Magnetic anisotropy driven by ligand in 4d transition metal oxide SrRuO3

Abstract

The origin of magnetic anisotropy in magnetic compounds is a longstanding issue in solid state physics and nonmagnetic ligand ions are considered to contribute little to magnetic anisotropy. Here, we introduce the concept of ligand driven magnetic anisotropy in a complex transition-metal oxide. We conducted X ray absorption and X ray magnetic circular dichroism spectroscopies at the Ru and O edges in the 4d ferromagnetic metal SrRuO3. Systematic variation of the sample thickness in the range below 10 nm allowed us to control the localization of Ru 4d t2g states, which affects the magnetic coupling between the Ru and O ions. We found that the orbital magnetization of the ligand induced via hybridization with the Ru 4d orbital determines the magnetic anisotropy in SrRuO3.

Magnetic anisotropy that confers a preferred direction on the spin of a system is one of the most important properties of magnetic materials. Over the long history of studies on magnetic materials, various origins have been suggested for magnetic anisotropy: magnetic multipoles [1,2], electric quadrupole [3-6], and single-ion anisotropy, where the focus has been on crystal field splitting at dd- and/or ff- orbitals of transition metal elements [7-9]. Especially in magnetic oxides, such as perovskite manganites [6,10], ruthenates [11-13], spinel ferrites [14], pyrochlores [15], and their epitaxial heterostructures [16], the electric quadrupole moment due to the different dd orbital occupations and the anisotropy of the orbital magnetic moment based on the single-ion model or tight-binding model [17] have been considered to be the two main origins of magnetic anisotropy. Elucidating the origin of magnetic anisotropy in such magnetic oxides is vital for comprehending magnetism as well as utilizing spin degrees of freedom in oxide electronics [18,19].

The itinerant 4d4d ferromagnetic perovskite ruthenate SrRuO3_3 (SRO) [bulk Curie temperature (TCT_\mathrm{C}) = 165 K] has been used as a model system for understanding magnetic anisotropy in metallic oxides [20-29]. In addition, recent observations of Weyl fermions in SRO have brought renewed interest as an emergent platform for exploring quantum transport phenomena for topological oxide electronics [30-34]. In SRO films, the magnetic anisotropy is linked to epitaxial strain through the interplay between electrons (charges, spins), lattice, and orbital degrees of freedom [35-39]. Particularly, compressively strained SRO film on SrTiO3_3 (STO) (001) was the first oxide heterostructure in which perpendicular magnetic anisotropy was discovered [40]. The perpendicular magnetic anisotropy in compressively strained SRO has been considered to arise from the anisotropy of the Ru orbital magnetic moment [11-13]. However, our recent observations of the isotropic Ru orbital magnetic moment relative to the spin magnetic moment morb/mspinm_\mathrm{orb}/m_\mathrm{spin} in compressively strained SRO films contradict the conventional understanding [41]; the scenario in which magnetic anisotropy originates from an anisotropic variation in the crystal field splitting at the 4d4d orbitals of Ru due to strain [10-12] does not hold true. This implies that contributions from the ligand O 2p2p orbital should also be considered. In fact, polarized neutron scattering experiments have shown that O ions have unexpectedly large magnetic moments; the contribution to the total magnetization reaches 30% [42]. The contribution from oxygen may come from hybridization between Ru 4d4d t2gt_{2g} and O 2p2p orbitals in the itinerant system SRO. Since an increase in localization of the Ru 4d4d t2gt_{2g} states shrinks the wave function, resulting in lower hybridization strength, experiments that systematically vary the degree of localization of Ru 4d4d t2gt_{2g} states would provide cogent evidence for the oxygen ligand-driven magnetic anisotropy. A possible approach to controlling the degree of localization of Ru 4d4d t2gt_{2g} states is the introduction of interface-driven defects by controlling film thickness or an increase in the effective Coulomb interaction with dimensionality reduction [43]. The recent advances in machine-learning-assisted thin-film growth technology [44,45] have enabled systematic and precise control of the thickness of stoichiometric SRO films in the range of ≤10\leq10 nm.

In this study, we investigated the anisotropy of the Ru 4d4d and O 2p2p electronic structure and the magnetic properties of stoichiometric compressive-strained SRO films of various thicknesses tt = 1-10 nm grown on STO (001) substrates by using soft X-ray absorption spectroscopy (XAS) and X-ray magnetic circular dichroism (XMCD), which are highly sensitive to the local electronic structure and element-specific magnetic properties in magnetic materials [46-49]. By varying the localization of the Ru 4d4d t2gt_{2g} states through thickness control, we found that the perpendicular magnetic anisotropy originates from the anisotropy of the magnetic moments of O 2p2p orbitals. This finding is conceptually distinct from the conventional single-ion model that is based on the effect of the crystal field at the dd orbitals of magnetic elements.

We grew compressively strained epitaxial SRO films with a thickness tt of 1, 2, 3, 4, 5, and 10 nm on STO (001) substrates [Figure 1(a)] in a custom-designed molecular beam epitaxy (MBE) system [44]. The residual resistivity ratio (RRR) of the thickest SRO film (t=10t = 10 nm) was 21. This is high enough to observe the intrinsic quantum transport of Weyl fermions in SRO [50] and is a hallmark of the stoichiometric composition of the films [51]. The XAS and XMCD measurements were performed at the helical undulator beamline BL25SU of SPring-8 [52]. For the XMCD measurements, absorption spectra for circularly polarized X rays with the photon helicity parallel (μ+\mu^{+}) or antiparallel (μ−\mu^{-}) to the spin polarization were obtained by reversing the photon helicity at each photon energy hνh\nu and recorded in the total-electron-yield (TEY) mode. The measurement temperature was 20 K, which was low enough considering the TCT_{\mathrm{C}} of the SRO films (100-150 K) [50]. All XAS and XMCD spectroscopy measurements were performed at 1.92 T, the maximum applied magnetic field in the system [53]. To measure the perpendicular and in-plane magnetic moments, the angles of the external magnetic fields and incident X rays measured from the sample surfaces were set to θ=90∘\theta= 90^\circ and 20°, respectively [Figure 1(b) and Figure 1(c)]. The incident light was tilted at 10° to the magnetic field [53]. The details of the samples, growth conditions, and experimental set up for the XAS and XMCD measurements are described in § 5 of the Supplemental Material [54].

Schematic diagrams of the sample and crystal structures of the SRO films, with measurement configurations for perpendicular and in-plane XAS and XMCD measurements

Figure 1. Schematic diagrams of the sample and crystal structures of the SRO films. In the schematic crystal image, yellow, blue, red, and purple spheres indicate strontium, oxygen, ruthenium, and titanium, respectively. Illustrations of the measurement configurations for the (b) perpendicular and (c) in-plane XAS and XMCD measurements.

We will start with the XAS and XMCD spectra of the thickest film (10 nm) taken in the perpendicular configuration (θ=90∘\theta= 90^\circ). Figure 2(a) shows the Ru M2,3M_{2,3}-edge XAS and XMCD spectra for the SRO film with t=10t = 10 nm. The spectral features are essentially identical to what we have reported for much thicker (60-63 nm) SRO films on STO [13, 41]. The absorption peaks from the Ru 3p3/23p_{3/2} and 3p1/23p_{1/2} core levels into the Ru 4d4d states appear at around 463 and 485 eV, respectively, both in the XAS and XMCD spectra [55,56]. The details of the peak assignments of the Ru M2,3M_{2,3}-edge XAS and XMCD spectra are in § 6 of the Supplemental Material [54]. To further investigate the unoccupied electronic states hybridized with the O 2p2p orbitals and the magnetic properties of the O ions, we also measured the O KK-edge XAS and XMCD spectra of the 10-nm SRO film under the same conditions [Figure 2(b)]. The absorption peak at 529 eV arises from transitions to the Ru 4d4d t2gt_{2g} states hybridized with the O 2p2p states, while transitions to the Ru 4d4d ege_g states are observed in the energy range of 531.5-534.2 eV [57,58]. The range of 534.5-539.5 eV displays transitions to the Sr 4d4d states, and transitions to the Ru 5s5s states occur in 540-546 eV [57,58]. The intense coherent Ru 4d4d t2gt_{2g} peak [41] indicates the long lifetimes of quasiparticles in the hybridized Ru 4d4d t2gt_{2g}-O 2p2p states, which is also evidenced by observation of quantum oscillations in the resistivity of SRO film with t=10t = 10 nm [50]. A substantial orbital magnetic moment of the O 2p2p states was deduced from the O KK XMCD spectrum in the energy range corresponding to Ru 4d4d t2gt_{2g} [Figure 2(b)], indicating that spin-polarized bands crossing the Fermi level, EFE_{\mathrm{F}}, are formed by the Ru 4d4d t2gt_{2g} states hybridized with the O 2p2p states and that there was charge transfer [59] from the ligand O 2p2p orbitals to the Ru 4d4d orbitals. This interpretation is in accordance with our previous density functional theory (DFT) calculations [31], which show that the half-metallic hybridized Ru 4d4d t2gt_{2g}-O 2p2p states cross EFE_{\mathrm{F}}.

Ru M2,3-edge and O K-edge XAS and XMCD spectra

Figure 2. Ru M2,3M_{2,3}-edge XAS and XMCD spectra [(a),(c)] and O K-edge XAS and XMCD spectra [(b),(d)] for the SRO films with t=10t = 10 nm [(a),(b)] and 11 nm [(c),(d)] at 20 K under a magnetic field μ0H\mu_0 H of 1.92 T at θ=90∘\theta= 90^\circ.

Next, we turn to the tt and θ\theta dependences. When the film thickness was reduced to half (t=5t = 5 nm), similar Ru M2,3M_{2,3}- and O K-edge spectra to those above were observed Figure S1 and Figure S1 of the Supplemental Material [54]. Upon decreasing the film thickness (t≤4t \le4 nm) further, absorptions from the STO substrate [60] became prominent Figure 2(c) and Figure 2(d) for t=1t = 1 nm, Figure S1-Figure S1 and Figure S1-Figure S1 of the Supplemental Material [54] for t=2t = 2-4 nm. As in the Ru M2,3M_{2,3}-edge XAS spectrum for t=1t = 1 nm, the Ti L2,3L_{2,3}-edge absorptions were convoluted over the Ru M2,3M_{2,3} edges Figure 2(c). Similarly, the O K-edge XAS spectra for t=1t = 1 nm showed absorptions from the STO substrate, such as the absorption peak at 530.7 eV arising from transitions from O 1s states to the Ti 3d3d t2gt_{2g} states Figure 2(d) [60]. Nonetheless, the Ru M2,3M_{2,3}-edge and O K-edge XMCD could selectively extract information on the SRO films, since the Ti ions in the STO substrates are nonmagnetic. The Ru M2,3M_{2,3}-edge XMCD spectra normalized at the Ru M2M_2-edge XMCD peak taken at θ=90∘\theta= 90^\circ are plotted in Figure 3(a), in order to see the evolution of the morb/mspinm_{\mathrm{orb}}/m_{\mathrm{spin}} ratio with tt. From the XMCD sum rules, morb/mspinm_{\mathrm{orb}}/m_{\mathrm{spin}} ratio is determined solely from the ratio of the M3M_3-edge to M2M_2-edge XMCD absorption intensities see Sec. IV of the Supplemental Material [54]. The spectra almost completely overlap, indicating that the Ru4+^{4+} 4d4d states have a common morb/mspinm_{\mathrm{orb}}/m_{\mathrm{spin}} ratio (0.081), as estimated from the XMCD sum rules [46,47,48], irrespective of tt. This is in contrast to the case of SRO thin films prepared by pulsed-laser deposition (PLD), where ultrathin (1-2 nm) films became paramagnetic and showed a significant change in electronic structure [12]. This discrepancy may have arisen from the inevitable formation of Ru vacancies in the PLD-grown films [61]. We also compared the normalized Ru M2,3M_{2,3}-edge XMCD spectra for different θ\theta (90∘90^\circ and 20∘20^\circ) and found that they were identical, as exemplified by the data for the t=2t = 2 nm film in Figure 3(a). Altogether, the tt and θ\theta dependencies of XMCD indicate that the electronic structure and orbital magnetic moment are isotropic within the Ru4+^{4+} states.

Four-panel spectra and thickness-dependence plots

Figure 3. (a) Ru M2,3M_{2,3}-edge XMCD spectra normalized at the Ru M2M_2-edge XMCD peak for the SRO films with t=1t = 1-10 nm at θ=90∘\theta= 90^\circ or θ=20∘\theta= 20^\circ. (b) O KK-edge XAS spectra normalized at 529.5 eV for the SRO films with t=1t = 1-10 nm at θ=90∘\theta= 90^\circ after subtracting the absorption from the STO substrate. (c) Thickness dependence of the Ru 4d4d t2gt_{2g} peak in the O KK-edge XAS spectrum normalized at 529.5 eV, ratio of the XMCD intensity to the XAS intensity of the Ru M2M_2 edge peak at θ=90∘\theta= 90^\circ, and ratio of the XMCD intensity to the XAS intensity of the O KK-edge Ru 4d4d t2gt_{2g} peak at θ=90∘\theta= 90^\circ. (d) The ratios of the XMCD/XAS intensity at θ=20∘\theta= 20^\circ to that at θ=90∘\theta= 90^\circ. All measurements were performed at 20 K under a magnetic field μ0H\mu_0H of 1.92 T.

Ru M2,3-edge and O K-edge XAS and XMCD spectra for SRO films

Figure S1. (a)-(d) Ru M2,3M_{2,3}-edge XAS and XMCD spectra for the SRO films with t=(a)t = (a) 5, (b)(b) 4, (c)(c) 3, and (d)(d) 2 nm at 20 K under a magnetic field μ0H\mu_0H of 1.92 T at θ=90∘\theta= 90^\circ. (e)-(h) O KK-edge XAS and XMCD spectra for the SRO films with t=(e)t = (e) 5, (f)(f) 4, (g)(g) 3, and (h)(h) 2 nm.

Now that the magnetic anisotropy in SRO tuned out not to arise from the supposed anisotropy in the orbital magnetic moment of Ru, the key to clarifying the origin of the magnetic anisotropy becomes estimating the individual magnetic moments of Ru and O themselves. In XMCD measurements, the magnetic moments of each element are proportional to the ratios of XMCD to XAS intensities of the particular absorption peaks. However, the presence of absorptions from the STO substrates in the XMCD spectra for the SRO films with t=1t = 1-4 nm prevented a quantitative evaluation of the variation in the magnetic moment with film thickness and direction of the applied magnetic field. To overcome this difficulty, we developed an analytical procedure to subtract the signals from the substrate. The details of the deconvolution procedure and examples of using it on the XAS spectra of SRO film are described in § 9 of the Supplemental Material [54].

Using the O K-edge XAS spectra inherent to each thickness, we revealed that the intensity of the coherent Ru 4d4d t2gt_{2g} peak decreases with decreasing tt Figure 3(b), indicating that the lifetimes of the quasiparticles in the hybridized Ru 4d4d t2gt_{2g}-O 2p2p states become shorter and the localization of the Ru 4d4d t2gt_{2g} states become stronger due to disorder-induced localization near the interface or an increase in the effective Coulomb interaction with dimensionality reduction [62,63]. Here, the O KK-edge XAS spectra were normalized at the energy, where coherent absorption is reduced and incoherent absorption begins. The increase in the localization of the Ru 4d4d t2gt_{2g} states shrinks the wave function, resulting in weaker hybridization. The reduction in peak intensity became prominent when tt was reduced from 2 nm to 1 nm, which is consistent with the change in the global transport properties [50]: metallicity was barely observed in the SRO film with t=1t = 1 nm, while localization was noticeable at 20 K, the measurement temperature of XAS in this study.

Figure 3(c) shows the thickness dependence of the ratios of the XMCD intensity to the XAS intensity of the Ru M2M_2 and O KK-edge Ru 4d4d t2gt_{2g} peaks at θ=90∘\theta= 90^\circ, which are proportional to the magnetic moments of Ru and O ions, respectively. Note that XMCD at the KK edges is only able to probe the orbital magnetic moment [46]. The orbital magnetic moment of oxygen (red circles) decreases with decreasing tt. This trend coincides well with that of the O KK-edge Ru 4d4d t2gt_{2g} peak intensity (blue triangles), suggesting that the magnetic moment of oxygen decreases as a result of reduced charge transfer through orbital hybridization. In addition, the magnetic moment of Ru (green circles) decreases significantly below 2 nm, indicating that the Ru 4d4d t2gt_{2g}-O 2p2p hybridization is also important for the ferromagnetic ordering of Ru. Note that the conclusion of weakened ferromagnetic ordering in SRO films with t≤2t \leq2 nm is supported by the thickness-dependent Curie temperature (TCT_{\mathrm{C}}) determined from transport measurements [51]. To investigate the change in magnetic anisotropy of Ru and O ions with respect to the Ru 4d4d t2gt_{2g}-O 2p2p hybridization, we compared the ratios of the XMCD intensity to the XAS intensity in the perpendicular configuration (θ=90∘\theta= 90^\circ) and in the in-plane configuration (θ=20∘\theta= 20^\circ) [Fig. 3(d)]. All the XAS and XMCD spectra with t=1t = 1-10 nm at θ=20∘\theta= 20^\circ for extracting the data points in Figure 3(d) are in Figure S2 of the Supplemental Material [54]. The ratio represents the in-plane/perpendicular magnetization ratio rr, which means the magnetic moment has perpendicular magnetic anisotropy when rr is less than 1. For t≥3t \geq3 nm, except for t=5t = 5 nm, rr was 0.4-0.6 for Ru and O. Only t=5t = 5 nm showed a slightly weaker perpendicular magnetic anisotropy, with rr being 0.7-0.8 for Ru and O. Although there were variations in the magnitude of the magnetic anisotropy from sample to sample, the rr values for Ru and O were almost the same at each thickness, indicating that Ru and O had the same magnetic anisotropy and were magnetically coupled. Notably, the magnetic anisotropies of Ru and O were different in the SRO films with t=1t = 1 and 2 nm; O had an rr of about 0.7, while Ru had an rr of about 1.0, i.e., no magnetic anisotropy. As described earlier, the orbital hybridization became stronger in the range t≥3t \geq3 nm. The perpendicular magnetic anisotropy of Ru for t≥3t \geq3 nm is considered to be due to the magnetic coupling between O and Ru through orbital hybridization. In other words, the perpendicular magnetic anisotropy of SRO is due to not the Ru orbitals but rather the O orbitals and is induced through the Ru 4d4d t2gt_{2g}-O 2p2p orbital hybridization. Changes in the magnetic properties of Ru for the SRO film with t=1t = 1 and 2 nm were also found by studying the Ru M3M_3-edge XMCD-μ0H\mu_0H curves [see Sec. VI] of the Supplemental Material [54].

Ru M₂,₃-edge and O K-edge XAS and XMCD spectra for SRO films

Figure S2. (a)–(f) Ru M2,3M_{2,3}-edge XAS and XMCD spectra for the SRO films with tt = (a) 10, (b) 5, (c) 4, (d) 3, (e) 2 and (f) 1 nm at 20 K under a magnetic field μ0H\mu_0 H of 1.92 T at θ\theta = 20°. (g)–(l) O KK-edge XAS and XMCD spectra for the SRO films with tt = (g) 10, (h) 5, (i) 4, (j) 3, (k) 2 and (l) 1 nm.

Conventionally, the magnetic anisotropy in SRO films has been interpreted in terms of a strain-induced anisotropic variation in the crystal field splitting at the dd orbitals of Ru (single-ion picture) [10-12]. Such an interpretation contradicts the new finding in this study that the magnetic anisotropy is driven by oxygen ligands. The magnetic moment of Ru4+\mathrm{Ru}^{4+} ions also shows the breakdown of the single-ion model, as follows. In the case of a large crystal field splitting, Ru4+\mathrm{Ru}^{4+} ions are expected to be in a low-spin state with an electron configuration of t2g4t_{2g}^{4} (3↑, 1↓) corresponding to 2 μB/Ru4+2\ \mu_{\mathrm{B}}/\mathrm{Ru}^{4+} ions [11,23]. However, the total magnetic moment, mtotal=mspin+morbm_{\mathrm{total}} = m_{\mathrm{spin}} + m_{\mathrm{orb}}, estimated from the XAS and XMCD spectra in Figure 2(a) by using the XMCD sum rules [46-48] is 0.71 μB/Ru4+0.71\ \mu_{\mathrm{B}}/\mathrm{Ru}^{4+}, indicating a limitation to the local picture. Recently, polarized neutron diffraction measurements on bulk SRO were used to observe the cubic faces of the Ru spin density distribution and the disk-shaped O spin density distribution, both perpendicular to the Ru 4d t2g4d\ t_{2g}-O 2p2p bonds [42]; the results suggested that, for the Ru-O bond along the xx direction, the dxyd_{xy} and dxzd_{xz} form π\pi bonds with oxygen pyp_y and pzp_z orbitals, respectively. A possible origin of the ligand-driven magnetic anisotropy found in this study is a strain-induced change in such anisotropic spin distributions at the O ions. It has been widely acknowledged that Ru 4d t2g4d\ t_{2g}-O 2p2p hybridization, as is evidenced by the intense coherent O KK-edge Ru 4d t2g4d\ t_{2g} peak [Fig. 4(a)], is the key to ferromagnetism and metallicity emerging in SRO [31,64]. The present study indicates that it is also the case for magnetic anisotropy.

Recently, magnetic moments of nonmagnetic ligand induced by charge transfer through the orbital hybridization from 3d3d or 5d5d orbitals were measured in the 3d3d and 5d5d ferromagnetic compounds [65,66], confirming the significant contribution of ligands to the ferromagnetism in 3d3d and 5d5d systems. Exploring the existence of ligand-driven magnetic anisotropy even in such 3d3d and 5d5d systems would be crucial for universal understanding of the origin of magnetic anisotropy. In systems where magnetic moments are induced in nonmagnetic ligands through pp-dd hybridization, ligand-driven magnetic anisotropy could dominate the magnetic anisotropy.

In conclusion, a new type of magnetic anisotropy, ligand-driven magnetic anisotropy, has been discovered in 4d4d ferromagnetic Weyl semimetal SRO by making XAS and XMCD measurements. Systematic variation of the film thickness in the range of ≤10\leq10 nm for controlling the localization of the Ru 4d t2g4d\ t_{2g} states revealed that the magnetic moments of the nonmagnetic ligand (O) are induced by charge transfer through the orbital hybridization from Ru 4d4d orbitals, and the anisotropy of the ligand determines the magnetic anisotropy of SRO. The ligand-driven magnetic anisotropy is distinct from the conventional single-ion model dominated by the effects of the crystal field splitting at the dd orbitals of magnetic elements. Since this new concept can be extended to other magnetic materials, further theoretical calculations and experimental investigations on element-specific electronic structures near heterointerfaces are encouraged in order to elucidate the mechanism behind the emergence of anisotropy in the ligand.

Acknowledgments

This work was supported by a Grants-in-Aid (Grants No. 22H04948), of the Japan Science and Technology Agency. This work was partially supported by the Spintronics Research Network of Japan (Spin-RNJ). The synchrotron radiation experiments were performed at the BL25SU of SPring-8 with the approval of the Japan Synchrotron Radiation Research Institute (JASRI) (Proposals No. 2022B1403 and No. 2023A1369).

AUTHORS' CONTRIBUTIONS

Y.K.W. and M. Kobayashi conceived the idea, designed the experiments, and directed and supervised the project. M. Kobayashi and Y.K.W. planned the synchrotron experiments. Y.K.W. and Y. Krockenberger grew the samples. Y.K.W. carried out the sample characterizations. Y.K.W., M. Kobayashi, Y.S., Y. Kotani, T.O., K.Y., and M. Kitamura carried out the XMCD measurements. Y.K.W. analyzed and interpreted the data. Y.K.W. wrote the paper with input from all authors.

DATA AVAILABILITY

The data that support the findings of this study are available from the corresponding authors upon reasonable request.

Figures and figure captions

*Corresponding author: [email protected]

Samples, growth conditions, and experimental set up for XAS and XMCD measurements

Epitaxial growth of the SRO films was confirmed by the sharp streaky reflection high energy electron diffraction patterns [49]. The growth parameters were optimized by Bayesian optimization, a machine learning technique [44]. All SRO films were prepared under the same growth conditions as in Refs. [67] [50, 51], in which the thickness-dependent magnetic and electrical properties together with crystallographic analyses of the SRO films were also reported. The growth rate of 1.05 Å/s was deduced from the thickness calibration of the film using cross-sectional scanning transmission electron microscopy. Further information about the MBE setup and preparation of the substrates is available elsewhere [24]. The residual resistivity ratio (RRR) of the thickest SRO film (t=10t = 10 nm) was 21. This was high enough to observe the intrinsic quantum transport of Weyl fermions in SRO [50], such as quantum oscillations of the high mobility carriers from the bulk three-dimensional Weyl fermions [31] and two-dimensional Weyl fermions from surface Fermi arcs [32], and it is a hallmark of the stoichiometric composition of the films. The availability of such stoichiometric SRO films with precise thicknesses in the range of ≤10\le10 nm allows for systematic investigation of the coherent Ru 4d4d t2gt_{2g}–O 2p2p hybridized states and magnetic anisotropy of Ru and O ions while the degree of hybridization is being varied.

XAS and XMCD are the tools of choice for investigating the electronic structures and element-specific magnetic properties of magnetic materials [68, 69]. The monochromator resolution E/ΔEE/\Delta E was over 10,000. The designed beam spot size was 10×10010 \times100–200 μm2200\,\mu\mathrm{m}^{2}. For the XMCD measurements, absorption spectra for circularly polarized X rays with the photon helicity parallel (μ+\mu^{+}) or antiparallel (μ−\mu^{-}) to the spin polarization were obtained by reversing the photon helicity at each photon energy hνh\nu and recording them in the total-electron-yield (TEY) mode. The μ+\mu^{+} and μ−\mu^{-} spectra at the Ru M2,3M_{2,3} edges and O KK edge were taken under both positive and negative applied magnetic fields and averaged to eliminate spurious dichroic signals. In order to estimate the integrated values of the XAS spectra at the Ru M2,3M_{2,3} edges, hyperbolic tangent functions as background were subtracted from the spectra.

Details of the peak assignments of the Ru M2,3M_{2,3}-edge XAS and XMCD spectra for the SRO film with t=10t = 10 nm

Figure 2(a) in the main text shows the Ru M2,3M_{2,3}-edge XAS and XMCD spectra for the SRO film with t=10t = 10 nm. The absorption peaks from the Ru 3p3/23p_{3/2} and 3p1/23p_{1/2} core levels into the Ru 4d4d states appeared at around 463 and 485 eV, respectively, both in the XAS and XMCD spectra [55,56]. The absorption peaks at 477.5 eV (Ru 3p3/2→3p_{3/2} \rightarrow Ru 5s) and 499 eV (Ru 3p1/2→3p_{1/2} \rightarrow Ru 5s) which were observed in only XAS can be assigned to the Ru 5s states having no spin polarization [55,56]. The Ru M3M_3-edge XMCD peaks are observed at lower energies than the corresponding Ru M3M_3-edge XAS peaks. While the Ru M3M_3-edge XAS and XMCD peaks arise from transitions to unoccupied Ru 4d4d t2gt_{2g} and ege_g states [55], the different peak positions between the XAS and XMCD peaks can be explained assuming that only the Ru 4d4d t2gt_{2g} states crossing the Fermi level (EFE_\mathrm{F}) exhibit spin polarization. This interpretation is in accordance with our previous Ru M2,3M_{2,3} XMCD studies [13] and density functional theory (DFT) calculations [31], which show that the half-metallic Ru 4d4d t2gt_{2g} states cross EFE_\mathrm{F}.

Ru M2,3M_{2,3}-edge and O KK-edge XAS and XMCD spectra for the SRO films with t=1t = 1-10 nm at θ=90∘\theta= 90^\circ and θ=20∘\theta= 20^\circ

XMCD sum rules for estimating morb/mspinm_{\mathrm{orb}}/m_{\mathrm{spin}}

According to the XMCD sum rules, the orbital magnetic moment morbm_{\mathrm{orb}} and the spin magnetic moment mspinm_{\mathrm{spin}} of the Ru4+^{4+} 4d4d states are described as follows [46-48]:

morb=−4(10−n4d)3r∫M2+M3(μ+−μ−)dE,(1)m_{\mathrm{orb}}=-\frac{4(10-n_{4d})}{3r}\int_{M_2+M_3}(\mu^+-\mu^-)\mathrm{d}E, \tag*{(1)}
mspin+mT=−2(10−n4d)r[∫M3(μ+−μ−)dE−2∫M2(μ+−μ−)dE].(2)m_{\mathrm{spin}}+m_T=-\frac{2(10-n_{4d})}{r}\left[\int_{M_3}(\mu^+-\mu^-)\mathrm{d}E-2\int_{M_2}(\mu^+-\mu^-)\mathrm{d}E\right]. \tag*{(2)}

Here, r=∫M2+M3(μ++μ−)dEr=\int_{M_2+M_3}(\mu^++\mu^-)\mathrm{d}E, and n4dn_{4d} is the number of electrons in 4d4d orbitals, which is assumed to be four. For ions in octahedral symmetry, the magnetic dipole moment mTm_T is a small number and can be neglected compared to mspinm_{\mathrm{spin}} [70]. By dividing equation (S1) by equation (S2), morb/mspinm_{\mathrm{orb}}/m_{\mathrm{spin}} is expressed by

morbmspin=32∫M3(μ+−μ−)dE−2∫M2(μ+−μ−)dE∫M2+M3(μ+−μ−)dE.(3)\frac{m_{\mathrm{orb}}}{m_{\mathrm{spin}}}=\frac{3}{2}\frac{\int_{M_3}(\mu^+-\mu^-)\mathrm{d}E-2\int_{M_2}(\mu^+-\mu^-)\mathrm{d}E}{\int_{M_2+M_3}(\mu^+-\mu^-)\mathrm{d}E}. \tag*{(3)}

Thus, we can obtain morb/mspinm_{\mathrm{orb}}/m_{\mathrm{spin}} directly from the XMCD spectra without an assumption of the n4dn_{4d} value.

Deconvolution of the XAS spectra to subtract signals from the substrate

Figure S3 and Figure S3 show examples of the deconvolution procedure of the XAS spectra for the SRO film with t=3t=3 nm at θ=90∘\theta=90^\circ. The procedure consists of two steps. First, to estimate the contribution of the STO substrate to the XAS spectrum, the raw XAS spectrum (red curves) is fitted by a weighted sum of the XAS spectrum for a pristine STO substrate (black dashed curves) and that for the SRO film with t=10t=10 nm, free from the substrate signals (blue dashed curves). Then, subtraction of the substrate spectrum in accordance with the weighting provides the XAS spectrum inherent to the 3-nm-thick SRO film (black curves). The examples of the deconvolution procedure for the SRO film with t=2t=2 nm at θ=20∘\theta=20^\circ are also shown in Figure S3 and Figure S3.

Ru M2,3-edge and O K-edge XAS spectra for SRO films and the STO substrate

Figure S3. Ru M2,3M_{2,3}-edge XAS spectra for the SRO films with t=10t = 10 nm (blue dashed curves) and 3 nm (red curve) and for the STO substrate (black dashed curve) at 20 K under a magnetic field μ0H=1.92\mu_{0}H = 1.92 T at θ=90∘\theta= 90^\circ. (b) O KK-edge XAS spectra for the SRO films with t=10t = 10 nm (blue dashed curve) and 3 nm (red curve) and for the STO substrate (black dashed curve) at 20 K under a magnetic field μ0H\mu_{0}H of 1.92 T at θ=90∘\theta= 90^\circ. The red dashed curves in (a) and (b) are the weighted sum of the XAS spectra for the SRO film with t=10t = 10 nm and for the STO substrate. The black curves are the XAS spectra for the SRO film with t=3t = 3 nm after subtracting the absorption from the STO substrate. (c),(d) The same deconvolution procedure as that in (a) and (b) for the SRO film with t=2t = 2 nm at θ=20∘\theta= 20^\circ.

XMCD-μ0H\mu_{0}H curves measured at the Ru M3M_{3}-edge for the SRO film with t=1t = 1–10 nm at 20 K with θ=90∘\theta= 90^\circ

Figure S4 shows the XMCD-μ0H\mu_{0}H curves measured at the Ru M3M_{3}-edge for the SRO film with t=1t = 1–10 nm at 20 K and θ=90∘\theta= 90^\circ. The coercive field HcH_{\mathrm{c}} increases with decreasing thickness from 10 nm to 2 nm [Fig. S4]. Since the magnetic domains tend to be pinned by grain boundaries and other defects, the large HcH_{\mathrm{c}} likely stems from disorder near the interface [71]. Notably, HcH_{\mathrm{c}} at t=1t = 1 nm, contrary to the above described trend of HcH_{\mathrm{c}}, becomes smaller than those at t≥2t \ge2 nm, and the Ru magnetic moments for the SRO films with t=1t = 1 and 2 nm at B=2B = 2 T are smaller than those at t≥3t \ge3 nm. The small magnetic moments for the SRO films with t=1t = 1 and 2 nm at B=2B = 2 T imply that the SRO films are no longer single-domain magnetic films due to the incoherence of the hybridized Ru 4d4d t2gt_{2g}-O 2p2p states from disorder-induced localization near the interface or increase in the effective Coulomb interaction with dimensionality reduction [62,63]. Together with the difference in the magnetic anisotropy of Ru and O ions in the SRO films with t=1t = 1 and 2 nm, these results also confirm that the magnetic states of the SRO films with t=1t = 1 and 2 nm are different.

XMCD-$\mu_0H$ curves for SRO films of different thicknesses

Figure S4. XMCD-μ0H\mu_0H curves measured at the Ru M3M_3-edge for the SRO film with t=1t = 1–10 nm at 20 K and θ=90∘\theta= 90^\circ.

References

  1. [67]S. K. Takada, Y. K. Wakabayashi, Y. Krockenberger, H. Irie, S. Ohya, M. Tanaka, Y. Taniyasu, and H. Yamamoto, Scattering-dependent transport of SrRuO3 films: From Weyl fermion transport to hump-like Hall effect anomaly, Phys. Rev. Mater. 7, 054406 (2023).arxiv.org/abs/2302.04568
  2. [68]Y. K. Wakabayashi, S. Sakamoto, Y. Takeda, K. Ishigami, Y. Takahashi, Y. Saitoh, H. Yamagami, A. Fujimori, M. Tanaka, and S. Ohya, Room-temperature local ferromagnetism and its nanoscale expansion in the ferromagnetic semiconductor Ge₁−xFeₓ, Sci. Rep. 6, 23295 (2016).DOI
  3. [69]Y. K. Wakabayashi, R. Akiyama, Y. Takeda, M. Horio, G. Shibata, S. Sakamoto, Y. Ban, Y. Saitoh, H. Yamagami, A. Fujimori, M. Tanaka, and S. Ohya, Origin of the large positive magnetoresistance in Ge₁-xMnₓ granular thin films, Phys. Rev. B 95, 014417 (2017).DOI
  4. [70]Y. Teramura, A. Tanaka, and T. Jo, J. Phys. Soc. Jpn. 65, 1053 (1996).
  5. [71]M. Izumi, K. Nakazawa, Y. Bando, Y. Yoneda, and H. Terauchi, Magnetotransport of SrRuO₃ Thin Film on SrTiO₃ (001), J. Phys. Soc. Jpn. 66, 3893 (1997).

Paper details

vlnc:W_scd5qrs7
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents