WorksPhysics and Astronomy
Layered semiconductors integrated with polyimide thin films for high-quality valleytronic and quantum-photonic systems
Abstract
Dielectric integration of layered semiconductors is a prerequisite for fabricating high-quality optoelectronic, valleytronic, and quantum-photonic devices. While hexagonal boron nitride (hBN) is the current benchmark dielectric, exploration of the most suitable dielectric materials covering the complete substrates continues to expand. This work demonstrates the formation of high optical-quality excitons in two widely explored layered semiconductors, WSe and WS, integrated into polyimide (PI) thin films of thicknesses 500 nm. The photoluminescence (PL) studies at = 296 K show the formation of neutral excitons and trions in fully-PI-encapsulated 1L-WSe with 2-sigma () spatial-inhomogeneity of 4.5 (3.4) meV in emission energy (linewidth), which is 1/3rd (1/5th), respectively, that of inhomogeneity measured in fully-hBN-encapsulated 1L-WSe. A smaller of 2.1 (2.3) meV in emission energy (linewidth) has been shown for fully-PI-encapsulated 1L-WS. Polarization-resolved and excitation power-dependent PL measurements of PI-isolated 1L-TMDs at = 4 K further reveal formations of high-quality neutral-biexcitons and negatively-charged biexcitons, with degrees of valley-polarization up to 21 under non-resonant excitation. Furthermore, the fully-PI-encapsulated 1L-WSe also hosts single quantum emitters with narrow linewidths and high-spectral stability. This work indicates that PI thin films may serve the purpose of high-quality dielectric material for integrating the layered materials on a wafer scale.
Transition metal dichalcogenides (TMDs) in their monolayer (1L) and a few layers (nL) thicknesses limit exhibit strong Coulomb interaction owing to weak dielectric screening, favors the formation of stable excitons with large binding energy (0.2 - 1.0 eV)[1, 2]. Besides the neutral-excitons (), the formations of high-order excitons, including negative-triexcitons (), neutral-biexcitons (), and negative-biexcitons (), combined with exotic spin-locked valley properties of 1L-TMDs makes them attractive candidates for realizing spintronic[3], valleytronic[4] and exciton-transport[5] devices. Moreover, the capability to host single quantum emitters[6, 7, 8] (SQEs) and their ease of integration into photonic structures promises potential application in rapidly growing quantum technologies[9, 10].
Excitonic- and single-photon emission- properties of 1L-TMDs are extremely sensitive to the dielectric environments present in the van der Waals heterostructures and devices. The exfoliated flakes of thicknesses nm[11, 12] of high-pressure and high-temperature conditions grown hexagonal boron nitride (hBN)[13, 14] crystals are utilized as the most promising dielectric materials for various TMD-based heterostructures and devices. The small dimensions ( m)[15] of these hBN flakes are utilized for the purposes of gate insulators[16, 17], charge-carrier tunneling barriers[12, 18], and encapsulating/protective layers[19], that are posing a major challenge in producing the large numbers of circuit and devices on a wafer-scale. The epitaxial growth of hBN demands specific template substrates and complex two-stage processes[20, 21]. At the same time, CVD-grown hBN lacks purity[19, 22, 23] compared to mechanically exfoliated hBN flakes[17].
Utilization of crystalline dielectrics other than hBN such
as SiO[24], AlO[24, 25], and perovskites[26, 27] have lead to the degradation in the optical quality of 1L-TMDs. Recent studies have shown that some sections of SQE generation in 1L-TMDs also demand mechanical flexibility and plastic deformation properties of the dielectric materials. For instance, the AFM nanoindentation technique enables deterministic creation of SQEs in 1L-TMD placed on a polymethyl methacrylate (PMMA) thin film[28, 29, 30]. Additionally, TMD deposited on patterned Polystyrene (PS) nano-bulges exhibited stable SQEs[31]. Among various dielectric polymers, polyimide (PI) is notable for its excellent dielectric properties[32], chemical resistance[33], and more importantly, excellent structural stability at cryogenic temperatures up to 4 K[34, 35].
In this work, we demonstrate that the utilization of PI thin film as a dielectric and/or encapsulating material substantially improves the optical properties of excitons, multiexcitons, and charged excitons that are formed in 1L-TMDs. Two types of PI-based van der Waals heterostructures, in particular, 1L-WSe and 1L-WS as the active materials, were characterized at both room-temperature (296 K) and low-temperature (4 K). To prepare PI-based 1L-TMD heterostructures, we fabricated PI thin films via spin-coating PI precursor solution (Polyamic acid) on a Si/SiO/Au substrate followed by thermal imidization process at an elevated temperature (see Methods for details of fabrication). We then mechanically exfoliated TMD crystals, which were transferred to the desired location via the all-dry transfer method[36]. The degree of imidization of PI thin films was monitored using FTIR spectroscopy (see Figure S1 of Supporting Information).
Figure S1. FT-IR spectra of polyimide thin films prepared at different imidization temperatures. The peaks at 780, 1385, and 1500 cm corresponds to out-of-plane deformation of the imide ring, C-N stretching of the imide bond, and C-C stretching of the benzene ring. The spectra were normalized with respect to the peak intensity of C-C stretching of each sample.
As fully-hBN-encapsulated 1L-TMDs heterostructures are the current benchmarks of providing the highest opticalquality delocalized neutral-excitons (), charged-excitons (), biexcitons (), and multi-excitons, we compared the PL characteristics of fully PI-encapsulated 1L-TMDs with those of fully hBN-encapsulated 1L-TMDs. We observed that PI-encapsulation reduces spectral- and spatial-inhomogeneities in 1L-TMDs compared to the hBN-encapsulated samples. Furthermore, Raman spectroscopy measurements indicated negligible strain in PI-encapsulated 1L-TMDs. At 4 K, high-order excitonic complexes were revealed, which reflects the excellent dielectric quality of PI thin film. Notably, to the best of the authors’ knowledge, observation of such excitonic complexes has not been reported on polymer-based TMD heterostructures. In addition, 2L- and 3L-WSe flakes showed remarkably enhanced excitonic emission. The polarization-dependent PL measurements demonstrated preserved valley-locking properties in 1L-WS under a dielectric PI environment. Further, we demonstrate localized SQEs in 1L-TMDs with sharp linewidth and high spectral stability.
Results and Discussion
High-quality excitons with ultra-low spatial- and spectral-inhomogeneities in fully-PI-encapsulated 1L-TMDs
Firstly, we characterized the fully-PI-encapsulated heterostructures containing 1L-WSe (PI/1L-WSe/PI, Sample PIS1) and 1L-WS (PI/1L-WS/PI, Sample PIS2) as light-emitting layers. We also fabricated and characterized the control sample 1 (hBN/1L-WSe/hBN, CS1) with the aim of presenting one-to-one comparisons of the excitonic properties in the PI-encapsulated 1L-WSe with respect to the hBN-encapsulated 1L-WSe. As a few layers-thick hBN works very well for a high- tunneling barrier[12], we also covered a portion of the 1L-WSe flake with a 5-6 layers-thick hBN flake before encapsulating it with the top-PI layer in Sample PIS1.
Figure 1a and 1b shows -PL spatial maps of the peak emission energies of the WSe flakes in the 1.4 - 1.8 eV range from the h-BN encapsulated Sample CS1, and the PI-encapsulated Sample PIS1. The PL spectra for both samples were acquired at room temperature (RT) under a continuous-wave (CW) laser excitation at nm with a power of 100 W. The representative spectra from each sample are depicted in Figure 1c. These spectra were fitted using multi-Gaussian peaks for deconvoluting the various emission peaks. The thick-, thin-, dotted- curves represent the emission peaks due to formations of delocalized neutral-exciton (), delocalized trions (), and localized excitons. The detailed investigation of these localized excitons at a 4 K temperature, leading to the emission of single photons, is presented in the later section of this work. All the PI-based samples have shown broadband weak-emission-peaks (dashed curve in Figure 1c) centered at 1.820 eV. Although the flakes of 1L-WSe for fully-PI-encapsulated Sample PIS1 are smaller in dimensions, it can clearly be seen in Figure 1b that they show similar peak emission energies through a single color contrast. On the other hand, a noticeable variation in the peak energies of PL emission of 1L-WSe can be seen in Figure 1a in the fully-hBN-encapsulated Sample CS1.
Figure 1. High-uniformity in PL properties of excitons in a fully-PI-encapsulated 1L-WSe heterostructure at 296 K. μ-PL peak-energy spatial map of (a) Fully-hBN-encapsulated and (b) Fully-PI-encapsulated 1L-WSe flakes. The thick dotted curve in (a) and (b) is the 1L-WSe region. Thin dotted curve in (b) separates the left-side region where thin hBN is deposited on top of 1L-WSe prior to the deposition of the top-PI thin film. The color codes correspond to PL peak energies in the range 1.4–1.8 eV. Scale bar for (a) and (b): 10 μm. (c) PL spectra of 1L-WSe under fully-PI-encapsulated (top panel) and fully-hBN-encapsulated (bottom panel) dielectric environments. The thick and thin curves are the deconvoluted peaks for delocalized exciton () and trion (), respectively, whereas the dotted curve is for emission due to localized excitons. Histograms of fully-hBN(PI)-encapsulated 1L WSe: (d) Peak energy and (e) Linewidth of (). Empty (filled) pillars correspond to fully-hBN(PI)-encapsulated 1L-WSe. Bin size in (d) and (e): 1 meV. Bin samples for empty (filled) pillar: 66 (130). (f) Raman spectra of fully-encapsulated 1L-WSe. The measured data with open (closed) circles (triangles) are for fully-hBN(PI)-encapsulated samples. Solid lines are multi-Gaussian fits.
For understanding the spatial inhomogeneity in PL signals from these two samples further, we analyzed the statistical distribution of peak emission energies and emission linewidths of PL spectra obtained from many different locations on both the samples. The PL spectra were collected from area of Sample CS1, and from area of Sample PIS1, by avoiding the edges of the flake where abrupt changes in the emission properties are expected. Figure 1d shows peak energy histograms of delocalized of Sample CS1 (filled pillars) and Sample PIS1 (empty pillars). The solid thick lines are the Gaussian fits of the bin heights of the histograms. To our surprise, ensemble emissions of () for both types of encapsulation lead to the same values at 1.651 eV that are consistent with the literature[11], and signifying the fact that PI can be seen as a suitable alternative dielectric at the place of hBN. Interestingly, in comparison to the fully-hBN-encapsulated Sample CS1, the fully-PI-encapsulated Sample PIS1 shows a narrow distribution in the () peak-energies.
We quantify these statistical distributions in terms of degrees of inhomogeneous broadening in () emission energy, , that are the widths of the peak-energy histograms shown in Figure 1d. We obtained meV for Sample CS1, while a significantly reduced value of meV for Sample PIS1. We attribute higher of Sample CS1 is possible because thin hBN is prone to create wrinkles and bubbles at the interface between the flakes as reported previously[37] that may cause local strains. Alternatively, we explain 15.1 meV of energy distribution correspond to considerable amount of 0.10 % strain (taking 153 meV/% strain as the gauge factor[38]) in Sample CS1. At the same time, reduced PL inhomogeneity in Sample PIS1 can be explained by the uniform clean interface provided by PI thin film over the complete substrate, which shows potential for realizing valleytronic and quantum photonic devices on PI platform. Besides the energy, a similar observation was noted in the statistics of linewidths of () emissions. Figure 1e shows () linewidth histograms of both the Samples CS1 and PIS1. The obtained degree of inhomogeneous broadening in () linewidths in Sample PIS1 () was much smaller than observed in Sample CS1 (). This further confirms the formation of high-optical quality excitons throughout the fully-PI-encapsulated 1L-WSe flake.
The substrate and/or encapsulation layers play important roles in determining the static doping of the TMD materials. Both qualitative and quantitative information on such doping can be obtained by monitoring the emission intensities of the trions-related emission peaks. The trion spectral weight (defined as , where is the integrated peak intensity of ) obtained for both the Samples CS1 and PIS1 are , indicating to a conclusion that the dielectric quality of PI is comparable with hBN. To investigate the changes in the crystal structure of 1L-WSe, we measured room-temperature -Raman spectra from both Samples CS1 and PIS1, as shown in Figure 1f, using a laser emitting at nm. The fully-hBN-encapsulated
Sample CS1 displays a dominant peaks at 250.64 cm corresponding to the Raman mode. Taking 250 cm as a reference peak for suspended (unstrained) 1L-WSe[39], a blueshift of 0.64 cm in Raman mode, that corresponds to a 0.15% compressive strain[38], was observed in the fully-hBN-encapsulated Sample CS1. Whereas the fully-PI-encapsulated Sample PIS1 showed a smaller blueshift of 0.40 cm and hence a reduced compressive strain of only 0.09% in the 1L-WSe that is further confirming high crystallinity of PI encapsulated 1L-WSe.
To demonstrate that the PI encapsulation is suitable for other widely used 1L-TMD materials, we fabricated a fully-PI-encapsulated 1L-WS Sample PIS2 (PI/1L-WS/PI heterostructure). Figure 2a shows room temperature μ-PL spatial maps of the Sample PIS2 containing a large dimensions flake of 1L-WS. Figure 2b displays a typical PL spectrum from the map. Fit results shows delocalized and peaks are located at 2.006 eV (FWHM = 35.6 meV) and 1.981 meV (FWHM = 95.9 meV) with trion spectral weight, = 0.42. For the PL statistical analysis, spectra were collected from a nearly three times bigger area than the Sample PIS1, ≈31 μm. The energy histogram (see Figure 2c) reveals reduced inhomogeneity broadening with = 2.1 meV. Similarly, linewidth histogram of fully-PI-encapsulated 1L-WS (see Figure 2d) also reflects reduced inhomogeneous broadening with = 2.3 meV. This further proves that PI encapsulation provides a nearly uniform dielectric environment irrespective of the choice of active TMD materials.
Figure 2. High-uniformity in PL properties of excitons in a fully-PI-encapsulated 1L-WS₂ heterostructure at 296 K. (a) μ-PL peak-energy spatial map of Sample PIS2 (fully-PI-encapsulated 1L-WS₂ region enclosed by thick dotted curve). (b) A representative PL spectrum showing contributions from X⁰ and X⁻ emission lines. The open circles are the measured data, and solid lines are the multi-Gaussian fit. Histograms of (c) delocalized X⁰ energy and (d) Linewidth of 1L-WS₂ emission. Bin size in (c) and (d): 1 meV. Bin samples in (c) and (d): 181.
High-order excitonic complexes in PI-based 1L-TMD heterostructures
For inspecting high-order excitons, we prepared Samples PIS3 and PIS4, where 1L-WSe and 1L-WS were isolated from substrates via PI thin films, respectively. Figure 3a shows low-temperature (4 K) μ-PL spatial map of Sample PIS3. The flake of WSe consists of 1L, 2L, and 3L-regions, whose representative spectra are shown in Figure 3b. At low excitation power, 1L-WSe PL has a peak at 1.750 eV that is identified as delocalized and another peak at 1.695 eV assigned to negative biexciton (). The linewidth is as low as 10 meV, close to the observed value in our fully-hBN-encapsulated Sample CS1[40]. Notably, the PL intensities of the 2L and 3L flakes are only decreased by factors of 4 and 12, respectively, indicating high exciton formation rates. The peak energy for 2L (3L) were observed at 1.541 eV (1.410 eV), that are consistent with previously reported values[41]. The measured binding energy () of 54.5 meV agrees with the literature[40, 42, 43]. Figure 3c shows the statistical distribution of values obtained from fitted values of PL spectra taken from 1L-WSe region of the flake marked in Figure 3c (red curve). The considerably low fluctuations of (=2.7 meV), indicate a uniform dielectric environment provided by PI film at 4 K temperature. This result further complements the reduced local inhomogeneity observed in 1L-WSe at room-temperature, as discussed previously, indeed reflecting the structural stability of dielectric PI films at low temperatures. Figure 3d shows PL spectra acquired at different laser powers. Interestingly, when excitation power was increased above 11.8 μW, a new peak identified as neutral-biexciton[40] (XX) appeared at 1.725 eV. The measured neutral-biexciton binding energy () of 25.0 meV is in close agreement with the previous reports[40, 42, 43]. To further investigate the nature of the biexciton complexes, we studied PL intensities of various peaks as a function of excitation power, as depicted in Figure 3e. The extracted intensities of multiple peaks were fitted using the power-law function of the form , where and stand for integrated PL intensity and excitation power, respectively. For the peak, we obtain . Due to the linear behavior of with an increase in power, we attribute their origin is free from defect-bound sites[44]. On the other hand, power-dependence shows a superlinear behavior[45, 46] with . Ideally, exhibits . However, a reduced value of in our sample is possibly due to competition between equilibrium states of excitons and biexcitons[47]. A similar decrease was also observed in (=1.22) for . In addition to 1L-WSe₂, we also investigated excitonic complexes in 1L-WS₂ based Sample PIS4 (PI/WS₂). In contrast to 1L-WSe₂, the 1L-WS₂ exhibited more complex excitonic features as shown in Figure 4a (see also power-dependent spectra in Figure S3 of Supporting Information). The charac-
Figure 3. Excitonic complexes in PI-based 1L-WSe₂ at 4 K. (a) μ-PL peak-energy spatial map of Sample PIS3 (PI/WSe₂) containing 1L-, 2L-, and 3L-WSe₂ flakes marked by dotted curves. (b) PL spectra of 1L-, 2L-, and 3L WSe₂ from Sample PIS3 indicate strong emission from 2L and 3L regions. (c) Histogram of binding energies () of the negative biexcitons () showing a narrow 2-sigma (σ)-spreading of 2.3 meV. Bin size: 0.2 meV. Bin samples: 471. (d) PL spectra from 1L-WSe₂ of Sample PIS3 measured at various excitation powers showing the emergence of biexcitons () at and above 11.8 μW. (e) PL intensity as a function of excitation power for different excitonic species: X⁰ (circle), XX (triangle), and XX⁻ (rectangle). The solid lines are the power-law fits, indicating linear behavior for X⁰ and superlinear behavior for XX and XX⁻.
Figure 4. Valley polarization of excitons in PI-based 1L-WS at 4 K. (a) Polarization-resolved PL spectra of Sample PIS4 (PI/1L-WS) showing significant valley-polarization locking. The spectrum with thick (thin) curve is for co-polarized, (cross-polarized, ) polarization configuration. (b) Excitation power-dependent PL integrated intensities of different excitonic complexes: (filled circle), (empty rectangle), and (filled rectangle). The solid lines represent power-law fits, indicating linear behavior for and , and superlinear behavior for .
Figure S3. PL spectra from 1L-WS of Sample PIS3 measured at various excitation powers.
the characteristic peak at 2.109 eV is the emission. The lower energy peaks at 2.077 eV and 2.058 eV are attributed to and , respectively. The binding energy of these excitonic complexes are =30.2 meV and =57 meV agrees with the literature[48]. However, a clear, distinct peak was not observed in our Sample PIS4. Other peaks may arise from localized states and need further investigations. Interestingly, the power-law fit results (Figure 4b) clearly indicate linear behavior of and with exponents and , while as expected shows superlinear trend with .
Valley polarization of PI-based 1L-WS₂ heterostructure:
Valley polarizability in 1L-TMDs is an unprecedented property for manipulating the quantum states of a valley. We study the effect of PI on valley polarizability via performing polarization-resolved PL of Sample PIS4 at a temperature of 4 K. We excited 1L-WS₂ using (right-handed) circularly polarized light at nm and detected PL spectra in and (left-handed) in both polarization basis. Figure 4a shows valley-polarized PL spectra. The solid and dotted curves are taken in and basis, respectively. Interestingly, PL intensity between and of the peaks shows clear variation, suggesting the capability to maintain spin-locking information of 1L-WS₂ under a PIdielectric environment. To quantitatively measure the valley polarization information, we define the degree of circular polarization: , where () represents PL intensity with the same (opposite) helicity in the excitation and detection. The extracted values of 0.11, 0.21, and 0.19 for , , and , respectively, demonstrate the ability of dielectric-PI to sustain valley polarization properties in 1L-TMDs even under non-resonant excitation conditions. These values are comparable to those reported for hBN-encapsulated 1L-WS [49].
SQEs in fully-PI-encapsulated 1L-WSe heterostructure
Finally, we demonstrate the effect of the PI dielectric environment on optical properties of SQEs in 1L-WSe. For consistent comparison, we measured PL spectra at 4 K for sample only with bottom PI layer (i.e., PI/1L-WSe) and fully-PI-encapsulated (i.e., PI/1L-WSe/PI) of the same WSe flake. Figure 5a shows narrow PL spectra of SQEs from different bright spots observed in μ-PL map before (dotted blue curve) and after (solid red curve) full encapsulation. Such bright emission spots at nanoparticle (NP) locations (see Fig. S4 of Supporting Information) arise from localized excitonic states[50, 51] with peak energy typically spreading in the range 1.49-1.72 eV (see Methods for details). Both the half- and fully-encapsulated samples exhibited isolated emission lines, a key factor for improving single-photon emission purity[30] by reducing multi-photon and background emission. However, some of the emitters disappeared upon full encapsulation, and new narrow peaks were formed. We ascribe this effect to the thermal treatment involved during the top-PI capping process (see Methods for details), which removes unstable emitters originating from unstable defect states in 1L-WSe[52]. The optical properties of these emitters were characterized by measuring their FWHM linewidths and spectral wanderings of their emission lines. Figure 5b compares the linewidth histogram of emitters in half- and full-encapsulated samples.
Figure 5. Single quantum emitters. (a) PL spectra of single quantum emitters (SQEs) from multiple NP locations comparing the effect of full-PI-encapsulations. Dotted and solid curves represents PI/1L-WSe and PI/1L-WSe/PI, respectively. (b) Excitation power dependence of the integrated intensity of SQEs from the fully-PI-encapsulated sample (PI/1L-WSe/PI). Solid curve represent fit using the relation . is the normalization excitation power at which PL intensity becomes half of the saturation intensity . The intensity saturation behavior indicates the quantum nature of the emitters. (c) A low excitation power (125 nW) PL spectra showing a few SQEs shown in (b). (d) Histograms of (d) Linewidth of SQEs and (e) Spectral wandering recorded for 120 s. The empty and filled pillars represent the samples PI/1L-WSe and PI/1L-WSe/PI. Bin size in (d) and (e): 30 eV and 10 eV respectively. Bin samples for empty (filled) pillars: 43 (46).
Remarkably, in both the samples, we observed linewidth as low as the resolution limit (50 μeV) of our instrument. However, the spreading of the linewidth distribution significantly reduced in the case of fully-PI-encapsulated sample. To investigate the stability of SQEs, we measured spectral-wandering, , (one-standard-deviation energy from the time-averaged emission energy) as shown in Figure 5c. This wandering is likely due to local fluctuations in the charge environment around the SQE site. We noticed no significant changes in spectral wandering statistics in both the samples (Figure 5c), signifying no adverse effects of polymeric dielectric environment. Finally, to verify the quantum nature characteristics of SQEs, we measured the excitation power dependence of PL intensity of a few emitters from fully-PI-encapsulated sample (Figure 5e). The measured data was fitted for a two-level system using the relation . is excitation power, and is the normalization excitation power at which intensity becomes half of the saturation intensity . The PL intensity saturation behavior of emitters clearly indicates quantum nature.
Conclusion
In summary, we have studied the optical quality of polymer (PI)-encapsulated 1L-TMDs, including WSe and WS at both the temperatures of 296 K and 4 K. The high optical quality of our PI-encapsulated samples was evidenced by significantly low spatial- and spectral inhomogeneities with -statistical spreads within both the exciton-emission-energy and exciton-emission-linewidth at 296 K as low as 2.1 meV and 2.3 meV, respectively. The average value of both exciton energy and trion spectral weight in PI-encapsulated 1L-WSe was nearly identical to that in hBN-encapsulated 1L-WSe, indicating that PI offers a dielectric quality on par with the current benchmark where hBN is used. At 4 K, the uniform and clean PI-dielectric environment enabled 1L-TMDs to exhibit high-order excitonic states, including neutral- and negative-biexcitons. Such complex excitonic states were previously observed predominantly in hBN-encapsulated TMD heterostructures. Moreover, PI encapsulation leads to enhanced excitonic emission even from 2L- and 3L-WSe. Polarization-resolved PL measurements under non-resonant CW excitation at 4 K demonstrated that PI thin films can preserve the valley polarization property with degree-valley-polarization values of 11%, 21%, and 19% for excitons, trions, and negative biexcitons, respectively in 1L-WS. Further, we demonstrated localized single quantum emitters in PI-encapsulated 1L-WSe exhibited resolution-limited linewidth and low spectral wandering. Our results show the capability of fabricating and obtaining high-quality polymer-based TMD heterostructures towards the development of room-temperature and low-temperature valleytronic and quantum photonic devices.
Methods
Sample preparation
PI thin films were prepared via spin coating of commercially available polyamic acid (PPA) precursor solution (Sigma-Aldrich:431176) on a Si/SiO/Au (100 nm) chip. For the uniform dispersion of PAA, a two-step spin coating was followed: first at 500 rpms for 2 s, followed by 4000 rpms for 60 s. The film was then thermally cured was at 250C for 1 hour to complete the imidization process. In order to achieve high-quality PI films, the spin-coating and thermal curing steps were carried out inside glove-box (Ar atmosphere). Thickness of PI films (500 nm) were measured using ellipsometry method.
The TMDs (WSe and WS) and hBN flakes were mechanically exfoliated from their bulk counterparts. The 1L-TMDs were qualitatively identified by optical color contrast and further confirmed by Raman spectroscopy. We employed the conventional dry-transfer method using polydimethylsiloxane (PDMS) stamp for transfer the flakes on a PI thin film. To deposit top-PI layer a few drops of PPA precursor solution was dispensed onto the PI/1L-TMD, followed by spin-coating for 60 s at 4000 rpms, and subsequently thermally cured at 250C for 1 hour. To produce localized SQEs, Silica NPs of average diameter 150 nm purchased from Sigma-Aldrich were spin-coated (8000 rpm) onto the bottom-PI layer. These NPs act as nano stressors on 1L-TMDs as demonstrated in our previous work [52].
Experimental setup
Photoluminescence and Raman measurements were performed using a home-built confocal microscope. The samples were mounted on an XYZ nanopositioner in a closed-cycle cryogen-free cryostat (Attodry800 from attocube systems AG) at K equipped with an LT APO objective (NA = 0.82). A diode-pumped solid-state CW laser emitting at nm was used for both PL and Raman measurements. An ultra-steep longpass filter designed at an edge of 533.3 nm was used to block the reflected laser. All the spectra were acquired with a 0.5 m focal length spectrometer and water-cooled charge-coupled device providing a best spectral resolution of 50 eV (125 eV) at nm ( nm) on an 1800 lines/mm grating. Polarization-dependent PL measurements were performed at 4 K under non-resonant CW excitation condition. Polarization basis controlled via a combination of polarizer, half wave plate, and quarter wave plate.
Author information
Corresponding Author
*E-mail (S.K.): [email protected]
Acknowledgment
We thank E. S. Kannan, S. R. Parne, and A. Rahman for the fruitful discussion and A. Rastelli for the data analysis software. This work was supported by the DST Nano Mission grant (DST/NM/TUE/QM-2/2019) and the matching grant from IIT Goa. We also thank CoE: PCI, IIT Goa for access to Raman and FTIR spectroscopy facilities. I.D.P. thanks The Council of Scientific & Industrial Research (CSIR), New Delhi, for the doctoral fellowship. K.W. and T.T. acknowledge support from the JSPS KAKENHI (Grant Numbers 21H05233 and 23H02052) and World Premier International Research Center Initiative (WPI), MEXT, Japan.
Supporting Information
Sample Fabrication and Methods
Preparation of Polyimide thin film: To fabricate polyimide (PI) thin films, we utilize commercially available polyimide precursor solution polyamic acid (PAA) purchased from Sigma Aldrich. The fabrication consists of mainly two steps: (1) spin-coating of PAA on a Si/SiO (270 nm)/Au (100 nm) substrate (2) Thermal treatment of PAA (known as imidization process). The spin-coating parameters used to prepare the sample described in the main text are: spin speed of 4000 rpm for 60 s with two-step acceleration, first, 500 rpm s for 2 s followed by 2000 rpm s for 2 s. Immediately after spin-coating, the substrate was placed on a hot plate and thermally cured at 120°C for 2 minutes followed by heating at an elevated temperature (referred to as imidization temperature) of 250°C for 45 minutes. During the imidization process, the PAA is converted into PI form. The structural quality of PI thin films was measured by performing FT-IR spectroscopy. A comparison illustrating changes in spectra is shown in Figure S1. The peaks at 780, 1385, and 1500 cm correspond to out-of-plane deformation of the imide ring, C-N stretching of the imide bond, and stretching of the benzene ring, respectively. The conversion of PAA to PI film was determined by calculating the degree-of-imidization (DoI) expressed as [53],
where represents the integrated area of the peak, and the reference sample corresponds to PI film prepared at 300°C imidization temperature with 60 minutes of imidization time. The DoI values for samples prepared at 120°C and 250°C are 66% and 99% respectively.
Preparation of heterostructures: The WSe and WS bulk crystals were purchased from 2D Semiconductors (Scottsdale, USA). Monolayer (1L) flakes were exfoliated from their bulk counterparts via the Scotch tape method. The 1L flakes were qualitatively identified by the optical color contrast method and further confirmed by photoluminescence and Raman spectroscopy. The flakes were then deposited on the desired substrates via the all-dry transfer method. Figure S2 shows optical images of some of the samples mentioned in the main text.
Figure S2. Optical image of Samples (a) CS1 (b) PIS1 (c) PIS3 (d) PIS4.
High-order excitons in 1L-WS
References
- [1]T. Mueller and E. Malic, “Exciton physics and device application of two-dimensional transition metal dichalcogenide semiconductors,” npj 2D Mater. Appl. 2, 29 (2018).DOI
- [2]A. Ch. Kumar, A. M. Van Der Zande, H. M. Hill, A. F. Rigosı, A. Velau-thapillaı, J. Hone, and T. F. Heinz, “Electrical tuning of exciton binding energies in monolayer WS₂,” Phys. Rev. Lett. 115, 126802 (2015).
- [3]Y. P. Feng, L. Shen, M. Yang, A. Wang, M. Zeng, Q. Wu, S. Chintalapati, and C.-R. Chang, “Prospects of spintronics based on 2D materials,” Wiley Interdiscip. Rev. Comput. Mol. Sci. 7, e1313 (2017).DOI
- [4]J. R. Schlaeih, H. Yu, G. Clark, P. Rivera, J. S. Ross, K. L. Seyler, W. Yao, and X. Xu, “Valleytronics in 2D materials,” Nat. Rev. Mater. 1, 1–15 (2016).
- [5]A. Sharma, Y. Zhu, R. Haĺbich, X. Sun, L. Zhang, B. Wang, and Y. Lu, “Engineering the dynamics and transport of excitons, trions, and biexcitons in monolayer WS₂,” ACS Appl. Mater. Interfaces 14, 41165–41177 (2022).DOI
- [6]Y.-M. He and et al., “Single quantum emitters in monolayer semiconductors,” Nat. Nanotechnol. 10, 497–502 (2015).
- [7]A. Srivastava, M. Sidler, A. V. Allain, D. S. Lembke, A. Kis, and A. Imamoğlu, “Optically active quantum dots in monolayer WSe₂,” Nat. Nanotechnol. 10, 491–496 (2015).
- [8]A. Branny, S. Kumar, R. Proux, and B. D. Gerardot, “Deterministic strain-induced arrays of quantum emitters in a two-dimensional semiconductor,” Nat. Commun. 8, 15053 (2017).DOI
- [9]J. L. O’Brien, A. Furusawa, and J. Vučković, “Photonic quantum technologies,” Nat. Photonics 3, 687–695 (2009).
- [10]T. Gao, M. von Hsvelersen, C. Antón-Solanas, C. Schneider, and T. Heindel, “Atomically-thin single-photon sources for quantum communication,” npj 2D Mater. Appl. 7, 4 (2023).
- [11]O. A. Ajayi and et al., “Approaching the intrinsic photoluminescence linewidth in transition metal dichalcogenide monolayers,” 2D Mater. 4, 031011 (2017).arxiv.org/abs/1702.05857
- [12]M. Brons-Gisbert, A. Branny, S. Kumar, R. Picard, R. Proux, M. Gray, K. S. Burch, K. Watanabe, T. Taniguchi, and B. D. Gerardot, “Coulomb blockade in an atomically thin quantum dot coupled to a tunable fermi reservoir,” Nat. Nanotechnol. 14, 442–446 (2019).
- [13]T. Taniguchi and K. Watanabe, “Synthesis of high-purity boron nitride single crystals under high pressure by using ba–bn solvent,” J. Cryst. Growth 303, 525–529 (2007).DOI
- [14]C. R. Dean and et al., “Boron nitride substrates for high-quality graphene electronics,” Nat. Nanotechnol. 5, 722–726 (2010).DOI
- [15]Y. Huang and et al., “Universal mechanical exfoliation of large-area 2D crystals,” Nat. Commun. 11, 2453 (2020).DOI
- [16]G.-H. Lee and et al., “Highly stable, dual-gated MoS₂ transistors encapsulated by hexagonal boron nitride with gate-controllable contact, resistance, and threshold voltage,” ACS Nano 9, 7019–7026 (2015).DOI
- [17]C. S. Lau, S. Das, I. A. Verzhbitskiy, D. Huang, Y. Zhang, T. Talha-Dean, W. Fu, D. Venkatakrishnarao, and K. F. Johnson Goh, “Dielectrics for two-dimensional transition-metal dichalcogenide applications,” ACS nano 17, 9870–9905 (2023).DOI
- [18]G. Pande, J.-Y. Siao, W.-L. Chen, C.-J. Lee, R. Sankar, Y.-M. Chang, C.-D. Chen, W.-H. Chang, F.-C. Chou, and M.-T. Lin, “Ultralow schottky barriers in hexagonal boron nitride-encapsulated monolayer WSe₂ tunnel field-effect transistors,” ACS Appl. Mater. Interfaces 12, 18667–18673 (2020).
- [19]K. Zhang, Y. Feng, W. Fang, Z. Yang, and J. Wang, “Two dimensional hexagonal boron nitride (2D-hbn): synthesis, properties and applications,” J. Mater. Chem. C 5, 11992–12022 (2017).DOI
- [20]A. K. Dabrowska, M. Tokarczyk, G. Kowalski, J. Binder, R. Bozek, J. Borysiuk, R. Stepniewski, and A. Wysmolek, “Two stage epitaxial growth of wafer-size multilayer h-bn by metal-organic vapor phase epitaxy—a homoepitaxial approach,” 2D Mater. 8, 015017 (2020).DOI
- [21]K. Ludwiczak, A. K. Dabrowska, J. Binder, M. Tokarczyk, J. Iwanski, B. Kurowska, J. Turczynski, G. Kowalski, R. Bozek, R. Step-niewski, W. Pacuski, and A. Wysmolek, “Heteroepitaxial growth of high optical quality, wafer-scale van der waals heterostructures,” ACS Appl. Mater. Interfaces 13, 47904–47911 (2021).
- [22]C. Kumar and A. Das, “Effect of boron nitride defects and charge inhomogeneity on 1/f noise in encapsulated graphene,” Appl. Phys. Lett. 119 (2021).DOI
- [23]Y. Y. Illarionov and et al., “Insulators for 2D nanoelectronics: the gap to bridge,” Nat. Commun. 11, 3385 (2020).
- [24]J. Martín-Sánchez and et al., “Effects of dielectric stoichiometry on the photoluminescence properties of encapsulated WSe₂ monolayers,” Nano Research 11, 1399–1414 (2018).
- [25]S. Y. Kim, H. I. Yang, and W. Choi, “Photoluminescence quenching in monolayer transition metal dichalcogenides by Al₂O₃ encapsulation,” Appl. Phys. Lett. 113 (2018).DOI
- [26]Q. Wang and et al., “Optoelectronic properties of a van der waals WS₂ monolayer/2D perovskite vertical heterostructure,” ACS Appl. Mater. Interfaces 12, 45235–45242 (2020).DOI
- [27]A. Elbanna, K. Chaykun, Y. Lekina, Y. Liu, B. Febriansyah, S. Li, J. Pan, Z. X. Shen, and J. Teng, “Perovskite-transition metal dichalcogenides heterostructures: recent advances and future perspectives,” Opto-Electron. Sci. 1, 220006–1 (2022).DOI
- [28]A. N. Abramov, I. Y. Chestnov, E. S. Alimova, T. Ivanova, I. S. Mukhin, D. N. Krizhavskii, I. A. Shelykh, I. V. Iorsh, and K. Kravtsov, “Photoluminescence imaging of single photon emitters within nanoscale strain profiles in monolayer WSe₂,” Nat. Commun. 14, 5737 (2023).DOI
- [29]M. R. Rosenberger, C. K. Dass, H.-J. Chuang, S. V. Sivaram, K. M. McCreary, J. R. Hendrickson, and B. T. Jonker, “Quantum calligraphy: writing single-photon emitters in a two-dimensional materials platform,” ACS nano 13, 904–912 (2019).
- [30]H.-J. Chuang, C. E. Stevens, M. R. Rosenberger, S.-J. Lee, K. M. McCreary, J. R. Hendrickson, and B. T. Jonker, “Enhancing single photon emission purity via design of van der waals heterostructures,” Nano Lett. 24, 5529–5535 (2024).DOI
- [31]S. Chen and et al., “Realization of single-photon emitters with high brightness and high stability and excellent monochromaticity,” Matter 7, 1106–1116 (2024).DOI
- [32]Y. Li, G. Sun, Y. Zhou, G. Liu, J. Wang, and S. Han, “Progress in low dielectric polyimide film—a review,” Prog. Org. Coat. 172, 107103 (2022).DOI
- [33]A. Sezer Hicyilmaz and A. Celik Bedeloglu, “Applications of polyimide coatings: A review,” SN Appl. Sci. 3, 363 (2021).
- [34]V. Geidarov, I. Braud, N. Gal’tsov, and Y. M. Pohlibnaya, “Influence of low temperature on deformation changes in the structure of the polyimide film PMA,” Mol. Cryst. Liq. Cryst. 661, 20–24 (2018).DOI
- [35]V. Soldatov, G. Kirichenko, V. Abraimov, I. Braude, and V. Geidarov, “The laws of deformation of an amorphous polyimide (PI) film when it is stretched in the temperature range 1.6–300 K,” Low Temp. Phys. 42, 817–824 (2016).DOI
- [36]A. Castellanos-Gomez, M. Buscema, R. Molenaar, V. Singh, L. Janssen, H. S. Van der Zant, and G. A. Steele, “Deterministic transfer of two-dimensional materials by all-dry viscoelastic stamping,” 2D Mater. 1, 011002 (2014).
- [37]P. Ares, Y. B. Wang, C. R. Woods, J. Dougherty, L. Fumagalli, F. Guinea, B. Davidovitch, and K. S. Novoselov, “Van der waals interaction affects wrinkle formation in two-dimensional materials,” Proc. Natl. Acad. Sci. U.S.A. 118, e2025870118 (2021).DOI
- [38]S. Roy, J. Gao, and X. Yang, “Upconversion photoluminescence of monolayer WSe₂ with biaxial strain tuning,” Opt. Express 32, 3308–3315 (2024).DOI
- [39]H. Sahin, S. Tongay, S. Horzum, W. Fan, J. Zhou, J. Li, J. Wu, and F. Peeters, “Anomalous raman spectra and thickness-dependent electronic properties of WSe₂,” Phys. Rev. B 87, 165409 (2013).DOI
- [40]Z. Li and et al., “Revealing the biexciton and trion-exciton complexes in bn encapsulated WSe₂,” Nat. Commun. 9, 3719 (2018).
- [41]P. Tonndorf et al., “Photoluminescence emission and raman response of monolayer MoS₂, MoSe₂, and WSe₂,” Opt. Express 21, 4908–4916 (2013).
- [42]Z. Ye and et al., “Efficient generation of neutral and charged biexcitons in encapsulated WSe₂ monolayers,” Nat. Commun. 9, 3718 (2018).DOI
- [43]M. Barbone and et al., “Charge-tuneable biexciton complexes in monolayer WSe₂,” Nat. Commun. 9, 3721 (2018).
- [44]S. Tongay and et al., “Defects activated photoluminescence in two-dimensional semiconductors: interplay between bound, charged and free excitons.” Sci. Rep. 3, 2657 (2013).
- [45]J. Kim, D. Wake, and J. Wolfe, “Thermodynamics of biexcitons in a GaAs quantum well,” Phys. Rev. B 50, 15099 (1994).pubmed.ncbi.nlm.nih.gov/9975860
- [46]Y. Yu, X.-F. Zhang, T. C. Berkelbach, M. S. Hybertsen, D. R. Reichman, and T. F. Heinz, “Observation of biexcitons in monolayer WSe₂,” Nat. Phys. 11, 477–481 (2015).DOI
- [47]D. Birkedal, J. Singh, V. Lyssenko, J. Erland, and J. M. Hvam, “Binding of quasi-two-dimensional biexcitons,” Phys. Rev. Lett. 76, 672 (1996).pubmed.ncbi.nlm.nih.gov/10061518
- [48]M. Paur, A. J. Molina-Mendoza, R. Bratschitsch, K. Watanabe, T. Taniguchi, and T. Mueller, “Electroluminescence from multi-particle exciton complexes in transition metal dichalcogenide semiconductors,” Nat. Commun. 10, 1709 (2019).DOI
- [49]S. Das, D. Huang, I. A. Verzhbitsky, Z.-E. Ooi, C. S. Lau, R. Lee, C. P. Y. Wong, and K. E. J. Goh, “Electrical control of valley polarized charged exciton species in monolayer WS₂,” ACS Nano 18, 30805–30815 (2024).DOI
- [50]P. Tonndorf, R. Schmidt, R. Schneider, J. Kern, M. Buscema, G. A. Steele, A. Castellanos-Gomez, H. S. van der Zant, S. Michaelis de Vasconcellos, and R. Bratschitsch, “Single-photon emission from localized excitons in an atomically thin semiconductor,” Optica 2, 347–352 (2015).DOI
- [51]L. Linhart, M. Paur, V. Smejkal, J. Burgdörfer, T. Mueller, and F. Libisch, “Localized intervalley defect excitons as single-photon emitters in WSe₂,” Phys. Rev. Lett. 123, 146401 (2019).DOI
- [52]J. T. Suresh, Y. Waheed, S. Shit, I. D. Prasad, K. Watanabe, T. Taniguchi, and S. Kumar, “Nanoparticle stressor-induced single-photon sources in monolayer WS₂ emitting into a narrowband visible spectral range,” 2D Mater. 11, 031002 (2024).
- [53]H.-T. Kim and J.-K. Park, “Effect of imidization temperature and spinning condition on structure of polyimide film derived from cyclobutanedianhydride and 2, 2-bis (4-aminophenoxyphenyl) propane,” Polym. J. 29, 1002–1006 (1997).DOI