betaFeedback

WorksPhysics and Astronomy

Ab-initio insights into the physical properties of XIr3 (X = La, Th) superconductors: A comparative analysis

Abstract

Here we report the structural, elastic, bonding, thermo-mechanical, optoelectronic and superconducting state properties of recently discovered XIr3 (X = La, Th) superconductors utilizing the density functional theory (DFT). The elastic, bonding, thermal and optical properties of these compounds are investigated for the first time. The calculated lattice and superconducting state parameters are in reasonable agreement to those found in the literature. In the ground state, both the compounds are mechanically stable and possess highly ductile character, high machinability, low Debye temperature, low bond hardness and significantly high melting point. The thermal conductivities of the compounds are found to be very low which suggests that they can be used for thermal insulation purpose. The population analysis and charge density distribution map confirm the presence of both ionic and covalent bonds in the compounds with ionic bond playing dominant roles. The calculated band structure and DOS profiles indicate metallic character. Unlike the significant anisotropy observed in elastic and thermal properties, all the optical constants of these compounds exhibit almost isotropic behavior. The optical constants correspond very well with the electronic band structure and DOS features. We have estimated the superconducting transition temperature of the compounds in this work.

Introduction

Superconductivity is one of the most interesting and significant topics in both theoretical and experimental condensed matter physics. Nowadays the investigation of superconductors has piqued the interest of modern society owing to their features suitable for wide range of applications. Many binary systems made of rare earth and transition metals have been found to exhibit superconductivity. The addition of rare earth and 5d5d transition metal element such as Ir (Iridium) can create a compound that displays superconductivity and other attractive electronic, mechanical and optical features [1, 2, 3, 4]. LaIr3\mathrm{LaIr}_3, ThIr3\mathrm{ThIr}_3, CeIr3\mathrm{CeIr}_3, CaIr2\mathrm{CaIr}_2, IrGe\mathrm{IrGe}, and Mg10Ir19B16\mathrm{Mg}_{10}\mathrm{Ir}_{19}\mathrm{B}_{16} are a few examples of such compounds, where the superconductivity arises mainly from the Ir-5d5d electronic states close to the Fermi level [1, 4, 5, 6, 7, 8].

In this paper, the physical properties of two superconducting compounds XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) [1, 4], that crystallizes in a rhombohedral structure with space group R-3mR\text{-}3m, have been studied. In this work, we investigate the structural, elastic, bonding, thermo-mechanical, optoelectronic and superconducting state properties of these two promising compounds. The obtained results were compared to existing experimental and theoretical data, where applicable. It is worth noting that many technologically essential physical features of XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) materials are still unknown in comparison to other systems such as chalcogenides, oxides, and pnictides. We focus particularly on the unexplored physical characteristics of XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}).

Recently, the superconducting compound LaIr3\mathrm{LaIr}_3 was synthesized and characterized experimentally by Bhattacharyya et al. [9]. They investigated the superconducting ground state in LaIr3\mathrm{LaIr}_3 and observed that it is a bulk type-II superconductor with TC=2.5T_C = 2.5 K. Furthermore, Haldolaarachchige et al. [1] examined the physical characteristics of LaIr3\mathrm{LaIr}_3 both experimentally and theoretically. They suggested that LaIr3\mathrm{LaIr}_3 is a BCS-type superconductor which exhibits superconductivity at 3.3 K. Moreover, they discovered that the superconductivity in LaIr3\mathrm{LaIr}_3 is arising from the Ir-5d5d states at the Fermi surface. Górnicka et al. [4] prepared a polycrystalline sample of ThIr3\mathrm{ThIr}_3 and examined its electronic and magnetic characteristics using dc magnetization, electrical resistivity, and heat capacity assessment. They concluded that ThIr3\mathrm{ThIr}_3 is a dd-band, moderately coupled type-II superconductor with Tc=4.41T_c = 4.41 K. They also stated that the 5d5d-states of Ir play the most important role in the appearance of superconductivity in ThIr3\mathrm{ThIr}_3 with some contributions from the Th-6d6d states. Moreover, Górnicka et al. [5] also synthesized and investigated the superconducting state properties of CeIr3\mathrm{CeIr}_3. Based on the specific-heat data analysis, they estimated that CeIr3\mathrm{CeIr}_3 is a moderately coupled type-II superconductor which is superconducting below 2.5 K. There are few other related studies on the materials CaIr2\mathrm{CaIr}_2 [6], IrGe\mathrm{IrGe} [7], and Mg10Ir19B16\mathrm{Mg}_{10}\mathrm{Ir}_{19}\mathrm{B}_{16} [8] where the superconductivity is derived from the Ir-dd electronic orbitals.

Several physical characteristics, such as structural characterization, band structure calculation, electronic energy density of states, Fermi surface, and superconducting state features of XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) have been investigated theoretically as well as experimentally so far [1, 4, 9]. To the best of our knowledge, most of the physical features of these compounds, such as elastic, chemical bonding, charge density distribution, Mulliken population analysis, thermo-mechanical properties, and energy dependent optical constants have not been studied so far. For instance, no citable work has yet to be found on the elastic characteristics of these compounds such as the Poisson's ratio, machinability index, Kleinman parameter, hardness, anisotropy in elastic moduli etc. Moreover, the various thermo-mechanical parameters of these compounds such as the Debye temperature, lattice thermal conductivity, melting temperature, sound velocities, and thermal expansion coefficient have not been explored at all. In addition, still there are lack of theoretical understanding of the bonding and optical characteristics of these materials.

Therefore, it is obvious from the preceding discussion that many physical features of these compounds remain unexplored. In this study, we want to overcome this research gap, which is the key motivation for the current investigations. Hence, it is our crucial theoretical interest to study the structural, elastic, mechanical, bonding, acoustic, optoelectronic, thermal and superconducting state properties of XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds thoroughly in this paper. It is worth keeping in mind that information on all these hitherto unexplored physical properties are essential to unlock the potential of XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) for possible applications.

The remaining part of this study is organized as follows: In Section 2, we provide an overview of our computational scheme. We discussed the calculated results of various properties of XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds in Section 3. Finally, the major findings of this investigation are summarized in Section 4.

Computational scheme

The CASTEP (CAмbridge Serial Total Energy Package) code [10] is a comprehensive software package which is designed to calculate the ground state energy of a system as well as various other physical properties based on the quantum mechanical density functional theory (DFT) [11]. The ground state of a crystalline system can be obtained in DFT formalism by solving the Kohn-Sham equation [12]. In this investigation, we employed the local density approximation (LDA) [13] for the exchange-correlation energy calculations because it yields better outcomes of ground state structural properties for XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds than the other schemes including the Perdew-Burke-Ernzerhof generalized gradient approximation (PBE-GGA) [14]. To model the coulomb potential energy that arises from the interaction of valence electrons with ion cores of XX (X=La,ThX = \mathrm{La}, \mathrm{Th}) and Ir atoms, we employed Vanderbilt-type ultra-soft pseudopotential [15]. Ultra-soft pseudopotential saves a large amount of processing time while compromising just a little bit of computational accuracy. To find the lowest energy structure, we adopted The BFGS (Broyden-Fletcher-Goldferb-Shanno) minimization technique [16] for geometry optimization.

To execute the pseudo atomic operations, the valence electron configurations used in this study were [5s25p65d16s2][5s^{2}5p^{6}5d^{1}6s^{2}] for the La atom, [6s26p66d27s2][6s^{2}6p^{6}6d^{2}7s^{2}] for the Th atom, and [5d76s2][5d^{7}6s^{2}] for the Ir atom, respectively. In this work, the plane-wave cut off energy was set at 400 eV to obtain the total energy convergence. The sampling of the Brillouin zone of XIr3X\mathrm{Ir}_3 compounds was performed using a mesh size of 11×11×211 \times11 \times2 k-points based on the Monkhorst-Pack scheme [17]. Employing finite basis set corrections [18], the geometry optimization of LaIr3\mathrm{LaIr}_3 was accomplished with convergence thresholds of 0.5×10−50.5 \times10^{-5} eV/atom for the total energy, 0.5×10−30.5 \times10^{-3} Å for maximum ionic displacement, 0.02 GPa for maximum stress component and 0.01 eV/Å for maximum ionic force. On the other hand, for the ThIr3\mathrm{ThIr}_3 compound, the geometry optimization was performed with convergence within 10−510^{-5} eV/atom for the total energy, within 10−310^{-3} Å for maximum ionic displacement, within 0.05 GPa for maximum stress component and within 0.03 eV/Å for maximum ionic force. These chosen tolerance levels provide very good results of structural, elastic and optoelectronic properties with an optimum computing speed. In this work, all the DFT computations of XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds were carried out in the ground state with default temperature (0 K) and pressure (0 GPa).

After the geometry optimization, the elastic constants, Mulliken bond population, charge density distribution, band structure, density of states (DOS) and optical properties were evaluated. The stress-strain approach [19] was used to compute the independent elastic constants, CijC_{ij}, of rhombohedral crystal structure. The computations provide six independent elastic constants. The bulk modulus BB, shear modulus GG, and many other elastic properties were calculated from these independent elastic constants utilizing the Voigt-Reuss-Hill (VRH) method [20, 21]. The computed elastic constants are used to calculate various thermophysical parameters such as Debye temperature, thermal conductivity, melting temperature, thermal expansion coefficient, heat capacity, and so on. The Mulliken bond population analysis was used in order to gain a better knowledge of the bonding features of XIr3\mathrm{XIr}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds using a projection of the plane-wave states onto a linear combination of atomic orbital basis sets [22, 23, 24]. The Mulliken bond population analysis was accomplished with the Mulliken density operator, which is written on an atomic (or quasi-atomic) basis in the following manner:

PμνM(g)=∑g′∑ν′Pμν′(g′)Sν′ν(g−g′)=L−1∑ke−ikg(PkSk)μν(1)P_{\mu\nu}^{M}(g)=\sum_{g'}\sum_{\nu'}P_{\mu\nu'}(g')S_{\nu'\nu}(g-g')=L^{-1}\sum_{k}e^{-ikg}(P_{k}S_{k})_{\mu\nu} \tag*{(1)}

and the total charge that exists on an atomic species AA can be stated as:

QA=ZA−∑μ∈APμμm(o)(2)Q_{A}=Z_{A}-\sum_{\mu\in A}P_{\mu\mu}^{m}(o) \tag*{(2)}

where ZAZ_{A} refers to the charge of the atomic core.

All the optical parameters of XIr3\mathrm{XIr}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) in the ground state can be fully investigated by utilizing the complex dielectric function, ε(ω)=ε1(ω)+iε2(ω)\varepsilon(\omega)=\varepsilon_{1}(\omega)+i\varepsilon_{2}(\omega). Utilizing the Kramers-Kronig equations, we can simply determine the real part of the dielectric function from its imaginary part. CASTEP computes the imaginary part, ε2(ω)\varepsilon_{2}(\omega), by employing the following formula [25, 26]:

ε2(ω)=2e2πΩε0∑k,ν,c∣⟨ψkc|u^⋅r⃗|ψkv⟩∣2δ(Ekc−Ekv−E)(3)\varepsilon_{2}(\omega)=\frac{2e^{2}\pi}{\Omega\varepsilon_{0}}\sum_{k,\nu,c}\left|\left\langle\psi_{k}^{c}\middle|\hat{u}\cdot\vec{r}\middle|\psi_{k}^{v}\right\rangle\right|^{2}\delta(E_{k}^{c}-E_{k}^{v}-E) \tag*{(3)}

In the above equation, ω\omega refers to the angular frequency of the electromagnetic wave, Ω\Omega denotes the volume of the unit cell, ee is the electronic charge, and at a particular wave-vector kk, ψkv\psi_{k}^{v} and ψkc\psi_{k}^{c} represent the valence and conduction band wave functions, respectively. The other optical parameters, such as the refractive index, reflectivity, absorption coefficient, optical conductivity, and energy loss function can be evaluated from the complex dielectric function, ε(ω)\varepsilon(\omega) by employing the following set of relations [27, 28]:

n(ω)=12[{ε1(ω)2+ε2(ω)2}1/2+ε1(ω)]1/2(4)n(\omega)=\frac{1}{\sqrt{2}}\left[\left\{\varepsilon_{1}(\omega)^{2}+\varepsilon_{2}(\omega)^{2}\right\}^{1/2}+\varepsilon_{1}(\omega)\right]^{1/2} \tag*{(4)}
k(ω)=12[{ε1(ω)2+ε2(ω)2}1/2−ε1(ω)]1/2(5)k(\omega)=\frac{1}{\sqrt{2}}\left[\left\{\varepsilon_{1}(\omega)^{2}+\varepsilon_{2}(\omega)^{2}\right\}^{1/2}-\varepsilon_{1}(\omega)\right]^{1/2} \tag*{(5)}
R(ω)=∣n~−1n~+1∣=(n−1)2+k2(n+1)2+k2(6)R(\omega)=\left|\frac{\tilde{n}-1}{\tilde{n}+1}\right|=\frac{(n-1)^{2}+k^{2}}{(n+1)^{2}+k^{2}} \tag*{(6)}
α(ω)=4πk(ω)λ(7)\alpha(\omega) = \frac{4\pi k(\omega)}{\lambda} \tag*{(7)}
σ(ω)=2WcvℏωE02(8)\sigma(\omega) = \frac{2W_{cv}\hbar\omega}{E_0^2} \tag*{(8)}
L(ω)=Im(−1ε(ω))(9)L(\omega) = Im\left(-\frac{1}{\varepsilon(\omega)}\right) \tag*{(9)}

where, n(ω)n(\omega) and k(ω)k(\omega) are the real and imaginary parts of the complex refractive index, R(ω)R(\omega) is the reflectivity, α(ω)\alpha(\omega) is the absorption coefficient, σ(ω)\sigma(\omega) is the optical conductivity, WcvW_{cv} refers to the transition probability per unit time and L(ω)L(\omega) is the energy loss function.

Results and discussions

Structural properties

As we described in the earlier that XIr3\mathrm{XIr}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) crystallize in the rhombohedral structure (space group R-3mR\text{-}3m, No.166) [1, 4]. The schematic view of the optimized unit cell of our chosen compounds is depicted in Figure 1. This unit cell contains 36 atoms (9 XX and 27 Ir) and has nine formula units (Z=9Z = 9). It consists of three unique positions of Ir atoms and two unique positions of XX (X=La,ThX = \mathrm{La}, \mathrm{Th}) atoms. Atomic environments of all the sites in XIr3\mathrm{XIr}_3 compounds are Frank-Kasper polyhedron [29]. In one of its positions, XX-site is surrounded by sixteen Ir atoms, while in the other XX-site is centered by twelve Ir atoms.

Figure 1. Three-dimensional schematic illustration of the conventional unit cell of XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds.

The geometry optimization yields the fully relaxed lattice parameters of the chosen compounds. Table 1 summarized these optimized lattice parameters together with available experimental findings for comparison. It is seen from the Table 1 that the values of aa, cc and V0V_0 calculated by the functional LDA deviate from the experimental values by not more than 0.86%, 0.35% and 2.05%, respectively. These findings suggest that the experimental data and the theoretical outcomes are in fair agreement. On the other hand, the values of aa, cc and V0V_0 calculated by the functional GGA(PBE) differ from the reported experimental values by more than 1.23%, 1.82% and 4.35%, respectively. For this reason, we estimated the elastic, mechanical, bonding, optoelectronic and thermal properties of XIr3\mathrm{XIr}_3 compounds using the LDA approach.

CompoundFunctionalsa=ba = bccc/ac/aV0V_0Ref.
LaIr3_3LDA5.35526.3534.921654.472This work
LaIr3_3GGA(PBE)5.45826.8814.925693.499This work
LaIr3_3-5.32026.3404.951645.609[1, 4] Expt.
ThIr3_3LDA5.29426.3304.974638.997This work
ThIr3_3GGA(PBE)5.40526.9044.978680.735This work
ThIr3_3-5.33926.4234.950652.371[4] Expt.

Table 1. The optimized unit cell parameters (a=ba = b and cc in Å, optimized cell volume V0V_0 in Å3^3) of XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds along with corresponding experimental (Expt.) values.

Elastic and mechanical properties

Elastic constants are the physical properties that measure the response of a material to external stress. They determine the stiffness of material, and are used to calculate how the material behaves when subjected to a given force on different crystal planes. A compound with rhombohedral crystal structure has six independent elastic constants (CijC_{ij}), which are C11C_{11}, C12C_{12}, C13C_{13}, C14C_{14}, C33C_{33} and C44C_{44}. These single crystal elastic constants are utilized to calculate the various other elastic parameters of our chosen compounds. The computed values of the single crystal elastic constants of our chosen compounds are shown in Table 2. In order to be mechanically stable, a rhombohedral crystal structure must fulfill the following Born-Huang [30] stability criteria:

CompoundC11C_{11}C12C_{12}C13C_{13}C14C_{14}C33C_{33}C44C_{44}(C12C_{12} - C44C_{44})
LaIr3_3329.33204.30149.5742.62409.4754.49149.81
ThIr3_3424.35230.21171.4726.30457.4726.75203.46

Table 2. Computed elastic constants, CijC_{ij} (in GPa) and Cauchy pressure (C12C_{12} - C44C_{44}), (in GPa) of XXIr3_3 (XX = La, Th) compounds.

C44>0;(C11−C12)>0;(C11−C12)C44−2C142>0;(C11+C12)C33−2C132>0(10)\begin{aligned} C_{44} &> 0; \\ (C_{11} - C_{12}) &> 0; \\ (C_{11} - C_{12})C_{44} - 2C_{14}^{2} &> 0; \\ (C_{11} + C_{12})C_{33} - 2C_{13}^{2} &> 0 \tag*{(10)} \end{aligned}

At zero pressure, all of the computed elastic constants of XXIr3_3 (XX = La, Th) compounds meet the above mechanical stability conditions. This implies that all of the compounds under study are mechanically stable.

The results presented in Table 2 are novel and no comparison can be made. The independent elastic constants C11C_{11} and C33C_{33} determine the crystalline solid's responses to uniaxial strain whereas the resistance to shape deformation is described by the elastic constant C44C_{44}. The three off-diagonal elements, C12C_{12}, C13C_{13} and C14C_{14} describe the shape deforming shearing strain brought on by forces on various crystal planes. Table 2 shows that the elastic constants C11C_{11} and C33C_{33} for both the compounds are significantly greater than the elastic constant C44C_{44}. These findings suggest that shear deformation of the compounds is significantly easier than unidirectional strain along any of the three crystallographic axes. The compound ThIr3_3 is stiffer than LaIr3_3 when uniaxial elastic strengths are considered. The elastic constants C11C_{11} and C33C_{33} assess the crystal's ability to endure the uniaxial stress that imposed to the crystallographic a(b)a(b)- and cc-directions, respectively. Table 2 shows that the value of C33C_{33} is larger than C11C_{11} for both the studied materials. This result is interesting since the cc-axis lattice parameter of the unit cell is much larger than the a(b)a(b)-axis. We think that the cage-like structural units of Ir atoms along the cc-direction gives the high mechanical strength of the XIr3\mathrm{XIr}_{3} (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds in this particular crystallographic direction. These results imply that the compounds' structures are more contractible along the a(b)a(b)-direction compared to the cc-direction. Thus, it can be said that the atomic bonding in the abab-plane will be weaker compared to the out-of-plane directions. The large discrepancy in tensor C11C_{11} and C33C_{33} suggests that both the compounds have significant amount of elastic anisotropy. This discrepancy is much higher for the compound LaIr3\mathrm{LaIr}_{3} compared to ThIr3\mathrm{ThIr}_{3} which further implies that LaIr3\mathrm{LaIr}_{3} is comparatively more anisotropic in nature. The difference between the elastic constants C12C_{12} and C44C_{44} is defined as the Cauchy pressure (C12−C44C_{12} - C_{44}), which is widely used to evaluate the type of chemical bonding in a crystal and to predict the ductile or brittle nature of solids [31]. It is observed from the Table 2 that both the compounds have large positive Cauchy pressure. This suggests that their chemical bonding is dominated by ionic/metallic bondings and they are expected to show high level of ductility.

The single crystal elastic constants may be used to calculate different polycrystalline elastic moduli, Pugh's ratio, and Poisson's ratio. To evaluate the values of polycrystalline bulk modulus (BB), shear modulus (GG), Young’s modulus (YY), and Poisson’s ratio (η\eta), following equations [32] are used and the calculated results are listed in Table 3.

CompoundBVB_VBRB_RBBGVG_VGRG_RGGYYB/GB/Gη\eta
LaIr3_3230.56230.37230.4771.9532.2452.10145.354.420.39
ThIr3_3272.50272.33272.4278.9836.5457.76161.844.720.40

Table 3. Calculated bulk modulus (BVB_V, BRB_R, BB in GPa), shear modulus (GVG_V, GRG_R, GG in GPa), Young’s modulus (YY in GPa), Pugh's ratio (B/GB/G), and Poisson's ratio (η\eta) of XIr3\mathrm{XIr}_{3} (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds.

B=BV+BR2(11)B = \frac{B_{V}+B_{R}}{2} \tag*{(11)}
G=GV+GR2(12)G = \frac{G_{V}+G_{R}}{2} \tag*{(12)}
Y=9BG3B+G(13)Y = \frac{9BG}{3B+G} \tag*{(13)}
η=3B−2G2(3B+G)(14)\eta= \frac{3B-2G}{2(3B+G)} \tag*{(14)}

The Voigt [33] and Reuss [34] values of the bulk modulus and shear modulus are represented in the above equations by the symbols BVB_{V}, BRB_{R} and GVG_{V}, GRG_{R}, respectively.

The bulk and shear moduli of crystals can be utilized to evaluate their overall mechanical behaviors. Bulk modulus describes the resistance of a material to volume deformation by hydrostatic pressure while shear modulus measures the resistance to shape deformations caused by shearing stress [35]. The larger value of bulk modulus (BB) compared to shear modulus (GG) (see Table 3), suggesting that the mechanical strengths of XIr3\mathrm{XIr}_{3} compounds will be governed by the shearing strain.

The Young's modulus of a material can be used to estimate its stiffness and thermal shock resistance [36, 37]. From Table 3, it is seen that the compound LaIr3\mathrm{LaIr}_{3} has a lower value of YY than the compound ThIr3\mathrm{ThIr}_{3} indicating that ThIr3\mathrm{ThIr}_{3} is stiffer than LaIr3\mathrm{LaIr}_{3}. Since the critical thermal shock resistance is inversely proportional to the Young’s modulus [38] it can be suggested that among the two compounds LaIr3\mathrm{LaIr}_{3} will exhibit better thermal shock resistance.

The failure mode (ductile or brittle nature) of a given system can be explained from the ratio of BB to GG, which is called the Pugh’s ratio (B/GB/G) [39]. Pugh predicted that if this ratio is less than 1.75, a material will be brittle; otherwise, the material will be ductile. From Table 3, it is noticed that the B/GB/G ratio of our two studied compounds is much higher than 1.75, which suggests once again that they are highly ductile in nature.

The Poisson's ratio (η\eta) is another elastic parameter that can be used to understand nature of the bonding forces and to predict the crystal stability against shear. Materials with low values of Poisson's ratio possess stability against shear [40]. Thus, all our chosen compounds should be unstable against shear because they have high Poisson's ratio. Again, it is known that the stability of the crystal systems is governed by the central forces if the Poisson's ratio lies between 0.25 and 0.50 [41]. Therefore, from Table 3 it can be said that the interatomic forces in XIr3\mathrm{XIr}_{3} (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds are the central forces. Moreover, the Poisson's ratio can predict the ductility or brittle nature of a crystal as well as the type of chemical bonding in a crystal. Brittle failure occurs in solids when η\eta is less than a critical value of 0.26, while ductile failure occurs with η\eta greater than 0.26 [38, 42]. Thus, from Table 3, it can be concluded that studied compounds should show ductility. This result confirms the prediction from the analysis of Cauchy pressure and Pugh's ratio. A crystal with a Poisson's ratio of 0.1 is considered as purely covalent crystal, whereas one with a Poisson's ratio of 0.33 is considered as metallic compound [43]. Since both the compounds have η\eta greater than 0.33 they are characterized by metallic bonding. Furthermore, the plasticity of a solid against shear can also be estimated from the Poisson's ratio. High value of η\eta indicates that our compounds will have a high degree of plasticity.

Table 3 confirms that the bulk mechanical strength of ThIr3\mathrm{ThIr}_{3} is higher than that of LaIr3\mathrm{LaIr}_{3}.

In order to calculate the dimensionless Kleinman parameter (ζ\zeta), machinability index (μM\mu^{M}), bulk modulus under uniaxial strain (BaB_a, BbB_b and BcB_c) and isotropic bulk modulus (BrelaxB_{\mathrm{relax}}), the following formulae are employed [44, 45] and the outcomes are given in Table 4.

The dimensionless Kleinman parameter (ζ\zeta), machinability index (μM\mu^{M}), isotropic bulk modulus (BrelaxB_{relax} in GPa), and bulk modulus under uniaxial strain (BaB_a, BbB_b and BcB_c in GPa of XIr3\mathrm{XIr}_3 (X = La, Th).

Compoundζ\zetaμM\mu^{M}BrelaxB_{relax}BaB_aBbB_bBcB_c
LaIr3_30.724.23285.99829.38829.38921.53
ThIr3_30.6610.18337.631043.281043.28957.14

Table 4. The dimensionless Kleinman parameter (ζ\zeta), machinability index (μM\mu^{M}), isotropic bulk modulus (BrelaxB_{relax} in GPa), and bulk modulus under uniaxial strain (BaB_a, BbB_b and BcB_c in GPa of XIr3\mathrm{XIr}_3 (X = La, Th).

ζ=C11+8C127C11+2C12(15)\zeta= \frac{C_{11}+8C_{12}}{7C_{11}+2C_{12}} \tag*{(15)}
μM=BC44(16)\mu^{M} = \frac{B}{C_{44}} \tag*{(16)}
Ba=adPda=Λ1+α+β(17)B_a = a\frac{dP}{da} = \frac{\Lambda}{1+\alpha+\beta} \tag*{(17)}
Bb=bdPdb=Baα(18)B_b = b\frac{dP}{db} = \frac{B_a}{\alpha} \tag*{(18)}
Bc=cdPdc=Baβ(19)B_c = c\frac{dP}{dc} = \frac{B_a}{\beta} \tag*{(19)}
Brelax=Λ(1+α+β)2(20)B_{relax} = \frac{\Lambda}{(1+\alpha+\beta)^2} \tag*{(20)}

with, Λ=C11+2C12α+C22α2+2C13β+C33β2+2C33αβ\Lambda= C_{11}+2C_{12}\alpha+C_{22}\alpha^2+2C_{13}\beta+C_{33}\beta^2+2C_{33}\alpha\beta

α={(C11−C12)(C33−C13)}−{(C23−C13)(C11−C13)}{(C33−C13)(C22−C12)}−{(C13−C23)(C12−C23)}\alpha= \frac{\{(C_{11}-C_{12})(C_{33}-C_{13})\}-\{(C_{23}-C_{13})(C_{11}-C_{13})\}}{\{(C_{33}-C_{13})(C_{22}-C_{12})\}-\{(C_{13}-C_{23})(C_{12}-C_{23})\}}
β={(C22−C12)(C11−C13)}−{(C11−C12)(C23−C12)}{(C22−C12)(C33−C13)}−{(C12−C23)(C13−C23)}\beta= \frac{\{(C_{22}-C_{12})(C_{11}-C_{13})\}-\{(C_{11}-C_{12})(C_{23}-C_{12})\}}{\{(C_{22}-C_{12})(C_{33}-C_{13})\}-\{(C_{12}-C_{23})(C_{13}-C_{23})\}}

A compound's resistance to stretching and bending forces can be estimated from the Kleinman parameter (ζ\zeta) [32, 44]. Its value typically lies between 0 and 1. It is seen from the Table 4 that both the compounds have ζ\zeta value higher than 0.5. This result inferred that mechanical strength in XIr3\mathrm{XIr}_3 (X = La, Th) compounds is mainly provided by the bond bending contributions. The machinability index (μM\mu^{M}) is another parameter with which we can estimate how easily a material can be machined. This index can be used to compare the machinability of different materials and to determine the optimal cutting parameters for a given material. Furthermore, this index can also be used to assess the plasticity and dry lubricating feature of a material [32]. Table 4 shows that both the compounds have very high machinability index. The machinability index ThIr3_3 is in fact extraordinarily high. Both the compounds are expected to possess excellent dry lubricating properties, lower friction value and lower feed forces. Moreover, the levels of machinability of ThIr3_3 and LaIr3_3 are significantly higher than many technologically important MAX and MAB phase compounds [46, 47, 48, 49].

To understand a material's mechanical behavior in practical applications it is essential to calculate its hardness value. There are a number of theoretical schema for determining the hardness as a function of Poisson’s ratio (η\eta), Young’s modulus (YY), bulk modulus (BB), and shear modulus (GG). Some of the prominent schemes are given by N. Miao et al. [50, 51], X. Chen et al. [52], Y. Tian et al. [53], and D. M. Teter [54], and E. Mazhnik et al. [55]. Using these approaches, we have calculated the values of (HV)micro(H_V)_{micro}, (HV)macro(H_V)_{macro}, (HV)Tian(H_V)_{Tian}, (HV)Teter(H_V)_{Teter}, and (HV)Mazhnik(H_V)_{Mazhnik} via Eqns. (21) – (25). The obtained values are disclosed in Table 5.

Compound(HV)micro(HV)_{micro}(HV)macro(HV)_{macro}(HV)Tian(HV)_{Tian}(HV)Teter(HV)_{Teter}(HV)Mazhnik(HV)_{Maz hnik}KICK_{IC}
LaIr3_33.830.552.797.878.371.85
ThIr3_33.850.502.798.729.322.32

Table 5. Calculated hardness (in GPa) with different schemes and fracture toughness (in MPa m1/2^{1/2}) of XIr3_3 (XX = La, Th) compounds.

(HV)micro=(1−2η)Y6(1+η)(21)(H_V)_{micro} = \frac{(1-2\eta)Y}{6(1+\eta)} \tag*{(21)}
(HV)macro=2[(GB)2G]0.585−3(22)(H_V)_{macro} = 2\left[\left(\frac{G}{B}\right)^2 G\right]^{0.585} - 3 \tag*{(22)}
(HV)Tian=0.92(G/B)1.137G0.708(23)(H_V)_{Tian} = 0.92(G/B)^{1.137}G^{0.708} \tag*{(23)}
(HV)Teter=0.151G(24)(H_V)_{Teter} = 0.151G \tag*{(24)}
(HV)Mazhnik=γ0χ(η)Y(25)(H_V)_{Mazhnik} = \gamma_0\chi(\eta)Y \tag*{(25)}

where, χ(η)\chi(\eta) is a function of the Poisson’s ratio (η\eta), which can be obtained from:

χ(η)=1−8.5η+19.5η21−7.5η+12.2η2+19.6η3\chi(\eta) = \frac{1-8.5\eta+19.5\eta^2}{1-7.5\eta+12.2\eta^2+19.6\eta^3}

and γ0\gamma_0 is a dimensionless constant with a value of 0.096.

It is observed from the Table 5 that, the scheme suggested by X. Chen et al. yields the lowest values of hardness while the scheme suggested by Mazhnik et al. yields the highest values of hardness for both the compounds. It can also be estimated from the Table 5 that the compound ThIr3_3 is fairly harder than the compound LaIr3_3. This result is consistent with the results on elastic parameters.

The formation of cracks, particularly in metals and ceramic materials, is one of the major issues with surface hard coatings on heavy-duty devices. Fracture toughness, KICK_{IC}, of a material is a measure of its resistance to surface crack formation. This parameter plays a vital role in the design of engineering materials. The following equation is used to calculate the fracture toughness (KICK_{IC}) [56]:

KIC=α0−1/2V01/6[ξ(η)Y]3/2(26)K_{IC} = \alpha_0^{-1/2}V_0^{1/6}[\xi(\eta)Y]^{3/2} \tag*{(26)}

where, V0V_0 is the atomic volume; α0\alpha_0 = 8840 GPa; ξ(η)\xi(\eta) is a function of the Poisson’s ratio (η\eta) which can be found from:

ξ(η)=1−13.7η+48.6η21−15.2η+70.2η2−81.5η3\xi(\eta)=\frac{1-13.7\eta+48.6\eta^{2}}{1-15.2\eta+70.2\eta^{2}-81.5\eta^{3}}

The fracture toughness is also shown in Table 5. It is seen from the Table 5 that the value of KICK_{IC} of ThIr3_3 compound is higher than LaIr3_3 compound. This result suggests that ThIr3_3 will offer higher resistance to surface crack formation than LaIr3_3 and ThIr3_3. The mechanical hardness, on the other hand, of the two compounds is a fairly similar.

The anisotropy in elasticity of a crystalline solid describes the directional dependence of its mechanical characteristics. Elastic anisotropy influences many physical processes, including the microcrack formation in solids, the development of plastic deformations in crystals, crack propagation dynamics, etc. Understanding elastic anisotropy has important consequences in both crystal physics and applied engineering fields. Therefore, it is essential to calculate the elastic anisotropy factors of our studied compounds in detail. For a thorough knowledge of elastic anisotropy, we have determined the Zener anisotropy parameter (AA), shear anisotropy parameters (A1A_1, A2A_2, and A3A_3), anisotropy in compressibility (ABA_B), anisotropy in shear (AGA_G), the universal anisotropy index (AUA^U, dEd_E), the equivalent Zener anisotropy index (AeqA^{eq}), the universal log-Euclidean index (ALA^L) and the anisotropies of the bulk modulus along aa- and cc-axes relative to the bb-axis (ABaA_{Ba} and ABcA_{Bc}) by using the following equations [40, 41, 44] and the outcomes are disclosed in Table 6 and Table 7.

CompoundAAA1A_1A2A_2A3A_3ABA_BAGA_G
LaIr3_30.870.500.5010.00040.3811
ThIr3_30.280.200.2010.00030.3674

Table 6. The Zener anisotropy parameter (AA), shear anisotropy parameters (A1A_1, A2A_2, and A3A_3), anisotropy in compressibility (ABA_B) and anisotropy in shear (AGA_G) of XIr3_3 (X = La, Th).

Table 7. The universal anisotropy index (AUA^{U}, dEd_E), equivalent Zener anisotropy index (AeqA^{eq}), universal log-Euclidean index (ALA^{L}), anisotropies of the bulk modulus along aa- and cc-axis (ABaA_{Ba} and ABcA_{Bc}) of XIr3_3 (X = La, Th).

CompoundAUA^{U}dEd_EAeqA^{eq}ALA^{L}ABaA_{Ba}ABcA_{Bc}
LaIr3_36.163.497.002.4211.11
ThIr3_35.813.446.691.9310.92

Table 7.

A=2C44C11−C12(27)A=\frac{2C_{44}}{C_{11}-C_{12}} \tag*{(27)}
A1=4C44C11+C33−2C13(28)A_1=\frac{4C_{44}}{C_{11}+C_{33}-2C_{13}} \tag*{(28)}
A2=4C55C22+C33−2C23(29)A_2=\frac{4C_{55}}{C_{22}+C_{33}-2C_{23}} \tag*{(29)}
A3=4C66C11+C22−2C12(30)A_3=\frac{4C_{66}}{C_{11}+C_{22}-2C_{12}} \tag*{(30)}
AB=BV−BRBV+BR(31)A_B=\frac{B_V-B_R}{B_V+B_R} \tag*{(31)}
AG=GV−GRGV+GR(32)A_G = \frac{G_V-G_R}{G_V+G_R} \tag*{(32)}
AU=BVBR+5GVGR−6≥0(33)A^U = \frac{B_V}{B_R} + 5\frac{G_V}{G_R} - 6 \ge0 \tag*{(33)}
dE=AU+6(34)d_E = \sqrt{A^U+6} \tag*{(34)}
Aeq=(1+512AU)+(1+512AU)2−1(35)A^{eq} = \left(1+\frac{5}{12}A^U\right) + \sqrt{\left(1+\frac{5}{12}A^U\right)^2-1} \tag*{(35)}
AL=[ln⁡(BVBR)]2+5[ln⁡(C44VC44R)]2(36)A^L = \sqrt{\left[\ln\left(\frac{B_V}{B_R}\right)\right]^2+5\left[\ln\left(\frac{C_{44}^V}{C_{44}^R}\right)\right]^2} \tag*{(36)}

with,

C44R=(53)C44(C11−C12)3(C11−C12)+4C44C_{44}^R = \left(\frac{5}{3}\right)\frac{C_{44}(C_{11}-C_{12})}{3(C_{11}-C_{12})+4C_{44}}

is the Reuss value of C44C_{44}

C44V=C44R+(35)(C11−C12−2C44)23(C11−C12)+4C44C_{44}^V = C_{44}^R+\left(\frac{3}{5}\right)\frac{(C_{11}-C_{12}-2C_{44})^2}{3(C_{11}-C_{12})+4C_{44}}

is the Voigt value of C44C_{44}

ABa=BaBb=α(37)A_{B_a} = \frac{B_a}{B_b} = \alpha \tag*{(37)}
ABc=BcBb=αβ(38)A_{B_c} = \frac{B_c}{B_b} = \frac{\alpha}{\beta} \tag*{(38)}

The shear anisotropy parameters A1A_1, A2A_2, and A3A_3 correspond to the shear planes {100}\{100\}, {010}\{010\}, and {001}\{001\}, respectively. It is seen from the Table 6 that the values of A1A_1 and A2A_2 are not equal to one which indicates that both the compound are elastically anisotropic in terms of shearing stress on different crystal planes. From the values of A1A_1 and A2A_2, it can be suggested that LaIr3_3 is elastically less anisotropic than ThIr3_3. It is also observed that the values of A1A_1 and A2A_2 are equal reflecting the rhombohedral structure of our studied compounds. Moreover, we found that the shear anisotropy factor A3A_3 is equal to unity for both the compounds, suggesting that the compounds are isotropic between the [110][110] and [010][010] directions in the {001}\{001\} shear planes. The values of anisotropy in compressibility (ABA_B) and anisotropy in shear (AGA_G) are equal to zero for an isotropic crystal, while a value of 1 refers to the maximum probable anisotropy of the crystal [57]. For both the materials the calculated value of ABA_B is much lower than AGA_G, which implies that the anisotropy in compressibility is much lower than the anisotropy in shear.

The universal anisotropy index (AUA^{U}) is called ‘universal’ since it applies to all types of crystal symmetries. For an elastically isotropic crystal, AUA^{U} is equal to zero, but any other positive number suggests a level of anisotropy of the crystal [58]. In this study, we found that the value of AUA^{U} is much higher than zero (see Table 7) for XIr3_3 (X = La, Th) compounds, which implies a strong anisotropy of the compounds. Again, from Table 7 it is observed that the value of equivalent Zener anisotropy index (AeqA^{eq}) is greater than unity, which also indicates the anisotropic nature of the compounds. For crystalline materials, the universal log-Euclidean index (ALA^{L}) ranges from 0 to 10.26 (0≤AL≤10.260 \leq A^{L} \leq10.26) while AL=1A^{L} = 1 for an elastically isotropic crystal [59]. Both the compounds in this study have the values of ALA^{L} greater than one, which indicates a degree of anisotropy of the compounds. Furthermore, the estimated ABaA_{Ba} and ABcA_{Bc} values (see Table 7) indicate that the bulk moduli of our investigated compounds are isotropic along the aa-axis and anisotropic along the cc-axis; a consequence of the rhombohedral structure.

For an isotropic crystal, the three-dimensional (3D) directional variation of Young's modulus (YY), compressibility (β\beta), shear modulus (GG), and Poisson's ratio (η\eta) should be spherical in shape, and any deviation from this configuration would indicate a level of elastic anisotropy. In this study, we have obtained 2D and 3D visualization of YY, β\beta, GG, and η\eta by using elastic tensor analysis (ELATE) [60]. Figure 2 to Figure 5 illustrate the 2D and 3D plots generated by ELATE. The 3D plots of YY, GG, and η\eta show a larger deviation from spherical shape, suggesting a significant amount of elastic anisotropy. On the other hand, the 3D plot of β\beta shows a small deviation from spherical configuration, signifying a low level of anisotropy in compressibility. Again, it is also seen from the plots that the elastic parameters are fully isotropic in the abab-plane as also indicated by the value of ABaA_{Ba} (Table 7).

Figure 2. 2D and 3D directional variation of Young’s modulus (YY) for XIr3X\mathrm{Ir}_{3} (X=La,ThX = \mathrm{La}, \mathrm{Th}).

Figure 5. 2D and 3D directional variation of Poisson’s ratio (η\eta) for XIr3_3 (XX = La, Th).

Figure 3. 2D and 3D directional variation of linear compressibility (β\beta) for XIr3X\mathrm{Ir}_{3} (X=La,ThX = \mathrm{La}, \mathrm{Th}).

Figure 4. 2D and 3D directional variation of shear modulus (GG) for XIr3_3 (XX = La, Th).

Mulliken and Hirshfeld population analysis

The Mulliken bond population analysis is a widely used method in quantum chemistry to comprehend the nature of chemical bonds (ionic, covalent and metallic) in a material. In this section, we have employed both Mulliken population analysis (MPA) [22] and Hirshfeld population analysis (HPA) [61] to explore the bonding natures of our chosen compounds. The results obtained from the bond population analysis (MPA and HPA) of XIr3\mathrm{XIr}_{3} (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds are disclosed in Table 8.

CompoundCharge spillingAtomsssppddffTotalMulliken chargeEVCHirshfeld charge
LaIr3_30.12La1.446.051.830.009.321.681.320.15
LaIr3_30.12La1.665.961.990.009.611.391.610.11
LaIr3_30.12Ir0.810.997.690.009.49-0.49-2.51-0.03
LaIr3_30.12Ir0.860.817.760.009.44-0.44-2.56-0.09
LaIr3_30.12Ir0.840.977.700.009.51-0.51-2.49-0.04
LaIr3_30.12Th2.415.962.200.5711.140.862.140.19
LaIr3_30.12Th2.495.802.370.6411.300.702.300.11

Table 8. Charge spilling parameter (%), orbital charges (electronic charge), atomic Mulliken charge (electronic charge), EVC (electronic charge), and Hirshfeld charge (electronic charge) of XIr3\mathrm{XIr}_{3} (X=La,ThX = \mathrm{La}, \mathrm{Th}).

The charge spilling index determines how much valence charge is missing in a projection. A low value of this parameter suggests that electronic bonding is efficiently represented in the MPA. Table 8 shows that the charge spilling parameters are very low, which indicates that the projections of atomic orbitals are efficiently represented in the MPA.

The analysis also shows that the Mulliken and Hirshfeld charges are positive for the XX (X=La,ThX = \mathrm{La}, \mathrm{Th}) atoms (act as cation) while these charges are negative for the Ir atom (acts as anion). The value of Mulliken charge and Hirshfeld charge (see Table 8) of our studied compounds indicates that electrons are partially transferred from Ir to XX atoms. This result implies the presence of ionic bonds the XX and Ir atoms. It is also noticed from the Table 8 that the Mulliken charge transfer between La and Ir atoms are higher than the charge transfer between Th and Ir atoms.

The difference between the formal ionic charge and the computed Mulliken charge is known as the effective valence charge (EVC) of an atom [24]. In this study, we have measured the EVC of XIr3\mathrm{XIr}_{3} (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds in order to predict the degree of covalency or iconicity. EVC values larger than zero imply increasing degree of covalency, while the zero value of EVC denotes an ideal ionic bond. The non-zero values of EVC (see Table 8) implies the existence of both covalent and ionic bonds in XIr3\mathrm{XIr}_{3} (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds.

ThIr3_3Ir0.720.827.700.009.25-0.25-2.75-0.05
ThIr3_3Ir0.760.697.740.009.19-0.19-2.81-0.07
ThIr3_3Ir0.750.827.690.009.26-0.26-2.74-0.04

Table 18.

Theoretical bond hardness

Hardness is a fundamental mechanical property of a material which measures its resistance to deformation, abrasion, or indentation. It also describes the ability of a material to endure localized stresses without considerable plastic deformation or damage. In industry, the relative hardness of a material is also frequently employed. A material's hardness is a crucial physical parameter to comprehend its applicability, particularly when used as an abrasive and radiation tolerant element [62]. In general, a harder material has higher bond population, higher degree of covalency, and shorter bond length. In general, a solid with a higher bulk modulus and shear modulus also has a higher crystal stiffness and hardness. Although the bulk modulus and shear modulus give some information on hardness, there is no straightforward relationship with hardness and bulk or shear modulus [63]. The two forms of hardness are intrinsic and extrinsic. In general, the hardness of a single crystal is regarded as intrinsic, whereas the hardness of polycrystalline materials is considered as extrinsic. The bond hardness is an useful intrinsic measure of a material and can be obtained by using the following expressions [64, 65]:

Hvμ=[∏μ{740(Pμ−Pμ′)(vbμ)−5/3}nμ]1/∑nμ(39)H_{v}^{\mu}=\left[\prod_{\mu}\left\{740(P^{\mu}-P^{\mu'})(v_{b}^{\mu})^{-5/3}\right\}^{n^{\mu}}\right]^{1/\sum n^{\mu}} \tag*{(39)}
Hv=[∏μ(Hvμ)nμ]1/∑nμ(40)H_{v}=\left[\prod_{\mu}(H_{v}^{\mu})^{n^{\mu}}\right]^{1/\sum n^{\mu}} \tag*{(40)}
Pμ′=nfreeV0(41)P^{\mu'}=\frac{n_{free}}{V_{0}} \tag*{(41)}
nfree=∫EPEFN(E) dE(42)n_{free}=\int_{E_{P}}^{E_{F}}N(E)\,\mathrm{d}E \tag*{(42)}
vbμ=(dμ)3∑ν[(dμ)3nbμ](43)v_{b}^{\mu}=\frac{(d^{\mu})^{3}}{\sum_{\nu}[(d^{\mu})^{3}n_{b}^{\mu}]} \tag*{(43)}

where, HvμH_{v}^{\mu} signifies the bond hardness of the μ\mu-type bond, HvH_{v} is the total hardness of the compound, PμP^{\mu} and Pμ′P^{\mu'} are the Mulliken bond overlap population and metallic population, nfreen_{free} is the number of free electrons, V0V_{0} is the cell volume, EFE_{F} and EPE_{P} refer to the energy at the Fermi level and at the pseudo-gap, nμn^{\mu} denotes the total number of μ\mu-type bond, vbμv_{b}^{\mu} refers to the bond volume of μ\mu-type bond, dμd^{\mu} is the bond length of μ\mu-type bond, and nbμn_{b}^{\mu} refers to the μ\mu-type bond density per cubic angstroms.

The metallic nature of bonds in a solid can also be estimated from the Mulliken bond population analysis. In this study, we have calculated the metallicity (fmf_m) of XIr3_3 (X = La, Th) compounds by using the following equations [66]:

fm=Pμ′Pμ(44)f_m = \frac{P^{\mu\prime}}{P^\mu} \tag*{(44)}

The calculated number of free electrons, bond length, Mulliken and metallic population, total number of each type of bonds, metallicity, bond volume and bond hardness of each type of bonds and the total hardness of our investigated compounds are listed in Table 9. The Mulliken bond populations of a compound indicate the degree of overlapping of the electron clouds generating bonds between the compound's two relevant atoms. For a purely ionic bond, the value of overlap population is equal to zero but any other positive value indicates a level of covalency of the bond. The bonding and anti-bonding kind of interactions between the relevant pairs of atoms can be identified from the positive and negative values of a compound's Mulliken bond overlap populations, respectively [67]. From Table 9 it is seen that, both the studied compounds have positive values of bond populations for the Ir-Ir bonding which implies the bonding type of interaction between these atoms. Metallic populations for XIr3_3 (X = La, Th) compounds are found to be very low (see Table 9). This result suggesting the existence of weak metallic bond in the compounds. It is also noticed from the Table 9 that LaIr3_3 compound has a higher total bond hardness value than ThIr3_3 compound. This result is contradictory with the results obtained in the elastic and mechanical properties section. Discuss in conclusion

Compoundnfreen_{free}Bonddμd^\munμn^\muPμP^\muPμ′P^{\mu\prime}fmf_mvbμv_b^\muHvμH_v^\muHvH_v
LaIr3_340.08Ir-Ir2.61180.430.060.148.577.637.36
LaIr3_340.08Ir-Ir2.64180.350.060.178.915.607.36
LaIr3_340.08Ir-Ir2.65180.800.060.088.9714.147.36
LaIr3_340.08Ir-Ir2.74180.360.060.179.914.867.36
ThIr3_321.05Ir-Ir2.64180.550.030.058.6910.485.05
ThIr3_321.05Ir-Ir2.65180.250.030.128.744.395.05
ThIr3_321.05Ir-Ir2.65180.230.030.138.813.945.05
ThIr3_321.05Ir-Ir2.70180.230.030.139.293.605.05

Table 9. The calculated number of free electrons (nfreen_{free}), bond length (dμd^\mu in Å), bond number (nμn^\mu), Mulliken bond overlap population (PμP^\mu), metallic population (Pμ′P^{\mu\prime}), metallicity (fmf_m), bond volume (vbμv_b^\mu in Å3^3), bond hardness of the μ\mu-type bond (HvμH_v^\mu in GPa), and total hardness (HvH_v in GPa) of XIr3_3 (X = La, Th) compounds.

Electronic charge density distribution

The electronic charge density distribution map illustrates detailed information about the bonding nature and amount of charge transfer among the atoms of a compound. To estimate the bonding nature of the XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds, we have computed the electronic charge density distribution maps within the (110) and (111) crystal planes using LDA functionals and the obtained results are depicted in Figure 6. The total electron density is shown by the color scale placed between the panels. In the map, high charge density is indicated by the blue color and low charge density is indicated by the red color. From Figure 6 it is seen that, the electron density around the XX (X=La,ThX = \mathrm{La}, \mathrm{Th}) atoms is much higher compared to the Ir atoms. Since the charge density is found to be almost spherical around the XX atoms (see Figure 6), it can be concluded that no charge sharing occurs between the XX and the Ir atoms. Thus, the bonding among the XX-Ir atoms is of ionic nature. Again, charge overlapping is seen between the relevant Ir atoms of XIr3X\mathrm{Ir}_3 compounds. This point towards the covalent bonding nature in the crystal. Therefore, both ionic and covalent bonds coexist in XIr3X\mathrm{Ir}_3 compounds where the ionic bond dominates. Far from the atomic sites, we have found uniform low density charge distribution in these compounds. This result suggests the presence of a weak metallic bond in these compounds. The overall outcomes in this section are well matched with the bond population analysis that was previously addressed.

Electronic charge density distribution maps for XIr3 compounds

Figure 6.

Electronic charge density maps in the (110) and (111) planes of XIr3 compounds

Figure 6 (PDF p. 21). The electronic charge density map in the (a) (110) and (b) (111) planes of XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds. The scale for the charge density map is given between the panels.

Electronic properties

Electronic band structure

One of the most significant topics of condensed matter physics is the study of electronic band structure, which is strongly linked to a compound's electrical conductivity, thermopower, heat capacity, bonding features, Hall effect, optoelectronic properties, magnetic properties, and superconductivity. The electronic energy band structures of optimized XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds have been calculated along the path Γ\Gamma-AA-HH-KK-Γ\Gamma-MM-LL-HH in the first Brillouin zone (BZ). The results obtained from the band structure calculations are depicted in Figure 7. It is seen from the Figure 7 that the band structures of XIr3X\mathrm{Ir}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds are quite similar to each other. The horizontal broken line at zero energy represents the Fermi level (EFE_\mathrm{F}). LaIr3\mathrm{LaIr}_3 and ThIr3\mathrm{ThIr}_3 compounds have a total number of 469 and 468 electronic energy bands, respectively. It is evident from the Figure 7 that there is no band gap at the Fermi level since considerable overlapping occurs between the valence and conduction bands. The result suggests that both the compounds have metallic character. The red lines in Figure 7 indicate the bands that cross the Fermi level. There are six LaIr3\mathrm{LaIr}_3 bands (bands 170, 171, 172, 173, 174 and 175) and five ThIr3\mathrm{ThIr}_3 bands (bands 174, 175, 176, 177 and 178) which cross the Fermi level. In the BZ, these bands have both electron-like and hole-like nature in different directions. It is noticed from the Figure 7 that for both the compounds, the bands near the Γ\Gamma-point are highly dispersive which suggests high mobility and low effective mass of the charge carriers [68, 69, 70]. It is also observed from Figure 7 that the bands around the Fermi level of ThIr3_3 compound are flatter than the LaIr3_3 compound. Flat bands give rise to high electron effective mass and stronger electronic correlations.

Electronic band structures of LaIr3 and ThIr3 compounds

Figure 7. The electronic band structure of LaIr3_3 and ThIr3_3 compounds along several high symmetry directions in the first BZ.

Electronic energy density of states (DOS)

The electronic energy density of states (DOS) of a crystalline material is linked with the electronic, optical, superconducting, and magnetic features of a material. The DOS of a material is also crucial to understand how each atom contributes to bonding and anti-bonding states. In this study, we have computed the total and partial density of states (TDOS and PDOS, respectively) of XIr3\mathrm{XIr}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) to gain a better understanding of the electronic features. The results obtained from the TDOS and PDOS calculations of our chosen materials are depicted in Figure 8. The vertical broken line at zero energy represents the Fermi level (EFE_F). From figure 8 it is seen that the TDOS values at the Fermi level are finite. This result confirms again the metallic nature of the compounds.

Total and partial density of states plots of LaIr₃ and ThIr₃

Figure 8. The total and partial density of states (TDOS and PDOS, respectively) plots of XIr3X\mathrm{Ir}_{3} (X=LaX = \mathrm{La}, Th\mathrm{Th}) as a function of energy.

At EFE_F, the TDOS values of the investigated compounds are quite large (see Figure 8). This suggests that the compounds should exhibit high electrical conductivity. The TDOS values at EFE_F of LaIr3\mathrm{LaIr}_3 and ThIr3\mathrm{ThIr}_3 compounds are found to be 31.12 states/eV-unit cell (3.46 states/eV-formula unit) and 28.88 states/eV-unit cell (3.21 states/eV-formula unit), respectively. The value of the TDOS of a compound at the Fermi level, N(EF)N(E_F), is an important parameter for the purpose of determining electronic stability of the compound. Compounds with lower N(EF)N(E_F) values are more stable compared to those with higher N(EF)N(E_F) values [71, 72]. As a result, it can be estimated that ThIr3\mathrm{ThIr}_3 will be more electronically stable than LaIr3\mathrm{LaIr}_3. From previous study, the values of TDOS were found to be 3.90 states/eV-formula unit [5] for LaIr3\mathrm{LaIr}_3 and 3.46 states/eV-formula unit [4] for ThIr3\mathrm{ThIr}_3. Thus, the results obtained in this study are in good agreement with the previous values.

In order to understand the contribution of XX (X=La,ThX = \mathrm{La}, \mathrm{Th}) and Ir atoms in the TDOS separately, we have computed the PDOS of each atom at different energies. It is seen from Figure 8 that the Ir-5dd orbitals of the two compounds under study largely contribute to the TDOS in the proximity of EFE_F. Thus, the metallic conductivity in XIr3\mathrm{XIr}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds are governed by the 5dd states of Ir atom. Moreover, the compound LaIr3\mathrm{LaIr}_3 will exhibit more metallic nature than ThIr3\mathrm{ThIr}_3 since the Ir-5dd states at EFE_F is stronger in LaIr3\mathrm{LaIr}_3 than in ThIr3\mathrm{ThIr}_3. The valence band of LaIr3\mathrm{LaIr}_3 compound is mainly composed by the 5dd orbital of Ir with a modest input from the La-5dd orbital. On the other hand, the conduction band of LaIr3\mathrm{LaIr}_3 is mainly formed by the La-5dd states with some contribution from the Ir-5dd states. Again, for the ThIr3\mathrm{ThIr}_3 compound, the Ir-5dd orbital dominates the valence band, while above EFE_F, the Th-5ff orbital mainly contribute to the large DOS peak. From Figure 8, it can be inferred that the La-6ss, Th-7ss and Ir-6ss states have no effect on the DOS at the EFE_F.

The existence of a deep valley in the TDOS plot close to the EFE_F is referred to a pseudogap or quasi-gap. It is linked to a material's electronic stability and distinguishes the bonding states from the antibonding states [71, 72, 73]. The bonding peak is defined as the nearest negative energy peak of TDOS in the vicinity of EFE_F and the anti-bonding peak is defined as the nearest positive energy peak of TDOS in the vicinity of EFE_F. It can be inferred from the Figure 8 that for XIr3\mathrm{XIr}_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds the bonding and anti-bonding peaks are positioned within 2 eV apart from the EFE_F.

Thermal properties

Debye temperature and acoustic velocities

In solid-state physics, the Debye temperature (θD\theta_{\mathrm{D}}) of a material determines the highest energy mode of lattice vibration and acts as a cutoff for the phonon energy distribution. This parameter also gives useful information on the lattice dynamics, specific heat capacity, thermal conductivity, melting temperature, and elastic constants of a material. In this study, we have employed the Anderson method [74] to calculate the θD\theta_{\mathrm{D}}. This method uses the sound velocity (vav_{\mathrm{a}}) to calculate θD\theta_{\mathrm{D}} via the following equation:

θD=hkB[3n4πV0]13va(45)\theta_{\mathrm{D}} = \frac{h}{k_{\mathrm{B}}} \left[\frac{3n}{4\pi V_{0}}\right]^{\frac{1}{3}} v_{\mathrm{a}} \tag*{(45)}

In the above equation, V0V_{0} signifies the cell volume, nn defines the total number of atoms in the cell, hh refers to the Planck’s constant and kBk_{\mathrm{B}} denotes the Boltzmann’s constant. The following expression can be used to calculate the average sound velocity (vav_{\mathrm{a}}) [75]:

va=[13(2vt3+1vl3)]−13(46)v_{\mathrm{a}} = \left[\frac{1}{3}\left(\frac{2}{v_{\mathrm{t}}^{3}}+\frac{1}{v_{\mathrm{l}}^{3}}\right)\right]^{-\frac{1}{3}} \tag*{(46)}

here, vlv_l and vtv_t refer to the longitudinal and transverse sound velocities, respectively. The vlv_l and vtv_t can be obtained from:

vl=3B+4G3ρ(47)v_l = \sqrt{\frac{3B + 4G}{3\rho}} \tag*{(47)}
vt=Gρ(48)v_t = \sqrt{\frac{G}{\rho}} \tag*{(48)}

where, ρ\rho refers to the density of the solid. The calculated values of θD\theta_D of XIr3\mathrm{XIr}_3 (X=La,Th\mathrm{X} = \mathrm{La}, \mathrm{Th}) compounds along with the mass density (ρ\rho) and acoustic velocities (vlv_l, vtv_t and vav_a) are presented in Table 10.

Compoundρ\rhovlv_lvtv_tvav_aθD\theta_DRef.
LaIr3\mathrm{LaIr}_316345.594283.651785.332019.61229This work
LaIr3\mathrm{LaIr}_3----366[1]Expt.
ThIr3\mathrm{ThIr}_318920.584297.491747.221978.15226This work
ThIr3\mathrm{ThIr}_3----169[4]Expt.

Table 10. The calculated density (ρ\rho in kg/m3^3), acoustic velocities (vlv_l, vtv_t and vav_a, all in m/sec) and Debye temperature (θD\theta_D in K) of XIr3\mathrm{XIr}_3 (X=La,Th\mathrm{X} = \mathrm{La}, \mathrm{Th}) along with the previously estimated experimental (Expt.) values.

It is seen from the table 10 that the calculated vav_a and θD\theta_D of LaIr3\mathrm{LaIr}_3 are considerably larger than that of ThIr3\mathrm{ThIr}_3. This happens due to the lower mass density of LaIr3\mathrm{LaIr}_3 compounds than the ThIr3\mathrm{ThIr}_3 compounds. Moreover, the values of vtv_t are found to be much lower than vlv_l (see Table 10) in XIr3\mathrm{XIr}_3 (X=La,Th\mathrm{X} = \mathrm{La}, \mathrm{Th}) compounds. The overall θD\theta_D of XIr3\mathrm{XIr}_3 compounds are found to be low. This result suggests a low thermal conductivity of the compounds which is further discussed in the subsequent section. It is also worth noting that the calculated value of θD\theta_D for LaIr3\mathrm{LaIr}_3 is significantly lower than the previously anticipated experimental result [1]. However, the calculated value of θD\theta_D for ThIr3\mathrm{ThIr}_3 is found to be significantly higher than the experimental result [4].

Anisotropies in acoustic velocity

A solid's acoustic velocity is an essential feature that is linked to its thermal and electrical properties. A solid's atoms produce three vibrational modes: two transverse (vt1v_{t1} and vt2v_{t2}) modes and one longitudinal (vlv_l) mode. These vibrational modes are excited by sound wave when it travels through a solid. The presence of elastic anisotropy in a solid can be detected by the anisotropy in sound velocities, and vice versa. For rhombohedral crystal structure, the pure longitudinal and transverse modes can be determined only along [100][100] and [001][001] crystallographic directions. In this work, we have measured the acoustic velocities of XIr3_3 (X = La, Th) compounds along the [100][100] and [001][001] propagation directions in order to comprehend the anisotropic nature of acoustic velocities. We have employed the following equations [76] to calculate the acoustic velocities and the outcomes are presented in Table 11.

Propagation directionsLaIr3_3ThIr3_3
[100][100][100]vl[100]v_l1955.652265.04
[100][100][010]vt1[010]v_{t1}4488.654735.82
[100][100][001]vt2[001]v_{t2}1825.821189.04
[001][001][001]vl[001]v_l5005.084917.16
[001][001][100]vt1[100]v_{t1}1825.821189.04
[001][001][010]vt2[010]v_{t2}1825.821189.04

Table 11. Anisotropic acoustic velocities (m/s) in XIr3_3 (X = La, Th) along various propagation directions.

[100][100] direction:

[100]vl=C11−C122ρ;[010]vt1=C11ρ;[001]vt2=C44ρ(49)[100]v_l = \sqrt{\frac{C_{11}-C_{12}}{2\rho}};\quad[010]v_{t1} = \sqrt{\frac{C_{11}}{\rho}};\quad[001]v_{t2} = \sqrt{\frac{C_{44}}{\rho}} \tag*{(49)}

[001][001] direction:

[001]vl=C33ρ;[100]vt1=[010]vt2=C44ρ(50)[001]v_l = \sqrt{\frac{C_{33}}{\rho}};\quad[100]v_{t1} = [010]v_{t2} = \sqrt{\frac{C_{44}}{\rho}} \tag*{(50)}

here, vlv_l denotes the longitudinal mode, vt1v_{t1} refers to the first transverse mode and vt2v_{t2} denotes the second transverse mode.

Table 11 shows that the sound velocities of XIr3_3 materials along [100][100] and [001][001] directions are not same which implies that the materials will have lattice dynamical anisotropy. Thus, we can estimate that our materials will exhibit direction-dependent thermal and charge transport properties.

Except the [100]vl[100]v_l mode, all the other sound velocities are higher in LaIr3_3 compared to those in ThIr3_3.

Lattice thermal conductivity

The lattice thermal conductivity (kphk_{ph}) can be defined as the measurement of the ability of a material to conduct heat via phonons through its crystal structure. It demonstrates how heat is efficiently conducted through a material as a result of the phonons propagation. High thermal conductivity materials are desirable for efficient heat dissipation for applications such as in electronic devices, whereas low thermal conductivity materials are useful for thermal barriers. In this study, we have calculated the kphk_{ph} of XIr3_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds at room temperature (300K) by employing the following empirical formula proposed by [77] and the obtained values are disclosed in Table 12:

Compoundkphk_{ph}nn (102810^{28})[100] kmin⁡k_{\min}[1] kmin⁡k_{\min}kmin⁡k_{\min} Cahillkmin⁡k_{\min} Clarke
LaIr3_30.805.500.670.700.630.40
ThIr3_30.785.630.670.600.640.39

Table 12. Lattice thermal conductivity (kphk_{ph} in W/m-K) evaluated by Slack method at 300 K, number of atoms per unit volume (nn in m−3^{-3}), and minimum thermal conductivity (kmin⁡k_{\min} in W/m-K) evaluated by Cahill and Clarke model along [100] and [1] crystallographic directions of XXIr3_3 (XX = La, Th) compounds.

kph=A(γ)MavθD3δγ2n2/3T(51)k_{ph}=A(\gamma)\frac{M_{av}\theta_D^3\delta}{\gamma^2 n^{2/3}T} \tag*{(51)}

In the above formula, θD\theta_D is the Debye temperature, MavM_{av} stands for the average atomic mass, δ\delta refers to the cubic root of the average atomic volume, nn denotes the total number of atoms in the unit cell, γ\gamma is the Grüneisen parameter and TT stands for the absolute temperature. The following relations [77, 78] can be employed to obtain the parameter γ\gamma and the factor A(γ)A(\gamma):

γ=3(1+η)2(2−3η)(52)\gamma=\frac{3(1+\eta)}{2(2-3\eta)} \tag*{(52)}
A(γ)=5.720×107×0.8492×(1−0.514γ+0.228γ2)(53)A(\gamma)=\frac{5.720\times10^7\times0.849}{2\times\left(1-\frac{0.514}{\gamma}+\frac{0.228}{\gamma^2}\right)} \tag*{(53)}

where, η\eta stands for the Poisson’s ratio.

It is observed from the Table 12 that the lattice thermal conductivities of XIr3_3 (X=La,ThX = \mathrm{La}, \mathrm{Th}) materials are extremely low. The low values of kphk_{ph} and θD\theta_D of XIr3_3 materials suggesting that they can be used for thermal insulation purpose. It is also found that the kphk_{ph} value of LaIr3_3 is larger than that of ThIr3_3. Therefore, the compound LaIr3_3 is more thermally conductive than the ThIr3_3 compound.

Minimum thermal conductivity and its anisotropy

The lowest possible phonon thermal conductivity that a material exhibits at high temperatures is defined as the minimum thermal conductivity (kmink_{min}) of the material. The investigation of a material's minimal thermal conductivity has played vital role in the identification and development of material that can be utilized as TBC (thermal barrier coating) material. The presence of defects in a crystal has no effect on the kmink_{min}. In this work, we have calculated the kmink_{min} of XIr3_3 materials by employing the following formula proposed by Clarke [79]:

kmin=kBva(Vatomic)−2/3(54)k_{min}=k_Bv_a\left(V_{atomic}\right)^{-2/3} \tag*{(54)}

here, VatomicV_{atomic} refers to the atomic volume, vav_a denotes the average sound velocity and kBk_B is the Boltzmann constant.

The transfer of heat via thermal vibrations is dominated by the propagation of elastic waves. Since both the compounds under study are elastically anisotropic, they will have anisotropy in minimum thermal conductivity. The kmin⁡k_{\min} of XXIr3_3 materials along different crystallographic directions can be obtained by using the estimated acoustic velocities of the materials. In this study, we have employed the Cahill and Clarke [80] expression to estimate the kmin⁡k_{\min} of XXIr3_3 materials along [100] and [1] directions.

kmin⁡=kB2.48n2/3(vl+vt1+vt2)(55)k_{\min} = \frac{k_{\mathrm{B}}}{2.48} n^{2/3}(v_l + v_{t1} + v_{t2}) \tag*{(55)}

where, nn denotes the number of atoms per mole. The values of kmin⁡k_{\min} estimated from the Cahill and Clarke model are presented in Table 12.

Table 12 shows that the values of kmin⁡k_{\min} for both the materials are equal in [100] direction while in [1] direction the kmin⁡k_{\min} of LaIr3_3 is larger than that of ThIr3_3. Different values of kmin⁡k_{\min} in deferent directions indicate the presence of thermal anisotropy in the materials. It is also noted that the Cahill model estimates slightly higher kmin⁡k_{\min} than the Clarke model (see Table 12). It is noted that a material should have a kmin⁡k_{\min} value equal to or less than 1.25 W/m-K to be used as suitable TBC material [43, 81]. Therefore, the investigated materials can be used as potential TBC material.

Thermal expansion coefficient, heat capacity and wavelength of the dominant phonon

A material's thermal expansion coefficient (α\alpha) is a physical parameter that measures how much its dimensions change in response to a change in temperature. The potential of a material to be employed as a TBC material is strongly correlated with this parameter. This parameter is also linked to a variety of other physical properties, such as the thermal conductivity, melting temperature, specific heat, and so on. It is known that the α\alpha of a material is inversely related to its melting temperature (TmT_m), as follows: α≈0.02/Tm\alpha\approx0.02 / T_m [79, 82].

Another essential thermophysical parameter is the heat capacity per unit volume (ρCP\rho C_P). This parameter is also known as volumetric heat capacity. The change in heat energy of a unit volume in a material by one degree Kelvin change in temperature is called the ρCP\rho C_P of the material. It measures a material's capacity to store thermal energy as well as its thermal response to temperature changes.

Phonons are responsible for the heat and sound energy transmission in solids. It is defined as the quanta of lattice vibrations. Phonon plays a crucial role to determine the thermal conductivity, heat capacity and many other thermal and electrical properties. The wavelength corresponding to the peak of the phonon distribution function is known as the dominant phonon wavelength (λdom\lambda_{dom}).

In this section, we have estimated the α\alpha, ρCP\rho C_P and λdom\lambda_{dom} of XIr3_3 (X = La, Th) by using the relationships [79, 82, 83] given below and the results are disclosed in Table 13.

Table 13. The calculated thermal expansion coefficient (α\alpha in K−1^{-1}), volumetric heat capacity (ρCP\rho C_P in JK−1^{-1}m−3^{-3}), dominant phonon wavelength at 300K (λdom\lambda_{dom} in m) and melting point (TmT_m in K) of XIr3_3 (X = La, Th) materials.

α=1.6×10−3G(56)\alpha= \frac{1.6 \times10^{-3}}{G} \tag*{(56)}
ρCP=3kBΩ(57)\rho C_P = \frac{3k_B}{\Omega} \tag*{(57)}
λdom=12.566 vaT×10−12(58)\lambda_{dom} = \frac{12.566\,v_a}{T} \times10^{-12} \tag*{(58)}

In the above expressions, GG is the shear modulus, Ω\Omega denotes the volume per atom, and vav_a is the average sound velocity. It is seen from the Table 13 that the values of α\alpha and λdom\lambda_{dom} are much higher in LaIr3_3 than that of ThIr3_3. This happens due to the fact that the compound LaIr3_3 has smaller shear modulus and larger sound velocity compared to those of the ThIr3_3 compound. On the other hand, the value of ρCP\rho C_P is found to be higher in ThIr3_3 compared to the LaIr3_3.

Melting temperature

A material's melting temperature, also known as its melting point, is the temperature at which it transforms from a solid to a liquid phase at a certain atmospheric pressure. Nowadays the melting temperature (TmT_m) of a material is a fascinating and necessary topic of research. Higher melting temperature materials have lower thermal expansion, higher cohesive energy, and higher bonding energy [83]. Using the optimized elastic constants, we have calculated the TmT_m of XIr3_3 compounds by employing the formula given below [84]:

Tm=354+1.5(2C11+C33)(59)T_m = 354 + 1.5(2C_{11} + C_{33}) \tag*{(59)}

The calculated values of TmT_m of XIr3_3 materials are listed in Table 13. It is found that both the studied compounds have high melting point. This result suggests that they are suitable for high-temperature applications. It is also noticed that the compound ThIr3_3 has much higher melting point compared to the LaIr3_3 compound. Thus, ThIr3_3 will have higher bonding and cohesive energy compared to LaIr3_3.

Compoundα\alpha (10−5)(10^{-5})ρCP\rho C_{\mathrm{P}} (106)(10^{6})λdom\lambda_{\mathrm{dom}} (10−11)(10^{-11})TmT_{\mathrm{m}}
LaIr3_{3}3.072.288.461956.20
ThIr3_{3}2.772.338.282313.26

Table 15.

Optical properties

The optical properties of a material are essential for understanding how the material interacts with light and how light is reflected, refracted, absorbed, scattered, and transmitted as it travels through it. A number of energy-dependent optical parameters, including the absorption coefficient α(ω)\alpha(\omega), reflectivity R(ω)R(\omega), optical conductivity σ(ω)\sigma(\omega), refractive index n(ω)n(\omega), dielectric function ε(ω)\varepsilon(\omega), and energy loss function L(ω)L(\omega), can be used to predict the overall optical response of a material. In this study, we have calculated these optical parameters for XXIr3_{3} (X=La,ThX = \mathrm{La}, \mathrm{Th}) compounds and the outcomes are depicted in Figures 9 and 10. These optical constants have significant consequences for a variety of practical applications, such as optoelectronics, optical data storage, display systems, solar energy conversion, materials research etc. From the previously calculated elastic properties, it was found that the two compounds under study are elastically anisotropic. This suggests that the optical constants of XXIr3_{3} compounds might also show anisotropic nature. In this study, we have computed α(ω)\alpha(\omega), R(ω)R(\omega), σ(ω)\sigma(\omega), n(ω)n(\omega), ε(ω)\varepsilon(\omega), and L(ω)L(\omega) of XXIr3_{3} along [100] and [1] polarization directions for photon energies up to 40 eV. Since both the compounds under study are metallic in nature, Drude damping must be included while analyzing the optical parameters [85, 86]. Therefore, we have taken a Drude damping of 0.05 eV for the analysis of the optical parameters. The obtained results are discussed in the following sub-sections.

Absorption coefficient

The absorption coefficient (α\alpha) of a material determines the amount of photon energy absorbed by the material. From the absorption spectra, we can estimate the electronic nature of a material (metal, semiconductor or insulator). This parameter also provides information on the optimal solar energy conversion efficiency. The absorption spectra of XXIr3_{3} compounds are shown in Figures 9(a), and 10(a). These plots show that absorption begins from zero photon energy for both the compounds. This confirms the metallic nature of the compounds. It is also noticed that the α(ω)\alpha(\omega) are quite high in the ultraviolet region (UV) from 20 eV to 30 eV. In this energy range the peak value of α(ω)\alpha(\omega) of XXIr3_{3} is slightly higher in [1] direction compared to that in [100] direction which indicates small optical anisotropy of the compounds. It is also important to note that the α(ω)\alpha(\omega) of XXIr3_{3} compounds reduces drastically around 35 eV, which is closely associated with the location of the loss peak.

Reflectivity

The computed frequency dependent optical reflectivity (RR) profiles of XXIr3_{3} compounds along [100] and [1] directions are depicted in Figure 9(b) and Figure 10(b). For both the compounds, the calculated R(ω)R(\omega) along [100] and [1] directions have roughly the similar shape, but the peak heights and positions differ slightly. It is also found that the maximum value (about 70% to 78%) of R(ω)R(\omega) occurs at zero photon energy. The value of R(ω)R(\omega) then decreases drastically in the infrared and visible energy region (see Figure 9(b) and Figure 10(b)). In the mid UV region, R(ω)R(\omega) increases abruptly and reaches a peak then decreases sharply around 35 eV.

Figure 9. The computed (a) absorption coefficient, (b) reflectivity, (c) conductivity, (d) refractive index, (e) dielectric function, and (f) loss function of LaIr3\mathrm{LaIr}_3 along [100][100] and [001][001] polarization directions as a function of energy.

Computed absorption coefficient, reflectivity, conductivity, refractive index, dielectric function, and loss function of ThIr3

Figure 10. The computed (a) absorption coefficient, (b) reflectivity, (c) conductivity, (d) refractive index, (e) dielectric function, and (f) loss function of ThIr3_3 along [100] and [1] polarization directions as a function of energy.

Optical conductivity

The conductivity (σ\sigma) spectra of a material can be used to understand its electromagnetic response in the presence of a time-varying electric field. This parameter also provides important details regarding the electronic band structure and photoconductivity of a material. Figure 9(c) and Figure 10(c) show that the σ(ω)\sigma(\omega) of XIr3\mathrm{XIr}_{3} compounds begins from 0 eV which indicates once again the metallic nature of the compounds. The maximum values of σ(ω)\sigma(\omega) of both the studied compounds occur in the lower photon energy (about 1 to 5 eV). Again, the values of σ(ω)\sigma(\omega) tends to zero in the higher photon energy (about 35 eV). Slight change is observed in σ(ω)\sigma(\omega) spectra with respect to the [100] and [1] polarization directions which implies small amount of anisotropy in XIr3\mathrm{XIr}_{3}. This anisotropy is slightly higher in ThIr3_3 compound compared to that in the LaIr3_3 compound.

Refractive index

The real (Re), n(ω)n(\omega) and imaginary (Im), k(ω)k(\omega) parts of refractive index are two important optical constants. The imaginary part k(ω)k(\omega) is also known as the extinction coefficient. The n(ω)n(\omega) of refractive index determines the phase velocity of an electromagnetic wave and the amount of bending of light, while the extinction coefficient governs the amount of absorption or attenuation of light within the medium. For the optimal design of photoelectric devices, accurate knowledge of the complex refractive index of a material is necessary. The variation of n(ω)n(\omega) and k(ω)k(\omega) of XIr3\mathrm{XIr}_{3} materials for [100] and [1] polarizations of the incident electric field are shown in Figure 9(d) and Figure 10(d). The n(0)n(0) (static) values of XIr3\mathrm{XIr}_{3} materials are quite high (between 10 and 14), indicating that these materials have the potential to be utilized in applications involving display devices and wave-guides. It can be concluded from the plots that for both the materials, n(ω)n(\omega) decreases sharply in the lower energy region (0 to 3 eV) and then almost have the same value in the higher energy region. Again, the extinction coefficient (kk) of XIr3\mathrm{XIr}_{3} materials reaches its peak value in the lower energy region. Furthermore, the value of k(ω)k(\omega) decreases gradually in the mid-ultraviolet region and then tends to zero in the higher energy region (about 35 eV).

Dielectric function

The complex dielectric function, ε(ω)\varepsilon(\omega) of a material can be used to calculate the other optical constants, including optical conductivity, refractive index, reflectivity, energy loss function and absorption of light. The real (Re), ε1(ω)\varepsilon_{1}(\omega) part of the dielectric function describes the polarization of the material. This part is also connected to the permittivity component. On the other hand, the imaginary (Im), ε2(ω)\varepsilon_{2}(\omega) part of the dielectric function corresponds to the dielectric loss in the optical system. Figure 9(e) and Figure 10(e) illustrate the variation of ε1(ω)\varepsilon_{1}(\omega) and ε2(ω)\varepsilon_{2}(\omega) of XIr3\mathrm{XIr}_{3} compounds as a function of photon energy. From these plots it is seen that the ε1(ω)\varepsilon_{1}(\omega) of XIr3\mathrm{XIr}_{3} crosses zero from below in the mid UV range (about 14 to 16 eV), suggesting that the compounds are metal. It is also noticed that for both the compounds the peak value of ε2(ω)\varepsilon_{2}(\omega) occurs in the lower photon energy. This suggests that the dielectric loss will be maximum at that peak energy. Furthermore, at ∼30\sim30 eV the value of ε2(ω)\varepsilon_{2}(\omega) of both the compounds reduces to zero, which suggests that these compounds will be transparent above this energy. Despite the nearly identical shapes of the dielectric spectra of XIr3\mathrm{XIr}_{3} compounds along [100] and [1] directions, there is some anisotropy over the whole energy/frequency range.

Energy loss function

The energy loss function, L(ω)L(\omega) of a material provides valuable information about the electronic structure, plasmon resonance, absorption coefficient and reflectivity of the material [87, 88]. This parameter also defines how much energy is lost when a fast electron traverses through the material. Furthermore, the plasma frequency (ωp\omega_{p}) of a material is associated with the peak value of L(ω)L(\omega). The L(ω)L(\omega) spectra of XIr3\mathrm{XIr}_{3} compounds are presented in Figure 9(f) and Figure 10(f) along [100] and [1] polarization directions. The peak values of L(ω)L(\omega) of LaIr3\mathrm{LaIr}_{3} compound in both the polarization directions are found at 32.8 eV. On the other hand, the peak values of L(ω)L(\omega) of ThIr3\mathrm{ThIr}_{3} compound along [100] and [1] polarization directions are found at 32.3 and 31.8 eV, respectively. Thus, for ThIr3\mathrm{ThIr}_{3} compound the value of ωp\omega_{p} is larger in [100] direction than [1] direction which indicates small amount of optical anisotropy in the compound. It can also be concluded from the Figure 9 and Figure 10 that ωp\omega_{p} coincide with the sudden change in the absorption and reflectivity spectra of XIr3\mathrm{XIr}_{3} compounds. Therefore, both the compounds will show optical properties similar to an insulator and will become transparent to incident light at energies above the ωp\omega_{p}. Moreover, it is observed from the plots (see Figure 9 and Figure 10) that in the lower photon energy (0 to 10 eV) the L(ω)L(\omega) spectra have no peaks. This is caused by the high value of ε2(ω)\varepsilon_{2}(\omega) in that energy range [89].

Superconducting state properties

Superconducting materials possess some very special electrical and magnetic properties which make them useful for a variety of technological applications. The superconducting state of a material is largely influenced by the electron-phonon coupling constant (λe−p\lambda_{e-p}) of the material. In this section, we have employed the well-known McMillan equation [90] to estimate the superconducting transition temperature (TcT_c) of the XIr3_3 (X = La, Th) compounds.

Tc=θD1.45exp⁡[−1.04(1+λe−p)λe−p−μ∗(1+0.62λe−p)](60)T_c = \frac{\theta_D}{1.45}\exp\left[\frac{-1.04(1+\lambda_{e-p})}{\lambda_{e-p}-\mu^{*}(1+0.62\lambda_{e-p})}\right] \tag*{(60)}

here, θD\theta_D is the Debye temperature and μ∗\mu^{*} refers to the repulsive screened Coulomb part (also known as the Coulomb pseudopotential) of the material. We have calculated the μ∗\mu^{*} of XIr3_3 materials by employing the equation given below [91]:

μ∗=0.26N(EF)1+N(EF)(61)\mu^{*} = \frac{0.26N(E_F)}{1+N(E_F)} \tag*{(61)}

where, N(EF)N(E_F) is the value of the TDOS of the compound at the Fermi level. The strength of the electron-phonon coupling of a material is described by the constant λe−p\lambda_{e-p}. In this study, we have calculated the λe−p\lambda_{e-p} of XIr3_3 materials by using the following expression [92, 93]:

λe−p=γexpγcal−1(62)\lambda_{e-p} = \frac{\gamma_{exp}}{\gamma_{cal}}-1 \tag*{(62)}

In the above expression, γexp\gamma_{exp} is the experimental linear coefficient of the electronic specific heat and γcal\gamma_{cal} is its theoretical counterpart calculated from the TDOS at the Fermi level found from the band structure calculations. In this work, we have calculated γcal\gamma_{cal} of XIr3_3 materials by using the following equation [93, 94, 95]:

γcal=π2kB2N(EF)3(63)\gamma_{cal} = \frac{\pi^2 k_B^2 N(E_F)}{3} \tag*{(63)}

The calculated values of superconducting parameters including the critical temperatures of XIr3_3 compounds are presented in Table 14. The Tc values obtained show reasonable agreement with the experimental ones [1, 4].

ParameterUnitLaIr3_3ThIr3_3Ref.
TcT_\mathrm{c}K4.915.01This work
TcT_\mathrm{c}K3.324.41[1, 4]
μ∗\mu^{*}---0.2010.198This work
μ∗\mu^{*}---0.150.13[1, 4]
λe−p\lambda_{e-p}---0.850.86This work
λe−p\lambda_{e-p}---0.570.74[1, 4]
γcal\gamma_\mathrm{cal}mJ/(mol-K2^2)8.177.57This work
γexp\gamma_\mathrm{exp}mJ/(mol-K2^2)15.3217.60[4, 9]

Table 14. Superconducting state parameters of XIr3_3 (X = La, Th) compounds along with the previously estimated values.

For ThIr3_3 compound, the value of λe−p\lambda_{e-p} calculated from Eqn. (62) is in reasonable agreement with the value obtained from the Eliashberg spectral function. From the calculated values of λe−p\lambda_{e-p}, it can be suggested that both the compounds under study are moderately coupled electron-phonon superconductor. It is also noticed from the Table 14 that the computed values of μ∗\mu^{*} of XIr3_3 compounds are much higher than those used in the previous studies [1, 4]. In earlier works [1.4] the values of μ∗\mu^{*} were selected ad-hoc without taking consideration of the material specific electronic features. Furthermore, it is found that the parameters (θD\theta_D, λe−p\lambda_{e-p}, and μ∗\mu^{*}) determining the superconducting critical temperatures of LaIr3_3 and ThIr3_3 are almost identical. It is instructive to note that the electron phonon coupling constant can be expressed as a product of two terms, N(EF)N(E_F) and Ve−phV_{e-ph} [96], where Ve−phV_{e-ph} is the electron-phonon interaction energy. Thus almost identical values of λe−p\lambda_{e-p} of XIr3_3 (X = La, Th) compounds imply that the electron-phonon interaction energy is stronger in ThIr3_3, since N(EF)N(E_F) is found to be higher for LaIr3_3.

Conclusions

A large number of unexplored physical properties of XIr3_3 (XX = La, Th) compounds have been investigated in details. Some of the properties have been revisited and fair agreements with previous results are found. The compounds under study are mechanically stable, highly ductile, elastically anisotropic, and extremely machinable with moderate hardness. The computed Debye temperatures, minimum thermal conductivities are low. At the same time, the melting temperatures are high. High ductility, machinability, dry lubricity, and high fracture toughness indicates that the XIr3_3 (XX = La, Th) compounds have desirable traits for structural engineering applications. Low phonon thermal conductivity and high melting point imply that these to materials can be used for thermal insulation at high temperatures. The bonding nature has been investigated in details. Both the compounds show prominent ionic character with some covalent contributions.

The optical properties were investigated thoroughly for the first time. The optical parameters show weakly anisotropic features and reconfirm the metallic characters. The compounds are found to be efficient absorber of ultraviolet light. They are also good reflector (R>50%R > 50\%) of visible light that suggests that these materials can be used as efficient solar energy reflector. Very high values of low energy refractive index [n(0)>10n(0) > 10] further suggest that XIr3_3 (XX = La, Th) compounds possess features suitable for optoelectronic device applications. Nearly same plasma frequency for both the compounds indicates that carrier effective mass and concentrations are almost identical.

Highly dispersive bands are seen near the Γ\Gamma-point in the band profiles of the compounds which implies low effective mass and high mobility of the charge carriers. It is found from the DOS profiles of XIr3_3 compounds that the Ir-5d5d states largely contribute to the TDOS near the Fermi level. This indicates that the metallic conductivity in the compounds is governed mainly by the 5d5d states of Ir atom.

The calculated values of superconducting transition temperatures of XIr3_3 compounds are in close agreement with the previously estimated experimental values. Interestingly, the Fermi level of LaIr3_3 is located at a rapidly changing part of the TDOS profile. Therefore, any shift in the Fermi energy due to applied pressure or suitable atomic substitution is expected to change the N(EF)N(E_{\mathrm{F}}) significantly. Such modifications should significantly change the normal state charge transport properties, superconducting transition temperature, and superconducting condensation energy [97].

To conclude, a large number of physical features of the XIr3_3 (XX = La, Th) compounds have been investigated theoretically in this article. Most of the studied physical features are novel and can be used as references in further research.

Acknowledgments

Authors are grateful to the Department of Physics, Chittagong University of Engineering & Technology (CUET), Chattogram-4349, Bangladesh, for providing the computing facilities for this work. This work was also carried out with the aid of a grant (grant number: 21-378 RG/PHYS/AS_G-FR3240319526) from UNESCO-TWAS and the Swedish International Development Cooperation Agency (SIDA). The views expressed herein do not necessarily represent those of UNESCO-TWAS, SIDA, or its Board of Governors.

Author Contributions

Md. Sajidul Islam: Methodology, Formal analysis, Writing − original draft; Razu Ahmed: Methodology, Formal analysis; M. A. Ali: Formal analysis, Writing − original draft, Validation; M. M. Hossain: Formal analysis, Writing review & editing, Validation; M. M. Uddin: Writing review & editing, Validation; S. H. Naqib: Conceptualization, Formal analysis, Writing review & editing, Validation, Supervision.

Declaration of interest

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

Data availability

The data sets generated and/or analyzed in this study are available from the corresponding author on reasonable request.

References

  1. [1]N. Haldolaarachchige, L. Schoop, M. A. Khan, W. Huang, H. Ji, K. Hettiarachchilage, and D. P. Young, Ir d-band Derived Superconductivity in the Lanthanum-Iridium System LaIr₃, J. Phys.: Condens. Matter 29, 475602 (2017).DOI
  2. [2]S. Disseler, C. Dhital, A. Amato, S. Giblin, C. de la Cruz, S. Wilson, and M. Graf, Magnetic order in the pyrochlore iridates A₂Ir₂O₇ (A = Y, Yb), Phys. Rev. B 86, 014428 (2012).DOI
  3. [3]K. H. J. Buschow, Intermetallic compounds of rare-earth and 3d transition metals, Rep. Prog. Phys. 40, 1179 (1977).
  4. [4]K. Górnicka, D. Das, S. Gutowska, B. Wiendlocha, M. J. Winiarski, T. Klimczuk, and D. Kaczorowski, Iridium 5d-electron driven superconductivity in ThIr₃, Phys. Rev. B 100, 214514 (2019).DOI
  5. [5]K. Górnicka, E. M. Carnicom, S. Gołąb, M. Łapiński, B. Wiendlocha, W. Xie, D. Kaczorowski, R. J. Cava, and T. Klimczuk, CeIr₃: Superconductivity in a phase based on tetragonally close packed lusters, Supercond. Sci. Technol. 32, 025008 (2019).DOI
  6. [6]N. Haldolaarachchige, Q. Gibson, L. M. Schoop, H. Luo, and R. J. Cava, Characterization of the Heavy Metal Pyrochlore Lattice Superconductor CaIr₂, J. Phys.: Condens. Matter 27, 185701 (2015).DOI
  7. [7]D. Hirai, M. N. Ali, and R. J. Cava, Strong Electron-Phonon Coupling Superconductivity Induced by a Low-Lying Phonon in IrGe, J. Phys. Soc. Japan 82, 124701 (2013).DOI
  8. [8]T. Klimczuk, F. Ronning, V. Sidorov, R. J. Cava, and J. D. Thompson, Physical Properties of the noncentrosymmetric superconductor Mg₁₀Ir₁₉B₁₆, Phys. Rev. Lett. 99, 257004 (2007).
  9. [9]A. Bhattacharyya, D. T. Adroja, P. K. Biswas, Y. J. Sato, M. R. Lees, D. Aoki, and A. D. Hillier, Ir 5d-Band Derived Superconductivity in LaIr₃, J. Phys.: Condens. Matter 32, 065602 (2020).DOI
  10. [10]M. D. Segall, P. J. D. Lindan, M. J. Probert, C. J. Pickard, P. J. Hasnip, S. J. Clark, and M. C. Payne, First-principles simulation: ideas, illustrations and the CASTEP code, J. Phys.: Condens. Matter 14, 2717 (2002).
  11. [11]J. A. Pople, P. M. W. Gill, and B. G. Johnson, Kohn-Sham density-functional theory within a finite basis set, Chem. Phys. Lett. 199, 557 (1992).DOI
  12. [12]W. Kohn and L. J. Sham, Self-Consistent Equations Including Exchange and Correlation Effects, Phys. Rev. 140, A1133 (1965).
  13. [13]M. Lewin, E. H. Lieb, and R. Seiringer, The Local Density Approximation in Density Functional Theory, Pure Appl. Anal. 2, 35 (2019).
  14. [14]J. P. Perdew, K. Burke, and M. Ernzerhof, Generalized Gradient Approximation Made Simple, Phys. Rev. Lett. 77, 3865 (1996).
  15. [15]D. Vanderbilt, Soft self-consistent pseudopotentials in a generalized eigenvalue formalism, Phys. Rev. B Condens. Matter 41, 7892 (1990).
  16. [16]T. H. Fischer and J. Almlof, General methods for geometry and wave function optimization, J. Phys. Chem. 96, 9768 (1992).
  17. [17]H. J. Monkhorst and J. D. Pack, Special points for Brillouin-zone integrations, Phys. Rev. B 13, 5188 (1976).
  18. [18]G. P. Francis and M. C. Payne, Finite basis set corrections to total energy pseudopotential calculations, J. Phys.: Condens. Matter 2, 4395 (1990).
  19. [19]O. H. Nielsen and R. M. Martin, First-Principles Calculation of Stress, Phys. Rev. Lett. 50, 697 (1983).
  20. [20]J. P. Watt, Hashin-Shtrikman bounds on the effective elastic moduli of polycrystals with orthorhombic symmetry, J. Appl. Phys. 50, 6290 (2008).
  21. [21]J. P. Watt and L. Peselnick, Clarification of the Hashin-Shtrikman bounds on the effective elastic moduli of polycrystals with hexagonal, trigonal, and tetragonal symmetries, J. Appl. Phys. 51, 7 (1980).DOI
  22. [22]R. S. Mulliken, Electronic Population Analysis on LCAO-MO Molecular Wave Functions. I, J. Chem. Phys. 23, 1833 (1955).DOI
  23. [23]D. Sanchez-Portal, E. Artacho, and J. M. Soler, Projection of plane-wave calculations into atomic orbitals, Solid State Commun. 95, 685 (1995).DOI
  24. [24]M. D. Segall, R. Shah, C. J. Pickard, and M. C. Payne, Population analysis of plane-wave electronic structure calculations of bulk materials, Phys. Rev. B 54, 16317 (1996).
  25. [25]F. Parvin and S. H. Naqib, Structural, Elastic, Electronic, Thermodynamic, and Optical Properties of Layered BaPd₂As₂ Pnictide Superconductor: A First Principles Investigation, J. Alloys Compd. 780, 452 (2019).arxiv.org/abs/1810.12694
  26. [26]R. Ahmed, M. Mahamudujjaman, M. A. Afzal, M. S. Islam, R. S. Islam, and S. H. Naqib, DFT based comparative analysis of the physical properties of some binary transition metal carbides XC (X = Nb, Ta, Ti), J. Mater. Res. Technol. 24, 4808 (2023).
  27. [27]G. Murtaza, N. Yousaf, M. Yaseen, A. Laref, and S. Azam, Systematic studies of the structural and optoelectronic characteristics of CaZn₂X₂ (X = N, P, As, Sb, Bi), Mater. Res. Express 5, 016304 (2018).DOI
  28. [28]Md. Sajidul Islam, R. Ahmed, Md. Mahamudujjaman, R. S. Islam, and S. H. Naqib, A comparative study of the structural, elastic, thermophysical, and optoelectronic properties of CaZn₂X₂ (X = N, P, As) semiconductors via ab-initio approach, Results Phys. 44, 106214 (2023).
  29. [29]F. C. Frank and J. S. Kasper, Complex alloy structures regarded as sphere packings. I. Definitions and basic principles, Acta Crystallogr. 11, 3 (1958).DOI
  30. [30]F. Mouhat and F. X. Coudert, Necessary and Sufficient Elastic Stability Conditions in Various Crystal Systems, Phys. Rev. B 90, 224104 (2014).DOI
  31. [31]D. G. Pettifor, Theoretical predictions of structure and related properties of intermetallics, Mater. Sci. and Technol. 8, 345 (1992).DOI
  32. [32]M. I. Naher and S. H. Naqib, Structural, elastic, electronic, bonding, and optical properties of topological CaSn₃ semimetal, J. Alloys Compd. 829, 154509 (2020).
  33. [33]W. Voigt, Lehrbuch der kristallphysik (mit ausschluss der kristalloptik), Nachdruck der ersten Aufl. (B.G. Teubner, [J.W. Edwards], Leipzig, Berlin, 1928).
  34. [34]A. Reuss, Berechnung der Fließgrenze von Mischkristallen auf Grund der Plastizitätsbedingung für Einkristalle ., Z. angew. Math. Mech. 9, 49 (1929).DOI
  35. [35]J. A. Majewski and P. Vogl, Simple model for structural properties and crystal stability of sp-bonded solids, Phys. Rev. B 35, 9666 (1987).
  36. [36]C. Kittel, Introduction to Solid State Physics, 8th ed (Wiley, Hoboken, NJ, 2005).
  37. [37]K. H. Yildirim A, First-principles study of the structural, elastic, electronic, optical, and vibrational properties of intermetallic Pd₂Ga, Chin. Phys. B 21, 37101 (2012).
  38. [38]B. Rahman Rano, I. M. Syed, and S. H. Naqib, Elastic, Electronic, Bonding, and Optical Properties of WTe₂ Weyl Semimetal: A Comparative Investigation with MoTe₂ from First Principles, Results Phys 19, 103639 (2020).DOI
  39. [39]S. F. Pugh, XCII. Relations between the elastic moduli and the plastic properties of polycrystalline pure metals, London, Edinburgh, Dublin Philos. Mag. J. Sci. 45, 823 (1954).DOI
  40. [40]P. Ravindran, L. Fast, P. A. Korzhavyi, B. Johansson, J. Wills, and O. Eriksson, Density functional theory for calculation of elastic properties of orthorhombic crystals: Application to TiSi₂, J. Appl. Phys. 84, 4891 (1998).DOI
  41. [41]O. L. Anderson and H. H. Demarest Jr., Elastic constants of the central force model for cubic structures: Polycrystalline aggregates and instabilities, J. Geophys. Res. 76, 1349 (1971).DOI
  42. [42]G. Vaitheeswaran, V. Kanchana, A. Svane, and A. Delin, Elastic properties of MgCNi₃−a superconducting perovskite, J. Phys.: Condens. Matter 19, 326214 (2007).DOI
  43. [43]M. Roknuzzaman, M. A. Hadi, M. J. Abedin, M. T. Nasir, A. K. M. A. Islam, M. S. Ali, K. Ostrikov, and S. H. Naqib, Physical properties of predicted Ti₂CdN versus existing Ti₂CdC MAX phase: An ab initio study, Computational Materials Science 113, 148 (2016).
  44. [44]L. Kleinman, Deformation Potentials in Silicon. I. Uniaxial Strain, Phys. Rev. 128, 2614 (1962).
  45. [45]Z. Sun, D. Music, R. Ahuja, and J. M. Schneider, Theoretical investigation of the bonding and elastic properties of nanolayered ternary nitrides, Phys. Rev. B 71, 193402 (2005).DOI
  46. [46]M. A. Ali, M. M. Hossain, M. A. Hossain, M. T. Nasir, M. M. Uddin, M. Z. Hasan, A. K. M. A. Islam, and S. H. Naqib, Recently synthesized (Zr₁−xTix)₂AlC (0 ≤ x ≤ 1) solid solutions: Theoretical study of the effects of M mixing on physical properties, J. Alloys Compd. 743, 146 (2018).
  47. [47]M. A. Ali, M. A. Hadi, M. M. Hossain, S. H. Naqib, and A. K. M. A. Islam, Theoretical investigation of structural, elastic, and electronic properties of ternary boride MoAlB, Phys. Status Solidi b 254, 17000010 (2017).DOI
  48. [48]H. Mebtouche, O. Baraka, A. Yakoubi, R. Khenata, S. A. Tahir, R. Ahmed, S. H. Naqib, A. Bouhemadou, S. Bin Omran, and X. Wang, First-principles calculations of the structural, electronic, mechanical and thermodynamic properties of MAX phase Moₙ₊₁GeCₙ (n = 1–3) compounds, Mater. Today Commun. 25, 101420 (2020).DOI
  49. [49]M. A. Ali and S. H. Naqib, Recently synthesized (Ti₁−xMox)₂AlC (0 ≤ x ≤ 0.20) solid solutions: deciphering the structural, electronic, mechanical and thermodynamic properties via ab initio simulations, RSC Adv. 10, 31535 (2020).
  50. [50]N. Miao, B. Sa, J. Zhou, and Z. Sun, Theoretical investigation on the transition-metal borides with Ta₃B₄-type structure: a class of hard and refractory materials, Comput. Mater. Sci. 50, 1559 (2011).DOI
  51. [51]A. Bouhemadou, First-principles study of structural, electronic and elastic properties of Nb₄AlC₃, Braz. J. Phys. 40, 52 (2010).
  52. [52]X. Q. Chen, H. Niu, D. Li, and Y. Li, Modeling hardness of polycrystalline materials and bulk metallic glasses, Intermetallics 19, 1275 (2011).DOI
  53. [53]Y. Tian, B. Xu, and Z. Zhao, Microscopic theory of hardness and design of novel superhard crystals, Int. J. Refract. Hard Mat. 33, 93 (2012).DOI
  54. [54]D. M. Teter, Computational Alchemy: The Search for New Superhard Materials, MRS Bull. 23, 22 (1998).DOI
  55. [55]E. Mazhnik and A. R. Oganov, A model of hardness and fracture toughness of solids, J. Appl. Phys. 126, 125109 (2019).
  56. [56]H. Niu, S. Niu, and A. R. Oganov, Simple and accurate model of fracture toughness of solids, J. Appl. Phys. 125, 065105 (2019).DOI
  57. [57]D. H. Chung and W. R. Buess​​em, The Elastic Anisotropy of Crystals, J. Appl. Phys. 38, 2010 (2004).
  58. [58]S. I. Ranganathan and M. Ostoja-Starzewski, Universal Elastic Anisotropy Index, Phys. Rev. Lett. 101, 055504 (2008).
  59. [59]C. M. Kube and M. de Jong, Elastic constants of polycrystals with generally anisotropic crystals, J. Appl. Phys. 120, 165105 (2016).DOI
  60. [60]R. Gaillac, P. Pullumbi, and F.-X. Coudert, ELATE: an open-source online application for analysis and visualization of elastic tensors, J. Phys.: Condens. Matter 28, 275201 (2016).DOI
  61. [61]F. L. Hirshfeld, Bonded-atom fragments for describing molecular charge densities, Theoret. Chim. Acta 44, 129 (1977).DOI
  62. [62]R. C. D. Richardson, The wear of metals by hard abrasives, Wear 10, 291 (1967).
  63. [63]V. V. Brazhkin, A. G. Lyapin, and R. J. Hemley, harder than diamond: dreams and reality, Philos. Mag. A 82, 231 (2002).DOI
  64. [64]F. Gao, Theoretical model of intrinsic hardness, Phys. Rev. B 73, 132104 (2006).
  65. [65]F. Birch, Finite strain isotherm and velocities for single-crystal and polycrystalline NaCl at high pressures and 300°K, J. Geophys. Res. 83, 1257 (1978).DOI
  66. [66]M. I. Naher and S. H. Naqib, A comprehensive study of the thermophysical and optoelectronic properties of Nb₂P₅ via ab-initio technique, Results Phys. 28, 104623 (2021).arxiv.org/abs/2103.16027
  67. [67]R. D. Harcourt, Diatomic antibonding Σ*s orbitals as “metallic orbitals” for electron conduction in alkali metals, J. Phys. B: Atom. Mol. Phys. 7, L41 (1974).DOI
  68. [68]K. Boudiaf, A. Bouhemadou, Y. Al-Douri, R. Khenata, S. Bin-Omran, and N. Guechi, Electronic and thermoelectric properties of the layered BaFAgCh (Ch = S, Se and Te): first-principles study, J. Alloys Compd. 759, 32 (2018).
  69. [69]A. Bekhti-Siad, K. Bettine, D. P. Rai, Y. Al-Douri, X. Wang, R. Khenata, A. Bouhemadou, and C. H. Voon, Electronic, optical and thermoelectric investigations of Zintl phase AE₃AlAs₃ (AE = Sr, Ba): First-principles calculations, Chinese J. Phys. 56, 870 (2018).DOI
  70. [70]A. Belhachemi, H. Abid, Y. Al-Douri, M. Sehil, A. Bouhemadou, and M. Ameri, First-principles calculations to investigate the structural, electronic and optical properties of Zn₁₋ₓMgₓTe ternary alloys, Chinese J. Phys. 55, 1018 (2017).
  71. [71]J. H. Xu, T. Oguchi, and A. J. Freeman, Solid-solution strengthening: Substitution of V in Ni₃Al and structural stability of Ni₃(Al,V), Phys. Rev. B 36, 4186 (1987).
  72. [72]T. Hong, T. J. Watson-Yang, A. J. Freeman, T. Oguchi, and J. Xu, Crystal structure, phase stability, and electronic structure of Ti-Al intermetallics: TiAl₃, Phys. Rev. B 41, 12462 (1990).
  73. [73]F. Parvin and S. H. Naqib, Pressure dependence of structural, elastic, electronic, thermodynamic, and optical properties of van der Waals-type NaSn₂P₂ pnictide superconductor: insights from DFT study, Results Phys. 21, 103848 (2021).
  74. [74]O. L. Anderson, A simplified method for calculating the Debye temperature from elastic constants, J. Phys. Chem. Solids 24, 909 (1963).DOI
  75. [75]E. Schreiber, O. L. Anderson, and N. Soga, Elastic Constants and Their Measurement (McGraw-Hill, 1974).
  76. [76]Y. H. Duan, Y. Sun, M. J. Peng, and S. G. Zhou, Anisotropic elastic properties of the Ca–Pb compounds, J. Alloys Compd. Complete, 14 (2014).DOI
  77. [77]G. A. Slack, The Thermal Conductivity of Nonmetallic Crystals, Solid-State Phys. 34, 1 (1979).
  78. [78]C. L. Julian, Theory of Heat Conduction in Rare-Gas Crystals, Phys. Rev. 137, A128 (1965).
  79. [79]D. R. Clarke, Materials selection guidelines for low thermal conductivity thermal barrier coatings, Surf. Coat. Technol. 163–164, 67 (2003).
  80. [80]D. G. Cahill, S. K. Watson, and R. O. Pohl, Lower limit to the thermal conductivity of disordered crystals, Phys. Rev. B 46, 6131 (1992).
  81. [81]Y. Liu, V. R. Cooper, B. Wang, H. Xiang, Q. Li, Y. Gao, J. Yang, Y. Zhou, and B. Liu, Discovery of ABO₃ perovskites as thermal barrier coatings through high-throughput first principles calculations, Mater. Res. Lett. 7, 145 (2019).
  82. [82]M. I. Naher, M. A. Afzal, and S. H. Naqib, A comprehensive DFT based insights into the physical properties of tetragonal superconducting Mo₅PB₂, Results Phys. 28, 104612 (2021).
  83. [83]M. I. Naher and S. H. Naqib, An ab-initio study on structural, elastic, electronic, bonding, thermal, and optical properties of topological Weyl semimetal TaX (X = P, As), Sci. Rep. 11, 1 (2021).
  84. [84]M. E. Fine, L. D. Brown, and H. L. Marcus, Elastic constants versus melting temperature in metals, Scr. Meter. 18, 951 (1984).
  85. [85]A. H. Reshak, V. V. Atuchin, S. Auluck, and I. V. Kityk, First and second harmonic generation of the optical susceptibilities for the non-centro-symmetric orthorhombic AgCd₂GaS₄, J. Phys.: Condens. Matter 20, 325234 (2008).
  86. [86]S. Li, R. Ahuja, M. W. Barsoum, P. Jena, and B. Johansson, Optical properties of Ti₃SiC₂ and Ti₄AlN₃, Appl. Phys. Lett. 92, 221907 (2008).
  87. [87]J. Sun, H. T. Wang, J. He, and Y. Tian, Ab initio investigations of optical properties of the high-pressure phases of ZnO, Phys. Rev. B 71, 125132 (2005).
  88. [88]Y. C. Cheng, X. L. Wu, J. Zhu, L. L. Xu, S. H. Li, and P. K. Chu, Optical properties of rocksalt and zinc blende AlN phases: First-principles calculations, J. Appl. Phys. 103, 073707 (2008).
  89. [89]M. Roknuzzaman, M. A. Hadi, M. A. Ali, M. M. Hossain, N. Jahan, M. M. Uddin, J. A. Alarco, and K. Ostrikov, First hafnium-based MAX phase in the 312 family, Hf3AlC2: A first-principles study, J. Alloys Compd. 727, 616 (2017).
  90. [90]W. L. McMillan, Transition Temperature of Strong-Coupled Superconductors, Phys. Rev. 167, 331 (1968).
  91. [91]N. Sadat Khan, B. Rahman Rano, I. M. Syed, R. S. Islam, and S. H. Naqib, First-principles prediction of pressure dependent mechanical, electronic, optical, and superconducting state properties of NaC6: A potential high-Tc superconductor, Results Phys. 33, 105182 (2022).
  92. [92]S. Ram, V. Kanchana, G. Vaitheswaran, A. Svane, S. B. Dugdale, and N. E. Christensen, Electronic topological transition in LaSn3 under pressure, Phys. Rev. B 85, 174531 (2012).
  93. [93]Z. Lin, L. V. Zhigilei, and V. Celli, Electron-phonon coupling and electron heat capacity of metals under conditions of strong electron-phonon nonequilibrium, Phys. Rev. B 77, 075133 (2008).
  94. [94]J. Islam, S. K. Mitro, M. M. Hossain, M. M. Uddin, N. Jahan, A. K. M. A. Islam, S. H. Naqib, and M. A. Ali, Exploration of the physical properties of the newly synthesized kagome superconductor LaIr3Ga2 using different exchange-correlation functionals, Phys. Chem. Chem. Phys. 24, 29640 (2022).
  95. [95]Z. Guguchia et al., Tunable anomalous Hall conductivity through volume-wise magnetic competition in a topological kagome magnet, Nat. Commun. 11, 1 (2020).
  96. [96]A. K. M. A. Islam and S. H. Naqib, Possible Explanation of High-Tc in Some 2D Cuprate Superconductors, J. Phys. Chem. Solids 58, 1153 (1997).
  97. [97]S. H. Naqib and R. S. Islam, Interrelations among zero-field critical current density, irreversibility field and pseudogap in hole doped high-Tc cuprates, Physica C 608, 1354255 (2023).

Paper details

vlnc:W_txz52v45
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents