betaFeedback

WorksPhysics and Astronomy

Fracture Characteristics of Rare-earth Phosphate under Molten Calcium Magnesium Aluminosilicate Corrosion

Abstract

The fracture characteristics of LuPO4 rare-earth phosphate environmental barrier coating (EBC) material under molten calcium-magnesium aluminosilicate (CMAS) corrosion is quantified. EBCs are crucial for protecting SiC-based ceramic matrix composite components in the hot section of gas turbine engines. Recent research has highlighted the potential of rare-earth phosphates as better EBC materials than third-generation rare-earth silicates for CMAS corrosion resistance. However, the fracture of EBCs under CMAS corrosion during service remains a significant concern. This work investigates the fracture behavior of LuPO4 using mesoscale simulation and experiments. The model uses micrographs taken from fabricated EBC samples for mesoscale fracture simulations. The simulation results are compared with experimental fracture toughness data and validated using statistical tests (p<0.01). The simulation results and experimental observations demonstrate that LuPO4 may exhibit higher fracture resistance than Lu2SiO5 rare-earth silicate under similar CMAS corrosion conditions, offering potential insights for future EBC design and development.

Manuscript

Introduction

Environmental barrier coatings (EBCs) are used to protect silicon carbide (SiC) based ceramic matrix composites (CMC) from high-temperature corrosion in the hot-section of gas turbine engines [1]. Recently, rare-earth phosphates are shown to have significant advantages over third-generation rare-earth silicates for molten calcium-magnesium aluminosilicate (CMAS) corrosion resistance [2], [3], [4], [5]. However, it is unclear if the advantages of corrosion resistance translate into improved fracture resistance for rare-earth phosphates compared to silicates. Improving fracture resistance is crucial for EBCs to avoid microcracking, which is one of the primary reasons for spallation and eventual failure [6], [7], [8]. This work investigates the fracture behavior of rare-earth phosphate in comparison to rare-earth silicate EBCs under CMAS corrosion using mesoscale simulations and experiments.

Silicon carbide (SiC) based ceramic matrix composites (CMC) have been proven to be a suitable replacement for Ni-based superalloys used in the hot section components of gas turbine engines due to their stable high-temperature performance [1], [9]. However, when SiC-based CMCs are subject to high-temperature gas streams at high speed within the gas turbines, they undergo different reactions and surface recession (corrosion) [10]. One of the leading causes of corrosion in CMCs is the reaction and penetration of molten CMAS formed from ingested debris, i.e., sand, dust or volcanic ash [11]. To protect CMCs from corrosion, environmental barrier coatings (EBCs) are used. EBCs are designed to be mechanically and chemically stable at high temperatures, providing a protective barrier between the high-temperature gas stream and CMCs [12].

In the past several decades, numerous materials have been developed for EBC applications. These materials are broadly categorized into three generations based on their increasing high-temperature capability realized by introducing different high-temperature resistant compounds. The first generation EBCs contain mullite (Al2O3⋅SiO2\mathrm{Al}_2\mathrm{O}_3\cdot\mathrm{SiO}_2), the second generation contains BSAS (BaO⋅SrO⋅Al2O3⋅SiO2\mathrm{BaO}\cdot\mathrm{SrO}\cdot\mathrm{Al}_2\mathrm{O}_3\cdot\mathrm{SiO}_2) and the third generation contains rare-earth (RE) silicates (RE2Si2O7/RE2SiO5\mathrm{RE}_2\mathrm{Si}_2\mathrm{O}_7/\mathrm{RE}_2\mathrm{SiO}_5) in their composition [13]. Among these, the third generation EBCs based on rare-earth disilicates are more durable and offer better protection against CMAS corrosion than earlier generations [12]. However, rare-earth disilicates still corrode rapidly when exposed to molten CMAS at temperatures of 1300∘C1300^\circ\mathrm{C} and above, as the CMAS melt penetrates along the grain boundaries, forming large cracks and severe swelling [14], [15]. Recently, this shortcoming has been addressed by replacing disilicates with phosphates, which form a continuous and dense reaction layer that halts CMAS penetration into the bulk pellet and limits corrosion [4], [5]. With less CMAS corrosion, rare-earth phosphates are a promising EBC material with durable high-temperature performance for hot sections of gas turbine engines.

This work focuses on quantifying the effects of CMAS corrosion on the fracture strength of EBCs using mesoscale simulations. During CMAS corrosion, molten CMAS penetrates the EBC microstructure with randomly oriented ceramic grains and causes structural changes [5], [14]. The penetration into the microstructure is driven by total energy reduction through the formation of two CMAS-ceramic interfaces (low energy) replacing one ceramic-ceramic interface (high-energy grain boundary) [16]. The penetrated CMAS forms a brittle and glassy phase along ceramic grain boundaries that degrade the fracture strength of EBC [12, 14]. However, it is crucial to analyze and quantify the extent of degradation caused by penetrated CMAS, which might help understand the fracture performance of EBCs under CMAS corrosion. Hence, the structural degradation of EBC microstructures is analyzed by estimating fracture resistance for different CMAS penetration levels based on experimental observations.

Among the available computational fracture models for polycrystalline materials, phase field and cohesive zone-based models are the most frequently used [17, 18, 19, 20, 21, 22]. This work uses a mesoscale model based on the cohesive finite element model (CFEM) for fracture simulation and estimating fracture resistance of EBC microstructures [23, 24]. The cohesive finite element model (CFEM) has been used in the past to identify microstructural fracture patterns, i.e., intergranular/transgranular fracture, in metals and ceramics [24, 25, 26, 27] and for estimating fracture resistance of microstructures [23, 26, 28, 29].

This work uses the CFEM to simulate fracture through EBC microstructures before and after CMAS penetration [23]. The microstructures used in the models consist of randomly oriented ceramic grains and their grain boundaries. The CMAS penetration is modeled by adding CMAS along the grain boundaries [14]. The fracture is tracked using cohesive elements inserted along all element edges throughout the model, as described in the Methods section. The cohesive elements are assigned different traction-separation laws based on the material or interface they represent (see Methods section). Complex fracture patterns arising due to anisotropic ceramic grains, orientation-dependent grain boundaries, and the presence of CMAS are accounted using different material properties and traction separation laws. The fracture resistance of the EBC is estimated by computing JJ-integral [30] and fracture toughness (KIcK_{\mathrm{Ic}}). The computed KIcK_{\mathrm{Ic}} is validated with the experimental KIcK_{\mathrm{Ic}} measured from indentation fracture tests on EBC samples before and after CMAS penetration. Additionally, statistical tests are performed to asses similarities or differences between the simulation results and experimental measurements (Supplementary Figure 3 and Table 1-Table 3). A detailed description of the CFEM, JJ-integral, and KIcK_{\mathrm{Ic}} computation and measurement of experimental fracture toughness is provided in the Methods section. This work uses a combination of simulations and experiments to get meaningful insights into the fracture behavior of the EBC materials under CMAS penetration, as depicted in Figure 1. Based on the observations in this work, the approach comprising simulations and experiments may be a promising way to obtain actionable insights into the behavior of new materials for whom extensive testing is infeasible.

Image not extracted

Figure 1. A schematic flow diagram showing the combined experiments and simulation approach adopted in this work. The cohesive finite element models (CFEM) are formulated using experimentally obtained electron backscattered diffraction (EBSD) micrographs of EBC samples. The CFEM is used for fracture simulations and fracture toughness (KIcK_{\mathrm{Ic}}) computation. The computed KIcK_{\mathrm{Ic}} is validated with the experimental KIcK_{\mathrm{Ic}} obtained using micro and nanoindentation tests [44] performed on EBC samples before and after CMAS penetration. The validated model is then used to investigate the fracture characteristics of EBCs with CMAS penetration. The microstructural characterization of EBC samples is carried out using scanning electron microscopy (SEM) and energy-dispersive X-ray spectroscopy (EDS). The computed KIcK_{\mathrm{Ic}} values and microstructural characterization are used to compare the fracture resistance of rare-earth phosphate and silicate EBCs.

Supplementary Figure 3. Statistical testing flow chart for comparing fracture toughness obtained from CFEM simulations and indentation experiments.

Hypothesis testNull hypothesis (H0H_0)
Shapiro-Wilk normality testThe data was drawn from a normal distribution
Two-sample FF-testTwo data samples were drawn from normal distributions of same variance
Two-sample Kolmogorov-Smirnov testTwo data samples were independently drawn from distributions that have the same shape but may have a different mean
Two-sample tt-test (Equal variances)Two data samples were drawn independently from two normal distributions with equal means but unknown and equal variances
Two-sample tt-test (Unequal variances)Two data samples were drawn independently from normal distributions with equal means but unknown and unequal variances
Wilcoxon rank-sum testTwo data samples were drawn from continuous distributions with the same shape and equal medians

Table 1. Null hypotheses for the statistical tests used in this work

LuPO4_4 + 5% CMASLuPO4_4 + 8% CMASLu2_2SiO5_5 + 5% CMASLu2_2SiO5_5 + 8% CMAS
Material →\toExpCFEMExpCFEMExpCFEMExpCFEM
Hypothesis tests ↓\downarrow
Shapiro-Wilk normality testpp-value0.22500.00420.24350.04120.13670.00220.45210.0574
Normal distribution?YesNoYesYesYesNoYesYes
Two-sample FF-testpp-value---0.5329---0.4204
Equal variance?---Yes---Yes
Kolmogorov-Smirnov testpp-value0.0111---0.3516---
Same distribution?Yes---Yes---
Two-sample tt-test (Equal variance)pp-value---0.006---0.1069
Equal means?---No---Yes
Two-sample tt-test (Unequal variance)pp-value------------
Equal means?------------
Wilcoxon rank-sum testpp-value0.2073---0.8018---
Equal medians?Yes---Yes---
OutcomeSimilarNot SimilarSimilarSimilar

Table 3. Supplementary Table 3: The pp-values of various statistical tests used to assess similarity (p<0.01p < 0.01) of experiment and simulation data for CMAS-penetrated materials.

RESULTS

Model Validation

Among the available rare-earth (RE) metals for EBC applications, lutetium (Lu) is chosen in this work as lutetium phosphate (LuPO4\mathrm{LuPO}_{4}) and lutetium silicate (Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5}). They exhibit better CMAS resistance and thermal expansion compatibility as EBC topcoats than other RE phosphates and silicates [5, 12, 31]. Unlike single-layered coating designs used in phosphate EBCs ([4, 32]), multi-layered coating designs are generally adopted in silicate EBC applications [12]. The multi-layered design consists of Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} (monosilicate) top coat and an interlayer of Lu2Si2O7\mathrm{Lu}_{2}\mathrm{Si}_{2}\mathrm{O}_{7} (disilicate) below the top coat but above the bond coat. As a result, Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} (monosilicate), being the top coat, serves as the first line of defense against CMAS in silicate EBC and is thus chosen for analysis in this work.

Validation of CFEM without CMAS penetration

The mesoscale simulations are carried out for LuPO4\mathrm{LuPO}_{4} and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} using eight different microstructure (EBSD) images taken from fabricated EBC samples (Supplementary Figures 12). A schematic representation of the CFEM model with boundary conditions is shown in Figure 7 (Methods section). A total of 32 simulations are carried out by initiating fracture on each of the four sides of the experimentally obtained microstructures. The simulation results for the LuPO4_4 and Lu2_2SiO5_5 without CMAS penetration are shown in Figure 2. The pure EBCs exhibit a tortuous fracture propagation (Figure 2a-Figure 2b), which could be attributed to the material anisotropy and difference in the fracture strengths of grains and grain boundaries. The anisotropy and inhomogeneity in the microstructure cause the crack path to pass through grains (transgranular fracture) and along grain boundaries (intergranular fracture). The crack path is quantified using a crack path fraction parameter defined as fractions of crack path inside grains, i.e., HGR=LGRLGB+LGRH_{\mathrm{GR}} = \frac{L_{\mathrm{GR}}}{L_{\mathrm{GB}}+L_{\mathrm{GR}}}, and fraction of crack path along the grain boundaries, i.e., HGB=LGBLGR+LGBH_{\mathrm{GB}} = \frac{L_{\mathrm{GB}}}{L_{\mathrm{GR}}+L_{\mathrm{GB}}}, where LGBL_{\mathrm{GB}} and LGRL_{\mathrm{GR}} are crack lengths within grains and along grain boundaries, respectively [23]. The mean values of crack path fraction are found to be around 0.6 and 0.4 for the grains and grain boundaries, respectively, for both the LuPO4_4 and Lu2_2SiO5_5 EBCs (Figure 2c). The similarity of the crack path fractions indicates the dominant effect of the microstructure on the fracture behaviour of EBCs, where same set of microstructures are used for the fracture simulations of both EBCs.

Image not extracted

Figure 2. Simulation results from cohesive finite element model (CFEM) for LuPO4_4 and Lu2_2SiO5_5 EBCs, and CMAS. Fracture patterns in the (a) LuPO4_4 and (b) Lu2_2SiO5_5 microstructures through grains and along grain boundaries (c) The box plots show crack path fractions for EBCs. The JJ-integral values for (d) LuPO4_4 and (e) Lu2_2SiO5_5 EBCs with evolving crack length. The variations in JJ-integral values for all the microstructures are shown as light-colored bands and their average is the dark-colored curve. Panel (f) compares fracture toughness (KIcK_{\mathrm{Ic}}) obtained from CFEM simulations with that of experimentally obtained values. The ‘*’ indicates similarity of the data from experiments and CFEM simulations based on two-sample tt-test and Wilcoxon rank-sum test, see supplementary data for details.

Image not extracted

Figure 7. Schematic representation of the (a) cohesive finite element discretization and (b) computational model for CFEM simulations subjected to surfing boundary condition.

The model is validated by comparing fracture toughness KIcK_{\mathrm{Ic}} of the EBCs obtained from CFEM simulations to that of the experimentally measured values. The KIcK_{\mathrm{Ic}} is estimated from the JJ-integral values obtained from simulations using the relation outlined in the Methods section. The JJ-integral values for LuPO4_4 and Lu2_2SiO5_5 EBCs with evolving crack length are shown in Figure 2d and 2e, respectively. The noticeable variation in the JJ-integral values for different microstructures could be attributed to the tortuosity of the crack path (Figure 2a and Figure 2b) [33]. Hence, the mean JJ-integral values for the middle 50% of the sample length are used to estimate the KIcK_{\mathrm{Ic}} of the samples mitigating the edge-effects. The estimated KIcK_{\mathrm{Ic}} values for the LuPO4_4, Lu2_2SiO5_5, and CMAS samples are compared with that of the experimentally measured values in Figure 2f [25, 34]. Notice that the KIcK_{\mathrm{Ic}} for homogenous and isotropic CMAS is almost constant with zero variance (Figure 2f).

For validation in Figure 2f, 10, 11 and 15 experimental measurements of indentation fracture toughness (KIcK_{\mathrm{Ic}}) are used for LuPO4_4, Lu2_2SiO5_5 and CMAS respectively, with 32 values computed for each material from the simulations. The similarity between computed and experimentally measured KIcK_{\mathrm{Ic}} values is assessed using statistical tests based on a two-sample tt-test and Wilcoxon rank-sum test with p<0.01p < 0.01 (Supplementary Table 2). The tests show that the KIcK_{\mathrm{Ic}} values estimated from simulations are indeed statistically similar to that of experimentally measured values, thus validating simulation results for pure EBCs and CMAS. The observations demonstrate the ability of the CFEM to simulate fracture accurately in pure LuPO4_4, Lu2_2SiO5_5 and CMAS.

Validation of CFEM with CMAS penetration

The CFEM is further validated to describe the fracture behavior of CMAS-penetrated EBCs.

Two levels of CMAS penetration, i.e., 5% and 8% by volume, are introduced along the grain boundaries within the microstructures obtained from the fabricated EBC samples. These two levels are chosen based on experimental observations in this work and literature [35] that indicate CMAS penetration along the grain boundaries within the in the range of 0–15% by volume. The CFEM simulations are carried out using boundary conditions and material properties presented in the Methods section. The KIcK_{\mathrm{Ic}} values estimated from the JJ-integral values are compared with the experimental KIcK_{\mathrm{Ic}} of LuPO4\mathrm{LuPO}_{4} and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} with CMAS (5% and 8% by volume) measured from indentation fracture testing.

The simulation results for 5% and 8% CMAS-penetrated LuPO4\mathrm{LuPO}_{4} and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} EBC samples are shown in Figure 3. A total of 32 simulations are carried out for each of the EBCs with CMAS penetration by initiating fracture on each of the four sides of the microstructure obtained from eight EBSD images of EBCs. The tortuous fracture patterns observed in a LuPO4\mathrm{LuPO}_{4} microstructure at 5% and 8% CMAS penetration are shown in Figure 3a through 3d. Fracture patterns show that the crack predominantly propagates through the penetrated CMAS regions. This behavior is expected as the fracture strength of CMAS and CMAS-grain interfaces are considered lower than the grains and grain boundaries (Table 2). The crack path fractions for the CMAS-penetrated microstructures are shown in Figure 3e. The crack path fractions are defined as fractions of the crack path inside grains, i.e., HGR=LGRLGR+LGB+LCM+LCIH_{\mathrm{GR}} = \frac{L_{\mathrm{GR}}}{L_{\mathrm{GR}}+L_{\mathrm{GB}}+L_{\mathrm{CM}}+L_{\mathrm{CI}}}, along the grain boundaries, i.e., HGB=LGBLGR+LGB+LCM+LCIH_{\mathrm{GB}} = \frac{L_{\mathrm{GB}}}{L_{\mathrm{GR}}+L_{\mathrm{GB}}+L_{\mathrm{CM}}+L_{\mathrm{CI}}}, inside CMAS, i.e., HCM=LCMLGR+LGB+LCM+LCIH_{\mathrm{CM}} = \frac{L_{\mathrm{CM}}}{L_{\mathrm{GR}}+L_{\mathrm{GB}}+L_{\mathrm{CM}}+L_{\mathrm{CI}}}, and along grain-CMAS interface, i.e., HCI=LCILGR+LGB+LCM+LCIH_{\mathrm{CI}} = \frac{L_{\mathrm{CI}}}{L_{\mathrm{GR}}+L_{\mathrm{GB}}+L_{\mathrm{CM}}+L_{\mathrm{CI}}}, where LGRL_{\mathrm{GR}}, LGBL_{\mathrm{GB}}, LCML_{\mathrm{CM}} and LCIL_{\mathrm{CI}} are crack lengths within grains, along grain boundaries, within penetrated CMAS, and grain-CMAS interface, respectively. The crack path fractions indicate that increasing CMAS penetration from 5% to 8% causes increased crack propagation through CMAS-grain interfaces (CI) in both LuPO4\mathrm{LuPO}_{4} and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} samples. Conversely, cracks passing through grains (GR) and grain boundaries (GB) decrease.

Image not extracted

Figure 3. Simulation results from cohesive finite element model (CFEM) for 5% and 8% CMAS-penetrated LuPO₄ and Lu₂SiO₅ EBCs. Panels (a)–(b) and (c)–(d) show fracture patterns in the 5% and 8% CMAS-penetrated LuPO₄ and Lu₂SiO₅ EBC microstructures respectively. The box plots in panel (e) shows crack path fractions for EBCs with CMAS penetration. The JJ-integral values for (f) LuPO₄ and (g) Lu₂SiO₅ with and without CMAS penetration are compared with that of the pure CMAS with evolving crack length. The variations in JJ-integral values for all the microstructures are shown as light-colored bands and their average is presented with the dark-colored curve. Panel (h) compares fracture toughness (KIcK_{\mathrm{Ic}}) obtained from CFEM simulations with that of experimentally obtained values. The ‘*’ indicates similarity of the data from experiments and CFEM simulations based on two-sample tt-test and Wilcoxon rank-sum test, see supplementary data for details.

The JJ-integral values computed using CFEM simulations for CMAS-penetrated LuPO4\mathrm{LuPO}_{4} and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} are shown in Figure 3f and Figure 3g as a function of evolving crack length. The mean value of JJ-integral for both 5% and 8% CMAS penetration lies below the JJ-integral value of pure LuPO4/Lu2SiO5\mathrm{LuPO}_{4}/\mathrm{Lu}_{2}\mathrm{SiO}_{5}, indicating degradation due to the presence of CMAS in the microstructure.

The model is validated by comparing fracture toughness KIcK_{\mathrm{Ic}} of CMAS-penetrated EBCs with that of the experimentally measured values. The JJ-integral from the middle 50% of the simulation length is used to estimate KIcK_{\mathrm{Ic}} to mitigate the edge effects. The distribution of KIcK_{\mathrm{Ic}} for EBCs with the 5% and 8% CMAS penetration is presented using box plots in Figure 3h. For validation in Figure 3h, 06 and 05 values of experimentally measured indentation fracture toughness (KIcK_{\mathrm{Ic}}) are used for LuPO₄ with 5% and 8% CMAS, respectively, with 32 values for each material from the simulations. While for Lu₂SiO₅, 10 values of experimental KIcK_{\mathrm{Ic}} are used. for both 5% and 8% CMAS penetrated microstructures. The KIcK_{\mathrm{Ic}} values obtained from simulations and experiments are compared and their similarity is assessed using statistical tests based on a two-sample tt-test and Wilcoxon rank-sum test with p<0.01p < 0.01. The tests in Figure 3f show that the estimated KIcK_{\mathrm{Ic}} is statistically similar to that of experimentally measured values for three out of four cases (Supplementary Table 3). The fracture toughness for LuPO4_4 with 8% CMAS penetration does not show statistical similarity with the experimental values (Figure 3f). This could be due to insufficient experimental observations needed to test the statistical similarity between measured and computed KIcK_{\mathrm{Ic}}. Nonetheless, the comparison shows reasonable agreement for both LuPO4_4 and Lu2_2SiO5_5 in most cases. In addition, it is seen that an increase in CMAS penetration from 5% to 8% led to a decrease in KIcK_{\mathrm{Ic}}, indicating higher degradation in fracture resistance with increasing CMAS penetration.

The statistical tests further reinforce the efficacy of CFEM in predicting the fracture behavior of CMAS-penetrated EBCs.

Fracture Resistance of LuPO4_4 and Lu2_2SiO5_5 with CMAS Penetration

The validated CFEM is employed to investigate the fracture behavior of LuPO4_4 and Lu2_2SiO5_5 EBCs with increasing CMAS penetration. Based on observations from CMAS reaction tests on EBC samples and literature [35], five levels of CMAS penetration are considered for fracture simulations: 3%, 5%, 8%, 11% and 15% by volume. Similar to the validation studies, a total of 32 simulations are carried out for each penetration level, and their results are shown in Figure 4.

Image not extracted

Figure 4. Simulation results obtained using cohesive finite element model (CFEM) for LuPO4 and Lu2SiO5 microstructures at different levels of CMAS penetration. The fracture patterns in (a) LuPO4 and (b) Lu2SiO5 EBC microstructures are shown with 0% CMAS (pure), 3% CMAS, 8% CMAS and 15% CMAS penetration. Panels (c) and (d) show average crack path fractions before and after CMAS penetration in LuPO4 and Lu2SiO5, respectively. The JJ-integral values for (e) LuPO4 and (f) Lu2SiO5 before and after CMAS penetration are compared with that of the pure CMAS with evolving crack length. Panels (g) and (h) compare fracture toughness (KIcK_{\mathrm{Ic}}) and residual strength before and after CMAS penetration in LuPO4 and Lu2SiO5, respectively.

The tortuous fracture patterns obtained using CFEM before and after CMAS penetration for both LuPO4_4 and Lu2_2SiO5_5 EBC microstructures are shown in Figure 4a and Figure 4b, respectively. The tortuosity of fracture in EBCs without CMAS penetration (Pure EBC) is due to the anisotropy of grains. On the other hand, crack path tortuosity after CMAS penetration can be attributed to the presence of CMAS along the grain boundaries and its lower fracture strength than grains and grain boundaries. The lower fracture strength of CMAS and its interfaces causes the fracture to pass through CMAS regions in the CMAS-penetrated microstructures (Figure 4a and Figure 4b). It is observed that the fraction of total crack length passing through grains and grain boundaries decreases with increasing CMAS penetration, while the fraction of crack length passing through CMAS and CMAS-grain interface increases at the same time (Figure 4c and Figure 4d). Moreover, a steep decrease in the fraction of crack path passing through grains and grain boundaries at 3% CMAS penetration compared to pure LuPO4_4 and Lu2_2SiO5_5 indicates a significant change in fracture behavior caused by CMAS.

The average JJ-integral curves obtained from simulation for LuPO4 and Lu2SiO5 with different CMAS penetration levels are shown in Figure 4e and Figure 4f. For reference, the average JJ-integral curves of pure LuPO4, Lu2SiO5, and CMAS are shown as dashed curves at the top and bottom of the plots. It is observed that the average JJ-integral curves of CMAS-penetrated LuPO4 and Lu2SiO5 microstructures progressively degrade with increasing CMAS penetration level and approach the average JJ-integral curve of CMAS. The JJ-integral values in the middle 50% sample lengths are used to estimate KIcK_{\mathrm{Ic}}. The distribution of KIcK_{\mathrm{Ic}} values estimated from all 32 simulations performed on eight experimentally obtained microstructures are plotted as box plots for CMAS-penetrated LuPO4\mathrm{LuPO}_{4} and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} in Figure 4g and Figure 4h, respectively. The degradation due to CMAS penetration can be seen more clearly in the box plots. The KIcK_{\mathrm{Ic}} degradation at different levels of CMAS penetration is indicated as residual strength percentages by assuming the fracture strength of pure LuPO4\mathrm{LuPO}_{4} and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} as 100% and that of the CMAS as 0%. The degradation of KIcK_{\mathrm{Ic}} in LuPO4\mathrm{LuPO}_{4} is observed to be higher than in Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5}. With a further increase in CMAS penetration, the KIcK_{\mathrm{Ic}} values degrade further and approach CMAS values. A steep drop in KIcK_{\mathrm{Ic}} caused by low levels of CMAS penetration in LuPO4\mathrm{LuPO}_{4} emphasizes the need for mechanisms that can limit CMAS penetration into the microstructures.

Discussion

A cohesive finite element analysis framework is developed to investigate the effect of CMAS penetration on the fracture behavior in EBCs. The CFEM is first validated with the experimentally measured fracture toughness of pure and CMAS-penetrated EBCs. The validated model is then employed to investigate fracture characteristics of LuPO4\mathrm{LuPO}_{4} in comparison with Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} with increasing CMAS penetration. The simulation results reveal that CMAS corrosion causes degradation of fracture resistance (KIcK_{\mathrm{Ic}}) in both LuPO4\mathrm{LuPO}_{4} and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} EBCs, with more degradation observed in LuPO4\mathrm{LuPO}_{4} (Figure 4g and Figure 4h). It is seen that before CMAS penetration, the KIcK_{\mathrm{Ic}} of LuPO4\mathrm{LuPO}_{4} was slightly higher than that of Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5}. However, after CMAS penetration, the KIcK_{\mathrm{Ic}} values of LuPO4\mathrm{LuPO}_{4} are generally lower than Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5}. The lower values of KIcK_{\mathrm{Ic}} for LuPO4\mathrm{LuPO}_{4} are also observed experimentally in the indentation test results shown in Figure 3h.

These observations indicate that the fracture resistance of CMAS-penetrated LuPO4\mathrm{LuPO}_{4} is lower than that of Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5}. Interestingly, it also emphasizes that a higher fracture resistance of LuPO4\mathrm{LuPO}_{4}, in comparison with Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5}, could be achieved by eliminating or minimizing CMAS corrosion. To test this hypothesis, we have experimentally studied the CMAS corrosion in LuPO4\mathrm{LuPO}_{4} and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} by exposing them to molten CMAS at 1300 °C for 45 and 5 hours, respectively. Notice that the LuPO4\mathrm{LuPO}_{4} sample was subjected to a 45-hour CMAS reaction to observe its CMAS corrosion resistance under more severe conditions with a longer duration.

The backscattered scanning electron microscopy (SEM) and energy dispersive X-ray spectroscopy (EDS) images of LuPO4\mathrm{LuPO}_{4} and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} after the CMAS reaction are shown in Figure 5 and Figure 6, respectively. Figure 5a and Figure 6a show the epoxy, CMAS, and bulk EBC pellet after CMAS reaction in LuPO4\mathrm{LuPO}_{4} and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} samples. It is observed that Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} delaminates after the CMAS reaction of 5 hours, whereas the LuPO4_4 remains intact even after 45 hours.

Image not extracted

Figure 5. SEM backscattered electron images of LuPO4 interaction with molten CMAS at 1300 °C for 45 hours. (a) Cross-section SEM image, (b) Higher resolution cross-section SEM image, (c) EDS elemental maps.

Image not extracted

Figure 6. SEM backscattered electron images of Lu2_2SiO5_5 interaction with molten CMAS at 1300 °C for 5 hours. (a) Cross-section SEM image, (b) Higher resolution cross-section SEM image, (c) EDS elemental maps.

The delamination in Lu2_2SiO5_5 could be attributed to the mismatch in the coefficient of thermal expansion between Lu2_2SiO5_5 (~6.7×10−66.7 \times10^{-6} in the temperature range 200°C-1350°C) and oxyapatite Ca2_2Lu8_8(SiO4_4)6_6O2_2 phase formed in the reaction layer [36]. Further investigation is needed to achieve a mechanistic understanding of the stress distribution and delamination in the Lu2_2SiO5_5.

The high-resolution SEM images of the reaction zone in LuPO4_4 and Lu2_2SiO5_5 samples are shown in Figure 5b and Figure 6b, respectively. It is seen that a reaction layer is formed at the interface of CMAS and EBCs during the CMAS reaction. The average thicknesses of the reaction layer for LuPO4_4 and Lu2_2SiO5_5 are measured (at 20 locations on the SEM image) to be 32.8±3.832.8 \pm3.8 µm and 6.1±1.46.1 \pm1.4 µm, respectively. LuPO4_4 forms a continuous and dense reaction layer than the Lu2_2SiO5_5. This aligns with the observations that RE silicates form porous and non-uniform reaction layers under CMAS corrosion [37]. At the same time, the RE phosphates have been observed to form continuous and denser reaction layers [4].

The EDS maps of CMAS-LuPO4_4 and -Lu2_2SiO5_5 interfaces are shown in Figure 5c and Figure 6c, respectively. In LuPO4_4, calcium (Ca) did not penetrate through the reaction layer. However, a noticeable penetration of Ca is seen in Lu2_2SiO5_5. The penetration of Ca in LuPO4_4 is restricted, possibly due to the formation of a continuous and dense reaction layer of Ca8_8MgLu(PO4_4)7_7 along the CMAS-LuPO4_4 interface. On the other hand, in Lu2_2SiO5_5, a porous and non-uniform reaction layer of oxyapatite Ca2_2Lu8_8(SiO4_4)6_6O2_2 may have allowed Ca to penetrate in bulk Lu2_2SiO5_5. Magnesium (Mg) and Aluminum (Al) penetration is observed to be similar in both LuPO4_4 and Lu2_2SiO5_5.

The color intensity of the EDS maps suggests that the amount of Lu present in the reaction layer is less in LuPO4_4 (Figure 5c) than in Lu2_2SiO5_5 (Figure 6c). This indicates that less LuPO4_4 is needed to form a dense reaction layer compared to Lu2_2SiO5_5. A lower stoichiometric ratio of Lu:Ca in Ca8_8MgLu(PO4_4)7_7 (at the CMAS-LuPO4_4 reaction layer) as compared to a higher Lu:Ca ratio in Ca2_2Lu8_8(SiO4_4)6_6O2_2 (at CMAS-Lu2_2SiO5_5 reaction layer) may have played a role in the amount of Lu in the reaction layer [38]. In contrast, a high concentration of Ca is required to form the Ca8_8MgLu(PO4_4)7_7 interfacial phase, limiting its penetration into the EBC matrix as compared with that of Lu2_2SiO5_5, and with the formation of the dense reaction layer at the interface, inhibiting the penetration of CMAS.

The abovementioned observations indicate that LuPO4 might perform better than Lu2SiO5 at restricting the amount of CMAS penetrating into the bulk region by forming a dense and thicker reaction layer [32] with higher contents of Ca and less Lu. As a result, LuPO4 might be able to avoid degradation of KIcK_{\mathrm{Ic}} from CMAS penetration and retain its fracture resistance for a longer duration of time with the formation of the dense interfacial layer. The dense reaction layer was also observed in the LuPO4 upon CMAS interaction at 5 hours at 1300 °C with a thickness of 16.2±3.6 μm. The greater amount of CMAS penetration in the Lu2SiO5 may significantly alter the thermal expansion coefficient of the matrix as well, leading to the delamination of the bulk matrix underneath the reaction layer, in contrast to the well-maintained structural integrity of the LuPO4 matrix without cracking or delamination upon CMAS interaction at the same temperature but elongated duration.

The experimental observations clearly indicate that LuPO4 may be able to retain a higher fracture resistance (KIcK_{\mathrm{Ic}}) due to less CMAS penetration than Lu2SiO5 under similar CMAS corrosion conditions.

METHODS

EBC Microstructure Models

The microstructures used in CFEM simulations are constructed from micrographs obtained using electron backscatter diffraction (EBSD). EBSD is a scanning electron microscope-based technique that scans the surface of a crystalline sample [39]. This work uses eight EBSD micrographs obtained by scanning different locations on the surface of a spark plasma sintered lutetium phosphate (LuPO4_4) sample. The EBSD micrographs represent data as a 2D array of pixels representing multiple scanned points on the sample surface. The color of each pixel indicates a unique orientation, i.e., Euler angles: ϕ1\phi_1, Φ\Phi, ϕ2\phi_2, based on the crystal structure at a particular point on the sample surface. The scan size of each micrograph used is 40×40 sqμm with 133 × 133 pixels along the x and y direction (Supplementary Figure 1). The raw EBSD data is processed through an open-source MATLAB® (MathWorks Inc., Natick, Massachusetts, USA) toolbox MTEX [36]. While processing, the microstructure is assumed to have no porosity, and missing data in the EBSD is filled using the nearest neighbor algorithm to get a microstructure with contiguous grains [37]. After processing the EBSD data, a uniformly meshed grid of 2D plane strain quadrilateral finite elements is laid on the EBSD microstructure and sectioned according to different grains in the microstructure. Each section representing a different grain in the microstructure is assigned material properties based on their orientations. This creates the microstructure models before CMAS penetration (Supplementary Figure 2).

Image not extracted

Supplementary Figure 1. Electron backscattered diffraction (EBSD) micrographs obtained from the LuPO4_4 sample. Panels (a) through (h) show the raw EBSD micrographs. The orientations of each individual grain in micrographs are shown with reference to the sample coordinate system. Their respective colors represent the rendering based on the values of individual Euler angles.

Generation of Abaqus model from electron backscatter diffraction (EBSD) micrographs, with panels (a)–(f)

Supplementary Figure 2. Generation of Abaqus model from electron backscatter diffraction (EBSD) micrographs. Panels (a) and (d) show the raw EBSD micrographs. The raw EBSD micrographs are processed to remove non-indexed data in (b) and (e). The grains and grain boundaries are assigned different sections in Abaqus, and material properties are assigned based on orientation and misorientation as shown in (c) and (f).

The microstructure models with CMAS penetration are generated by introducing CMAS layer along the grain boundaries. The grains are displaced to make space for CMAS by applying outward radial translation to their centroids with reference to the center of the entire microstructure. The outward radial translation is adjusted such that the overall empty spaces created along the grain boundaries reflect the desired level of CMAS penetration, i.e., 3%, 5%, 8%, 11% and 15% by volume, into the microstructure. Similar to the microstructure models without CMAS penetration, a uniform mesh of 2D plane strain quadrilateral finite elements is laid and sectioned based on different microstructure regions that include grains and CMAS along the grain boundaries (Figure 4a and Figure 4b).

Cohesive Finite Element Model (CFEM)

A cohesive finite element model (CFEM) with zero-thickness cohesive elements embedded along the edges of all the 2D plane strain quadrilateral elements (Figure 7a) [23], [24], [25] is employed to investigate the fracture characteristics of EBCs. The CFEM model is implemented in Abaqus® (Dassault Systemes Simulia Corporation, Providence, Rhode Island, USA) [40] and uses its standard bilinear traction separation law of the form,

t={tnts}=(1−D)[Knn00Kss]{δnδs},(1)\mathbf{t} = \begin{Bmatrix} t_n \\ t_s \end{Bmatrix} = (1-D) \begin{bmatrix} K_{nn} & 0 \\ 0 & K_{ss} \end{bmatrix} \begin{Bmatrix} \delta_n \\ \delta_s \end{Bmatrix}, \tag*{(1)}

where t\mathbf{t} is the traction vector on the cohesive element, DD is scalar damage, KK is the cohesive stiffness of the element, and δ\delta is the separation between its faces. A linear scalar damage law is defined as,

D=δc(δ−δ0)δ(δc−δ0),(2)D = \frac{\delta_c(\delta-\delta_0)}{\delta(\delta_c-\delta_0)}, \tag*{(2)}

where δ\delta is the current effective separation, i.e., δ=δn2+δs2\delta= \sqrt{\delta_n^2+\delta_s^2}, δ0\delta_0 is the initial separation for damage initiation, and δc\delta_c is the critical separation at failure. The initial separation (δ0\delta_0) is defined as the separation when the damage initiation criterion

{(tnTmax⁡)2+(tsTmax⁡)2}0.5=1(3)\left\{\left(\frac{t_n}{T_{\max}}\right)^2+\left(\frac{t_s}{T_{\max}}\right)^2\right\}^{0.5}=1 \tag*{(3)}

based on quadratic traction is satisfied. The maximum traction Tmax⁡T_{\max} is assumed same for normal and shear directions [23]. The cohesive parameters used in this study are listed in Table 2.

A schematic diagram of the computational model used in CFEM simulations is shown in Figure 7b. A total of 32 CFEM simulations are performed by initiating crack along all four edges of each of the EBC microstructures obtained from eight EBSD images shown in Supplementary Figure 1. The cohesive element size is taken as 0.3μm to ensure convergence of fracture simulations for the given material properties and cohesive zone parameters [23, 41]. Surfing boundary conditions are used to induce stable crack propagation through the microstructures as shown in Figure 7b [33]. The JJ-integral is computed using a contour integral approach on a homogenous region surrounding the microstructures (Figure 7b) [33, 34, 42]. All the materials in this work are considered brittle and their material properties are given in Table 2. The computed JJ-integral is used to estimate the fracture toughness using the relation,

KIc=JEˉ1−νˉK_{Ic} = \sqrt{\frac{J\bar{E}}{1-\bar{\nu}}}

where JJ is the computed JJ-integral, Eˉ\bar{E} is the effective Youngs modulus and νˉ\bar{\nu} is the effective Poisson’s ratio [30]. The homogeneous region surrounding the microstructure is assigned homogenized material properties of the microstructure it surrounds. The cohesive zone parameters based on bilinear traction separation laws are used for the cohesive elements inside the ceramic grains, i.e., LuPO4_4 and Lu2_2SiO5_5, and CMAS regions. For cohesive elements along the grain boundaries a sinusoidal fracture strength variation is assumed. It takes maximum and minimum value as 100% and 58% of the fracture strength of the grain, respectively [23]. The fracture strengths are assigned to the cohesive elements on grain boundaries based on misorientation between the adjacent grains [25]. The cohesive zone parameters are derived from the fracture toughness measured from indentation fracture experiments performed in this work. While the isotropic elastic properties are experimentally measured and the anisotropic elastic properties are taken from the literature [2, 36, 43]. The elastic properties of the homogenous regions surrounding CMAS-penetrated microstructures are computed using the rule of mixtures [33].

Elastic PropertiesCohesive Zone Parameters
MaterialIsotropicAnisotropic (GPa)Cohesive Stiffness (Knn=KssK_{nn}=K_{ss})Critical Separation (δc\delta_c)Max Traction (Tmax⁡T_{\max})
LuPO4_4E=193.4E=193.4 GPa; ν=0.29\nu=0.29C11=326.9C_{11}=326.9; C12=32.6C_{12}=32.6; C13=111C_{13}=111; C22=282.9C_{22}=282.9; C33=403.8C_{33}=403.8; C44=80.4C_{44}=80.4; C66=31.9C_{66}=31.91000 N/μm2^20.01 μm0.0016 N/μm2^2
Lu2_2SiO5_5E=148.6E=148.6 GPa; ν=0.24\nu=0.24C11=240C_{11}=240; C12=67C_{12}=67; C13=86C_{13}=86; C15=9C_{15}=9; C22=221C_{22}=221; C23=49C_{23}=49; C25=−20C_{25}=-20; C33=194C_{33}=194; C35=−35C_{35}=-35; C44=52C_{44}=52; C46=11C_{46}=11; C55=81C_{55}=81; C66=71C_{66}=711000 N/μm2^20.01 μm0.0015 N/μm2^2
CMASE=104.5E=104.5 GPa; ν=0.26\nu=0.26---1000 N/μm2^20.01 μm0.0008 N/μm2^2
CMAS-grain Interface------1000 N/μm2^20.01 μm0.0004 N/μm2^2
Grain Boundaries------1000 N/μm2^20.01 μmTmax⁡×{0.785+0.215sin⁡(4θ)}∗T_{\max}\times\{0.785+0.215\sin(4\theta)\}^{*}

Table 2. Material properties and cohesive zone parameters.

Material Preparation and CMAS Reaction

The EBCs pellets were sintered using spark plasma sintering (SPS) method. The LuPO4_4 powder used in the experiments was synthesized as reported by Bryce et al. [32]. Lu2_2SiO5_5 was synthesized via a solid-state reaction, where the appropriate ratios of Lu2_2O3_3 and SiO2_2 were milled together via high-energy ball milling (HEBM) at 500 rpm using ethanol as the mixing solvent and ZrO2\mathrm{ZrO}_{2} milling balls as the grinding material. The model CMAS (33CaO33\mathrm{CaO}-9MgO9\mathrm{MgO}-13AlO1.513\mathrm{AlO}_{1.5}-45SiO245\mathrm{SiO}_{2}) is prepared by mixing oxide powders CaO\mathrm{CaO} (99.99%, Sigma-Aldrich), MgO\mathrm{MgO} (99.99%, Sigma-Aldrich), Al2O3\mathrm{Al}_{2}\mathrm{O}_{3} (99.99%, Sigma-Aldrich), and SiO2\mathrm{SiO}_{2} (99.9%, Alfa Aesar) according to the stoichiometric ratio. The mixture was then heated at the rate of 10 ∘C min−110\,^{\circ}\mathrm{C}\,\mathrm{min}^{-1} up to 1300 ∘C1300\,^{\circ}\mathrm{C} for 8 hours and, finally, quenched in water to prepare the model CMAS. The LuPO4\mathrm{LuPO}_{4}-CMAS and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5}-CMAS composites (with 5% and 8% CMAS) were also synthesized via solid-state ball milling of LuPO4\mathrm{LuPO}_{4} and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} powders with the model CMAS powder in their appropriate volume ratios. The milled powders were dried and then ground into fine powders, which were loaded into 10 mm diameter cylindrical graphite dies and sintered into dense pellets using SPS (Model 10−310^{-3} SPS system, Thermal Tech. LLC, Santa Rosa, CA). The powder samples were heated from room temperature to the sintering temperature of 1500 ∘C1500\,^{\circ}\mathrm{C} at a rate of 200 ∘C min−1200\,^{\circ}\mathrm{C}\,\mathrm{min}^{-1}, then held at 1500 ∘C1500\,^{\circ}\mathrm{C} and under a uniaxial pressure of 50 MPa for 15 min. The sintered pellets were then ground with SiC abrasive papers and then polished with 0.06 μm0.06\,\mu\mathrm{m} silica colloid to achieve a mirror finish. The CMAS reactions on LuPO4\mathrm{LuPO}_{4} and Lu2SiO5\mathrm{Lu}_{2}\mathrm{SiO}_{5} were performed in a box furnace at 1300 ∘C1300\,^{\circ}\mathrm{C} with a heating rate of 10 ∘C min−110\,^{\circ}\mathrm{C}\,\mathrm{min}^{-1} for 5 hours. The reacted samples were cut in half, processed, and polished for analysis.

Measurement of Indentation Fracture Toughness

Fracture toughness was estimated from a combination of micro indentation and nanoindentation measurements. A micro-hardness tester (Leco M-400) was used to create 10 indentations, each sample with a load of 1 kgf (∼9.8\sim9.8 N), and each indentation lasted for 15 seconds. The crack lengths of these indentations were measured from the SEM image of each indentation. Nanoindentation tests were also carried out for each sample with a load of 1000 μN1000\,\mu\mathrm{N} used to measure the hardness and elastic modulus of each sample. The fracture toughness (KcK_{\mathrm{c}}) was evaluated using Eq (4),

Kc=δ(EH)0.5Pc1.5,(4)K_{\mathrm{c}} = \delta\left(\frac{E}{H}\right)^{0.5}\frac{P}{c^{1.5}}, \tag*{(4)}

where EE is the elastic modulus, HH is the hardness, PP is the load for each micro indentation, cc is the average value of all crack lengths from the micro indentation test and δ\delta is the indenter geometry related parameter.

DATA AVAILABILITY

The datasets/codes/scripts generated and/or analyzed during the current study are available from the corresponding author upon reasonable request.

Author Contributions

R.R., L.Z., L.H., J.L., and S.D. conceived the research. S.S. developed the methodology, implemented simulation models and analyzed the results. B.P.M. and K.B. synthesized and characterized the EBC samples and measured the material properties. R.R., L.Z., L.H., J.L., and S.D. supervised the project. All authors reviewed and edited the manuscript.

Acknowledgements

This work was funded by the Division of Materials Research, National Science Foundation under Award DMREF-2119423. The funder played no role in study design, data collection, analysis and interpretation of data, or the writing of this manuscript.

Competing Interests

All authors declare no financial or non-financial competing interests.

Supplementary_data

Electron back scattered diffraction (EBSD) micrographs

Abaqus models from EBSD micrographs

Statistical Analysis

The flowchart of the statistical analysis to determine the similarity between simulation results and experimental measurements using univariate hypothesis testing is shown in Supplementary Figure 3. The null hypotheses for each of the hypothesis tests used in the statistical analysis are listed in Supplementary Table 1. Based on the univariate hypothesis tests, the calculated pp-values are shown in Supplementary Tables 2 and 3 for pure and CMAS-penetrated materials, respectively. In Supplementary Tables 2 and 3, the boldface text represents the pp-value of the hypothesis test that determines the similarity between simulations and experiments.

Material →\toPure LuPO4_4Pure Lu2_2SiO5_5Pure CMAS
Hypothesis tests ↓\downarrowExpCFEMExpCFEMExpCFEM
Shapiro-Wilk normality testpp-value0.21820.00990.84120.35230.49560.1847
Normal distribution?YesNoYesYesYesYes
Two-sample FF-testpp-value------0.90150.000
Equal variance?------YesNo
Kolmogorov-Smirnov testpp-value0.1306------
Same distribution?Yes------
Two-sample tt-test (Equal variance)pp-value---0.1063---
Equal means?---Yes---
Two-sample tt-test (Unequal variance)pp-value------0.8857
Equal means?------Yes
Wilcoxon rank-sum testpp-value0.2095------
Equal medians?Yes------
OutcomeSimilarSimilarSimilar

Table 2. The pp-values of various statistical tests used to assess similarity (p<0.01p < 0.01) of experiment and simulation data for pure materials.

References

  1. [1]N. S. Jacobson, “Corrosion of Silicon-Based Ceramics in Combustion Environments,” Journal of the American Ceramic Society, vol. 76, no. 1, pp. 3–28, 1993, doi: 10.1111/J.1151-2916.1993.TB03684.X.DOI
  2. [2]J. Han, Y. Wang, R. Liu, and F. Wan, “Theoretical and experimental investigation of Xenotime-type rare earth phosphate REPO4 (RE = Lu, Yb, Er, Y and Sc) for potential environmental barrier coating applications,” Scientific Reports 2020 10:1, vol. 10, no. 1, pp. 1–13, Aug. 2020, doi: 10.1038/s41598-020-70648-0.DOI
  3. [3]Y. Wang, X. Chen, W. Liu, L. Cheng, and L. Zhang, “Exploration of YPO4 as a potential environmental barrier coating,” Ceram Int, vol. 36, no. 2, pp. 755–759, Mar. 2010, doi: 10.1016/J.CERAMINT.2009.10.014.DOI
  4. [4]M. Ridley, B. McFarland, C. Miller, and E. Opila, “YbPO4: A novel environmental barrier coating candidate with superior thermochemical stability,” Materialia (Oxf), vol. 21, Mar. 2022, doi: 10.1016/j.mtla.2021.101289.DOI
  5. [5]X. Hu, F. Xu, K. Li, Y. Zhang, Y. Xu, and X. Zhao, “Thermal properties and Calcium-Magnesium-Alumina-Silicate (CMAS) resistance of LuPO4 as environmental barrier coatings,” J Eur Ceram Soc, vol. 40, no. 4, pp. 1471–1477, Apr. 2020, doi: 10.1016/J.JEURCERAMSOC.2019.11.018.DOI
  6. [6]F. Stolzenburg, P. Kenesei, J. Almer, K. N. Lee, M. T. Johnson, and K. T. Faber, “The influence of calcium-magnesium-aluminosilicate deposits on internal stresses in Yb2Si2O7 multilayer environmental barrier coatings,” Acta Mater, vol. 105, pp. 189–198, Feb. 2016, doi: 10.1016/j.actamat.2015.12.016.DOI
  7. [7]R. P. Panakajrupally, M. J. Presby, K. Manigandan, J. Zhou, G. G. Chase, and G. N. Morscher, “Thermomechanical Characterization of SiC/SiC Ceramic Matrix Composites in a Combustion Facility,” Ceramics 2019, Vol. 2, Pages 407-425, vol. 2, no. 2, pp. 407–425, Jun. 2019, doi: 10.3390/CERAMICS2020032.
  8. [8]J. Liu, L. Zhang, Q. Liu, L. Cheng, and Y. Wang, “Structure design and fabrication of environmental barrier coatings for crack resistance,” J Eur Ceram Soc, vol. 34, no. 8, pp. 2005–2012, Aug. 2014, doi: 10.1016/J.JEURCERAMSOC.2013.12.049.DOI
  9. [9]“Ceramic matrix composites taking flight at GE Aviation.” Accessed: May 16, 2023. [Online]. Available: https://bulletin-archive.ceramics.org/is-cacheable/1576757776052/19q281t.pdf
  10. [10]F. W. Zok, V. E. Collier, and M. R. Begley, “Coating recession effects in ceramic matrix composite strength,” J Mech Phys Solids, vol. 156, p. 104608, Nov. 2021, doi: 10.1016/J.JMPS.2021.104608.DOI
  11. [11]D. Tejero-Martin, C. Bennett, and T. Hussain, “A review on environmental barrier coatings: History, current state of the art and future developments,” J Eur Ceram Soc, vol. 41, no. 3, pp. 1747–1768, Mar. 2021, doi: 10.1016/J.JEURCERAMSOC.2020.10.057.
  12. [12]K. N. Lee, D. Zhu, and R. S. Lima, “Perspectives on Environmental Barrier Coatings (EBCs) Manufactured via Air Plasma Spray (APS) on Ceramic Matrix Composites (CMCs): A Tutorial Paper,” Journal of Thermal Spray Technology, vol. 30, no. 1–2, pp. 40–58, Jan. 2021, doi: 10.1007/S11666-021-01168-0.DOI
  13. [13]Y. Xu, X. Hu, F. Xu, and K. Li, “Rare earth silicate environmental barrier coatings: Present status and prospective,” Ceram Int, vol. 43, no. 8, pp. 5847–5855, Jun. 2017, doi: 10.1016/J.CERAMINT.2017.01.153.DOI
  14. [14]L. R. Turcer, A. R. Krause, H. F. Garces, L. Zhang, and N. P. Padture, “Environmental-barrier coating ceramics for resistance against attack by molten calcia-magnesia-aluminosilicate (CMAS) glass: Part II, β-Yb2Si2O7 and β-Sc2Si2O7,” J Eur Ceram Soc, vol. 38, no. 11, pp. 3914–3924, Sep. 2018, doi: 10.1016/J.JEURCERAMSOC.2018.03.010.DOI
  15. [15]V. L. Wiesner, D. Scales, N. S. Johnson, B. J. Harder, A. Garg, and N. P. Bansal, “Calcium–magnesium aluminosilicate (CMAS) interactions with ytterbium silicate environmental barrier coating material at elevated temperatures,” Ceram Int, vol. 46, no. 10, pp. 16733–16742, Jul. 2020, doi: 10.1016/J.CERAMINT.2020.03.249.DOI
  16. [16]T. M. Shaw and P. R. Duncombe, “Forces between Aluminum Oxide Grains in a Silicate Melt and Their Effect on Grain Boundary Wetting,” Journal of the American Ceramic Society, vol. 74, no. 10, pp. 2495–2505, Oct. 1991, doi: 10.1111/J.1151-2916.1991.TB06791.X.DOI
  17. [17]A. Abdollahi and I. Arias, “Numerical simulation of intergranular and transgranular crack propagation in ferroelectric polycrystals,” Int J Fract, vol. 174, no. 1, pp. 3–15, Mar. 2012, doi: 10.1007/S10704-011-9664-0.DOI
  18. [18]T. T. Nguyen, J. Réthoré, J. Yvonnet, and M. C. Baietto, “Multi-phase-field modeling of anisotropic crack propagation for polycrystalline materials,” Comput Mech, vol. 60, no. 2, pp. 289–314, Aug. 2017, doi: 10.1007/S00466-017-1409-0/FIGURES/34.DOI
  19. [19]H. Hirshikesh and A. Alankar, “On the interplay of elastic anisotropy and fracture toughness anisotropy in fracture of single and multiphase polycrystals,” Eng Fract Mech, vol. 273, p. 108696, Oct. 2022, doi: 10.1016/J.ENGFRACMECH.2022.108696.DOI
  20. [20]J. Qian and S. Li, “Application of multiscale cohesive zone model to simulate fracture in polycrystalline solids,” J Eng Mater Technol, vol. 133, no. 1, Jan. 2011, doi: 10.1115/1.4002647/465311.DOI
  21. [21]G. Geraci and M. H. Aliabadi, “Micromechanical modeling of cohesive thermoelastic steady-state and transient cracking in polycrystalline materials,” Int J Numer Methods Eng, vol. 117, no. 12, pp. 1205–1233, Mar. 2019, doi: 10.1002/NME.5997.DOI
  22. [22]S. M. Taheri Mousavi, N. Richart, C. Wolff, and J. F. Molinari, “Dynamic crack propagation in a heterogeneous ceramic microstructure, insights from a cohesive model,” Acta Mater., vol. 88, pp. 136–146, Apr. 2015, doi: 10.1016/J.ACTAMAT.2015.01.003.DOI
  23. [23]U. Roy and M. Zhou, “A computational framework for predicting the fracture toughness of metals as a function of microstructure,” J Mech Phys Solids, vol. 142, p. 103955, Sep. 2020, doi: 10.1016/J.JMPS.2020.103955.DOI
  24. [24]X. P. Xu and A. Needleman, “Numerical simulations of fast crack growth in brittle solids,” J Mech Phys Solids, vol. 42, no. 9, pp. 1397–1434, Sep. 1994, doi: 10.1016/0022-5096(94)90003-5.DOI
  25. [25]U. Roy, D. L. McDowell, and M. Zhou, “Effect of grain orientations on fracture behavior of polycrystalline metals,” J Mech Phys Solids, vol. 151, p. 104384, 2021, doi: https://doi.org/10.1016/j.jmps.2021.104384.
  26. [26]Y. Li and M. Zhou, “Effect of competing mechanisms on fracture toughness of metals with ductile grain structures,” Eng Fract Mech, vol. 205, pp. 14–27, 2019, doi: https://doi.org/10.1016/j.engfracmech.2018.11.006.
  27. [27]J. Zhai, V. Tomar, and M. Zhou, “Micromechanical simulation of dynamic fracture using the cohesive finite element method,” J. Eng. Mater. Technol., vol. 126, no. 2, pp. 179–191, 2004, doi: https://doi.org/10.1115/1.1647127.
  28. [28]Y. Li, D. L. McDowell, and M. Zhou, “A multiscale framework for predicting fracture toughness of polycrystalline metals,” Mater Perform Charact, vol. 3, no. 3, pp. 157–172, 2014, doi: http://dx.doi.org/10.1520/MPC20130064.
  29. [29]Y. Li and M. Zhou, “Prediction of fracture toughness of ceramic composites as function of microstructure: I. Numerical simulations,” J Mech Phys Solids, vol. 61, no. 2, pp. 472–488, Feb. 2013, doi: 10.1016/j.jmps.2012.09.013.DOI
  30. [30]J. R. Rice, “A Path Independent Integral and the Approximate Analysis of Strain Concentration by Notches and Cracks,” J Appl Mech, vol. 35, pp. 379–386, 1968.
  31. [31]Z. Tian et al., “General trend on the phase stability and corrosion resistance of rare earth monosilicates to molten calcium–magnesium–aluminosilicate at 1300 oC,” Corros Sci, vol. 148, pp. 281–292, Mar. 2019, doi: 10.1016/J.CORSCI.2018.12.032.DOI
  32. [32]K. Bryce, Y. T. Shih, L. Huang, and J. Lian, “Calcium-Magnesium-Aluminosilicate (CMAS) corrosion resistance of high entropy rare-earth phosphate (Luo0.2Yb0.2Er0.2Y0.2Gd0.2)PO4: A novel environmental barrier coating candidate,” J Eur Ceram Soc, vol. 43, no. 14, pp. 6461–6472, Nov. 2023, doi: 10.1016/j.jeurceramsoc.2023.06.030.DOI
  33. [33]M. Z. Hossain, C. J. Hsueh, B. Bourdin, and K. Bhattacharya, “Effective toughness of heterogeneous media,” J Mech Phys Solids, vol. 71, no. 1, pp. 15–32, Nov. 2014, doi: 10.1016/J.JMPS.2014.06.002.DOI
  34. [34]A. Lotfolahpour and M. Asle Zaeem, “Effects of cleavage plane and material strength on fracture of polycrystalline brittle materials: A phase-field modeling study,” Comput Mater Sci, vol. 197, Sep. 2021, doi: 10.1016/j.commatsci.2021.110642.DOI
  35. [35]N. P. Padture, M. Gell, and E. H. Jordan, “Thermal barrier coatings for gas-turbine engine applications,” Science (1979), vol. 296, no. 5566, pp. 280–284, Apr. 2002, doi: 10.1126/SCIENCE.1068609/ASSET/377DB6FF-9DA8-433A-823D-4441A59DBAD6/ASSETS/GRAPHIC/SE1420362004.JPEG.pubmed.ncbi.nlm.nih.gov/11951028
  36. [36][36*] Z. Tian, L. Sun, J. Wang, and J. Wang, “Theoretical prediction and experimental determination of the low lattice thermal conductivity of Lu2SiO5,” J Eur Ceram Soc, vol. 35, no. 6, pp. 1923–1932, Jun. 2015, doi: 10.1016/J.JEURCERAMSOC.2015.01.001.
  37. [37]M. Wolf, D. E. Mack, O. Guillon, and R. Valßen, “Resistance of pure and mixed rare earth silicates against calcium-magnesium-aluminosilicate (CMAS): A comparative study,” Journal of the American Ceramic Society, vol. 103, no. 12, pp. 7056–7071, Dec. 2020, doi: 10.1111/JACE.17328.DOI
  38. [38]X. Hu, F. Xu, K. Li, Y. Zhang, Y. Xu, and X. Zhao, “Thermal properties and Calcium-Magnesium-Alumina-Silicate (CMAS) resistance of LuPO4 as environmental barrier coatings,” J Eur Ceram Soc, vol. 40, no. 4, pp. 1471–1477, Apr. 2020, doi: 10.1016/J.JEURCERAMSOC.2019.11.018.DOI
  39. [39]“EBSD Data Processing best practice - Oxford Instruments.” Accessed: Jun. 12, 2023. [Online]. Available: https://www.oxinst.com/blogs/ebsd-data-processing-best-practice
  40. [40]“Abaqus 2022 Documentation.” Accessed: May 29, 2023. [Online]. Available: https://docs.software.vt.edu/abaqusv2022/English/?show=SIMACAELMRRefMap/simaelm-c-cohesiveusage.htm
  41. [41]V. Tomar, J. Zhai, and M. Zhou, “Bounds for element size in a variable stiffness cohesive finite element model,” Int J Numer Methods Eng, vol. 61, no. 11, pp. 1894–1920, Nov. 2004, doi: 10.1002/NME.1138.DOI
  42. [42]C. J. Hsueh and K. Bhattacharya, “Homogenization and Path Independence of the J-Integral in Heterogeneous Materials,” Journal of Applied Mechanics, Transactions ASME, vol. 83, no. 10, Oct. 2016, doi: 10.1115/1.4034294/422264.DOI
  43. [43]V. L. Wiesner and N. P. Bansal, “Mechanical and thermal properties of calcium–magnesium aluminosilicate (CMAS) glass,” J Eur Ceram Soc, vol. 35, no. 10, pp. 2907–2914, 2015, doi: https://doi.org/10.1016/j.jeurceramsoc.2015.03.032.
  44. [44]B. Gong, D. Frazer, T. Yao, P. Hosemann, M. Tonks, and J. Lian, “Nano-and micro-indentation testing of sintered UO2 fuel pellets with controlled microstructure and stoichiometry,” Journal of Nuclear Materials, vol. 516, pp. 169–177, 2019, doi: https://doi.org/10.1016/j.jnucmat.2019.01.021.

Paper details

vlnc:W_uae6xtym
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents