Vitrification-Devitrification Enables Tunable Photonic and Gas Sorption Properties of Zeolitic Imidazolate Frameworks

Abstract

Zeolitic imidazolate framework (ZIF) glasses represent an emerging family of melt-quenched glasses, which exhibit immense potential for applications in gas separation, energy storage, and optics. However, their intrinsic porosity remains elusive due to the inherent challenges in resolving their disordered atomistic structures. Here, we systematically investigate the porosity of ZIF-4 and ZIF-62 crystals and their corresponding glasses. CO2 sorption at 195 K enables quantitative assessment of microporosity in both crystalline and glassy states, allowing the accessible micropore volume of the ZIF glasses to be determined. Moreover, establishing a direct relationship between photonic properties and structural porosity in Zn-based ZIF glasses remains challenging. Here we demonstrate striking broadband blue-light emission from ZIF-4 glass annealed under optimized conditions. A pronounced red shift is observed when increasing the annealing temperature above the glass transition temperature. By correlating the evolution of photoluminescence with structural porosity, we reveal the interplay between the photonic and gas sorption properties of ZIF glasses. These findings provide new insights into the structure-property relationships of ZIF glasses and offer a pathway toward the rational design of multifunctional MOF glasses.

Introduction

Metal-organic frameworks (MOFs), known as nanoporous crystals, consist of metal ions coordinated to organic ligands and possess both large specific surface areas and tunable pore structures that enable various applications in gas adsorption[1, 2, 3], catalysis[4], and energy storage[5].

Zeolitic imidazolate frameworks (ZIFs), a subclass of MOFs, are constructed through Werner-type metal-ligand coordination[6] and can be transformed into the glass state via melt-quenching. In addition, ZIF glasses largely retain the pore structures of their crystalline precursor[7]. Although more than 250 crystalline ZIFs spanning over 50 distinct network topologies have been reported[8], only a small fraction have been demonstrated to melt and form glasses via melt-quenching. ZIF-4 (M(Im)2\mathrm{M}(\mathrm{Im})_2) and ZIF-62 (M(Im)2−x(bIm)x\mathrm{M}(\mathrm{Im})_{2-x}(\mathrm{bIm})_x) are representative glass-forming ZIFs, where M denotes a metal node such as Zn2+\mathrm{Zn}^{2+} or Co2+\mathrm{Co}^{2+}, and Im and bIm are imidazolate (C3H3N2−\mathrm{C}_3\mathrm{H}_3\mathrm{N}_2^{-}) and benzimidazolate (C7H5N2−\mathrm{C}_7\mathrm{H}_5\mathrm{N}_2^{-}) linkers, respectively[9, 10].

ZIF-62 demonstrates ultrahigh glass-forming ability and a wide temperature window of the molten state between its liquidus and decomposition temperatures[11]. Thus, ZIF-62 can be easily vitrified, e.g., by using the spark plasma sintering (SPS) technique[12]. The compounds Im and BIm play a critical role in organic luminescence due to their outstanding optical absorption and π\pi-π∗\pi^{*} electronic transition in the pp-orbital[13], while crystalline ZIF-62 exhibits luminescent properties that differ from those of its individual linkers[14]. That is, the luminescence behaviour depends on its structure and metal-ligand interactions, such as metal-to-ligand charge transfer (MLCT) and ligand-to-metal charge transfer (LMCT)[15]. However, ZIF-62 crystal only exhibits strong ultraviolet light emission, but not visible light emission for white LEDs, because of its too wide band gap (around 3.5 eV). To obtain visible light emission in ZIF-62, Li et al reported white-light emission, which was achieved by a vitrification-pressurization-annealing strategy. However, the white-light emission mechanism of annealed ZIF-62 glasses remains elusive due to the presence of two distinct emission centers associated with the Im and bIm ligands. Consequently, establishing a direct relationship between the photonic properties and ligand chemistry of Zn-based ZIF glasses remains challenging.

In addition to ZIF-62, ZIF-4 should be a simple case to establish a direct relationship between the photonic properties and ligand chemistry. Upon heating, crystalline ZIF-4 first collapses into a low-density amorphous phase at ~315 °C, subsequently transforms into a high-density amorphous phase, and then recrystallizes into the denser ZIF-zni polymorph at ~460 °C before melting at ~580 °C. Quenching the melt to room temperature yields a melt-quenched ZIF-4 glass[16]. Positron annihilation lifetime spectroscopy (PALS) revealed that melt-quenched ZIF-4 possesses residual microporosity[17]. However, this method cannot determine whether the pores identified in ZIF glasses are accessible to gas molecules, and thus whether they form an open pore network[18]. Therefore, PALS cannot readily provide a quantitative measure of porosity, such as the specific pore volume of ZIF glasses.

In this work, we discovered broad blue light emission in ZIF-4 glasses upon hot-pressing and subsequent annealing, which was much stronger than that in their crystalline counterparts. This function was significantly enhanced by annealing above the glass transition temperature, and simultaneously a red shift was induced. We clarified the structural and electronic origin of both the emission enhancement and the red shift. For the gas sorption, we demonstrate that CO₂ gas sorption measurements at 195 K provide deep insights into the intrinsic porosity (pore volume) of ZIF-4 and ZIF-62 glasses. This study provides important insights into the intrinsic porosity of ZIF glasses and advances our understanding of the relationship between structural porosity and photonic properties in these materials.

Results and Discussion

Thermal and structural analyses

fig:1a shows the preparation procedure of the studied samples. The crystalline or amorphous nature of the studied samples was identified from the X-ray diffraction (XRD) and high-energy synchrotron XRD (HEXRD) analyses (fig:1b and fig:S1, Supporting Information). ZIF-4 crystals were successfully synthesized by using the modified method based on that reported in [19], as confirmed by the good agreement between the experimental XRD pattern and the simulated one. The as-synthesized ZIF-4 crystals were subsequently vitrified to form a high-density amorphous (HDA) glass[7], as evidenced by the disappearance of the ZIF-4 diffraction peaks (fig:1b). HDA glass was subjected to hot-pressing using spark plasma sintering (SPS), resulting in a hot-pressed high-density amorphous (HPHDA) glass. Interestingly, several weak XRD diffraction peaks emerge on the broad amorphous hump of HPHDA (fig:1b and fig:S2, Supporting Information), suggesting the formation of tiny ZIF-zni crystals in the glass matrix. To study the impact of annealing on the growth of ZIF-zni crystals, HPHDA was annealed under different conditions to obtain Axxx−yy_{\mathrm{xxx-yy}}HPHDA, where xxx and yy denote the annealing temperature (in K) and annealing time (in min), respectively. In this procedure, HPHDA was annealed at 593 K for 30 min, yielding A593−30_{593-30}HPHDA (see Methods). The HEXRD patterns of A300−10_{300-10}HPHDA and A360−10_{360-10}HPHDA prove that the crystallinity of HPHDA increases with annealing temperatures (Supplementary fig:3b).

To characterize the morphologies of tiny ZIF-zni crystals in the glass matrix, transmission electron microscopy (TEM) analysis was conducted on HPHDA and A613−10_{613-10}HPHDA. fig:1c and fig:S3 (Supporting Information) show TEM and high-resolution TEM (HRTEM) images of HPHDA. Unlike HDA glass, the HRTEM image of HPHDA reveals abundant crystal-like clusters or paracrystallites (shown in white dashed circles) with sizes of around 2–3 nm, which can be assigned to the ZIF-zni phase. This observation is consistent with the XRD results of HPHDA, but the selected area electron diffraction (SAED) pattern shows no diffraction spots. Compared with the diffuse diffraction rings observed in the SAED pattern of HDA glass, the well-defined diffraction rings A613−10_{613-10}HPHDA suggest a higher degree of crystalline ordering (Figs. 1d and S4, Supporting Information). The ZIF-zni crystals grow to approximately 6 nm. In addition, the SAED photograph (Fig. S5, Supporting Information) confirms the identity of the forming crystals. Energy dispersive X-ray spectroscopy (EDS) mapping analysis, as collected from the high-angle annular dark-field imaging scanning TEM (HAADF-STEM) images, confirms the homogeneous distribution of Zn, C, and N elements in the samples (Fig. S6, Supporting Information).

Synthesis and characterization of ZIF-4 crystal and glasses

Figure 1. Synthesis and characterization of ZIF-4 crystal and glasses. (a) Flow chart of high-density amorphization (HDA) glass applied to ZIF-4 crystal, hot-pressing (HP) applied to HDA glass powder, and annealing applied to hot-pressed HDA (HPHDA) glass. (b) XRD patterns of simulated ZIF-4, ZIF-4 crystal, HDA glass, simulated ZIF-zni, HPHDA glass, and A553−10A_{553-10}HPHDA glass. (c-d) Transmission electron microscopy (TEM) images of HPHDA glass (c) and A613−10A_{613-10}HPHDA glass (d).

To investigate the thermodynamic features of ZIF-4, HDA, HPHDA, and A613−10A_{613-10}HPHDA, the differential scanning calorimetry (DSC) analysis was performed, and the obtained DSC curves are shown in Fig. 2a. The endotherm (between 475 and 575 K) in the DSC upscan curve of ZIF-4 is attributed to the desolvation of DMF, which does not cause framework collapse1. Upon further heating to 663 K, the crystalline ZIF-4 transforms into a low-density liquid (LDL) phase and further converts to a high-density liquid (HDL) phase, without recrystallization into the dense ZIF-zni structure. After completion of the liquid-liquid transition (LLT), cooling the HDL phase to room temperature results in the formation of HDA glass, which exhibits a glass transition temperature (TgT_\mathrm{g}) of 564 K upon reheating. Upon hot-pressing (HP), the TgT_\mathrm{g} of HDA glass decreases from 564 K to around 523 K in HPHDA. This decrease was attributed to the pressure-induced weakening of the intermediate-range structural connectivity[12][14]. Upon annealing at 613 K (90 K above TgT_\mathrm{g} of HPHDA) for 10 min, TgT_\mathrm{g} of HPHDA increases to around 563 K, which is similar to that of HDA glass. To study the impact of annealing on the increase in TgT_\mathrm{g} value, the HPHDA sample was subjected to 5 cycles of DSC scan up to the maximum scanning temperature (613 K) at 10 K min−1^{-1}. It is seen that TgT_\mathrm{g} first sharply increases and then slowly increases with cycling numbers, and approaches 563 K in the fifth upscan. Finally, the TgT_\mathrm{g} of the HPHDA sample remains unchanged upon increasing annealing temperatures (633, 653, and 673 K) for 10 min (fig:S7, Supporting Information). This implies that annealing relaxes the hot-pressed-induced distorted structure and increases glass network connectivity, allowing the structure to return toward that of HDA glass. This phenomenon could also be attributed to the partial crystallization of ZIF-zni, in contrast to the annealing-induced structural evolution observed in hot-pressed ZIF-62 glass[14].

To understand the structure changes caused by vitrification, hot-pressing, and annealing, we analyze the Raman spectra of ZIF-4, HDA, HPHDA, and A673−30_{673-30}HPHDA samples (fig:2c). The peaks in the range of 600–1600 cm−1^{-1} at 1065 cm−1^{-1} are assigned to the different vibration modes of the Im ring for the four samples[20]. These vibration bands occur almost at the same frequencies, confirming the integrity of organic linkers in the samples[11]. However, compared to the vibration peaks of the Im ring in ZIF-4, those in the other three samples become weaker and broader. In the low-frequency range (below 600 cm−1^{-1}), the vibration bands in ZIF-4 were observed at 145 and 179 cm−1^{-1} corresponding to Zn-N stretching. Two peaks weaken and merge to form a broad Zn-N peak upon vitrification, hot-pressing, and annealing, implying that vitrification distorts [ZnIm4] tetrahedra and consequently leads to structural disordering in different length scales.

The HEXRD technique is further performed to probe the short-, medium-, and long-range structural evolution of the ZIF-4 crystal upon vitrification, hot-pressing, and annealing. fig:2d shows the Faber-Ziman structure factor S(Q)S(Q) curve of ZIF-4, HDA, HPHDA, and A633_{633}-10HPHDA, where sharp diffraction peaks are present in ZIF-4 and broad peaks appear in HDA glass. The glassy nature of HDA is further verified by the lack of sharp diffraction peaks in the S(Q)S(Q) curves. Some weak diffraction peaks emerge in the S(Q)S(Q) curves of HDA upon hot-pressing and become more pronounced with increasing annealing temperature, further confirming the occurrence of a disorder-to-order transition during both hot-pressing and annealing. The reduced pair correlation functions G(r)G(r) curves (Fig. 2e) show five main atom-atom correlation peaks in the four samples. The atom-atom pair correlations include those of C-C(N) (1.36 Å), Zn-N (2.02 Å), Zn-C (3.03 Å), Zn-N (4.17 Å), and Zn-Zn (5.94 Å), as shown in fig:2f. The local coordination environments of Zn2+^{2+} in the HDA, HPHDA, and A633_{633}-10HPHDA samples slightly differ from those in ZIF-4. The Zn-Zn correlation of 5.94 Å suggests the integrity of Zn-ligand-Zn linkages, and the correlation in the glasses is weaker than that in ZIF-4, confirming that the three glasses possess a higher degree of intermediate-range disorder. However, as shown in the ΔG(r)\Delta G(r) curves (Fig. S8, Supporting Information), the short-range correlations of Zn-N (2.02 Å), Zn-C (3.03 Å), and Zn-N (4.17 Å) become more evident upon hot-pressing and annealing, implying that the coordination Zn-N bonds get stronger.

Structural analyses of ZIF-4 crystal and glasses

Figure 2. Structural analyses of ZIF-4 crystal and glasses. (a) Thermogravimetric curve (magenta color) of ZIF-4 and differential scanning calorimetry (DSC) curves of ZIF-4, HDA glass, HPHDA, and A613-10_{613\text{-}10}HPHDA. (b) The variation of glass transition temperature (TgT_\mathrm{g}) for HDA-g with annealing via both dynamic heating to 613 K for 4 times and isothermal heating at 613, 633, 653, and 673 K for 10 min. (c) Raman spectra of ZIF-4, HAD glass, HPHDA, and A593-30_{593\text{-}30}HPHDA. (d) Faber-Ziman structure factors S(Q)S(Q) of ZIF-4, HDA glass, HPHDA, and A633-30_{633\text{-}30}HPHDA. (e) Reduced pair correlation functions G(r)G(r) of ZIF-4, HDA glass, HPHDA, and A633-30_{633\text{-}30}HPHDA. (f) Schematic diagram of the atomic relationships in the ZIF-4 structure. Note: magenta spheres represent Zn, gray spheres represent C, cyan-green spheres represent N, and light pink spheres represent H.

Photoluminescence performance

Based on the observation of the strong fluorescence of HDA glass, HPHDA, and A593-10_{593\text{-}10}HPHDA (Fig. 2c), it is interesting to study the significant impact of the subtle tetrahedral rearrangement on the electronic structure of the glasses, leading to photonic performance. Fig. S9 (Supporting Information) shows the optical absorption spectra of ZIF4, HDA glass, and HPHDA. ZIF-4 and HDA glass exhibit weak absorption in the visible range, but show a bit stronger absorption in the ultraviolet range (below 350 nm). In addition, the electronic structure of ZIF-4 is calculated using periodic density functional theory (PDFT) to gain insight into the PL mechanism. As shown in Fig. 3c, we observe a flat band electronic structure with a band gap of 5.02 eV. Based on the analysis of the total/partial density of states (DOS) (Fig. 3c), the electronic density is mainly determined by the pp-orbitals of C and N atoms. Furthermore, the highest occupied molecular orbital (HOMO) and the lowest unoccupied molecular orbital (LUMO) are dominated by the pp-orbitals of C and N in the Im rings (fig:10, Supporting Information). This indicates that the photoluminescence (PL) of the ZIF-4 crystal is primarily attributed to the π\pi-π∗\pi^{*} interaction within the rings. However, a sharp increase in absorbance with decreasing wavelength is observed at around 400 nm in HPHDA.

Figs. fig:3a-fig:3d show the two-dimensional (excitation-emission) PL spectra of ZIF-4, HDA, HPHDA, and A593−10_{593-10}HPHDA, respectively. A strong narrow emission peak is observed at 310 nm in the crystal under excitation in the wavelength range of 290 nm (fig:2g), whereas a weak broad emission peak is seen in the visible range for HDA, HPHDA, and A593−10_{593-10}HPHDA. Under excitation at 270 nm, HDA glass exhibits a narrow emission peak at 290 nm and a weak broad emission peak at 431 nm (fig:3f). Interestingly, compared to the ZIF-4 crystal, the narrow and the broad emission peaks in HDA glass and HPHDA shift with excitation wavelength towards shorter wavelengths, i.e., leading to a blue shift[21]. Under excitation at 310 nm, the narrow emission peak at 353 nm in ZIF-4 becomes weak or disappears upon vitrification (fig:3h). Interestingly, the weak emission at around 443 nm in ZIF-4 is strongly enhanced through vitrification, hot-pressing, and annealing after HP (fig:3i). Moreover, this emission peak shows a blue shift upon vitrification and hot-pressing, and exhibits a red shift upon annealing after hot-pressing. The structural origin of the observed PL behaviors can be explained as follows. First, the narrow emission peaks at 310 and 353 nm in the crystal appear only when Im rings are periodically arranged, which are attributed to their π∗\pi^{*}-π\pi transitions in Im rings. Second, the blue shift of narrow emission peaks from 310 to 290 nm and the vanishing of the emission peak at 290 nm may be ascribed to the increased orientational disorder of the Im linkers and distortion of the local Zn-N coordination environment[22]. Third, the red shift could be attributed to the annealing-induced increase of ligand-to-ligand charge transfer (LLCT), resulting in increased conjugation area and therefore lowering of the energy level of the antibonding π∗\pi^{*} electron orbital[14].

The chromaticity coordinates of ZIF-4, HDA, HPHDA, and A593−10_{593-10}HPHDA under 270, 290, 310, and 370 nm excitation are marked in CIE 1931 color spaces (fig:S11, Supporting Information). The color point of A593−10_{593-10}HPHDA lies in the light-blue lighting region, whereas those of ZIF-4, HDA, and HPHDA are located in the blue lighting region. fig:3j shows the absolute internal (black column) and external (red column) photoluminescence quantum yield (PLQY) values for ZIF-4, HDA, HPHDA, and A593−10_{593-10}HPHDA under excitation at 365 nm. The internal PLQY of the ZIF-4 crystal under excitation at 365 nm first increases from 3.8 to 9.3% upon vitrification and then decreases to 5.2% by hot-pressing and finally reaches 8.6% upon annealing at 593 K for 30 min. The external PLQY of the ZIF-4 crystal follows the same trend as the internal PLQY, but with different absolute values. The fluorescence lifetime for ZIF-4 at 435 nm under excitation at 375 nm (fig:3k) is shortened by vitrification and hot-pressing, and then is extended by annealing at 593 K for 30 min.

Photoluminescence performance of ZIF-4 crystal and glasses

Figure 3. Photoluminescence (PL) performance of ZIF-4 crystal and glasses. (a-d) Two-dimensional fluorescence (Excitation/Emission) spectra of (a) ZIF-4, (b) HDA, (c) HPHDA, and (d) A593−30_{593-30}HPHDA. Inset: Optical photos of (a) ZIF-4, (b) HDA, (c) HPHDA, and (d) A593−30_{593-30}HPHDA under a 365 nm laser. (b) Band structure and corresponding total/partial density of states (TDOS/PDOS) of ZIF-4. (e-h) Comparison of emission spectra of ZIF-4, HDA, HPHDA, and A593−30_{593-30}HPHDA excited at 270 (f), 290 (g), 310 (h), and 370 nm (i), respectively. (j) Absolute internal and external PLQY of ZIF-4, HDA, HPHDA, and A593−30_{593-30}HPHDA under excitation at 365 nm. (K) Room-temperature lifetime of ZIF-4, HDA, HPHDA, and A593−30_{593-30}HPHDA samples under excitation at 375 nm.

Gas sorption performance

To evaluate the pore structure of ZIF-4 upon vitrification, hot-pressing, and annealing, the gas adsorption properties were preliminarily investigated. Based on Henke's report on N2\mathrm{N}_2 and Ar physisorption for ZIF-4 and ZIF-62 samples [23], the smaller kinetic diameter of CO2\mathrm{CO}_2 (3.30 A˚\mathring{A}) relative to those of N2\mathrm{N}_2 (3.64 A˚\mathring{A}) and Ar (3.40 A˚\mathring{A}), combined with the higher adsorption temperature (195 vs. 77 K), facilitates CO2\mathrm{CO}_2 diffusion into narrow micropores (<5 A˚\mathring{A}) [23, 24, 25]. Compared to the CO2\mathrm{CO}_2 sorption experiments performed at 273 or 298 K, measurements at 195 K enable complete filling of the micropores at 100 kPa. At 195 K, CO2\mathrm{CO}_2 would normally solidify in nonporous or macroporous systems. However, within micropores (≤20\le20 A˚\mathring{A}), nanoscale confinement suppresses crystallization, allowing the adsorbed CO2\mathrm{CO}_2 to remain in a supercooled liquid state. Consequently, the micropores can be effectively filled with fluid CO2\mathrm{CO}_2, enabling the accessible micropore volume to be determined from the CO2\mathrm{CO}_2 uptake. Consequently, the maximum gas capacities (nadsn_{\mathrm{ads}}) determined at 95 kPa can be used to determine the specific micropore volume (VporeV_{\mathrm{pore}}) of the investigated ZIF-4 and ZIF-62 samples by taking into account the density of supercooled liquid CO2\mathrm{CO}_2 at 195 K (fig:4a and fig:4b). Therefore, the porosity of ZIF-4, HDA, HPHDA, A633-10HPHDAA_{633\text{-}10\mathrm{HPHDA}}, and A773-5HDAA_{773\text{-}5\mathrm{HDA}} was probed by CO2\mathrm{CO}_2 physisorption at 195 K. Remarkably, all these phases adsorb CO2\mathrm{CO}_2 as evident from the Langmuir-shaped isotherms (fig:4a and fig:4b).

The CO2\mathrm{CO}_2 adsorption isotherms reveal that ZIF-4 crystals exhibit the highest VporeV_{\mathrm{pore}} of 0.275 cm3⋅g−1\mathrm{cm}^3\cdot\mathrm{g}^{-1}, whereas vitrification into HDA glass drastically reduces VporeV_{\mathrm{pore}} to 0.112 cm3⋅g−1\mathrm{cm}^3\cdot\mathrm{g}^{-1}. This pronounced decrease reflects substantial framework collapse and densification; nevertheless, approximately 41% of the micropore volume remains accessible in the HDA glass. In addition, upon hot-pressing and annealing at both 633 K for 10 min and 773 K for 5 min, the VporeV_{\mathrm{pore}} of HDA glass reduces to 0.093, 0.092, and 0.069 cm3⋅g−1\mathrm{cm}^3\cdot\mathrm{g}^{-1}, respectively. Based on XRD and TEM results shown in fig:1b-fig:1d, both the size of ZIF-zni crystals and the crystallinity of HDA glass increase with increasing annealing temperature. Notably, ZIF-zni is the densest and most stable Zn(Im)2_2 crystal, indicating that the micropore size becomes small upon annealing.

Compared to ZIF-4, the micropore volume of crystalline ZIF-62 decreases to 0.201 cm3^3·g−1^{-1}. This correlates with the implementation of the secondary bulky imidazolate linkers (bIm) in ZIF-62, reducing the void space of the crystalline framework. The pore volume of the melt-quenched glass (MQG), derived from a ZIF-62 crystal, is 0.137 cm3^3·g−1^{-1}, showing a reduction of 25% compared to that of the ZIF-62 crystal. This observation suggests that MQG has a more similar pore structure to that of its crystalline ZIF-62, while HDA glass differs strongly from crystalline ZIF-4. Interestingly, the VporeV_{\mathrm{pore}} of MQG reduces to 0.110 cm3^3·g−1^{-1} upon hot-pressing, and increases to 0.148 cm3^3·g−1^{-1} upon annealing at 653 K for 10 min. Moreover, direct annealing of MQG at 653 K for 10 min induces an increase in VporeV_{\mathrm{pore}} from 0.137 to 0.142 cm3^3·g−1^{-1}, which is different from that in HPHDA glass. This significant improvement in CO2_2 adsorption for ZIF-62 glass suggests that the relaxation of the distorted structure towards a less distorted structure upon annealing above TgT_{\mathrm{g}}. This relaxation leads to annealed MQG and HPG staying at a lower potential energy level state[14]. Consequently, band-gap energy (EgE_{\mathrm{g}}) between the valence band and the conduction band decreases upon annealing, resulting in a slight red shift in the PL of both HPG and MQG. For the above reasons, the mechanism of the PL red shift upon annealing above TgT_{\mathrm{g}} needs to be further investigated. However, it is important to note that the pore structure have an srong impact on the position of PL. Moreover, the mechanical performance of the studied ZIF glasses remains inferior to that of conventional oxide glasses[26][27], highlighting the need for further efforts to enhance their mechanical properties[28].

CO2 gas sorption analysis of ZIF-4 and ZIF-62 crystals and glasses

Figure 4. CO2_2 gas sorption analysis of ZIF-4 and ZIF-62 crystals and glasses. (a) CO2_2 sorption isotherms collected at 195 K of ZIF-4, HDA, HPHDA, A633−10_{633-10}HPHDA, and A773−5_{773-5}HDA. (b) CO2_2 sorption isotherms collected at 195 K of ZIF-62, MGQ, HPG, A653−10_{653-10}HPG, and A653−10_{653-10}MQG. (c) Bar plot of the micropore volumes (VporeV_{\mathrm{pore}}) for ZIF-4, HDA, HPHDA, A633−10_{633-10}HPHDA, and A773−5_{773-5}HDA derived from the CO2_2 isotherms at 195 K. (d) Bar plot of the micropore volumes (VporeV_{\mathrm{pore}}) for all crystalline ZIF-62 and their corresponding glasses derived from the CO2_2 isotherms at 195 K.

Conclusions

We synthesized ZIF-4 crystals via the solvothermal approach and prepared HDA glasses through quenching high-density liquid, hot-pressing, and annealing. We discovered the narrowband ultraviolet emission and the weak broadband visible light emission from the ZIF-4 crystal. More importantly, the broadband visible light emission was enhanced by means of vitrification, hot-pressing, and annealing, while a significant red shift was induced by annealing at a temperature above TgT_{\mathrm{g}}. These phenomena were attributed to the band gap decrease caused by structure relaxation. Such structural evaluation was verified by high-energy synchrotron X-ray diffraction measurements. Based on gas adsorption results, we found that the VporeV_{\mathrm{pore}} of MQG reduces to 0.110 cm3⋅^{3}\cdotg−1^{-1} upon hot-pressing, and increases to 0.148 cm3⋅^{3}\cdotg−1^{-1} upon annealing at 653 K for 10 min. Moreover, direct annealing of MQG at 653 K for 10 min induces an increase in VporeV_{\mathrm{pore}} from 0.137 to 0.142 cm3⋅^{3}\cdotg−1^{-1}, which is different from that in HPHDA glass. This work provides important insights into the porosity of MOF glasses and thus contributes to the understanding of the structure of such glasses. Future advancements, such as new design concepts for tuning and adjusting the porosity and sorption selectivity of MOF glasses, must be developed.

Acknowledgments

The authors acknowledge the support from the i15 beamline (Proposal No. CY39002) at Diamond Light Source (DLS) in Didcot, United Kingdom. The authors also acknowledge the Carlsberg Foundation (Grant No. CF21-0371) for funding the STA 449 F3 DSC used in this work.

Conflict of Interest

The authors declare no conflicts of interest.

References

References

  1. [1]K. S. Park, Z. Ni, A. P. Côté, et al., “Exceptional Chemical and Thermal Stability of Zeolitic Imidazolate Frameworks,” Proceedings of the National Academy of Sciences of the United States of America 103, no. 27 (2006): 10186–10191, https://doi.org/10.1073/pnas.0602439103.
  2. [2]Y. Wang, H. Jin, Q. Ma, et al., “A MOF Glass Membrane for Gas Separation,” Angewandte Chemie - International Edition 59, no. 11 (2020): 4365–4369, https://doi.org/10.1002/anie.201915807.
  3. [3]Z. Yang, Y. Belmabkhout, L. N. McHugh, et al., “ZIF-62 Glass Foam Self-Supported Membranes to Address CH4/N2 Separations,” Nature Materials 22, no. 7 (2023): 888–894, https://doi.org/10.1038/s41563-023-01545-w.
  4. [4]R. Lin, X. Li, A. Krajnc, et al., “Mechanochemically Synthesised Flexible Electrodes Based on Bimetallic Metal–Organic Framework Glasses for the Oxygen Evolution Reaction,” Angewandte Chemie - International Edition 61, no. 4 (2022), https://doi.org/10.1002/anie.202112880.
  5. [5]C. Gao, Z. Jiang, S. Qi, et al., “Metal-Organic Framework Glass Anode with an Exceptional Cycling-Induced Capacity Enhancement for Lithium-Ion Batteries,” Advanced Materials 34, no. 10 (2022): 1–13, https://doi.org/10.1002/adma.202110048.
  6. [6]E. C. Constable, and C. E. Housecroft, “Coordination Chemistry: The Scientific Legacy of Alfred Werner,” Chemical Society Reviews 42, no. 4 (2013): 1429–1439, https://doi.org/10.1039/c2cs35428d.
  7. [7]T. D. Bennett, J. C. Tan, Y. Yue, et al., “Hybrid Glasses from Strong and Fragile Metal-Organic Framework Liquids,” Nature Communications 6 (2015): 1–7, https://doi.org/10.1038/ncomms9079.
  8. [8]K. Noh, J. Lee, and J. Kim, “Compositions and Structures of Zeolitic Imidazolate Frameworks,” Israel Journal of Chemistry 58, no. 9 (2018): 1075–1088, https://doi.org/10.1002/ijch.201800107.
  9. [9]L. Frentzel-Beyme, M. Klob, P. Kolodzeiski, R. Pallach, and S. Henke, “Meltable Mixed-Linker Zeolitic Imidazolate Frameworks and Their Microporous Glasses: From Melting Point Engineering to Selective Hydrocarbon Sorption,” Journal of the American Chemical Society 141, no. 31 (2019): 12362–12371, https://doi.org/10.1021/jacs.9b05558.
  10. [10]M. A. Ali, J. Ren, T. Zhao, et al., “Broad Mid-Infrared Luminescence in a Metal-Organic Framework Glass,” ACS Omega 4, no. 7 (2019): 12081–12087, https://doi.org/10.1021/acsomega.9b01559.
  11. [11]A. Qiao, T. D. Bennett, H. Tao, et al., “A Metal-Organic Framework with Ultrahigh Glass-Forming Ability,” Science Advances 4, no. 3 (2018): 1–8, https://doi.org/10.1126/sciadv.aao6827.
  12. [12]A. Qiao, S. S. Sørensen, M. Stepniewska, et al., “Hypersensitivity of the Glass Transition to Pressure History in a Metal–Organic Framework Glass,” Chemistry of Materials 34, no. 11 (2022): 5030–5038, https://doi.org/10.1021/acs.chemmater.2c00325.
  13. [13]R. Grau-Crespo, A. Aziz, A. W. Collins, et al., “Modelling a Linker Mix-and-Match Approach for Controlling the Optical Excitation Gaps and Band Alignment of Zeolitic Imidazolate Frameworks,” Angewandte Chemie - International Edition 55, no. 52 (2016): 16012–16016, https://doi.org/10.1002/anie.201609439.
  14. [14]Z. Li, Z. Wang, H. Zhang, et al., “White-Light Emission in Zeolitic Imidazolate Framework Glasses,” Advanced Materials 38, no. 25 (2026), https://doi.org/10.1002/adma.72968.
  15. [15]A. M. May, and J. L. Dempsey, “A New Era of LMCT: Leveraging Ligand-to-Metal Charge Transfer Excited States for Photochemical Reactions,” Chemical Science 15, no. 18 (2024): 6661–6678, https://doi.org/10.1039/d3sc05268k.
  16. [16]T. D. Bennett, Y. Yue, P. Li, et al., “Melt-Quenched Glasses of Metal-Organic Frameworks,” Journal of the American Chemical Society 138, no. 10 (2016): 3484–3492, https://doi.org/10.1021/jacs.5b13220.
  17. [17]R. Gaillac, P. Pullumbi, K. A. Beyer, et al., “Liquid Metal–Organic Frameworks,” Nature Materials 16, no. 11 (2017): 1149–1155, https://doi.org/10.1038/NMAT4998.
  18. [18]J. Fonseca, T. Gong, L. Jiao, and H. L. Jiang, “Metal-Organic Frameworks (MOFs) beyond Crystallinity: Amorphous MOFs, MOF Liquids and MOF Glasses,” Journal of Materials Chemistry A 9, no. 17 (2021): 10562–10611, https://doi.org/10.1039/d1ta01043c.
  19. [19]R. N. Widmer, G. I. Lampronti, S. Anzellini, et al., “Pressure Promoted Low-Temperature Melting of Metal–Organic Frameworks,” Nature Materials 18, no. 4 (2019): 370–376, https://doi.org/10.1038/s41563-019-0317-4.
  20. [20]G. Kumari, K. Jayaramulu, T. K. Maji, and C. Narayana, “Temperature Induced Structural Transformations and Gas Adsorption in the Zeolitic Imidazolate Framework ZIF-8: A Raman Study,” Journal of Physical Chemistry A 117, no. 43 (2013): 11006–11012, https://doi.org/10.1021/jp407792a.
  21. [21]Y. Zou, S. Abednatanzi, P. Gohari Derakshandeh, et al., “Red Edge Effect and Chromoselective Photocatalysis with Amorphous Covalent Triazine-Based Frameworks,” Nature Communications 13, no. 1 (2022): 1–13, https://doi.org/10.1038/s41467-022-29781-9.
  22. [22]S. Liu, Z. R. Wang, X. Lin, et al., “Structural Comparisons, Fluorescence Properties, and Glass-to-Crystal Transformations of Heat-Cooled and Melt-Quenched Zeolitic Imidazolate Framework Glass,” Inorganic Chemistry 63 (2024): 18574–18580, https://doi.org/10.1021/acs.inorgchem.4c01886.
  23. [23]L. Frentzel-Beyme, P. Kolodziejski, J. B. Weiß, A. Schneemann, and S. Henke, “Quantification of Gas-Accessible Microporosity in Metal-Organic Framework Glasses,” Nature Communications 13, no. 1 (2022): 1–11, https://doi.org/10.1038/s41467-022-35372-5.
  24. [24]O. Smirnova, S. Hwang, R. Sajzew, et al., “Precise Control over Gas-Transporting Channels in Zeolitic Imidazolate Framework Glasses,” Nature Materials 23, no. 2 (2024): 262–270, https://doi.org/10.1038/s41563-023-01738-3.
  25. [25]H. Marsh, and B. Rand, “The Characterization of Microporous Carbons by Means of the Dubinin-Radushkevich Equation,” Journal of Colloid And Interface Science 33, no. 1 (1970): 101–116, https://doi.org/10.1016/0021-9797(70)90077-9.
  26. [26]T. To, S. S. Sørensen, M. Stepniewska, et al., “Fracture Toughness of a Metal–Organic Framework Glass,” Nature Communications 11, no. 1 (2020): 1–9, https://doi.org/10.1038/s41467-020-16382-7.
  27. [27]M. Stepniewska, K. Januchta, C. Zhou, A. Qiao, M. M. Smedskjaer, and Y. Yue, “Observation of Indentation-Induced Shear Bands in a Metal-Organic Framework Glass,” Proceedings of the National Academy of Sciences of the United States of America 117, no. 19 (2020): 10149–10154, https://doi.org/10.1073/pnas.2000916117.
  28. [28]T. Xu, Z. Li, J.-X. Wu, et al., “Glass Formation of Metal Organic-Inorganic Complexes,” National Science Review (2026), https://doi.org/10.1093/nsr/nwag349.

Paper details

vlnc:W_uywj6s8b
Version
v1 · latest
Published
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents