Material radioactivity compilations, such as the one presented here, are important enablers of science. They are useful for the selection of radiopure materials used in the design and construction of low-energy rare-event search experiments. They allow researchers developing such experiments to save time on material studies and avoid costly duplication of effort. The data presented here were generated in support of the planned nEXO double-beta decay search. This work contains among the most restrictive constraints on the natural radioactivity content of materials of general interest to the low-radioactivity community, found in any tabulation of this kind. In this study, various techniques were employed; they are described here.

Introduction

Access to materials containing the smallest possible amount of radioactivity is important for a number of scientific and technical applications. Random energy deposits arising from minute amounts of primordial, cosmogenic, and man-made radioactivity in materials can limit the sensitivity of radiation detectors used in scientific, health, and national security applications. Unwanted radioactivity in materials can lead to quantum decoherence in superconducting quantum circuits [1]. The ever-present naturally-occurring radioisotopes 40K{}^{40}\mathrm{K}, 232Th{}^{232}\mathrm{Th}, and 238U{}^{238}\mathrm{U} and associated radioactive decay progeny are of particular concern for a broad range of applications. Below, we discuss a range of applications that require low-radioactivity materials. Searches for phenomena forbidden within the framework of the Standard Model of Particle Physics (SM) are a tool for the discovery of new physics, often without requiring large particle accelerators. Such experiments often play out at keV or MeV energy scales and involve searching for exceedingly rare phenomena. Because of this combination of circumstances, the avoidance of background events arising from radioactivity in and on the materials comprising the apparatus is an important and often time-consuming aspect of experiment planning, design, and construction. Radioactivity-induced background events often limit the achievable sensitivity by masking the signature of the phenomena of interest.

Searches for neutrinoless double-beta decay (0νββ0\nu\beta\beta) are a means to explore physics beyond the SM, and they require radiopure materials. The relevant energy for 0νββ0\nu\beta\beta is on the order of a few MeV [2]. Detection of this never-observed ultra-rare nuclear decay mode would demonstrate that neutrinos and anti-neutrinos are the same species, requiring physics beyond the SM. To be scientifically relevant, future searches aim for half-life sensitivities of 102710^{27} to 102810^{28} yr. At this level of stability, tonnes of decaying material will undergo only a few decays per year. Given the rarity of these decays, experiments are utilizing various techniques for active background suppression. However, as a starting point, all require the use of structural and technical components containing minimal amounts of radioactivity in order to not overwhelm them. To meet their extreme radiopurity requirements, proposed 0νββ0\nu\beta\beta experiments such as nEXO [3], LEGEND-1000 [4], and CUPID [5], conduct extensive materials screening campaigns to identify materials and components.

The work reported here was performed in support of the technical development of the planned nEXO experiment. This paper reports on the assay data for materials of interest to nEXO [3]. However, the reported data are of broad interest. Given its connection to nEXO, the paper briefly outlines the tools developed by this project to interpret the large body of radioactivity data and place it within the framework of a background rate compilation. This approach allows for real-time materials decision-making.

Material radioactivity compilations, similar to this one, have been published by various solar neutrino, double-beta decay and dark matter searches—BOREXINO [6], EDELWEISS [7], EXO-200 [8, 9], GERDA [10], LUX [11], LZ [12], Majorana Demonstrator [13], NEXt-100 [14], SNO [15], XENON100 [16], XENON1T [17], and XMASS [18]—to document the body of knowledge in selecting suitable low-radioactivity materials, which has been accumulated by the low background community. These compendia of material assay results provide future experiments with a general assessment of what is currently achievable with various low-radioactivity materials, an essential input for current and future low-background applications.

To provide useful constraints and driven by the technical complexity of modern experimental designs, numerous radioactivity measurements must be performed at the level of μ\muBq/kg or even nBq/kg across a variety of materials. Such material assays are technically challenging.

Two approaches are typically chosen to meet this analytical challenge: decay counting and atom counting. These approaches differ in what they determine and in the analytical sensitivity they reach. For experiments where backgrounds created by energetic β\beta and γ\gamma radiation are a concern, e.g., double-beta decay searches, 232Th{}^{232}\mathrm{Th} and 238U{}^{238}\mathrm{U} progeny are important background sources. These are primordial radioactive isotopes that have been present since before the formation of our solar system. These nuclides have half-lives of 14.0×10914.0 \times10^{9} yr and 4.468×1094.468 \times10^{9} yr, respectively, and are typically found in all materials at trace levels. To meet this analytical challenge, the effort described here utilized both approaches.

  1. Decay counting is based on the determination of the 40K{}^{40}\mathrm{K}, 228Ac{}^{228}\mathrm{Ac}, 212Pb{}^{212}\mathrm{Pb}, 212Bi{}^{212}\mathrm{Bi}, 208Tl{}^{208}\mathrm{Tl}, 234mPa{}^{234\mathrm{m}}\mathrm{Pa}, 226Ra{}^{226}\mathrm{Ra}, 214Pb{}^{214}\mathrm{Pb}, 214Bi{}^{214}\mathrm{Bi} decay rates. The conversion of activities into background event rates is often independent of assumptions about decay-chain equilibrium. While non-destructive, this approach typically offers limited sensitivity (tens of ppt for Th and U, or roughly the 100 μ\muBq/kg range), requires large samples (kg-scale) and is time-consuming (2–3 weeks per unique sample). The following techniques were used in this work: low background α\alpha and γ\gamma spectrometry and radon counting.

  1. The atom counting approach for natK{}^{\mathrm{nat}}\mathrm{K}, 232Th{}^{232}\mathrm{Th}, and 238U{}^{238}\mathrm{U} only requires limited amounts of samples (g-scale and smaller), offers fast turn-around (days to weeks per unique sample) and has excellent sensitivity (sub-ppt, equating to μ\muBq/kg or sub-μ\muBq/kg), but is destructive. This approach is generally sensitive to much lower activities than decay counting, but is only sensitive to the top of the 232Th{}^{232}\mathrm{Th} and 238U{}^{238}\mathrm{U} decay chains. The following techniques were used in this work: inductively coupled plasma mass spectrometry (ICP-MS), glow discharge mass spectrometry (GD-MS), and neutron activation analysis (NAA).

This work exploits both approaches to meet the analytical challenge. If decay-chain equilibrium is assumed, the high sensitivity of atom counting can be used to improve constraints on the lower-chain activities. However, assumptions about decay-chain equilibrium breakage need to be evaluated on a case-by-case basis. This evaluation must account for the chemical and physical properties (electrochemical potential, melting point, boiling point, possible oxidation states) of the material under study, as well as the associated naturally occurring radioisotopes with half-lives on or longer than the timescales relevant to the experiment and the processes. The processes used to purify the material also need to be considered. Equilibrium breakage is of particular importance in the 238U{}^{238}\mathrm{U} decay series. 226Ra{}^{226}\mathrm{Ra} and 210Pb{}^{210}\mathrm{Pb} can decay at higher or lower rates than 238U{}^{238}\mathrm{U}. The chemical or physical process responsible for the imbalance determines the type and extent of fractionation among decay-chain isotopes. As

an example, the EXO-200 experiment applied such an equilibrium assumption to all ICP-MS and NAA measurements; the pre-data-taking background rate predictions were later found to overlap with the data-derived rates [19]; in this instance, the success of that experiment justified the approach and the assumptions made about decay-chain equilibrium post hoc.

Thus, the choice of assay method must strike a balance between sensitivity and the risk of background misestimation due to decay-chain equilibrium breakage. Currently, no analysis approach that addresses both issues simultaneously exists.

Various assay installations are used in support of the study described here. They are operated by nEXO collaborating or associated institutions, some are above ground, some underground.

The sections below provide a summary of the tools, followed by an extensive compilation of results.

Gamma spectrometry

High-resolution γ\gamma-ray spectroscopy with high-purity germanium detectors (HPGe), or γ\gamma counting, provides a direct measurement of the Th and U progeny responsible for the emission of energetic, MeV-scale γ\gamma radiation. In particular, γ\gamma counting is directly sensitive to decays of 208Tl{}^{208}\mathrm{Tl} and 214Bi{}^{214}\mathrm{Bi}, isotopes in the natural radioactive decay chains of 232Th{}^{232}\mathrm{Th} and 238U{}^{238}\mathrm{U}, respectively. In cases where breakage of secular equilibrium exists, γ\gamma counting is the only way to determine the decay rates of the progeny, but with limited sensitivity.

High-sensitivity, low-background γ\gamma counters are located deep underground, where they are shielded from cosmic rays. Given the limited availability of underground γ\gamma counters, less-sensitive above-ground gamma counters are used to pre-screen high-purity materials or to analyze materials with less stringent radiopurity requirements.

Measurements presented here were obtained using two γ\gamma counters located in a surface laboratory at the University of Alabama (UA). The specifications of these counters are listed in Table I under Ge-II and Ge-III. Both are equipped with anti-coincident plastic scintillator cosmic-ray muon detectors with almost 4π4\pi coverage [22]. The sensitivity of these γ\gamma counters is limited by background from neutron-induced delayed-coincidence photons. In addition, some of the data were obtained by seven underground gamma counters. Ge-IV, operated by nEXO collaborators, is located on the 1500 m level of the Sanford Underground Research Facility (SURF). PGT, CWELL, Lively, Gopher, and Vue-des-Alpes (VdA) are operated by the SNOLAB Low Background Counting Facility [23] located 2100 m underground. The VdA counter, 80% of which was dedicated to the nEXO Project, was initially operated 620 m underground in the Vue-des-Alpes underground laboratory in Switzerland. One of the measurements presented here was performed with the GeMPI 2

NameEfficiency (rel %)609 keV1332 keV1461 keV2615 keVLocation
Ge-II60<7.6102.30.75UA
Ge-III1059.61.72.5<0.53UA
Ge-IV1110.330.480.190.25SURF
PGT550.580.221.40.50SNOLAB
CWELL800.041<0.009<0.008<0.007SNOLAB
Lively1071.030.1180.570.94SNOLAB
Gopher1203.00.0850.300.050SNOLAB
VdA1201.40.0591.30.51SNOLAB
GeMPI 2100<0.12<0.11<0.13<0.10LNGS

Table 1. Overview of the properties1 of HPGe detectors used to assay samples as presented in this work. All detectors are p-type. All detectors are coaxial, except for CWELL, which is a well detector. Data were provided by the detector operators. A description of GeMPI 2 has been published in [20, 21]. Relative efficiencies are based on original manufacturer-provided values. The background rates are quoted for various peak energies and are per unit mass of the Ge crystal.

counter at the INFN Gran Sasso National Laboratory (LNGS), 1400 m underground. The number of assays performed with the Ge-IV and VdA counters was limited by extended periods during which these detectors were not operational.

ICP-MS

ICP-MS can identify and, with varying sensitivities, quantify almost all isotopes in the periodic table of nuclides, including K, Th, and U. The technique is based on the analysis of the distribution of ion momenta of a sample. ICP-MS is a destructive technique and typically requires the sample to be dissolved in acid before being introduced, as a fine-mist aerosol via a nebulizer, into the mass spectrometer using a stream of argon gas. In a plasma, ions are formed and extracted into a high-vacuum region, where, using ion lenses, they are focused into a beam and directed to the mass analyzer. The analyte components are then analyzed based on their mass-to-charge ratio. Calibration standards are used for quantitation either by using an external calibration curve, standard addition, or isotope dilution methods. The latter is the most accurate and precise method, applied to most of the ICP-MS assays reported here.

Because ICP-MS can detect 232Th{}^{232}\mathrm{Th}, 238U{}^{238}\mathrm{U}, and natural K with high sensitivity when coupled with ultra-clean sample preparation procedures, it is widely employed in the realm of low-background experiments for detector material validation, e.g., [24, 25, 26, 27, 28, 29, 30]. Quantities of material on the order of a gram or a fraction of a gram are required to perform assays at sensitivities relevant to the ultra-low-background community. The advantage of analyzing very small amounts, however, raises the question of how representative the analyzed mass is of a large mass of the material, and how homogeneity can be verified. In this work, whenever possible, ICP-MS analysis of multiple sub-samples was performed for materials intended to be used in large masses, where homogeneity could not be guaranteed. An industry-inspired approach to part sampling, as described in [31], is planned for implementation in nEXO. Analysis times are on the order of days, including the sample preparation, which is the most time-consuming aspect of the measurement process. The instrumental analysis requires only minutes, and multiple elements can be monitored in a single run. For the results reported here, sensitivities in the parts-per-trillion (ppt) and sub-ppt ranges have been routinely achieved for the assay of Th and U in materials. The best sensitivities for 232Th{}^{232}\mathrm{Th} and 238U{}^{238}\mathrm{U} determinations were obtained for a sample of heat-transfer fluid at 1.3 parts per quadrillion (ppq), or 5.3 nBq/kg, and 4.3 ppq, or 53 nBq/kg, respectively. Three collaborating facilities contributed ICP-MS capability to this study: Pacific Northwest National Laboratory (PNNL) in the USA, the IBS Center for Underground Physics (CUP) in Korea, and the Institute of High Energy Physics (IHEP) in China.

In addition to analyses of bulk radiopurity, ICP-MS can be leveraged to optimize and validate material manufacturing processes and cleaning procedures owing to its high sensitivity, relatively short analysis time, and rapid sample throughput via batching. In the work reported in [26, 27], over 300 unique assays were performed to understand the contamination of complex part processing, namely flexible cable manufacturing. These investigations allow for the ability to isolate the contaminating steps, to develop mitigating steps toward clean processing, and/or to develop surface cleaning techniques to remove contamination from surfaces.

NAA

Neutron activation analysis (NAA) is a well-proven, ultra-sensitive technique for trace-element detection and quantification. It involves irradiating a sample in a nuclear reactor, thereby transmuting stable or long-lived radioactive nuclides to those with comparatively short half-lives, such as 238U^{238}\mathrm{U} to 239Np^{239}\mathrm{Np}. It can be used to detect chemical impurities with large neutron-capture cross sections and activation products with sufficiently long lifetimes. Knowledge of the neutron flux, activation duration, and capture cross sections allows for the conversion of measured activation-product activities into concentrations of the parent element. Aside from careful surface cleaning, no chemical sample preparation is required. Typical sample mass is on the order of a few grams. As with ICP-MS, it measures the long-lived heads of the natural decay series. The NAA effort is conducted by the UA group, using the MIT research reactor MITR as the neutron source. For 232Th^{232}\mathrm{Th} and 238U^{238}\mathrm{U}, ppt-sensitivities have been routinely achieved, with sub-ppt results reached in exceptional cases.

The EXO-200 double beta decay experiment made extensive use of NAA in their materials assay campaign [8, 9]. Apart from the improvements described below, the work presented here largely uses the same technique as EXO-200. For an overview of the method, see the two EXO-200 Refs. [8, 9].

Compared to EXO-200, a new analysis code was developed for NAA data. Analysis is done with a system of ROOT macros, simultaneously fitting peaks for multiple activities, similar to the EXO-200 code [32], which is still under active development. The ROOT macros have high automation and can fit many peaks in many spectra rapidly. Based on the significance of the candidate peak, it automatically finds peaks in γ\gamma spectra. The automation features enable the rapid analysis of multiple isotopes.

To increase sensitivity for 238U^{238}\mathrm{U}, γγ\gamma\gamma-coincidence counting can be used. This approach makes use of correlated γ\gamma emissions observed in the level scheme of 239Np^{239}\mathrm{Np}. A computational study showed, for example, that this method can enhance U-sensitivity by a factor of 8 for the activation analysis of sapphire [33], where large side-activities limit traditional NAA sensitivity. A measurement with two HPGe detectors, performed on an activated sapphire sample (# 47 in Table IV), demonstrated the validity of the method when compared with a previous assay (# 46 in Table IV) that did not use coincidence counting [34].

#MaterialTechniqueInstituteU early [ppt]U late [ppt]Th [ppt]K [ppb]
1†SCS OFHC C10100A.G. GeUA<20<20<43<40
2SCS OFHC C10100GD-MSNRC<20<20<20<20
3SCS OFHC C10100A.G. GeUA<8.7<28<28<32
4Canberra Ge crystal holderGD-MSNRC<30<30<30<0.60
5Norddeutsche Affinerie OFRP, EXO-200 cryostatGD-MSNRC<20<20<20<0.60
6GRIKIN Advanced Materials, target for PECVDICP-MSIHEP<0.34<0.80
7Electroformed by PNNLICP-MSPNNL<0.00940.0060±0.0010
8Anode before electrolysisGD-MSNRC<20<20<20<0.90
9Anode before electrolysisICP-MSUSeoul3.1±1.12.4±0.9
10Cathode after electrolysisGD-MSNRC<20<20<20<0.90
11Cathode after electrolysisICP-MSUSeoul<0.84<0.90
12Cast and rolled wireGD-MSNRC<20<20<20<0.80
13Cast and rolled wireICP-MSUSeoul<0.341.6±1.1
14Electrolytic cathode (ASTM B115 and BS EN 1978)GD-MSNRC<30<30<30<0.80
15Electrolytic cathode (ASTM B115 and BS EN 1978)GD-MSNRC<30<30<30<0.80
16Electrolytic cathode (ASTM B115 and BS EN 1978)GD-MSNRC<30<30<30<1.0
17†AnodeU.G. GeVdA15.8±1.127.8±2.23.7±1.9
18†AnodeU.G. GeVdA<0.406.9±2.6<7.4
19AnodeICP-MSCUP<16104±9
20AnodeICP-MSCUP<9.6<21
21AnodeICP-MSCUP<11<20
22†CathodeU.G. GeVdA<1.2<2.23.0±2.0
23CathodeICP-MSCUP<7.1<11
24CathodeICP-MSPNNL0.254±0.0080.13±0.06
25CathodeGD-MSNRC<20<20<20<0.70
26VSMPO-AVISMA titanium (VT1-00)GD-MSNRC1000−500+10001000^{+1000}_{-500}<80<4.0
27CVMR CVD nickel, raw dilutionICP-MSPNNL<1.6<80<0.99
28CVMR CVD nickel, after matrix separationICP-MSPNNL0.040±0.0160.80±0.300.91±0.10
29Western Grade CVMR CVD nickel [44]ICP-MSPNNL<0.0980.065±0.0290.91±0.10
30Canberra high purityGD-MSNRC<100<100<5.0
31†Materion Advanced Chemicals pellets, 99.999% pureU.G. GeSURF70±40<410490±120130±90
32Norsk HydroGD-MSNRC<70<70<5.0
33Norsk HydroGD-MSNRC<60<70<5.0
34Norsk HydroGD-MSNRC<80<90<5.0
35Norsk HydroICP-MSPNNL145±9134±11<5.0
36Norsk HydroICP-MSPNNL160±60<430<5.0
37Norsk HydroICP-MSPNNL145.0±2.1366±32
38El-Cat SC wafer, high resistivity float zone (D161)NAAUA<0.63<0.330.50±0.06
39Topsil SC, float zone, 33-1204-10 seed endICP-MSPNNL0.74±0.263.4±1.12.6±0.7
40Topsil SC, float zone, 33-1204-40 centralICP-MSPNNL1.0±0.42.6±0.62.0±0.7
41Topsil SC, float zone, 33-1204-40 central, machined by McCarter MachineNAAUA<1.8<0.167.1±0.7
42Topsil SC, float zone, 33-1204-40 non-seed endICP-MSPNNL1.12±0.153.3±0.43.6±1.2
No.MaterialMethodLaboratory238^{238}U232^{232}Th40^{40}K226^{226}Ra
43GT Advanced Technology LIGONAAUA<1.8<1.86.0±1.26.0 \pm1.29.5±2.29.5 \pm2.21800±12001800 \pm1200
44GT Advanced Technology crackleNAAUA<270<270<1100<110018001800±1200\pm1200
45Saint-Gobain Crystals, as-grownNAAUA(2.6±0.4)×104(2.6 \pm0.4)\times10^{4}8.1±2.88.1 \pm2.83.0±1.13.0 \pm1.1<1.4<1.4
46Saint-Gobain Crystals, ground, cut, annealedNAAUA5.1±3.85.1 \pm3.8<0.10<0.103.0±1.13.0 \pm1.1<1.4<1.4
47Saint-Gobain Crystals, ground, cut, annealed [34]NAATUNL<1.4<1.40.53±0.320.53 \pm0.32(3.3±0.4)×104(3.3 \pm0.4)\times10^{4}1800±6001800 \pm600
48Saint-Gobain Crystals alumina (SA27628, lot 1605)A.G. GeUA<790<790(3.3±0.4)×104(3.3 \pm0.4)\times10^{4}6100±15006100 \pm1500<270<270
49Saint-Gobain Crystals alumina (SA19645, lot 1555.2)A.G. GeUA<270<2701800±6001800 \pm600<580<5802600±6002600 \pm600
50Saint-Gobain Crystals alumina (SA27335, lot 1617.2)A.G. GeUA2600±6002600 \pm6006500±13006500 \pm1300<1200<1200<1200<1200
51Precision Sapphire TechnologiesNAAUA990±100990 \pm100410±40410 \pm403.4±1.63.4 \pm1.62900±332900 \pm33
52SIOM molten, re-formed natural quartzNAAUA340±50340 \pm5011.7±1.711.7 \pm1.7290±33290 \pm334.3±0.54.3 \pm0.5
53Corning UV grade (7980 1-D)NAAUA550±50550 \pm504.3±0.54.3 \pm0.50.55±0.060.55 \pm0.063.09±0.153.09 \pm0.15
54Heraeus Spectrosil 2000NAAUA<1.4<1.4<0.11<0.110.55±0.060.55 \pm0.063.09±0.153.09 \pm0.15
55SNF Heraeus Suprasil 300ICP-MSPNNL23.6±0.623.6 \pm0.64.40±0.204.40 \pm0.203.09±0.153.09 \pm0.1513.00±0.2013.00 \pm0.20
56SNF Heraeus Suprasil 300, Si CVD @ 530 ∘C530\,^\circ\mathrm{C}, Ti and Pd end metalizedICP-MSPNNL5.41±0.105.41 \pm0.107.1±0.57.1 \pm0.513.00±0.2013.00 \pm0.2078.8±1.178.8 \pm1.1
57SNF Heraeus Suprasil 300, Si CVD @ 580 ∘C580\,^\circ\mathrm{C}, Ti and Pd end metalizedICP-MSPNNL10.6±0.410.6 \pm0.47.60±0.307.60 \pm0.3078.8±1.178.8 \pm1.1<6000<6000
58MBNL Heraeus Suprasil 300ICP-MSPNNL0.220±0.0200.220 \pm0.0200.72±0.090.72 \pm0.09<0.63<0.63<2800<2800
59MBNL Heraeus Suprasil 300, aSi CVD @ 550 ∘C550\,^\circ\mathrm{C}, no metalizationICP-MSPNNL0.540±0.0300.540 \pm0.0300.82±0.060.82 \pm0.0615.40±0.2015.40 \pm0.20<6000<6000
60MBNL Heraeus Suprasil 300, aSi CVD @ 550 ∘C550\,^\circ\mathrm{C}, Ti and Pd end metalizedICP-MSPNNL4.30±0.204.30 \pm0.202.00±0.162.00 \pm0.167.90±0.207.90 \pm0.20<2800<2800
61SCC resin, cured-ESM611+A.G. GeUA<350<350<2800<2800<6000<6000<6000<6000
62SCC resin, cured-ESM611+A.G. GeUA<160<160450±230450 \pm230<990<990<1100<1100
63SCC resin, cured-ESM611+U.G. GeSNOLAB100100<320<320<170<170<280<280
64SCC resin, cured-ESM70A.G. GeUA<1700<1700<1400<1400<4200<4200<4200<4200
65SCC resin, cured-ESM70A.G. GeUA<130<130<430<430<220<220<220<220
66SCC resin, cured-ESM70U.G. GeSNOLAB<73<73740±220740 \pm220<170<170<170<170
67SCC resin, cured-862/81kA.G. GeUA<720<720<1700<1700<9400<9400<9400<9400
68SCC resin, cured-862/81kA.G. GeUA<300<300<240<240<100<100<100<100
69SCC resin, cured-862/81kU.G. GeSNOLAB<200<200<160<160<160<160<160<160
70SCC resin, cured-862/81kU.G. GeVdA<6.0<6.0<8.3<8.3<21<21<21<21
71Mitsubishi Rayon Pyrofil fiberA.G. GeUA<350<350<890<890<2580<2580<5100<5100
72Mitsubishi Rayon Pyrofil fiberU.G. GeSNOLAB<250<250510±200510 \pm200<640<640<640<640
73Mitsubishi Rayon Pyrofil fiberU.G. GeVdA82±3482 \pm34280±90280 \pm90670±170670 \pm1702580±902580 \pm90
74Grafil fiber (34-12K, lot 2700I)A.G. GeUA<230<230<340<3401600±5001600 \pm500<1600<1600
75Grafil fiber (34-12K, lot 2700I)U.G. GeSNOLAB104104<240<2402150±2202150 \pm220<280<280
76Grafil fiber (34-12K, lot 2700I)U.G. GeVdA40±1440 \pm14130±40130 \pm401080±1001080 \pm100<280<280
77Grafil fiber (34-12K R, lot 2922I)A.G. GeUA<140<140420±310420 \pm3101717<270<270
78Grafil fiber (34-12K R, lot 2922I)U.G. GeSNOLAB<140<140<110<110<25<25<860<860
79Grafil fiber (34-12K R, lot 2922I)U.G. GeVdA<110<110<110<110<25<25<410<410
80EPON 862 resinA.G. GeUA<110<110<110<110<25<25<410<410
81Hexcel IM-7-GP-6k fiberA.G. GeUA<5700<5700<5000<5000<7500<7500<860<860
82Tenax HTS40-12k fiber + EPON 862-WY resin, plateU.G. GeSNOLAB<550<550<4400<4400<990<990<660<660
83Toray T700-12k fiber + EPON 862-W resin, tubeU.G. GeSNOLAB<990<990<6400<6400<990<990<410<410
84Toray T700-12k fiber + EPON 862-W resin, tubeU.G. GeSNOLAB<990<990<6400<6400<990<990<410<410
85Toray T700-12k fiber + EPON 862-W resin, tubeU.G. GeSNOLAB<140<140<6400<64001390±1501390 \pm1501800±4001800 \pm400
86Zoltek (PX30MF010, lot 1M14015)U.G. GeSNOLAB<140<140<6400<64001920±1301920 \pm130(1.26±0.13)×104(1.26 \pm0.13)\times10^{4}
No.MaterialMethodLabLocation238^{238}U232^{232}Th40^{40}K
87†Canberra o-ringsA.G. GeUA6.6±0.8×1046.6\pm0.8\times10^{4}1.7±0.7×1051.7\pm0.7\times10^{5}<2.0×104<2.0\times10^{4}
88Marco Rubber white FKM o-ring (V1012-154)A.G. GeUA(7.0±0.9)×104(7.0\pm0.9)\times10^{4}(1.37±0.19)×105(1.37\pm0.19)\times10^{5}(9.2±2.4)×104(9.2\pm2.4)\times10^{4}
89Marco Rubber off white FKM o-ring (PAI-9725-151)A.G. GeUA(2.33±0.24)×105(2.33\pm0.24)\times10^{5}(4.4±0.5)×104(4.4\pm0.5)\times10^{4}(2.19±0.24)×105(2.19\pm0.24)\times10^{5}
90Marco Rubber dark brown FKM o-ring (16110247)A.G. GeUA(2.41±0.24)×105(2.41\pm0.24)\times10^{5}(2.75±0.27)×105(2.75\pm0.27)\times10^{5}(8.4±1.4)×105(8.4\pm1.4)\times10^{5}
91Marco Rubber light brown FKM o-ring (EV17550304)A.G. GeUA(2.09±0.21)×105(2.09\pm0.21)\times10^{5}(1.01±0.10)×105(1.01\pm0.10)\times10^{5}(8.5±0.9)×105(8.5\pm0.9)\times10^{5}
92Marco Rubber off white FKM o-ring (TBD-152)A.G. GeUA(7.3±0.7)×104(7.3\pm0.7)\times10^{4}(1.17±0.17)×105(1.17\pm0.17)\times10^{5}(6.5±0.6)×105(6.5\pm0.6)\times10^{5}
93Marco Rubber white FKM o-ring (TBD-152)A.G. GeUA(5.1±0.5)×104(5.1\pm0.5)\times10^{4}(3.33±0.34)×104(3.33\pm0.34)\times10^{4}(1.15±0.24)×104(1.15\pm0.24)\times10^{4}
94†Marco Rubber white FFKM o-rings (Z1216-152)A.G. GeUA<1400<14007000±40007000\pm4000<2.3×104<2.3\times10^{4}
95†Marco Rubber black FFKM o-rings (Z1319-152)A.G. GeUA(9.5±1.1)×104(9.5\pm1.1)\times10^{4}(2.34±0.26)×105(2.34\pm0.26)\times10^{5}(1.34±0.22)×105(1.34\pm0.22)\times10^{5}
96Shanghai Red CoralA.G. GeUA<120<120310±180310\pm180<180<180
97†Jiangyin Golden HarvestA.G. GeUA100100
98SciCron ITO-coated (AC-300)ICP-MSPNNL6.7±1.06.7\pm1.07.0±0.77.0\pm0.7
99†DS semi-conductive-PE HV cable 2308U.G. GeVdA500±260500\pm260<970<970<1700<1700
100†DS semi-conductive-PE HV cable 2308U.G. GeVdA<180<180<750<750
101†DS semi-conductive-PE HV cable 2343, layers A and BU.G. GeSNOLAB<170<1701630±2901630\pm290<640<640
102†DS semi-conductive-PE HV cable 2343, layers A–CU.G. GeSNOLAB490490<380<380770±280770\pm280
103†DS semi-conductive-PE HV cable 2343, layers A–C, cleanedU.G. GeSNOLAB100100<340<340610±240610\pm240
104DS semi-conductive-PE HV cable 2353 (2014 batch), layers A–CNAAUA100±40100\pm4064±764\pm7350350
105DS semi-conductive-PE HV cable 2353 (2014 batch), layer ANAAUA440±200440\pm200370±40370\pm401990±2201990\pm220
106DS semi-conductive-PE HV cable 2353 (2014 batch), layer BNAAUA<110<11018.6±2.018.6\pm2.0132132
107DS semi-conductive-PE HV cable 2353 (2014 batch), layer CNAAUA760±330760\pm330900±100900\pm1002690±3002690\pm300
108†DS semi-conductive-PE HV cable 2353 (2014 batch), layers A–CU.G. GeSNOLAB<160<160<500<500<990<990
109†DS semi-conductive-PE HV cable 2353 (2023 batch), layers A–CA.G. GeUA<1.7×104<1.7\times10^{4}<580<580900±500900\pm500
110†DS semi-conductive-PE HV cable 2353, all layers (DUNE-NC)A.G. GeUA<4300<4300<330<330<1100<1100
111McMaster-Carr C-filled PTFE (8775K56)ICP-MSPNNL11.5±1.711.5\pm1.714.1±0.614.1\pm0.6
112Applied Plastics Technology C-filled PTFE (08120891)ICP-MSPNNL14.1±1.014.1\pm1.011.4±0.411.4\pm0.4
113CS Hyde 1% C-loaded semi-conductive UHMW PE (19-5F-BLK-24)ICP-MSPNNL4.47±0.274.47\pm0.272.3±0.42.3\pm0.4
114QEP (MCAM) TIVAR 1000 ESD, C-filled UHMW PEICP-MSPNNL224±32224\pm3210.1±1.410.1\pm1.4
115MCAM TIVAR ESD, C-filled UHMW PE (SHUMWPE-AS1, 205BK)ICP-MSPNNL242±32242\pm3210.1±1.410.1\pm1.4
116MCAM TIVAR ESD, C-filled UHMW PEICP-MSPNNL224±32224\pm3210.1±1.410.1\pm1.4
117Solvay Torlon 4200 (DP TR 4200 9 mm)NAAUA<190<190<200<200820±270820\pm270
118Solvay Torlon 4203 PAI (DP TR 4203 4 mm)NAAUA<550<550<450<4503800±7003800\pm700
119ARP Natural Semi PEI, Sabic Utem 1000 (PP RULT1000NA,250)NAAUA<15<15484±10484\pm10<28<28
120Ensign TECA PEI, Sabic Utem 1000 (TP RR00250X120000)NAAUA<15<159.5±2.39.5\pm2.3<28<28
121Ensinger TECA PEI, Sabic Utem 1000 (TP RR00250X120000)NAAUA<14<1428.5±3.428.5\pm3.453±353\pm3
122MCAM Duratron U1000 (PEI, Sabic Utem 1000 (PP RQ4203-PEI, Sabic Utem 1000 (BR-AR478-00187))NAAUA<580<580<28<28290±140290\pm140
123MCAM Duratron U1000 PEI, Sabic Utem 1000 (BR-AR478-00187)NAAUA<18<186767106±12106\pm12
124Nippon Micrometal Corporation Ausn 100 μm spheres (LF60)ICP-MSPNNL90±2090\pm2068±1468\pm14230±1100230\pm1100
125†Kester lead-free, no flux (14-7068-0062)U.G. GeSURF280±60280\pm60<75<75<1300<1300
126†Kester lead-free, no flux (14-7068-0062)U.G. GeSURF1100±5001100\pm500<110<110300300
127†Kester lead-free, no flux (14-7068-0062)ICP-MSPNNL<94<942.9±1.02.9\pm1.0<180<180
128†Alpha lead-free, no flux (147002)U.G. GeSURF1600±6001600\pm600<280<280<2820<2820
129†Alpha lead-free, no flux (147002)ICP-MSPNNL<180<1802.3±1.32.3\pm1.31160±2501160\pm250
130†Alpha lead-free, flux core (24-7068-6422)U.G. GeSURF180±100180\pm100<100<100<2100<2100
131†Alpha lead-free, flux core (24-7068-6422)U.G. GeSURF<480<480<310<310<2100<2100
132
CategoryNo.MaterialMethodLaboratoryUTh
Wires133†W. L. Gore AWG 28 Cu conductor, 0.015″ Teflon insulation (012749900)U.G. Ge<44<44<51<51<150<150
Wires134Ametek Al bonding, Al-1% Si alloy (109433 / A4)ICP-MSPNNL(1.4±0.4)×104(1.4 \pm0.4)\times10^{4}(7.7±1.3)×104(7.7 \pm1.3)\times10^{4}
Wires135Ametek gold bonding, 99.99% Au (10190)ICP-MSPNNL<230<23026±926 \pm9
Wires136Hamamatsu Sn-Au bump bondingICP-MSPNNL22±922 \pm96.0±3.06.0 \pm3.0
Wires137Hamamatsu Sn-Cu bump bondingICP-MSPNNL22±622 \pm6<14<14
Polyimide flex cables138†McMaster-Carr Kapton film (2271K5)A.G. GeUA<4400<4400(1.8±0.4)×104(1.8 \pm0.4)\times10^{4}<3700<3700
Polyimide flex cables139CS Hyde DuPont Kapton HN (18-5F-12″) [26]ICP-MSPNNL921±11921 \pm1186.0±1.386.0 \pm1.3
Polyimide flex cables140CS Hyde DuPont Kapton HN (18-5F-12″)ICP-MSIHEP961±12961 \pm1277.0±2.077.0 \pm2.0
Polyimide flex cables141CS Hyde DuPont Kapton HN (18-5F-12″)NAAUA1300±901300 \pm90140±70140 \pm70
Polyimide flex cables142DuPont Pyralux AP Cu-clad laminate, double-sided (8535R) [26]ICP-MSPNNL158±6158 \pm624.1±0.924.1 \pm0.9
Polyimide flex cables143DuPont Kapton 100HN [26]ICP-MSPNNL966±14966 \pm1489.8±3.289.8 \pm3.2
Polyimide flex cables144DuPont Kapton 100HN [26]ICP-MSPNNL931±5931 \pm5115.0±1.2115.0 \pm1.2
Polyimide flex cables145DuPont Kapton 300HN [26]ICP-MSPNNL1080±401080 \pm40250±8250 \pm844±1844 \pm18
Polyimide flex cables146DuPont Kapton 500HN [26]ICP-MSPNNL830±70830 \pm7073±773 \pm7
Polyimide flex cables147DuPont Kapton 200DR9, C-loadedICP-MSPNNL58±1058 \pm1045.2±2.345.2 \pm2.3
Polyimide flex cables148DuPont Kapton 300DR12, C-loadedICP-MSPNNL6900±5006900 \pm5004880±1704880 \pm170
Polyimide flex cables149DuPont Kapton 100XC, C-loadedICP-MSPNNL(1.62±0.11)×104(1.62 \pm0.11)\times10^{4}(1.70±0.04)×104(1.70 \pm0.04)\times10^{4}
Polyimide flex cables150DuPont Kapton 200HH, R&D line [26]ICP-MSPNNL12.3±1.912.3 \pm1.918.5±2.318.5 \pm2.334±1434 \pm14
Polyimide flex cables151DuPont Kapton XC KSW, C-loaded, R&D lineICP-MSPNNL(4.5±0.9)×104(4.5 \pm0.9)\times10^{4}(2.2±0.6)×104(2.2 \pm0.6)\times10^{4}
Polyimide flex cables152Sheldahl Novaclad, Cu clad, double-sided (146319-009) [26]ICP-MSPNNL283±21283 \pm2150±450 \pm4
Polyimide flex cables153Sheldahl/Multek 1000A 100CB, Ge-coated (147361)ICP-MSPNNL830±50830 \pm50627±10627 \pm10
Polyimide flex cables154Sheldahl/Multek 1500A HN (160759-009)ICP-MSPNNL<1.8×104<1.8\times10^{4}115±7115 \pm7
Polyimide flex cables155Fralock XC (0.001″), C-loadedICP-MSPNNL(1.2±0.4)×104(1.2 \pm0.4)\times10^{4}(1.4±0.4)×104(1.4 \pm0.4)\times10^{4}
Polyimide flex cables156Fralock Cirlex, Cu-clad (8010121083) [26]ICP-MSPNNL410±50410 \pm5071.4±2.171.4 \pm2.1
QFlex Taiflex custom two-layer cables (2FPDR2005JA)157Original cable (uncleaned)ICP-MSPNNL6200±1006200 \pm10063±563 \pm5
QFlex Taiflex custom two-layer cables (2FPDR2005JA)158Base material (copper clad PI) [27]ICP-MSPNNL9±49 \pm48±68 \pm6
QFlex Taiflex custom two-layer cables (2FPDR2005JA)159PNNL cleaned cableICP-MSPNNL60±2060 \pm2036.0±3.036.0 \pm3.0
QFlex Taiflex custom two-layer cables (2FPDR2005JA)160Base material (copper clad PI)ICP-MSPNNL3.9±0.93.9 \pm0.9<9.0<9.0
QFlex Taiflex custom two-layer cables (2FPDR2005JA)161Finished uncleaned cableICP-MSPNNL1300±3001300 \pm30016±616 \pm6
QFlex Taiflex custom two-layer cables (2FPDR2005JA)162Finished uncleaned cable, cleaned by QFlexICP-MSPNNL18.0±1.018.0 \pm1.018±518 \pm5
QFlex Taiflex custom two-layer cables (2FPDR2005JA)163Copper from base material (normalized to laminate mass)ICP-MSPNNL4.0±0.74.0 \pm0.71.2±0.71.2 \pm0.7
QFlex Taiflex custom two-layer cables (2FPDR2005JA)164Copper from uncleaned cable (normalized to laminate mass)ICP-MSPNNL1500±3001500 \pm30017±617 \pm6
QFlex Taiflex custom two-layer cables (2FPDR2005JA)165Copper from cleaned cable (normalized to laminate mass)ICP-MSPNNL12.0±3.012.0 \pm3.012±412 \pm4
QFlex Taiflex custom two-layer cables (2FPDR2005JA)166PI from base material (normalized to laminate mass)ICP-MSPNNL0.90±0.200.90 \pm0.201.1±0.51.1 \pm0.5
QFlex Taiflex custom two-layer cables (2FPDR2005JA)167PI from uncleaned cable (normalized to laminate mass)ICP-MSPNNL530±340530 \pm340<38±40<38 \pm40
QFlex Taiflex custom two-layer cables (2FPDR2005JA)168PI from cleaned cable (normalized to laminate mass)ICP-MSPNNL900±400900 \pm400<38<38
Other1693M flat cable (SL8802/-08-2013-5-CU-T)A.G. GeUA(1.34±0.33)×105(1.34 \pm0.33)\times10^{5}6900±9006900 \pm9002500±4002500 \pm400
Other170Cinch axial cable, one only (8F36-A105-XXX-ND)A.G. GeUA(6.8±2.0)×105(6.8 \pm2.0)\times10^{5}1800±1001800 \pm100<840<840
Other1713M twin axial cable, one only (8F36-A105-XXX-ND)A.G. GeUA<7.2×105<7.2\times10^{5}<2300<2300<840<840
Other1723M twin axial cable (8F36-A105-XXX-ND)A.G. GeUA<2.7×105<2.7\times10^{5}<3100<3100<2300<2300
Other173Meritec twin axial connectors (94824)A.G. GeUA<2.1×105<2.1\times10^{5}<560<560<2500<2500
Other174Meritec twin axial connectors (94824)A.G. GeUA<2.1×105<2.1\times10^{5}<560<560<2500<2500
Other175Samtec twin axial, connectors (HDR-218107-04-NVAC)A.G. GeUA3.6×1053.6\times10^{5}(1.89±0.20)×105(1.89 \pm0.20)\times10^{5}3200±11003200 \pm1100
Other176Samtec twin axial connectors (HDR-218107-04-NVAC)A.G. GeUA3.6×1053.6\times10^{5}1800±1001800 \pm100390±50390 \pm50
Other177Samtec custom twin axial, cable only (HDR-192192-03)A.G. GeUA3.7×1063.7\times10^{6}(4.5±0.4)×106(4.5 \pm0.4)\times10^{6}(2.5±0.5)×105(2.5 \pm0.5)\times10^{5}
Other178Samtec custom twin axial, connectors (HDR-192192-03)A.G. GeUA1.7×1061.7\times10^{6}(4.8±0.6)×105(4.8 \pm0.6)\times10^{5}(3.9±0.6)×105(3.9 \pm0.6)\times10^{5}

Table IV. TABLE IV. Table of radioassay. Additional isotopic data is listed in Table V for entries marked with †.

Radon Emanation

This effort quantifies the amount of 222Rn^{222}\mathrm{Rn} gas released from materials into the surrounding environment. The different methods used to acquire the results in Table IV are described below.

Electrostatic counters

Electrostatic counters (ESCs) collect ionized radon progeny that decay in the counter vessel and are electrostatically guided onto an alpha detector, where subsequent decays can be measured. Instruments operated by Laurentian University were initially built to assay radium content in water for SNO. These are described in [35, 36, 37]. Similar instruments at SLAC National Accelerator Laboratory (SLAC) are newly constructed by nEXO; these instruments are described by Anker et al. [38]. Both suites of instruments operate under the same principle.

The material to be assayed is placed in a gas recirculation loop with the ESC and a pump. The loop is pumped out, and a high-purity carrier gas (Ar/N2_2/He/Xe) is filled into the system at pressures between 20 mbar and 1 bar, depending on the compatibility of the sample and goal of the measurement. The pump recirculates the gas in the system, carrying the radon atoms from the sample to the electrostatic vessel. A large-area silicon photodiode in the ESC is biased with negative high-voltage to attract ionized progeny where they plate out, and subsequent α\alpha decays in the series may be detected. Decays that deposit energy on the photodiode create a proportional amount of charge signal that is amplified and recorded, along with the time of the event. Since the sample is connected to the ESC during the measurement, it is possible to observe all three natural decay series containing radon—222Rn^{222}\mathrm{Rn} with T1/2=3.8222 dT_{1/2}=3.8222\ \mathrm{d}, 220Rn^{220}\mathrm{Rn} with T1/2=55.6 sT_{1/2}=55.6\ \mathrm{s}, and 219Rn^{219}\mathrm{Rn} with T1/2=3.96 sT_{1/2}=3.96\ \mathrm{s}—using these instruments. Lower carrier gas pressures reduce the transport time for a given mass flow, thereby delivering the short-lived radon isotopes to the counting chamber before they decay.

The data analysis uses the α\alpha energies and times—from the decay of 218Po^{218}\mathrm{Po}, 216Po^{216}\mathrm{Po}, 214Po^{214}\mathrm{Po}, 212Po^{212}\mathrm{Po}, 212Bi^{212}\mathrm{Bi}, and 211Bi^{211}\mathrm{Bi}—to fit to the Bateman equations for the various radon decay series to determine the rate of radon emanation. The detectors are calibrated using a 222Rn^{222}\mathrm{Rn} source to determine the overall detection efficiency, which scales the counts detected to the actual rate of emanation. Detection sensitivities of 20 μ\muBq (supported steady-state activity) have been observed. The analysis and calibration are described in more detail by Anker et al. [38].

Liquid scintillation-based radon counting

The UA radon counting facility measures the radon emanation rate of material samples by counting delayed coincidences of 214Bi^{214}\mathrm{Bi} β\beta decay and 214Po^{214}\mathrm{Po} α\alpha decay (Bi-Po events) from 222Rn^{222}\mathrm{Rn} dissolved in organic liquid scintillator (LS).

A sample is first placed in an electropolished stainless-steel emanation chamber to allow radon to emanate into a boil-off nitrogen atmosphere for two weeks. The nitrogen, containing any emanated radon, is then transferred to a volume of LS using boil-off nitrogen as the carrier gas. A sparger promotes the transfer of the radon from the gas into the LS. The LS used is a mixture of dodecane (C12_{12}H26_{26}, 80% vol), pseudocumene (1,2,4-trimethylbenzene, 20% vol), and 1.5 g/L of PPO (2,5-diphenyloxazole). After bubbling the carrier gas through the LS, the LS is transferred to an acrylic counting cell, which is viewed by a Hamamatsu R1307 photomultiplier tube. Counting occurs in a lead-shielded dark box within a stainless steel enclosure to reduce the effects of external γ\gamma radiation and light.

Coincident 214Bi^{214}\mathrm{Bi} and 214Po^{214}\mathrm{Po} decays are identified by the amount of light detected, which indicates the energy of the decays, and the time between two consecutive light detections. The time difference is expected to follow an exponential distribution with a decay constant corresponding to the mean lifetime of 214Po^{214}\mathrm{Po} if the signals are due to Bi and Po decays. Data taking is divided into runs, each lasting approximately three days. An exponential fit to the coincidence times determines the radon concentration in the cell for each run. An exponential fit to all runs, where the individual rates are expected to diminish with the mean lifetime of 222Rn^{222}\mathrm{Rn}, is performed to determine the radon-induced rate at the time of loading. After accounting for detection and transfer efficiencies, the radon emanation rate of the sample is calculated. A detailed description of this approach is provided by Sazzad et al. [39]. A 90% CL detection limit of 1.6 mBq and minimal detectable activity of 3.0 mBq (both in terms of the supported steady state activity) have been reported by Sazzad et al. [39].

Inter-lab comparison

To ensure the reliability of the dataset, the correctness and consistency of the measurement results need to be verified. This is particularly important for a measurement program that relies on data collected across multiple laboratories. The quality control program described in this paper relied on comparative sample measurements.

The compatibility and correctness of the Ge detector results were tested by counting six samples, prepared at Laurentian University from activity-certified IAEA material [40]. The activity of the samples was not known to the analyzers. All samples were counted, in turn, using six low-background Ge detectors located at UA, and underground at SNOLAB, SURF, and Yangyang Underground Laboratory (Y2L), operated by CUP. Excluding the VdA detector at SNOLAB, which experienced reliability issues at the time of the study, the average ratio of measured to design activities was 0.89±0.07 (standard deviation). The average was taken over all detectors and all activities. Figure 1a shows the individual specific activities for all detectors and radionuclides. The horizontal lines indicate the design-specific activity of the samples; the shaded bands their uncertainty. The level of agreement is judged to be acceptable for this purpose.

Figure 1. (a) Non-destructive testing of standards containing primarily 40K^{40}\mathrm{K} (◆), 228Th^{228}\mathrm{Th} (●), and 238U^{238}\mathrm{U} (■). Pairs of points represent two samples of the same standard. Horizontal bars indicate the 1σ1\sigma calibrated activity of the standards. 40K^{40}\mathrm{K} is scaled by a factor of 0.5.

(b) Destructive testing of samples 139 to 141 (●), samples 195 and 196 (■), samples 185 to 187 (◆), and sample 7 (▷). Open markers are 232Th^{232}\mathrm{Th}; solid markers are 238U^{238}\mathrm{U}. Horizontal lines indicate averages where appropriate. Only one of the samples could be analyzed via NAA.

FIG. 1. Assay results from six HPGe detectors—VdA underground at SNOLAB, GeII and GeIII above ground at UA, GeIV underground at SURF, and CC1 and CC2 underground at Y2L—for three pairs of calibrated standards; and the results from three samples using destructive assay techniques—NAA at UA and ICP-MS at CUP, IHEP, and PNNL—of four samples.

The comparative study of ICP-MS and NAA capabilities used low-activity materials: electroformed Cu, a P-doped Si wafer, a processed Si wafer, and Kapton. Due to the low activity requirement, it did not benefit from activity-certified standard materials which are not

Sample (Table IV)232Th^{232}\mathrm{Th}/ppt238U^{238}\mathrm{U}/ppt
Kapton (139 to 141)101±341060±210
P-doped Si (195 and 196)0.305±0.0070.46±0.35
Processed Si (185 to 187)0.28±0.230.5±0.6
Copper (7)0.07±0.09

Table 2. TABLE II. Mean and standard deviation of measurements of samples for destructive testing comparison. Measured limits omitted from the mean.

available at these low-activity levels. Therefore, it only tested assay compatibility between the participating labs, within the heterogeneity of the samples tested. Measurements performed at UA using NAA and at Y2L, IHEP, and PNNL using ICP-MS are compared.

Figure 1a shows the distribution of analysis results. Due to interfering side activities, NAA could only be performed on the Kapton sample. As expected, due to the smallness of the concentrations tested, the variability is greater than observed for Ge counting. The average, with standard deviation, measured activity of the four test samples are listed in Tab. II. The IHEP measurement of 232Th^{232}\mathrm{Th} in the copper sample is likely anomalous. The PNNL measurement employs an efficiency tracer and consistently measures ppq levels of uranium and thorium in electroformed copper, implying that the IHEP sample suffered from some external contamination rather than a fundamental limit to their sensitivity. We highlight this discrepancy to emphasize the need for repeated, competitive testing of important samples with such low levels of residual contamination.

Data interpretation

The radioactivity data set reported here has intrinsic value. It is useful for multiple projects and differing scientific applications. However, it is instructive to put the data in some context. Such context is provided by the procedures put into place by the nEXO Collaboration, designed to interpret the radioactivity data and answer the question “what is good enough?”. An online database, with associated applications, can be used to convert specific activities into background rates in real time [41]. Its associated applications enable material acceptance decisions, formalize material analysis requests, communicate assay completion, and enable background rate accounting between major simulation updates. An application enables simplified acceptance decisions using a web browser and the database content.

Coupled with GEANT4-based detector simulations, also stored in the database, the radioactivity data can be converted into component-specific background event rates for various event classes, fiducial detector masses, and energy windows. The results are presented as a large spreadsheet, which serves as the interface to the engineering component of the project. Component-specific probability density functions (PDFs) are stored in the same database and then used to convert decay rates into event rates. All non-linear aspects of the background estimation are contained in the PDFs. The database and its associated applications, in contrast, aggregate the product of component mass, specific activities, and hit efficiencies as a linear combination of all component background rates.

During development, the experiment design is evolving. For nEXO, significant upgrades to the detailed detector and background models were made infrequently, primarily for major publications or reviews. The database bookkeeping function allows for continuous development of the background model between simulation updates. This is done by assigning hit-efficiency proxies to new detector regions and incorporating them into an approximate background model. It has been found that the background rates of major model updates are approximated reasonably well by the running model. This approach enables real-time decision-making on new detector components during the design phase, and not only when major model updates occur. It leaves documentation in the form of the computer-generated background rate spreadsheet summary.

The database and associated suite of applications allow nEXO to identify the leading background contributors in real time. Within nEXO, this capability has been used to assign assay priorities and manage the various analysis laboratories. The database is online, and its various capabilities are available to all collaborators. The question of “what is the current background rate” can be answered at any time and is entirely data-driven.

Results

Hundreds of materials have been measured for the R&D of nEXO using the techniques described above. The results of these measurements have been stored in the nEXO Materials Database [41]. The assay results for early chain 238U^{238}\mathrm{U}, late chain 238U^{238}\mathrm{U} (226Ra^{226}\mathrm{Ra}), 232Th^{232}\mathrm{Th}, and 40K^{40}\mathrm{K} are shown in Table IV. Results for other isotopes, corresponding to entries in Table IV that are flagged with a † following their number, are shown in Table V. Radon counting results, together with some from EXO-200 that had not yet been published, are shown in Table VI. Results are shown following the precision and rounding convention of Ref. [42]. All uncertainties are 1σ1\sigma. Limits are calculated following the prescription of Navas et al. [42] at the 90% C.L., except for results that are less than −3σ-3\sigma, for which the limit shown is 1.645σ. These results, all in Table V, are indicated with a ~. For many results presented as limits, the central value and associated uncertainty are available upon request. To save space, abbreviations have been used in Table IV and Table VI. Descriptions of the abbreviations used are provided in Table III.

AbbreviationDescription
A.G. GeAbove Ground Germanium Counting
APTAdvanced Polymer Technologies (Now MCAM)
AWGAmerican Wire Gauge
ASICApplication-specific Integrated Circuit
BNLBrookhaven National Laboratory
BPBoedeker Plastics
CASChemical Abstracts Service Registration Number
CMOSComplementary Metal-Oxide-Semiconductor
CUPIBS Center for Underground Physics
CVDChemical Vapor Deposition
DPDrake Plastics
DSDielectric Sciences
DUNEDeep Underground Neutrino Experiment
ECElectro Static Dissipative
ESCElectrostatic Collection
ESDElectrically Conductive
FBKFondazione Bruno Kessler
FEFrontend Electronics
FFKMPerfluoroelastomer
FKMFluoroelastomer (Viton)
GD-MSGlow Discharge Mass Spectrometry
HSSCHigh Stability Silicon Capacitors
HVHigh Voltage
ICP-MSInductively Coupled Plasma Mass Spectrometry
IHEPInstitute of High Energy Physics
IMEInstitute of Microelectronics
IPInterstate Plastics
ITOIndium Tin Oxide
IZMInstitut für Zuverlässigkeit und Mikrointegration
LIGOLaser Interferometer Gravitational-Wave Observatory
LNGSLaboratori Nazionali del Gran Sasso
LULaurentian University
LZLUX-ZEPLIN Experiment
MBNLMarvell Berkeley Nanofabrication Laboratory
MCAMMitsubishi Chemical Advanced Materials
MIGMetal Inert Gas (Welding)
MOSISMetal Oxide Semiconductor Implementation Service
MPIKMax-Planck-Institut für Kernphysik
MPPCMulti-Pixel Photon Counters
NAANeutron Activation Analysis
NCNonconducting (defective conductor)
NRCNational Research Council Canada
OFHCOxygen-free High-conductivity
OFRPOxygen-free radiopure [43]
PAIPolyamide-imide
PCBPrinted Circuit Board
PCTFEPolychlorotrifluoroethylene
PECVDPlasma-enhanced CVD
PEPolyethylene
PEIPolyetherimide
PIPolyimide
PMTPatz Materials and Technologies
PNNLPacific Northwest National Laboratory
PPProfessional Plastics
PTFEPolytetrafluoroethylene (Teflon)
QEPQuadrant Engineering Plastic
RMDRadiation Monitoring Devices
SAESSocietà Apparecchi Elettrici e Scientifici
SCSingle Crystal
SCCSpencer Composites Corporation
SCSSouthern Copper and Supply
SIOMShanghai Institute of Optics and Fine Mechanics
SiPMSilicon Photomultipliers
SLACSLAC National Accelerator Laboratory
SNFStanford Nanofabrication Facility
SURFSanford Underground Research Facility
TIGTungsten Inert Gas (Welding)
TMCTechnical Marketing Company
TSMCTaiwan Semiconductor Manufacturing Company
TUNLTriangle University Nuclear Laboratory
UAUniversity of Alabama
U.G. GeUnderground Germanium Counting
UHMWUltra-high-molecular-weight
UKUniversity of Kentucky
USeoulUniversity of Seoul
UVUltraviolet
VCSELVertical-cavity surface-emitting Laser
VdAVue-des-Alpes detector operated by the University of Bern and later SNOLAB

Table III. Table of abbreviations used in Tab. IV and Tab. VI

#26Al^{26}\mathrm{Al}60Co^{60}\mathrm{Co}110mAg^{110m}\mathrm{Ag}137Cs^{137}\mathrm{Cs}210Pb^{210}\mathrm{Pb}210Po^{210}\mathrm{Po}
10.102±0.0350.102\pm0.035
30.05±0.040.05\pm0.04
17<0.0054<0.00540.008±0.0050.008\pm0.005
18<0.0066<0.0066<0.011<0.011710±70710\pm70
22<0.0033<0.0033<0.010<0.010
310.34±0.180.34\pm0.180.70±0.230.70\pm0.23<0.23<0.23<0.18<0.18<5.9<5.9
44<0.25<0.254.0±1.84.0\pm1.83.0±1.53.0\pm1.5
48<1.0<1.0<5.4<5.4<5.6<5.6
49<0.30<0.30<3.4<3.42.9±1.52.9\pm1.5
50<2.4<2.4<3.2<3.2<5.5<5.5
61<4.1<4.1<10<10
62<1.3∼<1.3\sim<2.2<2.2
63<0.11<0.11<0.44<0.44
64<13<13<7.6<7.6
65<0.25<0.25<2.1<2.1
66<0.074<0.074<0.27<0.27
67<17<17<19<19
68<0.14<0.14<1.6<1.6
69<0.078<0.078<0.14<0.14
70<0.0060<0.0060<0.094<0.094
71<8.0<8.0<11<11
72<0.48<0.48<0.51<0.51
73<0.22<0.22<1.0<1.0
74<2.8<2.8<1.5<1.5
75<0.18∼<0.18\sim<0.26<0.26
76<0.13<0.13<0.54<0.54
77<0.31<0.31<1.3<1.3
78<0.062<0.062<0.47<0.47
79<0.10<0.100.62±0.230.62\pm0.23
80<0.19<0.19<1.8<1.8
81<140<140<78<78
82<0.41<0.41<2.3<2.3
83<5.5<5.5<10<10
84<0.88<0.88<5.0<5.0
85<0.20∼<0.20\sim<0.099<0.099
86<0.93<0.93<0.67<0.67
87<22<22<20<20
94<13<13<7.0<7.0
95<30∼<30\sim<54<54
96<0.77∼<0.77\sim
97<0.31<0.31<0.69<0.69
99<1.4<1.4<2.1<2.1
100<0.10<0.10<1.3<1.3
101<0.14<0.14<0.64<0.64
102<0.20<0.20<0.77<0.77
103<0.078<0.078<0.82∼<0.82\sim
108<0.11<0.11<0.95<0.95
1093.0±1.73.0\pm1.7<140<140
1105.2±1.85.2\pm1.8<0.20<0.20
125<0.27<0.27<0.096<0.096<0.41<0.41(1.13±0.11)×106(1.13\pm0.11)\times10^{6}(9.1±1.0)×105(9.1\pm1.0)\times10^{5}
126<3.9<3.9<1.8<1.8<8.1<8.19000±5009000\pm500
128<0.78<0.78<0.053<0.053<0.089<0.089
129<3.7<3.7<1.4<1.4<9.9<9.9
131<0.20<0.20<0.45<0.45
1323.6±2.63.6\pm2.6<2.4<2.4<12<12<0.20<0.20
133<0.063<0.063<0.23<0.23
138<14<14<26<26
169<3.5<3.5<1.6<1.6
170<6.8∼<6.8\sim<4.0<4.0
188<1.2<1.2<1.9<1.9
203<12<12<23<23
207<590<590<530<530
2124600±28004600\pm28003300±19003300\pm1900
213<360<360370±280370\pm280
214<130<130<160<160
217<100<100<550<550
220<680<680<5200<5200
2300.094±0.0230.094\pm0.023
2310.053±0.0160.053\pm0.016
232<0.018<0.018
237<0.88<0.88<0.56<0.56
243<0.32<0.32<0.52<0.52
244<19<19<15<15
245<5.9<5.9<23<23
246<110<11070±4070\pm40
248<0.23<0.23<0.059<0.059
249<23<2325±1125\pm11

Table V. Table V: Table of radioassay - additional isotopic data in mBq/kg. Entry # references the entry # in Tab. IV. The 210^{210}Po results are all from α counting, except for #126, which is from γ counting. α-counting samples are of the same material as those listed in Tab. IV but are not the same sample. As detailed in the text, limits marked with ∼\sim are more than 3σ negative.

R##MaterialLabQuantity222Rn^{222}\mathrm{Rn} (µBq)
R1BeCu compression spring (10 of Century Spring 10693CS)SLAC360 cm2^{2}42±2942 \pm29
Getter materials
R2237ST707 Pill/4-2/50 getter material extracted from EXO-200 SAES PS4-MT3, opened 2021LU410 g334±162334 \pm162
R3241ALB Materials ALB-Z001 (99.95% Zr, <300<300 ppm Hf) pellets, 2x2 mmLU501 g477±137477 \pm137
R4241ALB Materials ALB-Z001 (99.95% Zr, <300<300 ppm Hf) pellets, 2x2 mmSLAC438 g168±45168 \pm45
R5SAES getter PS4-MT50-R-535 (offline/cold)SLAC1 unit176±48176 \pm48
R6SAES getter PS4-MT50-R-535 (purifying/hot)SLAC1 unit428±61428 \pm61
R7EXO-200 SAES PS4-MT3 purifier (offline/cold)SLAC1 unit<73<73
R8EXO-200 SAES PS4-MT3 purifier (purifying/hot)SLAC1 unit<70<70
R9GetterMax133 copper catalysts pelletsSLAC357 g1840±1501840 \pm150
Welds
R10MIG weld coupon, passivated with pickling pasteLU0.1 m2^{2}<290<290
R11MIG weld coupon, unpassivatedLU0.1 m2^{2}<120<120
R12TIG weld coupon, passivated with pickling pasteLU0.1 m2^{2}<390<390
R13TIG weld coupon, unpassivatedLU0.1 m2^{2}<270<270
HV cable
R14109Dielectric Sciences semi-conductive-PE 2353, layers A–C (nEXO)SLAC10 m<81<81
R15109Dielectric Sciences semi-conductive-PE 2353, layers A–C (nEXO)UA10.4 m<1200<1200
R16Dielectric Sciences semi-conductive-PE 2353, all layers? (LZ?)UA7.5 m<1800<1800
R17110Dielectric Sciences semi-conductive-PE 2353, all layers (DUNE-NC)UA10.8 m<1200<1200
EXO-200
R18DuPont Teflon TE-6472 fuseable granular resin, lot 0503830033LU602.1 g417±81417 \pm81
R19DuPont Teflon TE-6472 fuseable granular resin, lot 0506830001LU718.3 g<35<35
R20Espanex polyimide laminate cables MC18-25-00CEMLU0.8 m2^{2}<116<116
R21CeramTec ceramic electrical breaks (12 of 9998-06-W and 2 of 17199-01-W)LUnet<95<95
R22GXe valve seats for APTech AP3000 (12 PCTFE and 12 polyimide)LUnet<236<236
R23Teflon coated o-rings for Fluitron compressors (4 total)LU23.3 cm2^{2}<58<58
R24Photo etched phosphor bronze “spider” springs (10 units)LU169 cm2^{2}<1050<1050
R25Photo etched phosphor bronze anode wires plate #1 scrapsLU70 cm2^{2}<230<230
R26Photo etched phosphor bronze anode wires plate #2 scrapsLU82 cm2^{2}<490<490
R27Master Bond epoxy EP29LPSPLU0.276 m2^{2}<140<140
R28Mott filter GSP515H3FF11 (6812039)LU1 unit570±70570 \pm70
R29McMaster-Carr UHMW polyethylene 8701K54LU0.16 m2^{2}170±110170 \pm110
R30SAES purifier PS4-MT3 #1LU1 unit<200<200
R31SAES purifier PS4-MT3 #2LU1 unit<350<350
R32NuPure Eliminator 600-CGLU1 unit(150.0±1.2)×103(150.0 \pm1.2) \times10^{3}
R33SAES purifier HP400-903FLU1 unit∼49×103\sim49 \times10^{3}

Table VI. Table of 222Rn^{222}\mathrm{Rn} emanation measurements in µBq representing the rate of 226Ra^{226}\mathrm{Ra} decay supporting the emanation rate from the sample.

Photodetector
179RMD SiPMNAAUA<20<20<120<120<8.7<8.7
180FBK SiPM, batch 1NAAUA<130<130<210<210<5.4<5.4
181FBK SiPM, batch 2NAAUA<20<20<4.6<4.6<16<16
182FBK SiPM, batch 3NAAUA<2.0<2.03.15±0.233.15 \pm0.23<4.7<4.7
183FBK SiPM, batch 4NAAUA<11<110.17±0.120.17 \pm0.123.8±0.43.8 \pm0.4
184FBK low field SiPM (63XFBK)ICP-MSPNNL0.86±0.050.86 \pm0.050.45±0.120.45 \pm0.12
185FBK low field SiPM (63XFBK)NAAUA<68<68<22<22
186FBK standard field SiPM (64XFBK)ICP-MSPNNL0.986±0.0140.986 \pm0.0140.44±0.050.44 \pm0.05
187FBK standard field SiPM (64XFBK)ICP-MSIHEP0.070±0.0200.070 \pm0.0200.110±0.0300.110 \pm0.030
Silicon wafers
188†BNL pulverizedA.G. GeUA<300<300<230<230<2400<2400
189BNL pulverizedICP-MSPNNL13.20±0.1013.20 \pm0.1025.7±0.725.7 \pm0.7
190FBK P1B blankNAAUA<0.29<0.29<0.67<0.671.82±0.231.82 \pm0.23
191FBK P1B blankICP-MSPNNL<0.62<0.620.501±0.0320.501 \pm0.032
192FBK P3B-TiNAAUA<0.60<0.600.35±0.150.35 \pm0.150.60±0.130.60 \pm0.13
193Teledyne DALSA Semiconductor blankICP-MSPNNL0.62±0.110.62 \pm0.110.84±0.060.84 \pm0.06
194Teledyne DALSA Semiconductor CMOSICP-MSPNNL0.20±0.090.20 \pm0.090.11±0.040.11 \pm0.04
195Hamamatsu VUV3 MPPC without tungstenICP-MSPNNL0.72±0.190.72 \pm0.190.31±0.200.31 \pm0.20
196Hamamatsu VUV3 MPPC without tungstenICP-MSIHEP0.210±0.0300.210 \pm0.0300.310±0.0300.310 \pm0.030
197Hamamatsu, 625 μ\mum Si, 0–2 μ\mum W, 0–0.2 μ\mum TiN (S13375-SI-WAFER)ICP-MSPNNL0.24±0.040.24 \pm0.04<15<15
198IME custom interposer (2020)ICP-MSPNNL4.6±0.94.6 \pm0.92.3±0.92.3 \pm0.9
199Sherbrooke-IZM polyimide layerICP-MSPNNL<7.3<7.312±712 \pm7
200Sherbrooke-IZM AlSi layerICP-MSPNNL<0.70<0.701.9±0.41.9 \pm0.4
201Sherbrooke-IZM copper layerICP-MSPNNL0.70±0.100.70 \pm0.103.3±0.83.3 \pm0.8
202FBK benzocyclobutene filmICP-MSPNNL55.9±3.255.9 \pm3.2211±15211 \pm15<1300<1300
ASIC
203†MicroBooNE cryogenicU.G. GeVdA(1.00±0.29)×104(1.00 \pm0.29) \times10^{4}<9800<9800(2.5±1.3)×104(2.5 \pm1.3) \times10^{4}
204Global Foundry 350 nm (NTO-LCSA-GF 0.35 ANALOG-20141120)ICP-MSPNNL0.35±0.130.35 \pm0.131.3±0.71.3 \pm0.7
205TSMC CMOS, standard 0.25 μ\mum VCSEL 1–2′′ICP-MSLU<850<850<59<59
206TSMC CMOS, standard 0.25 μ\mum PIN diode 3–4′′ICP-MSLU<1300<1300<300<300
207†TSMC CMOS, standard 0.25 μ\mum assorted chipsU.G. GeVdA<4.4×104<4.4 \times10^{4}<1.8×105<1.8 \times10^{5}
208TSMC 180 nm LAr cold FE ASIC (V68T#2-AA)ICP-MSPNNL2.2±0.62.2 \pm0.6<7.0<7.0
209TSMC 130 nm (run TMGI86 of 06/16/2015 Fab14)ICP-MSPNNL0.67±0.300.67 \pm0.300.97±0.230.97 \pm0.23
210MOSIS/TSMC 65 nm (V98G-AA)ICP-MSPNNL<13<13<48<48
211MOSIS/TSMC 65 nm (V98G-AA)ICP-MSPNNL2.000±0.0192.000 \pm0.0191.500±0.0131.500 \pm0.013
Electronic components
212†Mini-Systems 1.8 GΩ\Omega resistors (WA-5-PG-1807-M-N-S62)A.G. GeUA<2.2×105<2.2 \times10^{5}<2.2×106<2.2 \times10^{6}<9.5×105<9.5 \times10^{5}
213†Canberra field-effect transistorA.G. GeUA<7.6×104<7.6 \times10^{4}<9.1×104<9.1 \times10^{4}(1.1±0.5)×105(1.1 \pm0.5) \times10^{5}
214MPIK Heidelberg field-effect transistorA.G. GeUA(3.8±2.4)×104(3.8 \pm2.4) \times10^{4}<1.3×105<1.3 \times10^{5}(1.3±0.4)×105(1.3 \pm0.4) \times10^{5}
215MPIK Heidelberg 1 pF feedback capacitorsA.G. GeUA<5.3×105<5.3 \times10^{5}(1.86±0.06)×105(1.86 \pm0.06) \times10^{5}(8.9±1.0)×104(8.9 \pm1.0) \times10^{4}
216American Technical Ceramics 1 pF feedback capacitors (100B11R10CAV50-2X)A.G. GeUA<7.1×104<7.1 \times10^{4}146±4×104146 \pm4 \times10^{4}<8.7×104<8.7 \times10^{4}
217Idia (Murata) 10 nF (9351524225610-T3N)U.G. GeVdA<3.8×104<3.8 \times10^{4}<3.3×106<3.3 \times10^{6}(2.6±1.2)×106(2.6 \pm1.2) \times10^{6}
218Murata 100 nF (GRM188R71C105KA12J)ICP-MSPNNL<3.3×107<3.3 \times10^{7}<1.8×106<1.8 \times10^{6}(2.3±0.9)×105(2.3 \pm0.9) \times10^{5}
219Murata 100 nF (GRM188R71C105KA12J)U.G. GeVdA<1.2×106<1.2 \times10^{6}<2.9×106<2.9 \times10^{6}8.8±1.38.8 \pm1.3
220Murata 470 pFU.G. GeVdA<1.2×106<1.2 \times10^{6}<2.9×106<2.9 \times10^{6}4.7±2.24.7 \pm2.2
221Kyocera 470 pFICP-MSIHEP(2.1±0.5)×105(2.1 \pm0.5) \times10^{5}(8.6±0.4)×104(8.6 \pm0.4) \times10^{4}
222Kyocera 470 pFICP-MSPNNL<2.2×105<2.2 \times10^{5}<2.0×104<2.0 \times10^{4}
223Empower Semiconductor 220 nF (EC1001P)ICP-MSPNNL36.0±3.036.0 \pm3.0
224Empower Semiconductor 670 nF (EC1100P)ICP-MSPNNL
No.MaterialAssayLab238^{238}U232^{232}Th40^{40}K226^{226}Ra
225BNL generic assemblyA.G. GeUA(4.5±1.0)×105(4.5\pm1.0)\times10^{5}(6.0±0.6)×105(6.0\pm0.6)\times10^{5}(1.82±0.18)×106(1.82\pm0.18)\times10^{6}(1.68±0.17)×105(1.68\pm0.17)\times10^{5}
226PCBWay.com unassembled (W148965ASS19)A.G. GeUA(1.5±0.9)×106(1.5\pm0.9)\times10^{6}(8.7±0.9)×105(8.7\pm0.9)\times10^{5}(4.7±0.5)×106(4.7\pm0.5)\times10^{6}(5.8±0.6)×105(5.8\pm0.6)\times10^{5}
227PCBWay.com unassembled (W148965ASS28)A.G. GeUA(2.2±0.4)×106(2.2\pm0.4)\times10^{6}(1.66±0.17)×106(1.66\pm0.17)\times10^{6}(7.9±0.8)×106(7.9\pm0.8)\times10^{6}(1.00±0.10)×106(1.00\pm0.10)\times10^{6}
228Palpilot unassembledA.G. GeUA(1.09±0.22)×106(1.09\pm0.22)\times10^{6}(1.16±0.12)×106(1.16\pm0.12)\times10^{6}(5.5±0.6)×106(5.5\pm0.6)\times10^{6}(6.4±0.7)×105(6.4\pm0.7)\times10^{5}
229Palpilot unassembled (C180001067)A.G. GeUA(1.97±0.26)×106(1.97\pm0.26)\times10^{6}(1.93±0.19)×106(1.93\pm0.19)\times10^{6}(8.9±0.9)×106(8.9\pm0.9)\times10^{6}(1.09±0.11)×106(1.09\pm0.11)\times10^{6}
230†3M NOVEC-7000ICP-MSPNNL0.0034±0.00050.0034\pm0.0005<0.0013<0.0013
2313M NOVEC-7200ICP-MSPNNL<0.0043<0.0043<0.0013<0.0013
232TMC reclaimed 3M NOVEC-7200ICP-MSPNNL0.0019±0.00100.0019\pm0.00100.0030±0.00200.0030\pm0.0020
233JuFu JF7100 (2023060390)ICP-MSPNNL<0.0017<0.0017<0.0012<0.0012
234JuFu HFE6512 (202305158120)ICP-MSPNNL0.0074±0.00130.0074\pm0.00130.0045±0.00040.0045\pm0.0004
235St 707 Pill/4-2/50 getter material from SAES PS4-MT3, opened 2015ICP-MSPNNL(1.60±0.09)×105(1.60\pm0.09)\times10^{5}8800±13008800\pm1300
236St 707 Pill/4-2/50 getter material from SAES PS4-MT3, opened 2021A.G. GeUA(1.15±0.20)×105(1.15\pm0.20)\times10^{5}<1500<1500(1.88±0.21)×104(1.88\pm0.21)\times10^{4}
237†St 707 Pill/4-2/50 getter material from SAES PS4-MT3, opened 2021U.G. GeSNOLAB(10.1±1.0)×104(10.1\pm1.0)\times10^{4}760±120760\pm120(1.51±0.09)×104(1.51\pm0.09)\times10^{4}<340<340
238St 707 Pill/4-2/50 getter material from SAES PS4-MT3, opened 2021ICP-MSPNNL(7.5±0.4)×104(7.5\pm0.4)\times10^{4}(1.00±0.30)×104(1.00\pm0.30)\times10^{4}
239ALB Materials ALB-Z001 (99.95% Zi, <300 ppm Hf) pelletsA.G. GeUA<680<680<470<470<460<460
240ALB Materials ALB-Z001 (99.95% Zi, <300 ppm Hf) pelletsICP-MSPNNL2000±4002000\pm400300±200300\pm200
241ALB Materials ALB-Z001 (99.95% Zi, <300 ppm Hf) pelletsU.G. GeLNGS<1600<1600<110<110540±150540\pm150<310<310
242ALB Materials ALB-Z001 (99.95% Zi, <300 ppm Hf) GD-MS rodGD-MSNRC<1000<1000<800<800
243†McMaster-Carr UHMW PE for gasket (8701K67)U.G. GeVdA150±40150\pm40<150<150<190<190
244†Canberra Mylar sheetA.G. GeUA<3500<3500<1.1×104<1.1\times10^{4}6800±35006800\pm3500
245Canberra TeflonA.G. GeUA<1300<1300<8900<8900<1.4×104<1.4\times10^{4}
246Canberra tinA.G. GeUA<4900<4900(3.5±1.4)×104(3.5\pm1.4)\times10^{4}<1.3×104<1.3\times10^{4}
247Gold washer for thermal couplingA.G. GeUA<5.0×105<5.0\times10^{5}<2.0×104<2.0\times10^{4}(7±5)×104(7\pm5)\times10^{4}<1.1×104<1.1\times10^{4}
248†Canberra screws (S3) and washers (W1 and W2)A.G. GeUA<23<2369±3369\pm33<30<30
249†Canberra screws (S3) and washers (W3)A.G. GeUA<3000<3000<8400<8400<1.6×104<1.6\times10^{4}
250†Canberra screws (S2)A.G. GeUA5000±40005000\pm4000(2.3±1.0)×104(2.3\pm1.0)\times10^{4}(1.0±0.6)×104(1.0\pm0.6)\times10^{4}
251CoorsTek silicon carbideNAAUA<0.76<0.760.58±0.150.58\pm0.150.11±0.060.11\pm0.06
252Corning high vacuum greaseA.G. GeUA(5.2±1.1)×104(5.2\pm1.1)\times10^{4}(1.0±0.6)×104(1.0\pm0.6)\times10^{4}(5.6±2.1)×104(5.6\pm2.1)\times10^{4}
253DuPont Teijin Melinex 1311 antistatic film, 440 gaICP-MSPNNL9.9±1.99.9\pm1.917.3±2.017.3\pm2.0
254†Merck KGaA Patinal Mg granules (CAS RN No: 7783-40-6)ICP-MSPNNL<1.5×106<1.5\times10^{6}<1900<1900(3.9±0.4)×106(3.9\pm0.4)\times10^{6}
255Merck KGaA Patinal Mg granules (CAS RN No: 7783-40-6)ICP-MSPNNL<2.9×106<2.9\times10^{6}<110<110(2.48±0.26)×106(2.48\pm0.26)\times10^{6}
256SNOLAB dust, J-DriftU.G. GeSNOLAB(3.8±0.4)×105(3.8\pm0.4)\times10^{5}<2400<2400(4.89±0.52)×106(4.89\pm0.52)\times10^{6}
257SNOLAB dust, J-Drift (large debris removed)A.G. GeUA(3.5±0.6)×105(3.5\pm0.6)\times10^{5}<2400<2400(4.50±0.9)×106(4.50\pm0.9)\times10^{6}
258SNOLAB dust, J-DriftA.G. GeUA(2.02±0.20)×106(2.02\pm0.20)\times10^{6}<1900<1900(7.5±0.8)×106(7.5\pm0.8)\times10^{6}
259Canberra zeolite molecular sieve type 5A 1/16 pelletA.G. GeUA(3.13±0.34)×105(3.13\pm0.34)\times10^{5}<4300<4300(2.21±0.22)×105(2.21\pm0.22)\times10^{5}
260Canberra activated carbon pellet, activated, acid washedA.G. GeUA<400<400<220<220<6100<6100
261GE50 Advanced activated carbonA.G. GeUA<3.0×104<3.0\times10^{4}<2.3<2.317001700
262Phosphor bronze springsICP-MSPNNL3.6±2.43.6\pm2.4<7.5<7.532±0.3232\pm0.32
263LOTTIE EA0151 epoxy resinICP-MSPNNL<0.3<0.3<2.4<2.4211±0.05211\pm0.05
264LOTTIE EA0151 epoxy resinICP-MSPNNL<4.0<4.0<14<14<40<40
265LOTTIE EA0151 epoxy hardenerICP-MSPNNL<4.3<4.3<6.0<6.0<80<80
266Materbond EP29LSP epoxy resinICP-MSPNNL<5.0<5.0<14<14<40<40
267Materbond EP29LSP epoxy hardenerICP-MSPNNL<0.32<0.32<0.70<0.702.8±1.92.8\pm1.9

Table 3 (PDF p. 13).

250<64<47
2545.8±3.2<6.5
256<5.6×10^{4}
257<1.1×10^{5}
259(2.3±0.6)×10^{4}
26130±9<1600

Table 4.

Conclusion

This paper reports the results of an extensive radioactivity study conducted in support of the planned nEXO double-beta decay experiment. The large body of data reported here can be useful for a variety of rare event searches. It will help other collaborations save time and expenses by avoiding duplication of effort. Data of the type reported here are an important enabler for a broad spectrum of science.

Acknowledgments

The authors gratefully acknowledge support for nEXO from the Office of Nuclear Physics within DOE’s Office of Science under grants/contracts DE-AC02-76SF00515, DE-FG02-01ER41166, DE-SC002305, DE-FG02-93ER40789, DE-SC0021388, DE-SC0012447, DE-SC0012704, DE-AC52-07NA27344, DE-SC0017970, DE-AC05-76RL01830, DE-SC0012654, DE-SC0021383, DE-SC0014517, DE-SC0024666, DE-SC0020509, DE-SC0024677 and support by the US National Science Foundation grants NSF PHY-2111213 and NSF PHY-2011948; from NSERC SAPPJ-2022-00021, CFI 39881, FRQNT 2019-NC-255821, and the CFREF Arthur B. McDonald Canadian Astroparticle Physics Research Institute in Canada; from IBS-R016-D1 in South Korea; and from CAS in China. This work was supported in part by Laboratory Directed Research and Development (LDRD) programs at Brookhaven National Laboratory (BNL), Lawrence Livermore National Laboratory (LLNL), Pacific Northwest National Laboratory (PNNL), and SLAC National Accelerator Laboratory, United States.

References

  1. [1]B. Loer, P. Harrington, B. Archambault, E. Fuller, B. Pierson, I. Arnaquist, K. Harouaka, T. Schlie­der, D. Kim, A. Melville, B. Niedzielski, J. Yoder, K. Ser­niak, W. Oliver, J. Orrell, R. Bunker, B. VanDevender, and M. Warner, J. Instrum. 19, P09001 (2024).
  2. [2]M. Agostini, G. Benato, J. A. Detwiler, J. Menéndez, and F. Vissani, Rev. Mod. Phys. 95, 025002 (2023).
  3. [3]G. Adhikari et al. (nEXO Collaboration), J. Phys. G 49, 015104 (2021).
  4. [4]N. Abgrall et al. (LEGEND-1000 Collaboration), Legend-1000 preconceptual design report (2021), arXiv:2107.11462 [physics.ins-det].arxiv.org/abs/2107.11462
  5. [5]The CUPID Interest Group (CUPID Collaboration), CUPID pre-CDR (2019), arXiv:1907.09376 [physics.ins-det].
  6. [6]C. Apresella et al. (BOREXINO Collaboration), Astropart. Phys. 18, 1 (2002).
  7. [7]E. Armengaud et al. (EDELWEISS Collaboration), Astropart. Phys. 47, 1 (2013).
  8. [8]D. Leonard, P. Grinberg, P. Weber, E. Baussan, Z. Djurcic, G. Keefer, A. Piepke, A. Pocar, J.-L. Vuilleumier, J.-M. Vuilleumier, et al., Nucl. Instrum. Methods A 591, 490 (2008).
  9. [9]D. Leonard, D. Auty, T. Didberidze, R. Gornea, P. Grinberg, R. MacLellan, B. Methven, A. Piepke, J.-L. Vuilleumier, et al., Nucl. Instrum. Methods A 871, 169 (2017).
  10. [10]D. Budjáš, A. Gangapshev, J. Gasparro, W. Hampel, M. Heisel, G. Heusser, M. Hult, A. Klimenko, V. Kuzminov, M. Laubenstein, W. Maensh, H. Simgen, A. Smolnikov, C. Tomei, and S. Vasiliev, Appl. Radiat. Isot. 67, 755 (2009), 5th international conference on radionuclide metrology - low-level radioactivity measurement techniques ICRM-LLRMT’08.
  11. [11]D. Akerib et al. (LUX Collaboration), Astropart. Phys. 62, 33 (2015).
  12. [12]D. S. Akerib et al. (LZ Collaboration), Eur. Phys. J. C 80, 1044 (2020).
  13. [13]N. Abgrall et al. (MAJORANA Collaboration), Nucl. Instrum. Methods A 828, 22 (2016).
  14. [14]V. Álvarez et al. (NEXT Collaboration), J. Instrum. 8, T01002 (2013).
  15. [15]P. Jagam and J. Simpson, Nucl. Instrum. Methods A 324, 389 (1993).
  16. [16]E. Aprile et al., Astropart. Phys. 35, 43 (2011).
  17. [17]E. Aprile et al. (XENON Collaboration), Eur. Phys. J. C 77, 890 (2017).
  18. [18]K. Abe et al. (XMASS Collaboration), J. Instrum. 15, P09027 (2020).
  19. [19]J. B. Albert et al. (EXO-200 Collaboration), Phys. Rev. C 92, 015503 (2015).
  20. [20]G. Heusser, M. Laubenstein, and H. Neder, in Radionuclides in the Environment, Radioactivity in the Environment, Vol. 8, edited by P. Povinec and J. Sanchez-Cabeza (Elsevier, 2006) pp. 495–510.
  21. [21]N. Ackermann, H. Bonet, C. Buck, O. Chkvorets, J. Hak­enmüller, G. Heusser, M. Laubenstein, M. Lindner, W. Maenschg, J. Schreiner, and H. Strecker, Appl. Radiat. Isot. 194, 110652 (2023).
  22. [22]Some older measurements were taken with a less efficient muon detection system, prior to it being upgraded.
  23. [23]I. Lawson, PoS TAUP2023, 303 (2023).
  24. [24]B. LaFerriere, T. Maiti, I. Arnquist, and E. Hoppe, Nucl. Instrum. Methods A 775, 93 (2015).
  25. [25]I. Arnquist, M. di Vacri, and E. Hoppe, Nucl. Instrum. Methods A 965, 163761 (2020).
  26. [26]I. J. Arnquist, C. Beck, M. L. di Vacri, K. Harouaka, and R. Saldanha, Nucl. Instrum. Methods A 959, 163573 (2020).
  27. [27]I. J. Arnquist, M. L. di Vacri, N. Rocco, R. Saldanha, T. Schlie­der, R. Patel, J. Patil, M. Perez, and H. Uka, EPJ Tech. Instrum. 10, 17 (2023).
  28. [28]K. Harouaka, E. W. Hoppe, and I. J. Arnquist, J. Anal. At. Spectrom. 35, 2859 (2020).
  29. [29]M. L. di Vacri, I. J. Arnquist, H. O. Back, M. Bliss, M. Bronikowski, E. Edwards, B. R. Hackett, E. W. Hoppe, S. M. Lyons, N. D. Rocco, R. Rosero, A. Seifert, A. Swindle, and M. Yeh, J. Radioanal. Nucl. Chem. 331, 5597 (2022).
  30. [30]I. J. Arnquist, E. W. Hoppe, M. Bliss, and J. W. Grate, Anal. Chem. 90, 1432 (2018).
  31. [31]American Society for Quality, Sampling procedures and tables for inspection by variables for percent nonconforming, ASQ/ANSI Z1.9-2003 (R2018) (2018).
  32. [32]A. Agrawal et al. (AMoRE Collaboration), Front. Phys. 12, 1362209 (2024).
  33. [33]R. Tsang, O. Nusair, and A. Piepke, J. Instrum. 16, P10007 (2021).
  34. [34]D. Chernyak, I. J. Arnquist, T. Daniels, S. W. Finch, L. Hissong, M. Hughes, R. MacLellan, A. Piepke, A. Pocar, R. Roshong, R. Saldanha, , and R. H. M. Tsang, Phys. Rev. C , (2025).
  35. [35]J.-X. Wang, T. C. Andersen, and J. J. Simpson, Nucl. Instrum. Methods A 421, 601 (1999).
  36. [36]T. Andersen, I. Blevis, J. Boger, E. Bonvin, M. Chen, B. Cleveland, X. Dai, F. Dalnoki-Veress, G. Doucas, J. Farine, et al., Nucl. Instrum. Methods A 501, 399 (2003).
  37. [37]J. Farine (2005) pp. 199–208, https://pubs.aip.org/aip/acp/article-pdf/785/1/199/12046559/199-1_online.pdf.
  38. [38]A. Anker, P. Breur, B. Mong, et al. (nEXO Collaboration), Nucl. Instrum. Methods A 1081, 170786 (2026).
  39. [39]A. Sazzad, P. Acharya, P. Back, J. Busenitz, D. Chernyak, Y. Meng, A. Piepke, C. Rhyne, and R. Tsang, J. Instrum. 20, P01020 (2025).
  40. [40]Preparation and certification of IAEA gamma-ray spectrometry reference materials RGU-1, RGTh-1 and RGK-1, Tech. Rep. (1987) IAEA/RL/148.
  41. [41]R. Tsang, A. Piepke, et al. (nEXO Collaboration), Nucl. Instrum. Methods A 1055, 168477 (2023).
  42. [42]S. Navas, C. Amsler, T. Gutsche, C. Hanhart, J. J. Hernández-Rey, C. Lourenço, A. Masoni, M. Mikhasenko, R. E. Mitchell, C. Patrignani, C. Schwanda, S. Spanier, G. Venanzoni, C. Z. Yuan, et al. (Particle Data Group), Phys. Rev. D 110, 030001 (2024).
  43. [43]T. Szücs, D. Bemmerer, D. Degering, A. Domula, M. Grießer, F. Ludwig, K. Schmidt, J. Steckling, S. Turkat, and K. Zuber, Eur. Phys. J. A 55, 174 (2019).
  44. [44]T. Roosendaal, C. Overman, G. Ortega, T. Schlieder, N. Rocco, L. Horkley, K. Hobbs, K. Harouaka, J. Orrell, et al., Nucl. Instrum. Methods A 1087, 171402 (2026).

Paper details

vlnc:W_tsf9bh53
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents