betaFeedback

WorksPhysics and Astronomy

The Intercalation Chemistry of the Disordered RockSalt Li3V2O5 Anode from Cluster Expansions and Machine Learning Interatomic Potentials

Abstract

Disordered rocksalt (DRX) Li3V2O5 is a promising candidate for anode in rechargeable lithium-ion batteries because of its ideal low voltage, high rate capability, and superior cycling stability. Herein, we presents a comprehensive study of intercalation chemistry of the DRX-Li3V2O5 anode using density functional theory calculations combined with machine learning cluster expansions and interatomic potentials. The predicted voltage profile of the disordered Li3V2O5 anode at room temperature based on Monte Carlo simulations with a fitted cluster expansion model is in excellent agreement with experiments. In contrast to previous DFT results, we find that Li ions predominately intercalate into tetrahedral sites during charging, while the majority of Li and V ions at octahedral sites remain stable. In addition, MD simulations with a fitted moment tensor potential attribute the fast-charging capability of DRX-Li3V2O5 to the facile diffusivity of Li+ via tetrahedral - octahedral - tetrahedral pathway. We further suggest tuning the Li:V ratio as a means to trade off increased lithiation capacity and decreased anode voltage in this system. This work provides in-depth insights into the high-performance DRX-Li3V2O5 anode, and paves the way to the discovery of other disordered anode materials.

further suggest tuning the Li:V ratio as a means to trade off increased lithiation capacity and decreased anode voltage in this system. This work provides in-depth insights into the high-performance DRX-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} anode, and paves the way to the discovery of other disordered anode materials.

Introduction

Rocksalt oxides have been extensively studied as electrodes for rechargeable lithium-ion batteries (LIBs).[1] As the name implies, the O2−\mathrm{O}_{2}^{-} anions in rocksalt oxides are arranged in a close-packed face-centered-cubic (fcc) framework, with the cations occupying the tetrahedral and octahedral interstitial sites, as shown in Figure 1(a). For instance, the common layered transition metal (M) oxide LiMO2\mathrm{LiMO}_{2} cathode used in LIBs is formed by an ordered arrangement of Li and M in this framework. In the past decade or so, lithium-rich disordered rocksalt (DRX) oxides have emerged as a promising class of alternative electrode materials with extraordinarily high specific capacities and high rate capabilities.[1, 2, 3, 4]

While DRX materials have been extensively studied as cathodes, relatively few have been explored as anodes.[5, 6, 7] Among the most promising is the DRX-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} recently reported by Liu et al. 5. The DRX-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} anode operates at a near-optimal average voltage of ∼0.6\sim0.6 V vs Li/Li+{}^{+} - high enough to alleviate the safety concerns attributed to Li plating that occurs during fast charge/discharge of the commercial graphite anode used in LIBs. At the same time, it is substantially lower than the 1.5 V operating voltage of lithium titanate, thereby yielding a much higher energy density.

Despite its great promise, there remains major ambiguity on the intercalation chemistry of DRX-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5}. Previously, Zheng et al. 8 proposed that the related DRX-Li0.78+xV0.75O2\mathrm{Li}_{0.78+x}\mathrm{V}_{0.75}\mathrm{O}_{2} anode undergoes a conversion-type reaction, in which the single phase material converts to VO2\mathrm{VO}_{2} and Li2O\mathrm{Li}_{2}\mathrm{O} as it is discharged to 0.55 V vs Li/Li+{}^{+}. However, previous density functional theory (DFT) calculations by the present authors attributed the low voltage and high rate capability of DRX-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} to a redistributive lithium intercalation mechanism with low energy barriers.[5] These initial conclusions were reached based on 0K DFT calculations with small model cells, which did not fully explore the configurational space of the DRX anode at finite temperatures.

In this work, we revisit the intercalation chemistry of the DRX-Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_{2}\mathrm{O}_{5} (0≤x≤20 \le x \le2) at finite temperatures using large-scale simulations with machine-learned energy models. Monte Carlo simulations using a fitted cluster expansion model predict that Li primarily inserts into the tetrahedral sites of DRX-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} while Li occupancy in octahedral sites remains largely unchanged, in contrast with earlier DFT results. Molecular dynamics (MD) simulations using a machine learning interatomic potential reveal that Li+\mathrm{Li}^{+} diffusivity reaches the maximum at intermediate states of charge, but sharply decreases at the start of charge/discharge. The exceptionally high rate capability and superior cycling stability of DRX-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} anode are a result of facile diffusion of Li ions through tetrahedral - octahedral - tetrahedral pathway, consistent with previous nudged elastic band calculations.

Methods

Structure model

Figure 1(a) shows the crystal structure of DRX-Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_{2}\mathrm{O}_{5}, which has an fcc lattice with spacegroup Fm3ˉmFm\bar{3}m. The O2−\mathrm{O}^{2-} anions occupy 4a4a sites. The initial composition of Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} has a cation: anion ratio of 1:1. Based on our previous studies, the lowest DFT energy structure is one where all Li/V cations fully occupy the octahedral 4b4b sites.[5] Henceforth, we will use the anion-normalized composition, e.g., [Li0.6V0.4]octO[\mathrm{Li}_{0.6}\mathrm{V}_{0.4}]_{\mathrm{oct}}\mathrm{O} for Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5}, to emphasize the site occupancies. During discharge, inserted Li+\mathrm{Li}^{+} also occupy the tetrahedral 8c8c sites, forming Lixtet[LiyV0.4]octO\mathrm{Li}^{\mathrm{tet}}_{x}[\mathrm{Li}_{y}\mathrm{V}_{0.4}]_{\mathrm{oct}}\mathrm{O}.

For more costly DFT and climbing image nudged elastic band (NEB) calculations, a set of 64 special quasi-random structures (SQSs)[9] with formula Li19V13O32\mathrm{Li}_{19}\mathrm{V}_{13}\mathrm{O}_{32} (corresponding to [Li0.59375V0.40625]octO[\mathrm{Li}_{0.59375}\mathrm{V}_{0.40625}]_{\mathrm{oct}}\mathrm{O}) were generated using 2×2×22 \times2 \times2 supercells of the conventional rocksalt cubic unit cell. The three relaxed SQS structures with the lowest energies were used for site energy and migration barrier calculations.

Density functional theory calculations

Spin-polarized density functional theory (DFT) calculations were performed using the Vienna ab initio simulation (VASP) package within the projected-augmented wave method. [10, 11] The Perdew-Burke-Ernzerhof (PBE) functional [12] was used for the structural relaxation and electronic energy calculations with an effective Hubbard UU [13, 14] value of 3.25 eV for V, which is in line with the parameters used in the Materials Project. [15] All calculations were initialized in a ferromagnetic high-spin configuration. A plane wave energy cutoff of 450 eV and a kk-point density of at least 100 per reciprocal volume were adopted. The electronic energies and forces were converged to 10−510^{-5} eV and 0.02 eV Å−1^{-1}, respectively.

Li site energies

The Li site energies were determined by inserting one Li+^{+} into each symmetrically distinct tetrahedral site of the three lowest energy SQSs. The Litet^{\mathrm{tet}} site energies are given by the following expression:

ELitet=EDoped−EHost−ELi0(1)E_{\mathrm{Li}^{\mathrm{tet}}} = E_{\mathrm{Doped}} - E_{\mathrm{Host}} - E_{\mathrm{Li}}^{0} \tag*{(1)}

where EDopedE_{\mathrm{Doped}}, EHostE_{\mathrm{Host}}, and ELi0E_{\mathrm{Li}}^{0} are the DFT calculated energies of the SQS with one Li atom inserted into the tetrahedral site, the SQS and Li metal, respectively.

Order parameter

To quantify the degree of ordering, the average Steinhardt order parameter (Dˉj\bar{D}_j) [16] over all atoms in each structure was calculated. The Steinhardt order parameter DjD_j for each atom j and the bounded atom kk in the structure is given by:

Dj=1nbj∑k∈bonded[Sij+Skk−2Sjk](2)D_j = \frac{1}{n_b^j}\sum_{k\in\mathrm{bonded}} \left[S_{ij}+S_{kk}-2S_{jk}\right] \tag*{(2)}
Sjk=∑−l≤m≤lqlmj(qlmk)∗(3)S_{jk}=\sum_{-l\le m\le l}q_{lm}^{j}(q_{lm}^{k})^{*} \tag*{(3)}

where SjkS_{jk} is the correlation between atoms jj and kk, nbjn_b^j is the number of the atoms bonded to the atom jj. For fcc cation lattice, nbj=12n_b^j=12 and l=6l=6 is used. For a perfect ordered crystal such as the layered Rˉ3m\bar{R}3m LiVO2_2, Dˉj=0\bar{D}_j=0. The higher the degree of disordering of a system, the larger the value of Dˉj\bar{D}_j. For example in glass material, the Dˉj\bar{D}_j ranges from 0.2 ∼\sim 0.3.[16] In this work, the Dˉj\bar{D}_j was calculated using the pyscal package.[17]

Cluster expansion

A cluster expansion (CE) lattice model[18, 19, 20, 21] for the DRX Lix_x[Liy_yV0.4_{0.4}]oct^{\mathrm{oct}}O system was parameterized using the Clusters Approach to Statistical Mechanics (CASM) software.[22, 23] The DFT calculated total energies of the structure configurations were mapped into an expansion of crystal basis functions Φ(m⃗,σˉ)\Phi(\vec{m},\bar{\sigma}) as given by

E(σˉ)=∑m⃗V(m⃗)Φα(m⃗,σˉ)(4)E(\bar{\sigma})=\sum_{\vec{m}}V(\vec{m})\Phi_{\alpha}(\vec{m},\bar{\sigma}) \tag*{(4)}

where Φ(m⃗,σˉ)=∏n=1Nϕ(n,mn,σn)\Phi(\vec{m},\bar{\sigma})=\prod_{n=1}^{N}\phi(n,m_n,\sigma_n) is a polynomial of site basis functions ϕ(n,mn,σn)\phi(n,m_n,\sigma_n), and V(m⃗)V(\vec{m}) are the fitted effective cluster interactions (ECIs).

To fit the CE, the [Li/V/Va]oct^{\mathrm{oct}} and [Li/Va]tet^{\mathrm{tet}} configurations of different compositions were exhaustively enumerated in cubic rocksalt supercells up to a maximum cell size of 25 times the primitive unit cell. It should be noted that V is allowed to occupy only the 4b octahedral sites, given that its occupancy at tetrahedral sites is extremely energetically unfavorable (EVtet∼3E_{Vtet}\sim3 eV). Li can occupy either the 4b octahedral or 8c tetrahedral sites. We note that only structures with basis deformation <0.1<0.1 were used in the fit, which is a typical threshold used to identify structures that match with the primitive unit cell. The basis deformation is determined by the mean-square atomic displacement relative to the positions of the ideal ions in cubic rocksalt lattice. [22] In total, DFT computed energies of about 4500 symmetrically distinct configurations were used to fit the ECIs. All symmetrically distinct pairs, triplets, and quadruplets in the rocksalt cell within a radius of 7.1 Å, 4.1 Å and 4.1 Å, respectively, were used to construct the CE model.

The ECIs were obtained from a L1L_1 regularized linear regression fit with α=10−8\alpha= 10^{-8} to minimize over-fitting (Figure S4). The cross-validation mean absolute error in energies is 8.94 meV atom−1^{-1}.

Cross-validation score and root mean square error as a function of the regularization parameter

Figure S4. Cross-validation (CV) score and root mean square error (RMSE) of the fitted cluster expansion model as a function of the regularization parameter (α\alpha).

The calculated formation energy of Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_2\mathrm{O}_5 structures is given by

Eform[Li3+xV2O5]=E[Li3+xV2O5]−(1−x2)E[Li3V2O5]−x2E[Li5V2O5](5)E_{\mathrm{form}}[\mathrm{Li}_{3+x}\mathrm{V}_2\mathrm{O}_5] = E[\mathrm{Li}_{3+x}\mathrm{V}_2\mathrm{O}_5] - \left(1-\frac{x}{2}\right)E[\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5] - \frac{x}{2}E[\mathrm{Li}_5\mathrm{V}_2\mathrm{O}_5] \tag*{(5)}

Monte Carlo simulations

Monte Carlo (MC) simulations were performed using the fitted cluster expansion model. A 5×5×55 \times5 \times5 supercell (2000 sites) was used for these simulations; larger supercells produced similar results (see Figure S5). Canonical MC simulations were performed at the [Li0.6V0.4]Ooct[\mathrm{Li}_{0.6}\mathrm{V}_{0.4}]_{\mathrm{O}}^{\mathrm{oct}} composition to probe the temperature under which the system undergoes an order-disorder transition.

Monte Carlo simulations of order-disorder phase transition of Li₃V₂O₅ in the 10×10×10 supercell

Figure S5. Monte Carlo simulations of order-disorder phase transition of Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5 in the 10×10×1010 \times10 \times10 supercell.

Semi-grand canonical MC (GCMC) simulations at 300 K were performed to study the intercalation of Li ions into the DRX-Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5 structure. In a semi-grand canonical ensemble, the composition and energy of the system with a fixed number of sites were allowed to fluctuate while the temperature (TT) and the chemical potentials of Li (μLi\mu_{\mathrm{Li}}) and V (μV\mu_{\mathrm{V}}) were externally imposed. The chemical potentials were referenced to that of bulk Li and V metals, which have μLi=μV=0\mu_{\mathrm{Li}} = \mu_{\mathrm{V}} = 0. The semi-GCMC simulations were carried out by scanning μLi\mu_{\mathrm{Li}} with a step of δμLi=0.01\delta\mu_{\mathrm{Li}} = 0.01 eV at constant μV\mu_{\mathrm{V}} within the chemical potential ranges of −2.0≤μLi≤0.0-2.0 \le\mu_{\mathrm{Li}} \le0.0 and −2.0≤μV≤0.0-2.0 \le\mu_{\mathrm{V}} \le0.0 at 300 K. The initial disordered structures were obtained from equilibrated semi-GCMC simulations by heating the system from 5 K up to 1500 K at fixed chemical potentials. In this work, the semi-GCMC simulations were performed on only Li and vacancy occupancy in the tetrahedral and octahedral sites, while all V ions were fixed in the initial equilibrated octahedral sites due to the large V migration barriers.

The voltage of an electrochemical cell was related to the Li chemical potential of the electrodes according to the Nernst equation:

V=−(μLi−μLi0)/e(6)V = -(\mu_{Li} - \mu_{Li}^{0})/e \tag*{(6)}

where μLi\mu_{Li} is the chemical potential of Li in DRX-Li3+x_{3+x}V2_2O5_5, μLi0\mu_{Li}^{0} is the reference chemical potential of Li metal and ee is the elementary charge.

Moment tensor potential

A machine learning interatomic potential (ML-IAP) based on the moment tensor potential (MTP) formalism[24] was developed for DRX-Li3+x_{3+x}V2_2O5_5 using a protocol similar to that developed by Qi et al. 25 for lithium superionic conductors. The initial training structures included DFT calculated ground state structures in the Li-V-O chemical space (supercells of Li2_2O, Li3_3VO4_4, LiV2_2O5_5 and LiVO2_2 with lattice parameters larger than 10 Å). To further sample the energy landscape of different Li/V arrangements, a set of SQSs with compositions Li19_{19}V13_{13}O32_{32} ([Li0.59375_{0.59375}V0.40625_{0.40625}]oct^{\mathrm{oct}}O) ≈\approx Li3_3V2_2O5_5), Li25_{25}V13_{13}O32_{32}([Li0.1875_{0.1875}]tet^{\mathrm{tet}}[Li0.59375_{0.59375}V0.40625_{0.40625}]oct^{\mathrm{oct}}O) ≈\approx Li4_4V2_2O5_5) and Li32_{32}V13_{13}O32_{32}([Li0.40625_{0.40625}]tet^{\mathrm{tet}}[Li0.59375_{0.59375}V0.40625_{0.40625}]oct^{\mathrm{oct}}O) ≈\approx Li5_5V2_2O5_5) were generated in 2×2×2 supercells of the conventional rocksalt cubic unit cell. It should be noted that changes in the occupancy of tetrahedral and octahedral sites in SQSs can occur upon DFT relaxation. The SQS with the lowest energy configuration of each composition were included in the fitting procedure.

Non-spin polarized ab initio molecular dynamics (AIMD) simulations using NVT ensembles were performed on relaxed supercells of all initial structures with a plane-wave energy cut-off of 280 eV and Gamma kk-point. To diversify the sampled local environments, the simulations were carried out at three strains (0, ±0.05\pm0.05) and four temperatures (300 K - 1200 K at an interval of 300 K). All simulations were performed for at least 30 ps with a 2 fs timestep using Nose-Hoover thermostat. [26, 27] The training structures were collected from 15 ps-equilibrated runs at 0.1 ps intervals, and more accurate energies and forces were obtained by static self-consistent calculations with a kk-point density of at least 100 per reciprocal volume and an energy cutoff of 520 eV.

Molecular dynamics simulations

Molecular dynamic (MD) simulations were performed in the NpTNpT ensemble to investigate the Li+^+ diffusion properties of DRX-Li3_3V2_2O5_5 using the fitted MTP potential. The time step of all MD calculations was set to 1 fs, and the total simulation time was at least 1 ns. The diffusivity (DLi+D_{\mathrm{Li}^+}) of Li+^+ was calculated by performing a linear fitting of the mean square displacement (MSD) versus 2dt2dt:

D=12dt⟨[Δr(t)]2⟩(7)D = \frac{1}{2dt}\langle[\Delta r(t)]^2 \rangle \tag*{(7)}

where dd is the dimensionality factor, which equals 3 for bulk structures. ⟨[Δr(t)]2⟩\langle[\Delta r(t)]^2 \rangle is the average MSD over a time duration tt. The activation energy of EaE_a was determined by the Arrhenius relationship,

D=D0exp⁡(−Ea/kT)(8)D = D_0 \exp(-E_a/kT) \tag*{(8)}

where D0D_0 is the maximum diffusivity at infinite temperature, kk is the Boltzmann constant and T is the temperature.

All the training, evaluations and MD simulations were performed using MLIP, [28, 29] Large-scale Atomic/Molecular Massively Parallel Simulator (LAMMPS) [30] and the open-source Materials Machine Learning (maml) Python package. [31]

Diffusion barriers

The migration barriers of Li+\mathrm{Li}^{+} and Vn+\mathrm{V}^{n+} (n=3n=3, 4) vacancy were calculated using the climbing image nudged elastic band (CI-NEB) method.[32, 33] All NEB calculations were performed in three SQSs with the lowest DFT total energy created in the previous sections. For Li+\mathrm{Li}^{+} migration barriers, the starting point of each NEB calculation was determined by inserting one Li+\mathrm{Li}^{+} into the tetrahedral site, and then the structure was fully relaxed. Five linearly interpolated intermediate images were used to generate the initial guess for the minimum energy path. For Litet\mathrm{Li}_{\mathrm{tet}} in varied local environments, the energy barriers for the Li+\mathrm{Li}^{+} hoping were calculated in three configurations with the lowest Litet\mathrm{Li}_{\mathrm{tet}} site energy. The kinetically resolved activation (KRA)[34] Li+\mathrm{Li}^{+} migration barrier (ΔEKRA\Delta E_{KRA}), which is independent of hop direction, was determined by the following expression:

ΔEKRA=E(σt)−12(E(σi+E(σf))(9)\Delta E_{KRA} = E(\sigma_t) - \frac{1}{2}\left(E(\sigma_i + E(\sigma_f)\right) \tag*{(9)}

where E(σt)E(\sigma_t), E(σiE(\sigma_i and E(σf)E(\sigma_f) refer to the energy of the activated transition state, the initial state and the end state from the CI-NEB calculations, respectively. The PBE functional without Hubbard UU was adopted to avoid the possible mixing of the diffusion barrier with a charge transfer barrier.[35] The force and energy convergence criterion was 0.05 eV/Å and 5×10−55 \times10^{-5} eV.

Results

Li-V-O phase diagram

Figure 1(b) shows the DFT-calculated Li-V-O phase diagram at 0 K. Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} ([Li0.6V0.4]octO[\mathrm{Li}_{0.6}\mathrm{V}_{0.4}]_{\mathrm{oct}}\mathrm{O}), represented by the red square, is unstable at 0 K relative to LiVO2\mathrm{LiVO}_{2} and Li3VO4\mathrm{Li}_{3}\mathrm{VO}_{4}. Both ordered layered and DRX-LiVO2\mathrm{LiVO}_{2} as well as ordered Li3VO4\mathrm{Li}_{3}\mathrm{VO}_{4} have been explored as potential LIB anodes.[36, 37, 38] All three electrode materials have a cation: anion ratio of 1:1 and differ purely in their Li: V ratio and therefore active redox couple. Li3VO4\mathrm{Li}_3\mathrm{VO}_4 has a formal vanadium oxidation state of 5+, and all cations are ordered in tetrahedral sites. It can therefore be represented using the anion-normalized composition of [Li0.75V0.25]tetO[\mathrm{Li}_{0.75}\mathrm{V}_{0.25}]^{\mathrm{tet}}\mathrm{O}. LiVO2\mathrm{LiVO}_2, on the other hand, has full octahedral occupancy like Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5 and a formal V oxidation state of 3+. It can therefore be represented using the anion-normalized composition of [Li0.5V0.5]octO[\mathrm{Li}_{0.5}\mathrm{V}_{0.5}]^{\mathrm{oct}}\mathrm{O}. It should be noted that Li2O\mathrm{Li}_2\mathrm{O} ([Li2]tetO[\mathrm{Li}_2]^{\mathrm{tet}}\mathrm{O}) also has a cubic rocksalt structure with full occupancy in the tetrahedral sites and a cation: anion ratio of 2.

Crystal structure and calculated phase diagram of disordered rocksalt Li3+xV2O5

Figure 1. (a) The crystal structure of disordered rocksalt Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_2\mathrm{O}_5. Red: O2−\mathrm{O}^{2-} anions forming an fcc sublattice. Light blue: Li+\mathrm{Li}^{+} in tetrahedral interstitials. Green/purple: Disordered Li+/V2+−4+\mathrm{Li}^{+}/\mathrm{V}^{2+}-4+ in octahedral interstitials. (b) Calculated phase diagram of Li-V-O chemical system at 0 K. The green circles refer to ground states and the red square refers to the metastable phase. The red dashed line refers to the limit of V2+\mathrm{V}^{2+} oxidation state. The blue dashed line refers to the lithiation pathway in DRX-Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5.

During charging, lithiation of [Li0.6V0.4]octO[\mathrm{Li}_{0.6}\mathrm{V}_{0.4}]^{\mathrm{oct}}\mathrm{O} occurs along the pathway indicated by the dashed blue line. The thermodynamically most favorable pathway is a conversion reaction given by the phase triangle of Li2O\mathrm{Li}_2\mathrm{O}-Li3VO4\mathrm{Li}_3\mathrm{VO}_4-LiVO2\mathrm{LiVO}_2([Li2]tetO[\mathrm{Li}_2]^{\mathrm{tet}}\mathrm{O}-[Li0.75V0.25]tetO[\mathrm{Li}_{0.75}\mathrm{V}_{0.25}]^{\mathrm{tet}}\mathrm{O}-[Li0.5V0.5]octO[\mathrm{Li}_{0.5}\mathrm{V}_{0.5}]^{\mathrm{oct}}\mathrm{O}). However, kinetic considerations may favor lithium insertion instead of conversion, as has been observed experimentally.[5] The ultimate limit of insertion into the rock salt Li1−xVxO\mathrm{Li}_{1-x}\mathrm{V}_x\mathrm{O} is given by the red dashed line representing Li2−2xVxO\mathrm{Li}_{2-2x}\mathrm{V}_x\mathrm{O}, i.e., a V2+\mathrm{V}^{2+} oxidation state. For a V cation content of 0.4, i.e., Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5, this limit is given by Li1.2V0.4O\mathrm{Li}_{1.2}\mathrm{V}_{0.4}\mathrm{O} or Li6V2O5\mathrm{Li}_6\mathrm{V}_2\mathrm{O}_5. Experimentally, this limit is never reached and the highest lithiated state has a composition of Li1V0.4O\mathrm{Li}_{1}\mathrm{V}_{0.4}\mathrm{O} or Li5V2O5\mathrm{Li}_5\mathrm{V}_2\mathrm{O}_5. [5]

Li+\mathrm{Li}^{+} insertion into the Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5 anode at 0 K were studied by DFT calculations. Figure 2(a) shows the DFT calculated pseudo-binary Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5-Li5V2O5\mathrm{Li}_5\mathrm{V}_2\mathrm{O}_5 phase diagram with the candidate structures colored in terms of their basis deformation. The larger the basis deformation, the greater the deviation of the DFT-relaxed structure from the ideal cubic rocksalt lattice. At x=0x = 0, low energy structures have low basis deformation and Li/V atoms are all in octahedral sites. At x≥0.5x \ge0.5, the DFT ground states comprise phases that are highly distorted (basis deformation >0.1> 0.1) from the parent cubic rocksalt lattice; the cubic phases (basis deformation ≤0.1\le0.1) are metastable. A Li site occupancy analysis of DFT ground states structures (Figure 2(b)) indicates that redistribution of Li from octahedral sites to tetrahedral sites occurs at x∼0.75x \sim0.75, where the occupancy of Lioct\mathrm{Li}^{oct} sharply decreases to 0.1 and the occupancy of Litet\mathrm{Li}^{tet} increases to 0.65. These results are qualitatively in line with previous DFT studies. [5] However, this redistribution of Li is accompanied by a considerably large volume change (∼20%\sim20\%) and lattice distortion, contradicting with the experimental observations that the anode retains a stable cubic lattice with a small volume change of 5.9%. [5] In contrast, the Li site occupancy analysis of metastable cubic phases (Figure 2 (c)) suggests that a redistribution of Li only takes place at the end of charging. The volume change of these metastable cubic phases ranges from 8 to 15%, which is close to the experimental results. [5]

DFT calculated pseudo-binary compound phase diagram, site occupancy evolution, and relative energy and disorder distributions

Figure 2. (a) DFT calculated pseudo-binary Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5-Li5V2O5\mathrm{Li}_5\mathrm{V}_2\mathrm{O}_5 compound phase diagram. The configurations are colored in terms of their basis deformation. The red line represents the convex hull of the cubic phase, i.e., structures with low basis deformation (<0.1< 0.1). The blue line represents the convex hull of all the DFT relaxed structures. (b) Evolution of the occupancy of Lioct\mathrm{Li}^{oct} and Litet\mathrm{Li}^{tet} within Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5-Li5V2O5\mathrm{Li}_5\mathrm{V}_2\mathrm{O}_5 at 0 K. (c) Evolution of the occupancy of Lioct\mathrm{Li}^{oct} and Litet\mathrm{Li}^{tet} within Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5-Li5V2O5\mathrm{Li}_5\mathrm{V}_2\mathrm{O}_5 in cubic phase. At each composition, the three lowest-energy structures were used for site occupancy calculations. The average values with error bars are shown in the plot. The most stable structures of ground states and metastable cubic phase of Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_2\mathrm{O}_5 (x=0,1,2x = 0, 1, 2) are shown in Figure S3. (d) The distribution in DFT relative energies and average Steinhardt order parameter Dˉj\bar{D}_j of the initial Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5 structures corresponding to the cubic and distorted lithiated Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_2\mathrm{O}_5 (x≥1x \ge1) structures. For each composition, no more than 50 structures with the lowest energies were used for the analysis.

Structures of lowest energy metastable cubic phase and ground state of Li3+xV2O5

Figure S3. The structures of lowest energy metastable cubic phase and the ground state of Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_2\mathrm{O}_5 (x=0,1,2x = 0, 1, 2).

Figure 2(d) shows the distribution in relative energies and the average Steinhardt order parameter (Dˉj\bar{D}_j) of the initial Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5 structures corresponding to the cubic and distorted lithiated Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_2\mathrm{O}_5 (x≥1x \ge1) structures. It can be seen that the lithiated structures that maintain a cubic-like structure have greater Dˉj\bar{D}_j, i.e., more Li/V disorder, and higher relative energies than those that are highly distorted (see Figure S2). These cubic-like structures also exhibit only moderate Li redistribution at the end of charge. In contrast, the low DFT energy lithiated structures correspond to initial Li/V arrangements that are less disordered. In fact, the DFT ground state Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5 exhibit an ordered layered-like Li/V arrangement akin to LiVO2\mathrm{LiVO}_2 with Dˉj=6×10−4\bar{D}_j = 6 \times10^{-4}.

Relative energies and crystal structures of LiVO2 and Li3V2O5

Figure S2. (a) Relative energies of (a) LiVO2_2 and (b) Li3_3V2_2O5_5 structures as a function of order parameter (Dj‾\overline{D_j}). The blue star in (a) represents R3ˉmR\bar{3}m LiVO2_2 and the yellow star in (b) represents the Li3_3V2_2O5_5 structure with the lowest calculated energy. (c) Crystal structure of the calculated ground state R3ˉmR\bar{3}m LiVO2_2 and Li3_3V2_2O5_5.

It should be noted that the initial Li/V disorder is controlled via synthesis levers such as temperature. Given that the as-synthesized DRX-Li3V2O5\mathrm{Li}_3\mathrm{V}_2\mathrm{O}_5 anode is highly cubic and exhibits Li/V disorder, we may surmise from the above results that the relevant lithiation pathway is one in which Li primarily inserts into the tetrahedral sites with minimal redistribution of Lioct\mathrm{Li}^{oct} to Litet\mathrm{Li}^{tet} while maintaining a cubic-like framework with low distortion.

Validation of cluster expansion model

Figure 3 (a) plots the 112 non-zero ECIs of the fitted CE model versus cluster size. It may be observed that the magnitude of the ECIs converge to near 0 at the cutoff radius. From Figure 3 (b), it may be observed that the fitted CE model accurately captures the DFT computed ground states (structures with formation energy on the convex hull).

Fitted effective cluster interactions and formation energies

Figure 3. (a) Fitted effective cluster interactions (ECI) values with respect to the size of the clusters (b) DFT calculated and cluster expansion (CE) predicted formation energy of Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_{2}\mathrm{O}_{5} (x=0.0x = 0.0 - 2.0)

Order-disorder transition of cubic Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5}

To further understand the effect of cation disorder in DRX-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} anode, we performed Monte Carlo simulation using the fitted CE model. Figure 4 shows the calculated formation energy EfE_{\mathrm{f}} and specific heat capacity CvC_{\mathrm{v}} as a function of temperature from MC simulations with the fitted CE model. The critical temperature (TcT_{\mathrm{c}}) of order-disorder phase transition is predicted to be ∼1000\sim1000 K, which is somewhat lower than that experimentally measured from LiVO2\mathrm{LiVO}_{2} (1775 K).[39] At temperatures below TcT_{\mathrm{c}}, both EfE_{\mathrm{f}} and CvC_{\mathrm{v}} remain relatively constant with temperature, characteristic of a highly ordered crystal. At TcT_{\mathrm{c}}, a discontinuous increase in the EfE_{\mathrm{f}} and a sharp peak in the configurational CvC_{\mathrm{v}} is observed, indicative of a phase transition taking place. The calculated average configurational specific heat capacity of the DRX phase (T>1000T > 1000 K) is 2.973 J mol−1\mathrm{mol}^{-1} K−1\mathrm{K}^{-1}. Figure 4 (b) shows two sampled configurations from the equilibrated MC simulations at 500K (ordered phase) and 1500 K (fully disordered phase). At temperatures above TcT_{\mathrm{c}}, Li/V disordering occurs mostly on the octahedral 4b4b sites and only a small fraction of Li (∼0.0125\sim0.0125 %) ions occupy the tetrahedral sites. These observations are consistent with the fact that the DRX is synthesized under the application of an external driving force, such as high temperatures, ball milling, or electrochemical lithiation. [5, 6, 40]

Calculated formation energy, heat capacity, and structures from equilibrated Monte Carlo simulations

Figure 4. (a) Calculated formation energy (EfE_{\mathrm{f}}) and heat capacity (CvC_{\mathrm{v}}) as a function of temperature (TT). Structures from equilibrated Monte Carlo simulations at (b) 500 K and 1500 K. The MC simulations were initialized in the DFT calculated most energetically stable Li3_3V2_2O5_5 structure, in which all Li and V ions occupy the octahedral sites. The initial configuration was then heated from 10 K to 2000K in intervals of = 10 K. At each temperature, the properties were then obtained by averaging the results from 1000 equilibrated MC runs. The configurational heat capacity CvC_{\mathrm{v}} is given by the second derivative of the formation energy EfE_{\mathrm{f}} with respect to temperature TT, Cv=∂2Ef/∂2TC_{\mathrm{v}} = \partial^2 E_{\mathrm{f}}/\partial^2 T.

Lithium intercalation mechanism and predicted voltage profile

The intercalation mechanism of Li+^{+} into DRX structures is strongly affected by the distribution of the tetrahedral sites with different local environments and connectivity. The Li in tetrahedral sites share faces with four neighboring octahedral sites. As shown in previous works, [1, 2, 3, 5] the Li/transition metal occupancy of these neighboring octahedral sites have a strong influence on the local site occupancies and Li+^{+} migration barriers. The local environment of a tetrahedral site can be denoted by nn-V (n=0∼4n = 0 \sim4), where nn represents the number of face-shared V atoms. Figure 5 (a) shows the distribution of the calculated Litet^{\mathrm{tet}} site energies in 0-V, 1-V, 2-V and 4-V clusters in the three SQSs with the lowest DFT energies.

Four-panel figure showing site energies, lithium insertion sites, calculated voltage, and site occupancies

Figure 5. (a) Site energy of Litet\mathrm{Li}^{tet} in various local environments (i.e., diffusion sites). (b) 0-V, 1-V, and 2-V tetrahedral Li insertion sites and off-center displacements of the neighboring octahedral sites and the inserted tetrahedral Li sites. (c) Calculated voltage as a function of Li content xx in Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_{2}\mathrm{O}_{5}. The experimental and DFT (0 K) results are extracted from Liu et al. [5] (d) Evolution of Li site occupancies in tetrahedral and octahedral sites upon Li insertion from semi-GCMC simulations with the position of VoctV^{oct} fixed.

The Litet\mathrm{Li}_{\mathrm{tet}} site energy in 3-V is not presented because Litet\mathrm{Li}_{\mathrm{tet}} is unstable in this local environment and the electrostatic repulsive effect between the inserted Litet\mathrm{Li}_{\mathrm{tet}} and the neighboring Lioct\mathrm{Li}^{\mathrm{oct}} ion caused local environment rearrangements during structure relaxations. In general, the Litet\mathrm{Li}_{\mathrm{tet}} site energy and the distortion of neighboring LiO6\mathrm{LiO}_{6} octahedra increase with the number of neighboring V atoms. The Li insertion into 0-V sites is the most energetically favourable and the four neighboring Lioct\mathrm{Li}^{\mathrm{oct}} sites are displaced off-center by 0.4-0.5 Å due to the electrostatic repulsion between Li+\mathrm{Li}^{+} (Figure 5(b)). The 1-V Litet\mathrm{Li}_{\mathrm{tet}} site energy is on average 660 meV higher than that of 0-V sites and the inserted Li displaces ∼0.4\sim0.4 Å from the center of the tetrahedron in the direction away from the V ions. The off-center displacements of neighboring Lioct\mathrm{Li}^{\mathrm{oct}} are 0.3-0.6 Å, whereas that for the neighboring Voct\mathrm{V}^{\mathrm{oct}} are only 0.16 Å. The 2-V Litet\mathrm{Li}^{\mathrm{tet}} sites are relatively energetically unstable and is positioned ∼0.4\sim0.4 Å away from the tetrahedral center due to large repulsive interactions between V3+/V4+\mathrm{V}^{3+}/\mathrm{V}^{4+} and Li+\mathrm{Li}^{+}. The neighboring Li atoms are pushed 0.5 - 0.6 Å away from the center of the octahedron, causing large distortions in the local lattice structure.

The migration of V vacancies between neighboring octahedral sites was also investigated by introducing one Voct\mathrm{V}^{\mathrm{oct}} vacancy in the configuration with the lowest Voct\mathrm{V}^{\mathrm{oct}} vacancy energy. The average Voct\mathrm{V}^{\mathrm{oct}} migration barrier is extremely high, up to 2100 meV (Figure S1). This suggests that V ions in DRX\mathrm{DRX}-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} are unlikely to migrate during charge/discharge under operating conditions.

NEB barriers and minimum energy paths for V migration

Figure S1. (a) NEB barriers for V4+/V3+\mathrm{V}^{4+}/\mathrm{V}^{3+} migration through 2-V, 3-V and 4-V sites, (b) Illustration of the minimum energy path of V atoms in various local environments.

Figure 5(c) shows the calculated voltage profile by GCMC simulations. The GCMC-predicted voltage profile exhibits a solid solution-like behavior and is in good agreement with the experimentally-measured voltage profile. [5] Li starts to insert into DRX\mathrm{DRX}-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} at ∼1.43\sim1.43 V and the predicted voltage profile exhibits two voltage steps at around 0.9 and 0.25 V vs Li/Li+\mathrm{Li}/\mathrm{Li}^{+}. As the voltage decreases to 0.01 V, the predicted average composition of the lithiated anode is Li5.11V2O5\mathrm{Li}_{5.11}\mathrm{V}_{2}\mathrm{O}_{5}, close to that observed in experiments (Li4.86V2O5\mathrm{Li}_{4.86}\mathrm{V}_{2}\mathrm{O}_{5}). [5] In contrast, due to the limited supercell sizes used, DFT calculations [5] predict a multiple voltage steps at 0.98V, 0.54 V, 0.46 V and 0.45 V.

Figure 5 (d) shows the evolution of Li site occupancies in DRX\mathrm{DRX}-Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_{2}\mathrm{O}_{5} as a function of inserted Li content xx. It should be noted that as an anode, insertion of Li into the DRX\mathrm{DRX}-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} corresponds to the charging process in a typical Li-ion battery. As Li ions are introduced into the tetrahedral sites, the Li occupancy in the octahedral sites first remains constant at around 0.6 until x≈0.3x \approx0.3, following which there is a small, gradual reduction in Lioct\mathrm{Li}^{oct} occupancy. The insertion of Li ions into the tetrahedral sites consists of two steps. Li+\mathrm{Li}^{+} first intercalate into 0-V sites, which is consistent with the energies predicted by DFT calculations (Figure 5 (a)) and previous results that the insertion into 0-V tetrahedral sites is the most energetically favorable. [5] This process coincides with the formation of the first plateau at around 0.9 V on the voltage profile. At x=0.31x = 0.31, 0-V sites are fully occupied and further lithiation insertion occurs in the energetically less favorable 1-V and 2-V sites. The occupancy of 1-V and 2-V sites rise to ∼0.1\sim0.1 till the end of charge. At the end of charge, only ∼0.1%\sim0.1\% 3-V tetrahedral sites are occupied, and all 4-V sites are vacant.

Validation of moment tensor potential

The mean absolute errors (MAEs) of training energies and forces (shown in Figure 6) of the fitted MTP are 3.15 meV/atom and 0.15 eV/Å, respectively, comparable to those of other MTPs in the literature. [41, 42] As shown in Table 1, the MTP is able to accurately reproduce the lattice parameters and densities of training structures, with errors of within ±3.12%\pm3.12\% and ±4.42%\pm4.42\% relative to DFT values, respectively.

Plots of the MTP predicted versus DFT energies and forces

Figure 6. Plots of the (a) MTP predicted versus DFT energies and (b) MTP predicted versus DFT forces with levmax=20lev_{max} = 20.

Compositiona (Å)b (Å)c (Å)Density (g/cm3^{3})
LiVO2_{2}3.02 (1.75 %)5.16 (-1.24 %)5.25 (1.19 %)3.88 (1.69 %)
LiV2_{2}O5_{5}6.75 (0.98 %)7.68 (0.41 %)7.58 (-1.65 %)3.18 (-0.28 %)
Li3_{3}VO4_{4}5.06 (0.48 %)5.54 (0.51 %)6.37 (-0.41 %)2.52 (-0.57 %)
Li2_{2}O3.30 (0.056 %)3.29 (0.056 %)3.29 (0.056%)1.96 (-0.17%)
DRX-Li3_{3}V2_{2}O5_{5}8.46 (0.66 %)8.45 (1.26 %)8.42 (0.84 %)3.60 (-2.71 %)
DRX-Li3.9_{3.9}V2_{2}O5_{5}8.62 (1.26 %)8.62 (1.25 %)8.62 (1.24 %)3.18 (-3.66 %)
DRX-Li5_{5}V2_{2}O5_{5}9.48 (3.12 %)7.72 (-1.03 %)9.43 (2.519 %)3.36 (-4.42 %)

Table 1. Lattice parameters and densities of the structures in the training set (zero strain) relaxed with the trained MTP at 0K, in comparison with DFT calculated lattice parameters and densities at 0K. Values in brackets are the percentage differences between the MTP and DFT computed values, respectively.

Diffusion properties

MD simulations were carried out to investigate the Li+\mathrm{Li}^{+} diffusion in the DRX\mathrm{DRX}-Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_{2}\mathrm{O}_{5} anode as a function of Li concentration using the fitted MTP potential. The initial structures were obtained from the equilibrium semi-GCMC simulations in the preceding section. Figure 7 shows the calculated diffusivity DLi+D_{\mathrm{Li}^{+}} and activation energy EaE_a as a function of Li content xx in DRX\mathrm{DRX}-Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_{2}\mathrm{O}_{5} at room temperature (300 K). The Arrhenius plot from NpTNpT MD

Calculated diffusivity, activation energy, Li trajectories, migration pathways, and NEB barriers for Li migration in DRX-Li3+xV2O5

Figure 7. (a) Calculated diffusivity and activation energy of Li+\mathrm{Li}^{+} in DRX-Li3+x_{3+x}V2_2O5_5 as a function of Li content at 300 K. (b) Li trajectories (colored as grey) from MD simulations of Li3.5_{3.5}V2_2O5_5 at 600 K, projected in the crystallographic a-b planes. Illustrations of “t-o-t” migration mechanisms of Li+\mathrm{Li}^{+} are shown in red arrows. The green balls, purple balls, and red balls represent Li, V, and O atoms, respectively.) (c) Illustration of Li+\mathrm{Li}^{+} migration path in DRX-Li3_3V2_2O5_5. The opposing and corner-sharing pathways indicate cooperative migration mechanisms of Li+\mathrm{Li}^{+} via the octahedral site and its next tetrahedral site. (d) Calculated NEB barriers for possible Li migration hops. The barriers are categorized in terms of their mechanisms and local environments.

simulations for each composition is shown in Figure S6. At the start of lithiation, a sharp increase in DLi+D_{\mathrm{Li}^{+}} to ∼10−9 cm2 s−1\sim10^{-9}\ \mathrm{cm}^{2}\ \mathrm{s}^{-1} with a corresponding decrease in EaE_{\mathrm{a}} from 450 meV to 280 meV is observed up to x=0.5x = 0.5. However, further lithiation results in a gradual decrease in DLi+D_{\mathrm{Li}^{+}} from ∼10−9 cm2 s−1\sim10^{-9}\ \mathrm{cm}^{2}\ \mathrm{s}^{-1} to ∼10−11 cm2 s−1\sim10^{-11}\ \mathrm{cm}^{2}\ \mathrm{s}^{-1} accompanied by an increase in EaE_{\mathrm{a}} from 280 to 460 meV.

Arrhenius plot from NpT MD simulations of different Li₃₊ₓV₂O₅ compositions

Figure S6. Arrhenius plot from NpT MD simulations of different Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_2\mathrm{O}_5 compositions.

We further analyzed the Li+\mathrm{Li}^{+} trajectories from 1 ns MD simulations at 600 K and the results for selected configurations are presented in Figure 7 (b). For x<1.5x < 1.5, Li+\mathrm{Li}^{+} ions migrate via a cooperative tetrahedral - octahedral - tetrahedral (“t-o-t”) mechanism, in agreement with previous NEB calculations.[5] For x>1.5x > 1.5, the increased amount of inserted Li+\mathrm{Li}^{+} in tetrahedral sites and vacancies in octahedral sites may result in Li+\mathrm{Li}^{+} migration between neighboring tetrahedral - tetrahedral (“t-t”) sites via the vacant octahedral sites along with the “t-o-t” migration.

To confirm the above results, DFT NEB calculations were also performed to calculate the Li+\mathrm{Li}^{+} migration barriers. Similar to the previous NEB calculations,[5] a cooperative mechanism of Li+\mathrm{Li}^{+} migration was considered, where the tetrahedral Li+\mathrm{Li}^{+} migrates to a neighboring octahedral site and the octahedral Li+\mathrm{Li}^{+} migrates into another neighboring tetrahedral site (Figure 7 (c)). Here, we consider cooperative migration that occurs between corner-sharing and opposing tetrahedral sites, given that migration between edge-sharing tetrahedral sites is extremely energetically unfavorable due to the close proximity of the Li during migration (Figure S8 and S9(c)). Figure 7(d) shows the calculated Li+\mathrm{Li}^{+} migration barriers between connected 0-V/1-V sites. We note that migration from 2-V site to 0-V and 1-V sites are energetically downhill due to the large site energy differences (Figure S11). The cooperative migration of Li+\mathrm{Li}^{+} via opposing “t-o-t” paths exhibits the lowest calculated average energy barriers, ranging from 230 to 340 meV in 0-V and 1-V sites. The average energy barriers of Li+\mathrm{Li}^{+} transport through corner-sharing ’t-o-t’ pathways exhibit higher energy barriers of 334 to 628 meV. In general, the migration barriers of Li+\mathrm{Li}^{+} increase as more V atoms gather around the local environment of tetrahedral Li+\mathrm{Li}^{+} sites. At the end of discharge, the formation of

Three-panel plots of DFT-calculated Li+ migration barriers in 0-V sites: (a) Opposing, (b) Corner-Sharing, and (c) Edge-sharing, with migration barrier values labeled in meV

Figure S8. DFT calculated Li+^{+} migration barriers in 0-V sites. (a) 0-V to 0-V (Opposing), (b) 0-V to 0-V (Corner-Sharing) and (c) 0-V to 0-V (Edge-Sharing).

DFT calculated Li+ migration barriers via connected 1-V and 2-V sites

Figure S11. DFT calculated Li+^{+} migration barriers via connected 1-V and 2-V sites (Opposing).

vacancies at the octahedral sites allows for direct hopping of Li+\mathrm{Li}^{+} from one tetrahedral site to its next edge-sharing tetrahedral site (’t - t’), as illustrated in Figure S13, with a low energy barrier of 241 meV. These results are in line with the activation energies obtained by MD simulations and previous theoretical studies[5] that the facile migration of Li+\mathrm{Li}^{+} across opposing ’t-o-t’ pathways results in high rate capability of DRX\mathrm{DRX}-Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_{2}\mathrm{O}_{5} anode. In previous studies,[5] Li+\mathrm{Li}^{+} hopping via 0-V sites is the only mechanism that was considered while our results show that Li+\mathrm{Li}^{+} migration in 0-V, 1-V and 2-V sites is facile. Similar results have also been observed in LTO anodes that the transportation of Li+\mathrm{Li}^{+} in face-sharing octahedral-tetrahedral motif contributes to fast kinetics.[43]

Illustration of Li+ migration via direct path in DRX-Li3V2O5

Figure S13. Illustration of Li+\mathrm{Li}^{+} migration via “t-t” path in DRX-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5}. The direct pathway indicates a divacancy mechanism of Li+tet\mathrm{Li}^{+\mathrm{tet}} vacancies at the end of discharge.

Conclusions

A major conclusion from this work is that the lithium insertion mechanism in Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} depends greatly on the initial Li/V disorder. For highly ordered Li/V arrangements with lower energies, Li insertion occurs via a redistribution mechanism with the formation of highly distorted structures and accompanied by large volume changes. This is consistent with previous DFT results, but inconsistent with experimental observations for the DRX\mathrm{DRX}-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} electrode.[5] In contrast, Li/V disorder leads to Li inserting primarily into the tetrahedral sites, while retaining a cubic-like structure with small volume changes. The MC-predicted voltage profile based on this latter mechanism is also in much better agreement with the experimental voltage profile.

The Li+\mathrm{Li}^{+} insertion mechanism and transport depends on the local environment around each tetrahedral site and the distribution of sites. Our results show that Li+\mathrm{Li}^{+} in 0-V sites are the most energetically favorable and have the lowest migration barrier and ≥\geq2-V sites are highly energetically unfavorable. Assuming a fully cation-disordered DRX\mathrm{DRX}-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} ([Li0.6V0.4]octO[\mathrm{Li}_{0.6}\mathrm{V}_{0.4}]^{\mathrm{oct}}\mathrm{O}), the probability of a nn-V site P(n)P(n) is given by the binomial distribution:

P(n)=4!n!(4−n)!0.4n0.64−n(10)P(n) = \frac{4!}{n!(4-n)!}0.4^n0.6^{4-n} \tag*{(10)}

The fractions of 0-V, 1-V and ≥\geq2-V are therefore 0.13, 0.35, and 0.52, respectively. The highest experimentally-realized lithiation state is Li5V2O5\mathrm{Li}_5\mathrm{V}_2\mathrm{O}_5 (∼Li1V0.4O\sim\mathrm{Li}_1\mathrm{V}_{0.4}\mathrm{O}), which approximately corresponds to the full occupancy of the most energetically favored 0-V sites and about 0.77 occupancy of the 1-V tetrahedral sites. Hence, we can surmise that the inability of DRX-Li3+xV2O5\mathrm{Li}_{3+x}\mathrm{V}_2\mathrm{O}_5 to reach the theoretical V2+\mathrm{V}^{2+} limit of Li6V2O5\mathrm{Li}_6\mathrm{V}_2\mathrm{O}_5 is due to the lack of low energy sites for further Li insertion.

The above analysis suggest that one potential avenue to tune the electrochemical properties of the DRX anode is by varying the Li:V ratio in [Li1−xVx]octO[\mathrm{Li}_{1-x}\mathrm{V}_x]^{\mathrm{oct}}\mathrm{O}. Increasing the Li:V ratio would increase the fraction of 0-V/1-V tetrahedral sites, but at the price of increasing the V oxidation state and hence, the anode voltage. Conversely, lowering the Li:V ratio would decrease lithiation capacity but also decrease the anode voltage. The optimal ratio would depend on the specific application, for example, whether a high rate or a high energy density anode is prioritized.

Acknowledgement

This work is supported by the Materials Project, funded by the U.S. Department of Energy, Office of Science, Office of Basic Energy Sciences, Materials Sciences and Engineering Division under Contract no. DEAC02-05-CH11231: Materials Project program KC23MP. The authors acknowledge the computing resources provided by Triton Shared Computing Cluster (TSCC) at UC San Diego, the National Energy Research Scientific Computing Center (NERSC) and the Extreme Science and Engineering Discovery Environment (XSEDE) supported by the National Science Foundation, under Grant No. ACI-1053575. The authors would also like to acknowledge extremely helpful discussions with Dr Sanjeev Kolli and Prof Anton van der Ven of the University of California Santa Barbara on the use of the CASM code.

References

Supplementary Information for The Intercalation Chemistry of the Disordered RockSalt Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5} Anode from Cluster Expansions and Machine Learning Interatomic Potentials

Xingyu Guo; Chi Chen; Shyue Ping Ong

Four rows of paired crystal-structure projections labeled a–d

Figure 1 (PDF p. 32).

Calculated Li+ trajectories obtained from MD simulations

Figure S7. Calculated Li+\mathrm{Li}^{+} trajectories obtained from MD simulations. (a) Li3.25V2O5\mathrm{Li}_{3.25}\mathrm{V}_{2}\mathrm{O}_{5}, (b) Li3.5V2O5\mathrm{Li}_{3.5}\mathrm{V}_{2}\mathrm{O}_{5}, (c) Li3.75V2O5\mathrm{Li}_{3.75}\mathrm{V}_{2}\mathrm{O}_{5}, (d) Li4.0V2O5\mathrm{Li}_{4.0}\mathrm{V}_{2}\mathrm{O}_{5}, (e) Li4.25V2O5\mathrm{Li}_{4.25}\mathrm{V}_{2}\mathrm{O}_{5}, (f) Li4.50V2O5\mathrm{Li}_{4.50}\mathrm{V}_{2}\mathrm{O}_{5}, (g) Li4.75V2O5\mathrm{Li}_{4.75}\mathrm{V}_{2}\mathrm{O}_{5} and (h) Li5.0V2O5\mathrm{Li}_{5.0}\mathrm{V}_{2}\mathrm{O}_{5}.

DFT calculated Li+ migration barriers via 0-V and 1-V sites

Figure S9. DFT calculated Li+\mathrm{Li}^{+} migration barriers via 0-V and 1-V sites. (a) 0-V to 1-V (Opposing), (b) 0-V to 1-V (Corner-sharing) and (c) 0-V to 1-V (Edge-sharing).

DFT calculated Li+ migration barriers via 1-V sites, with opposing and corner-sharing configurations

Figure S10. DFT calculated Li+^{+} migration barriers via 1-V sites. (a) 1-V to 1-V (Opposing), (b) 1-V to 1-V (Corner Sharing).

Illustration of Li+ migration via edge-sharing path in DRX-Li3V2O5

Figure S12. Illustration of Li+\mathrm{Li}^{+} migration via edge-sharing “t-o-t” path in DRX-Li3V2O5\mathrm{Li}_{3}\mathrm{V}_{2}\mathrm{O}_{5}.

References

  1. [1]Clément, R.; Lun, Z.; Ceder, G. Cation-disordered rocksalt transition metal oxides and oxyfluorides for high energy lithium-ion cathodes. Energy & Environmental Science 2020, 13, 345–373.DOI
  2. [2]Lee, J.; Urban, A.; Li, X.; Su, D.; Hautier, G.; Ceder, G. Unlocking the potential of cation-disordered oxides for rechargeable lithium batteries. science 2014, 343, 519–522.DOI
  3. [3]Urban, A.; Matts, I.; Abdellahi, A.; Ceder, G. Computational design and preparation of cation-disordered oxides for high-energy-density Li-ion batteries. Advanced Energy Materials 2016, 6, 1600488.DOI
  4. [4]Kitchaev, D. A.; Lun, Z.; Richards, W. D.; Ji, H.; Clément, R. J.; Balasubramanian, M.; Kwon, D.-H.; Dai, K.; Papp, J. K.; Lei, T., et al. Design principles for high transition metal capacity in disordered rocksalt Li-ion cathodes. Energy & Environmental Science 2018, 11, 2159–2171.
  5. [5]Liu, H.; Zhu, Z.; Yan, Q.; Yu, S.; He, X.; Chen, Y.; Zhang, R.; Ma, L.; Liu, T.; Li, M., et al. A disordered rock salt anode for fast-charging lithium-ion batteries. Nature 2020, 585, 63–67.DOI
  6. [6]Barnes, P.; Zuo, Y.; Dixon, K.; Hou, D.; Lee, S.; Ma, Z.; Connell, J. G.; Zhou, H.; Deng, C.; Smith, K., et al. Electrochemically induced amorphous-to-rock-salt phase transformation in niobium oxide electrode for Li-ion batteries. Nature Materials 2022, 1–9.DOI
  7. [7]Xiong, H.; Slater, M. D.; Balasubramanian, M.; Johnson, C. S.; Rajh, T. Amorphous TiO2 nanotube anode for rechargeable sodium ion batteries. The journal of physical chemistry letters 2011, 2, 2560–2565.
  8. [9]Zunger, A.; Wei, S.-H.; Ferreira, L.; Bernard, J. E. Special quasirandom structures. Physical review letters 1990, 65, 353.pubmed.ncbi.nlm.nih.gov/10042897
  9. [10]Kresse, G.; Furthmüller, J. Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set. Physical review B 1996, 54, 11169.pubmed.ncbi.nlm.nih.gov/9984901
  10. [11]Blöchl, P. E. Projector augmented-wave method. Physical review B 1994, 50, 17953.pubmed.ncbi.nlm.nih.gov/9976227
  11. [12]Perdew, J. P.; Burke, K.; Ernzerhof, M. Generalized gradient approximation made simple. Physical review letters 1996, 77, 3865.pubmed.ncbi.nlm.nih.gov/10062328
  12. [13]Dudarev, S.; Botton, G.; Savrasov, S.; Humphreys, C.; Sutton, A. Electron-energy-loss spectra and the structural stability of nickel oxide: An LSDA+ U study. Physical Review B 1998, 57, 1505.DOI
  13. [14]Jain, A.; Hautier, G.; Ong, S. P.; Moore, C. J.; Fischer, C. C.; Persson, K. A.; Ceder, G. Formation enthalpies by mixing GGA and GGA+ U calculations. Physical Review B 2011, 84, 045115.DOI
  14. [15]Jain, A.; Ong, S. P.; Hautier, G.; Chen, W.; Richards, W. D.; Dacek, S.; Cholia, S.; Gunter, D.; Skinner, D.; Ceder, G., et al. Commentary: The Materials Project: A materials genome approach to accelerating materials innovation. Apl Materials 2013, 1, 011002.DOI
  15. [16]Kawasaki, T.; Onuki, A. Construction of a disorder variable from Steinhardt order parameters in binary mixtures at high densities in three dimensions. The Journal of chemical physics 2011, 135, 174109.
  16. [17]Menon, S.; Leines, G. D.; Rogal, J. pyscal: A python module for structural analysis of atomic environments. Journal of Open Source Software 2019, 4, 1824.DOI
  17. [18]Van der Ven, A.; Thomas, J.; Xu, Q.; Bhattacharya, J. Linking the electronic structure of solids to their thermodynamic and kinetic properties. Mathematics and computers in simulation 2010, 80, 1393–1410.DOI
  18. [19]Sanchez, J. M.; Ducastelle, F.; Gratias, D. Generalized cluster description of multi-component systems. Physica A: Statistical Mechanics and its Applications 1984, 128, 334–350.
  19. [20]De Fontaine, D. Cluster approach to order-disorder transformations in alloys. 1994, 47, 33–176.DOI
  20. [21]Thomas, J. C.; Van der Ven, A. Finite-temperature properties of strongly anharmonic and mechanically unstable crystal phases from first principles. Physical Review B 2013, 88, 214111.DOI
  21. [22]CASM, v1.1.1. 2021; https://github.com/prisms-center/CASMcode.
  22. [23]Li, W.; Reimers, J.; Dahn, J. Lattice-gas-model approach to understanding the structures of lithium transition-metal oxides LiM O 2. Physical Review B 1994, 49, 826.DOI
  23. [24]Novikov, I. S.; Gubaev, K.; Podryabinkin, E. V.; Shapeev, A. V. The MLIP package: moment tensor potentials with MPI and active learning. Machine Learning: Science and Technology 2020, 2, 025002.arxiv.org/abs/2007.08555
  24. [26]Nosé, S. A unified formulation of the constant temperature molecular dynamics methods. The Journal of chemical physics 1984, 81, 511–519.DOI
  25. [27]Hoover, W. G. Canonical dynamics: Equilibrium phase-space distributions. Physical review A 1985, 31, 1695.pubmed.ncbi.nlm.nih.gov/9895674
  26. [28]Shapeev, A. V. Moment tensor potentials: A class of systematically improvable interatomic potentials. Multiscale Modeling & Simulation 2016, 14, 1153–1173.DOI
  27. [29]Gubaev, K.; Podryabinkin, E. V.; Hart, G. L.; Shapeev, A. V. Accelerating high-throughput searches for new alloys with active learning of interatomic potentials. Computational Materials Science 2019, 156, 148–156.arxiv.org/abs/1806.10567
  28. [30]Thompson, A. P.; Aktulga, H. M.; Berger, R.; Bolintineanu, D. S.; Brown, W. M.; Crozier, P. S.; in’t Veld, P. J.; Kohlmeyer, A.; Moore, S. G.; Nguyen, T. D., et al. LAMMPS-a flexible simulation tool for particle-based materials modeling at the atomic, meso, and continuum scales. Computer Physics Communications 2022, 271, 108171.DOI
  29. [31]Chen, C.; Yunxing Zuo, Q. J., Weike Ye; Ong, S. P. Maml - materials machine learning package. https://github.com/materialsvirtuallab/maml, 2020.
  30. [32]Henkelman, G.; Uberuaga, B. P.; Jónsson, H. A climbing image nudged elastic band method for finding saddle points and minimum energy paths. The Journal of chemical physics 2000, 113, 9901–9904.DOI
  31. [33]Henkelman, G.; Jónsson, H. Improved tangent estimate in the nudged elastic band method for finding minimum energy paths and saddle points. The Journal of chemical physics 2000, 113, 9978–9985.DOI
  32. [34]Van der Ven, A.; Ceder, G.; Asta, M.; Tepesch, P. First-principles theory of ionic diffusion with nondilute carriers. Physical Review B 2001, 64, 184307.DOI
  33. [35]Ong, S. P.; Chevrier, V. L.; Hautier, G.; Jain, A.; Moore, C.; Kim, S.; Ma, X.; Ceder, G. Voltage, stability and diffusion barrier differences between sodium-ion and lithium-ion intercalation materials. Energy & Environmental Science 2011, 4, 3680–3688.
  34. [36]Armstrong, A. R.; Lyness, C.; Panchmatia, P. M.; Islam, M. S.; Bruce, P. G. The lithium intercalation process in the low-voltage lithium battery anode LiI1 + xVI1- xO2. Nature materials 2011, 10, 223–229.DOI
  35. [37]Li, H.; Liu, X.; Zhai, T.; Li, D.; Zhou, H. Li3VO4: a promising insertion anode material for lithium-ion batteries. Advanced Energy Materials 2013, 3, 428–432.DOI
  36. [38]Baur, C.; Chable, J.; Klein, F.; Chakravadhanula, V. S. K.; Fichtner, M. Reversible delithiation of disordered rock salt LiVO2. ChemElectroChem 2018, 5, 1484–1490.DOI
  37. [39]Hewston, T.; Chamberland, B. A survey of first-row ternary oxides LiMO2 (M = Sc-Cu). Journal of Physics and Chemistry of Solids 1987, 48, 97–108.DOI
  38. [40]Delmas, C.; Cognac-Auradou, H. Formation of the ω-type phase by lithium intercalation in (Mo, V) oxides deriving from V2O5. Journal of power sources 1995, 54, 406–410.DOI
  39. [41]Zuo, Y.; Chen, C.; Li, X.; Deng, Z.; Chen, Y.; Behler, J.; Csányi, G.; Shapeev, A. V.; Thompson, A. P.; Wood, M. A., et al. Performance and cost assessment of machine learning interatomic potentials. The Journal of Physical Chemistry A 2020, 124, 731–745.DOI
  40. [42]Wang, C.; Aoyagi, K.; Wisesa, P.; Mueller, T. Lithium ion conduction in cathode coating materials from on-the-fly machine learning. Chemistry of Materials 2020, 32, 3741–3752.DOI
  41. [43]Zhang, W.; Seo, D.-H.; Chen, T.; Wu, L.; Topsakal, M.; Zhu, Y.; Lu, D.; Ceder, G.; Wang, F. Kinetic pathways of ionic transport in fast-charging lithium titanate. Science 2020, 367, 1030–1034.

Paper details

vlnc:W_qq3rxcpa
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents