Abstract

Spin waves in magnetic materials are promising information carriers for future computing technologies due to their ultra-low energy dissipation and long coherence length. Antiferromagnets are strong candidate materials due, in part, to their stability to external fields and larger group velocities. Multiferroic aniferromagnets, such as BiFeO3_3 (BFO), have an additional degree of freedom stemming from magnetoelectric coupling, allowing for control of the magnetic structure, and thus spin waves, with electric field. Unfortunately, spin-wave propagation in BFO is not well understood due to the complexity of the magnetic structure. In this work, we explore long-range spin transport within an epitaxially engineered, electrically tunable, one-dimensional (1D) magnonic crystal. We discover a striking anisotropy in the spin transport parallel and perpendicular to the 1D crystal axis. Multiscale theory and simulation suggests that this preferential magnon conduction emerges from a combination of a population imbalance in its dispersion, as well as anisotropic structural scattering. This work provides a pathway to electrically-reconfigurable magnonic crystals in antiferromagnets.

Introduction

In the push to design next-generation memory and logic technologies that utilize spin, antiferromagnets are particularly attractive due to their stability against external magnetic fields and large magnon propagation group velocities [1, 2, 3]. One pathway to control magnon transport is by lithographically patterning periodic structures to create a so-called magnonic crystal [4, 5, 6, 7, 8, 9]. A disadvantage of these extrinsic structures, however, is that the periodic structure is fixed. Their utility would be enhanced if they were tunable or reconfigurable [10]. To this end, the interaction of spin waves with magnetic domain walls has been studied in ferromagnets [11, 12, 13, 14], since domain walls can be written and moved using current-induced effects [15, 16, 17]. In order to design and create a magnonic crystal, however, periodic arrays of domain walls would need to be created. Here, we investigate magnon-transport behavior in a room temperature magnetoelectric with an intrinsically periodic, one-dimensional-cycloidal magnetic structure. Because this spin-texture-lattice is intrinsic to a multiferroic material and governed by the directionality of the polarization, we demonstrate that electric fields can be used to manipulate the magnonic crystal and control transport behavior.

For this study, BiFeO3\mathrm{BiFeO}_3 (BFO) is used as a model system. BFO is a well-studied antiferromagnetic oxide due to the strong coupling between polarization (ferroelectricity) and magnetic (antiferromagnetism) order at room temperature, enabling all-electric-field control of magnetization [18, 19, 20, 21]. Due to this interaction, BFO has garnered interest in the field of spintronics, especially with recent observations showing that electric-field control of spin transport is possible. [22]. The fundamental magnetic order in BFO consists of G-type antiferromagnetism, which is modulated by broken symmetries stemming from the polarization and from antiferrodistortive FeO6\mathrm{FeO}_6 octahedral rotations. These phenomena give rise to a long-period (λ≈65\lambda\approx65 nm) spin cycloid [23]. In its equilibrium structure, this antiferromagnetic cycloid propagates along three symmetry-equivalent directions: k1k_1 ([1ˉ10][\bar{1}10]), k2k_2 ([1ˉ01][\bar{1}01]), and k3k_3 ([01ˉ1][0\bar{1}1]), when polarization, PP, is parallel to [111][111] [24], with Fe atomic moments rotating in the (112ˉ)(11\bar{2}), (12ˉ1)(1\bar{2}1), and (2ˉ11)(\bar{2}11), for k1k_1, k2k_2, k3k_3, respectively [25]. The antiferromagnetic cycloid is then further perturbed by the Dzyaloshinskii-Moriya interaction (DMI), canting the moments slightly out of the P−kP-k plane and resulting in a spin-density wave (MM) with the same period as the antiferromagnetic cycloid [26, 27]. This intrinsic, periodic magnetic structure in BFO can be modulated by an electric field, a capability attributed to its strong magnetoelectric coupling [28, 29]. Despite its fundamental nature, the behavior of spin propagation within such a complex spin structure remains not fully understood. This gap in knowledge suggests that the cycloid’s periodicity could have significant, yet unexplored, effects on magnon dispersion.

The intimate coupling between magnetic order and ferroelectric polarization in BFO allows for the use of its ferroelectric structure as a tool to design periodic magnetic lattices, facilitating spin-wave transport. Previous studies have shown that the ferroelectric domain structure of thin-film BFO can be controlled using electrostatics and the epitaxial strain arising from the lattice mismatch to the substrate [30], leading to quasi-ordered arrays of either 71∘71^\circ or 109∘109^\circ domains [31]. This directly influences the magnetic structure [32, 33]. Our current study demonstrates that by engineering these phenomena through the boundary conditions imposed by electrostatics and lattice-mismatch strain, we can effectively guide the ferroelectric domain structure to modulate the spin cycloid. This manipulation results in the creation of a long-range, intrinsic, quasi-1D-ordered lattice. Such a lattice structure creates a gap in the magnon dispersion and introduces a significant spin-transport anisotropy, which is further tunable with an electric field.

1D ordered lattice

Figure 1. 1D ordered lattice. In the two BFO variants, the ferroelectric domains are arranged into ground states containing 71° (a) and 109° (b) ferroelastic domain walls. Insets depict the two types of domain walls and their corresponding polarizations in the BFO unit cell. In films deposited on DSO substrates, the cycloid prefers the k1k_1 variant, which results in a chevron-like pattern across the ferroelectric domains (c). For films on TSO, however, the domain structure allows selection of the other symmetry allowed axis, in this case k2k_2 (d). Corresponding Fourier transforms are shown as insets revealing the period and symmetry of the magnetic structures. (e) Zoom of the area shown in green, where the cycloid is unperturbed by the fine, 10–30 nm ferroelastic domain walls. (f) This occurs due to the symmetry of k2k_2 across the 109° domain wall, where the directionality of the cycloid is preserved with the fixed net polarization PnetP_{\mathrm{net}} imposed by the ferroelectric domains.

Designing the multiferroic structure

To control the ferroelectric and magnetic structure of BFO, we synthesize epitaxial thin films on both DyScO3_3 (DSO, ∼0.3%\sim0.3\% compressive strain) and TbScO3_3 (TSO, ∼0%\sim0\% strain) substrates (Methods). From X-ray diffraction studies (Extended data Figure S1), films are confirmed to be ∼100\sim100 nm thick and of excellent crystalline quality. In addition to slightly different epitaxial strain states from the choice of substrate, these systems are chosen to engineer films with different ferroelectric domain structures. These films host characteristic stripe-like 71° ferroelastic domains on DSO and 109° ferroelastic domains on TSO [34]. Piezoresponse force microscopy (PFM) images (Figure 1a,b) demonstrate the two-variant stripe patterns along [100][100]. The nanoscale magnetic structures of these different strain and domain configurations are then investigated in real space using scanning nitrogen-vacancy (NV) magnetometry (Methods) [24, 29, 33, 35].

Comparison of measurement schemes and non-local voltage measurements

Figure S1. Comparison of measurement schemes a,b PFM and schematics of three terminal device for magnon-driven non-local voltage without an external electric field. The non-local voltage detector is fixed at the center and current is injected left or right to create two different qq while PP remains invariant. c Plots showing nonlocal signal in different configurations, switching PP under constant qq and vice versa. In all four permutations, ΔV≈100 nV\Delta V \approx100\ \mathrm{nV} and the signs of the same states (e.g. P↓q↑P \downarrow q \uparrow) are consistent. This ±10 nV\pm10\ \mathrm{nV} signal may be due to the intrinsic device anisotropy, but should be mitigated when averaging across devices. d Power dependence of fixed PP variable qq measurements, showing the appropriate scaling and consistency of the sign.

In films deposited on DSO (Figure 1c), NV magnetometry shows a chevron-like magnetic texture of the stray magnetic field, revealing a k1k_1-oriented cycloid that switches direction with the change of the PP directions across the 71° ferroelastic domain walls. This is consistent with previous reports [29] and is a result of the magnetoelastic anisotropy from the substrate lattice mismatch [32, 35]. Strikingly, in the sample deposited on TSO (Figure 1d), only a single kk variant of the cycloid is observed, projected along [100][100]. The longer period of these oscillations indicates that this corresponds to a k2k_2, [101][101] axis of the cycloid, which is now preferred due to the lower magnetoelastic energy from the smaller epitaxial strain of TSO. Importantly, this variant of the cycloid even persists across the approximately 20-30 nm wide 109° ferroelectric domains and extends over long distances (up to at least 20 μ\mum). This results in the formation of a quasi-long-range, 1D magnonic crystal, as illustrated in (Figure 1e).

This propagation of the k2k_2 cycloid variant across ferroelectric domains can be understood through the symmetry of the 109° ferroelastic domain walls. Starting with the 71° domains in films on DSO substrates, the in-plane k1k_1 directions are strongly magnetoelastically preferred. At the ferroelectric domain walls, where polarization PP rotates from [1ˉ11][\bar{1}11] to [111][111], the cycloid wave vector directions must be shifted, for example, from [110][110] to [1ˉ10][\bar{1}10], to ensure the perpendicular relation k1⊥Pk_1 \perp P. This shift leads to a chevron-like pattern being favored as an equilibrium state. In contrast, in films on TSO substrates, the magnetoelastic energy is lowered, making the k2k_2 and k3k_3 variants closer in energy. Furthermore, considering the 109° domain walls in the films on TSO substrates, assuming k2k_2 is now an allowed direction, the propagation axis would not need to alter with the polarization change. This is because [101][101] is perpendicular to both [1ˉ11][\bar{1}11] and [111ˉ][11\bar{1}] (Figure 1f), making k2k_2 also a symmetry-favored equilibrium in this configuration. Consequently, k2k_2 emerges as the globally preferred equilibrium state, leading to a single cycloid variant that persists across the 109° ferroelastic domain walls, despite their ∼20-30 nm period [30].

Magnon transport

To test spin transport with respect to the directions defined by the quasi-1D spin-spiral lattice, we fabricated test structures that are schematically shown in Figure 2a. These structures consist of source and detector wires aligned both parallel and perpendicular to kk. The magnon-induced voltage signal in these structures is compared along multiple directions with respect to kk to show anisotropy, as well as in both the quasi-1D and chevron-like cycloid structures (Figure 1c). First, considering thermally excited magnons in a two-wire scheme, a current in the source wire is used to create a temperature gradient (∇T\nabla T) in the device, causing thermally excited spin waves to propagate q∥−∇Tq \parallel-\nabla T, where qq is the magnon propagation direction, via the spin Seebeck effect [22]. These magnons are then sensed in the detector wire through the inverse spin Hall effect (ISHE), which converts the spin current to a DC voltage, ΔVNL,2ω\Delta V_{NL,2\omega} [36, 37]. To preserve the ferroeletric domains, we performed this measurement again by reversing the directionality of the thermal transport with respect to the in-plane polarization (details in Supp. Note 1). Confirmation that the signal is magnetic in origin comes from testing with different detector materials. For example, changing the detector wire from Pt to W (with a larger, opposite-signed spin-Hall angle compared to Pt) reverses the sign of ΔVNL,2ω\Delta V_{\mathrm{NL},2\omega}. Similarly, moving to a material with a much larger spin-Hall angle, such as SrIrO3_3 (SIO) [38],

Spin wave anisotropy schematic and plots

Figure 2. Spin wave anisotropy. (a) Schematic of the sample geometry of the test structures ∥\parallel (θ=0∘\theta= 0^\circ) and ⊥\perp (θ=90∘\theta= 90^\circ) to kk. These structures give rise to different magnon conductivities due to the directionality of the cycloid. In the quasi-1-D lattice of 109∘109^\circ domains, (b), there is high conductivity along the ferromagnetically coupled direction, [010][010], and low conductivity along kk, [100][100]. Conversely, for the 71∘71^\circ domain scenario, (c), the cycloid, and thus the conductivity, display no distinct anisotropy between the θ=0∘\theta= 0^\circ and 90∘90^\circ directions. This reflects the magnetic cycloid’s interaction with both the 109∘109^\circ and 71∘71^\circ ferroelastic domain walls. In the case of 109∘109^\circ cycloid, viewed along the directions parallel to [010][010] (θ=0∘\theta= 0^\circ), d), or [100][100] (θ=90∘\theta= 90^\circ, e), the magnetic moments only deviate slightly across the ferroelectric domain walls, but cycle by 2π2\pi in the projected direction of k2k_2. In e, the 109∘109^\circ ferroelastic domain walls are shown along with the deviation of MM across the wall. In e, the antiferromagnetic Fe moments rotate in the k−Pk-P plane, along with the magnitude of MM traced by the green line. Unit cells are shown in an approximately 15:1 scale. The orientation of schematics d and e is viewed along the orthogonal directions shown in a.

proportionally increases the ISHE voltage.

In films featuring the quasi-1D ordered cycloid lattice, a strong anisotropy is observed with respect to directions q∥kq \parallel k and q⊥kq \perp k. We define θ\theta as the angle between qq and kk. Notably, the ISHE voltage signal, indicative of spin wave conductivity, is approximately three times larger when θ=90∘\theta= 90^\circ, aligning with the cycloid’s uniform direction. In contrast, samples with the alternating chevron-like structure, characterized by a net knet=∑k=0k_{\mathrm{net}} = \sum k = 0, exhibit minimal spin transport anisotropy (Figure 2c). Additionally, in the chevron-like samples, where locally θ=45∘\theta= 45^\circ, ΔVNL,2ω\Delta V_{\mathrm{NL},2\omega} lies between the values at θ=90∘\theta= 90^\circ and 0∘0^\circ seen in the 1D ordered system. This behavior can be initially understood by examining the nanoscopic magnetic spin structure within the cycloid as described schematically in Figure 2d,Figure 2e. In a line cut ⊥k\perp k, the spins are modulated by the presence of the 109° ferroelastic domain walls, but possess a persistent net magnetization component, illustrated in Figure 2e. In contrast, oriented parallel to kk, the spins rotate by a full 2π2\pi over the period of the cycloid (65 nm, Figure 2d). To further evaluate the physics associated with transport in the quasi-1D structure, we turn to both mesoscale phase-field simulations and model Hamiltonian calculations of spin transport ∥\parallel and ⊥k\perp k.

From phase-field simulations, we observe an anisotropy characterized by reduced spin-wave conductivity along the q∥kq \parallel k direction, compared to q⊥kq \perp k. Simulations are carried out by imposing a cycloidal magnetic ground state comparable to those observed experimentally and by initiating spin waves within a specified frequency range at one edge of the sample (Methods). The efficiency of these waves was quantified by comparing the magnetization precession at the point of origin and a defined distance from the source. In scenarios where q⊥kq \perp k, the initial waveform exhibits negligible damping even at a distance equivalent to 10λ10\lambda (Figure 3a). When q∥kq \parallel k, however, the spin wave exhibits significant attenuation over the same distance. This attenuation is evident in both the spectrum of the magnetization precession angle and its integrated energy across the spectrum, which is shown to be influenced by the magnitude of the anisotropy within the cycloid. As illustrated in Figure 3b, a scenario with an anisotropy of K=100 kJ m−3K = 100\ \mathrm{kJ\,m^{-3}} leads to approximately 50% damping in spin-wave-energy magnitude over the same length scale. This transport efficiency can then be studied as a function of KK to compare with previous calculations and experimental results, defining a reasonable window for the value of KK. The precession angles corresponding to other values of KK are shown in Extended data Figure 5.

Simulation of magnon conductivity

Figure 3. Simulation of magnon conductivity. Simulations of frequency-dependent magnon power when the spin wave is driven along the direction of q\mathbf{q}, which is (a) perpendicular, and (b) parallel to, k\mathbf{k}, respectively, in the quasi-1D lattice. Energy carried by the magnons is extracted as Ω×f\Omega\times f, i.e., the product of the conical angle, Ω\Omega, of the time-dependent procession of magnetization in Fourier space, and the frequency ff. Input and output spectra are measured at the initialization location and far side of the simulated cell. The integral of this spectra is then reported as a relative conductivity, (c), simulated as a function of the 1D anisotropy, KK, of the cycloid texture. The shaded region represents a range of energies reported in the literature, as well as values matched to the experimental and analytical results presented here. The horizontal dashed line corresponds to the measured efficiency, which is related to the plot by the intercept shown. (d) Calculated magnon dispersion, illustrating the emergence of a gap along the q∥k\mathbf{q} \parallel\mathbf{k} direction which leads to the reduced spin wave conductivity. XX and YY are the high symmetry points corresponding to the [100] (∥k\parallel\mathbf{k}) and [10] (⊥k\perp\mathbf{k}), respectively.

At the microscopic scale, analytical calculations of the momentum-dependent magnon dispersion in the quasi-1D lattice illustrate the difference in the magnon conduction ⊥k\perp k and ∥k\parallel k. Analytical solutions for the magnon bands of BFO are based on a continuum Hamiltonian whose density is given by [39]:

H=A(∇n)2−αP⋅[n(∇⋅n)+n×(∇×n)]−2βM0P⋅(m×n)−Kunc2+λm2(1)\mathcal{H} = A(\nabla\mathbf{n})^2 - \alpha\mathbf{P} \cdot\left[\mathbf{n}(\nabla\cdot\mathbf{n}) + \mathbf{n} \times(\nabla\times\mathbf{n})\right] - 2\beta M_0 \mathbf{P} \cdot(\mathbf{m} \times\mathbf{n}) - K_u n_c^2 + \lambda m^2 \tag*{(1)}

where the first term is the exchange energy, the second and third terms are DMI terms, the fourth term is the anisotropy, and the last term represents the suppression of the net magnetization due to strong antiferromagnetic coupling. The ground-state configuration can then be obtained (Supp. Note 3), showing the well-known anharmonic spin-cycloid structure [39, 40, 41]. Solving the time-dependent Euler-Lagrange equation for the small fluctuations, two spin-wave modes result: 1) An in-plane mode with spin fluctuations within the spin-cycloid plane and 2) an out-of-plane mode whose spin fluctuations are orthogonal to the spin-cycloid plane. By considering the quasi-2D geometry of the plane-wave-like spin texture of BFO and neglecting the Hamiltonian term ∝β\propto\beta that is known to be much weaker than the rest of the terms in the Hamiltonian [42], the band structures of

in-plane (IP) magnons and out-of-plane (OOP) magnon modes are obtained analytically (Figure 3d). This clearly shows the formation of a gap in the dispersion along the q∥kq \parallel k direction, due to the periodicity of the magnetic lattice. This gap indicates a lower density of states along this direction, resulting in an anisotropic, lower magnon conductivity.

In parallel to measurements of thermally excited magnons, non-local transport measurements have been performed using injected spin currents via the spin-Hall effect (SHE) of the source wire [36] (Figure 4a). In this case, the sign of the output signal will correspond directly to the sign of the input signal (i.e., a positive voltage will result in a positively polarized spin current, which then results in a positive voltage at the detector), rather than only the amplitude of the input (so-called first-harmonic and second-harmonic measurements). While the spin Hall angles of platinum and tungsten are too low to generate an appreciable ISHE signal at the 2 μ\mum electrode spacing, the efficient spin-charge transduction of SIO allows detection of the SHE excited magnon signal [38]. In the device geometry where qq is perpendicular to the domain walls, where electric fields allow the ferroelastic domain walls to remain largely stationary [19, 22, 35] (Extended Data Figure 2), combining the engineered spin texture with an epitaxial, large SHE oxide can further optimize functionality. This should allow for deterministic switching of the magnetic structure under a continuous rotation of PP [35].

Polarization control of magnon propagation

Figure 4. Polarization control of magnon propagation. (a) Schematic showing the non-local device geometry with magnons generated by injection of spin from the source wire. (b) We hypothesize that the non-reciprocity of the transport is due to a Rashba-like asymmetry of the magnon dispersion emerges from the crystal asymmetry, which is coupled directly to the ferroelectric polarization and DMI. (c,d) Illustration showing the sense of the cycloid with respect to the device geometry for films deposited on the two different substrates. In this orientation, the ferroelectric domain structure remains stationary with cycling electric field. (e,f) Switchable non-local signal overlaid with the ferroelectric hysteresis for both the single variant and chevron-like cases. (g) Combined with the above measurements, we hypothesize that the anisotropy can be explained by a split and anisotropic magnon dispersion, where the magnon conductivity maps to a surface with directions defined by qq and kk. The distance from the origin is representative of the conductivity, and thus the population. θ=90∘\theta= 90^\circ (P⊥kP \perp k) is high conductivity, θ=0∘\theta= 0^\circ (P∥kP \parallel k) is low, θ=45∘\theta= 45^\circ is intermediate, and θ=90∘\theta= 90^\circ and θ=−90∘\theta= -90^\circ carry an opposite sign angular momentum.

Schematics showing symmetry-allowed $k$ directions at 109° and 71° domain walls, and NV images showing magnetic structures at different permutations of strain and domain wall symmetry

Extended Data Figure 2. Strain and domain wall competition a,b Schematics showing the symmetry allowed kk directions at 109° and 71° domain walls. c NV images showing the magnetic structure at different permutations of strain and domain wall symmetry. When strain is high, as in DSO, k1k_1 is preferred, but becomes frustrated in 109° domain walls, leading to competition between the type-i and type-ii cycloids. In samples with 71° domains, it appears that k1k_1 is also preferentially chosen as the ground state. It is only through the combination of low strain and allowed symmetry where k2k_2, and the single variant state, is preferred.

In test structures using SIO electrodes, we observe a similar anisotropic spin transport, dependent on the underlying magnetic structure. Here, magnons are excited by the SHE and the ferroelectric polarization (noted P↑P \uparrow and P↓P \downarrow, where the direction of magnon propagation, q↑q \uparrow, is fixed), is switched using an in-plane electric field. Upon switching the in-plane component of the polarization, where the direction of magnon propagation, qq, is fixed, the detected first-harmonic non-local voltage, VNL,1ωV_{\mathrm{NL},1\omega}, switches hysteretically on the scale of ∼1 μV\sim1 \,\mu\mathrm{V} for a device spacing of 2 μ\mum. The repeatable difference between the P↑ q↑P \uparrow\, q \uparrow and P↓ q↑P \downarrow\, q \uparrow states is indicative of a non-reciprocity in the magnon dispersion tied to the direction of PP. This can be qualitatively rationalized in the form of a Rashba-like, DMI-induced splitting of the spin-dependent magnon bands (sketched in Figure 4b) [43, 44, 45, 46, 47]. The result is a VNL,1ωV_{\mathrm{NL},1\omega} that is both nonreciprocal and switchable. Since the samples under investigation exhibit no net magnetic moment, the inference is that magnon non-reciprocity in BFO should stem from a chiral component of the magnetic cycloid, which interacts with PP.

Under an applied electric field, this hysteresis in VNL,1ωV_{\mathrm{NL},1\omega} follows the switching of PP, where PP and ΔVNL,1ω\Delta V_{\mathrm{NL},1\omega} both flip signs at the same coercive voltage (Figure 4d,Figure 4e) [48]. As the ferroelastic domain walls remain stationary during this event (Extended Data Figure 2), a comparison can be made between samples with quasi-1D and chevron-like configurations (Figure 4c,Figure 4d). In quasi-1D samples with a single kk state, the magnitude of VNL,1ω⊥kV_{\mathrm{NL},1\omega} \perp k is two-times higher than that of the samples showing a chevron-like magnetic cycloid. The magnitude of this scaling directly parallels the observations in Figure 2, where the chevron-like texture shows a two-times lower conductivity than in the single kk samples when q⊥kq \perp k. Taken together, these measurements allow us to sketch the approximate shape of the magnon dispersion projected into the plane of the film (Figure 4g), where

These results demonstrate control of the magnetic structure of BFO and a method for effectively decoupling the magnetic structure from the ferroelectric domains. This has significant implications for magnonic devices using BFO, in that fundamental anisotropies of the cycloid structure can be used to optimize transport. The formation of a quasi-1D ordered magnonic lattice comprised of the spin cycloid should be of fundamental interest in terms of phase transitions in a 1D lattice and the possibility of obtaining long-range order in them. In this sense, future studies could be directed towards controlling the ferroelectric/ferroelastic domain structure through the use of vicinally cut substrates [30].

Conclusion

Using heteroepitaxy as a building block and imposing a combination of electrostatic and elastic constraints, we can strategically design both the ferroelectric and magnetic domain structure of multiferroic BFO. By doing so, a quasi-1D crystal of the antiferromagnetic spin cycloid can be chosen as the ground state. This anisotropic structure results in preferential spin-wave conduction orthogonal to its axis, due to the opening of a gap in the magnon dispersion created by the periodicity of the magnetic lattice. Leveraging magnetoelectric coupling, this magnonic crystal can be dynamically tuned using an electric field, allowing us to empirically map the magnon dispersion in the film plane with respect to the direction of ferroelectric polarization. This opens the door for the design of magnonic devices utilizing the anisotropy of the spin texture, as well as providing fundamental insights into the conduction of spin waves in complex magnetic systems.

Methods

Sample Fabrication 100 nm thick BFO samples were deposited on DSO and TSO substrates using both molecular-beam epitaxy (MBE) and pulsed laser deposition (PLD). MBE films were grown by reactive MBE in a VEECO GEN10 system using a mixture of 80 % ozone (distilled) and 20 % oxygen. Elemental sources of bismuth and iron were used at fluxes of 1.5×10141.5 \times10^{14} and 2×10132 \times10^{13} atoms/cm2^{2}s respectively. All films were grown at a substrate temperature of 675 °C and chamber pressure of 5×10−65 \times10^{-6} Torr. PLD samples were deposited using a 248 nm KrF laser with ∼1.5\sim1.5 J cm−2^{-2} at 700 °C and 90 mTorr O2_2. Pt (15 nm) and W (15 nm) layers were deposited using magnetron sputtering at room temperature. SIO layers were deposited using MBE using a mixture of 80 % ozone and 20 % O2_2 along with elemental sources of strontium and iridium. Due to the high temperatures needed to generate an iridium flux, an electron beam was used to evaporate iridium. The samples were grown at a substrate temperature of 695 °C and a background pressure of 1×10−61 \times10^{-6} Torr. Devices were fabricated using standard optical lithography followed by ion milling.

Sample Characterization X-ray diffraction was performed on a PANalytical Xpert3 diffractometer. Piezoresponse force microscopy was performed on an Asylum MFP3D. NV magnetometry was performed on a Qnami ProteusQ system with a parabolic Quantilever MX+ diamond cantilever.

Phase Field Simulations We employed MagneX, a substantial GPU-enabled micromagnetic simulation code package (available on GitHub), to phenomenologically explore the directionality of magnon transport in the cycloid. The time-domain Landau-Lifshitz-Gilbert equation is solved, incorporating exchange coupling, DMI coupling, anisotropy coupling, and demagnetization coupling. A set of abstract ferromagnetic properties is utilized to phenomenologically represent the antiferromagnetic material. The magnetization is pinned by an external applied magnetic field that mimics the cycloid texture. The Gilbert damping constant is set to be 0.0005, the exchange coupling constant is 3.0×10−123.0 \times10^{-12} J m−1^{-1}, and the DMI coupling constant is 1.0935×10−31.0935 \times10^{-3} J m−2^{-2}. The anisotropic hard axis is set to the [111] direction, while the anisotropy constant is swept in the range of 1.0×1041.0 \times10^{4} J m−3^{-3} and 2.0×1062.0 \times10^{6} J m−3^{-3}. The total magnetization is normalized to be one. On one side of the sample, a modified Gaussian pulse in the effective magnetic field is applied in both the xx and yy direction, mimicking injected spins from the top SHE electrode. The pulse is in the mathematical form of e−(t−t0)2/2T02cos⁡(2πf0t)e^{-(t-t_{0})^{2}/2T_{0}^{2}}\cos(2\pi f_{0}t), where f0f_{0} is 700 GHz. The output port is on the opposite side of the input port in the in-plane direction. The simulated time-varying magnetization components are converted into the frequency domain with the Fourier transform, from which we calculate the cone angle of the magnetization. For more details, see Supp. Note 2.

Analytical Calculations See Supp. Note 3.

Transport Measurements Transport measurements were performed using 3-terminal devices where two were used to inject current and two for output. Two cross-terminals were used to apply electric field for polarization control. All operations were controlled through the in-house developed code. VNLV_{NL} was measured using an SR830 lock-in amplifier and locking to the second (in the case of thermally excited magnons) or first (in the case of spin Hall excited magnons) harmonic of the excitation voltage. An AC signal at 7 Hz was used for both first- and second-harmonic measurements. In the first-harmonic measurement, the magnitude of the injected current is chosen to be small to avoid the thermal drift in the output voltage.

Author Contributions

PM designed experiments. MR and SH deposited samples. PM and SH performed PFM. PM, SZ, and PS performed NV microscopy. ZY performed phase field simulations. HWP and SKK performed analytical calculations. IH and HT fabricated devices. SH and IH performed spin transport. PM, MR, and SH wrote the manuscript. All authors have contributed to manuscript edits.

This work was primarily supported by the U.S. Department of Energy, Office of Science, Office of Basic Energy Sciences, Materials Sciences and Engineering Division under Contract No. DE-AC02-05-CH11231 (Codesign of Ultra-Low-Voltage Beyond CMOS Microelectronics (MicroelecLBLRamesh)) for the development of materials for low-power microelectronics. P.M., R.R., M.R. and D.G.S. additionally acknowledge funding from the Army Research Office under the ETHOS MURI via cooperative agreement W911NF-21-2-0162. S.Z. and L.C. acknowledge funding from Brown School of Engineering and Office of the Provost. P.S. acknowledges support from the Massachusetts Technology Collaborative, Award number 22032. Computations in this paper were performed using resources of the National Energy Research Scientific Computing Center (NERSC), a U.S. Department of Energy Office of Science User Facility operated under contract no. DE-AC02-05CH11231. The work performed at the Molecular Foundry was supported by the Office of Science, Office of Basic Energy Sciences, of the U.S. Department of Energy under Contract No. DEAC02-05CH11231. S.K.K. and H.W.P. acknowledge support from the Brain Pool Plus Program through the National Research Foundation of Korea funded by the Ministry of Science and ICT (2020H1D3A2A03099291).

The authors declare no competing interests

Data relevant to this manuscript have been uploaded to zenodo under accession code XYZ. Other data is available from the corresponding author upon reasonable request.

Extended Data

Extended data for "Designed spin-texture-lattice to control anisotropic magnon transport in antiferromagnets"

X-ray diffraction line scans and reciprocal space maps of BiFeO₃/DyScO₃ and BiFeO₃/TbScO₃ samples

Figure 1 (PDF p. 20). Extended Data Figure 1: X-ray diffraction a 2θ−ω2\theta- \omega line scans of the two samples with Pendellösung fringes around the film peaks, showing the crystalline quality. b Reciprocal space maps of the 332O332_{\mathrm{O}} diffraction peak. Differences are due to the different configurations of the rhombohedral BFO unit cell in the different domain configurations [30].

Extended Data Figure 4: Material and power dependence

Extended Data Figure 4. Material and power dependence a The thermally-driven non-local conductivity changes with the sign and magnitude of the spin Hall angle of the detector wire material (Pt, W, and SIO), demonstrating its magnetic origin. Symbols are the raw data and solid lines represent the time average. PP and qq are the polarization and the magnon-propagation direction, respectively. b The output voltage also scales with the magnitude of the spin Hall angle of the detector material. The dotted lines correspond to orders of magnitude.

Spectral dependence of magnetocrystalline anisotropy

Extended Data Figure 5. Spectral dependence of magnetocrystalline anisotropy. Resonant spectra of excited spin waves extracted from phase field simulations in both the q⊥kq \perp k and q∥kq \parallel k cases, used to calculate the efficiency scaling in Figure 3c. Frequency dependent cone angles, Ω\Omega, are calculated as the Fourier transforms of the time dependent magnetization procession. Anisotropy (KK) values are intentionally chosen both above and below the expected range.

2D magnon dispersion visualizations of the lowest IP and OOP bands

Extended Data Figure 6. 2D magnon dispersion visualizations of the of the lowest IP (a) and OOP (b) bands, showing both qx⊥kq_x \perp k (red) and qy∥kq_y \parallel k (blue). The in-plane and out-of-plane mode corresponds to the spin fluctuations within the spin-cycloid plane and perpendicular to the spin-cycloid plane, respectively. The striking difference between these energy bands demonstrates the anisotropic magnon-dispersion within the spin cycloid 1D lattice.

Ferroelectric switching hysteresis loops and corresponding PFM images

Extended Data Figure 7. Ferroelectric switching Ferroelectric hysteresis loops (a,e) and corresponding PFM (c,d,g,h) of the poled ferroelectric states. In both cases, devices can be electrically poled with E⊥E \perp the domain walls and conserve the domain structure (b). When E∥E \parallel to the domain walls, (h) however, the domains reorient into the striped 71° structure such that E⊥E \perp the domain walls, regardless of the starting configuration (f). This can be observed in the hysteresis loop in d, where, starting from the as-deposited state, parallel 109° domains are progressively transformed into perpendicular 71° domains as the device is cycled 3-4 times.

Supplementary Information for Designed spin texture lattice to control magnon transport in antiferromagnets

Magnon transport measurements

In thermally excited magnon transport experiments, the magnitude of non-local inverse spin Hall voltage (VNLV_{NL}) is reported as the difference (ΔVNL\Delta V_{NL}) between two measurement configurations where the propagation direction, qq from the thermal gradient, ∇T\nabla T, is changed and the ferroelectric polarization (PP) remains fixed. This was chosen due to the response of domains to an electric field parallel to the domain wall, which leads to reconfiguration of the domain structure. The application of an electric field parallel to the two-variant domain walls transforms the domain structure into 71∘71^{\circ} domains running perpendicular to the electric field. This in turn changes the magnetic structure of the spin cycloid, making determination of the native anisotropy ⊥\perp and ∥k\parallel k impossible.

In samples where the electric field does not perturb the domain structure (E⊥E \perp the domain walls), we find that the difference in ΔVNL\Delta V_{NL} for the two polarization states is equivalent to the difference in VNLV_{NL} for the two configurations (Figure S1). This is reasonable following from the symmetry of the material. As there is no net magnetization, and thus no net magnon polarization as in ferromagnetic magnon experiments, a difference in the nonlocal voltage is only expected to arise if the efficiency of magnon spin transport along qq is dependent on the underlying magnetic structure of the BFO. Using an electric field to switch the polarization direction, and thus the underlying magnetic structure, while leaving qq unchanged should be equivalent to switching qq while leaving PP and the underlying magnetic structure unchanged. In other words, we expect ΔVNL=P↑q↑−P↓q↑≈P↑q↑−P↑q↓\Delta V_{NL} = P^{\uparrow}q^{\uparrow} - P^{\downarrow}q^{\uparrow} \approx P^{\uparrow}q^{\uparrow} - P^{\uparrow}q^{\downarrow} when averaged across devices. This is shown in Figure S1. We note that while small differences in the heater and detector wire will lead to asymmetries in VNLV_{NL} unrelated to the magnon transport, averaging ΔVNL\Delta V_{NL} across different devices negates this asymmetry.

Supplementary Note 2: Micromagnetic modeling

We employed MagneX, a substantial GPU-enabled micromagnetic simulation code package (available on GitHub), to phenomenologically explore the directionality of magnon transport in the cycloid. The time-domain Landau-Lifshitz-Gilbert equation is solved, incorporating exchange coupling, DMI coupling, anisotropy coupling, and demagnetization coupling. A set of abstract ferromagnetic properties is utilized to phenomenologically represent the antiferromagnetic material.

The size of the sample is set to be 640 nm×640 nm×10 nm640\ \mathrm{nm} \times640\ \mathrm{nm} \times10\ \mathrm{nm}, with a 512×512×16512 \times512 \times16 mesh resulting in grid sizes of Δx=Δy=1.25 nm\Delta x = \Delta y = 1.25\ \mathrm{nm}, and Δz=0.625 nm\Delta z = 0.625\ \mathrm{nm}. The magnetization is pinned by a strong external applied magnetic field that mimics the cycloid texture, which gives the magnetization profile shown in Figure S2. The period of the cycloid is 62 nm. The Gilbert damping constant is set to be 0.0005, the exchange coupling constant is 3.0×10−12 J m−13.0 \times10^{-12}\ \mathrm{J}\ \mathrm{m}^{-1}, and the DMI coupling constant is 1.0935×10−3 J m−21.0935 \times10^{-3}\ \mathrm{J}\ \mathrm{m}^{-2}. The anisotropic hard axis is set to the [111] direction, while the anisotropy constant is swept in the range of 1.0×104 J m−31.0 \times10^{4}\ \mathrm{J}\ \mathrm{m}^{-3} and 2.0×106 J m−32.0 \times10^{6}\ \mathrm{J}\ \mathrm{m}^{-3}. The magnitude of the magnetization is normalized to one.

Initialized magnetization ground state in the simulation

Figure S2. Initialized magnetization ground state in the simulation, with a period of 62 nm. Colored values show the magnitude of MM projected along MxM_x. Black arrows show the local MM vector.

Starting from t=0t = 0, an additional time-dynamic external magnetic field is added on top of the existing pinning bias field. As shown in Figure S3, on one side of the sample, a modified Gaussian pulse in the effective magnetic field is applied in both the xx and yy direction, mimicking injected spins from the top SOC electrode. The pulse is in a mathematical form of e−(t−t0)2/2T02cos⁡(2πf0t)e^{-(t-t_0)^2/2T_0^2}\cos(2\pi f_0t), where f0f_0 is 700 GHz. T0T_0 is chosen such that the excitation bandwidth is approximately 300 GHz. The output port is on the opposite side of the input port in the in-plane direction. By measuring the magnetization components, we can compute the spin wave transmission efficiency from the input port to the output port.

Modeling setup for magnon transport along and perpendicular to the cycloid direction

Figure S3. Modeling setup. The left figure illustrates the measurement of magnon transport along the cycloid direction (q∥kq \parallel k), while the right figure depicts magnon transport along the uniform direction of the cycloid (q⊥kq \perp k).

Figure S4,Figure S4 show the raw magnetization components at the input and output ports for both transport directions. The spots were selected where the ground-state magnetization is oriented in the out-of-plane direction, enabling straightforward analysis of the magnon excitation. These simulated time-varying magnetization components are then converted into the frequency domain through the Fourier transform, given in Figure S4,Figure S4.

Time-domain and frequency-domain magnetization components at input and output ports

Figure S4. Time-domain and frequency-domain magnetization components at the input and output ports for both transport directions.

To calculate the solid angles of the oscillating magnetization, we begin by expressing the spectral magnetization components at each frequency point in their time-harmonic form: m=∣M(f0)∣×cos⁡(2πf0t+∠M(f0))m = \lvert M(f_0)\rvert\times\cos(2\pi f_0t + \angle M(f_0)). This time-harmonic form provides an MM trajectory at each frequency point, with a cone area corresponding to the solid angle of the MM trajectory. For instance, Figure S5 illustrates the magnetization trajectory at 700 GHz for input and output ports along the cycloid KK direction.

Magnetization trajectories at the input and output ports

Figure S5. Magnetization trajectory at 700 GHz. Input and output ports are along xx direction, i.e. the KK direction of the cycloid.

Considering the small solid angle of magnetization, we simplify the calculation of the 3D cone area to a planar cross-sectional area S(f)S(f) by integrating over all sectors forming the trajectory. The cone angles at each frequency are then determined by Ω(f)=S(f)/∣M(f=0)∣2\Omega(f) = S(f)/\lvert M(f = 0)\rvert^{2}, as illustrated in Extended Data Figure 3 in the main manuscript. Subsequently, we calculate the magnon energy by integrating over its entire spectrum E=∑f(Ω(f)×f)E = \sum_f(\Omega(f) \times f). Finally, the transport efficiencies for both along-xx and along-yy scenarios are determined by computing the power efficiency ξ=Eoutput/Einput\xi= E_{\mathrm{output}}/E_{\mathrm{input}}, leading to the plot in Figure 4c in the main manuscript.

Antiphase boundaries

Extended Data Figure 3. Antiphase boundaries The 109° domain samples exhibit a hierarchical domain pattern characteristic of BFO. Superimposed on the fine-scale 109° domain ensemble with a spacing of 20-30nm, families of domains with net antiparallel in-plane polarization components are also observed. Comparing the ferroelectric polarization from PFM with the NV data, we observe discontinuities in the 1-D cycloid lattice that correlate with the family domain walls (a,b). Though k2k_2 does not change across the fine-scale (20-30nm) domain walls, it does change (e.g. k2[101]k_2[101] to k2′[1ˉ01]k'_2[\bar{1}01]) across these large domains with a different in-plane polarization (c). Though k2k_2 and k2′k'_2 in these two domains are orthogonal to each other, the in-plane component of the cycloid does not change, giving the appearance of discontinuities (akin to an antiphase boundary in ordered alloys) when projected in-plane. When the material is electrically poled, these macro domain walls are annealed out of the sample.

Analytical solution for the magnon bands

Our theory for BiFeO3_3 is based on the following continuum Hamiltonian [39] and the corresponding Lagrangian [?], whose densities are respectively given by

H=A(∇n)2−αP⋅[n(∇⋅n)+n×(∇×n)]−2βM0P⋅(m×n)−Kunc2+λm2(2)\mathcal{H}=A(\nabla\mathbf{n})^2-\alpha\mathbf{P}\cdot\left[\mathbf{n}(\nabla\cdot\mathbf{n})+\mathbf{n}\times(\nabla\times\mathbf{n})\right]-2\beta M_0\mathbf{P}\cdot(\mathbf{m}\times\mathbf{n})-K_u n_c^2+\lambda m^2 \tag*{(2)}
L=sm⋅(n×n˙)−H.(3)\mathcal{L}=s\mathbf{m}\cdot(\mathbf{n}\times\dot{\mathbf{n}})-\mathcal{H}. \tag*{(3)}

Here, the magnetic state is described by the Neel order parameter n(r,t)\mathbf{n}(\mathbf{r},t) whose length is unity and the net magnetization m(r,t)\mathbf{m}(\mathbf{r},t) which is perpendicular to the Neel order parameter, i.e., n⋅m=0\mathbf{n}\cdot\mathbf{m}=0. The coefficients in the continuum Hamiltonian are related to the parameters in the microscopic spin Hamiltonian as follows: λ=6S2V(−3J+6J′)\lambda=\frac{6S^2}{V}(-3\mathcal{J}+6\mathcal{J}'), A=6S2V3J−4J′4ahex2A=\frac{6S^2}{V}\frac{3\mathcal{J}-4\mathcal{J}'}{4}a_{hex}^2, α=6S2V1Psahex2Du\alpha=\frac{6S^2}{V}\frac{1}{P_s}a_{hex}^2\mathcal{D}_u, β=6S2V1M0PsDc\beta=\frac{6S^2}{V}\frac{1}{M_0P_s}\mathcal{D}_c, and Ku=6S2VKK_u=\frac{6S^2}{V}\mathcal{K}, where J=4.38\mathcal{J}=4.38 meV, J′=0.15\mathcal{J}'=0.15 meV, Du=0.11\mathcal{D}_u=0.11 meV, Dc=0.05\mathcal{D}_c=0.05 meV, K=0.003\mathcal{K}=0.003 meV, S=52(52+1)S=\sqrt{\frac{5}{2}\left(\frac{5}{2}+1\right)}, ahex=5.58×10−8a_{hex}=5.58\times10^{-8} cm, and V=375.9×10−24V=375.9\times10^{-24} cm3^3 [39]. The microscopic spin Hamiltonian can be found in Ref. [39]. It is convenient to use the spherical angles θ(r,t)\theta(\mathbf{r},t) and ϕ(r,t)\phi(\mathbf{r},t) to represent n=(sin⁡θcos⁡ϕ,sin⁡θsin⁡ϕ,cos⁡θ)\mathbf{n}=(\sin\theta\cos\phi,\sin\theta\sin\phi,\cos\theta) and mθ(r,t)m_\theta(\mathbf{r},t) and mϕ(r,t)m_\phi(\mathbf{r},t) to represent m=(mθcos⁡θcos⁡ϕ−mϕsin⁡ϕ,mϕcos⁡ϕ+mθcos⁡θsin⁡ϕ,−mθsin⁡θ)\mathbf{m}=(m_\theta\cos\theta\cos\phi-m_\phi\sin\phi,m_\phi\cos\phi+m_\theta\cos\theta\sin\phi,-m_\theta\sin\theta). In terms of these variables, the Euler-Lagrange equation of the Lagrangian is given by

−smθ∂tϕcos⁡θ−s∂tmϕ+2A(∇2θ)+2αPzsin⁡2θ(sin⁡ϕ(∂xϕ)−cos⁡ϕ(∂yϕ))−sin⁡2θ(A(∇ϕ)2+Ku)−2βM0Pzmϕcos⁡θ=0,(4)\begin{aligned} -sm_\theta\partial_t\phi\cos\theta-s\partial_t m_\phi+2A(\nabla^2\theta)+2\alpha P_z\sin^2\theta\left(\sin\phi(\partial_x\phi)-\cos\phi(\partial_y\phi)\right)\\ -\sin2\theta\left(A(\nabla\phi)^2+K_u\right)-2\beta M_0P_zm_\phi\cos\theta&=0, \tag*{(4)} \end{aligned}
s∂t(mθsin⁡θ)+2A∇⋅(sin⁡2θ(∇ϕ))−2αPzsin⁡2θ(sin⁡ϕ(∂xθ)−cos⁡ϕ(∂yθ))=0,(5)s\partial_t(m_\theta\sin\theta)+2A\nabla\cdot\left(\sin^2\theta(\nabla\phi)\right)-2\alpha P_z\sin^2\theta\left(\sin\phi(\partial_x\theta)-\cos\phi(\partial_y\theta)\right)=0, \tag*{(5)}
−s∂tϕsin⁡θ−mθχ=0,(6)-s\partial_t\phi\sin\theta-\frac{m_\theta}{\chi}=0, \tag*{(6)}
s∂tθ−mϕχ−2βM0Pzsin⁡θ=0.(7)s\partial_t\theta-\frac{m_\phi}{\chi}-2\beta M_0P_z\sin\theta=0. \tag*{(7)}

The ground-state configuration n0(r)\mathbf{n}_0(\mathbf{r}) and m0(r)\mathbf{m}_0(\mathbf{r}) can be obtained by solving the Euler-Lagrange equation with no time dependence. The resulting ground state of BiFeO3_3 has an anharmonic spin cycloid structure as well known, e.g., in Refs. [39, 40, 41]. Here, we focus on the cases where β=0\beta=0, as often done due to its smallness [39]. The explicit expression for a ground state is given by

ϕ=const.,θ=am⁡(CAx,KuC)−π2,(8)\phi=\mathrm{const.},\qquad\theta=\operatorname{am}\left(\sqrt{\frac{C}{A}}x,\frac{K_u}{C}\right)-\frac{\pi}{2}, \tag*{(8)}

with vanishing mm, where am⁡(u,m)\operatorname{am}(u,m) is the Jacobi amplitude function and CC is the integral constant determined by minimizing the free energy of the aforementioned solution with respect to CC [39]. Here, the spin-cycloid direction is chosen to be the xx-axis without loss of generality.

By solving the time-dependent Euler-Lagrange equation for the small fluctuations, δn=n−n0\delta\mathbf{n}=\mathbf{n}-\mathbf{n}_0 and δm=m−m0\delta\mathbf{m}=\mathbf{m}-\mathbf{m}_0, on top of the ground state up to linear order in the fluctuations δn\delta\mathbf{n} and δm\delta\mathbf{m}, we can obtain two spin-wave modes: in-plane mode with spin fluctuations within the spin-cycloid plane and out-of-plane mode whose spin fluctuations are perpendicular to the spin-cycloid plane. The corresponding equations of motion for δθ\delta\theta, δϕ\delta\phi, δmθ\delta m_\theta, and δmϕ\delta m_\phi are given by

−s∂tδmϕ+2A(∇2δθ)+2αPz(sin⁡2θg)(sin⁡ϕg(∂xδϕ)−cos⁡ϕg(∂yδϕ))−(2δθcos⁡2θg)(Ku)=0(9)\begin{aligned} -s\partial_t\delta m_\phi+2A(\nabla^2\delta\theta)+2\alpha P_z(\sin^2\theta_g)(\sin\phi_g(\partial_x\delta\phi)-\cos\phi_g(\partial_y\delta\phi))\\ -(2\delta\theta\cos2\theta_g)(K_u)&=0 \tag*{(9)} \end{aligned}
s∂t(δmθsin⁡θg)+2A∇⋅(sin⁡2θg(∇(δϕ)))−2αPz(sin⁡2θg)(sin⁡ϕg(∂xδθ)+δϕcos⁡ϕg(∂xθg)−cos⁡ϕg(∂yδθ)+δϕsin⁡ϕg(∂yθg))=0(10)\begin{aligned} s\partial_t(\delta m_\theta\sin\theta_g)+2A\nabla\cdot(\sin^2\theta_g(\nabla(\delta\phi)))\\ -2\alpha P_z(\sin^2\theta_g)(\sin\phi_g(\partial_x\delta\theta)+\delta\phi\cos\phi_g(\partial_x\theta_g)-\cos\phi_g(\partial_y\delta\theta)+\delta\phi\sin\phi_g(\partial_y\theta_g))&=0 \tag*{(10)} \end{aligned}
−sδϕ˙sin⁡θg−δmθχ=0(11)-s\delta\dot{\phi}\sin\theta_g-\frac{\delta m_\theta}{\chi}=0 \tag*{(11)}
θ˙−δmϕsχ=0(12)\dot{\theta}-\frac{\delta m_\phi}{s\chi}=0 \tag*{(12)}

The translational symmetry along the zz axis allows us to use the plane-wave ansatz δθ(x,z,t)=δθ(x;kz,ω)exp⁡(ikzz−iωt)\delta\theta(x,z,t)=\delta\theta(x;k_z,\omega)\exp(ik_z z-i\omega t) and δη(x,z,t)=δη(x;kz,ω)exp⁡(ikzz−iωt)\delta\eta(x,z,t)=\delta\eta(x;k_z,\omega)\exp(ik_z z-i\omega t) with δη=sin⁡θgδϕ\delta\eta=\sin\theta_g\delta\phi, in terms of which the above four equations can be combined into the following two equations for δθ(x;kz,ω)\delta\theta(x;k_z,\omega) and δη(x;kz,ω)\delta\eta(x;k_z,\omega):

[(s2ω2χ−2Akz2)+2A∂x2−2Kucos⁡2θg]δθ=0(13)[(s^2\omega^2\chi-2Ak_z^2)+2A\partial_x^2-2K_u\cos2\theta_g]\delta\theta=0 \tag*{(13)}
[(s2ω2χ−2Akz2)+2A∂x2−4Kucos⁡2(θg)+2C−2αPz(∂xθg)]δη=0(14)[(s^2\omega^2\chi-2Ak_z^2)+2A\partial_x^2-4K_u\cos^2(\theta_g)+2C-2\alpha P_z(\partial_x\theta_g)]\delta\eta=0 \tag*{(14)}

where δη=sin⁡θgδϕ\delta\eta=\sin\theta_g\delta\phi. By solving these equations numerically, we obtained the band structures of in-plane magnons and out-of-plane magnons as shown in the Figure 3 of the main manuscript. It is apparent that the band structure for the two modes is anisotropic. We remark that the anisotropy is the most visible in the lowest bands, which makes sense since low-energy magnons are expected to be more affected by the spin-cycloid structure than high-energy magnons and therefore exhibit anisotropic behavior more strongly.

References

  1. [1]Jungwirth, T., Marti, X., Wadley, P., Wunderlich, J.: Antiferromagnetic spintronics. Nature Nanotechnology 11(3), 231–241 (2016) https://doi.org/10.1038/nnano.2016.18 . Number: 3 Publisher: Nature Publishing Group. Accessed 2023-06-29
  2. [2]Han, J., Cheng, R., Liu, L., Ohno, H., Fukami, S.: Coherent antiferromagnetic spintronics. Nature Materials 22(6), 684–695 (2023) https://doi.org/10.1038/s41563-023-01492-6 . Number: 6 Publisher: Nature Publishing Group. Accessed 2023-06-29
  3. [3]Jungwirth, T., Sinova, J., Manchon, A., Marti, X., Wunderlich, J., Felser, C.: The multiple directions of antiferromagnetic spintronics. Nature Physics 14(3), 200–203 (2018) https://doi.org/10.1038/s41567-018-0063-6 . Number: 3 Publisher: Nature Publishing Group. Accessed 2023-10-02
  4. [4]Qiu, R.-k., Huang, T., Zhang, Z.-d.: Magnon band structure and magnon density in one-dimensional magnonic crystals. Journal of Magnetism and Magnetic Materials 368, 180–190 (2014) https://doi.org/10.1016/j.jmmm.2014.05.033 . Accessed 2023-12-18
  5. [5]Chumak, A.V., Serga, A.A., Hillebrands, B.: Magnonic crystals for data processing. Journal of Physics D: Applied Physics 50(24), 244001 (2017) https://doi.org/10.1088/1361-6463/aa6a65 . Publisher: IOP Publishing. Accessed 2023-12-19
  6. [6]Deng, D.S., Jin, X.F., Tao, R.: Magnon energy gap in a periodic anisotropic magnetic superlattice. Physical Review B 66(10), 104435 (2002) https://doi.org/10.1103/PhysRevB.66.104435 . Publisher: American Physical Society. Accessed 2023-12-18
  7. [7]Zivieri, R., Montoncello, F., Giovannini, L., Nizzoli, F., Tacchi, S., Madami, M., Gubbiotti, G., Carlotti, G., Adeyeye, A.O.: Collective spin modes in chains of dipolarly interacting rectangular magnetic dots. Physical Review B 83(5), 054431 (2011) https://doi.org/10.1103/PhysRevB.83.054431 . Publisher: American Physical Society. Accessed 2023-12-18
  8. [8]Chumak, A.V., Pirro, P., Serga, A.A., Kostylev, M.P., Stamps, R.L., Schultheiss, H., Vogt, K., Hermsdorfer, S.J., Laegel, B., Beck, P.A., Hillebrands, B.: Spin-wave propagation in a microstructured magnonic crystal. Applied Physics Letters 95(26), 262508 (2009) https://doi.org/10.1063/1.3279138 . Accessed 2023-12-18
  9. [9]Chumak, A.V., Tiberkevich, V.S., Karenowska, A.D., Serga, A.A., Gregg, J.F., Slavin, A.N., Hillebrands, B.: All-linear time reversal by a dynamic artificial crystal. Nature Communications 1(1), 141 (2010) https://doi.org/10.1038/ ncomms1142 . Number: 1 Publisher: Nature Publishing Group. Accessed 2023-12-18
  10. [10]Wessler, C., Roessli, B., Krämer, K.W., Stuhr, U., Wildes, A., Braun, H.B., Kenzelmann, M.: Dirac spin-waves and tunable band gap at the Dirac points in the 2D magnet ErBr3. Communications Physics 5(1), 1–7 (2022) https://doi.org/10.1038/s42005-022-00965-5 . Number: 1 Publisher: Nature Publishing Group. Accessed 2023-12-18
  11. [11]Hertel, R., Wulfhekel, W., Kirschner, J.: Domain-Wall Induced Phase Shifts in Spin Waves. Physical Review Letters 93(25), 257202 (2004) https://doi.org/10.1103/PhysRevLett.93.257202 . Publisher: American Physical Society. Accessed 2023-12-19
  12. [12]Li, R., Riddiford, L.J., Chai, Y., Dai, M., Zhong, H., Li, B., Li, P., Yi, D., Zhang, Y., Broadway, D.A., Dubois, A.E.E., Maletinsky, P., Hu, J., Suzuki, Y., Ralph, D.C., Nan, T.: A puzzling insensitivity of magnon spin diffusion to the presence of 180-degree domain walls. Nature Communications 14(1), 2393 (2023) https://doi.org/10.1038/s41467-023-38095-3 . Number: 1 Publisher: Nature Publishing Group. Accessed 2023-12-19
  13. [13]Pirro, P., Vasyuchka, V.I., Serga, A.A., Hillebrands, B.: Advances in coherent magnonics. Nature Reviews Materials 6(12), 1114–1135 (2021) https://doi.org/10.1038/s41578-021-00332-w . Number: 12 Publisher: Nature Publishing Group. Accessed 2023-12-19
  14. [14]Hämäläinen, S.J., Madami, M., Qin, H., Gubbiotti, G., Dijken, S.: Control of spin-wave transmission by a programmable domain wall. Nature Communications 9(1), 4853 (2018) https://doi.org/10.1038/s41467-018-07372-x . Number: 1 Publisher: Nature Publishing Group. Accessed 2023-12-19
  15. [15]Caretta, L., Oh, S.-H., Fakhrul, T., Lee, D.-K., Lee, B.H., Kim, S.K., Ross, C.A., Lee, K.-J., Beach, G.S.D.: Relativistic kinematics of a magnetic soliton. Science 370(6523), 1438–1442 (2020) https://doi.org/10.1126/science.aba5555 . Publisher: American Association for the Advancement of Science. Accessed 2023-12-19
  16. [16]Avci, C.O., Rosenberg, E., Caretta, L., Büttner, F., Mann, M., Marcus, C., Bono, D., Ross, C.A., Beach, G.S.D.: Interface-driven chiral magnetism and current-driven domain walls in insulating magnetic garnets. Nature Nanotechnology 14(6), 561–566 (2019) https://doi.org/10.1038/s41565-019-0421-2 . Number: 6 Publisher: Nature Publishing Group. Accessed 2023-12-19
  17. [17]Thomas, L., Hayashi, M., Jiang, X., Moriyama, R., Rettner, C., Parkin, S.S.P.: Oscillatory dependence of current-driven magnetic domain wall motion on current pulse length. Nature 443(7108), 197–200 (2006) https://doi.org/10.1038/nature05093 . Number: 7108 Publisher: Nature Publishing Group. Accessed
  18. [18]ncomms1142 . Number: 1 Publisher: Nature Publishing Group. Accessed 2023-12-18 Bibes, M., Barthélémy, A.: Multiferroics: Towards a magnetoelectric memory. Nature Materials 7(6), 425–426 (2008) https://doi.org/10.1038/nmat2189
  19. [19]Heron, J.T., Bosse, J.L., He, Q., Gao, Y., Trassin, M., Ye, L., Clarkson, J.D., Wang, C., Liu, J., Salahuddin, S., Ralph, D.C., Schlom, D.G., Íñiguez, J., Huey, B.D., Ramesh, R.: Deterministic switching of ferromagnetism at room temperature using an electric field. Nature 516(7531), 370–373 (2014) https://doi.org/10.1038/nature14004 . Accessed 2017-10-12
  20. [20]Spaldin, N.A., Ramesh, R.: Advances in magnetoelectric multiferroics. Nature Materials 18(3), 203–212 (2019) https://doi.org/10.1038/s41563-018-0275-2 . Number: 3 Publisher: Nature Publishing Group. Accessed 2023-12-13
  21. [21]Rovillain, P., Sousa, R., Gallais, Y., Sacuto, A., Méasson, M.A., Colson, D., Forget, A., Bibes, M., Barthélémy, A., Cazayous, M.: Electric-field control of spin waves at room temperature in multiferroic BiFeO3. Nature Materials 9(12), 975–979 (2010) https://doi.org/10.1038/nmat2899 . Number: 12 Publisher: Nature Publishing Group. Accessed 2023-12-18
  22. [22]Parsonnet, E., Caretta, L., Nagarajan, V., Zhang, H., Taghinejad, H., Behera, P., Huang, X., Kavle, P., Fernandez, A., Nikonov, D., Li, H., Young, J., Analytis, J., Ramesh, R.: Nonvolatile Electric Field Control of Thermal Magnons in the Absence of an Applied Magnetic Field. Physical Review Letters 129(8), 087601 (2022) https://doi.org/10.1103/PhysRevLett.129.087601 . Publisher: American Physical Society. Accessed 2023-05-15
  23. [23]Burns, S.R., Paull, O., Juraszek, J., Nagarajan, V., Sando, D.: The Experimentalist’s Guide to the Cycloid, or Noncollinear Antiferromagnetism in Epitaxial BiFeO3. Advanced Materials 32(45), 2003711 (2020) https://doi.org/10.1002/adma.202003711 . _eprint: https://onlinelibrary.wiley.com/doi/pdf/10.1002/adma.202003711. Accessed 2023-04-25
  24. [24]Zhong, H., Finco, A., Fischer, J., Haykal, A., Bouzounane, K., Carrétéro, C., Godel, F., Maletsky, P., Munsch, M., Fusil, S., Jacques, V., Garcia, V.: Quantitative Imaging of Exotic Antiferromagnetic Spin Cycloids in BiFeO3 Thin Films. Physical Review Applied 17(4), 044051 (2022) https://doi.org/10.1103/PhysRevApplied.17.044051 . Publisher: American Physical Society. Accessed 2023-04-20
  25. [25]Sosnowska, I., Neumaier, T.P., Steichele, E.: Spiral magnetic ordering in bismuth ferrite. Journal of Physics C: Solid State Physics 15(23), 4835 (1982) https://doi.org/10.1088/0022-3719/15/23/020 . Accessed 2023-04-26
  26. [26]Ramazanoglu, M., Laver, M., Ratcliff, W., Watson, S.M., Chen, W.C., Jackson, A., Kothapalli, K., Lee, S., Cheong, S.-W., Kirykhin, V.: Local Weak Ferromagnetism in Single-Crystalline Ferroelectric BiFeO3. Physical Review Letters 107(20), 207206 (2011) https://doi.org/10.1103/PhysRevLett.107.207206 . Publisher: American Physical Society. Accessed 2023-04-21
  27. [27]Rahmedov, D., Wang, D., Íñiguez, J., Bellaiche, L.: Magnetic Cycloid of BiFeO3 from Atomistic Simulations. Physical Review Letters 109(3), 037207 (2012) https://doi.org/10.1103/PhysRevLett.109.037207 . Publisher: American Physical Society. Accessed 2023-07-09
  28. [28]Lebeugle, D., Colson, D., Forget, A., Viret, M., Bataille, A.M., Gukasov, A.: Electric-Field-Induced Spin Flop in BiFeO3 Single Crystals at Room Temperature. Physical Review Letters 100(22), 227602 (2008) https://doi.org/10.1103/PhysRevLett.100.227602 . Publisher: American Physical Society. Accessed 2023-04-21
  29. [29]Gross, I., Akhtar, W., Garcia, V., Martínez, L.J., Chouaie b, S., Garcia, K., Car-rét er o, C., Barthélémy, A., Appel, P., Maletinsky, P., Kim, J.-V., Chauleau, J.Y., Jaouen, N., Viret, M., Bibes, M., Fusil, S., Jacques, V.: Real-space imaging of non-collinear antiferromagnetic order with a single-spin magnetometer. Nature 549(7671), 252 (2017) https://doi.org/10.1038/nature23656 . Accessed 2017-12-04
  30. [30]Chu, Y.-H., Zhan, Q., Martin, L.W., Cruz, M.P., Yang, P.-L., Pabst, G.W., Zavaliche, F., Yang, S.-Y., Zhang, J.-X., Chen, L.-Q., Schlom, D.G., Lin, I.-N., Wu, T.-B., Ramesh, R.: Nanoscale Domain Control in Multiferroic BiFeO3 Thin Films. Advanced Materials 18(17), 2307–2311 (2006) https://doi.org/10.1002/adma.200601098 . _eprint: https://onlinelibrary.wiley.com/doi/pdf/10.1002/adma.200601098. Accessed 2023-07-14
  31. [31]Martin, L.W., Chu, Y.-H., Holcomb, M.B., Huijben, M., Yu, P., Han, S.-J., Lee, D., Wang, S.X., Ramesh, R.: Nanoscale Control of Exchange Bias with BiFeO3 Thin Films. Nano Letters 8(7), 2050–2055 (2008) https://doi.org/10.1021/nl801391m
  32. [32]Sando, D., Agbelele, A., Rahmedov, D., Liu, J., Rovillain, P., Toulouse, C., Infante, I.C., Pyatakov, A.P., Fusil, S., Jacquet, E., Carrétero, C., Deranlot, C., Lisenkov, S., Wang, D., Le Breton, J.-M., Cazayous, M., Sacuto, A., Juraszek, J., Zvezdin, A.K., Bellaiche, L., Dkhil, B., Barthélémy, A., Bibes, M.: Crafting the magnonic and spintronic response of BiFeO3 films by epitaxial strain. Nature Materials 12(7), 641–646 (2013) https://doi.org/10.1038/nmat3629 . Accessed 2018-03-25
  33. [33]Haykal, A., Fischer, J., Akhtar, W., Chauleau, J.-Y., Sando, D., Finco, A., Godel, F., Birkhölzer, Y.A., Carrétero, C., Jaouen, N., Bibes, M., Viret, M., Fusil, S., Jacques, V., Garcia, V.: Antiferromagnetic textures in BiFeO3 controlled by strain and electric field. Nature Communications 11(1), 1704 (2020) https://doi.org/10.1038/s41467-020-15501-8 . Number: 1 Publisher: Nature Publishing Group. Accessed 2023-06-15
  34. [34]Chu, Y.-H., Cruz, M.P., Yang, C.-H., Martin, L.W., Yang, P.-L., Zhang, J.-X., Lee, K., Yu, P., Chen, L.-Q., Ramesh, R.: Domain Control in Multiferroic BiFeO3 through Substrate Vicinality. Advanced Materials 19(18), 2662–2666 (2007) https://doi.org/10.1002/adma.200602972 . _ eprint: https://onlinelibrary.wiley.com/doi/pdf/10.1002/adma.200602972. Accessed 2023-10-02
  35. [35]Meisenheimer, P., Moore, G.C., Zhou, S., Zhang, H., Huang, X., Husain, S., Chen, X., Martin, L.W., Persson, K.A., Griffin, S.M., Caretta, L., Stevenson, P., Ramesh, R.: Persistent anisotropy of the spin cycloid in BiFeO3 through ferroelectric switching. Science Advances under review
  36. [36]Cornelissen, L.J., Liu, J., Duine, R.A., Youssef, J.B., Wees, B.J.: Long-distance transport of magnon spin information in a magnetic insulator at room temperature. Nature Physics 11(12), 1022–1026 (2015) https://doi.org/10.1038/nphys3465 . Number: 12 Publisher: Nature Publishing Group. Accessed 2023-09-12
  37. [37]Wesenberg, D., Liu, T., Balzar, D., Wu, M., Zink, B.L.: Long-distance spin transport in a disordered magnetic insulator. Nature Physics 13(10), 987–993 (2017) https://doi.org/10.1038/nphys4175 . Number: 10 Publisher: Nature Publishing Group. Accessed 2023-10-04
  38. [38]Huang, X., Sayed, S., Mittelstaedt, J., Susarla, S., Karimeddiny, S., Caretta, L., Zhang, H., Stoica, V.A., Gosavi, T., Mahfouzi, F., Sun, Q., Ercius, P., Kioussis, N., Salahuddin, S., Ralph, D.C., Ramesh, R.: Novel Spin–Orbit Torque Generation at Room Temperature in an All-Oxide Epitaxial La0.7Sr0.3MnO3/SrIrO3 System. Advanced Materials 33(24), 2008269 (2021) https://doi.org/10.1002/adma.202008269 . _ eprint: https://onlinelibrary.wiley.com/doi/pdf/10.1002/adma.202008269. Accessed 2023-01-08
  39. [39]Park, J.-G., Le, M.D., Jeong, J., Lee, S.: Structure and spin dynamics of multiferroic BiFeO3. Journal of Physics: Condensed Matter 26(43), 433202 (2014) https://doi.org/10.1088/0953-8984/26/43/433202 . Publisher: IOP Publishing. Accessed 2023-07-07
  40. [40]Sosnowska, I., Zvezdin, A.K.: Origin of the long period magnetic ordering in BiFeO3. Journal of Magnetism and Magnetic Materials 140–144, 167–168 (1995) https://doi.org/10.1016/0304-8853(94)01120-6 . Accessed 2023-12-03
  41. [41]Kadomtseva, A.M., Popov, Y.F., Pyatakov, A.P., Vorob’ev, G.P., Zvezdin, A.K., Viehland, D.: Phase transitions in multiferroic BiFeO3 crystals, thin-layers, and ceramics: enduring potential for a single phase, room-temperature magnetoelectric ‘holy grail’. Phase Transitions 79(12), 1019–1042 (2006) https://doi.org/10.1080/01411590601067235 . Publisher: Taylor & Francis _eprint: https://doi.org/10.1080/01411590601067235. Accessed 2023-12-03
  42. [42]Park, H.S., Yu, X., Aizawa, S., Tanigaki, T., Akashi, T., Takahashi, Y., Matsuda, T., Kanazawa, N., Onose, Y., Shindo, D., Tonomura, A., Tokura, Y.: Observation of the magnetic flux and three-dimensional structure of skyrmion lattices by electron holography. Nature Nanotechnology 9(5), 337–342 (2014) https://doi.org/10.1038/nnano.2014.52 . Number: 5 Publisher: Nature Publishing Group. Accessed 2023-05-11
  43. [43]Gitgeatpong, G., Zhao, Y., Piyawongwatthana, P., Qiu, Y., Harriger, L., Butch, N., Sato, T., Matan, K.: Nonreciprocal Magnons and Symmetry-Breaking in the Noncentrosymmetric Antiferromagnet. Physical Review Letters 119(4), 047201 (2017) https://doi.org/10.1103/PhysRevLett.119.047201 . Publisher: American Physical Society. Accessed 2023-11-07
  44. [44]Santos, F.J., Santos Dias, M., Lounis, S.: Nonreciprocity of spin waves in noncollinear magnets due to the Dzyaloshinskii-Moriya interaction. Physical Review B 102(10), 104401 (2020) https://doi.org/10.1103/PhysRevB.102.104401 . Publisher: American Physical Society. Accessed 2023-11-07
  45. [45]Kawano, M., Onose, Y., Hotta, C.: Designing Rashba–Dresselhaus effect in magnetic insulators. Communications Physics 2(1), 1–8 (2019) https://doi.org/10.1038/s42005-019-0128-6 . Number: 1 Publisher: Nature Publishing Group. Accessed 2023-11-07
  46. [46]Kawano, M., Hotta, C.: Discovering momentum-dependent magnon spin texture in insulating antiferromagnets: Role of the Kitaev interaction. Physical Review B 100(17), 174402 (2019) https://doi.org/10.1103/PhysRevB.100.174402 . Publisher: American Physical Society. Accessed 2023-11-07
  47. [47]Shiomi, Y., Takashima, R., Okuyama, D., Gitgeatpong, G., Piyawongwatthana, P., Matan, K., Sato, T.J., Saitoh, E.: Spin Seebeck effect in the polar antiferromagnet α-Cu₂Mn₂O₇. Physical Review B 96(18), 180414 (2017) https://doi.org/10.1103/PhysRevB.96.180414 . Publisher: American Physical Society. Accessed 2023-11-07
  48. [48]Bhattacharjee, S., Rahmedov, D., Wang, D., Íñiguez, J., Bellaiche, L.: Ultrafast Switching of the Electric Polarization and Magnetic Chirality in BiFeO3 by an Electric Field. Physical Review Letters 112(14), 147601 (2014) https://doi.org/10.1103/PhysRevLett.112.147601

Paper details

vlnc:W_ur2sc46g
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents