betaFeedback

WorksPhysics and Astronomy

Temperature dependence of 7Li NMR relaxation rates in Li3InCl6, Li3YCl6, Li1.48Al0.48Ge1.52(PO4)3 and LiPS5Cl

Abstract

Inorganic solid-state battery electrolytes show high ionic conductivities and enable the fabrication of all solid-state batteries. In this work, we present the temperature dependence of spin-lattice relaxation time (T1), spin-spin relaxation time (T2), and resonance linewidth of the 7Li nuclear magnetic resonance (NMR) for four solid-state battery electrolytes (Li3InCl6 (LIC), Li3YCl6 (LYC), Li1.48Al0.48Ge1.52(PO4)3 (LAGP) and LiPS5Cl (LPSC)) from 173 K to 403 K at a 7Li resonance frequency of 233 MHz, and from 253 K to 353 K at a 7Li resonance frequency of 291 MHz. Additionally, we measured the spin-lattice relaxation rates at an effective 7Li resonance frequency of 133 kHz using a spin-locking pulse sequence in the temperature range of 253 K to 353 K. In LPSC, the 7Li NMR relaxation is consistent with the Bloembergen-Pound-Purcell (BPP) theory of NMR relaxation of dipolar nuclei. In LIC, LYC and LAGP, the BPP theory does not describe the NMR relaxation rates for the temperature range and frequencies of our measurements. The presented NMR relaxation data assists in providing a complete picture of Li diffusion in the four solid-state battery electrolytes.

Introduction

Solid-state battery electrolytes overcome the traditional safety concerns of leakage and unimpeded dendrite growth in liquid state electrolytes and can be used with a lithium metal anode [1, 2]. The high capacity of lithium metal anodes[3], combined with stacking efficiency due to structural integrity of the solid-state electrolytes[4] means that high volumetric and specific energy densities can be achieved in solid-state batteries. Inorganic solid-state electrolytes show significantly higher ionic conductivities compared to solid polymer electrolytes[3], and therefore make all solid-state batteries with inorganic solid electrolytes a promising next-generation technology for energy storage.

NMR spectroscopy of solid-state battery electrolytes have been used to measure the diffusion constant and its temperature dependence[2, 5, 6]. The diffusion constant is intrinsically linked to the ionic conductivity of the solid-state electrolyte through the Nernst-Einstein equation[2, 6]. Puled field gradient (PFG) NMR allows for direct measurement of the Li diffusion constant[6, 7, 8]. However, due to small values of the diffusion constant and the short Li spin-spin relaxation time, measurements of the Li diffusion in solid-state electrolytes typically requires specialized PFG probes with gradient strength >10> 10 T/m[7, 8]. Alternatively, the Bloembergen-Bloom-Purcell (BPP) model[9] for the dipolar interaction between two Li nuclei is used to relate the NMR relaxation rates with the correlation time of interaction between two lithium ions. The correlation time is then used to estimate Li diffusion constant through the Einstein-Smoluchowski equation[2, 5, 6].

In this work, we measure the spin-lattice relaxation time (T1T_1), spin-spin relaxation rate (T2T_2), resonance linewidth (Δν\Delta\nu) and the consequent coherence time of the resonance (T2∗=1ΔνT_2^* = \frac{1}{\Delta\nu}) of Li3InCl6\mathrm{Li_3InCl_6} (lithium indium chloride or LIC), Li3YCl6\mathrm{Li_3YCl_6} (lithium yttrium chloride or LYC), Li1.48Al0.48Ge1.52(PO4)3\mathrm{Li_{1.48}Al_{0.48}Ge_{1.52}(PO_4)_3} (lithium aluminum germanium phosphate or LAGP) and LiPS5Cl\mathrm{LiPS_5Cl} (lithium phosphoroussulphur chloride or LPSC) as a function of temperature at 233 MHz and 291 MHz. Additionally, using spin-locking sequence[10] at 17.1T, we also measure the spin-spin relaxation time at an effective rotational frame of reference frequency of 133 kHz. The data presented here shows that while the BPP model for dipolar interaction of two nuclei is applicable for LiP5SCl\mathrm{LiP}_{5}\mathrm{SCl} at the 7Li{}^{7}\mathrm{Li} nuclear resonance frequencies and temperature of our study, the BPP model does not describe the 7Li{}^{7}\mathrm{Li} NMR relaxation in Li3InCl6\mathrm{Li}_{3}\mathrm{InCl}_{6}, Li3YCl6\mathrm{Li}_{3}\mathrm{YCl}_{6} and Li1.48Al0.48Ge1.52(PO4)3\mathrm{Li}_{1.48}\mathrm{Al}_{0.48}\mathrm{Ge}_{1.52}(\mathrm{PO}_{4})_{3}.

Experimental Details

Material Synthesis

Li3YCl6\mathrm{Li}_{3}\mathrm{YCl}_{6} and Li3InCl6\mathrm{Li}_{3}\mathrm{InCl}_{6} solid electrolytes (SEs) were synthesized via intermittent high energy ball milling as previously reported[11, 12]. In summary, LiCl\mathrm{LiCl} (Sigma-Aldrich) and YCl3\mathrm{YCl}_{3} (Alfa Aesar), or LiCl\mathrm{LiCl} and InCl3\mathrm{InCl}_{3} (Alfa Aesar) were hand mixed using a mortar with a 3:1 stoichiometry. The mixture was then milled intermittently for 3 hours. In the case of Li3YCl6\mathrm{Li}_{3}\mathrm{YCl}_{6}, a 10% molar excess of YCl3\mathrm{YCl}_{3} was added to account for loss of material due to strong adhesion to the milling reactor. Material manipulation and synthesis was carried out in an Ar glovebox (O2\mathrm{O}_{2} and H2O\mathrm{H}_{2}\mathrm{O}, <0.1 ppm). Li6PS5Cl\mathrm{Li}_{6}\mathrm{PS}_{5}\mathrm{Cl} (NEI Corporation) and Li1.48Al0.48Ge1.52(PO4)3\mathrm{Li}_{1.48}\mathrm{Al}_{0.48}\mathrm{Ge}_{1.52}(\mathrm{PO}_{4})_{3} (MSE Supplies) were purchased as powders. The vendor specified average particle of Li6PS5Cl\mathrm{Li}_{6}\mathrm{PS}_{5}\mathrm{Cl} and Li1.48Al0.48Ge1.52(PO4)3\mathrm{Li}_{1.48}\mathrm{Al}_{0.48}\mathrm{Ge}_{1.52}(\mathrm{PO}_{4})_{3} were 1 μm\mu\mathrm{m} and 500 nm respectively.

Materials Characterization

The X-ray diffraction (XRD) patterns of the solid-state electrolytes were collected using a Bruker D8 Advance Plus instrument at the Materials Research Lab at the University of Illinois. The XRD experiment was carried out in powder mode (Cu Kα\alpha, λ\lambda=1.5418 Å) from 10° to 80° in 2θ2\theta. To protect the air and moisture sensitive electrolytes, a custom holder and a Kapton film (Chemplex) were used.

The ionic conductivity of the solid-state electrolytes (SEs) was measured via electrochemical impedance spectroscopy (EIS). The SEs were first pelletized by weighing approximately 100 mg of SE, then pressed to ~360 MPa between two Ti rods. The Ti rods also served as blocking electrodes. In the case of LAGP, it was first pelletized to ~360 MPa, then sintered at 700°C for 12 hours in air since LAGP is air stable[12]. Then, to ensure good electrical contact, the sintered LAGP pellet coated with 100 nm Au on both sides via thermal evaporation using a Kurt J. Lesker Nano36 thermal evaporator. The EIS measurements were recorded in the frequency range from 1 MHz to 100 mHz with a 10 mV ac amplitude using a Bio-Logic VMP3 impedance analyzer.

Energy dispersive X-ray fluorescence (EDXRF) measurements were performed using a Shimadzu EDXRF 7000 instrument to ensure the stoichiometry of In and Cl in LiInCl6_6, Y and Cl in LiYCl6_6, P and Cl and P and S in LiPS5_5Cl, and Al and P in Li1.48_{1.48}Al0.48_{0.48}Ge1.52_{1.52}(PO4_4)3_3 were as expected. The EDXRF measurements were carried out using x-rays generated by a Rh anode with acceleration voltage of 50 kV. The measured stoichiometries were determined from calibration curve method using standard samples (InCl3_3, YCl3_3, PCl5_5, PS5_5 and Al(PO4_4)3_3) using K-α x-ray emissions for Cl, P, S and Al; and L-α x-ray emissions for In and Y. The experimental uncertainty determined from repeated measurements on the standard sample was approximately 1% for each element.

NMR measurements were performed at 233 MHz in a 14.1 T Unity Inova NMR spectrometer over a temperature range of 173 K to 403 K. We used a 5 mm Varian broadband probe in the temperature range 213 K to 373 K, and a 10 mm probe for measurements below 213 K and above 373 K. We used a 17.1 T Agilent VNMRS system with a 4mm Varian solid-state probe for measurements at 291 MHz. Additionally, rotational frame of reference measurement with spin-locking sequence was performed in VNMRS system with effective resonance frequency of 133 kHz.

We calibrated the temperature of the NMR probes using the relative chemical shifts between two proton peaks of ethylene glycol for temperatures above 308 K and methanol below 308 K[13].

Spin-Lattice relaxation times (T1T_1) were measured using the inversion recovery sequence[14], spin-spin relaxation times (T2T_2) were measured using the Carr-Purcell-Meiboom-Gill (CPMG) sequence[15] and the resonance linewidths were obtained by Fourier transforming the free induction decay (FID) of the resonance. T1,δT_{1,\delta} measurements at 17.1 T were performed using a spin-locking sequence[10].

All NMR data were processed in Mnova with single exponential fits for the determination of T1T_1, T2T_2 and T1,δT_{1,\delta} values.

Results

X-ray diffraction (XRD) data verify that the correct phases were obtained in all four solid-state electrolytes, see Figure 1. XRD showed that Li3InCl6\mathrm{Li}_{3}\mathrm{InCl}_{6} crystalized in the monoclinic phase, with the C2/mC2/m space group[16].

Figure 1. Powder x-ray diffraction of (a) Li3InCl6\mathrm{Li_3InCl_6}, (b) Li3YCl6\mathrm{Li_3YCl_6}, (c) Li1.48Al0.48Ge1.52(PO4)3\mathrm{Li_{1.48}Al_{0.48}Ge_{1.52}(PO_4)_3} and (d) Li6PS5Cl\mathrm{Li_6PS_5Cl}. The powder x-ray diffraction intensities collected in θ\theta-2θ2\theta geometry using Cu Kα\alpha x-rays is displayed in black and the simulated spectra for corresponding space groups is displayed in red. The diffuse scattering background, prominent for lower scattering angles, is from Kapton layer used to prevent exposure of the electrolytes to air.

The XRD pattern for Li3YCl6\mathrm{Li}_{3}\mathrm{YCl}_{6} shows a crystalline phase indexed to the trigonal structure with the P3‾m1P\overline{3}m1 space group, in agreement with previous reports[4, 12, 17]. XRD also confirmed Li6PS5Cl\mathrm{Li}_{6}\mathrm{PS}_{5}\mathrm{Cl} has an argyrodite-type structure (space group F4‾3mF\overline{4}3m)[18] and Li1.48Al0.48Ge1.52(PO4)3\mathrm{Li}_{1.48}\mathrm{Al}_{0.48}\mathrm{Ge}_{1.52}(\mathrm{PO}_{4})_{3} crystallizes in the R3‾cR\overline{3}c space group[19].

EXDRF measurements showed a In:Cl ratio of 1:6.1 in Li3InCl6\mathrm{Li}_{3}\mathrm{InCl}_{6}, a Al:P ratio of 1:6.2 in Li1.48Al0.48Ge1.52(PO4)3\mathrm{Li}_{1.48}\mathrm{Al}_{0.48}\mathrm{Ge}_{1.52}(\mathrm{PO}_{4})_{3}, and P:Cl and P:S ratios of 1:1 and 1:4.9 in Li6PS5Cl\mathrm{Li}_{6}\mathrm{PS}_{5}\mathrm{Cl}. In Li3YCl6\mathrm{Li}_{3}\mathrm{YCl}_{6}, a 1:5.7 ratio of Y:Cl was observed, consistent with the 10% additional YCl3\mathrm{YCl}_{3} added for stabilization.

The ionic conductivity was measured using electrochemical impedance spectroscopy (EIS). We derive the bulk ionic resistance (RbR_b) of the electrolytes from the Nyquist plots using a simple equivalent circuit [20, 21].

We calculate the the ionic conductivity using σ=tRbA\sigma= \frac{t}{R_b A} where tt is the thickness and AA is the area of the pelletized solid-state electrolyte. The corresponding Nyquist plots and ionic conductivities are shown in Figure 2. The measured conductivities of LIC, LYC, LPSC and LAGP agree with previous reports[4, 11, 16, 18, 22].

Figure 2. Electrochemical impedance spectroscopy (EIS) Nyquist plots for (a) LiInCl₆, (b) LiYCl₆, (c) Li₁.₄₈Al₀.₄₈Ge₁.₅₂(PO₄)₃ and (d) Li₆PS₅Cl taken between 1 MHz to 100 mHz. The behavior at higher frequencies are represented by the insets in the plots. The determined conductivities are 0.75 mS cm⁻¹, 0.66 mS cm⁻¹, 9×10−39 \times10^{-3} mS cm⁻¹ and 2.63 mS cm⁻¹ for LiInCl₆, LiYCl₆, Li₁.₄₈Al₀.₄₈Ge₁.₅₂(PO₄)₃ and Li₆PS₅Cl respectively.

In LAGP, the measured ionic conductivity increased after sintering, but still remained low, typical when the grain boundary resistance is high[22, 23]. Larger grain boundary resistance did not affect NMR measurements as the NMR results in LAGP did not change significantly before and after sintering.

The 7^{7}Li NMR relaxation times T1T_1, T2T_2 and the NMR linewidth at 291 MHz and 233 MHz as well as the relaxation rate T1,δT_{1,\delta} in the effective rotational frame of reference frequency of 133 kHz for LiInCl₆, LiYCl₆, Li₁.₄₈Al₀.₄₈Ge₁.₅₂(PO₄)₃ and Li₆PS₅Cl for different temperatures are displayed in Tables 1–4.

respectively. The relaxation rates 1/T11/T_1, 1/T21/T_2, 1/T2∗1/T_2^* and 1/T1,δ1/T_{1,\delta} are plotted as a function of temperatures for in Figure 3.

Figure 3. NMR relaxation rates for different values of 1000/T1000/T(K) for (a) LiInCl6_6 (LIC), (b) LiYCl6_6 (LYC), (c) Li1.48_{1.48}Al0.48_{0.48}Ge1.52_{1.52}(PO4_4)3_3 (LAGP) and (d) Li6_6PS5_5Cl (LPSC). The data at 233 MHz are plotted as open symbols and at 291 MHz are plotted as filled symbols. The spin-lattice relaxation rate (1/T11/T_1) are represented by circles, spin-spin relaxation rate (1/T21/T_2) are represented by triangles and the rate of FID relaxation (1/T2∗=2π(Δν)1/T_2^* = 2\pi(\Delta\nu)) are represented by hexagons. The spin-lattice relaxation rate at the effective rotational frame of reference frequency of 133 kHz is represented by open diamonds. In (d) the rates determined by Schlenkar et al.[2] of spin-lattice relaxation rates at 77.8 MHz (orange filled circles) and at an effective field of 37 kHz (orange open diamonds) are included for comparison.

T(K)Δν\Delta\nu (Hz)T1T_1 (s)T2T_2 (ms)T1,δT_{1,\delta} (ms), feff=133f_{eff}=133 kHz
3539670.502.995.49
34310220.502.294.37
32311200.552.042.77
31311780.551.332.40
30311240.541.202.10
29314410.571.131.75
27314810.810.881.48
25315580.970.721.49

Table 1. NMR spin-lattice relaxation time (T1T_1), spin-spin relaxation time (T2T_2), NMR linewidth (Δν\Delta\nu) at 291 MHz and 233 MHz and the rotational frame of reference spin-lattice relaxation time T1,δT_{1,\delta} at an effective frequency of 133 kHz for Li3_3InCl6_6.

T(K)Δν\Delta\nu (Hz)T1T_1 (s)T2T_2 (ms)
3739100.324.33
3539350.352.55
3339920.321.71
31310720.330.91
29811580.260.70
27312810.320.51
25314120.330.48
23315950.260.38
21319720.460.25
17339371.440.38

Table 5.

291 MHz
T(K)T(\mathrm{K})Δν\Delta\nu (Hz)T1T_{1} (s)T2T_{2} (ms)T1,δT_{1,\delta} (ms), feff=133f_{\mathrm{eff}} = 133 kHz
35316810.0430.290.41
34319750.0500.250.32
33325020.0610.220.25
32329830.0720.180.20
31335770.0860.150.17
30341000.110.150.16
29347220.120.120.17
27356220.170.120.19
25363570.230.110.29
233 MHz
T(K)T(\mathrm{K})Δν\Delta\nu (Hz)T1T_{1} (s)T2T_{2} (ms)
4034090.0150.65
3736370.0190.30
35313520.036
33317760.036
29831010.086
27832810.082
27333760.12
25336950.14
23341520.19
21354230.22
19363750.36
17376780.86

Table 2. NMR spin-lattice relaxation time (T1T_{1}), spin-spin relaxation time (T2T_{2}), NMR linewidth (Δν\Delta\nu) at 291 MHz and 233 MHz and the rotational frame of reference spin-lattice relaxation time T1,δT_{1,\delta} at an effective frequency of 133 kHz for Li3YCl6\mathrm{Li}_{3}\mathrm{YCl}_{6}.

Table 3. NMR spin-lattice relaxation time (T1T_1), spin-spin relaxation time (T2T_2), NMR linewidth (Δν\Delta\nu) at 291 MHz and 233 MHz and the rotational frame of reference spin-lattice relaxation time T1,δT_{1,\delta} at an effective frequency of 133 kHz for Li1.48Al0.48Ge1.52(PO4)3\mathrm{Li}_{1.48}\mathrm{Al}_{0.48}\mathrm{Ge}_{1.52}(\mathrm{PO}_4)_3.

291 MHz

TT (K)Δν\Delta\nu (Hz)T1T_1 (s)T2T_2 (ms)T1,δT_{1,\delta} (ms), feff=133f_{\mathrm{eff}} = 133 kHz
33316650.274.48.50
32316710.293.887.02
30317820.431.774.11
29316640.601.663.10
27317011.000.903.02
25316751.290.551.42

233 MHz

TT (K)Δν\Delta\nu (Hz)T1T_1 (s)T2T_2 (ms)
37311260.227.59
33313350.362.15
31312100.432.08
29813230.571.32
27314090.791.09
23315081.300.24
19320141.440.21
17324841.870.32

Table 3.

Table 4. NMR spin-lattice relaxation time (T1T_{1}), spin-spin relaxation time (T2T_{2}), NMR linewidth (Δν\Delta\nu) at 291 MHz and 233 MHz and the rotational frame of reference spin-lattice relaxation time T1,δT_{1,\delta} at an effective frequency of 133 kHz for Li6PS5Cl\mathrm{Li}_{6}\mathrm{PS}_{5}\mathrm{Cl}.

291 MHz
T(K)Δν\Delta\nu (Hz)T1T_{1} (s)T2T_{2} (ms)T1,δT_{1,\delta} (ms), fefff_{\mathrm{eff}} = 133 kHz
2936510.4210.3811.15
3036600.3514.7216.69
233 MHz
T(K)Δν\Delta\nu (Hz)T1T_{1} (s)T2T_{2} (ms)
4035890.3945.17
3835810.2941.29
3635820.2437.46
3435880.2228.79
3236020.2323.13
3136000.2419.71
3036010.2715.17
2986040.2812.66
2935850.309.97
2886120.366.99
2736700.463.66
2537270.621.33
2337511.010.64
2138141.180.38
19311421.660.36
17321312.450.37

In the BPP model of dipolar interaction between two nuclei, the rate of spin-lattice relaxation is given by[2, 6, 9]

1T1=Cτc1+(ωτc)1+β\frac{1}{T_1}=\frac{C\tau_c}{1+(\omega\tau_c)^{1+\beta}}

where CC is a constant of dipolar interaction, τc\tau_c is the correlation time of the dipolar interaction, and ω\omega is the resonance frequency. The spin-spin relaxation time is given by[5]:

1T2=C[32τc+52τc1+ω2τc2+τc1+4ω2τc2]\frac{1}{T_2}=C\left[\frac{3}{2}\tau_c+\frac{5}{2}\frac{\tau_c}{1+\omega^2\tau_c^2}+\frac{\tau_c}{1+4\omega^2\tau_c^2}\right]

Therefore, according to BPP theory, the rate of spin-lattice relaxation reaches a maximum when the rate of atomic scale hopping, i.e., the inverse of the correlation time of Li-Li interaction, is equal to the resonance frequency ω\omega. In LPSC, we observe a spin-lattice relaxation around 343 K at 233 MHz, indicating, according to BPP theory, the rate of atomic scale hopping is comparable to 2π(233×106)2\pi(233 \times10^6)/s at 343 K. In all other electrolytes, we do not observe a maximum in the T1T_1 relaxation in the temperature range of investigation at 233 MHz or 291 MHz.

The T1,δT_{1,\delta} measurements at 133 kHz were carried out to understand the field dependence of T1T_1 relaxation, since the difference between 233 MHz and 291 MHz was not significant. However, in the range of temperatures available on the VNS 750 solid-state probe, T1,δT_{1,\delta} is T2T_2-limited, and therefore, we cannot make conclusions on the field dependence on T1T_1 based on our rotational frame of reference T1,δT_{1,\delta} measurements.

In LIC, LYC and LAGP the spin-spin relaxation times do not seem to have a field dependence, consistent with the BPP theory when 1τc≪ω\frac{1}{\tau_c}\ll\omega. For the limited data we have obtained for LPSC at 291 MHz at 293 K and 303 K, the T2T_2 values are similar to the values at 233 MHz for the same temperatures. The data obtained in LPSC at 233 MHz above 343 K shows the temperature dependence of T2T_2 decreases compared to the temperature dependence below 343 K. This is consistent with the BPP theory where there are additional terms contributing to the T2T_2 relaxation when the rate of atomic scale hopping is comparable to the resonance frequency of the experiment.

In all the battery electrolytes, the temperature dependence of T2T_2 is stronger than the temperature dependence of T1T_1 for most of the temperature range in the measurement. This would indicate in the BPP model a value of β\beta: 0<β<10 < \beta< 1. In the BPP model, the expected field dependence of the spin-lattice relaxation rate when the relaxation rate is much smaller than the resonance frequency ω\omega is 1T1∝1ωβ+1\frac{1}{T_1} \propto\frac{1}{\omega^{\beta+1}}.

In LPSC, Schlenkar et.al[2] found β=0.52\beta= 0.52. Our observations at 233 MHz and 291 MHz and comparison to the data by Schelnkar et.al at are consistent with the field dependence of ∼1ω1.52\sim\frac{1}{\omega^{1.52}} for T1T_1 relaxation. The consequent hopping rates are also consistent with the results from ionic conductivity measurements[2].

In LIC and LYC, the field dependence of the spin-lattice relaxation rate is even larger than 1ω2\frac{1}{\omega^2} while for LAGP there does not seem to be a field dependence.

Therefore, in the temperature and fields investigated, the BPP model for dipolar interaction between two nuclei consistently explains the NMR relaxation rates in LPSC and does not explain the NMR relaxations in LIC, LYC and LAGP.

Conclusions

Temperature dependence of NMR relaxation rates in LiInCl6\mathrm{LiInCl_6}, LiYCl6\mathrm{LiYCl_6}, Li1.48Al0.48Ge1.52(PO4)3\mathrm{Li_{1.48}Al_{0.48}Ge_{1.52}(PO_4)_3} and Li6PS5Cl\mathrm{Li_6PS_5Cl} were studied from 173 K to 403 K at 7Li^7\mathrm{Li} resonance frequency of 233 MHz and from 253 K to 353 K at 7Li^7\mathrm{Li} resonance frequency of 291 MHz and an effective frequency of 133 KHz. The electrolytes were characterized by XRD, EIS and EDXRF to ensure expected crystallinity, ionic conductivity and stoichiometry. In the temperature range and frequencies studied, the relaxation rates in Li6PS5Cl\mathrm{Li_6PS_5Cl} seem to be consistent with the Bloembergen-Pound-Purcell (BPP) theory for dipolar interaction of two Li nuclei while in LiInCl6\mathrm{LiInCl_6}, LiYCl6\mathrm{LiYCl_6} and Li1.48Al0.48Ge1.52(PO4)3\mathrm{Li_{1.48}Al_{0.48}Ge_{1.52}(PO_4)_3} BPP theory is insufficient to explain the rates of NMR relaxation.

Acknowledgements

The authors thank Dr. Lingyang Zhu and Dr. Andre Sutrisno of the School of Chemical Science, University of Illinois at Urbana-Champaign for assistance with the NMR measurements. Part of the research was carried out at the Materials Research Laboratory at the University of Illinois. This research was partly supported by US Army CERL W9132T-19-2-0008 and Semiconductor Research Corporation (Task ID: 3044.001).

References

  1. [1]Marbella, L. E.; Zekoll, S.; Kasemchainan, J.; Emge, S. P.; Bruce, P. G.; Grey, C. P. 7 Li NMR Chemical Shift Imaging to Detect Microstructural Growth of Lithium in All-Solid-State Batteries. Chem. Mater. 2019, 31 (8), 2762–2769. https://doi.org/10.1021/acs.chemmater.8b04875.
  2. [2]Schlenker, R.; Hansen, A. L.; Senyshyn, A.; Zinkevich, T.; Knapp, M.; Hupfer, T.; Ehrenberg, H.; Indris, S. Structure and Diffusion Pathways in Li6PS5Cl Argyroditе from Neutron Diffraction, Pair-Distribution Function Analysis, and NMR. Chem. Mater. 2020, 32 (19), 8420–8430. https://doi.org/10.1021/acs.chemmater.0c02418.
  3. [3]Kim, D.; Liu, X.; Yu, B.; Mateti, S.; O’Dell, L.; Rong, Q.; Chen, Y. Amine-Functionalized Boron Nitride Nanosheets: A New Functional Additive for Robust, Flexible Ion Gel Electrolyte with High Lithium-Ion Transference Number. Adv. Funct. Mater. 2020, 30, 1910813–1910822.DOI
  4. [4]Asano, T.; Sakai, A.; Ouchi, S.; Sakaida, M.; Miyazaki, A.; Hasegawa, S. Solid Halide Electrolytes with High Lithium-Ion Conductivity for Application in 4 V Class Bulk-Type All-Solid-State Batteries. Adv. Mater. 2018, 30 (44), 1–7. https://doi.org/10.1002/adma.201803075.
  5. [5]Wagemaker, M.; Van de Krol, R.; Kentgens, A. P. M.; Van Well, A. A.; Mulder, F. M. Two Phase Morphology Limits Lithium Diffusion in TiO2 (Anatase): A 7Li MAS NMR Study. J. Am. Chem. Soc. 2001, 123 (46), 11454–11461. https://doi.org/10.1021/ja0161148.
  6. [6]Buschmann, H.; Dölle, J.; Berendts, S.; Kuhn, A.; Bottke, P.; Wilkening, M.; Heitjans, P.; Senyshyn, A.; Ehrenberg, H.; Lotnyk, A.; Duppel, V.; Kienle, L.; Janek, J. Structure and Dynamics of the Fast Lithium Ion Conductor “Li 7La3Zr2O12.” Phys. Chem. Chem. Phys. 2011, 13 (43), 19378–19392. https://doi.org/10.1039/c1cp22108f.
  7. [7]Hayamizu, K.; Seki, S.; Haishi, T. Lithium Ion Micrometer Diffusion in a Garnet-Type Cubic Li7La3Zr2O12 (LLZO) Studied Using 7Li NMR Spectroscopy. J. Chem. Phys. 2017, 146 (2). https://doi.org/10.1063/1.4973827.
  8. [8]Hayamizu, K.; Terada, Y.; Kataoka, K.; Akimoto, J. Toward Understanding the Anomalous Li Diffusion in Inorganic Solid Electrolytes by Studying a Single-Crystal Garnet of LLZO-Ta by Pulsed-Gradient Spin-Echo Nuclear Magnetic Resonance Spectroscopy. J. Chem. Phys. 2019, 150 (19). https://doi.org/10.1063/1.5089576.
  9. [9]Bloembergen, N.; Purcell, E. M.; Pound, R. V. Relaxation Effects in Nuclear Magnetic Resonance Absorption. Phys. Rev. 1948, 73 (7), 679–712. https://doi.org/10.1103/PhysRev.73.679.
  10. [10]Petkova, A. T.; Tycko, R. Sensitivity Enhancement in Structural Measurements by Solid State NMR through Pulsed Spin Locking. J. Magn. Reson. 2002, 155 (2), 293–299. https://doi.org/10.1006/jmre.2002.2519.
  11. [11]Zahiri, B.; Patra, A.; Kiggins, C.; Yong, A. X. Bin; Ertekin, E.; Cook, J. B.; Braun, P. V. Revealing the Role of the Cathode–Electrolyte Interface on Solid-State Batteries. Nat. Mater. 2021, 20 (10), 1392–1400. https://doi.org/10.1038/s41563-021-01016-0.
  12. [12]Cheng, Z.; Zahiri, B.; Ji, X.; Chen, C.; Chalise, D.; Braun, P. V.; Cahill, D. G. Good Solid-State Electrolytes Have Low, Glass-Like Thermal Conductivity. Small 2021, 17 (28). https://doi.org/10.1002/smll.202101693.
  13. [13]Raiford, D. S.; Fisk, C. L.; Becker, E. D. Calibration of Methanol and Ethylene Glycol Nuclear Magnetic Resonance Thermometers Determination of Cobalt by Lophine Chemiluminescence. Anal. Chem. 1979, 51 (12), 2050–2051.
  14. [14]Bydder, G. M.; Hajnal, J. V.; Young, I. R. MRI: Use of the Inversion Recovery Pulse Sequence. Clin. Radiol. 1998, 53 (3), 159–176. https://doi.org/10.1016/S0009-9260(98)80096-2.
  15. [15]Carr, H. Y.; Purcell, E. M. Effects of Diffusion on Free Precession in Nuclear Magnetic Resonance Experiments. Phys. Rev. 1954, 94 (3), 630–638. https://doi.org/10.1103/PhysRev.94.630.
  16. [16]Li, X.; Liang, J.; Luo, J.; Norouzi Banis, M.; Wang, C.; Li, W.; Deng, S.; Yu, C.; Zhao, F.; Hu, Y.; Sham, T. K.; Zhang, L.; Zhao, S.; Lu, S.; Huang, H.; Li, R.; Adair, K. R.; Sun, X. Air-Stable Li3InCl6 Electrolyte with High Voltage Compatibility for All-Solid-State Batteries. Energy Environ. Sci. 2019, 12 (9), 2665–2671. https://doi.org/10.1039/c9ee02311a.
  17. [17]Schlem, R.; Banik, A.; Ohno, S.; Suard, E.; Zeier, W. G. Insights into the Lithium Sub-Structure of Superionic Conductors Li3YCl6and Li3YBr6. Chem. Mater. 2021, 33 (1), 327–337. https://doi.org/10.1021/acs.chemmater.0c04352.
  18. [18]Kraft, M. A.; Culver, S. P.; Calderon, M.; Böcher, F.; Krauskopf, T.; Senyshyn, A.; Dietrich, C.; Zevalkink, A.; Janek, J.; Zeier, W. G. Influence of Lattice Polarizability on the Ionic Conductivity in the Lithium Superionic Argyrodites Li6PS5X (X = Cl, Br, I). J. Am. Chem. Soc. 2017, 139 (31), 10909–10918. https://doi.org/10.1021/jacs.7b06327.
  19. [19]Weiss, M.; Weber, D. A.; Senyshyn, A.; Janek, J.; Zeier, W. G. Correlating Transport and Structural Properties in Li1+ XAlxGe2- x(PO4)3 (LAGP) Prepared from Aqueous Solution. ACS Appl. Mater. Interfaces 2018, 10 (13), 10935–10944. https://doi.org/10.1021/acsami.8b00842.
  20. [20]Uddin, M. J.; Cho, S. J. Reassessing the Bulk Ionic Conductivity of Solid-State Electrolytes. Sustain. Energy Fuels 2018, 2 (7), 1458–1462. https://doi.org/10.1039/c8se00139a.
  21. [21]van den Broek, J.; Afyon, S.; Rupp, J. L. M. Interface-Engineered All-Solid-State Li-Ion Batteries Based on Garnet-Type Fast Li+ Conductors. Adv. Energy Mater. 2016, 6 (19), 1–11. https://doi.org/10.1002/aenm.201600736.
  22. [22]Kotobuki, M.; Hanc, E.; Yan, B.; Molenda, J.; Lu, L. Preparation and Characterization of Ba-Substituted Li1+xAlxGe2−x(PO4)3 (x = 0.5) Solid Electrolyte. Ceram. Int. 2017, 43 (15), 12616–12622. https://doi.org/10.1016/j.ceramint.2017.06.140.
  23. [23]Ling, S. G.; Peng, J. Y.; Yang, Q.; Qiu, J. L.; Lu, J. Z.; Li, H. Enhanced Ionic Conductivity in LAGP/LATP Composite Electrolyte. Chinese Phys. B 2018, 27 (3). https://doi.org/10.1088/1674-1056/27/3/038201.

Paper details

vlnc:W_tzu36reu
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents