Abstract

Interfacial magnetism stimulates the discovery of giant magnetoresistance and spin-orbital coupling across the heterointerfaces, facilitating the intimate correlation between spin transport and complex magnetic structures. Over decades, functional heterointerfaces composed of nitrides are seldomly explored due to the difficulty in synthesizing high-quality and correct composition nitride films. Here we report the fabrication of single-crystalline ferromagnetic Fe3N thin films with precisely controlled thickness. As film thickness decreasing, the magnetization deteriorates dramatically, and electronic state transits from metallic to insulating. Strikingly, the high-temperature ferromagnetism maintains in a Fe3N layer with a thickness down to 2 u. c. (~ 8 Å). The magnetoresistance exhibits a strong in-plane anisotropy and meanwhile the anomalous Hall resistance reserves its sign when Fe3N layer thickness exceeds 5 u. c. Furthermore, we observe a sizable exchange bias at the interfaces between a ferromagnetic Fe3N and an antiferromagnetic CrN. The exchange bias field and saturation moment strongly depend on the controllable bending curvature using cylinder diameter engineering (CDE) technique, implying the tunable magnetic states under lattice deformation. This work provides a guideline for exploring functional nitride films and applying their interfacial phenomena for innovative perspectives towards the practical applications.

Article type: Communications

Main Text

Magnetic materials possessing ultra-large remanent magnetization and small coercive field are generally useful in the magnetic recording and energy harvest industries, such as motors, generators, actuators, etc.[1, 2, 3] Typically, Fe-Co alloys and compounds containing rare-earth elements (such as Sm, Nd, etc.) are historically choices for the beforehand applications [4, 5].

However, the cost for manufacturing and maintenance of such materials are too high to develop high-efficient, compact, and reliable devices for future technologies. Transition metal nitrides (TMNs) are a class of functional materials in which the nitrogen atoms are integrated into the interstitial sites of parent metals.[6, 7, 8] Therefore, TMNs exhibit extremely rich physical properties, for instance, high dielectricity,[9, 10] high thermal conductivity,[11] superconductivity,[12, 13] ferroelectricity,[14, 15, 16] as well as magnetism.[17, 18, 19] Except for these remarkable physical properties, the characteristics of superior hardness, corrosion resistance, and antioxidant make TMNs stable in air and are suitable for coating layers of functional devices.[1, 2, 3] Although TMNs have many advantages, the challenges in synthesizing single crystalline TMNs thin films with high crystallinity and correct chemical composition hinder the research in their intrinsic properties and intriguing interfacial phenomena. Taking iron nitrides as example, Fe16N2\mathrm{Fe}_{16}\mathrm{N}_{2} has been theoretically predicted as one of the most promising rare-earth-free strong magnet candidates with a giant saturation moment (∼3.5 μB/Fe\sim3.5\ \mu_{\mathrm{B}}/\mathrm{Fe}), which is 36% larger than that of a single-crystalline iron (∼2.2 μB/Fe\sim2.2\ \mu_{\mathrm{B}}/\mathrm{Fe}).[20, 21] Increasing the nitrogen content, Fe3N\mathrm{Fe}_{3}\mathrm{N} exhibits ferromagnetism with slightly reduced saturation moment. It holds the potential applications in the magnetic tunneling junctions (MTJs) and spin-polarized light-emitting diodes due to its ultra large spin polarization.[22, 23, 24, 25, 26, 27] However, Fe3N\mathrm{Fe}_{3}\mathrm{N} often appears in other iron nitride forms due to the close thermally stable energy. The magnetic and electrical properties of Fe3NFe_3N have been greatly influenced by the impurities, chemical disorders, and nitrogen vacancies (NVs).[28] At present, most work are mainly focus on the amorphous, polycrystalline, and nanoparticle nitrides.[22, 23, 24, 25, 26, 27, 28] The sample quality hinders the deep investigation of their intrinsic properties in its thin film form. Therefore, mastering the advanced preparation method of TMN magnetic films with accurate stoichiometric ratio is particularly important for understanding the structure of objective substances and investigating the coupling mechanism between spin and other degrees of freedom. These factors are the core constraints that restrict the practical applications of this excellent magnetic materials.

Previously, most TMNs thin films were fabricated by reactive magnetron sputtering, radio-frequency nitrogen plasma-assisted molecular beam epitaxy (MBE) or metalorganic chemical vapor deposition (MOCVD).[29, 30, 31] The crystallinity is relatively poor because of the formation of polycrystalline grains and NVs. Recently, our group reported the fabrication of high-crystalline stoichiometric CrNCrN ultrathin films using pulsed laser deposition (PLD) technique.[32, 33, 34, 35] The specimens were prepared by laser ablating from a high-pressure synthesized stoichiometric target and compensating the NVs using in-situ atomic nitrogen plasma source. The CrNCrN thin films fabricated in this manner exhibit a paramagnetic-to-antiferromagnetic transition at a temperature close to its bulk value ∼283\sim283 K,[36, 37] indicating the correct stoichiometry of high-quality CrNCrN films. Thus, their intrinsic physical properties depending on the thickness, orientation, stacking sequence, and emergent interfacial phenomena have been explored in a controlled manner,[32, 33, 34, 35] similar to the extensively investigated transition metal oxides.

In this work, we report the fabrication of stoichiometric single-crystalline Fe3NFe_3N thin films and their integration of antiferromagnetic CrNCrN films with atomically sharp interfaces. The thickness-dependent magnetic and electrical phase transitions were observed. The ferromagnetic ground state of a Fe3N\mathrm{Fe}_3\mathrm{N} film is maintained when its thickness reduces to 2 unit cells (u. c.). We observe a significant anomaly in the out-of-plane magnetic hysteresis loops depending on the film thickness and temperature, which may be attributed to the reorientation of canted spins. We note that the magnetic properties of a freestanding Fe3N/CrN\mathrm{Fe}_3\mathrm{N}/\mathrm{CrN} bilayer are extremely sensitive (∼2680 emu/cm3\sim2680\ \mathrm{emu}/\mathrm{cm}^{3} per mm−1\mathrm{mm}^{-1}) to the bending stress, providing an innovative strategy for designing uniaxial-strain sensors.

The nitridation of iron leads to a variety of phases, which strongly depend on the nitrogen content. Among them, ε-phase Fe3N\mathrm{Fe}_3\mathrm{N} (ε-Fe3N\mathrm{Fe}_3\mathrm{N}, abbreviation Fe3N\mathrm{Fe}_3\mathrm{N} thereafter) exhibits interesting magnetic states and extends over a wide range of phase diagram.[38] A typical crystallized form of Fe3N\mathrm{Fe}_3\mathrm{N} is present in Figure 1a. A succession of Fe-N layers is arranged along the cc axis with N layers as spacers between Fe layers, resulting in an out-of-plane lattice constant of 4.38 Å. When viewed from [1] direction, Fe3N\mathrm{Fe}_3\mathrm{N} consists of alternating atomic planes of Fe3+\mathrm{Fe}^{3+} and N3−\mathrm{N}^{3-} ions with a buckled hexagonal structure (Figure 1b). The atomic arrangement of Fe3N\mathrm{Fe}_3\mathrm{N} is similar to that of a (0001) surface of α\alpha-Al2O3\mathrm{Al}_2\mathrm{O}_3 (point group R3ˉc\mathit{R}\bar{3}c) (Figure 1c). The lattice constants of Fe3N\mathrm{Fe}_3\mathrm{N} and α\alpha-Al2O3\mathrm{Al}_2\mathrm{O}_3 are very close, yielding to a moderate lattice mismatch of -1.8%. The similar crystal symmetry and small lattice mismatch allow us to fabricate ε-phase Fe3N\mathrm{Fe}_3\mathrm{N} films on the α\alpha-Al2O3\mathrm{Al}_2\mathrm{O}_3 substrates epitaxially using plasma-assisted PLD technique. The highly reactive N atoms generated by a radio-frequency plasma source in-situ compensate the NVs during the growth. This process guarantees the correct stoichiometry of Fe3N\mathrm{Fe}_3\mathrm{N} films. Microstructures around the interfaces between Fe3N\mathrm{Fe}_3\mathrm{N} and α\alpha-Al2O3\mathrm{Al}_2\mathrm{O}_3 are shown in Figure 1d, performed by scanning transmission electron microscopy (STEM) in the high-angle annular dark field (HAADF) mode. The STEM image indicates the high crystallinity of Fe3N\mathrm{Fe}_3\mathrm{N} single layers, and the sample is free of obvious defects. The HAADF-STEM image confirms the epitaxial growth of Fe3N\mathrm{Fe}_3\mathrm{N} on the substrates with atomically sharp interfaces. To note, we observe an ultrathin transition layer with a thickness of ~ 1 nm (marked in yellow arrows) between Fe3N\mathrm{Fe}_3\mathrm{N} and α\alpha-Al2O3\mathrm{Al}_2\mathrm{O}_3. This fact can be attributed to the accommodation of misfit strain. The inset of Figure 1d on the upper right shows the high magnified STEM image of a region in Fe3N\mathrm{Fe}_3\mathrm{N}. The bright features indicate the positions of Fe atom columns, matching well with the atomic structure of single-phase ε\varepsilon-Fe3N\mathrm{Fe}_3\mathrm{N}.[39] The light element N cannot be observed clearly in these STEM images due to the small atomic number (ZZ).

Structure and electronic state characterizations of single crystalline Fe₃N films

Figure 1. Structure and electronic state characterizations of single crystalline Fe3_3N films. (a) Schematic of a Fe3_3N single unit cell. (b) and (c) Top-views of Fe3_3N and Al2_2O3_3 lattice structures, respectively, yielding to highly compatible group symmetry and relatively small misfit strain of ~ −1.8%-1.8\%. (d) Atomic-resolved STEM image across the Fe3_3N/Al2_2O3_3 interface. Inset shows a representative zoom-in STEM image with atomic structures. (e) XRD θ\theta-2θ2\theta scan of a 30-u.c.-thick Fe3_3N film. Inset of (e) shows the RSM around the 006 reflection of Al2_2O3_3 substrate. (f) and (g) N 1s and Fe 2p core-level XPS of a typical Fe3_3N single film, confirming the presence of sufficient nitrogen content.

X-ray diffraction (XRD) measurements were carried out on a Panalytical MRD diffractometer equipped with a monochromator (only Kα1K\alpha_1 is allowed, λ\lambda = 1.54 Å). The film thickness is controlled by counting number of laser pulse, further confirmed by X-ray reflectivity (XRR) (Figure S1). Figure 1e shows the XRD θ\theta-2θ2\theta scans for a 30-u. c.-thick Fe3N\mathrm{Fe}_3\mathrm{N} on α\alpha-Al2O3\mathrm{Al}_2\mathrm{O}_3 substrates. Only 00l00l reflections from both films and substrates are observed, suggesting the epitaxial growth of Fe3N\mathrm{Fe}_3\mathrm{N} films. Inset of Figure 1e presents a reciprocal space map (RSM) around substrates’ 006 reflection. The clear Kiessig fringes up to three orders together with a narrow rocking curve at Fe3N\mathrm{Fe}_3\mathrm{N} 002 reflection with full width at half maximum (FWHM) of ~ 0.03° (not shown) indicate the high crystallinity of as-grown Fe3N\mathrm{Fe}_3\mathrm{N} films. We determined that the out-of-plane lattice constant of Fe3N\mathrm{Fe}_3\mathrm{N} is ~ 4.38 Å, which is close to its bulk value. The relaxation of epitaxial misfit strain is attributed to the sharp structural transition at interfaces (Figure 1d). XPS analysis of Fe3N\mathrm{Fe}_3\mathrm{N} films was carried out by investigating N 1s (Figure 1f) and Fe 2p (Figure 1g) core level spectra. The binding energy was carefully calibrated by taking C 1s peak at 284.6 eV as a reference. Only one main peak centered at 397.4 eV was observed corresponding to N 1s state due to the N content in Fe3N\mathrm{Fe}_3\mathrm{N}. The prominent components of Fe 2p2p peaks at 710 and 725 eV indicate hybridization between Fe and N. We notice that there are two weak pre-peaks at 706 and 720 eV, which may associate with metallic unbonded Fe termination layers on the top surface.[40]

The magnetic and electrical transport properties of Fe3N\mathrm{Fe}_3\mathrm{N} films were investigated as a function of film thickness. Figure 2a and Figure 2b shows the temperature dependent magnetization (MM) and resistivity (ρ\rho) of 6- and 30-u.c.-thick Fe3N\mathrm{Fe}_3\mathrm{N} films, respectively. MM-TT and ρ\rho-TT curves for Fe3N\mathrm{Fe}_3\mathrm{N} single films with various film thicknesses are shown in Figure S2. Thickness dependent Curie temperature (TCT_\mathrm{C}), saturation moment (MSM_\mathrm{S}), and ρ300K\rho_{300\mathrm{K}} are summarized in Figure 2e-Figure 2g, respectively. TCT_\mathrm{C} of a 30-u.c.-thick Fe3N\mathrm{Fe}_3\mathrm{N} film is ∼440\sim440 K and reduces to ∼385\sim385 K for a 2-u.c.-thick Fe3N\mathrm{Fe}_3\mathrm{N} film. Accompany to the reduction of TCT_\mathrm{C}, MSM_\mathrm{S} of Fe3N\mathrm{Fe}_3\mathrm{N} films reduces dramatically on decreasing the thickness below 10 u. c. (Figure 2c). Surprisingly, we find that MSM_\mathrm{S} of a 2-u.c.-thick Fe3N\mathrm{Fe}_3\mathrm{N} film is ∼150\sim150 emu/cm3^3. In fact, this saturation moment at sub-nanometer thickness is much larger than those of most correlated magnetic oxide and nitride films. For the transport behavior of Fe3N\mathrm{Fe}_3\mathrm{N} films, we obverse a clear metal-to-insulator transition as decreasing film thickness. For a 30-u.c.-thick Fe3N\mathrm{Fe}_3\mathrm{N} single film, a metallic phase maintains at all temperatures.

Thickness dependent magnetic and transport properties of Fe$_3$N single films

Figure 2. Thickness dependent magnetic and transport properties of Fe3_3N single films. (a) and (b) Temperature-dependent magnetization and resistivity of 6-u.c.- and 30-u.c.-thick Fe3_3N films, respectively. (c) and (d) Field-dependent magnetization of 6-u.c.- and 30-u.c.-thick Fe3_3N films when magnetic field is applied along in-plane (H//abH//ab) and out-of-plane (H//cH//c) direction, respectively. (e) Curie temperature (TcT_\mathrm{c}), (f) room-temperature saturation magnetization (MsM_\mathrm{s}), and (g) resistivity (ρ\rho) as a function of Fe3_3N film thickness. (h) and (i) MOKE images for a 30-u.c.-thick Fe3_3N film with magnetic fields applied along the in-plane and out-of-plane direction at room temperature, respectively. The dark contrast represents the magnetization along the yy (or zz) axis, and light contrast represents the magnetization along the −y-y (or −z-z) axis when the magnetic field is applied along the in-plane (or out-of-plane) direction.

Please note that ρ300K\rho_{300\mathrm{K}} of a 30-u.c.-thick Fe3N\mathrm{Fe}_3\mathrm{N} is only 9.5 μΩ⋅\mu\Omega\cdotcm, which is comparable to those of most noble metals, for instance Pt (ρ300K=10.6\rho_{300\mathrm{K}} = 10.6 μΩ⋅\mu\Omega\cdotcm) and Au (ρ300K=2.2\rho_{300\mathrm{K}} = 2.2 μΩ⋅\mu\Omega\cdotcm).[41, 42]

However, the Fe3N\mathrm{Fe}_3\mathrm{N} films transit into an insulator when the thickness falls below 10 u. c. The low-temperature transport property of a 6-u.c.-thick Fe3N\mathrm{Fe}_3\mathrm{N} film can be described using variable-range hopping (VRH) conduction mechanism with involving electron-electron interaction.[43] This is a typical electrical phase transition associated with a thickness-reduction induced dimensional confinement. For an ultrathin Fe3N\mathrm{Fe}_3\mathrm{N} film, the free electrons are strongly localized; thus, the carrier density is significantly reduced, resulting in a sharp increase of ρ\rho by four orders of magnitude at low temperatures.

The magnetic easy-axis of Fe3N\mathrm{Fe}_3\mathrm{N} films aligns in the film-plane, similar to most of strongly correlated thin films. The coercive field (HCH_{\mathrm{C}}) increases on the increment of film thickness (Figure 2c). Figure 2d shows the magnetic hysteresis loops of 6- and 30-u.c.-thick Fe3N\mathrm{Fe}_3\mathrm{N} films when H//cH \mathbin{//} c. We observe a consistent anomaly in all MM-HH loops of Fe3N\mathrm{Fe}_3\mathrm{N} films with different film thickness. As sweeping magnetic fields from positive to negative values, the moment firstly reduces linearly and then increases abnormally at ∼0.2\sim0.2 T. As further reducing magnetic field, the moment decreases monotonically. This behavior has seldomly been observed in other magnetic TMN thin films. To ensure the consistency, we record this anomaly in the MM-HH loops of a 30-u.c.-thick Fe3N\mathrm{Fe}_3\mathrm{N} film as a function of temperature (Figure S3). The maximum moment at ∼0.1\sim0.1–0.20.2 T as well as the coercive field continuously decreases as increasing temperature. We performed the MOKE measurements on a 30-u.c.-thick Fe3N\mathrm{Fe}_3\mathrm{N} film. Figure 2h and Figure 2i show two typical field-dependent evolutions of magnetic domain patterns captured by MOKE when H//abH \mathbin{//} ab and H//cH \mathbin{//} c, respectively. The white areas represent the magnetic domains, with a negative magnetization (M<0M < 0) created by the application of a negative field to positively saturated films with M>0M > 0 (black areas). The density of effective nucleation sites in our films are relatively low, indicating a rather high homogeneity of samples. Please note that the switching field along the in-plane direction is an order of magnitude smaller than that along the out-of-plane direction. Therefore, we hypothesize that the anomaly in MM-HH loops (H//cH \mathbin{//} c) is attributed to the reorientation of Fe spins from in-plane to out-of-plane through a metastable state, where the partial magnetic domains align in the film plane during field-switching. The magnetoresistance (MR) of 6-u.c.- and 30-u.c.-thick Fe3N\mathrm{Fe}_3\mathrm{N} films were measured as a function of temperature and magnetic field (Figures S4–S6). MR of both samples exhibit the butterfly hysteresis loops at small fields which are coupled with HCH_C as comparatively shown in Figure 2c and Figure 2d.

Comparing MR at high fields indicates that both Fe3N\mathrm{Fe}_3\mathrm{N} films have negative linear responses that increase systematically in magnitude with decreasing temperature. Interestingly, we observe a strong in-plane anisotropy in MR strongly depending on the current direction when H∥cH \parallel c. For a 30-u.c.-thick Fe3N\mathrm{Fe}_3\mathrm{N} film, the MR(I∥aI \parallel a) is opposite to MR(I∥bI \parallel b). However, MR trends for both current directions are similar when the thickness of Fe3N\mathrm{Fe}_3\mathrm{N} films reduces to 6 u.c. We believe that the interesting magnetotransport behaviors are caused by the anisotropic spin alignments which are confined by its lattice structure. These results are consistent with the typical results for ferromagnets that possess strong in-plane anisotropy.

Furthermore, we investigated the magnetic exchange coupling at the interfaces between ferromagnetic Fe3N\mathrm{Fe}_3\mathrm{N} and antiferromagnetic CrN\mathrm{CrN} layers. Figure 3a shows a HAADF-STEM image of a Fe3N/CrN\mathrm{Fe}_3\mathrm{N}/\mathrm{CrN} bilayer. The bright layer indicates the Fe3N\mathrm{Fe}_3\mathrm{N} layer, while the dark layer is the CrN\mathrm{CrN} layer, because the scattering intensity of HAADF-STEM image is approximately proportional to the square of the atomic number and meanwhile the stacking density is higher in Fe3N\mathrm{Fe}_3\mathrm{N} layer. This result reveals that both layers are flat and continuous over long lateral distances, suggesting the formation of high-quality interfaces. High-magnification image around Fe3N/CrN\mathrm{Fe}_3\mathrm{N}/\mathrm{CrN} interface (Figure 3b) and compositional EELS maps (Figure 3c-Figure 3f) obtained from the analysis of the Fe L3,2L_{3,2}-, Cr L3,2L_{3,2}-, N KK-, and O KK-edges signals reveal both layers that are epitaxially grown and chemically uniformed, as well as the interfaces are atomically sharp and contains negligible chemical intermixing.

Chemical and magnetization depth profiles across CrN/Fe3N interface

Figure 3. Chemical and magnetization depth profiles across CrN/Fe3_3N interface. (a) Low-magnified STEM image of a CrN/Fe3_3N bilayer grown on Al2_2O3_3 substrates. (b) A high-magnified STEM image across CrN/Fe3_3N/Al2_2O3_3 interfaces marked with a yellow dashed square in (a). (c)–(f) Spatial resolved EELS maps were taken at the Fe LL-, Cr LL-, N KK-, and O KK-edges, respectively. The EELS results clearly indicate the uniformed chemical distribution and atomically sharp interfaces with a minimum chemical intermixing. (g) Neutron reflectivities of a CrN/Fe3_3N bilayer as a function of wave factor (qq). The open symbols (or lines) represent the reflectivities of experiment data (or best fits). (h) Calculated spin asymmetry (SA) from (R+−R−)/(R++R−)(R^{+}-R^{-})/(R^{+}+R^{-}). Open symbols and solid line are experimental data and best fit, respectively. (i) and (j) Nuclear scattering length density (nSLD) and magnetization depth profiles, respectively. Inset of (j) shows the zoom-in magnetization depth profile across the interface between CrN and Fe3_3N.

The chemical and magnetization distributions across entire sample were firstly examined using polarized neutron reflection (PNR) technique. The measurements were conducted at 10 K after field-cooling at 1 T from room temperature. The specular neutron reflectivities are plotted in Figure 3g as a function of wave factor (q=4πsin⁡θi/λq = 4\pi\sin\theta_i/\lambda) for the spin-up (R+R^{+}) and spin-down (R−R^{-}) polarized neutrons, where θi\theta_i is the incident angle and λ\lambda is the wavelength of incident neutrons. The solid lines are the best fits to the experimental data (open symbols). The figure of merit (FOM) of PNR fit yields a value of 1.89. Figure 3h shows the calculated spin asymmetry (SA) and its corresponding fit, from which the chemical (Figure 3i) and magnetization (Figure 3j) depth profiles can be obtained. The atomic density of Fe3N\mathrm{Fe}_3\mathrm{N} layer is larger than that of CrN\mathrm{CrN} layer. We find that the CrN\mathrm{CrN} layer separates into two parts: an interface layer and a top layer. The density of CrN\mathrm{CrN} interface layer is slightly smaller than its bulk value. This fact is possibly due to the strain compensation between structural dissimilar materials. The magnetic depth profile indicates the Fe3N\mathrm{Fe}_3\mathrm{N} layer exhibits a large magnetization (∼1000\sim1000 emu/cm3\mathrm{emu}/\mathrm{cm}^3) and deteriorates slightly when it is close to the CrN\mathrm{CrN} layer. We also notice that the CrN\mathrm{CrN} interface layer shows a small net moment of ∼54\sim54 emu/cm3\mathrm{emu}/\mathrm{cm}^3 after field cooling. The existence of non-zero moment in the CrN\mathrm{CrN} interface layer is robust because the PNR fits with constraint of zero or negative MM in CrN\mathrm{CrN} interface layer have a large deviation from the experiment data, yielding FOM of 4.3 and 5.6, respectively. The field-cooled PNR data suggest that the CrN\mathrm{CrN} interface layer is magnetized due to the spins of Cr ions are pinned to those of Fe ions during the field cooling.[44, 45] The magnetization integrated over the entire depth profile obtained from PNR is in good quantitative agreement with the magnetometry data.

The unique transport properties were measured across the Fe3N/CrN\mathrm{Fe}_3\mathrm{N}/\mathrm{CrN} interfaces from [(CrN)n/(Fe3N)n]5[(\mathrm{CrN})_n/(\mathrm{Fe}_3\mathrm{N})_n]_5 (Cn/FnC_n/F_n) superlattices, where nn represents the number of unit cell of Fe3N\mathrm{Fe}_3\mathrm{N} and CrN\mathrm{CrN} layer, and five is the stacking periodicity of superlattices. Prior to the transport measurements, we performed the room-temperature PNR measurements on two representative C5/F5C_5/F_5 and C10/F10C_{10}/F_{10} superlattices (Figures S7 and S8). These results demonstrate the uniformities of chemical and magnetization distributions within Fe3NFe_{3}N layers. The averaged saturation magnetization of Fe3NFe_{3}N layers in C5/F5C_{5}/F_{5} is nearly identical to those of Fe3NFe_{3}N layers in C10/F10C_{10}/F_{10}. MR of Cn/FnC_{n}/F_{n} superlattices are recorded by applying currents along aa and bb direction at various temperatures. Figure 4a-Figure 4f shows MRs at 10 K when H∥cH \parallel c. We notice that MR does not show significant difference as a function of applied field when nn is below 5 u. c. However, when nn is beyond 5 u. c., the degeneracy of MR between two current directions appears. In Figure 4g and Figure 4h, we show the contour plots of MR when I∥aI \parallel a and I∥bI \parallel b as a function of layer thickness and temperature. At low temperatures, the MR transits from negative to positive values at a critical thickness (tt) and tt reduces as further increasing the temperature. The strong temperature dependency in MR become subtle for thick layers. Furthermore, we also measured the Hall resistance (ρxy\rho_{xy}) of Cn/FnC_{n}/F_{n} superlattices when H∥cH \parallel c in order to probe the intriguing magnetic properties across the interfaces. We subtracted the ordinary Hall resistance (R0HR_{0}H) from ρxy\rho_{xy} to separate the anomalous Hall effect (AHE) from Hall resistance. Figure 4i-Figure 4n show the field dependent (ρxy−R0H\rho_{xy}-R_{0}H) from Cn/FnC_{n}/F_{n} superlattices at 10 K. A saturation (ρxy−R0H\rho_{xy}-R_{0}H) appears for each Cn/FnC_{n}/F_{n} superlattice above a critical field. For n=2n = 2–44, the square-like open hysteresis loops are observed, but the value of (ρxy−R0H\rho_{xy}-R_{0}H) is negative. When nn is above 5, we observe a sign reversal from negative to positive in (ρxy−R0H\rho_{xy}-R_{0}H) at 3 T. As further increasing nn, (ρxy−R0H\rho_{xy}-R_{0}H) increases approximately linearly. Since the saturation magnetizations are almost identical in Cn/FnC_{n}/F_{n} (n>5n > 5) superlattices, we attribute that the thickness-driven AHE signal reversal possibly originates from the band topology (e. g. the number of crossing points) and is associated with kk-space Berry curvature.[46] However, we do not observe the typical hump-like topological Hall signals that exist in other ferromagnetic metallic systems.[47, 48] Figure 4o shows the (ρxy−R0H\rho_{xy}-R_{0}H) reduces towards zero as gradually increasing temperature for all Cn/FnC_{n}/F_{n} superlattices. Temperaturedriven AHE reduction can be understood by the slight Fermi level shift with respect to the avoided band crossing points. It is worth noting that the present spatial magnetic measurements could not detect a submicrometer-scale magnetic domains (e. g. chiral magnetic bubble-like or skyrmions) in Fe3_3N single films or Cn_n/Fn_n superlattices across the critical thickness. Further measurements to identify the nanoscale magnetic domains and possible existing room-temperature skyrmions in such systems are needed using either magnetic force microscopy (MFM) [48, 49] or Lorentz transmission electron microscopy (L-TEM).[50]

Electrical transport across the interfaces

Figure 4. Electrical transport across the [(CrN)n/(Fe3N)n][(\mathrm{CrN})_n/(\mathrm{Fe}_3\mathrm{N})_n] (CnFn\mathrm{C}_n\mathrm{F}_n) interfaces, where nn represents the number of unit cells in the individual layer. (a)–(f) Magnetoresistance (MR) of CnFn\mathrm{C}_n\mathrm{F}_n superlattices as a function of magnetic field at 10 K. The magnetic fields were applied perpendicular to the film plane. The currents were applied in parallel to aa (solid symbols) and bb (open symbols) orientations. (g) and (h) MR as a function of temperature and unit cell numbers when the current was applied in parallel to aa and bb orientation, respectively. (i)–(n) Anomalous Hall resistance (ρxy\rho_{xy}-R0HR_0H) of CnFn\mathrm{C}_n\mathrm{F}_n superlattices as a function of magnetic field at 10 K. (o) ρxy\rho_{xy}-R0HR_0H as function of temperature and unit cell numbers. For the Hall measurements, the magnetic field was applied along the surface plane.

Besides the intriguing thickness-sensitive magnetotransport behaviors towards the spintronic applications, we further demonstrate that the exchange coupling across the Fe3_3N/CrN interface is highly tunable to the mechanical bending stress. We fabricated the Fe3_3N/CrN freestanding membranes using water-soluble single-crystalline sodium chloride substrates. The Fe3_3N/CrN membranes attach firmly to the sapphire cylinders with pre-determined curvatures ranging from 0 to 0.25 mm−1^{-1}. The variations of bending curvature led to the successful tuning of lattice deformation.[51, 52, 53] We can deliver a roughly linear relationship between the bending stress and the cylinder curvature (RR). The membranes support on cylinders with larger RR will suffer a larger lattice deformation. Figure 5a shows MM-HH loops of an as-grown Fe3_3N/CrN membrane with R=0R = 0 at 10 K. The magnetic hysteresis exhibits open loops with its center shifted to negative (positive) fields by an exchange bias field (HEBH_{\mathrm{EB}}) of ~ 115 Oe after 3 T (−3 T) field cooling from room temperature. This behavior suggests the presence of exchange coupling in the antiferromagnetic/ferromagnetic systems. As increasing RR from 0 to 0.25 mm−1^{-1}, HEBH_{\mathrm{EB}} increases from 115 to 350 Oe, whereas the magnitude of MSM_{\mathrm{S}} reduces dramatically from 950 to 280 emu/cm2^2 (Figure 5b-Figure 5d). The ratio between the bending curvatures and MSM_{\mathrm{S}} is approximately 2680 emu/cm3^3 per mm−1^{-1}, demonstrating a significant advantage of applying such system for detection micro-deformation. Figure 5e and Figure 5f summarize the curvature and temperature dependent HEBH_{\mathrm{EB}} and MSM_{\mathrm{S}}, respectively. We find that HEBH_{\mathrm{EB}} reduces with increasing temperature and reaches zero value at the blocking temperature (TBT_{\mathrm{B}}) ~ 150 K (Figure S9), which is consistent with the TNT_{\mathrm{N}} of antiferromagnetic CrN layers.[32, 33, 34, 35] The transition temperature of HEBH_{\mathrm{EB}} shifts to high temperature as increasing RR. This strategy provides a convenient and continuous way to tune the magnetic properties of freestanding membranes. The advantage of this cylinder diameter engineering strategy lies in the uniform uniaxial lattice deformation of quasi-2D crystals and is readily applicable to tune other intriguing physical properties.

Tunable magnetic states at the CrN/Fe$_3$N interfaces under bending stress

Figure 5. Tunable magnetic states at the CrN/Fe3_3N interfaces under bending stress. (a) Exchange bias at the CrN/Fe3_3N interface at 10 K. The red and blue curves are magnetic hysteresis loops after 3 and −3-3 T, respectively. (b)–(d) Room-temperature in-plane MM–HH loops when a freestanding CrN/Fe3_3N bilayer was bended with a curvature of 0, 0.1, and 0.25 mm−1^{-1}, respectively. (e) Exchange bias field (HEBH_{\mathrm{EB}}) and (f) saturation magnetization (MSM_{\mathrm{S}}) as a function of temperature and bending curvature.

In summary, we fabricated the high-crystalline and stoichiometric Fe3_3N single films and heterostructures using plasma-assisted PLD technique. The intrinsic magnetic and electronic phase transitions at a critical thickness of ~ 5 u. c. were determined upon the reduced dimensionality. The anomaly in the out-of-plane magnetic hysteresis loop is attributed to the reorientation of magnetic domains during field sweeping. Furthermore, we investigated the evolution of magnetoresistance and AHE depending on the film thickness. The degeneracy in the in-plane magnetic responses and AHE signal reversal appears as gradually increasing layer thickness. We attribute such behaviors to the band topology that is strongly associated with kk-space Berry curvature, a typical character for ferromagnets with chiral spin texture. Finally, a sizable in-plane exchange bias field of an AFM/FM heterointerface changes sign after field cooling to below the Néel temperature of CrN. We demonstrate that the magnetic property of such functional interface is highly tunable by modifying the diameter of supporting sapphire cylinder in a large range. To this end, our work on manipulation of physical properties of high-quality nitride single films and all nitride heterostructures can be extended to various similar systems. The application of rare-earth-element-free nitrides with emergent magnetic properties will stimulate combination with other low-dimensional nanomaterials.

Materials and Methods

Fabrication of high-quality samples

The Fe3N\mathrm{Fe}_{3}\mathrm{N} thin films were fabricated by pulsed laser deposition (PLD) assisted by radio-frequency (RF) plasma source supplying highly active nitrogen atoms. A stoichiometric ceramic Fe3N\mathrm{Fe}_{3}\mathrm{N} target was synthesized using a high-pressure reaction route from a mixed FeCl3\mathrm{FeCl}_{3} and NaNH2\mathrm{NaNH}_{2} powder. The high-quality target fabrication was conducted at the High-Pressure Lab of South University of Science and Technology (SUSTech). This technique was used in our previous work and the details of fabrication process for the nitride bulk ceramics or single-crystals were described in previous works. The Fe3N\mathrm{Fe}_{3}\mathrm{N} thin films were deposited at an optimized condition that is the substrate temperature of 400 ∘C400\,^{\circ}\mathrm{C}, laser density of ∼1 J/cm2\sim1\,\mathrm{J}/\mathrm{cm}^{2}, and base pressure of 1×10−81\times10^{-8} Torr. The samples were cooled down to room-temperature under the irradiation of nitrogen plasma in order to compensate the nitrogen vacancies. The CrN/Fe3N\mathrm{CrN}/\mathrm{Fe}_{3}\mathrm{N} bilayer and superlattices were fabricated under the same experimental conditions. The layer thickness was carefully controlled by counting the number of laser pulses and further confirmed by X-ray reflectivity measurements. The number of bilayer repeats keeps the same for all superlattices in order to maintain the identical number of interfaces.

Manipulation of bending curvatures of Fe₃N/CrN freestanding membranes using cylinder diameter engineering (CDE)

The Fe3N/CrN\mathrm{Fe}_{3}\mathrm{N}/\mathrm{CrN} bilayers were fabricated on the single-crystalline sodium chloride substrates under the same conditions. After the growth, the Fe3N/CrN\mathrm{Fe}_{3}\mathrm{N}/\mathrm{CrN} bilayers were immersed into the de-ionized water to dissolve the sodium chloride substrates. Then, the bilayers float on the water surface. We used the sapphire cylinders with different curvatures (00, 0.10.1, and 0.25 mm−10.25\,\mathrm{mm}^{-1}) to scoop up the Fe3N/CrN\mathrm{Fe}_{3}\mathrm{N}/\mathrm{CrN} freestanding membranes. Thus, the membranes attach to the sticks firmly. The samples were hot dried in the oven at 100 ∘C100\,^{\circ}\mathrm{C} for 2 hours. The membranes suffer the bending stress from sapphire cylinders with different curvatures. This leads to the lattice deformation and successful tuning of magnetic properties of membranes.

Physical properties characterizations

The crystallinity of samples was checked by in-house high-resolution four-circle X-ray diffractometer (XRD) using a Cu Kα1\alpha_{1} source (Panalytical MRD X’Pert 3). The microstructures of a Fe3_3N single layer and a Fe3_3N/CrN bilayer were examined using JEM ARM 200CF electron microscopy at the Institute of Physics, Chinese Academy of Sciences. We performed elementalspecific EELS mapping at the Fe LL-, Cr LL-, N KK-, and O KK-edges from the interested regions after background subtracting. The magnetic properties of samples were characterized by a SQUID equipped with a high-temperature unit. Both in-plane and out-of-plane magnetization were obtained ranging from 10 to 500 K. The exchange bias was recorded at low temperatures after the sample was field-cooled down to 10 K under magnetic fields of ±3\pm3 T. The transport properties were performed using standard van der Pauw geometry with wire-bonding technique. The measurements were conducted using a 9T-PPMS. The ac current was kept at a minimum requirement of 1 μ\muA to avoid the joule heating. XPS measurements were performed at the Institute of Physics, Chinese Academy of Sciences. Spectra were collected at both Fe 2p2p and N 1s1s core-level peaks at room-temperature.

Room-temperature Magneto-optical Kerr effect (MOKE) measurements

The MOKE measurements were performed using a commercial MOKE microscope from Evico Magnetics. The evolution of the magnetic domain structures was imaged and recorded using a quasi-static technique. The images were taken simultaneously by sweeping magnetic fields. Both in-plane and out-of-plane fields were applied during the imaging.

Polarized Neutron Reflectivity (PNR) measurements

The PNR experiments on the Fe3_3N/CrN superlattices were performed at the BL-4A of Spallation Neutron Source, Oak Ridge National Laboratory. An in-plane magnetic field of 0.5 T was applied during the measurements. The two superlattices were measured simultaneously at room temperature to avoid any arbitrary effects. The PNR measurements on a Fe3_3N/CrN bilayer were conducted at the Multipurpose Reflectometer at the Chinese Spallation Neutron Source. In this experiment, an in-plane magnetic field of 1 T was applied during the sample cooling. The measurements were conducted at the same magnetic field at 10 K. In both PNR measurements, the specular reflectivities were recorded as a function of the wave factor transfer along the film surface normal. R+R^{+} and R−R^{-} reflect the specular reflectivities from spin-up and spin-down polarized neutrons, respectively. The nuclear and magnetic scattering length densities (SLD) were obtained simultaneously by fitting the PNR data using GenX software.

Supporting Information

Supporting Information is available from the Wiley Online Library or from the author.

Acknowledgements

This work was supported by the National Key Basic Research Program of China (Grant Nos. 2020YFA0309100 and 2019YFA0308500), the National Natural Science Foundation of China (Grant Nos. 11974390, 11721404, 11874412, and 12174437), the Beijing Nova Program of Science and Technology (Grant No. Z191100001119112), the Beijing Natural Science Foundation (Grant No. 2202060), the Guangdong-Hong Kong-Macao Joint Laboratory for Neutron Scattering Science and Technology, and the Strategic Priority Research Program (B) of the Chinese Academy of Sciences (Grant No. XDB33030200). The PNR experiments on a CrN/Fe3N\mathrm{CrN}/\mathrm{Fe}_{3}\mathrm{N} bilayer were conducted at Multiple purpose Reflectometry (MR) at the Chinese Spallation Neutron Source (CSNS) and the PNR experiments on the CrN/Fe3N\mathrm{CrN}/\mathrm{Fe}_{3}\mathrm{N} superlattices were conducted via a user proposal at Magnetism Reflectometer (BL-4A) at the Spallation Neutron Source (SNS), a DOE Office of Science User Facility operated by Oak Ridge National Laboratory (ORNL).

Figures and figure captions

References

  1. [1]O. Gutfleisch, M. A. Willard, E. Bruck, C. H. Chen, S. G. Sankar, J. P. Liu, Advanced Materials 2011, 23, 821.
  2. [2]B. Saha, A. Shakouri, T. D. Sands, Applied Physics Reviews 2018, 5, 021101.
  3. [3]T. Mikolajick, S. Slesazeck, H. Mulaosmanovic, M. H. Park, S. Fichtner, P. D. Lomenzo, M. Hoffmann, U. Schroeder, Journal of Applied Physics 2021, 129, 100901.
  4. [4]C. Rong, Y. Zhang, N. Poudyal, X. Xiong, M. J. Kramer, J. P. Liu, Applied Physics Letters 2010, 96, 102513.
  5. [5]S. A. Wolf, D. D. Awschalom, R. A. Buhrman, J. M. Daughton, S. von Molnar, M. L. Roukes, A. Y. Chtchelkanova, D. M. Treger, Science 2001, 294, 1488.
  6. [6]R. S. Ningthoujam, N. S. Gajbhiye, Progress in Materials Science 2015, 70, 50.
  7. [7]R. Kumar, S. Nayak, M. Garbrecht, V. Bhatia, A. Indiradevi Kamalasanan Pillai, M. Gupta, S. M. Shivaprasad, B. Saha, Journal of Applied Physics 2021, 129, 055305.
  8. [8]G. Serghiou, G. Ji, N. Odling, H. J. Reichmann, D. J. Frost, J. P. Wright, High Pressure Res 2015, 35, 28.
  9. [9]A. Fuertes, APL Materials 2020, 8, 020903.
  10. [10]C.-C. Chiang, V. Ostwal, P. Wu, C.-S. Pang, F. Zhang, Z. Chen, J. Appenzeller, Applied Physics Reviews 2021, 8, 021306.
  11. [11]B. Anasori, M. R. Lukatskaya, Y. Gogotsi, Nature Reviews Materials 2017, 2, 16098.
  12. [12]F. I. Ajami, R. K. Maccrone, Journal of Physics and Chemistry of Solids 1975, 36, 7.
  13. [13]Y. Zhang, N. Haberkorn, F. Ronning, H. Wang, N. A. Mara, M. Zhuo, L. Chen, J. H. Lee, K. J. Blackmore, E. Bauer, A. K. Burrell, T. M. McCleskey, M. E. Hawley, R. K. Schulze, L. Civale, T. Tajima, Q. Jia, Journal of the American Chemical Society 2011, 133, 20735.
  14. [14]P. Wang, D. Wang, N. M. Vu, T. Chiang, J. T. Heron, Z. Mi, Applied Physics Letters 2021, 118, 223504.
  15. [15]S. Yasuoka, T. Shimizu, A. Tateyama, M. Uehara, H. Yamada, M. Akiyama, Y. Hiranaga, Y. Cho, H. Funakubo, Journal of Applied Physics 2020, 128, 114103.
  16. [16]S. Fichtner, N. Wolff, F. Lofink, L. Kienle, B. Wagner, Journal of Applied Physics 2019, 125, 114103.
  17. [17]Seema, D. Kumar, U. P. Deshpande, M. Gupta, Journal of Applied Physics 2021, 130, 125106.
  18. [18]A.-M. Zieschang, J. D. Bocarsly, M. Dürrschnabel, H.-J. Kleebe, R. Seshadri, B. Albert, Chemistry of Materials 2018, 30, 1610.
  19. [19]T. K. Kim, M. Takahashi, Applied Physics Letters 1972, 20, 492.
  20. [20]T. Waki, S. Terazawa, Y. Tabata, K. Sato, A. Kondo, K. Kindo, H. Nakamura, Physical Review B 2014, 90, 014416.
  21. [21]N. Ji, L. F. Allard, E. Lara-Curzio, J.-P. Wang, Applied Physics Letters 2011, 98, 092506.
  22. [22]P. Wojciechowski, M. Lewandowski, Crystal Growth & Design 2022, 22, 4618.
  23. [23]K. Yamaguchi, T. Yui, K. Yamaki, I. Kakeya, K. Kadowaki, T. Suemasu, Journal of Crystal Growth 2007, 301, 597.
  24. [24]L.-Y. Yuan, L. Ma, W. He, H.-Y. Wu, Y.-B. Sun, C. Wen, G.-K. Li, C.-M. Zhen, J.-J. Shen, J.-J. Zhao, Y. Lu, D.-L. Hou, Journal of Alloys and Compounds 2019, 789, 730.
  25. [25]H. Fang, R. Zhang, B. Liu, Z. Tao, X. Wang, Z. Xie, X. Xiu, Y. Zheng, Journal of Physics D: Applied Physics 2012, 45, 315002.
  26. [26]H. Fang, J. Chen, X. Peng, Y. Li, Z. Tao, Materials Letters 2018, 233, 191.
  27. [27]Y. H. Cheng, R. K. Zheng, H. Liu, Y. Tian, Z. Q. Li, Physical Review B 2009, 80, 174412.
  28. [28]A.-M. Zieschang, J. D. Bocarsly, M. Dürrschnabel, L. Molina-Luna, H.-J. Kleebe, R. Seshadri, B. Albert, Chemistry of Materials 2017, 29, 621.
  29. [29]S. Leone, J. Ligl, C. Manz, L. Kirste, T. Fuchs, H. Menner, M. Prescher, J. Wiegert, A. Žukauskaitė, R. Quay, O. Ambacher, Physica Status Solidi (RRL) – Rapid Research Letters 2019, 14, 1900535.
  30. [30]Y. H. Liu, K. Wang, W. Lin, A. Chinchore, M. Shi, J. Pak, A. R. Smith, C. Constantin, Thin Solid Films 2011, 520, 90.
  31. [31]A. Garzon-Fontecha, H. A. Castillo, E. Restrepo-Parra, W. De La Cruz, Surface and Coatings Technology 2018, 334, 98.
  32. [32]Q. Jin, H. Cheng, Z. Wang, Q. Zhang, S. Lin, M. A. Roldan, J. Zhao, J. O. Wang, S. Chen, M. He, C. Ge, C. Wang, H. B. Lu, H. Guo, L. Gu, X. Tong, T. Zhu, S. Wang, H. Yang, K. J. Jin, E. J. Guo, Advanced Materials 2021, 33, 2005920.
  33. [33]Q. Jin, Z. Wang, Q. Zhang, Y. Yu, S. Lin, S. Chen, M. Qi, H. Bai, A. Huon, Q. Li, L. Wang, X. Yin, C. S. Tang, A. T. S. Wee, F. Meng, J. Zhao, J.-o. Wang, H. Guo, C. Ge, C. Wang, W. Yan, T. Zhu, L. Gu, S. A. Chambers, S. Das, T. Charlton, M. R. Fitzsimmons, G.-Q. Liu, S. Wang, K.-j. Jin, H. Yang, E.-J. Guo, Physical Review Letters 2022, 128, 017202.
  34. [34]Q. Jin, Z. Wang, Q. Zhang, J. Zhao, H. Cheng, S. Lin, S. Chen, S. Chen, H. Guo, M. He, C. Ge, C. Wang, J.-O. Wang, L. Gu, S. Wang, H. Yang, K.-j. Jin, E.-J. Guo, Physical Review Materials 2021, 5, 023604.
  35. [35]Q. Jin, J. Zhao, M. A. Roldan, W. Qi, S. Lin, S. Chen, H. Hong, Y. Fan, D. Rong, H. Guo, C. Ge, C. Wang, J.-O. Wang, S. Wang, K.-j. Jin, E.-J. Guo, Applied Physics Letters 2022, 120, 073103.
  36. [36]A. Filippetti, N. A. Hill, Physical Review Letters 2000, 85, 5166.
  37. [37]C. X. Quintela, J. P. Podkaminer, M. N. Luckyанова, T. R. Paudel, E. L. Thies, D. A. Hillsberry, D. A. Tenne, E. Y. Tsymbal, G. Chen, C. B. Eom, F. Rivadulla, Advanced Materials 2015, 27, 3032.
  38. [38]A. Leineweber, H. Jacobs, F. Huning, H. Lueken, H. Schilder, W. Kockelmann, Journal of Alloys and Compounds 1999, 288, 79.
  39. [39]S. Matar, B. Siberchicot, M. Penicaud, G. Demazeau, Journal De Physique I 1992, 2, 1819.
  40. [40]E. J. Miola, S. D. de Souza, P. A. P. Nascente, M. Olzon-Dionysio, C. A. Olivieri, D. Spinelli, Applied Surface Science 1999, 144, 272.
  41. [41]J. W. Arblaster, Johnson Matthey Technology Review 2015, 59, 174.
  42. [42]Seitz, Frederick. The Modern Theory of Solids. New York: Dover Publications, 1987: 10.
  43. [43]X. Y. Zhang, J. S. Chawla, B. M. Howe, D. Gall, Physical Review B 2011, 83, 165205.
  44. [44]C. Leighton, J. Nogues, H. Suhl, I. K. Schuller, Physical Review B 1999, 60, 12837.
  45. [45]M. R. Fitzsimmons, C. Dufour, K. Dumesnil, J. Dou, M. Pechan, Physical Review B 2009, 79, 144425.
  46. [46]J. Matsuno, N. Ogawa, K. Yasuda, F. Kagawa, W. Koshibae, N. Nagaosa, Y. Tokura, M. Kawasaki, Science Advances 2016, 2, e1600304.
  47. [47]H. Tsai, T. Higo, K. Kondou, T. Nomoto, A. Sakai, A. Kobayashi, T. Nakano, K. Yakushiji, R. Arita, S. Miwa, Y. Otani, S. Nakatsuji, Nature 2020, 580, 608.
  48. [48]L. Wang, Q. Feng, Y. Kim, R. Kim, K. H. Lee, S. D. Pollard, Y. J. Shin, H. Zhou, W. Peng, D. Lee, W. Meng, H. Yang, J. H. Han, M. Kim, Q. Lu, T. W. Noh, Nature Materials 2018, 17, 1087.
  49. [49]K. Y. Meng, A. S. Ahmed, M. Bacani, A. O. Mandru, X. Zhao, N. Bagues, B. D. Esser, J. Flores, D. W. McComb, H. J. Hug, F. Yang, Nano Letters 2019, 19, 3169.
  50. [50]J. Tang, L. Kong, W. Wang, H. Du, M. Tian, Chinese Physics B 2019, 28, 087503.
  51. [51]H. Zhu, Y. Wang, J. Xiao, M. Liu, S. Xiong, Z. J. Wong, Z. Ye, Y. Ye, X. Yin, X. Zhang, Nature Nanotechnology 2015, 10, 151.
  52. [52]M. Zeng, J. Liu, L. Zhou, R. G. Mendes, Y. Dong, M. Y. Zhang, Z. H. Cui, Z. Cai, Z. Zhang, D. Zhu, T. Yang, X. Li, J. Wang, L. Zhao, G. Chen, H. Jiang, M. H. Rummeli, H. Zhou, L. Fu, Nature Materials 2020, 19, 528.
  53. [53][53]H. Yao, K. Jin, Z. Yang, Q. Zhang, W. Ren, S. Xu, M. Yang, L. Gu, E. J. Guo, C. Ge, C. Wang, X. Xu, D. Zhang, G. Yang, Advanced Materials Interfaces 2021, 8, 2101499.

Paper details

vlnc:W_vgdcn9xw
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents