WorksPhysics and Astronomy
Laser-Synthesized Amorphous PdSe Nanoparticles: A Defect-Rich Platform for High-Efficiency SERS, Photocatalysis, and Photothermal Conversion
Abstract
The control of material properties at the atomic scale remains a central challenge in materials science. Transition metal dichalcogenides (TMDCs) offer remarkable electronic and optical properties, but their functionality is largely dictated by their stable crystalline phases. Here we demonstrate a single-step, ligand-free strategy using femtosecond laser ablation in liquid to transform crystalline, stoichiometric palladium diselenide (PdSe) into highly stable, amorphous, and non-stoichiometric nanoparticles (PdSe, with x1). This laser-driven amorphization creates a high density of selenium vacancies and coordinatively unsaturated sites, which unlock a range of emergent functions absent in the crystalline precursor, including plasmon-free surface-enhanced Raman scattering with an enhancement factor exceeding 10, a 50-fold increase in photocatalytic activity, and near-infrared photothermal conversion efficiency reaching 83. Our findings establish laser-induced amorphization as a powerful top-down approach for defect-engineered TMDCs and advances their practical usage in optics, catalysis, and nanomedicine.
Introduction
The "materials by design" paradigm largely relies on effective synthesis routes and the ability to manipulate the atomic structure to unlock novel or enhanced functionalities for energy, photonics, and medicine. Two-dimensional () van der Waals (vdW) materials [1, 2], particularly transition metal dichalcogenides (TMDCs), became an outstanding platform for the concept realization, offering highly tunable electronic [3, 4], optical [5], and mechanical [6, 7] properties.
Recently, platinum group metal chalcogenides, e.g., Pd, Pt, and Rh, have attracted attention as promising materials in catalysis [8], electronic semiconducting devices [9] and thin film absorbers for solar panels [10]. A distinctive feature of platinum group metals is the filled or nearly filled d orbital, leading to the (semi)metallic behavior of their chalcogenides and a high electrical conductivity.
Among these, palladium diselenide () stands out due to its unusual puckered pentagonal lattice structure, in-plane optical anisotropy [11] and high air stability [12] making it a promising candidate for near-infrared optoelectronics [13, 14, 15] and catalysis. Interestingly, most of the Pd-Se studies are concentrated in electrocatalysis [16, 17, 18, 19], whereas only a few are devoted to SERS applications [20, 21, 22]. The reason for it are quite moderate enhancement factors (EF) due to the chemical (non-plasmonic) SERS mechanism of the crystalline , far below the EF routinely obtained with plasmonic nanostructures. An interesting approach for SERS improvement is a defect engineering [21] in bilayer nanosheets by keeping the overall structure, however, predominantly crystalline. In this context, the material properties are still largely dictated by its thermodynamically stable, ordered crystalline forms, including [23], [16], [24], [23]. This crystalline constraint inspires a question: what new properties could be accessed in the amorphous counterpart of the material? The abundance of - systems indicated above suggests the existence of a stable amorphous phase of palladium selenide with inherently high density of defects and coordinatively unsaturated sites. Such a material should possess excellent SERS and catalytic performance at the coordinatively unsaturated surface. The primary obstacle, however, is the synthesis and stabilization of these amorphous TMDC phases, because conventional bottom-up (CVD) and top-down (liquid-phase exfoliation) approaches are optimized for crystallinity. Thus, a method capable of driving a material far from its thermodynamic equilibrium is required to access and stabilize these metastable amorphous states.
Here, we introduce femtosecond pulsed laser ablation in liquid (PLAL) as a unique material processing tool to overcome this challenge. Using PLAL we show that an ordered, stoichiometric crystalline target can be controllably converted into a stable, disordered, non-stoichiometric, and highly functional amorphous nanomaterial, . The obtained nanoparticles offer significant advantages over conventional planar plasmon-free substrates due to the synergetic combination of mechanisms: a large coordinatively unsaturated surface, defect-state energy levels for improved charge transfer and plasmon-free hotspots in nanoparticle aggregates. In contrast to the reported amorphization in "wet" chemistry, we use a non-demanding, simple one-step method that does not require a glovebox with an inert atmosphere [25] or high temperatures [26] with lengthy stirring. In addition, the proposed method allows direct manufacturing scaling via a continuous-flow reactor [27].
Results and discussion
Structural analysis of palladium selenide nanoparticles and flakes
Figure 1 outlines the structural properties of nanoparticles, synthesized via femtosecond laser ablation in DI water (refer to the Methods section for detailed information). A high-purity () commercial crystal (SixCarbon Technology Co., Limited, Shenzhen) is used as a target and a single precursor for pulsed laser nanoparticle synthesis, see Figure 1a,Figure 1b. Micron-sized flakes (Figure 1c), produced via the ultrasound-assisted liquid phase exfoliation method [28], preserve the crystallinity of the bulk source, which is confirmed by diffraction rings in SAED and high-resolution TEM images in Figure 1c. The measured lattice constants , agree well with the experimental values and DFT calculations (, $b = 5.87 Å) [5, 12, 29]. In contrast, the nanoparticles produced via pulsed laser ablation demonstrate an amorphous structure (Figure 1d): a single-particle SAED demonstrates amorphous halos, different from those of TEM amorphous carbon film. In addition, the nanoparticles have abrupt edges without an onionlike shell typically found in crystalline TMDC NPs [30].

Figure 1. (a) Photograph of crystal used as a target and its crystal structure, the unit cell is denoted as a dashed box; (b) Schematic view of PLAL; (c) From left to right: typical TEM image and SAED of flakes, and a high-resolution TEM photograph of a zoomed area of a single flake proving its crystalline structure; (d) From left to right: typical TEM image and SAED of nanoparticles, and a zoomed TEM image of a single nanoparticle edge; (e) Raman spectra of bulk crystal, crystalline flakes and amorphous nanoparticles; (f) Photographs of colloids separated by centrifugation at different rotation speeds; (g) Size distributions and average sizes of nanoparticles, obtained at different rotational speeds and measured by counting on TEM image.
Raman spectroscopy (Figure 1e) provides further evidence of the NPs amorphous state, in contrast to both bulk crystal and flakes. The Raman spectra of the latter samples exhibit all characteristic vibrational modes of [31, 21, 32], as shown in Figure 1e. The spectra have strong, well-defined peaks at 142 and 256 , which are assigned to the and Raman-active modes, respectively. Furthermore, we observe two distinct modes at 203 () and 220 (), consistent with previous reports. The identical Raman features observed in both the initial crystal and derived flakes confirm their common crystalline structure, ruling out amorphous phase formation during the flake preparation process.
The Raman spectrum of NPs exhibits broad overlapping bands that contrast sharply with the well-defined peaks of distinct vibrational modes observed in crystalline samples (Figure 1e). The absence of discrete Raman modes in nanoparticles reflects structural disorder: broken translational symmetry broadens vibrational bands, while non-stoichiometric bonding (Pd:Se about 1:1) suppresses zone-center phonons detectable in crystalline .
For the photothermal conversion tests (see § 2.2), several size fractions of the originally synthesized colloid were obtained via the differential centrifugation method [33], see § 4.1 for details. Interestingly, the darkest solution was obtained after 1000 rpm (Figure 1f), suggesting the highest concentration of NPs with a mean size 40 nm in the synthesized colloid. We obtained mean NPs sizes from 51 nm down to 11 nm at different rotation speeds, as shown in Figure 1g.
The synthesized nanoparticles PdSe₂₋ₓ are expected to have pronounced catalytic and Raman enhancement properties in light of recent studies of amorphization-induced electronic transport [34, 35, 36, 37]. In this regard, stoichiometric analysis is required to understand the type and concentration of active sites/vacancies. The EDX spectra of the flakes, prepared via ultrasound-assisted exfoliation, yield an approximate 1:2 Pd-to-Se ratio for with a minor content of O, see Figure 2a. A slight oxidation likely appears during the storage of the prepared flakes in DI water. In contrast, amorphous nanoparticles exhibit noticeably stronger oxidation and have almost equal amounts of Pd and Se atoms (see Figure 2b), which resembles NPs [23]. A significant fraction of incorporated oxygen leads to a high concentration of defects in the nanoparticles, compared to the crystalline flakes. The presence of defects is also revealed via photoluminescence (PL) measurements. As shown in Figure 2c, crystalline flakes have PL spectra with no peaks below the wavelength of 600 nm under excitation at wavelengths of 350-410 nm. It agrees with the minimal energy of 0.9 eV for direct optical transitions in bulk crystalline [38], which increases up to 1.1-1.3 eV for monolayer flakes [39, 21]. It leads to the infrared interband recombination and PL peak at nm [21]. In contrast, the amorphous NPs have a slight PL signal in the visible range (Figure 2c). The signal maximum shifts towards larger wavelengths together with excitation wavelengths because of the excitation of various defect states inside the nanoparticles.

Figure 2. a),b) EDX of (a) flakes of PdSe₂ and (b) nanoparticles of PdSe₂₋ₓ with TEM photographs in the insets; c) Photoluminescence spectra of PdSe₂ flakes (grey region) and PdSe₂₋ₓ nanoparticles (red, green and blue regions) acquired at excitation wavelengths of 350 nm, 380 nm and 410 nm; d),e) XPS characterization of bulk crystal PdSe₂ for (d) Pd 3d and (e) Se 3d, with shirley baseline fitted spectra; f), g) XPS characterization of PLAL-synthesized PdSe₂₋ₓ NPs for (f) Pd 3d and (g) Se 3d, with Shirley baseline fitted spectra.
For catalytic applications and Raman scattering enhancement, surface defects play a major role. In this regard, in addition to the EDX analysis of particle volume, we performed XPS surface analysis, see Figure 2d-Figure 2g. For crystalline , the binding energies of (341.97 eV), (336.69 eV ), and binding energies of (54.84 eV) and (55.64 eV) are consistent with the reported values [40]. In amorphous NPs the core-level peaks of Pd and Se show a uniform shift toward lower binding energies compared to those of the pristine ; this effect is attributed to the Fermi level lowering upon p-type doping, consistent with previous reports on p-type doping of TMDCs [41]. Notably, new distinct binding energy peaks associated with Pd 3d core levels at 343.70 eV and 337.90 eV () and Se 3d core levels at 58.50 eV appear after femtosecond ablation, indicating the formation of Pd-O and Se-O bonds [42, 21]. The ratio on the surface of nanoparticles is 1:1.2, which is close to the EDX data 1:1.1 (see the insets in Figure 2b,Figure 2f). However, a sufficiently large amount of Se-O (see Supplementary Note 1) indicates the appearance of Se- and O-saturated Se vacancies, preferential for catalytic and Raman-enhanced properties.
Photothermal properties of palladium selenide nanoparticles
Photothermal therapy (PTT) is an emerging nanomedicine approach due to the adaptation of novel materials and attempts to perform a combined therapeutic effect. Sub-100 nm NPs are known to be required for their accumulation in tumors due to the enhanced permeability and retention (EPR) effect [43]. A variety of materials, shapes and hybrid systems have recently been proposed to enhance the photothermal performance of nanoagents in NIR [44, 43, 45, 46, 47, 48, 49, 50, 51, 53, 54, 55] [52]. Figure 3a summarizes the experimental findings of these works, paying attention to the measured photothermal conversion efficiency (PCE) and the size of photothermal agents. Metallic and semimetallic systems appear to cover wider ranges of both metrics compared to semiconducting and polymer NPs. PCE calculations (see Supplementary Note 2) for sub-100 nm spherical nanoparticles made of conventional (Si, Au, TiN) and novel (MXene , TMDC and others) materials for NIR-I wavelength 830 nm allow their classification from low- to high PCE, see Figure 3b. Among others, crystalline nanoparticles demonstrate one of the highest PCE in a size range, easily achievable via femtosecond laser ablation. Although the synthesized NPs are amorphous, they retain high photothermal efficiency both in absolute value (measured for the average NP size of 38 nm) and in comparison with NPs obtained via femtosecond laser ablation of other materials, see Figure 3c. All NPs were dispersed in DI water and PCE was measured under 830 nm illumination. Analogously to Figure 3b, we performed PCE tests for NPs with different average size fractions, obtained via differential centrifugation (see § 2.1 for details). Smaller NPs scatter less light, which increases their PCE from 72% for the average size 51 nm up to 82% for the average size 11 nm, see Figure 3d. In contrast to the theoretically predicted PCE curves for crystalline and NPs (see Supplementary Note 3 for refractive index data), the experimental PCE curve for NPs asymptotically tends to the value at the zero size limit; it could be caused by NP agglomeration. Nevertheless, the experimentally measured PCE approves the suitability of amorphous for highly efficient photothermal agents in NIR-I transparency window.

Figure 3. Photothermal conversion efficiency (PCE) analysis of nanoparticle systems: (a) Literature survey comparing reported PCE values for various materials versus photothermal agent size; (b) Calculated PCE for sub-100 nm spherical nanoparticles of conventional (Si, Au, TiN) and emerging (MXene TiC, TMDC MoS) materials at 830 nm (NIR-I window); (c) Experimental PCE values for femtosecond-laser-ablated PdSe nanoparticles compared with other materials (TiN, Au, WSe, Si); (d) Theoretical PCE for crystalline PdSe and PdSe nanoparticles versus experimental results for amorphous PdSe as a function of particle diameter.
Palladium Diselenide Flakes and Nanoparticles for SERS
SERS activity analysis of synthesized nanoparticles and flakes performed using a series of dyes: rhodamine 6G (Rh6G), rhodamine B (RhB), crystal violet (CV) and methyl orange (MO) with concentrations ranging from to M. Representative Raman peaks for the entire set of dyes were identified. The Raman spectra of Rh6G molecules obtained from the substrates show prominent peaks at approximately 612, 772, 1127, 1186, 1310, 1360, 1505, 1573, and 1649 under 532 nm excitation. These peaks align well with previously reported Raman spectra of Rh6G [56, 57]. The SERS spectra of crystal violet obtained with 633 nm excitation clearly show characteristic Raman bands at 425, 916, 802, 1175, 1375, and 1619 , consistent with data from the literature [58]. Under 532 nm excitation, the most intense Raman peaks were observed at 622, 1198, 1279, 1358, 1506, 1529, and 1646 , which are characteristic of RhB [59, 44, 60].
The most representative SERS spectra, which were measured with crystal violet on a NP-based substrate, are shown in Figure 4a. As anticipated, the SERS intensity decreased progressively with lower dye concentrations. At concentrations as low as M for NP-based substrates, dye peaks remained detectable within the 400 to 1700 range, although with reduced intensity (see Figure 4a). This indicates that the limit of detection (LOD) of the NP-based substrates was M. Similar LOD values were also achieved for Rh6G, RhB and MO.

Figure 4. (a) SERS spectra of CV acquired using PdSe NP-based substrates; b),c) Enhancement factors (EF) calculated for NP-based PdSe (b) and flake-based PdSe (c) substrates across all tested dyes; (d) Measured photoluminescence spectra of M CV on glass substrate, SERS spectrum of NP-based PdSe/ CV and flake-based PdSe/ CV.
Recent studies [21, 20] have confirmed the high efficiency of SERS sensors utilizing structures, reporting LOD values ranging from to M. These findings underscore the potential of -based substrates for sensitive SERS applications.
To evaluate the performance of SERS of both substrate types, we determined the enhancement factor (EF) defined as , where and are the signal intensities from SERS and conventional Raman measurements, respectively, and and represent the analyte concentrations corresponding to these intensity measurements. The calculated enhancement factors for each substrate are presented in Figure 4b, Figure 4c and summarized in Table 1.
| Dye concentrations | Crystal Violet | Rhodamine B | Rhodamine 6G | Methyl Orange |
| 1617 cm | 1649 cm | 607 cm | 1113 cm / 1139 cm | |
| M | 170 | 100 | 620 | 10 / 10 |
| M | 1550 | 890 | 5330 | 40 / 50 |
| M | 7130 | 1660 | 14200 | 300 / 280 |
| M | 23930 | 3680 | 57210 | 2150 / 2520 |
| M | 147290 | 25410 | 60110 | ND / ND |
| M | 1226420 | 111570 | ND | ND / ND |
Table 1. SERS enhancement factors for PdSe nanoparticles at varying dye concentrations. "ND" (Not detectable) symbols indicate values below the detection limit.
The results demonstrate that PdSe NPs can serve as effective SERS substrates, enabling the detection of dyes at low concentrations ( M) with EF reaching as high as . In contrast, crystalline PdSe flakes are significantly less effective, requiring higher dye concentrations ( − M) for detection with EF ∼ − , depending on the specific dye. These results correlate with previous reports [20, 21, 31].
The origin of the exceptionally high enhancement factor of observed for CV on PdSe nanoparticle substrates is a combination of synergistic effects that go beyond the traditional chemical mechanism (CM) of SERS enhancement. CM typically provides EFs in the range of – [61], so the significantly higher enhancement seen in this system arises from several interconnected processes. One key factor is the resonant charge transfer between CV molecules and PdSe nanoparticles, facilitated by the alignment of energy levels. When illuminated, electrons from the dye’s molecular orbitals can efficiently transfer to the conduction band of PdSe, creating a charge-transfer complex that dramatically increases Raman scattering cross-sections [20, 21, 62].
The unique electronic structure of PdSe plays a crucial role in this enhancement. Unlike conventional plasmonic metals, PdSe possesses a tunable optical bandgap that can be engineered to match the electronic transitions of target molecules such as CV. This energy matching creates optimal conditions for resonant enhancement, where both the incident laser light and the Raman scattered photons interact strongly with the charge-transfer states. Furthermore, the two-dimensional nature of PdSe NPs provides a large surface area with numerous active sites for molecular adsorption, which further amplifies the signal.
Defects and nanostructural features on the PdSe substrate also con tribute significantly to the observed enhancement [21, 63, 64]. Selenium vacancies and edge sites in the nanoparticles create localized electronic states that act as efficient charge traps [65]. These defect sites not only facilitate charge transfer processes but may also generate localized electromagnetic hotspots through dielectric confinement effects. The nanoscale roughness and particle aggregation create electromagnetic field enhancements similar to those observed in traditional plasmonic systems, despite the absence of conventional plasmon resonance in [21].
The combination of these effects – resonant charge transfer, defect-mediated enhancement, and nanoscale field concentration – creates a multiplicative effect that explains the unusually high EF values [66]. This is particularly evident in the fluorescence quenching shown in Figure 4d, where the suppression of radiative decay may be attributed to efficient charge transfer. The result is a system where Raman signals are dramatically enhanced, while fluorescence is minimized, creating ideal conditions for sensitive SERS detection [21].
The lower enhancement factor observed for flakes () (see Figure 4c) compared to nanoparticles () can be attributed to several key structural and morphological differences. Unlike the amorphous nanoparticles, the flakes possess a well-ordered crystalline structure with a much lower number of defects and vacancies. While this crystalline perfection is advantageous for many electronic applications, it actually hinders SERS performance by limiting the availability of active sites for dye adsorption and charge transfer processes [62].
The nanoparticles’ amorphous nature, with their abundant defects and non-stoichiometric composition (), creates numerous favorable sites for molecular interaction and charge transfer enhancement [62]. In contrast, stoichiometric flakes () possess fewer broken Se bonds on the surface compared to the nanoparticles. Missing Se atoms in the nanoparticle structure create vacancies that serve as ideal anchoring points for dye molecules such as crystal violet. The more perfect surface of the flakes, while structurally superior, lacks these natural adsorption sites, making it more difficult for dye molecules to attach and participate in the charge transfer processes that amplify SERS signals. This difference in surface chemistry directly impacts the efficiency of the chemical enhancement mechanism.
The morphological differences between the flakes and the nanoparticles also play a significant role. The two-dimensional, planar structure of the flakes offers a much smaller specific surface area compared to that of the three-dimensional nanoparticles. This reduced surface area means that fewer sites are available for dye adsorption, further limiting the overall enhancement.
Fluorescence quenching, which is so prominent in the nanoparticle samples, is also less pronounced in the flake structures (see Figure 4d). The reduced defect density and different surface chemistry of the flakes result in less effective competition between charge transfer pathways and radiative decay processes. This explains why the fluorescence background is more noticeable in flake-based SERS measurements compared to that of nanoparticle samples, where charge transfer dominates the relaxation pathways.
The variation in SERS signals observed for different dyes (Rh6G, RhB, CV, and MO) on NP-based substrates stems from a combination of molecular adsorption, charge transfer efficiency, and resonance effects. Planar aromatic dyes like Rh6G, RhB, and CV exhibit stronger SERS signals due to their ability to -stack efficiently with the surface, facilitated by Se vacancies that act as preferential adsorption sites [67]. Crystal violet shows particularly strong enhancement owing to its triple aromatic ring system and N-dimethyl groups that enable multi-point binding to Pd sites, while Rh6G and RhB benefit from favorable energy alignment of the lowest unoccupied molecular orbital with the substrate’s conduction band, enabling resonant charge transfer under typical excitation wavelengths. In contrast, methyl orange’s non-planar structure and sulfonate group hinder effective adsorption and charge transfer, resulting in weaker signals [68]. The amorphous nature of the nanoparticles further enhances these effects through defect-mediated mechanisms: Se vacancies create mid-gap states that selectively boost dye-specific charge transfer when electronic transitions align with the laser excitation. Additionally, dye aggregation plays a role; Rh6G’s tendency to form J-aggregates on nanoparticle surfaces creates localized electromagnetic hotspots even without plasmonic effects.
These differences highlight how molecular structure dictates interaction strength with the substrate, where planar, electron-rich dyes with compatible energy levels achieve optimal enhancement through combined chemical and defect-assisted mechanisms. The substrate’s selectivity for specific dye architectures suggests potential for tailored sensing applications, where the SERS response could be engineered by controlling the nanoparticle defect density and surface chemistry to target particular molecular features.
These findings suggest that careful engineering of two-dimensional material substrates could open new possibilities for ultra-sensitive molecular detection beyond the limitations of conventional SERS platforms [60, 69, 70].
Photocatalytic activity of palladium selenide nanoparticles and flakes
Figure 5 provides a comprehensive analysis of the photocatalytic activity of amorphous nanoparticles and flakes in the degradation of methylene blue (MB) under simulated solar irradiation (100 mW/cm, AM 1.5G).

Figure 5. (a) UV–visible absorption spectra of nanoparticles and flakes; (b) The dependence of the normalized MB concentration () on irradiation time for both catalysts; (c) Fitting of versus time.
Figure 5a displays the UV-Vis absorption spectra for both materials. The amorphous nanoparticles, at a concentration of 0.022 mg/mL, exhibit a broad absorption band extending into the visible region, attributed to defect states induced by selenium vacancies. These defects enhance solar energy capture, which is crucial for photocatalysis under visible light. In contrast, flakes, at a much higher concentration of 0.66 mg/mL, show a sharper absorption edge, typical of their crystalline structure and bandgap absorption, with minimal defect contribution.
Figure 5b illustrates the dependence of the normalized MB concentration () on irradiation time for both catalysts. Despite their lower concentration, nanoparticles achieve fast MB degradation within 12 minutes, while the flakes, with a 30-fold higher concentration, require more time to reach a comparable level of degradation. The rapid degradation by the nanoparticles underscores their superior efficiency per unit mass, highlighting the impact of morphology and defect states.
Figure 5 confirms the pseudo-first-order kinetics of MB degradation through linear dependencies of on time. The calculated rate constants are for the nanoparticles and for the flakes. These values reveal the nanoparticles’ enhanced photocatalytic efficiency, even at a significantly lower concentration. Normalizing the rate constants by concentration further emphasizes this disparity: the nanoparticles exhibit two orders of magnitude higher specific activity (/concentration) of approximately , compared to for the flakes—a 50-fold higher efficiency per unit mass. This can be attributed to the nanoparticles’ increased surface area, improved charge transfer dynamics due to defects, and the stronger light absorption. Overall, the data highlight the critical role of morphology, defect structure, and concentration in determining the photocatalytic performance of . Amorphous nanoparticles not only demonstrate broader light absorption but also achieve significantly higher degradation rates under visible light, even at a fraction of the concentration of the flakes. These findings suggest that optimizing material morphology and defect engineering can substantially enhance the photocatalytic efficiency, opening prospects for the practical application of in sustainable technologies, such as water purification.
Conclusion
In conclusion, we introduced PLAL as a material processing tool for fabrication of stable amorphous nanomaterials () from the crystalline target. The synthesized nanoparticles achieve a record-high for CV and for RhB, what exceeds the crystalline flakes by more than an order of magnitude. The measured photocatalytic activity of NPs demonstrates a 50-fold higher efficiency per unit mass, which is attributed to the nanoparticles’ increased surface area, improved charge transfer dynamics due to defects, and stronger light absorption. Interestingly, the nanoparticles inherit strong optical absorption of the crystalline precursor. Their high photothermal conversion up to puts them on par with recognized highly efficient photoheating agents made of TiN and . Our findings establish amorphous NPs as a promising multipurpose platform for plasmon-free sensing, photocatalysis and photoheating applications.
Experimental Section
Nanoparticles synthesis via femtosecond laser ablation
PdSe nanoparticles were synthesized via pulsed laser ablation in liquid (PLAL) using a femtosecond laser. A bulk PdSe crystal served as the ablation target. In the PLAL process, the target material absorbs laser pulse energy through nonlinear optical processes, leading to plasma plume formation and subsequent confinement within a cavitation bubble. The subsequent bubble growth and collapse dynamics strongly depend on the surrounding liquid properties (i.e., liquid density, heat capacity and conductivity, boiling point), defines the plasma condensation rate and, consequently, the resulting NPs content and crystallinity.
The ytterbium-doped potassium gadolinium tungstate (Yb:KGW) laser system (TETA-10, Avesta, Moscow, Russia) was used as a source of femtosecond pulses (wavelength 1030 nm, pulse duration 270 fs, repetition rate 1 kHz); the pulse energy for PLAL was set at 100 µJ. A synthetic bulk PdSe crystal (dimensions: mm, SixCarbon Technology Co., Limited, ShenZhen) was used as the ablation target and the source of the crystalline flakes. The ultrasonic-assisted liquid phase exfoliation method [28] was employed for PdSe flakes production. Under this approach, the probe tip sonicator (CL-18 benchtop ultrasonic processor, Qsonica L.L.C., Newtown, USA) delivers ultrasonic energy (100 W for 4 hours) directly to the bulk crystal fragment, weighted in advance to get a mass concentration of 2 mg/ml.
For the pulsed laser ablation process, a bulk PdSe crystal was placed at the bottom of a glass cuvette filled with 2 ml of deionized water as the ablation medium. The laser beam was focused on the target surface using a 100-mm focal lens, creating a spot diameter of µm. To ensure uniform ablation across the target, the cuvette was translated in a mm area using two motorized stages (scan speed: 5 mm/s), thereby exposing the entire crystal surface to the laser. The pulse energy was fixed at 100 µJ, corresponding to a fluence of J/cm at the focal spot. A series of PLAL experiments were conducted by varying the distance between the focal plane and the crystal surface. In each trial, the ablation was limited to 15 minutes. Within minutes of irradiation, the solution developed a visible tint, confirming the successful generation of PdSe nanoparticles.
After laser ablation, colloid remained stable and did not show visible changes in color for at least a month. The samples were stored in closed 2 ml Eppendorf microcentrifuge tubes at to prevent contamination or evaporation.
To narrow the size distribution of the synthesized NPs, we employed differential centrifugation. The nanoparticle colloid was centrifuged (Eppendorf centrifuge 5424 R, Hamburg, Germany) at progressively increasing speeds from 500 to 4000 rpm, enabling separation by size.
Sample characterization
Microscopy and energy-dispersive X-ray spectroscopy
Nanoparticle colloids were characterized by the high-resolution TEM system (JEOL JEM 2100, Japan) with an acceleration voltage of 200 kV. 2-µl drops of sample colloids were drop-casted on carbon-coated TEM copper grids and dried under ambient conditions.
A scanning SEM system (MAIA 3; Tescan) with an integrated EDX detector (X-act; Oxford Instruments) was used to examine a bulk crystal surface before and after ablation.
Photoluminescence spectroscopy
Photoluminescence spectroscopy was performed on colloidal suspensions of flakes and nanoparticles using a BioTek Synergy H4 Hybrid Multi-Mode Microplate Reader (BioTek Instruments, Inc., Vermont, USA). Spectra were acquired at room temperature under controlled excitation conditions.
X-ray photoelectron spectroscopy
We analyzed the surface composition and optical band gap of both bulk crystals and synthesized nanoparticles using X-ray photoelectron spectroscopy (XPS). Measurements were performed with a Theta Probe instrument (Thermo Scientific) under high-vacuum conditions, employing a monochromatic Al-K X-ray source (1486.6 eV). All spectra were recorded in fixed analyzer transmission mode with a pass energy of 50 eV, and the spectrometer energy scale was meticulously calibrated using the Au line at 84.0 eV. The XPS spectra for , and were measured along with the spectra of the valence bands. For nanoparticle characterization, samples were prepared by depositing 1 mL of the NP solution onto silicon substrates, followed by drying under ambient conditions.
Photothermal studies
Photoheating experiments were performed with a tunable titanium-sapphire laser source at a NIR-I wavelength of 830 nm. The temperature dynamics was monitored in real time using a calibrated HIKMICRO M10 thermal imaging camera. Colloidal extinction was measured using transmission through a cuvette with deionized water as a baseline.
Raman spectroscopy and SERS
For surface-enhanced Raman spectroscopy (SERS) measurements, 2 µl of sample colloids were drop casted onto an aluminum surface and spin-coated to form thin films. The prepared SERS substrates were then coated with 2 µl of dye solutions at various concentrations ranging from – M and allowed to dry under ambient conditions for 1 hour. Raman spectroscopy was carried out using a Horiba LabRAM HR Evolution system equipped with excitation wavelengths of 532 and 633 nm, a diffraction grating of 600 lines/mm, and a microscope objective with a numerical aperture (NA) of 0.9. The measurements demonstrated good spectral reproducibility.
Photocatalytic Studies
Preparation of photocatalytic Suspensions
Amorphous nanoparticles were synthesized and dispersed in deionized water to form a stable colloidal suspension. The suspension was adjusted to a concentration of 0.022 mg/mL and combined with a 20 mg/L methylene blue solution (Sigma-Aldrich, purity 98%) in quartz tubes. For comparative studies, flakes were prepared at a concentration of 0.66 mg/mL in identical MB solutions. All chemicals were used as received without further purification.
Photocatalytic experiments
To ensure adsorption–desorption equilibrium, the suspensions were stirred continuously at 500 rpm in the dark for 30 minutes at using a magnetic stirrer. Photocatalytic degradation was initiated by exposing the suspensions to simulated solar irradiation generated by a solar simulator (Numi Technology ESS-500-a, , AM 1.5G spectrum). The light intensity was calibrated using a silicon reference cell. The reaction mixtures were constantly stirred to ensure uniform irradiation and mass transfer.
Sample analysis
At designated time intervals (0, 2, 4, 6, 8, and 12 minutes), 1 mL aliquots were taken from the reaction mixture and immediately centrifuged at 15000 rpm for 10 minutes (Eppendorf 5424R centrifuge) to separate the nanoparticles. The supernatant was carefully decanted and analyzed using a UV-Vis spectrophotometer (Agilent Cary 5000) to measure the absorbance of MB at its characteristic peak of 665 nm. The photodegradation efficiency was calculated as the ratio of MB concentration at time () to the initial concentration at adsorption equilibrium (), based on the Lambert–Beer law.
Kinetic analysis
The kinetics of MB photodegradation were modeled using a pseudo-first-order rate equation: , where is the apparent rate constant (min) and is the irradiation time (min). Experimental data were fitted to determine the rate constants and assess the photocatalytic performance of the PdSe nanoparticles and flakes. All experiments were performed in triplicate and the results were reported as mean values with standard deviations.
Acknowledgments
The authors acknowledge Alexander Ushkov for the graphical illustration of the PLAL setup.
Conflicts of Interest
The authors declare no conflict of interest.
Author Contributions
A.A. conceived the idea, supervised the project and edited the manuscript. A.U. designed and performed the experiments and wrote the manuscript. D.D. performed the experiments. N.B. conducted the characterizations, performed the experiments and wrote the manuscript. I.M. designed and performed the experiments and wrote the manuscript. A.S. conducted the TEM/SAED characterizations. D.T. performed the experiments. G.E., S.V.B. and R.I.R. conducted characterizations. I.K. performed DFT simulations. A.A.P., A.C. and S.N. provided experimental resources. A.D.B., G.I.T., A.V.K. and V.V. supervised the project. A.A.V. supervised the project and edited the manuscript. All authors discussed the results. All authors have read and agreed to the published version of the manuscript.
Data Availability Statement
The data that support the findings of this study are available from the corresponding author upon reasonable request.
Supporting Information
Abbreviations
The following abbreviations are used in this manuscript:
| Abbreviation | Meaning |
| vdW | Van der Waals |
| DI water | Deionized water |
| TMDC | Transition Metal Dichalcogenide |
| NP | Nanoparticle |
| PLAL | Pulsed Laser Ablation in Liquid |
| DFT | Density functional theory |
| SEM | Scanning Electron Microscope |
| TEM | Transmission Electron Microscope |
| SAED | Selected Area Electron Diffraction |
| EDX | Energy-dispersive X-ray spectroscopy |
| PL | Photoluminescence |
| XPS | X-Ray Photoelectron Spectroscopy |
| SERS | Surface-Enhanced Raman Scattering |
| LOD | Limit of Detection |
| EF | Enhancement factor |
| Rh6G | Rhodamine 6G |
| RhB | Rhodamine B |
| MO | Methyl Orange |
| CV | Crystal Violet |
| MB | Methylene Blue |
| NA | Numerical Aperture |
| EPR | Enhanced Permeability and Retention |
| PCE | Photothermal Conversion Efficiency |
Table 2.
References
- [1]D. L. Duong, S. J. Yun, Y. H. Lee, van der waals layered materials: opportunities and challenges, ACS nano 11 (12) (2017) 11803–11830.DOI
- [2]Y. Gogotsi, B. Anasori, The rise of mxenes, in: MXenes, Jenny Stanford Publishing, 2023, pp. 3–11.
- [3]M. F. Hossen, S. Shendokar, S. Aravamudhan, Defects and defect engineering of two-dimensional transition metal dichalcogenide (2d tmdc) materials, Nanomaterials 14 (5) (2024) 410.DOI
- [4]A. Falin, M. Holwill, H. Lv, W. Gan, J. Cheng, R. Zhang, D. Qian, M. R. Barnett, E. J. Santos, K. S. Novoselov, et al., Mechanical properties of atomically thin tungsten dichalcogenides: Ws2, wse2, and wte2, ACS nano 15 (2) (2021) 2600–2610.DOI
- [5]J. Sun, H. Shi, T. Siegrist, D. J. Singh, Electronic, transport, and optical properties of bulk and mono-layer pdse2, Applied Physics Letters 107 (15) (2015).DOI
- [6]Y. Qi, M. A. Sadi, D. Hu, M. Zheng, Z. Wu, Y. Jiang, Y. P. Chen, Recent progress in strain engineering on van der waals 2d materials: Tunable electrical, electrochemical, magnetic, and optical properties, Advanced Materials 35 (12) (2023) 2205714.DOI
- [7]Z. Huang, Z. He, Y. Zhu, H. Wu, A general theory for the bending of multilayer van der waals materials, Journal of the Mechanics and Physics of Solids 171 (2023) 105144.DOI
- [8]D. Saraf, S. Chakraborty, A. Kshirsagar, R. Ahuja, In pursuit of bifunctional catalytic activity in pds2 pseudo-monolayer through reaction coordinate mapping, Nano Energy 49 (2018) 283–289.DOI
- [9]L. Zeng, D. Wu, J. Jie, X. Ren, X. Hu, S. P. Lau, Y. Chai, Y. H. Tsang, Van der waals epitaxial growth of mosaic-like 2d platinum ditelluride layers for room-temperature mid-infrared photodetection up to 10.6 μm, Advanced materials 32 (52) (2020) 2004412.
- [10]A. D. Alfieri, M. J. Motala, M. Snure, J. Lynch, P. Kumar, H. Zhang, S. Post, T. Bowen, C. Muratore, J. A. Robinson, et al., Ultrathin broadband metasurface superabsorbers from a van der waals semimetal, Advanced Optical Materials 11 (4) (2023) 2202011.arxiv.org/abs/2208.13269
- [11]Y. Gu, H. Cai, J. Dong, Y. Yu, A. N. Hoffman, C. Liu, A. D. Oyedele, Y.-C. Lin, Z. Ge, A. A. Puretzky, et al., Two-dimensional palladium diselenide with strong in-plane optical anisotropy and high mobility grown by chemical vapor deposition, Advanced Materials 32 (19) (2020) 1906238.
- [12]A. D. Oyedele, S. Yang, L. Liang, A. A. Puretzky, K. Wang, J. Zhang, P. Yu, P. R. Pudasaini, A. W. Ghosh, Z. Liu, et al., Pdse2: pentagonal two-dimensional layers with high air stability for electronics, Journal of the American Chemical Society 139 (40) (2017) 14090–14097.DOI
- [13]Q. Liang, Q. Wang, Q. Zhang, J. Wei, S. X. Lim, R. Zhu, J. Hu, W. Wei, C. Lee, C. Sow, et al., High-performance, room temperature, ultra-broadband photodetectors based on air-stable pdse2, Advanced Materials 31 (24) (2019) 1807609.DOI
- [14]L.-H. Zeng, D. Wu, S.-H. Lin, C. Xie, H.-Y. Yuan, W. Lu, S. P. Lau, Y. Chai, L.-B. Luo, Z.-J. Li, et al., Controlled synthesis of 2d palladium diselenide for sensitive photodetector applications, Advanced Functional Materials 29 (1) (2019) 1806878.
- [15]Y. Wang, J. Pang, Q. Cheng, L. Han, Y. Li, X. Meng, B. Ibarlucea, H. Zhao, F. Yang, H. Liu, et al., Applications of 2d-layered palladium diselenide and its van der waals heterostructures in electronics and optoelectronics, Nano-Micro Letters 13 (1) (2021) 143.DOI
- [16]Z. Hu, N. Yang, Y. Feng, L. Xu, C. Hu, H. Liu, S. Tian, J. Yang, Synthesis of unconventional pd–se nanoparticles for phase-dependent ethanol electrooxidation, Chemical Communications 59 (27) (2023) 4020–4023.DOI
- [17]S. Kukunuri, K. Naik, S. Sampath, Effects of composition and nanostructuring of palladium selenide phases, pd 4 se, pd 7 se 4 and pd 17 se 15, on orr activity and their use in mg–air batteries, Journal of Materials Chemistry A 5 (9) (2017) 4660–4670.DOI
- [18]Z. Lin, B. Xiao, Z. Wang, W. Tao, S. Shen, L. Huang, J. Zhang, F. Meng, Q. Zhang, L. Gu, et al., Planar-coordination pdse2 nanosheets as highly active electrocatalyst for hydrogen evolution reaction, Advanced Functional Materials 31 (32) (2021) 2102321.DOI
- [19]Y. Qin, W. Zhang, F. Wang, J. Li, J. Ye, X. Sheng, C. Li, X. Liang, P. Liu, X. Wang, et al., Extraordinary p–d hybridization interaction in heterostructural pd-pdse nanosheets boosts c- c bond cleavage of ethy- lene glycol electrooxidation, Angewandte Chemie International Edition 61 (16) (2022) e202200899.
- [20]Z. Lei, X. Zhang, Y. Zhao, A. Wei, L. Tao, Y. Yang, Z. Zheng, L. Tao, P. Yu, J. Li, Enhanced raman scattering on two-dimensional palladium diselenide, Nanoscale 14 (11) (2022) 4181–4187.DOI
- [21]T. Jena, M. T. Hossain, U. Nath, M. Sarma, H. Sugimoto, M. Fujii, P. Giri, Evidence for intrinsic defects and nanopores as hotspots in 2d pdse2 dendrites for plasmon-free sers substrate with a high enhancement factor, npj 2D Materials and Applications 7 (1) (2023) 8.DOI
- [22]X. Zhang, Z. Lei, Z. Pan, J. Hu, L. Tao, Z. Zheng, X. Feng, J. Xue, L. Tao, Y. Zhao, A general approach to hybrid platform of au nanoparticles on monolayer semiconductor for ultrasensitive raman enhancement of 2d materials and molecule detection, Journal of Alloys and Compounds 938 (2023) 168468.DOI
- [23]K. Ibrahim, K. C. Matthews, M. Coupin, J. H. Warner, Phase engineering of palladium selenide using chalcogen flux control, Chemistry of Materials 34 (22) (2022) 9982–9988.DOI
- [24]V. V. Singh, G. K. Rao, A. Kumar, A. K. Singh, Palladium (ii)–selenoether complexes as new single source precursors: First synthesis of pd 4 se and pd 7 se 4 nanoparticles, Dalton transactions 41 (4) (2012) 1142–1145.DOI
- [25]B. Wu, X. Liu, P. Liu, G. Wu, L. Tian, X. Han, J. Li, X. Hong, Synthesis of amorphous metal oxides via a crystalline to amorphous phase transition strategy, Nature Synthesis (2025) 1–10.DOI
- [26]Z. Yu, S. Lv, Q. Yao, N. Fang, Y. Xu, Q. Shao, C.-W. Pao, J.-F. Lee, G. Li, L.-M. Yang, et al., Low-coordinated pd site within amorphous palladium selenide for active, selective, and stable h2o2 electrosynthesis, Advanced Materials 35 (6) (2023) 2208101.DOI
- [27]M. Wu, X. Li, D.-F. Yin, W. Chen, J. Qi, M. Hu, J. Xu, Y. Cheng, Real-time spectroscopic monitoring of continuous-flow synthesis of zinc oxide nano-structures in femtosecond laser fabricated 3d microfluidic microchannels with integrated on-chip fiber probe array, Lab on a Chip 23 (17) (2023) 3785–3793.DOI
- [28]P. Chavalekvirat, W. Hirunpinyopas, K. Deshsorn, K. Jitapunkul, P. Iamprasertkun, Liquid phase exfoliation of 2d materials and its electrochemical applications in the data-driven future, Precision Chemistry 2 (7) (2024) 300–329.DOI
- [29]C. Soulard, X. Rocquefelte, P.-E. Petit, M. Evain, S. Jobic, J.-P. Itié, P. Munsch, H.-J. Koo, M.-H. Whangbo, Experimental and theoretical investigation on the relative stability of the pds2-and pyrite-type structures of pdse2, Inorganic chemistry 43 (6) (2004) 1943–1949.
- [30]G. I. Tselikov, G. A. Ermolaev, A. A. Popov, G. V. Tikhonowski, D. A. Panova, A. S. Taradin, A. A. Vyshnevy y, A. V. Syuy, S. M. Klimen-tov, S. M. Novikov, et al., Transition metal dichalcogenide nanospheres for high-refractive-index nanophotonics and biomedical theranostics, Proceedings of the National Academy of Sciences 119 (39) (2022) e2208830119.
- [31]T. Jena, G. Choudhary, M. T. Hossain, U. Nath, M. Sarma, P. Giri, Salt-catalyzed directed growth of bilayer palladium diselenide (pdse2) dendrites and pd nanoparticle-decorated pdse2–pd2se3 junction exhibiting very high surface enhanced raman scattering sensitivity, Chemistry of Materials 36 (12) (2024) 5922–5934.DOI
- [32]O. Abdul-Aziz, D. Wolverson, C. J. Sayers, E. Carpene, F. Parmigiani, H. Hedayat, P. H. van Loosdrecht, Resonance-induced anomalies in temperature-dependent raman scattering of pdse 2, Journal of Materials Chemistry C 12 (30) (2024) 11402–11411.
- [33]M. A. Livshits, E. Khomyakova, E. G. Evtushenko, V. N. Lazarev, N. A. Kulemin, S. E. Semina, E. V. Generozov, V. M. Govorun, Isolation of exosomes by differential centrifugation: Theoretical analysis of a commonly used protocol, Scientific reports 5 (1) (2015) 17319.DOI
- [34]Z. Zheng, S. Cong, W. Gong, J. Xuan, G. Li, W. Lu, F. Geng, Z. Zhao, Semiconductor sers enhancement enabled by oxygen incorporation, Nature communications 8 (1) (2017) 1993.DOI
- [35]S. Cong, Y. Yuan, Z. Chen, J. Hou, M. Yang, Y. Su, Y. Zhang, I. Li, Q. Li, F. Geng, et al., Noble metal-comparable sers enhancement from semiconducting metal oxides by making oxygen vacancies, Nature communications 6 (1) (2015) 7800.DOI
- [36]I. V. Chepkasov, V. S. Baidyshev, A. V. Iosimovska, I. S. Zamulin, A. G. Kvashnin, Adsorption properties of crystalline and amorphous pdir nanoparticles. a systematic first-principles study, Journal of Catalysis (2025) 116102.DOI
- [37]Q. Fu, L. W. Wong, F. Zheng, X. Zheng, C. S. Tsang, K. H. Lai, W. Shen, T. H. Ly, Q. Deng, J. Zhao, Unraveling and leveraging in situ surface amorphization for enhanced hydrogen evolution reaction in alkaline media, Nature communications 14 (1) (2023) 6462.DOI
- [38]V. Volkov, A. Slavich, G. Ermolaev, N. Pak, D. Grudinin, K. Kravtsov, M. Tatmyshevskiy, V. Semkin, A. Syuy, A. Mazitov, et al., All-in-one van der waals material for light detection, guiding and modulation, Research Square [Preprint] (11 March 2025) Available from: https://doi.org/10.21203/rs.3.rs-6156048/v1.
- [39]M. Wei, J. Lian, Y. Zhang, C. Wang, Y. Wang, Z. Xu, Layer-dependent optical and dielectric properties of centimeter-scale pdse2 films grown by chemical vapor deposition, npj 2D Materials and Applications 6 (1) (2022) 1.
- [40]A. N. Hoffman, Y. Gu, L. Liang, J. D. Fowlkes, K. Xiao, P. D. Rack, Exploring the air stability of pdse2 via electrical transport measurements and defect calculations, npj 2D Materials and Applications 3 (1) (2019) 50.DOI
- [41]G. Zhou, J. Ji, Z. Chen, J. Shuai, Q. Liang, Q. Zhang, Scalable electronic and optoelectronic devices based on 2d tmds, Materials Futures 3 (4) (2024) 042701.DOI
- [42]Q. Liang, Q. Zhang, J. Gou, T. Song, Arramel, H. Chen, M. Yang, S. X. Lim, Q. Wang, R. Zhu, et al., Performance improvement by ozone treatment of 2d pdse2, ACS nano 14 (5) (2020) 5668–5677.DOI
- [43]C. Ayala-Orozco, C. Urban, M. W. Knight, A. S. Urban, O. Neumann, S. W. Bishnoi, S. Mukherjee, A. M. Goodman, H. Charron, T. Mitchell, et al., Au nanomatryoshkas as efficient near-infrared photothermal transducers for cancer treatment: benchmarking against nanoshells, ACS nano 8 (6) (2014) 6372–6381.
- [44]A. Ushkov, D. Dyubo, N. Belozerova, I. Kazantsev, D. Yakubovsky, A. Syuy, G. V. Tikhonowski, D. Tselikov, I. Martynov, G. Ermolaev, et al., Tungsten diselenide nanoparticles produced via femtosecond ablation for sers and theranostics applications, Nanomaterials 15 (1) (2024) 4.DOI
- [45]X. Li, L. Liu, S. Li, Y. Wan, J.-X. Chen, S. Tian, Z. Huang, Y.-F. Xiao, X. Cui, C. Xiang, et al., Biodegradable π-conjugated oligomer nanoparticles with high photothermal conversion efficiency for cancer theranostics, Acs Nano 13 (11) (2019) 12901–12911.DOI
- [46]Y. Jiang, X. Duan, J. Bai, H. Tian, D. Ding, Y. Geng, Polymerization-induced photothermy: A non-donor-acceptor approach to highly effective near-infrared photothermal conversion nanoparticles, Biomaterials 255 (2020) 120179.DOI
- [47]J. Zhou, Z. Lu, X. Zhu, X. Wang, Y. Liao, Z. Ma, F. Li, Nir photothermal therapy using polyaniline nanoparticles, Biomaterials 34 (37) (2013) 9584–9592.DOI
- [48]J.-W. Xiao, S.-X. Fan, F. Wang, L.-D. Sun, X.-Y. Zheng, C.-H. Yan, Porous pd nanoparticles with high photothermal conversion efficiency for efficient ablation of cancer cells, Nanoscale 6 (8) (2014) 4345–4351.DOI
- [49]D. Xi, M. Xiao, J. Cao, L. Zhao, N. Xu, S. Long, J. Fan, K. Shao, W. Sun, X. Yan, et al., Nir light-driving barrier-free group rotation in nanoparticles with an 88.3% photothermal conversion efficiency for photothermal therapy, Advanced Materials 32 (11) (2020) 1907855.DOI
- [50]X.-M. Zhu, H.-Y. Wan, H. Jia, L. Liu, J. Wang, Porous pt nanoparticles with high near-infrared photothermal conversion efficiencies for photothermal therapy, Advanced Healthcare Materials 5 (24) (2016) 3165–3172.DOI
- [51]J. Song, F. Wang, X. Yang, B. Ning, M. G. Harp, S. H. Culp, S. Hu, P. Huang, L. Nie, J. Chen, et al., Gold nanoparticle coated carbon nanotube ring with enhanced raman scattering and photothermal conversion F. Ye, A. Ayub, R. Karimi, S. Wettig, J. Sanderson, K. P. Musselman, Defect-rich mose2 2h/1t hybrid nanoparticles prepared from femtosec-ond laser ablation in liquid and their enhanced photothermal conversion efficiencies, Advanced Materials 35 (30) (2023) 2301129.
- [53]S.-F. Pan, W.-X. Xia, W.-L. Feng, L. Ma, S.-J. Ding, X.-B. Chen, Enhanced photothermal conversion in res2/bi2se3 nanoflowers for solar-driven thermoelectric power generation and water evaporation, Journal of Alloys and Compounds 1020 (2025) 179390.
- [54]H. Xie, M. Liu, B. You, G. Luo, Y. Chen, B. Liu, Z. Jiang, P. K. Chu, J. Shao, X.-F. Yu, Biodegradable bi2o2se quantum dots for photoacous-tic imaging-guided cancer photothermal therapy, Small 16 (1) (2020) 1905208.DOI
- [55]W. Feng, L. Chen, M. Qin, X. Zhou, Q. Zhang, Y. Miao, K. Qiu, Y. Zhang, C. He, Flower-like pegylated mos2 nanoflakes for near-infrared photothermal cancer therapy, Scientific reports 5 (1) (2015) 17422.DOI
- [56]K. E. Jebakumari, N. Murugasenapathi, T. Palanisamy, Engineered two-dimensional nanostructures as sers substrates for biomolecule sensing: A review, Biosensors 13 (1) (2023) 102.DOI
- [57]Q. Lv, J. Tan, Z. Wang, L. Yu, B. Liu, J. Lin, J. Li, Z.-H. Huang, F. Kang, R. Lv, Femtomolar-level molecular sensing of monolayer tung-sten diselenide induced by heteroatom doping with long-term stability, Advanced Functional Materials 32 (34) (2022) 2200273.DOI
- [58]J. Bonse, S. V. Kirner, J. Krüger, Laser-induced periodic surface struc-tures (lipss), Handbook of laser micro-and nano-engineering (2020) 1–59.
- [59]M. J. Becher, J. Jagosz, C. Bock, A. Ostendorf, E. L. Gurevich, Formation of low-and high-spatial frequency laser-induced periodic surface structures (lipsss) in ald-deposited mos2, Frontiers in Nanotechnology 5 (2023) 1227025.DOI
- [60]X. N. He, Y. Gao, M. Mahjouri-Samani, P. Black, J. Allen, M. Mitchell, W. Xiong, Y. Zhou, L. Jiang, Y. Lu, Surface-enhanced raman spectroscopy using gold-coated horizontally aligned carbon nanotubes, Nanotechnology 23 (20) (2012) 205702.DOI
- [61]B. N. J. Persson, K. Zhao, Z. Zhang, Chemical contribution to surface-enhanced raman scattering, Physical review letters 96 (20) (2006) 207401.pubmed.ncbi.nlm.nih.gov/16803204
- [62]J. Kang, F. Li, Z. Xu, X. Chen, M. Sun, Y. Li, X. Yang, L. Guo, How amorphous nanomaterials enhanced electrocatalytic, sers, and mechanical properties, JACS Au 3 (10) (2023) 2660–2676.DOI
- [63]D. Majumdar, 2d material-based surface-enhanced raman spectroscopy platforms (either alone or in nanocomposite form)- from a chemical enhancement perspective, ACS omega 9 (38) (2024) 40242–40258.DOI
- [64]N. Zhao, Y. Jin, G. Chen, A. Zhu, Y. Zhang, W. Xie, Metallic and semiconductor nanomaterials for surface-enhanced raman spectroscopy, Chemical Communications (2025).DOI
- [65]G. Xu, R. Dong, D. Gu, H. Tian, L. Xiong, Z. Wang, W. Wang, Y. Shao, W. Li, G. Li, et al., Selenium vacancies and synergistic effect of near-and far-field-enabled ultrasensitive surface-enhanced raman-scattering-active substrates for malaria detection, The Journal of Physical Chemistry Letters 13 (6) (2022) 1453–1463.DOI
- [66]A. Berestennikov, H. Hu, A. Tittl, Molecular spectroscopies with semiconductor metasurfaces: towards dual optical/chemical sers, Journal of Materials Chemistry C 13 (23) (2025) 11499–11514.DOI
- [67]M. V. Canamares, C. Chenal, R. L. Birke, J. R. Lombardi, Dft, sers, and single-molecule sers of crystal violet, The Journal of Physical Chemistry C 112 (51) (2008) 20295–20300.DOI
- [68]H. Laguna, S. Loera, I. A. Ibarra, E. Lima, M. A. Vera, V. Lara, Azoic dyes hosted on hydrotalcite-like compounds: Non-toxic hybrid pigments, Microporous and Mesoporous Materials 98 (1-3) (2007) 234–241.DOI
- [69]S. Sil, N. Kuhar, S. Acharya, S. Umapathy, Is chemically synthesized graphene ‘really’ a unique substrate for sers and fluorescence quenching?, Scientific Reports 3 (1) (2013) 3336.DOI
- [70]H. Watanabe, N. Hayazawa, Y. Inouye, S. Kawata, Dft vibrational calculations of rhodamine 6g adsorbed on silver: analysis of tip-enhanced raman spectroscopy, The Journal of Physical Chemistry B 109 (11) (2005) 5012–5020.pubmed.ncbi.nlm.nih.gov/16863161