betaFeedback

WorksPhysics and Astronomy

Epitaxial CeO2 Films as a Host for Quantum Applications

Abstract

In highly purified host, the coherence of quantum emitters is ultimately limited by hyperfine interactions between the emitter and lattice nuclei possessing non-zero nuclear magnetic moments. This limitation can only be mitigated through isotopic purification. In this work, we investigate CeO2 as a host composed entirely of nuclei with zero nuclear moment. High-quality CeO2 thin films were grown by PLD and doped with Tm and Er ions. Structural characterization using X-ray diffraction, atomic force microscopy, and ion channeling confirms single-crystalline, atomically smooth films with dopants substitutionally incorporated at Ce lattice sites. Photoluminescence lifetime measurements show significantly longer lifetimes for Er-doped CeO2 (2.9 - 5.3 ms) compared with Tm-doped films (14 - 68 μs). Moreover, the Er-doped PLD films exhibit longer lifetimes at ~1% dopant concentration than previously reported for MBE-grown films. Density functional theory calculations reveal a substantial overlap between unoccupied O 2p and Tm 4f states near the valence band maximum, whereas Er 4f states remain well isolated. This electronic interaction likely introduces non-radiative recombination pathways in Tm-doped CeO2, explaining the reduced lifetimes. These findings highlight the importance of selecting appropriate dopant-host combinations and optimized growth conditions to minimize non-radiative channels for quantum applications.

combinations and optimized growth conditions to minimize non-radiative channels for quantum applications.

Introduction

Currently, many quantum emitters have been identified in a diverse set of host matrices, including nitrogen-vacancy [1, 2] and silicon-vacancy (SiV) [3, 4, 5] centers in diamond, divacancies and silicon vacancies in silicon carbide (SiC) [6, 7], or color centers in two-dimensional materials [8]. The presence of isotopes with non-zero nuclear spin, such as 13C{}^{13}\mathrm{C} (1.1%) in diamond or 29Si{}^{29}\mathrm{Si} (4.7%) in SiC, introduces spin bath decoherence via hyperfine interaction [9]. While impressive spin coherence times, longer than one millisecond, have been observed in these materials, such demonstrations typically require isotopically purified hosts to remove the decoherence stemming from nuclei with non-zero magnetic moment.

Recently, wide bandgap oxides have emerged as promising hosts for quantum emitters [10, 11, 12, 13]. These materials allow for cost-effective single-crystal growth and offer a broad choice of lattice-matched substrates. Among various strategies, doping with rare-earth (RE) ions such as Er3+\mathrm{Er}^{3+}, Eu3+\mathrm{Eu}^{3+}, and Tm3+\mathrm{Tm}^{3+} has gained attention due to the characteristic 4f4f-4f4f optical transitions, which are well shielded by the outer 5s25s^{2} and 5p65p^{6} shells [14, 15, 16, 17]. This shielding renders transitions relatively immune to perturbations from the host lattice, enabling long radiative lifetimes and high optical coherence. For example, Er3+\mathrm{Er}^{3+} ions in Y2SiO5\mathrm{Y}_{2}\mathrm{SiO}_{5} exhibit radiative lifetimes on the order of ~ 11 ms [18], while Eu3+\mathrm{Eu}^{3+} in Y2O3\mathrm{Y}_{2}\mathrm{O}_{3} demonstrates lifetimes around 0.8 ms [19]. Other notable systems include Pr3+\mathrm{Pr}^{3+} in YAlO3\mathrm{YAlO}_{3} [20] and Nd3+\mathrm{Nd}^{3+} in LaF3\mathrm{LaF}_{3} [21], both of which exhibit narrow linewidths and long coherence under cryogenic conditions. Today, various deposition processes like molecular beam epitaxy, pulsed-laser deposition (PLD), and sputtering have demonstrated the capability to grow such oxides with atomic-level control.

Oxygen is nearly void of magnetic nuclei, which puts oxides at an advantage as a host with enhanced spin coherence. In particular, Cerium oxide (CeO2\mathrm{CeO}_{2}) offers a unique advantage as all of cerium’s stable isotopes have zero nuclear spin, and oxygen’s only spin-active isotope (17O{}^{17}\mathrm{O}) has a natural abundance of just 0.04%, making CeO2\mathrm{CeO}_{2} effectively a magnetically purified host [22, 23, 24]. This feature significantly suppresses spin bath-induced decoherence, preserving the intrinsic coherence of rare-earth dopants and potentially color centers. Indeed, Er3+\mathrm{Er}^{3+} doped in CeO2\mathrm{CeO}_{2} has demonstrated optical lifetimes as high as 1.5 ms at 4 K [25, 26], double that of Eu3+\mathrm{Eu}^{3+} in Y2O3\mathrm{Y}_{2}\mathrm{O}_{3} [19], highlighting the potential of CeO2\mathrm{CeO}_{2} for rare earth-based quantum emitters. Furthermore, large-area single-crystalline CeO2\mathrm{CeO}_{2} can be grown on a range of substrates, including silicon.

Among the rare-earth dopants, thulium (Tm3+\mathrm{Tm}^{3+}) is a compelling candidate. Its strong 3H4→3H6{}^{3}\mathrm{H}_{4} \rightarrow{}^{3}\mathrm{H}_{6} emission at ~ 794 nm [27] lies within the first biological transparency window and the near-infrared (NIR) telecommunication band. In addition, Tm3+\mathrm{Tm}^{3+} ions have an ionic radius (88 pm) closely matching that of Ce4+\mathrm{Ce}^{4+} (87 pm), facilitating efficient substitution at the Ce Wyckoff sites in the fluorite CeO2\mathrm{CeO}_{2} lattice.

Experimental Details

Growth of epitaxial films of RE3+^{3+}: CeO2_2

High-density ceramic targets of CeO2_2, Ce0.99_{0.99}Er0.01_{0.01}O3_3, and Ce0.9_{0.9}Tm0.1_{0.1}O3_3 were synthesized from high-purity precursors of CeO2_2 (99.999%), Er2_2O3_3, and Tm2_2O3_3 (99.999%), procured from Sigma-Aldrich. The powders were homogeneously mixed, compacted using a cold isostatic press (CIP), and subsequently sintered at 1300° C to achieve dense, crack-free 1 inch diameter targets. Epitaxial thin films of Tm3+^{3+}-doped CeO2_2, with Tm concentrations of 10, and 1 at.% were deposited on single-crystal YSZ (001) and Si (001) substrates using pulsed laser deposition (PLD, Neocera) in an ultra-high vacuum (UHV) chamber with in-situ reflection high-energy electron diffraction (RHEED) monitoring. Prior to deposition, YSZ (001) and Si (001) substrates were cleaned sequentially with deionized (DI) water, acetone, and isopropanol (IPA), followed by a final rinse with DI water to eliminate organic residues and particulates. The cleaned YSZ (001) substrates were then annealed in ambient air at 1000° C for 3 hours to enhance surface crystallinity and morphological uniformity. On the other hand, single-side polished Si (001) substrates with native SiO2_2 surface layers were introduced into the PLD chamber and subjected to a tailored deposition protocol to accommodate the amorphous interfacial oxide. Once the base pressure in the chamber was reduced significantly below 1×10−51 \times10^{-5} Torr (a reducing condition), the substrates were gradually heated to the final deposition temperature. An initial buffer layer of ∼7\sim7 nm CeO2_2 was deposited at a repetition rate of 2 Hz in vacuum, serving to facilitate epitaxial alignment along CeO2_2 (111) by sequential removal of the native oxide layer. This was followed by the growth of 500 nm CeO2_2 (or Tm-doped CeO2_2 using a multi-target carousel) under a controlled oxygen partial pressure (1.1×10−31.1 \times10^{-3} Torr). In contrast, depositions on single-crystal YSZ (001) substrates were performed directly under the desired oxygen ambience, without the buffer layer, owing to the favorable lattice match and absence of an interfacial oxide layer. This facilitates to grow CeO2_2 (or Tm:CeO2_2) film along (001) orientation. Epitaxial thin films of Er3+^{3+}-doped CeO2_2 with Er concentration of 1 at.% were deposited on Si (001) and YSZ (001) substrates following the protocols discussed above. A KrF excimer laser (λ=248\lambda= 248 nm) was employed for ablation, with the laser fluence maintained at ∼1.5\sim1.5 J/cm2^2 and a target-to-substrate distance of ∼5\sim5 cm. The depositions were performed at a substrate temperature of ∼820∘\sim820^{\circ}C under an oxygen partial pressure of 1.1×10−31.1 \times10^{-3} Torr, followed by a 30-minute annealing at the same temperature with the oxygen pressure remaining unchanged during the annealing and cooling process.

Structural, crystalline quality characterization

X-ray diffraction (XRD) and X-ray reflectivity (XRR) measurements were conducted using a Rigaku SmartLab diffractometer equipped with a Cu Kα_{\alpha} radiation source (λ=1.5406\lambda= 1.5406 Å), operating at an accelerating voltage of 45 kV and a current of 200 mA. High-resolution XRD scans were performed in the 2θ2\theta-ω\omega configuration to evaluate the crystallographic structure, phase purity, and out-of-plane orientation of the deposited thin films. XRR measurements were employed to determine film thickness, and interfacial roughness, utilizing a reflectivity mode with an angular resolution finer than 0.005∘0.005^{\circ}, ensuring precise quantification of the film structure and surface morphology.

Rutherford Backscattering Spectrometry (RBS) and ion channeling (RBS/C) measurements were conducted using a NEC 9SH 3MV Pelletron accelerator at the Ion Beam Laboratory (IBL), University of North Texas (UNT) [28]. The details of the measurement are in supplementary information (S.I.) section S1.

For scanning transmission electron microscopy (STEM) and energy-dispersive X-ray spectroscopy (EDS) analysis, cross-sectional lamellas of the thin film samples were prepared in the Tescan dual beam SEM-FIB via FIB lift-out method. To enable atomic-resolution analysis, the lamellas were further thinned to ∼30\sim30 nm using a Fischione 1040 Nanomill. STEM imaging and EDS characterization were performed on a JEOL JEM-ARM300F TEM, operated at 300 kV with aberration correction. For this study the probe size was calibrated to 0.09 nm, with a convergence semi-angle of 24 mrad and 68 pA probe current. High-resolution STEM images were collected using a high-angle annular dark field (HAADF) detector (42 mrad -180 mrad). For atomic-resolution EDS mapping, a scan area of <4×4< 4 \times4 nm2^2 with <5< 5 Å step size and 0.1 ms dwell time was used, with drift correction applied after each scan.

Computational Methods

Geometry optimizations and the densities of states (DOS) were carried out using density functional theory (DFT) as implemented in the Vienna ab-initio Simulation Package (VASP) version 6.5 [29, 30], with the projector augmented wave (PAW) method [31]. The generalized gradient-corrected exchange and correlation functional of Perdew-Burke-Ernzerhof (PBE) [32] was employed, and the Ce 4f15s25p65d16s24f^{1}5s^{2}5p^{6}5d^{1}6s^{2}, O 2s22p42s^{2}2p^{4}, Tm 4f135s25p66s24f^{13}5s^{2}5p^{6}6s^{2}, and Er 4f125s25p66s24f^{12}5s^{2}5p^{6}6s^{2} electrons were treated explicitly in all of the calculations. A simple rotationally invariant approach [33] was considered with an effective Hubbard U parameter of U = 5.0 eV for Ce [34], and U = 7.3 eV [35, 36, 37] for Tm and Er to account for localized Ce and Tm 4f electrons, as recommended in the literature. The plane-wave basis set energy cutoffs were 700 eV in DFT+U calculations, and the energy converged within 1 meV/atom. All spin-polarized calculations were performed in a 2×2×22 \times2 \times2 supercell of Fm3ˉm\mathrm{Fm}\bar{3}\mathrm{m} CeO2\mathrm{CeO}_{2} containing 96 atoms using a 3×3×33 \times3 \times3 Γ\Gamma-centered Monkhorst-Pack k-point mesh [38]. Magnetic moments were obtained from spin-polarized calculations.

Results and Discussion

Structural and crystalline quality of the RE3+\mathrm{RE}^{3+}: CeO2\mathrm{CeO}_{2} films

To achieve epitaxial growth and maintain stoichiometry in Tm3+\mathrm{Tm}^{3+}: CeO2\mathrm{CeO}_{2} thin films, key deposition parameters including substrate temperature, target to substrate distance, laser fluence, and partial oxygen pressure (PO2P_{\mathrm{O}_{2}}) were systematically optimized. Figure 1a presents the high-resolution X-ray diffraction (HRXRD) 2θ2\theta-ω\omega scan of a 10 at.% Tm-doped CeO2\mathrm{CeO}_{2} film grown on YSZ (001) substrate using these optimized conditions. Whereas HRXRD pattern of other films grown on both YSZ (001) and Si (001), following the same growth parameters, are shown in the S.I. (Figure S1-S4). The HRXRD pattern unequivocally confirms the formation of a single-phase fluorite-structured Tm and Er-doped CeO2\mathrm{CeO}_{2} as shown in Figure 1a and Figure S4. In Figure 1a, the diffraction peaks observed at ∼33.06∘\sim33.06^{\circ} and ∼69.42∘\sim69.42^{\circ} correspond to the (002) and (004) reflections of Tm-doped CeO2\mathrm{CeO}_{2}, respectively. This yielded an average out-of-plane lattice constant for film of ∼5.405\sim5.405 Å. Based on the cubic lattice parameters of YSZ (∼5.14\sim5.14 Å) and the film (∼5.405\sim5.405 Å), the in-plane lattice mismatch is estimated to be ∼5.16%\sim5.16\%, indicating that the film experiences compressive strain when coherently grown on the YSZ substrate. No noticeable shift in the CeO2\mathrm{CeO}_{2} peak position is observed in any of the samples, as the ionic radii of Tm and Ce are close.

X-ray diffraction, rocking curve, and X-ray reflectivity measurements

Figure 1. (a) 2θ−ω2\theta-\omega spectrum of 10% Tm-doped CeO2\mathrm{CeO_2} (001) grown epitaxially on YSZ (001). (b) shows the Rocking Curve measured around (002) peaks of substrate (black color) and film (red color), and (c) shows X-ray reflectivity data of the film (black color) for thickness optimization along with fitting (red color).

The inset of Figure 1a highlights a magnified view around the (002) reflection of the film, revealing well-defined Kiessig (thickness) fringes. The presence of these interference fringes is indicative of coherent layer-by-layer growth and underscores the high structural quality of the film. The film thickness estimated from the fringe periodicity is ∼37\sim37 nm, in excellent agreement with values obtained from both XRR and RBS. To further evaluate crystalline quality, rocking curve (RC) measurements were performed around the (002) reflections of both the YSZ substrate and the Tm: CeO2\mathrm{CeO}_{2} film. The substrate exhibited a sharp RC with a full width at half maximum (FWHM) of ∼0.01∘\sim0.01^{\circ}, indicative of its excellent crystallinity. The RC of the film displayed a composite profile featuring a sharp component atop a broader base. This suggests a strained interface region within the initial few nanometers of the film, yielding a sharp RC peak (FWHM ∼0.04∘\sim0.04^{\circ}). Beyond a critical thickness, the film relaxes (due to large lattice mismatch), resulting in a broader RC component (FWHM ∼0.6∘\sim0.6^{\circ}), while maintaining its epitaxial orientation along the (001) direction. A similar observation was reported by Yezhou Shi et al. [39] in highly strained CeO2\mathrm{CeO}_{2} films grown on YSZ.

The XRR measurement and corresponding fitting results, shown in Figure 1c, further confirm a film thickness of ∼38 nm\sim38\ \mathrm{nm}, consistent with the value derived from HRXRD interference fringes. The XRR derived surface roughness was estimated to be ∼0.6 nm\sim0.6\ \mathrm{nm}, indicative of an atomically smooth film surface. This result was independently corroborated via atomic force microscopy (AFM), as shown in the S. I. (Figure S5), which yielded a comparable root mean square surface roughness of ∼0.5 nm\sim0.5\ \mathrm{nm}.

Figure S3 shows the 2θ−ω2\theta-\omega X-ray diffraction scan of the 10 at.% Tm-doped CeO2\mathrm{CeO_2} thin film grown on a Si (001) substrate. The film exhibits a strong preferential orientation along the (111) direction. Distinct diffraction peaks corresponding to the (111) and (222) planes are observed at ∼28.8∘\sim28.8^\circ and ∼59.7∘\sim59.7^\circ, respectively, yielding an average out-of-plane lattice parameter of ∼5.35 A˚\sim5.35\ \mathring{\mathrm{A}} for the Tm:CeO2\mathrm{CeO_2} film. The stabilization of the (111) orientation on Si (001) is likely governed by the lower surface energy of the CeO2\mathrm{CeO_2} (111) plane [40]. Considering the in-plane lattice constant of Si (∼5.431 A˚\sim5.431\ \mathring{\mathrm{A}}), the film exhibits an in-plane lattice mismatch of ∼−1.56%\sim-1.56\%, indicating tensile strain in the film. Rocking curve measurements of the CeO2\mathrm{CeO_2} (111) reflection show a broader FWHM of ∼4.2∘\sim4.2^\circ, whereas the Si (004) substrate peak exhibits a significantly narrower FWHM of ∼0.002∘\sim0.002^\circ. Structural analysis indicates that films grown on YSZ (001) substrates possess superior crystalline quality compared to those grown on Si (001). The use of Si (001) substrates in this study was primarily intended to independently verify the photoluminescence emission from the Tm:CeO2\mathrm{CeO_2} film, since YSZ substrates contain rare-earth Y ions that may exhibit optical transitions similar to Tm, whereas Si does not contribute to any such rare-earth-related emission.

Figure 2a and Figure 2b present the Rutherford backscattering (RBS) spectra and the corresponding elemental concentrations for a CeO2\mathrm{CeO}_{2} sample doped with 10 at.% Tm. The fitting of the RBS data confirms a Tm concentration of 10 at%, consistent with the intended Ce0.9Tm0.1O2\mathrm{Ce}_{0.9}\mathrm{Tm}_{0.1}\mathrm{O}_{2} stoichiometry based on the growth parameters. Figure 2c shows the random and channeled yield for the Ce0.9Tm0.1O2\mathrm{Ce}_{0.9}\mathrm{Tm}_{0.1}\mathrm{O}_{2}/YSZ(001) sample, showing a significant decrease in the ion channeling yield with a χmin⁡\chi_{\min} of ~ 5.49% and ~ 3.09% for Tm and Ce atoms, suggesting excellent crystallinity of the sample. It is worth noting that the YSZ substrate exhibited a reduced χmin⁡\chi_{\min}, although the value remained relatively high at approximately 26.99%. This increase in substrate χmin⁡\chi_{\min} is primarily attributed to beam dechanneling as it traverses the top Ce0.9Tm0.1O2\mathrm{Ce}_{0.9}\mathrm{Tm}_{0.1}\mathrm{O}_{2} layer. Such dechanneling is due to energy loss during interactions with near-surface atoms, and even minor disturbances in the beam’s path can cause its profile to spread as it penetrates deeper into the target. Figure 2d presents the angular yield curves recorded at various θ1\theta_{1} angles, revealing that the profiles for YSZ, Ce, and Tm are nearly identical, with their respective χmin⁡\chi_{\min} values all occurring at θ1=0∘\theta_{1} = 0^\circ. The Ψ1/2\Psi_{1/2} values were also closely matched and found to be 0.80° for Ce and 0.90° for Tm, indicating that Tm atoms are successfully occupying regular Ce lattice positions. While dechanneling caused the Ψ1/2\Psi_{1/2} for YSZ to differ slightly, around 0.56°, the centroid of the angle still aligns with those of Ce and Tm, implying good lattice matching between the YSZ substrate and the deposited Ce0.9Tm0.1O2\mathrm{Ce}_{0.9}\mathrm{Tm}_{0.1}\mathrm{O}_{2} film. Using the χmin⁡\chi_{\min} values derived from Figure 2d, the substitutional fraction, fsf_{\mathrm{s}}, for Tm atoms was calculated to be ~ 98.22%, indicating that most Tm atoms are incorporated at the regular Ce lattice sites.

Experimental and simulated RBS spectra, areal density and atomic concentration table, channeling spectra, and angular yield curves

Figure 2. (a) Experimental and simulated RBS spectrum of Ce0.9Tm0.1O2\mathrm{Ce}_{0.9}\mathrm{Tm}_{0.1}\mathrm{O}_{2}/YSZ sample showing individual contributions from the Ce, O, and Tm species. (b) The areal density and atomic concentration of the Ce, O, and Tm species derived from the RBS results. (c) RBS spectra in random and channeling orientation showing a comparable and significant drop in the Ce (χmin⁡=5.49%\chi_{\min}=5.49\%) and Tm (χmin⁡=3.09%\chi_{\min}=3.09\%) yield, indicating excellent crystallinity of the Ce0.9Tm0.1O2\mathrm{Ce}_{0.9}\mathrm{Tm}_{0.1}\mathrm{O}_{2} layer. (Inset highlights the Tm signal in the spectrum) (d) Angular yield curves for YSZ, Tm, and Ce obtained at different tilt angles (θ1\theta_{1}) from the normal incidence. The angular curves show that the χmin⁡\chi_{\min} for both Ce and Tm occur at θ1=0∘\theta_{1}=0^\circ, with closely aligned profiles. The Ψ1/2\Psi_{1/2} values for Ce and Tm are 0.80∘0.80^\circ and 0.90∘0.90^\circ, respectively, and a calculated substitutional fraction (fsf_{s}) for Tm is 98.22%98.22\%, supporting the conclusion that Tm atoms are effectively substituted into Ce lattice sites. (Note: Slight discrepancies in χmin⁡\chi_{\min} between Figures 2c and 2d may arise from factors such as damage accumulation from the He+\mathrm{He}^{+} beam or minor positioning errors from the goniometer.)

Further verification of Tm dopant incorporation into the CeO2\mathrm{CeO}_{2} thin film was obtained via high-resolution STEM analysis, wherein the atomic structure of the lattice is directly imaged. Figure 3a presents a low-magnification cross-sectional STEM-HAADF image of the 10 at. % Tm doped CeO2\mathrm{CeO}_{2} film along [100] zone axis. The dark region within the CeO2\mathrm{CeO}_{2} film arises from thickness variations introduced during FIB thinning, rather than from intrinsic defects, and does not affect the evident single-crystalline quality of the film. Figure 3b shows a high-magnification STEM-HAADF image of the area highlighted in red in Figure 3a. Corresponding EDS elemental maps of Ce, O, and Tm are displayed in Figure 3c-Figure 3e, respectively. EDS maps of Ce and O show their respective atomic lattices, while the map of Tm confirms homogeneous substitutional doping throughout the CeO2\mathrm{CeO}_{2} lattice. The STEM results align well with RBS and XRR measurements, which estimate the film thickness at approximately 35 nm.

STEM results of Ce$_{0.9}$Tm$_{0.1}$O$_2$/YSZ thin film

Figure 3. STEM results of Ce0.9_{0.9}Tm0.1_{0.1}O2_2/YSZ thin film. (a) Low magnification STEM-HAADF image of cross-sectional Ce0.9_{0.9}Tm0.1_{0.1}O2_2/YSZ thin film. (b) High-magnification STEM-HAADF image of the red-highlighted region in (a). (c) EDS mapping of Ce L edge signal. (d) EDS mapping of O K edge signal. (e) EDS mapping of Tm M edge signal.

AtomAreal Density (×1015\times10^{15} atoms/cm2^{2})Atomic Concentration
Ce649.500.300
O1444.060.667
Tm71.440.033
Total2165Total = 1

Table b.

Optical Characterization

Figure 4a presents the NIR PL spectra obtained from a CeO2_2(200nm)/Ce0.99_{0.99}Tm0.01_{0.01}O2_2(150nm)/CeO2_2(200nm) grown on both YSZ (001) and Si (001) substrates under optimal conditions. The spectra were recorded under an excitation wavelength of 355 nm. Cerium oxide (CeO2_2) is a wide-bandgap semiconductor with an optical bandgap of approximately 3.2 eV [41], corresponding to an excitation wavelength near 380 nm and hence the excitation wavelength lies well above the bandgap. The NIR emission lines can be attributed to radiative transitions within the Tm3+^{3+} ion. The prominent emission at ~793 nm arises from the 3H4→3H6^{3}H_{4}\rightarrow{}^{3}H_{6} transition, which shows the highest intensity under 355 nm excitation. A comparably strong band near 808 nm is also observed; we attribute this feature to crystal-field induced Stark splitting within the Tm3+^{3+} manifolds rather than assigning it to a distinct electronic transition. The excitation mechanism has been understood as follows: photoexcitation at 355 nm promotes electrons from the Oxygen 2p valence band to the Ce 4f conduction states, forming a charge transfer state. Energy is then non-radiatively transferred from this charge transfer state to the 1G4^{1}G_{4} level of Tm3+^{3+}, followed by radiative relaxation through intra-4f transitions [42]. To definitively attribute the observed emission to the doped films rather than substrate contributions, additional PL measurements were performed on substrates without films and pure CeO2_2 films which showed no intrinsic emission in this spectral range shown as shown in the S.I. (Figure S6-S9).

Temperature-dependent photoluminescence spectra, photoluminescence excitation map, and up-conversion emission

Figure 4. (a) Temperature-dependent PL spectra of 1 at.% Tm3+\mathrm{Tm}^{3+}:CeO2\mathrm{CeO}_{2}/Si film excited at 355 nm, showing the thermal quenching behavior of the 3H4→3H6{}^{3}\mathrm{H}_{4} \to{}^{3}\mathrm{H}_{6} transition near 800 nm. (b) Photoluminescence (PL) spectra of 1 at.% Tm3+\mathrm{Tm}^{3+}:CeO2\mathrm{CeO}_{2} films grown on YSZ(001) (blue) and Si(001) (red) substrates with a 355 nm laser. The inset (identical in both PL panels) illustrates the Tm3+\mathrm{Tm}^{3+} energy levels involved in the excitation and emission processes. (c) Photoluminescence excitation (PLE) map of 1 at.% Tm3+\mathrm{Tm}^{3+}:CeO2\mathrm{CeO}_{2}/Si film obtained by scanning the excitation laser across the 3H4→3H6{}^{3}\mathrm{H}_{4} \to{}^{3}\mathrm{H}_{6} transition region while monitoring longer-wavelength emissions. The colormap is intentionally saturated to highlight Tm3+\mathrm{Tm}^{3+} emission features. To enhance visibility of weaker spectral features at longer emission wavelengths, the signal on the right side of the map (λ>1350\lambda> 1350 nm) is multiplied by a factor of 3. A vertical dashed line indicates the boundary where this scaling is applied. (d) Up-conversion emission from Tm3+\mathrm{Tm}^{3+} ions in CeO2\mathrm{CeO}_{2} under near-infrared excitation: a pulsed laser is tuned from 1170 nm to 1250 nm, and visible/near-infrared emission is recorded. A strong up-conversion response is observed when the excitation is resonant with the transition near 1210 nm.

A comparison between the room-temperature and low-temperature PL spectra (Figure 4b) reveals that cooling significantly sharpens the emission lines and enhances their relative intensity contrast. At 4 K, the fine spectral structure around 793–810 nm becomes clearly resolved, indicating reduced phonon broadening and enhanced population stability of the Stark sublevels within the 3H4→3H6{}^{3}\mathrm{H}_{4} \to{}^{3}\mathrm{H}_{6} transition manifold [27]. In contrast, at room temperature, phonon-assisted relaxation processes lead to broader and partially merged emission peaks. This temperature-dependent evolution highlights the role of lattice vibrations in modulating the crystal-field splitting and line broadening of Tm3+\mathrm{Tm}^{3+} emission in the CeO2\mathrm{CeO}_{2} host.

The energy levels within the 3H4{}^{3}\mathrm{H}_{4} manifold of Tm3+\mathrm{Tm}^{3+} are weakly split due to the crystal-field effect originating from the cubic fluorite structure of CeO2\mathrm{CeO}_{2}, in which Tm3+\mathrm{Tm}^{3+} ions occupy highly symmetric lattice sites. Given the total angular-momentum quantum number J=4J = 4, the 3H4{}^{3}\mathrm{H}_{4} energy level can split into a maximum of 2J+1=92J + 1 = 9 Stark sublevels. However, the PL spectra reveal the presence of five distinct emission peaks, each corresponding to a different energy level.

Figure 4(c) presents the two-dimensional photoluminescence (PL) excitation map of the Tm3+^{3+}:CeO2_2/Si film recorded at 4 K, where the excitation wavelength was systematically tuned while monitoring emission in the infrared region. Two intense and persistent emission bands centered at approximately ∼\sim1107 nm and ∼\sim1168 nm are observed across all excitation wavelengths, indicating transitions that are efficiently populated under various excitation conditions. In contrast, a distinct set of six weaker emission peaks at ∼\sim1205 nm, ∼\sim1210 nm, ∼\sim1406 nm, ∼\sim1464 nm, ∼\sim1492 nm, and ∼\sim1542 nm emerges only when the excitation wavelength lies within the narrow range of ∼\sim793−-796 nm. This resonant behavior demonstrates that these infrared transitions are selectively driven through excitation of the 3H4^{3}H_{4} manifold of Tm3+^{3+} ions, corresponding to the 3H6→3H4^{3}H_{6} \to{}^{3}H_{4} absorption around ∼\sim793 nm. Based on their spectral positions, the peaks at ∼\sim1205 nm and ∼\sim1210 nm are attributed to the 3H5→3H6^{3}H_{5} \to{}^{3}H_{6} transition, while the ∼\sim1464 nm feature is assigned to the 3H4→3F4^{3}H_{4} \to{}^{3}F_{4} transition. The remaining bands at ∼\sim1406 nm, ∼\sim1492 nm, and ∼\sim1542 nm are interpreted as satellite Stark components associated with crystal-field splitting of these manifolds. Notably, excitation near ∼\sim808 nm, despite being in proximity to a strong PL band, does not produce additional infrared features beyond the two dominant peaks near ∼\sim1150 nm.

To further probe excitation-dependent emission behavior, up-conversion photoluminescence measurements were performed by tuning the excitation wavelength in the infrared range from 1135 nm to 1250 nm while monitoring emission in the visible and near-infrared regions, as shown in Figure 4(d). Emission features near 800 nm appear when the excitation wavelength is tuned around ∼\sim1210 nm, along with another strong up-conversion intensity for excitation near 1150 nm. While the precise excitation mechanism remains under investigation, the resonant nature of the up-conversion signal at ∼\sim1210 nm points to Tm3+^{3+} ion’s role in the up-conversion process and the existence of long-lived excited states of the Tm ions.

Time-resolved photoluminescence lifetime measurements were performed using a time-correlated single-photon counting approach. The sample emission was collected using the optical setup and directed to a superconducting nanowire single-photon detector from Single Quantum. The detector output was connected to a Swabian Instruments Time Tagger, which recorded photon arrival times with high temporal resolution. A pulsed excitation laser was used to excite the sample. The repetition rate of the excitation pulses was controlled using an acousto-optic modulator placed in the beam path. The AOM allowed precise adjustment of the effective pulse repetition rate by gating the laser pulses, which ensured that the interval between excitation pulses was longer than the measured decay time. This prevented pulse overlap and enabled accurate extraction of the photoluminescence lifetime from the recorded photon arrival histogram.

Under excitation at 1210 nm, an up-conversion process populates the 3H4{}^{3}\mathrm{H}_{4} level, leading to emission in the ~ 800 nm region. This emission is characterized by two distinct peaks at ~ 793 nm and ~ 808 nm. The emission was isolated using a 700 nm long-pass filter and an 850 nm short-pass filter. The resulting decay trace (Figure 5a) follows a bi-exponential decay profile, yielding a fast component of τ1\tau_{1} ~ 3.81 μ\mus and a slower component of τ2\tau_{2} ~ 14.77 μ\mus. This two-component decay is likely due to the different lifetimes of the two transitions at ~ 795 nm and ~ 808 nm. We found these lifetimes to be independent of the dopant concentration from 0.01-1%, indicating possible non-radiative processes.

Lifetimes measurements on Tm3+ transitions

Figure 5. Lifetimes measurements on Tm3+^{3+} transitions, (a) for 3H4→3H6{}^{3}\mathrm{H}_{4} \rightarrow{}^{3}\mathrm{H}_{6} excited using the up-conversion process using a 1210 nm laser. The bi-exponential decay curve is likely due to the mixing of two crystal-field sublevels at ~ 793 nm and ~ 808 nm. (b) Decay curve for 3H5→3H6{}^{3}\mathrm{H}_{5} \rightarrow{}^{3}\mathrm{H}_{6} transition excited using a 795 nm laser resonant with 3H4→3H6{}^{3}\mathrm{H}_{4} \rightarrow{}^{3}\mathrm{H}_{6} transition.

The lifetime of the 1210 nm transition (3H5→3H6{}^{3}\mathrm{H}_{5} \rightarrow{}^{3}\mathrm{H}_{6}) was measured directly by exciting it through the 3H4→3H6{}^{3}\mathrm{H}_{4} \rightarrow{}^{3}\mathrm{H}_{6} transition. This emission was isolated using a specialized spectral filtering setup, providing a narrow ~ 3 nm bandwidth to ensure the purity of the signal from the 1210 nm level. As shown in Figure 5b, the 1210 nm decay is well-described by a single-exponential model with a lifetime of τ1\tau_{1} ~ 68.81 μ\mus. This significantly longer lifetime roughly 5 to 20 times longer than the 800 nm decay components confirms that the 1210 nm level (3H5{}^{3}\mathrm{H}_{5}) serves as a stable intermediate reservoir. Its long-lived nature is essential for the up-conversion process, as it allows sufficient time for the second excitation step required to reach the 3H4{}^{3}\mathrm{H}_{4} state.

To more clearly elucidate the origin of the short Tm lifetimes in the CeO2_{2} host, we compare these lifetimes with those of Er-doped CeO2_{2} films grown under identical conditions. The photoluminescence properties of the CeO2_{2}(200nm)/Ce0.99_{0.99}Er0.01_{0.01}O2_{2}(150nm)/CeO2_{2}(200nm) film grown on YSZ (001) was investigated under 1418 nm excitation. The emission spectrum, shown in Figure 6a, exhibits two distinct peaks centered at ~ 1530 nm and ~ 1535 nm, corresponding to transitions from the Stark-split 4I13/2{}^{4}\mathrm{I}_{13/2} excited state to the 4I15/2{}^{4}\mathrm{I}_{15/2} ground state manifold. To isolate these features, the emission was passed through the same high-resolution spectral filtering setup used for the 1210 nm Tm3+^{3+} measurements, utilizing a narrow 3 nm bandwidth to ensure the purity of the individual transition signals.

Photoluminescence spectrum and decay dynamics of 1 at.% Er:CeO$_2$ films

Figure 6. Photoluminescence and decay dynamics of 1 at.% Er:CeO2_2 films grown on YSZ. (a) Emission spectrum under 1418 nm excitation, showing primary peaks at ~ 1530 nm and ~ 1535 nm. (b) Single-exponential decay fit for the 1534 nm transition, yielding τ1∼5.32\tau_1 \sim5.32 ms. (c) Single-exponential decay fit for the 1530 nm transition, yielding τ1∼2.94\tau_1 \sim2.94 ms. Spectral isolation for these measurements was achieved using the same filtering setup employed for the 1210 nm Tm3+^{3+} measurements, incorporating a narrow 3 nm spectral selection bandwidth.

Time-resolved measurements revealed distinct decay dynamics for these transitions, presented in Figure 6 (b & Figure 6c). The 1534 nm emission exhibits a single-exponential decay with a lifetime of τ1∼5.32\tau_1 \sim5.32 ms, and the 1530 nm emission exhibits a faster decay rate, characterized by a lifetime of τ1∼2.94\tau_1 \sim2.94 ms. The observed variation in lifetimes between the 1530 nm and 1534 nm peaks indicates that these transitions originate from different Stark levels within the 4I13/2{}^{4}I_{13/2} manifold, which are likely influenced by local site symmetry.

The relatively longer lifetimes observed for 1 at.% Er in the CeO2_2 host are noteworthy, as comparable lifetimes have previously been reported for MBE grown Er-doped CeO2_2 films with concentrations < 0.01%. This behavior may be associated with a reduced density of oxygen vacancies in the present films, which can influence the nonradiative recombination pathways and thereby impact the excited-state lifetime.

To identify whether a host-specific electronic-structure mechanism contributes to the difference in the lifetimes of Tm and Er, spin-polarized DFT+U calculations were performed by substituting a single Ce with Tm or Er in a 2×2×22 \times2 \times2 fluorite supercell (96 atoms, ~ 3% doping), and the geometry was fully relaxed. The atom-projected density of states (PDOS) is shown in Figure 7, with contributions from the rare-earth 4f4f (blue), O 2p2p (red), and Ce 4f4f (green) orbitals resolved separately. The valence band maximum (VBM) of pristine CeO2_2 is set to 0 eV.

Spin-polarized density of states for Tm-doped and Er-doped CeO₂

Figure 7. Spin-polarized density of states for (a) various elements in Tm-Doped CeO₂, (b) Tm 4f4f orbital in Tm-Doped CeO₂, (c) O 2p2p orbital in Tm-Doped CeO₂, (d) various elements in Er-Doped CeO₂, (e) Er 4f4f orbital in Er-Doped CeO₂, and (f) O 2p2p orbital in Er -Doped CeO₂. The top of the valence band maximum (VBM) from pristine of CeO₂ is set to 0 eV.

For the Er-doped system (Figure 7, bottom), the Er 4f4f manifold lies deep within the valence band, with the occupied states centered between approximately −8 and −4 eV below the VBM. At these energies the O 2p2p band, which carries its principal spectral weight between −4 and 0 eV, has negligible density. Because the Er 4f4f and O 2p2p states are not co-energetic, they do not mix: the 4f4f peaks remain narrow and atomic-like, preserving the standard picture of 4f4f electrons shielded by the closed 5s25p65s^{2}5p^{6} subshell [43, 44]. No unoccupied Er-derived states appear near the VBM or within the host band gap.

The Tm-doped system (Figure 7, top) presents a different electronic structure. The occupied Tm 4f4f manifold sits at higher energies within the valence band relative to Er, with spin-up states between −6 and −4 eV. Several spin-down 4f4f components extend above −4 eV, entering the energy window where the O 2p2p band carries substantial spectral weight. Where the Tm 4f4f and O 2p2p states become co-energetic, the sharp atomic-like peaks characteristic of isolated 4f4f levels give way to broadened features, revealing the covalent hybridization between the dopant and host states. In addition, an unoccupied spin-down state appears just above the VBM, and real-space charge density visualization shows its wavefunction extends mainly onto neighboring O sites with mixed Tm 4f4f + O 2p2p character (Figure SI).

The site-projected magnetic moments also provide a measure of the hybridization contrast. For Er3+^{3+} (4f114f^{11}), the Er site carries 2.97 μB\mu_{\mathrm{B}} with negligible spin density on the neighboring oxygen sublattice, confirming that the 4f4f spin density remains fully localized on the rare-earth site. For Tm3+^{3+} (4f124f^{12}), the Tm site carries 2 μB\mu_{\mathrm{B}} (the expected Hund value for 12 electrons in the 4f4f shell) while ∼1 μB\sim1\,\mu_{\mathrm{B}} of spin density resides on the neighboring oxygen atoms. This delocalization of one full Bohr magneton onto the sublattice directly quantifies the covalent Tm 4f4f–O 2p2p mixing and confirms that the 5s35p65s^{3}5p^{6} shielding that normally isolates 4f4f electrons from the host is weakened for Tm in CeO2_2.

Collectively, these rare-earth-doped systems highlight the critical role of the host lattice in mediating radiative and non-radiative relaxation processes. By contrasting the long-lived nature of the Er metastable states with the complex, fast-decaying up conversion channels of Tm, we establish a comprehensive experimental foundation for understanding dopant-host interactions. This data sets the stage for future theoretical modeling to quantify the crystal field parameters and electronic density of states that govern these distinct lifetime signatures.

Conclusions

In summary, we have investigated CeO2_2 as a host system for quantum emitters with a focus on rare-earth ions. We have demonstrated epitaxial growth of crystalline Tm and Er doped CeO2_2 films on YSZ (001), and Si (001) substrates. We have observed efficient photoluminescence from Tm ions, along with an up-conversion signal. Short excited-state lifetimes are observed in Tm-doped CeO2_2 films, whereas comparatively longer lifetimes are measured in Er-doped CeO2_2 films. This difference arises from the distinct interaction between the rare-earth dopants and the CeO2_2 host lattice, particularly through the hybridization of RE 4f4f orbitals with O 2p2p states, as corroborated by first-principles DFT calculations. These findings provide important insight into the role of dopant-host electronic interactions and suggest a viable strategy for selecting appropriate rare-earth dopants as quantum sources in the non-magnetic CeO2_2 host matrix for potential quantum applications. Another important result to be investigated further may be the role of oxygen vacancies in reducing the PL lifetimes which may explain the difference in the dopant density dependence of the lifetimes in MBE and PLD grown films.

Acknowledgements

This material is based upon work supported by the U.S. Department of Energy, Office of Science, Office of Basic Energy Sciences under Award Number E-SC0025486. This award supported the thin film growth, X-ray-based characterization, and photoluminescence measurements. We gratefully acknowledge fruitful discussions with Mahdi Hosseini.

References

  1. [1]Jelezko, F. and J. Wrachtrup, Single defect centres in diamond: A review. physica status solidi (a), 2006. 203(13): p. 3207-3225.DOI
  2. [2]Childress, L. and R. Hanson, Diamond NV centers for quantum computing and quantum networks. MRS Bulletin, 2013. 38(2): p. 134-138.DOI
  3. [3]Hepp, C., et al., Electronic Structure of the Silicon Vacancy Color Center in Diamond. Physical Review Letters, 2014. 112(3): p. 036405.pubmed.ncbi.nlm.nih.gov/24484153
  4. [4]Sukachev, D.D., et al., Silicon-Vacancy Spin Qubit in Diamond: A Quantum Memory Exceeding 10 ms with Single-Shot State Readout. Physical Review Letters, 2017. 119(22): p. 223602.DOI
  5. [5]Evans, R.E., et al., Photon-mediated interactions between quantum emitters in a diamond nanocavity. Science, 2018. 362(6415): p. 662-665.DOI
  6. [6]Koehl, W.F., et al., Room temperature coherent control of defect spin qubits in silicon carbide. Nature, 2011. 479(7371): p. 84-87.DOI
  7. [7]Christle, D.J., et al., Isolated Spin Qubits in SiC with a High-Fidelity Infrared Spin-to-Photon Interface. Physical Review X, 2017. 7(2): p. 021046.
  8. [8]Esmann, M., S.C. Wein, and C. Anton-Solanas, Solid-State Single-Photon Sources: Recent Advances for Novel Quantum Materials. Advanced Functional Materials, 2024. 34(30): p. 2315936.DOI
  9. [9]Graf, F.R., et al., Photon-echo attenuation by dynamical processes in rare-earth-ion-doped crystals. Physical Review B, 1998. 58(9): p. 5462-5478.
  10. [10]Seo, H., et al., Designing defect-based qubit candidates in wide-gap binary semiconductors for solid-state quantum technologies. Physical Review Materials, 2017. 1(7): p. 075002.DOI
  11. [11]Zhang, G., et al., Material platforms for defect qubits and single-photon emitters. Applied Physics Reviews, 2020. 7(3).arxiv.org/abs/2008.06458
  12. [12]Somjit, V., et al., An NV− center in magnesium oxide as a spin qubit for hybrid quantum technologies. npj Computational Materials, 2025. 11(1): p. 74.arxiv.org/abs/2409.00246
  13. [13]Johnson, J.M., et al., Unusual Formation of Point-Defect Complexes in the Ultrawide-Band-Gap Semiconductor $\ensuremath{\beta}\text{\ensuremath{-}}\mathrm{Ga}_{2}\mathrm{O}_{3}$. Physical Review X, 2019. 9(4): p. 041027.
  14. [14]Bertaina, S., et al., Rare-earth solid-state qubits. Nature Nanotechnology, 2007. 2(1): p. 39-42.
  15. [15]O’Brien, C., et al., Interfacing Superconducting Qubits and Telecom Photons via a Rare-Earth-Doped Crystal. Physical Review Letters, 2014. 113(6): p. 063603.DOI
  16. [16]Thiel, C.W., T. Böttger, and R.L. Cone, Rare-earth-doped materials for applications in quantum information storage and signal processing. Journal of Luminescence, 2011. 131(3): p. 353-361.DOI
  17. [17]Ortu, A., et al., Storage of photonic time-bin qubits for up to 20 ms in a rare-earth doped crystal. npj Quantum Information, 2022. 8(1): p. 29.DOI
  18. [18]Böttger, T., et al., Spectroscopy and dynamics of $\mathrm{Er}^{3+}:\mathrm{Y}_{2}\mathrm{Si}_{2}\mathrm{O}_{5}$ at $1.5\phantom{\rule{0.3em}{0ex}}\ensuremath{\mu}\mathrm{m}$. Physical Review B, 2006. 74(7): p. 075107.
  19. [19]Williams, D.K., et al., Preparation and Fluorescence Spectroscopy of Bulk Monoclinic Eu3+:Y2O3 and Comparison to Eu3+:Y2O3 Nanocrystals. The Journal of Physical Chemistry B, 1998. 102(6): p. 916-920.DOI
  20. [20]Serrano, D., et al., Coherent optical and spin spectroscopy of nanoscale $\mathrm{Pr}^{3+}:\phantom{\rule{0.28em}{0ex}}\mathrm{Y}_{2}\mathrm{O}_{3}$. Physical Review B, 2019. 100(14): p. 144304.
  21. [21]Stouwdаm, J.W. and F.C.J.M. van Veggel, Near-infrared Emission of Redisperisible Er3+, Nd3+, and Ho3+ Doped LaF3 Nanoparticles. Nano Letters, 2002. 2(7): p. 733-737.
  22. [22]de Leon, N.P., et al., Materials challenges and opportunities for quantum computing hardware. Science, 2021. 372(6539): p. eabb2823.DOI
  23. [23]Burkard, G., et al., Semiconductor spin qubits. Reviews of Modern Physics, 2023. 95(2): p. 025003.DOI
  24. [24]Kanai, S., et al., Generalized scaling of spin qubit coherence in over 12,000 host materials. Proceedings of the National Academy of Sciences, 2022. 119(15): p. e2121808119.
  25. [25]Inaba, T., et al., Epitaxial growth and optical properties of Er-doped CeO2 on Si(111). Optical Materials Express, 2018. 8(9): p. 2843-2849.DOI
  26. [26]Grant, G.D., et al., Optical and microstructural characterization of Er3+ doped epitaxial cerium oxide on silicon. APL Materials, 2024. 12(2).arxiv.org/abs/2309.16644
  27. [27]Kramida, A., Ralchenko, Yu., Reader, J., and NIST ASD Team (2024), NIST Atomic Spectra Database, G. National Institute of Standards and Technology, Editor. 2024.
  28. [28]Parashar, M., et al., Probing elemental diffusion and radiation tolerance of perovskite solar cells via non-destructive Rutherford backscattering spectrometry. APL Energy, 2024. 2(1).DOI
  29. [29]Kresse, G. and J. Hafner, Ab initio molecular dynamics for liquid metals. Physical Review B, 1993. 47(1): p. 558-561.
  30. [30]Kresse, G. and D. Joubert, From ultrasoft pseudopotentials to the projector augmented-wave method. Physical Review B, 1999. 59(3): p. 1758-1775.DOI
  31. [31]Blöchl, P.E., Projector augmented-wave method. Physical Review B, 1994. 50(24): p. 17953-17979.pubmed.ncbi.nlm.nih.gov/9976227
  32. [32]Perdew, J.P., K. Burke, and M. Ernzerhof, Generalized Gradient Approximation Made Simple. Physical Review Letters, 1996. 77(18): p. 3865-3868.pubmed.ncbi.nlm.nih.gov/10062328
  33. [33]Dudarev, S.L., et al., Electron-energy-loss spectra and the structural stability of nickel oxide: An LSDA+U study. Physical Review B, 1998. 57(3): p. 1505-1509.DOI
  34. [34]Castleton, C.W.M., J. Kullgren, and K. Hermansson, Tuning LDA+U for electron localization and structure at oxygen vacancies in ceria. The Journal of Chemical Physics, 2007. 127(24).DOI
  35. [35]Larson, P., et al., Electronic structure of rare-earth nitrides using the $\mathrm{LSDA}+U$ approach: Importance of allowing the $4f$ orbitals to break the cubic crystal symmetry. Physical Review B, 2007. 75(4): p. 045114.DOI
  36. [36]Sanna, S., et al., Rare-earth defect pairs in GaN: $\text{LDA}+U$ calculations. Physical Review B, 2009. 80(10): p. 104120.DOI
  37. [37]Denawi, H., P. Karamanis, and M. Rérat, Electronic and magnetic properties of yttria-stabilized zirconia (6.7 mol% in Y2O3) doped with Er3+ ions from first-principle computations. Journal of Materials Science, 2021. 56(13): p. 8014-8023.DOI
  38. [38]Monkhorst, H.J. and J.D. Pack, Special points for Brillouin-zone integrations. Physical Review B, 1976. 13(12): p. 5188-5192.DOI
  39. [39]Shi, Y., et al., Growth of Highly Strained CeO2 Ultrathin Films. ACS Nano, 2016. 10(11): p. 9938-9947.pubmed.ncbi.nlm.nih.gov/27934073
  40. [40]Skorodumova, N.V., M. Baudin, and K. Hermansson, Surface properties of $\{\mathrm{CeO}\}_{2}$ from first principles. Physical Review B, 2004. 69(7): p. 075401.
  41. [41]Phoka, S., et al., Synthesis, structural and optical properties of CeO2 nanoparticles synthesized by a simple polyvinyl pyrrolidone (PVP) solution route. Materials Chemistry and Physics, 2009. 115(1): p. 423-428.DOI
  42. [42]Chrysochoos, J. and A.H. Qusti, Cross-relaxation of the 1G4 state of Tm3+ in POCl3:SnCl4. Journal of the Less Common Metals, 1989. 148(1): p. 253-257.DOI
  43. [43]Dieke, G.H. and H.M. Crosswhite, The Spectra of the Doubly and Triply Ionized Rare Earths. Applied Optics, 1963. 2(7): p. 675-686.DOI
  44. [44]Carnall, W.T., et al., A systematic analysis of the spectra of the lanthanides doped into single crystal LaF3. The Journal of Chemical Physics, 1989. 90(7): p. 3443-3457.DOI

Paper details

vlnc:W_uc67vu8f
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents