betaFeedback

WorksPhysics and Astronomy

Controlling magnetic configuration in soft-hard bilayers probed by polarized neutron reflectometry

Abstract

Hard/soft magnetic bilayer thin films have been widely used in data storage technologies and permanent magnet applications. The magnetic configuration and response to temperatures and magnetic fields in these heterostructures are considered to be highly dependent on the interfacial coupling. However, the intrinsic properties of each of the layers, such as the saturation magnetization and layer thickness, also strongly influence the magnetic configuration. Changing these parameters provides an effective method to tailor magnetic properties in composite magnets. Here, we use polarized neutron reflectometry (PNR) to experimentally probe the interfacial magnetic configurations in hard/soft bilayer thin films: L10-FePt/A1-FePt, [Co/Pd] /CoPd, [Co/Pt] /FeNi and L10-FePt/Fe, which all have a perpendicular magnetic anisotropy in the hard layer. These films were designed with different soft and hard layer thicknesses (t_soft and t_hard) and saturation magnetization (M_s^soft and M_s^hard), respectively. The influences of an in-plane magnetic field (H_ip) and temperature (T) are also studied using a L10 FePt/A1-FePt bilayer sample. Comparing the PNR results to micromagnetic simulations reveals that the interfacial magnetic configuration is highly dependent on t_soft, M_s^soft and the external factors (H_ip and T), and has a relatively weak dependence on t_hard and M_s^hard. Key among these results, for thin t_soft, the hard and soft layers are rigidly coupled in the out-of-plane direction, then undergo a transition to relax in-plane. This transition can be delayed to larger t_soft by decreasing M_s^soft. Understanding the influence of these parameters on the magnetic configuration is critical to designing functional composite magnets for applications.

Introduction

Heterostructures of coupled, magnetically hard/soft composites [1, 2, 3, 4, 5] have played a critical role in many modern data storage [6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17] and permanent magnet [1, 18, 19, 20] technologies. In magnetic recording media, the high-anisotropy (magnetically hard) layer is frequently coupled to a magnetically soft layer which aids in the data-writing process [21, 22, 23]. In these exchange coupled composite (ECC) systems, the soft layer nucleates a domain wall that is easily pushed into the hard layer, reducing the writing field. As the anisotropy of the hard layer has been increased to allow for smaller grains, and thus higher recording densities[16, 24, 25, 26], the writability provided by the soft layer has become indispensable [27, 28]. In another example, high-anisotropy magnetic materials are coupled to high moment materials to develop a composite magnetic structure with a large maximum energy product for permanent magnet applications [1, 29]. The magnetic configuration in composite magnets thus reflect each layer’s intrinsic properties, propagated across the interface by the interface exchange and dipolar fields. Since the interfaces are highly imperfect – rich in dislocations and vacancies, becoming a virtual grain boundary – the resultant properties are an enigmatic mixture of each materials properties and can be challenging to predict. Understanding the full range of interactions within hard/soft coupled systems is critical for composite applications. Magnetic hard/soft bilayers can provide a model system to gain critical understanding of the magnetic interactions and their impacts on technological applications [30, 31].

In hard/soft bilayers with perpendicularly magnetized hard layer, the magnetic interactions are highly dependent on the thickness of the soft layer, tsoftt_{soft} [32, 33]. For the case of a thin soft layer with a thickness less than the classical exchange length (lexl_{ex}), it is typically accepted that the magnetic moments are rigidly coupled to the hard layer by the exchange interaction. Furthermore, as tsoftt_{soft} increases, it is expected that the magnetic moment relaxes in-plane, especially away from the hard/soft interface, resulting in exchange spring-like behavior [34]. In addition to tsoftt_{soft}, the magnetic configuration is also influenced by the material properties including the saturation magnetization (MshardM_s^{hard} and MssoftM_s^{soft}), exchange stiffness (AhardA_{hard} and AsoftA_{soft}), the hard layer magnetocrystalline anisotropy (KuK_u) and the hard/soft interfacial coupling stiffness (AintA_{int}) [30, 31, 35]. While some of these magnetic material parameters have predictable relationships with the magnetic configuration, e.g. KuK_u and AhardA_{hard} can be used to determine an exchange length (≈πAhardKu\approx\pi\sqrt{\frac{A_{hard}}{K_u}}) in hard magnets, the dependence on MshardM_s^{hard} and MssoftM_s^{soft} or the film thickness, is not as straightforward. For modern applications in heat assisted magnetic recording (HAMR) technologies, understanding the temperature dependence of these properties and its effect on the magnetic configuration is critical to device functionality [36, 37, 38, 39, 40]. This quality is manifested in HAMR devices where high temperatures are used to reduce KuK_u, but simultaneously also reduce MshardM_s^{hard} and MssoftM_s^{soft}, establishing an optimization problem to achieve the ideal writability. Finally, the applied magnetic field also strongly influences the magnetic configuration; while most of the magnetic energy terms are uniaxial, the field dependent Zeeman energy is unidirectional and establishes a new balance between the various energy terms. Therefore, to better design and control hard/soft magnetic heterostructures, it is important to understand the roles of sample geometry (tsoftt_{soft}), materials properties (MshardM_s^{hard}, MssoftM_s^{soft}) and external influences (applied in-plane magnetic field, HipH_{ip}, and temperature, TT) in determining the magnetic configuration.

Methods

Four series of samples covering a range of MssoftM_{s}^{soft}, MshardM_{s}^{hard} and tsoftt_{soft} are synthesized by magnetron sputtering and the details can be found elsewhere [32, 41, 42, 43]: 1). The Si/SiO2_2 (200 nm) /L10L1_{0}-FePt (4 nm)/A1-FePt (tsoftt_{soft})/Ti (4 nm) samples were prepared in a vacuum system with a base pressure of 8×10−88 \times10^{-8} Torr. The oriented L10L1_{0}-FePt was prepared by rapid thermal annealing, as described previously [26, 32, 44]. Without breaking vacuum, the A1-FePt soft layer (2 nm or 5 nm) was deposited on L10L1_{0}-FePt by co-sputtering of elemental targets, followed by a Ti capping layer. 2). The preparation process of Si/SiO2_2 (200 nm) /L10L1_{0}-FePt (4 nm)/Fe (9 nm)/Pt (2 nm) is similar to the Si/SiO2_2 (200 nm) /L10L1_{0}-FePt (4 nm)/A1-FePt (tsoftt_{soft})/Ti (4 nm) samples, but sputtering 9 nm Fe and 2 nm Pt as the soft and capping layers, respectively. 3). For Si/SiO2_2/[Co(0.4 nm)/Pt(0.7 nm)]4_4/FeNi (tsoftt_{soft})/Pd (2 nm) samples, 4 repeats of Co (0.4 nm)/Pt (0.7 nm) multilayer stack were first sputtered on Si/SiO2_2 substrate. Four different thicknesses of soft Fe0.2_{0.2}Ni0.8_{0.8} (0, 1, 3, 7 nm) layers are then deposited, followed by a 2 nm Pd capping layer. 4). The Si/Pd (20 nm)/[Co (0.3 nm)/Pd (0.9 nm)]25_{25}/CoPd(tsoftt_{soft})/Pd (5 nm) samples were magnetron sputtered in an ultrahigh vacuum chamber with a base pressure of 9×10−99 \times10^{-9} Torr. Magnetically hard [Co (0.3 nm)/Pd (0.9 nm)]25_{25} multilayers were sputtered onto Si substrates, with a 20 nm Pd buffer layer. Different thicknesses of tsoftt_{soft} (2, 5, 9 nm) were then deposited, followed by a 5 nm Pd capping layer. For all the samples, the underlayer films (L10L1_{0} FePt, Co/Pt and Co/Pd multilayers) have strong perpendicular magnetic anisotropy (PMA).

Polarized neutron reflectometry was performed at the NIST Center for Neutron Research on both the PBR and MAGIK instruments, which uses 4.75 Å and 5.00 Å wavelength neutrons, respectively. For the L10L1_{0}-FePt/A1-FePt samples to study the influence of tsoftt_{soft} on magnetic configuration, the film was rotated into a grazing incidence with the neutron beam. The films were first saturated with a magnetic field (700 mT) parallel to the film normal direction and then the field was reduced to 50 mT. Then, the film was rotated such that the 50 mT field is applied along the film normal direction; this field is insufficient to significantly change the magnetic configuration, and acts to preserve the orientation of the neutrons, i.e. as a guide field. The out-ofplane guide field sets the orientation of the neutron spin moment always along the out-of or into-the-plane direction. The PNR measurement is executed by performing a coupled theta-2theta specular scan, with control and sensitivity to the incident and scattered neutron spin. The non-spin-flip PNR cross-sections (R++R^{++} and R−−R^{--}, where RR is the reflection intensity, with the superscript indicating the spin configuration of the incident and reflected neutrons, + (–) indicting the spin-up (spin-down) geometries) typically provide sensitivity to the nuclear structure and the magnetization parallel to the neutron spin moment. However, the neutron scattering rules prohibit scattering from magnetization parallel to the momentum transfer vector, which for PNR, is in the out-of-plane direction. PNR is sensitive only to the in-plane magnetization, and with an out-of-plane guide field, the non-spin flip cross section encodes only the nuclear structure. Using an out-of-plane guide field, any net in-plane magnetization is orthogonal to the neutron spin and thus contributes to the spin-flip (R+−R^{+-}, R−+R^{-+}) cross section. In this geometry, sensitivity to the orientation of the in-plane magnetization is lost, however the signal is increased by including all of the magnetic signal into the spin-flip cross section.[45, 46] For all other PNR measurements, the samples were saturated in the out-of-plane direction, then returned to remanence and measured in a small in-plane guide field (1 mT). In this configuration, R++R^{++} and R−−R^{--}, provide sensitivity to both the nuclear depth profile, and the depth profile of the net in-plane magnetization component parallel to the applied field. Spin-flip scattering for this configuration is not considered here. All the experimental data are then model fitting by REFL1D software [45].

Three dimensional micromagnetic simulations are performed using the object oriented micromagnetic framework (OOMMF) platform,[47] with a simulation volume of 200 nm × 1 nm × (thard+tsoftt_{hard}+t_{soft}) and a mesh of 0.5 nm × 0.5 nm × 0.2 nm. The exchange stiffness for hard magnet (AhA_h), hard/soft interface (AintA_{int}), and soft magnetic (AsA_s) are Ah=As=Aint=1.15×10−11A_h=A_s=A_{int}=1.15 \times10^{-11} J/m. The uniaxial anisotropy for hard magnet (KuK_u) is chosen to be 1×1061 \times10^{6} J/m3^{3} while the anisotropy for soft magnet (KsK_s) is 0.

Experimental results

Effect of soft layer thickness

With the above experimental preparations, the first set of measurements were performed to study the influence of tsoftt_{soft} on the magnetic configuration. Using an out-of-plane guide field, reflectometry data for the L10L1_0-FePt(4 nm)/Al-FePt(tsoftt_{soft}) bilayer films, with tsoftt_{soft} = 2 nm and 5 nm, is shown in Figure 1a and Figure 1b, respectively. Data on the same sample, but taken at a different time, was shown in reference [32], and reflects a similar profile; differences in the capping layer structure are captured in this work, likely due to the higher qq-range measured. For the tsoftt_{soft}=2 nm film, the experimental non-spin-flip R++R^{++} and R−−R^{--} are essentially identical, and the spin-flip R+−R^{+-} and R−+R^{-+} are virtually zero. This indicates that there is little net in-plane magnetization anywhere in the film. In comparison, for the tsoftt_{soft}=5 nm film, the R++R^{++} and R−−R^{--} are still overlapping, but R+−R^{+-} and R−+R^{-+} are now non-zero, indicating the presence of appreciable in-plane magnetization. These interpretations are confirmed by model fitting (solid lines in Figure 1a and Figure 1b) that yields the scattering length density (SLD) [48] depth profiles for the two films, shown in Figure 1c and Figure 1d. The profiles have a nuclear component (NSLD) indicative of the nuclear composition, and a magnetic component (MSLD) proportional to the in-plane magnetization. Notably, the MSLD is approximately zero for tsoft=2t_{soft}=2 nm, and non-zero for tsoft=5t_{soft}=5 nm. These results confirm that tsoftt_{soft} can influence the magnetic configuration in the soft layer. Interestingly, this influence extends all the way to the interface: while both the hard and soft layers in the 2nm sample are oriented out-of-plane, the soft layer in the 5nm sample is almost entirely in-plane.

Model-fitted PNR data and associated scattering length density profiles

Figure 1. Model-fitted PNR data of L10_{10}-FePt (4 nm)/A1-FePt for (a) tsoft=2t_{\mathrm{soft}}=2 (b) tsoft=5t_{\mathrm{soft}}=5 nm and the associated scattering length density profiles (c) tsoft=2t_{\mathrm{soft}}=2 (d) tsoft=5t_{\mathrm{soft}}=5 nm. The red, green, blue and yellow regions correspond to the depth profile of SiO2_2, L10_{10}-FePt, A1-FePt and capping Ti layers, respectively.

Effect of saturation magnetization

Besides tsoftt_{soft}, MshardM_s^{hard} and MssoftM_s^{soft} are expected to influence the magnetic configurations in these bilayer films. PNR measurements are also performed on a series of samples with Mshard≪MssoftM_s^{hard} \ll M_s^{soft}, Mshard<MssoftM_s^{hard} < M_s^{soft} and Mshard>MssoftM_s^{hard} > M_s^{soft}, including L1₀-FePt(4nm)/Fe(9nm), [Co (0.3 nm)/Pd(0.9 nm)]₂₅/CoPd(9nm), and [Co(0.4 nm)/Pt(0.7nm)]₄/FeNi (7 nm), respectively. For the case of Mshard≪MssoftM_s^{hard} \ll M_s^{soft} shown in Figure 2a, the experimental R++R^{++} and R−−R^{--} curves are significantly separated, which indicates a net in-plane magnetization. The corresponding magnetic depth profiles, in Figure 2b, show a large MSLD in the soft layer (Fe region). Using the MSLD for bulk iron (4.85 ×10−4\times10^{-4} nm−2^{-2}) [48], the soft Fe layer is confirmed to be almost entirely in-plane throughout its thickness. For Mshard<MssoftM_s^{hard} < M_s^{soft} and Mshard>MssoftM_s^{hard} > M_s^{soft}, the experimental R++R^{++} and R−−R^{--} curves are strongly overlapping, as shown in Figure 2c and Figure 2e, respectively. The corresponding magnetic depth profiles show almost no MSLD in Figure 2d and Figure 2f, respectively. These results suggest that in both the [Co (0.3 nm)/Pd (0.9 nm)]₂₅/CoPd (9 nm) and [Co (0.4 nm)/Pt (0.7nm)]₄/FeNi (7 nm) films, even at these relatively larger thicknesses, the soft layer magnetization remains mostly in the out-of-plane direction. The PNR measurements are also performed on another five [Co (0.3 nm)/Pd(0.9 nm)]₂₅/CoPd and [Co(0.4 nm)/Pt(0.7nm)]₄/FeNi samples with thinner soft layer thickness, shown in S1. These films also show very little in-plane magnetization.

Six-panel plots showing fitted reflectivities and nuclear and magnetic SLD profiles for three multilayer systems

Figure 2. L10\mathrm{L}_{10}-FePt/Fe (a) Fitted R++R^{++} and R−−R^{--} and (b) the corresponding nuclear (black) and magnetic (red) SLD profiles, where pink, green, blue and yellow regions are the SiO2\mathrm{SiO_2}, L10\mathrm{L}_{10}-FePt, Fe and Pt capping layers, respectively. [Co/Pd]-multilayers/CoPd (c) Fitted R++R^{++} and R−−R^{--} and (d) nuclear (black) and magnetic (red) SLD profiles where pink, green, blue, yellow and orange regions correspond to the Si, Pd seed layer, [Co/Pd] multilayers, CoPd soft layer and Pd capping layer, respectively. [Co/Pt]-multilayers/FeNi (e) fitted R++R^{++} and R−−R^{--} and corresponding nuclear (black) and magnetic (red) SLD profiles with SiO2\mathrm{SiO_2} (pink), Pt buffer layer (green), [Co/Pt] multilayers (blue), FeNi (yellow) and Pd capping layer (orange).

Effect of in-plane field and temperature

The results above implicate a complex competition within these systems to define the soft-layer orientation, which depends on both MssoftM_s^{soft} and tsoftt_{soft}. Besides these intrinsic material parameters, the interfacial magnetic configuration is also dependent on the external variables (HipH_{ip} and TT). Six PNR measurements were performed on the L1₀-FePt/A1-FePt (2 nm) bilayer sample with μ0Hip\mu_0H_{ip} from 100 mT to 700 mT at TT=295 K and TT=500 K, shown in Figure 3a and Figure 3b, respectively. For each in-plane magnetic field, the corresponding R++R^{++} and R−−R^{--} curves are separated, which indicates a net in-plane magnetization. This result can be alternatively confirmed by the spin asymmetry (SA) shown in Figure 3c and Figure 3d for TT=295 K and TT=500 K, respectively. SA is a quantity expressed as R++−R−−R+++R−−\frac{R^{++}-R^{--}}{R^{++}+R^{--}}, which highlights magnetic contributions to the scattering. Both Figure 3c and Figure 3d show a non-zero SA feature at all HipH_{ip} and TT, indicating the presence of a net in-plane magnetization for all the measurements. Fitted by REFL1D, the nuclear and magnetic depth profiles determined from model fitting are shown in Figure 3e and Figure 3f, respectively. The fitting constrained the nuclear depth profiles to be the same for all the measurements since the nuclear structure was not expected to change with TT and HipH_{ip}. The magnetic depth profiles here are presented using both MSLD (left axis) and the converted in-plane magnetization (right axis). All the PNR measurements show an appreciable in-plane component of the magnetization. This relaxation follows a power law fall off from the maximal magnetization in the soft layer (MtopM^{top}) to the in-plane component of the magnetization of hard underlayer (MbotM^{bot}). As an example, the position of MtopM^{top} and MbotM^{bot} for μ0Hip=100\mu_0 H_{ip}=100 mT and T=295T=295 K is demonstrated (dotted blue line). At both T=295T=295 K and T=500T=500 K, increasing HipH_{ip} results an overall increase of the in-plane magnetization, including MtopM^{top} and MbotM^{bot}, which can be attributed to the increase of in-plane Zeeman energy.

Polarized neutron reflectivity and fitted depth profiles

Figure 3. Polarized neutron reflectivity for L10_{10}-FePt (4 nm)/A1_{1}-FePt (2nm) with in-plane magnetic fields of 100 mT, 300 mT and 700 mT at (a) 295 K and (b) 500 K. The spin asymmetry for each field at (c) 295 K and (d) 500 K. The fitted (e) nuclear and (f) magnetic depth profiles and (g) the normalized magnetic depth profile. MtopM^{top} corresponds to the maximal in-plane magnetization of the soft layer and MbotM^{bot} is the magnetization of the hard layer.

An alternative analysis of the magnetic relaxation is performed by normalizing the magnetic depth profiles by their respective MtopM^{top}, shown in Figure 3g. For each HipH_{ip}, the maximum normalized magnetization (M/Mtop=1M/M^{top}=1) appears at almost the same position in the soft layer, about 5.8 nm away from the SiO2_2 interface. Notably, increasing HipH_{ip} causes an increase of the interfacial domain wall width, lintl_{int},[49] particularly by extending further into the hard layer. The HipH_{ip} presents an important role in determining the interfacial magnetic configurations by inducing an external Zeeman energy, while increasing TT enhances thermal fluctuations in the bilayer, reducing the anisotropy and competing with the exchange coupling. At each HipH_{ip}, increasing the temperature results in an overall reduction of the total magnetization including MtopM^{top} and MbotM^{bot}. For μ0Hip=100\mu_0H_{ip}=100 mT, MtopM^{top} changes from 320 kA/m at 295 K to 180 kA/m at 500 K, more than 40% reduction. This temperature driven reduction of MtopM^{top} decreases with increasing HipH_{ip}, becoming 30% for μ0Hip=300\mu_0H_{ip}=300 mT and only 16% for μ0Hip=700\mu_0H_{ip}=700 mT. These results indicate that increasing HipH_{ip} can compensate the thermal fluctuations, therefore increasing the in-plane soft layer magnetization. The normalized magnetic depth profiles for each HipH_{ip} shows that the interfacial magnetic configuration at 500 K is similar to the configuration at 295 K, indicating that there is almost no change in lintl_{int} or the normalized relaxation rate with temperature between 295 K and 500 K. These PNR experimental results reveal the influence of MssoftM_s^{soft}, tsoftt_{soft}, HipH_{ip} and TT on the interfacial magnetic configuration, summarized in Table 1.

SampleTsoftT_{soft} (nm)Soft-layer MSLD (×10−4\times10^{-4} nm−2^{-2})Guide Field (mT)Temperature (K)
L10L_{10}-FePt/A1-FePt20.0750 (out-of-plane)295
51.4650 (out-of-plane)295
20.93100295
21.41300295
21.77700295
20.491500
20.991500
21.441500
[Co/Pd]/CoPd20.011295
50.041295
90.081295
[Co/Pt]/FeNi10.371295
30.221295
70.191295
L10L_{10}-FePt/Fe94.821295

Table 1. the summary of PNR experimental results

Discussion and micromagnetic simulation

The PNR results provide a direct measurement of the magnetic relaxation within the bilayer system; the simulated magnetic depth profiles suggest this relaxation follows a power law from MtopM^{top} to MbotM^{bot}. PNR measurements show that this magnetic relaxation is dependent on sample geometry (tsoftt_{soft}), material properties (MssoftM_s^{soft}) and external factors (HipH_{ip} and TT). For tsoftt_{soft} larger than a critical thickness, the magnetic configuration changes from a rigid coupling, in which the soft layer has an out-of-plane orientation reflecting the hard underlayer, to an in-plane relaxation, in which the soft layer rotates from out-of-plane to in-plane moving from the interface; this critical soft layer thickness increases with decreasing MssoftM_s^{soft}. Increasing HipH_{ip} is shown to increase the overall in plane magnetization and lintl_{int}, while increasing TT from room temperature to 500 K result in a reduction of the in-plane magnetization, but lintl_{int} remains almost unchanged. In a simplified model, the in-plane relaxation can be considered as a balance among the magnetostatic energy of the soft layer, perpendicular anisotropy of the hard layer, the interfacial exchange coupling between the soft and hard layers and the Zeeman interaction. The increase of tsoftt_{soft} or MssoftM_s^{soft} results in the increase of total demagnetization energy, as well as the decrease of energy gap between the ground state to the excited magnon state [50, 51]. When the thermal energy (kBTk_BT) is high enough to overcome this energy gap, it will cause the transition from rigid coupling to the underlayer, which favors an in-plane orientation for the soft layer magnetization. As a result, the interfacial magnetic configuration relaxes in-plane. For increasing HipH_{ip}, the Zeeman energy favors an in-plane orientation parallel to HipH_{ip}, which increases MtopM^{top} and MbotM^{bot}. However, while increasing HipH_{ip}, the in-plane magnetic component of the soft layer increases more than the hard layer, due to the much larger saturation magnetization and the absence of a perpendicular anisotropy. The angle between the magnetization vector of the bottom hard layer and that of the top of the soft layer increases. This increased angle causes the interfacial exchange coupling energy to increase commensurately. To compensate this increase of energy, lintl_{int} extends further into the hard layer. Increasing TT to 500 K, the thermal fluctuations are enhanced which decreases MssoftM_s^{soft}, MshardM_s^{hard} and KuK_u. The reduction of MssoftM_s^{soft} decreases lintl_{int}, while the reduced KuK_u should increase lintl_{int}; these two factors can compensate each other, resulting an almost unchanged lintl_{int}. Indeed, in the experimental results lintl_{int} is almost unchanged. Ideally, increasing lintl_{int} improves writability in HAMR media[52], suggesting that, in this bilayer system, reducing the temperature dependence of MssoftM_s^{soft} by e.g. increasing the Curie temperature, would be a promising direction for improvement. The PNR measurements reveal the important roles of tsoftt_{soft}, MssoftM_s^{soft}, HipH_{ip} and TT in determining the configuration of the magnetic bilayer. The following simulations reinforce these observations and provide a more complete picture which must also include thardt_{hard} and MshardM_s^{hard}.

The first set of simulations that are presented explore the case of MssoftM_s^{soft} (300 kA/m) < MshardM_s^{hard} (900 kA/m), over a range of tsoftt_{soft} similar to our experiments with [Co/Pt]/NiFe, shown in Figure 4a. For thin tsoftt_{soft} (2 nm and 5 nm), the magnetic moments in the soft layer are strictly orientated in the out-of-plane direction. This magnetic configuration can be understood by the classical exchange length, lexl_{ex}: that for tsoft<lext_{soft} < l_{ex} the interfacial exchange coupling dominates the energy landscape, and rigidly couples the hard and soft layers. Increasing tsoftt_{soft} to 9 nm, the in-plane magnetic component of the soft layer begins to increase. Interestingly, the relaxation in the soft layer extends all the way to the interface, challenging the initial idea that the hard/soft exchange coupling is dominant in the interfacial region. Further increasing tsoftt_{soft} to 20 nm and 30 nm, the relaxation rate of magnetic configuration in the soft layer decreases, e.g. the soft layer recovers an out-of-plane orientation at the hard/soft interface. These results show a complex and nonmonotonic dependence of the soft-layer orientation on tsoftt_{soft}. For completeness, the dependence of the magnetic relaxation on thardt_{hard} was also investigated in the case of Mssoft=Mshard=700M_s^{soft}=M_s^{hard}=700 kA/m, shown in Figure 4b. Increasing thardt_{hard} does not significantly impact the magnetic configuration in the soft layer, indicating that the interfacial exchange interaction dominates the interaction between hard and soft layers.

OOMMF simulation plots of out-of-plane magnetization

Figure 4. OOMMF simulation for the out-of-plane magnetization for (a) Mshard=900M_s^{hard}=900 kA/m and Mssoft=300M_s^{soft}=300 kA/m and thard=4t^{hard}=4 nm with tsoft=(2,5,9,20,30)t^{soft}=(2, 5, 9, 20, 30) nm (b) Mshard=700M_s^{hard}=700 kA/m and Mssoft=700M_s^{soft}=700 kA/m and tsoft=9t^{soft}=9 nm with thard=(4,9,15,20,30)t^{hard}=(4, 9, 15, 20, 30) nm, (c) Mshard=700M_s^{hard}=700 kA/m and Mssoft=(300,500,700,1000,1700)M_s^{soft}=(300, 500, 700, 1000, 1700) kA/m (d) Mssoft=500M_s^{soft}=500 kA/m and Mshard=(300,500,700,1000,1300)M_s^{hard}=(300, 500, 700, 1000, 1300) kA/m, where thard=4t^{hard}=4 nm and tsoft=9t^{soft}=9 nm

These results show a tsoftt_{soft} dependent and non-thardt_{hard} related magnetic relaxation: for tsoft<lext_{soft}<l_{ex}, the hard and soft layers are rigidly exchange coupled, while for thicker tsoftt_{soft}, the soft layer relaxes in-plane with a relaxation rate which decreases as increasing tsoftt_{soft}. The next set of simulations explore the role of MssoftM_s^{soft} and MshardM_s^{hard} in determining the magnetic bilayer configuration while fixing tsoftt_{soft} and thardt_{hard}. For a fixed Mshard=700M_s^{hard}=700 kA/m, MssoftM_s^{soft} is varied between (300-1700) kA/m, and the out-of-plane magnetization is shown in Figure 4c. Increasing MssoftM_s^{soft} significantly accelerates the in-plane relaxation of the magnetic soft layer. This acceleration can be seen by evaluating the distance from the hard/soft interface at which the soft layer relaxes in-plane. For Mssoft=300M_s^{soft}=300 kA/m, this distance is >30 nm, while for Mssoft=1700M_s^{soft}=1700 kA/m this distance is only 2 nm. In contrast, models with a fixed MssoftM_s^{soft} and variable MshardM_s^{hard} between 300 kA/m and 1300 kA/m, Figure 4d, show comparably little change. The bilayer simulations show generally that increasing MshardM_s^{hard} causes the in-plane relaxation to occur over a larger thickness, e.g. the out-of-plane component of the soft-layer magnetization extends further from the hard/soft interface.

These simulations agree with the experimental results. For example, in the FePt/Fe(9 nm) sample the soft-layer was almost fully in-plane, in strong contrast with the [Co/Pd]/CoPd(9 nm) sample which was about fully out-of-plane. The simulations would suggest that the differences in the hard layer have little effect, while the MssoftM_s^{soft} dominates the magnetic configuration. Indeed, with a much-larger MssoftM_s^{soft}, Fe (Mssoft=1700M_s^{soft}=1700 kA/m) is expected to be in-plane, while CoPd (Mssoft≈750M_s^{soft}\approx750 kA/m) could remain out of plane.

Conclusion

In summary, we have investigated magnetic configurations in perpendicularly-coupled hard/soft bilayer films as a function of their geometric structure (tsoftt_{soft}), material properties (MssoftM_s^{soft} and MshardM_s^{hard}) and external influences (HipH_{ip} and TT). Using polarized neutron reflectometry, the depth profiles for these coupled systems are experimentally determined and compared to micromagnetic simulations. For very thin tsoftt_{soft}, on the order of lexl_{ex}, the magnetic moments in the soft layer are rigidly coupled to the hard layer throughout their entire thickness, while for thicker tsoftt_{soft} the magnetic moments in the soft layer tend to relax in plane. Surprisingly, the in-plane relaxation extends into regions which were oriented in the out-of-plane direction for smaller tsoftt_{soft}, indicating the relaxation is not simply progressive with increasing tsoftt_{soft}. The in-plane relaxation is also shown to be dependent on MssoftM_s^{soft}, with increasing MssoftM_s^{soft} significantly increasing its rate. These results are directly demonstrated in [Co/Pd]/CoPd, [Co/Pt]/FeNi, L10\mathrm{L1_0}-FePt/Fe, and L10\mathrm{L1_0}-FePt/A1\mathrm{A1}-FePt bilayer films using PNR, then confirmed by micromagnetic simulations. Moreover, the simulation results suggest that increasing MshardM_s^{hard} decreases the relaxation rate in the soft layer, while changes in thardt_{hard} may not significantly influence the magnetic configuration. PNR experiments also reveal the importance of HipH_{ip} and TT on the magnetic configuration. Specifically for the L10\mathrm{L1_0}-FePt/A1\mathrm{A1}-FePt system, increasing HipH_{ip} or decreasing TT results in an overall increase of the in-plane magnetization. This result corresponds to the temperature-dependent balance of the magnetocrystalline anisotropy and the magnetostatic energy. Meanwhile, increasing HipH_{ip} causes the measured lintl_{int} to increase, while increasing TT leaves lintl_{int} almost unchanged. The PNR and simulation results together show that the magnetic configuration in the bilayer samples can be modulated by varying tsoftt_{soft}, MshardM_s^{hard} and MssoftM_s^{soft} as well as HipH_{ip} and TT. Understanding the impact of these parameters is critical for the design of hard/soft bilayer devices.

Acknowledgement

This material is based upon work supported by the U.S. Department of Energy, Office of Science, Office of Basic Energy Sciences Energy Early Career Research Program under Award Number DE-SC0021344. Work at G.U. has been supported by the NSF (ECCS- 1933527).

Supplementary materials

PNR measurements are also performed on [Co/Pd]-multilayers/CoPd with tsoft=2t_{soft}=2 nm and 5 nm. The samples are first saturated with 500 mT magnetic field along film normal direction, and then reduce to 0. An in-plane guide field 1 mT was applied while measuring. The reflectivity of R++\mathrm{R}^{++} and R−−\mathrm{R}^{--} are largely overlapped with each other for tsoft=2t_{soft}=2 (Figure S1 a and b), which indicates there is not net in plane magnetization. This is then proved by converged magnetic depth profiles that no net MSLD can be probed. This non-in-plane magnetic behavior is also probed in tsoft=5t_{soft}=5 nm (Figure S1 c and d).

With the same experimental set up on the above, PNR measurements and the model fitting on [Co/Pt]/FeNi with tsoft=0t_{soft}=0, 1 and 3 nm are shown in Figure S2 (a, b), (c,d) and (e,f), respectively. For each tsoftt_{soft}, R++\mathrm{R}^{++} and R−−\mathrm{R}^{--} are largely converged with each other and the corresponding magnetic depth profile presents no MSLD. These results indicate that the magnetization in the soft layer is along the perpendicular anisotropy orientation.

Figures

References

  1. [1]E. F. Kneller and R. Hawig, IEEE Trans. Magn. 27, 3588 (1991).
  2. [2]E. E. Fullerton, J. S. Jiang, M. Grim­sditch, C. H. Sowers, and S. D. Bader, Phys. Rev. B 58, 12193 (1998).
  3. [3]J. S. Jiang, E. E. Fullerton, C. H. Sowers, A. Inomata, S. D. Bader, A. J. Shapiro, R. D. Shull, V. S. Gornakov, and V. I. Nikitenko, IEEE Trans. Magn. 35, 3229 (1999).
  4. [4]L. H. Lewis, J. Kim, K. Barmak, and D. C. Crew, J. Phys. D: Appl. Phys. 37, 2638 (2004).
  5. [5]J. E. Davies, O. Hellwig, E. E. Fullerton, J. S. Jiang, S. D. Bader, G. T. Zimanyi, and K. Liu, Appl. Phys. Lett. 86, 262503 (2005).
  6. [6]Y. Sonobe, D. Weller, Y. Ikeda, K. Takano, M. Schabes, G. Zeltzer, H. Do, B. Yen, and M. Best, J. Magn. Magn. Mater. 235, 424 (2001).
  7. [7]Y. Sonobe et al., IEEE Trans. Magn. 37, 1667 (2001).
  8. [8]Y. Sonobe et al., IEEE Trans. Magn. 38, 2006 (2002).
  9. [9]R. H. Victora and X. Shen, IEEE Trans. Magn. 41, 2828 (2005).
  10. [10]J. P. Wang, W. K. Shen, and J. M. Bai, IEEE Trans. Magn. 41, 3181 (2005).
  11. [11]G. Choe, M. Zheng, B. Acharya, E. Abarra, and J. Zhou, IEEE Trans. Magn. 41, 3172 (2005).
  12. [12]D. Suess, Appl. Phys. Lett. 89, 113105 (2006).
  13. [13]Y. Shiroishi, K. Fukuda, I. Tagawa, H. Iwasaki, S. Takenoiri, H. Tanaka, H. Mutoh, and N. Yoshikawa, IEEE Trans. Magn. 45, 3816 (2009).
  14. [14]B. J. Kirby, J. E. Davies, K. Liu, S. M. Watson, G. T. Zimanyi, R. D. Shull, P. A. Kienzle, and J. A. Borchers, Phys. Rev. B 81, 100405 (2010).
  15. [15]D. Suess, C. Vogler, C. Abert, F. Bruckner, R. Windl, L. Breth, and J. Fidler, J. Appl. Phys. 117, 163913 (2015).
  16. [16]D. Weller, G. Parker, O. Mosendz, A. Lyberatos, D. Mitin, N. Y. Safonova, and M. Albrecht, J. Vac. Sci. Technol. B 34, 060801 (2016).
  17. [17]W. Zhu, K. Gao, and E. Gage, (Google Patents, 2016).
  18. [18]H. Yang, T. Ye, Y. Lin, M. Liu, G. Zhang, and P. Kang, Mater. Lett. 145, 19 (2015).
  19. [19]D. Roy and P. A. Kumar, J. Appl. Phys. 106, 073902 (2009).
  20. [20]A. Quesada et al., Adv. Electron. Mater. 2, 1500365 (2016).
  21. [21]D. Litvinov, M. H. Kryder, and S. Khizroev, J. Magn. Magn. Mater. 232, 84 (2001).
  22. [22]T. Suzuki, Z. Zhang, A. K. Singh, J. Yin, A. Perumal, and H. Osawa, IEEE Trans. Magn. 41, 555 (2005).
  23. [23]J. W. Liao et al., Phys. Rev. B 82, 014423 (2010).
  24. [24]A. Q. Wu et al., IEEE Trans. Magn. 49, 779 (2013).
  25. [25]R. E. Rottmayer et al., IEEE Trans. Magn. 42, 2417 (2006).
  26. [26]D. A. Gilbert, L. W. Wang, T. J. Klemmer, J. U. Thiele, C. H. Lai, and K. Liu, Appl. Phys. Lett. 102, 132406 (2013).
  27. [27]D. Goll and S. Macke, Appl. Phys. Lett. 93, 152512 (2008).
  28. [28]F. Casoli, F. Albertini, L. Nasi, S. Fabbrici, R. Cabassi, F. Bolzoni, and C. Bocchi, Appl. Phys. Lett. 92, 142506 (2008).
  29. [29]H. Zeng, J. Li, J. P. Liu, Z. L. Wang, and S. H. Sun, Nature 420, 395 (2002).
  30. [30]E. E. Fullerton, J. Jiang, and S. Bader, J. Magn. Magn. Mater. 200, 392 (1999).
  31. [31]G. Asti, M. Ghidini, R. Pellicelli, C. Pernechele, M. Solzi, F. Albertini, F. Casoli, S. Fabbrici, and L. Pareti, Phys. Rev. B 73, 094406 (2006).
  32. [32]D. A. Gilbert, J.-W. Liao, B. J. Kirby, M. Winklhofer, C.-H. Lai, and K. Liu, Sci. Rep. 6, 32842 (2016).
  33. [33]A. Zambano, H. Oguchi, I. Takeuchi, Y. Choi, J. Jiang, J. Liu, S. Lofland, D. Josell, and L. A. Bendersky, Phys. Rev. B 75, 144429 (2007).
  34. [34]G. Lavorato, E. Winkler, B. Rivas-Murias, and F. Rivadulla, Phys. Rev. B 94, 054405 (2016).
  35. [35]D. Suess, T. Schrefl, S. Fähler, M. Kirschner, G. Hrkaç, F. Dorfbauer, and J. Fidler, Appl. Phys. Lett. 87, 012504 (2005).
  36. [36]L. Pan and D. B. Bogy, Nat. Photonics 3, 189 (2009).
  37. [37]M. H. Kryder, E. C. Gage, T. W. McDaniel, W. A. Challenger, R. E. Rottmayer, G. Ju, Y.-T. Hsia, and M. F. Erden, Proc. IEEE 96, 1810 (2008).
  38. [38]M. Kief and R. Victora, MRS Bulletin 43, 87 (2018).
  39. [39]B. C. S. Varaprasad, M. Chen, Y. Takahashi, and K. Hono, IEEE Trans. Magn. 49, 718 (2013).
  40. [40]A. Y. Dobin and H. Richter, Appl. Phys. Lett. 89, 062512 (2006).
  41. [41]J.-W. Liao, K.-F. Huang, L.-W. Wang, W.-C. Tsai, W.-C. Wen, C.-C. Chiang, H.-J. Lin, F.-H. Chang, and C.-H. Lai, Appl. Phys. Lett. 102, 062420 (2013).
  42. [42]P. K. Greene, J. Osten, K. Lenz, J. Fassbender, C. Jenkins, E. Arenholz, T. Endo, N. Iwata, and K. Liu, Appl. Phys. Lett. 105, 072401 (2014).
  43. [43]J. E. Davies, O. Hellwig, E. E. Fullerton, G. Denbeaux, J. Kortright, and K. Liu, Phys. Rev. B 70, 224434 (2004).
  44. [44]D. A. Gilbert, J. W. Liao, L. W. Wang, J. W. Lau, T. J. Klemmer, J. U. Thiele, C. H. Lai, and K. Liu, APL Mater. 2, 086106 (2014).
  45. [45]B. J. Kirby, P. A. Kienzle, B. B. Maranville, N. F. Berk, J. Krycka, F. Heinrich, and C. F. Majkrzak, Curr. Opin. Colloid. Interface. Sci. 17, 44 (2012).
  46. [46]D. A. Gilbert, B. B. Maranville, A. L. Balk, B. J. Kirby, P. Fischer, D. T. Pierce, J. Unguris, J. A. Borchers, and K. Liu, Nature Communications 6, 8462 (2015).
  47. [47]M. J. Donahue and D. G. Porter, OOMMF User's Guide, Interagency Report NISTIR 6376, 1999.
  48. [48]Y. Zhu, Application of polarized neutron reflectometry to studies of artificially structured magnetic materials (Springer Science & Business Media, 2005), p. 107.DOI
  49. [49]Z.-P. Li, O. Petracic, R. Morales, J. Olamit, X. Battle, K. Liu, and I. K. Schuller, Phys. Rev. Lett. 96, 217205 (2006).
  50. [50]A. Belemuk and S. T. Chui, J. Appl. Phys. 113, 123906 (2013).
  51. [51]A. Belemuk and S. Chui, J. Appl. Phys. 113, 043913 (2013).
  52. [52]D. Suess, J. Lee, J. Fidler, and T. Schrefl, J. Magn. Magn. Mater. 321, 545 (2009).

Paper details

vlnc:W_ry4k43gw
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents