Electrical Stability of Cr2O3/\b{eta}-Ga2O3 and NiOx/\b{eta}-Ga2O3 Heterojunction Diodes
Abstract
This work reports the electrical characteristics comparison study between Cr2O3 and NiOx based heterojunction diodes (HJD) on halide vapor phase epitaxy (HVPE) grown \b{eta}-Ga2O3 epitaxial layers. Both as-fabricated Cr2O3 and NiOx HJDs exhibited forward current density in a range of 130-150 A/cm^2 at 5 V with rectifying ratios >10^10 and a reverse leakage current density at 10^-8 A/cm^2 at -5 V. The differential specific on-resistance of Cr2O3 and NiOx HJDs was 12.01 mΩcm^2 and 12.05 mΩcm^2, respectively. Breakdown voltages of Cr2O3 HJDs ranged from 1.4-1.9 kV and 1.5-2.3 kV for NiOx HJDs. Theoretical band alignment between Cr2O3 and \b{eta}-Ga2O3 was calculated from first principles. The ambient exposed NiOx/HVPE \b{eta}-Ga2O3 HJDs forward current density degraded after 10 days while that of Cr2O3/HVPE \b{eta}-Ga2O3 HJDs remained nearly unchanged after the same amount of time. It was later confirmed that the ambient exposed sputtered NiOx sheet resistance (Rsh) degradation gave rise to the reduction of the forward current density of the NiOx based HJDs, and water (H2O) was qualitatively determined to be the agent attributed to the forward conduction degradation by measuring the Rsh of NiOx-on-sapphire reference wafer after exposing it to different environments. The Cr2O3/HVPE \b{eta}-Ga2O3 HJD also exhibited enhanced thermal stability compared to the NiOx/\b{eta}-Ga2O3 heterostructures at elevated temperatures. Interfacial nickel gallate (Ga2NiO4) phase formation expected from phase diagrams can explain the reduced thermal stability of NiOx/\b{eta}-Ga2O3 HJDs. This study indicates that Cr2O3 is a stable p-type oxide for the realization of robust multi-kV \b{eta}-Ga2O3 HJDs.
Introduction
In recent years of wide/ultra-wide bandgap (WBG/UWBG) semiconductor advancements, β- offers promising potential for medium-voltage power applications (1-35 kV) in applications of grid transmission, renewable energy processing, and data centers for artificial intelligence (AI). The high critical electric field strength and availability of the shallow hydrogenic dopants[1] in epitaxial β-[2, 3, 4, 5] can be leveraged to demonstrate power devices with much lower differential specific on-resistance while operating at a higher blocking voltage[6, 7, 8] compared to silicon carbide (SiC) and gallium nitride (GaN)[9, 10]. Although reliable p-type doping with mobile holes in β- is currently unavailable, p-type oxides, such as nickel oxide (NiO), have been integrated with β- to form P-N heterojunctions that readily enable multi-kV junctions[11, 12, 13, 14, 15, 16] with breakdown voltage kV[17, 18, 19] and high electric field at 7.5 MV/[20]. Several materials issues in NiO/-GaO heterojunction-based power devices. For example, instability of sputtered NiO under ambient exposure results in fluctuation of acceptor concentration () in this material, requiring a 15-minute nitrogen () anneal at 275 °C for stabilization[19, 21, 22, 23, 24]. Recently, it was also reported that the NiO/-GaO heterojunction interface is susceptible to secondary nickel gallate (GaNiO) phase formation[25, 26], which affects the thermal stability of the junction characteristics. Stable p-type oxide/-GaO heterojunction diodes with no interfacial phase formation are therefore necessary for reliable applications in -GaO-based power electronics.
Chromium oxide (CrO), a p-type oxide[27] with a bandgap of ~3.6 eV[28, 29], has recently been explored to form P-N heterojunctions[30, 31, 32] with -GaO as an alternative to NiO-based junctions, exhibiting enhanced thermal stability under high temperature environment at 600 °C[32].
In this work, we compared the electrical characteristics of as-fabricated CrO/HVPE -GaO and NiO/HVPE -GaO HJDs. Theoretical band alignment between CrO and -GaO is reported by first-principles calculations. Forward current density of HJDs and oxide sheet resistance variation under ambient exposure were also tracked to compare the material stability. Water vapor (HO) in the air was qualitatively found to be the cause for degradation of the sheet resistance in sputtered NiO exposed to ambient conditions. Temperature-dependent J-V measurements confirmed the enhanced thermal stability of CrO-based HJDs at elevated temperatures. The enhanced thermal stability of CrO/-GaO interface is further corroborated from the absence of a stable ternary phase in the Cr-Ga-O system compared to the GaNiO phase formation at the NiO/-GaO heterojunction interface by comparing their theoretical phase diagrams.
Device Fabrication
The CrO/HVPE -GaO heterojunction diode (HJD) fabrication began with a backside Ti/Au (50/150 nm) Ohmic metallization on n -GaO bulk substrate using e-beam evaporation followed by a 60-seconds rapid thermal annealing (RTA) at 470 °C in . Following the backside Ohmic contact formation, a photoresist lift-off mask was patterned using optical lithography after standard solvent clean (acetone/isopropanol/de-ionized water). Then, a ~20-nm p CrO layer (R ~1 M/□) was directly deposited on the HVPE -GaO via reactive radio frequency (RF) magnetron sputtering by using a 99.95%-pure metallic chromium (Cr) target under an oxygen-deficient condition (Ar/O~22/10 sccm) at a 3.7 mTorr chamber pressure and 150 W RF power. To enhance the Ohmic contact quality to CrO, a ~20-nm p CrO contact layer (R~600 k/□) was sputtered under an oxygen-rich condition (Ar/O~8/10 sccm) at a 3 mTorr chamber pressure and the same RF power. The atomic percentage of Cr (30.6%) and O (69.4%) were confirmed by using energy dispersive spectroscopy (EDS) on reference silicon monitor wafer, closely matching the stoichiometry of CrO reported[30] earlier. Immediately following the sputter deposition, a (50/50/200 nm) metal stack was deposited via e-beam evaporation to serve as an Ohmic contact to and a hard mask for subsequent plasma dry etching[20, 33]. The /Ohmic metal stack was later lifted off in a heated N-methyl pyrrolidone (NMP) solution. To mitigate the electric field crowding, the diodes were dry-etched m below the /- heterojunction interface under inductively coupled plasma at 200 W, as shown in Figure 1(a). This self-aligned plasma-etch served as edge termination for the device. Similarly, the /HVPE - HJDs, as shown in Figure 1(b), were also fabricated on the same wafer by using a sputtering condition of Ar/O sccm at a 3.7 mTorr chamber pressure and 150 W RF power for 20-nm of p ( k/□) and Ar/O sccm at a 3 mTorr chamber pressure and 150 W RF power for 20-nm of p (–9 k/□) by using the identical fabrication process[20, 33]. The layers were sputtered from a 99.999% purity nickel (Ni) metallic target.
Figure 1. (a) /HVPE - heterojunction diode with m plasma-etch edge termination schematics. (b) /HVPE - heterojunction diode with m plasma-etch edge termination schematics.
/- Band Alignment Calculation
We use the electronic transition level of hydrogen to align the band structures.[34] We perform first-principles calculations to locate the (+/−) transition level of interstitial hydrogen in - and corundum . Our calculations are based on the generalized Kohn-Sham theory[35] using the HSE hybrid functional[36] implemented with projector augmented wave (PAW) potentials[37, 38] in the VASP code.[39] In the HSE functional, the mixing parameters are fitted to reproduce experimental band gaps and lattice constants: 34% for - and 18% for corundum . With these parameters, we obtain for - an indirect band gap of 4.81 eV and lattice parameters Å, Å and Å. For corundum CrO we obtain an indirect band gap of 3.45 eV and lattice parameters Å and Å.
We employed 120-atom supercells; for -GaO this corresponds to a multiple of the 20-atom monoclinic conventional cell, and for corundum CrO to a multiple of the 30-atom hexagonal conventional cell. Calculations are performed using a k-point grid and a plane-wave cutoff energy of 500 eV. Spin polarization is included. For an interstitial hydrogen impurity in charge state (), the formation energy is given by40
where is the formation energy of the interstitial hydrogen in charge state , and are the total energies of the defective and pristine supercells, and is the chemical potential of hydrogen. The term accounts for the exchange of electrons with the reservoir, where the Fermi level is referenced to the VBM. represents the finite-size correction for charged supercells, following established schemes.41,42
Due to the monoclinic crystal structure of -GaO, multiple configurations are possible for H and H. In the lowest energy structures, H bonds to a lone pair of three-fold coordinated oxygen atom whereas H relaxes to a site near two Ga atoms within the mirror plane perpendicular to the axis. These configurations yield a (+/−) transition level 0.04 eV above the CBM as shown in Figure 2, in agreement with previous work.43 In corundum CrO, both H and H bond to a four-fold coordinated oxygen atom. In the donor state (H), the four Cr-O bonds elongate by 3%, 4%, 6% and 10%. In the acceptor state H, three Cr-O bonds elongate by 0.5%, 15%, 20% while the fourth shortens by 1%. The resulting (+/−) level is located 0.44 eV below the CBM. In Figure 2, we align the transition level (+/-) of interstitial hydrogen in -GaO and corundum CrO, resulting in a type-II band alignment for the heterojunction, with valence- and conduction-band offsets of eV and eV.

Figure 2. Band alignment between -GaO and corundum CrO. The valence bands are shown in red and the conduction bands in blue. The dashed line indicates the (+/−) transition level of interstitial hydrogen.
-GaO HJDs Electrical Characteristics Analysis
High-Voltage Capacitance-Voltage (C-V) Analysis
The punch-through electric field profile of CrO/-GaO HJDs beyond V was confirmed via high-voltage capacitance–voltage measurements at 1 MHz, as shown in Figure 3(a). The HVPE layer was fully depleted above 600 V reverse bias, where measured capacitance remained flat and no longer changed as a function of applied reverse bias. Moreover, the built-in potential () of the HVPE HJD was extracted to be V from the vs voltage characteristics shown in Figure 3(a) inset, closely matching the extracted from NiO/-GaO HJDs from our early reports[20, 33]. The average HVPE drift layer's apparent charge density was extracted to be cm with a corresponding thickness of m using a relative permittivity of 12.4[44] for (001) -GaO, as shown in Figure 3(b).

Figure 3. (a) High-voltage C–V characteristics on 1-mm area pad at 1 MHz with inset showing the built-in potential of CrO/HVPE β-GaO HJD. (b) Extracted apparent charge density vs depth profile of the plasma-etched CrO/HVPE β-GaO vertical HJD.
J-V & Reverse Breakdown Characteristics
The forward linear J-V characteristics of the CrO/HVPE β-GaO and NiO/HVPE β-GaO HJDs on 100-μm dia. devices are shown in Figure 4(a) by considering a 45°-angle current spreading[33, 45]. Both types of HJDs exhibit comparable on-state current density in a range of 130–150 A/cm at 5 V. The rectifying ratio of both types of HJDs are >10 with a reverse leakage of ~10 A/cm at -5 V and ideality factors of 1.72 and 1.63 for CrO and NiO HJDs, respectively, as shown in Figure 4(b). The minimum differential specific on-resistance of the CrO and NiO-based HJDs are extracted to be 12.01 mΩ•cm and 12.05 mΩ•cm, respectively, as shown in Figure 4(c). The reverse leakage and breakdown characteristics of the HJDs (submerged in FC-40 Fluorinert liquid) on HVPE β-GaO for 100-μm dia. devices are shown in Figure 4(d), showing a breakdown voltage range of 1.4–1.9 kV for CrO/β-GaO HJDs and 1.5–2.3 kV for NiO/β-GaO HJDs with noise-floor reverse leakage current densities (10~10 A/cm, nA) at 80% of the devices’ catastrophic breakdown voltage for both types of HJDs.

Figure 4. (a) Linear J-V characteristics of Cr₂O₃/β-Ga₂O₃ and NiOₓ/HVPE β-Ga₂O₃ HJDs on 100-μm dia. device with a 45°-angle current spreading effect. (b) Semi-log scale J-V characteristics of Cr₂O₃/β-Ga₂O₃ and NiOₓ/HVPE β-Ga₂O₃ HJD on 100-μm dia. device with a 45°-angle current spreading effect. (c) vs. voltage of Cr₂O₃/β-Ga₂O₃ and NiOₓ/HVPE β-Ga₂O₃ HJDs on 100-μm dia. device with a 45°-angle current spreading effect. (d) Reverse breakdown characteristics of Cr₂O₃/β-Ga₂O₃ and NiOₓ/HVPE β-Ga₂O₃ HJD on 100-μm dia. devices.
Electrical Stability under Ambient Conditions & Elevated Temperatures
The J-V characteristics of both as-fabricated Cr₂O₃/β-Ga₂O₃ and NiOₓ/HVPE β-Ga₂O₃ HJDs were tracked as deposited, after 3 days, and after 10 days by exposing samples to the ambient. It was observed that the as-deposited current density of Cr₂O₃ HJD exhibited comparable value with that of NiOₓ HJD at 4 V, as shown in Figure 5(a). After 3 days of ambient exposure, the Cr₂O₃ HJD current density decreased slightly in the vicinity of 120 A/cm² at 4 V similar to what it was as deposited, but the NiOₓ HJD current density significantly dropped below 15 A/cm². After 10 days of ambient exposure, the Cr₂O₃ HJD remained around 120 A/cm² at 4 V while the NiOₓ HJD current density continued to decrease to < 1 A/cm², indicating electrical instability of NiOₓ/HVPE β-Ga₂O₃ HJDs. To identify the cause of this degradation of the HJD’s on-state degradation, Cr₂O₃ and NiOₓ layers were sputtered on sapphire with Ni/Au Ohmic contact for four-point Van Der Pauw measurements. It was observed that the sheet resistance () of the sputtered NiOₓ on sapphire gradually increased to 50% of its original value within 21 days, as shown in Figure 5(b) while the of Cr₂O₃ varied less than 10% of its original value, implying enhanced electrical stability of Cr₂O₃ under ambient exposure compared to NiOₓ. To further investigate the origin of the sheet resistance degradation in sputtered NiOₓ degradation, the NiOₓ on sapphire was exposed to different environments, and the sheet resistance variation was tracked after 72 hours exposure, as shown in Figure 5(c). A metal-organic chemical vapor deposition (MOCVD) reactor with high purity oxygen (O₂, 500 Torr) and nitrogen gas (N₂, 500 Torr) flow was used to expose the sample to N₂ and O₂. It was observed that the of sputtered NiOₓ varied insignificantly within 72 hours when it was placed in pure N₂ and O₂, and the variation was comparable to the case where the reference sputtered NiOₓ on sapphire was sealed in vacuum post deposition. Upon submerging the NiOₓ-on-sapphire sample in de-ionized water (H₂O), the degraded ~10% within 72 hours, which was similar to the extent of degradation when the NiO/AlO was exposed in ambient for the same amount of time. Therefore, it was qualitatively concluded that HO is the agent that potentially causes the degradation in sputtered NiO.

Figure 5. (a) Linear J-V characteristics of CrO/β-GaO and NiO/HVPE β-GaO HJDs tracked as deposited, after 3-day, and after 10-day. (b). Sheet resistance variation of sputtered CrO and NiO on reference sapphire wafers within 30-day. (c) Sheet resistance variation of sputtered NiO under various exposure conditions within 72 hours.
Beyond J-V characterization of ambient exposed CrO HJDs, temperature-dependent J-V characteristics of the HJDs were measured to examine the diodes’ thermal stability under elevated temperatures from 25 °C to 175 °C, as shown in Figure 6(a).

Figure 6. (a) Temperature-dependent J-V characteristics of CrO/HVPE β-GaO HJDs from 25 °C to 175 °C in semi-log scale (left) and linear scale (right). (b) CrO/HVPE β-GaO HJDs on-resistance vs. temperature power law fit.
The temperature-resistance dependent coefficient (α) was extracted from the power law fit of the on-resistance of the HJD as a function of temperatures, as shown in Figure 6(b). The extracted α of the CrO/HVPE β-GaO HJD was lower than that of NiO/HVPE β-GaO HJD (α=1.56)[33] from previous literatures, indicating thermal stability[32] of sputtered CrO relative to NiO. Since the temperature-dependent sweep was carried out 10 days after the diode’s ambient exposure, the NiO/HVPE -GaO HJDs’ on-state characteristics were heavily degraded, and no consistent variation trend was observed.
Ternary (Ga-Ni-O, Ga-Cr-O) Compositional Phase Diagram
To further investigate the thermal instability in NiO/-GaO heterojunction, the ternary compositional phase diagram of Ga-Ni-O and Ga-Cr-O systems generated by The Materials Project[46] database are compared in Figure 7(a) and Figure 7(b), respectively, to examine any interfacial reaction hindering thermal stability of HJDs.
Figure 7. (a) Ternary phase diagram of Ga-Ni-O system. (b) Ternary phase diagram of Ga-Cr-O system.
Experimental observation of nickel gallate (GaNiO)[25, 26] for the NiO/-GaO heterostructure system matches well with the stable phase predicted from the phase diagram. For the Ga-Cr-O system, there is no predicted stable intermediate phase formation at the CrO/-GaO heterojunction, indicating enhanced material system stability.
Conclusion
In summary, this work explored the comparison of electrical performances of NiO/HVPE -GaO and CrO/HVPE -GaO heterojunction diodes. It was discovered that the as-deposited NiO and CrO HJDs exhibited similar electrical characteristics in terms reverse leakage current density, differential specific on-resistance, and breakdown voltages. A type-II band alignment between CrO and -GaO was determined from first-principles calculations. The NiO HJDs’ forward conduction gradually degraded over extended period while the CrO HJDs’ forward conduction remained nearly constant, and HO is qualitatively identified as the agent that caused sheet resistance degradation in ambient exposed sputtered . Temperature dependent J-V characteristics also revealed thermal stability in /HVPE - heterostructures relative to as-fabricated /HVPE - HJDs.
Acknowledgments
The authors acknowledge funding from the U.S. Department of Energy (DOE) ARPA-E ULTRAFAST program (DE-AR0001824) and Coherent/II-VI Foundation Block Gift Program, and SUPREME, one of seven centers in JUMP 2.0, a Semiconductor Research Corporation program sponsored by the Defense Advanced Research Projects Agency. This research also used resources of the National Energy Research Scientific Computing Center, a DOE Office of Science User Facility supported by the Office of Science of the U.S. Department of Energy under Contract No. DE-AC02-05CH11231 using NERSC Award No. BES-ERCAP0028497. A portion of this work was performed at the UCSB Nanofabrication Facility, an open access laboratory.
Data Availability
The data that supports the findings of this study are available from the corresponding authors upon reasonable request.
References
- [1]1 A.T. Neal, S. Mou, S. Rafique, H. Zhao, E. Ahmadi, J.S. Speck, K.T. Stevens, J.D. Blevins, D.B. Thomson, and N. Moser, “Donors and deep acceptors in β-Ga₂O₃,” Applied Physics Letters 113(6), (2018).DOI
- [2]2 A. Bhattacharyya, C. Peterson, K. Chanchaiworawit, S. Roy, Y. Liu, S. Rebollo, and S. Krishnamoorthy, “Over 6 μm thick MOCVD-grown low-background carrier density (10¹⁵ cm⁻³) high-mobility (010) β-Ga₂O₃ drift layers,” Applied Physics Letters 124(1), (2024).DOI
- [3]3 C. Peterson, A. Bhattacharyya, K. Chanchaiworawit, R. Kahler, S. Roy, Y. Liu, S. Rebollo, A. Kallistova, T.E. Mates, and S. Krishnamoorthy, “200 cm²/Vs electron mobility and controlled low 1015 cm - 3 Si doping in (010) β-Ga₂O₃ epitaxial drift layers,” Applied Physics Letters 125(18), (2024).
- [4]4 S. Rebollo, Y. Liu, C. Peterson, S. Krishnamoorthy, and J.S. Speck, “Growth of nitrogen-doped (010) β-Ga₂O₃ by plasma-assisted molecular beam epitaxy using an O₂/N₂ gas mixture,” Applied Physics Letters 126(8), (2025).DOI
- [5]5 C. Peterson, C.N. Saha, R. Kahler, Y. Liu, A. Mattapalli, S. Roy, and S. Krishnamoorthy, “Kilovolt-class β-Ga₂O₃ field-plated Schottky barrier diodes with MOCVD-grown intentionally 1015 cm- 3 doped drift layers,” Journal of Applied Physics 138(18), (2025).DOI
- [6]S. Roy, B. Kostroun, Y. Liu, J. Cooke, A. Bhattacharyya, C. Peterson, B. Sensale-Rodriguez, and S. Krishnamoorthy, “Low QCVF 20A/1.4 kV β-Ga₂O₃ Vertical Trench High-k RESURF Schottky Barrier Diode with Turn-on Voltage of 0.5 V,” IEEE Electron Device Letters, (2024).
- [7]S. Roy, B. Kostroun, J. Cooke, Y. Liu, A. Bhattacharyya, C. Peterson, B. Sensale-Rodriguez, and S. Krishnamoorthy, “Ultra-low reverse leakage in large area kilo-volt class β-Ga₂O₃ trench Schottky barrier diode with high-k dielectric RESURF,” Applied Physics Letters 123(24), (2023).DOI
- [8]“2.34 kV β-Ga₂O₃ vertical trench RESURF Schottky barrier diode with sub-micron fin width | APL Electronic Devices | AIP Publishing,” (n.d.).
- [9]Y. Zhang, and J.S. Speck, “Importance of shallow hydrogenic dopants and material purity of ultra-wide bandgap semiconductors for vertical power electron devices,” Semiconductor Science and Technology 35(12), 125018 (2020).DOI
- [10]B.J. Baliga, Fundamentals of Power Semiconductor Devices (Springer Science & Business Media, 2010).
- [11]J. Wan, H. Wang, C. Zhang, Y. Li, C. Wang, H. Cheng, J. Li, N. Ren, Q. Guo, and K. Sheng, “3.3 kV-class NiO/β-Ga₂O₃ heterojunction diode and its off-state leakage mechanism,” Applied Physics Letters 124(24), (2024).DOI
- [12]H.H. Gong, X.H. Chen, Y. Xu, F.-F. Ren, S.L. Gu, and J.D. Ye, “A 1.86-kV double-layered NiO/β-Ga₂O₃ vertical p–n heterojunction diode,” Applied Physics Letters 117(2), (2020).DOI
- [13]J.-S. Li, C.-C. Chiang, X. Xia, H.-H. Wan, F. Ren, and S.J. Pearton, “7.5 kV, 6.2 GW cm⁻² NiO/β-Ga₂O₃ vertical rectifiers with on–off ratio greater than 10¹³,” Journal of Vacuum Science & Technology A 41(3), (2023).DOI
- [14]J.-S. Li, H.-H. Wan, C.-C. Chiang, T.J. Yoo, F. Ren, H. Kim, and S.J. Pearton, “NiO/Ga₂O₃ Vertical Rectifiers of 7 kV and 1 mm² with 5.5 A Forward Conduction Current,” Crystals 13(12), 1624 (2023).DOI
- [15]M. Xiao, B. Wang, J. Spencer, Y. Qin, M. Porter, Y. Ma, Y. Wang, K. Sasaki, M. Tadjer, and Y. Zhang, “NiO junction termination extension for high-voltage (> 3 kV) Ga₂O₃ devices,” Applied Physics Letters 122(18), (2023).DOI
- [16]F. Zhou, H. Gong, M. Xiao, Y. Ma, Z. Wang, X. Yu, L. Li, L. Fu, H.H. Tan, Y. Yang, F.-F. Ren, S. Gu, Y. Zheng, H. Lu, R. Zhang, Y. Zhang, and J. Ye, “An avalanche-and-surge robust ultrawide-bandgap heterojunction for power electronics,” Nat Commun 14(1), 4459 (2023).DOI
- [17]J.-S. Li, H.-H. Wan, C.-C. Chiang, T.J. Yoo, M.-H. Yu, F. Ren, H. Kim, Y.-T. Liao, and S.J. Pearton, “Breakdown up to 13.5 kV in NiO/β-Ga₂O₃ vertical heterojunction rectifiers,” ECS Journal of Solid State Science and Technology 13(3), 035003 (2024).DOI
- [18]Y. Qin, Z. Yang, H. Gong, A.G. Jacobs, J. Spencer, M. Porter, B. Wang, K. Sasaki, C.-H. Lin, and M. Tadjer, “10 kV, 250°C Operational, Enhancement-Mode Ga₂O₃ JFET with Charge-Balance and Hybrid-Drain Designs,” in 2024 IEEE International Electron Devices Meeting (IEDM), (IEEE, 2024), pp. 1–4.DOI
- [19]Y. Qin, M. Xiao, M. Porter, Y. Ma, J. Spencer, Z. Du, A.G. Jacobs, K. Sasaki, H. Wang, and M. Tadjer, “10-kV Ga₂O₃ charge-balance Schottky rectifier operational at 200° C,” IEEE Electron Device Letters 44(8), 1268–1271 (2023).DOI
- [20]Y. Liu, S.M. Witsell, J.F. Conley, and S. Krishnamoorthy, “Orientation-dependent β-Ga₂O₃ heterojunction diode with atomic layer deposition (ALD) NiO,” Applied Physics Letters 127(12), (2025).DOI
- [21]Y. Qin, M. Xiao, R. Zhang, Q. Xie, T. Palacios, B. Wang, Y. Ma, I. Kravchenko, D.P. Briggs, and D.K. Hensley, “1 kV GaN-on-Si quasi-vertical Schottky rectifier,” IEEE Electron Device Letters 44(7), 1052–1055 (2023).DOI
- [22]Y. Ma, Y. Qin, M. Porter, J. Spencer, Z. Du, M. Xiao, B. Wang, Y. Wang, A.G. Jacobs, H. Wang, M. Tadjer, and Y. Zhang, “Wide-Bandgap Nickel Oxide with Tunable Acceptor Concentration for Multidimensional Power Devices,” Adv Elect Materials 11(1), 2300662 (2025).
- [23]Y. Qin, M. Porter, M. Xiao, Z. Du, H. Zhang, Y. Ma, J. Spencer, B. Wang, Q. Song, and K. Sasaki, “2 kV, 0.7 mΩ• cm² Vertical Ga₂O₃ Superjunction Schottky Rectifier with Dynamic Robustness,” in 2023 International Electron Devices Meeting (IEDM), (IEEE, 2023), pp. 1–4.DOI
- [24]M. Xiao, Y. Ma, Z. Du, Y. Qin, K. Liu, K. Cheng, F. Udrea, A. Xie, E. Beam, and B. Wang, “First demonstration of vertical superjunction diode in GaN,” in 2022 International Electron Devices Meeting (IEDM), (IEEE, 2022), pp. 35–6.DOI
- [25]K. Egbo, E.M. Garrity, W.A. Callahan, C. Chae, C.-W. Lee, B. Tellekamp, J. Hwang, V. Stevanovic, and A. Zakutayev, “NiGa₂O₄ interfacial layers in NiO/Ga₂O₃ heterojunction diodes at high temperature,” Appl. Phys. Lett. 124(17), 173512 (2024).arxiv.org/abs/2401.06924
- [26]D.S. Yu, L. Meng, V.G. Tripathi, V. Vangiparuk, C. Chae, J. Hwang, and H. Zhao, “Metal–organic chemical vapor deposition of p-type NiO and NiO/β-Ga₂O₃ PN diodes,” APL Electronic Devices 1(4), (2025).DOI
- [27]M.T. Greiner, M.G. Helander, W.-M. Tang, Z.-B. Wang, J. Qiu, and Z.-H. Lu, “Universal energy-level alignment of molecules on metal oxides,” Nature Materials 11(1), 76–81 (2012).DOI
- [28]S. Ghosh, M. Baral, R. Kamparath, R.J. Choudhary, D.M. Phase, S.D. Singh, and T. Ganguli, “Epitaxial growth and interface band alignment studies of all oxide α-Cr₂O₃/β-Ga₂O₃ pn heterojunction,” Applied Physics Letters 115(6), (2019).DOI
- [29]H. Mashiko, T. Oshima, and A. Ohtomo, “Band-gap narrowing in α-(CrₓFe₁₋ₓ)₂O₃ solid-solution films,” Applied Physics Letters 99(24), (2011).
- [30]C. Su, H. Zhou, Z. Hu, C. Wang, Y. Hao, and J. Zhang, “1.96 kV p-Cr₂O₃/β-Ga₂O₃ heterojunction diodes with an ideality factor of 1.07,” Appl. Phys. Lett. 126(13), 132104 (2025).DOI
- [31]Y. Feng, H. Zhou, J. Ma, H. Fang, X. Zhang, Y. Chen, G. Tian, J. Yuan, R. Peng, S. Xu, Y. Hao, and J. Zhang, “120 A/1.78 kV p-Cr₂O₃/n-β-Ga₂O₃ Heterojunction PN Diodes With Slanted Mesa Edge Termination,” IEEE Electron Device Letters 46(10), 1705–1708 (2025).DOI
- [32]W.A. Callahan, K. Egbo, C.-W. Lee, D. Ginley, R. O’Hayre, and A. Zakutayev, “Reliable operation of Cr₂O₃:Mg/ β-Ga₂O₃ p–n heterojunction diodes at 600 °C,” Appl. Phys. Lett. 124(15), 153504 (2024).DOI
- [33]Y. Liu, S. Roy, C. Peterson, A. Bhattacharyya, and S. Krishnamoorthy, “Ultra-low reverse leakage NiOₓ/β-Ga₂O₃ heterojunction diode achieving breakdown voltage> 3 kV with plasma etch field-termination,” AIP Advances 15(1), (2025).DOI
- [34]C.G. Van De Walle, and J. Neugebauer, “Universal alignment of hydrogen levels in semiconductors, insulators and solutions,” Nature 423(6940), 626–628 (2003).pubmed.ncbi.nlm.nih.gov/12789334
- [35]W. Kohn, and L.J. Sham, “Self-Consistent Equations Including Exchange and Correlation Effects,” Phys. Rev. 140(4A), A1133–A1138 (1965).DOI
- [36]J. Heyd, G.E. Scuseria, and M. Ernzerhof, “Erratum: ‘Hybrid functionals based on a screened Coulomb potential’ [J. Chem. Phys. 118, 8207 (2003)],” The Journal of Chemical Physics 124(21), 219906 (2006).
- [37]P.E. Blöchl, “Projector augmented-wave method,” Phys. Rev. B 50(24), 17953–17979 (1994).pubmed.ncbi.nlm.nih.gov/9976227
- [38]G. Kresse, and D. Joubert, “From ultrasoft pseudopotentials to the projector augmented-wave method,” Phys. Rev. B 59(3), 1758–1775 (1999).DOI
- [39]G. Kresse, and J. Furthmüller, “Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set,” Phys. Rev. B 54(16), 11169–11186 (1996).pubmed.ncbi.nlm.nih.gov/9984901
- [44]A. Fiedler, R. Schewski, Z. Galazka, and K. Irmscher, “Static dielectric constant of β-Ga2O3 perpendicular to the principal planes (100),(010), and (001),” ECS Journal of Solid State Science and Technology 8(7), Q3083 (2019).
- [45]S. Roy, A. Bhattacharyya, C. Peterson, and S. Krishnamoorthy, “2.1 kV (001)-β-Ga2O3 vertical Schottky barrier diode with high-k oxide field plate,” Applied Physics Letters 122(15), (2023).DOI
- [46]A. Jain, S.P. Ong, G. Hautier, W. Chen, W.D. Richards, S. Dacek, S. Cholia, D. Gunter, D. Skinner, G. Ceder, and K.A. Persson, “Commentary: The Materials Project: A materials genome approach to accelerating materials innovation,” APL Mater. 1(1), 011002 (2013).DOI