betaFeedback

WorksPhysics and Astronomy

Strain Effect on Rashba Splitting and Phonon Scattering to Improve Thermoelectric Performance of 2D Heterobilayer MoTe2_{2}/PtS2_{2}

Abstract

Rashba spin-orbit coupling significantly modifies the electronic band structure in two-dimensional (2D) van der Waals (vdW) heterobilayers, which may enhance their thermoelectric (TE) properties. In this study, we use first-principles calculations and Boltzmann transport theory to explore the strain effect on the TE performance of the 2D vdW heterobilayer MoTe2_{2}/PtS2_{2}. A strong Rashba spin-splitting is observed in the valence band, resulting in an increase in the Seebeck coefficient for p-type. The lattice thermal conductivity of MoTe2_{2}/PtS2_{2} is remarkably low about of 0.6 Wm−1^{-1}K−1^{-1} at T=300T = 300 K due to large anharmonic scattering. Furthermore, biaxial strain enhances the power factor (PF) by introducing band convergence. At a strain of 2%, the optimal PF for the n-type material reaches 170 μμW/cmK2^{2}, indicating approximately 84.78% increase compared to the unstrained state (92 μμW/cmK2^{2}). Given the low lattice thermal conductivity, the optimized figure of merit ZTZT achieves up to 0.88 at 900 K for n-type. Our findings indicate that MoTe2_{2}/PtS2_{2} is a highly promising candidate for 2D heterobilayer TE materials, owing to its strong Rashba splitting and significant anharmonicity.

K for n-type. Our findings indicate that MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} is a highly promising candidate for 2D heterobilayer TE materials, owing to its strong Rashba splitting and significant anharmonicity.

Keywords

Introduction

Nowadays, fossil energy sources are causing environmental pollution and are gradually depleting due to the increasing energy demand. Therefore, a thermoelectric (TE) generator, which can directly convert waste heat into electricity, is a practical solution to address the issue of fossil energy.[1, 2, 3] To evaluate the performance of the energy conversion of the TE device, the figure of merit, ZT=S2σT/(κel+κph)ZT = S^{2}\sigma T/(\kappa_{\mathrm{el}} + \kappa_{\mathrm{ph}}), is used, where SS, σ\sigma, κel\kappa_{\mathrm{el}}, κph\kappa_{\mathrm{ph}}, and TT are the Seebeck coefficient, electrical conductivity, thermal conductivities by electron, thermal conductivities by lattice, and temperature, respectively.[4] Here, the S2σS^{2}\sigma is the TE power factor (PF). A material considered suitable for the TE device should have a high ZTZT or PF.[5]

Several methods have been proposed to enhance the PF and ZTZT, such as resonant state,[6] chemical material,[7] quantum enhancement effect in low-dimensional semiconductors,[8, 9, 10, 11] band convergence,[12, 13] and Rashba spin-orbit coupling (SOC).[14] Among them, the Rashba SOC depends only on the intrinsic properties of the material without requiring additional external factors. The Rashba SOC leads to the enhanced electronic density of states, resulting in a larger Seebeck coefficient.[15] Yuan et al.14`` indicated that Rashba SOC can enhance the TE performance by 78% for BiSb monolayer. They point out that Rashba SOC not only induces a one-dimensional (1D) density of states near the band edge but also improves the carrier lifetimes in the Rashba spin-splitting system, leading to a significant enhancement of the PF. Bera [16] studied the effect of Rashba SOC on the TE properties of HfX2_2 (X = S, Se) and Janus HfSSe monolayers, and they indicated that Rashba SOC enhances the PF for n-type carriers of these materials. The highest achieved ZTZT values of HfS2_2, HfSe2_2, and HfSSe monolayers are 0.90, 0.84, and 0.81 at 600 K, respectively. Some recent studies also demonstrated that the Rashba SOC can play a crucial role in enhancing the TE properties of monolayer materials. [17, 18] However, monolayer materials with strong Rashba SOC often exhibit high thermal conductivity. For example, κph\kappa_{\mathrm{ph}} of Si2_2AsSb and Si2_2AsSb is 72.2 W/mK and 49.3 W/mK at room temperature, respectively, [15] which is larger than that of well-known TE materials, such as Bi2_2Te3_3 (∼1.4\sim1.4 W/mK),[19] and PbTe (∼2.0\sim2.0 W/mK).[20] Thus, searching for two-dimensional (2D) materials with high Rashba SOC to enhance PF, along with low κph\kappa_{\mathrm{ph}}, is essential to achieve a high ZTZT.

The 2D van der Waals (vdW) heterobilayers could be a potential candidate for 2D materials with both high Rashba SOC and low κph\kappa_{\mathrm{ph}}. Gupta et al.[21] found that the 2D vdW heterobilayer MoTe2_2/PtS2_2 with AB stacking structure has a strong Rashba SOC,[21] in which the Rashba parameter, αR∼8\alpha_R \sim8 eVÅ, is much larger than that of other 2D materials, such as Janus WSeTe (αR=0.92\alpha_R = 0.92 eVÅ)[22] and BiTeI monolayers (αR=1.86\alpha_R = 1.86 eVÅ).[23] In addition, it was suggested that forming vdW heterobilayers can effectively reduce the lattice thermal conductivity. [24, 25, 26] Hu et al.[27] reported that κph\kappa_{\mathrm{ph}} of the 2D vdW heterobilayer black-phosphorus/blue-phosphorus at T=300T = 300 K is 3.85 and 4.18 W/mK along the xx- and yy-directions, respectively. These values are significantly lower than those of black-phosphorus monolayer (7.49 and 23.43 W/mK) and blue-phosphorus monolayer (21.76 and 21.76 W/mK), respectively. Thus, it suggest that heterobilayer MoTe2_2/PtS2_2 could has low lattice thermal conductivity. Moreover, in a previous theoretical study, Yin et al.[28] indicated that the energy band gap of MoTe2_2/PtS2_2 is 1.26 eV by using the hybrid functional HSE calculation, which is a suitable band gap for TE materials. On the other hand, the 2D vdW heterobilayer MoSe2_2/PtSe2_2, which has a similar structure of MoTe2_2/PtS2_2, has also been successfully synthesized experimentally. [29] A combination of large Rashba SOC, a suitable band gap, and possible low κph\kappa_{\mathrm{ph}} and forming heterobilayer suggests that 2D vdW heterobilayers MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} could be a promising candidate for 2D TE material.

In this study, we investigate the effect of strain on the electron, phonon, and TE performance of 2D vdW heterobilayer MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} by using first-principles calculations and Boltzmann transport theory. The strain promotes the convergence of multivalley bands, resulting in an enhancement of both the PF and ZTZT. We find that the band convergence can be achieved for both n-type and p-type by a biaxial strain of ε=0.02\varepsilon= 0.02 and ε=0.03\varepsilon= 0.03, respectively. The maximum PF of n-type MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} reaches 170 μW/cmK2 W/mK2170\,\mu\mathrm{W}/\mathrm{cmK}^{2}\ \mathrm{W}/\mathrm{mK}^{2} at T=300T = 300 K. The lattice thermal conductivity of MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} is remarkably low about of 0.6 W/mK at room temperature) because of strong phonon scattering, and the maximum ZTZT is 0.88 at 900 K for n-type.

Methodology

We use density functional theory (DFT) with the Quantum ESPRESSO package [30, 31] to perform the calculations. The optimized norm-conserving Vanderbilt pseudopotentials [32] are adopted to calculate the exchange-correlation functionals, [33] in which we use the Perdew-Burke-Ernzerhof (PBE) functionals. The Heyd-Scuseria-Ernzerhof (HSE) method [34] is used to accurately calculate the band gap. The Wannier90 package [35] is used to interpolate the band dispersion from the HSE calculation. The SOC is considered in our calculations. An energy cutoff of 80 Ry is used for the plane wave basis set. To eliminate interactions due to periodic boundary conditions, a vacuum region of 20 Å is set along the zz-direction, perpendicular to the sheet plane. The phonon dispersion is calculated by using density-functional perturbation theory (DFPT) [36] with a qq-point grid of 8×8×18 \times8 \times1, which is selected based on the convergence test. The lattice constants and atomic positions are optimized via the BFGS algorithm [31] with convergence criteria of 0.00001 Ry/a.u. and 0.05 GPa for atomic forces and stress components, respectively. The Grimme-D2 method is used to describe the van der Waals (vdW) interaction between the MoTe2_2 and PtS2_2 layers.[37] For the optimization of the structure and the calculation of electronic properties, the kk-mesh is set to 12×12×112 \times12 \times1. The ab initio molecular dynamics (AIMD) simulations are performed to evaluate thermal stability. A 3×3×13 \times3 \times1 supercell is employed within the NVT ensemble, with temperature control regulated by the Nose-Hoover method[38] and a time step of 1 fs.

The Seebeck coefficient SS, electrical conductivity σ\sigma, and electronic thermal conductivity κel\kappa_{\mathrm{el}} are calculated by solving the Boltzmann transport theory for electrons by using the BoltzWann code.[39] The deformation potential approximation is applied to estimate the relaxation time constant for the Boltzmann transport theory, which is estimated by both longitudinal acoustic (LA) and longitudinal optical (LO) phonon modes in the present study. The lattice thermal conductivity κph\kappa_{\mathrm{ph}} is calculated by solving the Boltzmann transport equation for phonons by using the ShengBTE package.[40] The anharmonic interatomic force constants are calculated using the THIRDORDER.py tool[40] with the 3×3×13 \times3 \times1 supercell. A dense grid of 48×48×148 \times48 \times1 is used to evaluate the Boltzmann transport equation for phonons. The Bader code[41] is used to analyze the charge transfer. The parameters in the present calculations, including cutoff energy, kk-points, and qq-points, are carefully selected based on convergence testing.

Results and discussion

Optimized structure and structural stability

In Figure 1(a) and (Figure 1b), we show the top and side views of the optimized structure of the 2D vdW heterobilayer MoTe2_2/PtS2_2 with AB stacking order, respectively. In the AB stacking, the S atom from the PtS2_2 layer is aligned with the Mo atom from the MoTe2_2 layer, as shown in Figure 1(b). The optimized lattice constant aa, interlayer distance dmidd_{\mathrm{mid}} and outer distance douterd_{\mathrm{outer}} of the heterobilayer are 3.560 Å, 6.062 Å and 9.096 Å, respectively. We note that the optimized lattice constants of the MoTe2_2 and PtS2_2 monolayers are 3.550 Å and 3.580 Å, respectively. Thus, the lattice mismatch between MoTe2_2 and PtS2_2 is small (∼0.85%\sim0.85\%), which suggests that heterobilayer MoTe2_2/PtS2_2 can be formed without bending strain or moiré patterns. The Pt-S1_1, Pt-S2_2, Mo-Te1_1 and Mo-Te2_2 bond lengths (see Figure 1(b)) are l1=2.404l_1 = 2.404 Å, l2=2.396l_2 = 2.396 Å, l3=2.735l_3 = 2.735 Å, and l4=2.737l_4 = 2.737 Å, respectively, which are in good agreement with previous report. [42]

Top and side views of the 2D vdW heterobilayer MoTe$_2$/PtS$_2$

Figure 1. Top (a) and side (b) views of the 2D vdW heterobilayer MoTe2_2/PtS2_2, in which the black box indicates the unit cell, and aa, l1,2,3,4l_{1,2,3,4}, dmidd_{\mathrm{mid}}, and douterd_{\mathrm{outer}} denote the lattice constant, bond lengths, interlayer distance, and distance between the two outermost atoms, respectively.

To examine the stability of the 2D vdW heterobilayer MoTe2_2/PtS2_2, we first calculate the binding energy EbE_b:

Eb=EMoTe2/PtS2−EMoTe2−EPtS2,(1)E_b = E_{\mathrm{MoTe_2/PtS_2}} - E_{\mathrm{MoTe_2}} - E_{\mathrm{PtS_2}}, \tag*{(1)}

where EMoTe2/PtS2E_{\mathrm{MoTe_2/PtS_2}}, EMoTe2E_{\mathrm{MoTe_2}}, and EPtS2E_{\mathrm{PtS_2}} are the total energy of the heterobilayer, MoTe2_2, and PtS2_2 monolayers, respectively. The calculated Eb=−0.36E_b = -0.36 eV is consistent with the previous report (-0.33 eV). [28] Moreover, Almayyalia et al. [42] also indicated that the AB stacking has the lowest binding energy compared to that of the AA, AA′, and AB stacking orders. Therefore, the AB stacking is chosen to investigate the TE properties of MoTe2_2/PtS2_2 in the present study.

Next, to examine the dynamic stability of MoTe2_2/PtS2_2, we calculate the phonon dispersion. As shown in Figure 3(a), MoTe2_2/PtS2_2 exhibits good dynamic stability, as its phonon dispersion contains no imaginary frequencies. In additional, the calculated the elastic constants C11=184.04C_{11} = 184.04 N/m, ∣C12∣=51.94\lvert C_{12}\rvert= 51.94 N/m, and C66=66.5C_{66} = 66.5 N/m, satisfy the Born criterion for mechanical stability (C11>∣C12∣>0C_{11} > \lvert C_{12}\rvert> 0 and C66>0C_{66} > 0).[43] Thus, MoTe2_2/PtS2_2 is mechanical stable. We also perform the AIMD simulations at 900 K, as shown in Figure S1 in Supporting Information, to evaluate the thermal stability. The obtained results reveal that the energy fluctuation is small, and the atomic configuration remains stable, showing no obvious distortion. This implies that MoTe2_2/PtS2_2 exhibits strong thermal stability and is well-suited for high-temperature TE applications.

Figure 3. (a) Phonon dispersion and (b) phonon density of states (phDOS) of 2D vdW heterobilayer MoTe2_2/PtS2_2. (c) Side view of the atomic vibrations of the longitudinal optical phonon modes at the Γ\Gamma point, in which LO1_1 and LO2_2 phonon modes are found on the MoTe2_2 and PtS2_2 layers, respectively.

Energy band structure and carrier mobility

In Figure 2(a), we show the band structure of MoTe2_2/PtS2_2 by using HSE + SOC calculations. Our calculations show that MoTe2_2/PtS2_2 exhibits an indirect band gap, with the conduction band minimum (CBM) located at K1_1 (along the Γ\Gamma-K direction) and the valence band maximum (VBM) located at the K point. The calculated band gap of MoTe2_2/PtS2_2 is 0.93 eV, which is consistent with previous theoretical reports (1.06 eV).[28]

Figure 2. (a) Energy band structure along the high symmetry points and (b) electronic density of states (eDOS) of the 2D vdW heterobilayer MoTe2_2/PtS2_2 using the HSE + SOC method. The blue and red colors indicate the contribution of the MoTe2_2 and PtS2_2 layers, respectively.

In Figure 2(b), we calculate the projected electronic density-of-states (eDOS) to examine the contribution of each material layer to the overall band structure. The calculated results indicate that the CBM is mainly contributed by the PtS2_2 layer, while the VBM mainly originates from the MoTe2_2 layer. As shown in Figure 2(a), the Rashba splitting and a VBM in the valence band are found near the Γ\Gamma point (−0.8 eV) and at the K point (−0.5 eV), respectively. This leads to one-dimensional (1D) van Hove singularity and a constant 2D density of states around −0.8 eV and −0.5 eV,[44] respectively, as shown in Figure 2(b). These eDOS characteristics could make the outstanding TE properties of 2D materials, such as Janus γ\gamma-Ge2_2SSe$[45] and InSe.[13, 44] Thus, we also expect that the 2D vdW MoTe2_2/PtS2_2 heterobilayer will show high TE performance.

Since carrier mobility plays a crucial role in TE properties, we next determine the carrier mobility of MoTe2_2/PtS2_2. For 2D systems, the deformation potential approximation (DPA) is widely used to calculate mobility.[45, 46, 47] However, conventional DPA accounts only for electron-phonon scattering by longitudinal acoustic (LA) phonons. Thus, the DPA often overestimates the carrier mobility values by ignoring other scattering. For example, in a previous theoretical study, Cheng and Liu⁴⁸ reported that the electron mobility of H-MoTe2_2 is 37 cm2^2V−1^{-1}s−1^{-1} by considering both LA and longitudinal optical (LO) phonon scattering, whereas the DPA method predicts a value of 338 cm2^2V−1^{-1}s−1^{-1}. It highlights the significant contribution of LO phonon scattering to carrier mobility, particularly in the 2D polar system.[49, 50] Thus, in the present study, we also considered the influence of LO phonons when calculating the carrier mobility of the 2D vdW heterobilayer MoTe2_2/PtS2_2.

The carrier mobilities μ0LA\mu_0^{\mathrm{LA}} and μ0LO\mu_0^{\mathrm{LO}} for the 2D material are given by:[45, 46, 47, 49]

μ0LA=eℏ3C2DkBTmx(y)∗mx∗my∗Ed2(2)\mu_0^{\mathrm{LA}} = \frac{e\hbar^3 C_{\mathrm{2D}}}{k_{\mathrm{B}}T m_{x(y)}^* \sqrt{m_x^*m_y^*} E_{\mathrm{d}}^2} \tag*{(2)}

and

μ0LO=MAMBS0d02(ϵϵ0)2(ℏω)2e3ℏnℏωmx(y)∗1ZA2MB+4ZB2MA+4MAMB∣ZAZB∣(3)\mu_0^{\mathrm{LO}} = \frac{M_{\mathrm{A}}M_{\mathrm{B}}S_0d_0^2(\epsilon\epsilon_0)^2(\hbar\omega)^2}{e^3\hbar n_{\hbar\omega}m_{x(y)}^*}\frac{1}{Z_{\mathrm{A}}^2M_{\mathrm{B}}+4Z_{\mathrm{B}}^2M_{\mathrm{A}}+4\sqrt{M_{\mathrm{A}}M_{\mathrm{B}}}\lvert Z_{\mathrm{A}}Z_{\mathrm{B}}\rvert} \tag*{(3)}

for the LA and LO phonon scattering, respectively, where ee, ℏ\hbar, kBk_{\mathrm{B}}, and TT are the elementary charge, reduced Planck constant, Boltzmann constant, and temperature, respectively. d0d_0, ϵ\epsilon, and ϵ0\epsilon_0 represent effective thickness, in-plane dielectric constant, and vacuum permittivity, respectively. Here, d0d_0 is determined using the following expression: d0=douter+rS+rSed_0 = d_{\mathrm{outer}} + r_{\mathrm{S}} + r_{\mathrm{Se}}, where rSr_{\mathrm{S}} and rSer_{\mathrm{Se}} are the vdW radii of S and Se atoms, respectively.[51] MAM_{\mathrm{A}} and MBM_{\mathrm{B}} are the atomic mass, and ZAZ_{\mathrm{A}} and ZBZ_{\mathrm{B}} are the Born effective charges of metal A and chalcogen B atoms, respectively (see Table S1 in Supporting Information). nℏωn_{\hbar\omega} is the Bose-Einstein distribution at the LO phonon frequency at the Γ\Gamma point. mx∗m_x^* and my∗m_y^* are the effective masses along the xx- (armchair) and yy-directions (zigzag). To calculate mx∗m_x^* and my∗m_y^*, we use a 3×1\sqrt{3} \times1 supercell (see Figure S2 in Supporting Information). C2DC_{\mathrm{2D}} denotes the elastic constant and is defined as C2D=[∂2Etotal/∂(Δl/l0)2]/S0C_{\mathrm{2D}} = [\partial^2 E_{\mathrm{total}}/\partial(\Delta l/l_0)^2]/S_0, where S0S_0 is the equilibrium unit cell area, EtotalE_{\mathrm{total}} is the total energy after applying a uniaxial strain, l0l_0 is the lattice constant, Δl=(l−l0)/l0\Delta l = (l-l_0)/l_0 is the corresponding lattice distortion (see Figure S3 in Supporting Information). EdE_{\mathrm{d}} is the deformation potential constant and can be calculated as Ed=ΔE/εE_d = \Delta E/\varepsilon where ΔE\Delta E is the shift in the energy level of the CBM (or the VBM) relative to the vacuum level (see Figure S4 in Supporting Information).

The 2D vdW heterobilayer MoTe2_2/PtS2_2 has two distinct LO phonon modes, LO1 and LO2, correspond to the vibrations of the MoTe2_2 and PtS2_2 layers, respectively, as shown in Figure 3(c). Therefore, the total mobility μ0total\mu_0^{\mathrm{total}} can be obtained by using Matthiessen’s rule as follows:[48]

1μ0total=1μ0LO1+1μ0LO2+1μ0LA.(4)\frac{1}{\mu_0^{\mathrm{total}}} = \frac{1}{\mu_0^{\mathrm{LO1}}} + \frac{1}{\mu_0^{\mathrm{LO2}}} + \frac{1}{\mu_0^{\mathrm{LA}}}. \tag*{(4)}

The calculated values of μ0LO1\mu_0^{\mathrm{LO1}}, μ0LO2\mu_0^{\mathrm{LO2}} and μ0total\mu_0^{\mathrm{total}} of MoTe2_2/PtS2_2 without strain at T=300T = 300 K are listed in Table 1.

DirectionCarrierm∗/m0m^*/m_0EdE_dC2DC_{2D}μ0LO1\mu_0^{\mathrm{LO1}}μ0LO2\mu_0^{\mathrm{LO2}}μ0LA\mu_0^{\mathrm{LA}}μ0total\mu_0^{\mathrm{total}}τel\tau^{\mathrm{el}}
armchaire1.3441.23184.0434.5899.381434.1625.201.926
armchairh-0.761-1.2161.07175.514634.5844.871.942
zigzage1.344-1.27184.0434.5899.381345.2425.171.924
zigzagh-0.757-1.2161.40176.444659.0745.111.942

Table 1. Effective masses m∗/m0m^*/m_0, where m0m_0 is the mass of free electron, deformation potential EdE_d (eV), elastic modulus C2DC_{2D} (N/m), carrier mobilities contributed by LO1 (μ0LO1\mu_0^{\mathrm{LO1}}), LO2 (μ0LO2\mu_0^{\mathrm{LO2}}), LA modes (μ0LA\mu_0^{\mathrm{LA}}) and combined of these modes (μ0total\mu_0^{\mathrm{total}}) (cm2^2V−1^{-1}s−1^{-1}), and total relaxation time τel\tau^{\mathrm{el}} (×10−14\times10^{-14} s) of the 2D vdW heterobilayer MoTe2_2/PtS2_2 at 300 K.

Our results indicate that LO phonon scattering significantly limits the mobility of the 2D vdW heterobilayer MoTe2_2/PtS2_2, resulting in lower carrier mobility compared to the values predicted using DPA alone, as listed in Table 1. For example, the hole mobility μ0LO1\mu_0^{\mathrm{LO1}} is 61.07 (or 61.40) cm2^2V−1^{-1}s−1^{-1}, which leads to reduce two orders of magnitude of μ0total\mu_0^{\mathrm{total}} about 44.87 (or 45.11) cm2^2V−1^{-1}s−1^{-1} compared with μ0LA\mu_0^{\mathrm{LA}} about 4634.58 (or 4659.07) cm2^2V−1^{-1}s−1^{-1}) in the armchair (or zigzag) direction. This is because of the large Born effective charge of Mo (ZMo=−2.2eZ_{\mathrm{Mo}} = -2.2e) and Te (ZTe=1.1eZ_{\mathrm{Te}} = 1.1e) atoms of the MoTe2_2 layer, which is much larger than that of the WSe2_2 layer (ZW=−0.57eZ_{\mathrm{W}} = -0.57e and ZSe=0.27eZ_{\mathrm{Se}} = 0.27e[49]) in the Janus heterobilayer WSe2_2/SWSe. Since the strength of the LO phonon scattering is closely related to the magnitude of the Born effective charge. Thus, a large Born effective charge correlates with stronger carrier scattering, leading to reduced mobility in Eq. (3). Nevertheless, the Born effective charge reflects strong polarizability, which is the cause of a strong Rashba effect.[21] The total relaxation time τel=m∗μ0total/∣e∣\tau^{\mathrm{el}} = m^*\mu_0^{\mathrm{total}}/|e| is also listed in Table 1. The relationship between temperature and the relaxation time τel\tau^{\mathrm{el}} at different strain values is shown in Figures S5 to S8 (Supporting Information).

Mechanical properties

When applying the 2D vdW heterobilayer MoTe2_2/PtS2_2 in flexible devices, it is essential to consider both the mechanical properties and the thermoelectric (TE) performance under strain. The mechanical behavior of 2D materials in the elastic regime can be characterized by Young’s modulus, Y2D(θ)Y_{2D}(\theta), and Poisson’s ratio, ν(θ)\nu(\theta), which is determined using the following equations:[5, 45, 50]

Y2D(θ)=C11C22−C122C11sin⁡4(θ)+C22cos⁡4(θ)−(2C12−C11C22−C122C66)sin⁡2(θ)cos⁡2(θ)(5)Y_{2D}(\theta)=\frac{C_{11}C_{22}-C_{12}^{2}}{C_{11}\sin^{4}(\theta)+C_{22}\cos^{4}(\theta)-\left(2C_{12}-\frac{C_{11}C_{22}-C_{12}^{2}}{C_{66}}\right)\sin^{2}(\theta)\cos^{2}(\theta)} \tag*{(5)}

and

ν(θ)=C12(sin⁡4(θ)+cos⁡4(θ))−(C11+C22−C11C22−C122C66)sin⁡2(θ)cos⁡2(θ)C11sin⁡4(θ)+C22cos⁡4(θ)−(2C12−C11C22−C122C66)sin⁡2(θ)cos⁡2(θ)(6)\nu(\theta)=\frac{C_{12}\left(\sin^{4}(\theta)+\cos^{4}(\theta)\right)-\left(C_{11}+C_{22}-\frac{C_{11}C_{22}-C_{12}^{2}}{C_{66}}\right)\sin^{2}(\theta)\cos^{2}(\theta)}{C_{11}\sin^{4}(\theta)+C_{22}\cos^{4}(\theta)-\left(2C_{12}-\frac{C_{11}C_{22}-C_{12}^{2}}{C_{66}}\right)\sin^{2}(\theta)\cos^{2}(\theta)} \tag*{(6)}

where θ\theta represents the angular dependence of Young’s modulus and Poisson’s ratio.

In Figure 4(a), we plot Young’s modulus and Poisson’s ratio as a function of the angle θ\theta, respectively. Our calculations indicate that both quantities exhibit isotropic behavior. The calculated Y2DY_{2D} of MoTe2_2/PtS2_2 is 170 N/m, which is higher than that of the PtS2_2 monolayer (80.59 N/m)[52] but lower than that of the MoTe2_2 monolayer (116 N/m).[53] Similarly, the Poisson’s ratio (ν\nu) of 0.28 lies between the values for PtS2_2 (0.27)[52] and MoTe2_2 (0.32).[53]

Figure 4. (a) Young’s modulus Y2D(θ)Y_{2\mathrm{D}}(\theta) and Poisson’s ratio (ν(θ))(\nu(\theta)) as a function of the angle θ\theta. (b) Stress-strain curves along the biaxial strain and uniaxial strains along the xx- and yy-directions.

In Figure 4(b), we plot the stress-strain curves of MoTe2_2/PtS2_2 under biaxial strain and uniaxial strains along xx- and yy-directions. The maximum stress and its corresponding strain are known as the ideal strength (σi\sigma^{i}) and critical strain εc\varepsilon^{c}, respectively, representing the mechanical strength.[5, 45, 54, 55] For biaxial strain, σi\sigma^{i} and εc\varepsilon^{c} are 20.71 N/m and 0.18, respectively. The mechanical strength of MoTe2_2/PtS2_2 under biaxial strain are smaller than that of the AA-stacked MoSSe2_2/MoS2_2 (23.4 N/m, 0.21) and AB-stacked MoSSe2_2/MoS2_2 (23.1 N/m, 0.19),[55] respectively. For uniaxial strains, σi\sigma^{i} is 19.20 N/m and 22.25 N/m for the xx- and yy-directions, corresponding to εc\varepsilon^{c} of 0.24 and 0.20, respectively. The critical strain, varying between 0.20 and 0.24 (or 20% − 24%), highlights the suitability of MoTe2/PtS2\mathrm{MoTe_2/PtS_2} for use in flexible TE devices. In the next section, we will focus on investigating the effect of the biaxial strain on the TE properties. In the experiment, biaxial strain can be achieved using various techniques, such as external pressure or atomic force microscopy tip. [56]

Strain effect on electron and phonon properties

In Figure 5(a) and (Figure 5b), we plot the energy band structures and eDOS of MoTe2/PtS2\mathrm{MoTe_2/PtS_2} under several values of biaxial strain ε\varepsilon, respectively. The calculated results show that the CBM at the K1K_1 point shifts upward, while the conduction band at the M1M_1 point shifts downward, as shown in Figure 5(a). In contrast, the VBM at the K point moves downward, whereas the valence band at the Γ\Gamma point shifts upward, potentially enhancing band convergence. For nn-type MoTe2/PtS2\mathrm{MoTe_2/PtS_2}, band convergence is achieved at ε=0.02\varepsilon= 0.02 with the different energy between valley bands ΔE≈0\Delta E \approx0 eV, while for p-type MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2}, it occurs at ε=0.03\varepsilon= 0.03. This strain-induced band convergence can significantly improve the TE performance of MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2}.

Figure 5. (a) Energy dispersion, (b) electronic density of states (eDOS), (c) phonon dispersion, and (d) phonon density of states (phDOS) of the 2D vdW heterobilayer MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} under the several values of biaxial strain ε\varepsilon.

In Figure 5(c) and (Figure 5d), we plot the phonon dispersion and phonon density of states (phDOS) of MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} under several values of ε\varepsilon, respectively. We find that there are no negative phonon frequencies, indicating that MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} is dynamically stable under biaxial strain. ε\varepsilon in the range of 0.00–0.03 almost does not change the acoustic phonon branches but leads to a slight reduction in the frequencies of the optical phonon branches. The optical phonon modes shift to lower frequencies, leading to a reduced phonon gap between the optical and acoustic modes. The frequencies of the LO1 and LO2 branches under strain can be found in Table S2 (Supporting Information) of the Supporting Information for reference. This suggests that the κph\kappa_{\mathrm{ph}} of MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} may not be significantly affected within this strain range. However, the biaxial strain can optimize band convergence, which could enhance the Seebeck coefficient and thereby improve the PF, as shown in § 4.5.

Strain effect on thermoelectric power factor

In Figure 6(a), we show SS as a function of chemical potential μ\mu for both p-type and n-type MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} at T=300T = 300 K under the biaxial strain ε\varepsilon. We find that SS increases with increasing strain in both p-type and n-type materials. It is noted that a high SS is often associated with a large density-of-states effective mass md∗m_d^*, which is defined as md∗=Nv2/3m∗m_d^* = N_v^{2/3}m^*, [13, 57] where NvN_v represents the number of degenerate band valleys. When the energy bands converge, NvN_v increases, leading to a larger md∗m_d^* and, consequently, to an enhanced SS. In the present study, band convergence is achieved for both the n-type and p-type by applying biaxial strain, as shown in Figure 5(a). Without strain (ε=0.00\varepsilon= 0.00), the peak value of SS for MoTe2_2/PtS2_2 can be more than 1500 μ\muV/K, which is higher than that of 2D vdW heterobilayer P/GeC (1210 μ\muV/K), [58] heterobilayer GeS/SiSe (1166 μ\muV/K) [59] and heterobilayer Sb/As (550 μ\muV/K).[60] Additionally, we also calculated SS of MoTe2_2/PtS2_2 for several temperatures (see in Figure S7(a) in Supporting Information). In Figure 7(b) and (Figure 7c), we show the electrical conductivity σ\sigma and the thermal conductivities by electron κel\kappa_{\mathrm{el}} as functions of μ\mu for p-type and n-type materials. We note that the σ\sigma and κel\kappa_{\mathrm{el}} values are scaled by h/d0h/d_0, where h=30h = 30 Å and d0=13.452d_0 = 13.452 Å represent the unit cell thickness and the effective material thickness, respectively.

Figure 6. (a) Seebeck coefficient SS, (b) electrical conductivity σ\sigma, (c) electronic thermal conductivity κel\kappa_{\mathrm{el}}, and (d) power factor PF are plotted as a function of the chemical potential μ\mu at several values of biaxial strain ε\varepsilon for the p-type and n-type MoTe2_2/PtS2_2 at room temperature T=300T = 300 K.

Figure 7. (a) Lattice thermal conductivity κph\kappa_{\mathrm{ph}} as a function of temperature under several values of biaxial strain ε\varepsilon, (b) phonon group velocity vgv_g, (c) phonon-phonon scattering rate, and (d) Grüneisen parameter at T=300T = 300 K of the 2D vdW heterobilayer MoTe2_2/PtS2_2.

It is noted that to calculate σ\sigma and κel\kappa_{\mathrm{el}}, the relaxation time is also calculated for each ε\varepsilon, as listed in Table S3 (Supporting Information).

In Figure 6(d), we show the PF for p-type and n-type MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} as a function of μ\mu at T=300T = 300 K under the biaxial strain ε\varepsilon. Our results reveal that the n-type material achieves a significantly higher maximum PF compared to its p-type counterpart. This higher PF in the n-type material can be attributed to larger eDOS at near CBM compared with VBM, as shown in Figure 5(b). At ε=0.00\varepsilon= 0.00, the optimum PF (PFopt_{\mathrm{opt}}) of the n-type and p-type materials are 92 μW/cmK2\mu\mathrm{W}/\mathrm{cmK}^{2} and 16 μW/cmK2\mu\mathrm{W}/\mathrm{cmK}^{2}, respectively. The PFopt_{\mathrm{opt}} of the n-type is higher than that of other materials, such as the 2D vdW heterobilayer Sb/As (40 μW/cmK2\mu\mathrm{W}/\mathrm{cmK}^{2}) [60] and CoSb3_{3} (40 μW/cmK2\mu\mathrm{W}/\mathrm{cmK}^{2}).[61] The maximum of PFopt_{\mathrm{opt}} for the n-type is found at ε=0.02\varepsilon= 0.02 (or 2%) because of the band convergence. The PFopt_{\mathrm{opt}} for the n-type with strain (170 μW/cmK2\mu\mathrm{W}/\mathrm{cmK}^{2} at ε=0.02\varepsilon= 0.02) is enhanced by nearly 84.78% of that without strain (92 μW/cmK2\mu\mathrm{W}/\mathrm{cmK}^{2} at ε=0.00\varepsilon= 0.00). For p-type, at ε=0.00\varepsilon= 0.00, the PFopt_{\mathrm{opt}} exhibits two peaks at optimized chemical potential μopt=−0.44\mu_{\mathrm{opt}} = -0.44 and −0.83-0.83 eV, in which the peak at μopt=−0.83\mu_{\mathrm{opt}} = -0.83 eV originates from the contribution of the Rashba SOC at the Γ\Gamma point, as shown in Figure 5(a). Under biaxial strain, these two peaks degenerate into one peak at μopt=−0.53\mu_{\mathrm{opt}} = -0.53 at ε=0.03\varepsilon= 0.03 due to the band convergence of the p-type case. In addition, SS, σ\sigma, κel\kappa_{\mathrm{el}}, and PF at different temperatures T=500T = 500, 700, and 900 K under biaxial strain are also calculated and shown in Figures S9, S10, and S11 in Supporting Information, respectively.

Strain effect on lattice thermal conductivity

In Figure 7(a), we show the lattice thermal conductivity κph\kappa_{\mathrm{ph}} of MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} as a function of temperature under several biaxial strains. We note that κph\kappa_{\mathrm{ph}} is scaled by a factor of h/d0h/d_{0}. We find that κph\kappa_{\mathrm{ph}} exhibits isotropic behavior and almost does not change with increasing strain from ε=0.00\varepsilon= 0.00 to ε=0.03\varepsilon= 0.03. On the other hand, κph\kappa_{\mathrm{ph}} decreases rapidly in the temperature range from 100 to 500 K. At temperatures above 500 K, the decreasing rate of κph\kappa_{\mathrm{ph}} slows down and tends to converge as the temperature increases. This phenomenon mainly originates from the intrinsic enhancement of phonon-phonon scattering because of the Umklapp process and κph∝1/T\kappa_{\mathrm{ph}} \propto1/T.[58, 62] At T=300T = 300 K, the calculated values of κph\kappa_{\mathrm{ph}} is 0.6 and 0.56 Wm−1^{-1}K−1^{-1} at ε=0.00\varepsilon= 0.00 and 0.03, respectively. These values are lower than those of the well-known TE materials, such as Bi2_2Te3_3 and Mg3_3Bi2_2 (κph∼1−2\kappa_{\mathrm{ph}} \sim1 - 2 Wm−1^{-1}K−1^{-1}).[63, 64] Thus, MoTe2_2/PtS2_2 with extremely low κph\kappa_{\mathrm{ph}} can play a crucial role in achieving high ZTZT value.

The origin low κph\kappa_{\mathrm{ph}} of MoTe2_2/PtS2_2 can be attributed to the avoided crossing points between the acoustic phonon and optical phonon, which occur below 40 cm−1^{-1}, as shown in Figure 3. Furthermore, the Bader charge-based ionic charge states of MoTe2_2/PtS2_2 are Mo0.559+^{0.559+}, Te10.234−_1^{0.234-}, Te20.289−_2^{0.289-}, Pt0.458+^{0.458+}, S10.235−_1^{0.235-}, and S20.259−_2^{0.259-}, indicating that Mo-Te1_1, Mo-Te2_2, Pt-S1_1, and Pt-S2_2 form metavalent bonds. The presence of metavalent bonding leads to strong anharmonicity and a short phonon relaxation time, as observed in the Janus γ\gamma-Ge2_2SSe[45] and

Figure of merit as a function of chemical potential and temperatureVector (PDF)

caption: (a) Figure of merit ZTZT is plotted as a function of μ\mu at several values of biaxial strain ε\varepsilon for p-type and n-type MoTe2_2/PtS2_2 at room temperature T=300T = 300 K. (b) The maximum value of ZTZT as a function of temperature for p-type and n-type MoTe2_2/PtS2_2 at several ε\varepsilon values.

B2_2P6_6 monolayers. As shown in Figure 7(c), MoTe2_2/PtS2_2 shows short phonon relaxation time of 0.01−1.00.01 - 1.0 ps−1^{-1}, indicating strong phonon scattering, consequently, a low κph\kappa_{\mathrm{ph}}.

Another factor that contributes to reducing κph\kappa_{\mathrm{ph}} is the phonon group velocity. As shown in Figure 7(b), the calculated group velocity of the ZA and TA modes is about 1.9−4.61.9 - 4.6 km/s. The acoustic phonon branches, which exhibit higher group velocities compared to the optical branches, mainly contribute to κph\kappa_{\mathrm{ph}}. To more understand the low lattice thermal conductivity, we calculate the Grüneisen parameter ∣γ∣\lvert\gamma\rvert to measure the strength of anharmonicity of MoTe2_2/PtS2_2. The calculated results show that the highest ∣γ∣\lvert\gamma\rvert value of about 80 appears in the ZA branch, as shown in Figure 7(d), which would greatly suppress the phonon transport in the high-temperature region.

Strain effect on thermoelectric figure of merit

In Figure 8(a), we show ZTZT as a function of μ\mu at T=300T = 300 for several values of ε\varepsilon. The maximum values of ZTZT are about 0.40 and 0.74 for p-type and n-type, respectively. These ZTZT values are comparable with that of the Janus Rashba monolayer Si2_2SbBi (0.31 at 500 K), Si2_2AsSb (0.38 at 500 K), [15] Rashba monolayer of WSTe (0.55 at 500 K), [65] and 2D vdW heterobilayer MoSe2_2/BAs (0.58 at 1200 K), [66], and well-known TE materials (ZTZT value typically ranges from 0.8 to 1.0 at 300 K). The ZTZT is not significantly affected by the strain, although the PF value of n-type is significantly increased by band convergence. This is because at the optimum μ\mu value of ZTZT for n-type (μoptZT∼0.45\mu_{\mathrm{opt}}^{ZT} \sim0.45 eV), which is smaller than that of the PF for n-type (μoptPF∼0.55\mu_{\mathrm{opt}}^{\mathrm{PF}} \sim0.55 eV), the PF is not significantly changed by the band convergence, as shown in Figure 6(d).

In Figure 8(b), we show the maximum ZTZT (ZTmax⁡ZT_{\max}) as a function of temperature ranging from 300 to 900 K for ε\varepsilon ranging from 0.00 to 0.03. ZTmax⁡ZT_{\max} are 0.88 and 0.71 for the n-type and p-type, respectively, at T=900T = 900 K and ε=0.02\varepsilon= 0.02. Since ZTmax⁡ZT_{\max} of the n-type changes about 19–37% for the temperature ranging from 300 to 900 K, it suggests that 2D vdW heterobilayer MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} could be a good candidate material for the TE application in the mid-range temperature.

Conclusions

In summary, we have investigated the effect of strain on the mechanical, electronic, phonon, and thermoelectric properties of the 2D vdW heterobilayer MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2}. A strong Rashba splitting is observed in MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2}, and the critical strain of about 20–24% suggests that MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} can be utilized in flexible TE devices. The Fröhlich interaction model is employed to evaluate carrier mobility, which indicates the significant contribution of longitudinal-optical-phonon scattering to the TE properties of MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2}. We find that at a strain of ε=0.02\varepsilon= 0.02, the PF of the n-type material is significantly enhanced, reaching a high value of 170 μW/cmK2\mu\mathrm{W}/\mathrm{cmK}^{2} W/mK2\mathrm{W}/\mathrm{mK}^{2} at 300 K, due to band convergence. The optimum ZTZT values for n-type and p-type materials reach 0.88 and 0.71 at 900 K, respectively. Our calculated results demonstrate that the 2D vdW heterobilayer MoTe2/PtS2\mathrm{MoTe}_{2}/\mathrm{PtS}_{2} holds potential as a flexible TE material in the mid-range temperature.

Supporting Information

The Supporting Information is available free of charge at https://pubs.acs.org/doi/xxx.

Table of Born effective charges, frequencies of the LO1 and LO2 phonon branches. Figure of the total energy and temperature as a function of time at T=900T = 900 K, figure of the band structure of MoTe2/PtS2\mathrm{MoTe}_2/\mathrm{PtS}_2 heterobilayer (3×1\sqrt{3} \times1 supercell), figure of the total energy-strain relationship, figure of the calculated band energies, figure of the temperature-dependent relaxation time at several strain values, figure of the Seebeck coefficient SS, electrical conductivity σ\sigma, electronic thermal conductivity κel\kappa_{\mathrm{el}}, and power factor PF are plotted as function of the chemical potential μ\mu at T=500T = 500 K, 700 K and 900 K.

Acknowledgements

N.T.H. acknowledges the financial support from Frontier Research Institute for Interdisciplinary Sciences, Tohoku University.

References

  1. [1]Biswas, K.; Ren, Z.; Grin, Y.; Lee, K. H.; Mori, T.; Chen, L. Thermoelectric Materials Science and Technology Toward Applications. Appl. Phys. Lett. 2022, 121.DOI
  2. [2]Heremans, J. P.; Dresselhaus, M. S.; Bell, L. E.; Morelli, D. T. When Thermoelectrics Reached the Nanoscale. Nat. Nanotechnol 2013, 8, 471–473.DOI
  3. [3]Vining, C. B. An Inconvenient Truth about Thermoelectrics. Nat. Mater. 2009, 8, 83–85.DOI
  4. [4]Goldsmid, H. J.; others Introduction to Thermoelectricity; Springer, 2010; Vol. 121.
  5. [5]Van Thanh, V.; Hung, N. T.; others Janus 2D B₂P₆: A promising anisotropic thermoelectric material with high power factor. Surf. Interfaces 2024, 44, 103829.DOI
  6. [6]Kaidanov, V.; Nemov, S.; Ravich, Y. I. Resonant scattering of carriers in IV-VI semiconductors. Soviet physics. Semiconductors 1992, 26, 113–125.
  7. [7]Zhao, W.; Ding, J.; Zou, Y.; Di, C.-a.; Zhu, D. Chemical doping of organic semiconductors for thermoelectric applications. Chem. Soc. Rev. 2020, 49, 7210–7228.DOI
  8. [8]Hicks, L.; Dresselhaus, M. Use of Quantum-Well Superlattices to Obtain a High Figure of Merit from Nonconventional Thermoelectric Materials. MRS Online Proceedings Library (OPL) 1993, 326.
  9. [9]Dresselhaus, M. S.; Chen, G.; Tang, M. Y.; Yang, R.; Lee, H.; Wang, D.; Ren, Z.; Fleurial, J.-P.; Gogna, P. New Directions for Low-Dimensional Thermoelectric Materials. Adv. Mater. 2007, 19, 1043–1053.
  10. [10]Hung, N. T.; Hasdeo, E. H.; Nugraha, A. R.; Dresselhaus, M. S.; Saito, R. Quantum Effects in the Thermoelectric Power Factor of Low-Dimensional Semiconductors. Phys. Rev. Lett. 2016, 117, 036602.DOI
  11. [11]Hung, N. T.; Saito, R. The Origin of Quantum Effects in Low-Dimensional Thermoelectric Materials. Adv. Quantum Technol. 2021, 4, 2000115.
  12. [12]Tang, Y.; Gibbs, Z. M.; Agapito, L. A.; Li, G.; Kim, H.-S.; Nardelli, M. B.; Curtarolo, S.; Snyder, G. J. Convergence of multi-valley bands as the electronic origin of high thermoelectric performance in CoSb₃ skutterudites. Nat. Mater. 2015, 14, 1223–1228.DOI
  13. [13]T. Hung, N.; Nugraha, A. R.; Yang, T.; Zhang, Z.; Saito, R. Thermoelectric Performance of Monolayer InSe Improved by Convergence of Multivalley Bands. J. Appl. Phys. 2019, 125, 082502.DOI
  14. [14]Yuan, J.; Cai, Y.; Shen, L.; Xiao, Y.; Ren, J.-C.; Wang, A.; Feng, Y. P.; Yan, X. One- dimensional thermoelectrics induced by Rashba spin-orbit coupling in two-dimensional BiSb monolayer. Nano Energy 2018, 52, 163–170.DOI
  15. [15]Xia, Q.; Xu, Z.; Zhang, L.; Gao, G. Thermoelectric transport properties in Janus Rashba semiconductors of monolayer Si₂AsSb and Si₂SbBi. J. Appl. Phys. 2024, 136.
  16. [16]Bera, J.; Betal, A.; Sahu, S. Spin orbit coupling induced enhancement of thermoelectric performance of HfX₂ (X = S, Se) and its Janus monolayer. J. Alloys Compd. 2021, 872, 159704.DOI
  17. [17]Wang, H.-X.; Mao, L.-S.; Tan, X.; Liu, G.-Q.; Xu, J.; Shao, H.; Hu, H.; Jiang, J. Nontrivial thermoelectric behavior in cubic SnSe driven by spin-orbit coupling. Nano Energy 2018, 51, 649–655.DOI
  18. [18]Duan, S.; Wang, H.; Liu, G.-Q.; Wu, Q.; Man, N.; Zhang, Q.; Tan, X.; Yin, Y.; Xiao, Y.; Hu, H.; others Improved thermoelectric performance in PbSe–AgSbSe₂ by manipulating the spin-orbit coupling effects. Nano Energy 2020, 78, 105232.DOI
  19. [19]Qiu, B.; Ruan, X. Molecular dynamics simulations of lattice thermal conductivity of bismuth telluride using two-body interatomic potentials. Phys. Rev. B Condens. Matter 2009, 80, 165203.DOI
  20. [20]Pei, Y.; LaLonde, A.; Iwanaga, S.; Snyder, G. J. High thermoelectric figure of merit in heavy hole dominated PbTe. Energy Environ. Sci. 2011, 4, 2085–2089.DOI
  21. [21]Gupta, S.; Yakobson, B. I. What dictates Rashba splitting in 2D van der Waals heterobilayers. J. Am. Chem. Soc. 2021, 143, 3503–3508.DOI
  22. [22]Yao, Q.-F.; Cai, J.; Tong, W.-Y.; Gong, S.-J.; Wang, J.-Q.; Wan, X.; Duan, C.-G.; Chu, J. Manipulation of the large Rashba spin splitting in polar two-dimensional transition-metal dichalcogenides. Phys. Rev. B. 2017, 95, 165401.DOI
  23. [23]Ma, Y.; Dai, Y.; Wei, W.; Li, X.; Huang, B. Emergence of electric polarity in BiTeX (X= Br and I) monolayers and the giant Rashba spin splitting. Phys. Chem. Chem. Phys. 2014, 16, 17603–17609.DOI
  24. [24]Noshin, M.; Khan, A. I.; Subrina, S. Thermal transport characterization of Stanene/Silicene heterobilayer and stanene bilayer nanostructures. Nanotechnol. 2018, 29, 185706.DOI
  25. [25]Jia, P.-Z.; Zeng, Y.-J.; Wu, D.; Pan, H.; Cao, X.-H.; Zhou, W.-X.; Xie, Z.-X.; Zhang, J.-X.; Chen, K.-Q. Excellent thermoelectric performance induced by interface effect in MoS₂/MoSe₂ van der Waals heterostructure. J. Condens. Matter Phys. 2019, 32, 055302.
  26. [26]Mohanta, M. K.; Rawat, A.; Jena, N.; Ahammed, R.; De Sarkar, A.; others Superhigh out-of-plane piezoelectricity, low thermal conductivity and photocatalytic abilities in ultrathin 2D van der Waals heterostructures of boron monophosphide and gallium nitride. Nanoscale 2019, 11, 21880–21890.DOI
  27. [27]Hu, R.; Zhou, Z.; Sheng, C.; Wang, L.; Liu, J.; Han, S.; Liu, H. Surprisingly good thermoelectric performance of a black phosphorus/blue phosphorus van der Waals heterostructure. Phys. Chem. Chem. Phys. 2020, 22, 22390–22398.DOI
  28. [28]Yin, S.; Luo, Q.; Wei, D.; Guo, G.; Sun, X.; Tang, Y.; Dai, X. A type-II PtS₂/MoTe₂ van der Waals heterostructure with adjustable electronic and optical properties. Results Phys. 2022, 33, 105172.DOI
  29. [29]Wang, J.; He, D.; Bai, Z.; Li, G.; Bai, J.; Liu, K.; Ren, F.; Liu, X.; He, J.; Zhou, W.; others Enhanced exciton diffusion from interlayer charge-transfer transitions in PtSe₂/MoSe₂ van der Waals heterojunction. Nano Res. 2023, 16, 12809–12816.DOI
  30. [30]Giannozzi, P.; Baroni, S.; Bonini, N.; Calandra, M.; Car, R.; Cavazzoni, C.; Ceresoli, D.; Chiarotti, G. L.; Cococcioni, M.; Dabo, I.; others QUANTUM EXPRESSO: A Modular and Open-Source Software Project for Quantum Simulations of Materials. J. Phys. Condens. Matter. 2009, 21, 395502.DOI
  31. [31]Hung, N. T.; Nugraha, A. R.; Saito, R. Quantum ESPRESSO Course for Solid-State Physics; Jenny Stanford Publishing, New York, 2022.DOI
  32. [32]Hamann, D. Optimized norm-conserving Vanderbilt pseudopotentials. Phys. Rev. B - Condens. Matter Mater. Phys. 2013, 88, 085117.DOI
  33. [33]Perdew, J. P.; Burke, K.; Ernzerhof, M. Generalized Gradient Approximation Made Simple. Phys. Rev. Lett. 1996, 77, 3865.pubmed.ncbi.nlm.nih.gov/10062328
  34. [34]Heyd, J.; Scuseria, G. E.; Ernzerhof, M. Hybrid Functionals Based on a Screened Coulomb Potential. Chem. Phys. 2003, 118, 8207–8215.DOI
  35. [35]Mostofi, A. A.; Yates, J. R.; Pizzi, G.; Lee, Y.-S.; Souza, I.; Vanderbilt, D.; Marzari, N. An Updated Version of Wannier90: A Tool for Obtaining Maximally-Localised Wannier Functions. Comput. Phys. Commun. 2014, 185, 2309–2310.
  36. [36]Baroni, S.; De Gironcoli, S.; Dal Corso, A.; Giannozzi, P. Phonons and Related Crystal Properties from Density-Functional Perturbation Theory. Rev. Mod. Phys. 2001, 73, 515.DOI
  37. [37]Grimme, S.; Hansen, A.; Brandenburg, J. G.; Bannwarth, C. Dispersion-corrected mean-field electronic structure methods. Chem. Rev. 2016, 116, 5105–5154.DOI
  38. [38]Martyna, G. J.; Klein, M. L.; Tuckerman, M. Nosé–Hoover Chains: The Canonical Ensemble via Continuous Dynamics. J. Chem. Phys. 1992, 97, 2635–2643.DOI
  39. [39]Pizzi, G.; Volja, D.; Kozinsky, B.; Fornari, M.; Marzari, N. BoltzWann: A Code for the Evaluation of Thermoelectric and Electronic Transport Properties with a Maximally-Localized Wannier Functions Basis. Comp. Phys. Commun. 2014, 185, 422–429.DOI
  40. [40]Li, W.; Carrete, J.; Katcho, N. A.; Mingo, N. ShengBTE: A Solver of the Boltzmann Transport Equation for Phonons. Comput. Phys. Commun. 2014, 185, 1747–1758.
  41. [41]Tang, W.; Sanville, E.; Henkelman, G. A grid-based Bader analysis algorithm without lattice bias. J. Phys.: Condens. Matter 2009, 21, 084204.DOI
  42. [42]Almayyali, A. O. M.; Kadhim, B. B.; Jappor, H. R. Stacking impact on the optical and electronic properties of two-dimensional MoSe₂/PtS₂ heterostructures formed by PtS₂ and MoSe₂ monolayers. Chem. Phys. 2020, 532, 110679.DOI
  43. [43]Mouhat, F.; Coudert, F. Necessary and Sufficient Elastic Stability Conditions in Various Crystal Systems. Phys. Rev. B 2014, 90, 224104.DOI
  44. [44]Hung, N. T.; Nugraha, A. R.; Saito, R. Two-Dimensional InSe as a Potential Thermoelectric Material. Appl. Phys. Lett. 2017, 111, 092107.DOI
  45. [45]Thanh, V. V.; Truong, D. V.; Tuan Hung, N. Janus γ-Ge₂SSe Monolayer as a High-Performance Material for Photocatalysis and Thermoelectricity. ACS Appl. Energy Mater. 2023, 6, 910–919.
  46. [46]Yuan, G.; Ma, X.; Liao, J.; Xie, T.; Xie, Q.; Yuan, Z. First-principles calculations of 2D Janus WSSiN₂ monolayer for photocatalytic water splitting. ACS Appl. Nano Mater. 2023, 6, 1956–1964.DOI
  47. [47]Luo, Y.; Sun, M.; Yu, J.; Schwingenschlogl, U. Pd₄S₃Se₃, Pd₄S₃Te₃, and Pd₄Se₃Te₃: Candidate two-dimensional Janus materials for photocatalytic water splitting. Chem. Mater. 2021, 33, 4128–4134.DOI
  48. [48]Cheng, L.; Liu, Y. What limits the intrinsic mobility of electrons and holes in two dimensional metal dichalcogenides? J. Am. Chem. Soc. 2018, 140, 17895–17900.DOI
  49. [49]Bao, N. T. G.; Trang, T. N. Q.; Thoai, N.; Phan, T. B.; Thu, V. T. H.; Tuan Hung, N. Rational design 2D heterobilayers transition-metal dichalcogenide and their Janus for efficient water splitting. ACS Applied Energy Materials 2025,DOI
  50. [50]Hung, N. T.; Nugraha, A. R.; Saito, R. Two-Dimensional MoS₂ Electromechanical Actuators. J. Phys. D: Appl. Phys. 2018, 51, 075306.
  51. [51]Alvarez, S. A cartography of the van der Waals territories. Dalton Trans. 2013, 42, 8617–8636.DOI
  52. [52]Du, J.; Song, P.; Fang, L.; Wang, T.; Wei, Z.; Li, J.; Xia, C. Elastic, electronic and optical properties of the two-dimensional PtX₂ (X = S, Se, and Te) monolayer. Appl. Surf. Sci. 2018, 435, 476–482.DOI
  53. [53]Van Thanh, V.; Hung, N. T.; others Charge-induced electromechanical actuation of Mo-and W-dichalcogenide monolayers. RSC Adv. 2018, 8, 38667–38672.DOI
  54. [54]Li, T. Ideal strength and phonon instability in single-layer MoS₂.DOI
  55. [55]Hung, N. T.; Zhang, K.; Van Thanh, V.; Guo, Y.; Puretzky, A. A.; Geoghegan, D. B.; Kong, J.; Huang, S.; Saito, R. Nonlinear optical responses of Janus MoSSe/MoS₂ heterobilayers optimized by stacking order and strain. ACS Nano 2023, 17, 19877–19886.DOI
  56. [56]Dai, Z.; Liu, L.; Zhang, Z. Strain engineering of 2D materials: issues and opportunities at the interface. Adv. Mater. 2019, 31, 1805417.DOI
  57. [57]Lv, H.; Lu, W.; Shao, D.; Sun, Y. Enhanced thermoelectric performance of phosphorene by strain-induced band convergence. Phys. Rev. B. 2014, 90, 085433.DOI
  58. [58]Ahmad, I.; Wang, X.-P.; Shahid, I.; Ali, A.; Shah, S. H.; Li, E.; Lyu, T.; Ding, K.; Chen, X.; Rao, F. The van der Waals heterostructures of blue phosphorene with GaN/GeC for high-performance thermoelectric applications. APL Mater. 2025, 13.
  59. [59]Noshin, M.; Khan, A. I.; Chakraborty, R.; Subrina, S. Modeling and computation of thermal and optical properties in silicene supported honeycomb bilayer and heterobilayer nanostructures. Mater. Sci. Semicond. 2021, 129, 105776.DOI
  60. [60]Tang, Q.; Li, X.; Hu, R.; Han, S.; Yuan, H.; Singh, D. J.; Liu, H.; Yang, J. Designing Rashba systems for high thermoelectric performance based on the van der Waals heterostructure. Mater. Today Phys. 2022, 27, 100788.DOI
  61. [61]Shi, X.; Yang, J.; Salvador, J. R.; Chi, M.; Cho, J. Y.; Wang, H.; Bai, S.; Yang, J.; Zhang, W.; Chen, L. Multiple-filled skutterudites: high thermoelectric figure of merit through separately optimizing electrical and thermal transports. J. Am. Chem. Soc. 2011, 133, 7837–7846.DOI
  62. [62]Zhu, X.-L.; Hou, C.-H.; Zhang, P.; Liu, P.-F.; Xie, G.; Wang, B.-T. High thermoelectric performance of new two-dimensional IV–VI compounds: A first-principles study. J. Phys. Chem. C 2019, 124, 1812–1819.DOI
  63. [63]Hung, N. T.; Nugraha, A. R.; Saito, R. Designing High-Performance Thermoelectrics in Two-Dimensional Tetradymites. Nano Energy 2019, 58, 743–749.DOI
  64. [64]Hung, N. T. The role of spin-orbit interaction in low thermal conductivity of Mg₃Bi₂. Appl. Phys. Lett. 2023, 123.arxiv.org/abs/2310.14639
  65. [65]Duan, X.; Ren, J.-C.; Zhang, X.; Li, S.; Liu, W. Room-Temperature Thermoelectric Conversion by Dipole-Enhanced Rashba Spin-Orbit Coupling. Cell Rep. Phys. Sci. 2021, 2.DOI
  66. [66]Li, Y.; Feng, Z.; Sun, Q.; Ma, Y.; Tang, Y.; Dai, X. Electronic, thermoelectric, transport and optical properties of MoSe₂/BAs van der Waals heterostructures. Results Phys. 2021, 23, 104010.DOI

Paper details

vlnc:W_p7dy9k3d
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 5

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents