betaFeedback

WorksPhysics and Astronomy

Optically Resolved Exchange Splittings in the Doped Van der Waals Ferromagnet CrBr3:Yb3+

Abstract

The chromium-trihalides (CrX3; X = Cl, Br, I) have long served as model systems for understanding magnetism and magneto-optics in ionic crystals, and they have recently also emerged as archetypes of magnetic two-dimensional (2D) Van der Waals materials. Although the physical properties of CrX3 compounds have now been explored in great depth, the use of impurity doping to generate new properties remains surprisingly underexplored. Here we report on the magnetic and magneto-optical properties of lanthanide-doped CrBr3, in which Yb3+ is introduced as a spin-bearing optical point defect. Narrow-line near-infrared dopant photoluminescence is efficiently sensitized by CrBr3-to-Yb3+ energy transfer. Magneto-optical measurements show facile spin manipulation of the paramagnetic Yb3+ impurities by the surrounding CrBr3 lattice. Photoluminescence data reveal that the Kramers spin degeneracies of the ground- and excited-state Yb3+ doublets are spontaneously lifted by strong magnetic exchange with neighboring Cr3+ ions, such that individual Yb3+ spin transitions are easily resolved even at zero external magnetic field. The temperature and field dependence of these splittings can be used to probe both local and long-range spin correlations. These results highlight the use of extrinsic optical impurities to add new spin-photonic functionality to this classic 2D Van der Waals magnet.

Introduction

The intriguing optical and magneto-optical properties of the layered chromium-trihalide (CrX3\mathrm{CrX}_3; X=Cl,Br,IX = \mathrm{Cl}, \mathrm{Br}, \mathrm{I}) magnetic insulators have been studied for several decades. As relatively simple ionic crystals, early studies of CrX3\mathrm{CrX}_3 compounds sought to unravel the fundamental origins of their large magnetic rotations of linearly polarized light[1] and the modification of excited energy levels by magnetic states, particularly exchange-related phenomena in the crystal-field transitions of Cr3+\mathrm{Cr}^{3+}.[2, 3, 4] The recent demonstration of ferromagnetism in monolayer CrI3\mathrm{CrI}_{3}[5] triggered a rapid resurgence in interest in the chromium trihalides (CrX3\mathrm{CrX}_{3}).[6, 7, 8] Since then, discoveries involving CrX3\mathrm{CrX}_{3} compounds have ranged from topological spin textures[9, 10, 11] to spin-filtering magnetic tunnel junctions constructed from stacked Van der Waals heterostructures.[12, 13] The broad, featureless dd-dd luminescence and poor spin coherence of CrX3\mathrm{CrX}_{3}[14, 15, 16, 17] do not lend themselves to applications in quantum or classical spin-photonic technologies, however, and they obscure any interplay between magnetic ordering and optical transition energies or electronic structure. Harnessing optical defects in crystals, whether intrinsic or extrinsic, offers a pathway for achieving unique and powerful new functionalities, as demonstrated by the examples of nitrogen-doped diamond, diluted magnetic semiconductors, and the ruby laser.[18, 19, 20] In magnetic 2D Van der Waals materials, recent reports have investigated the (magneto-)optical properties of vacancies in CrSBr\mathrm{CrSBr}[21, 22] but deliberate incorporation of optical impurities remains almost entirely unexplored.

Recently, our group reported on the magneto-optical properties of impurity-doped CrI3\mathrm{CrI}_{3}.[23] Paramagnetic Yb3+\mathrm{Yb}^{3+} ions added to this lattice are tightly coupled to the surrounding spins and their photoluminescence (PL) allows optical sensing of spontaneous or induced magnetization in bulk CrI3\mathrm{CrI}_{3}. The specifics of the Yb-Cr coupling remain unclear, however, because anomalously high Yb3+\mathrm{Yb}^{3+} ff-orbital covalency[17] in CrI3\mathrm{CrI}_{3}:Yb3+\mathrm{Yb}^{3+} broadens the ff-ff PL, impeding in-depth analysis of the underlying electronic structure.

Here, we report a detailed investigation of the PL of CrBr3\mathrm{CrBr}_{3} crystals doped with Yb3+\mathrm{Yb}^{3+}. Yb3+\mathrm{Yb}^{3+} ff-orbital covalency in this material is substantially smaller than in CrI3\mathrm{CrI}_{3}:Yb3+\mathrm{Yb}^{3+}.[17] As a consequence, the PL of CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+} is dramatically narrower and reveals extensive fine structure that has not been resolvable in CrI3\mathrm{CrI}_{3}:Yb3+\mathrm{Yb}^{3+}. Variable-temperature and variable-field measurements allow assignment of the fine structure to specific Yb3+\mathrm{Yb}^{3+} electronic transitions between states whose Kramers spin degeneracies are lifted via exchange coupling with the surrounding magnetic CrBr3\mathrm{CrBr}_{3} lattice. Analysis of these data allows the microscopic Yb3+\mathrm{Yb}^{3+}-Cr3+\mathrm{Cr}^{3+} exchange-coupling strength to be quantified and indicates an effective exchange field of ∼30\sim30 tesla experienced by Yb3+\mathrm{Yb}^{3+} in the low-temperature limit. The observation of well-resolved exchange-split impurity spin levels at zero magnetic field in CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+} may have interesting ramifications for optical spin preparation and readout, inverse Faraday effect, or other spin-photonic functionalities in this modified magnetic Van der Waals material.

Experimental

General considerations. All sample preparation and manipulation was done in a glovebox under an atmosphere of purified dinitrogen.

Synthesis of CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+} and YBr3:Yb3+\mathrm{YBr}_{3}:\mathrm{Yb}^{3+} single crystals. The synthesis of single crystals of CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+} grown through chemical vapor transport is detailed in Snoeren et al.[17] The synthesis of YBr3:Yb3+\mathrm{YBr}_{3}:\mathrm{Yb}^{3+} was carried out under similar conditions. YBr3\mathrm{YBr}_{3} (99.9%, ultra-dry, ThermoFisher Scientific) and Yb metal (99.9%, 40 mesh, BeanTown Chemical) were used as precursors. The precursors were mixed at the desired stoichiometry and sealed in an evacuated quartz ampoule. The ampoule was placed in a tube furnace with the precursors at the center. The sample was kept at 800°C for 4 days.

Photoluminescence (PL) measurements. A single crystal of the material was placed between two quartz disks and loaded into a closed-cycle helium cryostat. Measurements were performed under high vacuum (10−610^{-6} Pa). For CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+}, the sample was excited using a continuous-wave 405 nm (3.06 eV) diode. YBr3:Yb3+\mathrm{YBr}_{3}:\mathrm{Yb}^{3+} was excited using a continuous wave 340 nm (3.64 eV) diode. The diode output was focused down to a spot size of approximately 1 mm2^{2} at an excitation power of approximately 4 mW/cm2^{2}. Sample emission was focused into a monochromator with a spectral bandwidth of 0.25 nm for CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+} and a spectral bandwidth of 0.02 nm for YBr3:Yb3+\mathrm{YBr}_{3}:\mathrm{Yb}^{3+}. The 4 K CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+} PL spectrum shown in the Supplemental Material was collected with a spectral bandwidth of 0.002 nm. Spectra were collected using a LN2_{2}-cooled silicon CCD camera and were corrected for instrument response.

Photoluminescence excitation (PLE) measurements. PLE measurements were likewise carried out in a closed-cycle helium cryostat under high vacuum. The sample was excited using a broadband tungsten-halogen lamp. The excitation wavelength was selected using a monochromator with a spectral bandwidth of 2.15 nm. Excitation light was focused onto the sample with a spot size of approximately 1 mm2^{2}. Sample emission was focused onto a monochromator with a spectral bandwidth of 16 nm and emission counts were monitored using a Hamamatsu InGaAs/InP NIR photomultiplier tube. Spectra were corrected for lamp output.

Absorption measurements. Absorption measurements were carried out using a Cary 5000 UV-Vis Spectrophotometer in dual beam mode. Scan rates of 2 nm/s were used with a step size of 1 nm and a spectral bandwidth of 1 nm. Due to the air-sensitive nature of the material, special care was taken to avoid air exposure during the measurement: a single crystal of the material was placed between two quartz disks, spaced with a rubber o-ring to avoid distortion of the crystal while also excluding ambient atmosphere. The ensemble was held together by two metal plates with a circular aperture for light transmission. To ensure all light passed through the sample, a mask with a diameter of about 1 mm was placed on the exterior of one of the quartz disks.

Magnetic circularly polarized luminescence (MCPL) measurements. A single crystal was placed between two quartz disks and loaded into a Cryo-Industries SMC-1650 OVT superconducting magneto-optical cryostat oriented in the Faraday configuration. The magnetic field was applied parallel to the CrBr3\mathrm{CrBr}_{3} easy axis (crystallographic cc axis). The sample was excited with a 405 nm (3.06 eV) diode at approximately 4 mW/cm2^{2}. Sample emission was collected along the magnetic field axis and passed through a liquid-crystal variable retardation plate set at λ/4\lambda/4, followed by a linear polarizer to separate the left- and right-circularly polarized components, and then focused onto a fiber-optic cable. Sample emission was then passed through a monochromator with a spectral bandwidth of 0.25 nm and was collected using a LN2_{2}-cooled silicon CCD camera. Field-sweep measurements were performed by continuously monitoring the sample emission using a monochromator with a spectral bandwidth of 9.9 nm. Emission counts were monitored using a Hamamatsu InGaAs/InP NIR photomultiplier tube with an integration time of 0.1 s. The field was swept at a rate of 1.5 mT/s (0.09 T/min).

Polarization ratios are defined as ρ=(σ−−σ+)/(σ−+σ+)=(IL−IR)/(IL+IR)\rho= (\sigma^{-} - \sigma^{+})/(\sigma^{-} + \sigma^{+}) = (I_{L} - I_{R})/(I_{L} + I_{R}), following the sign conventions outlined in Piepho and Schatz.[24]

Results and analysis

Optical spectroscopy

Figure 1a shows the room-temperature absorption spectrum of a single-crystal flake of Yb3+\mathrm{Yb}^{3+}-doped CrBr3\mathrm{CrBr}_{3}. The absorption spectrum shows two main bands that are assigned to the spin-allowed 4 ⁣A2g→4 ⁣T2g{}^{4}\!A_{2g} \rightarrow{}^{4}\!T_{2g} and 4 ⁣T1g{}^{4}\!T_{1g} ligand-field transitions, two shoulders assigned to the spin-forbidden 4 ⁣A2g→2 ⁣T1g{}^{4}\!A_{2g} \rightarrow{}^{2}\!T_{1g} and 2 ⁣T2g{}^{2}\!T_{2g} ligand-field transitions, and a broad band at high energy assigned as a ligand-to-metal charge-transfer (LMCT) transition. All transitions are in good agreement with those previously reported for CrBr3\mathrm{CrBr}_{3}.[4] The weak, parity-forbidden Yb3+\mathrm{Yb}^{3+} ff-ff transitions are not observed due to the low Yb3+\mathrm{Yb}^{3+} doping concentration of ∼\sim0.4% relative to the total cation concentration. Figure 1a also shows the 5 K photoluminescence excitation (PLE) spectrum of CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+}, collected by monitoring the Yb3+\mathrm{Yb}^{3+} emission at 1043 nm (vide infra). The PLE spectrum shows the same features as the absorption spectrum, with narrower peaks due to the lower temperature, demonstrating efficient sensitization of Yb3+\mathrm{Yb}^{3+} PL by CrBr3\mathrm{CrBr}_{3}.

Figure 1b shows the sensitized Yb3+\mathrm{Yb}^{3+} PL spectrum measured at 5 K. The spectrum is characterized by very narrow linewidths – the highest energy peak has a full width at half maximum (FWHM) of ∼1.1 cm−1\sim1.1\ \mathrm{cm}^{-1} (0.14 meV, see Figure S1{sup}25). This is in contrast to the PL spectrum of $\mathrm{CrI}_{3}$:$\mathrm{Yb}^{3+}$, where the FWHM of the narrowest feature is about 30x larger, even at liquid helium temperatures.{citep}23 Aside from the assigned electronic origins, separate sets of peaks (indicated by dashed lines) are found at fixed energy spacings of $\sim 145\ \mathrm{cm}^{-1}$ from the origins. This spacing does not exactly match an $A_{1g}$ vibration in either $\mathrm{CrBr}_{3}${citep}26 or $\mathrm{YbBr}_{3}${citep}27; these peaks are assigned to coupling of the electronic transitions with local $[\mathrm{YbBr}_{6}]^{3-}$ cluster vibrations. The main $\mathrm{Yb}^{3+}$ transitions are schematically indicated in {xref}Figure 1c`, where the orbital degeneracies of the Γ8\Gamma_{8} spin-orbit states in both the 2F7/2{}^{2}F_{7/2} and 2F5/2{}^{2}F_{5/2} multiplets are lifted as a result of a small reduction in site symmetry from OhO_{h}.

Image not extracted

Figure 1. (a) 300 K absorption spectrum (red) of a CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+} (0.4%) single crystal. Several Cr3+ 4A2g→2S+1Γ\mathrm{Cr}^{3+}\,{}^{4}A_{2g} \rightarrow{}^{2S+1}\Gamma transitions are labeled. The same transitions are observed in the 5 K Yb3+\mathrm{Yb}^{3+} PLE spectrum (λem=1043\lambda_{\mathrm{em}} = 1043 nm, see panel (b)), indicating energy transfer between Cr3+\mathrm{Cr}^{3+} and Yb3+\mathrm{Yb}^{3+}. The shifts in PLE peak positions relative to the absorption measurement are due to the measurement temperature. (b) 5 K PL spectrum (λex=405\lambda_{\mathrm{ex}} = 405 nm) of CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+} (0.4%), showing sharp near-IR Yb3+\mathrm{Yb}^{3+} emission peaks. The electronic origins are labeled and vibronic features are indicated with dashed lines. (c) Schematic overview of the observed transitions in the Yb3+\mathrm{Yb}^{3+} PL spectrum. A slightly distorted octahedral crystal field splits the orbital degeneracies of the Γ8\Gamma_{8} levels.

Image not extracted

Figure S1. Zoom-in on the 0′→00^\prime\to0 transition in the 4 K PL spectrum of CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+} collected at a spectral bandwidth of 0.002 nm. A Lorentzian fit of peak A1_1 (red) gives a full width at half max (FWHM) of 1.1 cm−1\mathrm{cm}^{-1} (0.14 meV).

Magneto-optical properties

The top part of Figure 2a shows low-temperature magnetic circularly polarized luminescence (MCPL) spectra of CrBr3_3:Yb3+^{3+} (0.4%) measured for σ−\sigma^- and σ+\sigma^+ circular polarizations at an external magnetic field of 6.0 T. At this field, the lattice is fully magnetized and the polarization ratio, defined as ρ=(σ−−σ+)/(σ−+σ+)\rho= (\sigma^- - \sigma^+)/(\sigma^- + \sigma^+),[24] is maximized. The bottom half of Figure 2a plots the temperature dependence of ρ\rho for the full spectrum measured at 0.5 T. It is evident that ρ\rho decreases in magnitude as the temperature increases, and almost vanishes at temperatures above TCT_\mathrm{C}. Simultaneously, most peaks show a blueshift in the center of gravity, in part due to the appearance of hot bands.

Image not extracted

Figure 2. (a) Top: MCPL spectra of CrBr3_3:Yb3+^{3+} (0.4%) showing left- and right-circularly polarized emission, denoted σ−\sigma^- and σ+\sigma^+, respectively. Spectra were collected at Bext=6.0B_\mathrm{ext} = 6.0 T. Bottom: temperature dependence of the polarization ratio (ρ\rho) of the full Yb3+^{3+} PL spectrum collected at Bext=0.5B_\mathrm{ext} = 0.5 T, where ρ=(σ−−σ+)/(σ−+σ+)\rho= (\sigma^- - \sigma^+)/(\sigma^- + \sigma^+). (b) Polarization ratio of the highest-energy Yb3+^{3+} 0′→00' \rightarrow0 PL peak (A1_1, see section C) plotted as a function of temperature. The derivative of these data shows a minimum at 36 K, in close agreement with the reported CrBr3_3 Curie temperature of 37 K. (c) Normalized polarization ratio of the Yb3+^{3+} 0′→00' \rightarrow0 PL plotted as a function of external magnetic field, BextB_\mathrm{ext}. The saturation field of ∼\sim0.3 T agrees well with reported CrBr3_3 magnetic data.

Figure 2b plots the polarization ratio of the highest-energy transition (∼\sim10110 cm−1^{-1}) as a function of temperature, highlighting the rapid drop in ρ\rho as the temperature approaches the CrBr3_3 Curie temperature. Some polarization is observed above TCT_\mathrm{C}, up to a temperature of around 50 K. The inset shows the derivative of ρ\rho with respect to temperature, which has a minimum at 36 K, in good agreement with the reported CrBr3_3 Curie temperature of 37 K.[28]

fig:2c shows a magnetic field-sweep hysteresis loop obtained by monitoring the polarization ratio of the 10110 cm−1^{-1} Yb3+^{3+} emission as a function of external magnetic field. The saturation field of ∼\sim0.3 T agrees well with magnetization measurements of bulk CrBr3_3.[29, 30] As previously shown for CrI3_3:Yb3+^{3+}[23], this correlation of Yb3+^{3+} and Cr3+^{3+} magnetization indicates pinning of the Yb3+^{3+} spins to the magnetic host lattice under these conditions. Due to the similarity in magneto-optical properties of CrBr3_3:Yb3+^{3+} and CrI3_3:Yb3+^{3+}, we can make use of the highly resolved spectral data on CrBr3_3:Yb3+^{3+} to deepen our understanding of both materials.

Yb3+^{3+} exchange splitting

Figure 3a shows an enlarged view of the Yb3+^{3+} 0′→00' \to0 transition, plotting spectra in this region collected at various temperatures up to slightly above TCT_\mathrm{C}. Full spectra are shown in Figure S2 and Figure S3.[25] At 5 K, only peaks A1_1 and A2_2 are clearly visible, separated by 27 cm−1^{-1}. At 10 K, two new peaks (B1_1 and B2_2) appear, and these are also separated from one another by 27 cm−1^{-1}. The energy spacing between A1_1 and B1_1 is equal to the energy spacing between A2_2 and B2_2, 16 cm−1^{-1} at 5 K. At 15 K, A2_2 and B2_2 begin to shift to higher energies and the linewidths of all transitions increase. Above 25 K, another peak (C1_1) starts to grow at ∼\sim32 cm−1^{-1} above A1_1. Following the splitting patterns of the other peaks described above, a sixth peak (C2_2) may also be expected 27 cm−1^{-1} below C1_1, but this peak is not clearly observed and may be present only as a shoulder on A1_1. Above 30 K, all transitions become severely broadened and individual features are poorly resolved.

Image not extracted

Figure S2. Full assignment of the CrBr3_3:Yb3+^{3+} PL spectrum. At 5 K, only the lowest-energy excited state (0′0^{\prime}) is populated and only peaks labeled A are observed. As the temperature increases, B peaks arise from the higher-energy spin level of the exchange-split 0′0^{\prime} state. At even higher temperatures, C peaks appear, arising from the 1′1^{\prime} excited state. At a fixed energy spacing of ∼145 cm−1\sim145\ \mathrm{cm}^{-1} from the purely electronic transitions, vibronic transitions are observed. These peaks are labeled with a prime (′^{\prime}). Another set of vibronic peaks is possibly observed between the main and primed peaks. The 5 and 20 K spectra are plotted on a logarithmic y-axis in Figure S3 below.

Image not extracted

Figure S3. Full CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+} PL spectrum collected at 5 K (top) and 20 K (bottom), plotted on a logarithmic yy-axis to facilitate identification of weak peaks. Peaks are labeled according to the diagram shown in Figure S2.

Image not extracted

Figure 3.

Image not extracted

Figure 3 (PDF p. 8). (a) Variable-temperature PL spectra of CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+} measured in the region of the 0′→00' \to0 transition. Fine-structure peaks and relevant splitting energies are labeled. The peaks shift as the temperature is increased, and the fine structure largely becomes unresolved when TT approaches TCT_C. Colored bars indicate the energy spacings tracked in panel (d). (b) Enlarged view of the 0′→00' \to0 transition in CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+} (blue) and a reference sample involving a non-magnetic host lattice, YBr3\mathrm{YBr}_{3}:Yb3+\mathrm{Yb}^{3+} (red), measured at 5 K. The spectra are normalized and offset for comparison. The A2_2 peak, which results from exchange splitting of the ground state (0), is absent in YBr3\mathrm{YBr}_{3}:Yb3+\mathrm{Yb}^{3+}. (c) Energy diagram for Yb3+\mathrm{Yb}^{3+} showing the 5 K exchange splittings of ground- and excited-state Kramers doublets at zero field, based on the observations of panel (a). The corresponding PL transitions of panel (a) are indicated. The colors indicate if the transition is allowed (green) or forbidden (red), as judged from peak intensities. Individual Yb3+\mathrm{Yb}^{3+} spin states are indicated, as explained in section D. (d) Ground-state (0) and first-excited-state (0') exchange splittings (ΔEexch\Delta E_{\mathrm{exch}}) at zero field plotted as a function of temperature, as determined from the PL peak energies in panel (a). The decrease in ΔEexch\Delta E_{\mathrm{exch}} with increasing temperature is attributed to loss of lattice spin correlation at higher temperatures.

The rich fine structure in the CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+} PL spectrum can be explained by the presence of magnetic exchange splittings in both the ground and excited crystal-field states of Yb3+\mathrm{Yb}^{3+} at zero external field. To illustrate the magnetic character of these peaks, crystals of YBr3\mathrm{YBr}_{3}:Yb3+\mathrm{Yb}^{3+} were prepared and their 5 K PL was investigated. YBr3\mathrm{YBr}_{3} is isostructural to CrBr3\mathrm{CrBr}_{3} (space group R3̄h), but due to the full dd shell of Y3+\mathrm{Y}^{3+}, the lattice is diamagnetic. The two spectra show the same main features, with the YBr3\mathrm{YBr}_{3}:Yb3+\mathrm{Yb}^{3+} spectrum shifted to slightly higher energies and spaced closer together due to a reduced crystal field compared to CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+} (see Figure S5[25]). Both observations can be attributed to the longer metal-ligand bond lengths of YBr3\mathrm{YBr}_{3}:Yb3+\mathrm{Yb}^{3+}. Figure 3b compares the 5 K PL spectra of CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+} and YBr3\mathrm{YBr}_{3}:Yb3+\mathrm{Yb}^{3+} zoomed in at the first Yb3+\mathrm{Yb}^{3+} electronic origin (plotted as energy shift from the respective 0′→00' \to0 origin), highlighting the fact that the YBr3\mathrm{YBr}_{3}:Yb3+\mathrm{Yb}^{3+} spectrum shows no feature analogous to the A2_2 peak of CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+}. Similar differences are identified for each of the electronic origins when comparing the full spectra (Figure S5[25]), and higher-temperature spectra show the absence of hot bands analogous to the B peaks in YBr3\mathrm{YBr}_{3}:Yb3+\mathrm{Yb}^{3+} (Figure S6[25]). These results support the assertion that the rich structure described in Figure 3a arises from magnetic exchange. Notably, the low-temperature linewidth of CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+} in Figure 3b is essentially indistinguishable from that of Yb3+\mathrm{Yb}^{3+} in the non-magnetic YBr3\mathrm{YBr}_{3} lattice, consistent with minimal spin disorder in CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+} at 5 K. At higher temperatures, spin fluctuations cause the CrBr3\mathrm{CrBr}_{3}:Yb3+\mathrm{Yb}^{3+} linewidths to increase rapidly until TCT_C is reached, while the linewidths of the diamagnetic YBr3\mathrm{YBr}_{3}:Yb3+\mathrm{Yb}^{3+} increase only marginally over the same temperature range (Figure S6[25]). This result highlights the sensitivity of Yb3+\mathrm{Yb}^{3+} optical transitions to spin fluctuations in CrBr3\mathrm{CrBr}_{3}.

Image not extracted

Figure S5. 5 K PL spectra of CrBr3_3:Yb3+^{3+} (blue) and YBr3_3:Yb3+^{3+} (red). Several peaks associated with exchange splitting are indicated by filled circles for CrBr3_3:Yb3+^{3+}. Prime symbols (’) indicate vibronic features. The absence of the corresponding peaks in the non-magnetic YBr3_3:Yb3+^{3+} is indicated by empty circles. The CrBr3_3:Yb3+^{3+} spectrum is offset vertically for easier comparison.

Comparison of FWHM spectra and temperature dependence for CrBr3:Yb3+ and YBr3:Yb3+

Figure S6. Top: Comparison of the full width at half maximum (FWHM) of the highest-energy peak (A1\mathrm{A}_{1}) in both CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+} 0.4% (blue) and YBr3:Yb3+\mathrm{YBr}_{3}:\mathrm{Yb}^{3+} (red) at various temperatures. The CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+} FWHM increases more rapidly than that of YBr3:Yb3+\mathrm{YBr}_{3}:\mathrm{Yb}^{3+} due to spin fluctuations. Offset spectra of both are shown at select temperatures for visual comparison. Above ~30 K, the CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+} A1\mathrm{A}_{1} peak broadening is too large to quantify reliably. Bottom: FWHM of the lowest-energy peak (A7\mathrm{A}_{7}) in both CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+} 0.4% (blue) and YBr3:Yb3+\mathrm{YBr}_{3}:\mathrm{Yb}^{3+} (red) at various temperatures. A clear discontinuity is seen at TCT_{\mathrm{C}} in the CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+} FWHM that is attributed to magnetic ordering of the Cr3+\mathrm{Cr}^{3+} lattice. The reduction in Cr3+\mathrm{Cr}^{3+} nearest-neighbor spin fluctuations results in a sharpening of the Yb3+\mathrm{Yb}^{3+} peaks at lower temperatures. The absence of peaks B2\mathrm{B}_{2} (top) and B7\mathrm{B}_{7} (bottom) in the YBr3:Yb3+\mathrm{YBr}_{3}:\mathrm{Yb}^{3+} spectrum is further evidence that the CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+} spin states are split via exchange interactions (see Figure S2 for peak assignment). Note that unlike the A1\mathrm{A}_{1} peak, the exchange splitting of this A7\mathrm{A}_{7} peak in CrBr3:Yb3+\mathrm{CrBr}_{3}:\mathrm{Yb}^{3+} is not resolved and its temperature dependence is thus embedded in these linewidths.

Figure 3c summarizes the results of Figure 3a, assigning each peak to a specific transition between exchange-split Yb3+\mathrm{Yb}^{3+} levels. From this diagram, it is clear that the splitting between peaks A1\mathrm{A}_{1} and A2\mathrm{A}_{2} (or B1\mathrm{B}_{1} and B2\mathrm{B}_{2}) reveals the ground-state exchange splitting (ΔEexch\Delta E_{\mathrm{exch}}), whereas the splitting between peaks A1\mathrm{A}_{1} and B1\mathrm{B}_{1} (or A2\mathrm{A}_{2} and B2\mathrm{B}_{2}) corresponds to ΔEexch\Delta E_{\mathrm{exch}} of the 0′0' excited state. Figure 3d plots the ground-state (00) and first-excited-state (0′0') splittings (ΔEexch\Delta E_{\mathrm{exch}}) at zero external magnetic field as a function of temperature. For both states, ΔEexch\Delta E_{\mathrm{exch}} decreases with increasing temperature, consistent with a decrease in magnetization of the host lattice at higher temperatures. By 37 K, the splitting is unresolved and only a broad shoulder is observed. The spectrum at 50 K (above TCT_{\mathrm{C}}) is nearly indistinguishable from that at 37 K, indicating a discontinuity at TCT_{\mathrm{C}} and confirming the magnetic source of these splittings. For both the ground and excited states, ΔEexch\Delta E_{\mathrm{exch}} above TCT_{\mathrm{C}} is around half as large as at 4 K.

Yb3+^{3+} spin alignment in CrBr3_{3}

Figure 4a shows CrBr3_{3}:Yb3+^{3+} 0′→00' \rightarrow0 PL spectra collected at different external magnetic fields, measured at 18 K where B1\mathrm{B}_{1} and B2\mathrm{B}_{2} peaks are visible. Peaks B1\mathrm{B}_{1} and A2\mathrm{A}_{2} do not shift with field, whereas peaks A1\mathrm{A}_{1} and B2\mathrm{B}_{2} shift in opposite directions. The absence of a conventional Zeeman splitting of any of the individual peaks – which would amount to ∼1\sim1 cm−1^{-1}/T assuming a gg value of ∼2.0\sim2.0 – is consistent with the spin-degeneracy of the Yb3+^{3+} sublevels having already been lifted at zero external field. The remaining regions of the spectrum match this interpretation (see Figure S7[25]).

PL spectra, splitting energies, and energy diagrams for CrBr3:Yb3+

Figure 4. (a) Top: PL spectra of CrBr3_3:Yb3+^{3+} (0.4%) measured in the region of the 0′→00' \to0 transition at 18 K and at various external magnetic fields (Bext∥cB_{\mathrm{ext}} \parallel c). Colored bars indicate the energy spacings tracked in panel (b). Bottom: False-color plot of PL in the same region vs BextB_{\mathrm{ext}}. (b) Splittings of the Yb3+^{3+} Kramers doublets (ΔEexch\Delta E_{\mathrm{exch}}) plotted as a function of BextB_{\mathrm{ext}}. The solid lines represent linear fits of the data above 0.5 T. (c) Energy diagram summarizing the dependence of the Yb3+^{3+} states on BextB_{\mathrm{ext}}, with Yb3+^{3+} spins coupled antiferromagnetically to the surrounding Cr3+^{3+} lattice in the ground state and ferromagnetically in the excited state. The colors of the arrows indicate whether the transition redshifts, blueshifts, or is insensitive to the magnetic field. The splittings at Bext=0B_{\mathrm{ext}} = 0 are the exchange splittings (ΔEexch\Delta E_{\mathrm{exch}}) summarized in Figure 3.

PL spectra and false-color plots of CrBr₃:Yb³⁺

Figure S7. Top: PL spectra of CrBr3_3:Yb3+^{3+} 0.4% measured in the region of the 0′ →\to 0vib_{\mathrm{vib}}, 1, 2, and 3 transitions at 18 K and at various external magnetic fields (Bext∥cB_{\mathrm{ext}} \parallel c). Bottom: False-color plots of the PL in the same region vs BextB_{\mathrm{ext}}. See Figure S2 for peak assignments. Note that peaks A7_7 and A8_8 are (nearly) degenerate (ΔEexch≈0\Delta E_{\mathrm{exch}} \approx0 cm−1^{-1}) at Bext=0B_{\mathrm{ext}} = 0 T and both are labeled together as A7_7 in other figures, where only a single peak is visible. At higher external magnetic field the degeneracy is lifted and A7_7 shifts to lower energies like the other odd-value A peaks, while A8_8 stays in place like the even-value A peaks.

Using the peak assignments of Figure 3c, Figure 4b plots the ground- and excited-state splitting energies (ΔEexch\Delta E_{\mathrm{exch}}) as a function of external magnetic field. Up to ∼\sim0.3 T, the Yb3+^{3+} splittings are nearly insensitive to the external magnetic field, attributed to the presence of cancelling magnetic domains at zero field: the external field’s effect on Yb3+^{3+} spins in domains magnetized parallel to that field is cancelled out by its effect on Yb3+^{3+} spins in domains having the opposite magnetization. At field strengths greater than ∼\sim0.3$ T, the lattice is fully magnetized (Figure 2c) and ΔEexch\Delta E_{\mathrm{exch}} of the Yb3+^{3+} ground state decreases while ΔEexch\Delta E_{\mathrm{exch}} of the excited state increases, with slopes corresponding to gg values of similar magnitude ($\sim$1.9, eq (1)) but opposite signs. The field-dependence of the Yb3+^{3+} energies is summarized schematically in Figure 4c. From ΔEexch\Delta E_{\mathrm{exch}} and the gg value obtained from Figure 4b, the exchange field experienced by Yb3+^{3+} can be estimated to be ∼\sim30 T at 5 K.

g=∣1μB∂ΔEexch∂B∣(1)g = \left|\frac{1}{\mu_{\mathrm{B}}}\frac{\partial\Delta E_{\mathrm{exch}}}{\partial B}\right| \tag*{(1)}

The difference in sign between ground- and excited-state gg values indicates that the Yb3+^{3+} spins reverse their orientation in the magnetic field between the ground and emissive excited states. This change in Yb3+^{3+} spin orientation is a direct consequence of the difference in total angular momentum JJ between the 2F7/2^{2}\mathrm{F}_{7/2} and 2F5/2^{2}\mathrm{F}_{5/2} parent terms.[31] Importantly, the magnetic field dependence of the individual spin sublevels also reveals that the Yb3+^{3+} spins are antiferromagnetically coupled with CrBr3_3 in the Yb3+^{3+} ground state but are ferromagnetically coupled with CrBr3_3 in the emissive Yb3+^{3+} excited state (Figure 4c). Note that this analysis does not provide information on any possible canting of the Yb3+^{3+} spins relative to Cr3+^{3+} spins or to the CrBr3_3 plane, and further experiments would be required to determine the full details of the Yb3+^{3+} spin tensor in this material.

The low-temperature value for the ground-state exchange splitting can be used to estimate the Yb-Cr pairwise exchange coupling parameter JYb−CrJ_{\mathrm{Yb-Cr}}, using the exchange Hamiltonian H=−∑ijJijSi⋅SjH=-\sum_{ij}J_{ij}\mathbf{S}_i\cdot\mathbf{S}_j. In the absence of an external field, Heff=HmolH_{\mathrm{eff}}=H_{\mathrm{mol}}, so we can rewrite the Curie-Weiss molecular field expression for HeffH_{\mathrm{eff}}[32] to get eq (2).

JYb−Cr=gμBHmolYbz⟨SCr⟩=ΔEexchz⟨SCr⟩(2)J_{\mathrm{Yb-Cr}}=\frac{g\mu_{\mathrm{B}}H_{\mathrm{mol}}^{\mathrm{Yb}}}{z\langle S_{\mathrm{Cr}}\rangle}=\frac{\Delta E_{\mathrm{exch}}}{z\langle S_{\mathrm{Cr}}\rangle} \tag*{(2)}

In this equation, zz is the number of nearest-neighbor Cr3+^{3+} ions (3) surrounding a given Yb3+^{3+} impurity and ⟨SCr⟩\langle S_{\mathrm{Cr}}\rangle is the Cr3+^{3+} spin expectation value, which has an absolute value of 3/23/2 in the fully ordered state of CrBr3_3 (low-temperature limit). Using an extrapolated 0 K ground-state exchange splitting of 27.6 cm−1^{-1} (Figure 3d) and accounting for the antiferromagnetic alignment of Yb3+^{3+}, JYb−CrJ_{\mathrm{Yb-Cr}} is calculated to equal -6.2 cm−1^{-1} (-0.77 meV). This value is half as large as the experimental nearest-neighbor JCr−CrJ_{\mathrm{Cr-Cr}} found for CrBr3_3 (+12 cm−1^{-1} (+1.5 meV)).[33, 34] Lanthanide ff-orbital exchange interactions are typically weak due to high shielding, but this comparison suggests considerable overlap between Yb3+^{3+} 4f4f and Cr3+^{3+} 3d3d wavefunctions in CrBr3_3:Yb3+^{3+}.

The data in Figure 3d show that for both the 0 and 0′ states of Yb3+^{3+}, ΔEexch\Delta E_{\mathrm{exch}} at high temperature (paramagnetic) equals ∼\sim50% of its value at the lowest temperature (ferromagnetic). The persistence of a sizeable exchange splitting even above TCT_{\mathrm{C}} can be understood by considering that the Yb-Cr interaction is short-range, depending only on the immediately neighboring Cr3+^{3+} ions, and it is not affected by the presence or absence of long-range spin correlation. Thus, although ⟨SCr⟩=0\langle S_{\mathrm{Cr}}\rangle=0 in the high-temperature (paramagnetic) regime at zero field, the three nearest-neighbor Cr3+\mathrm{Cr}^{3+} ions exchange coupled to a given Yb3+\mathrm{Yb}^{3+} dopant may have non-zero net spin. A 2D Ising spin lattice has two phases: ferromagnetic (e.g., all Cr3+\mathrm{Cr}^{3+} spins have Sz=+3/2S_z = +3/2) and paramagnetic (spins disordered, e.g., SzS_z is randomly +3/2+3/2 or −3/2-3/2 for Cr3+\mathrm{Cr}^{3+}). Considering all possible spin configurations of the cluster of three neighboring Cr3+\mathrm{Cr}^{3+} ions acting independently in the Ising paramagnetic phase, two have S3Cr=9/2S_{3\mathrm{Cr}} = 9/2 and six have S3Cr=3/2S_{3\mathrm{Cr}} = 3/2. Due to interconversion among these configurations, the observed Yb3+\mathrm{Yb}^{3+} ΔEexch\Delta E_{\mathrm{exch}} will reflect the average magnitude of S3CrS_{3\mathrm{Cr}}. Thus, one predicts a ratio of ΔEexch(PM)/ΔEexch(FM)=1/2\Delta E_{\mathrm{exch}}(\mathrm{PM})/\Delta E_{\mathrm{exch}}(\mathrm{FM}) = 1/2 for CrBr3 ⁣:Yb3+\mathrm{CrBr}_3\!:\mathrm{Yb}^{3+}, agreeing well with our experimental observations. This same consideration holds even in more complicated (and realistic) descriptions of the magnetism of this extended lattice, but the fact that the value of ΔEexch\Delta E_{\mathrm{exch}} above TCT_{\mathrm{C}} predicted in this simple Ising approximation is similar to the one observed experimentally (Figure 3d) suggests that this system remains strongly anisotropic up to at least ∼\sim50 K. The exchange splittings observed above TCT_{\mathrm{C}} in Figure 3d therefore reflect non-cancelling short-range coupling between Yb3+\mathrm{Yb}^{3+} and its three nearest-neighbor Cr3+\mathrm{Cr}^{3+} ions, whereas the PL line broadening in this regime reflects spin disorder among these nearest-neighbor Cr3+\mathrm{Cr}^{3+} ions.

Conclusion

We have shown that incorporation of Yb3+\mathrm{Yb}^{3+} impurities into CrBr3\mathrm{CrBr}_3 yields sharp Yb3+\mathrm{Yb}^{3+} ff-ff emission centered at ∼\sim10,000 cm−1^{-1}, sensitized through Cr3+\mathrm{Cr}^{3+} dd-dd absorption. Variable-field MCPL measurements show that Yb3+\mathrm{Yb}^{3+} spins are pinned to the CrBr3\mathrm{CrBr}_3 magnetization, providing unusually facile control over the dopant’s magnetization. The highly resolved ff-ff PL spectra allow direct optical quantification of Yb3+\mathrm{Yb}^{3+}-Cr3+\mathrm{Cr}^{3+} exchange splittings, revealing them to vastly exceed kTkT at 5 K and showing that Yb3+\mathrm{Yb}^{3+}-Cr3+\mathrm{Cr}^{3+} coupling inverts from antiferromagnetic to ferromagnetic upon photoexcitation. The large spontaneous exchange splittings observed in CrBr3 ⁣:Yb3+\mathrm{CrBr}_3\!:\mathrm{Yb}^{3+} present unique opportunities for optical spin manipulation of point defects in the absence of external magnetic fields, or for in situ monitoring of short-range spin fluctuations and magnetic phase transitions. Such optically addressable spin defects may also have interesting ramifications for influencing spin textures and domain wall pinning in CrBr3\mathrm{CrBr}_3 itself, for generating localized strain effects, or for adding spin-photonic functionality to exfoliated or stacked Van der Waals nanostructures.

Acknowledgments

This work was primarily supported by the University of Washington Molecular Engineering Materials Center, a U.S. National Science Foundation Materials Research Science and Engineering Center (DMR-2308979). Additional support was received from the UW Clean Energy Institute (graduate fellowship to T.J.S.). The authors thank Prof. Rémi Beaulac for valuable discussions. Part of this work was conducted at the Molecular Analysis Facility, a National Nanotechnology Coordinated Infrastructure (NNCI) site at the University of Washington that is supported in part by the National Science Foundation (NNCI-1542101 and NNCI-2025489), the University of Washington, the Molecular Engineering & Sciences Institute, the Clean Energy Institute, and the National Institutes of Health.

Supplemental Material for

Image not extracted

Figure S4. False-color plot of the CrBr3_3:Yb3+^{3+} 0.4 % spectrum plotted versus temperature. At higher temperatures, the center of mass of the peaks blueshifts due to the appearance of hot bands.

References

  1. [1]Dillon, J. F.; Kamimura, H.; Remeika, J. P. Magnetic Rotation of Visible Light by Ferromagnetic CrBr₃. Phys. Rev. Lett. 1962, 9, 161-163.DOI
  2. [2]Dillon, J. F., Jr.; Olson, C. E. Magnetization, Resonance, and Optical Properties of the Ferromagnet CrI₃. J. Appl. Phys. 1965, 36, 1259-1260.DOI
  3. [3]Bermudez, V. M.; McClure, D. S. Spectroscopic Studies of the Two-Dimensional Magnetic Insulators Chromium Trichloride and Chromium Tribromide—I. J. Phys. Chem. Solids 1979, 40, 129-147.
  4. [4]Bermudez, V. M.; McClure, D. S. Spectroscopic Studies of the Two-Dimensional Magnetic Insulators Chromium Trichloride and Chromium Tribromide—II. J. Phys. Chem. Solids 1979, 40, 149-173.
  5. [5]Huang, B.; Clark, G.; Navarro-Moratalla, E.; Klein, D. R.; Cheng, R.; Seyler, K. L.; Zhong, D.; Schmidgall, E.; McGuire, M. A.; Cobden, D. H.; Yao, W.; Xiao, D.; Jarillo-Herrero, P.; Xu, X. Layer-Dependent Ferromagnetism in a van der Waals Crystal Down to the Monolayer Limit. Nature 2017, 546, 270-273.DOI
  6. [6]McGuire, M. A.; Dixit, H.; Cooper, V. R.; Sales, B. C. Coupling of Crystal Structure and Magnetism in the Layered, Ferromagnetic Insulator CrI₃. Chem. Mater. 2015, 27, 612-620.
  7. [7]Chen, W.; Sun, Z.; Wang, Z.; Gu, L.; Xu, X.; Wu, S.; Gao, C. Direct Observation of Van der Waals Stacking–Dependent Interlayer Magnetism. Science 2019, 366, 983-987.DOI
  8. [8]McGuire, M. A.; Clark, G.; Santosh, K. C.; Chance, W. M.; Jellison, G. E.; Cooper, V. R.; Xu, X.; Sales, B. C. Magnetic Behavior and Spin-Lattice Coupling in Cleavable Van der Waals Layered CrCl₃ Crystals. Phys. Rev. Mater. 2017, 1, 014001.arxiv.org/abs/1706.01796
  9. [9]Grebenchuk, S.; McKeever, C.; Grzeszczyk, M.; Chen, Z.; Šiškins, M.; McCray, A. R. C.; Li, Y.; Petford-Long, A. K.; Phatak, C. M.; Rüshauin, D.; Zheng, L.; Novoselov, K. S.; Santos, E. J. G.; Koperski, M. Topological Spin Textures in an Insulating van der Waals Ferromagnet. Adv. Mater. 2024, 36, 2311949.DOI
  10. [10]Augustin, M.; Jenkins, S.; Evans, R. F. L.; Novoselov, K. S.; Santos, E. J. G. Properties and Dynamics of Meron Topological Spin Textures in the Two-Dimensional Magnet CrCl₃. Nat. Commun. 2021, 12, 185.
  11. [11]Sun, Q.-C.; Song, T.; Anderson, E.; Brunner, A.; Förster, J.; Shalomayeva, T.; Taniguchi, T.; Watanabe, K.; Gräfe, J.; Stöhr, R.; Xu, X.; Wrachtrup, J. Magnetic Domains and Domain Wall Pinning in Atomically Thin CrBr₃ Revealed by Nanoscale Imaging. Nat. Commun. 2021, 12, 1989.
  12. [12]Song, T.; Cai, X.; Tu, M. W.-Y.; Zhang, X.; Huang, B.; Wilson, N. P.; Seyler, K. L.; Zhu, L.; Taniguchi, T.; Watanabe, K.; McGuire, M. A.; Cobden, D. H.; Xiao, D.; Yao, W.; Xu, X. Giant Tunneling Magnetoresistance in Spin-Filter Van der Waals Heterostructures. Science 2018, 360, 1214-1218.
  13. [13]Wang, Z.; Gutiérrez-Lezama, I.; Ubrig, N.; Kroner, M.; Gibertini, M.; Taniguchi, T.; Watanabe, K.; Imamoglu, A.; Giannini, E.; Morpurgo, A. F. Very Large Tunneling Magnetoresistance in Layered Magnetic Semiconductor CrI₃. Nat. Commun. 2018, 9, 2516.
  14. [14]Seyler, K. L.; Zhong, D.; Klein, D. R.; Gao, S.; Zhang, X.; Huang, B.; Navarro-Moratalla, E.; Yang, L.; Cobden, D. H.; McGuire, M. A.; Yao, W.; Xiao, D.; Jarillo-Herrero, P.; Xu, X. Ligand-Field Helical Luminescence in a 2D Ferromagnetic Insulator. Nature Phys. 2018, 14, 277-281.
  15. [15]Zhang, Z.; Shang, J.; Jiang, C.; Rasmita, A.; Gao, W.; Yu, T. Direct Photoluminescence Probing of Ferromagnetism in Monolayer Two-Dimensional CrBr₃. Nano Lett. 2019, 19, 3138-3142.DOI
  16. [16]Cai, X.; Song, T.; Wilson, N. P.; Clark, G.; He, M.; Zhang, X.; Taniguchi, T.; Watanabe, K.; Yao, W.; Xiao, D.; McGuire, M. A.; Cobden, D. H.; Xu, X. Atomically Thin CrCl₃: An In-Plane Layered Antiferromagnetic Insulator. Nano Lett. 2019, 19, 3993-3998.DOI
  17. [17]Snoeren, T. J.; Pressler, K.; Kluherz, K. T.; Walsh, K. M.; De Yoreo, J. J.; Gamelin, D. R. Luminescence and Covalency in Ytterbium-Doped CrX₃ (X = Cl, Br, I) van der Waals Compounds. J. Am. Chem. Soc. 2023, 145, 17427-17434.DOI
  18. [18]Doherty, M. W.; Manson, N. B.; Delaney, P.; Jelezko, F.; Wrachtrup, J.; Hollenberg, L. C. L. The Nitrogen-Vacancy Colour Centre in Diamond. Phys. Rep. 2013, 528, 1-45.DOI
  19. [19]Furdyna, J. K.; Kossut, J. Diluted Magnetic Semiconductors; Academic: 1988.
  20. [20]Maiman, T. H. Stimulated Optical Radiation in Ruby. Nature 1960, 187, 493-494.
  21. [21]Klein, J.; Song, Z.; Pingault, B.; Derringer, F.; Chi, H.; Curtis, J. B.; Dana, R.; Bushati, R.; Quan, J.; Dekanovsky, L.; Sofer, Z.; Alù, A.; Menon, V. M.; Moodera, J. S.; Lončar, M.; Narang, P.; Ross, F. M. Sensing the Local Magnetic Environment Through Optically Active Defects in a Layered Magnetic Semiconductor. ACS Nano 2023, 17, 288-299.DOI
  22. [22]Torres, K.; Kuc, A.; Maschio, L.; Pham, T.; Reidy, K.; Dekanovsky, L.; Sofer, Z.; Ross, F. M.; Klein, J. Probing Defects and Spin-Phonon Coupling in CrSBr via Resonant Raman Scattering. Adv. Funct. Mater. 2023, 33, 2211366.DOI
  23. [23]Pressler, K.; Snoeren, T. J.; Walsh, K. M.; Gamelin, D. R. Magnetic Amplification at Yb³⁺ “Designer Defects” in the van der Waals Ferromagnet CrCl₃. Nano Lett. 2023, 23, 1320-1326.DOI
  24. [24]Piephlo, S. B.; Schatz, P. N. Group Theory in Spectroscopy: With Applications to Magnetic Circular Dichroism; Wiley: 1983.
  25. [25]See Supplemental Material at https:// for additional spectroscopic data.
  26. [28]Tsubokawa, I. On the Magnetic Properties of a CrBr₃ Single Crystal. J. Phys. Soc. Jpn. 1960, 15, 1664-1668.DOI
  27. [29]Shen, X.; Chen, H.; Li, Y.; Xia, H.; Zeng, F.; Xu, J.; Kwon, H. Y.; Ji, Y.; Won, C.; Zhang, W.; Wu, Y. Multi-Domain Ferromagnetic Resonance in Magnetic Van der Waals Crystals CrI3 and CrBr3. J. Magn. Magn. Mater. 2021, 528, 167772.DOI
  28. [30]Grzeszczyk, M.; Acharya, S.; Pashov, D.; Chen, Z.; Vaklinova, K.; van Schilfgaarde, M.; Watanabe, K.; Taniguchi, T.; Novoselov, K. S.; Katsnelson, M. I.; Koperski, M. Strongly Correlated Exciton-Magnetization System for Optical Spin Pumping in CrBr3 and CrI3. Adv. Mater. 2023, 35, 2209513.DOI
  29. [31]Kojima, N.; Tsushima, K.; Tsujikawa, I. Optical Investigations of YbCrO3. I. Optical Absorption Spectra of Yb3+ Ion. J. Phys. Soc. Jpn. 1980, 49, 1449-1455.DOI
  30. [32]Smart, J. S. Effective Field Theories of Magnetism; Saunders: 1966.DOI
  31. [33]Cai, Z.; Bao, S.; Gu, Z.-L.; Gao, Y.-P.; Ma, Z.; Shangguan, Y.; Si, W.; Dong, Z.-Y.; Wang, W.; Wu, Y.; Lin, D.; Wang, J.; Ran, K.; Li, S.; Adroja, D.; Xi, X.; Yu, S.-L.; Wu, X.; Li, J.-X.; Wen, J. Topological Magnon Insulator Spin Excitations in the Two-Dimensional Ferromagnet CrBr3. Phys. Rev. B 2021, 104, L020402.DOI
  32. [34]Nikitin, S. E.; Fåk, B.; Krämer, K. W.; Fennell, T.; Normand, B.; Läuchli, A. M.; Rüegg, C. Thermal Evolution of Dirac Magnons in the Honeycomb Ferromagnet CrBr3. Phys. Rev. Lett. 2022, 129, 127201.DOI

Paper details

vlnc:W_u8jcqya9
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents