Abstract

Two-dimensional (2D) heterocrystals comprising molecules and semiconductors can serve as an ideal platform for studying interfacial excitons and for future optoelectronic applications, yet the energy and charge flow across these atomically sharp interfaces remain unclear. In this work, we investigated PTCDA-MoS2 as a prototypical 2D organic-inorganic heterostructure and revealed dual-mode exciton coupling between the constituent crystals. Monolayer-resolved PTCDA molecular crystals were grown on monolayer MoS2 via physical vapor assembly, and their crystallographic details, including the stacking angle, were determined by electron diffraction. Upon the formation of the heterostructures, PTCDA's photoluminescence was completely quenched because of organic-to-inorganic hole transfer, whereas that of MoS2 increased markedly with PTCDA thickness. Using differential reflectance and photoluminescence excitation spectroscopy, we found that the enhancement arises from two distinct mechanisms. Ground-state charge transfer injects holes into MoS2, which suppresses negative trion formation and enhances the radiative recombination of neutral excitons. In addition, resonant energy transfer, enabled by spectral overlap between PTCDA and MoS2, diverts excitation energy from PTCDA to MoS2. Our findings reconcile previously proposed mechanisms and establish a unified framework in which charge and energy transfer cooperate to govern exciton coupling at organic-inorganic interfaces.

Introduction

Two-dimensional molecular crystals (2DMCs) provide an ideal platform for investigating excitonic phenomena governed by intermolecular interactions[1] under reduced dimensionality. Their atomically thin geometry enables control over thickness[2, 3, 4], dielectric screening[5], and epitaxial registry[6, 7], allowing systematic tuning of electronic structure and excitonic coupling. Previous studies have shown that high-quality 2DMCs exhibit long-range order[2, 7], optical anisotropy[4], and Davydov splitting[4, 8], establishing polarization-resolved spectroscopy as a direct probe of molecular packing and transition dipoles[4, 8, 9]. Notably, molecular excitons in monolayer (1L) 2DMCs are highly delocalized, showing room-temperature superradiance[10, 11] and supertransport[3] behavior. The excitonic structure also evolves with thickness: excitations in perylene systems, for example, are predominantly Frenkel-like in the monolayer limit, whereas increasing thickness introduces charge-transfer (CT) character through intermolecular π\pi-stacking, leading to Frenkel-CT mixing[8, 10] and reconfiguration of transition dipoles[8].

While these studies establish the intrinsic excitonic properties of 2DMCs, parallel efforts have extended their functionality by interfacing them with photoactive 2D semiconductors. Hybrid organic–inorganic heterostructures[7, 9, 12] combine strong molecular absorption with efficient excitonic emission in transition metal dichalcogenides (TMDs), providing a platform for engineering interfacial exciton dynamics[13, 14, 15, 16, 17, 18, 19]. Molecular orientation and packing depend sensitively on substrate interactions, leading to face-on or edge-on configurations and varying degrees of crystallinity[20]. Mechanistic studies have demonstrated charge transfer[16], energy transfer[14, 17], and band alignment effects[17] in organic/TMD heterostructures, enabling functionalities such as vertical transport[21], hybrid pn junctions[22], and phototransistors[23]. Despite these advances, existing studies have largely focused on polycrystalline molecular films deposited on inorganic 2D semiconductors[16, 17, 21, 22], thus lacking thickness control. Whereas recent work has demonstrated control of optical anisotropy and charge localization in monolayer molecular crystals on TMDs[9, 12], the evolution of intermolecular coupling along the out-of-plane direction and its interplay with interfacial processes remain unclear.

In this work, we grow thickness-controlled 2D PTCDA crystals on 1L MoS2_2 with epitaxial registry and reveal dual-mode excitonic coupling in the prototypical 2D organic-inorganic heterostructure. Electron diffraction confirms orientational registry and long-range order at the molecule-TMD interface. Davydov-split molecular excitons identified by polarization-resolved absorption spectroscopy are strongly coupled to MoS2\mathrm{MoS}_2 via hole transfer, resulting in near-complete quenching of photoluminescence (PL). In contrast, excitonic emission from MoS2\mathrm{MoS}_2 is doubly enhanced by both ground-state charge-transfer doping and resonant energy transfer. We also reveal that strong out-of-plane π\pi–π\pi interactions reinforce charge doping and maintain highly efficient hole transfer as thickness increases. This work identifies key factors governing excitonic coupling between organic and inorganic 2D crystals.

Results and Discussion

Formation and excitonic basis of PTCDA/MoS2_2 heterocrystals

The transient flow of photoexcitation across atomically sharp interfaces may proceed through resonance energy transfer (RET) or charge transfer (CT), as illustrated in Fig. 1a. To establish a well-defined platform for interfacial exciton coupling, we first characterize the structural and excitonic properties of thickness-controlled PTCDA/MoS2\mathrm{MoS}_2 heterocrystals. Using physical vapor assembly, uniform single- and few-layer PTCDA crystals (denoted as nLPn\mathrm{L}_{\mathrm{P}}; n=1n = 1–55) were grown on monolayer MoS2\mathrm{MoS}_2 (1LM1\mathrm{L}_{\mathrm{M}}). Based on the systematic characterization that follows, we found that nLPn\mathrm{L}_{\mathrm{P}} is essentially a herringbone-patterned array of 1D π\pi-stacked PTCDA columns, as depicted in Fig. 1a. Figure 1b (middle) shows an AFM image of an edge region of a partially grown 2LP2\mathrm{L}_{\mathrm{P}} sample, which was selected to show PTCDA-MoS2\mathrm{MoS}_2 steps. The majority of the grown samples were completely and uniformly covered with molecular layers. The step height of 0.62 ±\pm 0.12 nm (Fig. 1b, top) corresponds to two-layer thickness based on the interplanar spacing of the (102) plane in bulk PTCDA[24]. These results suggest layer-by-layer growth with crystallographic fidelity. The narrow height distribution (Fig. 1b, bottom) further indicates high surface quality.

Optical transitions in the organic-inorganic heterocrystal are fundamentally different in the two constituents. Whereas optical absorption in 1L MoS2\mathrm{MoS}_2 originates from direct interband transitions between delocalized Bloch states near the K valleys[25, 26], photoexcitation in PTCDA involves transitions between localized molecular orbitals accompanied by vibronic progressions (Fig. 1c). This fundamental contrast provides an ideal platform for exploring interfacial energy and charge flow between molecular excitons and delocalized band excitons. To characterize the electronic structure of the heterocrystals, we employed differential reflectance (DR) spectroscopy: the absorptance of a thin sample supported on a dielectric substrate is proportional to DR, defined as (Rsam−Rsub)/Rsub(R_{\mathrm{sam}} - R_{\mathrm{sub}})/R_{\mathrm{sub}}, where RsamR_{\mathrm{sam}} and RsubR_{\mathrm{sub}} are the reflectances of the sample and substrate areas, respectively[27]. As shown in Fig. 1d, the unpolarized DR spectrum of 3LP/1LM3\mathrm{L}_{\mathrm{P}}/1\mathrm{L}_{\mathrm{M}} exhibits both the A, B and C excitons of an isolated 1LM1\mathrm{L}_{\mathrm{M}} (denoted as XAX_{\mathrm{A}}, XBX_{\mathrm{B}} and XCX_{\mathrm{C}})[25, 26] and two vibronic peaks of an isolated 3LP3\mathrm{L}_{\mathrm{P}} grown on hexagonal BN (hBN)[8], assigned to the S1←S0\mathrm{S}_{1} \leftarrow\mathrm{S}_{0} transitions (denoted as 0-0 and 1-0)[28]. The characteristic excitonic resonances of both constituents remain clearly identifiable in the heterocrystals, indicating that their fundamental excitonic structures are largely retained upon heterocrystal formation. However, the MoS2_2 A exciton blueshifts whereas the molecular resonances redshift, indicating non-negligible interlayer coupling. The thickness dependence of the spectral changes is also different for the two constituents: with increasing thickness, XAX_{\mathrm{A}} and XBX_{\mathrm{B}} blueshift, whereas the molecular peaks remain largely constant (Fig. 1e). Note that the spectra in Fig. 1e are shown with baseline subtracted (see Fig. S1 for detailed analysis). The origin of these spectral changes will be discussed below using polarization-resolved measurements. Quantitative analysis in Fig. 1f shows that molecular absorption scales linearly with thickness, enabling optical determination of the number of layers. It should be noted that the optical contrast[8] obtained from optical micrographs misidentifies thickness due to annealing effects on MoS2_2’s optical response (Fig. S2).

Lattice structure and epitaxial registry of heterocrystals. The layer-by-layer growth suggests long-range order and epitaxial registry. Electron diffraction of 2LP/1LM2\mathrm{L}_{\mathrm{P}}/1\mathrm{L}_{\mathrm{M}} (Figure 2a) reveals well-defined rectangular molecular lattices, which were verified across multiple spots and samples (Table S1). As found for PTCDA grown on hBN and graphene[8], the molecular lattices correspond to the (102) plane of bulk alpha-type crystals[24]. However, quantitative analysis revealed that the 2D unit cell spanned by m\boldsymbol{m} and n\boldsymbol{n} unit vectors is significantly dependent on the assembly templates: Whereas m\boldsymbol{m} of 1LP1\mathrm{L}_{\mathrm{P}} is 4.2% lengthened on hBN[8], m\boldsymbol{m} (n\boldsymbol{n}) of 2LP2\mathrm{L}_{\mathrm{P}} is 6.7% (1.0%) lengthened (shortened) on MoS2_2. A clear epitaxial registry was also revealed in low-magnification diffraction patterns (data are not shown): the reciprocal primitive vectors (a∗\boldsymbol{a}^{*} and b∗\boldsymbol{b}^{*}) of the hexagonal lattice of 1LM1\mathrm{L}_{\mathrm{M}} are given with m∗\boldsymbol{m}^{*} and n∗\boldsymbol{n}^{*} of 2LP2\mathrm{L}_{\mathrm{P}} (Figure 2a). The stacking angle, defined by the angle between n∗\boldsymbol{n}^{*} and b∗b^{*}, was found to be constant (∼13∘\sim13^\circ) for multiple samples of 2LP2\mathrm{L}_{\mathrm{P}} and 4LP4\mathrm{L}_{\mathrm{P}} (Table S1), which indicates preferential orientation of the molecular lattice on MoS2\mathrm{MoS}_{2}. Noting that the hexagonal lattice of MoS2\mathrm{MoS}_{2} is 26% larger than that of hBN or graphene, these findings indicate that the molecule-template epitaxial registry is an important factor governing molecular packing structure. With increasing PTCDA thickness to 4L, mm decreased to within ∼2%\sim2\% of the bulk value, further suggesting 2D-to-3D convergence[8].

Image not extracted

Figure 2. Epitaxial registry and optical anisotropy of PTCDA/MoS2\mathrm{MoS}_2 heterocrystals. (a) SAED pattern of graphene-encapsulated 2LP/1LM2\mathrm{L}_{\mathrm{P}}/1\mathrm{L}_{\mathrm{M}}, showing the reciprocal primitive vectors of PTCDA (m∗\mathbf{m}^* and n∗\mathbf{n}^*) and MoS2\mathrm{MoS}_2 (a∗\mathbf{a}^* and b∗\mathbf{b}^*). The latter are reduced in size threefold. See Table S1 for quantitative analysis and statistics. (b) Exciton splitting in a coupled molecular dimer, illustrating the formation of the lower and upper Davydov states (LDS and UDS). ∣φj⟩\lvert\varphi_j\rangle and ∣φj∗⟩\lvert\varphi_j^*\rangle represent the ground and excited states of the jj-th molecule, respectively. (c) Polarization-resolved parallel-configuration differential reflectance (DR∥\mathrm{DR}^{\parallel}) spectra of 2LP/1LM2\mathrm{L}_{\mathrm{P}}/1\mathrm{L}_{\mathrm{M}} at representative polarization angles shown with baseline subtracted. The full-set spectra at all angles (Fig. S3a) were globally fitted using five Gaussian functions (colored shades) to represent the XA\mathrm{X}_{\mathrm{A}}, XB\mathrm{X}_{\mathrm{B}}, LDS, UDS and 1-0 transitions. (d) Polar graph of DR∥\mathrm{DR}^{\parallel} area for the LDS, UDS, XA\mathrm{X}_{\mathrm{A}} and XB\mathrm{X}_{\mathrm{B}} transitions, showing the orthogonality between the two Davydov states represented by the transition dipole moments (μLDS\mu_{\mathrm{LDS}} and μUDS\mu_{\mathrm{UDS}}).

Using polarization-resolved DR measurements, we confirm the presence of two basis molecules in the unit cell, which is consistent with the (102) plane of bulk crystals. Coulomb interaction between two transition dipoles localized at two basis molecules leads to two superposition states, lower (symmetric) and upper (antisymmetric) Davydov states (LDS and UDS), as depicted in Figure 2b. Unlike the unpolarized DR spectra in Fig. 1, the parallel-configuration spectra (DR∥ defined in Methods) of 2LP2\mathrm{L}_{\mathrm{P}} for selected orientation angles (Figure 2c) show that the 00-00 absorption consists of two subcomponents due to the Davydov splitting, a hallmark of multiple bases[29]. As shown in the full-set spectra (Fig. S3), their contributions vary systematically with sample orientation, arising because the two Davydov states are orthogonally polarized (Figure 2d). Their orthogonality, consistent with Kasha’s dimeric exciton model[4, 30], suggests little orbital hybridization between the two constituents. The dipolar character of the molecular transitions contrasts with the isotropic responses of MoS2\mathrm{MoS}_{2}, which originate from its threefold rotational symmetry (Figure 2d). We also note that the 11-00 absorption also reveals a slight but similar energy splitting (Fig. S2).

Static interlayer coupling: dielectric screening and charge-transfer doping. We next examine static interlayer coupling manifested in absorption spectra and exciton energies. The observed epitaxial registry suggests strong electronic coupling between the two crystals, which can be hinted from ∼100\sim100 meV stabilization and broadening of 00-00’s LDS of 1LP1\mathrm{L}_{\mathrm{P}}/1LM1\mathrm{L}_{\mathrm{M}} with respect to a reference, 1LP1\mathrm{L}_{\mathrm{P}}/hBN (Figure 3a). Assuming negligible electronic coupling of PTCDA with dielectric hBN[8, 31], the observed redshift and broadening on MoS2\mathrm{MoS}_{2} may result from dielectric screening[32] or wavefunction mixing[16]. First of all, the redshift of the 00-00 transition was observed for LDS and UDS of all thicknesses, as shown in Figure 3b. With decreasing thickness from 5LP5\mathrm{L}_{\mathrm{P}} to 2LP2\mathrm{L}_{\mathrm{P}}, both 00-00 transitions blueshift because of reduced polarization stabilization in thinner layers[33]. Then, a drastic redshift for 1LP1\mathrm{L}_{\mathrm{P}}, ∼30\sim30 meV (LDS) and 37 meV (UDS), indicates a significant interaction between MoS2_2 and the neighboring molecular layer. We attribute the coupling to interfacial dielectric screening by MoS2_2[32] relative to hBN, reflecting its larger dielectric response and electronic polarizability. Whereas electronic wavefunction mixing$[16] may further contribute to the observed spectral shifts, it is not significant enough to modify the orthogonality of LDS and UDS (Figure 2d). The linewidths of LDS and UDS of 1LP increased by ∼90%\sim90\% and ∼40%\sim40\%, respectively, compared to the reference (Figure 3c). Noting that PTCDA forms high-quality crystals on both MoS2_2 and hBN, as supported by our structural analyses, the increased linewidths cannot be solely attributed to inhomogeneous broadening but to lifetime broadening. As will be shown by the drastic quenching of molecular PL below, the organic-inorganic interlayer coupling mediates a highly efficient nonradiative decay channel$[15] via hole transfer. The DS energy noticeably reduced relative to that of the reference is also due to interlayer interactions (Figure 3d). Interestingly, the degree of the splitting is maintained for all thicknesses.

Image not extracted

Figure 3. Static interlayer coupling in PTCDA/MoS2_2 heterocrystals. (a) DR∥DR_{\parallel} spectra of 1LP_{\mathrm{P}}/1LM_{\mathrm{M}} and the reference 1LP_{\mathrm{P}}/hBN. (b) Thickness dependence of the LDS, UDS and XA_{\mathrm{A}} energies. (c) Thickness dependence of the spectral linewidth (FWHM) of the LDS, UDS and XA_{\mathrm{A}} resonances. (d) Davydov splitting energy (DSE) as a function of PTCDA thickness. The horizontal dashed lines in (b–d) indicate the corresponding reference energies.

A complementary insight into the organic-inorganic coupling is provided by the DR response of MoS2_2 excitons, which blueshift upon formation of heterocrystals. The gradual increase of ∼15\sim15 meV in XA_\mathrm{A} energy with increasing thickness (Figure 3b) is due to the interplay between neutral and charged A excitons. PTCDA molecules with a large electron affinity (∼4.12\sim4.12 eV) have a strong tendency to withdraw electrons from (or inject holes into) MoS2_2[16, 18], which has significant native negative charges[34]. As shown by the electrical gating experiments[34], hole doping diminishes the absorption of the predominant negatively charged trions and increases that of the neutral excitons. Because the two peaks are barely resolved due to their small energy difference, the change appears as an apparent upshift, which is in fact a population shift towards high-energy neutral excitons. The PTCDA-induced narrowing of XA_\mathrm{A} in Figure 3c is also consistent with this interpretation. In other words, the large linewidth of bare MoS2_2 is due to the contributions from neutral excitons and trions.

PL spectra of heterocrystals further reveal PTCDA-induced charge-transfer doping of MoS2_2. Compared with bare MoS2_2, the XA_\mathrm{A} of heterocrystals blueshifts and increases in intensity (Figure 4a). The increase in exciton energy (Figure 4b) and PL intensity (Figure 4c) was proportional to the thickness of PTCDA, which was consistently observed for 514 and 633 nm excitation (Figure 4b). In particular, the change in exciton energy was essentially equivalent for the two wavelengths. Noting that 633 nm does not reach the optical gap of PTCDA, thus sub-gap excitation, we conclude that the blueshift does not require molecular excitation but results from ground-state PTCDA via charge-transfer doping[18, 35]. To obtain an order-of-magnitude estimate of the electron density reduced by PTCDA, we compared the trion fraction in XA_{\mathrm{A}}’s PL intensity with the gate-dependent calibration reported by Mak et al. for monolayer MoS2_2[34]. As shown for 1L in Figure 4a, XA_{\mathrm{A}} of all thicknesses could be decomposed into negative trion (XA−_{\mathrm{A}}^-) and neutral exciton (XA0_{\mathrm{A}}^0) subcomponents (Figure 4d). With increasing thickness, the trion fraction decreased (Figure 4e): According to the calibration data in Fig. S4, our bare MoS2_2 (0LP_\mathrm{P}) corresponds to an electron density (nen_{\mathrm{e}}) of 8.2×10128.2 \times10^{12} cm−2^{-2}, whereas 1L PTCDA/MoS2_2 corresponds to ne=7.4×1012n_{\mathrm{e}} = 7.4 \times10^{12} cm−2^{-2}. Thus, deposition of a single PTCDA layer effectively removes 8×10128 \times10^{12} electrons/cm2^2. This corresponds to approximately 0.01 electrons per PTCDA molecule, given the molecular packing density of 1L PTCDA (8.7×10138.7 \times10^{13} molecules/cm2^2; see Table S1).

Image not extracted

Figure 4. Photoluminescence modulation and ground-state charge-transfer doping. (a) Steady-state PL spectra of 1LP/1LM1\mathrm{L}_{\mathrm{P}}/1\mathrm{L}_{\mathrm{M}} with bare 1LM1\mathrm{L}_{\mathrm{M}} (annealed) and 1LP/hBN1\mathrm{L}_{\mathrm{P}}/\mathrm{hBN} reference samples. XAX_{\mathrm{A}} is decomposed into two Voigt functions, representing the neutral exciton (XA0X_{\mathrm{A}}^{0}) and negative trion (XA−X_{\mathrm{A}}^{-}). PTCDA’s Raman peak is marked with an asterisk. (b) Thickness dependence of the XAX_{\mathrm{A}} energy under above-gap (514 nm) and sub-gap (633 nm) excitations. (c) Thickness dependence of the PL enhancement of XAX_{\mathrm{A}} for the two excitation wavelengths. (d) Energies of the XA0X_{\mathrm{A}}^{0} and XA−X_{\mathrm{A}}^{-} components extracted from spectral fitting. (e) Thickness dependence of the PL intensities, XA0X_{\mathrm{A}}^{0} and XA−X_{\mathrm{A}}^{-}, and the trion fraction in intensity, XA−/(XA−+XA0)X_{\mathrm{A}}^{-}/(X_{\mathrm{A}}^{-}+X_{\mathrm{A}}^{0}). (f) Schematic illustration of ground-state charge-transfer doping, showing electron transfer from MoS2\mathrm{MoS}_{2} and the resulting conversion of XA−X_{\mathrm{A}}^{-} to XA0X_{\mathrm{A}}^{0}.

It is notable that not only the PTCDA layer directly adjacent to MoS2_2 but also the overlayers inject holes: a similar estimate in Fig. S4 reveals that 5L PTCDA removes 1.7×10121.7 \times10^{12} electrons/cm2^2, twice that of 1L. This indicates that each layer is electronically coupled along the out-of-plane direction, so that the entire PTCDA crystals cooperate in charge-transfer doping. Such an electronic coupling, responsible for the out-of-plane charge delocalization, can be rationalized by the fact that PTCDA crystals consist of π\pi-stacked 1D PTCDA columns[36], which possess a Frenkel-CT excitonic band with a sizable bandwidth (>300> 300 meV)[37]. XA_{\mathrm{A}}’s PL enhancement for the 633 nm excitation in Figure 4c also agrees with the static charge-transfer doping: with increasing thickness, the residual electron density of MoS2_2 decreases due to the doping, and XA_{\mathrm{A}} state is more populated by neutral excitons (XA0_{\mathrm{A}}^0) with higher PL quantum yield than negative trions (XA−_{\mathrm{A}}^-)[38, 39], as illustrated in Figure 4f. To avoid complications arising from annealing-induced PL modulation[39], the PL enhancement was referenced to bare 1L MoS2_2 annealed at the growth temperature.

Dynamic interlayer coupling: photoluminescence modulation. The PL response of the heterocrystals is also substantially modified by excited-state interlayer coupling. The prominent molecular PL is reduced by a quenching factor of ∼500\sim500 for 1LP_{\mathrm{P}}/1LM_{\mathrm{M}} (Figure 4a). In contrast, the XA_{\mathrm{A}} emission is enhanced with increasing thickness for the 514 nm excitation (Figure 4c). Notably, the enhancement is twice as large as that for the 633 nm excitation: for the maximum thickness of 5LP_{\mathrm{P}}, the steady-state coupling caused a fivefold enhancement for 633 nm, and the dynamic coupling induced an additional twofold increase for 514 nm. To shed light on the origin of the additional PL enhancement by the above-gap excitation, we obtained PL excitation (PLE) spectra for 1LP1\mathrm{L}_{\mathrm{P}} and 4LP4\mathrm{L}_{\mathrm{P}} in Figure 5a. The PLE signals, given in the form of the PL enhancement, closely follow the DR spectra, indicating that photoexcitation is transferred from PTCDA to MoS2\mathrm{MoS_2}.

Image not extracted

Figure 5. Dynamic interlayer coupling and exciton transfer pathways. (a) PLE spectra of 1LP/1LM^{1}\mathrm{LP}/^{1}\mathrm{LM} and 4LP/1LM^{4}\mathrm{LP}/^{1}\mathrm{LM}, plotted with the corresponding DR spectra. (b) Spectral overlap between PTCDA’s PL (1LP/hBN^{1}\mathrm{LP}/\mathrm{hBN}) and MoS2\mathrm{MoS}_{2}’s absorption represented by DR (1LM/quartz^{1}\mathrm{LM}/\mathrm{quartz}). (c–d) Schematic energy-level diagram for above-gap excitation: RET from photoexcited PTCDA to MoS2\mathrm{MoS}_{2} (c) and hole transfer (hT) from PTCDA to MoS2\mathrm{MoS}_{2} (d). (e–f) Schematic energy-level diagram for sub-gap excitation, illustrating possible forward (e) and backward (f) electron transfer (eT) from photoexcited MoS2\mathrm{MoS}_{2} to PTCDA. The processes of (e–f) may occur for above-gap excitation.

We now address the microscopic origin of dynamic interlayer coupling, which underlies the broadening of the 0-0 absorptions, the drastic quenching of molecular PL, and the enhancement of XA\mathrm{X_A} PL. The substantial spectral overlap between the PTCDA PL and the MoS2\mathrm{MoS_2} absorption (Figure 5b), together with the in-plane alignment of their transition dipoles[8], provides favorable conditions for efficient RET. The close correspondence between the PLE and molecular absorption spectra (Figure 5a) further supports RET as the dominant mechanism underlying the additional PL enhancement, as depicted in Figure 5c. Park et al. also proposed efficient RET from PTCDA to MoS2\mathrm{MoS_2} to explain a sub-ps decay in the absorption of excited PTCDA[17]. In parallel with RET, interfacial resonance-controlled nonadiabatic CT[15] also contributes to the excited-state dynamics. The highest occupied molecular orbital (HOMO) of PTCDA is 0.5 eV lower than the valence band (VB) maximum of MoS2\mathrm{MoS_2}, providing a favorable downhill driving force for hole transfer. Combined with the substantial electronic coupling across the interface, this energetic alignment promotes efficient resonance-controlled nonadiabatic hole transfer from PTCDA to MoS2\mathrm{MoS_2} (Figure 5d), which explains the drastic quenching of the molecular PL. Such ultrafast hole transfer may also contribute to the ∼\sim35 meV broadening of the LDS absorption in Figure 3c. If the additional linewidth broadening is treated as a Lorentzian homogeneous contribution from interfacial hole transfer, the 35-meV increase corresponds to a transfer time of ∼\sim20 fs, which is comparable to the experimental timescale observed for interfacial CT in 2D heterocrystals[40]. This value, however, should be regarded as a lower-bound transfer time, because inhomogeneous broadening and exciton–phonon scattering may also contribute.

Overall, our PTCDA-MoS2\mathrm{MoS_2} system exhibits type-I-like exciton dynamics, in which photoinjected energy is funneled into MoS2\mathrm{MoS_2}, which has a smaller bandgap. We note, however, that nonadiabatic interfacial CT competes for a significant fraction of the photoexcitation. For the above-gap excitation, ultrafast hole transfer diverts excitonic energy in PTCDA toward MoS2\mathrm{MoS_2} to form interlayer CT excitons (Figure 5d). For the sub-gap excitation, the role of nonadiabatic electron transfer from MoS2\mathrm{MoS_2} to PTCDA is intriguing. Because the PTCDA LUMO and MoS2\mathrm{MoS_2} CBM are nearly resonant[17], forward (Figure 5e) and backward (Figure 5f) electron transfer processes may compete. Consequently, persistent interfacial charge separation is suppressed because electrons transferred to PTCDA can readily return to the MoS2\mathrm{MoS}_2 conduction band. As the lifetime of XAX_{\mathrm{A}} is ultrashort[41], this dynamic balance is therefore unlikely to quench the XAX_{\mathrm{A}} emission. This interpretation is consistent with the PL enhancement induced by the sub-gap excitation (Figure 4b), under which RET is not operative.

Finally, we connect the current work with previous studies on several-nm-thick polycrystalline PTCDA films/MoS2\mathrm{MoS}_2. Using two-photon photoemission, Rijal et al. observed ultrafast electron transfer from MoS2\mathrm{MoS}_2 to PTCDA, followed by the formation of interlayer excitons[15]. Despite the technical difficulty posed by their low oscillator strength, PL detection of interlayer excitons warrants experimental effort, as it will complete the picture of exciton dynamics in this heterosystem. Park et al. characterized a type-I interfacial electronic structure using angle-resolved photoemission and observed 100% PL enhancement[17], which is consistent with the current work. Whereas Obaidulla et al. assumed a type-II structure[16], they observed enhanced PL, which was attributed to multiple origins including static charge transfer doping, orbital hybridization and morphology-dependent nonradiative decay. It should be noted that the thick polycrystalline films employed in those studies can host molecular excimers and provide dielectric and electrostatic environments that differ substantially from those experienced by the few-layer epitaxial crystals investigated here.

Conclusions

In this work, we investigated thickness-controlled PTCDA/MoS2\mathrm{MoS}_2 heterocrystals and established a comprehensive picture of their structural and electronic properties. Electron diffraction combined with polarization-resolved spectroscopy revealed long-range crystalline order, epitaxial registry, and Davydov-split molecular excitons, demonstrating that the organic layer forms a structurally and excitonically well-defined interface with MoS2\mathrm{MoS}_2. Systematic optical measurements showed that interlayer coupling manifests through both spectral shifts and linewidth broadening, reflecting dielectric screening and the emergence of efficient nonradiative decay channels. In parallel, MoS2\mathrm{MoS}_2 excitons exhibit thickness-dependent energy shifts and linewidth narrowing, which we attribute to hole injection induced by ground-state charge transfer from PTCDA. By employing excitation-dependent photoluminescence, we separated the contributions of static and dynamic interlayer interactions. Ground-state charge transfer modifies exciton populations in MoS2\mathrm{MoS_2}, whereas photoexcited PTCDA introduces an additional enhancement channel. Photoluminescence excitation measurements further reveal that resonance energy transfer is the dominant mechanism underlying this dynamic coupling, whereas charge transfer primarily contributes to exciton quenching and doping. Overall, our results demonstrate that excitonic coupling in organic–inorganic heterostructures can be systematically tuned by molecular thickness. The ability to disentangle and control charge and energy transfer processes provides a framework for designing hybrid optoelectronic systems with tailored interfacial exciton dynamics.

Methods

_Preparation of 2D heterocrystals._ Single and few-layer PTCDA molecular crystals were formed by physical vapor assembly using 1L MoS2\mathrm{MoS_2} and few-layer hBN\mathrm{hBN} as assembly templates, as reported previously[8]. Briefly, the inorganic 2D crystals were prepared by mechanically exfoliating[42] their bulk counterparts (2D Semiconductors Inc., flux-grown MoS2\mathrm{MoS_2}) onto amorphous quartz substrates (SPI, SuperSmooth), unless otherwise noted. Although SiO2\mathrm{SiO_2}/Si substrates yielded flatter surfaces, they were not employed for optical measurements due to significant optical interference arising from multiple reflections[43]. Quartz substrates were cleaned using piranha solution, followed by UV-generated ozone treatment immediately prior to exfoliation. For growth, PTCDA powder (TCI, >98%) and the assembly templates were placed in the upstream and downstream zones of a three-zone tube furnace, respectively. After thoroughly purging the tube with Ar gas (99.999%) for 30 min at a flow rate of 500 mL/min, the same gas conditions were maintained at 100 mL/min throughout the growth process (20–40 min). The molecular source and template zones were maintained at 280–330 °C and 240–300 °C, respectively, with the source kept at a higher temperature. The thickness of PTCDA layers was determined with DR spectroscopy. The average thickness per growth batch was controlled by varying the growth time and temperature. Compared to the previous report using a single-zone furnace[8], the overall uniformity of PTCDA thickness was significantly improved, which was attributed to a reduced temperature gradient within the deposition area.

AFM measurements. The topographical details of the samples were characterized by an atomic force microscope (Park Systems Inc., XE-70). Height images were obtained in a non-contact mode using Si tips with a nominal radius of 8 nm (MicroMasch Inc., NSC-15).

TEM measurements. To enhance stability under electron-beam irradiation, thin graphene layers were laminated onto the heterocrystals of PTCDA and 1L MoS2\mathrm{MoS}_{2}[8]. Then, polydimethylsiloxane (PDMS) film (∼0.6\sim0.6 mm thick), supported on a glass slide, was overlaid on the sandwich of graphene/PTCDA/MoS2\mathrm{MoS}_{2}/quartz. While immersed in ethanol/DI water mixtures (ethanol 50%, DI water 50%) for 3 h, the stack was released from the quartz substrate and attached to the PDMS film. The PDMS-supported stack was dried under ambient conditions for 3–24 h. Subsequently, the stack was transferred onto holey SiN membrane TEM grids (Norcada Inc., hole diameter = 2 μ\mum) under optical microscope observation using a conventional dry transfer method[44]. Selected area electron diffraction (SAED) measurements were obtained at 80 kV using a JEOL JEM-F200, with a typical selected probing diameter of 0.8 μ\mum.

PL spectroscopy. The micro-spectroscopy setup used in this study has been described elsewhere[39]. Briefly, excitation was provided by solid-state (514.3 nm; Cobolt, Fandango) and He-Ne (632.8 nm; Melles Griot) lasers, focused onto the samples to a spot size of ∼1\sim1 μ\mum using a microscope objective (40×40\times, NA = 0.60). The emitted signals were collected using a spectrometer (Princeton Instruments, SP2300) equipped with a CCD camera (Princeton Instruments, PyLon). The overall spectral accuracy was better than 5 cm−1\mathrm{cm}^{-1}. All measurements were performed under ambient conditions. The average power was maintained below 70 nW to minimize photoinduced degradation.

PLE and DR spectroscopies. The two measurements were performed with another micro-spectroscopy system[45], similar to the one described above, except for light sources. Each of the source beams was focused onto the sample, and signals collected in a backscattering geometry using a 40×40\times objective lens (NA = 0.6) were then directed to a spectrometer equipped with a thermoelectrically cooled CCD detector (Andor Inc., DU971P). For PLE measurements, the excitation wavelength was tuned from 540 nm to 595 nm using an optical parametric oscillator (OPO; Coherent Inc., Chameleon Compact OPO-Vis) pumped by the Ti:sapphire laser (Coherent Inc., Chameleon Ultra II). The PL signals in the 640–730 nm range were integrated without polarization selection. The DR spectra were acquired using a collimated tungsten-halogen lamp as a broadband source in both unpolarized and polarization-resolved configurations, with the latter used for constructing polarization-dependent intensity plots.

Associated Content

Supporting Information.

Extraction of molecular absorption from DR of heterocrystals; DR spectra of pristine 1LM1\mathrm{L}_{\mathrm{M}} MoS2_2 (1LM1\mathrm{L}_{\mathrm{M}}), annealed 1LM1\mathrm{L}_{\mathrm{M}} and 1LP/1LM1\mathrm{L}_{\mathrm{P}}/1\mathrm{L}_{\mathrm{M}} heterocrystal (HC); Polarization-dependent DR spectra of 2LP/1LM2\mathrm{L}_{\mathrm{P}}/1\mathrm{L}_{\mathrm{M}}; Estimation of the excess electron density in MoS2_2 of heterocrystals; Crystallographic parameters of nLP/1LMn\mathrm{L}_{\mathrm{P}}/1\mathrm{L}_{\mathrm{M}} heterocrystals.

Author Information

Corresponding Author

*E-mail: [email protected]

Author Contributions

S.R. conceived the project. E.J. and S.R. designed the experiments. E.J., K.L., J.Y., K.W. and T.T. prepared samples. E.J., K.L., J.Y. and J.O. performed experiments and analyzed the data. E.J., K.K. and S.R. wrote the manuscript with contributions from all authors.

Notes

The authors declare no conflict of interest.

Acknowledgments

This work was supported by the National Research Foundation of Korea (NRF-RS-2024-00336324, NRF-RS-2024-00411134, NRF-2021R1A6A1A10042944) and the Glocal University 30 project.

Figure and Captions

Image not extracted

Figure 1. Structural and optical characterization of thickness-controlled PTCDA/MoS2_2 heterocrystals. (a) Schematic diagram of the 2D molecular lattice (top) and side-view structure of the 3LP/1LM3\mathrm{L}_{P}/1\mathrm{L}_{M} heterostructure (bottom), illustrating interfacial interactions via charge transfer (CT) and resonant energy transfer (RET). (b) AFM height image (middle) of 2LP/1LM2\mathrm{L}_{P}/1\mathrm{L}_{M} with the height line profile (top) and height histogram (bottom). The profile was averaged over the red-shaded area in the image. (c) Schematic energy-level diagrams for PTCDA and monolayer MoS2_2, illustrating the molecular 0-0 and 1-0 vibronic transitions with the XA_A and XB_B excitons of MoS2_2. (d) Unpolarized DR spectra of the 3LP/1LM3\mathrm{L}_{P}/1\mathrm{L}_{M} heterocrystal (denoted as HC), monolayer MoS2_2 (1LM1\mathrm{L}_{M}) and trilayer PTCDA on hBN (3LP3\mathrm{L}_{P}). (e) Baseline-subtracted unpolarized DR spectra of 00–5LP/1LM5\mathrm{L}_{P}/1\mathrm{L}_{M}. The DR spectra of HCs were fitted using 5 Gaussian functions and a quadratic baseline (see Fig. S1 for details). (f) Peak areas of 0-0 and 1-0 molecular absorption and their sum as a function of PTCDA thickness.

Image not extracted

Figure 1 (PDF p. 23).

References

  1. [1]Hestand, N. J.; Spano, F. C., Expanded Theory of H- and J-Molecular Aggregates: The Effects of Vibronic Coupling and Intermolecular Charge Transfer. Chem. Rev. 2018, 118 (15), 7069–7163.DOI
  2. [2]He, D.; Zhang, Y.; Wu, Q.; Xu, R.; Nan, H.; Liu, J.; Yao, J.; Wang, Z.; Yuan, S.; Li, Y.; Shi, Y.; Wang, J.; Ni, Z.; He, L.; Miao, F.; Song, F.; Xu, H.; Watanabe, K.; Taniguchi, T.; Xu, J.-B.; Wang, X., Two-dimensional quasi-freestanding molecular crystals for high-performance organic field-effect transistors. Nat. Commun. 2014, 5 (1), 5162.DOI
  3. [3]Sharma, A.; Zhang, L.; Tollerud, J. O.; Dong, M.; Zhu, Y.; Halbich, R.; Vogl, T.; Liang, K.; Nguyen, H. T.; Wang, F.; Sanwlani, S.; Earl, S. K.; Macdonald, D.; Lam, P. K.; Davis, J. A.; Lu, Y., Supertransport of excitons in atomically thin organic semiconductors at the 2D quantum limit. Light Sci. Appl. 2020, 9 (1), 116.DOI
  4. [4]Koo, S.; Park, L.; Watanabe, K.; Taniguchi, T.; Shim, J. H.; Ryu, S., Extraordinary photostability and Davydov splitting in BN-sandwiched single-layer tetracenemolecular crystals. Nano Lett. 2021, 21 (15), 6600–6608.DOI
  5. [5]Carvalho, A.; Wang, M.; Zhu, X.; Rodin, A. S.; Su, H. B.; Neto, A. H. C., Phosphorene: from theory to applications. Nat. Rev. Mater. 2016, 1 (11), 16061.DOI
  6. [6]Ludwig, C.; Gompf, B.; Petersen, J.; Strohmaier, R.; Eisenmenger, W., STM investigations of PTCDA and PTCDI on graphite and MoS2. A systematic study of epitaxy and STM image contrast. Z. Phys. B 1994, 93 (3), 365–373.DOI
  7. [7]Wang, Q. H.; Hersam, M. C., Room-temperature molecular-resolution characterization of self-assembled organic monolayers on epitaxial graphene. Nat. Chem. 2009, 1 (3), 206–211.DOI
  8. [8]Kim, D.; Lee, S.; Park, J.; Lee, J.; Choi, H. C.; Kim, K.; Ryu, S., In-plane and out-of-plane excitonic coupling in 2D molecular crystals. Nat. Commun. 2023, 14 (1), 2736.DOI
  9. [9]Chowdhury, T.; Mujid, F.; Naqvi, Z.; Ray, A.; Liang, C.; Muller, D. A.; Guisinger, N. P.; Park, J., Spectra-Orthogonal Optical Anisotropy in Wafer-Scale Molecular Crystal Monolayers. Nano Lett. 2025, 25 (14), 5852–5859.arxiv.org/abs/2502.01629
  10. [10]Zhao, H.; Zhao, Y.; Song, Y.; Zhou, M.; Lv, W.; Tao, L.; Feng, Y.; Song, B.; Ma, Y.; Zhang, J.; Xiao, J.; Wang, Y.; Lien, D.-H.; Amani, M.; Kim, H.; Chen, X.; Wu, Z.; Ni, Z.; Wang, P.; Shi, Y.; Ma, H.; Zhang, X.; Xu, J.-B.; Troisi, A.; Javey, A.; Wang, X., Strong optical response and light emission from a monolayer molecular crystal. Nat. Commun. 2019, 10 (1), 5589.DOI
  11. [11]Hasan, M. M.; Hume, P. A.; Zhang, L.; Lu, Y., Excitonic Dark States in Molecular Monolayer Crystals. Nano Lett. 2025, 25 (1), 383–390.DOI
  12. [12]Gao, M.; Hong, H.; Fan, S.; Chowdhury, T.; Naqvi, Z.; Ge, J.; Liang, C.; Han, Y.; Guisinger, N. P.; Qiu, Y.; Kim, D. H.; Vaikuntanathan, S.; Liu, C.; Park, J., Room-temperature charge localization in ion-coupled bilayer transistors. Science 2025, 390 (6771), 356–360.DOI
  13. [13]Zhang, L.; Sharma, A.; Zhu, Y.; Zhang, Y.; Wang, B.; Dong, M.; Nguyen, H. T.; Wang, Z.; Wen, B.; Cao, Y.; Liu, B.; Sun, X.; Yang, J.; Li, Z.; Kar, A.; Shi, Y.; Macdonald, D.; Yu, Z.; Wang, X.; Lu, Y., Efficient and Layer-Dependent Exciton Pumping across Atomically Thin Organic–Inorganic Type-I Heterostructures. Adv. Mater. 2018, 30 (40), 1803986.DOI
  14. [14]Chen, X.; Zhao, H.; Fei, R.; Huang, C.; Qiao, J.; Sun, C.; Zhu, H.; Zhan, L.; Hu, Z.; Li, S.; Yang, L.; Tang, Z.; Wang, L.; Shi, Y.; Ji, W.; Xu, J.-B.; Gao, L.; Gan, X.; Wang, X.; Efficient energy transfer in a hybrid organic-inorganic van der Waals heterostructure. Sci. Adv. 2025, 11 (36), eadw3969.
  15. [15]Rijal, K.; Rudayni, F.; Kafle, T. R.; Chan, W.-L., Collective Effects of Band Offset and Wave Function Dimensionality on Impeding Electron Transfer from 2D to Organic Crystals. J. Phys. Chem. Lett. 2020, 11 (18), 7495–7501.DOI
  16. [16]Obaidulla, S. M.; Habib, M. R.; Khan, Y.; Kong, Y.; Liang, T.; Xu, M., Photoluminescence: MoS2 and Perylene Derivative Based Type-II Heterostructure: Bandgap Engineering and Giant Photoluminescence Enhancement (Adv. Mater. Interfaces 2/2020). Adv. Mater. Interfaces 2020, 7 (3), 2070014.
  17. [17]Park, S.; Mutz, N.; Kovalenko, S. A.; Schultz, T.; Shin, D.; Aljarb, A.; Li, L.-J.; Tung, V.; Amsalem, P.; List-Kratochvil, E. J. W.; Stähler, J.; Xu, X.; Blumstengel, S.; Koch, N., Type-I Energy Level Alignment at the PTCDA—Monolayer MoS2 Interface Promotes Resonance Energy Transfer and Luminescence Enhancement. Adv. Sci. 2021, 8 (12), 2100215.DOI
  18. [18]Le, O. K.; Chihaiа, V.; Van On, V.; Son, D. N., N-type and p-type molecular doping on monolayer MoS2. ACS Appl. Mater. Interfaces 2021, 11 (14), 8033–8041.DOI
  19. [19]Rijal, K.; Amos, S.; Valencia-Acuna, P.; Rudayni, F.; Fuller, N.; Zhao, H.; Peelers, H.; Chan, W.-L., Nanoscale Periodic Trapping Sites for Interlayer Excitons Built by Deformable Molecular Crystal on 2D Crystal. ACS Nano 2023, 17 (8), 7775–7786.DOI
  20. [20]Singha Roy, S.; Bindl, D. J.; Arnold, M. S., Templating Highly Crystalline Organic Semiconductors Using Atomic Membranes of Graphene at the Anode/Organic Interface. J. Phys. Chem. Lett. 2012, 3 (7), 873–878.DOI
  21. [21]Mativetsky, J. M.; Wang, H.; Lee, S. S.; Whittaker-Brooks, L.; Loo, Y.-L., Face-on stacking and enhanced out-of-plane hole mobility in graphene-templated copper phthalocyanine. Chem. Commun. 2014, 50 (40), 5319–5321.DOI
  22. [22]Jariwala, D.; Howell, S. L.; Chen, K.-S.; Kang, J.; Sangwan, V. K.; Filippone, S. A.; Turrisi, R.; Marks, T. J.; Lauhon, L. J.; Hersam, M. C., Hybrid, Gate-Tunable, van der Waals p–n Heterojunctions from Pentacene and MoS2. Nano Lett. 2016, 16 (1), 497–503.DOI
  23. [23]Zhang, Y.; Qiao, J.; Gao, S.; Hu, F.; He, D.; Wu, B.; Yang, Z.; Xu, B.; Li, Y.; Shi, Y.; Ji, W.; Wang, P.; Wang, X.; Xiao, M.; Xu, H.; Xu, J.-B.; Wang, X., Probing Carrier Transport and Structure-Property Relationship of Highly Ordered Organic Semiconductors at the Two-Dimensional Limit. Phys. Rev. Lett. 2016, 116 (1), 016602.DOI
  24. [24]Ogawa, T.; Kuwamoto, K.; Isoda, S.; Kobayashi, T.; Karl, N., 3,4:9,10-Perylenetetracarboxylic dianhydride (PTCDA) by electron crystallography. Acta Crystallogr. B 1999, 55 (1), 123–130.pubmed.ncbi.nlm.nih.gov/10927346
  25. [25]Mak, K. F.; Lee, C.; Hone, J.; Shan, J.; Heinz, T. F., Atomically thin MoS2: A new direct-gap semiconductor. Phys. Rev. Lett. 2010, 105 (13), 136805.DOI
  26. [26]Splendiani, A.; Sun, L.; Zhang, Y. B.; Li, T. S.; Kim, J.; Chim, C. Y.; Galli, G.; Wang, F., Emerging photoluminescence in monolayer MoS2. Nano Lett. 2010, 10 (4), 1271–1275.DOI
  27. [27]Mak, K. F.; Sfeir, M. Y.; Wu, Y.; Lui, C. H.; Misewich, J. A.; Heinz, T. F., Measurement of the Optical Conductivity of Graphene. Phys. Rev. Lett. 2008, 101 (19), 196405.DOI
  28. [28]Bulovic, V.; Burrows, P. E.; Forrest, S. R.; Cronin, J. A.; Thompson, M. E., Study of localized and extended excitons in 3,4,9,10-perylenetetracarboxylic dianhydride (PTCDA) I. Spectroscopic properties of thin films and solutions. Chem. Phys. 1996, 210 (1), 1–12.DOI
  29. [29]Davydov, A. S., The theory of molecular excitons. Sov. Phys. Usp. 1964, 7 (2), 145–178.
  30. [30]Kasha, M.; Rawls, H. R.; El-Bayoumi, M. A., The exciton model in molecular spectroscopy. Pure Appl. Chem. 1965, 11 (3-4), 371–392.DOI
  31. [31]Martinez-Galera, A. J.; Gomez-Rodriguez, J. M., Structural and Electronic Properties of 3,4,9,10-Perylene Tetracarboxylic Dianhydride on h-BN/Rh(110). J. Phys. Chem. C 2019, 123 (9), 1866–1873.
  32. [32]Zheng, Y. J.; Huang, Y. L.; Chen, Y.; Zhao, W.; Eda, G.; Spataru, C. D.; Zhang, W.; Chang, Y.-H.; Li, L.-J.; Chi, D.; Quek, S. Y.; Wee, A. T. S., Heterointerface Screening Effects between Organic Monolayers and Monolayer Transition Metal Dichalcogenides. ACS Nano 2016, 10 (2), 2476–2484.DOI
  33. [33]So, F. F.; Forrest, S. R., Evidence for exciton confinement in crystalline organic multiple quantum wells. Phys. Rev. Lett. 1991, 66 (20), 2649–2652.pubmed.ncbi.nlm.nih.gov/10043576
  34. [34]Mak, K. F.; He, K.; Lee, C.; Lee, G. H.; Hone, J.; Heinz, T. F.; Shan, J., Tightly bound trions in monolayer MoS₂. Nat. Mater. 2013, 12 (3), 207–211.DOI
  35. [35]Zhang, X.; Shao, Z.; Zhang, X.; He, Y.; Jie, J., Surface Charge Transfer Doping of Low-Dimensional Nanostructures toward High-Performance Nanodevices. Adv. Mater. 2016, 28 (47), 10409–10442.DOI
  36. [36]Gisslen, L.; Scholz, R., Crystalloсhromy of perylene pigments: Interference between Frenkel excitons and charge-transfer states. Phys. Rev. B 2009, 80 (11), 115309.DOI
  37. [37]Knupfer, M.; Schwieger, T.; Fink, J.; Leo, K.; Hoffmann, M., Excitons in quasi-one-dimensional organic crystals. Phys. Rev. B 2002, 66 (3), 035208.DOI
  38. [38]Tongay, S.; Zhou, J.; Ataca, C.; Liu, J.; Kang, J. S.; Matthews, T. S.; You, L.; Li, J.; Grossman, J. C.; Wu, J., Broad-range modulation of light emission in two-dimensional semiconductors by molecular physisorption gating. Nano Lett. 2013, 13 (6), 2831–2836.DOI
  39. [39]Park, K.; Kang, H.; Koo, S.; Lee, D.; Ryu, S., Redox-governed charge doping dictated by interfacial diffusion in two-dimensional materials. Nat. Commun. 2019, 10 (1), 4931.DOI
  40. [40]Hong, X. P.; Kim, J.; Shi, S. F.; Zhang, Y.; Jin, C. H.; Sun, Y. H.; Tongay, S.; Wu, J. Q.; Zhang, Y. F.; Wang, F., Ultrafast charge transfer in atomically thin MoS₂/WS₂ heterostructures. Nat. Nanotechnol. 2014, 9 (9), 682–686.DOI
  41. [41]Shi, H. Y.; Yan, R. S.; Bertolazzi, S.; Brivio, J.; Gao, B.; Kis, A.; Jena, D.; Xing, H. G.; Huang, L. B., Exciton Dynamics in Suspended Mono layer and Few-Layer MoS2 2D Crystals. ACS Nano 2013, 7 (2), 1072–1080.DOI
  42. [42]Novoselov, K. S.; Jiang, D.; Schedin, F.; Booth, T. J.; Khotkevich, V. V.; Morozov, S. V.; Geim, A. K., Two-dimensional atomic crystals. Proc. Natl. Acad. Sci. U. S. A. 2005, 102 (30), 10451–10453.pubmed.ncbi.nlm.nih.gov/16027370
  43. [43]Yoon, D.; Moon, H.; Son, Y. W.; Choi, J. S.; Park, B. H.; Cha, Y. H.; Kim, Y. D.; Cheong, H., Interference effect on Raman spectrum of graphene on SiO2/Si. Phys. Rev. B 2009, 80 (12), 125422.DOI
  44. [44]Ryu, Y.; Kim, W.; Koo, S.; Kang, H.; Watanabe, K.; Taniguchi, T.; Ryu, S., Interface-confined doubly anisotropic oxidation of two-dimensional MoS₂. Nano Lett. 2017, 17 (12), 7267–7273.DOI
  45. [45]Kim, W.; Ahn, J. Y.; Oh, J.; Shim, J. H.; Ryu, S., Second-harmonic Young’s interference in atom-thin heterocrystals. Nano Lett. 2020, 20 (12), 8825–8831.

Paper details

vlnc:W_pdxpbyf6
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents