High Thermoelectric Cooling Performance of Junction Thermoelectric Transistors

Abstract

To achieve high performance thermoelectric materials and devices, thermoelectric transistors, which integrate thermoelectric effects with transistor technology, represent a promising approach. Here p type Bi0.5Sb1.5Te3 and n type Bi2Te2.97Se0.03 are used as the constituent materials for an NPN transistor. By applying forward bias to the emitter and reverse bias to the collector to form a common-base triode configuration, the thermoelectric effect, transistor effect, and interfacial effects within the NPN heterostructure are coupled. This NPN heterostructure induces temperature increase (heat release) at the forward biased end and temperature decrease (heat absorption) at the reverse biased end. Therefore, this device becomes a new type of thermoelectric transistor cooler. Furthermore, a DC equivalent circuit method is introduced to analyze the cooling performance of the thermoelectric transistor cooler. The results show that when the emitter voltage of the NPN thermoelectric transistor cooler is 0.01925V, the collector voltage is 0.2124V, the corresponding base region width is 0.17nm, the maximum temperature difference of 242.89K can be obtained. Even if the base region width is limited to a level of 10 nanometers, for example when the base region width is 12.78nm, the maximum temperature differenced can still reach 174.15K. The research results above indicate that the thermoelectric transistor, which synergistically combines the thermoelectric effect with transistor technology, can effectively enhance the maximum temperature difference that typical thermoelectric cooling can achieve.

Introduction

The continuous demand for energy-efficient cooling solutions, combined with environmental concerns, highlights the importance of exploring innovative methods to reduce global energy consumption and greenhouse gas emissions. Therefore, thermoelectric (TE) cooling has become one of the preferred solutions that attracts much attention.

Thermoelectric cooling, also called semiconductor refrigeration or thermoelectric refrigeration, is a new refrigeration technology developed in the late 1950s. It achieves refrigeration through the Peltier effect by directly using electrical energy. The Peltier effect was discovered by J. Peltier [1] in 1834, referring to the phenomenon that when electric current flows through the junction of two different materials, heat is absorbed from or released into the external environment. In practical applications, thermoelectric cooling possesses the advantages of: fast response, no pollution, no noise, no moving parts, small size, light weight, strong adaptability (adjustable in size, shape, temperature, power, etc.), high reliability (no wear, basically no maintenance required), high mechanical strength, strong impact resistance, long service life, coefficient of performance not depending on capacity, easy speed control, reversible operation [2, 3]. As a result, thermoelectric cooling has been widely applied.

Despite having significant advantages in specific application domains such as aerospace, electronic devices, and healthcare, thermoelectric cooling technology is still constrained for large-scale commercialization by its relatively low conversion efficiency [4]. In recent years, scholars have pursued three primary strategies to enhance the performance of thermoelectric coolers:

First, enhancing the thermoelectric properties of materials [5, 6]. The performance of thermoelectric materials is principally determined by the dimensionless figure of merit ZT=S2σT/κZT = S^{2}\sigma T/\kappa, where SS, σ\sigma, TT, and κ\kappa denote the Seebeck coefficient, electrical conductivity, absolute temperature, and total thermal conductivity (comprising lattice contribution κl\kappa_{\mathrm{l}} and electronic contribution κe\kappa_{\mathrm{e}}) respectively [7, 8, 9, 10, 11, 12]. Material optimization approaches include alloying [13, 14, 15], synthesis of nanocomposite structures [16, 17, 18, 19], low-dimensional engineering [20, 21, 22, 23, 24]. Second, geometric and structural optimization of thermoelectric devices. Currently, the mainstream thermoelectric cooling device structures are three types: unipolar/layered devices constructed from series/parallel-connected π\pi-type thermoelements (fundamental N/P-type material units), multistage thermoelectric coolers, Y-shaped structural devices [25]. Third, exploring novel concepts and operational principles – the primary focus of this research.

The combination of thermoelectric principles and transistor technology has attracted widespread attention, including electric-field-driven thermoelectric devices [26, 27, 28, 29, 30] and purely temperature-gradient-driven junction thermoelectric transistors [31, 32, 33]. Research indicates that in electric-field-driven thermoelectric devices, under the combined action of temperature gradient and gate voltage, thermoelectric performance can be optimized by independently regulating internal material parameters and decoupling the Seebeck coefficient and electrical conductivity [26]. Bejenari et al. used theoretical models to study the influence of gate voltage on the thermoelectric properties of Bi2_2Te3_3 nanowires [27]. The results indicated that the ZTZT of 7nm-thick Bi2_2Te3_3 nanowires could reach up to 3.4. Subsequently, experimental results from Qin et al. showed that under gate voltage, the ZTZT values of n-type and p-type Bi2_2Te3_3 thin films could achieve 1.22 and 1.02, respectively [28]. Through experimental measurements, Yang et al. discovered that the power factor (S2σS^{2}\sigma) of 2D-Bi2_2O2_2Se could exceed 400 μ\muWm−1^{-1}K−2^{-2} due to gate voltage effects [29]. Additionally, Wu et al. found that under gate voltage, 2D Nb2_2SiTe4_4-based transistors realized the Seebeck diode effect at room temperature [30].

Thermoelectric junction transistors based on PNP/NPN heterostructures demonstrate substantial potential in thermoelectric by overcoming the inherent limitations of strong parameter coupling in conventional systems. With advancing applications of P-N junctions in thermoelectricity, research confirms that interfacial effects at P-N junctions enable significantly enhanced Seebeck coefficients near the depletion layer [31, 32, 33, 34, 35, 36]. In 1986, Balmush et al. postulated that voltages across P-N junctions under non-isothermal conditions could increase dramatically near depletion regions [37]. Subsequent theoretical work in the 1990s by Zakhidov, Ravich, and collaborators demonstrated through detailed calculations that P-N junctions could substantially elevate both Seebeck coefficient and ZTZT values via interfacial phenomena [38, 39, 40]. Nan et al. systematically investigated the thermoelectric conversion performance of (Bi1−xSbx)2(Te1−ySey)3(\mathrm{Bi}_{1-x}\mathrm{Sb}_x)_2(\mathrm{Te}_{1-y}\mathrm{Se}_y)_3-based PNP junction thermoelectric transistors [31, 32, 33]. Through optimizing the carrier concentrations of the emitter, base, and collector, as well as the device dimensions, and utilizing thermal equilibrium equations, the PNP thermoelectric junction transistor achieves a maximum output power of 17.8mW under a 50K temperature difference drive, with a corresponding conversion efficiency of 8.69%, under maximum power output mode without considering the Thomson effect [32]. This efficiency would require conventional thermoelectric generators to achieve ZT>9ZT > 9, underscoring the substantial potential of junction thermoelectric transistors for breakthrough performance enhancement.

Accordingly, in this paper, P-type Bi0.5Sb1.5Te3\mathrm{Bi}_{0.5}\mathrm{Sb}_{1.5}\mathrm{Te}_{3} and N-type Bi2Te2.97Se0.03\mathrm{Bi}_{2}\mathrm{Te}_{2.97}\mathrm{Se}_{0.03} are used to construct NPN junction thermoelectric transistors. Positive and negative bias voltages are applied to the emitter and collector respectively to regulate the thermoelectric effect, interface effect and transistor effect of the junction-type thermoelectric transistor, thereby decoupling material parameters and improving the thermoelectric cooling performance. A systematic study is conducted on the output performance of the thermoelectric transistor cooling device.

Principles and Analytical Methods

Working principle and material selection of TE transistor cooling devices

The working principle of the general thermoelectric cooling device or the Peltier effect in semiconductor materials can be explained by Figure 1[41]. As can be seen from Figure 1, when the current flows from the N type region to the P type region, the charge carriers continuously flow out at the pn junction (1). Therefore, new charge carriers need to be generated accordingly, which requires energy consumption, thus causing the temperature to decrease. When the charge carriers flow to the pn junction (2), the two types of charge carriers move towards each other, resulting in the recombination of electrons and holes, thereby releasing energy and causing the temperature to rise. It can also be seen from Figure 1 that the pn junction (1) is reverse-biased, and the pn junction (2) is forward-biased. That is, reverse bias causes the interface temperature to decrease, and forward bias causes the interface temperature to increase. Moreover, the currents passing through the two pn junctions in Figure 1 cannot be independently controlled because they share a single power supply.

Schematic diagram of the Peltier effect of semiconductor materials

Figure 1. Schematic diagram of the Peltier effect of semiconductor materials

Here, the rectangular structure design of the NPN heterojunction is shown in Figure 2 (a). Along the X direction, Wn1W_{\mathrm{n1}}, WpW_{\mathrm{p}}, and Wn2W_{\mathrm{n2}} represent the widths of N1_1-type, P-type, and N2_2-type materials, respectively. In the YZ plane, the cross-sectional area of the NPN heterojunction is A. The P-type region is fully depleted to eliminate the effects of bipolar diffusion. Therefore, there are no free minority carriers (holes) in this P-type region. And the dimensions of Wn1W_{\mathrm{n1}} and Wn2W_{\mathrm{n2}} are at the nanoscale. The circuit connection structure diagram of this NPN junction transistor used for refrigeration is shown in Figure 2 (b). The voltages applied between the N1_1-P junction and the N2_2-P junction ensure that the N1_1-P junction is in reverse bias while the N2_2-P junction is in forward bias. When current flows through the circuit, the temperature at the right end of the N2_2 region will increase, while the temperature at the left end of the N1_1 region will decrease, thereby creating a temperature difference between the two ends of the the N1_1PN2_2 junction thermoelectric transistor. Compared with Figure 1, the fundamental difference between the two figures lies in that the voltages of the two pn junctions in Figure 2 can be independently controlled. Therefore, by adjusting their voltages, the temperature of the N2_2-P junction at the high-temperature end in Figure 2 can be lowered, which is more conducive to improving the cooling effect of the semiconductor cooling device.

Schematic diagram of the thermoelectric transistor structure and circuit configuration

Figure 2. (a) Schematic diagram of the thermoelectric transistor structure; (b) Circuit configuration of the thermoelectric transistor

The working principle is as follows: By controlling the carrier concentration of emitter N2_2 and base P, as well as V2_2, the current through the interface between collector N1_1 and base P can be regulated. By adjusting the carrier concentration of N1_1 and V1_1, the cooling capacity can be controlled. This is because in a junction transistor, the emitter current Je_e is approximately equal to the collector current Jc_c, i.e., Je_e ≈\approx Jc_c. Therefore, by optimizing and controlling the carrier concentration of emitter N2_2, base P, and collector N1_1, as well as the applied voltages V2_2 and V1_1, the cooling capacity of the collector can be maximized.

In this work, N1_1-Bi2_2Te2.97_{2.97}Se0.03_{0.03}, P-Bi0.5_{0.5}Sb1.5_{1.5}Te3_3, and N2_2-Bi2_2Te2.97_{2.97}Se0.03_{0.03} are employed as the collector, base, and emitter materials, respectively, with their essential parameters summarized in Table 1.

ParametersEmitterBaseCollectorReferences
ni(×1025 m−3)n_i(\times10^{25}\,\mathrm{m}^{-3})0.160.140.16[32]
k(W/mK)k(\mathrm{W}/\mathrm{mK})1.74741.74741.7474[42, 43]
εr\varepsilon_r909090[40]
μ(m2/Vs)\mu(\mathrm{m}^2/\mathrm{Vs})0.120.02750.12[44]
L(μm)L(\mu\mathrm{m})403040[45]
m∗/mem^*/m_e1.391.441.39[46, 47]

Table 1. Material Parameters of TE transistors

Carrier concentration analysis

In thermoelectric transistors, since the P type region is completely depleted, only the charge carriers (electrons) in the N-type region can move through the NP or PN junction. In this work, N-type Bi2Te2.97Se0.03\mathrm{Bi}_{2}\mathrm{Te}_{2.97}\mathrm{Se}_{0.03} is used as the N type thermoelectric material; therefore, the majority electrons contribute more to the thermoelectric process than the minority holes [48]. Hereafter, we focus on the electron concentration distribution of N-type Bi2Te2.97Se0.03\mathrm{Bi}_{2}\mathrm{Te}_{2.97}\mathrm{Se}_{0.03}. The distribution of electrons can be obtained through a theoretical analysis method. This method consists of three equations: the current density expression for DC current transport [49], the one-dimensional Poisson equation [47], and the current continuity equation [50]:

The current density equation governing DC charge transport can be expressed as formula (1):

Jn(x)=σn(x)[E(x)−Sn(x)∇T](1)J_n(x)=\sigma_n(x)[E(x)-S_n(x)\nabla T] \tag*{(1)}

The one-dimensional Poisson equation can be expressed as formula (2):

E(x)=dφ(x)dx(2)E(x)=\frac{\mathrm{d}\varphi(x)}{\mathrm{d}x} \tag*{(2)}
d2φ(x)dx2=−eεrε0(n(x)−Nd)(3)\frac{\mathrm{d}^{2}\varphi(x)}{\mathrm{d}x^{2}}=-\frac{e}{\varepsilon_r\varepsilon_0}(n(x)-N_d) \tag*{(3)}

The current continuity equation can be expressed as formula (3):

∂n∂t=−1e∂Jn(x)∂x+(Gn−Rn)(4)\frac{\partial n}{\partial t}=-\frac{1}{e}\frac{\partial J_n(x)}{\partial x}+(G_n-R_n) \tag*{(4)}

Where Jn(x)J_n(x) represents the current density, σn(x)\sigma_n(x) and Sn(x)S_n(x) denote the electrical conductivity and Seebeck coefficient of N-type Bi2Te2.97Se0.03\mathrm{Bi}_{2}\mathrm{Te}_{2.97}\mathrm{Se}_{0.03}, ∇T\nabla T signifies the temperature gradient, E(x)E(x) stands for the electric field, φ(x)\varphi(x) indicates the electric potential, ee is the charge, εr\varepsilon_r is the relative dielectric constant, ε0\varepsilon_0 is the vacuum dielectric constant, n(x)n(x) is the electron concentration distribution in N-type Bi2Te2.97Se0.03\mathrm{Bi}_{2}\mathrm{Te}_{2.97}\mathrm{Se}_{0.03}, NdN_d represents the acceptor doping concentration of N-type Bi2Te2.97Se0.03\mathrm{Bi}_{2}\mathrm{Te}_{2.97}\mathrm{Se}_{0.03}, GnG_n represents the generation rate of electron carriers, and RnR_n denotes the recombination rate of electron carriers.

Since the N-type Bi2Te2.97Se0.03\mathrm{Bi}_{2}\mathrm{Te}_{2.97}\mathrm{Se}_{0.03} used in this work can be approximated as a degenerate semiconductor, the conductivity σn(x)\sigma_n(x) and the seebeck coefficient Sn(x)S_n(x) can be expressed as formula (4) [47][51]:

σn(x)=n(x)eμn(5)\sigma_n(x)=n(x)e\mu_n \tag*{(5)}
Sn(x)=[8π3mn∗kB2(r+32)35/3h2e]T(x)n(x)2/3(6)S_n(x)=\left[\frac{8\pi^{3}m_n^{*}k_B^{2}\left(r+\frac{3}{2}\right)}{3^{5/3}h^{2}e}\right]\frac{T(x)}{n(x)^{2/3}} \tag*{(6)}

Where μn\mu_n is the electron mobility, kBk_B is the Boltzmann constant, ee is the electron charge, r=−1/2r=-1/2 is the scattering factor, mn∗m_n^{*} is the effective mass of the carrier, hh is the Planck constant, and T(x)T(x) is the temperature distribution.

At the high-temperature end (the right end of N2), a constant temperature boundary condition is adopted. Assuming that the temperature in the N-type Bi2Te2.97Se0.03\mathrm{Bi}_{2}\mathrm{Te}_{2.97}\mathrm{Se}_{0.03} is linearly distributed, with the temperature at the high-temperature end (the right end of N2) being ThT_h and the temperature at the low-temperature end (the left end of N1) being TcT_c, the temperature distribution can be expressed as:

T(x)=−Th−Tclxx+Th(7)T(x)=-\frac{T_h-T_c}{l_x}x+T_h \tag*{(7)}

Since the simulation temperature is lower than the intrinsic excitation temperature of the N-type Bi₂Te₂.₉₇Se₀.₀₃ and it can be assumed that the electron generation rate equals the recombination rate, thus the electron concentration remains unchanged.

∫0lxNd dx=∫0lxn(x) dx(8)\int_{0}^{l_x} N_d\,dx = \int_{0}^{l_x} n(x)\,dx \tag*{(8)}

Then, formula (1b) becomes:

E(x)=dφ(x)dx=∫0lxeεrε0(n(x)−Nd)dx=0(9)E(x)=\frac{d\varphi(x)}{dx}=\int_{0}^{l_x}\frac{e}{\varepsilon_r\varepsilon_0}\left(n(x)-N_d\right)dx=0 \tag*{(9)}

Substituting equation (7) into equation (1a) yields

Jn(x)=−σn(x)Sn(x)∇T(10)J_n(x)=-\sigma_n(x)S_n(x)\nabla T \tag*{(10)}

Meanwhile, assuming that the temperature of the N-type Bi₂Te₂.₉₇Se₀.₀₃ (including the N₁ and N₂ regions) is in a dynamically stable distribution state, then

∂n∂t=−1q∂Jn(x)∂x=0(11)\frac{\partial n}{\partial t}=-\frac{1}{q}\frac{\partial J_n(x)}{\partial x}=0 \tag*{(11)}

Finally, based on equations (4a), (4b), (5), (8), and (9), the electron concentration distribution in N-type Bi₂Te₂.₉₇Se₀.₀₃ can be calculated.

In the thermoelectric transistor of this work, both the N₁ and N₂ regions are composed of N-type Bi₂Te₂.₉₇Se₀.₀₃. Since the P-type region is extremely thin (only a few nanometers in thickness), it is assumed that its temperature remains constant at T0T_0. The temperature distributions are as follows:

T1(x1)=−T0−Tcwn1x1+T0(12)T_1(x_1)=-\frac{T_0-T_c}{w_{n1}}x_1+T_0 \tag*{(12)}
T2(x2)=−Th−T0wn2x2+Th(13)T_2(x_2)=-\frac{T_h-T_0}{w_{n2}}x_2+T_h \tag*{(13)}

Where wn1w_{n1} and wn2w_{n2} represent the widths of the N₁ and N₂ regions, respectively. Based on equations (4a), (4b), (5), (8), (9), (10), and (11), the electron concentration distributions in the N₁ and N₂ regions are given by:

N1(x1)=2Nd1wn1[(T0wn1Tc−T0)−2−(Tcwn1Tc−T0)−2]∗(x1+T0wn2Tc−T0)−3(14)N_1(x_1)=\frac{2N_{d1}w_{n1}}{\left[\left(\frac{T_0w_{n1}}{T_c-T_0}\right)^{-2}-\left(\frac{T_cw_{n1}}{T_c-T_0}\right)^{-2}\right]}\ast\left(x_1+\frac{T_0w_{n2}}{T_c-T_0}\right)^{-3} \tag*{(14)}
N2(x1)=2Nd2wn2[(Thwn2T0−Th)−2−(T0wn2T0−Th)−2]∗(x2+Thwn2T0−Th)−3(15)N_2(x_1)=\frac{2N_{d2}w_{n2}}{\left[\left(\frac{T_hw_{n2}}{T_0-T_h}\right)^{-2}-\left(\frac{T_0w_{n2}}{T_0-T_h}\right)^{-2}\right]}\ast\left(x_2+\frac{T_hw_{n2}}{T_0-T_h}\right)^{-3} \tag*{(15)}

Thus, the electron concentration n1n_1 in the N₁ region at the N₁-P interface and the electron concentration n2n_2 in the N₂ region at the N₂-P interface are respectively:

n1=N1(0)(16)n_1=N_1(0) \tag*{(16)}
n2=N2(wn2)(17)n_2=N_2(w_{n2}) \tag*{(17)}

Operating States of the TE Transistor

In this thermoelectric transistor, the N₁, P and N₂ regions are used as the collector, base, and emitter, respectively. The applied voltages V1V_1 and V2V_2 divide the thermoelectric transistor into reverse-biased and forward-biased sections.

In the reverse-biased section of the thermoelectric transistor, the P-type region is fully depleted. Consequently, the Seebeck voltage Vs1V_{s1} and Seebeck coefficient Sn1S_{n1} in the N1N_1 region are given by:

Vs1=Sn1(T0−Tc)(18)V_{s1}=S_{n1}(T_0-T_c) \tag*{(18)}
Sn1=[8π32mn∗kB2(r+32)353h2e](Tc+T02)Nd123(19)S_{n1}=\left[\frac{8\pi^{\frac{3}{2}}m_n^{*}k_B^2\left(r+\frac{3}{2}\right)}{3^{\frac{5}{3}}h^2e}\right]\frac{\left(\frac{T_c+T_0}{2}\right)}{N_{d1}^{\frac{2}{3}}} \tag*{(19)}

Where kBk_B is the Boltzmann constant, ee is the electron charge, r=−1/2r=-1/2 is the scattering factor, mn∗m_n^{*} is the carrier effective mass, and hh is the Planck constant.

The built-in voltage Vd1V_{d1} of the N1N_1-P junction is given by:

Vd1=kBT0eln⁡n1p1nninpi(20)V_{d1}=\frac{k_BT_0}{e}\ln\frac{n_1p_1}{n_{ni}n_{pi}} \tag*{(20)}

Where nnin_{ni} and npin_{pi} represent the intrinsic carrier concentrations of N-type Bi2_2Te2.97_{2.97}Se0.03_{0.03} and P-type Bi0.5_{0.5}Sb1.5_{1.5}Te3_3, respectively. n1n_1 denotes the electron concentration in the N1N_1 region at temperature T0T_0, p1p_1 is the hole concentration in the P-type region. Since the P-type region is at the nanoscale, it is assumed that p1p_1 is equal to the doping concentration PaP_a of the P-type region.

Similarly, the Seebeck voltage Vs2V_{s2} and Seebeck coefficient Sn2S_{n2}, in the N2N_2 region, and the built-in voltage Vd2V_{d2} at the N2N_2-P interface are given by:

Vs2=Sn2(Th−T0)(21)V_{s2}=S_{n2}(T_h-T_0) \tag*{(21)}
Sn2=[8π32mn∗kB2(r+32)353h2e](Th+T02)Nd223(22)S_{n2}=\left[\frac{8\pi^{\frac{3}{2}}m_n^{*}k_B^2\left(r+\frac{3}{2}\right)}{3^{\frac{5}{3}}h^2e}\right]\frac{\left(\frac{T_h+T_0}{2}\right)}{N_{d2}^{\frac{2}{3}}} \tag*{(22)}
Vd2=kBT0eln⁡n2p2nninpi(23)V_{d2}=\frac{k_BT_0}{e}\ln\frac{n_2p_2}{n_{ni}n_{pi}} \tag*{(23)}

Where Sn2S_{n2} represents the Seebeck coefficient in the N2N_2 region, n2n_2 denotes the electron concentration in the N2N_2 region at temperature T0T_0 (which equals its acceptor doping concentration), and p2p_2 is the hole concentration in the P-type region. Since the P-type region is at the nanoscale, it is assumed that p2p_2 is equal to the doping concentration PaP_a of the P-type region.

Working Principle and DC Equivalent Circuit Diagram of the TE Transistor Cooling Devices

In the thermoelectric transistor circuit, the base-collector leakage current and Early voltage effects are neglected. The equivalent DC circuit is illustrated in Figure 2. The left section represents the reverse-biased part, where Vs1V_{s1} is the Seebeck voltage of the N1N_1-P region, R1R_1 is the total resistance of the N1N_1-P region including the resistances of both N1N_1 and P regions as well as the interface resistance, and Vd1V_{d1} is the interface voltage between N1N_1 and P. The right part corresponds to the forward-biased section, where Vs2V_{s2} is the Seebeck voltage generated by the N2N_2-P region, R2R_2 is the total resistance of the N2N_2-P region including the resistances of both N2N_2 and P regions as well as the interface resistance, and Vd2V_{d2} is the interface voltage between N2N_2 and P. Additionally, the contact resistance between the thermoelectric transistor and electrodes is neglected in this model.

The internal equivalent circuit of the TE transistor is represented within the black dashed box in the Figure 3.

DC equivalent circuit diagram of the thermoelectric transistor cooling device

Figure 3. DC equivalent circuit diagram of the thermoelectric transistor cooling device.

According to Kirchhoff's laws, the relationships between these electrical parameters in the thermoelectric transistor can be expressed as:

V1=I1R1+Vs1+Vd1(24)V_1 = I_1 R_1 + V_{s1} + V_{d1} \tag*{(24)}
V2=I2R2+Vs2−Vd2(25)V_2 = I_2 R_2 + V_{s2} - V_{d2} \tag*{(25)}
I1=I2=J∗A(26)I_1 = I_2 = J * A \tag*{(26)}
R1=Rn1+Rp1+Rj1(27)R_1 = R_{n1} + R_{p1} + R_{j1} \tag*{(27)}
R2=Rn2+Rp2+Rj2(28)R_2 = R_{n2} + R_{p2} + R_{j2} \tag*{(28)}

Additionally

Rn1=1Nd1eμn∗wn1A(29)R_{n1} = \frac{1}{N_{d1}e\mu_n} * \frac{w_{n1}}{A} \tag*{(29)}
Rp1=1Paeμp∗wp1A(30)R_{p1} = \frac{1}{P_a e\mu_p} * \frac{w_{p1}}{A} \tag*{(30)}
Rn2=1Nd2eμn∗wn2A(31)R_{n2} = \frac{1}{N_{d2}e\mu_n} * \frac{w_{n2}}{A} \tag*{(31)}
Rp2=1Paeμp∗wp2A(32)R_{p2} = \frac{1}{P_a e\mu_p} * \frac{w_{p2}}{A} \tag*{(32)}
Rj1=kBT0Ae2(Dp1nniLp+Dn1npiLn)−1(33)R_{j1} = \frac{k_B T_0}{A e^2}\left(\frac{D_{p1}n_{ni}}{L_p} + \frac{D_{n1}n_{pi}}{L_n}\right)^{-1} \tag*{(33)}
Rj2=kBT0Ae2(Dp2nniLp+Dn2npiLn)−1(34)R_{j2} = \frac{k_B T_0}{A e^2}\left(\frac{D_{p2}n_{ni}}{L_p} + \frac{D_{n2}n_{pi}}{L_n}\right)^{-1} \tag*{(34)}

Where JJ represents the current density, AA denotes the cross-sectional area of the thermoelectric transistor, LpL_p and LnL_n are the diffusion lengths of P-type Bi0.5Sb1.5Te3\mathrm{Bi}_{0.5}\mathrm{Sb}_{1.5}\mathrm{Te}_3 and N-type Bi2Te2.97Se0.03\mathrm{Bi}_2\mathrm{Te}_{2.97}\mathrm{Se}_{0.03}, respectively, and μp\mu_p and μn\mu_n are the charge carrier mobilities of P-type Bi0.5Sb1.5Te3\mathrm{Bi}_{0.5}\mathrm{Sb}_{1.5}\mathrm{Te}_3 and N-type Bi2Te2.97Se0.03\mathrm{Bi}_2\mathrm{Te}_{2.97}\mathrm{Se}_{0.03}. The diffusion coefficients Dp1D_{p1}, Dn1D_{n1}, Dp2D_{p2}, and Dn2D_{n2} correspond to the reverse-biased and forward-biased regions of P-type Bi0.5Sb1.5Te3\mathrm{Bi}_{0.5}\mathrm{Sb}_{1.5}\mathrm{Te}_3 and N-type Bi2Te2.97Se0.03\mathrm{Bi}_2\mathrm{Te}_{2.97}\mathrm{Se}_{0.03}, respectively. These diffusion coefficients (DD) can be derived from the Einstein relation:

D=kBTeμ(35)D = \frac{k_B T}{e}\mu \tag*{(35)}

Since the thermoelectric cooling process belongs to high current injection, the current density formula is given by:

J=2e(DpnniLp+DnnpiLn)exp⁡(eV22kBT0)(36)J = 2e\left(\frac{D_p n_{ni}}{L_p}+\frac{D_n n_{pi}}{L_n}\right)\exp\left(\frac{eV_2}{2k_B T_0}\right) \tag*{(36)}

Since P₁ and P₂ are completely depleted, wp1w_{p1} and wp2w_{p2} can be expressed as

wp1=2ε1ε0Vd1e∗n1Pa∗(Pa+n1)(37)w_{p1} = \sqrt{\frac{2\varepsilon_1\varepsilon_0 V_{d1}}{e} * \frac{n_1}{P_a * (P_a+n_1)}} \tag*{(37)}
wp2=2ε2ε0Vd2e∗n2Pa∗(Pa+n2)(38)w_{p2} = \sqrt{\frac{2\varepsilon_2\varepsilon_0 V_{d2}}{e} * \frac{n_2}{P_a * (P_a+n_2)}} \tag*{(38)}
Wp=Wp1+Wp2(39)W_p = W_{p1}+W_{p2} \tag*{(39)}

Where ε₁ and ε₂ represent the relative permittivity of the P₁ and P₂ regions, respectively, while ε₀ denotes the vacuum permittivity.

Thermoelectric Transistor Cooling Performance

Thermoelectric Transistor Conversion Efficiency

The conversion efficiency (η) of a thermoelectric cooler is defined as:

η=QcP(40)\eta= \frac{Q_c}{P} \tag*{(40)}

Where η is the conversion efficiency, Qc denotes the heat absorption at the cold end, and P stands for the input electrical power.

When considering the coupling between the Seebeck effect and interface effects in NPN heterostructures, QcQ_c can be expressed as:

Qc=(Sn1T0+Vd1)I1−12I12R1−12I22R2−k(Th−Tc)(41)Q_c = (S_{n1}T_0+V_{d1})I_1-\frac{1}{2}I_1^2R_1-\frac{1}{2}I_2^2R_2-k(T_h-T_c) \tag*{(41)}
k=ANlNλN+APlPλP(42)k = \frac{A_N}{l_N}\lambda_N+\frac{A_P}{l_P}\lambda_P \tag*{(42)}

In the equation above, λP and λN represent the thermal conductivities of the P-type and N-type materials, respectively, while AP, lP and AN, lN are the cross-sectional areas and lengths of the P-type and N-type materials, respectively.

Cooling Temperature Difference

The input power P of the refrigeration device can be expressed as:

P=I1V1+I2V2(43)P = I_1V_1+I_2V_2 \tag*{(43)}

By substituting equations (39) and (41) into the equation of efficiency (40), we can obtain

η=(Sn1T0+Vd1)I1−12I12R1−12I22R2−k(Th−Tc)I1V1+I2V2(44)\eta= \frac{(S_{n1}T_0+V_{d1})I_1-\frac{1}{2}I_1^2R_1-\frac{1}{2}I_2^2R_2-k(T_h-T_c)}{I_1V_1+I_2V_2} \tag*{(44)}

Another important performance indicator of a thermoelectric cooler is the temperature difference that can be established across its two ends, that is

ΔT=Th−Tc(45)\Delta T = T_h - T_c \tag*{(45)}

Using the thermal equilibrium equation of the cold end of the device (Equation (42)), the result can be obtained

ΔT=(Sn1T0+Vd1)I1−12I12R1−12I22R2−Qck(46)\Delta T = \frac{(S_{n1}T_0 + V_{d1})I_1 - \frac{1}{2}I_1^2R_1 - \frac{1}{2}I_2^2R_2 - Q_c}{k} \tag*{(46)}

When the cooler works with no external heat load (Qc=0Q_c=0), the maximum temperature difference ΔTmax⁡\Delta T_{\max} that the cooler can achieve can be obtained.

Calculation of T0T_0

Since the thermoelectric transistor dissipates heat only at the forward bias and absorbs heat at the reverse bias, the heat absorbed at the forward bias portion, Qc2Q_{c2}, equals the heat dissipated at the reverse bias portion, Qh1Q_{h1}. This can be expressed as

Qc2=(αn2T0−Vd2)I2−12I22R2−k(Th−T0)(47)Q_{c2} = (\alpha_{n2}T_0 - V_{d2})I_2 - \frac{1}{2}I_2^2R_2 - k(T_h-T_0) \tag*{(47)}
Qc1=(αn1T0+Vd1)I1−12I12R1−k(T0−Tc)(48)Q_{c1} = (\alpha_{n1}T_0 + V_{d1})I_1 - \frac{1}{2}I_1^2R_1 - k(T_0-T_c) \tag*{(48)}
P1=I1V1=I12R1+αn1(T0−Tc)I1+I1Vd1(49)P_1 = I_1V_1 = I_1^2R_1 + \alpha_{n1}(T_0-T_c)I_1 + I_1V_{d1} \tag*{(49)}
Qh1=Qc1+P1=[αn1(2T0−Tc)+2Vd1]I1+12I12R1−k(T0−Tc)(50)Q_{h1} = Q_{c1} + P_1 = [\alpha_{n1}(2T_0-T_c)+2V_{d1}]I_1 + \frac{1}{2}I_1^2R_1 - k(T_0-T_c) \tag*{(50)}

Based on equations (48) and (51), we can determine T0T_0, which is

T0=2Vd1I1+Vd2I2−αn1TcI1+12(I12R1+I22R2)+k(Th+Tc)αp2I2−2αp1I1+2k≈Th+Tc2(51)T_0 = \frac{2V_{d1}I_1 + V_{d2}I_2 - \alpha_{n1}T_cI_1 + \frac{1}{2}(I_1^2R_1+I_2^2R_2)+k(T_h+T_c)}{\alpha_{p2}I_2-2\alpha_{p1}I_1+2k} \approx\frac{T_h+T_c}{2} \tag*{(51)}

During the calculation process, T0T_0 can be approximated as (Th+Tc)/2(T_h+T_c)/2.

Calculation Methods and Process

The results of this work are computed using MATLAB R2020a. During the computation, Nd1N_{d1} is set equal to Nd2N_{d2}, and ThT_h was fixed at 300K. Figure 4 illustrates the schematic of the optimization design and computational process. Using the trial-and-error method, first determine the values of PaP_a, Nd1N_{d1}, and Nd2N_{d2}. Then, substitute the values of PaP_a, Nd1N_{d1}, Nd2N_{d2}, and V2V_2 into formula (43). Under the condition of Tc<ThT_{\mathrm{c}} < T_{\mathrm{h}} and η>0\eta> 0, adjust the value of V2V_2 and calculate the corresponding values of V1V_1, ΔT\Delta T, and η\eta. Finally, obtain the allowable range of changes in V2V_2, V1V_1, ΔT\Delta T, and η\eta. Based on the results above, the parameters PaP_{\mathrm{a}}, Nd1N_{\mathrm{d1}}, and Nd2N_{\mathrm{d2}} are optimized. The maximum temperature difference ΔTmax⁡\Delta T_{\max} under different doping concentrations is calculated, respectively. After comparison, the optimal doping concentration was obtained.

Calculation flowchart of optimal doping concentration

Figure 4. Calculation flowchart of optimal doping concentration

Results and Discussion

In this work, the thickness of the thermoelectric transistor along the Y and Z directions is 0.1 mm, and the width of the N1_1 and N2_2 regions along the X direction is 0.06 mm. The high-temperature end temperature ThT_{\mathrm{h}} is maintained at 300 K, and it is assumed that the carrier concentrations of the emitter N1and the collector N2 are Nd1N_{\mathrm{d1}} and Nd2N_{\mathrm{d2}}, respectively, with Nd1=Nd2N_{\mathrm{d1}} = N_{\mathrm{d2}}. The performance parameters of other materials are shown in Table 1. In this calculation, since the maximum temperature difference is obtained when Nd1=Nd2=1.5N_{\mathrm{d1}} = N_{\mathrm{d2}} = 1.5–3.5×1025 m−33.5 \times10^{25}\ \mathrm{m}^{-3} at relatively low PaP_{\mathrm{a}}, the numerical simulation results for Nd1=Nd2=0.6N_{\mathrm{d1}} = N_{\mathrm{d2}} = 0.6–3.5×1025 m−33.5 \times10^{25}\ \mathrm{m}^{-3} are provided.

The calculation result of Nd1=Nd2=0.6×1025 m−3N_{\mathrm{d1}}=N_{\mathrm{d2}}=0.6\times10^{25}\ \mathrm{m}^{-3}

Figure 5 (a), (b), (c), and (d) show the variation laws of collector voltage V1V_1, base thickness WpW_{\mathrm{p}}, temperature difference ΔT\Delta T across the device, and thermoelectric conversion efficiency η\eta with respect to emitter voltage V2V_2 and base carrier concentration PaP_{\mathrm{a}} under N type region doping concentrations Nd1=Nd2=0.6×1025 m−3N_{\mathrm{d1}} = N_{\mathrm{d2}} = 0.6 \times10^{25}\ \mathrm{m}^{-3}. From Figure 5 (a), under the same PaP_{\mathrm{a}}, as the voltage V2V_2 applied to the emitter increases, the collector voltage V1V_1 increases. Additionally, as the base carrier concentration PaP_{\mathrm{a}} increases, the minimum and maximum allowable values of V2V_2 also increase, as do the initial and maximum reverse bias voltages V1V_1 that need to be applied to the collector. From Figure 5 (b), it can be observed that the base thickness WpW_{\mathrm{p}} decreases as the voltage V2V_2 applied to the emitter and the base carrier concentration PaP_{\mathrm{a}} increases. From Figure 5 (c), when PaP_{\mathrm{a}} is constant, as V2V_2 increases, the temperature difference ΔT\Delta T across the device decreases. When V2V_2 is constant, as PaP_{\mathrm{a}} increases, ΔT\Delta T increases, and the maximum temperature difference ΔTmax⁡\Delta T_{\max} across the device also increases with PaP_{\mathrm{a}}. In Figure 5 (d), the thermoelectric conversion efficiency η\eta decreases as PaP_{\mathrm{a}} increases when V2V_2 is constant and increases as V2V_2 increases when PaP_{\mathrm{a}} is constant. Combining Figure 5 (a), (Figure 5b), (Figure 5c), and (Figure 5d), it can be seen that when PaP_{\mathrm{a}} is constant, the temperature difference ΔT\Delta T across the device is maximized when V2V_2 is at its minimum allowable value, with corresponding minimum values of V1V_1 and WpW_{\mathrm{p}}, and η=0\eta= 0. Comparing the maximum temperature differences ΔTmax⁡\Delta T_{\max} under different PaP_{\mathrm{a}} conditions, the maximum temperature difference across the device increases from ΔTmax⁡=225.17\Delta T_{\max} = 225.17 K at V2=0.00014V_2 = 0.00014 V, V1=0.1794V_1 = 0.1794 V, and Pa=43×1025 m−3P_{\mathrm{a}} = 43 \times10^{25}\ \mathrm{m}^{-3} to ΔTmax⁡=241.10\Delta T_{\max} = 241.10 K at V2=0.00928V_2 = 0.00928 V, V1=0.1960V_1 = 0.1960 V, and Pa=100×1025 m−3P_{\mathrm{a}} = 100 \times10^{25}\ \mathrm{m}^{-3}. At these points, the base thickness WpW_{\mathrm{p}} is 0.36 nm and 0.16 nm, respectively.

Plots of collector voltage, base thickness, temperature difference, and thermoelectric conversion efficiency

Figure 5. V1V_1 (a), WpW_{\mathrm{p}} (b), ΔT\Delta T (c), η\eta (d) as functions of V2V_2 and PaP_{\mathrm{a}} when Nd=0.6×1025 m−3N_{\mathrm{d}}=0.6\times10^{25}\ \mathrm{m}^{-3}

The calculation result of Nd1=Nd2=0.7×1025 m−3N_{\mathrm{d1}}=N_{\mathrm{d2}}=0.7\times10^{25}\ \mathrm{m}^{-3}

Figure 6 (a), (Figure 6b), (Figure 6c), and (Figure 6d) show the variation laws of collector voltage V1V_1, base thickness WpW_{\mathrm{p}}, temperature difference ΔT\Delta T across the device, and thermoelectric conversion efficiency η\eta with respect to emitter voltage V2V_2 and base carrier concentration PaP_{\mathrm{a}} under N type region doping concentrations Nd1=Nd2=0.7×1025 m−3N_{\mathrm{d1}} = N_{\mathrm{d2}} = 0.7\times10^{25}\ \mathrm{m}^{-3}. From Figure 6 (a), under the same PaP_{\mathrm{a}}, as the emitter voltage V2V_2 increases, the collector voltage V1V_1 also increases. Additionally, as the base carrier concentration PaP_{\mathrm{a}} increases, the minimum and maximum allowable values of V2V_2 increase, as do the initial and maximum reverse bias voltages V1V_1 that need to be applied to the collector. From Figure 6 (b), it can be observed that the base thickness WpW_\mathrm{p} decreases as the emitter voltage V2V_2 and base carrier concentration PaP_\mathrm{a} increases. From Figure 6 (c), when PaP_\mathrm{a} is constant, the temperature difference ΔT\Delta T across the device decreases as V2V_2 increases. When V2V_2 is constant, ΔT\Delta T increases with PaP_\mathrm{a}, and the maximum temperature difference ΔTmax\Delta T_\mathrm{max} across the device also increases with PaP_\mathrm{a}. In Figure 6 (d), the thermoelectric conversion efficiency η\eta decreases as PaP_\mathrm{a} increases when V2V_2 is constant and increases as V2V_2 increases when PaP_\mathrm{a} is constant. Combining Figure 6 (a), (Figure 6b), (Figure 6c), and (Figure 6d), it can be seen that when PaP_\mathrm{a} is constant, the temperature difference ΔT\Delta T across the device is maximized when V2V_2 is at its minimum allowable value, with corresponding minimum values of V1V_1 and WpW_\mathrm{p}, and η=0\eta= 0. Comparing the maximum temperature differences ΔTmax\Delta T_\mathrm{max} under different PaP_\mathrm{a} conditions, the maximum temperature difference across the device increases from ΔTmax=214.49\Delta T_\mathrm{max} = 214.49 K at V2=0.00028V_2 = 0.00028 V, V1=0.1667V_1 = 0.1667 V, and Pa=16×1025 m−3P_\mathrm{a} = 16 \times10^{25}\ \mathrm{m}^{-3} to ΔTmax=242.89\Delta T_\mathrm{max} = 242.89 K at V2=0.01925V_2 = 0.01925 V, V1=0.2124V_1 = 0.2124 V, and Pa=100×1025 m−3P_\mathrm{a} = 100 \times10^{25}\ \mathrm{m}^{-3}. At these points, the base thickness WpW_\mathrm{p} is 0.98 nm and 0.17 nm, respectively.

Four-panel plots of $V_1$, $W_{\mathrm{p}}$, $\Delta T$, and $\eta$ as functions of $V_2$ and $P_{\mathrm{a}}$

Figure 6. V1V_1 (a), WpW_{\mathrm{p}} (b), ΔT\Delta T (c), η\eta (d) as functions of V2V_2 and PaP_{\mathrm{a}} when Nd=0.7×1025 m−3N_{\mathrm{d}}=0.7\times10^{25}\ \mathrm{m}^{-3}

The calculation result of Nd1=Nd2=0.8×1025 m−3N_{\mathrm{d1}}=N_{\mathrm{d2}}=0.8 \times10^{25}\ \mathrm{m}^{-3}

Figure 7 (a), (Figure 7b), (Figure 7c), and (Figure 7d) show the variation laws of collector voltage V1V_1, base thickness WpW_\mathrm{p}, temperature difference ΔT\Delta T across the device, and thermoelectric conversion efficiency η\eta with respect to emitter voltage V2V_2 and base carrier concentration PaP_\mathrm{a} under N type region doping concentration Nd1=Nd2=0.8×1025 m−3N_{\mathrm{d1}} = N_{\mathrm{d2}} = 0.8 \times10^{25}\ \mathrm{m}^{-3}. From Figure 7 (a), under the same PaP_\mathrm{a}, as the emitter voltage V2V_2 increases, the collector voltage V1V_1 increases. Additionally, as the base carrier concentration PaP_{\mathrm{a}} increases, the minimum and maximum allowable values of V2V_2 also increase, as the initial and maximum reverse bias voltages V1V_1 required to be applied to the collector. From Figure 7 (b), it can be observed that the base thickness WpW_{\mathrm{p}} decreases as the emitter voltage V2V_2 and base carrier concentration PaP_{\mathrm{a}} increase. From Figure 7 (c), when PaP_{\mathrm{a}} is constant, the temperature difference ΔT\Delta T across the device decreases as V2V_2 increases. When V2V_2 is constant, ΔT\Delta T increases with PaP_{\mathrm{a}}, and the maximum temperature difference ΔTmax⁡\Delta T_{\max} across the device also increases with PaP_{\mathrm{a}}. In Figure 7(d), the thermoelectric conversion efficiency η\eta decreases as PaP_{\mathrm{a}} increases when V2V_2 is constant and increases as V2V_2 increases when PaP_{\mathrm{a}} is constant. Combining Figure 7 (a), (Figure 7b), (Figure 7c), and (Figure 7d), it can be concluded that when PaP_{\mathrm{a}} is constant, the temperature difference ΔT\Delta T across the device is maximized when V2V_2 is at its minimum allowable value, with corresponding minimum values of V1V_1 and WpW_{\mathrm{p}}, and η=0\eta= 0. Comparing ΔTmax⁡\Delta T_{\max} under different PaP_{\mathrm{a}} conditions, the maximum temperature difference across the device increases from ΔTmax⁡=207.02 K\Delta T_{\max} = 207.02\ \mathrm{K} at V2=0.00156 VV_2 = 0.00156\ \mathrm{V}, V1=0.1585 VV_1 = 0.1585\ \mathrm{V}, and Pa=8×1025 m−3P_{\mathrm{a}} = 8 \times10^{25}\ \mathrm{m}^{-3} to ΔTmax⁡=238.23 K\Delta T_{\max} = 238.23\ \mathrm{K} at V2=0.02656 VV_2 = 0.02656\ \mathrm{V}, V1=0.2329 VV_1 = 0.2329\ \mathrm{V}, and Pa=100×1025 m−3P_{\mathrm{a}} = 100 \times10^{25}\ \mathrm{m}^{-3}. At these conditions, the base thickness WpW_{\mathrm{p}} is 1.96 nm and 0.19 nm, respectively.

Plots of $V_1$, $W_\mathrm{p}$, $\Delta T$, and $\eta$ as functions of $V_2$ and $P_\mathrm{a}$

Figure 7. V1V_1 (a), WpW_\mathrm{p} (b), ΔT\Delta T (c), η\eta (d) as functions of V2V_2 and PaP_\mathrm{a} when Nd=0.8×1025 m−3N_{\mathrm{d}}=0.8 \times10^{25}\ \mathrm{m}^{-3}

The calculation result of Nd1=Nd2=0.9×1025 m−3N_{\mathrm{d1}}=N_{\mathrm{d2}}=0.9 \times10^{25}\ \mathrm{m}^{-3}

Figure 8 (a), (Figure 8b), (Figure 8c), and (Figure 8d) show the variation laws of collector voltage V1V_1, base thickness WpW_{\mathrm{p}}, temperature difference ΔT\Delta T across the device, and thermoelectric conversion efficiency η\eta with respect to emitter voltage V2V_2 and base carrier concentration PaP_{\mathrm{a}} under the condition of N type region doping concentration Nd1=Nd2=0.9×1025 m−3N_{\mathrm{d1}} = N_{\mathrm{d2}} = 0.9 \times10^{25}\ \mathrm{m}^{-3}. From Figure 8 (a), under the same PaP_{\mathrm{a}}, as the emitter voltage V2V_2 increases, the collector voltage V1V_1 also increases. Additionally, as the base carrier concentration PaP_{\mathrm{a}} increases, the minimum and maximum allowable values of V2V_{2} increase, as do the initial and maximum reverse bias voltages V1V_{1} that need to be applied to the collector. From Figure 8 (b), it can be observed that the base thickness WpW_{\mathrm{p}} decreases as the emitter voltage V2V_{2} and base carrier concentration PaP_{\mathrm{a}} increases. From Figure 8 (c), when PaP_{\mathrm{a}} is constant, the temperature difference ΔT\Delta T across the device decreases as V2V_{2} increases. Conversely, when V2V_{2} is constant, ΔT\Delta T increases with PaP_{\mathrm{a}}, and the maximum temperature difference ΔTmax⁡\Delta T_{\max} also increases as PaP_{\mathrm{a}} increases. In Figure 8(d), the thermoelectric conversion efficiency η\eta decreases as PaP_{\mathrm{a}} increases when V2V_{2} is constant and increases as V2V_{2} increases when PaP_{\mathrm{a}} is constant. Combining the information from Figure 8 (a), (Figure 8b), (Figure 8c), and (Figure 8d), it can be concluded that when PaP_{\mathrm{a}} is constant, the temperature difference ΔT\Delta T across the device is maximized when V2V_{2} is at its minimum allowable value, with corresponding minimum values of V1V_{1} and WpW_{\mathrm{p}}, and η=0\eta= 0. Comparing the maximum temperature differences ΔTmax⁡\Delta T_{\max} under different PaP_{\mathrm{a}} conditions, the maximum temperature difference increases from ΔTmax⁡=196.75\Delta T_{\max} = 196.75 K at V2=0.000154V_{2} = 0.000154 V, V1=0.1485V_{1} = 0.1485 V, and Pa=4.1×1025P_{\mathrm{a}} = 4.1 \times10^{25} m−3^{-3} to ΔTmax⁡=230.12\Delta T_{\max} = 230.12 K at V2=0.03245V_{2} = 0.03245 V, V1=0.2548V_{1} = 0.2548 V, and Pa=100×1025P_{\mathrm{a}} = 100 \times10^{25} m−3^{-3}. At these conditions, the base thickness WpW_{\mathrm{p}} is 3.70 nm and 0.20 nm, respectively.

Plots of $V_1$ (a), $W_{\mathrm{p}}$ (b), $\Delta T$ (c), and $\eta$ (d) as functions of $V_2$ and $P_{\mathrm{a}}$

Figure 8. V1V_1 (a), WpW_{\mathrm{p}} (b), ΔT\Delta T (c), η\eta (d) as functions of V2V_2 and PaP_{\mathrm{a}} when Nd=0.9×1025 m−3N_{\mathrm{d}} = 0.9 \times10^{25}\ \mathrm{m}^{-3}

The calculation result of Nd1=Nd2=1.0×1025 m−3N_{\mathrm{d1}}=N_{\mathrm{d2}}=1.0\times10^{25}\,\mathrm{m}^{-3}

Figure 9 (a), (Figure 9b), (Figure 9c), and (Figure 9d) show the variation laws of collector voltage V1V_{1}, base thickness WpW_{\mathrm{p}}, temperature difference ΔT\Delta T across the device, and thermoelectric conversion efficiency η\eta with respect to emitter voltage V2V_{2} and base carrier concentration PaP_{\mathrm{a}} under the condition of N type region doping concentration Nd1=Nd2=1.0×1025N_{\mathrm{d1}} = N_{\mathrm{d2}} = 1.0\times10^{25} m−3^{-3}. From Figure 9 (a), under the same PaP_{\mathrm{a}}, as the emitter voltage V2V_2 increases, the collector voltage V1V_1 also increases. Additionally, as the base carrier concentration PaP_a increases, the minimum and maximum allowable values of V2V_2 increase, as do the initial and maximum reverse bias voltages V1V_1 that need to be applied to the collector. From Figure 9 (b), it can be observed that the base thickness WpW_p decreases as the emitter voltage V2V_2 and base carrier concentration PaP_a increases. From Figure 9 (c), when PaP_a is constant, the temperature difference ΔT\Delta T across the device decreases as V2V_2 increases. Conversely, when V2V_2 is constant, ΔT\Delta T increases with PaP_a, and the maximum temperature difference ΔTmax⁡\Delta T_{\max} also increases as PaP_a increases. In Figure 9 (d), the thermoelectric conversion efficiency η\eta decreases as PaP_a increases when V2V_2 is constant and increases as V2V_2 increases when PaP_a is constant. Combining the information from Figure 9 (a), (Figure 9b), (Figure 9c), and (Figure 9d), it can be concluded that when PaP_a is constant, the temperature difference ΔT\Delta T across the device is maximized when V2V_2 is at its minimum allowable value, with corresponding minimum values of V1V_1 and WpW_p, and η=0\eta= 0. Comparing the maximum temperature differences ΔTmax⁡\Delta T_{\max} under different PaP_a conditions, the maximum temperature difference increases from ΔTmax⁡=190.46\Delta T_{\max} = 190.46 K at V2=0.00092V_2 = 0.00092 V, V1=0.1430V_1 = 0.1430 V, and Pa=2.6×1025P_a = 2.6 \times10^{25} m−3^{-3} to ΔTmax⁡=219.97\Delta T_{\max} = 219.97 K at V2=0.03750V_2 = 0.03750 V, V1=0.2768V_1 = 0.2768 V, and Pa=100×1025P_a = 100 \times10^{25} m−3^{-3}. At these conditions, the base thickness WpW_p is 5.58 nm and 0.22 nm, respectively.

Four plots showing V1, Wp, ΔT, and η as functions of V2 and Pa

Figure 9. V1V_{1} (a), WpW_{\mathrm{p}} (b), ΔT\Delta T (c), η\eta (d) as functions of V2V_{2} and PaP_{\mathrm{a}} when Nd=1.0×1025 m−3N_{\mathrm{d}}=1.0\times10^{25}\,\mathrm{m}^{-3}

The calculation result of Nd1=Nd2=1.5×1025 m−3N_{d1}=N_{d2}=1.5 \times10^{25}\,\mathrm{m}^{-3}

Figure 10 (a), (Figure 10b), (Figure 10c), (Figure 10d) show the variation laws of collector voltage V1V_1, base depletion layer thickness WpW_p, temperature difference ΔT\Delta T across the device, and thermoelectric conversion efficiency η\eta with respect to emitter voltage V2V_2 and base carrier concentration PaP_a under the condition of N type region doping concentration Nd1=Nd2=1.5×1025 m−3N_{d1}=N_{d2}=1.5\times10^{25}\ \mathrm{m}^{-3}. From Figure 10 (a), under the same PaP_a, as the emitter voltage V2V_2 increases, the collector voltage V1V_1 also increases. Additionally, as the base carrier concentration PaP_a increases, the minimum and maximum allowable values of V2V_2, as well as the initial and maximum reverse bias voltages V1V_1 required to be applied to the collector, also increase. From Figure 10 (b), it can be observed that the base thickness WpW_p decreases as the emitter voltage V2V_2 and the base carrier concentration PaP_a increases. From Figure 10 (c), when PaP_a PaP_a is constant, the temperature difference ΔT\Delta T across the device decreases with increasing V2V_2. When V2V_2 is constant, ΔT\Delta T increases with increasing PaP_a. Furthermore, the maximum temperature difference ΔTmax⁡\Delta T_{\max} across the device first increases and then decreases as PaP_a increases, reaching its maximum value when Pa=2.0×1025 m−3P_a=2.0\times10^{25}\ \mathrm{m}^{-3}. From the comprehensive analysis of Figure 10 (a), (Figure 10b), (Figure 10c), and (Figure 10d), it can be concluded that when PaP_a is constant, the temperature difference ΔT\Delta T across the device is maximized when V2V_2 is at its minimum allowable value, with corresponding minimum values of V1V_1 and WpW_p, and η=0\eta=0. By comparing the maximum temperature differences ΔTmax⁡\Delta T_{\max} under different PaP_a conditions, the maximum temperature difference across the device increases from ΔTmax⁡=165.44 K\Delta T_{\max}=165.44\ \mathrm{K} at V2=0.00318 VV_2=0.00318\ \mathrm{V}, V1=0.1260 VV_1=0.1260\ \mathrm{V}, and Pa=0.6×1025 m−3P_a=0.6\times10^{25}\ \mathrm{m}^{-3}, to ΔTmax⁡=176.48 K\Delta T_{\max}=176.48\ \mathrm{K} at V2=0.02717 VV_2=0.02717\ \mathrm{V}, V1=0.1880 VV_1=0.1880\ \mathrm{V}, and Pa=2.0×1025 m−3P_a=2.0\times10^{25}\ \mathrm{m}^{-3}, and then decreases to ΔTmax⁡=175.75 K\Delta T_{\max}=175.75\ \mathrm{K} at V2=0.03325 VV_2=0.03325\ \mathrm{V}, V1=0.2150 VV_1=0.2150\ \mathrm{V}, and Pa=3.5×1025 m−3P_a=3.5\times10^{25}\ \mathrm{m}^{-3}. The corresponding base thicknesses WpW_p are 17.23 nm, 8.22 nm, and 5.53 nm, respectively.

Four plots showing $V_1$, $W_p$, $\Delta T$, and $\eta$ as functions of $V_2$ and $P_a$

Figure 10. V1V_1 (a), WpW_p (b), ΔT\Delta T (c), η\eta (d) as functions of V2V_2 and PaP_a when Nd=1.5×1025 m−3N_d = 1.5 \times10^{25}\,\mathrm{m}^{-3}

The calculation result of Nd1=Nd2=2.0×1025 m−3N_{d1}=N_{d2}=2.0\times10^{25}\ \mathrm{m}^{-3}

Figure 11 (a), (Figure 11b), (Figure 11c), and (Figure 11d) show the variation laws of collector voltage V1V_1, base region depletion layer thickness WpW_p, temperature difference ΔT\Delta T across the device, and thermoelectric conversion efficiency η\eta with respect to emitter voltage V2V_2 and base carrier concentration PaP_a, under the condition of N type region doping concentration Nd1=Nd2=2.0×1025 m−3N_{d1}=N_{d2}=2.0\times10^{25}\ \mathrm{m}^{-3}. From Figure 11(a), it can be observed that under the same PaP_a, as the voltage V2V_2 applied to the emitter increases, the collector biot voltage V1V_1 also increases. Additionally, as the base carrier concentration PaP_a increases, the minimum and maximum allowable values of V2V_2, as well as the initial and maximum reverse bias voltages V1V_1 required to be applied to the collector, also increase. Furthermore, compared with Figure 5 to Figure 10, it can be found that as NdN_d increases, the initial allowable value of V1V_1 increases, and the numerical range decreases rapidly. From Figure 11 (b), the base region thickness WpW_p decreases as the voltage V2V_2 applied to the emitter and the base carrier concentration PaP_a increases. From Figure 11 (c), when PaP_a is constant, it can be observed that as V2V_2 increases, the temperature difference ΔT\Delta T across the device decreases. When V2V_2 is constant, as PaP_a increases, ΔT\Delta T increases. Moreover, the maximum temperature difference ΔTmax⁡\Delta T_{\max} across the device first increases and then decreases as PaP_a increases, reaching its maximum value when Pa=0.4×1025 m−3P_a=0.4\times10^{25}\ \mathrm{m}^{-3}, with ΔTmax⁡=149.56 K\Delta T_{\max}=149.56\ \mathrm{K}. From Figure 11 (d), the thermoelectric conversion efficiency η\eta decreases as PaP_a increases when V2V_2 is constant and increases as V2V_2 increases when PaP_a is constant. Integrating the information from Figure 11 (a), (Figure 11b), (Figure 11c), and (Figure 11d), it can be concluded that when PaP_a is constant, the temperature difference ΔT\Delta T across the device is maximized when V2V_2 is at its minimum allowable value, with corresponding minimum values of V1V_1 and WpW_p, and η=0\eta=0. Comparing the maximum temperature differences ΔTmax⁡\Delta T_{\max} under different PaP_a conditions, the maximum temperature difference across the device increases from ΔTmax⁡=149.56 K\Delta T_{\max}=149.56\ \mathrm{K} at V2=0.00962 VV_2=0.00962\ \mathrm{V}, V1=0.1263 VV_1=0.1263\ \mathrm{V}, and Pa=0.3×1025 m−3P_a=0.3\times10^{25}\ \mathrm{m}^{-3}, to ΔTmax⁡=151.05 K\Delta T_{\max}=151.05\ \mathrm{K} at V2=0.01806 VV_2=0.01806\ \mathrm{V}, V1=0.1452 VV_1=0.1452\ \mathrm{V}, and Pa=0.4×1025 m−3P_a=0.4\times10^{25}\ \mathrm{m}^{-3}, and then decreases to ΔTmax⁡=133.12\Delta T_{\max}=133.12 K at V2=0.04699V_2=0.04699 V, V1=0.2697V_1=0.2697 V, and Pa=3.5×1025P_a=3.5\times10^{25} m−3^{-3}. The corresponding base region thicknesses WpW_p are 26.33 nm, 23.20 nm, and 6.74 nm, respectively.

Plots of collector voltage, base region thickness, temperature difference, and thermoelectric conversion efficiency as functions of emitter voltage and base carrier concentration

Figure 11. V1V_1 (a), WpW_p (b), ΔT\Delta T (c), η\eta (d) as functions of V2V_2 and PaP_a when Nd=2.0×1025N_d=2.0\times10^{25} m−3^{-3}

The calculation result of Nd1=Nd2=2.5×1025N_{d1}=N_{d2}=2.5\times10^{25} m−3^{-3}

Figure 12 (a), (b), (c), and (d) show the variation laws of collector voltage V1V_1, base region thickness WpW_p, temperature difference ΔT\Delta T across the device, and thermoelectric conversion efficiency η\eta with respect to emitter voltage V2V_2 and base carrier concentration PaP_a under the condition of N type region doping concentration Nd1=Nd2=2.5×1025N_{d1}=N_{d2}=2.5\times10^{25} m−3^{-3}. From Figure 12 (a), under the same PaP_a, as the emitter voltage V2V_2 increases, the collector voltage V1V_1 also increases. Additionally, as the base carrier concentration PaP_a increases, the minimum and maximum allowable values of V2V_2 increase, as do the initial and maximum reverse bias voltages V1V_1 that need to be applied to the collector. Comparing with Figure 5 to Figure 11, it can be observed that as NdN_d increases, the initial allowable value of V1V_1 further increases, and its numerical range further decreases. From Figure 12 (b), the base region thickness WpW_p decreases as the emitter voltage V2V_2 and base carrier concentration PaP_a increases. From Figure 12 (c), when PaP_a is constant, it can be observed that as V2V_2 increases, the temperature difference ΔT\Delta T across the device decreases. Conversely, when V2V_2 is constant, as PaP_a increases, ΔT\Delta T increases. From the comprehensive analysis of Figure 12 (a), (Figure 12b), (Figure 12c) and (Figure 12d), it can be observed that when PaP_a is constant, V2V_2 attains its minimum allowable value, resulting in the maximum temperature difference ΔT\Delta T across the device terminals. Correspondingly, V1V_1 and WpW_p also reach their minimum values, with η=0\eta=0. By comparing ΔTmax⁡\Delta T_{\max} under different PaP_a conditions, the maximum temperature difference across the device terminals increases from ΔTmax⁡=133.90K\Delta T_{\max}=133.90\mathrm{K} at V2=0.00569VV_2=0.00569\mathrm{V}, V1=0.1136VV_1=0.1136\mathrm{V}, and Pa=0.16×1025m−3P_a=0.16\times10^{25}\mathrm{m}^{-3}, to ΔTmax⁡=134.54K\Delta T_{\max}=134.54\mathrm{K} at V2=0.01168VV_2=0.01168\mathrm{V}, V1=0.1241VV_1=0.1241\mathrm{V}, and Pa=0.18×1025m−3P_a=0.18\times10^{25}\mathrm{m}^{-3}, and then decreases to ΔTmax⁡=89.92K\Delta T_{\max}=89.92\mathrm{K} at V2=0.05743VV_2=0.05743\mathrm{V}, V1=0.3165VV_1=0.3165\mathrm{V}, and Pa=3.5×1025m−3P_a=3.5\times10^{25}\mathrm{m}^{-3}. The corresponding base region thicknesses WpW_p are 36.06nm36.06\mathrm{nm}, 34.54nm34.54\mathrm{nm}, and 7.81nm7.81\mathrm{nm}, respectively.

Plots of collector voltage, base thickness, temperature difference, and thermoelectric conversion efficiency as functions of emitter voltage and base carrier concentration

Figure 12. V1V_1 (a), WpW_p (b), ΔT\Delta T (c), η\eta (d) as functions of V2V_2 and PaP_a when Nd=2.5×1025 m−3N_d=2.5\times10^{25}\,\mathrm{m}^{-3}

The calculation result of Nd1=Nd2=3.0×1025 m−3N_{d1}=N_{d2}=3.0\times10^{25}\,\mathrm{m}^{-3}

Figure 13 (a), (b), (c), and (d) show the variation laws of collector voltage V1V_1, base thickness WpW_p, temperature difference ΔT\Delta T across the device, and thermoelectric conversion efficiency η\eta with respect to emitter voltage V2V_2 and base carrier concentration PaP_a under N type region doping concentrations Nd1=Nd2=3.0×1025 m−3N_{d1}=N_{d2}=3.0\times10^{25}\,\mathrm{m}^{-3}. From Figure 13 (a), under the same PaP_a, as the voltage V2V_2 applied to the emitter increases, the collector voltage V1V_1 increases. Additionally, as the base carrier concentration PaP_a increases, the minimum and maximum allowable values of V2V_2 also increase, as do the initial and maximum reverse bias voltages V1V_1 that need to be applied to the collector. Comparing with Figures 5 to 12, it can be observed that as NdN_d increases, the initial allowable value of V1V_1 further increases, and its numerical range further decreases. From Figure 13 (b), the base thickness WpW_p decreases as the voltage V2V_2 applied to the emitter and the base carrier concentration PaP_a increase. From Figure 13 (c), it can be observed that when PaP_a is constant, the temperature difference ΔT\Delta T across the device decreases as V2V_2 increases. When V2V_2 is constant, ΔT\Delta T increases as PaP_a increases, and the maximum temperature difference ΔTmax⁡\Delta T_{\max} across the device decreases as PaP_a increases. From Figure 13 (d), the thermoelectric conversion efficiency η\eta decreases as PaP_a increases when V2V_2 is constant and increases as V2V_2 increases when PaP_a is constant. Combining Figures 13 (a), (b), (c), and (d), it can be concluded that when PaP_{\mathrm{a}} is constant, the minimum allowable value of V2V_{2} is taken, resulting in the maximum temperature difference ΔT\Delta T across the device, with the corresponding V1V_{1} and WpW_{\mathrm{p}} also taking their minimum values, and η=0\eta= 0. Comparing the maximum temperature differences ΔTmax⁡\Delta T_{\max} under different PaP_{\mathrm{a}} conditions, the maximum temperature difference across the device decreases from ΔTmax⁡=122.95\Delta T_{\max} = 122.95 K at V2=0.00613V_{2} = 0.00613 V, V1=0.1107V_{1} = 0.1107 V, and Pa=0.11×1025P_{\mathrm{a}} = 0.11 \times10^{25} m−3^{-3} to ΔTmax⁡=49.69\Delta T_{\max} = 49.69 K at V2=0.06584V_{2} = 0.06584 V, V1=0.3568V_{1} = 0.3568 V, and Pa=3.5×1025P_{\mathrm{a}} = 3.5 \times10^{25} m−3^{-3}. The corresponding base thicknesses WpW_{\mathrm{p}} are 42.26 nm and 8.73 nm, respectively.

The calculation result of Nd1=Nd2=3.5×1025N_{\mathrm{d1}} = N_{\mathrm{d2}} = 3.5 \times10^{25} m−3^{-3}

Figure 14 (a), (b), (c), and (d) show the variation laws of collector voltage V1V_{1}, base thickness WpW_{\mathrm{p}}, temperature difference ΔT\Delta T across the device, and thermoelectric conversion efficiency η\eta with respect to emitter voltage V2V_{2} and base carrier concentration PaP_{\mathrm{a}} under N type region doping concentrations Nd1=Nd2=3.5×1025N_{\mathrm{d1}} = N_{\mathrm{d2}} = 3.5 \times10^{25} m−3^{-3}. From Figure 14 (a), under the same PaP_{\mathrm{a}}, as the emitter voltage V2V_{2} increases, the collector voltage V1V_{1} also increases. Additionally, as the base carrier concentration PaP_{\mathrm{a}} increases, the minimum and maximum allowable values of V2V_{2}, as well as the starting and maximum reverse bias voltages V1V_{1} required to be applied to the collector, also increase. Comparing with Figure 5 to Figure 13, it can be observed that as NdN_{\mathrm{d}} increases, the starting value of allowable V1V_{1} further increases, and its numerical range further decreases. From Figure 14 (b), the base thickness WpW_{\mathrm{p}} decreases as the emitter voltage V2V_{2} and base carrier concentration PaP_{\mathrm{a}} increases. From Figure 14 (c), it can be observed that when PaP_{\mathrm{a}} is constant, the temperature difference ΔT\Delta T across the device decreases as V2V_2 increases; when V2V_2 is constant, ΔT\Delta T increases as PaP_{\mathrm{a}} increases, and the maximum temperature difference ΔTmax⁡\Delta T_{\max} across the device decreases as PaP_{\mathrm{a}} increases. In Figure 14 (d), the thermoelectric conversion efficiency η\eta decreases as PaP_{\mathrm{a}} increases when V2V_2 is constant and increases as V2V_2 increases when PaP_{\mathrm{a}} is constant. From the comprehensive analysis of Figure 14 (a), (Figure 14b), (Figure 14c), and (Figure 14d), it can be seen that when PaP_{\mathrm{a}} is constant, the temperature difference ΔT\Delta T across the device is maximized when V2V_2 is set to its minimum allowable value, and the corresponding V1V_1 and WpW_{\mathrm{p}} are also minimized, with η=0\eta= 0. By comparing the maximum temperature differences ΔTmax⁡\Delta T_{\max} under different PaP_{\mathrm{a}} conditions, the maximum temperature difference across the device decreases from ΔTmax⁡=114.32\Delta T_{\max} = 114.32 K at V2=0.00295V_2 = 0.00295 V, V1=0.1038V_1 = 0.1038 V, and Pa=0.08×1025P_{\mathrm{a}} = 0.08 \times10^{25} m−3^{-3} to ΔTmax⁡=12.78\Delta T_{\max} = 12.78 K at V2=0.07312V_2 = 0.07312 V, V1=0.3924V_1 = 0.3924 V, and Pa=3.5×1025P_{\mathrm{a}} = 3.5 \times10^{25} m−3^{-3}. The corresponding base thicknesses WpW_{\mathrm{p}} are 50.05 nm and 9.53 nm, respectively.

Four panels showing V1, Wp, ΔT, and η as functions of V2 and Pa

Figure 13. V1V_{1} (a), WpW_{\mathrm{p}} (b), ΔT\Delta T (c), η\eta (d) as functions of V2V_{2} and PaP_{\mathrm{a}} when Nd=3.0×1025N_{\mathrm{d}} = 3.0 \times10^{25} m−3^{-3}

Four-panel plots of V1, Wp, ΔT, and η as functions of V2 and Pa

Figure 14. V1V_1 (a), WpW_{\mathrm{p}} (b), ΔT\Delta T (c), η\eta (d) as functions of V2V_2 and PaP_{\mathrm{a}} when Nd=3.5×1025N_{\mathrm{d}} = 3.5 \times10^{25} m−3^{-3}

Comprehensive Data Analysis

Figure 15 shows ΔTmax⁡\Delta T_{\max}, V1V_1, V2V_2, and WpW_p versus base region concentration PaP_a when the N type region doping concentration NdN_d is 0.60.6-3.5×1025 m−33.5 \times10^{25}\,\mathrm{m}^{-3}. As shown in Figure 15 (e), when NdN_d is 1.51.5-3.5×1025 m−33.5 \times10^{25}\,\mathrm{m}^{-3}, the maximum value of ΔTmax⁡\Delta T_{\max} has already appeared in the range of Pa=0.08P_a = 0.08-2.1×1025 m−32.1 \times10^{25}\,\mathrm{m}^{-3}. Therefore, in Figure 15 (e) to (Figure 15h), only the calculation results for Pa≤3.5×1025 m−3P_a \le3.5 \times10^{25}\,\mathrm{m}^{-3} are provided. In contrast, in Figure 15 (a) to (Figure 15d), the calculation results are presented when the value of PaP_a ranging from 4.14.1 to 100×1025 m−3100 \times10^{25}\,\mathrm{m}^{-3}.

Plots of $\Delta T_{\max}$, $V_2$, $V_1$, and $W_p$ versus base region concentration $P_a$ for different donor concentrations

Figure 15. ΔTmax⁡\Delta T_{\max} (a), V2V_2 (b), V1V_1 (c), and WpW_p (d) versus base region concentration PaP_a when Nd=0.6N_d=0.6–1.0×1025 m−31.0 \times10^{25}\,\mathrm{m}^{-3}, and ΔTmax⁡\Delta T_{\max} (e), V2V_2 (f), V1V_1 (g), and WpW_p (h) versus base region concentration PaP_a when Nd=1.5N_d=1.5–3.5×1025 m−33.5 \times10^{25}\,\mathrm{m}^{-3}

From Figure 15 (a), when the N type region doping concentration NdN_d is in the range of 0.60.6-1.0×1025 m−31.0 \times10^{25}\,\mathrm{m}^{-3}, the N type region doping concentration NdN_d increases, the minimum permissible base region carrier concentration Pmin⁡P_{\min} decreases. For any given NdN_d value, ΔTmax⁡\Delta T_{\max} increases with the increase of PaP_a, Moreover, as PaP_a increases, ΔTmax⁡\Delta T_{\max} increases rapidly at first, reaches a certain inflection point, and then increases slowly or even tends to stabilize. The maximum value of ΔTmax⁡\Delta T_{\max} corresponding to all 5 NdN_d values is obtained at Pa=100×1025 m−3P_a = 100 \times10^{25}\,\mathrm{m}^{-3}. Besides changing with PaP_a, ΔTmax⁡\Delta T_{\max} also changes with NdN_d, that is, ΔTmax⁡\Delta T_{\max} changes simultaneously with both PaP_a and NdN_d. When 2.6≤Pa<4.1×1025 m−32.6 \le P_a < 4.1 \times10^{25}\,\mathrm{m}^{-3}, the maximum temperature difference ΔTmax⁡\Delta T_{\max} reaches its maximum value of 190.53190.53-196.45196.45 K when Nd=1.0×1025 m−3N_d = 1.0 \times10^{25}\,\mathrm{m}^{-3}, and the corresponding WpW_p is 5.585.58-3.923.92 nm. When 4.1≤Pa<20×1025 m−34.1 \le P_a < 20 \times10^{25}\,\mathrm{m}^{-3}, ΔTmax⁡\Delta T_{\max} reaches its maximum value of 196.75196.75-222.53222.53 K when Nd=0.9×1025 m−3N_d = 0.9 \times10^{25}\,\mathrm{m}^{-3}, and the corresponding WpW_p is 3.703.70-0.910.91 nm. When 20≤Pa<40×1025 m−320 \le P_a < 40 \times10^{25}\,\mathrm{m}^{-3}, ΔTmax⁡\Delta T_{\max} reaches its maximum value of 224.71224.71-232.13232.13 K when Nd=0.8×1025 m−3N_d = 0.8 \times10^{25}\,\mathrm{m}^{-3}, and the corresponding WpW_p is 0.840.84-0.440.44 nm When 40≤Pa≤100×1025 m−340 \le P_a \le100 \times10^{25}\,\mathrm{m}^{-3}, ΔTmax⁡\Delta T_{\max} reaches its maximum value of 232.55232.55-242.89242.89 K when Nd=0.7×1025 m−3N_d = 0.7 \times10^{25}\,\mathrm{m}^{-3}, and the corresponding WpW_p is 0.410.41-0.170.17 nm. That is, as the N type region doping concentration NdN_d increases, ΔTmax⁡\Delta T_{\max} first increases, reaches a maximum, and then decreases. For example, starting from ΔTmax⁡=241.10\Delta T_{\max} = 241.10 K at Nd=0.6×1025 m−3N_d = 0.6 \times10^{25}\,\mathrm{m}^{-3} and Pa=100×1025 m−3P_a = 100 \times10^{25}\,\mathrm{m}^{-3}, ΔTmax⁡\Delta T_{\max} increases, reaching its maximum of 242.93242.93 K at Nd=0.7×1025 m−3N_d = 0.7 \times10^{25}\,\mathrm{m}^{-3} and Pa=100×1025 m−3P_a = 100 \times10^{25}\,\mathrm{m}^{-3}, and then begins to decrease, such as reaching a maximum of 219.97219.97 K at Nd=1.0×1025 m−3N_d = 1.0 \times10^{25}\,\mathrm{m}^{-3} and Pa=100×1025 m−3P_a = 100 \times10^{25}\,\mathrm{m}^{-3}. The maximum values of ΔTmax⁡\Delta T_{\max} for N type region doping concentrations of 0.60.6, 0.70.7, 0.80.8, 0.90.9, and 1.0×1025 m−31.0 \times10^{25}\,\mathrm{m}^{-3} are 241.12241.12 K, 242.93242.93 K, 238.23238.23 K, 230.12230.12 K, and 219.97219.97 K, respectively. That is, the maximum temperature difference ΔTmax⁡=242.93\Delta T_{\max} = 242.93 K is achieved at Nd1=Nd2=0.7×1025 m−3N_{d1} = N_{d2} = 0.7 \times10^{25}\,\mathrm{m}^{-3} and Pa=100×1025 m−3P_a = 100 \times10^{25}\,\mathrm{m}^{-3}, which is also the maximum temperature difference obtained in this study. Corresponding to ΔTmax⁡=242.93\Delta T_{\max} = 242.93 K, V1=0.2124V_1 = 0.2124 V, V2=0.01924V_2 = 0.01924 V, and Wp=0.17W_p = 0.17 nm.

From Figure 15 (e), when the N type region doping concentration NdN_d is in the range of $1.5$-3.5×1025 m−33.5 \times10^{25}\,\mathrm{m}^{-3}, the ΔTmax⁡\Delta T_{\max} decreases with the increasing of NdN_d, and the corresponding PaP_a value also decreases. Therefore, there is no calculation for ΔT\Delta T under the condition of Nd>3.5×1025 m−3N_d > 3.5 \times10^{25}\,\mathrm{m}^{-3}. Additionally, for different NdN_d values, the law of ΔTmax⁡\Delta T_{\max} changing with PaP_a is different. When the N type region doping concentration NdN_d is in the range of 1.51.5-2.5×1025 m−32.5 \times10^{25}\,\mathrm{m}^{-3}, ΔTmax⁡\Delta T_{\max} varies with PaP_a in a parabolic pattern. As PaP_a increases, ΔTmax⁡\Delta T_{\max} first increases, reaches its maximum at the vertex of the parabola, and then gradually decreases. Moreover, the maximum value of ΔTmax⁡\Delta T_{\max} decreases as the doping concentration NdN_d in the N region increases. When NdN_d is 1.5×1025 m−31.5 \times10^{25}\,\mathrm{m}^{-3}, and the maximum value of ΔTmax⁡\Delta T_{\max} is 176.48176.48 K and the corresponding parameters are Pa=2×1025 m−3P_a = 2 \times10^{25}\,\mathrm{m}^{-3}, V1=0.1880V_1 = 0.1880 V, V2=0.02717V_2 = 0.02717 V, and Wp=8.22W_p = 8.22 nm. When the N type region doping concentration NdN_d increases to 2.0×1025 m−32.0 \times10^{25}\,\mathrm{m}^{-3}, the extremum point of ΔTmax⁡\Delta T_{\max} shifts to Pa=0.4×1025 m−3P_a = 0.4 \times10^{25}\,\mathrm{m}^{-3}, achieving a value of 151.04151.04 K, with corresponding parameters V1=0.1452V_1 = 0.1452 V, V2=0.01806V_2 = 0.01806 V, and Wp=23.20W_p = 23.20 nm. When Nd=2.5×1025 m−3N_d = 2.5 \times10^{25}\,\mathrm{m}^{-3}, the extremum point of ΔTmax⁡\Delta T_{\max} occurs at Pa=0.18×1025 m−3P_a = 0.18 \times10^{25}\,\mathrm{m}^{-3}, reaching 134.54134.54 K, with V1=0.1241V_1 = 0.1241 V, V2=0.01168V_2 = 0.01168 V, and Wp=34.54W_p = 34.54 nm. For N type region doping concentrations $N_d \ge 3.0×1025 m−33.0 \times10^{25}\ \mathrm{m}^{-3}, ΔTmax⁡\Delta T_{\max} decreases as PaP_{\mathrm{a}} increases, that is, ΔTmax⁡\Delta T_{\max} attains its maximum value at the minimum value of PaP_{\mathrm{a}}. When Nd=3.0×1025 m−3N_{\mathrm{d}} = 3.0 \times10^{25}\ \mathrm{m}^{-3}, the maximum value of ΔTmax⁡\Delta T_{\max} is 122.95 K, with Pa=0.11×1025 m−3P_{\mathrm{a}} = 0.11 \times10^{25}\ \mathrm{m}^{-3}, V1=0.1107V_{1} = 0.1107 V, V2=0.00613V_{2} = 0.00613 V, and Wp=43.26W_{\mathrm{p}} = 43.26 nm. When Nd=3.5×1025 m−3N_{\mathrm{d}} = 3.5 \times10^{25}\ \mathrm{m}^{-3}, the maximum value of ΔTmax⁡\Delta T_{\max} is 114.32 K, and the corresponding parameters are Pa=0.08×1025 m−3P_{\mathrm{a}} = 0.08 \times10^{25}\ \mathrm{m}^{-3}, V1=0.1038V_{1} = 0.1038 V, V2=0.00295V_{2} = 0.00295 V, and Wp=50.05W_{\mathrm{p}} = 50.05 nm.

From Figure 15 (b), (Figure 15c), (Figure 15f), and (Figure 15g), the externally applied voltages V2V_{2} and V1V_{1} at the emitter and collector increase with the base thickness and base concentration PaP_{\mathrm{a}}, and also increase with the emitter and collector concentrations NdN_{\mathrm{d}}. The reason is that according to equations (21) and (24), the interface voltage of the PN junction increases as carrier concentration increases, thus requiring a larger external voltage. From Figure 15 (d) and (Figure 15h), it can be observed that the base thickness decreases with increasing base concentration PaP_{\mathrm{a}} and increases with increasing emitter and collector concentrations NdN_{\mathrm{d}}, which aligns with equations (38) and (39).

Conclusion

In this study, an NPN junction thermoelectric transistor cooling device model composed of N-type Bi2Te2.97Se0.03\mathrm{Bi}_{2}\mathrm{Te}_{2.97}\mathrm{Se}_{0.03} and P-type Bi0.5Sb1.5Te3\mathrm{Bi}_{0.5}\mathrm{Sb}_{1.5}\mathrm{Te}_{3} is constructed. By separately regulating the externally applied voltages on the emitter and collector, and coupling the transistor effect, thermoelectric effect, and interface effect within the NPN heterostructure, the temperature at the forward-biased end (emitter) increases while releasing heat, and the temperature at the reverse-biased end (collector) decreases while absorbing heat, thereby forming a thermoelectric transistor refrigerator and enhancing its cooling performance. Using the equivalent circuit method to convert the PNP heterostructure into a common-base circuit of a junction thermoelectric transistor, When the doping concentration in the N region is Nd=0.6N_{\mathrm{d}} = 0.6–3.5×1025 m−33.5 \times10^{25}\ \mathrm{m}^{-3} and the doping concentration in the P region is Pa=0P_{\mathrm{a}} = 0–100×1025 m−3100 \times10^{25}\ \mathrm{m}^{-3}, the effects of different applied voltages on the maximum temperature difference between the two ends of the thermoelectric transistor device and the base region thickness are investigated. The results are as follows:

  1. Under different N type region doping concentrations NdN_{\mathrm{d}} and base (P type region) doping concentrations PaP_{\mathrm{a}}, as the voltage V2V_{2} applied to the emitter increases, the collector voltage V1V_{1}, the base depletion layer thickness WpW_{\mathrm{p}}, and the thermoelectric conversion efficiency η\eta all increase, while the temperature difference ΔT\Delta T between the two ends of the thermoelectric transistor decreases;

  1. When the N type region doping concentration NdN_{\mathrm{d}} is in the range of 0.60.6–1.0×1025 m−31.0 \times10^{25}\ \mathrm{m}^{-3}, ΔTmax⁡\Delta T_{\max} increases rapidly at first with increasing PaP_{\mathrm{a}}, reaches a certain inflection point, then increases slowly or even tends to stabilize. As the N type region doping concentration NdN_{\mathrm{d}} increases, ΔTmax⁡\Delta T_{\max} first increases, reaches a maximum at Nd=0.7×1025 m−3N_{\mathrm{d}} = 0.7 \times10^{25}\ \mathrm{m}^{-3}, and then decreases. When NdN_{\mathrm{d}} is greater than 1.5×1025 m−31.5 \times10^{25}\ \mathrm{m}^{-3}, ΔTmax⁡\Delta T_{\max} decreases as NdN_{\mathrm{d}} increases. When NdN_{\mathrm{d}} increases from 1.5×1025 m−31.5 \times10^{25}\ \mathrm{m}^{-3} to 3.5×1025 m−33.5 \times10^{25}\ \mathrm{m}^{-3}, ΔTmax⁡\Delta T_{\max} decreases from 176.51 to 114.32 K. When NdN_{\mathrm{d}} is in the range of 1.51.5–2.5×1025 m−32.5 \times10^{25}\ \mathrm{m}^{-3}, ΔTmax⁡\Delta T_{\max} varies with PaP_{\mathrm{a}} in a parabolic pattern, where ΔTmax⁡\Delta T_{\max} increases with increasing PaP_{\mathrm{a}}, reaches its maximum at the vertex of the parabola, and then decreases slowly. When Nd≥3.0×1025 m−3N_{\mathrm{d}} \geq3.0 \times10^{25}\ \mathrm{m}^{-3}, ΔTmax⁡\Delta T_{\max} decreases as PaP_{\mathrm{a}} increases, the maximum value of ΔTmax⁡\Delta T_{\max} is obtained at the minimum value of PaP_{\mathrm{a}}. Overall, as the N type region doping concentration NdN_{\mathrm{d}} increases, the minimum allowable base carrier concentration Pmin⁡P_{\min} decreases.

  1. The maximum temperature difference ΔTmax⁡\Delta T_{\max} obtained is ΔTmax⁡=242.89\Delta T_{\max} = 242.89 K under the conditions of emitter voltage V2=0.01925V_{2} = 0.01925 V, collector voltage V1=0.2124V_{1} = 0.2124 V, P type region

carrier concentration Pa=100×1025 m−3P_{\mathrm{a}} = 100 \times10^{25}\ \mathrm{m}^{-3}, and N type region carrier concentration Nd=0.7×1025 m−3N_{\mathrm{d}} = 0.7 \times10^{25}\ \mathrm{m}^{-3}. However, the corresponding base width Wp=0.17 nmW_{\mathrm{p}} = 0.17\ \mathrm{nm} is not only difficult to achieve but also poses a risk of breakdown due to its extremely small size. Therefore, in actual production, suitable doping concentrations and external voltages need to be selected based on the actual process and the results of the optimized design. Even if the base region width is limited to the ?nm level, when the carrier concentration in the N region (NdN_{\mathrm{d}}) is 1.5×1025 m−31.5 \times10^{25}\ \mathrm{m}^{-3}, the carrier concentration in the base region (PaP_{\mathrm{a}}) is 1.0×1025 m−31.0 \times10^{25}\ \mathrm{m}^{-3}, the emitter voltage V2V_{2} is 0.01686 V0.01686\ \mathrm{V}, the collector voltage V1V_{1} is 0.1838 V0.1838\ \mathrm{V}, and the base region width (WpW_{\mathrm{p}}) is 12.78 nm12.78\ \mathrm{nm}, the maximum temperature difference ΔTmax⁡\Delta T_{\max} that can be obtained is approximately 174.15 K174.15\ \mathrm{K}. Therefore, the thermoelectric transistor device, which combines the thermoelectric effect with transistor technology can effectively enhance the maximum temperature difference that thermoelectric cooling technology can achieve.

Acknowledgments

This work was financially supported by The National Key Research and Development Program of China [Grand No. 2017YFF0204706] and the Fundamental Research Funds for the Central Universities [Grant No. FRF-MP-18-005 and FRF-MP-19-005].

References

  1. [1]PELТIER J. Nouvelles experiences sur la caloricite des courants electrique[J]. Annales de Chimie et de Physique, 1834,56: 371-386.
  2. [2]J. Mao, G. Chen, Z. Ren. Thermoelectric cooling materials. Nat. Mater. 2021, 20, 454.
  3. [3]J. Yang, G. Li, H. Zhu, N. Chen, T. Lu, J. Gao, L. Guo, J. Xiang, P. Sun, Y. Yao, R. Yang, H. Zhao. Next-generation thermoelectric cooling modules based on high-performance Mg₃(Bi, Sb)₂ material. Joule 2022, 6, 193.DOI
  4. [4]Y. Xiao, H. Wu, H. Shi, L. Xu, Y. Zhu, Y. Qin, G. Peng, Y. Zhang, Z. H. Ge, X. Ding, L. D. Zhao. High-Ranged ZT Value Promotes Thermoelectric Cooling and Power Generation in n-Type PbTe. Adv. En-ergy Mater. 2022.DOI
  5. [5]Sun J-C, Su X-L, Yan Y-G, Liu W, Tan G-J, Tang X-F. Enhancing thermoelectric performance of n-type PbSe through forming solid solution with PbTe and PbS. ACS Appl. Energy Mater. 2020; 3: 2-8 (2020).DOI
  6. [6]Perumal S, Samanta M, Ghosh T, Shenoy U-S, Bohra AK, Bhattacharya S, Singh A, Waghmare U V, Biswas K. Realization of high thermoelectric figure of merit in GeTe by complementary Co-doping of Bi and In. Joule. 2019; 3: 2565-80.DOI
  7. [7]G.D. Mahan Introduction to thermoelectrics. APL Mater. 4 (2016), 104806.
  8. [8]J.T. Wei, L.L. Yang, Z. Ma, P.S. Song, M.L. Zhang, J. Ma, F.H. Yang, X.D. Wang, J. Mater. Review of current high-ZT thermoelectric materials. Sci. 55 (2020) 12642–12704.
  9. [9]M. Bala, A. Masarrat, V. Kumar, S. Ojha, K. Asokan, S. Annapoorni. Effect of thermal annealing on thermoelectric properties of BiₓSb₂−ₓTe₃ thin films grown by sputtering. J. Appl. Phys. 127 (2020), 245108.DOI
  10. [10]I. Malik, T. Sribastava, K.K. Surthi, C. Gayner, K.K. Kar, Enhanced thermoelectric performance of n-type Bi₂Te₃ alloyed with low cost and highly abundant sulfur, Mater. Chem. Phys. 255 (2020), 123598.DOI
  11. [11]J.L. Gao, T. Mao, T. Lv, Z.M. Li, G.Y. Xu. Thermoelectric performance of n-type (PbTe)₁₋ₓ(CoTe)ₓ composite prepared by high pressure sintering method. J. Mater. Sci.-Mater. El 29 (2018) 5327–5336.DOI
  12. [12]N.T. Hung, E.H. Hasdeo, A.R.T. Nugraha, M.S. Dresselhaus, R. Saito. Quantum Effects in the Thermoelectric Power Factor of Low-Dimensional Semiconductors. Phys. Rev. Lett. 117 (2016), 036602.
  13. [13]L.P. Hu, T.J. Zhu, X.H. Liu, X.B. Zhao. Point Defect Engineering of High-Performance Bismuth-Telluride-Based Thermoelectric Materials. Adv. Funct. Mater. 24 (2014) 5211–5218.DOI
  14. [14]B.C. Qin, Y. Xiao, Y.M. Zhou, L.D. Zhao. Thermoelectric transport properties of Pb–Sn–Te–Se system. Rare Metals 37 (2018) 343–350.
  15. [15]S. Bathula, M. Jayasimhadri, N. Singh, A.K. Srivastava, J. Pulikkotil, A. Dhar, R. C. Budhani. Enhanced thermoelectric figure-of-merit in spark plasma sintered nanostructured n-type SiGe alloys. Appl. Phys. Lett. 101 (2012), 213902.DOI
  16. [16]C. Lan, A.J. Minnich, G. Chen, Z.F. Ren. Enhancement of Thermoelectric Figure-of-Merit by a Bulk Nanostructuring Approach. Adv. Funct. Mater. 20 (2010) 357–376.
  17. [17]J.R. Sootsman, R.J. Pcionek, H.J. Kong, C. Uher, M.G. Kanatzidis. Strong Reduction of Thermal Conductivity in Nanostructured PbTe Prepared by Matrix Encapsulation. Chem. Mater. 18 (2006) 4993.DOI
  18. [18]A. Gueguen, P.F.P. Poudeu, C.P. Li, S. Moses, C. Uber, J.Q. He, V. Dravid, K. A. Paraskevopoulos, M.G. Kanatzidis. Thermoelectric Properties and Nanostructuring in the p-Type Materials NaPb₁₈₋ₓSnₓMTe₂₀ (M=Sb, Bi). Chem. Mater. 21 (2009) 1683–1694.DOI
  19. [19]G.H. Zhu, H. Lee, Y.C. Lan, X.W. Wang, G. Joshi, D.Z. Wang, J. Yang, D. Vashaee, H. Guilbert, A. Pillitteri, M.S. Dresselhaus, G. Chen, Z.F. Ren. Increased Phonon Scattering by Nanograins and Point Defects in Nanostructured Silicon with a Low Concentration of Germanium. Phys. Rev. Lett. 102 (2009), 196803.
  20. [20]L.D. Hicks, M.S. Dresselhaus. Effect of quantum-well structures on the thermoelectric figure of merit. Phys. Rev. B 47 (1993) 12727.
  21. [21]R. Venkatasubramanian, E. Siivola, T. Colpitts, B. O’Quinn. Thin-film thermoelectric devices with high room-temperature figures of merit. Nature 413 (2001) 597–602.
  22. [22]T.C. Harman, M.P. Walsh, B.E. Laforge, G.W. Turner, J. Electron. Nanostructured thermoelectric materials. Mater. 34 (2005) L19–L22.
  23. [23]A.I. Boukai, Y. Bunimovich, J. Tahir-Kheli, J.K. Yu, W.A. Goddard, J.R. Heath. Silicon nanowires as efficient thermoelectric materials. Nature 451 (2008) 168–171.DOI
  24. [24]B. Hinterleitner, I. Knapp, M. Poneder, Y.P. Shi, H. Muller, G. Eguchi, C. Eisenmenger-Sittner, M. Stoger-Pollach, Y. Kakefuda, N. Kawamoto. Thermoelectric performance of a metastable thin-film Heusler alloy. Nature 576 (2019) 85.DOI
  25. [25]曹海山. 热电制冷技术进展与展望[J]. 制冷学报, 2022, 43 (04): 26–34.
  26. [26]Feliczo J-C, Uenuma M, Fujii M-N, Uraoka Y. Improved Thermoelectric Power Factor of InGaZnO/SiO₂ Thin Film Transistor via Gate-Tunable Energy Filtering. IEEE. Electron. Device. L. 2021; 42: 1236-1239.DOI
  27. [27]Bejenari I, Kantser V, Balandin AA. Thermoelectric properties of electrically gated bismuth telluride nanowires. Phys. Rev. B. 2010; 81: 075316.DOI
  28. [28]Qin D-L, Pan F, Zhou J, Xu Z-B, Deng Y. High ZT and performance controllable thermoelectric devices based on electrically gated bismuth telluride thin films. Nano Energy. 2021; 89: 106472.DOI
  29. [29]Y ang F, Wu J, Suwardi A, Zhao Y-S, Laing B-Y, Jiang J, Xu J-W, Chi D-Z, Hippalgaonkar K, Lu J-P , Ni, Z-H. Gate-Tunable Polar Optical Phonon to Piezoelectric Scattering in Few-Layer Bi₂O₂Se for High-Performance Thermoelectrics. Adv. Mater. 2021; 4: 33.DOI
  30. [30]Wu X-M, Gao G-Y, Hu L, Qin D. 2D Nb2SiTe4 and Nb2GeTe4: promising thermoelectric figure of merit and gate-tunable thermoelectric performance. Nanotechnology. 2021; 32: 245203.DOI
  31. [31]Bohang Nan, Tao Guo, Hao Deng, Guangbing Zhang, Ran Shi, Jiakai Xin, Chen Tang, Guiying Xu, Output performance improvement for thermoelectric transistor with the consideration of the Thomson effect and geometry optimization, Applied Energy, 2024, 357, 122523DOI
  32. [32]Nan B H, Xu G Y, Yang Q X, Zhang B, Zhou X J, Innovative design and optimized performance of thermoelectric transistor driven by the Seebeck effect, Energy Conversion and Management[J]. 2023, 283, 116880DOI
  33. [33]Nan Bohang, Xu Guiying, Liu Wu-Ming, Yang Quanxin, Zhang Bin, Dong Yuan, Tie Jian, Guo Tao, Zhou Xiaojing, High thermoelectric performance of PNP abrupt heterostructures by independent regulation of the electrical conductivity and Seebeck coefficient, Materials Today Communications, 2022, 31: 103343.DOI
  34. [34]M. Zebarjadi, A. Shakouri, K. Esfarjani. Thermoelectric transport perpendicular to thin-film heterostructures calculated using the Monte Carlo technique Phys. Rev. B 74(2006), 195331.DOI
  35. [35]V.N. Agarev. Nonstationary thermoelectric power in multilayered structures with p-n junctions. Semiconductors 31 (1997) 784.DOI
  36. [36]K. Kim, J. Park, S.U. Kim, O. Kwon, J.S. Lee, S.H. Park, Y.K. Choi. Thermopower profiling of a silicon p-n Junction. Appl. Phys. Lett. 90 (2007) 43107.
  37. [37]X.Y. Wang, H.J. Wang, B. Xiang, L.W. Fu, H. Zhu, D. Chai, B. Zhu, Y. Yu, N. Gao, Z. Y. Huang, F.O. Zu. Thermoelectric Performance of Sb₂Te₃-Based Alloys is Improved by Introducing PN Junctions. ACS Appl. Mater. Interfaces 10 (2018) 23277.DOI
  38. [38]I.I. Balmush, Z.M. Dashevskii, A.I. Kasiyan. Potential Distribution in Semiconductor Structure with p−n Junction in the Presence of Temperature Gradient. Fiz. i Tekh. Poluprovodn. 20 (1986)1541 (In Russian).
  39. [39]Z.M. Dashevsky, S. Ashmontas, L. Vingelis, I. Gradauskas, Al. Kasian. The thermoelectric power on p-n junction. In 15th Int. Conf. on Thermoelectrics. IEEE. 336 (1996).
  40. [40]A.A. Zakhidov, Y.I. Ravich, D.A. Pchenoy-Severin. Thermopower enhancement and optimal ZT in p-n junction arrays. In 18th Int. Conf. on Thermoelectrics. IEEE. 193 (1999).
  41. [41]Y.I. Ravich, D.A. Pshenai-Severin. Thermoelectric figure of merit of a p-n junction. Semiconductors 35 (2001) 1161–1165.
  42. [42]Chen Z W, Jian Z Z, Li W, et al. Lattice dislocations enhancing thermoelectric PbTe in addition to band convergence [J]. Advanced Materials, 2017, 29(23): 1606768.DOI
  43. [43]He J, Xu J T, Liu G Q, et al. Enhanced thermopower in rock-salt SnTe–CdTe from band convergence [J]. RSC Advances, 2016, 6(38): 32189-32192.DOI
  44. [44]V. A. Kulbachinskii, M. Inoue, M. Sasaki, H. Negishi, W. X. Gao, K. Takase, Y. Giman, P. Lostak, and J. Horak. Valence-band changes in Sb₂−xInxTe₃ and Sb₂Te₃−ySey by transport and Shubnikov–de Haas effect measurements. Phys. Rev. B 50, 16921pubmed.ncbi.nlm.nih.gov/9980190
  45. [45]Xu G-Y, Ren P, Lin T, Wu X-F, Zhang Y-H, Niu S-T, Bailey TP. Mechanism and application method to analyze the carrier scattering factor by electrical conductivity ratio based on thermoelectric property measurement. J. Appl. Phys. 2018; 123: 015101.
  46. [46]Wang S-Y, Tan G-J, Xie W-J, Zheng G, Li H, Yang J-H, Tang X-F. Enhanced thermoelectric properties of Bi₂(Te₁−xSex)₃-based compounds as n-type legs for low temperature power generation. J. Mater. Chem. 2012; 22: 20943.DOI
  47. [47]Dai W, Liu W-K, Yang J, Xu C, AlabastrI A, Liu C, Nordlander P, Guan Z-Q, Xu H-X. Giant photothermoelectric effect in silicon nanoribbon photodetectors. Light Sci. Appl. 2020; 9: 120.DOI
  48. [48]Ge Y, He K, Xiao L-H, Yuan W-Z, Huang S-M. Geometric optimization for the thermoelectric generator with variable cross-section legs by coupling finite element method and optimization algorithm. Renew Energ. 2022; 183: 294.DOI
  49. [49]Fu D, Levander A-X, Zhang R, Ager III J-W, Wu J. Electrothermally driven current vortices in inhomogeneous bipolar semiconductors. Phys. Rev. B. 2011; 84: 045205.DOI
  50. [50]Lv T, Li Z-M, Yang Q-X, Benton A, Zheng H-T, Xu G-Y. Synergistic regulation of electrical-thermal effect leading to an optimized thermoelectric performance in Co doping n-type Bi₂(Te₀.₉₇Se₀.₀₃)₃. Intermetallics. 2020; 118: 106683.DOI
  51. [51]Chavez R, Angst S, Hall J, Stoetzel J, Kessler V, Bitzer L, Maculewicz F, Benson N, Wiggers H, Wolf D, Schierning G, Schmechel R. High Temperature Thermoelectric Device Concept Using Large Area PN Junctions. J. Electron. Mater. 2014; 43: 2376.DOI

Paper details

vlnc:W_qnrv78t3
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents