Transport anomalies in the layered compound BaPt4Se6

Abstract

We report a layered ternary selenide BaPt4Se6 featuring sesqui-selenide Pt2Se3 layers sandwiched by Ba atoms. The Pt2Se3 layers in this compound can be derived from the Dirac-semimetal PtSe2 phase with Se vacancies that form a honeycomb structure. This structure results in a Pt (VI) and Pt (II) mixed-valence compound with both PtSe6 octahedra and PtSe4 square net coordination configurations. Temperature dependent electrical transport measurements suggest two distinct anomalies: a resistivity crossover, mimic to the metal-insulator (M-I) transition at ~150K, and a resistivity plateau at temperatures below 10K. The resistivity crossover is not associated with any structural, magnetic or charge order modulated phase transitions. Magnetoresistivity, Hall and heat capacity measurements concurrently suggest an existing hidden state below 5K in this system. Angle-resolved photoemission spectroscopy measurements reveal a metallic state and no dramatic reconstruction of the electronic structure up to 200K.

structural, magnetic or charge order modulated phase transitions. Magnetoresistivity, Hall and heat capacity measurements concurrently suggest an existing hidden state below 5K in this system. Angle-resolved photoemission spectroscopy measurements reveal a metallic state and no dramatic reconstruction of the electronic structure up to 200K.

Introduction

Two-dimensional (2D) transition metal dichalcogenides (TMDs), with various polytype structures such as 1T, 1T’, 2H, and 3R phases, have provided a fertile ground for fundamental quantum materials research and emergent potential applications in the past decade due to the fascinating physical properties discovered in these materials[1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17]. In most cases, structural defects such as vacancies and grain boundaries disrupt the translational symmetry of these pristine lattices and significantly impact their physical and chemical properties. Typically, these defects are detrimental to the carrier mobility and associated charge transport performance[18, 19, 20]. However, defect-engineering through carefully controlled atomic defects has recently emerged as a versatile and effective tool which can significantly improve the physical properties, tune the electronic structures, and tailor their device performances for 2D materials. It has been demonstrated that different types of controlled defect structures have led to the enhancement of electrical transport, optical, and chemical properties, for various TMD materials[21, 22, 23]. If such defects are well-ordered, a new type of structure or even unprecedented physical properties could also be developed[24, 25]. For example, Mo6Te6\mathrm{Mo}_{6}\mathrm{Te}_{6} nanowire forms at the boundaries of 2H-MoTe2\mathrm{MoTe}_{2} through thermal annealing under vacuum[26]; novel Mo2S3\mathrm{Mo}_{2}\mathrm{S}_{3} is fabricated through a periodic assembly of chalcogen vacancy lines in the corresponding MoS2\mathrm{MoS}_{2} monolayers[27]. Point defects and line defects of chalcogen atoms induce magnetism in PtSe2\mathrm{PtSe}_{2} and ReS2\mathrm{ReS}_{2} where magnetism does not exist in the pristine materials[28, 29]. Besides defect engineering, chemical intercalation that introduces guest species into the van der Waals gaps can also effectively change the band filling and the chemical potential of TMD materials and lead to drastic changes of their electronic, transport and optical properties[30, 31, 32]. These intercalates can range from cations, anions, neutral atoms and even organic molecules, and could also introduce charge orders[33, 34], superconductivity[35, 36], or magnetic orders[37, 38] into the host TMD materials.

Among the known TMDs, PtSe2\mathrm{PtSe}_{2} has been well-known for its high performance in photocatalysis, electrocatalysis, and high mobility in field-effect transistors[39, 40, 41, 42, 43, 44, 45]. With dimension reduction of PtSe2\mathrm{PtSe}_{2}, the physical properties will change from that of a bulk Dirac semimetal to a monolayer semiconductor with an indirect bandgap of 1.2 eV[46]. Different types of defects have been found in the bulk and thin films of PtSe2\mathrm{PtSe}_{2}, and they have experimentally and theoretically impacted the related properties[28, 47]. Thickness-independent semiconducting-to-metallic conversion, in contrast to semiconducting-to-metal transition with reduced thickness, has been observed through plasma-driven atomic defect engineering in PtSe2\mathrm{PtSe}_{2} films[48]. Theoretical calculations suggested that large spin-orbit splitting can be induced by introducing point defects in the PtSe2\mathrm{PtSe}_{2}[49], and the Se vacancy line defects in monolayer PtSe2\mathrm{PtSe}_{2} could cause a sizable spin splitting in the defect states[50]. This large spin-orbital splitting gives rise to persistent spin textures which protect the spin from decoherence and induce an extraordinarily long spin lifetime for designing spintronic devices.

As a part of chemical doping studies with controlled defects synthesis for bulk PtSe2\mathrm{PtSe}_{2} materials[51], we report herein a ternary compound of BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} of layered structure featured with sesqui-selenide Pt2Se3\mathrm{Pt}_{2}\mathrm{Se}_{3} layers sandwiched by Ba atoms. Each sesqui-selenide Pt2Se3\mathrm{Pt}_{2}\mathrm{Se}_{3} layer could be considered as a PtSe2\mathrm{PtSe}_{2} structure with ordered Se vacancies. It has an atomic coordination within the structure of both the PtSe6_6 octahedra and the PtSe4_4 square planar, which results in a mixed-valence compound with Pt (II):Pt (IV) = 3:1. It is also interesting to note that the Se atom framework in this compound could be viewed as stacks of distorted Kagome nets formed by Se atoms. We observe a resistivity crossover, mimic to the metal-insulator transition around 150K and a resistivity plateau at temperatures below 10K. The X-ray single crystal diffraction, temperature dependent electrical resistivity, magnetoresistivity, Hall, effect, heat capacity, and angle-resolved photoemission spectroscopy (ARPES) measurements are carried out to fully characterize this compound and understand the intriguing transport anomalies observed in this system.

Results and Discussions

X-ray diffraction and structure description

The details of the X-ray single crystal refinements and the associated crystallographic parameters for BaPt4_4Se6_6 at both 300K and 100K are provided in Table. Table 1. Additional atomic coordination, selected interatomic distances, angles, and precession images are presented in the supplementary information. In sharp contrast to PtSe2_2 in the space group of P3ˉm1P\bar{3}m1, BaPt4_4Se6_6 crystallizes in a distinct structure type (mC44mC44) and the centrosymmetric monoclinic space group C2/cC2/c (#15) with lattice parameters aa=12.715(4) Å, bb= 7.406 (2) Å, cc= 12.461 (3) Å, and β\beta= 118.089(7) °. The X-ray diffraction pattern with peaks in the preferred orientation is shown in Figure 1a, together with a photograph of the crystals on the mm scale grid. The crystal structure (Figure 1b) consists of three distinct Pt sites (Pt1 and Pt2 atoms are at 4e4e sites and Pt3 atoms are at the general position 8f8f, as labeled in Figure 1b). Pt1 atoms at the 4e4e site are octahedrally coordinated with six neighboring Se atoms and have a formal Pt4+^{4+} valence. The Pt2 atoms at 4e4e site and the Pt3 atoms at 8f8f site, have a square planar environment with near-by Se atoms, and have a formal Pt2+^{2+} valence (Supplementary Figure 1). The PtSe6\mathrm{PtSe}_{6} octahedra formed by Pt1 atoms are edge shared with the square planar PtSe4\mathrm{PtSe}_{4} formed by both Pt2 and Pt3 atoms (Figure 1b). Each PtSe6\mathrm{PtSe}_{6} octahedra is surrounded by six PtSe4\mathrm{PtSe}_{4} square planar, and each PtSe4\mathrm{PtSe}_{4} square planar is shared by two PtSe6\mathrm{PtSe}_{6} octahedra, together they form a sesqui-selenide Pt2Se3\mathrm{Pt}_{2}\mathrm{Se}_{3} layer structure with the stacking along the cc-axis. The interlayer Se-Se distance is 3.478 Å, suggesting weak van der Waals interactions between the sesqui-selenide layers.

Temperature300K100K
Crystal systemMonoclinicMonoclinic
Space groupC2/c (No. 15)C2/c (No. 15)
aa12.715(4) Å12.709(2) Å
bb7.406(2) Å7.4004(14) Å
cc12.461(3) Å12.406(2) Å
β\beta118.089(7) °118.374(8) °
ZZ44
Atomic position
Ba1(4c)1/43/41/21/43/41/2
Pt1(4e)00.35664(5)1/400.35783(4)1/4
Pt2(4e)00.85699(5)1/400.85812(4)1/4
Pt3(8f)0.25059(2)0.59819(3)0.24539(3)0.25057(2)0.59922(3)0.24530(2)
Se1(8f)0.03278(6)0.61103(8)0.13512(7)0.03223(5)0.61205(7)0.13456(5)
Se2(8f)0.22316(6)0.35380(9)0.36289(7)0.22376(5)0.35499(7)0.36357(5)
Se3(8f)0.03163(6)0.10257(8)0.13610(7)0.03117(5)0.10391(7)0.13565(5)
Absorption coefficient78.633 mm−178.633\ \mathrm{mm}^{-1}79.292 mm−179.292\ \mathrm{mm}^{-1}
θ\theta range3.30 to 30.57 °3.30 to 30.54 °
Independent reflections15991575
Refine Parameters5454
R(int)0.05640.0458
Final R indicesR1=0.027R_{1}=0.027, wR2=0.058wR_{2}=0.058R1=0.022R_{1}=0.022, wR2=0.055wR_{2}=0.055
Goodness-of-fit1.0561.076

Table 1. Crystal structure of BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} at room temperature and 100K

Structural analysis of BaPt₄Se₆

Figure 1. Structural analysis of the BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6}. a Powder X-ray diffraction on single crystal with the preferred orientation along cc-axis, inset is the optical image of the BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} single crystals. b Side view of BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} structure, with the PtSe6\mathrm{PtSe}_{6} octahedra and the adjacent PtSe4\mathrm{PtSe}_{4} square planar. c Projection of the Pt2Se3\mathrm{Pt}_{2}\mathrm{Se}_{3} layer, with the red open circles denote the vacancy of Se atoms and compare to d top view of the PtSe2\mathrm{PtSe}_{2} layer from 1T1T-PtSe2\mathrm{PtSe}_{2}.

The Ba atoms are sandwiched between layers and can be charge-balanced as (Ba2+)(Pt2+)3(Pt4+)(Se2−)6(\mathrm{Ba}^{2+})(\mathrm{Pt}^{2+})_{3}(\mathrm{Pt}^{4+})(\mathrm{Se}^{2-})_{6} with Pt (II):Pt (IV) = 3:1. The Pt (II)-Se distances in the square-planar configuration range from 2.4371(9) Å- 2.4704(9) Å, and are generally shorter than the Pt(IV)-Se distances with octahedral configurations [2.5008(9) Å- 2.5169(9) Å]. Both the PtSe6\mathrm{PtSe}_{6} octahedra and PtSe4\mathrm{PtSe}_{4} square planar are highly distorted resulting from the monoclinic symmetry of the crystal structures (Supplementary Figure 1and Supplementary Table 1 & 2).

The sesqui-selenide Pt2Se3\mathrm{Pt}_{2}\mathrm{Se}_{3} layer in this BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} compound could be considered as the Se-defect-ordered structure of TMD PtSe2\mathrm{PtSe}_{2} layers. Figure 1c represents the projection of the Pt2Se3\mathrm{Pt}_{2}\mathrm{Se}_{3} slab in BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6}. In comparison with the projected monolayer PtSe2\mathrm{PtSe}_{2} slab (Figure 1d), one-third of the Se atomic positions in the Pt2Se3\mathrm{Pt}_{2}\mathrm{Se}_{3} slab remain vacant, as highlighted by red open circles, and the vacancies are alternatively shifted to form a well-ordered honeycomb defect pattern. This ordered vacancy pattern is apparently different from the linear vacancy line pattern observed in the Mo2S3\mathrm{Mo}_{2}\mathrm{S}_{3} structures and suggests a likely significant change in the electronic structures and transport properties comparing to the parent compound PtSe2\mathrm{PtSe}_{2}.

Electrical transport data and discussions

The temperature dependent resistivity data of the BaPt4_4Se6_6 are shown in Figure 2a. In sharp contrast to the overall semi-metallic behavior of the bulk PtSe2_2, this vacancy-ordered sesqui-selenide shows a drastic resistivity crossover at ~150K with metallic behavior from room temperature down to 150K and semiconducting behavior below 150K. Using the thermal activation model formula of

Electrical resistivity and heat capacity data

Figure 2. Electrical resistivity and heat capacity data. a Temperature dependent resistivity in log scale to show the low temperature resistivity saturation, the red solid line is the fitted data using the activation energy model. b Heat capacity of BaPt4Se6\mathrm{BaPt_4Se_6} from 2K to 200K where no clear anomalies or jumps are observed, and the inset is the low temperature heat capacity and first derivative (in red) data from 2K to 10K.

ρ∝eEa/kBT\rho\propto e^{E_a/k_B T}

within the temperature range from 150K to 90K, we obtain an activation energy of 0.82 meV. However, the resistivity begins to deviate from the thermal activation model below 80K, starts to saturate below 20K, and reaches a plateau between 10K and 2K, reminiscent of the resistivity plateau observed in SmB6_6.

Both the resistivity crossover at 150K and resistivity plateau at lower temperatures are quite intriguing, as they hint at a number of potential causes ranging from a magnetic phase transition, charge density wave (CDW) transition, Kondo effect, topological effects, and localization. We therefore carried out temperature dependent magnetization, single crystal X-ray diffraction, and heat capacity measurements to further examine the origins of these transport anomalies. Firstly, no magnetic transition is observed from temperature-dependent magnetization measurement (Supplementary Figure 4). This is consistent with the electron configuration of 5d85d^8 for Pt (II) atoms in the square planar coordination and 5d65d^6 for Pt (IV) atoms in the octahedral coordination as for both configurations the 5d5d electrons are fully paired. In addition, there are no magnetic ions in this system. Hence resistivity anomalies cannot be induced by the Kondo effect. Secondly, no clear structural transformation is observed from X-ray single crystal diffraction in the low temperature regime down to 100K. The overnight low temperature X-ray single crystal diffraction at 100K is collected and the refined crystal structures are shown in Table 1. Clearly no symmetry changes nor splitting of Wyckoff positions is observed between 100 K and 300 K. The integrated precession images that represent the reciprocal space diffraction spots (Supplementary Figure 2) also do not reflect any CDW-modulated structural distortions at 100K compared with the refined structural model at 300K shown in Table 1. In addition, no clear jumps or anomalies are observed from heat capacity data between 2K and 200K (Figure 2b), which further supports that no structure transition nor other first order phase transitions exist in this system. Therefore, electron localization is the most likely cause of the resistivity upturn at 150K in this system. A combination of the thermal activation model and variable range hopping model using different dimension indices to represent the strong localization effect have been used to fit the data between 80K and 20K, and yield an unreasonably small activation energy less than 1 μeV1\,\mu\mathrm{eV}. This suggests that the weak localization rather than strong localization exists in the system.

Regarding the origin of the resistivity plateau observed at low temperatures, magnetic effects such as Kondo effect or magnetic field-induced resistivity saturation as observed in WTe2\mathrm{WTe}_{2} system are not applicable here. One possible explanation could be the contribution of some additional metallic states, which could originate from multiple conducting channels or surface states competing with the localization effects at low temperatures.

The low temperature range heat capacity data is shown in the inset of Figure 2b. Interestingly, the heat capacity does not exhibit a linear relationship of C/TC/T vs T2T^{2} following the Debye model C=γNT+βT3C = \gamma_{N}T + \beta T^{3} between 2K and 10K. By taking the first order derivative of the nonlinear behavior from 2K to 10K, we can clearly observe a broad peak with a maximum at around 6K. This peak may suggest an existing hidden order in the BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} system, which could be responsible for the resistivity plateau observed from the electrical resistivity measurement.

Resistivities with and without applying a magnetic field at 9T in the whole temperature range are shown in Figure 3a. A clear change of magnetoresistance sign is observed at ~100K, from negative in the low temperature range to positive in the high temperature range. The isothermal magnetoresistivity up to 9T at different temperatures are shown in Figure 3b, which is consistent with Figure 3a. Three small yet non-negligible anomalies could be observed: (i) a broad hump at 150K which is on par with the M-I transition temperature observed in Figure 2a; (ii) a change of sign of the magnetoresistance at 100K from positive to negative is observed; (iii) the magnetoresistance upturn below 5K. As the localization are typically induced by disorder, the broad hump at 150K could be explained by the enhanced scattering caused by disorder under magnetic field. However, at low temperatures, a negative magnetoresistivity due to the localization effect will emerge and become stronger with decreasing temperature. The positive and negative magnetoresistance will compensate each other at intermediate temperatures, which could explain the sign changes of magnetoresistance at around 100K. Below 100K, the negative magnetoresistance induced by localization becomes predominant. Interestingly, an upturn of the magnetoresistivity below 5K is observed, which could also be clearly noticed from the inset of Figure 3b. In comparison with the 5K data, the magnetoresistivity at 2K bends down at high magnetic fields.

In-plane magnetoresistivity data and related analysis

Figure 3. In-plane magnetoresistivity data and related analysis. a Temperature-dependent in-plane resistivity data at zero magnetic field and with applied magnetic field up to 9T. b Magnetoresistivity at different temperatures under 9T. The inset shows the isothermal magnetic field-dependent resistivity behavior. c Magneto conductance at low magnetic field range fitted by the HLN formula (solid line) at several temperatures, and d Temperature dependent phase coherence length at different temperatures derived from the HLN formula with linear fitting in the double log scales.

In order to demonstrate the weak localization effect in this system, we convert the magnetoresistance data to the magnetoconductance at low field range with temperatures far below 100K to minimize the influence of the classical magnetoresistance and fit the data using the Hikami-Larkin-Nagaoka (HLN) formula[52]

Δσ(B)G0=α[Ψ(12+BϕB)−ln⁡(BϕB)](1)\frac{\Delta\sigma(B)}{G_0}=\alpha\left[\Psi\left(\frac{1}{2}+\frac{B_\phi}{B}\right)-\ln\left(\frac{B_\phi}{B}\right)\right] \tag*{(1)}

which describes the quantum correction to conductivity due to weak localization. In the equation G0=e2/(2π2ℏ)G_0=e^2/(2\pi^2\hbar), α\alpha is the parameter in the renormalization group equation, Ψ(x)\Psi(x) is the digamma function, Bϕ=ℏ/(4eLϕ2)B_\phi=\hbar/(4eL_\phi^2) is the characteristic value of the magnetic field with LϕL_\phi as the phase coherent length. The fitting results are shown in Figure 3c where the data generally are described reasonably well by the HLN formula, some deviation of the fits from experimental values are observed at our lowest measured temperature of 2K and 5K, which likely is due to the additional metallic states as seen in the previous resistivity data in Figure 2a. The phase coherence length LϕL_\phi extracted from BϕB_\phi, changes from ~47 nm at 2K to ~12 nm at 30K (Figure 3d). As we increase temperature, the phase coherence length decreases, typically following the power-law relationship Lϕ∝T−nL_\phi\propto T^{-n}. As the coherence length value at 2K is affected by additional metallic states (Figure 3c), we therefore only perform a linear fitting from 5K to 30K (red solid line) (Figure 3d) and obtain a fitted index of n=0.62n=0.62—a value close to ½ indicating the two-dimensional nature of this system.

In order to further understand the carrier contributions at low temperatures for BaPt4_4Se6_6, we performed Hall measurement (Figure 4a). By sweeping the magnetic field at different temperatures, the Hall resistivity shows a linear relationship with the magnetic field. The Hall resistivity is positive throughout the whole temperature range, suggesting the predominant hole charge carriers in the system. The absolute Hall resistivity value does not change much in the whole temperature range, and the obtained room temperature hole concentration is on the order of 1019 cm−310^{19}\,\mathrm{cm}^{-3}. This is consistent with the resistivity data where no significant change of resistivity is observed despite the M-I transition at 150K. The temperature dependent Hall resistivity data at 9T is shown in Fig. 4b. Both a broad maximum at 150K and a small upturn below 20K are observed, consistent with both temperature dependent resistivity and magnetoresistivity results discussed previously.

Hall resistivity data

Figure 4. Hall resistivity data. a Field-dependent Hall resistivity of BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} at different temperatures up to 9T. b Temperature-dependent Hall resistivity at 9T.

Band structure calculations and ARPES measurements

To visualize the electronic structure of BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} and its evolution with temperature, we performed ARPES experiments on the high-quality single crystals. From Density Functional Theory (DFT) calculations on the nominal crystal structure, BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} is expected to be a semiconductor (Figure 5d). The measured dispersions, however, indicate a metallic state. To introduce the measured dispersions, we first show the three-dimensional (3D) Brillouin zone (BZ) notation of BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} (Figure 5a) and the corresponding projected (001) plane sketched in grey and appended to the measured Fermi surface (FS) in Figure 5b. Note that due to the low symmetry of the BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} crystal structure, the FS intensity shows a C2C_{2} symmetric pattern with respect to the Γˉ−Mˉ2\bar{\Gamma} - \bar{M}_{2} direction only. In the kzk_z mapping displayed in Figure 5c, the FS shows an anti-symmetric intensity distribution across kzk_z, of which the apparent periodicity is twice that of the BZ size. Such observed intensity pattern is due to the structural factor originating from the two stacked Pt4Se6\mathrm{Pt}_{4}\mathrm{Se}_{6} layers within each unit cell. Consequently, the kzk_z FS mapping intensity manifests more strongly the periodicity of the single layer Pt4Se6\mathrm{Pt}_{4}\mathrm{Se}_{6}. The measured FS shows Fermi pockets around the BZ boundaries. Along Γˉ−Mˉ2\bar{\Gamma} - \bar{M}_{2}, we observe these pockets to be small hole pockets from two linear bands crossing the Fermi level consistent with a metallic nature, albeit near the valence band top (Figure 5e). From a comparison to the calculation, we observe that the bands away from Fermi level present better consistencies with the calculation. The origin of the mismatch here is likely due to Se vacancies in the material that slightly hole-dopes the sample. The electronic dispersions of BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} indicate a degree of resemblance to that of PtSe2\mathrm{PtSe}_{2}, albeit with distinction. The dispersions at the Γˉ\bar{\Gamma} point emerge from a X-shape feature at near −1.3-1.3 eV (Figure 5f top figure and Supplementary Figure 5). A pair of bands are observed at the M‾2\overline{M}_{2} point, which in PtSe2_2 are observed to carry spin-texture due to Rashba splitting[45]. However, the measured FS and dispersions show much lower symmetry compared to PtSe2_2.

Angle-resolved photoemission spectroscopy results for BaPt4Se6

Figure 5. Angle-resolved photoemission spectroscopy (ARPES) results. a 3D BZ of BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} where the grey shaded area denotes the projected (001) surface. b FS map integrated within a 20 meV window of the projected (001) surface using 88eV LH photons at T=13.5 KT=13.5\,\mathrm{K}. Polarization of incident photons is indicated by ε\varepsilon. c FS map along the kzk_z direction. d DFT calculation for bulk BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} with SOC included showing a semiconducting ground state. e Band dispersions along the Γˉ−Mˉ2\bar{\Gamma}-\bar{M}_{2} and Γˉ−Cˉ\bar{\Gamma}-\bar{C} directions where the momentum directions have been marked in b. f Band dispersions along the Γˉ−Mˉ2\bar{\Gamma}-\bar{M}_{2} direction at 14K, 151K and 196K, respectively, indicated by a yellow vertical line in panel b. Red triangles extracted from MDCs serve as visual guidance for the metallic states crossing the Fermi level.

We also carried out temperature-dependent measurements to examine the connection to the transport anomalies. The middle panel in Figure 5f shows the Γ‾−M‾2\overline{\Gamma}-\overline{M}_{2} cut at 151K corresponding to the M-I transition shown above, while the figure at the bottom is taken at temperature high above the transition. Evidently, considering thermal broadening, major features of the band structure, especially the bands crossing Fermi level remain largely unchanged between 14K and 196K. The red triangles in Figure 5f are fitted from momentum distribution curves (MDCs) to highlight the band crossing the Fermi level. Our observation supports the argument that the resistivity crossover around 150K is not caused by any change of the density of states near EFE_{\mathrm{F}}, but according to the analysis above can be attributed to the weak localization effect.

In summary, A layered ternary compound BaPt4_4Se6_6 has been discovered with sesqui-selenide layered feature and mix-valence Pt oxidation states. The sesqui-selenide layer is similar to the TMD PtSe2_2 structure with ordered Se vacancies. Electrical resistivity measurements reveal two transport anomalies: one resistivity crossover at ∼\sim150K and a resistivity plateau below 10K. Extensive studies from X-ray diffraction and heat capacities suggest the resistivity crossover is due to weak localization that is related to the structural distortion and ordered honeycomb Se vacancy of the structure. Temperature-dependent ARPES measurements reveal a metallic state between 14K and 196K, and does not show any abrupt electronic changes in the whole temperature range, further supporting the weak localization effect in this compound. Magnetoresistivity, Hall and heat capacity measurements concurrently suggest an existing hidden state below 5K, which should be responsible for the resistivity plateau at low temperatures. The hole-like band in the MDC curves from the ARPES measurements is consistent with hole charge carriers from our Hall data. Unfortunately, no clear evidence of the existence of the in-gap state is observed from ARPES measurements down to 14K, which is slightly higher than the resistivity plateau below 10K. The exact origin of the emerged metallic ground state at low temperatures responsible for the resistivity plateau is subject for future studies.

METHODS

Material Synthesis and X-ray Diffraction

The compound was initially discovered during the chemical doping studies for BaxPtSe2\mathrm{Ba}_{x}\mathrm{PtSe}_{2}. The small grain crystals are isolated first for chemical analysis and initial X-ray diffraction studies. The large size of single crystals of BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} were later directly synthesized through solid state reaction using Ba pieces (99.9%, Alfa Aesar), Pt pieces (99%) and Se shots (99.999%, Alfa Aesar).

Stoichiometric amount of the starting materials were placed into a graphite crucible and then sealed in the fused quartz tube under vacuum. The tube was placed in a furnace, slowly heat with a rate of 30°C /h up to 1100 °C, and maintained for 48 hours before slowly cooled down to 800 °C with the rate of 3 °C /h. Thin shinning black crystals can be obtained by carefully cleaving the melt ingot and with preferred cc-axis orientations (Figure 1a). The exact crystal structure was determined by Bruker D8 Quest Kappa single-crystal X-ray diffractometer equipped with a Mo Kα\alpha Iμ\muS microfocus source (λ=0.71073\lambda= 0.71073 Å) operating at 50 kV and 1 mA with a HELIOS optic monochromator and a CMOS detector. The collected data set was integrated with Bruker SAINT and scaled with Bruker SADABS (multiscan absorption correction). The refined chemical composition from single crystal diffraction was subsequently confirmed by scanning electron microscope energy-dispersive X-ray spectroscopy (Supplementary Figure 3).

Physical Properties Measurements

The electric resistivity and Hall coefficient were measured by employing standard six probe method using golden wires and silver paste on a 2×1×0.1 mm32 \times1 \times0.1\ \mathrm{mm}^{3} crystal with the temperature down to 2K and magnetic field up to 9T. The magnetoresistivity measurement using standard six probe method with magnetic field perpendicular to the crystal plane and current, the heat capacity measurement using the relaxation method down to 2K, were performed in a Quantum Design Physical Property Measurement System. ARPES measurements were performed at the MERLIN beamline 4.0.3 at the Advanced Light Source, equipped with a SCIENTA R8000 electron analyzer. The single crystal was cleaved in-situ at 13 K and measured in an ultra-high vacuum with a base pressure better than 5×10−115 \times10^{-11} Torr. Photon energy dependent measurements were carried out from 30 to 120 eV, and 88 eV linear horizontal (LH) light was selected to obtain highest data quality.

Electronic Structure Calculations

The electronic structure of BaPt4Se6\mathrm{BaPt}_{4}\mathrm{Se}_{6} was calculated in the framework of DFT within the generalized gradient approximation[53]. The projector-augmented-wave method implemented in Vienna Ab Initio Simulation Package is employed with the default energy cutoff specified in the pseudopotential file. The momentum grid is taken as 9×9×99 \times9 \times9. The SOC is included in the calculation self-consistently. The calculations are performed at the HPC Platform of ShanghaiTech University Library and Information Services and School of Physical Science and Technology.

Data Availability

The authors declare that all essential data supporting the findings of this study are available within the paper and its supplementary information.

Acknowledgements

This work at University of Texas at Dallas is supported by US Air Force Office of Scientific Research Grant No. FA9550-19-1-0037. This project is also partially funded by NSF-DMREF-1921581, and the University of Texas at Dallas Office of Research through the Seed Program for Interdisciplinary Research (SPIRe) and Core Facility Voucher Program. J.Y.C. also acknowledges partial support from NSF DMR-1700030. Work at Rice University was supported by the Gordon and Betty Moore Foundation's EPiQS Initiative through grant No. GBMF9470, the Robert A. Welch Foundation Grant No. C-2024, the Alfred P. Sloan Foundation, as well as in part by NSF-DMREF-1921847. Work at UC Berkeley is funded by NSF-DMR-1921798. This research used resources of the Advanced Light Source, a U.S. DOE Office of Science User Facility under contract no. DE-AC02-05CH11231.

Author Contributions

B. L. conceived and initiated this project, S. L., H. W., H. Z., W. L., and D. P. P. performed the sample growth and transport data measurements, Y. Z. and J. S. O. performed the ARPES experiments with the help of J. D. under the guidance of R.J.B. and M. Y., G. T. M. performed the single crystal X-ray diffraction experiments, G. L. performed the theoretical calculations. S. L. M. Y, and B. L. wrote the paper with input from all authors.

Competing Interests

The authors declare no competing interests.

Figure Legends

References

  1. [1]Splendiani, A. et al. Emerging photoluminescence in monolayer MoS₂. Nano Lett. 10, 1271–1275 (2010).DOI
  2. [2]Jaramillo, T. F. et al. Identification of active edge sites for electrochemical H₂ evolution from MoS₂ nanocatalysts. Science 317, 100–102 (2007).pubmed.ncbi.nlm.nih.gov/17615351
  3. [3]Deng, K. et al. Experimental observation of topological Fermi arcs in type-II Weyl semimetal MoTe₂. Nat. Phys. 12, 1105–1110 (2016).DOI
  4. [4]Wang, Z. et al. MoTe₂: a type-II Weyl topological metal. Phys. Rev. Lett. 117, 056805 (2016).DOI
  5. [5]Tang, S. et al. Quantum spin Hall state in monolayer 1T′-WTe₂. Nat. Phys. 13, 683–687 (2017).DOI
  6. [6]Wang, Y. et al. Structural phase transition in monolayer MoTe₂ driven by electrostatic doping. Nature 550, 487–491 (2017).DOI
  7. [7]Zhao, C. et al. Enhanced valley splitting in monolayer WSe₂ due to magnetic exchange field. Nat. Nanotechnol. 12, 757–762 (2017).DOI
  8. [8]Fatemi, V. et al. Electrically tunable low-density superconductivity in a monolayer topological insulator. Science 362, 926–929 (2018).DOI
  9. [9]Xu, S.-Y. et al. Electrically switchable Berry curvature dipole in the monolayer topological insulator WTe₂. Nat. Phys. 14, 900–906 (2018).DOI
  10. [10]Sajadi, E. et al. Gate-induced superconductivity in a monolayer topological insulator. Science 362, 922–925 (2018).DOI
  11. [11]Hou, W. et al. Strain-based room-temperature non-volatile MoTe₂ ferroelectric phase change transistor. Nat. Nanotechnol. 14, 668–673 (2019).DOI
  12. [12]Yu, W. et al. Chemically exfoliated VSe₂ monolayers with room-temperature ferromagnetism. Adv. Mater. 31, 1903779 (2019).DOI
  13. [13]Choi, Y.-B. et al. Evidence of higher-order topology in multilayer WTe₂ from Josephson coupling through anisotropic hinge states. Nat. Mater. 19, 974–979 (2020).DOI
  14. [14]Wang, W. et al. Evidence for an edge supercurrent in the Weyl superconductor MoTe₂. Science 368, 534–537 (2020).DOI
  15. [15]Ali, M. N. et al. Large, non-saturating magnetoresistance in WTe₂. Nature 514, 205–208 (2014).DOI
  16. [16]Liu, W. et al. Enhanced superconductivity in the Se-substituted 1T-PdTe₂. Phys. Rev. Mater. 5, 014802 (2021).DOI
  17. [17]Wu, H. et al. Spacing dependent and doping independent superconductivity in intercalated 1T two dimensional SnSe₂. 2D Mater. 6, 045048 (2019).arxiv.org/abs/1903.08036
  18. [18]Zhang, C. et al. Strain distributions and their influence on electronic structures of WSe₂–MoS₂ laterally strained heterojunctions. Nat. Nanotechnol. 13, 152–158 (2018).DOI
  19. [19]Edelberg, D. et al. Approaching the intrinsic limit in transition metal diselenides via point defect control. Nano Lett. 19, 4371–4379 (2019).DOI
  20. [20]Yu, Z. et al. Analyzing the carrier mobility in transition-metal dichalcogenide MoS₂ field-effect transistors. Adv. Funct. Mater. 27, 1604093 (2017).DOI
  21. [21]Lin, Z. et al. Defect engineering of two-dimensional transition metal dichalcogenides. 2D Mater. 3, 022002 (2016).DOI
  22. [22]Wang, X. et al. Deriving 2D M₂X₃ (M= Mo, W, X= S, Se) by periodic assembly of chalcogen vacancy lines in their MX₂ counterparts. Nanoscale 12, 8285–8293 (2020).DOI
  23. [23]Liang, Q., Zhang, Q., Zhao, X., Liu, M. & Wee, A. T. S. Defect engineering of two-dimensional transition-metal dichalcogenides: applications, challenges, and opportunities. ACS Nano 15, 2165–2181 (2021).DOI
  24. [24]Liu, E. et al. Giant anomalous Hall effect in a ferromagnetic kagome-lattice semimetal. Nat. Phys. 14, 1125–1131 (2018).DOI
  25. [25]Little, A. et al. Three-state nematicity in the triangular lattice antiferromagnet Fe₁/₃NbS₂. Nat. Mater. 19, 1062–1067 (2020).DOI
  26. [26]Zhu, H. et al. New Mo₆Te₆ Sub-nanometer-diameter nanowire phase from 2H-MoTe₂. Adv. Mater. 29, 1606264 (2017).DOI
  27. [27]Tiwari, R. K., Yang, J., Saeys, M. & Joachim, C. Surface reconstruction of MoS₂ to Mo₂S₃. Surf. Sci. 602, 2628–2633 (2008).
  28. [28]Avsar, A. et al. Defect induced, layer-modulated magnetism in ultrathin metallic PtSe₂. Nat. Nanotechnol. 14, 674–678 (2019).DOI
  29. [29]Zhang, J. et al. Distorted monolayer ReS₂ with low-magnetic-field controlled magnetoelectricity. ACS Nano 13, 2334–2340 (2019).DOI
  30. [30]Jung, Y., Zhou, Y. & Cha, J. J. Intercalation in two-dimensional transition metal chalcogenides. Inorg. Chem. Front. 3, 452–463 (2016).DOI
  31. [31]Zhang, Q., Mei, L., Cao, X., Tang, Y. & Zeng, Z. Intercalation and exfoliation chemistries of transition metal dichalcogenides. J. Mater. Chem. A 8, 15417–15444 (2020).DOI
  32. [32]Wang, Z., Li, R., Su, C. & Loh, K. P. Intercalated phases of transition metal dichalcogenides. SmartMat 1, e1013 (2020).DOI
  33. [33]Novello, A. M. et al. Stripe and short-range order in the charge density wave of 1T-CuₓTiSe₂. Phys. Rev. Lett. 118, 017002 (2017).DOI
  34. [34]Liao, J.-H., Zhao, Y.-C., Zhao, Y.-J., Yang, X.-B. & Chen, Y. Doping induced charge density wave in monolayer TiS₂ and phonon-mediated superconductivity. J. Appl. Phys. 127, 044301 (2020).DOI
  35. [35]Bhoi, D. et al. Interplay of charge density wave and multiband superconductivity in 2H-PdₓTaSe₂. Sci. Rep. 6, 24068 (2016).DOI
  36. [36]Zhu, L. et al. Superconductivity in potassium-intercalated Tᵈ-WTe₂. Nano Lett. 18, 6585–6590 (2018).DOI
  37. [37]Nair, N. L. et al. Electrical switching in a magnetically intercalated transition metal dichalcogenide. Nat. Mater. 19, 153–157 (2020).
  38. [38]Sanikop, R., Budumuru, A. K., Gautam, S., Chae, K. H. & Sudakar, C. Robust ferromagnetism in Li-intercalated and-deintercalated MoS₂ nanosheets: implications for 2D spintronics. ACS Appl. Nano Mater. 3, 11825–11837 (2020).DOI
  39. [39]Yim, C. et al. High-performance hybrid electronic devices from layered PtSe₂ films grown at low temperature. ACS Nano 10, 9550–9558 (2016).
  40. [40]Chia, X. et al. Layered platinum dichalcogenides (PtS₂, PtSe₂, and PtTe₂) electrocatalysis: monotonic dependence on the chalcogen size. Adv. Funct. Mater. 26, 4306–4318 (2016).DOI
  41. [41]Wang, Z., Li, Q., Besenbacher, F. & Dong, M. Facile synthesis of single crystal PtSe₂ nanosheets for nanoscale electronics. Adv. Mater. 28, 10224–10229 (2016).DOI
  42. [42]Li, Y. et al. Topological origin of the type-II Dirac fermions in PtSe₂. Phys. Rev. Mater. 1, 074202 (2017).
  43. [43]Zhang, K. et al. Experimental evidence for type-II Dirac semimetal in PtSe₂. Phys. Rev. B 96, 125102 (2017).DOI
  44. [44]Zhao, Y. et al. High-electron-mobility and air-stable 2D layered PtSe₂ FETs. Adv. Mater. 29, 1604230 (2017).DOI
  45. [45]Yao, W. et al. Direct observation of spin-layer locking by local Rashba effect in monolayer semiconducting PtSe₂ film. Nat. Commun. 8, 14216(2017).DOI
  46. [46]Wang, Y. et al. Monolayer PtSe₂, a new semiconducting transition-metal-dichalcogenide, epitaxially grown by direct selenization of Pt. Nano Lett. 15, 4013–4018 (2015).DOI
  47. [47]Zheng, H. et al. Visualization of point defects in ultrathin layered 1T-PtSe₂. 2D Mater. 6, 041005 (2019).DOI
  48. [48]Shawkat, M. S. et al. Thickness-independent semiconducting-to-metallic conversion in wafer-scale two-dimensional PtSe₂ layers by plasma-driven chalcogen defect engineering. ACS Appl. Mater. Interfaces 12, 14341–14351 (2020).DOI
  49. [49]Absor, M. A. U. et al. Defect-induced large spin-orbit splitting in monolayer PtSe₂. Phys. Rev. B 96, 115128 (2017).DOI
  50. [50]Sajjad, M., Singh, N. & Schwingenschlögl, U. Strongly bound excitons in monolayer PtS₂ and PtSe₂. Appl. Phys. Lett. 112, 043101 (2018).DOI
  51. [51]Xu, H. et al. Controlled doping of wafer-scale PtSe₂ films for device application. Adv. Funct. Mater. 29, 1805614 (2019).
  52. [52]Hikami, S., Larkin, A. I. & Nagaoka, Y. Spin-orbit interaction and magnetoresistance in the two-dimensional random system. Prog. Theor. Phys. 63, 707–710 (1980).DOI
  53. [53]Perdew, J. P., Burke, K. & Ernzerhof, M. Generalized gradient approximation made simple. Phys. Rev. Lett. 77, 3865 (1996).pubmed.ncbi.nlm.nih.gov/10062328

Paper details

vlnc:W_sqqkrug7
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents