139^{139}La nuclear quadrupole resonance studies of pressurized La4_4Ni3_3O10_{10}

Abstract

Density-wave (DW) orders are considered as competing orders to unconventional superconductivity and are commonly seen in a variety of superconductors including but not limited to the recently discovered Ruddlesden-Popper-phase nickelates. By utilizing 139^{139}La nuclear quadrupole resonance, we systematically investigate into the nature of DW orders and their evolution under pressure in La4_4Ni3_3O10_{10}. Spin and charge DW orders are found to be intertwined in this material, which is in stark contrast to those in La3_3Ni2_2O7_7. Short-range DW orders are observed near 150 K, well above the development of long-range DW orders at around 139 K. Upon applying a hydrostatic pressure of 2.3 GPa, the transition temperatures of the short-range and long-range orders decrease at rates of 1 K/GPa and 10 K/GPa, respectively. Our results thus affirm that both spin density wave and charge density wave as competing orders with the superconducting state in La4_4Ni3_3O10_{10}, and provide new insights into the interplay between DW orders and unconventional superconductivity.

Introduction

The recent discovery of pressure-induced superconductivity (SC) with a critical temperature (TcT_\mathrm{c}) exceeding 80 K in bilayer Ruddlesden-Popper (RP) structured nickelates La3_3Ni2_2O7_7 [1, 2, 3, 4, 5] establishes a novel correlated high-TcT_\mathrm{c} superconductor family alongside cuprates [6] and iron-based [7] superconductors. Extensive studies have been motivated to look into the interplay between competing orders and unconventional SC in these layered systems [8, 9, 10, 11, 12, 13]. Stoichiometric RP-type nickelates adopt the general chemical formula Lnn+1_{n+1}Nin_nO3n+1_{3n+1} (Ln = Lanthanides) [14]; besides the bilayer La3_3Ni2_2O7_7 (n=2n = 2), the trilayer La4_4Ni3_3O10_{10} (n=3n = 3) was also reported to exhibit signatures of SC under high pressure [15, 16, 17], reaching a maximum Tc≈30T_\mathrm{c} \approx30 K [18]. Systematic comparisons across these structural variants are essential to elucidate the microscopic origin of SC.

At ambient pressure, both La3_3Ni2_2O7_7 and La4_4Ni3_3O10_{10} display some kind of density-wave (DW) orders at low temperatures [19, 20, 21]. Under pressure, they undergo a structural phase transition, and meanwhile, the DW orders are assumed to be suppressed before SC state emerges [10, 22]. In La3_3Ni2_2O7_7, two kinds of DW orders were observed, a spin-density-wave (SDW) transition at ∼150\sim150 K [23, 24, 25], followed by another DW transition at ∼130\sim130 K whose nature remains unclear yet [24, 25, 26]. These two DW orders seem to be decoupled, and evolve differently under pressure [24, 26, 27]. The situation in La4_4Ni3_3O10_{10}, however, appears more elusive in that the SDW and charge-density-wave (CDW) transitions were suggested to take place simultaneously [28, 29, 30, 31, 32, 33]. A natural question then concerns whether they remain intertwined and how they evolve under pressure. To clarify this issue, local and microscopic measurements that can distinguish the spin and charge degrees of freedom are needed.

Nuclear quadrupole resonance (NQR) exploits I>1/2I > 1/2 nuclei as local probes [34], where II is quantum number of nuclear spin. Via hyperfine coupling to both internal magnetic field and electric field gradient (EFG), hopefully, the information about spin and charge orders can be extracted and disentangled by NQR. Here, we report systematic 139^{139}La NQR studies on single crystalline La4_4Ni3_3O10_{10} at ambient and hydrostatic (2.3 GPa) pressures. Our results unveil the appearance of short-range DW orders prior to the long-range orders. The intertwining of SDW and CDW orders is manifested by a non-vanishing magnetic-quadrupolar coupling term. Under pressure, both the long-range and short-range orders are suppressed, at the rates of 10 K/GPa and 1 K/GPa, respectively. These results are rather different from those in La3_3Ni2_2O7_7, and establish both SDW and CDW as competing orders to SC, offering new insights into the mechanism of SC in RP-phase nickelates.

Experimental details

High-quality single crystalline La4_4Ni3_3O10_{10} studied in this work was grown by the high-pressure optical floating-zone technique [35]. The samples were verified by magnetic susceptibility measurements in a magnetic property measurement system (MPMS, Quantum Design) equipped with a vibrating sample magnetometer (VSM) option, which confirms the density-wave transition near TDW≈139T_\mathrm{DW} \approx139 K, in agreement with literature [18] (See Figure S1 in Supplemental Material (SM) [36]). Hydrostatic pressure up to ∼2.3\sim2.3 GPa was applied using a piston-cylinder pressure cell (CTF-HHPCC60, TOHO HARMONY), and the pressure was determined by monitoring the in-situ 63^{63}Cu NQR frequency of Cu2_2O mounted in the same coil [37]. 139^{139}La NQR measurements for temperatures between 80–300 K were carried out using a custom-built liquid-nitrogen measurement system. 139^{139}La NQR spectra were recorded in a stepped frequency-sweep method, while the spin-lattice relaxation time (T1T_1) was obtained by fitting the recovery curve of the ±5/2↔±7/2\pm5/2 \leftrightarrow\pm7/2 transition to the stretched formula

Figure S1. Magnetic susceptibility (χ\chi) of La4_4Ni3_3O10_{10} measured after a zero-field cooling process. Two samples (S1 and S2) were measured. (a) χ(T)\chi(T); (b) dχ/dTd\chi/dT. A density-wave transition (DW) is identified at TDW=139T_{\mathrm{DW}} = 139 K, consistent with literature.

M(t)=M(∞){1−2F[257412012exp⁡(−(3tT1)b)+780012012exp⁡(−(10tT1)b)+163812012exp⁡(−(21tT1)b)]},(1)M(t)=M(\infty)\left\{1-2F\left[\frac{2574}{12012}\exp\left(-\left(\frac{3t}{T_1}\right)^b\right)+\frac{7800}{12012}\exp\left(-\left(\frac{10t}{T_1}\right)^b\right)+\frac{1638}{12012}\exp\left(-\left(\frac{21t}{T_1}\right)^b\right)\right]\right\}, \tag*{(1)}

where M(∞)M(\infty), FF, T1T_1, bb are fitting parameters. When the stretching exponent b=1b = 1, (1) reduces to the standard fitting formula.

Results and Discussion

139La NQR at p = 0

At ambient pressure, La4_4Ni3_3O10_{10} crystallizes in a monoclinic P21_1/a structure [18, 38, 39, 40]. A doubly expanded cell can be viewed as quasi-tetragonal, as illustrated in fig:1a. It contains two crystallographically inequivalent La sites: La(1) – the one sits within the NiO6_6 double layers, and La(2) – the one resides in the La-O fluorite-type layers outside the NiO6_6 bilayers. Owing to the much lower NQR frequency and weaker signal intensity of the La(1) site [41], we here only focus on the La(2) site as a local probe. Figure fig:1b shows the full 139^{139}La(2) NQR spectrum measured at 180 K at ambient pressure. No additional peaks arising from other Lan+1_{n+1}Nin_nO3n+1_{3n+1} phases can be identified [23, 24, 42].

The nuclear quadrupole Hamiltonian is expressed as

HQ=eQVzz4I(2I−1)[3I^z2−I^2+η(I^x2−I^y2)].(2)\mathcal{H}_Q=\frac{eQV_{zz}}{4I(2I-1)}\left[3\hat{I}_z^2-\hat{I}^2+\eta\left(\hat{I}_x^2-\hat{I}_y^2\right)\right]. \tag*{(2)}

where I^=(I^x,I^y,I^z)\hat{I}=(\hat{I}_x,\hat{I}_y,\hat{I}_z) is the nuclear spin operator, QQ is nuclear quadrupole moment, and η=(Vxx−Vyy)/Vzz\eta=(V_{xx}-V_{yy})/V_{zz} is the asymmetry parameter with VxxV_{xx}, VyyV_{yy} and VzzV_{zz} being the components of the EFG tensor. For I=7/2I = 7/2 nuclear spin, three NQR peaks are expected arising from the transitions ±1/2↔±3/2\pm1/2 \leftrightarrow\pm3/2, ±3/2↔±5/2\pm3/2 \leftrightarrow\pm5/2 and ±5/2↔±7/2\pm5/2 \leftrightarrow\pm7/2. For brevity, we hereafter refer to them as f1f_1, f2f_2 and f3f_3, respectively. At 180 K, these values are 5.32, 10.31 and 15.53 MHz, consistent with previous reports [29, 41, 42]. In Figure 1(c) and (d), we display the temperature evolution of the ±3/2↔±5/2\pm3/2 \leftrightarrow\pm5/2 and ±5/2↔±7/2\pm5/2 \leftrightarrow\pm7/2 transitions. On the whole, both resonance peaks shift towards right-handed upon cooling, as expected. To elucidate the temperature-dependent peak behavior, we implemented a fitting analysis. While a single Lorentzian peak fits the spectra well in the high-temperature regime (>150> 150 K), this turns out to be inadequate as lineshape broadening and asymmetry develop below 150 K. Attributing these anomalies to a precursor effect of the short-range DW transition (whose onset temperature is denoted by T∗=150T^* = 150 K), we decomposed the spectra into a disordered-state Lorentzian (L) and an ordered-state Gaussian (G) contribution. It should be mentioned here that we did not observe any peak splitting in our NQR spectra at all temperatures, which implies that the DW orders are incommensurate, and this is totally different from La3_3Ni2_2O7_7 where commensurate DW order was detected [23, 26, 43]. Below TDWT_{\mathrm{DW}}, the intensity of the peak shrinks rapidly, and the NQR signals become hardly distinguishable out of the background noise.

Figure 1. (a) Crystal structure of La4_4Ni3_3O10_{10} showing two distinct La sites. The cell is doubly expanded to show the quasi-tetragonal structure. (b) 139^{139}La(2) NQR spectrum at ambient pressure and 180 K. All three NQR transitions for nuclear spin I=7/2I = 7/2 are identified. (c) The ±3/2↔±5/2\pm3/2 \leftrightarrow\pm5/2 spectra at selected temperatures. The spectra are vertically shifted for clarity. Above 150 K, the peak conforms exclusively to a Lorentzian lineshape (orange). Below this temperature, an additional Gaussian contribution (blue) is required. (d) ibid, but for the ±5/2↔±7/2\pm5/2 \leftrightarrow\pm7/2 transition.

This behavior is likely attributable to the magnetic wipe-out effect when approaching the SDW transition. The coexistence of L and G components below 150 K manifests the presence of short-range ordering prior to the long-range DW orders, in agreement with a recent report [42]. The temperature dependence of f2f_2 and f3f_3 are extracted and summarized in Figure 2(a-b). Quasi-linear temperature dependence is found in both f2L(T)f_{2\mathrm{L}}(T) and f3L(T)f_{3\mathrm{L}}(T) above TDWT_{\mathrm{DW}}, in accordance with the Bayer–Kushida relation [44], whereas no anomaly is discernible across T∗T^*. The f2Gf_{2\mathrm{G}} and f3Gf_{3\mathrm{G}}, in contrast, exhibit small changes about T∗T^* with respect to the L counterparts, cf the insets to Figure 2(a-b). (The subscripts “L” and “G” denote the L and G components, respectively; same below.) From the frequencies of f2Lf_{2\mathrm{L}} and f3Lf_{3\mathrm{L}}, the asymmetry parameter η≈0.088\eta\approx0.088 is derived at 180 K, indicating a relatively small EFG asymmetry [41, 42]. The details for estimating η\eta and its temperature dependence are presented in Figure S2[36]. Within the full temperature window of this work, η\eta is essentially constant. It seems that both f2Gf_{2G} and f3Gf_{3G} tend to drop below TDWT_{\mathrm{DW}}; however, since we lost NQR signal just below TDWT_{\mathrm{DW}}, it is not clear for us how the EFG changes in the ordered phase.

Temperature dependencies of peak frequencies, relaxation rate, and linewidth contributions

Figure 2. (a) and (b) show the temperature dependencies of the peak frequencies associated with the disordered (Lorentzian-fit) and ordered (Gaussian-fit) states for the ±3/2↔±5/2\pm3/2 \leftrightarrow\pm5/2 and ±5/2↔±7/2\pm5/2 \leftrightarrow\pm7/2 transitions, respectively. The inset provides an enlarged plot near the DW transitions. (c) Temperature dependence of 1/T1T1/T_1T at La(2) site. The inset shows a zoom-in view, as well as the definition of TDWT_{\mathrm{DW}} and T∗T^*. (d) Magnetic (wGmw_{\mathrm{G}}^{\mathrm{m}}) and quadrupole (wGqw_{\mathrm{G}}^{\mathrm{q}}) contributions extracted from the linewidth analysis of the ordered state. (e) The separated linewidth contributions to the f2f_2 and f3f_3 peaks. The inset plots the ratio w3G/w2Gw_{3\mathrm{G}}/w_{2\mathrm{G}}.

Relationship between the frequency ratio and asymmetry parameter, and temperature dependence of the asymmetry parameter

Figure S2. (a) By iterating over different η\eta values, the relationship between the frequency ratio f3L/f2Lf_{3L}/f_{2L} and η\eta is established in the figure. Given that f3L/f2L≈1.505f_{3L}/f_{2L} \approx1.505 from experimental, the asymmetry parameter η≈0.088\eta\approx0.088 is obtained at 180 K. (b) Temperature dependence of η\eta at the La(2) site of La₄Ni₃O₁₀.

Figure 2 presents the temperature dependence of 1/T1T1/T_{1}T at the La(2) site. In the high temperature regime (180 K - 300 K), 1/T1T1/T_{1}T is nearly constant, reminiscent of a conventional metal behavior without local magnetic moments. Note that for a Fermi-liquid system, 1/T1T1/T_{1}T is a measure of N2(EF)N^{2}(E_{\mathrm{F}}), where N(EF)N(E_{\mathrm{F}}) is the density of states at the Fermi level [34, 45]. Upon further cooling, 1/T1T1/T_{1}T of La4_4Ni3_3O10_{10} undergoes a pronounced enhancement below 160 K due to the spin fluctuations nearby the SDW order, and then peaks at ∼139\sim139 K where the long-range DW transitions occur. The as-defined TDWT_{\mathrm{DW}} agrees well with that determined by magnetic susceptibility (cf Figure S1 [36]). Below TDWT_{\mathrm{DW}}, as the DW gaps open, presumably, 1/T1T1/T_{1}T should reduce drastically [29, 42]. Unfortunately, since the NQR signals vanish quickly below TDWT_{\mathrm{DW}} in our experiment, we are unable to see this feature. Notably, above TDWT_{\mathrm{DW}}, a small shoulder is observed. It should be pointed out that the point where 1/T1T1/T_{1}T starts to upturn coincides with T∗T^{*} at which the G component in the La(2) NQR spectra appears. Therefore, it is reasonable to attribute the shoulder behavior to spin fluctuations due to the short-range SDW.

To further clarify the short-range orders, we analyze La(2) NQR peaks more carefully. The full width at half maximum (FWHM) obtained from the two-component fitting is plotted in Figure 2 (e) as a function of temperature. The linewidth for I>1/2I > 1/2 nuclei generally receives contributions from both quadrupole (wqw^{\mathrm{q}}) and magnetic (wmw^{\mathrm{m}}) interactions, as described by [23, 29, 46]:

(wn)2=(wnq)2+(wm)2.(3)(w_{\mathrm{n}})^{2} = (w_{\mathrm{n}}^{\mathrm{q}})^{2} + (w^{\mathrm{m}})^{2}. \tag*{(3)}

Theoretically, w1q:w2q:w3q=1:2:3w_{1}^{\mathrm{q}} : w_{2}^{\mathrm{q}} : w_{3}^{\mathrm{q}} = 1 : 2 : 3, whereas wmw^{\mathrm{m}} has an identical effect on each of the three transition peaks. From the fitting analysis, w2Lw_{2L} and w3Lw_{3L} are found to be nearly temperature-independent, whereas w2Gw_{2G} and w3Gw_{3G} increase markedly with decreasing temperature. To compare their relative evolutions, the FWHM ratio w3G/w2Gw_{3G}/w_{2G} is plotted in the inset to Figure 2 (e). This ratio is about 1.1 near T∗T^{*}, indicating that magnetic broadening is dominant in this regime. It increases gradually upon cooling and attains ∼1.5\sim1.5 near TDWT_{\mathrm{DW}}, revealing a continuous growth of the quadrupolar contribution to the ordered-state linewidth. By combining the linewidths of the ±3/2↔±5/2\pm3/2 \leftrightarrow\pm5/2 and ±5/2↔±7/2\pm5/2 \leftrightarrow\pm7/2 peaks, we obtain the temperature dependence of wGmw^{\mathrm{m}}_{G} and wGqw^{\mathrm{q}}_{G} in Figure 2 (d). wGqw^{\mathrm{q}}_{G} begins to increase near 150 K, indicating that the spatial distribution of the local EFG starts to broaden. Concurrently, f2Gf_{2G} and f3Gf_{3G} change abruptly from their L counterparts at this temperature, reflecting a modification of the ensemble-averaged EFG. These features collectively signify that T∗T^{*} – which signifies the onset of short-range SDW order – is also onset of a short-range CDW order. In this sense, we claim here that the La(2) site is also capable of sensing the short-range CDW order that was proposed to appear first in the inner Ni–O layer [42].

Presumably, wGmw^{\mathrm{m}}_{G} is also anticipated to increase when magnetic order appears, as is the case in La3_3Ni2_2O7_7 [23]. However, to our surprise, a pronounced decrease rather than increase is observed. Considering the applicability of (3), when the linewidth contributions from the charge order and the spin order are mutually NOT independent, their interaction may give rise to a coupling term Cov⁡(δνq,δνm)\operatorname{Cov}(\delta\nu^{\mathrm{q}},\delta\nu^{\mathrm{m}}) [47], in which situation (3) changes into

(wn)2=(wnq)2+(wm)2+2Cov⁡(δνq,δνm).(4)(w_{\mathrm{n}})^{2} = (w_{\mathrm{n}}^{\mathrm{q}})^{2} + (w^{\mathrm{m}})^{2} + 2\operatorname{Cov}(\delta\nu^{\mathrm{q}},\delta\nu^{\mathrm{m}}). \tag*{(4)}

where δνq\delta\nu^{\mathrm{q}} is the quadrupolar frequency shift, and δνm\delta\nu^{\mathrm{m}} is the magnetic frequency shift. Given that the system is undergoing a transition from short-range to long-range order – a process during which all individual contributions are expected to increase – one arrives at the conclusion that Cov⁡(δνq,δνm)<0\operatorname{Cov}(\delta\nu^{\mathrm{q}},\delta\nu^{\mathrm{m}}) < 0. The negative coupling term may originate from antiphase modulation between CDW and SDW order parameters [48, 49], negative hyperfine coupling constant [50], or negative response coefficient of the local EFG [51]. Most crucially, the phenomena observed in La4_4Ni3_3O10_{10} differ remarkably from those in La3_3Ni2_2O7_7 [23], providing compelling evidence for intertwining between SDW and CDW orders in La4_4Ni3_3O10_{10}.

139La NQR at p≈2.3p \approx2.3 GPa

The aforementioned difference between La4_4Ni3_3O10_{10} and La3_3Ni2_2O7_7 reminds us to further look into the evolution of the DW orders of La4_4Ni3_3O10_{10} under pressure. For this purpose, we conducted the same NQR experiments under a hydrostatic pressure of ∼2.3\sim2.3 GPa, and the results are summarized in Figure 3.

Multi-panel plots of La(2) NQR spectra, relaxation rate, resonance frequency, linewidth, and stretching exponent

Figure 3. (a) La(2) ±5/2↔±7/2\pm5/2 \leftrightarrow\pm7/2 NQR transition peak of La₄Ni₃O₁₀ at 2.3 GPa. The areas colored by orange and blue depict the fittings to Lorentzian and Gaussian functions, respectively. (b) Temperature dependence of 1/T1T1/T_1T at La(2); comparison between ambient pressure (black) and 2.3 GPa (blue). (c) f3(T)f_3(T). (d) w3(T)w_3(T). (e) Stretching exponent bb obtained from T1T_1 fitting.

Figure 3 (a) displays the La(2) ±5/2↔±7/2\pm5/2 \leftrightarrow\pm7/2 transition spectra under 2.3 GPa at selected temperatures (Note [52]), and Figure 3 (b) shows the temperature dependence of 1/T1T1/T_{1}T in comparison with the ambient-pressure results. It is clearly seen that now the NQR signal survives until below 116 K, and meanwhile, 1/T1T1/T_{1}T also appears to peak at around 116 K; in other words, the long-range DW transition now is suppressed to TDW≈116T_{\mathrm{DW}} \approx116 K. Similar to the atmosphere case, a second small peak arising from short-range SDW is also observed above TDWT_{\mathrm{DW}} in 1/T1T1/T_{1}T; likewise, its characteristic temperature is defined as T∗≈148T^{*} \approx148 K, seeing the inset to Figure 3 (b). This explicitly implies that the suppression of long-range orders by pressure is much faster than the short-range ones. Another important feature is that the 1/T1T1/T_{1}T under pressure are consistently lower than those at ambient pressure in the high temperature regime (160 K - 300 K), indicating that pressure reduces the density of states near the Fermi level. This observation is consistent with theoretical predictions [53, 54, 55, 56].

Akin to that at atmosphere, the La(2) NQR resonance peak begins to deviate from the Lorentzian shape near T∗T^*, cf Figure 3(a). Therefore, we also decompose the signal into a disordered-state Lorentzian function and an ordered-state Gaussian function. The temperature dependencies of f3f_3 for both L and G components are displayed in Figure 3(c). The obtained f3Lf_{3\mathrm{L}} is also quasi-linear with TT, but their values are increased by ∼1\sim1 % when compared with those at atmosphere. The as-derived w3w_3 for both L and G components are presented in Figure 3(d). Both f3Gf_{3\mathrm{G}} and w3Gw_{3\mathrm{G}} change abruptly from their L counterparts at T∗T^*, indicating that the line broadening below T∗T^* is accompanied with a modification of the EFG, and hence the short-range SDW and CDW are also intertwined under this pressure.

To further elucidate the spin dynamics behavior across the phase transitions, we present in Figure 3(e) the stretching exponent bb from the T1T_1 fitting. In general, bb quantifies the homogeneity of spin-lattice relaxation process.

The necessity of employing this stretching exponent to the fitting is demonstrated in Figure S3 [36]. First of all, a common feature for p=0p = 0 and 2.3 GPa is that bb is close to 1 at high temperature, and starts to deviate obviously right below T∗T^* where short-range DW orders come into being. This suggests that the appearance of short-range DW orders is responsible for the reduction of relaxation homogeneity. Another salient feature is that the decrease of bb under pressure is much slower than that at atmosphere.

Figure S3. The spin-lattice relaxation time (T1T_1) was obtained by fitting the recovery curve of the ±5/2↔±7/2\pm5/2 \leftrightarrow\pm7/2 transition. bb is stretching exponent. A smaller bb corresponds to a broader T1T_1 distribution, indicative of greater inhomogeneity of the local environment. (a) At 180 K and ambient pressure, both stretched and standard fits yield similar results. (b) At 140 K and ambient pressure, b=0.679b=0.679. (c) At 120 K and 2.3 GPa, b=0.889b=0.889.

Based on these results, we construct the pressure - temperature phase diagram, as shown in Figure 4. The pressure dependent TDWT_{\mathrm{DW}} derived in this work is in line with the previous transport measurements [16, 18]. Moreover, our study reveals the emergence of short-range intertwined DW orders prior to the long-range DW transitions. Remarkably, while the short-range DW orders are suppressed at a rate of 1 K/GPa, the long-range orders exhibit a significantly faster suppression rate of 10 K/GPa. This leads to a larger window of short-range DW phase under pressure on the phase diagram, which is compatible with the much slower reduction of bb as mentioned above.

Pressure-temperature phase diagram of La4Ni3O10

Figure 4. Pressure - temperature phase diagram of La4_4Ni3_3O10_{10}. In the monoclinic phase (low pressure), short-range DW orders develop upon cooling at T∗T^*, followed by the establishment of long-range (LR) DW orders at TDWT_{\mathrm{DW}}. The CDW and SDW orders are intertwined and likely suppressed simultaneously by pressure, up to 2.3 GPa.

It is worthwhile to compare the phase diagram of La4_4Ni3_3O10_{10} with that of the bilayer La3_3Ni2_2O7_7. A major difference is that the SDW order was found to be enhanced by pressure in La3_3Ni2_2O7_7, which not only suggests that the SDW order is decoupled from the lower-temperature DW, but also indicates that SDW does not compete with superconductivity. The enhanced competition between the coexisting intertwined density waves and superconductivity in La4_4Ni3_3O10_{10} is probably a factor to the reduction of TcT_{\mathrm{c}}.

Finally, since our experiments only probed the interlayer La(2) sites and thus lacked the information on the La(1) sites, we are unable to confirm the sequential layer effect in the formation of SDW and CDW as was previously reported by other groups [28, 42]. 139{}^{139}La nuclear magnetic resonance (NMR) experiments under pressure will be needed to complement the present work. Nevertheless, our detailed NQR measurements demonstrate that weak short-range ordered SDW and CDW can be detected at the interlayer La(2) sites.

Conclusions

In summary, NQR measurements on the La(2) site of La4_4Ni3_3O10_{10} reveal successive short-range and long-range intertwined SDW and CDW orders at ambient pressure. Under a hydrostatic pressure up to 2.3 GPa, the intertwined DW orders appear to be suppressed simultaneously. It is also found that the long-range DW orders are suppressed much faster than the short-range orders. Compared to La3_3Ni2_2O7_7, the intertwined DW orders in La4_4Ni3_3O10_{10} appear to compete more strongly with superconductivity. These findings shed new light to the interplay between density-wave instabilities and superconductivity in RP-phase nickelates.

Acknowledgments

The authors thank Yaomin Dai, Tao Wu, Meng Wang, Jun Zhao, and Yuefeng Nie for helpful discussions. This work is supported by the National Key R&D Program of China (2023YFA1609600 and 2022YFA1602602), National Natural Science Foundation of China (U23A20580 and 52588101), and Beijing National Laboratory for Condensed Matter Physics (2024BNLCMPKF004).

Data availability

All data that support the findings of this study are available from the corresponding authors upon request.

Supplemental Material: 139La^{139}\mathrm{La} nuclear quadrupole resonance studies of pressurized La4_4Ni3_3O10_{10}

Meng Zhang; Zhuo Wang; Yantao Cao; Yang Yuan; Kangjian Luo; Shanxiang Gao; Hanjie Guo; Yongkang Luo

In this Supplemental Material (SM), we provide additional results that further support the discussion and conclusion in the main text, including magnetic susceptibility χ(T)\chi(T), determination of asymmetry parameter η\eta, and comparison of T1T_1 fittings with and without stretching exponent bb.

SM I. Magnetic susceptibility

SM II. Determining the EFG asymmetry parameter η\eta

The nuclear quadrupole resonance (NQR) Hamiltonian is given by:

HQ=eQVzz4I(2I−1)[3I^z2−I^2+η(I^x2−I^y2)].(5)\mathcal{H}_{Q} = \frac{eQV_{zz}}{4I(2I-1)} \left[3\hat{I}_{z}^{2} - \hat{I}^{2} + \eta\left(\hat{I}_{x}^{2} - \hat{I}_{y}^{2}\right)\right]. \tag*{(5)}

Diagonalization is achieved through the eigenvector matrix UU:

Hp=UHQU†.(6)\mathcal{H}_{p} = U\mathcal{H}_{Q}U^{\dagger}. \tag*{(6)}

The transition frequencies are derived by the absolute differences between the eigenvalues,

f=∣Hp(i,i)−Hp(j,j)∣/h.(7)f = \left|\mathcal{H}_{p}(i,i) - \mathcal{H}_{p}(j,j)\right|/h. \tag*{(7)}

f2f_{2} and f3f_{3} are obtained in this way, and their ratio f3/f2f_{3}/f_{2} as a function of η\eta can be computed and shown in Figure S2, whose comparison with the experimental yields the best fit η≈0.088\eta\approx0.088 at 180 K.

SM III. Fitting of T1T_1 recovery curves

M(t)=M(∞){1−2F[257412012exp⁡(−(3tT1)b)+780012012exp⁡(−(10tT1)b)+163812012exp⁡(−(21tT1)b)]}(8)M(t)=M(\infty)\left\{1-2F\left[\frac{2574}{12012}\exp\left(-\left(\frac{3t}{T_1}\right)^b\right)+\frac{7800}{12012}\exp\left(-\left(\frac{10t}{T_1}\right)^b\right)+\frac{1638}{12012}\exp\left(-\left(\frac{21t}{T_1}\right)^b\right)\right]\right\} \tag*{(8)}

References

  1. [1][1–5]
  2. [2][1–5]
  3. [3][1–5]
  4. [4][1–5]
  5. [5][1–5]
  6. [6][6]
  7. [7][7]
  8. [8][8–13]
  9. [9][8–13]
  10. [10][8–13]
  11. [11][8–13]
  12. [12][8–13]
  13. [13][8–13]
  14. [14][14]
  15. [15][15–17]
  16. [16][15–17]
  17. [17][15–17]
  18. [18][18]
  19. [19][19–21]
  20. [20][19–21]
  21. [21][19–21]
  22. [22][22]
  23. [23][23–25]
  24. [24][23–25]
  25. [25][23–25]
  26. [26][24–26]
  27. [27][24, 26, 27]
  28. [28][28–33]
  29. [29][28–33]
  30. [30][28–33]
  31. [31][28–33]
  32. [32][28–33]
  33. [33][28–33]
  34. [34][34]
  35. [35][35]
  36. [36][36]
  37. [37]K. Kitagawa, H. Gotou, T. Yagi, A. Yamada, T. Matsumoto, Y. Uwatoko, and M. Takigawa, Space Efficient Opposed-Anvil High-Pressure Cell and Its Application to Optical and NMR Measurements up to 9 GPa, J. Phys. Soc. Jpn. 79, 024001 (2010).DOI
  38. [38]F. Y. Li, Y. Q. Hao, N. Guo, D. H. Jia, J. Dou, D. Peng, G. T. Zhang, L. F. Xiao, J. Zhang, W. J. Zhou, Y. H. Huang, X. Y. Wang, Z. Y. Guo, M. Mezouar, J. E. F. S. Rodrigues, J. Luo, J. Yang, Q. S. Zeng, R. Zhou, H. Y. Gou, Q. Zheng, G. T. Liu, and J. J. Zhang, Single-Crystal Structure Determination of Superconducting High Pressure La₄Ni₃O₁₀−δ, Adv. Mater. 37, e07365 (2025).DOI
  39. [39]S. Ramakrishnan, Y. Gao, V. Olevano, E. Pachoud, A. Hadj-Azzem, G. Garbarino, M. dAstuto, O. Perez, A. Pautrat, D. Valenti, M. Quénot, S. Pairis, D. Chernyshov, L. Noohinejad, C. Paulmann, J. Bulled, A. Bosak, S. van Smaalen, P. Toulemonde, M.-A. Méasson, and P. Rodi‘ere, Tracing the horizon of tetragonal-to-monoclinic distortion in pressurized trilayer nickelate La₄Ni₃O₁₀, Commun. Mater. 7, 191 (2026).DOI
  40. [40]J. Li, C.-Q. Chen, C. Huang, Y. Han, M. Huo, X. Huang, P. Ma, Z. Qiu, J. Chen, X. Hu, L. Chen, T. Xie, B. Shen, H. Sun, D.-X. Yao, and M. Wang, Structural transition, electric transport, and electronic structures in the compressed trilayer nickelate La₄Ni₃O₁₀, Sci. China Phys. Mech. Astron. 67, 117403 (2024).DOI
  41. [41]Kakoi, M., Oi, T., Oshita, Y., Yashima, M., Kuroki, K., Kato, T., Takahashi, H., Ishiwata, S., Adachi, Y., Hatada, N., Uda, T., & Mukuda, H. (2024). Multiband metallic ground state in multilayered nickelates La3Ni2O7 and La4Ni3O10 probed by 139La-NMR at ambient pressure. J. Phys. Soc. Jpn., 93, 053702.
  42. [42]Y. Wang, D. Zhao, E. Zhang, L. Chen, Y. Zhou, M. Shi, Y. Zhu, J. Ying, J. Zhao, and T. Wu, Unconventional density-wave state in Ruddlesden–Popper nickelate La₄Ni₃O₁₀, Nat. Commun. 17, 6422 (2026).DOI
  43. [43]N. K. Gupta, R. Gong, Y. Wu, M. Kang, C. T. Parzyck, B. Z. Gregory, N. Costa, R. Subarto, S. Sarker, A. Singer, D. G. Schlom, K. M. Shen, and D. G. Hawthorn, Anisotropic spin stripe domains in bilayer La₃Ni₂O₇, Nat. Commun. 16, 6560 (2025).DOI
  44. [44]Samila, A., Safronov, I., & Hotra, O. (2020). Structural and functional synthesis of the continuous wave NQR temperature sensor with increased conversion linearity. Solid State Nucl. Magn. Reson., 110, 101700.
  45. [45]Abragam, A. (1961). Principles of Nuclear Magnetism.
  46. [46]Grafe, H.-J., Curro, N. J., Young, B. L., Vyalikh, J., Gu, G. D., Hücker, M., & Büchner, B. (2010). Charge order and low frequency spin dynamics in lanthanum cuprates revealed by Nuclear Magnetic Resonance. Eur. Phys. J. Spec. Top., 188, 89.
  47. [47]K. Chen, A Practical Review of NMR Lineshapes for Spin-1/2 and Quadrupolar Nuclei in Disordered Materials, Int. J. Mol. Sci. 21, 5666 (2020).DOI
  48. [48]J. M. Tranquada, J. D. Axe, N. Ichikawa, Y. Nakamura, S. Uchida, and B. Nachumi, Neutron-scattering study of stripe-phase order of holes and spins in La₁.₄₈Nd₀.₄Sr₀.₁₂CuO₄, Phys. Rev. B 54, 7489 (1996).pubmed.ncbi.nlm.nih.gov/9984376
  49. [49]H. Miao, R. Fumagalli, M. Rossi, J. Lorenzana, G. Seibold, F. Yakobou-Harris, K. Kummer, N. B. Brookes, G. D. Gu, L. Braicovich, G. Ghiringhelli, and M. P. M. Dean, Formation of Incommensurate Charge Density Waves in Cuprates, Phys. Rev. X 9, 031042 (2019).DOI
  50. [50]M. W. Pieper, H. Michor, and T. Ali, NMR compared to band structure calculations of the quaternary superconductor La₃Ni₂B₂N₃−x, Phys. Rev. B 85, 214510 (2012).DOI
  51. [51]A. Kanigel and A. Keren, In-plane hole density in (Ca₀.₁La₀.₉)(Ba₁.₆₅La₀.₃₅)Cu₃Oᵧ: Nuclear resonance study over the full doping range, Phys. Rev. B 74, 012505 (2006).DOI
  52. [52]Since there is a large noise near 10.4 MHz in our spectrometer, which hindered the measurements of the La(2) ±3/2 ↔ ±5/2 transition at 2.3 GPa. Consequently, only the ±5/2 ↔ ±7/2 transition was measured.. (n.d.). Since there is a large noise near 10.4 MHz in our spectrometer, which hindered the measurements of the La(2) ±3/2 ↔ ±5/2 transition at 2.3 GPa. Consequently, only the ±5/2 ↔ ±7/2 transition was measured..
  53. [53]Wang, J.-X., Ouyang, Z., He, R.-Q., & Lu, Z.-Y. (2024). Non-Fermi liquid and Hund correlation in La4Ni3O10 under high pressure. Phys. Rev. B, 109, 165140.
  54. [54]H. LaBollita, J. Kapeghian, M. R. Norman, and A. S. Botana, Electronic structure and magnetic tendencies of trilayer La₄Ni₃O₁₀ under pressure: Structural transition, molecular orbitals, and layer differentiation, Phys. Rev. B 109, 195151 (2024).DOI
  55. [55]Y. Zhang, L.-F. Lin, A. Moreo, T. A. Maier, and E. Dagotto, Prediction of $s^{\pm}$-wave superconductivity enhanced by electronic doping in trilayer nickelates La₄Ni₃O₁₀ under pressure, Phys. Rev. Lett. 133, 136001 (2024).DOI
  56. [56]Z. Huo, Z. Zhang, Z. Zhang, D. Duan, and T. Cui, Electronic correlations and Hund’s rule coupling in trilayer nickelate La₄Ni₃O₁₀, Sci. China Phys. Mech. Astron. 68, 127411 (2025).arxiv.org/abs/2407.00327

Paper details

vlnc:W_nqedhffd
Version
v1 · latest
Published
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents