Reducing TLS loss in tantalum CPW resonators using titanium sacrificial layers
Abstract
We demonstrate a substantial reduction in two-level system loss in tantalum coplanar waveguide resonators fabricated on high-resistivity silicon substrates through the use of an ultrathin titanium sacrificial layer. A 0.2nm titanium film, deposited atop pre-sputtered α-tantalum, acts as a solid-state oxygen getter that chemically modifies the native Ta oxide at the metal-air interface. After device fabrication, the titanium layer is removed using buffered oxide etchant, leaving behind a chemically reduced Ta oxide surface. Subsequent high-vacuum annealing further suppresses two-level system loss. Resonators treated with this process exhibit internal quality factors Qi exceeding an average of 1.5 million in the single-photon regime across ten devices, over three times higher than otherwise identical devices lacking the titanium layer. These results highlight the critical role of interfacial oxide chemistry in superconducting loss and reinforce atomic-scale surface engineering as an effective approach to improving coherence in tantalum-based quantum circuits. The method is compatible with existing fabrication workflows applicable to tantalum films, offering a practical route to further extending T1 lifetimes in superconducting qubits.
Reducing loss and decoherence in superconducting circuits through materials engineering is a direct and scalable approach to enhancing qubit coherence, compared to alternative circuit-level approaches such as participation ratio optimisation.[1, 2, 3, 4] By targeting the microscopic origins of decoherence[4, 5]—particularly dielectric loss from two-level systems (TLS) at device interfaces[6, 7, 8]—this strategy enables intrinsic improvements to and without requiring changes to qubit architecture. Crucially, materials-based methods have the advantage of being readily compatible with existing device layouts and fabrication workflows, making them broadly accessible.
The adoption of tantalum (Ta) as a superconducting material has led to major advances in the coherence times of superconducting quantum processors and internal quality factors of superconducting resonators,[9, 10, 11, 12, 13, 14] including recent demonstrations of 2D transmon qubits with energy relaxation times () exceeding 1.6 milliseconds.[15] This improvement is widely attributed to the chemically stable and high-quality native oxide formed on Ta, which plays a key role in suppressing dielectric loss from TLS.[7, 11] This confers a distinct advantage over other superconductors such as niobium (Nb), whose native oxide is comparatively lossy.[16, 17] However, despite the reduced intrinsic losses of Ta oxides, Ta-on-silicon superconducting resonators and qubits remain limited by TLS losses originating from surface oxides—particularly at the metal–air (MA) interface—underscoring the need for a more precise understanding and control of interfacial oxide chemistry and structure.[15, 18] Amorphous Ta pentoxide (-TaO)—the primary native oxide phase—grows spontaneously upon air exposure, owing to the highly negative formation energy of TaO.[19] Although thinner than native oxides on other superconductors, such as NbO, the Ta oxide still contributes significantly to decoherence through TLS dipoles associated with its amorphous structure.[7]
While oxides can be readily removed through techniques such as chemical or physical etching, their spontaneous regrowth is unavoidable during fabrication and device packaging. This has motivated studies on capping and passivation layers—such as gold, gold-palladium, magnesium oxide and organic self-assembled monolayers—deposited atop superconducting films to prevent or minimise oxide regrowth.[20, 21, 22] These methods are generally successful in reducing oxide regrowth and improving surface metallicity, however the resulting reductions in TLS loss are modest at best, and in some cases increased due to the added interface complexity on the measured devices.
In parallel to capping- or passivation-layers, sacrificial layers offer an approach to modify the underlying film surface without remaining in-place during device operation, typically being removed by selective etching at the end of device fabrication. Materials such as yttrium (Y)[23] and titanium (Ti)[24] have been employed as sacrificial layers—up to 10 nm in thickness—in high-mobility graphene devices to improve cleanliness, simplify large-scale fabrication, and reduce device-to-device variability. Deposited prior to critical fabrication steps and subsequently removed, the sacrificial layer serves to getter oxides and contaminants, and protect the active surface from residue accumulation.
Here, we demonstrate a surface engineering approach that enhances the quality factor of superconducting coplanar waveguide (CPW) resonators by modifying the Ta oxide through the application of an ultrathin Ti sacrificial layer, significantly reducing TLS loss at the MA interface and reducing device variability. Fabricating devices with such a sacrificial Ti layer, along with post-fabrication buffered oxide etching (BOE) and high temperature annealing, we observe up to a four-fold increase in the internal Q-factor () of Ta-on-Si CPW resonators compared to otherwise identical devices without the Ti layer. These resonators reach values above 2 million at single photon occupancy, and above 10 million at higher photon numbers.
Unlike traditional capping layers, which remain on the device and can complicate fabrication or introduce additional interfaces,[17, 20, 22] our method uses an ultrathin Ti film as a temporary, removable, and reactive surface modifier. Deposited on a Ta film, the Ti layer acts as a solid-state oxygen getter, preferentially reacting with ambient or residual oxygen to modify the formation dynamics of the native Ta oxide. This alters the interfacial chemistry, leading to a thinner, less defective Ta oxide with reduced TLS density, and therefore a lower MA loss tangent . Furthermore, the Ti layer has a dual-use of acting as a kinetic barrier to (re)oxidation, protecting the underlying Ta during lithographic fabrication steps. From the phase diagram of the Ta-Ti system, it can be seen that alloys are unable to form below 882 °C,[25] preventing detrimental inter-diffusion of the layers during annealing steps during fabrication. After lithography, the Ti is subsequently removed using buffered oxide etchant (BOE), eliminating it from the final device while retaining the favourable oxide modification. The process offers a clean and scalable route to improving dielectric interfaces and is highly compatible with standard thin-film deposition and microfabrication techniques, enabling rapid adoption by groups seeking to reduce surface losses in superconducting quantum circuits.
To assess the impact of the Ti sacrificial layer and to separate its contribution from other fabrication-dependent effects, we fabricate CPW resonators from 200 nm sputtered -Ta films on high-resistivity Si. The devices were designed and simulated using the open-source SQDMetal software stack[27].
A subset of chips are produced on films incorporating a 2 Å Ti sacrificial layer, deposited prior to any patterning (see Appendix for details). Following optical lithography and CF reactive ion etching, all chips undergo resist stripping and an O-plasma clean, which leaves both Ta and Si surfaces oxidised. After their final BOE treatment (described below), samples are wire-bonded and packaged within hours to minimise regrowth of surface oxides before cryostat loading.
To systematically explore how surface preparation influences resonator performance, we fabricate devices spanning a controlled range of post-processing parameters. Each chip receives some combination of: (i) BOE exposure—either a short 1 min etch (ID: S) or a long 20 min etch (ID: L); (ii) high-temperature annealing at 700°C for 10 h (ID: A) or no anneal; and (iii) inclusion (ID: T) or omission (ID: R) of the 2 Å Ti sacrificial layer. These IDs correspond to the device labels used in Table I and Figure 3. By independently varying BOE duration, annealing, and Ti-layer inclusion, we isolate the effect of each treatment on the resulting resonator quality.

Figure 3. Internal quality factor measurements for bare Ta reference samples, and variants of Ti/Ta devices. (a) Measured data (points) as a function of mean intracavity photon number with a saturable TLS model fit according to Eq. (2) (solid lines), yielding values given in Table I. (b) Box plot showing the distribution of values at single photon power () across resonators on each sample. The box spans the interquartile range (IQR) from the 25th (Q1) to the 75th (Q3) percentile, with a white dot at the median value. Whiskers extend to the most extreme data points within from the box.
Each device contains five CPW resonators capacitively coupled to a common feed-line, as shown in Figure 2(a). Complex transmission data was recorded in a 0.5 MHz span around the fundamental frequency of each resonator, designed to be between 5.5 GHz and 7.0 GHz for all samples.

Figure 2. (a) Schematic of the fabricated circuit with five resonators side-coupled to a transmission line. The resonator CPW has a 5 μm gap and 9 μm width. (b) Complex data (points) and circle fit (line) over a 100 kHz span around the centre frequency . The scattering data traces a circle in the complex plane (left) and produces a Lorentzian dip in amplitude (right)[26].
For power-dependent measurements, as shown in Figure 3, the applied power at the resonator input was varied from −72 dBm to −162 dBm, corresponding to average intracavity photon numbers from to . Complex resonance spectra—such as that shown in Figure 2(b)—were fit using a diameter-corrected circle-fit method developed by Probst et al.[28], allowing for the extraction of , and the coupling quality factor .
The magnitude of TLS loss was determined using a model accounting for losses due to TLSs (), quasiparticles (), and temperature- and power-independent high power losses ().[7]
The contributions from TLS losses are parametrised by
where is the geometry-dependent filling factor, is the linear TLS absorption, is the fundamental angular frequency of the resonator, and is the critical photon number above which TLS saturate, and is an exponent varying between for non-interacting TLS, and for interacting TLS.[29, 30] All power sweeps were taken at a constant temperature of mK.
Temperature-dependent measurements of are shown in Figure 4. The temperature dependence of TLS and thermal quasiparticle losses was quantified by extracting over a range from mK to mK, at six photon occupancies spanning approximately to . Temperature-dependent losses due to thermally excited quasiparticles are modelled as

Figure 4. Temperature dependence of for a single resonator at GHz on a Ti-treated and annealed sample (T-LA2). Experimental data is shown as points, with a fitted temperature- and power-dependent loss model (Eq. (1)) displayed as a solid line. The measurement was repeated at six evenly-spaced power levels between dBm (dark blue) and dBm (light blue), corresponding to intracavity photon numbers of and respectively.
| Sample ID | Ti layer | Post-BOE | Anneal | () | () | () | () |
| R-L | None | 20 min | None | 0.44 | |||
| R-LA | None | 20 min | , 10 hr | 0.66 | |||
| T-SA | 2 Å | 1 min | , 10 hr | 0.48 | |||
| T-L | 2 Å | 20 min | None | 0.68 | |||
| T-LA1 | 2 Å | 20 min | , 10 hr | 1.55 | |||
| T-LA2 | 2 Å | 20 min | , 10 hr | 2.14 |
Table 1. measurement results for resonator devices and filling-factor-adjusted TLS loss tangents extracted from power-dependent data (Figure 3). Sample IDs follow the format X-BA, where X denotes the material type (R = bare Ta, T = Ti-treated), B indicates the BOE treatment (L = long, S = short), and A marks whether the sample was annealed (A = annealed, omitted if not). Values are shown as the mean taken across all resonators on the sample, except which is the maximum single photon on each sample. The standard deviation on the average is also shown. Superscripts HP and LP refer to low- and high-power respectively, where , and . We note that losses in some samples losses had not yet saturated (i.e., reached a steady state with respect to photon number) at high power.
where is the linear absorption from thermal quasiparticles, is the superconducting gap (, and K is the superconducting critical temperature of the film), and is the zeroth order modified Bessel function of the second kind.[7, 29]
Figure 3 shows the power-dependent and single-photon for devices fabricated with variations in post-lithography treatment (short/long BOE), annealing, and the inclusion of a 2 Å Ti layer. We use sample R-L as a benchmark, fabricated using standard methods for high- Ta-on-Si CPW resonators (bare Ta, long BOE, no anneal)[7, 31], which exhibits a mean at single-photon power. This device serves as
a baseline for comparison, with its internal quality factor reflecting the intrinsic properties of our Ta-on-Si films. While not the focus of this study, our baseline is slightly lower than reported state-of-the-art resonators fabricated by similar methods (including post-lithography BOE/HF treatment) on optimised -Ta films ( to 4 million),[18, 32] and should be considered when evaluating the impact of the Ti sacrificial layer.
We first examine the impact of annealing on a bare Ta sample after a 20 min BOE treatment, observing a substantial increase in quality factor to , corresponding to a reduction in TLS losses. This improvement is attributed to a favourable rearrangement of the local coordination environment at the MAA interface, where annealing modifies both the Ta oxide and the underlying metal layer to suppress TLS formation.[7] The crystallisation of TaO films has been reported to onset between and , suggesting that regions of our oxide may begin to crystallise during the 10 hr anneal at [33, 34], however we were unable to confirm the existence of crystalline regions with grazing incidence X-ray scattering experiments. Similar restructuring and crystallisation of surface oxides have been observed in niobium devices, where they correlate with reduced losses.[35] Annealing consistently improves performance in both bare Ta and Ti-treated devices, and ongoing efforts aim to optimise the thermal budget of this step by lowering its duration. Devices R-LA (bare Ta, long-BOE, anneal), T-SA (2 Å Ti, short-BOE, anneal), and T-L (2 Å Ti, long-BOE, no anneal) exhibit similar low power losses to the baseline sample.
Consistent with previous studies, we find that the post-lithography BOE step substantially reduces surface losses, primarily by removing lossy SiO at the SA interface and partially thinning the native Ta oxide at the MA interface. Lozano et al. recently reported a similar effect in Ta-on-Si devices, showing that HF etching significantly suppresses loss contributions from SiO at the SA interface, resulting in a 2–4 reduction in total TLS losses.[18] In our devices, comparing samples T-SA (short 1 min BOE) and T-LA (long 20 min BOE), we likewise observe a 2–4 reduction in . We also observe that the device exposed to only 1 min BOE (T-SA) has a much higher critical photon number (see Eq. 2), suggesting a larger number of depolarising TLS. As confirmed by XPS measurements and shown in Figure 1, the 2 Å Ti sacrificial layer is fully removed after the long BOE treatment. By contrast, XPS on a sample equivalent to T-SA indicates that the Ti layer remains intact after the short BOE step (see Appendix). While BOE effectively reduces losses associated with TLS hosted at the SA interface, its influence on the MA interface is limited.[18]

Figure 1. (a) Schematic of CPW fabrication with a sacrificial Ti layer. Native Ta oxide was removed by Ar ion beam milling, followed by in situ deposition of a 2 Å Ti layer. Circuit patterning was performed using positive-tone optical lithography and CF-based reactive ion etching. Post-fabrication treatments consisted of buffered oxide etching (BOE) and annealing. (b) Surface atomic concentrations from XPS survey scans at stages marked in (a). The Ti layer is retained during lithography and etching, then removed by long-BOE prior to annealing.
To directly address losses at the MA interface, we introduce a Ti sacrificial layer as a complementary strategy. Comparing the bare-Ta reference sample R-LA with the Ti-treated samples T-LA1 and T-LA2, we observe an additional enhancement in the single-photon by a factor of ∼2–4, which we attribute to loss reduction enabled by the sacrificial layer. At high power, the of the Ti-treated devices further improves by a factor of ∼3–9 relative to the reference. The magnitude of these improvements is comparable to those achieved through long-BOE treatment, which is a well-established key step in the fabrication of ultra-high- Ta resonators. Taken together, these results demonstrate that the Ti sacrificial layer substantially enhances an already optimised Ta fabrication process, providing a clear pathway to longer coherence times in state-of-the-art superconducting qubits.
Devices with residual Ti (sample T-SA) exhibited reduced , indicative of additional loss channels likely associated with an amorphous TiO layer at the MA interface. This highlights the critical role of precise chemical control and selectivity in achieving oxide suppression, and clarifies that the Ti layer does not function as a capping layer.
Despite concerns from prior work that ion milling can degrade by restructuring oxides and introducing oxygen defects,[36, 37] we observe no performance loss following the argon ion milling step used to remove native Ta oxides prior to Ti deposition. We attribute this resilience to the oxygen-scavenging action of the Ti layer, which likely removes embedded defects, and to the beneficial effects of subsequent annealing, which may passivate surfaces or recrystallise near-surface regions.[35] Notably, even the un-annealed Ti/Ta sample (argon-milled) outperforms the bare Ta control (not milled), suggesting that the Ti layer alone substantially mitigates milling-induced damage.
Temperature-dependent measurements, as shown in Figure 4, demonstrate that quasiparticle losses become appreciable only at elevated temperatures ( mK, where the thermal energy is an appreciable fraction of the intracavity photon energy ), confirming that losses at qubit operating temperatures are dominated by dielectric TLSs. The extracted TLS loss tangents are near the lower bound expected for this material system and device geometry. Compared to state-of-the-art devices reported in the literature, such as the compilation by McRae et al., our resonators approach the performance limit for sub-10 μm features on silicon substrates.[38]
The use of a Ti sacrificial layer represents a novel approach to improving the internal quality factor of superconducting Ta-on-Si CPW resonators by addressing losses at the metal-air (MA) interface. Unlike conventional capping layers that are co-deposited with the bulk film and retained throughout processing, this method is applied post-deposition and fully removed prior to measurement. This decoupling of growth and oxide engineering enables greater flexibility and compatibility with standard fabrication workflows. As Ti is readily available in most electron beam evaporation systems, the technique is also broadly accessible. While demonstrated here on CPW resonators, the method is directly transferable to base-layer fabrication in planar qubit architectures such as the transmon.
In conclusion, we have demonstrated a Ti sacrificial layer approach for reducing losses in Ta-based superconducting circuits. Whereas previous improvements to the quality factor of Ta resonators have largely targeted the SM and SA interfaces, our method directly mitigates losses at the MA interface. We fabricated and characterised a broad set of superconducting CPW resonators, enabling direct comparison of TLS losses between otherwise identical devices. XPS measurements were employed to track chemical changes at the MA interface during fabrication and across device variants. Devices incorporating a 2 Å sacrificial Ti layer consistently exhibited single-photon above one million, representing a 2–4× enhancement compared to otherwise identical devices without the Ti layer. Temperature-dependent measurements confirm that losses in the operating regime are dominated by depolarising TLS. To further improve process robustness and accessibility, future work should explore the use of thicker Ti layers, which may simplify process control and increase fabrication tolerance. The impact of annealing steps with reduced thermal budget, and their compatibility with higher-throughput fabrication, should also be investigated.
Author Contributions
Zachary Degnan: Data curation (lead); Measurement (lead); Fabrication (lead); Simulation (equal); Conceptualisation (equal); Formal analysis (lead); XPS (lead); GIWAXS (lead); Investigation (equal); Validation (lead); Visualisation (lead); Writing – original draft (lead); Writing – review & editing (lead). Chun-Ching Chiu, Yi-Hsun Chen: Measurement (supporting); Fabrication (supporting); XPS (supporting). David Sommers: Simulation (equal); Measurement (supporting). Leonid Abdurakhimov, Lihuang Zhu: Fabrication (supporting); Investigation (supporting); Writing – review & editing (supporting). Arkady Fedorov: Investigation (equal); Funding acquisition (equal); Conceptualisation (equal). Peter Jacobson: Investigation (equal); Funding acquisition (equal); Conceptualisation (equal); Writing – original draft (supporting); Writing – review & editing (supporting).
Acknowledgements
The authors acknowledge that UQ operates on the land of the Jagera and Turrbal peoples. The authors pay respects to their ancestors and descendants who continue to uphold connection to country. GIWAXS measurements were undertaken on the NCD-SWEET beamline at the ALBA Synchrotron (Barcelona, Spain). The authors acknowledge the assistance of Dr. Julian Steele and Dr. Eduardo Solano with GIWAXS measurements. We acknowledge travel funding provided by the International Synchrotron Access Program (ISAP) managed by the Australian Synchrotron, part of ANSTO, and funded by the Australian Government. The authors also acknowledge the facilities, and the scientific and technical assistance from staff at the Centre for Microscopy and Microanalysis (CMM) at the University of Queensland. This work used the Queensland node of the NCRIS-enabled Australian National Fabrication Facility (ANFF). This work was partially supported by the Australian Research Council under the grant LP210200636.
Fabrication methods
To construct our Ti-Ta-Si material stack, we deposit a 2 Å sacrificial Ti layer atop a bcc -Ta film, which is known to host fewer TLS defects than the tetragonal -Ta phase.[11] A 200 nm -Ta film is grown by magnetron sputtering on high-resistivity Si at room temperature using a Nb buffer layer, which promotes high-quality single-phase -Ta growth due to its minimal () lattice mismatch with Ta.[32, 39, 40] The film phase is verified by synchrotron grazing-incidence wide-angle X-ray scattering (GIWAXS) measurements (Figure 8, Figure 9), where strong Bragg peaks corresponding to bcc -Ta are observed and no peaks from -Ta are detected. The sheet resistance of the -Ta film was measured using a Hall bar geometry to be , corresponding to a kinetic inductance of pH/.

Figure 8. (a) 2D colour map of background-subtracted GIWAXS 1D scattering profiles for Ta resonators measured at varying incidence angles. The horizontal axis corresponds to the incidence angle (), and the vertical axis shows the momentum transfer (). Intensity is plotted on a logarithmic scale, with darker regions indicating higher scattered intensity. Air background was subtracted using a separately measured reference scan. (b) GIWAXS 2D detector image of the bulk Ta film at incident angle (above the critical angle, . In-plane (IP) scattering is shown on the x-axis (), and out-of-plane (OOP) on the y-axis ().

Figure 9. Bragg peaks with labelled full width half maximum (FWHM) from a background-subtracted GIWAXS scan of a bare Ta film at an incident angle of .
To prepare the wafers for fabrication, 8" Ta-on-Si substrates are coated with 2 m of AZ1512 HS photoresist for protection before dicing into mm chiplets. After dicing, the photoresist is removed by sequential 5 min sonications in acetone and isopropyl alcohol (IPA). Bare Ta chips are then loaded into the load lock chamber of an electron beam evaporator (PLASSYS MEB-550S), which is pumped to a base pressure of mbar for in situ ion milling, Ti deposition, and oxidation.
The native Ta oxide is first removed by 5.5 min of gentle ion beam milling using a Kaufman ion source with low-energy (400 eV) Ar ions at a flux density of 15 mA cm. Without breaking vacuum, an ultrathin ( Å) Ti layer is deposited by electron beam evaporation at 0.2 Å s, followed by in situ oxidation for 10 min in 10 Torr of pure O. This Ti-coated sample is hereafter referred to as Ti/Ta. We emphasise that this method does not require in situ Ta and Ti co-deposition and is compatible with pre-existing Ta films.
For optical lithography, AZ1512 HS photoresist is spin-coated at 6000 RPM for 60 s (yielding 1.4 m thickness), soft-baked at 110 °C for 60 s, and allowed to cool to room temperature. Exposure is performed with a Heidelberg MLA 150 maskless aligner (405 nm laser), followed by a post-exposure bake (110 °C for 60 s). The pattern is developed in AZ726 MIF for 30 s, then rinsed in two successive DI water baths (30 s each). The developed resist serves as the etch mask for subsequent pattern transfer. All samples contain five transmission-line coupled resonators with a CPW width and gap of 9 m and 5 m respectively.
Etching is carried out in an Oxford Instruments PlasmaPro 80 RIE system using CF plasma. Prior to processing, a 20 min chamber pre-clean (50 sccm O, 25 sccm CF, 100 mTorr, 150 W) is performed. The sample is then transferred into the chamber, which is pumped to mbar.
A 10 s O plasma pre-clean (40 sccm O, 100 mTorr, 150 W) removes residual organics. The Ta/Ti film is etched in CF plasma for 20 min at a rate of nm min (30 sccm CF, 20 mTorr, 200 W). Under these conditions, the underlying Si etches at nm min, twice the rate of Ta. Thus, the 200 nm Ta layer is expected to be fully removed in 18 min, with nm of Si trenched in the remaining 2 min. Given that the Ta etch rate may vary by up to nm min, this margin ensures complete removal across all samples. After etching, a 2 min post-clean in O plasma (same parameters) helps remove fluorocarbon etch byproducts, which are known to contribute to TLS loss.[4, 41] Etch completion is verified optically, after which the sample is coated again with AZ1512 HS and diced into individual mm circuits.
To remove the protective photoresist, a 5 min sonication in acetone and IPA is performed. Residual organics and adsorbed fluorocarbons are removed by 5 min O plasma ashing at 200 W RF power in a Diener Atto low-pressure plasma system. Although this step is effective at residue removal, it leaves both Si and Ti/Ta surfaces heavily oxidised (see Supplementary Information). Samples are then vacuum-sealed and transported for post-processing.
Next, a buffered oxide etch (BOE) is used to remove surface oxides and dissolve the 2 Å Ti layer. Samples are transferred directly into a 6:1 BOE solution of NHF:HF for 20 min. After etching, the samples are rinsed in DI water (2 30 s) and sonicated in IPA for 3 min.
Samples are then transferred into the PLASSYS MEB-550S chamber, mounted on a molybdenum (Mo) stage, and pumped overnight to mbar. They are annealed at 700°C for 10 hr, with a ramp rate of °C min, and allowed to cool naturally to 30°C over approximately one day. Following annealing, samples undergo a final 1 min BOE step and rinse (DI water + IPA sonication).
Wire bonding and packaging are completed within 3 hr of the final BOE, minimising air exposure and suppressing regrowth of surface oxides before cryostat loading.

Figure 5. Wiring diagram for two-sample CPW resonator measurements.
Resonator measurements
For device measurement, the wire-bonded and packaged samples are shielded with mu-metal and aluminium cans, and mounted to the mixing chamber flange of a BlueFors SD dilution refrigerator, which reaches a base temperature of mK. Two chips with five resonators each are wire-bonded to a dual-slot PCB, allowing for the measurement of both in a single cooldown. Separate input lines are used for each sample, and a cryogenic microwave switch (Radiall R5927B2141) is used to route output signals. A Keysight P9375A two-port vector network analyser (VNA) was used to measure the complex scattering signals.
Temperature dependent measurements
The sample temperature was controlled via a 100 resistive heater mounted to the same mixing chamber flange as the sample enclosure. A heating power of 4.9 mW was required to raise the flange temperature to approximately 1 K. After each adjustment to the heater current, the flange temperature was given time to stabilise (typically within 1 hour), followed by an additional 1 hour to ensure thermal equilibrium of the sample. After thermalisation, the measurements corresponding to data-points in Figure 6 were performed.

Figure 6. Temperature dependent for four resonators on sample T-LA2. Experimental data is displayed as points with a fitted temperature dependent loss model displayed as solid lines. The power values shown in the legend are the applied powers at the on-chip transmission line, corresponding to a range of average intracavity photon numbers from dBm photons to dBm photons.
XPS
X-ray photoelectron spectroscopy (XPS) measurements were performed on a Kratos AXIS Supra+ system equipped with monochromated Al K (1486.6 eV) with beam spot size of 300 m. XPS chamber base pressure mbar. Survey scans (0 - 1200 eV) and high-resolution scans of the Ta 4f, O 1s, C 1s, and Ti 2p levels were obtained (Figure 7). Samples were grounded by clips and no sample charging was observed. Component analysis was performed in CasaXPS, where peaks were fitted using Gaussian/Lorentzian line-shapes and Shirley background subtraction was used.[42] The Ta 4f peak was fitted with doublet components from metallic Ta and . To use a minimal fitting model that accounts for details seen in angle resolved XPS data across all treatments, we implement an additional doublet at intermediate binding energy to account for suboxide contributions.

Figure 7. High resolution XPS scans of O 1s, Ti 2p, and Ta 4f levels tracking chemical changes for samples treated by: (a) no BOE (bare), (b) 1 min short BOE without annealing (T-S), (c) 20 min long BOE without annealing (T-L), and (d) long BOE with annealing (T-LA). The data shows that the Ti layer remains in place after short BOE, and consists primarily of TiO. The Ti layer is removed by long BOE. The broad shoulder in the Ti 2p data around 468 eV is the Ta 4p. The XPS measurements were taken on samples that underwent identical fabrication processes to those with measured devices in the main text.
GIWAXS
Grazing incidence wide angle X-ray scattering (GIWAXS) data, as shown in Figure 8 and Figure 9, was taken at the NCD-SWEET beamline (ALBA Synchrotron, Barcelona) with an incident X-ray energy of 9.25 keV ( Å) and a beam spotsize FWHM . GIWAXS data was visualised and analysed using Medved software.[43]
References
- [1]C. Wang, C. Axline, Y. Y. Gao, T. Brecht, Y. Chu, L. Frunzio, M. H. Deveret, and R. J. Schoelkopf, “Surface participation and dielectric loss in superconducting qubits,” Applied Physics Letters 107, 162601 (2015).DOI
- [2]G. Calusine, A. Melville, W. Woods, R. Das, C. Stull, V. Bolkhovsky, D. Braje, D. Hover, D. K. Kim, X. Miloshi, D. Rosenberg, A. Sevi, J. L. Yoder, E. Dauler, and W. D. Oliver, “Analysis and mitigation of interface losses in trenched superconducting coplanar waveguide resonators,” Applied Physics Letters 112, 062601 (2018).DOI
- [3]J. M. Martinis, “Surface loss calculations and design of a superconducting transmon qubit with tapered wiring,” npj Quantum Information 8, 26 (2022).DOI
- [4]X. Guo, Z. Degnan, J. A. Steele, E. Solano, B. C. Donose, K. Bertling, A. Fedorov, A. D. Rakić, and P. Jacobson, “Near-Field Localization of the Boson Peak on Tantalum Films for Superconducting Quantum Devices,” The Journal of Physical Chemistry Letters 14, 4892–4900 (2023).DOI
- [5]C. Müller, J. H. Cole, and J. Lisenfeld, “Towards understanding two-level-systems in amorphous solids: Insights from quantum circuits,” Reports on Progress in Physics 82, 124501 (2019).
- [6]W. Woods, G. Calusine, A. Melville, A. Sevi, E. Golden, D. Kim, D. Rosenberg, J. Yoder, and W. Oliver, “Determining Interface Dielectric Losses in Superconducting Coplanar-Waveguide Resonators,” Physical Review Applied 12, 014012 (2019).
- [7]K. D. Crowley, R. A. McLellan, A. Dutta, N. Shumiya, A. P. M. Place, X. H. Le, Y. Gang, T. Madhavan, N. Khedkar, Y. C. Feng, E. A. Umbarkar, X. Gui, L. V. H. Rodgers, Y. Jia, M. M. Feldman, S. A. Lyon, M. Liu, R. J. Cava, A. A. Houck, and N. P. de Leon, “Disentangling Losses in Tantalum Superconducting Circuits,” (2023), arXiv:2301.07848 [cond-mat, physics:quant-ph].DOI
- [8]R. A. McLellan, A. Dutta, C. Zhou, Y. Jia, C. Weiland, X. Gui, A. P. M. Place, K. D. Crowley, X. He, T. Madhavan, Y. Gang, L. Baker, A. R. Head, I. Waluyo, R. Li, K. Kisslinger, A. Hunt, I. Jarrige, S. A. Lyon, A. M. Barbour, R. J. Cava, A. A. Houck, S. L. Hulbert, M. Liu, A. L. Walter, and N. P. de Leon, “Chemical profiles of the oxides on tantalum in state of the art superconducting circuits,” (2023), arXiv:2301.04567 [cond-mat, physics:quant-ph].DOI
- [9]S. G. Wang, Y. Wang, Y. Lu, A. Banerjee, C. U. Lei, L. Krayzman, K. Kisslinger, C. Zhou, R. Li, Y. Jia, M. Liu, L. Frunzio, and R. J. Schoelkopf, “Surpassing millisecond coherence in on chip superconducting quantum memories by optimizing materials and circuit design,” Nature Communications 15, 3687 (2024).DOI
- [10]C. Wang, X. Li, H. Xu, Z. Li, J. Wang, Z. Yang, Z. Mi, X. Liang, T. Su, C. Yang, G. Wang, W. Wang, Y. Li, M. Chen, C. Li, K. Linghu, J. Han, Y. Zhang, Y. Feng, Y. Song, T. Ma, J. Zhang, R. Wang, P. Zhao, W. Liu, G. Xue, Y. Jin, and H. Yu, “Towards practical quantum computers: Transmon qubit with a lifetime approaching 0.5 milliseconds,” npj Quantum Information 8, 3 (2022).DOI
- [11]A. P. M. Place, L. V. H. Rodgers, P. Mundada, B. M. Smitham, M. Fitzpatrick, Z. Leng, A. Premkumar, J. Bryon, A. Vrajitoarea, S. Sussman, G. Cheng, T. Madhavan, H. K. Babla, X. H. Le, Y. Gang, B. Jack, A. Gyenis, N. Yao, R. J. Cava, N. P. de Leon, and A. A. Houck, “New material platform for superconducting transmon qubits with coherence times exceeding 0.3 milliseconds,” Nature Communications 12, 1779 (2021).DOI
- [12]L. Shi, T. Guo, R. Su, T. Chi, Y. Sheng, J. Jiang, C. Cao, J. Wu, X. Tu, G. Sun, J. Chen, and P. Wu, “Tantalum microwave resonators with ultra-high intrinsic quality factors,” Applied Physics Letters 121, 242601 (2022).DOI
- [13]D. P. Goronzy, W. W. Mah, P. G. Lim, T. Guess, S. Majumder, D. A. Garcia-Wietzen, M. J. Walker, J. Ramirez, W.-R. Syong, D. Bennett, M. Vissers, R. dos Reis, T. Pham, V. P. David, M. C. Hersam, M. J. Bedzyk, and C. R. H. McRae, “Comparison of Nb and Ta Pentoxide Loss Tangents for Superconducting Quantum Devices,” (2025), arXiv:2512.05407 [quant-ph].arxiv.org/abs/2512.05407
- [14]P. G. Pritchard and J. M. Rondinelli, “Suppressed paramagnetism in amorphous Ta 2 O 5 - x oxides and its link to superconducting-qubit performance,” Physical Review Applied 23, 064062 (2025).DOI
- [15]M. P. Bland, F. Bahrami, J. G. C. Martinez, P. H. Prestageard, B. M. Smitham, A. Joshi, E. Hedrick, A. Pakpour-Tabrizi, S. Kumar, A. Jindal, R. D. Chang, A. Yang, G. Cheng, N. Yao, R. J. Cava, N. P. de Leon, and A. A. Houck, “2D transmons with lifetimes and coherence times exceeding 1 millisecond,” (2025), arXiv:2503.14798 [quant-ph].arxiv.org/abs/2503.14798
- [16]J. Verjauw, A. Potočnik, M. Mongillo, R. Acharya, F. Mohiyaddin, G. Simion, A. Pacco, Ts. Ivanov, D. Wan, A. Vaneenhlove, L. Souriau, J. Jussot, A. Thiam, J. Swerts, X. Piao, S. Couet, M. Heyns, B. Govoreanu, and I. Radu, “Investigation of Microwave Loss Induced by Oxide Regrowth in High- Q Niobium Resonators,” Physical Review Applied 16, 014018 (2021).DOI
- [17]M. Bal, A. A. Murthy, S. Zhu, F. Crisa, X. You, Z. Huang, T. Roy, J. Lee, D. V. Zanten, R. Pilipenko, I. Nekrashevich, A. Lunin, D. Bafia, Y. Krasnikova, C. J. Kopas, E. O. Lachman, D. Miller, J. Y. Mutus, M. J. Reagor, H. Canzisoglu, J. Marshall, D. P. Pappas, K. Vu, K. Yadavalli, J.-S. Oh, L. Zhou, M. J. Kramer, F. Lecocq, D. P. Goronzy, C. G. Torres-Castanedo, P. G. Pritchard, V. P. Dravid, J. M. Rondinelli, M. J. Bedzyk, M. C. Hersam, J. Zasadzinski, J. Koch, J. A. Sauls, A. Romanenko, and A. Grassellino, “Systematic improvements in transmon qubit coherence enabled by niobium surface encapsulation,” npj Quantum Information 10, 43 (2024).DOI
- [18]D. P. Lozano, M. Mongillo, X. Piao, S. Couet, D. Wan, Y. Canvel, A. M. Vadiraj, T. Ivanov, J. Verjauw, R. Acharya, J. Van Damme, M. A. Fahd, J. Jussot, P. P. Gowda, A. Pacco, B. Raes, J. Van De Vondel, I. Radu, B. Govoreanu, J. Swerts, A. Potočnik, and K. DeGreve, “Low-loss alpha-tantalum coplanar waveguide resonators on silicon wafers: Fabrication, characterization and surface modification,” Materials for Quantum Technology (2024), 10.1088/2633-4356/ad4b8c.
- [19]K. Jacob, C. Shekhar, and Y. Waseda, “An update on the thermodynamics of Ta2O5,” The Journal of Chemical Thermodynamics 41, 748–753 (2009).DOI
- [20]R. D. Chang, N. Shumiya, R. A. McLellan, Y. Zhang, M. P. Bland, F. Bahrami, J. Mun, C. Zhou, K. Kisslinger, G. Cheng, B. M. Smitham, A. C. Pakpour-Tabrizi, N. Yao, Y. Zhu, M. Liu, R. J. Cava, S. Gopalakrishnan, A. A. Houck, and N. P. De Leon, “Eliminating Surface Oxides of Superconducting Circuits with Noble Metal Encapsulation,” Physical Review Letters 134, 097001 (2025).DOI
- [21]M. Alghadeer, A. Banerjee, A. Hajr, H. Hussein, H. Fariborzi, and S. G. Rao, “Surface Passivation of Niobium Superconducting Quantum Circuits Using Self-Assembled Monolayers,” ACS Applied Materials & Interfaces 15, 2319–2328 (2023).DOI
- [22]C. Zhou, J. Mun, Y. Yao, A. kumar Anbalagan, M. D. Hossain, R. A. McLellan, R. Li, K. Kisslinger, G. Li, X. Tong, A. R. Head, C. Weiland, S. L. Hulbert, A. L. Walter, Q. Li, Y. Zhu, P. V. Sushko, and M. Liu, “Ultrathin Magnesium-Based Coating as an Efficient Oxygen Barrier for Superconducting Circuit Materials,” Advanced Materials 36, 2310280 (2024).DOI
- [23]N. C. Wang, E. A. Carrion, M. C. Tung, and E. Pop, “Reducing graphene device variability with yttrium sacrificial layers,” Applied Physics Letters 110 (2017), 10.1063/1.4984090.DOI
- [24]C. A. Joiner, T. Roy, Z. R. Hesabi, B. Chakrabarti, and E. M. Vogel, “Cleaning graphene with a titanium sacrificial layer,” Applied Physics Letters 104 (2014), 10.1063/1.4881886.DOI
- [25]C. E. Murray, “Metallic matters in superconducting qubits,” Materials Science and Engineering: R: Reports 146, 100646 (2021).DOI
- [26]K. Rieger, S. Günzler, M. Spiecker, A. Nambisan, W. Wernsdorfer, and I. M. Pop, “Fano Interference in Microwave Resonator Measurements,” Physical Review Applied 20, 014059 (2023), arXiv:2209.03036 [quant-ph].DOI
- [27]D. Sommers, Z. Degnan, D. Gautam, Y.-H. Chen, C.-C. Chiu, A. Fedorov, and P. Pakkiam, “Open-Source Highly Parallel Electromagnetic Simulations for Superconducting Circuits,” (2025).arxiv.org/abs/2511.01220
- [28]S. Probst, F. B. Song, P. A. Bushev, A. V. Ustinov, and M. Weides, “Efficient and robust analysis of complex scattering data under noise in microwave resonators,” Review of Scientific Instruments 86, 024706 (2015).DOI
- [29]J. Gao, The Physics of Superconducting Microwave Resonators, Ph.D. thesis, California Institute of Technology, (2008).DOI
- [30]S. E. de Graaf, L. Faoro, J. Burnett, A. A. Adamyan, A. Ya. Tzalenchuk, S. E. Kubatkin, T. Lindström, and A. V. Danilov, “Suppression of low-frequency charge noise in superconducting resonators by surface spin desorption,” Nature Communications 9, 1143 (2018).DOI
- [31]D. P. Lozano, M. Mongillo, X. Piao, S. Couet, D. Wan, Y. Canvel, A. M. Vadilraj, T. Ivanov, J. Verjauw, R. Acharya, J. Van Damme, F. A. Mohyaddin, J. Jussot, P. P. Gowda, A. Pacco, B. Raes, J. Van de Vondel, I. P. Radu, B. Govoreanu, J. Swerts, A. Potočnik, and K. De Greve, “Manufacturing high-Q superconducting alpha-tantalum resonators on silicon wafers,” (2022), arXiv:2211.16437 [cond-mat, physics:physics, physics:quant-ph].DOI
- [32]G. Marcaud, D. Perello, C. Chen, E. Umbarkar, C. Weiland, J. Gao, S. Diez, V. Ly, N. Mahuli, N. D’Souza, Y. He, S. Aghaeimeibodi, R. Resnick, C. Jaye, A. K. Rumaiz, D. A. Fischer, M. Hunt, O. Painter, and I. Jarrige, “Low-Loss Superconducting Resonators Fabricated from Tantalum Films Grown at Room Temperature,” (2025), arXiv:2501.09885 [physics].
- [33]W. Ren, G.-D. Yang, A.-L. Feng, R.-X. Miao, J.-B. Xia, and Y.-G. Wang, “Annealing effects on the optical and electrochemical properties of tantalum pentoxide films,” Journal of Advanced Ceramics 10, 704–713 (2021).DOI
- [34]C. Xu, Q. Xiao, J. Ma, Y. Jin, J. Shao, and Z. Fan, “High temperature annealing effect on structure, optical property and laser-induced damage threshold of Ta2O5 films,” Applied Surface Science 254, 6554–6559 (2008).
- [35]Y. Kalboussi, B. Delatte, S. Bira, K. Dembele, X. Li, F. Miserque, N. Brun, M. Walls, J. L. Maurice, D. Dragoje, J. Leroy, D. Longuevergne, A. Gentils, S. Jublot-Leclerc, G. Jullien, F. Ezenou, M. Baudrier, L. Maurice, and T. Proslier, “Reducing two-level systems dissipations in 3D superconducting niobium resonators by atomic layer deposition and high temperature heat treatment,” Applied Physics Letters 124, 134001 (2024).DOI
- [36]J. Van Damme, T.s. Ivanov, P. Favia, T. Conard, J. Verjauw, R. Acharya, D. Perez Lozano, B. Raes, J. Van De Vondel, A. Vadiraj, M. Mongillo, D. Wan, J. De Boeck, A. Potočnik, and K. De Greve, “Argon-Milling-Induced Decoherence Mechanisms in Superconducting Quantum Circuits,” Physical Review Applied 20, 014034 (2023).DOI
- [37]S. Arabi, Q. Li, R. Dhundhwal, D. Fuchs, T. Reisinger, I. M. Pop, and W. Wulfhekel, “Magnetic bound states embedded in tantalum superconducting thin films,” Applied Physics Letters 126, 114001 (2025).
- [38]C. R. H. McRae, H. Wang, J. Gao, M. R. Vissers, T. Brecht, A. Dunsworth, D. P. Pappas, and J. Mutus, “Materials loss measurements using superconducting microwave resonators,” Review of Scientific Instruments 91, 091101 (2020).DOI
- [39]Y. Urade, K. Yakushiji, M. Tsujimoto, T. Yamada, K. Makise, W. Mizubayashi, and K. Nomata, “Microwave characterization of tantalum super conducting resonators on silicon substrate with niobium buffer layer,” APL Materials 12, 021132 (2024).DOI
- [40]D. W. Face and E. Prober, “Nucleation of body-centered-cubic tantalum films with a thin niobium underlayer,” Journal of Vacuum Science & Technology A: Vacuum, Surfaces, and Films 5, 3408–3411 (1987).DOI
- [41]M. Tuokkola, Y. Sunada, H. Kivijärvi, J. Albanese, L. Grönberg, J.-P. Kaikkonen, V. Vesterinen, J. Govenius, and M. Möttönen, “Methods to achieve near-millisecond energy relaxation and dephasing times for a superconducting transmon qubit,” (2025), 10.48550/arXiv.2407.18778, arXiv:2407.18778 [quant-ph].arxiv.org/abs/2407.18778
- [42]N. Fairley, V. Fernandez, M. Richard-Plouet, C. Guillot-Deudon, J. Walton, E. Smith, D. Flahaut, M. Greiner, M. Biesinger, S. Tougaard, D. Morgan, and J. Baltrusaitis, “Systematic and collaborative approach to problem solving using X-ray photoelectron spectroscopy,” Applied Surface Science Advances 5, 100112 (2021).DOI
- [43]D. Chernyshov, V. Dyadkin, W. Van Beek, and A. Urakawa, “Frequency analysis for modulation-enhanced powder diffraction,” Acta Crystallographica Section A Foundations and Advances 72, 500–506 (2016).DOI