betaFeedback

WorksPhysics and Astronomy

Robust Antiferromagnetic Ordering above 500 K in a Family of Bilayer van der Waals Materials

Abstract

Stabilizing magnetic order above room temperature in layered materials is highly desirable for low-dimensional spintronics applications. However, realizing room-temperature antiferromagnetism in layered magnets remains challenging. Here, we present a layered semiconducting oxyhalide material family, Sr3_3Fe2_2O5_5X2_2 (XX = F, Cl, Br), which exhibits robust high-temperature antiferromagnetic ordering. The two-dimensional nature and scalability of this system are demonstrated by atomically resolving the van der Waals gap of Sr3_3Fe2_2O5_5Br2_2 and synthesizing centimeter-scale single crystals of Sr3_3Fe2_2O5_5Cl2_2. Temperature-dependent neutron scattering and magnetization measurements determine their G-type magnetic structure and transition temperature. Remarkably, the Néel temperature of Sr3_3Fe2_2O5_5F2_2 (∼\sim580 K) is the highest among all reported layered antiferromagnets. Density functional theory calculations demonstrate that strong nearest-neighbor superexchange interactions along both out-of-plane and in-plane directions, particularly the magnetic couplings along lattice cc direction within the bilayer motif, are primarily responsible for the high Néel temperatures in Sr3_3Fe2_2O5_5X2_2. In contrast, inter-bilayer spin couplings are negligibly weak, without much influence on the stabilization of the antiferromagnetic order. Therefore, theoretical calculations predict that this robust antiferromagnetic order could persist or even strengthens at room-temperature even at the monolayer limit. Our results highlight iron-based layered oxyhalides as a promising platform for exploring beyond-room-temperature antiferromagnetism in the two-dimensional limit, holding immense potential in areas like information storage and spin-based devices.

Introduction

Magnetism in van der Waals (vdW) materials with dimensional confinement has emerged as a prominent frontier in condensed matter physics [1, 2, 3, 4, 5, 6]. Intrinsically weak interlayer couplings, because of the loose bondings by van der Waals force, facilitate easier isolation of monolayer and few-layer flakes via mechanical exfoliation. Such pronounced dimensional confinement provides an excellent platform for investigating unconventional physical properties and emergent phenomena at the nanoscale. The ability to arbitrarily stack these layers offers further remarkable flexibility in materials design, stimulating extensive research into engineered heterostructures and superlattices [3, 4]. Exceptional phenomena include unconventional superconductivity and fractional quantum anomalous Hall states are observed in twisted superlattices [7, 8]. The discovery of intrinsic magnetic order in atomically thin crystals [9, 10, 11] has further promoted device research, leading to advances in spin field-effect transistors [9], quantum light emitters [12], quantum computing [13, 14], etc.

A critical limitation, however, is that the magnetic transition temperatures of most vdW magnets are well below room temperature, hindering practical applications. To address this, considerable efforts have been devoted to elevating the magnetic ordering temperatures in recent years, with significant progress reported in ferromagnets such as Fe5_5GeTe2_2 [15, 16], Ni- and Co- doped Fe5_5GeTe2_2 [17, 18, 19, 20], Fe3_3GaTe2_2 [21, 22], etc. For antiferromagnetic vdW magnets, materials with Néel temperature (TNT_\mathrm{N}) reaching room temperature are still quite rare. A-type antiferromagnetic order with TN∼340T_\mathrm{N} \sim340 K was confirmed in 40% Co doped Fe5_5GeTe2_2 [18, 23]. This compound is metallic with in-plane ferromagnetism and is antiferromagnetically coupled along the out-of-plane direction, rendering a magnetic propagation wavevector k=(0,0,1/2)\mathbf{k} = (0, 0, 1/2) [23]. Still, vdW antiferromagnets with non-trivial spin textures and an insulating electronic ground state at or above room temperature are highly desired.

A promising strategy involves incorporating multiple anion species into the crystal lattice. The significant disparities in ionic radius, charge, and electronegativity between various anions expand the degrees of freedom for modulating the atomic and electronic structures of materials [24]. This mixed-anion strategy is particularly effective in Ruddlesden-Popper phase (RP-phase) oxyhalides. In these materials, halide atoms (F, Cl, Br, I) tend to occupy certain ordered oxygen sites, segregating oxygen and halide atoms into distinct layers. Such a unique configuration often forms low-dimensional layered structures, allowing control over the dimensionality, electronic tronic properties and spin exchange of magnetic interactions [24]. This principle is exemplified in superconducting compounds such as Sr2CuO2F2+δ\mathrm{Sr}_{2}\mathrm{CuO}_{2}\mathrm{F}_{2+\delta} [25] and (Ca,Na)2CuO2Cl2(\mathrm{Ca},\mathrm{Na})_{2}\mathrm{CuO}_{2}\mathrm{Cl}_{2} [26], as well as geometrically frustrated (CuCl)LaNd2O7(\mathrm{CuCl})\mathrm{LaNd}_{2}\mathrm{O}_{7} [27]. Notably, many RP-phase transition metal ion based oxyhalides exhibit high-temperature magnetic ordering [28]. Particularly, the iron-based oxyhalides Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2} and Sr3Fe2O5Cl2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Cl}_{2} serve as prototypical candidates within this extensive family, in which Néel temperatures above 500 K were reported [29, 30].

In this work, we optimize the systematic synthesis of the layered oxyhalide family Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2} (X=F,Cl,BrX = \mathrm{F}, \mathrm{Cl}, \mathrm{Br}) (Figure 1(a)), including the synthesis of both powder and single crystal sample forms. The largest lateral dimension of Sr3Fe2O5Cl2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Cl}_{2} single crystals can reach more than 20 mm. The phase purity, as well as the layered structure of Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2}, are confirmed by X-ray diffraction (XRD) and neutron powder diffraction (NPD). In addition, ultrathin flakes of Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2} are readily isolated via mechanical exfoliation down to the thickness of one-unit-cell (∼3\sim3 nm), and the intrinsic van der Waals spatial gaps are directly resolved at the atomic scale by scanning transmission electron microscopy (STEM). Magnetization measurements indicate AFM ground state in Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2}, with Néel temperature decreasing from the largest TN∼580T_{\mathrm{N}} \sim580 K for X=FX = \mathrm{F}, to ∼540\sim540 K for both X=ClX = \mathrm{Cl} and Br\mathrm{Br}. NPD studies reveal a G-type magnetic structure with in-plane spins and a magnetic propagation wavevector k=(1/2,1/2,0)\mathbf{k} = (1/2, 1/2, 0) in this material family. Theoretical calculations reveal that the robust high-temperature magnetic order in this system is primarily driven by strong out-of-plane and in-plane nearest-neighbor superexchange couplings. This long-range magnetic order is predicted to persist down to the two-dimensional (2D) limit without reducing its Néel temperature. Lastly, both UV-Vis diffuse reflectance spectroscopy (DRS) and angle-resolved photoemission spectroscopy (ARPES) studies indicate that all three compounds are semiconductors with both optical and electronic bandgaps larger than 2 eV. Our work highlights that Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2} (X=F,Cl,BrX = \mathrm{F}, \mathrm{Cl}, \mathrm{Br}) is a promising layered semiconducting material platform with Néel temperature approaching 600 K, and might still hold its Néel temperatures even down to the 2D limit.

Layered structure of Sr3Fe2O5X2

Figure 1. Layered structure of Sr3Fe2O5X2\mathrm{Sr_3Fe_2O_5X_2} (X=F, Cl, BrX = \mathrm{F},\ \mathrm{Cl},\ \mathrm{Br}). (a) Crystal structure of Sr3Fe2O5X2\mathrm{Sr_3Fe_2O_5X_2}, projected along the [1 0 0][1\ 0\ 0] crystallographic axis direction. (b) Bilayer structure with two corner sharing FeO5X\mathrm{FeO_5X} (X=F/Cl/BrX=\mathrm{F}/\mathrm{Cl}/\mathrm{Br}) octahedrons. (c) Atomic force microscopy image of the Sr3Fe2O5Br2\mathrm{Sr_3Fe_2O_5Br_2} (SFOB) flake exfoliated onto a SiO2\mathrm{SiO_2} substrate. (d) Height profile along the line cut in (c), indicating a thickness of ∼3\sim3 nm, which is about one unit cell of lattice cc. (e)-(f) High-angle annular dark-field (HAADF) image and projected multislice electron ptychography (MEP) reconstruction, along the [100][100] zone axis of single-crystal Sr3Fe2O5Br2\mathrm{Sr_3Fe_2O_5Br_2}, respectively.

Results and discussion

Sample synthesis and Crystal structure

Although some synthesis was reported before [30, 31], we further optimize the sample growth methods and extend to the whole Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2} (X=F,Cl,BrX = \mathrm{F}, \mathrm{Cl}, \mathrm{Br}) family. Both polycrystalline Sr3Fe2O5Cl2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Cl}_{2} and Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2} can be synthesized via conventional solid-state synthesis, while poly (vinylidene fluoride) (PVDF) to Sr3Fe2O7\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{7} is very critical and needs to be fine-tuned, in order to obtain a phase-pure, layered form of Sr3Fe2O5F2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{F}_{2}. As for the single-crystalline form of Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2}, Sr3Fe2O5Cl2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Cl}_{2} crystals can be readily obtained via the widely used SrCl2\mathrm{SrCl}_{2} flux method. We further optimize the flux growth parameters for Sr3Fe2O5Cl2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Cl}_{2}, producing large single crystals with lateral dimensions reaching ∼\sim 20 mm (Figure 2(a)). Similar method applied to the growth of Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2} single crystals, however, only yields small (sub-millimeter scale) and brittle thin flakes. To obtain large single crystals of Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2}, a new flux growth involves FeC2O6H4\mathrm{FeC}_{2}\mathrm{O}_{6}\mathrm{H}_{4} instead of Fe2O3\mathrm{Fe}_{2}\mathrm{O}_{3} in a Czochralski furnace with a temperature gradient is utilized, producing large single crystals with lateral dimensions reaching ∼\sim 5 mm (Figure 2(a)).

X-ray diffraction patterns and refined structural parameters of Sr3Fe2O5X2 powders

Figure 2. X-ray diffraction (XRD) patterns and refined structural parameters of Sr3_3Fe2_2O5_5X2_2 (XX = F, Cl, Br) powders at room temperature. (a) Optical micrographs of the Sr3_3Fe2_2O5_5Cl2_2 and Sr3_3Fe2_2O5_5Br2_2 single crystals. (b)(d)(f) Powder XRD pattern of polycrystalline Sr3_3Fe2_2O5_5X2_2 at room temperature: (b) XX = F, (d) XX = Cl and (f) XX = Br. The panels of (c) and (e) indicate the XRD patterns of Sr3_3Fe2_2O5_5Cl2_2 and Sr3_3Fe2_2O5_5Br2_2 single crystals along the (0 0 LL) direction. (g)-(i) Select structural information from powder XRD refinements of Sr3_3Fe2_2O5_5X2_2: (g) lattice parameters aa and cc, (h) Fe-X bond lengths and van der Waals spatial gaps, (i) Fe − O1_1 − Fe bond lengths dFe−O1−Fed_{\mathrm{Fe-O1-Fe}} and O2_2 − Fe − O2_2 bond angles θO2−Fe−O2\theta_{\mathrm{O2-Fe-O2}}.

In order to confirm the layered crystal structure and phase purity of Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2}, diffraction and imaging measurements were performed (Figure 1, Figure 2, S1). First, powder XRD measurements on all three polycrystalline samples were collected at room temperature. The XRD patterns can be indexed with a tetragonal structure with a space group I4/mmmI4/mmm, as shown in Figure 2(b), Figure 2(d), and Figure 2(f). From Rietveld refinements, all halide atoms occupy the outer apical oxygen sites (Figure 1(b)), because of which the neighboring planes of halides are bonded through van der Waals interactions, leading to a layered structure with vdW gaps and micaceous character. The plate-like single crystals of Sr3Fe2O5Cl2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Cl}_{2} and Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2} are also characterized by XRD, revealing only sharp (0 0 LL) Bragg reflections (Figure 2(c) and Figure 2(e)). To further confirm the crystalline quality of Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2}, single crystal XRD measurements are performed at 150 K (Figure S1). No impurity phase was detected and the I4/mmmI4/mmm tetragonal structure is verified as well.

Figure 2(g)-(Figure 2i) and Table 1 summarize the evolution of the obtained lattice parameters and some select bond lengths and angles from powder XRD refinements, as a function of the halide species XX. Upon halide substitution from X=FX = \mathrm{F} to Br\mathrm{Br}, both the lattice parameters aa and cc increase monotonically. However, this expansion is significantly more pronounced along the lattice cc direction than within the abab-plane. Quantitatively, from X=FX = \mathrm{F}, to Cl\mathrm{Cl} and Br\mathrm{Br}, lattice parameter aa increases from 3.91 Å to 3.95 Å and 3.96 Å, which displays an increase of only 0.05 Å (about 1% enhancement from X=FX = \mathrm{F} to X=BrX = \mathrm{Br}); while lattice parameter cc increases from 21.38 Å to 23.80 Å and eventually to 25.42 Å, marking an enormous elongation of 4.04 Å (about 19% increase from X=FX = \mathrm{F} to X=BrX = \mathrm{Br}). This anisotropic lattice expansion primarily originates from the increase in the ionic radius of the constituent halide ions and their electronegativity, where the halide ions only occupy the apical oxygen sites. Both a larger ionic radius and smaller electronegativity favor a longer bond length, as exemplified in the increase of the Fe-X bond distances (Figure 2(h)). This is directly related to the increase of lattice parameter cc, and the significant enlargement of the vdW spatial gaps as well, from 1.65 Å, to 2.13 Å, and eventually to 2.48 Å, for X=F,Cl,BrX = \mathrm{F}, \mathrm{Cl}, \mathrm{Br}, respectively (Figure 2(h)). It should be noted that, within the bilayer motif, the Fe-O1-Fe bond length dFe−O1−Fed_{\mathrm{Fe-O1-Fe}} and O2-Fe-O2 angle θO2−Fe−O2\theta_{\mathrm{O2-Fe-O2}} do not evolve monotonically, as shown in Figure 2(i).

Sr3Fe2O5F2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{F}_{2}Sr3Fe2O5Cl2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Cl}_{2}Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2}
aa (Å)3.908(1)3.947(1)3.960(1)
cc (Å)21.383(1)23.799(2)25.425(1)
vdW gap (Å)1.652(1)2.132(1)2.479(1)
Fe–O1 (Å)1.911(3)1.889(2)1.922(3)
Fe–O2 (Å)1.966(2)2.001(1)1.994(1)
Fe–X (Å)2.478(2)2.938(1)3.193(2)
Sr1–O1 (Å)2.764(1)2.791(1)2.800(1)
Sr1–O2 (Å)2.897(2)2.972(1)2.930(2)
Sr2–O2 (Å)2.579(2)2.485(1)2.543(1)
Sr2–X (Å)2.823(2)2.998(1)3.113(1)
Fe–O1–Fe (°)180.00180.00180.00
O2–Fe–O2 (°)167.18(1)160.82(1)166.27(1)
O1–Sr1–O1 (°)180.00180.00180.00
O2–Sr1–O2 (°)84.83(1)83.19(2)84.99(2)

Table 1. Refined lattice parameters, select bond lengths (in units of Å) and bond angles (in units of °) from powder x-ray diffraction patterns of Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2} at room temperature.

Scanning transmission electron microscopy (STEM)

Ultrathin nanosheets of Sr3Fe2O5Br2\mathrm{Sr_3Fe_2O_5Br_2} were isolated via mechanical exfoliation, with a typical optical micrograph shown in Figure S2(a). Atomic force microscopy was used to determine the thickness of the flakes. The atomic force microscopy measurements reveal a topographic height of approximately 3 nm (Figure 1(c) and Figure 1(d)). This value is close to the value of lattice parameter cc, which corresponds to one unit cell (u.c.) thickness. To directly observe the van der Waals spatial gap at the atomic scale, STEM was used to further characterize the local structure of Sr3Fe2O5Br2\mathrm{Sr_3Fe_2O_5Br_2} single crystals. Figure 1(e) and Figure 1(f) display a high-angle annular dark-field (HAADF) image and a multislice electron ptychography (MEP) image acquired along the [100] zone axis, respectively. The characteristic bilayer RP-phase structure is clearly resolved. Specifically, the apical sites are exclusively occupied by Br atoms across the entire field of view. This uniform occupation confirms the presence of long-range structural order and establishes a distinct van der Waals gap between adjacent Br atomic layers. These findings indicate the easily cleavable nature of the vdW materials Sr3Fe2O5X2\mathrm{Sr_3Fe_2O_5X_2}, particularly for X=BrX = \mathrm{Br}, where the interlayer spatial gap is largest (about 2.48 Å).

Magnetic properties

Figure 3 shows the magnetization data for all synthesized Sr3Fe2O5X2\mathrm{Sr_3Fe_2O_5X_2} compounds. The temperature dependent susceptibility of the polycrystalline Sr3Fe2O5X2\mathrm{Sr_3Fe_2O_5X_2} sample is presented in Figure 3(a)-(Figure 3c). Owing to strong antiferromagnetic interactions, the susceptibility data exhibit only weak temperature dependence and display smooth minima at approximately 580 K, 533 K and 540 K for X=F,Cl,BrX = \mathrm{F}, \mathrm{Cl}, \mathrm{Br}, respectively. These minima of the susceptibility data correspond to their Néel temperatures. For instance, the Néel temperature TN∼545T_N \sim545 K of Sr3Fe2O5Cl2\mathrm{Sr_3Fe_2O_5Cl_2} is determined from Mössbauer measurements [30], fully consistent with our susceptibility data. Above the AFM transition temperature, the susceptibility still increases, likely due to the presence of strong short-range correlations that are progressively suppressed towards even higher temperatures above TNT_{\mathrm{N}}. Isothermal magnetization measurements on these polycrystalline samples reveal linear behavior at select temperatures from 100 K to 400 K (Figure 3(d)-(Figure 3f)), directly confirming the AFM nature of Sr3Fe2O5X2\mathrm{Sr_3Fe_2O_5X_2} at room temperature. We also performed temperature dependent susceptibility study on the Sr3Fe2O5Cl2\mathrm{Sr_3Fe_2O_5Cl_2} and Sr3Fe2O5Br2\mathrm{Sr_3Fe_2O_5Br_2} single crystals with a 7 T magnetic field applied along the abab-plane direction, demonstrating similar characteristics to their polycrystalline counterparts (Figure 3(g)-(Figure 3h)). Combining all magnetization data together, it is evident that the layered oxyhalides Sr3Fe2O5X2\mathrm{Sr_3Fe_2O_5X_2} exhibit robust beyond room temperature antiferromagnetism.

Magnetization data of Sr₃Fe₂O₅X₂

Figure 3. Magnetization data of Sr₃Fe₂O₅X₂. (a)–(c) Temperature-dependent magnetization of the three polycrystalline samples measured under an applied magnetic field of 7 T. (d)–(f) Isothermal magnetization of Sr₃Fe₂O₅X₂ measured from 100 K to 400 K (step 100 K). Temperature-dependent magnetization of (g) Sr₃Fe₂O₅Cl₂ and (h) Sr₃Fe₂O₅Br₂ single crystals measured with the magnetic field applied parallel to the abab-plane. (i) The magnetic transition temperature as a function of halogen XX substitution. Solid diamond denotes the TNT_{\mathrm{N}} of Sr₃Fe₂O₅Cl₂ determined by Mössbauer spectroscopy [30].

Figure 3(i) summarizes the Néel temperature as a function of the halide species XX in Sr3Fe2O5X2\mathrm{Sr_3Fe_2O_5X_2}. The magnetic transition temperature shows a decreasing trend from X=FX = \mathrm{F} to Br\mathrm{Br}, Cl\mathrm{Cl}. In particular, Sr3Fe2O5F2\mathrm{Sr_3Fe_2O_5F_2} has the largest TN∼580T_{\mathrm{N}} \sim580 K among all reported, layered vdW antiferromagnets, as far as we are concerned. It should be noted that because of the much smaller ionic radius of F−\mathrm{F^-}, oxyfluorides tend to possess a significant amount of disorder. For example, Sr3Fe2O5.45F1.56\mathrm{Sr_3Fe_2O_{5.45}F_{1.56}} powder was synthesized before, but it exhibits pronounced static anion disorder. As a result, its reported TNT_{\mathrm{N}} is only ∼390\sim390 K [32], markedly lower than TN∼580T_{\mathrm{N}} \sim580 K in our work. As a further comparison, among single-layer RP oxyhalides, disordered oxyfluorides such as Sr2CoO3F\mathrm{Sr_2CoO_3F} (TN≈323T_{\mathrm{N}} \approx323 K) [33] and Sr2NiO3F\mathrm{Sr_2NiO_3F} (TN≈18T_{\mathrm{N}} \approx18 K) [34] all exhibit lower Néel temperatures than their Cl-ordered counterparts Sr2CoO3Cl\mathrm{Sr_2CoO_3Cl} (TN≈330T_{\mathrm{N}} \approx330 K) [35] and Sr2NiO3Cl\mathrm{Sr_2NiO_3Cl} (TN≈28T_{\mathrm{N}} \approx28 K) [34, 36]. Furthermore, Sr2FeO3F\mathrm{Sr_2FeO_3F} (S=5/2S = 5/2) with a low disorder level (∼5%\sim5\%) exhibits a transition temperature of approximately 340 K, approaching that of the fully ordered phase (∼358\sim358 K) [37]. Collectively, these results suggest that the Néel temperature of Sr3Fe2O5F2\mathrm{Sr_3Fe_2O_5F_2} is very sensitive to the degree of F-ion disorder, highlighting the importance and necessity to realize a fully ordered phase in Sr3Fe2O5F2\mathrm{Sr_3Fe_2O_5F_2} and other vdW magnets.

Having established the macroscopic AFM orders in Sr3Fe2O5X2\mathrm{Sr_3Fe_2O_5X_2}, temperature-dependent neutron powder diffraction measurements were performed on polycrystalline Sr3Fe2O5Br2\mathrm{Sr_3Fe_2O_5Br_2} samples, in order to probe the microscopic magnetic properties. Figure 4(a)-(Figure 4c) display the neutron diffraction patterns collected at select temperatures (4 K, 300 K and 550 K). Alongside nuclear Bragg reflections, additional magnetic Bragg peaks (marked by * symbols) are clearly observed at 4 K and 300 K. Their peak intensities decrease upon warming, completely vanishing at 550 K (Figure 4(d)), aligning with TNT_{\mathrm{N}} inferred from the susceptibility minimum point. These magnetic reflections can be indexed with a magnetic propagation vector of k=(1/2,1/2,0)\mathbf{k} = (1/2, 1/2, 0). Magnetic symmetry analysis based on the parent crystallographic space group I4/mmmI4/mmm allows the magnetic moments to be aligned either along the lattice cc axis or within the abab-plane. However, Mössbauer spectroscopy measurements [31] rule out the possibility of the c-axis spin configuration. Following the method proposed by Knee et al. [29], our refined G-type antiferromagnetic structure is illustrated in Figure 4(e), where the spins are coupled antiferromagnetically both within the abab-plane and between adjacent layers. The in-plane magnetic moments are canted approximately 13∘13^\circ from the [1 0 0] direction, similar to previous reports [29, 30]. Also, the magnitude of the ordered magnetic moment was refined at various temperatures, yielding approximately 4.08 μB4.08\,\mu_{\mathrm{B}}/Fe at 4 K.

Neutron diffraction patterns and magnetic structure of $\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2}$

Figure 4. Neutron diffraction patterns and magnetic structure of Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2}. Neutron diffraction patterns of Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2} collected at (a) 550 K, (b) 300 K (CMRR), and (c) 4 K (CSNS). * indicates magnetic diffraction peaks indexed by the propagation vector (1/2,1/2,0)(1/2, 1/2, 0). The upper tick marks (green) indicate the positions of the nuclear reflections, while the lower tick marks (red) denote the magnetic reflections. (d) Enlarged local neutron diffraction patterns, where | (red) represent the magnetic Bragg positions. (e) G-type magnetic structure model of Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2}, exhibiting antiparallel spin alignments both intra- and inter-layer. Here the black lines indicate enlarged magnetic (mag) cells with respect to nuclear (nuc) unit cells: amag=2anuca_{\mathrm{mag}} = 2a_{\mathrm{nuc}}, bmag=2bnucb_{\mathrm{mag}} = 2b_{\mathrm{nuc}}, and cmag=cnucc_{\mathrm{mag}} = c_{\mathrm{nuc}}.

Band gap

The semiconducting nature of Sr3Fe2O5X2\mathrm{Sr_3Fe_2O_5X_2} is verified by measuring both optical and electronic gaps (Figure 5 and Figure S4). The direct and indirect optical bandgaps of the three compounds were estimated via Tauc plot analysis [38, 39, 40], which was performed on their diffuse reflectance spectra. Detailed methodology is provided in the Supplementary Information Note 3. Because the Tauc method relies on a pre-assumed electronic transition type, the derivation of absorption spectrum fitting method (DASF) [41, 42] was adopted, assigning the peak position of the derivative curve as the bandgap value. As shown in Figure 5(j), the direct bandgap values extracted via the Tauc method are in agreement with the DASF results. The maximum transition index γ\gamma (the slope of the curve) derived from the DASF method is approximately 0.63 (Figure 5(k)), which is close to the theoretical index of 0.5 for a direct bandgap (2 for indirect bandgap). The electronic bandgap was measured by the ARPES study on Sr3Fe2O5Br2\mathrm{Sr_3Fe_2O_5Br_2} single crystals. The integrated intensity of density of states (DOS) is plotted against energy EE with respect to the Fermi energy EFE_{\mathrm F}. To exclude a space charge effect, different photoelectron count rates are used. It is evident that the DOS is only visible deeply below EFE_{\mathrm F}, yielding an electronic gap value greater than 2 eV (Figure 5(l)). This number is comparable to the optical bandgaps in Sr3Fe2O5X2\mathrm{Sr_3Fe_2O_5X_2}. Overall, the bandgap value of Sr3Fe2O5X2\mathrm{Sr_3Fe_2O_5X_2} displays a small decrease from XX = F, to XX = Cl and Br. This observation is likely because the halide species primarily modifies the local crystal-field environment rather than fundamentally altering the electronic band structure.

Bandgap characterizations of Sr$_3$Fe$_2$O$_5$X$_2$

Figure 5. Bandgap characterizations of Sr3_3Fe2_2O5_5X2_2. (a)-(i) Comparison of the optical bandgaps determined using Tauc plots (for direct and indirect transition models) and the DASF method. The determination of EgE_{\mathrm{g}} is shown by the dash lines; (j) Optical bandgap versus halide species XX; (k) Transition indices derived from the DASF method; the index values for the F, Cl, and Br systems are 0.29, 0.58, and 0.63, respectively; (l) Angle-resolved photoemission spectroscopy (ARPES) measurements of the Sr3_3Fe2_2O5_5Br2_2 single crystal, where the integrated density of states are plotted against energy using different photoelectron count rates (1/s). An electronic band gap ∼2\sim2 eV below the Fermi energy EFE_{\mathrm{F}} is indicated by the red arrow.

Density functional theory (DFT) calculations

To understand the electronic and magnetic properties of Sr3Fe2O5X2\mathrm{Sr}_3\mathrm{Fe}_2\mathrm{O}_5\mathrm{X}_2, theoretical calculations based on the density functional theory (DFT) via the VASP software package are performed, as shown in Figure 6 and Supplementary Information Note 4. Based on the Heisenberg model (Figure 6(a)), the out-of-plane 180∘180^\circ Fe-O1-Fe superexchange coupling constant (J1J_1) within the bilayer motifs and the in-plane Fe-O2-Fe superexchange interaction (J2J_2) are dominating (Figure 6(d)-(Figure 6e), Table 2). Upon halogen substitution from F to Br, J1J_1 increases from 102.41 meV, to 109.97 meV and 111.81 meV; while J2J_2 decreases from 54.88 meV to 50.52 and 49.66 meV. This is a bit surprising, since both the experimentally determined Fe-O1-Fe bond length dFe−O1−Fed_{\mathrm{Fe-O1-Fe}} and O2-Fe-O2 angle θO2−Fe−O2\theta_{\mathrm{O2-Fe-O2}} do not evolve monotonically. On the other hand, the J1J_1 and J2J_2 numbers are much larger than other spin exchange coupling constants J3J_3 to J6J_6, particularly the inter-bilayer coupling (JcJ_c), which is less than 1 meV. Resultingly, theoretical estimated Néel temperatures of bulk Sr3Fe2O5X2\mathrm{Sr}_3\mathrm{Fe}_2\mathrm{O}_5\mathrm{X}_2 display a decreasing trend from 624 K, 554 K, to 569 K, for X=FX = \mathrm{F} to X=BrX = \mathrm{Br} and X=ClX = \mathrm{Cl}, respectively (Figure 6(b)). This decreasing trend of TNT_\mathrm{N}, as well as other calculated quantities, such as bandgap magnitude (∼2.16\sim2.16 eV), lattice parameters and spin moment size (∼4 μB\sim4\,\mu_\mathrm{B}/Fe) are all consistent with the experimental numbers (Figure 6(b),(Figure 6c),(Figure 6f),(Figure 6g)).

MaterialsJ1J_1J2J_2J3J_3J4J_4J5J_5J6J_6JcJ_cTNT_{\mathrm{N}}
Bulk
Sr3Fe2O5F2Sr_3Fe_2O_5F_2102.4154.883.312.340.491.200.09624
Sr3Fe2O5Cl2Sr_3Fe_2O_5Cl_2109.9750.523.922.97-0.081.28-0.04554
Sr3Fe2O5Br2Sr_3Fe_2O_5Br_2111.8149.663.482.370.481.050.08569
One unit-cell
Sr3Fe2O5F2Sr_3Fe_2O_5F_295.2859.603.252.480.311.460.67633
Sr3Fe2O5Cl2Sr_3Fe_2O_5Cl_2106.7051.983.582.94-0.121.40-0.47544
Sr3Fe2O5Br2Sr_3Fe_2O_5Br_2110.8250.193.482.070.271.210.58548
Half unit-cell
Sr3Fe2O5F2Sr_3Fe_2O_5F_293.2461.533.533.150.171.93–655
Sr3Fe2O5Cl2Sr_3Fe_2O_5Cl_2104.8752.683.022.83-0.090.76–595
Sr3Fe2O5Br2Sr_3Fe_2O_5Br_2110.6750.773.502.680.191.65–547

Table 2. Exchange parameters JJ (meV) and Néel temperatures TNT_{\mathrm{N}} (K) obtained from DFT calculations.

Theoretical calculation results of Sr3Fe2O5X2

Figure 6. Theoretical calculation results of Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2}. (a) Schematic diagram of the magnetic unit cell and the Heisenberg exchange coupling model with the main considered spin exchange constants J1J_{1} to J6J_{6}, and JcJ_{\mathrm{c}} (amag=2anuca_{\mathrm{mag}} = \sqrt{2}a_{\mathrm{nuc}}, bmag=2bnucb_{\mathrm{mag}} = \sqrt{2}b_{\mathrm{nuc}}, cmag=cnucc_{\mathrm{mag}} = c_{\mathrm{nuc}}). Calculated (b) Néel temperature; (c) bandgaps; (d)-(e) Heisenberg exchange coupling constants J1J_{1} and J2J_{2}, respectively; (f) lattice parameter aa; and (g) magnetic moments. (h)-(j) The projected energy band structure with orbital weights for the three compounds of Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2}: (h) X=FX = \mathrm{F}; (i) X=ClX = \mathrm{Cl}; (j) X=BrX = \mathrm{Br}, respectively.

To examine the stability of the AFM order in the 2D limit, DFT calculations are performed on Sr3Fe2O5X2\mathrm{Sr}_3\mathrm{Fe}_2\mathrm{O}_5\mathrm{X}_2 from bulk to one unit cell (one-u.c.) and half unit cell (half-u.c.) thickness. As indicated from Figure 6(b)-(Figure 6g), nearly all quantities display small variations, even when the sample thickness is reduced from bulk to the 2D limit. Particularly, because the intrinsic inter-bilayer coupling (JcJ_c) is extremely weak, exfoliation does not disrupt the primary spin exchange interactions (J1J_1 and J2J_2). Therefore, the TNT_\mathrm{N} of Sr3Fe2O5X2\mathrm{Sr}_3\mathrm{Fe}_2\mathrm{O}_5\mathrm{X}_2 are maintained down to the 2D limit. More interestingly, the TNT_\mathrm{N} of Sr3Fe2O5F2\mathrm{Sr}_3\mathrm{Fe}_2\mathrm{O}_5\mathrm{F}_2 and Sr3Fe2O5Br2\mathrm{Sr}_3\mathrm{Fe}_2\mathrm{O}_5\mathrm{Br}_2 display a further increase, to the highest number of 655 K for monolayer Sr3Fe2O5F2\mathrm{Sr}_3\mathrm{Fe}_2\mathrm{O}_5\mathrm{F}_2 (TN∼595T_\mathrm{N} \sim595 K for monolayer Sr3Fe2O5Cl2\mathrm{Sr}_3\mathrm{Fe}_2\mathrm{O}_5\mathrm{Cl}_2) (Figure 6(b)), base on DFT calculations.

The orbitally projected band structures of Sr3Fe2O5X2\mathrm{Sr}_3\mathrm{Fe}_2\mathrm{O}_5\mathrm{X}_2 are shown in Figure 6(h)-(Figure 6j). The valence band maximum (VBM) is primarily derived from the O-pp orbitals, whereas the conduction band minimum (CBM) mainly originates from the Fe-dd orbitals. Obviously, the halogen pp orbitals are deeply buried below the Fermi level. This explains the nearly constant ∼2.1\sim2.1 eV magnitude of the electronic bandgap in Sr3Fe2O5X2\mathrm{Sr}_3\mathrm{Fe}_2\mathrm{O}_5\mathrm{X}_2. Based on the DFT-calculated electronic band structures, an indirect electronic bandgap is inferred, contrasting with the conclusions derived from the optical spectra. However, the energy difference between the indirect transition (N→PN \to P point) and the direct transition (N→NN \to N point) in this system is exceptionally small (only approximately 0.04 eV).

Discussion

The Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2} compounds are derived from Sr3Fe2O7\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{7} (TN=115T_{\mathrm{N}} = 115 K) [43] via substituting the apical O2−\mathrm{O}^{2-} site at the axial terminal of the FeO5\mathrm{FeO}_{5} square pyramid with halide ions X−\mathrm{X}^{-} (X=F,Cl,Br\mathrm{X} = \mathrm{F}, \mathrm{Cl}, \mathrm{Br}). This substitution reduces the planarity of the Fe-O2 planes and concurrently deviates the in-plane Fe-O2-Fe bond angles (equal to θO2−Fe−O2\theta_{\mathrm{O2-Fe-O2}}) from ∼176∘\sim176^\circ in Sr3Fe2O7\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{7}, resulting in highly distorted FeO5X\mathrm{FeO}_{5}\mathrm{X} (X=F,Cl,Br\mathrm{X} = \mathrm{F}, \mathrm{Cl}, \mathrm{Br}) octahedra. Despite these local structural distortions, the overall tetragonal symmetry (space group I4/mmmI4/mmm) is preserved. Importantly, with such substitution in Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2}, adjacent layers of halide atoms with vdW spatial gaps between the structural block motif are formed (Figure 1(a)), forming layered structures. On the other hand, the asymmetric mixed-anion coordination environment induces a strong elongation of the local octahedra along the zz-axis, leading to crystal-field splitting of the degenerate dd orbitals of the Fe ions. This non-centrosymmetric coordination environment relaxes the Laporte rule [44], allowing light absorption via dd-dd transitions, which are noticeable and have an energy scale ∼1.5\sim1.5 eV, as shown in Figure 6(a), Figure 6(d), Figure 6(g).

Although the halide ions of Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2} do not directly participate in the magnetic exchange pathways, their replacements of the apical oxygen in Sr3Fe2O7\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{7} fundamentally alter the microscopic magnetic properties. Firstly, due to charge balance, the average valence state of iron is an unstable Fe4+\mathrm{Fe}^{4+} in Sr3Fe2O7\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{7}, which displays a charge disproportionation at ∼343\sim343 K (2Fe4+→Fe3++Fe5+2\mathrm{Fe}^{4+} \to\mathrm{Fe}^{3+} + \mathrm{Fe}^{5+}) [43, 45, 46]. This phenomenon disappears in Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2}, because Fe3+\mathrm{Fe}^{3+} is a stable state. Consequently, the electronic structures of Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2} are relatively simple, maintaining a nearly 2.1 eV gap. While DFT calculations indicate an indirect bandgap, direct transition of optical excitation might dominate the absorption edge due to its higher transition probability. This leads to the appeared discrepancy between the theoretical calculations and the optical spectra. More sensitive experimental techniques, such as photothermal deflection spectroscopy, are required to determine the transition mechanism.

Secondly, in Sr3Fe2O5X2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{X}_{2}, the half-filled 3d53d^{5} shell of Fe3+\mathrm{Fe}^{3+} with a high spin state S=5/2S = 5/2 enables strong superexchange couplings through oxygen ligands. Based on DFT calculations, both out of-plane (Fe-O1-Fe, J1J_1) and in-plane (Fe-O2-Fe, J2J_2) nearest-neighbor superexchange couplings are cooperating synergistically, which is directly responsible for the enormous five-fold increase in Néel temperature, from TN∼115T_{\mathrm{N}} \sim115 K in Sr3_3Fe2_2O7_7 to TN∼580T_{\mathrm{N}} \sim580 K in Sr3_3Fe2_2O5_5F2_2. Microscopically, this strong superexchange arises from the pronounced hybridization between the Fe 3d3d and O 2p2p orbitals, which is facilitated by the ideal 180° Fe − O1_1 − Fe bond angle for J1J_1 and the large Fe − O2_2 − Fe bond angle (∼160∘\sim160^\circ–167∘167^\circ) for J2J_2. Such bonding geometries maximize the effective electron hopping integral, particularly the out-of-plane direction, yielding strong antiferromagnetic coupling. This synergy of magnetic couplings stabilizes a G-type AFM order with every Fe3+^{3+} spin antiparallel to all its nearest neighbors in Sr3_3Fe2_2O5_5X2_2. Although the calculated further-neighbor exchange interactions (J3J_3 to J6J_6, and JcJ_{\mathrm{c}}) are relatively weak, they still contribute to the large TNT_{\mathrm{N}} in Sr3_3Fe2_2O5_5X2_2. Consequently, even though calculated J1=102.41J_1 = 102.41 meV for bulk Sr3_3Fe2_2O5_5X2_2 (X = F) is smallest compared to that of 109.97 meV for X = Cl and 111.81 meV for X = Br, its calculated TNT_{\mathrm{N}} is highest for X = F. It should be noted that JcJ_{\mathrm{c}} is negligibly small compared to all other spin exchange constants. As a result, reducing the thickness of Sr3_3Fe2_2O5_5X2_2 down to the 2D limit, the TNT_{\mathrm{N}} still remains ∼600\sim600 K or becomes even higher after relaxing the spin exchange strengths, according to DFT calculations. It would be very interesting to experimentally monitor and verify this predicted evolution of TNT_{\mathrm{N}} in Sr3_3Fe2_2O5_5X2_2 as a function of flake thickness down to the true 2D limit.

Conclusion

In conclusion, we promote a layered vdW material family with beyond-room-temperature antiferromagnetic orders in Sr3_3Fe2_2O5_5X2_2. The layered form of Sr3_3Fe2_2O5_5F2_2 displays the largest TN∼580T_{\mathrm{N}} \sim580 K. Single crystals of Sr3_3Fe2_2O5_5Cl2_2 with lateral dimension reaching more than 20 mm are obtained; while one-unit-cell thick thin-flakes of Sr3_3Fe2_2O5_5Br2_2 are readily isolated via mechanical exfoliation, highlighting the layered nature of Sr3_3Fe2_2O5_5X2_2. DFT calculations demonstrate that the nearest neighbor out-of-plane and in-plane superexchange interactions (J1J_1 and J2J_2) within the bilayer motifs of Sr3_3Fe2_2O5_5X2_2 are mainly responsible for the large TNT_{\mathrm{N}}, which is predicted to persist even upon exfoliation down to the monolayer limit. Our work highlights that bilayer RP-phase iron-based oxyhalides Sr3_3Fe2_2O5_5X2_2 represent a novel class of van der Waals magnets with approaching ∼600\sim600 K AFM magnetic order. Its high TNT_{\mathrm{N}} far above room temperature and cleavable, mica-like nature, as well as the wide optical bandgap and semiconducting nature, offer an ideal platform for exploring magnetism in the two-dimensional limit, promising for spintronic devices and magnetic memory applications.

Materials and method

Synthesis

Polycrystalline Sr3Fe2O5F2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{F}_{2} samples were prepared via chemical fluorination [32, 47]. The Sr3Fe2O7\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{7} precursor was produced via a typical solid-state reaction method [48]. Fluorination was carried out in an evacuated quartz tube. Specifically, Sr3Fe2O7\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{7} and PVDF were mixed in a 1:1.5 molar ratio, ground together, and vacuum-sealed in the tube. The mixture was heated at 350 °C for 24 h, yielding a reddish-brown powder. Polycrystalline Sr3Fe2O5Cl2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Cl}_{2} and Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2} were synthesized using a similar solid-state approach as previously reported [29]. Stoichiometric amounts of SrO (decompose from SrCO3\mathrm{SrCO}_{3} at 1100 °C, 4 days), Fe2O3\mathrm{Fe}_{2}\mathrm{O}_{3} (dried at 200 °C for 2 h) and SrCl2\mathrm{SrCl}_{2} (SrBr2\mathrm{SrBr}_{2}) were mixed and ground thoroughly in an agate mortar within a glove box. The resulting mixture was pelletized and placed in an alumina crucible, before being vacuum-sealed in a quartz ampoule. Subsequently, the tube was sintered at 850 °C for 48 h to obtain a red product.

Single crystals of Sr3Fe2O5Cl2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Cl}_{2} and Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2} were grown using a high-temperature flux method. Sr3Fe2O5Cl2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Cl}_{2} was prepared following the protocol described in Ref. [30]. Starting materials with a molar ratio of SrCO3:Fe2O3:SrCl2=2:1:40\mathrm{SrCO}_{3} : \mathrm{Fe}_{2}\mathrm{O}_{3} : \mathrm{SrCl}_{2} = 2:1:40 were mixed, ground, and loaded into an alumina crucible with a lid. The crucible was placed in a box furnace, heated to 1100 °C, held for 24 h, and then cooled to 875 °C at a rate of 1 °C/h. Sr3Fe2O5Cl2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Cl}_{2} crystals were also obtained using the same heating profile with a molar ratio of SrCO3:Fe2O3:SrCl2=2:1:15\mathrm{SrCO}_{3} : \mathrm{Fe}_{2}\mathrm{O}_{3} : \mathrm{SrCl}_{2} = 2:1:15. A representative crystal is shown in Figure 2(a). Attempts to grow Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2} single crystals using this specific protocol failed. Instead, Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2} single crystals were successfully grown using SrCO3\mathrm{SrCO}_{3}, FeC2O6H4\mathrm{FeC}_{2}\mathrm{O}_{6}\mathrm{H}_{4}, and SrBr2\mathrm{SrBr}_{2} (from SrBr2⋅6H2O\mathrm{SrBr}_{2} \cdot6\mathrm{H}_{2}\mathrm{O} at 345 °C, 1 day), as starting materials in a molar ratio of 2:2:5. The loaded crucible was sintered at 850 °C for 5 h in a Czochralski furnace, followed by a slow cooling process to 600 °C over 72 h before the furnace was switched off. Plate-like Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2} single crystals with typical lateral dimensions of approximately 5 mm are shown in Figure 2(a). Notably, repeated growth attempts using a box furnace failed to yield the target phase. We attribute this successful crystallization to the enhanced vertical thermal gradient characteristic of the Czochralski furnace. Single-crystalline Sr3Fe2O5F2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{F}_{2} was not obtained, likely due to the high chemical stability of SrF2\mathrm{SrF}_{2}. High-pressure synthesis techniques may facilitate the growth of this compound [32].

Characterization

Single-crystal X-ray diffraction (SCXRD) data were collected using a Bruker APEX-II CCD X-ray diffractometer at 150 K, while powder X-ray diffraction (PXRD) measurements were performed at room temperature using a Rigaku MiniFlex diffractometer.

Temperature-dependent magnetic susceptibility measurements were performed on a Physical Property Measurement System (PPMS) from 300 to 700 K under a magnetic field of 70 kOe. Isothermal magnetization curves were recorded using a Magnetic Property Measurement System (MPMS).

Neutron diffraction data for the polycrystalline Sr3Fe2O5Br2\mathrm{Sr}_{3}\mathrm{Fe}_{2}\mathrm{O}_{5}\mathrm{Br}_{2} samples were collected at various temperatures. High-temperature neutron powder diffraction measurements were performed at the China Mianyang Research Reactor (CMRR, China), using a neutron wavelength of λ=1.8848\lambda= 1.8848 Å, and diffraction patterns were recorded at 300 K and 550 K, respectively. Low-temperature diffraction data at 4 K were collected using the General Purpose Powder Diffractometer (31113.02.CSNS.GPPD) at China Spallation Neutron Source (CSNS, China). Rietveld refinements of the diffraction data were conducted using the Fullprof suite [49], and magnetic structures were determined using SARAh [50].

The Ultraviolet-Visible (UV-Vis) diffuse reflectance spectra of all polycrystalline samples were measured using a Cary 5000 spectrophotometer (Agilent) in the spectral range of 300∼1500300 \sim1500 nm at room temperature.

ARPES measurements were performed using a home-lab ARPES system equipped with a DA30L electron analyzer and a helium lamp light source with 21.2 eV photon energy. The angle resolution was set to 0.3 degrees and the energy resolution was set to 20 meV.

TEM specimens were prepared using a focused ion beam (FIB) instrument (Thermo Fisher Helios 5CX) equipped with a Ga ion source. The specimens were sequentially thinned down to 20 nm using decreasing accelerating voltages, followed by a final low-voltage (1 kV) ion milling step to remove residual amorphous layers. Atomic-resolution structural characterization was performed using a spherical aberration-corrected transmission electron microscope (JEM NeoARM200, JEOL Ltd., Tokyo) operated at 200 kV. The dataset was acquired using a highspeed direct electron detection camera (DECTRIS ARINA), yielding a four-dimensional STEM with data volume of 192×192×400×400192 \times192 \times400 \times400.

First-principles calculations were performed using the Vienna Ab initio Simulation Package (VASP) [51, 52] with the projector augmented-wave (PAW) method and a plane-wave cutoff energy of 450 eV. The Perdew–Burke–Ernzerhof (PBE) functional within the generalized gradient approximation (GGA) was employed [53]. The DFT + UU method [54] was employed with an effective Hubbard parameter Ueff=4U_{\mathrm{eff}} = 4 eV for Fe 3d3d electrons. For bulk systems, the experimental lattice constants were adopted. For two-dimensional (2D) systems, the in-plane lattice constants were fully optimized. All atomic positions were relaxed until the Hellmann–Feynman forces on each atom were below 0.01 eV/A˚\mathring{A}. The van der Waals interactions were taken into account using the DFT-D3 correction scheme [55]. Brillouin-zone integrations were carried out using Γ\Gamma-centered Monkhorst–Pack kk-point meshes [56]. For the magnetic unit cell corresponding to a 2×2×1\sqrt{2} \times\sqrt{2} \times1 supercell of the primitive cell, 6×6×26 \times6 \times2 and 6×6×16 \times6 \times1 kk-point grids were employed for bulk and 2D systems, respectively.

References

Acknowledgments

Work at SYSU was supported by the National Natural Science Foundation of China (Grants No. 12574140, No. 12494591, No. 12425404, U25A20193, 92565303), the National Key Research and Development Program of China (Grant No. 2023YFA1406500), the CAS Superconducting Research Project (Grant No. SCZX-0101), the Guangdong Provincial Key Laboratory of Magnetoelectric Physics and Devices (Grant No. 2022B1212010008), Research Center for Magnetoelectric Physics of Guangdong Province (Grant No. 2024B0303390001), and the Fundamental Research Funds for the Central Universities, Sun Yat-sen University (Grant No. 74130-31610055). We thank the staff members of the General Purpose Powder Diffractometer (31113.02.CSNS.GPPD) at the China Spallation Neutron Source (CSNS), for providing technical support and assistance in data collection and analysis.

Competing interests

The authors declare that they have no conflict of interest.

Additional information

Supplementary information available.

Tables

Figures

References

  1. [1]J.-G. Park, Journal of Physics: Condensed Matter 28, 301001 (2016).
  2. [2]K. S. Burch, D. Mandrus, and J.-G. Park, Nature 563, 47 (2018).
  3. [3]M. Gibertini, M. Koperski, A. F. Morpurgo, and K. S. Novoselov, Nature Nanotechnology 14, 408 (2019).
  4. [4]C. Gong and X. Zhang, Science 363, eaav4450 (2019).
  5. [5]M.-C. Wang, C.-C. Huang, C.-H. Cheung, C.-Y. Chen, S. G. Tan, T.-W. Huang, Y. Zhao, Y. Zhao, G. Wu, Y.-P. Feng, et al., Annalen der Physik 532, 1900452 (2020).
  6. [6]J.-G. Park, K.-X. Zhang, H. Cheong, J. H. Kim, C. A. Belvin, D. Hsieh, H. Ning, and N. Gedik, Rev. Mod. Phys. 98, 025003 (2026).
  7. [7]Y. Cao, V. Fatemi, S. Fang, K. Watanabe, T. Taniguchi, E. Kaxiras, and P. Jarillo-Herrero, Nature 556, 43 (2018).
  8. [8]H. Park, J. Cai, E. Anderson, Y. Zhang, J. Zhu, X. Liu, C. Wang, W. Holtzmann, C. Hu, Z. Liu, et al., Nature 622, 74 (2023).
  9. [9]J.-U. Lee, S. Lee, J. H. Ryoo, S. Kang, T. Y. Kim, P. Kim, C.-H. Park, J.-G. Park, and H. Cheong, Nano Letters 16, 7433 (2016).
  10. [10]B. Huang, G. Clark, E. Navarro-Moratalla, D. R. Klein, R. Cheng, K. L. Seyler, D. Zhong, E. Schmidgall, and X. Xu, Nature 546, 270 (2017).
  11. [11]C. Gong, L. Li, Z. Li, H. Ji, A. Stern, Y. Xia, T. Cao, W. Bao, C. Wang, Y. Wang, et al., Nature 546, 265 (2017).
  12. [12]X. Li, A. C. Jones, J. Choi, H. Zhao, V. Chandrasekaran, M. T. Pettes, A. Piryatinski, M. A. Tschudin, P. Reiser, D. A. Broadway, P. Maletinsky, N. Sinitsyn, S. A. Crooker, and H. Htoon, Nature Materials 22, 1311 (2023).
  13. [13]S. Lee, Y. K. Kim, J. Noh, B. C. Jang, and S. Lee, ACS Nano 19, 29028 (2025).
  14. [14]J. Xiong, J. Xie, B. Cheng, Y. Dai, X. Cui, L. Wang, Z. Liu, J. Zhou, N. Wang, X. Xu, et al., Nat. Commun. 15, 4953 (2024).
  15. [15]A. F. May, D. Ovchinnikov, Q. Zheng, R. Hermann, S. Calder, B. Huang, Z. Fei, Y. Liu, X. Xu, and M. A. McGuire, ACS Nano 13, 4436 (2019).
  16. [16]H. Zhang, R. Chen, K. Zhai, X. Chen, L. Caretta, X. Huang, R. V. Chopdekar, J. Cao, J. Sun, J. Yao, et al., Phys. Rev. B 102, 064417 (2020).
  17. [17]X. Chen, Y.-T. Shao, R. Chen, S. Susarla, T. Hogan, Y. He, H. Zhang, S. Wang, J. Yao, P. Ercius, et al., Phys. Rev. Lett. 128, 217203 (2022).
  18. [18]A. F. May, M.-H. Du, V. R. Cooper, and M. A. McGuire, Phys. Rev. Mater. 4, 074008 (2020).
  19. [19]C. Tian, F. Pan, S. Xu, K. Ai, T. Xia, and P. Cheng, Applied Physics Letters 116, 10.1063/5.0006337 (2020).
  20. [20]H. Zhang, D. Raftrey, Y.-T. Chan, Y.-T. Shao, R. Chen, X. Chen, X. Huang, J. T. Reichenadter, K. Dong, S. Susarla, et al., Science advances 8, eabm7103 (2022).
  21. [21]G. Zhang, F. Guo, H. Wu, X. Wen, L. Yang, W. Jin, W. Zhang, and H. Chang, Nat. Commun. 13, 5067 (2022).
  22. [22]H. Zhang, Y.-T. Shao, X. Chen, B. Zhang, T. Wang, F. Meng, K. Xu, P. Meisenheimer, X. Chen, X. Huang, et al., Nat. Commun. 15, 3828 (2024).
  23. [23]X. Chen, E. Schierle, Y. He, M. Vranas, J. W. Freeland, J. L. McChesney, R. Ramesh, R. J. Birgeneau, and A. Frano, Phys. Rev. Mater. 6, 094404 (2022).
  24. [24]H. Kageyama, K. Hayashi, K. Maeda, J. P. Attfield, Z. Hiroi, J. M. Rondinelli, and K. R. Poeppelmeier, Nat. Commun. 9, 772 (2018).
  25. [25]M. Ai-Mamouri, P. Edwards, C. Greaves, and M. Slaski, Nature 369, 382 (1994).
  26. [26]Z. Hiroi, N. Kobayashi, and M. Takano, Nature 371, 139 (1994).
  27. [27]A. A. Tsirlin and H. Rosner, Phys. Rev. B 79, 214416 (2009).
  28. [28]C. S. Knee and M. T. Weller, Journal of Materials Chemistry 11, 2350 (2001).
  29. [29]C. S. Knee, M. A. Field, and M. T. Weller, Solid State Sciences 6, 443 (2004).
  30. [30]A. F. May, G. Yumnam, R. P. Hermann, S. Calder, B. M. Lefler, S. J. May, Z. E. Brubaker, M. Brahlek, X. Xu, and D. Ovchinnikov, Phys. Rev. Mater. 9, 034002 (2025).
  31. [31]J. F. Ackerman, Journal of Solid State Chemistry 92, 496 (1991).
  32. [32]Y. Tsujimoto, K. Yamaura, N. Hayashi, K. Kodama, N. Igawa, Y. Matsushita, Y. Katsuya, Y. Shirako, M. Akaogi, and E. Takayama-Muromachi, Chemistry of Materials 23, 3652 (2011).
  33. [33]Y. Tsujimoto, C. I. Sathish, K.-P. Hong, K. Oka, M. Azuma, Y. Guo, Y. Matsushita, K. Yamaura, and E. Takayama-Muromachi, Inorganic Chemistry 51, 4802 (2012).
  34. [34]Y. Tsujimoto, J. Sugiyama, M. Ochi, K. Kuroki, P. Manuel, D. D. Khalyavin, I. Umegaki, M. Månsson, D. Andreica, and S. Hara, Phys. Rev. Mater. 6, 114404 (2022).
  35. [35]C. S. Knee, D. J. Price, M. R. Lees, and M. T. Weller, Phys. Rev. B 68, 174407 (2003).
  36. [36]Y. Tsujimoto, K. Yamaura, and T. Uchikoshi, Inorganic Chemistry 52, 10211 (2013).
  37. [37]Y. Tsujimoto, Y. Matsushita, N. Hayashi, K. Yamaura, and T. Uchikoshi, Crystal Growth & Design 14, 4278 (2014).
  38. [38]J. Tauc, R. Grigorovici, and A. Vancu, Phy. Stat. sol. (b) 15, 627 (1966).
  39. [39]H. Zhong, F. Pan, S. Yue, C. Qin, V. Hadjiev, F. Tian, X. Liu, F. Lin, Z. Wang, and J. Bao, The Journal of Physical Chemistry Letters 14, 6702 (2023).
  40. [40]P. Makuła, M. Pacia, and W. Macyk, The Journal of Physical Chemistry Letters 9, 6814 (2018).
  41. [41]D. Souri and Z. E. Tahan, Applied Physics B 119, 273 (2015).
  42. [42]A. Kirsch, M. M. Murshed, M. Schowalter, A. Rosenauer, and T. M. Gesing, The Journal of Physical Chemistry C 120, 18831 (2016).
  43. [43]D. Peets, J.-H. Kim, P. Dosanjh, M. Reehuis, A. Maljuk, N. Aliouane, C. Ulrich, and B. Keimer, Phys. Rev. B 87, 214410 (2013).
  44. [44]O. Laporte and W. F. Meggers, Journal of the Optical Society of America 11, 459 (1925).
  45. [45]K. Kuzushita, S. Morimoto, S. Nasu, and S. Nakamura, Journal of the Physical Society of Japan 69, 2767 (2000).
  46. [46]J.-H. Kim, A. Jain, M. Reehuis, G. Khaliullin, D. Peets, C. Ulrich, J. Park, E. Faulhaber, A. Hoser, H. Walker, et al., Phys. Rev. Lett. 113, 147206 (2014).
  47. [47]C. A. Hancock, T. Herranz, J. F. Marco, F. J. Berry, and P. R. Slater, Journal of Solid State Chemistry 186, 195 (2012).
  48. [48]H. Kageyama, T. Watanabe, Y. Tsujimoto, A. Kitada, Y. Sumida, K. Kanamori, K. Yoshimura, N. Hayashi, S. Muranaka, and M. Takano, Angewandte Chemie 120, 5824 (2008).
  49. [49]J. Rodríguez-Carvajal, Physica B: Condensed Matter 192, 55 (1993).
  50. [50]A. Wills, Physica B: Condensed Matter 276, 680 (2000).
  51. [51]G. Kresse and J. Hafner, Phys. Rev. B 47, 558 (1993).
  52. [52]G. Kresse and J. Furthmüller, Phys. Rev. B 54, 11169 (1996).
  53. [53]J. P. Perdew, K. Burke, and M. Ernzerhof, Phys. Rev. Lett. 77, 3865 (1996).
  54. [54]S. L. Dudarev, G. A. Botton, S. Y. Savrasov, C. J. Humphreys, and A. P. Sutton, Phys. Rev. B 57, 1505 (1998).
  55. [55]S. Grimme, S. Ehrlich, and L. Goerigk, Journal of Computational Chemistry 32, 1456 (2011).
  56. [56]H. J. Monkhorst and J. D. Pack, Phys. Rev. B 13, 5188 (1976).

Paper details

vlnc:W_r47xhvb4
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 2

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents