Effect of Gd and Co content on electrochemical and electronic properties of La1.5_{1.5}Mg0.5_{0.5}Ni7_7 alloys: a combined experimental and first-principles study

Abstract

In this work, we investigate the effect of Gd and Co substitutions on the electrochemical and electronic properties of La1.5_{1.5}Mg0.5_{0.5}Ni7_7 alloy. Two series of La1.5−x_{1.5-x}Gdx_xMg0.5_{0.5}Ni7_7 (xx = 0.0, 0.25, 1.0) and La1.5_{1.5}Mg0.5_{0.5}Ni7−y_{7-y}Coy_y (yy = 0.0, 0.5, 1.5) alloys are produced using mechanical alloying technique. The X-ray diffraction indicates multiphase character of the samples, with the majority of hexagonal Ce2_2Ni7_7-type and rhombohedral Gd2_2Co7_7-type structures of (La,Mg)2_2Ni7_7 phase. Partial substitutions of La by Gd or Ni by Co in La1.5_{1.5}Mg0.5_{0.5}Ni7_7 phase result in increase of cycle stability of the metal hydride (MHx_x) electrodes. All considered alloys reach the maximum discharge capacity after three charging-discharging cycles. Two optimal compositions, in respect of electrochemical properties, are subsequently investigated by the X-ray photoelectron spectroscopy (XPS). The experimental analysis of the valence band is further extended by the density functional theory (DFT) calculations. We also discuss the effects of alloying and site preference of dopants on the position of the van Hove-type singularity, as observed in the electronic densities of states (DOS) in proximity of the Fermi level.

Introduction

The next generation of electrode materials for nickel-metal hydride (Ni-MHx_x) batteries are the (La,Mg)2_2Ni7_7-type hydrogen storage alloys [1, 2, 3, 4]. It has been found that the limited cycle stability of the AB2_2-type and AB5_5-type materials could be compensated in the A2_2B7_7-type alloys [4]. It has been shown that substitution of La with other rare-earth element [4, 5, 6, 7, 8, 9] and Ni with alternative 3d element [10, 11, 12] also modifies the electrochemical performance of the A2_2B7_7 materials. However, a cycling stability and high-rate discharge capacity, especially for high discharging rates and material and processing costs, still need improvements to satisfy increasing demands of the market [13, 14].

The most common phases of the multi-phase La-Mg-Ni-based alloys are (La,Mg)Ni3_3, (La,Mg)2_2Ni7_7 and (La,Mg)5_5Ni19_{19} [15, 16]. They are all composed of [A2_2B4_4] and [AB5_5] subunits stacked alternatively along the cc axis and forming superlattice structures [17]. Studies on the electrochemical performance of the A2_2B7_7-type single-phase La1.5_{1.5}Mg0.5_{0.5}Ni7_7 alloy have revealed that both the (La,Mg)5_5Ni19_{19} and the LaNi5_5 phases have catalytic effects on the fast discharge of the alloy [7]. A partial replacement of La by the rare earth (RE) atoms and Ni by Co or Al can affect the crystal structure of the A2_2B7_7 alloys. Nd and Co doped alloys can be applied as negative electrodes in Ni-MHx_x batteries, which are characterized by improved cyclic durability [8, 18]. By adjusting the RE concentration in the (RE-Mg)2_2Ni7_7 alloys it is possible to enhance the electrochemical hydrogen storage properties of the alloy electrodes. For La0.8_{0.8}Gdx_xMg0.2_{0.2}Ni3.15_{3.15}Co0.25_{0.25}Al0.1_{0.1} alloys (xx from 0.0 to 0.4) it has been shown that Gd substitution significantly affects the phase composition of the alloys [16]. Additionally, the partial substitution of Ni by Co atoms in the A2_2B7_7 alloy have also resulted in improving the electrochemical discharge capacity [19]. An addition of Co atoms to AB5_5 alloys reduces its volume expansion caused by hydriding, which in turn reduces the pulverization and corrosion of the alloys [20, 21]. Lately, it has been shown that the Pr, Nd and Co-free A2_2B7_7-type, La13.9_{13.9}Sm24.7_{24.7}Mg1.5_{1.5}Ni58_{58}Al1.7_{1.7}Zr0.14_{0.14}Ag0.07_{0.07} alloy exhibits excellent hydrogen-storage and electrochemical performance. The high rate discharge abilities were 97%, 86% and 78% at discharge current densities of 330, 970 and 1600 mAh/g, respectively [22]. The improvement of hydrogenation properties of the (La,Mg)2_2Ni7_7 system may be achieved by encapsulation of material particles with thin amorphous nickel coating [23]. The magnetron sputtering of La1.5_{1.5}Mg0.5_{0.5}Ni7_7 particles with 0.29 μ\mum thick Ni film appeared to have been efficient enough to inhibit corrosion degradation.

Recently, also the effect of Mg substitution on the electrochemical and electronic properties of La2−x_{2-x}Mgx_xNi7_7 materials has been investigated [24, 25]. The X-ray diffraction measurements have indicated a multiphase character of the samples with majority of (La,Mg)2_2Ni7_7 phases in hexagonal Ce2_2Ni7_7-type and rhombohedral Gd2_2Co7_7-type structures. Electrochemical measurements have shown that the maximum discharge capacity (Cmax⁡C_{\max}) increases with Mg concentration and reaches the highest value for the Mg concentration xx equal to 0.5. Furthermore, the valence band of the nanocrystalline La1.5_{1.5}Mg0.5_{0.5}Ni7_7 sample has been investigated by X-ray photoelectron spectroscopy (XPS) and from density functional theory (DFT) [25]. The valence band of isostructural hexagonal La2_2Co7_7 compound has been investigated already by DFT [26]. A systematic DFT study of every ordered configuration of (La,Mg)2_2Ni7_7 and several other La-Mg-Ni systems has been presented by Crivello et al. [27]. The authors have concluded that the stability of the (La,Mg)2_2Ni7_7 system decreases with Mg substitution. Crivello et al. have also presented a DFT study on the distribution of hydrogen in the La2_2Ni7_7, Mg2_2Ni7_7 and La1.5_{1.5}Mg0.5_{0.5}Ni7_7 hosts [28].

An effective method of synthesis of the hydrogen storage materials with reduced crystallite sizes is mechanical alloying (MA) [29]. Recent studies suggest that MA technique can improve the kinetics of hydrogen absorption and desorption of the synthesized alloys. This change comes from the large specific surface areas and from short hydrogen diffusion distances in the MA samples [15]. In this work we apply the MA technique with subsequent annealing in the argon atmosphere to produce the La1.5−x_{1.5-x}Gdx_xMg0.5_{0.5}Ni7_7 (xx = 0.0, 0.25, 1.0) and La1.5_{1.5}Mg0.5_{0.5}Ni7−y_{7-y}Coy_y (yy = 0.0, 0.5, 1.5) alloys. Subsequently, we investigate the influence of the substitutions on electrochemical and electronic properties of (La,Mg)2_2Ni7_7-type materials. With X-ray photoelectron spectroscopy and DFT calculations we study the valence band of the selected optimal compositions. In our theoretical analysis we put special emphasis on narrow energy region in the vicinity of the Fermi level.

Experimental and computational details

This section covers details of preparation of La1.5−x_{1.5-x}Gdx_xMg0.5_{0.5}Ni7_7 and La1.5_{1.5}Mg0.5_{0.5}Ni7−y_{7-y}Coy_y samples, the basic informations on the applied characterization techniques: X-ray diffraction (XRD), X-ray photoelectron spectroscopy (XPS) and electrochemical measurements and the computational parameters for the density functional theory (DFT) calculations.

Materials preparation

La and Gd powders – grated from rods (Alfa Aesar, 99.9%), Mg powder (Alfa Aesar, 45 μ\mum, 99.8%), Co powder (Aldrich, 1.6 μ\mum, 99.8%) and Ni powder (Aldrich, 5 μ\mum, 99.99%) were used to synthesized the La1.5−x_{1.5-x}Gdx_xMg0.5_{0.5}Ni7_7 (xx = 0.0, 0.25, 1.0) and La1.5_{1.5}Mg0.5_{0.5}Ni7−y_{7-y}Coy_y (yy = 0.0, 0.5, 1.5) alloy powders. The considered compositions were prepared by 48 h of mechanical alloying in the argon atmosphere and by subsequent annealing. The ratio of the weight of hard steel balls to the weight of powder was 4.2:1. Gd substituted alloys were annealed at 1123 K and Co substituted alloys at 973 K for 0.5 h in high purity argon atmosphere.

Structural characterization and electrochemical measurements

The crystallographic structure of samples was studied at room temperature using Panalytical Empyrean XRD with CuKα1_{\alpha1} (λ\lambda = 1.54056 Å) radiation. A scanning electron microscope (SEM, VEGA 5135 Tescan) with energy dispersive spectrometer (EDS, PTG Prision Avalon) was used to characterize the chemical compositions of the obtained powdered materials.

The electrochemical studies were performed at room temperature in a tri-electrode open cell. Electrodes were produced by cold pressing of a mixture of 0.4 g alloy with 0.04 g carbonyl nickel powders into a pellet of 8 mm diameter. The counter and reference electrodes were Ni(OH)2_2/NiOOH and Hg/HgO, respectively. As electrolyte was used 6 M KOH. Tested electrodes were charged and discharged at a current of 40 mA g−1^{-1}. A cut-off voltage was -0.7 V versus a Hg/HgO reference electrode. An extended description of the electrochemical studies has been presented in our previous work [24]. The cycle stability of the materials was evaluated by the capacity retaining rate after the nthn^{\mathrm{th}} cycle: (Cn/Cmax⁡C_n/C_{\max}) × 100%, where CnC_n is discharge capacity at nnth cycle and Cmax⁡C_{\max} is discharge capacity maximum.

XPS measurements

The XPS spectra measurements were performed at room temperature using the SPECS EA 10 PLUS energy spectrometer with Al-Kα_{\alpha} radiation of 1486.6 eV. The step size in the XPS valence band measurements was set to 0.05 eV. The energy spectra were analyzed with a hemispherical analyzer with full width at half maximum FWHMMg−Kα_{\mathrm{Mg-K}_{\alpha}} equal to 0.8 eV for Ag 3d5/2d_{5/2}. The calibration was performed based on the procedure given by Baer et al. [30]. The Au 4f7/2f_{7/2} peak was positioned at 84.0 eV and the Fermi level at 0 eV. The SPECS ion gun etching system was used to remove the surface layers (∼\sim 10 nm) of the studied bulk nanocrystalline samples. Etching was performed with a beam of Ar+^+ ions of energy 3 keV and inclined to the sample surface at 45°. The measurements have been preceded by the backing procedures of the analysis chamber (TT = 440 K) which made it possible to achieve a base vacuum of 4×10−114 \times10^{-11} mbar. More details of the XPS measurements can be found in our previous work [31].

Density functional theory calculations

We performed three sets of calculations with different approaches to model chemical disorder. The electronic band structure calculations of La2_2Ni7_7, La1.5_{1.5}Mg0.5_{0.5}Ni7_7, La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 and La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} compositions were carried out by using the full-potential local-orbital minimum-basis scheme (FPLO18.00-52) [32]. These calculations were performed in the scalar relativistic approach within the generalized gradient approximation (GGA) of the exchange-correlation potential in the form of Perdew-Burke-Ernzerhof (PBE) [33]. We used 20×20×520 \times20 \times5 kk-mesh and energy convergence criterion 10−810^{-8} Ha (2.72×10−72.72 \times10^{-7} eV). To simulate the chemical disorder we used primarily the so-called ordered compound method. We started with a model of La2_2Ni7_7 unit cell composed of four formula units (La8_8Ni28_{28}). In order to prepare the compositions corresponding to the experimental ones, within a single unit cell we substituted La by Mg, La by Gd, and Ni by Co atoms. Figure 1 presents the considered models as, visualized using the VESTA computer code [34]. For simplicity, we considered only the hexagonal Ce2_2Ni7_7-type structure and neglected the rhombohedral Gd2_2Co7_7-type structure. The crystallographic parameters of La2_2Ni7_7 in Ce2_2Ni7_7-type structure used for calculations are collected in Table 1. For the ordered compound models with Mg, Gd and Co we used the appropriate lattice parameters from our measurements, see Table 2. Although the hexagonal La2_2Ni7_7 phase undergoes the antiferromagnetic transition at TN=51T_\mathrm{N} = 51 K [36], we considered only non-magnetic models as consistent with a magnetic state of the samples in room temperature. However, based on our experience with modeling of Gd alloying [37], we made

Crystal structures of La2Ni7, La1.5Mg0.5Ni7, La1.25Gd0.25Mg0.5Ni7 and La1.5Mg0.5Ni6.5Co0.5

Figure 1. The crystal structures of (a) La2_2Ni7_7; (b) La1.5_{1.5}Mg0.5_{0.5}Ni7_7; (c) La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 and (d) La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5}. All ordered compound models are considered in Ce2_2Ni7_7-type structure. The different elements are denoted by different colors as follows: La – yellow, Ni – blue, Mg -red, Gd – black and Co – green.

atomsitexxyyzz
La1_14f4f1/31/32/32/30.03013
La2_24f4f1/31/32/32/30.17422
Ni1_12a2a000
Ni2_24e4e000.16898
Ni3_34f4f1/31/32/32/30.83616
Ni4_46h6h0.83410.66821/41/4
Ni5_512k12k0.83500.67000.08806

Table 1. Crystallographic parameters of La2_2Ni7_7 in Ce2_2Ni7_7-type structure reproduced after Levin et al. [35]. Lattice parameters a=5.0577a = 5.0577, c=24.7336c = 24.7336 Å, space group P63/mmcP6_3/mmc.

CompositionLattice parameters aa (Å)Lattice parameters cc (Å)Phase abundance (wt%) A2_2B7_7Phase abundance (wt%) AB5_5Phase abundance (wt%) La2_2O3_3CthC_{\mathrm{th}} (mAh/g)CmaxC_{\mathrm{max}} (mAh/g)C30C_{30} (mAh/g)C50C_{50} (mAh/g)C50/CmaxC_{50}/C_{\mathrm{max}} (%)
La1.5_{1.5}Mg0.5_{0.5}Ni7_75.0424.2088.98.03.153530420416755
La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_75.0124.1491.66.42.053130321819564
La0.5_{0.5}Gd1.0_{1.0}Mg0.5_{0.5}Ni7_74.9724.0770.929.10.052068656596
La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5}5.0524.1596.80.82.453329923821371
La1.5_{1.5}Mg0.5_{0.5}Ni5.5_{5.5}Co1.5_{1.5}5.0424.2095.80.93.352930723619965

Table 2. Lattice parameters of A2_2B7_7 phase, phase abundance, theoretical capacity (CthC_{\mathrm{th}}), maximum discharge capacity (CmaxC_{\mathrm{max}}), discharge capacity at 30 and 50 cycles (C30C_{30}, C50C_{50}) and C50/CmaxC_{50}/C_{\mathrm{max}} ratio for the considered alloys.

an exception for La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 system and simulated it as spin polarized.

The second method we used to simulate alloying was the virtual crystal approximation (VCA) [38]. The idea behind the VCA is to simulate a random homogeneous on-site occupation of two atom types by a single (virtual) atom with an averaged atomic number. The application of the VCA is, however, limited to the pairs of elements which atomic number differs by one. In the considered case of La1.5_{1.5}Mg0.5_{0.5}Ni7−y_{7-y}Cuy_y, in which the Cu/Ni alloying is described by the VCA, the atomic number of virtual Cu/Ni atom equals ZVCA=(1−y)ZNi+yZCuZ_{\mathrm{VCA}} = (1-y)Z_{\mathrm{Ni}} + yZ_{\mathrm{Cu}}.

Third and last method used to model chemical disorder was the coherent potential approximation (CPA) [39]. The CPA calculations, performed with the FPLO5.00 code [40, 41], were intended to find the site preference of Co dopants in the example phase of La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} (Gd2_2Co7_7-type). In contrast to the other presented results, the CPA calculations are performed with the Perdew and Wang form of the exchange-correlation potential [42] and 6×6×66 \times6 \times6 kk-mesh (limited by the complexity of the task).

The theoretical X-ray photoelectron spectra were obtained from the calculated densities of electronic states (DOS) convoluted by Gaussian with a half-width δ\delta and scaled using the proper atomic subshell photoionization cross-sections [31, 43, 44]. The purpose of the Gaussian convolution was to mimic an experimental resolution, a lifetime of the hole states and the thermal effects. The value of δ\delta equal to 0.50.5 eV was selected to be close to the instrumental value of spectrometer used to take the measurements.

Results and discussion

In this section we present the results and discussion of structural and electrochemical measurements, XPS valence band characterization and first-principles calculations.

Crystallographic structure and phase composition

The La1.5−x_{1.5-x}Gdx_xMg0.5_{0.5}Ni7_7 (x=0.0x = 0.0, 0.25, 1.0) and La1.5_{1.5}Mg0.5_{0.5}Ni7−y_{7-y}Cuy_y (y=0.0y = 0.0, 0.5, 1.5) alloys are produced by the MA and annealing process. Figure 2 (a)– (c) present the XRD spectra of the La1.5−x_{1.5-x}Gdx_xMg0.5_{0.5}Ni7_7 (x=0.0x = 0.0, 0.25, 1.0) alloys after 48 h of MA and additional heat treatment at 1123 K for 0.5 h in the argon atmosphere. The XRD measurements reveal a multiphase character of the considered alloys. The mass fractions of the phases in the La1.5−x_{1.5-x}Gdx_xMg0.5_{0.5}Ni7_7 and La1.5_{1.5}Mg0.5_{0.5}Ni7−x_{7-x}Cox_x MA and annealed alloys were established by the Rietveld refinement of the XRD data in a 2θ2\theta range of 20°–80°, see Table 2. The alloys are composed of the La2_2Ni7_7-type phase (Ce2_2Ni7_7-type hexagonal structure (space group P63/mmcP6_3/mmc) and the Gd2_2Co7_7-type rhombohedral structure (s.g. R3mR3m)), the CaCu5_5-type phase (s.g. P6/mmmP6/mmm) and the La2_2O3_3 phase (s.g. Pˉ3m1\bar{P}3m1). The content of the A2_2B7_7-type phase is the highest for x=0.25x = 0.25 and equal to 91.6 wt%. It decreases to 70.9 wt% for x=1.0x = 1.0 and further decreases to 60.0 wt% for x=1.5x = 1.5, see Table 2 and Ref. [45]. It has been shown that the La-Mg-Ni based alloys produced by inductive melting or arc melting have similar phase compositions [46, 47].

The X-ray diffraction patterns of alloys obtained by 48 h of mechanical alloying process and subsequent heat treatment

Figure 2. The X-ray diffraction patterns of alloys obtained by 48 h of mechanical alloying process and subsequent heat treatment. (a) La1.5_{1.5}Mg0.5_{0.5}Ni7_7, (b) La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7, (c) La0.5_{0.5}Gd1.0_{1.0}Mg0.5_{0.5}Ni7_7, (d) La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} and (e) La1.5_{1.5}Mg0.5_{0.5}Ni5.5_{5.5}Co1.5_{1.5}.

Figures 2 (d) and (e) show the XRD patterns of La1.5_{1.5}Mg0.5_{0.5}Ni7−y_{7-y}Coy_y alloys (y=0.5y = 0.5, 1.5) after 48 h of MA and additional heat treatment at 973 K for 0.5 h in argon atmosphere. All of the synthesized alloys are composed of the main La2_2Ni7_7 phase (Ce2_2Ni7_7-type hexagonal structure (s.g. P63/mmcP6_3/mmc) and the Gd2_2Co7_7-type rhombohedral structure (s.g. R3mR3m)) and a minor CaCu5_5-type phase (s.g. P6/mmmP6/mmm). Moreover, a small content of La2_2O3_3 phase is observed, see Table 2. The abundance of the A2_2B7_7-type phase increases from 88.9 wt% for La1.5_{1.5}Mg0.5_{0.5}Ni7_7 alloy to 96.8 wt% for La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5}. The substitution of Co for Ni efficiently prevents the formation of the LaNi5_5-type phase. Previously, a similar tendency has been observed for other Co-substituted La2_2Ni7_7-type alloys [19, 20, 21, 48]. However, it has been shown that a coexistence of the La2_2Ni7_7 phase with the LaNi5_5 phase increases the electrode stability [49].

Electrochemical measurements

The results of electrochemical measurements of the La1.5−x_{1.5-x}Gdx_xMg0.5_{0.5}Ni7_7 (x=0.0x = 0.0, 0.25, 1.0) and La1.5_{1.5}Mg0.5_{0.5}Ni7−y_{7-y}Coy_y (y=0.0y = 0.0, 0.5, 1.5) alloys are summarized in Figure 3 and Figure 4 and Table 2. All the considered electrodes display the maximum capacity (CmaxC_{\mathrm{max}}) at the 3rd cycle. The highest observed values of discharging capacity (CmaxC_{\mathrm{max}}) are 307 mAh/g for La1.5_{1.5}Mg0.5_{0.5}Ni5.5_{5.5}Co1.5_{1.5} and 303 mAh/g for La1.25Gd0.25Mg0.5Ni7\mathrm{La}_{1.25}\mathrm{Gd}_{0.25}\mathrm{Mg}_{0.5}\mathrm{Ni}_{7} alloy. Previously, for La1.5Mg0.5Ni7−xCox\mathrm{La}_{1.5}\mathrm{Mg}_{0.5}\mathrm{Ni}_{7-x}\mathrm{Co}_{x} alloy electrodes (xx ranging from 0 to 1.8) the much higher discharge capacities have been measured, in a range from 390 to 406 mAh/g [50]. For the considered A2B7\mathrm{A}_{2}\mathrm{B}_{7}-type alloys we evaluate a theoretical capacity (CthC_{\mathrm{th}}) in the same way as it has been done previously for LaNi5\mathrm{LaNi}_{5} [51]. For La2Ni7\mathrm{La}_{2}\mathrm{Ni}_{7} we use the maximum hydrogen capacity 1.4 H/M (hydrogen-to-metal atom ratio) as measured by Iwase et al. [52]. 1.4 H/M leads to a number of hydrogen atoms per formula unit equal to 12.6 (La2Ni7H12.6\mathrm{La}_{2}\mathrm{Ni}_{7}\mathrm{H}_{12.6}). The same maximum hydrogen capacity we assume for other considered A2B7\mathrm{A}_{2}\mathrm{B}_{7}-type alloys. An obtained theoretical capacity for pristine La2Ni7\mathrm{La}_{2}\mathrm{Ni}_{7} is equal to 490 mAh/g and for all considered compositions with Mg, Gd, and Co the CthC_{\mathrm{th}} is of about 530 mAh/g, see Table 2. The measured discharge capacity of all studied electrodes is degrading during the charge-discharge cycles. The mechanisms behind the degradation are: (a) partial oxidation of the electrode, (b) formation of stable hydride phases, (c) formation of the hydroxides surface layers (Mg(OH)2\mathrm{Mg(OH)}_{2} and La(OH)3\mathrm{La(OH)}_{3}) hindering the diffusion of hydrogen into/or from the alloy, (d) expansion and contraction of the unit cell volumes during the hydrogenation and dehydrogenation processes leading to a pulverization of the alloy particles [53, 54].

Discharge capacities of the alloys as a function of cycle number

Figure 3. Discharge capacities of the alloys as a function of cycle number for (a) La1.5Mg0.5Ni7\mathrm{La}_{1.5}\mathrm{Mg}_{0.5}\mathrm{Ni}_{7}, (b) La1.25Gd0.25Mg0.5Ni7\mathrm{La}_{1.25}\mathrm{Gd}_{0.25}\mathrm{Mg}_{0.5}\mathrm{Ni}_{7}, (c) La0.5Gd1.0Mg0.5Ni7\mathrm{La}_{0.5}\mathrm{Gd}_{1.0}\mathrm{Mg}_{0.5}\mathrm{Ni}_{7}, (d) La1.5Mg0.5Ni6.5Co0.5\mathrm{La}_{1.5}\mathrm{Mg}_{0.5}\mathrm{Ni}_{6.5}\mathrm{Co}_{0.5} and (e) La1.5Mg0.5Ni5.5Co1.5\mathrm{La}_{1.5}\mathrm{Mg}_{0.5}\mathrm{Ni}_{5.5}\mathrm{Co}_{1.5}.

Cyclic stability of electrodes

Figure 4. Cyclic stability of electrodes prepared with: (a) La1.5Mg0.5Ni7\mathrm{La}_{1.5}\mathrm{Mg}_{0.5}\mathrm{Ni}_{7}, (b) La1.25Gd0.25Mg0.5Ni7\mathrm{La}_{1.25}\mathrm{Gd}_{0.25}\mathrm{Mg}_{0.5}\mathrm{Ni}_{7}, (c) La0.5Gd1.0Mg0.5Ni7\mathrm{La}_{0.5}\mathrm{Gd}_{1.0}\mathrm{Mg}_{0.5}\mathrm{Ni}_{7}, (d) La1.5Mg0.5Ni6.5Co0.5\mathrm{La}_{1.5}\mathrm{Mg}_{0.5}\mathrm{Ni}_{6.5}\mathrm{Co}_{0.5} and (e) La1.5Mg0.5Ni5.5Co1.5\mathrm{La}_{1.5}\mathrm{Mg}_{0.5}\mathrm{Ni}_{5.5}\mathrm{Co}_{1.5}.

It is well known that the cycle stability of the alloy is positively correlated with the capacity retention rate. It is observed that this rate of the Gd free alloys is markedly lower than that of the alloy containing Gd or Co. For example, after 50 cycles, the capacity retaining rate (R50R_{50})

of the MA and annealed La1.5−xGdxMg0.5Ni7\mathrm{La}_{1.5-x}\mathrm{Gd}_{x}\mathrm{Mg}_{0.5}\mathrm{Ni}_{7} alloys increase from 55%, to 64% and 95% for xx = 0, 0.25 and 0.5, respectively. In the case of the MA and annealed La1.5Mg0.5Ni7−yCoy\mathrm{La}_{1.5}\mathrm{Mg}_{0.5}\mathrm{Ni}_{7-y}\mathrm{Co}_{y} alloys the R50R_{50} changes from 55%, to 71% and 65% for yy = 0, 0.5 and 1.5, respectively. Phase composition is one of the most significant factors influencing the electrochemical performance of La-Mg-Ni-based alloys. For example, a high-Sm, Pr/Nd-free, and low-Co La0.95Sm0.66Mg0.40Ni6.25La0.42Co0.32\mathrm{La}_{0.95}\mathrm{Sm}_{0.66}\mathrm{Mg}_{0.40}\mathrm{Ni}_{6.25}\mathrm{La}_{0.42}\mathrm{Co}_{0.32} alloy is reported as an A2B7\mathrm{A}_{2}\mathrm{B}_{7}-type electrode for Ni-MHx_x batteries [13]. This induction melted alloy is composed of La2Ni7\mathrm{La}_{2}\mathrm{Ni}_{7} (96.3%) and LaNi5\mathrm{LaNi}_{5} (3.7%) phases, and shows high discharge capacity and excellent cyclic properties. The discharge capacity can reach 311.8 mAh/g and 227.0 mAh/g at large discharge currents of 2C and 5C, respectively, and 80% of the capacity is retained after 239 cycles at 1C. The effects of plasma milling (PM) and graphene addition in La11.3Mg6.0Sm7.4Ni61.0Co7.2Al7.1\mathrm{La}_{11.3}\mathrm{Mg}_{6.0}\mathrm{Sm}_{7.4}\mathrm{Ni}_{61.0}\mathrm{Co}_{7.2}\mathrm{Al}_{7.1} alloy electrodes on the electrochemical properties and kinetics have been studied [55]. XRD analysis showed that the material was composed of Sm2Co7\mathrm{Sm}_{2}\mathrm{Co}_{7}, LaNi5\mathrm{LaNi}_{5} and a small amount of AlSm3\mathrm{AlSm}_{3}. It has been found that the discharge capacity of this composite at high discharge current density is significantly improved after the addition of graphene followed by PM. At a rate of 5C, the discharge capacity of MHx_x electrode after PM for only 10 min has increased from 172.2 mAh/g to 243.9 mAh/g, and has further increased to 263.8 mAh/g after addition of graphene. Moreover, the high-rate dischargeability and the exchange current density of the MHx_x electrodes has increased. The recent progress on the application of dielectric barrier discharge plasma assisted milling in preparation of the energy storage materials has been reviewed by Ouyang et al. [57].

The chemical substitution affects the kinetics of the hydrogen sorption reducing the same the time of the hydrogenation process [45]. Although the concentration and type of the considered substitutions do not affect substantially the maximum discharge capacities of our specimens, the alloying significantly improve the cyclic stability of the samples, see Figure 3 and Figure 4 and Table 2. The best capacity retaining rates after the 50th cycle are obtained for the La0.5_{0.5}Gd1.0_{1.0}Mg0.5_{0.5}Ni7_7 and La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} electrodes.

XPS measurements

The XPS technique provides information on the electronic structure of the valence band. The valence band is affected by chemical composition and microstructure. Furthermore, the valence band contains information about phase composition, local chemical disorder, impurities and local deformations. The bulk nanocrystalline

La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 and La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} samples, identified as having the most promising electrochemical properties among the considered series, are investigated by the X-ray photoelectron spectroscopy (XPS). The bulk nanocrystalline La2_2Ni7_7 sample is considered as the reference one. The measured XPS valence band spectra of the considered alloys are presented in Figure 5. We observe that the full widths at half maxima (FWHM) of the valence bands of La2_2Ni7_7, La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 and La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} are about 2.8 eV, 2.5 eV and 2.8 eV, respectively. In the XPS spectrum of the La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 we identify two main maxima, the

Figure 5. The experimental XPS valence band spectra (Al-Kα) of bulk nanocrystalline La2_2Ni7_7-based alloys: La2_2Ni7_7, La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7, and La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5}. All the intensities were normalized and separated by 0.3 arbitrary units for a better perception.

first one around -0.9 eV and the second one around -1.9 eV. Third much smaller maximum is observed at about -4.1 eV. As the amount of Gd substitution in La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 is relatively low, the overall shape of its spectrum does not change much in respect to the La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} and La2_2Ni7_7 spectra. The spectrum of the La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} is not much different from the reference spectrum of the La2_2Ni7_7 sample. It is almost featureless and exhibits a single maximum at around -1.5 eV. The main contributions to the all measured valence band spectra come from the 3d electrons of Ni [25]. The details of the electronic valence bands will be discussed in the next section based on the results from the first-principles calculations.

According to semi-empirical models of metal hydride formation [58, 59], a justification for maximum hydrogen absorption capacity in metallic matrices has been proposed. These models show that the energy of the metal-hydrogen interaction depends both on geometric and electronic factors. One of the important electronic factor is the full width at half maximum (FWHM) of the valence band of the metallic host material. In our case, the widths determined experimentally and theoretically for the considered samples are comparable, see Figure 5 and Figure 6. Therefore, the maximum discharge capacities (Cmax⁡_{\max}) measured for these samples are practically the same. Furthermore, a small substitution of Ni by Co in La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} practically does not change the FWHM of valence band, but it improves the cycle stability, as shown in Figure 3 and Figure 4.

Figure 6. Calculated XPS spectra of La2_2Ni7_7, La1.5_{1.5}Mg0.5_{0.5}Ni7_7, La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 and La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} phases (all in Ce2_2Ni7_7-type structures). The electronic densities of states are calculated with scalar-relativistic PBE FPLO scheme treating disorder with the ordered compound method. The δ parameter is set to 0.5.

Density functional theory calculations

In this section we continue the investigation of the electronic valence bands of two optimal compositions by using the DFT approach. The details of our calculations are described in the methods section 2.4. Figure 6

shows the calculated spectra for the optimal compositions La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 and La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} to gether with the results for the reference systems La2_2Ni7_7 and La1.5_{1.5}Mg0.5_{0.5}Ni7_7. As the calculated XPS spectra are a combination of the contributions from all the valence band electrons, they can be resolved for types of orbitals, elements and sites. Figure 7 presents the measured and calculated XPS spectra of La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7, together with the calculated contributions from Ni 3d3d and Gd 4f4f states. The valence band of La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 is dominated by the Ni 3d3d share, while the presence of Gd 4f4f states around −4.0-4.0 eV explains the corresponding local maximum in the experimental spectra. The Gd dopants contribute further to valence band with minor 5d5d and 6s6s shares, which are not shown. The total DOSs for the considered compositions are presented in Figure 8. The advantage of the DOS plots over the XPS spectra is the lack of a broadening, which provides a more detailed picture of the electronic structure. The DOSs of the all considered compositions reveal significant similarities. A higher resolution of DOSs in respect to XPS spectra allows us to track changes in electronic structure even for small differences in concentration of Gd or Co dopants. In all DOS plots from Figure 8 we observe two main maxima at about −1-1 eV and −2.5-2.5 eV, which are mainly related to the Ni 3d3d orbitals. Almost all systems, except the one with Co dopants, exhibit a characteristic narrow maximum close to the Fermi level, which can have a significant impact on the electrochemical properties of the considered alloys. Similar peak has been observed for the bcc Ni [25] and for some other Ni based compounds like for example MgCx_xNi3_3 [60] and YNi2_2B2_2X (X = B, C, N, and O) [61]. Sharp narrow peak in DOS is called the

Calculated and experimental XPS spectra of La1.25Gd0.25Mg0.5Ni7

Figure 7. The calculated XPS spectra of La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 phase (in Ce2_2Ni7_7-type structure), together with contributions from Ni 3d3d and Gd 4f4f states. The results are based on the spin-polarized scalar-relativistic PBE FPLO scheme treating chemical disorder with the ordered compound method. The δ\delta parameter is set to 0.5. For comparison, the experimental XPS valence band is presented.

Figure 8. Densities of states (DOS) for (a) La2_2Ni7_7, (b) La1.5_{1.5}Mg0.5_{0.5}Ni7_7, (c) La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 and (d) La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} phases as calculated with scalar-relativistic PBE FPLO scheme treating disorder with the ordered compound method. Results for (c) La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 show contributions from two spin channels (red and blue lines).

van Hove singularity and happens to be located close to the Fermi level. In opposition to the band-type states typical for valence band region, the van Hove singularity can be understood as a fingerprint of an atomic-like state of electrons. The van Hove singularity near the Fermi level observed in our calculation for La2_2Ni7_7 comes from the Ni 3d3d states of most of the inequivalent atomic positions of Ni. Unfortunately, the resolution of our XPS equipment is too low to investigate this narrow peak. For example, similar features in valence bands have been observed previously with BIS technique for CeIr2_2 and CeRu2_2 [62].

We conclude that small changes in the band structure in proximity of the Fermi level may have a significant effect on the electronic properties of the system. The alloying of the system with a specific element which is increasing the occupation of the valence band should result in moving the Fermi level over the van Hove singularity. In case of the considered La1.5_{1.5}Mg0.5_{0.5}Ni7_7 composition, an increasing of the valence band occupation by alloying can be accomplished by substituting, for example, Ni by Cu. The neutral copper atom has one more proton and one more electron than neutral Ni (atomic numbers: ZNi=28Z_{\mathrm{Ni}} = 28 and ZCu=29Z_{\mathrm{Cu}} = 29), thus Cu contributes to the La1.5_{1.5}Mg0.5_{0.5}Ni7_7 system by increasing the occupation of the valence band. Following this simple idea we perform the DFT calculations for alloying of Ni by Cu in the La1.5_{1.5}Mg0.5_{0.5}Ni7−y_{7-y}Cuy_y system, where y=0.0,0.5,1.0,1.5y = 0.0, 0.5, 1.0, 1.5.

Previously, it has been shown that an a ferromagnetism in Y2_2Ni7_7 is due to a peak in DOS near the Fermi level [63]. Fukase et al. , investigating the magnetic properties of La2_2Ni7_7 doped with Co or Cu, found that for more than 3% of Cu in place Ni the metamagnetic behavior disappears and ferromagnetic behavior appears and increase of Cu concentration up to 10% induces a transition to the paramagnetic state [64]. Tazuke et al. have later proposed that, if La2_2Ni7_7 has a similar peak as Y2_2Ni7_7 near the Fermi energy, the magnetic transitions observed along Cu alloying can be understood based on the evolution of electronic structure [65]. Tazuke et al. have suggested that around 3% of Cu concentration in La2_2Ni7_7 the Fermi energy reaches the maximum of the peak, satisfying the Stoner condition, and around 10% Cu concentration the EFE_\mathrm{F} goes beyond the peak, yielding the paramagnetic state. In our notation (La1.5_{1.5}Mg0.5_{0.5}Ni7−y_{7-y}Cuy_y) 3% and 10% Cu concentrations would correspond to yy equal to 0.21 and 0.7, respectively. Our results presented in Figure 9 qualitatively confirm the explanation proposed by Tazuke et al. [65]. In Figure 9 we show that for Cu concentration y∼0.5−1.0y \sim0.5-1.0 the position of the considered van Hove singularity falls on the Fermi level. This observation may also explain the sensitivity of the electrochemical properties of A2_2B7_7-type samples on small variations in chemical composition. The real samples are, however, not as uniformed as we consider in theoretical models. Thus, we should expect more a qualitative agreement between the calculated and measured trends, rather than a quantitative agreement between the corresponding values. The more advanced models should, among other, take into account the site preferences of the dopants and more accurately treat the chemical disorder, for example within the coherent potential approximation (CPA).

Densities of states for La1.5Mg0.5Ni7−yCuy phases

Figure 9. Effect of the composition on the electronic structure in the vicinity of Fermi level. Densities of states (DOS) for La1.5_{1.5}Mg0.5_{0.5}Ni7−y_{7-y}Cuy_y (y=0.0,0.5,1.0,1.5y = 0.0, 0.5, 1.0, 1.5) phases as calculated with scalar-relativistic PBE FPLO scheme treating La/Mg disorder with the ordered compound method and Ni/Cu disorder with virtual crystal approximation (VCA).

Here we present a CPA study of Co site preferences for La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} in rhombohedral Gd2_2Co7_7-type system. We observe the minimum energy for the Co dopants occupying the 9e sites, but the 18h sites are only slightly less energetically favored. All of the five inequivalent Ni positions identified by Virkar and Raman are: 3b, 6c1_1, 6c2_2, 9e, 18h [25, 66]. The most preferred sites are at the same time the most capacious ones (9e, 18h). Figure 10 presents a series of DOSs in the vicinity of the Fermi level for Co dopants occupying five different Ni sites in the La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} alloy. The purpose of presenting these results is to show how different site occupations influence the DOS around the Fermi level. The results from CPA confirm the limited application of our results from VCA and ordered structure approach to model the details of the electronic structure. However, even the CPA models do not cover the microstructural features of the real samples. Thus, they can serve more as a guide for performing conclusive experiments, rather to be a final settlement on the electronic properties of the bulk samples. Figure 10 shows that the van Hove singularity is present for each of the considered site occupation. The position of the narrow peak vary with the choice of the site. For the case of the energetically most preferred 9e site, the Fermi level is on the slope of the van Hove peak and close to its maximum.

Figure 10. Effect of Co site preference on the electronic structure in the vicinity of Fermi level. Densities of states (DOS) for La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} (Gd2_2Co7_7-type) phase as calculated with scalar-relativistic LDA FPLO scheme treating disorder with the coherent potential approximation (CPA).

Summary and conclusions

In this work we investigated the effect of substituting La by Gd and Ni by Co on electrochemical and electronic properties of the La1.5_{1.5}Mg0.5_{0.5}Ni7_7 alloy. The experimental preparation and characterization were accompanied by the density functional theory (DFT) calculations. Two series of La1.5−x_{1.5-x}Gdx_xMg0.5_{0.5}Ni7_7 (x=0.0,0.25,1.0x = 0.0, 0.25, 1.0) and La1.5_{1.5}Mg0.5_{0.5}Ni7−y_{7-y}Coy_y (y=0.0,0.5,1.5y = 0.0, 0.5, 1.5) alloys were obtained by mechanical alloying. They were characterized by XRD and electrochemical measurements, which showed that the obtained samples have a multiphase character and consist mainly of the Ce2_2Ni7_7-type and Gd2_2Co7_7-type structures of (La,Mg)2_2Ni7_7 phase with a minor contribution of LaNi5_5 and La2_2O3_3 phases. The most promising electrochemical properties were identified for La1.25_{1.25}Gd0.25_{0.25}Mg0.5_{0.5}Ni7_7 and La1.5_{1.5}Mg0.5_{0.5}Ni6.5_{6.5}Co0.5_{0.5} alloy electrodes. These two optimal compositions were a subject of the X-ray photoelectron spectroscopy (XPS) measurements. The experimentally investigated XPS valence band spectra were interpreted based on the corresponding spectra calculated from first principles. The theoretical analysis of valence bands focused on the van Hove singularity observed close to the Fermi level. Presence of this narrow peak is suggested as one of the causes of variations in electrochemical properties of the systems with Gd and Co substitutions.

Acknowledgements

Work supported by the National Science Centre Poland under the decision DEC-2014/15/B/ST8/00088. The computations were performed on the resources provided by the Poznań Supercomputing and Networking Center (PSNC).

References

References

  1. [1]L. Ouyang, J. Huang, H. Wang, J. Liu, M. Zhu, Progress of hydrogen storage alloys for Ni-MH rechargeable power batteries in electric vehicles: A review, Mater. Chem. Phys. 200 (2017) 164–178.DOI
  2. [2]H. Zhang, X. Zheng, X. Tian, Y. Liu, X. Li, New approaches for rare earth-magnesium based hydrogen storage alloys, Prog. Nat. Sci.-Mater. 27 (2017) 50–57.DOI
  3. [3]Y. Fan, L. Zhang, C. Xue, G. Fan, B. Liu, S. Han, Phase structure and electrochemical hydrogen storage performance of La₄MgNi₁₈M (M = Ni, Al, Cu and Co) alloys, J. Alloys Compd. 727 (2017) 398–409.DOI
  4. [4]J. Liu, S. Han, X. Li, L. Zhang, Y. Zhao, S. Yang, B. Liu, Phase structures and electrochemical properties of La–Mg–Ni-based hydrogen storage alloys with superlattice structure, Int. J. Hydrogen Energy 41 (2016) 20261–20275.
  5. [5]C. Xue, L. Zhang, Y. Fan, G. Fan, B. Liu, S. Han, Phase transformation and electrochemical hydrogen storage performances of La₃R MgNi₁₉ (R = La, Pr, Nd, Sm, Gd and Y) alloys, Int. J. Hydrogen Energy 42 (2017) 6051–6064.
  6. [6]W. Lv, J. Yuan, B. Zhang, Y. Wu, Influence of the substitution Ce for La on structural and electrochemical characteristics of La₀.₇₅−xCeₓMg₀.₂₅Ni₃Co₀.₅ (x = 0, 0.05, 0.1, 0.15, 0.2 at. %) hydrogen storage alloys, J. Alloys Compd. 730 (2018) 360–368.
  7. [7]J. Liu, S. Han, Y. Li, S. Yang, X. Chen, C. Wu, C. Ma, Effect of Pr on phase structure and cycling stability of La–Mg–Ni-based alloys with A₂B₇- and A₅B₁₉-type superlattice structures, Electrochimica Acta 184 (2015) 257–263.
  8. [8]C. Wu, L. Zhang, J. Liu, Y. Li, S. Yang, B. Liu, S. Han, Electrochemical characteristics of La₀.₅₉Nd₀.₁₄Mg₀.₂₇Ni₃.₃ alloy with rhombohedral-type and hexagonal-type A₂B₇ phases, J. Alloys Compd. 693 (2017) 573–581.
  9. [9]Y. Li, S. Han, J. Li, X. Zhu, L. Hu, The effect of Nd content on the electrochemical properties of low-Co La–Mg–Ni-based hydrogen storage alloys, J. Alloys Compd. 458 (2008) 357–362.
  10. [10]M. N. Guzik, J. Lang, J. Huot, S. Sartori, Effect of Al presence and synthesis method on phase composition of the hydrogen absorbing La–Mg–Ni-based compounds, Int. J. Hydrogen Energy 42 (2017) 30135–30144.
  11. [11]W. Li, B. Zhang, J. Yuan, Y. Yan, Y. Wu, Effect of Mo content on the microstructures and electrochemical performances of La₀.₇₅Mg₀.₂₅Ni₃.₂−xCo₀.₂Al₀.₁Moₓ (x = 0, 0.10, 0.15, 0.20) hydrogen storage alloys, J. Alloys Compd. 692 (2017) 817–824.
  12. [12]W. Lv, Y. Shi, W. Deng, J. Yuan, Y. Yan, Y. Wu, Microstructural evolution and performance of hydrogen storage and electrochemistry of Co-added La₀.₇₅Mg₀.₂₅Ni₃.₅−xCoₓ (x = 0, 0.2, 0.5 at%) alloys, Prog. Nat. Sci.-Mater. 27 (2017) 424–429.
  13. [13]Z. Cao, L. Ouyang, L. Li, Y. Lu, H. Wang, J. Liu, D. Min, Y. Chen, F. Xiao, T. Sun, R. Tang, M. Zhu, Enhanced discharge capacity and cycling properties in high-samarium, praseodymium/neodymium-free, and low-cobalt A₂B₇ electrode materials for nickel-metal hydride battery, Int. J. Hydrogen Energy 40 (2015) 451–455.
  14. [14]L.-j. Huang, Y.-x. Wang, J.-g. Tang, Y.-c. Zhao, G.-f. Liu, Y. Wang, J.-x. Liu, J.-q. Jiao, W. Wang, B. Jin, L. A. Belfiore, M. J. Kipper, Graphene/silver nanocomposites stabilize Mg-Ni-La electrode alloys and enhance electrochemical performance, J. Alloys Compd. 694 (2017) 1140–1148.DOI
  15. [15]X. Ma, X. Xie, P. Liu, L. Xu, T. Liu, Synergic catalytic effect of Ti hydride and Nb nanoparticles for improving hydrogenation and dehydrogenation kinetics of Mg-based nanocomposite, Prog. Nat. Sci.-Mater. 27 (2017) 99–104.
  16. [16]R. Li, J. Wan, F. Wang, C. Ding, R. Yu, Effect of non-stoichiometry on microstructure and electrochemical performance of La₀.₈GdₓMg₀.₂Ni₃.₁₅Co₀.₂₅Al₀.₁ (x = 0–0.4) hydrogen storage alloys, J. Power Sources 301 (2016) 229–236.
  17. [17]V. Yartys, R. Dens, Structure–properties relationship in RE₃−xMgₓNi₉H₁₀−₁₃ (RE = La, Pr, Nd) hydrides for energy storage, J. Alloys Compd. 645 (2015) S412–S418.
  18. [18]Z. Dong, L. Ma, X. Shen, L. Wang, Y. Wu, L. Wang, Cooperative effect of Co and Al on the microstructure and electrochemical properties of AB₃-type hydrogen storage electrode alloys for advanced MH/Ni secondary battery, Int. J. Hydrogen Energy 36 (2011) 893–900.
  19. [19]M. Anik, A. Aybar, N. B. Hatirnaz, D. Özdemir, Synthesis of La₂(Ni₁−xCoₓ)₇ (x = 0.05, 0.1, 0.2) Hydrogen Storage Alloys by the Electro-Deoxidation Technique, J. Electrochem. Soc. 162 (2015) A1080–A1084.
  20. [20]B. Liao, Y. Q. Lei, L. X. Chen, G. L. Lu, H. G. Pan, Q. D. Wang, Effect of Co substitution for Ni on the structural and electrochemical properties of La₂Mg(Ni₁−xCoₓ)₉ (x = 0.1–0.5) hydrogen storage electrode alloys, Electrochimica Acta 50 (2004) 1057–1063.
  21. [21]D. Wang, Y. Luo, R. Yan, F. Zhang, L. Kang, Phase structure and electrochemical properties of La₀.₆₇Mg₀.₃₃Ni₃.₀−xCoₓ (x = 0.0, 0.25, 0.5, 0.75) hydrogen storage alloys, J. Alloys Compd. 413 (2006) 193–197.
  22. [22]L. Ouyang, T. Yang, M. Zhu, D. Min, T. Luo, H. Wang, F. Xiao, R. Tang, Hydrogen storage and electrochemical properties of Pr, Nd and Co-free La₁₃.₉Sm₂₄.₇Mg₁.₅Ni₁₅.₈Al₁.₇Zr₀.₁₄Ag₀.₀₇ alloy as a nickel-metal hydride battery electrode, J. Alloys Compd. 735 (2018) 98–103.
  23. [23]M. Dymek, M. Nowak, M. Jurczyk, H. Bala, Encapsulation of La₁.₅Mg₀.₅Ni₇ nanocrystalline hydrogen storage alloy with Ni coatings and its electrochemical characterization, J. Alloys Compd. 749 (2018) 534–542.
  24. [24]M. Balcerzak, M. Nowak, M. Jurczyk, Hydrogenation and electrochemical studies of La–Mg–Ni alloys, Int. J. Hydrogen Energy 42 (2017) 1436–1443.
  25. [25]M. Werwiński, A. Szajek, A. Marczyńska, L. Smardz, M. Nowak, M. Jurczyk, Effect of substitution La by Mg on electrochemical and electronic properties in La₂−xMgₓNi₇ alloys: a combined experimental and ab initio studies, J. Alloys Compd. 763 (2018) 951–959.
  26. [26]M. D. Kuz’min, K. P. Skokov, I. Radulov, C. A. Schwöbel, S. Foro, W. Donner, M. Werwiński, J. Rusz, E. Delczeg-Czirjak, O. Gutfleisch, Magnetic anisotropy of La₂Co₇, J. Appl. Phys. 118 (2015) 053905–1–053905–5.DOI
  27. [27]J.-C. Crivello, J.-H. Zhang, M. Latroche, Structural Stability of ABᵧ Phases in the (La,Mg)–Ni System Obtained by Density Functional Theory Calculations, J. Phys. Chem. C 115 (2011) 25470–25478.
  28. [28]J.-C. Crivello, M. Gupta, M. Latroche, First principles calculations of (La,Mg)₂Ni₇ hydrides, J. Alloys Compd. 645 (2015) S5–S8.DOI
  29. [29]R. A. Varin, T. Czujko, Z. S. Wronski, Nanomaterials for Solid State Hydrogen Storage, Springer Science & Business Media, 2009.
  30. [30]Y. Baer, G. Busch, P. Cohn, Monochromatized x-ray source for high resolution electron spectroscopy, Rev. Sci. Instrum. 46 (1975) 466–469.
  31. [31]J. Skoryna, S. Pacanowski, A. Marczyńska, M. Werwiński, A. Rogowska, M. Wachowiak, Ł. Majchrzycki, R. Czajka, L. Smardz, XPS valence band studies of nanocrystalline ZrPd alloy thin films, Surf. Coat. Technol. 303 (2016) 125–130.
  32. [32]K. Koepernik, H. Eschrig, Full-potential nonorthogonal local-orbital minimum-basis band-structure scheme, Phys. Rev. B 59 (1999) 1743–1757.DOI
  33. [33]J. P. Perdew, K. Burke, M. Ernzerhof, Generalized gradient approximation made simple, Phys. Rev. Lett. 77 (1996) 3865–3868.
  34. [34]K. Momma, F. Izumi, VESTA : a three-dimensional visualization system for electronic and structural analysis, J. Appl. Crystallogr. 41 (2008) 653–658.
  35. [35]E. Levin, P. Donskoy, S. Lushnikov, V. Veretsky, T. Safonova, O. Petrii, Hydrogen sorption and electrochemical properties of intermetallic compounds La₂Ni₇ and La₂Ni₆Co, in: Hydrogen materials science and chemistry of carbon nanomaterials, Springer, 2004, pp. 503–510.DOI
  36. [36]F. T. Parker, H. Oesterreicher, Magnetic properties of La₂Ni₇, J. Less Common Met. 90 (1983) 127–136.
  37. [37]N. Pierunek, Z. Śniadecki, M. Werwiński, B. Wasilewski, V. Franco, B. Idzikowski, Normal and inverse magnetocaloric effects in structurally disordered Laves phase Y₁₋ₓGdₓCo₂ (0 < x < 1) compounds, J. Alloys Compd. 702 (2017) 258–265.
  38. [38]J. Kudrnowský, V. Drchal, P. Bruno, Magnetic properties of fcc Ni-based transition metal alloys, Phys. Rev. B 77 (2008) 224422–1– 224422–8.
  39. [39]P. Soven, Coherent-potential model of substitutional disordered alloys, Phys. Rev. 156 (1967) 809–813.DOI
  40. [40]K. Koepernik, B. Velický, R. Hayn, H. Eschrig, Self-consistent LCAO-CPA method for disordered alloys, Phys. Rev. B 55 (1997) 5717–5729.DOI
  41. [41]Z. Śniadecki, M. Werwiński, A. Szajek, U. K. Rößler, B. Idzikowski, Induced magnetic ordering in alloyed compounds based on Pauli paramagnet YCo₂, J. Appl. Phys. 115 (2014) 17E129–1–17E129–3.DOI
  42. [42]J. P. Perdew, Y. Wang, Accurate and simple analytic representation of the electron-gas correlation energy, Phys. Rev. B 45 (1992) 13244–13249.
  43. [43]J. J. Yeh, I. Lindau, Atomic subshell photoionization cross sections and asymmetry parameters: 1 <= Z <= 103, At. Data Nucl. Data Tables 32 (1985) 1–155.
  44. [44]J. A. Morokowski, G. Chelkowska, M. Werwiński, A. Szajek, R. Troć, C. Neise, X-ray photoemission spectrum, electronic structure, and magnetism of UCu₂Si₂, J. Alloys Compd. 509 (2011) 6994–6998.
  45. [45]M. Nowak, M. Balcerzak, M. Jurczyk, Hydrogen storage and electrochemical properties of mechanically alloyed La₁.₅₋ₓGdₓMg₀.₅Ni₇ (0 <= x <= 1.5), Int. J. Hydrogen Energy 43 (2018) 8897–8906.
  46. [46]S. Xiang, C. Y. Yungui, T. Mingda, W. Chaoling, D. Gang, K. Zhenzhen, The structure and 233 K electrochemical properties of La₀.₈₋ₓNdₓMg₀.₂Ni₃.₁Co₀.₂₅Al₀.₁₅ (x = 0.0–0.4) hydrogen storage alloys, Int. J. Hydrogen Energy 34 (2009) 2661–2669.
  47. [47]K. Iwase, K. Mori, A. Hoshikawa, T. Ishigaki, Hydrogenation and structural properties of Gd₂Ni₇ with superlattice structure, Int. J. Hydrogen Energy 37 (2012) 5122–5127.
  48. [48]Q. Ming, L. Shuhui, Q. P. A. L. Zhigiang, G. Jin, The influence of Co content on LaNi₃.₂₋ₓMn₀₃Coₓ (x = 0.2–0.8) Alloy Hydrogen Storage and Electrochemical Properties, Physics Proc. 22 (2011) 577–583.
  49. [49]Y.-H. Zhang, L.-C. Chen, T. Yang, C. Xu, H.-P. Ren, D.-L. Zhao, The electrochemical hydrogen storage performances of Si-added La–Mg–Ni–Co-based A₂B₇-type electrode alloys, Rare Met. 34 (2015) 569–579.
  50. [50]F. Zhang, Y. Luo, K. Sun, D. Wang, R. Yan, L. Kang, J. Chen, Effect of Co content on the structure and electrochemical properties of La₁.₅Mg₀.₅Ni₇₋ₓCoₓ (x = 0, 1.2, 1.8) hydrogen storage alloys, J. Alloys Compd. 424 (2006) 218–224.
  51. [51]J. J. G. S. A. Willems, Metal hydride electrodes stability of LaNi₅-related compounds, Ph.D. thesis (1984).
  52. [52]K. Iwase, K. Sakaki, Y. Nakamura, E. Akiba, In Situ XRD Study of La₂Ni₇Hₓ During Hydrogen Absorption–Desorption, Inorg. Chem. 52 (2013) 10105–10111.DOI
  53. [53]H. Miao, H. Pan, S. Zhang, N. Chen, R. Li, M. Gao, Influences of Co substitution and annealing treatment on the structure and electrochemical properties of hydrogen storage alloys La₀.₇Mg₀.₃Ni₂.₄₅₋ₓCo₀.₇₅₊ₓMn₀.₁Al₀.₂ (x = 0.00, 0.15, 0.30), Int. J. Hydrogen Energy 32 (2007) 3387–3394.
  54. [54]X.-l. Zhao, Y.-h. Zhang, B.-w. Li, H.-p. Ren, X.-p. Dong, X.-l. Wang, Investigation on microstructures and electrochemical performances of La₀.₇₅Mg₀.₂₅Ni₂.₅Coₓ (x = 0–1.0) hydrogen storage alloys, J. Alloys Compd. 454 (2008) 437–441.
  55. [55]L. Ouyang, Z. Cao, L. Li, H. Wang, J. Liu, D. Min, Y. Chen, F. Xiao, R. Tang, M. Zhu, Enhanced high-rate discharge properties of La₁.₁₃Mg₀.₆Sm₇.₄Ni₆₁.₀Co₇.₂Al₁.₇ with added graphene synthesized by plasma milling, Int. J. Hydrogen Energy 39 (2014) 12765–12772.
  56. [57]L. Ouyang, Z. Cao, H. Wang, R. Hu, M. Zhu, Application of dielectric barrier discharge plasma-assisted milling in energy storage materials – A review, J. Alloys Compd. 691 (2017) 422–435.
  57. [58]P. C. P. Bouten, A. R. Miedema, On the heats of formation of the binary hydrides of transition metals, J. Less Common Met. 71 (1980) 147–160.
  58. [59]R. Griessen, Heats of solution and lattice-expansion and trapping energies of hydrogen in transition metals, Phys. Rev. B 38 (1988) 3690–3698.
  59. [60]S. B. Dugdale, T. Jarlborg, Electronic structure, magnetism, and superconductivity of MgCₓNi₃, Phys. Rev. B 64 (2001) 100508–1–100508–4.
  60. [61]J. I. Lee, T. S. Zhao, I. G. Kim, B. I. Min, S. J. Youn, Electronic structure of Ni-based superconducting quaternary compounds: YNi₂B₂X (X = B, C, N, and O), Phys. Rev. B 50 (1994) 4030–4033.
  61. [62]J. W. Allen, S. J. Oh, M. B. Maple, M. S. Torikachvili, Large Fermi-level resonance in the electron-addition spectrum of CeRu₂ and CeIr₂, Phys. Rev. B 28 (1983) 5347–5349.
  62. [63]M. Shimizu, J. Inoue, S. Nagasawa, Electronic structure and magnetic properties of Y-Ni intermetallic compounds, J. Phys. F: Metal Phys. 14 (1984) 2673–2687.
  63. [64]M. Mukase, Y. Tazuke, H. Mitamura, T. Goto, T. Sato, Itinerant Electron Magnetism of Hexagonal La₂Ni₇, Mater. Trans., JIM 41 (2000) 1046–1051.
  64. [65]Y. Tazuke, H. Suzuki, H. Tanikawa, Metamagnetic transitions in hexagonal La₂Ni₇, Physica B 346–347 (2004) 122–126.
  65. [66]A. V. Virkar, A. Raman, Crystal structures of AB₃ and A₂B₇ rare earth-nickel phases, J. Less Common Met. 18 (1969) 59–66.

Paper details

vlnc:W_runatas3
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents