betaFeedback

WorksPhysics and Astronomy

Effect of Electron-Phonon Scattering on the Anomalous Hall Conductivity of Fe3_3Sn: A Kagome Ferromagnetic Metal

Abstract

We report on magnetic and magnetotransport studies of a Kagome ferromagnetic metal, Fe3_3Sn. Our studies reveal a large anomalous Hall conductivity (σzxσ_{zx}) in this system, mainly contributed by temperature independent intrinsic Hall conductivity (σzxintσ^{int}_{zx}=485±\pm60 S/cm) and temperature dependent extrinsic Hall conductivity (σzxextσ^{ext}_{zx}) due to skew-scattering. Although σzxextσ^{ext}_{zx} value is large and almost equivalent to the intrinsic Hall conductivity at low temperatures, it drastically decreases with increasing temperature, following the relation σzxext=σzx0ext(aT+1)2σ^{ext}_{zx}=\frac{σ_{zx0}^{ext}}{(aT+1)^2}, under the influence of electron-phonon scattering. The presence of electron-phonon scattering in this system is also confirmed by the linear dependence of longitudinal electrical resistivity at higher temperatures [ρ(T)∝Tρ(T)\propto T]. We further find that Fe3_3Sn is a soft ferromagnet with an easy-axis of magnetization lying in the ab\it{ab} plane of the crystal with magnetocrystalline anisotropy energy density as large as 1.02 ×\times 106^6

Introduction

Hall effect due to which the fast-moving charge carriers get deflected transversely under the external magnetic fields in metals and semiconductors [1] has found lately many real-life technological applications [2, 3]. While an ordinary Hall effect has been noticed in the nonmagnetic metals, an anomalous Hall effect (AHE) was found in the collinear ferromagnetic metals [4, 5] and in the non-collinear antiferromagnetic metals [6, 7]. Moreover, the anomalous Hall effect produces substantially higher Hall resistivity than the ordinary Hall effect, and the field dependent Hall resistivity perfectly scales with magnetization [4, 5]. Though the origin of AHE in non-collinear AFM metals is widely understood by the presence of non-zero Berry phase in momentum space, several mechanisms were proposed to understand the AHE in collinear ferromagnets.

Foremost, Karplus and Luttinger (KL) predicted that the AHE in ferromagnetic metals originates from the interband scattering of the charge carriers under spin-orbit coupling [8], which is recently connected to the Berry curvature of the electronic state of solids [9]. Since the KL theory does not take into account the impurity scattering effects and mainly talks on the intrinsic band structure, considered as the intrinsic theory of AHE. Later on, Smit et al. proposed an extrinsic theory of AHE by incorporating the impurity scattering [10]. The extrinsic AHE happens by two scattering mechanisms, (i) the skew-scattering: whereby the charge carriers scatter asymmetrically by the localized magnetic impurities [10] and (ii) the side-jump: whereby the charge carrier takes a small side jump upon scattering with impurity under spin-orbit coupling [11, 12]. Although many ferromagnetic metals are known to show the AHE [5], the Kagome ferromagnets are quite fascinating systems as they show an intrinsic geometrical frustration, leading to several exotic electronic properties such as the flat-bands near the Fermi level [13, 14, 15, 16], quantum spin-liquid ground state [17, 18], Chern insulating state [19, 20], Weyl fermions [21, 22, 23], Dirac fermions [21, 24, 25], and magnetic topological Skyrmions [26, 27], manifesting the anomalous and topological Hall effects.

Thus, the ferromagnetic metal Co3_3Sn2_2S2_2 is found to exhibit giant intrinsic anomalous Hall conductivity (σxy≈505\sigma_{xy}\approx505 S/cm) [28] due to the presence of Weyl nodes near the Fermi level [29] and Fe3_3Sn is found to show extremely large anomalous Hall conductivity (σxy≈1150\sigma_{xy}\approx1150 S/cm) [30] below 2K and large topological Hall conductivity (-0.875μΩ\mu\Omega cm) above room temperature [31, 32]. On the other hand, recently, a few reports on polycrystalline Fe3_3Sn suggested it to be a ferromagnetic metal in which the Fe atoms form a Kagome network in the abab plane. Further, it was also shown that Fe3_3Sn exhibits a large magnetocrystalline anisotropy energy [33] [34] in addition to the anomalous Nernst effect [35]. Although the previous report shows temperature-dependent anomalous Hall conductivity to some extent, a thorough understanding of the anomalous Hall effect in Fe3_3Sn is still missing, especially the influence of electron-phonon scattering on the AHC.

Fe3_3Sn belongs to the Ni3_3Sn-type family of crystal structure with an in-plane Kagome network. Unlike its sister compound Mn3_3Sn which is a non-collinear antiferromagnet metal, Fe3_3Sn is a collinear in-plane (abab-plane) ferromagnetic metal. In this paper, we mainly focus on the anomalous Hall effect of Fe3_3Sn as a function temperature. For this, we have grown high-quality single crystals of Fe3_3Sn and performed magnetic and magnetotransport studies. Our results unravel two important contributions to the total Hall conductivity of Fe3_3Sn. One of them is the temperature independent intrinsic Hall conductivity originated from the electronic band structure and the other one is the temperature dependent exintrinsic Hall conductivity originated from the asymmetric skew-scattering. Most importantly, we observe that the extrinsic skew-scattering Hall conductivity strongly depends on the inelastic electron-phonon scattering rate (γ\gamma), σzxext=σzxext(γ/γ0+1)2\sigma_{zx}^{ext}=\frac{\sigma_{zx}^{ext}}{(\gamma/\gamma_{0}+1)^{2}}. In addition, the linear dependence of longitudinal electrical resistivity confirms the presence of electron-phonon scattering at higher temperatures. We further show that Fe₃Sn is a soft ferromagnet with an easy-axis of magnetization lying parallel to the abab plane. We derive a magnetocrystalline anisotropy energy density as large as 1.02×1061.02 \times10^{6} J/m³.

Figure 1. (a) Schematic crystal structure and Kagome lattice of Fe₃Sn. (b) Powder XRD pattern of crushed Fe₃Sn single crystals. Inset of (b) shows intensity reflections correspond to (02ˉ\bar{2}20) Brag planes. Left panel in (c) presents EDS spectra of Fe₃Sn along with tabulated elemental ratios and photographic image showing typical Fe₃Sn single crystals. Right panels in (c) show the elemental mapping of measured single crystal for Fe and Sn.

Experimental Details

High quality single crystals of Fe₃Sn were grown by the solid-state crystal growth (SSCG) technique. In SSCG method, the crystals are grown out of polycrystalline matrix. Initially, Fe powder (99.99%, Stern chemicals) and Sn powder (99.995%, Alfa Aesar) were taken in stoichiometric ratio, grounded thoroughly, and heated at 810°C for 7 days. As prepared Fe₃Sn powder was again grounded and pressed into a pellet which was then annealed at 810°C for another 45 days. Several small rod-shaped shiny crystals with a typical size of 1 mm×0.2 mm×0.2 mm were grown on the surface of the pellet. X-ray diffraction (XRD) technique was performed on a rod-shaped single crystal and on the crushed crystals using Rigaku SmartLab 9kW Cu Kα_{\alpha} X-ray source. Elemental analysis was done using the Energy Dispersive X-ray Spectroscopy (EDS of EDAX) suggests an actual chemical composition of Fe₂.₉₈Sn, which is very close to the nominal composition of Fe₃Sn. For the electrical transport and magnetotransport measurements linear four-probe and Hall probe connections were made, respectively, using the copper wire and silver paint. Magnetic and magnetotransport measurements were carried out on the 9T Physical Properties Measurement Systems (PPMS, Quantum Design-DynaCool) using VSM and ETO options. To eliminate the longitudinal voltage contribution due to any misalignment of the connections, the Hall resistivity was measured by applying both positive and negative magnetic fields and average Hall resistivity was calculated by ρH=ρH(H)−ρH(−H)2\rho_{H}=\frac{\rho_{H}(H)-\rho_{H}(-H)}{2}.

Results and Discussions

Fig 1(a) depicts schematic crystal structure of Fe₃Sn where the Fe atoms form a Kagome structure with Sn sitting at the center of the Kagome lattice. Fig. 1(b) shows the powder XRD pattern of crushed Fe₃Sn single crystals, confirming the hexagonal Ni₃Sn type crystal structure with the space group of P6₃/mmc (No. 194). Inset of Fig. 1(b) depicts the XRD performed on a rod-shaped single crystal, showing intensity of reflections from the (0 2 2ˉ\bar{2} 0) Bragg plane, suggesting that the length of rod-shaped crystals is parallel to the cc-axis. Rietveld refinement performed on the powder XRD of crushed single crystals using the Fullprof software [36] derives the lattice parameters a=b=5.4631(4)a=b=5.4631(4) Å and c=4.3552(4)c=4.3552(4) Å, in good agreement with previous reports [33]. Left panel of Fig. 1(c) shows the EDS data from which the atomic and weight percentage of the elements are tabulated on the top-left inset of Fig. 1(c). Photographic image of typical Fe₃Sn single crystals is shown in Fig. 1(c). Elemental mapping performed for Fe and Sn using the EDAX is shown in the right-side panel of Fig. 1(c), implies good homogeneity of single crystals. Temperature dependent magnetization [M(T)][M(T)] between 2 and 300 K performed on Fe₃Sn single crystal with the field (HH) applied parallel to yy-axis (H∥yH \parallel y) and parallel to zz-axis (H∥zH \parallel z) in the field-cooled mode is shown in Figure 2(a). From Figure 2(a) it is evident that below 300 K, M(T)M(T) is completely temperature independent. Figure 2(b) shows M(T)M(T) performed between 300 and 800 K on Fe3_3Sn pellet in the zero-field-cooled mode in order to identify the ferromagnetic transition. From Curie-Weiss fitting of the inverse susceptibility (χ−1(T)\chi^{-1}(T)), using the formula χ=CT−θ\chi= \frac{C}{T-\theta}, we derive a Curie constant of C=7.1±0.1C = 7.1 \pm0.1 emu.mol−1^{-1}Oe−1^{-1}K−1^{-1} and a Curie-Weiss temperature of θ=689±2\theta= 689 \pm2 K, which are consistent with a previous report [33]. The effective magnetic moment of Fe atom in Fe3_3Sn is found to be μeff(Fe)=2.51 μB\mu_{eff}(\mathrm{Fe})=2.51\ \mu_B using the relation μeff=2.828C\mu_{eff}=2.828\sqrt{C} [37].

Figure 2. (a) and (b) Magnetization measured as a function of temperature on Fe3_3Sn single crystals and pellets, respectively. Inset of (b) is Curie-Weiss fitting of inverse susceptibility plotted as a function of temperature. (c) and (d) are the magnetization isotherms [M(H)][M(H)] for H∥yH \parallel y and H∥zH \parallel z, respectively. Insets in (c) and (d) show the saturation magnetization. (e) and (f) Hall resistivity and Hall conductivity, respectively, plotted as a function of field at various sample temperatures for H∥yH \parallel y.

Figure 2(c) and Figure 2(d) depict the magnetization isotherms [M(H)][M(H)] measured at various sample temperatures for H∥yH \parallel y and H∥zH \parallel z, respectively. The saturation field for H∥yH \parallel y is around 0.5 T whereas it is 2 T for H∥zH \parallel z, clearly suggesting that Fe3_3Sn has an easy-axis of magnetization parallel to the abab-plane. Also, the absence of hysteresis in the M(H)M(H) data for the filed applied parallel both directions makes this system a good soft ferromagnet. The saturation magnetic moment per Fe atom is found to be Ms=2.2 μBM_s=2.2\ \mu_B which is close to value of effective magnetic moment μeff=2.51 μB\mu_{eff}=2.51\ \mu_B. From the magnetization isotherms shown in Figure 2(c) and Figure 2(d), we estimated the magnetocrystalline anisotropic energy density Ku=1.02×106K_u = 1.02 \times10^6 J/m3^3 using the relation Ku=μ0∫0Ms[Hy(M)−Hz(M)] dMK_u = \mu_0 \int_0^{M_s} [H_y(M)-H_z(M)]\,dM after excluding the geometrical demagnetization factor [38]. See supplemental material for more details on the calculations of demagnetization factor [39]. Here, MsM_s represents saturation magnetization, HzH_z and HyH_y represent H∥zH \parallel z and H∥yH \parallel y, respectively.

Hall resistivity (ρzx\rho_{zx}) as a function of field is shown in Figure 2(e) measured at various sample temperatures. Here, the current is applied along the zz-axis and the magnetic field is applied along the yy-axis to measure the Hall voltage along the xx-axis of the crystal as depicted in the inset of Figure 2(e). It is evident from Figure 2(e) that Fe3_3Sn shows anomalous Hall effect with a little normal Hall effect that is visible at very high temperatures. Next, the Hall conductivity (σzx\sigma_{zx}) is calculated using the formula σzx=ρzxρzx2+ρzz2\sigma_{zx} = \frac{\rho_{zx}}{\rho_{zx}^2+\rho_{zz}^2}, where ρzx\rho_{zx} is the longitudinal resistivity measured along the zz-axis of the crystal. Figure 2(f) shows σzx\sigma_{zx} plotted as a function of field in which we observe a large anomalous Hall conductivity in the range of 410-425 S-cm−1^{-1} between 75 and 250 K when measured at 5 T, and a sudden drop to 370 S-cm−1^{-1} is observed upon lowering the sample temperature below 75 K. Though high temperature Hall conductivity obtained in this study is consistent with previous report made on polycrystalline Fe3_3Sn [35], the low temperature Hall conductivity of 200 S-cm−1^{-1} at 2 K observed in Ref. [35] is significantly smaller than our findings (≈370\approx370 S-cm−1^{-1} at 5 K).

Next, Figure 3(a) depicts temperature dependent longitudinal resistivity (ρzz\rho_{zz}) measured with current applied along the zz-axis of the crystal. We notice that ρzz\rho_{zz} quadratically depends on the temperature (ρzz∝T2\rho_{zz} \propto T^2) up to ∼\sim75 K, demonstrating a Fermi-liquid type nature of the resistivity at low temperatures [40]. Nevertheless, above 75 K, ρzz\rho_{zz} shows linear depends on the temperature (ρzz∝T\rho_{zz} \propto T) due to a strong electron-phonon interaction [41]. The temperature dependent resistivity profile of our Fe3_3Sn single crystal is consistent with previous report on the polycrystalline Fe3_3Sn [35]. Particularly, the linear dependence of ρzz\rho_{zz} above 75 K is in very good agreement with Ref. [35]. Temperature dependent longitudinal conductivity (σzz\sigma_{zz}) also is shown in Figure 3(a). In general, the total Hall resistivity presented in Figure 2(e) can be expressed by the empirical formula, ρH=ρHN+ρHA\rho_H=\rho_H^N+\rho_H^A [5]. Where, the first term represents normal Hall contribution ρHN=μ0R0H\rho_H^N=\mu_0R_0H and the second term represents the anomalous Hall contribution which in turn depends on the magnetization (MM) as ρHA=μ0RSM\rho_H^A=\mu_0R_SM. Here, R0R_0 and RSR_S are normal and the anomalous Hall coefficients, respectively. Further, with the help of normal Hall coefficient (R0R_0) one can calculate the charge carrier (qq) density using the relation, n=1R0∣q∣n=\frac{1}{R_0|q|}. Since the field dependent anomalous Hall effect is a replica of magnetization, anomalous Hall resistivity saturates beyond a critical field and becomes almost field independent while the normal Hall resistivity linearly depends with field. Thus, in order to separate the anomalous Hall resistivity from the normal Hall contribution, we fitted the high field region of the total Hall resistivity with a linear function of field and subtracted the normal Hall contribution from the total Hall resistivity. In this way, we extracted various important parameters such as the normal (R0R_0) and anomalous (RSR_S) Hall coefficients. Figure 3(b) depicts R0R_0 plotted as a function of temperature. The positive R0R_0 values throughout the measured temperature range as observed in Figure 3(b) suggest hole-carrier dominant electrical transport in Fe3_3Sn. Inset of Figure 3(b) demonstrates almost temperature independent hole carrier density (nhn_h) which is of the order of ∼1022 cm−3\sim10^{22}\ \mathrm{cm}^{-3}, suggesting Fe3_3Sn to be a good metal. Figure 3(c) shows the anomalous Hall coefficient (RSR_S) plotted as a function of temperature. Top-inset of Figure 3(c) presents the anomalous Hall scaling factor (SHS_H), defined as SH=−σzxAM=μ0RSρzz2(≅ρzxAMρzz2)S_H=\frac{-\sigma_{zx}^{A}}{M}=\frac{\mu_0R_S}{\rho_{zz}^2}\left(\cong\frac{\rho_{zx}^{A}}{M\rho_{zz}^2}\right), plotted as a function of temperature. We observe that SHS_H is almost temperature independent within the error-bars. Moreover, the value of SH=0.03±0.01 V−1S_H=0.03\pm0.01\ \mathrm{V}^{-1} derived in this study is within the range of 0.01–0.2 V−1\mathrm{V}^{-1}, for any typical ferromagnetic metal [42, 43]. Bottom-right inset of Figure 3(c) shows temperature dependent anomalous Hall angle (AHA), defined as the deviation of electron flow from the current direction, is calculated using the formula AHA(%)=σzxAσzz×100(%)=\frac{\sigma_{zx}^{A}}{\sigma_{zz}}\times100(\%). We clearly notice that AHA(%)≈3%\approx3\% at 250 K which decreases with temperature. The value of AHA(%)≈3%\approx3\% is close to the AHA values reported on a similar Kagome ferromagnetic system Fe3_3Sn2_2 (≈1.1%\approx1.1\%) [43], Kagome antiferromagnetic systems Mn3_3Sn (≈3.2%\approx3.2\%) [6] and Mn3_3Ge (≈5%\approx5\%) [7], but much smaller than the Shandite Kagome ferromagnet Co3_3Sn2_2S2_2 (≈20%\approx20\%) [28].

Figure 3. (a) Longitudinal electrical resistivity (ρzz\rho_{zz}) and electrical conductivity (σzz\sigma_{zz}) plotted as a function of temperature. (b) and (c) Normal Hall coefficient (R0R_0) and Anomalous Hall coefficient (RSR_S) plotted as a function of temperature, respectively. Charge carrier density (nn) is shown in the inset of (b). Top inset in (c) shows anomalous Hall scale factor (SHS_H) and bottom inset in (c) shows anomalous Hall angle percentage (AHA%). (d) Anomalous Hall conductivity (−σzxA-\sigma_{zx}^{A}) as a function of temperature. (e) −σzxA-\sigma_{zx}^{A} vs. σzz2\sigma_{zz}^{2} plot. The dashed line in (e) is a linear fitting using the relation −σzxA=ρzx0extσzz2+b-\sigma_{zx}^{A}=\rho_{zx0}^{\mathrm{ext}}\sigma_{zz}^{2}+b. (f) Extrinsic anomalous Hall conductivity σzxext\sigma_{zx}^{\mathrm{ext}} plotted as a function of temperature. The solid green curve in (f) is a fit with the equation σzxext=σzx0ext(aT+1)2\sigma_{zx}^{\mathrm{ext}}=\frac{\sigma_{zx0}^{\mathrm{ext}}}{(aT+1)^2}.

Thus, in order to separate the anomalous Hall resistivity from the normal Hall contribution, we fitted the high field region of the total Hall resistivity with a linear function of field and subtracted the normal Hall contribution from the total Hall resistivity. In this way, we extracted various important parameters such as the normal (R0R_0) and anomalous (RSR_S) Hall coefficients.

Several mechanisms were proposed for understanding the anomalous Hall effect in magnetic and nonmagnetic metals. In most of the proposals, the anomalous Hall resistivity (ρzxA\rho_{zx}^{A}) is represented mainly by the function of longitudinal resistivity (ρzz\rho_{zz}), ρzxA=f(ρzz)\rho_{zx}^{A}=f(\rho_{zz}). More explicitly, (i) The intrinsic Karplus-Luttinger mechanism of AHE describes the Hall resistivity ∝ρzz2\propto\rho_{zz}^{2} due to the interband scattering in presence of strong spin-orbit coupling [8], (ii) The extrinsic side-jump mechanism of AHE describes the Hall resistivity ∝ρzz2\propto\rho_{zz}^{2} due to side-jump scattering of charge carriers at the impurities [11], (iii) The extrinsic skew-scattering mechanism of AHE describes the Hall resistivity ∝ρzz\propto\rho_{zz} due to skew-scattering of charge carrier at the impurities [10], (iv) a ρzzα\rho_{zz}^{\alpha} (1<α<21<\alpha<2) dependency of ρzxA\rho_{zx}^{A} was proposed in the case of bad metals [44]. For our case, the mechanism (iv) can be ignored as the longitudinal conductivity of Fe3_3Sn is found to be σzz=31.4e2hc\sigma_{zz}=31.4\frac{e^{2}}{hc} (where cc is the lattice constant) which is in the metallic regime [45]. Recently, a new mechanism (TYJ) was proposed by Tian et al. [46] in order to understand the AHE in ferromagnetic metals. According to TYJ theory, the anomalous Hall resistivity is described by ρzxA=f(ρzz0,ρzz)\rho_{zx}^{A}=f(\rho_{zz0},\rho_{zz}) which includes the residual resistivity (ρzz0\rho_{zz0}). Thus, following the TYJ theory [46, 47], the anomalous Hall resistivity takes the form ρzxA=(αρzz0+βρzz02)+bρzz2\rho_{zx}^{A}=(\alpha\rho_{zz0}+\beta\rho_{zz0}^{2})+b\rho_{zz}^{2} and the anomalous Hall conductivity is represented by −σzxA=(ασzz0−1+βσzz0−2)σzz2+b=ρzx0Aσzz2+b-\sigma_{zx}^{A}=(\alpha\sigma_{zz0}^{-1}+\beta\sigma_{zz0}^{-2})\sigma_{zz}^{2}+b=\rho_{zx0}^{A}\sigma_{zz}^{2}+b. Here, α\alpha and β\beta are real constants, σzz0=1/ρzz0\sigma_{zz0}=1/\rho_{zz0} is the residual conductivity, and bb is the intrinsic Hall conductivity originated from the momentum space Berry curvature. It is well known that the intrinsic Hall conductivity (bb) is usually temperature independent [5, 28] except for the systems showing electronic or magnetic phase transitions [9, 48]. Since Fe3_3Sn shows neither electronic nor magnetic transition within the measured temperature range of 2-250 K, change in the Berry phase is not expected. From Figure 3(d), we notice that the anomalous Hall conductivity is almost constant at higher temperatures, but decreases below 150 K. To understand this phenomenon, we employed TYJ mechanism to fit the data of −σzxA-\sigma_{zx}^{A} vs. σzz2\sigma_{zz}^{2} as shown in Figure 3(e), demonstrating a good fitting within the error-bars. From the fitting, we extracted intrinsic Hall conductivity b=485±60b=485\pm60 S/cm that is close to the previously reported values on polycrystalline Fe3_3Sn (≈500\approx500 S/cm) [35] and predicted by a theoretical calculation (≈600\approx600 S/cm at EFE_F) [49].

Next, Figure 3(f) shows the extrinsic Hall conductivity (σzxext\sigma_{zx}^{ext}) extracted from the total conductivity by subtracting the intrinsic Hall contribution (bb). From Figure 3(f), it is evident that the extrinsic Hall conductivity decreases with increasing sample temperature. Further, the sign of extrinsic Hall conductivity is opposite to the intrinsic Hall conductivity, resulting into the reduced total Hall conductivity at lower temperatures. As we know, in the clean limit, for ℏ/τ→0\hbar/\tau\to0 (τ\tau is the relaxation time) the extrinsic skew-scattering contribution diverges [50]. On the other hand, from Figure 3(f), we can see that as the sample temperature decreases the extrinsic Hall conductivity rapidly increases. This observation indicates that skew-scattering playing a major role to generate the anomalous Hall conductivity in Fe3_3Sn. The longitudinal resistivity (ρzz\rho_{zz}) suggests electron-phonon scattering at higher temperatures in this system. In order to understand the phonon influence on the anomalous Hall conductivity, we employed the mechanism proposed by Shitade and Nagaosa [45] which involves the electron-phonon inelastic scattering rates (γ\gamma). In this mechanism, the extrinsic Hall conductivity decays with γ\gamma following the relation σzxext=σzx0ext(γ/γ0+1)2\sigma_{zx}^{ext}=\frac{\sigma_{zx0}^{ext}}{(\gamma/\gamma_{0}+1)^{2}}. Since the inelastic scattering rate is proportional to the longitudinal resistivity [γ∼(ρzz−ρzz0)][\gamma\sim(\rho_{zz}-\rho_{zz0})] and ρzz−ρzz0\rho_{zz}-\rho_{zz0} linearly depends on temperature [(ρzz−ρzz0)∝T][(\rho_{zz}-\rho_{zz0})\propto T] above 75 K (see Fig. 3(a)), we can rewrite the equation as σzxext=σzx0ext(aT+1)2\sigma_{zx}^{ext}=\frac{\sigma_{zx0}^{ext}}{(aT+1)^{2}}. Here, a=0.011±0.003a=0.011\pm0.003 K−1^{-1} represents the measure of inelastic electron-phonon scattering strength. In this way, we could fit the σzxext\sigma_{zx}^{ext} data very well as shown in Figure 3(f). Thus, our results clearly demonstrate the influence of electron-phonon interaction on the extrinsic skew-scattering anomalous Hall conductivity which decreases with increasing temperature. Finally, we would like to mention here that during the course of our manuscript preparation a preprint on the magnetic studies of Fe3_3Sn single crystals has appeared [51]. The magnetic properties presented in their study are consistent with our findings. Particularly, the magnetocrystalline anisotropy energy density of 1.23×1061.23\times10^{6} J/m3^{3} reported in Ref. [51] is in good agreement with the value of 1.02×1061.02\times10^{6} J/m3^{3} found in this study.

Summary

In summary, we have successfully grown high quality single crystals of Fe3_3Sn. In this study, we mainly focussed on understanding the anomalous Hall effect as a function temperature. Our results unravel two main contributions to the total Hall conductivity of Fe3_3Sn. One of them is the temperature independent intrinsic Hall conductivity originated from the electronic band structure and the other one is the temperature dependent extrinsic Hall conductivity due to the asymmetric skew-scattering. Most importantly, we find that the extrinsic skew-scattering Hall conductivity is significantly influenced by the electron-phonon scattering at higher temperatures and obeys the relation σzxext=σzx0ext(aT+1)2\sigma_{zx}^{ext}=\frac{\sigma_{zx0}^{ext}}{(aT+1)^{2}}. In addition, the longitudinal electrical resistivity (ρzz\rho_{zz}) confirm the presence of electron-phonon scattering as the resistivity linearly depends on the temperature. We show that Fe3_3Sn is a soft ferromagnet with easy-axis magnetization lying parallel to the abab plane. We estimate a magnetocrystalline anisotropic energy density as large as 1.02×1061.02\times10^{6} J/m3^{3} in Fe3_3Sn.

Acknowledgments

The authors thank the Science and Engineering Research Board (SERB), Department of Science and Technology (DST), India for the financial support (Grant No. SRG/2020/000393). This research has made use of the Technical Research Centre (TRC) Instrument Facilities of S. N. Bose National Centre for Basic Sciences, established under the TRC project of Department of Science and Technology, Govt. of India.

References

Supplementary Information

Figure 4. Magnetization isotherms [M(Heff)][M(H_{\rm eff})] measured at various sample temperatures for H∥yH \parallel y (a) and H∥zH \parallel z (b). Here, HeffH_{\rm eff} is the effective magnetization field after excluding the shape demagnetizing factor of the approximately rod-shaped sample using the formula, Heff=H−NdMH_{\rm eff}=H-N_dM, where NdN_d is the demagnetization factor. For our rod-shaped sample, the calculated Nd−1=2+12acN_d^{-1}=2+\frac{1}{\sqrt{2}}\frac{a}{c} for H∥yH \parallel y is 0.45 and Nd−1=1+1.6caN_d^{-1}=1+1.6\frac{c}{a} for H∥zH \parallel z is 0.15 [38]. Here, a=0.2a=0.2 mm and c=0.7c=0.7 mm are the sample diameter and length, respectively.

References

  1. [1]E. H. Hall, On a new action of the magnet on electric currents, American Journal of Mathematics 2, 287 (1879).
  2. [2]R. S. Popovic, Hall effect devices (CRC Press, 2003).
  3. [3]E. Ramsden, Hall-effect sensors: theory and application (Elsevier, 2011).
  4. [4]E. Hall, On the new action of magnetism on a permanent electric current, The London, Edinburgh, and Dublin Philosophical Magazine and Journal of Science 10, 301 (1880).
  5. [5]N. Nagaosa, J. Sinova, S. Onoda, A. H. MacDonald, and N. P. Ong, Anomalous Hall effect, Rev. Mod. Phys. 82, 1539 (2010).DOI
  6. [6]S. Nakatsuji, N. Kiyohara, and T. Higo, Large anomalous Hall effect in a non-collinear antiferromagnet at room temperature, Nature 527, 212 (2015).
  7. [7]A. K. Nayak, J. E. Fischer, Y. Sun, B. Yan, J. Karel, A. C. Komarek, C. Shekhar, N. Kumar, W. Schnelle, J. Kübler, C. Felser, and S. S. P. Parkin, Large anomalous Hall effect driven by a nonvanishing Berry curvature in the noncollinear antiferromagnet Mn3Ge, Sci. Adv. 2, e1501870 (2016).DOI
  8. [8]R. Karplus and J. M. Luttinger, Hall Effect in Ferromagnetics, Phys. Rev. 95, 1154 (1954).DOI
  9. [9]K. Manna, L. Muechler, T.-H. Kao, R. Stinshoff, Y. Zhang, J. Gooth, N. Kumar, G. Kreiner, K. Koepernik, R. Car, J. Kübler, G. H. Fecher, C. Shekhar, Y. Sun, and C. Felser, From Colossal to Zero: Controlling the Anomalous Hall Effect in Magnetic Heusler Compounds via Berry Curvature Design, Phys. Rev. X 8, 041045 (2018).DOI
  10. [10]J. Smit, The spontaneous hall effect in ferromagnetics II, Physica 24, 39 (1958).DOI
  11. [11]L. Berger, Side-Jump Mechanism for the Hall Effect of Ferromagnets, Phys. Rev. B 2, 4559 (1970).DOI
  12. [12]S. K. Lyo and T. Holstein, Side-Jump Mechanism for Ferromagnetic Hall Effect, Phys. Rev. Lett. 29, 423 (1972).DOI
  13. [13]B. Sutherland, Localization of electronic wave functions due to local topology, Phys. Rev. B 34, 5208 (1986).pubmed.ncbi.nlm.nih.gov/9940349
  14. [14]E. H. Lieb, Two theorems on the Hubbard model, Phys. Rev. Lett. 62, 1201 (1989).
  15. [15]D. Leykam, A. Andreanov, and S. Flach, Artificial flat band systems: from lattice models to experiments, Advances in Physics: X 3, 1473052 (2018).DOI
  16. [16]C. Wu, D. Bergman, L. Balents, and S. Das Sarma, Flat Bands and Wigner Crystallization in the Honeycomb Optical Lattice, Phys. Rev. Lett. 99, 074041 (2007).DOI
  17. [17]L. Savary and L. Balents, Quantum spin liquids: a review, Rep. Prog. Phys. 80, 016502 (2016).DOI
  18. [18]C. Broholm, R. J. Cava, A. A. Kivelson, D. G. Nocera, M. R. Norman, and T. Senthil, Quantum spin liquids, Science 367, eaay0668 (2020).
  19. [19]C. L. Kane and E. J. Mele, Quantum Spin Hall Effect in Graphene, Phys. Rev. Lett. 95, 226801 (2005).pubmed.ncbi.nlm.nih.gov/16384250
  20. [20]H. Huang, Z. Liu, H. Zhang, W. Duan, and D. Vanderbilt, Emergence of a Chern-insulating state from a semi-Dirac dispersion, Phys. Rev. B 92, 1611115 (2015).DOI
  21. [21]P. B. Pal, Dirac, Majorana, and Weyl fermions, Amer. J. Phys. 79, 485 (2011).DOI
  22. [22]G. Xu, H. Weng, Z. Wang, X. Dai, and Z. Fang, Chern Semimetal and the Quantized Anomalous Hall Effect in HgCr2Se4, Phys. Rev. Lett. 107, 186806 (2011).pubmed.ncbi.nlm.nih.gov/22107665
  23. [23]K. Landsteiner, Anomalous transport of Weyl fermions in Weyl semimetals, Phys. Rev. B 89, 075124 (2014).DOI
  24. [24]K. S. Novoselov, A. K. Geim, S. V. Morozov, D. Jiang, M. I. Katsnelson, I. V. Grigorieva, S. Dubonos, and a. Firsov, Two-dimensional gas of massless Dirac fermions in graphene, Nature 438, 197 (2005).DOI
  25. [25]K. Nomura and A. H. MacDonald, Quantum Transport of Massless Dirac Fermions, Phys. Rev. Lett. 98, 076602 (2007).pubmed.ncbi.nlm.nih.gov/17359041
  26. [26]N. Nagaosa and Y. Tokura, Topological properties and dynamics of magnetic skyrmions, Nat. Nanotechnol. 8, 899 (2013).DOI
  27. [27]A. Fert, N. Reyren, and V. Cros, Magnetic skyrmions: advances in physics and potential applications, Nat. Rev. Mater. 2, 1 (2017).DOI
  28. [28]E. Liu, Y. Sun, N. Kumar, L. Muechler, A. Sun, L. Jiao, S.-Y. Yang, D. Liu, A. Liang, Q. Xu, et al., Giant anomalous Hall effect in a ferromagnetic kagome-lattice semimetal, Nat. Phys. 14, 1125 (2018).DOI
  29. [29]N. Morali, R. Batabyal, P. K. Nag, E. Liu, Q. Xu, Y. Sun, B. Yan, C. Felser, N. Avraham, and H. Beidenkopf, Fermi-arc diversity on surface terminations of the magnetic Weyl semimetal Co3Sn2S2, Science 365, 1286 (2019).DOI
  30. [30]L. Ye, M. Kang, J. Liu, F. von Cube, C. R. Wicker, T. Suzuki, C. Jozwiak, A. Bostwick, E. Rotenberg, D. C. Bell, L. Fu, R. Comin, and J. G. Checkelsky, Massive Dirac fermions in a ferromagnetic kagome metal, Nature 555, 638 (2018).DOI
  31. [31]Z. Hou, W. Ren, B. Ding, G. Xu, Y. Wang, B. Yang, Q. Zhang, Y. Zhang, E. Liu, F. Xu, W. Wang, G. Wu, X. Zhang, B. Shen, and Z. Zhang, Observation of Various and Spontaneous Magnetic Skyrmionic Bubbles at Room Temperature in a Frustrated Kagome Magnet with Uniaxial Magnetic Anisotropy, Advanced Materials 29, 1701144 (2017).
  32. [32]H. Li, B. Ding, J. Chen, Z. Li, Z. Hou, E. Liu, H. Zhang, X. Xi, G. Wu, and W. Wang, Large topological Hall effect in a geometrically frustrated kagome magnet Fe3Sn2, Appl. Phys. Lett. 114, 192408 (2019).DOI
  33. [33]B. C. Sales, B. Saparov, M. A. McGuire, D. J. Singh, and D. S. Parker, Ferromagnetism of Fe3Sn and alloys, Sci. Rep. 4, 1 (2014). per, Tuning the magnetocrystalline anisotropy of Fe3Sn by alloying, Phys. Rev. B 99, 024421 (2019).
  34. [35]T. Chen, S. Minami, A. Sakai, Y. Wang, Z. Feng, T. Nomoto, M. Hirayama, R. Ishii, T. Koretsune, R. Arita, and S. Nakatsuji, Large anomalous Nernst effect and nodal plane in an iron-based kagome ferromagnet, Sci. Adv. 8, eabk1480 (2022).DOI
  35. [36]J. Rodríguez-Carvajal, FullProf, CEA/Saclay, France 1045, 132 (2001).
  36. [37]S. Mugiranzea and A. M. Hallas, Tutorial: a beginner’s guide to interpreting magnetic susceptibility data with the Curie-Weiss law, Communications Physics 5, 95 (2022).
  37. [38]R. Prozorov and V. G. Kogan, Effective Demagnetizing Factors of Diamagnetic Samples of Various Shapes, Phys. Rev. Appl. 10, 014030 (2018).DOI
  38. [39]See supplemental information for the calculations on geometrical demagnitization factor.
  39. [40]K. Behnia, On the Origin and the Amplitude of T-Square Resistivity in Fermi Liquids, Ann. Phys. 534, 2100588 (2022).DOI
  40. [41]G. Varelogiannis and E. N. Economou, Small-q electron-phonon scattering and linear dc resistivity in High-Tc oxides, Europhys. Lett. 42, 313 (1998).DOI
  41. [42]C. Zeng, Y. Yao, Q. Niu, and H. H. Weitering, Linear Magnetization Dependence of the Intrinsic Anomalous Hall Effect, Phys. Rev. Lett. 96, 037204 (2006).pubmed.ncbi.nlm.nih.gov/16486762
  42. [43]Q. Wang, S. Sun, X. Zhang, F. Pang, and H. Lei, Anomalous Hall effect in a ferromagnetic Fe3Sn2 single crystal with a geometrically frustrated Fe bilayer kagome lattice, Phys. Rev. B 94, 075135 (2016).DOI
  43. [44]J. M. Lavine, Extraordinary Hall-Effect Measurements on Ni, Some Ni Alloys, and Ferrites, Phys. Rev. 123, 1273 (1961).DOI
  44. [45]A. Shitade and N. Nagaosa, Anomalous Hall Effect in Ferromagnetic Metals: Role of Phonons at Finite Temperature, J. Phys. Soc. Jpn. 81, 083704 (2012).
  45. [46]Y. Tian, L. Ye, and X. Jin, Proper Scaling of the Anomalous Hall Effect, Phys. Rev. Lett. 103, 087206 (2009).DOI
  46. [47]D. Hou, G. Su, Y. Tian, X. Jin, S. A. Yang, and Q. Niu, Multivariable Scaling for the Anomalous Hall Effect, Phys. Rev. Lett. 114, 217203 (2015).DOI
  47. [48]N. H. Sung, F. Ronning, J. D. Thompson, and E. D. Bauer, Magnetic phase dependence of the anomalous Hall effect in Mn3Sn single crystals, Appl. Phys. Lett. 112, 132406 (2018).DOI
  48. [49]C. Shen, I. Samathrakis, K. Hu, H. K. Singh, N. Fortunato, H. Liu, O. Guthfleisch, and H. Zhang, Thermodynamical and topological properties of metastable Fe3Sn, npj Comput. Mater. 8, 248 (2022).arxiv.org/abs/2203.01172
  49. [50]S. Onoda, N. Sugimoto, and N. Nagaosa, Intrinsic Versus Extrinsic Anomalous Hall Effect in Ferromagnets, Phys. Rev. Lett. 97, 126602 (2006).pubmed.ncbi.nlm.nih.gov/17025988
  50. [51]L. Prodan, D. M. Evans, S. M. Griffin, A. Östlin, M. Althaler, E. Lysne, I. G. Filippova, S. Shova, L. Chioncel, V. Tsurkan, and I. Kézsmárki, Large ordered moment with strong easy-plane anisotropy and vortex-domain pattern in the kagome ferromagnet Fe3Sn (2023).

Paper details

vlnc:W_v6k23tcr
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents