betaFeedback

WorksPhysics and Astronomy

Si- and C-Induced Modifications in Vapor-Solid-Grown InGaAs Nanowires: From Crystal Structure to Carrier Dynamics

Abstract

Determining the impact of dopants in ternary III-V nanowires (NWs) is crucial for their applications in next-generation optoelectronic and photonic devices; however, the interplay between dopant species, crystal structure, and carrier dynamics in vapor-solid-grown InGaAs NWs remains underexplored. In this study, the influence of silicon (Si) and carbon (C) doping on the structural, morphological, and optical properties of catalyst-free, selective-area grown InGaAs NWs fabricated by molecular beam epitaxy is investigated. Scanning electron microscopy demonstrates that C-doping increases the NW aspect ratio by over 100% compared to undoped NWs, while a concomitant decrease in their planar defect density is observed, indicating enhanced crystal quality with C-doping. Despite their superior crystal quality, the C-doped NWs present a diminished photoluminescence intensity, due to point defects and increased surface recombination velocity. This is further supported by time-resolved photoluminescence spectroscopy, revealing accelerated non-radiative recombination in the C-doped NWs. Lastly, hot-carrier effects in these nanostructures are studied, and their signatures remain observable, albeit with reduced intensity in both Si- and C-doped NWs. This comprehensive study establishes clear correlations between doping parameters and the resulting material characteristics and carrier dynamics, offering valuable insights into the fundamental mechanisms governing the VS-grown InGaAs NWs and their implications in optoelectronic devices.

Introduction

III–V ternary semiconductor NWs have emerged as highly versatile building blocks for next-generation optoelectronic and photonic devices, mainly owing to their favorable one-dimensional (1D1\mathrm{D}) geometry, high photoabsorptivity, and the possibility of their monolithic integration onto silicon substrates [1, 2, 3]. InGaAs NWs on Si are the focus of extensive research due to their potential in next-generation photovoltaics [4, 5, 6], integrated photonics [7, 8], and high-performance gate-all-around III–V/Si transistors [9]. The small carrier effective mass, high carrier mobility, and the compositional tunability of this ternary alloy across a wide bandgap spectrum, encompassing significant near-infrared and telecommunications wavelengths, render these NWs particularly appealing for both classical and quantum photonic applications [10, 11].

One promising approach to fabricating InGaAs NWs and precisely controlling their chemical composition is the catalyst-free, vapor-solid (VS) growth mode. A crucial factor influencing the performance of InGaAs NWs is their crystalline structure [12]. Unlike bulk InGaAs, which predominantly crystallizes in the zinc blende (ZB) phase [13], NWs readily exhibit a mixed polytypic phase characterized by stacking faults and rotational-twin defects [10, 14]. Depending on the flux rate and growth kinetics, the NW microstructure alternates between ZB and wurtzite (WZ) domains, leading to a disordered layer stacking [15, 16, 17]. The fabrication of NWs by the VS-growth mode is particularly pertinent in this context, as it depends on an imbalance in facet-growth velocities and twin-defect formation, which typically yields a higher density of stacking faults than vapor–liquid–solid (VLS) growth [15, 18]. Therefore, understanding and mitigating these structural imperfections are crucial for the prospective applications of VS-grown InGaAs NWs. Numerous approaches have been implemented to reduce defect density and enhance the material properties of NWs, including precise control of growth parameters [19, 20], adjusting their diameters [18, 21], and incorporating dilute elements or surfactants during NW fabrication [22, 23, 24]. Many of these approaches modify the surface energy of NW facets and promote the formation of a specific crystal phase over others, thereby reducing defect density [19, 21].

An additional important aspect for NW-based devices is intentional doping, which is indispensable for controlling the carrier type, concentration, and, ultimately, the optical and transport properties [25, 26, 27]. Silicon (Si) and carbon (C) serve as the most prevalent n-type and p-type dopants for III–V compounds, respectively; however, owing to their amphoteric nature and growth conditions, their behavior within NWs is markedly complex [28, 29]. In other words, these elements may substitute either anion or cation lattice sites contingent upon flux conditions and growth parameters, thereby partially counteracting the intended doping effects [29]. Ruhstorfer et al. [30] demonstrated that Si-doping at low fluxes in VS-grown GaAs NWs predominantly exhibits n-type characteristics, whereas increasing the doping concentration induces self-compensation effects via the formation of Si-induced complexes, leading to reduced overall n-doping properties [31]. Furthermore, doping species have the potential to alter the microstructural and optical-electrical characteristics of the system by modifying defect densities and scattering centers [32, 33].

Despite significant advances in understanding the effects of individual doping elements in binary III–V NWs, a comprehensive and systematic investigation of how Si- and C-doping influences the material properties and carrier dynamics of VS-grown InGaAs NWs remains insufficiently explored. In the present study, we aim to address these aspects by providing a comprehensive structural and spectroscopic analysis of Si- and C-doped InGaAs NWs synthesized via vapor-solid molecular beam epitaxy (VS-MBE). Here, we conduct a thorough examination of the evolution of crystal phases, NW morphology, and the dynamics of carrier recombination, all as functions of the type of doping species employed and their respective concentrations.

Results and Discussions

High-uniformity arrays of In0.20Ga0.80As\mathrm{In}_{0.20}\mathrm{Ga}_{0.80}\mathrm{As} NWs were grown by catalyst-free, selective-area epitaxy on prepatterned SiO2/Si(111)\mathrm{SiO}_{2}/\mathrm{Si}(111) substrates using molecular beam epitaxy (MBE). Hereby, in the SiO2\mathrm{SiO}_{2}-mask layer (20-nm thick) periodic mask openings (diameter of 60 nm) were created through a combination of electron beam lithography and wet chemical etching to induce site-selective NW nucleation. Details regarding the wafer preparation process and conditions for NW nucleation are presented elsewhere [30]. Five NW-arrays were grown, one intrinsically undoped, two Si-doped, and two C-doped. The NWs were grown at a substrate temperature of 595 °C, as measured by an optical pyrometer, under an arsenic (As4\mathrm{As}_{4}) overpressure of 4.5×10−54.5 \times10^{-5} mbar, utilizing a valved As cracker source. The flux rates of the group-III elements, indium (In) and gallium (Ga), were maintained at 0.31 Å/s and 0.275 Å/s, respectively, resulting in a V/III ratio of 42. The growth duration for the core InGaAs NWs was 120 min, followed by the deposition of a 49-minute long In0.20Al0.80As\mathrm{In}_{0.20}\mathrm{Al}_{0.80}\mathrm{As} shell layer aimed at passivating the NWs and enhancing their quantum yield of luminescence.

DopantsHeating current (A)Doping Concentration (cm−3^{-3})
Si8[n] = 1 x 1018^{18}
Si9[n] = 3 x 1018^{18}
C46[p] = 4 x 1017^{17}
C49[p] = 2 x 1018^{18}

Table 1. Nominal Si- and C-doping concentrations of the InGaAs NWs determined by secondary ion mass spectrometry on GaAs(001) planar reference layers..

Doping was performed only during the core-InGaAs NW growth, while the InAlAs shell remains undoped in all structures. In this study, Si- and C-dopants were introduced by heating a silicon filament and a graphite filament within sublimation sources during NW growth. The evaporation rates of these dopants are controlled through precise adjustments to the heating current (in units of Ampere) supplied to the filaments, and calibrated using planar GaAs reference layers. Table 1 provides information regarding the nominal Si- and C-concentrations as determined by Secondary Ion Mass Spectrometry (SIMS) on the GaAs(001) planar reference layers. Although the chemical dopant concentration was not measured directly in the NW samples, we anticipate similar concentration values as for the planar reference layers. This was recently confirmed in correlated atom probe tomography studies performed on Si-doped GaAs NWs [31]. Likewise, unintentionally doped InGaAs NWs in the Ga-rich limit exhibit intrinsically n-type behavior with an estimated doping concentration in the ∼1017\sim10^{17} cm−3^{-3} range, based on recent studies [10, 34, 35].

Figure 1 shows scanning electron microscopy (SEM) images of the InGaAs NWs: (a) undoped, (b) low Si-doped (heating current of 8A), and (c) low C-doped (heating current of 46A). High-resolution X-ray diffraction (XRD) measurements confirm identical chemical compositions across all the investigated samples, irrespective of doping. It is observed that the Si-doped NWs exhibit a larger diameter compared to their undoped counterpart, while their length is reduced (see also Figure S1 in the Supporting Material). Conversely, the C-doped NWs demonstrate higher axial growth rates than the undoped NWs. This effect is reflected in the aspect ratio (the ratio of length to diameter) of the NWs, wherein C(46A)-doping approximately doubles the aspect ratio compared to undoped NWs, whereas Si-doping markedly decreases the aspect ratio of the InGaAs NWs. Salehzadeh et al. [36] observed a similar enhancement in the axial growth rate of gold-assisted GaAs NWs grown in the presence of CBr4\mathrm{CBr}_{4} precursor, and attributed this striking effect to the suppression of 2D planar growth induced by this precursor. Also, a possible passivation of dangling bonds on the surface of the GaAs NWs by the precursor was proposed [36], leading to enhanced adatom surface diffusion and an increased axial growth rate.

SEM images and aspect ratio of InGaAs NW arrays

Figure 1. SEM images of the (a) undoped, (b) Si(8Å)-doped, and (c) C(46Å)-doped InGaAs NW arrays. (d) Aspect ratio of the InGaAs NWs of different doping species and concentrations.

Dependence of the diameter and length of InGaAs NWs with various doping species and concentrations

Figure S1. Dependence of the diameter and length of InGaAs NWs with various doping species and concentrations is observed. It is noted that increasing Si doping results in thicker NWs compared to undoped structures, while their length diminishes. Conversely, C-doped NWs with a 46A heating current exhibit the smallest diameter and the greatest length. However, at the highest level of C doping, (49A), the radial growth rate increases, whereas the axial growth rate decreases to lower values.

The reduction in axial growth rate by Si-doping was also observed in Si-doped GaAs(Sb) NWs [23] and InAs NWs [37], where the doped NWs exhibit a decrease in their length. The underlying cause of this enhanced lateral growth was attributed to Si segregation at the NW sidewall and consequent reduction in the adatom diffusion length of group-III species, promoting radial growth along the side facets [37].

The doping species further influence the microstructural properties of the NW, such as crystal layer stacking and defect density. To obtain deeper insight into the distinct growth dynamics of Si- and C-doping in the InGaAs NWs, high-resolution scanning transmission-electron microscopy (HR-STEM) was conducted, as illustrated in Figure 2. The high angle annular dark field (HAADF) images in Figure 2(a) and (b) show small segments of the Si- and C-doped NWs, respectively; however, the analysis to estimate the defect density, as shown in Figure 2(c), was performed for various sections along the NWs to provide statistically relevant data. The STEM results reveal that while the ZB phase remains the predominant crystal structure, rotational twins are observed along the NWs. Such planar defects generate atomically sharp local type-II band alignment, which can trap carriers and create scattering centers, thereby degrading the optical and electrical performance of NWs [12, 38]. Figure 2(a) demonstrates that the incorporation of Si into the core NW substantially increases the density of twin defects along the growth direction, consequently affecting the crystal phase purity. Similar observations of increased defect density due to Si-doping have been reported in various III-V NWs [21, 39].

High-resolution TEM micrographs and defect density plot for Si-doped, C-doped, and undoped InGaAs NWs

Figure 2. High-resolution TEM micrographs of the (a) Si(8A)-doped and (b) C(46A)-doped InGaAs NWs. Zincblende (ZB) crystal layer stacking is observed, but with a high density of rotational twin domains (labeled as ZB-A, ZB-B). (c) Density of rotational twin defects for the InGaAs NWs of different doping. The change in contrast and brightness is due to a thickness gradient in that region.

In contrast, C-doping demonstrates an enhancement in crystal quality by decreasing the density of twin defects, as illustrated in Figure 2(c), leading to larger ZB domains within the InGaAs NWs.

A comparable observation has been reported in VLS-grown C-doped GaAs NWs, whereby in this growth mode a strong tendency towards phase-pure ZB crystal structure devoid of planar defects is seen [36]. The origin of such an enhanced crystal quality was ascribed to an increased axial growth rate, which leads to a decreased proportion of WZ to ZB. Similar findings regarding the relationship between the axial growth rate and the phase purity of NWs have also been reported by Joyce et al. [20] and Spirkoska et al. [40] concerning VLS-grown GaAs NWs.

Furthermore, dopant species can alter the optical properties of nanostructures by introducing subgap states and modifications in the crystal lattice [33]. Figure 3 illustrates the PL spectra of (a) the undoped, (b) the Si(8A)-doped, and (c) the C(46A)-doped InGaAs NWs at 10 K under various excitation powers, revealing discernible differences among the NWs. The PL spectra of the Si(9A)-doped and C(49A)-doped InGaAs NWs at 10 K are shown in Figure S2 in the Supporting Material for reference. The findings demonstrate that doping leads to linewidth broadening in the PL spectra and clearly affects the emission intensity. The increase in spectral linewidth is more pronounced in the Si-doped NWs than in the C-doped ones, due to greater crystalline disorder resulting from dopant incorporation and the band-filling (or Burstein-Moss) effect [33]. Arab et al. [35] examined the PL emission of Si-doped GaAs NWs and observed an increase in linewidth broadening correlated with increasing doping concentrations. They attributed this spectral broadening to the formation of various recombination centers induced by the doping process. In a separate study conducted by Ruhstorfer et al. [30], the impact of Si doping on the optical properties of GaAs NWs was also investigated, with findings indicating that increased doping concentrations lead to an expansion of the PL linewidth and a blue-shift of the peak position towards higher energies, attributable to the band-filling effect.

PL spectra and power-dependent integrated PL intensity of InGaAs nanowires

Figure 3. PL spectra of the (a) undoped, (b) Si(8A)-doped, and (c) C(46A)-doped InGaAs NWs at 10 K under absorbed power densities from 30 W/cm2^{2} to 6000 W/cm2^{2}. (d) Power-dependent integrated PL intensity of the NWs of varying doping species and concentrations at 10 K.

The PL spectra of the Si(9A)- and C(49A)-doped InGaAs NWs at 10 K under various excitation powers

Figure S2. The PL spectra of the Si(9A)- and C(49A)-doped InGaAs NWs at 10 K under various excitation powers.

Furthermore, the C-doped NWs also exhibit an increase in linewidth broadening relative to the undoped NWs. The origin of this effect is attributed to the Burstein-Moss effect, arising from a combination of direct and indirect optical transitions driven by deeper Fermi-level penetration into the valence band [41, 42]. As the excitation power increases, optical transitions are no longer confined to the band edge but can originate from a broader range of kk-states, thereby smearing the emission spectrum [43]. Additionally, the relaxation of kk-selection rules, induced by the disruption of crystal periodicity, makes phonon-assisted and indirect transitions optically active, thereby increasing the spectral width [41, 44, 45].

In addition, the influence of doping on the NWs is also reflected in their quantum yield of luminescence due to modifications of carrier dynamics at the presence of defects [42]. Figure 3(d) illustrates the results of the integrated PL intensity of the NWs at 10 K versus the absorbed power density. Increasing the excitation power increases the emitted PL intensity, irrespective of doping. However, while the undoped NWs maintain the highest intensity, the Si- and C-doped samples show an up to three orders of magnitude decrease in intensity. The stronger decrease in the quantum yield of luminescence observed in the C-doped InGaAs NWs compared with the Si-doped NWs (despite their lower dopant concentration), is most likely arising from an interplay between minority-carrier dynamics, surface recombination, and carbon-induced defects [46, 47, 48]. The rate equation analysis is carried out for the NWs with various dopant species, as illustrated in Figure S3 in the Supporting Material. The results indicate that, while Auger recombination predominantly contributes to the undoped NWs, increasing doping concentrations results in a shift in recombination dynamics toward the Shockley-Read-Hall (SRH) mechanism. In the Si- and C-doped NWs, one main distinction emerges from the nature of the minority carriers. In the C-doped NWs, the minority carriers are electrons, which exhibit substantially higher mobilities than holes in GaAs, due to the mismatch in their mass, by approximately an order of magnitude [49]. This elevated mobility enables their diffusion toward NW facets, where they can be captured by surface trap states and undergo non-radiative recombination. Conversely, in the Si-doped NWs, holes serve as the minority carriers, and due to their comparatively lower mobility, they are more prone to recombine within the bulk prior to reaching the surface, thereby increasing the likelihood of radiative recombination [46]. Consequently, the inherent differences in the nature of the minority carriers in these doped structures significantly influence their recombination dynamics.

Plot showing the slope of the rate equation for Si-doped, undoped, and C-doped InGaAs nanowires

Figure S3. The results of rate-equation analysis for InGaAs NWs with various dopings. The rate equation model is given by:

PAbs.=AIPL1/2+BIPL+CIPL3/2.(3)P_{\mathrm{Abs.}} = A I_{\mathrm{PL}}^{1/2} + B I_{\mathrm{PL}} + C I_{\mathrm{PL}}^{3/2}. \tag*{(3)}

The first term corresponds to Shockley-Read-Hall (SRH) recombination, the second to radiative recombination, and the third to Auger recombination. The coefficients assigned to these mechanisms are A, B, and C, respectively. Their relative impacts can be directly determined from the slope of the absorbed power density versus the integrated PL intensity in a double logarithmic plot. It is seen that Auger recombination is strongest for the undoped NWs, i.e. the slope is ~1.5, while by increasing doping (both Si- and C-doped), the recombination dynamics shift toward SRH recombination.

Furthermore, Boland et al. [49] studied the impact of band bending on the surface of Si- and C-doped GaAs NWs on the recombination dynamics of charge carriers. Their findings indicate that the downward band bending, induced by C-doping on the surface of the GaAs NWs [50], facilitates the injection of electrons into surface traps, thereby accelerating their non-radiative recombination [49]. In contrast, the n-doped NWs exhibit upward band-bending at the surface, and since holes, as minority carriers in these nanostructures, have lower mobility than electrons, they are therefore more likely to recombine within the bulk before reaching the nonradiative surface states. This phenomenon can indeed be effectively examined by determining the surface recombination velocity in the InGaAs NWs using time-resolved photoluminescence (TRPL) spectroscopy [12, 51].

Figure 4 illustrates the TRPL results of the InGaAs NWs under various excitation power densities at 10 K, and the dashed-gray line shows the instrument response function (IRF) of the system. The results of TRPL signals at 10 K for the Si(9A)- and C(49A)-doped NWs are shown in Figure S4 in the Supporting Materials. The results indicate a strong dependence in the recombination dynamics of photogenerated carriers on dopants in the NWs. At higher excitation power densities, where the contributions of Auger and radiative recombination are large, the decay rate is higher, whereas reducing the power density can intensify the contribution of the Shockley-Read-Hall (SRH) process in the system [52]. Moreover, the comparison of the TRPL results for the (a) undoped and the (b) Si- and (c) C-doped NWs indicates that the recombination dynamics accelerate when the InGaAs NWs are doped with Si and C, consistent with the results of the integrated PL intensity of the NWs, which originates from accelerated non-radiative recombination. Notably, this effect is significant for the C-doped NWs, particularly at higher excitation powers, where the accelerated recombination is beyond the time resolution of the optical apparatus. To determine the influence of trap states at the surface on the dynamics of recombination, the surface recombination velocity (vsv_s) of the NWs is determined using the following equation [51]:

TRPL spectra and surface recombination velocity for undoped, Si(8A)-doped, and C(46A)-doped InGaAs NWs

Figure 4. TRPL spectra at 10 K of (a) the undoped, (b) Si(8A)-doped, and (c) C(46A)-doped InGaAs NWs at various absorbed powers densities from 30 W/cm230\ \mathrm{W}/\mathrm{cm}^{2} to 6000 W/cm26000\ \mathrm{W}/\mathrm{cm}^{2}. The dashed-gray line indicates the instrument response function (IRF) of the optical setup. (d) Surface recombination velocity for different NWs at 10 K. It is seen that the undoped and the C-doped NWs show the lowest and the highest recombination velocities, respectively.

TRPL signals of the Si(9A)- and C(49A)-doped NWs at 10 K under various excitation powers

Figure S4. TRPL signals of the Si(9A)- and C(49A)-doped NWs at 10 K under various excitation powers. No noticeable change in the spectra is observed, as they exhibit behavior analogous to the instrument response function (IRF), suggesting that the recombination dynamics occur at a rate faster than the temporal resolution of the TRPL apparatus.

τTRPL−1=(4d)vs+τBulk−1,(1)\tau_{TRPL}^{-1} = \left(\frac{4}{d}\right) v_s + \tau_{Bulk}^{-1}, \tag*{(1)}

where "τTRPL\tau_{TRPL}" and "τBulk\tau_{Bulk}" are the lifetimes determined from the TRPL spectra and from the bulk, respectively, and "dd" is the NW diameter. The bulk lifetime is estimated to be 18 ns at 10 K, determined from core-shell InGaAs NWs of similar chemical composition [12], which is consistent with reported values for the recombination lifetime of core-shell InGaAs/InP NWs [53]. Figure 4(d) illustrates the surface recombination velocity for the undoped and doped NWs, and it is seen that the undoped NWs possess the lowest surface recombination velocity, which agrees with their higher PL intensities. Additionally, the results indicate that the C(46A)-doped NWs have the highest surface recombination velocity, suggesting that their higher rates of non-radiative recombination, despite their improved crystal quality, could originate from enhanced recombination at the surface [49].

In addition, the recombination dynamics can also influence the properties of non-equilibrium photogenerated carriers and their rates of thermalization in the system. To investigate these dynamics, the emitted PL spectra are analyzed by the generalized Planck’s radiation law, as given by [54, 55]:

IPL(E)=2πA(E)(E)2h3c2[exp⁡(E−ΔμkBT)−1]−1,(2)I_{PL}(E) = \frac{2\pi A(E)(E)^2}{h^3c^2}\left[\exp\left(\frac{E-\Delta\mu}{k_BT}\right)-1\right]^{-1}, \tag*{(2)}

where, "IPLI_{PL}" denotes the emitted PL intensity, "A(E)A(E)" the energy-dependent absorptivity, "hh" Planck’s constant, "kBk_B" Boltzmann’s constant, and "cc" the speed of light. The thermodynamic properties of hot carriers are characterized by the carrier temperature "TT" and the quasi-Fermi level splitting "Δμ\Delta\mu", respectively. The details of the analysis for similar material systems are presented elsewhere [6, 56].

Figure 5 demonstrates the dependence of the non-equilibrium hot carrier temperature (ΔT\Delta T: the temperature difference between the hot carrier temperature and the lattice) on the absorbed power density at 10 K for the three NW arrays. The system without doping has the highest carrier temperature, and the effects of hot carriers diminish as the NWs are doped with Si and C. The weaker hot-carrier effects in doped NWs are attributed to increased non-radiative thermalization channels, which accelerate hot-carrier relaxation and lower their temperature. These results are significant for NW-based hot-carrier solar cells, where the contributions of hot carriers in doped regions can further improve the performance of these devices.

Hot-carrier temperature of the InGaAs NWs with different doping as a function of the absorbed power density at 10 K

Figure 5. Hot-carrier temperature of the InGaAs NWs with different doping as a function of the absorbed power density at 10 K.

Conclusions

In summary, we have presented a thorough study of the effects of Si- and C-doping on the structural, morphological, and optical characteristics of catalyst-free, VS-grown InGaAs NWs fabricated by selective-area molecular beam epitaxy. The results indicate that the C-doped InGaAs NWs demonstrate a significant increase in axial growth rate and improved crystal quality with a reduced density of planar defects. Additionally, upon Si- and C-doping, the PL spectra broaden, with the effect being more pronounced in Si-doped NWs, consistent with their higher defect density and the band-filling effect. Despite the higher crystal quality of C-doped NWs, their integrated PL intensity diminishes, and their TRPL signals indicate an enhancement in the decay rates of photogenerated carriers within these nanostructures. The findings indicate that the origin of such accelerated non-radiative recombination is attributed to the enhanced surface recombination velocity, which can deplete carriers non-radiatively. Ultimately, evidence of non-equilibrium hot populations is observed in the InGaAs NWs (undoped and doped), a phenomenon of significance for hot-carrier-based devices.

Acknowledgements

This work was supported by the Deutsche Forschungsgemeinschaft (German Research Foundation, DFG) through Germany’s Excellence Strategy via the Cluster of Excellence econversion (EXC 2089/1-390776260). HE also acknowledges Marie Sklodowska-Curie Actions (MSCA) for support via the TUM EuroTechPostdoc2 Grant Agreement (No. 899987). LN acknowledges funding by the Deutsche Forschungsgemeinschaft via the Emmy Noether Programme – Project No. 578097784.

References

  1. [1]Qarony W, Hossain MI, Tamang A, Jovanov V, Shahiduzzaman Md, Ahamed MdS, et al. On the potential of optical nanoantennas for visibly transparent solar cells. ACS Photonics. 2023;10(12):4205–14. https://doi.org/10.1021/acsphotonics.3c00932
  2. [2]LaPierre RR, Chia ACE, Gibson SJ, Haapamaki CM, Boulanger J, Yee R, et al. III–V nanowire photovoltaics: Review of design for high efficiency. Physica Status Solidi (RRL) - Rapid Research Letters 2013;7(10):815–30. Available from: https://doi.org/10.1002/pssr.201307109
  3. [3]Hertenberger S, Funk S, Vizbaras K, Yadav A, Rudolph D, Becker J, et al. High compositional homogeneity in In-rich InGaAs nanowire arrays on nanoimprinted SiO2/Si (111). Applied Physics Letters 2012;101(4):043116. Available from: https://doi.org/10.1063/1.4738769
  4. [4]Treu J, Stettner T, Watzinger M, Morkötter S, Döblinger M, Matich S, et al. Lattice-Matched InGaAs–InAlAs Core–Shell Nanowires with Improved Luminescence and Photoresponse Properties. Nano Letters 2015;15(5):3533–40. Available from: https://doi.org/10.1021/acs.nanolett.5b00979
  5. [5]Fast J, Aeberhard U, Bremner SP, Linke H. Hot-carrier optoelectronic devices based on semiconductor nanowires. Applied Physics Reviews 2021;8(2). Available from: https://doi.org/10.1063/5.0038263
  6. [6]Esmaeilpour H, Isaev N, Makhfudz I, Döblinger M, Finley JJ, Koblmüller G. Strong dimensional and structural dependencies of hot carrier effects in InGaAs Nanowires: Implications for photovoltaic solar cells. ACS Applied Nano Materials 2024;7(3):2817–24. Available from: https://doi.org/10.1021/acsanm.3c05041
  7. [7]Kim H, Lee W-J, Farrell AC, Morales JSD, Senanayake P, Prikhodko SV, et al. Monolithic InGaAs nanowire array lasers on Silicon-on-Insulator operating at room temperature. Nano Letters 2017;17(6):3465–70. Available from: https://doi.org/10.1021/acs.nanolett.7b00384
  8. [8]Kim H, Lee W, Chang T, Huffaker DL. Room-Temperature InGaAs Nanowire array Band-Edge lasers on patterned Silicon-on-Insulator platforms. Physica Status Solidi (RRL) - Rapid Research Letters 2018;13(3). Available from: https://doi.org/10.1002/pssr.201800489
  9. [9]Tomioka K, Yoshimura M, Fukui T. A III–V nanowire channel on silicon for high-performance vertical transistors. Nature 2012;488(7410):189–92. Available from: https://doi.org/10.1038/nature11293
  10. [10]Koblmüller G, Abstreiter G. Growth and properties of InGaAs nanowires on silicon. Physica Status Solidi (RRL) - Rapid Research Letters 2013;8(1):11–30. Available from: https://doi.org/10.1002/pssr.201308207
  11. [11]Treu J, Speckbacher M, Saller K, Morkötter S, Döblinger M, Xu X, et al. Widely tunable alloy composition and crystal structure in catalyst-free InGaAs nanowire arrays grown by selective area molecular beam epitaxy. Applied Physics Letters 2016;108(5). Available from: https://doi.org/10.1063/1.4941407
  12. [12]Esmaielpour H, Isaev N, Finley JJ, Koblmüller G. Influence of Auger heating and Shockley-Read-Hall recombination on hot-carrier dynamics in InGaAs nanowires. Physical Review. B/Physical Review. B 2024a;109(23). Available from: https://doi.org/10.1103/physrevb.109.235303
  13. [13]S. Adachi, Properties of semiconductor alloys : group-IV, III-V and II-VI semiconductors, Wiley eBooks. 2009. Available from: http://ci.nii.ac.jp/ncid/BA89795341
  14. [14]Glas F, Harmand J-C, Patriarche G. Why does wurtzite form in nanowires of III-V zinc blende semiconductors? Physical Review Letters 2007;99(14):146101. Available from: https://doi.org/10.1103/physrevlett.99.146101
  15. [15]Ikeijiri K, Sato T, Yoshida H, Hiruma K, Motohisa J, Hara S, et al. Growth characteristics of GaAs nanowires obtained by selective area metal–organic vapour-phase epitaxy. Nanotechnology 2008;19(26):265604. Available from: https://doi.org/10.1088/0957-4484/19/26/265604
  16. [16]Liu Z, Merckling C, Rooyackers R, Richard O, Bender H, Mols Y, et al. Correlation between surface reconstruction and polytypism in InAs nanowire selective area epitaxy. Physical Review Materials 2017;1(7). Available from: https://doi.org/10.1103/physrevmaterials.1.074603
  17. [17]Morkötter S, Funk S, Liang M, Döblinger M, Hertenberger S, Treu J, et al. Role of microstructure on optical properties in high-uniformity In1−xGaAs nanowire arrays: Evidence of a wider wurtzite band gap. Physical Review B 2013;87(20). Available from: https://doi.org/10.1103/physrevb.87.205303
  18. [18]Yao M, Sheng C, Ge M, Chi C-Y, Cong S, Nakano A, et al. Facile Five-Step heteroepitaxial growth of GaAs nanowires on silicon substrates and the twin formation mechanism. ACS Nano 2016;10(2):2424–35. Available from: https://doi.org/10.1021/acsnano.5b07232
  19. [19]Yoshida H, Ikeijiri K, Sato T, Hara S, Hiruma K, Motohisa J, et al. Analysis of twin defects in GaAs nanowires and tetrahedra and their correlation to GaAs(111)B surface reconstructions in selective-area metal organic vapour-phase epitaxy. Journal of Crystal Growth 2009;312(1):52–7. Available from: https://doi.org/10.1016/j.jcrysgro.2009.10.006
  20. [20]Joyce HJ, Gao Q, Tan HH, Jagadish C, Kim Y, Fickenscher MA, et al. Unexpected benefits of rapid growth rate for III–V nanowires. Nano Letters 2008;9(2):695–701. Available from: https://doi.org/10.1021/nl803182c
  21. [21]Ruhstorfer D, Döblinger M, Riedl H, Finley JJ, Koblmüller G. Role of twin defects on growth dynamics and size distribution of undoped and Si-doped GaAs nanowires by selective area epitaxy. Journal of Applied Physics 2022;132(20). Available from: https://doi.org/10.1063/5.0124808
  22. [22]Sourribes MJL, Isakov I, Panfilova M, Liu H, Warburton PA. Mobility enhancement by SB-mediated minimisation of stacking fault density in INAS nanowires grown on silicon. Nano Letters 2014;14(3):1643–50. Available from: https://doi.org/10.1021/nl5001554
  23. [23]Ajay A, Jeong H, Schreitmüller T, Döblinger M, Ruhstorfer D, Mukhundhan N, et al. Enhanced growth and properties of non-catalytic GaAs nanowires via Sb surfactant effects. Applied Physics Letters 2022;121(7). Available from: https://doi.org/10.1063/5.0095952
  24. [24]Jeong HW, Koulas-Simos A, Limame I, Döblinger M, Kim SK, Palekar CC, Finley JJ, Reitzenstein S, Koblmüller G. Monolithic axial InGaAs quantum dot emitters in GaAs-based nanowires via Sb-mediated facet engineering. Nano Letters 2022;26(26;27):8834–8841. Available from: https://doi.org/10.1021/acs.nanolett.6c02123
  25. [25]Kim W, Güniat L, Morral AFI, Piazza V. Doping challenges and pathways to industrial scalability of III–V nanowire arrays. Applied Physics Reviews 2021;8(1). Available from: https://doi.org/10.1063/5.0031549
  26. [26]Chen H-L, Bidaud T, Scaccabarozzi A, De Lépinau R, Oehler F, Patriarche G, et al. Undoped and doped wurtzite GaAs probed by polarization- and time-resolved cathodoluminescence. Nanoscale Advances 2025;7(11):3387–95. Available from: https://doi.org/10.1039/d5na00206k
  27. [27]Orru M, Repiso E, Carapezzi S, Henning A, Rodaro S, Franciosi A, et al. A roadmap for controlled and efficient N-Type doping of Self-Assisted GaAs nanowires grown by molecular beam epitaxy. Advanced Functional Materials 2016;26(17):2836–45. Available from: https://doi.org/10.1002/adfm.201504853
  28. [28]Hijazi H, Monier G, Gil E, Trassoudaine A, Bougerol C, Leroux C, et al. Si doping of Vapor–Liquid–Solid GaAs nanowires: N-Type or P-Type? Nano Letters 2019;19(7):4498–504. Available from: https://doi.org/10.1021/acs.nanolett.9b01308
  29. [29]Ketterer B, Mikhееv E, Uccelli E, Morral AFI. Compensation mechanism in silicon-doped gallium arsenide nanowires. Applied Physics Letters 2010;97(22). Available from: https://doi.org/10.1063/1.3517254
  30. [30]Ruhstorfer D, Mejia S, Ramsteiner M, Döblinger M, Riedl H, Finley JJ, et al. Demonstration of n-type behavior in catalyst-free Si-doped GaAs nanowires grown by molecular beam epitaxy. Applied Physics Letters 2020;116(5). Available from: https://doi.org/10.1063/1.5134687
  31. [31]Schreitmüller T, Saluja DK, Mead CE, Ramsteiner M, Jeong HW, Esmaeilpour H, et al. Spatial dependence of dopant incorporation and electrical transport in Si-doped GaAs(Sb) nanowires. Physical Review Materials 2024;8(7). Available from: https://doi.org/10.1103/physrevmaterials.8.076002
  32. [32]Becker J, Hill MO, Sonner M, Treu J, Döblinger M, Hirler A, et al. Correlated chemical and electrically active dopant analysis in Catalyst-Free Si-Doped InAs nanowires. ACS Nano 2018;12(2):1603–10. Available from: https://doi.org/10.1021/acsnano.7b08197
  33. [33]Sonner M, Treu J, Saller K, Riedl H, Finley JJ, Koblmüller G. Carrier concentration dependent photoluminescence properties of Si-doped InAs nanowires. Applied Physics Letters 2018;112(9). Available from: https://doi.org/10.1063/1.5019350
  34. [34]Koblmüller G, Vizbaras K, Hertenberger S, Bolte S, Rudolph D, Becker J, et al. Diameter dependent optical emission properties of InAs nanowires grown on Si. Applied Physics Letters 2012;101(5):053103. Available from: https://doi.org/10.1063/1.4739001
  35. [35]Arab S, Yao M, Zhou C, Dapkus PD, Cronin SB. Doping concentration dependence of the photoluminescence spectra of n-type GaAs nanowires. Applied Physics Letters 2016;108(18). Available from: https://doi.org/10.1063/1.4947504
  36. [36]Salehzadeh O, Watkins SP. Effect of carbon tetrabromide on the morphology of GaAs nanowires. Nanotechnology 2011;22(16):165603. Available from: https://doi.org/10.1088/0957-4484/22/16/165603
  37. [37]Wirths S, Weis K, Winden A, Sladek K, Volk C, Alagha S, et al. Effect of Si-doping on InAs nanowire transport and morphology. Journal of Applied Physics 2011;110(5). Available from: https://doi.org/10.1063/1.3631026
  38. [38]Pemasiri K, Montazeri M, Gass R, Smith LM, Jackson HE, Yarrison-Rice J, et al. Carrier Dynamics and Quantum Confinement in type II ZB-WZ InP Nanowire Homostructures. Nano Letters 2009;9(2):648–54. Available from: https://doi.org/10.1021/nl802997p
  39. [39]Suzuki A, Fukuyama A, Suzuki H, Sakai K, Paek J-H, Yamaguchi M, et al. Zinc-blende and wurtzite phase separation in catalyst-free molecular beam epitaxy vapor–liquid–solid-grown Si-doped GaAs nanowires on a Si(111) substrate induced by Si doping. Japanese Journal of Applied Physics 2015b;54(3):035001. Available from: https://doi.org/10.7567/jjap.54.035001
  40. [40]Spirkoska D, Arbiol J, Gustafsson A, Conesa-Boj S, Glas F, Zardo I, et al. Structural and optical properties of high quality zinc-blende/wurtzite GaAs nanowire heterostructures. Physical Review B 2009;80(24). Available from: https://doi.org/10.1103/physrevb.80.245325
  41. [41]Olego D, Cardona M. Photoluminescence in heavily doped GaAs. I. Temperature and hole-concentration dependence. Physical Review B, Condensed Matter 1980;22(2):886–93. Available from: https://doi.org/10.1103/physrevb.22.886
  42. [42]Saddik KB, Braña AF, López N, García BJ, Fernández-Garrido S. Growth of silicon- and carbon-doped GaAs by chemical beam epitaxy using H2-diluted DTBSi and CBr4 precursors. Journal of Crystal Growth 2021;571:126242. Available from: https://doi.org/10.1016/j.jcrysgro.2021.126242
  43. [43]Kim S-I, Kim M-S, Kim Y, Eom KS, Min S-K, Lee C. Low temperature photoluminescence characteristics of carbon doped GaAs. Journal of Applied Physics 1993;73(9):4703–5. Available from: https://doi.org/10.1063/1.352740
  44. [44]Chen HD, Feng MS, Chen PA, Lin KCLKC, Wu JWJW. Photoluminescence of heavily P-Type-Doped GaAs: temperature and concentration dependences. Japanese Journal of Applied Physics 1994;33(4R):1920. Available from: https://doi.org/10.1143/jjap.33.1920
  45. [45]Sapriel J, Chavignon J, Alexandre F, Azoulay R, Sermage B, Rao K, et al. Above bandgap luminescence of p-type GaAs epitaxial layers. Solid State Communications 1991;79(6):543–6. Available from: https://doi.org/10.1016/0038-1098(91)90048-Z
  46. [46]Sager D, Gutsche C, Prost W, Tegude F -j., Bacher G. Recombination dynamics in single GaAs nanowires with an axial heterojunction: n- versus p-doped areas. Journal of Applied Physics 2013;113(17). Available from: https://doi.org/10.1063/1.4803488
  47. [47]Chang C-C, Chi C-Y, Yao M, Huang N, Chen C-C, Theiss J, et al. Electrical and optical characterization of surface passivation in GAAS nanowires. Nano Letters 2012;12(9):4484–9. Available from: https://doi.org/10.1021/nl301391h
  48. [48]Tan KH, Yoon SF, Huang QF, Zhang R, Sun ZZ, Jiang J, et al. Dicarbon defects in carbon-doped GaAs. Physical Review. B, Condensed Matter 2003;67(3). Available from: https://doi.org/10.1103/physrevb.67.035208
  49. [49]Boland JL, Casadei A, Tütncüoğlu G, Matteini F, Davies CL, Jabeen F, et al. Increased photoconductivity lifetime in GaAs nanowires by controlled N-Type and P-Type doping. ACS Nano 2016;10(4):4219–27. Available from: https://doi.org/10.1021/acsnano.5b07579
  50. [50]Chen H-L, De Lépinau R, Scaccabarozzi A, Oehler F, Harmand J-C, Cattoni A, et al. Quantitative Assessment of carrier density by Cathodoluminescence. II. GAAS nanowires. Physical Review Applied 2021;15(2). Available from: https://doi.org/10.1103/physrevapplied.15.024007
  51. [51]Ren D, Rong Z, Somsasudaram S, Azizur-Rahman KM, Liang B, Huffaker DL. A three-dimensional insight into correlation between carrier lifetime and surface recombination velocity for nanowires. Nanotechnology 2018;29(50):504003. Available from: https://doi.org/10.1088/1361-6528/aae365
  52. [52]Shao Y, Xiao Z, Bi C, Yuan Y, Huang J. Origin and elimination of photocurrent hysteresis by fullerene passivation in CH₃NH₃PbI₃ planar heterojunction solar cells. Nature Communications 2014;5(1):5784. Available from: https://doi.org/10.1038/ncomms6784
  53. [53]Azimi Z, Gopakumar A, Li L, Kremer F, Lockrey M, Wibowo AA, et al. Effective passivation of InGaAs nanowires for telecommunication wavelength optoelectronics. Advanced Optical Materials 2022;10(18). Available from: https://doi.org/10.1002/adom.202200739
  54. [54]Lasher G, Stern F. Spontaneous and stimulated recombination radiation in semiconductors. Physical Review 1964;133(2A):A553–63. Available from: https://doi.org/10.1103/physrev.133.a553
  55. [55]Wurfel P. The chemical potential of radiation. Journal of Physics C Solid State Physics 1982;15(18):3967–85. Available from: https://doi.org/10.1088/0022-3719/15/18/012
  56. [56]Esmaielpour H, Lombez L, Giteau M, Guillemoles J, Suchet D. Impact of excitation energy on hot carrier properties in InGaAs multi-quantum well structure. Progress in Photovoltaics Research and Applications 2022;30(11):1354–62. Available from: https://doi.org/10.1002/pip.3599

Paper details

vlnc:W_uxvkraju
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents