Solvent-Free High-Temperature Capillary Stamping of Stimuli-Responsive Polymers: Wettability Management by Orthogonal Substrate Functionalization

Abstract

The wettability of surfaces determines their antifouling, antifogging, anti-icing, and self-cleaning properties as well as their usability for sensing, oil-water separation, water collection, and water purification. Solvent-free high-temperature capillary stamping of stimuli-responsive polymers yielding arrays of stimuli-responsive polymer microdots on differently modified substrates enables the flexible generation of switchable surfaces with different water contact angles (WCAs). Potential problems associated with the deposition of polymer solutions, such as the handling of volatile organic solvents, phase separation induced by solvent evaporation, and capillarity-driven flow processes, are circumvented. We used composite stamps with topographically patterned contact surfaces consisting of metallic nickel cores and porous MnO2 coatings taking up the stimuli-responsive polymers. The short transport paths from the MnO2 contact layers to the counterpart substrates enabled the stamping of polymer melts containing components impeding flow, such as carbon nanotubes (CNTs). Thus-obtained arrays of polymer-CNT hybrid microdots prevent problems associated with continuous coatings including delamination and crack propagation. Moreover, the range within which the properties of the stamped stimuli-responsive polymer microdots are switchable can be tuned by orthogonal substrate modification. As an example, we stamped hybrid microdots consisting of poly(2-(methacryloyloxy)ethyl ferrocenecarboxylate) (PFcMA) and CNTs onto indium tin oxide (ITO) substrates. Coating the ITO substrates with a poly(ethylene oxide)-terminated silane shifted the WCAs obtained by switching the PFcMA between its oxidized and reduced states by nearly 50°.

Introduction

The additive lithographic deposition of stimuli-responsive polymers[1] is frequently applied to produce functionalized surfaces. Classical additive lithographic methods deployed to this end include inkjet and aerosol jet printing[2] as well as soft lithography[3, 4, 5, 6] and polymer pen lithography.[7, 8, 9] Commonly, solutions of the functional polymers in volatile organic solvents are lithographically deposited. The target patterns of the deposited functional polymers are obtained only after solvent evaporation. During the evaporation of volatile organic solvents hardly controllable structure formation processes, such as liquid-liquid phase separation[10] and flow processes related to, for example, capillarity[11, 12] may occur. Additional drying steps to remove residual solvent from as-deposited patterns may damage the latter. Moreover, the presence of volatile organic solvents reduces the amounts of the non-volatile functional polymeric components transferred per stamping step. If, on the other hand, functional polymers are transferred to substrates by ballistic methods, such as laser-induced forward transfer,[13] securing sufficient adhesion might be challenging. Melt processing of polymers by extrusion or electrospinning[14] is well established. Thus, the additive lithographic transfer of polymer melts in the absence of organic solvents might be a useful methodological extension of microcontact printing. In this way, polymers hardly soluble in solvents compatible with microcontact printing may be stamped also.

Wettability management is crucial to customize the antifouling, antifogging, anti-icing and self-cleaning properties of surfaces. Surfaces with tailored wettability may be used for applications like sensing, oil-water separation, water collection and water purification. Thus, the tailoring of the wettability of surfaces by additive surface manufacturing has attracted significant interest.[15, 16, 17, 18, 19] Surfaces with switchable wettability and, therefore, amplified functional versatility are accessible by functionalization with stimuli-responsive polymers.[20, 21, 22] Stimuli-responsive polymers may be chemically grafted onto substrates. However, non-reactive deposition significantly extends the range of deployable stimuli-responsive polymers and of counterpart substrates to be functionalized. Patterns of discrete stimuli-responsive polymer microdots may have additional advantages over continuous coatings, such as suppression of crack propagation and delamination. Moreover, the substrate properties may be customized by orthogonal functionalization of the substrate areas between the microdots.[23, 24]

Here, we show that solvent-free high-temperature capillary stamping is a potential manufacturing platform yielding tailored surfaces with switchable wettability by additive lithographic high-temperature deposition of stimuli-responsive polymers – optionally mixed with solid additives. As example, we performed high-temperature capillary stamping of melts of the stimuli-responsive ferrocene-containing polymer poly(2-(methacryloyloxy)ethyl ferrocenecarboxylate) (PFcMA)[25, 26, 27] blended with multiwalled carbon nanotubes (CNTs). We thus stamped arrays of PFcMA-CNT hybrid microdots onto conductive indium tin oxide (ITO) substrates. Electrochemical switching reversibly transformed the PFcMA-CNT hybrid microdots from a high-WCA state, in which the PFcMA is reduced, to a low-WCA state, in which the PFcMA is partially oxidized (the ferrocene units are positively charged), and vice versa. While the intrinsic conductivity of ITO is a prerequisite for the electrochemical switching of the PFcMA oxidation state, orthogonal functionalization of the ITO surface areas around the PFcMA-CNT hybrid microdots shifted the WCAs obtained for the two PFcMA oxidation states by nearly 50°.

Stamps exhibiting continuous pore systems[28, 29, 30, 31, 32] have been used for additive substrate patterning in automatized configurations[33] and even under the extreme conditions of solvothermal syntheses.[24] However, percolative transport of viscous mixtures containing polymers and additional components impeding flow, such as CNTs, through porous stamps might be too slow for efficient stamping procedures. Therefore, we devised Ni/MnO2_2 composite stamps for high-temperature capillary stamping by adapting a composite design involving the functionalization of dip pens or PDMS stamps with porous coatings for the deposition of proteins,[34, 35] viruses[36] and bacterial cells.[37]

Materials and Methods

Chemicals and materials

Lithium perchlorate (LiClO4_4), manganese sulfate (MnSO4_4), nickel sulfate (NiSO4_4), sodium acetate (C2_2H3_3NaO2_2), sodium chloride (NaCl), boric acid (H3_3BO3_3), sodium dodecyl sulfate (NaC12_{12}H25_{25}SO4_4; SDS), anisole (C7_7H8_8O), tert-butyl α\alpha-bromoisobutyrate (tBbib; C8_8H15_{15}BrO2_2), copper (I) bromide (CuBr), pentamethyldiethylentriamine (PMDETA; C9_9H23_{23}N3_3) and indium tin oxide (ITO) substrates [(In2_2O3_3)0.9_{0.9} · (SnO2_2)0.1_{0.1} with a resistance of 8-12 Ω\Omega sq−1^{-1} and a thickness of 1200–1600 Å] were purchased from Sigma-Aldrich. 3-[Methoxy(polyethyleneoxy)6−9_{6-9}]propyltrichlorosilane CH3_3O(C2_2H4_4O)6−9_{6-9}(CH2_2)3_3Cl3_3Si (PEO-silane) was purchased from Gelest. Multiwalled CNTs (NC7000) were purchased from Nanocyl. Macroporous silicon[38, 39] with macropores 1 μ\mum in diameter and a depth of 730 nm arranged in a hexagonal array with a lattice constant of 1.5 μ\mum was purchased from Smart Membranes (Halle). Pt wires were purchased from Rettberg Glasapparatebau and Ag/AgCl electrodes (c(KCl): 3 mol L−1^{-1}) from Metrohm. Polyimide tape (heat resistant adhesive 1810-DS tape) was purchased from M&S Lehner GmbH. If not stated otherwise, chemicals and materials were used as received.

Synthesis and characterization of PFcMA

1000 mg FcMA (4.35 mmol) and 4,7 μ\muL tBbib (0.025 mmol) were dissolved in 5 mL anisole. The solution was degassed by 3 freeze-pump-thaw cycles and heated to 90 °C. After the quick addition of 375 μ\muL of a CuPMDETABr solution (0.2 mol/L in anisole) the reaction mixture was stirred for 5 h. The polymer was then precipitated in a 10-fold excess of methanol, filtered, washed and dried in vacuo (SEC: MnM_n = 13400 g/mol, MwM_w = 21300 g/mol, DD = 1.58). The NMR spectrum of the obtained PFcMA was acquired at 400 MHz using a Bruker Avance II 400 spectrometer and processed with the software MestReNova (Mestrelab Research). The chemical shifts were referenced relative to the chemical shift originating from the used deuterated solvent (Figure S1). Size-exclusion chromatography (SEC) was carried out using an Agilent 1260 Infinity II setup with an SDV column set (1000 Å, 5000 Å, 6000 Å) from Polymer Standard Service (PSS, Mainz, Germany) and a PSS Security2 RI/UV detector. THF was used as the eluent at a flow rate of 1 mL/min and calibration was carried out using polystyrene standards (PSS, Mainz, Germany).

Preparation of Ni/MnO2_2 composite stamps

Pieces of macroporous silicon[38, 39] extending 1×11 \times1 cm containing macropores with a diameter of 1 μ\mum and a depth of 730 nm arranged in a hexagonal array with a lattice constant of 1.5 μ\mum (Figure 1a) were sputtered 3 times with gold for 15 s using a JEOL JFC 1200 fine coater to generate an electrically conductive surface (Figure 1b).

Image not extracted

Figure 1. Preparation of Ni/MnO2_2 composite stamps. a) Cross-sectional view of macroporous silicon (1; black) used as master template. b) Macroporous silicon coated with a thin gold layer (2; orange). c) Electrodeposition of nickel (3; blue) onto the gold-coated macroporous silicon. d) A heat-resistant adhesive polyimide tape (4, green) is glued on the flat exposed nickel surface and the nickel film supported by the polyimide tape is detached from the gold-coated macroporous silicon. e) A porous MnO2_2 coating (5; red) is electrodeposited onto the topographically patterned surface of the nickel film initially in contact with the cold-coated macroporous silicon.

Electrodeposition of nickel was performed in 20 mL of an aqueous solution containing 1 mol/L NiSO4\mathrm{NiSO_4}, 0.1 mol/L NaCl\mathrm{NaCl}, 0.4 mol/L H3BO3\mathrm{H_3BO_3} and 0.15 mol/L SDS.[40] A nickel plate was used as counter electrode and the gold-coated macroporous Si template as working electrode. The deposition was conducted with a current of 1 mA/cm2^2 for 600 s. The formed nickel film covering the gold-coated macroporous silicon (Figure 1c) was rinsed with water and dried. Heat-resistant adhesive polyimide tape was glued onto the smooth exposed surface of the nickel film, which were then detached from the silicon master templates. Thus, we obtained nickel films with a thickness of 2 μ\mum, which were topographically structured with hexagonal arrays of rods having a lattice constant of 1.5 μ\mum at their exposed surface opposite of the adhesive polyimide tape (Figure 1d and S2). The rods were replicas of the macropores of the macroporous Si and had round tips, a height of 730 nm and base diameters of 1 μ\mum. The adhesive polyimide tape mechanically stabilized the unsupported nickel film with an area of 1x1 cm2^2. In the next step, the topographically structured exposed surface of the nickel film was coated with a porous MnO2\mathrm{MnO_2} layer with a thickness of ∼\sim200 nm (Figure 1e) by electrodeposition using a three-electrode system with a platinum counter electrode and an Ag/AgCl reference electrode. The electrodeposition was carried out for 90 s in 20 mL of an aqueous electrolyte solution containing 0.33 mol/L MnSO4\mathrm{MnSO_4} and 0.33 mol/L sodium acetate with a current of 0.5 mA/cm2^2 following procedures reported elsewhere.[41] All electrodeposition steps were performed with a potentiostat Interface 1000 (Gamry).

High temperature capillary stamping

10 µL of a solution of 10 mg PFcMA and 0.2 mg CNTs in 10 mL toluene was pipetted onto the topographically patterned MnO2_2 surface of the Ni/MnO2_2 composite stamps in such a way that the whole stamp area extending 1 cm2^{2} was covered with a PFcMA-CNT film. After evaporation of the toluene under ambient conditions the PFcMA-CNT mixture was annealed at 190°C for 10 h (overnight) under a vacuum to remove residual solvent. The applied heating and cooling rates amounted to 20 K/min. For high-temperature capillary stamping we adapted a procedure reported elswhere[24] using a home-made stamping device (Figure S3). The flat nickel surface of the infiltrated Ni/MnO2_2 composite stamps was glued onto the upper part of a stamping device with heat-resistant double-sided adhesive tape. ITO counterpart substrates to be patterned were located on the lower part of the stamping device. Prior to high-temperature capillary stamping, some of the ITO counterpart substrates had been surface-modified with PEO-silane by oxygen plasma treatment for 10 minutes using a Diener Femto plasma cleaner followed by chemical vapor deposition of PEO-silane at 110 °C for 12 h following procedures reported elsewhere.[42] The stamping device was then assembled by placing its upper part onto its lower part (Figure 2a). Thus, a contact pressure of 3.9 kN/m2^{2} was exerted during the stamping process. The assembled stamping device was then transferred into a home-made precision vacuum furnace (Figure 2b) and heated to 190°C at a rate of 20 K/min. The contact time at the target temperature of 190°C amounted to 1 min. The upper part of the stamping device was then removed and the lower part with the counterpart substrate was cooled to room temperature at a rate of -20 K/min. All high-temperature steps were carried out under argon atmosphere. After cooling to room temperature, the ITO substrates patterned with PFcMA-CNT hybrid microdot arrays (Figure 2c) could be picked up from the lower parts of the stamping device. To check whether the stamping procedure had an impact on the molecular weight distribution of the PFcMA, we stamped molten PFcMA without CNTs as described above on ITO substrates, scraped them off and used them for SEC measurements as described above.

Image not extracted

Figure 2. Solvent-free high-temperature capillary stamping of PFcMA-CNT hybrid microdots. a) Polyimide tape (4) of a Ni/MnO2_2 composite stamp (7) is glued onto upper part (6a) of stamping device (6). ITO counterpart substrate (9) is placed on lower part (6b) of stamping device (6). The contact elements (8) of Ni/MnO2_2 composite stamp (7) covered with MnO2_2 layer (5) containing PFcMA-CNT mixture are brought into contact with ITO counterpart substrate (9). b) After insertion of stamping device (6) into vacuum furnace (10) and heating under Ar flow, the PFcMA-CNT mixture forms liquid bridges (11) between the contact elements (8) and ITO substrate (9). c) After detachment of Ni/MnO2_2 composite stamp (7) and cooling to room temperature, ITO substrate (9) is modified with submicron PFcMA-CNT hybrid microdots (12).

Electrochemical analyses and treatments of PFcMA-CNT hybrid microdot arrays

For cyclic voltammetry we used ITO substrates with an area of 1 cm2^{2} functionalized with PFcMA-CNT hybrid microdots. The cyclic voltammetry measurements were performed in 20 mL of an aqueous electrolyte solution containing 0.1 mol/L LiClO4_4 using a three-electrode setup with a platinum wire counter electrode and an Ag/AgCl reference electrode. The measurements were carried out at a scan rate of 20 mV/s. The oxidations and reductions of the PFcMA-CNT hybrid microdots for the wettability investigations were also carried out electrochemically. Oxidation and reduction steps were performed by applying a constant potential of 1 or 0 vs. Ag/AgCl, respectively, for 30 min in the setup described above.

Wettability tests

Apparent water contact angles (WCAs)[43] were measured by the sessile drop method with a DSA100 drop shape analyzer at 22 ∘C22\,^\circ\mathrm{C} and a relative humidity of 23 %. To this end, we deposited droplets of deionized water with an initial volume of 2 μL2\,\mu\mathrm{L} on the sample surfaces. All data points represent the average of 3 measurements at different sample positions.

Microscopic characterization of PFcMA-CNT hybrid microdot arrays

For imaging by scanning electron microscopy (SEM), the samples were dried overnight at 40 ∘C40\,^\circ\mathrm{C} in air and then sputter-coated 2-3 times for 15 s with platinum/iridium alloy using an EMITECH K575X sputter coater. SEM images were taken with a Zeiss Auriga device equipped with a field emission cathode and a Gemini column at a working distance of 5 mm applying an acceleration voltage of 3 kV. For image detection an InLens detector was used. Atomic force microscopy (AFM) topography images were recorded with an NTEGRA microscope (NT-MDT) in the tapping mode using HQ:NSC16/AL BS cantilevers from µmasch with a resonance frequency of 170 - 210 kHz and a force constant of 30 - 70 N/m.

Surface analysis by X-ray photoelectron spectroscopy

X-ray photoelectron spectroscopy measurements were carried out under ultra-high vacuum using an ESCA system Phi 5000 VersaProbe III with a base pressure of 1⋅10−91 \cdot10^{-9} mbar equipped with a monochromatized aluminum anode (Kα=1486.6 eV\mathrm{K}\alpha= 1486.6\,\mathrm{eV}) and a 32-channel electrostatic hemispherical electronic analyzer. An ion gun and an electron gun were used to prevent sample charging. A take-off angle of 45∘45^\circ was used. The XP spectra were calibrated using the carbon C 1s peak at 284.5 eV.[44] Lorentz fits of the XP spectra were obtained using the software Origin.

Results and discussion

High-temperature capillary stamping

The Ni/MnO2_2 composite stamps combined sufficient mechanical stability, stability at high temperatures, good heat conductivity and the capability of taking up sufficient amounts of the polymer melts to be transferred. The composite design enabled the deposition of mixtures containing components not able to flow, such as mixtures of molten polymers and CNTs, because the transport paths were shorter than in fully porous stamps. The Ni/MnO2_2 composite stamps devised here with an area of 1 cm2^2 contained nickel layers prepared by electrodeposition of nickel into macroporous silicon templates[38, 39] adapting procedures reported elsewhere (Figure 1a-Figure 1c).[40] The surface of the ~2 µm thick nickel layers in contact with the macroporous silicon was patterned with arrays of nickel rods, which were negative replicas of the macropores of the macroporous silicon templates. Thus, the nickel rods arranged in hexagonal arrays with a nearest-neighbor distance of 1.5 µm had a diameter of 1 µm, a height of 730 nm and hemispherical tips (Figure 1d and Figure 3a). SEM investigations revealed that no structural defects emerged from the detachment of the Ni layers from the macroporous Si templates (Figure S2). Nickel was selected because of its thermal conductivity and its mechanical properties.[45] These properties were combined with those of a ∼200\sim200 nm thick porous MnO2\mathrm{MnO_2} layer with pore diameters of ∼20\sim20 nm (Figure 1e and Figure 3b,Figure 3c) electrodeposited onto the topographically patterned nickel surface by adapting procedures reported elsewhere.[41] As a result, Ni/MnO2\mathrm{MnO_2} composite stamps having a topographically patterned porous MnO2\mathrm{MnO_2} contact surface were obtained. The topographic patterns of the contact surfaces consisted of arrays of rod-like contact elements with a height of ∼730\sim730 nm and a diameter of 1.2 μ\mum arranged in a hexagonal lattice with a lattice constant of 1.5 μ\mum (Figure 3b,Figure 3c). Using the Ni/MnO2\mathrm{MnO_2} composite stamps, we stamped PFcMA melts containing CNTs onto either pristine ITO substrates or ITO substrates modified with PEO-silane at 190°C under argon atmosphere. The contact time amounted to ∼9.5\sim9.5 min including the heating ramp and a dwell time of 1 min at the target temperature. Liquid bridges consisting of PFcMA melts mixed with CNTs connecting the contact elements of the Ni/MnO2\mathrm{MnO_2} composite stamps and the surfaces of the ITO counterpart substrates were formed (Figure 2a,Figure 2b).

Image not extracted

Figure 3. Figure 3. SEM images of Ni/MnO2_2 composite stamps. a) Topographically patterned nickel layer prior to electrodeposition of MnO2_2. b) Topographically patterned surface and c) cross section of a Ni/MnO2_2 composite stamp. d) SEM image of the contact surface of a Ni/MnO2_2 composite stamp after high-temperature capillary stamping.

Pattern quality

On the ITO counterpart substrates arrays of PFcMA-CNT hybrid microdots typically extending 1 cm2\mathrm{cm^2} – corresponding to the area of the contact surface of the Ni/MnO2\mathrm{MnO_2} composite stamps – were deposited (Figure 2c). A large-field SEM image of an array of PFcMA-CNT hybrid microdots is displayed in Figure 4. Inspection of higher-magnified SEM and AFM images (Figure 5) revealed that the nearest-neighbor distance between the PFcMA-CNT hybrid microdots amounted to 1.5 μ\mum, corresponding to the nearest-neighbor distance between the contact elements of the Ni/MnO2_2 composite stamps. The image field of Figure 4 extends 223 x 146 μ\mum2^2 and would contain 148 x 112 = 16576 PFcMA-CNT hybrid microdots if the latter were arranged in a defect-free hexagonal array. We evaluated a part of Figure 4 that allowed binarization without contrast saturation comprising an image field of 439 x 592 pixels corresponding to an area of 95 x 129 μ\mum2^2. This image field would ideally contain ~6237 PFcMA-CNT hybrid microdots. We actually identified 6012 objects with a size of at least 4 pixels in the probed image field using the software ImageJ, that is, 96 % of the objects expected for an ideal lattice. The occurrence of apparent defects may also be related to the surface roughness of the ITO substrates. Closer scrutinization of the SEM image shown as Figure 4 suggests that a certain proportion of the apparent defect sites is actually occupied by PFcMA-CNT hybrid microdots (Figure S4). Unlike most other PFcMA-CNT hybrid microdots, these PDcMA-CNT hybrid microdots do not show prevalent strong edge contrast because they have a modified shape, likely related to the impact of the local substrate topography on the formation of focal contacts with the contact elements of the Ni/MnO2_2 composite stamps.

Image not extracted

Figure 4. Large-field SEM top-view image of an array of PFcMA-CNT hybrid microdots on an ITO substrate obtained by high-temperature capillary stamping.

Image not extracted

Figure 5. Arrays of PFcMA-CNT hybrid microdots on non-modified ITO substrates produced by high-temperature capillary stamping of PFcMA melts containing CNTs. a)-c) First successive stamping step; d), e) fifth successive stamping step without replenishing of ink. a) SEM image. b), d) AFM topography images (the image fields extend b) 8×8 μm28 \times8\ \mu\mathrm{m}^{2} and d) 5×5 μm25 \times5\ \mu\mathrm{m}^{2}); c), e) Topographic height profiles along the red lines in panels b) and d).

It is reasonable to assume the fidelity of the deposited patterns crucially depends on the quality of the used stamps and their ability to form conformal contact with the counterpart substrates as well as on the roughness and the surface chemistry of the counterpart substrates – independent of whether a polymer melt or a polymer solution is used as ink. However, many polymers of interest, such as PFcMA, are only soluble in organic solvents with relatively high vapor pressure. Apart from unwanted structure formation processes including liquid-liquid phase separation[10] and flow processes related to capillarity,[11, 12] even vitrification of the polymer to be stamped may impede stamping. Problems related to solvent evaporation may be overcome by using spongy stamps penetrated by continuous mesopore systems, but this configuration is of limited use if the ink contains components of limited mobility, such as CNTs. Moreover, polymer solutions tend to spread on non-hydrophobized oxidic surfaces with high surface energy. Even if rapid adsorption of non-volatile ink components results in self-inhibition of spreading, only large, flat pancake-like structures are obtained.[31] High-temperature capillary stamping may help overcome these limitations in certain application scenarios.

Shapes of the PFcMA-CNT hybrid microdots

The diameter of the PFcMA-CNT hybrid microdots amounted to ∼800\sim800 nm (Figure 5a) and their mean height to 233 nm ±\pm 19 nm (Figure 5b,Figure 5c, Figure S5). Stamping of pure PFcMA melts without CNTs onto an pristine ITO substrate under exactly the same conditions as described above yielded PFcMA microdots with diameters and heights by and large identical to those of the PFcMA-CNT hybrid microdots; the mean height of the obtained PFcMA microdots amounted to 256 nm ±37\pm37 nm (Figure S6). Also, stamping of PFcMA-CNT mixtures onto ITO substrates modified with PEO-silane but otherwise under the same conditions as described above did not perceptibly alter diameter and height of the PFcMA-CNT hybrid microdots; their mean height amounted to 248 nm ±30\pm30 nm (Figure S7). The molecular weight distribution of PFcMA subjected to high-temperature capillary stamping as described above remained unaltered, as revealed by size exclusion chromatography (Figure S8). After detachment from the ITO counterpart substrates and cooling to room temperature, the Ni/MnO2_2 composite stamps were still intact (Figure 3d) and could be reused at least five times without replenishment and without apparent changes in the heights of the PFcMA-CNT hybrid microdots. After five consecutive stamping steps we obtained PFcMA-CNT hybrid microdots with a mean height is 239 nm ±10\pm10 nm (Figure 5d, Figure 5e; Figure S9).

The aliquots of the PFcMA-CNT solution administered by default to load the Ni/MnO2_2 composite stamps extending 1 cm21\ \mathrm{cm^2} with the PFcMA-CNT mixture contained 10 µg PFcMA and 0.2 µg CNT. We assume that the loading of the Ni/MnO2_2 composite stamps by dispension of PFcMA-CNT solution did not only result in the deposition of PFcMA-CNT mixture into the mesopores of the MnO2_2 layer but also into the interstices between the contact elements of the Ni/MnO2_2 composite stamps (cf. Figure 2 and Figure 3d). We assume that these PFcMA-CNT reservoirs fed contact elements of the Ni/MnO2_2 composite stamps during high-temperature capillary stamping. The stamping of the PFcMA-CNT mixture onto the ITO surface might also be facilitated by more pronounced van der Waals interactions between PFcMA and ITO as compared to PFcMA and MoO2_2. The metals contained in ITO, In and Sn, are period 5 elements, whereas Mn is a period 4 element so that the polarizability of ITO is likely be higher than that of MnO2_2.

The comparative evaluation of both PFcMA-CNT hybrid microdot arrays and PFcMA microdot arrays suggests that the microdot heights are only marginally influenced by the substrate chemistry (unmodified ITO vs. ITO functionalized with PEO-silane) and the manual retraction of the Ni/MnO2_2 composite stamps. However, loading the Ni/MnO2_2 composite stamps with significantly reduced amounts of PFcMA per stamp area prior to high-temperature capillary stamping modified the stamped patterns. For example, we reduced the PFcMA concentration in the solution used to load the Ni/MnO2_2 composite stamps with PFcMA-CNT mixture to one fifth of the default value, i.e., to 2 mg PFcMA per 10 mL solution, while all other variables were kept constant. Subsequent high-temperature capillary stamping onto a non-modified ITO substrate yielded arrays of irregularly shaped doughnut-like PFcMA-CNT hybrid microstructures (Figure S10). This outcome suggests that a certain excess of PFcMA-CNT mixture per stamp area located on the outer MnO2_2 surface of the Ni/MnO2_2 composite stamps or in the interstices between the contact elements is needed for reproducible high-temperature capillary stamping.

Electrochemical and wettability switching

The impact of the CNTs on the electrochemically induced oxidation and reduction of the PFcMA in PFcMA-CNT hybrid microdots and microdots consisting of pure PFcMA stamped onto pristine ITO substrates was evaluated by cyclic voltammetry. PFcMA-CNT hybrid microdots display narrow and pronounced oxidation and reduction peaks with a peak separation of 220 mV, a maximum oxidation current of 47 μA\mu\mathrm{A} and a reduction current of 53 μA\mu\mathrm{A} (Figure 6a). Pure PFcMA microdots also undergo electrochemical oxidation and reduction (Figure 6b). However, the oxidation and reduction peaks are less pronounced because of the lower conductivity of the PFcMA microdots in the absence of CNTs. The apparently larger peak separation can thus hardly be quantified. The oxidation current amounted to 17 μA\mu\mathrm{A}. Therefore, the presence of CNTs in the PFcMA microdots improved their electrochemical response.

Image not extracted

Figure 6. Cyclic voltammetry of a) PFcMA-CNT hybrid microdot arrays and b) arrays of pure PFcMA microdots deposited on non-modified ITO substrates extending 1 cm2^{2} by high-temperature capillary stamping.

We investigated the wettability of pristine ITO substrates and ITO substrates surface-modified with PEO-silane, which had been patterned with PFcMA-CNT hybrid microdots. To evaluate the impact of the electrochemical switching of the PFcMA-CNT hybrid microdots on the WCAs, we performed five successive electrochemical switching cycles from the reduced state to the oxidized state and vice versa. The apparent WCA measured here does not correspond to the equilibrium WCA or to the Young WCA.[43] However, we assume that it reasonably represents the practical wettability of PFcMA-CNT hybrid microdot arrays under operating conditions. The WCA for PFcMA-CNT hybrid microdot arrays on pristine ITO substrates in the reduced state amounted to 112∘±1∘112^\circ\pm1^\circ and in the oxidized state to 94∘±2∘94^\circ\pm2^\circ (Figure 7a-Figure 7c). Deposition of the PFcMA-CNT hybrid microdots onto ITO substrates modified with PEO-silane resulted in the reduction of the WCAs by nearly 50°. Thus, a WCA of 65∘±1∘65^\circ\pm1^\circ was obtained for the reduced state and of 46∘±1∘46^\circ\pm1^\circ for the oxidized state (Figure 7d). X-ray photoelectron spectroscopy (XPS) indicated that the PEO-silane coating in the ITO substrate was still intact after five electrochemical oxidation-reduction cycles (Figure S11). For a continuous PFcMA film spin-coated on an ITO substrate a WCA of 103∘±1∘103^\circ\pm1^\circ for the reduced and of 75∘±3∘75^\circ\pm3^\circ for the oxidized state was obtained (Figure 7e). In the course of the five successive electrochemical switching cycles no significant systematic change in the WCA values was apparent.

Image not extracted

Figure 7. a) Electrochemical wettability switching of ITO substrates functionalized with PFcMA-CNT hybrid microdot arrays. Blue denotes the reduced and red the oxidized state. a), b) Sessile water droplets on pristine ITO substrates functionalized with PFcMA-CNT hybrid microdot arrays. The PFcMA is a) in the reduced and b) in the oxidized state. The image widths correspond to 3 mm. c)-d) WCAs of sessile water droplets on c) a pristine ITO substrate patterned with a PFcMA-CNT hybrid microdot array, d) on an ITO substrate modified with PEO-silane followed by patterning with PFcMA-CNT hybrid microdot arrays and e) a continuous PFcMA film with a thickness of 300 nm spin-coated on an ITO substrate.

Conclusions

We have reported solvent-free high-temperature capillary stamping with Ni/MnO2\mathrm{Ni/MnO_2} composite stamps to generate arrays of stimuli-responsive polymer microdots. In contrast to continuous coatings, crack propagation and delamination are not possible if arrays of discrete microdots are deposited. Moreover, the exposed substrate areas between the microdots can be orthogonally functionalized, resulting in either synergistic or complementary interplay of the properties of the stimuli-responsive polymer and the second functional component. Solvent-free high-temperature capillary stamping of melts prevents problems associated with the use of polymeric solutions containing volatile organic solvents, such as hardly controllable structure formation processes including phase separation induced by solvent evaporation, capillarity-driven flow processes and ink spreading. The method reported here may also enable the lithographic deposition of polymers, which are hardly soluble or which are only soluble in solvents incompatible with commonly used stamps. As example, we generated arrays of hybrid microdots consisting of the stimuli-responsive polymer PFcMA and CNTs by solvent-free high-temperature capillary stamping at elevated temperatures where the PFcMA is molten. PFcMA-CNT hybrids are known to show electrochemically switchable wettability. For solvent-free high-temperature capillary stamping we used specifically designed composite stamps with a topographically patterned contact surface consisting of a nickel core and a MnO2\mathrm{MnO_2} coating. The latter takes up the PFcMA melt containing the CNTs. The short transport lengths associated with this stamp design allow stamping inks containing additives impeding flow, such as CNTs. Orthogonal functionalization of the ITO substrates between the PFcMA-CNT hybrid microdots with suitable silanes shifted the electrochemical switching range of the water contact angle by nearly 50∘50^\circ.

ASSOCIATED CONTENT

Supporting Information. NMR spectrum of as-synthesized PFcMA, SEM images of topographically structured Ni layers, photos of the stamping device, details of Figure 4, AFM images and height histograms of microdots, SEC characterization of PFcMA, XPS spectra of modified ITO substrates. This material is available free of charge via the Internet at http://pubs.acs.org.

AUTHOR INFORMATION

Corresponding Author

  • Martin Steinhart, Institut für Chemie neuer Materialien and CellNanOs, Universität Osnabrück, Barbarastr. 7, 49076 Osnabrück, Germany; https://orcid.org/0000-0002-5241-8498; Email: [email protected]

Author Contributions

The manuscript was written through contributions of all authors. All authors have given approval to the final version of the manuscript.

References

References

  1. [1]Stuart, M. A. C.; Huck, W. T. S.; Genzer, J.; Müller, M.; Ober, C.; Stamm, M.; Sukhorukov, G. B.; Szleifer, I.; Tsukruk, V. V.; Urban, M.; Winnik, F.; Zauscher, S.; Luzinov, I.; Minko, S. Emerging applications of stimuli-responsive polymer materials. Nat. Mater. 2010, 9, 101-113. https://doi.org/10.1038/nmat2614
  2. [2]Mondal, K.; McMurtrey, M. D. Present status of the functional advanced micro-, nano-printings - a mini review. Mater. Today Chem. 2020, 17, 100328. https://doi.org/10.1016/j.mtchem.2020.100328
  3. [3]Xia, Y., & Whitesides, G. M. (1998). Soft Lithography. Annu. Rev. Mater. Sci., 28, 153–184. https://doi.org/10.1146/annurev.matsci.28.1.153
  4. [4]Qin, D.; Xia, Y.; Whitesides, G. M. Soft lithography for micro- and nanoscale patterning. Nat. Protoc. 2010, 5, 491-502. https://doi.org/10.1038/nprot.2009.234
  5. [5]Kaufmann, T.; Ravoo, B. J. Stamps, inks and substrates: polymers in microcontact printing. Polym. Chem. 2010, 1, 371-387. https://doi.org/10.1039/b9py00281b
  6. [6]Rose, M. A.; Bowen, J. J.; Morin, S. A. Emergent Soft Lithographic Tools for the Fabrication of Functional Polymeric Microstructures. ChemPhysChem 2019, 20, 909-925. https://doi.org/10.1002/cphc.201801140
  7. [7]Huo, F.; Zheng, Z.; Zheng, G.; Giam, L. R.; Zhang, H.; Mirkin, C. A. Polymer pen lithography. Science 2008, 321, 1658-1660. https://doi.org/10.1126/science.1162193
  8. [8]Carbonell, C.; Valles, D. J.; Wong, A. M.; Tsui, M. W.; Niang, M.; Braunschweig, A. B. Massively Multiplexed Tip-Based Photochemical Lithography under Continuous Capillary Flow. Chem 2018, 4, 857-867. https://doi.org/10.1016/j.chempr.2018.01.020
  9. [9]Liu, G. Q.; Petrosko, S. H.; Zheng, Z. J.; Mirkin, C. A. Evolution of Dip-Pen Nanolithography (DPN): From Molecular Patterning to Materials Discovery. Chem. Rev. 2020, 120, 6009-6047. https://doi.org/10.1021/acs.chemrev.9b00725
  10. [10]van de Witte, P.; Dijkstra, P. J.; van den Berg, J. W. A.; Feijen, J. Phase separation processes in polymer solutions in relation to membrane formation. J. Membrane Sci. 1996, 117, 1-31. https://doi.org/10.1016/0376-7388(96)00088-9
  11. [11]Malkin, A. Y. Surface instabilities. Coll. J. 2008, 70, 673-689. https://doi.org/10.1134/s1061933x0806001x
  12. [12]Craster, R. V.; Matar, O. K. Dynamics and stability of thin liquid films. Rev. Mod. Phys. 2009, 81, 1131-1198. https://doi.org/10.1103/RevModPhys.81.1131
  13. [13]Serra, P.; Pique, A. Laser-Induced Forward Transfer: Fundamentals and Applications. Adv. Mater. Technol. 2019, 4, 1800099. https://doi.org/10.1002/admt.201800099
  14. [14]Robinson, T. M.; Hutmacher, D. W.; Dalton, P. D. The Next Frontier in Melt Electrospinning: Taming the Jet. Adv. Funct. Mater. 2019, 29, 1904664. https://doi.org/10.1002/adfm.201904664
  15. [15]Wang, Z. X.; Elimelech, M.; Lin, S. H. Environmental Applications of Interfacial Materials with Special Wettability. Environ. Sci. Technol. 2016, 50, 2132-2150. https://doi.org/10.1021/acs.est.5b04351
  16. [16]He, Z. K.; Lan, X. R.; Hu, Q. S.; Li, H. M.; Li, L. M.; Mao, J. Y. Antifouling strategies based on super-phobic polymer materials. Prog. Org. Coat. 2021, 157, 106285. https://doi.org/10.1016/j.porgcoat.2021.106285
  17. [17]Chi, J. J.; Zhang, X. X.; Wang, Y. T.; Shao, C. M.; Shang, L. R.; Zhao, Y. J. Bio-inspired wettability patterns for biomedical applications. Mater. Horiz. 2021, 8, 124-144. https://doi.org/10.1039/d0mh01293a
  18. [18]Abu Jarad, N.; Imran, H.; Imani, S. M.; Didar, T. F.; Soleymani, L. Fabrication of Superamphiphobic Surfaces via Spray Coating: a Review. Adv. Mater. Technol. 2022, 7, 2101702. https://doi.org/10.1002/admt.202101702
  19. [19]Load, M., & Ghule, B. (2022). Fabrication Techniques of Superhydrophobic Coatings: A Comprehensive Review.. Phys. Status Solidi A, 219, 2200109. https://doi.org/10.1002/pssa.202200109
  20. [20]Xin, B. W.; Hao, J. C. Reversibly switchable wettability. Chem. Soc. Rev. 2010, 39, 769-782. https://doi.org/10.1039/b913622c
  21. [21]Zhang, D. J.; Cheng, Z. J.; Liu, Y. Y. Smart Wetting Control on Shape Memory Polymer Surfaces. Chem. Eur. J. 2019, 25, 3979-3992. https://doi.org/10.1002/chem.201804192
  22. [22]Li, C.; Li, M.; Ni, Z. S.; Guan, Q. W.; Blackman, B. R. K.; Saiz, E. Stimuli-responsive surfaces for switchable wettability and adhesion. J. R. Soc. Interface 2021, 18, 20210162. https://doi.org/10.1098/rsif.2021.0162
  23. [23]Alarslan, F.; Vittadello, L.; Klein, J.; Khan, Q. A.; Kijatkin, C.; Haase, M.; Schäfer, H.; Imlau, M.; Steinhart, M. Thin Patterned Lithium Niobate Films by Parallel Additive Capillary Stamping of Aqueous Precursor Solutions. Adv. Eng. Mater. 2022, 24, 2101159. https://doi.org/10.1002/adem.202101159
  24. [24]Alarslan, F.; Frosinn, M.; Ruwisch, K.; Thien, J.; Jähnichen, T.; Eckert, L.; Klein, J.; Haase, M.; Enke, D.; Wollschläger, J.; Beginn, U.; Steinhart, M. Reactive Additive Capillary Stamping with Double Network Hydrogel-Derived Aerogel Stamps under Solvothermal Conditions. ACS Appl. Mater. Interfaces 2022, 14, 44992−45004. https://doi.org/10.1021/acsami.2c11781
  25. [25]Elbert, J.; Gallei, M.; Rüttiger, C.; Brunsen, A.; Didzoleit, H.; Stühn, B.; Rehahn, M. Ferrocene Polymers for Switchable Surface Wettability. Organometallics 2013, 32, 5873-5878. https://doi.org/10.1021/om400468p
  26. [26]Gallei, M.; Rüttiger, C. Recent Trends in Metallopolymer Design: Redox-Controlled Surfaces, Porous Membranes, and Switchable Optical Materials Using Ferrocene-Containing Polymers. Chem. Eur. J. 2018, 24, 10006-10021. https://doi.org/10.1002/chem.201800412
  27. [27]Hübner, H.; Candeago, R.; Schmitt, D.; Schiesser, A.; Xiong, B. C.; Gallei, M.; Su, X. Synthesis and covalent immobilization of redox-active metallopolymers for organic phase electrochemistry. Polymer 2022, 244, 124656. https://doi.org/10.1016/j.polymer.2022.124656
  28. [28]Xu, H.; Ling, X. Y.; van Bennekom, J.; Duan, X.; Ludden, M. J. W.; Reinhoudt, D. N.; Wessling, M.; Lammertink, R. G. H.; Huskens, J. Microcontact Printing of Dendrimers, Proteins, and Nanoparticles by Porous Stamps. J. Am. Chem. Soc. 2009, 131, 797-803. https://doi.org/10.1021/ja807611n
  29. [29]Han, W.; Hou, P.; Sadaf, S.; Schäfer, H.; Walder, L.; Steinhart, M. Ordered Topographically Patterned Silicon by Insect-Inspired Capillary Submicron Stamping. ACS Appl. Mater. Interfaces 2018, 10, 7451-7458. https://doi.org/10.1021/acsami.7b18163
  30. [30]Schmidt, M.; Philippi, M.; Münzner, M.; Stangl, J. M.; Wieczorek, R.; Harneit, W.; Müller-Buschbaum, K.; Enke, D.; Steinhart, M. Capillary nanostamping with spongy mesoporous silica stamps. Adv. Funct. Mater. 2018, 28, 1800700. https://doi.org/10.1002/adfm.201800700
  31. [31]Runge, M.; Hübner, H.; Grimm, A.; Manoharan, G.; Wieczorek, R.; Philippi, M.; Harneit, W.; Meyer, C.; Enke, D.; Gallei, M.; Steinhart, M. Capillary Stamping of Functional Materials: Parallel Additive Substrate Patterning without Ink Depletion. Adv. Mater. Interfaces 2021, 8, 2001911. https://doi.org/10.1002/admi.202001911
  32. [32]Guo, L. M.; Klein, J.; Thien, J.; Philippi, M.; Haase, M.; Wollschläger, J.; Steinhart, M. Phenolic Resin Dual-Use Stamps for Capillary Stamping and Decal Transfer Printing. ACS Appl. Mater. Interfaces 2021, 13, 49567-49579. https://doi.org/10.1021/acsami.1c17904
  33. [33]Hou, P.; Kumar, R.; Oberleiter, B.; Kohns, R.; Enke, D.; Beginn, U.; Fuchs, H.; Hirtz, M.; Steinhart, M. Scanner-based capillary stamping. Adv. Funct. Mater. 2020, 30, 2001531. https://doi.org/10.1002/adfm.202001531
  34. [34]Xu, H. P., Gomez-Casado, A., Liu, Z. H., Reinhoudt, D. N., Lammertink, R. G. H., & Huskens, J. (n.d.). Porous.
  35. [35]Wu, C.-C.; Xu, H.; Otto, C.; Reinhoudt, D. N.; Lammertink, R. G. H.; Huskens, J.; Subramaniam, V.; Velders, A. H. Porous Multilayer-Coated AFM Tips for Dip-Pen Nanolithography of Proteins. J. Am. Chem. Soc. 2009, 131, 7526-7527. https://doi.org/10.1021/ja901756a
  36. [36]Shin, Y. H.; Yun, S. H.; Pyo, S. H.; Lim, Y. S.; Yoon, H. J.; Kim, K. H.; Moon, S. K.; Lee, S. W.; Park, Y. G.; Chang, S. I.; Kim, K. M.; Lim, J. H. Polymer-Coated Tips for Patterning of Viruses by Dip-Pen Nanolithography. Angew. Chem. Int. Ed. 2010, 49, 9689-9692. https://doi.org/10.1002/anie.201004654
  37. [37]Kim, J.; Shin, Y. H.; Yun, S. H.; Choi, D. S.; Nam, J. H.; Kim, S. R.; Moon, S. K.; Chung, B. H.; Lee, J. H.; Kim, J. H.; Kim, K. Y.; Kim, K. M.; Lim, J. H. Direct-Write Patterning of Bacterial Cells by Dip-Pen Nanolithography. J. Am. Chem. Soc. 2012, 134, 16500-16503. https://doi.org/10.1021/ja3073808
  38. [38]Lehmann, V.; Föll, H. Formation Mechanism and Properties of Electrochemically Etched Trenches in N-Type Silicon. J. Electrochem. Soc. 1990, 137, 653-659. https://doi.org/10.1149/1.2086525
  39. [39]Birner, A.; Grüning, U.; Ottow, S.; Schneider, A.; Müller, F.; Lehmann, V.; Föll, H.; Gösele, U. Macroporous silicon: A two-dimensional photonic bandgap material suitable for the near-infrared spectral range. Phys. Status Solidi A 1998, 165, 111-117. https://doi.org/10.1002/(Sici)1521-396x(199801)165:1<111::Aid-Pssa111>3.0.Co;2-T
  40. [40]Ren, Z.; Li, Y.; Yu, J. A flexible supercapacitor with high true performance. iScience 2018, 9, 138-148.DOI
  41. [41]Broughton, J. N.; Brett, M. J. Variations in MnO2 electrodeposition for electrochemical capacitors. Electrochim. Acta 2005, 50, 4814-4819. https://doi.org/10.1016/j.electacta.2005.03.006
  42. [42]Fadeev, A. Y.; McCarthy, T. J. Self-Assembly Is Not the Only Reaction Possible between Alkyltrichlorosilanes and Surfaces: Monomolecular and Oligomeric Covalently Attached Layers of Dichloro- and Trichloroalkylsilanes on Silicon. Langmuir 2000, 16, 7268-7274. https://doi.org/10.1021/la000471z
  43. [43]Marmur, A.; Della Volpe, C.; Siboni, S.; Amirfazli, A.; Drelich, J. W. Contact angles and wettability: towards common and accurate terminology. Surf. Innov. 2017, 5, 3-8. https://doi.org/10.1680/jsuin.17.00002
  44. [44]Kundu, S.; Wang, Y.; Xia, W.; Muhler, M. Thermal stability and reducibility of oxygen-containing functional groups on multiwalled carbon nanotube surfaces: a quantitative high-resolution XPS and TPD/TPR study. J. Phys. Chem. C 2008, 112, 16869-16878. https://doi.org/10.1021/jp804413a
  45. [45]Buchheit, T. E.; LaVan, D. A.; Michael, J. R.; Christenson, T. R.; Leith, S. D. Microstructural and mechanical properties investigation of electrode posited and annealed LIGA nickel structures. Metall. Mater. Trans. A 2002, 33, 539-554. https://doi.org/10.1007/s11661-002-0116-3

Paper details

vlnc:W_v2c88w96
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 6

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents