉ (Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te}, Proposal n°. 20220436, co-resps. O.P. & A.P.) and CRISTAL (Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te} Proposal n°. 20110018, resp. A.P.) beamlines of synchrotron SOLEIL for the high-pressure X-ray diffraction measurements, from the Plate-forme de Spectroscopie – Institut de Minéralogie, de Physique des Matériaux et de Cosmochimie – Sorbonne Université (http://impmc.sorbonne-universite.fr/fr/plateformes-et-equipements/plateforme-de-spectroscopie.html), from the Nuclear Magnetic Resonance platform of Institut Jean Barriol (CNRS FR 3843, Université de Lorraine – https://www.ijb.univ-lorraine.fr), from the Ellipsometry core facility of LCP-A2MC (Université de Lorraine – https://lcp-a2mc.univ-lorraine.fr) and from the IJL core facility (Université de Lorraine – http://ijl.univ-lorraine.fr/recherche/centres-de-competences/rayons-X-et-spectroscopie-moessbauer-X-gamma) for the X-ray diffraction measurements at ambient pressure.

The SIESTA and QE calculations have been done using the facilities of the EXPLOR mesocentre of the Université de Lorraine (project 2019CPMXX0918). VJBT acknowledge the FCT through projects LA/P/0037/2020, UIDB/50025/2020 and UIDP/50025/2020 in relation to the AIMPRO calculations.

Affiliations

Université de Lorraine, LCP-A2MC, ER 4632, F-57000 Metz, France

A. Elmahjoubi, M. B. Shoker, O. Pagès, A.V. Postnikov, A. EnNaciri, L. Broch, R. Hajj Hussein & P. Franchetti

Departamento de Fisica and i3N, Universidade de Aveiro, 3810 – 193 Aveiro, Portugal

V. J. B. Torres

Institut de Minéralogie, de Physique des Matériaux et de Cosmochimie, Sorbonne Université — UMR CNRS 7590, F-75005 Paris, France

A. Polian, C. Bellin & K. Beneut

Université de Lorraine, Laboratoire de Cristallographie, Résonance Magnétique et Modélisations, CRM2, UMR 7036, Vandoeuvre-lès-Nancy, F-54506, France

C. Gardiennet & G. Kervern

Synchrotron SOLEIL, L’Orme des Merisiers Saint-Aubin, BP 48 F-91192 Gif-sur-Yvette Cedex, France

J.-P. Itié, L. Nataf & S. Ravy

Université de Lorraine, CNRS, IJL, F-57000, Metz, France

S. Diliberto & S. Michel

Faculty of Physics, Astronomy and Informatics, Institute of Physics, Nicolaus Copernicus University in Toruń, ul. Grudziądzka 5, 87-100 Toruń, Poland

A. Abouais & K. Strzałkowski

Chouaib Doukkali University of El Jadida, National School of Applied Sciences, Engineering Science for Energy Lab, El Jadida, Morocco

A. Abouais

Author Contributions Statement

High-quality / purity Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} (x≤0.11x \le0.11) and Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te} (x≤0.21x \le0.21) free-standing single crystals with zincblende structure were grown by using the Bridgman method (A.A. & K.S.). The Cd↔Be substitution was checked to be ideally random by applying solid-state nuclear magnetic resonance to a (large) powdered sample (x=0.07x = 0.07 – G.K. & C.G.). The composition of Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} alloys was determined by using the induced coupling plasma method (S.M.). X-ray diffraction measurements on powders were done in laboratory at ambient pressure across the sample series (S.D.) – to check the crystal structure and to determine the xx-dependence of lattice constant(s) – and under pressure at the PSICHÉ (Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} – A.P., M. B. S. & O. P. with the assistance of J.-P.I) and CRISTAL (Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te} – A.P., R. H. H. & O. P. with the assistance of L.N. & S.R.) beamlines of SOLEIL synchrotron – to determine the pressure domain of the native zincblende phase together with sequence of pressure-induced structural transitions. The high-pressure X-ray data were subsequently analyzed using the software DIOPTAS (A.E.) and DATLAB (M.B.S. & R.H.H.). The Be-Te Raman signal of Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} was studied at ambient-pressure / low-temperature (A.E., M.B.S & O.P., with the assistance of P. F.) and high-pressure / low-temperature (x=0.11x = 0.11 – A.P., C.B., K.B., A. E. & O.P.) using single crystals. Ab initio calculations of high-pressure Raman spectra, bulk modulus (B0B_0) and various parameters (ε∞\varepsilon_{\infty}, TO-LO splitting) needed to implement the linear dielectric function approach were done by using AIMPRO (V.J.B.T.), SIESTA (A.E. & A.V.P.) and QE (A.E.). Phenomenological modeling of the Raman cross section for a coupled system of harmonic oscillators within the linear dielectric function approach (O.P.) was implemented on MATLAB (A.E. & M.B.S.). O.P. wrote the manuscript, with the help of A.V.P and contributions from all co-authors. The figures were done by A.E.

Additional Information

Supplementary information accompanies this paper at https://...

Competing interests

The authors declare no competing interests.

Corresponding author

Correspondence to Olivier Pagès.

Vibrational-mechanical properties of the highly-mismatched Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} semiconductor alloy – Experiment and ab initio calculations

A. Elmahjoubi; M. B. Shoker; O. Pagès; V. J.B. Torres; A. Polian; A.V. Postnikov; C. Bellin; K. Beneut; C. Gardiennet; G. Kervern; A. EnNaciri; L. Broch; R. Hajj Hussein; J.-P. Itié; L. Nataf; S. Ravy; P. Franchetti; S. Diliberto; S. Michel; A. Abouais; K. Strzałkowski

In this annex, supplementary experimental, ab initio (AIMPRO) and modeling (linear dielectric approach) material is presented further supporting the discussion of the structural, optical (Sec. SI) and mechanical-vibrational properties of Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} (Sec. SII) done in the main text. Raw experimental data concerned with the structural properties of Be-dilute Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} studied at the lattice-macroscopic and bond-microscopic scales by high-pressure X-ray diffraction (HP-XRD) and by solid state nuclear magnetic resonance (SS-NMR) – completing Fig. 1 – are reported in Secs. SI.1 and SI.2, correspondingly, including a fruitful comparison with Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te} in the former case (HP-XRD, Sec. SI.1). Sec. SI.3 reports on the main Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} electronic interband transitions (E0E_0, E1E_1, E1+Δ1E_1+\Delta_1) determined by combining transmission and ellipsometry measurements in the visible. Sec. SII. provides ab initio insights into the Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} lattice relaxation for an isolated impurity (Sec. II.1), for paired impurities (Sec. II.2) and at intermediate composition (Sec. II.3). In Sec. II.1, an isolated Be impurity in CdTe – suffering a hydrostatic tensile strain from the host matrix – offers a benchmark to estimate in a full ab initio (SIESTA) approach how the local strain and the phonon dispersion separately impact the Raman frequencies of impurity modes. Sec. II.2 completes the high-pressure ab initio Raman study of paired-impurities in parent-like supercell done in the main text (Figs. 2c and 2e) by shifting the focus to the Cd-Te spectral range. Sec. II.3 provides an ab initio insight into the pressure dependence of the lattice relaxation within the Cd54Be54Te108\mathrm{Cd}_{54}\mathrm{Be}_{54}\mathrm{Te}_{108} cubic supercell used to calculate the ab initio high-pressure Raman spectra (Fig. 2d). Sec. SIII is concerned with the Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} lattice dynamics. Sec. III.1 reports on an experimental Raman study of the Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} vibrational properties at minor Be contents done at 0 GPa – in preparation for the high-pressure Raman study (Fig. 2b). Last, in Sec. SIII.2 we outline the linear dielectric approach used for contour modeling of the various Raman lineshapes (Fig. 2), referring to the four-mode {TOCd−TeBe,TOCd−TeCd,TOBe−TeBe,TOBe−TeCd}\{TO_{\mathrm{Cd-Te}}^{\mathrm{Be}},TO_{\mathrm{Cd-Te}}^{\mathrm{Cd}},TO_{\mathrm{Be-Te}}^{\mathrm{Be}},TO_{\mathrm{Be-Te}}^{\mathrm{Cd}}\} description across the composition domain at 0 GPa in absence of mechanical coupling (ω′=0 cm−1\omega'=0\ \mathrm{cm}^{-1}, Figure 2a), and to the punctual insight into the pressure dependence of the Be-Te Raman doublet at x∼1x \sim1 achieved by considering a weak mechanical coupling (ω′=50 cm−1\omega'=50\ \mathrm{cm}^{-1}, Figure 2f) impacting both the Raman frequencies and intensities.

Structural and optical properties of Be-dilute Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te}

(High-pressure) X-ray diffraction – Structural insight at the macroscopic (lattice) scale

Raw X-Ray diffractograms obtained at 0 GPa in laboratory using the CuKα\alpha radiation across the current Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} (x≤0.11x \le0.11) sample series (Figure S1) are characterized by sharp peaks at any composition xx value, the sign of a high structural quality. The individual peaks are labelled using the (hkl) Miller indices up to maximal angular deviation. The lattice constant aa is found to vary linearly with the composition xx (Figure S1), a standard feature of semiconductor alloys[2].

A selection of raw high-pressure X-ray diffractograms taken at increasing pressure on Cd0.89Be0.11Te\mathrm{Cd}_{0.89}\mathrm{Be}_{0.11}\mathrm{Te} at the PSICHÉ beamline of SOLEIL synchrotron using the 0.3738 Å radiation (Figure S1) reveal no extra peak besides the regular ones for a given crystal phase, the sign of a high structural purity. As pressure increases, Cd0.89Be0.11Te\mathrm{Cd}_{0.89}\mathrm{Be}_{0.11}\mathrm{Te} transforms from zincblende (0 GPa, abbreviated zb) to rocksalt (∼\sim5.5 GPa, rs) – the two phases coexisting over a rather large pressure domain (∼\sim5.5 – 9 GPa) – and subsequently to Cmcm (∼\sim13 GPa, cm), eventually surviving as a unique phase from ∼\sim18 GPa up to the maximum achieved pressure in this study (∼\sim24 GPa). The pressure dependence of lattice constants in each Cd0.89Be0.11Te\mathrm{Cd}_{0.89}\mathrm{Be}_{0.11}\mathrm{Te} phase (Figure 1c) is notably used to estimate the bulk modulus B0B_0 at 0 GPa in the native zincblende phase (Figure 1d) by fitting the pressure dependence of the volume of the unit cell to the Birch-Murnaghan equation of state[51](Figure S1).

Figure S2 displays selections of similar high-pressure X-ray diffractograms obtained with Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te} at (a) x=0.045x=0.045 and (b) 0.21 at the CRISTAL beamline of SOLEIL synchrotron using the 0.485 Å radiation – completing the already published x=0.14x=0.14 data[40] taken during the same run of experiment. The related experimental (symbols) volume versus pressure dependencies in the native zincblende phase fitted to the Birch-Murnaghan equation of state[51](curves) and resulting B0B_0 vs. xx variations are displayed in Figure S3 and Figure S3, respectively. The fit is done by fixing the reference volume at 0 GPa to the value obtained by considering a linear dependence of the lattice constant versus xx in Zn1−xBexTe\mathrm{Zn}_{1-x}\mathrm{Be}_{x}\mathrm{Te}[46]. The as-fitted B0B_0 (symbols) and B0′B'_0 values at x=(0.045, 0.14, 0.21)x=(0.045,\ 0.14,\ 0.21) are (52.857±\pm0.640, 52.846±\pm0.170, 52.542±\pm0.150) in GPa (the error bars is within the symbol size) and (3.94±\pm0.18, 4.05±\pm0.09, 4.03±\pm0.06), respectively. For all mixed crystals B0′B'_0 remains stable at around 4, found relevant for ZnTe[54] and BeTe[53]. A pronounced deviation from the B0B_0 vs. xx linearity (dashed line in Figure S3) in the sense of a negative bowing is observed – as in the case of Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} (Figure 1d) – with a minimal B0B_0 value at 21 at.% Be, quasi matched with the parent ZnTe value[54] – 52 GPa, well below the BeTe one[53] – 67 GPa.

Solid state nuclear magnetic resonance (SS-NMR) – Structural insight at the microscopic (atom) scale

In an alloy with zincblende structure such as Cd1−x_{1-x}Bex_xTe, the substituent (Cd and Be in this case) and invariant (Te) species are intercalated so a to form a (cubic) tetrahedral arrangement. Hence, Cd and Be exhibit a stable nearest-neighbor environment of four Te atoms at any xx value. In contrast the tetrahedral environment of Te diversifies into five variants depending on the number of Be and Cd atoms at the vertices. The five types of Te-centred tetrahedra are present in the crystal at any xx value, with various probabilities depending on xx, following the binomial Bernoulli’s distribution in their xx-dependence in the ideal case of a random Be↔Cd substitutionS1.

The pioneering 125{}^{125}Te solid-state nuclear magnetic resonance (NMR) measurements performed on Cd1−x_{1-x}Znx_xTe by Zamir et al. 39 have demonstrated a sensitivity of the NMR shift to the local environment at the nearest-neighbor scale. Hence, only the NMR data related to the invariant Te species (as opposed to the substitutional Cd and Be ones) of Cd1−x_{1-x}Bex_xTe can shed light on the nature of the Cd↔Be atom substitution – the reason for the emphasis on Te in the main text (Figure 1a). However, the 9{}^{9}Be (a) and 113{}^{113}Cd (b) NMR data related to both substituents are also provided (Figure S4), for the sake of completeness. A unique (well-defined) feature, reflecting the uniqueness of the local environment (all-Te), is visible in each case, as ideally expected.

Optical properties – Transmission and ellipsometry in combination

The main Cd1−x_{1-x}Bex_xTe electronic interband transitions are determined across the sample series in their xx-dependence by combining transmission (E0E_0) and ellipsometry (E1E_1, E1+Δ1E_1 + \Delta_1, E2E_2) measurements in the visible (Figure 1b). Selected data (Figure S5) illustrate how the interband transitions are estimated in practice from the raw spectrometric data at each composition, i.e., via a Tauc plot (transmission data, Figure S5 – curve, filled symbols in Figure 1b) or by direct (model free) inversion of the measured depolarization angles giving access to the imaginary part of the dielectric function within the 0.6 – 5.5 eV spectral range (ellipsometry data, Figure S5, hollow symbols in Figure 1b).

Cd1−x_{1-x}Bex_xTe lattice relaxation / dynamics – Ab initio insights

Cd31_{31}Be1_1Te32_{32} (SIESTA code) – isolated-impurity motif

An isolated Be atom in CdTe forms short Be-Te bonds suffering a hydrostatic tensile strain from CdTe corresponding to a large bond length. The Be-Te bond elongation Δl\Delta l with respect to the natural bond length in the pure BeTe crystal (l0l_0) softens the Be-Te impurity mode in CdTe – referred to as the impurity-ii mode in the main text – below the parent BeTe TO frequency (ωT,0\omega_{T,0}). The shift in TO frequency squared ΔωT2\Delta\omega_{T}^{2} relates to the variation in bond length Δl\Delta l via the relation63,S2,

ΔωT2ωT,02=−6γT⋅Δll0,(1)\frac{\Delta\omega_{T}^{2}}{\omega_{T,0}^{2}}=-6\gamma_{T}\cdot\frac{\Delta l}{l_{0}}, \tag*{(1)}

that involves the Grüneisen parameter of the parent TO mode, given byS3,

γT=B0ωT,0⋅(dωTdP)P=0,(2)\gamma_{T}=\frac{B_{0}}{\omega_{T,0}}\cdot\left(\frac{d\omega_{T}}{dP}\right)_{P=0}, \tag*{(2)}

where PP is the hydrostatic pressure and B0B_{0} the bulk modulus.

High-pressure ab initio (SIESTA) calculations of the lattice relaxation and of the Γ\Gamma-projected phonon density of states – that assimilates with the TO Raman spectrum in a crude approximation – done on a large 2×2×22\times2\times2 (64-atom) fully relaxed (l0∼2.406l_{0}\sim2.406 Å at ambient pressure) cubic BeTe supercell yield B0B_{0} and ωT,0\omega_{T,0} values of 63.7 GPa and 478 cm−1^{-1} (nearly matching the AIMPRO values in Figure 1d and Figure 2a), respectively, and further predict a linear increase of the TO frequency with pressure at low values (in the range 0 – 20 GPa) at the rate of ∼10.05\sim10.05 cm−1^{-1} per GPa. The resulting γT\gamma_{T} estimate via Eq. (2) for the parent BeTe TO mode is ∼1.33\sim1.33.

Similar SIESTA calculations done at 0 GPa on a similar zincblende-type Cd31_{31}Be1_{1}Te32_{32} supercell containing a unique Be atom give the Be-Te impurity-ii mode at ∼414\sim414 cm−1^{-1} (slightly above the experimental TOBe−TeCdTO_{\mathrm{Be-Te}}^{\mathrm{Cd}} one at x∼0x\sim0 – see Figure 2a) after relaxation (achieved via a Be-Te elongation of Δl∼0.063\Delta l\sim0.063 Å with respect to the natural-bulk l0l_{0} value – see above). This exceeds by ∼10\sim10 cm−1^{-1} the impurity-ii frequency due to the sole effect of the local strain given by Eq. (1). The difference is due to the (negative) dispersion of the BeTe TO mode, impacting all impurity (ii-to-iiiiii) modes (as emphasized by vertical arrows in Figure 2a), in principle[60]. Such study of the lattice relaxation / dynamics around an isolated Be impurity in CdTe (x∼0x\sim0), consistently conducted end-to-end within an ab initio (SIESTA) approach in reference to BeTe (x∼1x\sim1), points towards the important role of the phonon dispersion besides the local strain in shaping the Be-Te percolation doublet of Cd1−x_{1-x}Bex_xTe.

Cd106_{106}Be2_2Te108_{108} and Cd2_2Be108_{108}Te108_{108} (AIMPRO code) – Cd-Te signal vs. paired-impurity motifs

Figure S6 displays high-pressure ab initio (AIMPRO) CdTe-like TO Raman spectra due to large (216-atom) fully-relaxed (see methods) cubic Cd106_{106}Be2_2Te108_{108} (at 0 and 5 GPa – Figure S6) and Cd2_2Be108_{108}Te108_{108} (at 0 and 20 GPa – Figure S6) supercells containing similar (Be- and Cd) impurity-duos (connected via Te), in support to the discussion of the pressure dependence of the Cd-Te doublet of Cd1−x_{1-x}Bex_xTe (main text).

The Cd-Te doublet exhibits nearly the same spacing between the relevant (iiiiii-iviv, x∼0x\sim0) and (ii-iiii, x∼1x\sim1) Cd-Te modes at both ends of the composition domain. Under pressure the doublets either cross (Cd106Be2Te108\mathrm{Cd}_{106}\mathrm{Be}_{2}\mathrm{Te}_{108}, Figure S6) or freeze into a phonon exceptional point at the resonance (Cd2Be106Te108\mathrm{Cd}_{2}\mathrm{Be}_{106}\mathrm{Te}_{108}), already achieved at 0 GPa in this case – the frozen submode identified by its wavevector is spotted by an arrow (Figure S6).

Cd54Be54Te108 (AIMPRO code) – intermediary composition

Fig. S7 reports on ab initio (AIMPRO) calculations of the bond angle distribution depending on pressure within the large disordered zincblende-type Cd54Be54Te108\mathrm{Cd}_{54}\mathrm{Be}_{54}\mathrm{Te}_{108} (x=0.5x=0.5) supercell used to generate the corresponding ab initio (AIMPRO) Raman spectra (Figure 2d). The data reveal a prohibitive supercell distortion from 15 GPa onwards. This is manifested by a deviation of bond angles from the nominal zincblende value (109°), to such extent that two distinct groups of bond angles are identified (dotted lines). The zinclende structure is only preserved up to 10 GPa – being increasingly damped with pressure – thus fixing the limit for the Cd54Be54Te108\mathrm{Cd}_{54}\mathrm{Be}_{54}\mathrm{Te}_{108} ab initio Raman study (Figure 2d). A similar collapse is suffered by the CdTe-like Cd106Be2Te216\mathrm{Cd}_{106}\mathrm{Be}_{2}\mathrm{Te}_{216} supercell containing the isolated Be-duo from 10 GPa onwards (not shown) used to provide an ab initio (AIMPRO) insight into the pressure dependence of the Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} Raman spectra in the Be-dilute limit (x∼0x\sim0, Figure 2c).

Cd1-xBexTe lattice dynamics – Raman scattering

Experimental Raman study at ambient pressure (x≤0.11x \le0.11)

Fig. S8 displays a selection of unpolarized Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} (x≤0.11x \le0.11) Raman spectra taken at ambient pressure / temperature in the backscattering geometry on non-oriented crystal faces using the red (632.8 nm, x=0x=0 and 0.5) and blue (488.0 nm, x=0.11x=0.11) laser lines near-resonant with E0E_{0} and E0+Δ0E_{0}+\Delta_{0}, respectively (Figure 1b). The Raman signal consists of a quasi-degenerated TO-LO Be-Te impurity mode situated at much higher frequency than the CdTe-lattice TO-LO band (140 – 170 cm−1^{-1}). Near-resonance conditions favor the (polar) LO’s compared with the (non-polar) TO’s via the Fröhlich mechanismS4,S5. The LO emphasis is especially pronounced with the red laser excitation, manifested by the strong emergence of the second-order matrix signal (2×LOCd−Te2\times LO_{Cd-Te}). A pure Be-Te TO-insight is searched for at the largest available Be content (x=0.11x=0.11) by exciting a (110)-cleaved crystal face at normal incidence with the less resonant blue laser line, and collecting the scattered light in backscattering in the (TO-allowed, LO-forbidden) scattering geometryS5.

The Raman spectrum at minimal Be content (5 at.%) provides a crude experimental estimate of the Be-Te impurity-ii frequency in CdTe, i.e., ∼\sim390 cm−1^{-1}, in close agreement with existing data in the literatureS6,S7. Besides, the comparison between the LO-like (non-oriented crystal face) and TO-like (cleaved face) Cd0.89Be0.11Te\mathrm{Cd}_{0.89}\mathrm{Be}_{0.11}\mathrm{Te} Raman spectra resolves a finite Be-Te TO-LO splitting (emphasized by dotted lines, Fig. S7). By decreasing xx the lattice constant aa increases (Figure S1) which distances cations and anions and hence softens the chemical bonds, with concomitant impact on the TO (non-polar) Raman frequencies (scaling as the square roots of the effective bond force constant in a crude description[26]) being downward shifted. The LO (polar) Raman frequencies “mechanically follow”, converging progressively towards the (non-polar) TO’s when the bond fractions decrease until the TO-LO degeneracy is achieved in the dilute limits (x∼0x \sim0 for Be-Te and x∼1x \sim1 for Cd-Te). An overview of the experimental Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} Raman frequencies is given in Figure 2a (symbols).

Contour modeling of (high-pressure) TO Raman spectra – linear dielectric function approach

An overview of the TO Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} Raman frequencies (curves) and intensities (thickness of curves) calculated throughout the composition domain at 0 GPa in absence of mechanical coupling between TO oscillators (ω′=0\omega'=0, as sketched out) is given in Figure 2a.

Such contour modeling of the TO {εr(ω,x)→∞}\{\varepsilon_r(\omega,x) \to\infty\} Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_{x}\mathrm{Te} Raman spectra in their xx-dependence is achieved within a four-mode {2×(Cd−Te),2×(Be−Te)}\{2 \times(Cd-Te), 2 \times(Be-Te)\} version of the percolation model by calculating Im⁡{εr(ω,x)}\operatorname{Im}\{\varepsilon_r(\omega,x)\} – in a crude approximationS6,63 (see main text). At 0 GPa, the non-polar TO’s are presumably decoupled and hence are explicitly assigned by specifying both the bond vibration and the local environment (via a subscript and a superscript, respectively), i.e., {TOCd−TeBe,TOCd−TeCd,TOBe−TeBe,TOBe−TeCd}\{TO_{Cd-Te}^{Be}, TO_{Cd-Te}^{Cd}, TO_{Be-Te}^{Be}, TO_{Be-Te}^{Cd}\}. A classical form is used for εr(ω,x)\varepsilon_r(\omega,x) including a linear background electronic contribution ε∞(x)\varepsilon_\infty(x) at high (visible) frequencies besides the phonon (far-infrared) one, i.e., four oscillators in total (p=1p=1 to 4) modeled as pp-Lorentzian functions. In each Lorentzian, the numerator represents the available amount of oscillator strength per pp-mode Sp0(x)S_p^0(x) that scales as the parent value (Sp0=ε∞,p⋅Ωp2/ωT,p2S_p^0 = \varepsilon_{\infty,p} \cdot\Omega_p^2/\omega_{T,p}^2, with Ωp2=ωL,p2−ωT,p2\Omega_p^2 = \omega_{L,p}^2 - \omega_{T,p}^2) weighted by the pp-oscillator fraction (fpf_p-term below), directly impacting the pp-type TO Raman intensity. The denominator (ωT,p(x)−ω2−jγpω)(\omega_{T,p}(x) - \omega^2 - j\gamma_p\omega) monitors the position of the TO pp-resonance in its xx-dependence, given by ωT,p2(x)=kp(x)/μp\omega_{T,p}^2(x) = k_p(x)/\mu_p (the numerator and denominator referring to the effective mechanical bond force constant of oscillator-pp and to the reduced atomic mass of the pp-type chemical bond, respectively), with the phonon damping γp\gamma_p (introducing a friction force) fixing the full width at half maximum of the pp-type Raman peaks (taken minimal in Figure 2a, i.e., 1 cm−1^{-1}, for a clear resolution of neighboring features and direct comparison of the Raman intensities). We assume linear kp(x)k_p(x) vs. xx variations – in the spirit of the historical modified-random-element-isodisplacement (1-bond→1-mode) model[26] used to describe the Raman spectra of semiconductor alloys, leading to quadratic ωT,p2(x)\omega_{T,p}^2(x) variations. By analogy with Zn1−xBex\mathrm{Zn}_{1-x}\mathrm{Be}_{x}-chalcogenides[25, 40], a sensitivity of Be-Te vibrations to crystalline environment limited to nearest neighbors is considered. The corresponding 1D-oscillators behind the four TO’s (specified in brackets above) can be cast as {Te(Cd−Te)Be,Te(Cd−\{Te(Cd-Te)Be, Te(Cd- Te)Cd,Te(Be−Te)Be,Te(Be−Te)Cd}Te)Cd, Te(Be - Te)Be, Te(Be - Te)Cd\}, participating with weights {fCd−TeBe=x⋅(1−x),fCd−TeCd=(1−x)2,fBe−TeBe=x2,fBe−TeCd=x⋅(1−x)}\{f^{Be}_{Cd-Te} = x \cdot(1-x), f^{Cd}_{Cd-Te} = (1-x)^2, f^{Be}_{Be-Te} = x^2, f^{Cd}_{Be-Te} = x \cdot(1-x)\}. The TO Raman intensities (color code in Figure 2a) scale accordingly. Hence the two TO submodes forming a given (Cd-Te or Be-Te) doublet exhibit comparable Raman intensities at x∼0.5x \sim0.5.

Altogether, this leaves ten input parameters in total, out of which six relate to the parent compounds (ε∞,p,Ωp,ωT,p\varepsilon_{\infty,p}, \Omega_p, \omega_{T,p}) and four to the alloy taken in its (Cd,Be)-dilute limits. All parameters are determined ab initio, without leaving any adjustable one. The input frequencies (two per TO branch) are derived by implementing a simple ab initio (AIMPRO) protocol onto impurity Cd-duo and Zn-duo motifs (referring to the ii, iiii and iviv end frequencies in Figure 2a), the parent ωT,p\omega_{T,p} (bulk TO) frequencies (symbolized iiiiii in Figure 2a) coming out as by-products. The parent TO-LO splittings together with the parent ε∞,p\varepsilon_{\infty,p} values, needed to estimate the parent oscillator strengths—see methods, are obtained by resorting to QE.

Fair phenomenological modeling of the pressure-induced interplay between Raman intensities is achieved within a linear dielectric approach of the relaxed-inverted Be-Te percolation doublet of Cd1−xBexTe\mathrm{Cd}_{1-x}\mathrm{Be}_x\mathrm{Te} at x∼1x \sim1 (Figure 2f)—apparent in ab initio data (Figure 2e), by taking into account a (weak) mechanical coupling (ω′∼50 cm−1\omega' \sim50\ \mathrm{cm}^{-1}—see main text). A relevant expression for the corresponding Raman cross section has lately been derived—see Ref. 40 and specifically Eq. (7) therein. A simplified form is currently used in which the coupling term at the numerator is disregarded compared with the two main terms standing for the raw-uncoupled oscillators. The analysis is further displaced from the Be-dilute limit (x∼1x \sim1) to minor Be contents (x∼0.8x \sim0.8 in this case) for more convenience (see main text)—while artificially preserving the peak frequencies as such. A minimal phonon damping is uniformly taken (1 cm−11\ \mathrm{cm}^{-1}) for clarity.

Supplementary Information-only References

Bond-angle distribution within the Cd54Be54Te108 zincblende-type supercell

Figure S7. (High-pressure) ab initio (AIMPRO) insight into the Cd54Be54Te108\mathrm{Cd}_{54}\mathrm{Be}_{54}\mathrm{Te}_{108} lattice relaxation. Pressure dependence of the ab initio bond-angle distribution within the large (216-atom) Cd54Be54Te108\mathrm{Cd}_{54}\mathrm{Be}_{54}\mathrm{Te}_{108} zincblende-type supercell optimized to a random Ce↔Be substitution bonds used to calculate the ab initio (AIMPRO) Raman spectra discussed in the main text (Figure 2d). The nominal angle value in the zincblende structure (109°, dotted line) is indicated, for reference purpose. A significant deviation from 15 GPa onwards is emphasized (69°, dotted line).

Experimental Raman spectra of Cd$_{1-x}$Be$_x$Te

Figure S7 (PDF p. 44). Experimental Cd1−x_{1-x}Bex_xTe (x≤0.11x \le0.11) Raman spectra at ambient conditions. LO-like Cd1−x_{1-x}Bex_xTe Raman spectra taken in the backscattering geometry on unoriented crystal faces polished to optical quality in near-resonant conditions with the red (632.8 nm) and blue (488.0 nm) laser lines (Figure 1b). A pure-TO Cd0.89_{0.89}Be0.11_{0.11}Te Raman spectrum taken with the 488.0 nm laser line in the backscattering geometry at normal incidence onto a (110)-cleaved face is added, for comparison. Paired dotted lines mark a finite TO-LO splitting at x=0.11x=0.11.

References

  1. [1]Powalla, M. et al. Thin-film solar cells exceeding 22% solar cell efficiency: An overview on CdTe-, Cu(In,Ga)Se2-, and perovskite-based materials. Appl. Phys. Rev. 5, 041602 (2018).DOI
  2. [2]Adachi, S. Properties of Semiconductor Alloys : Group-IV, III-V and II-VI. Edited by John Wiley & Sons (2009).
  3. [3]Christensen, N.E., Satpathy, S. & Pawlowska, Z. Bonding and ionicity in semiconductors. Phys. Rev. B 36, 1032–1050 (1987).pubmed.ncbi.nlm.nih.gov/9942909
  4. [4]Vérié, C. Beryllium substitution-mediated covalency engineering of II-VI alloys for lattice elastic rigidity reinforcement. J. Cryst. Growth 184/185, 1061–1066 (1998).
  5. [5]Weyers, M., Sato, M. & Ando, H. Red shift of photoluminescence and absorption in dilute GaAsN alloy layers. Jpn. J. Appl. Phys. 31, L853–L855 (1992).DOI
  6. [6]Lugauer, H.-J. et al. P-type doping of beryllium chalcogenides. Mat. Sci. Eng. B 43, 88-91 (1997).DOI
  7. [7]Waag, A. et al. Novel Beryllium containing II-VI compounds : basic properties and potential applications. J. Cryst. Growth 184/185, 1–10 (1998).
  8. [8]Almamum Ahrafi, A. B. M. et al. Growth and characterization of hypothetical zincblende ZnO films on GaAs (001) substrates with ZnS buffer layers. Appl. Phys. Lett. 76, 550–552 (2000).DOI
  9. [9]Walukiewicz, W. & Zide, J. M. O. Highly mismatched semiconductor alloys: from atoms to devices. J. Appl. Phys. 127, 010401 (2020).DOI
  10. [10]Neugebauer, J. & Van de Walle, C. G. Electronic structure and phase stability of GaAs₁₋ₓNₓ alloys. Phys. Rev. B 51, 10568–10571 (1995).pubmed.ncbi.nlm.nih.gov/9977751
  11. [11]Wei, S.-H. & Zunger, A. Giant and composition-dependent optical bowing coefficient in GaAsN alloys. Phys. Rev. Lett. 76, 664–667 (1996).pubmed.ncbi.nlm.nih.gov/10061516
  12. [12]Hjalmarson, H. et al. theory of substitutional deep traps in covalent semiconductors. Phys. Rev. Lett. 44, 810–813 (1980).DOI
  13. [13]Shan, W. et al. Band anticrossing in GaAsN alloys. Phys. Rev. Lett. 82, 1221–1224 (1999).DOI
  14. [14]Wu, J., Walukiewicz, W. & Haller, E. E. Band structure of highly mismatched semiconductor alloys: coherent potential approximation. Phys. Rev. B 65, 233210 (2002).DOI
  15. [15]Chen, C. et al. Carrier dynamics of intermediate sub-bandgap transitions in ZnTeO. J. Appl. Phys. 126, 135701 (2019).DOI
  16. [16]Tanaka, T. et al. Cl-doping effect in ZnTe₁₋ₓOₓ highly mismatched alloys for intermediary band solar cells. J. Appl. Phys. 125, 243109 (2019).
  17. [17]Allami, H. & Krich, J. J. Absorption spectrum of doped highly mismatched alloys. ArXiv:2203.15528 [cond-mat.mtrl-sci].DOI
  18. [18]Maksimov, O. & Tamargo, M. C. Direct-to-indirect band gap crossover for the BeₓZn₁₋ₓTe alloy. Appl. Phys. Lett. 79, 782–784 (2001).DOI
  19. [19]Chauvet, C., Tournié, E. & Fourie, J.-P. Nature of the band gap of Zn₁₋ₓBeₓSe alloys. Phys. Rev. B 61, 5332–5336 (2000).DOI
  20. [20]Wilmers, K. et al. VUV-Ellipsometry on BeₓZn₁₋ₓSe and BeTe. J. Electron. Materials 28, 670–677 (1999).DOI
  21. [21]Buckley, M. R. et al. Dielectric functions and critical points of BeₓZn₁₋ₓTe alloys measured by spectroscopic ellipsometry. Appl. Phys. Lett. 81, 5156–5158 (2002).DOI
  22. [22]Wilmers, K. et al. Ellipsometric studies of BeₓZn₁₋ₓSe between 3 eV and 25 eV. Phys. Rev. B 59, 10071–10075 (1999).
  23. [23]Kozielski, M. et al. Study if the A₁₋ₓBₓC mixed crystals by Raman scattering. Cryst. Res. Technol. 34, 699–702 (1999).doi.org/10.1002/(sici)1521-4079(199906)34:5/6<699::aid-crat699>3.0.co;2-1
  24. [24]Mintairov, A. M. et al. Optical spectra of wide band gap BeₓZn₁₋ₓSe alloys. Semiconductors 33, 1021–1023 (1999).DOI
  25. [25]Pagès, O. et al. Vibrational evidence for a percolative behavior in Zn₁₋ₓBeₓSe. Phys. Rev. B 65, 035213 (2001).DOI
  26. [26]Chang, I.F. & Mitra, S.S. Long wavelength optical phonons in mixed crystals. Adv. Phys. 20, 359–404 (1971).
  27. [27]Shoker, M. B. et al. Phonon-based partition of (ZnSe-like) semiconductor mixed crystals on approach to their pressure-induced structural transition. Sci. Rep. 10, 19803 (2020) – and refs. therein.arxiv.org/abs/2008.07187
  28. [28]Wronkowska, A. A. et al. Optical spectra of Zn₁₋ₓBeₓTe mixed crystals determined by IR-VIS-UV ellipsometry and photoluminescence measurements. Thin Solid Films 519, 2795–2800 (2011).DOI
  29. [29]Postnikov, A. V., Pagès, O. & Hugel, J. Lattice dynamics of the mixed semiconductors (Be,Zn)Se from first-principles calculations. Phys. Rev. B 71, 115206 (2005).DOI
  30. [30]Bhalerao, G. M. et al. High-pressure x-ray diffraction and extended x-ray absorption fine structure studies on ternary alloy Zn₁₋ₓBeₓSe. J. Appl. Phys. 108, 083533 (2010).DOI
  31. [31]Eckner, S. & Schnohr, C. S. Private communication.
  32. [32]Proffen, Th., Billingue, S.J.L., Egami, T. & Louca D. Structural analysis of complex materials using the atomic pair distribution function – a practical guide. Z. Kristallogr. 218, 132–143 (2003).
  33. [33]Qiu, X. et al. Reciprocal-space instrumental effects on the real-space neutron atomic pair distribution function. J. Appl. Cryst. 37, 110–116 (2004).DOI
  34. [34]Boyce, J. B. & Mikkelsen, Jr., J. C. Local structure of pseudobinary semiconductor alloys: An X-ray absorption fine structure study. J. Cryst. Growth 98, 37–43 (1989).DOI
  35. [35]Mikkelsen, Jr., J. C. & Boyce, J. B. Atomic-scale structure of random solid solutions: Extended X-ray-absorption-fine-structure study of Ga₁₋ₓInₓAs. Phys. Rev. Lett. 49, 1412–1415 (1982).DOI
  36. [36]Pellicer-Pores, J. et al. X-ray-absorption fine-structure study of ZnSe₁₋ₓTeₓ alloys. J. Appl. Phys. 96, 1491–1498 (2004).DOI
  37. [37]Pagès, O. et al. Percolation picture for long wave phonons in zincblende mixed crystals: from (Zn,Be)-chalcogenides to (Ga,In)As. J. Phys. Condens. Matt. 18, 577–592 (2006).DOI
  38. [38]Schnohr, C.S. Compound semiconductor alloys from atomic scale structure to bandgap bowing. Appl. Phys. Rev. 2, 031304 (2015).DOI
  39. [39]Zamir, D. et al. Nuclear magnetic resonance studies of II-VI semiconductor alloys. J. Vac. Sci. Technol. A 6, 2612–2613 (1988).DOI
  40. [40]Shoker, M. B. et al. Exceptional phonon point versus free phonon coupling in Zn₁₋ₓBeₓTe under pressure: an experimental and ab initio Raman study. Sci. Rep. 12, 753 (2022).
  41. [41]Briddon, P. R. & Jones, R. LDA calculations using a basis of Gaussian orbitals. Phys. Stat. Sol. B 217, 131–171 (2000).
  42. [42]Rayson, M. J. & Briddon, P. R. Rapid iterative method for electronic-structure eigenproblems using localized basis functions. Comput. Phys. Commun. 178, 128–134 (2008).DOI
  43. [43]Soler, J. M. et al. The SIESTA method for ab-initio order-N materials simulation. J. Phys.: Condens. Matter 14, 2745–2779 (2002).DOI
  44. [44]García, A. et al. SIESTA: Recent developments and applications. J. Chem. Phys. 152, 204108 (2020).DOI
  45. [45]Giannozzi, P. et al. QUANTUM ESPRESSO: a modular and open-source software project for quantum simulations of materials. J. Phys.: Condens. Matter 21, 395502 (2009).DOI
  46. [46]De Almeida, J. S. & Ahuja, R. Tuning the structural, electronic and optical properties of BeₓZn₁₋ₓTe alloys. Appl. Phys. Lett. 89, 061913 (2006).DOI
  47. [47]Wagner, V. et al. Surface and overgrowth analysis of the II–VI compound BeTe. Appl. Surf. Sci. 212–213, 901–906 (2003).DOI
  48. [48]Cardona, M. & Greenaway, D. L. Fundamental reflectivity and band structure of ZnTe, CdTe and HgTe. Phys. Rev. 131, 98–103 (1963).DOI
  49. [49]Hododyský, P. & Hlĭdek, P. Free-exciton absorption in bulk CdTe: temperature dependence. Phys. Stat. Sol. (b) 243, 494–501 (2006).DOI
  50. [50]Mujica, A., Rubio, A., Muñoz, A. & Needs, R.J. High-pressure phases of group-IV, III-V and II-VI compounds. Rev. Mod. Phys. 75, 863–9012 (2003).DOI
  51. [51]Birch, F. Finite elastic strain of cubic crystals. Phys. Rev. 71, 809–824 (1947).DOI
  52. [52]McMahon, M. I., Nelmes, R. J., Wright, N. G. & Allan, D. R. Phase transitions in CdTe to 5 GPa. Phys. Rev. B 48, 16246–16251 (1993).pubmed.ncbi.nlm.nih.gov/10008204
  53. [53]Luo, H., Ghandehari, K., Greene, R. G. & Ruoff, A. L. Phase transformations of BeSe and BeTe to the NiAs structure at high pressure. Phys. Rev. B 52, 7058–7064 (1995).pubmed.ncbi.nlm.nih.gov/9979646
  54. [54]Pellicer-Pores, J. et al. High-pressure phase diagram of ZnSe₁₋ₓTeₓ alloys. Phys. Rev. B 71, 035210 (2005).DOI
  55. [55]Pagès, O. et al. Percolation behavior in the Raman spectra of ZnBeTe alloys. Appl. Phys. Lett. 80, 3081–3083 (2002).DOI
  56. [56]Sennet, C. T., Bosomworth, D. R., Hayes, W. & Spray, A. R. Infra-red absorption of beryllium in cadmium telluride: II. J. Phys. C. 2, 1137–1145 (1969).
  57. [57]Talwar, D. N., Feng, Z. C. & Yang, T.-Z. Vibrational signatures of isotopic impurities and complexes in II-VI compound semiconductors. Phys. Rev. B 85, 195203 (2012).DOI
  58. [58]Gilliland, S. et al. Pressure and temperature dependence of the band-gap in CdTe. Phys. Stat. Sol. (b) 235, 441–445 (2003).DOI
  59. [59]Talwar, D. N., Feng, Z. C., Lee, J.-F. & Becla, P. Extended x-ray absorption fine structure and micro-Raman spectra of Bridgman grown Cd₁₋ₓZnₓTe ternary alloys. Mat. Res. Express 1, 015018 (2014).DOI
  60. [60]Hajj Hussein, R. et al. Percolation-type multi-phonon pattern of Zn(Se,S): Backward/forward Raman scattering and ab initio calculations. J. Alloys Compd 644, 704–720 (2015).DOI
  61. [61]Rajput, B. D. & Browne, D. A. Lattice dynamics of II-VI materials using the adiabatic bond-charge model. Phys. Rev. B 53, 9052–9058 (1996).pubmed.ncbi.nlm.nih.gov/9982405
  62. [62]Srivastava, G. P., Tütüncü, H. M. & Günhan, N. First-principles studies of structural, electronic and dynamical properties of Be chalcogenides. Phys. Rev. B 70, 0825206 (2004).DOI
  63. [63]Groenen, J. et al. Optical-phonon behavior in Ga₁₋ₓInₓAs: The role of microscopic strains and ionic plasmon coupling. Phys. Rev. B 58, 10452–10462 (1998).DOI
  64. [64]Claus, R., Merten, L. & Brandmüller, J. Light scattering by Phonon-Polaritons, ed. by Höhler, G. (Springer-Verlag, Berlin, 1975), p. 62.
  65. [65]Gorgol, M. et al. Positron lifetime spectroscopy of defect structures in Cd₁₋ₓZnₓTe mixed crystals grown by vertical Bridgman-Stockbarger method. Acta Cryst. B 77, 515–525 (2021).DOI
  66. [66]Larsen, F. H., Jakobsen, H. J., Ellis, P. D. & Nielsen, N. C. Sensitivity-enhanced quadrupolar-echo NMR of half-integer quadrupolar nuclei. Magnitudes and Relative orientation of chemical shielding and quadrupolar coupling tensors. J. Phys. Chem. A 101, 8597–8606 (1997).DOI
  67. [67]Ganjoo, A. & Golovchack, R. Computer program PARAV for calculating optical constants of thin films and bulk materials/Case study of amorphous semiconductors. J. Opt. Adv. Mat. 10, 1328–1332 (2008).
  68. [68]Chervin, J. C., Canny, B., Besson, J. M. & Pruzan, P. A diamond anvil cell for IR microspectroscopy. Rev. Sci. Instrum. 66, 2595–2598 (1995).DOI
  69. [69]Prescher, C. & Prakapenka, V.B. DIOPTAS : a program for reduction of two-dimensional X-ray diffraction data and data exploration. High Press. Res. 35, 223–230 (2015).DOI
  70. [70]De Gironcoli, S. Phonons in Si-Ge systems : An ab initio interatomic-force-constant approach. Phys. Rev. B 46, 2412–2419 (1992).pubmed.ncbi.nlm.nih.gov/10003915
  71. [71]Klingshirn, C. F. Semiconductor Optics. Edited by Springer-Verlag (1997), p. 65.

Paper details

vlnc:W_nkxmhs8f
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents