betaFeedback

WorksPhysics and Astronomy

Robust field-free switching using large unconventional spin-orbit torque in an all-van der Waals heterostructure

Abstract

The emerging all-van der Waals (vdW) magnetic heterostructure provides a new platform to control the magnetization by the electric field beyond the traditional spintronics devices. One promising strategy is using unconventional spin-orbit torque (SOT) exerted by the out-of-plane polarized spin current to enable deterministic magnetization switching and enhance the switching efficiency. However, in all-vdW heterostructures, large unconventional SOT remains elusive and the robustness of the field-free switching against external magnetic field hasn't been examined, which hinder further applications. Here we demonstrate the field-free switching in an all-vdW heterostructure combining a type-II Weyl semimetal TaIrTe4 and above-room-temperature ferromagnet Fe3GaTe2. The fully field-free switching can be achieved at 2.56 x 10^10 A per m2 at 300K and a large SOT effective field efficiency of the out-of-plane polarized spin current generated by TaIrTe4 is determined to be 0.37. Moreover, we find that the switching polarity cannot be changed until the external in-plane magnetic field reaches 252mT, indicating a robust switching against the magnetic field. The numerical simulation suggests the large unconventional SOT reduces the switching current density and enhances the robustness of the switching. Our work shows that all-vdW heterostructures are promising candidates for future highly efficient and stable SOT-based devices.

Introduction

Since the discovery of long-range ferromagnetic order in two-dimensional (2D) materials [1, 2, 3], multiple methods have been used to control the magnetization by the electric field [3, 4, 5, 6, 7, 8]. Among those methods, using the spin current generated by one layer to exert spin-orbit torque (SOT) on the adjacent ferromagnetic layer can effectively switch the magnetization [9, 10]. Recently developed all-van der Waals (vdW) heterostructures provide new platforms to explore the advanced application[11, 12], and some advantages have been shown in all-vdW devices. In addition to the atomically flat interface[13, 14, 15], some vdW ferromagnets has intrinsically strong perpendicular magnetic anisotropy (PMA) even down to monolayer[3, 16, 17], which may enable dense and stable storage. Moreover, certain transition metal dichalcogenides (TMD) have exotic spin-momentum locking effects[18, 19] and large spin-orbit coupling[20, 21], which make them promising spin-generation layers. Particularly, low-symmetry TMD provides out-of-plane polarized spin current[22, 23, 24]. It enables magnetization switching without an external magnetic field by overcoming the intrinsic magnetic damping and enhances the switching efficiency[25, 26].

Recently discovered vdW metallic ferromagnet Fe3GaTe2\mathrm{Fe}_{3}\mathrm{Ga}\mathrm{Te}_{2} maintains strong PMA above room temperature[16, 17] and a few reports have used Pt and WTe2\mathrm{WTe}_{2} to achieve the magnetization switching[27, 28, 29, 30]. The vdW type-II Weyl semimetal TaIrTe4\mathrm{TaIrTe}_{4} has a space group 31 (Pmn21\mathrm{Pmn2}_{1}), and the crystal structure is similar to the TdT_{\mathrm{d}}-phase WTe2\mathrm{WTe}_{2} and MoTe2\mathrm{MoTe}_{2}[31, 32]. The glide plane n and the screw axis 212_{1} symmetry are broken near the surface of TaIrTe4\mathrm{TaIrTe}_{4}, where only a mirror plane m is preserved. When a current is injected perpendicularly to the mirror plane, the low crystal symmetry allows an out-of-plane polarized spin current to be generated. Recently, a few experiments revealed the charge-to-spin conversion in TaIrTe4\mathrm{TaIrTe}_{4} is higher than WTe2\mathrm{WTe}_{2}[33, 34, 56]. Due to the larger spin Hall conductivity of TaIrTe4\mathrm{TaIrTe}_{4} and atomically flat interface in the vdW heterostructure, more robust switching with higher switching efficiency should be expected in TaIrTe4\mathrm{TaIrTe}_{4}/Fe3GaTe2\mathrm{Fe}_{3}\mathrm{GaTe}_{2}. However, the strength of the unconventional SOT exerted by the out-of-plane polarized spin current in all-vdW heterostructures hasn’t been quantified so far and the robustness of switching against the magnetic field hasn’t been examined[29, 35, 36, 37]. These may hinder the further application of using all-vdW heterostructure for spintronics devices.

Here we report the realization of the field-free switching in the all-vdW heterostructure TaIrTe4\mathrm{TaIrTe}_{4}/Fe3GaTe2\mathrm{Fe}_{3}\mathrm{GaTe}_{2} using the unconventional SOT exerted by few-layer TaIrTe4\mathrm{TaIrTe}_{4}. The fully magnetization switching can be achieved at 2.56×1010 A/m22.56 \times10^{10}\,\mathrm{A}/\mathrm{m}^{2} at 300K with a high switching energy efficiency. The effective field induced by the unconventional SOT is around 2.2 mT/(1×1010 A/m2)2.2\,\mathrm{mT}/(1 \times10^{10}\,\mathrm{A}/\mathrm{m}^{2}) determined by the loop-shift method, which can be converted to the SOT effective field efficiency as 0.37. To verify the robustness of the switching against the external magnetic field, we also impose an in-plane magnetic field during the switching process. We find that the switching polarity cannot be changed until the magnetic field reaches 252mT, and this large critical magnetic field indicates a stable magnetization switching. Both unconventional SOT effective field and critical magnetic field are one order larger than previously reported TaIrTe4\mathrm{TaIrTe}_{4}/CoFeB[33, 34]. According to our numerical simulation result, we attribute the high switching efficiency and the stability against magnetic field to the large unconventional SOT that exerted on Fe3GaTe2\mathrm{Fe}_{3}\mathrm{GaTe}_{2}. Our work suggests that all-vdW heterostructure can be considered as a promising candidate for the future spintronics device.

Result

In this study, we fabricate TaIrTe4\mathrm{TaIrTe}_{4}/Fe3GaTe2\mathrm{Fe}_{3}\mathrm{GaTe}_{2} devices with covered hexagonal boron nitride (hBN) pieces to protect these devices from air-degradation (see Methods). The 6nm platinum electrode is used to reduce the effect of strain. hBN, few-layer TaIrTe4\mathrm{TaIrTe}_{4}, and Fe3GaTe2\mathrm{Fe}_{3}\mathrm{GaTe}_{2} are mechanically exfoliated on the silicon wafer and then transferred to the electrode. The schematic is shown in the left part of Figure 1a. The right part of Figure 1a shows the crystal structure of TaIrTe4\mathrm{TaIrTe}_{4} and Fe3GaTe2\mathrm{Fe}_{3}\mathrm{GaTe}_{2}. When the current J flows perpendicularly to the mirror plane m (along a-axis), the out-of-plane polarized spin current will be generated in addition to the conventional in-plane polarized spin current. Thus, the polarization direction will tilt to the out-of-plane direction with an angle of ψ\psi, which is defined as spin canting angle. Figure 1b shows the optical image of device D1. The a-axis of TaIrTe4_4 can be determined to be along the straight long side of the exfoliated flake. It is further confirmed by the angle-resolved polarized Raman spectroscopy (see Supplementary Note 1). The thickness of TaIrTe4_4 and Fe3_3GaTe2_2 in device D1 are 10.3nm and 4.8nm from the atom force microscope results.

Schematic diagram and magnetic characterization of TaIrTe4/Fe3GaTe2 heterostructure

Figure 1. Schematic diagram and magnetic characterization of TaIrTe4_4/Fe3_3GaTe2_2 heterostructure D1. a) Schematic diagram of TaIrTe4_4/Fe3_3GaTe2_2 heterostructure. The right part shows the crystal structure of TaIrTe4_4 and Fe3_3GaTe2_2. The inset shows the a, b and c axis of TaIrTe4_4 and the blue square m is the mirror plane of the few-layer TaIrTe4_4, which is perpendicular to a-axis. When current flows along a-axis, a spin current with polarization ss which tilts from the in-plane direction as ψ\psi angle will be generated. b) Optical image and the atom force microscope result of device D1. The a(b)-axis is indicated by the blue arrows in the picture. The thickness of TaIrTe4_4 and Fe3_3GaTe2_2 determined from AFM is shown in the figure. c,d) Hall resistance as a function of perpendicular magnetic field and in-plane magnetic field at different temperatures. Here an offset is added on RxyR_{xy} to separate different Hall resistance loops. e) Extracted coercivity field and magnetic anisotropy energy density at different temperatures.

The magnetotransport measurement results are shown in Figure 1c-Figure 1e (see Methods). When the magnetic field is perpendicular to the sample surface (along c-axis), a square anomalous Hall loop can be obtained from 180K to 320K, as shown in Figure 1c. The coercivity BcB_\mathrm{c} is 16mT and the anomalous Hall resistance is 4Ω4\Omega at 300K. At 340K, the square loop disappears, suggesting a Curie temperature above room temperature. When the magnetic field sweeps parallel with the sample surface, a parabolic shape appears in the low field range and the curve gradually becomes flat at the high field (Figure 1d), which indicates a strong effective PMA. The effective PMA field can be extracted by fitting the parabolic part, and the PMA energy density KuK_\mathrm{u} can be calculated by adopting the saturation magnetization MsM_\mathrm{s} from ref. 28. BcB_\mathrm{c} and KuK_\mathrm{u} decrease with increasing temperature, as shown in Figure 1e. The PMA energy density of Fe3_3GaTe2_2 is around 4.3×105 J/m34.3 \times10^{5}\,\mathrm{J}/\mathrm{m}^{3}, which is consistent with the previous report[16].

To verify the existence of unconventional SOT and quantify the strength, we do the loop-shift measurement without an in-plane magnetic field. To reduce the Joule heating at the large current (see Supplementary Note 2), a short pulse current (500 μ\mus) is imposed to measure the anomalous Hall loop. When the current flows along a-axis, the out-of-plane polarized spin current will exert unconventional SOT on Fe3_3GaTe2_2. If the unconventional SOT is large enough to overcome the intrinsic magnetic damping, a shift from the original point at the center of hysteresis loop will appear. The SOT effective field at a certain current can be extracted as Beff=(Bcenter+−Bcenter−)/2B_\mathrm{eff} = (B_\mathrm{center}^{+} - B_\mathrm{center}^{-})/2, where Bcenter+B_\mathrm{center}^{+} (Bcenter−B_\mathrm{center}^{-}) represents the center of the anomalous Hall loops when positive (minus) current is imposed.

In the Fe3_3GaTe2_2/TaIrTe4_4 device D1, the hysteresis loops are identical when a low current (±1\pm1mA) is injected along a-axis. While for a large current (±3\pm3mA), two AHE loops are well separated from each other, proving the existence of the unconventional SOT (Figure 2a). Note that we also see a large difference in coercive field BcB_\mathrm{c} when we apply positive and negative current (see Supplementary Note 3). By contrast, when we impose current along b-axis, we observe no clear shift, as shown in Figure 2b. To determine the strength of the unconventional SOT, we measure the current dependence of the SOT effective field, and three sets of AHE loops are collected at every current. The average value of the SOT effective field is calculated and plotted in Figure 2c. In the high current range, the SOT effective field can be fitted by a straight line and the slope represents the SOT effective field per current[33, 34, 38]. Taking the conductivity of Fe3_3GaTe2_2 and TaIrTe4_4 as 4.3×105 Ω−1m−14.3 \times10^{5}\,\Omega^{-1}\mathrm{m}^{-1} and 5.5×105 Ω−1m−15.5 \times10^{5}\,\Omega^{-1}\mathrm{m}^{-1} (a-axis), we extract SOT strength as 2.2mT/(1×1010\times10^{10} A/m2^{2}). The SOT effective field per current can be further converted to the SOT effective field efficiency as

Loop-shift result and the summary of unconventional SOT effective field efficiency and charge conductivity

Figure 2. Loop-shift result and the summary of unconventional SOT effective field efficiency, charge conductivity. a, b) Anomalous Hall loop under 1mA and 3.1mA when current is imposed along a-axis or b-axis. The centers of the anomalous Hall loops shift at I=±3.1mAI = \pm3.1\mathrm{mA} when I//aI // a suggests the existence of the unconventional SOT. c) The SOT-induced effective field as the function of current along a-axis and b-axis. When I//aI // a, The effective field at large currents can be well fitted by the red dash line and the unconventional SOT effective field efficiency can be extracted. While for I//bI // b, the nearly zero BeffB_{\mathrm{eff}} shows the absence of unconventional SOT. The error bar is the standard derivation of three repeated measurements. d) The summary unconventional SOT effective field efficiency and charge conductivity. FM represents the traditional ferromagnetic layer, including CoFeB, Pt/Co/Pt, etc. Benchmark data are from references 24,33,34,38,51–53. The error bar is the standard derivation of three repeated measurements.

0.370.37, according to the equation ξzBeff=2eMstBeff/ℏ\xi_{z}^{B_\mathrm{eff}} = 2eM_\mathrm{s}tB_\mathrm{eff}/\hbar. Here, ξzBeff\xi_{z}^{B_\mathrm{eff}} represents the unconventional SOT effective field efficiency, MsM_\mathrm{s} is the saturation magnetization (here we choose MsM_\mathrm{s} to be 1.7×1051.7 \times10^{5} A/m3^{3}), tt is the thickness of the ferromagnet layer, BeffB_\mathrm{eff} is the SOT effective field, and JJ is the electric current density. Note the SOT effective field efficiency defined here may deviate from the damping-like SOT efficiency determined from the second harmonic Hall measurement or spin torque-ferromagnetic resonance (ST-FMR), where the damping-like SOT field can be measured in the single magnetic domain. We cannot perform second harmonic or ST-FMR measurements to extract the damping-like SOT efficiency because of very small planar Hall resistance (or anisotropic magnetoresistance) and large PMA (see Supplementary Note 9). We also discuss the relation between the damping-like SOT efficiency and the slope extracted from the loop-shift method using numerical simulations (see Supplementary Note 8). On the other hand, when measured along b-axis, the slope is at least one order smaller than the result along a-axis, indicating a negligibly small contribution from unconventional SOT. Notice that due to the intrinsic damping is not compensated when the current is small, the fitted line does not cross the original point[33, 34, 38]. Here we summarize ξzBeff\xi_{z}^{B_{\mathrm{eff}}} and the charge conductivity σc\sigma_{c} in Figure 2d, and the comparison is limited within loop-shift results to avoid errors introduced by different measurement methods.

We also characterize the conventional SOT induced by the in-plane polarized spin current by measuring the loop-shift with in-plane external magnetic field[38]. The conventional SOT effective field is extracted by measuring the shift of AHE loops under positive and minus currents while fixing the magnitude of the current.

The SOT effective field efficiency ξyBeff\xi_{y}^{B_{\mathrm{eff}}} is determined to be 0.15-0.16 along b-axis, which are similar to the reported values in references[33, 34]. All results of loop-shift measurements for ξzBeff\xi_{z}^{B_{\mathrm{eff}}} and ξyBeff\xi_{y}^{B_{\mathrm{eff}}} in three devices are shown in Supplementary Notes 4-7 and Supplementary Table S1.

Using the large unconventional SOT, the field-free switching can be achieved above room temperature. The deterministic switching can be clearly observed when the current is applied along a-axis, and the full switching can be observed at I=±3 mAI=\pm3\,\mathrm{mA}. On the contrary, when I//bI \mathbin{//} b-axis, only in-plane spin polarization can be generated, and no switching can be achieved without the assistance of an external magnetic field. As shown in Figure 3a, the m=0m=0 final state when I//bI \mathbin{//} b-axis indicates a random distribution of m=1m=1 and m=−1m=-1 domain in Fe3GaTe2\mathrm{Fe}_{3}\mathrm{GaTe}_{2}. To examine the repeatability of the field-free switching, we use multiple pulses I=±3.4 mAI=\pm3.4\,\mathrm{mA} to switch the magnetization, and the device shows a highly repeatable high or low Hall resistance according to the positive or minus current (Figure 3b). To test the robustness of the switching against the temperature variation, we measure the magnetization switching at different temperatures. The full switching can be achieved at the temperatures from 285K to 305K (Figure 3c), and the critical current density JcJ_{c} decreases as the temperature rises (Figure 3d). Since the low temperature will enlarge the PMA effective field and saturation magnetization, it leads to a higher JcJ_{c}. At 300K, JcJ_{c} is 2.56×1010 A/m22.56 \times10^{10}\,\mathrm{A/m}^{2}, and the switching efficiency can be calculated as 1.49 according to the equation η=2eMstBc/ℏJc\eta=2eM_{s}t_{B}c/\hbar J_{c}[40, 41], when saturation magnetization MsM_{s} is taken as 1.7×105 A/m21.7 \times10^{5}\,\mathrm{A/m}^{2}[28].

Field-free switching of TaIrTe4/Fe3GaTe2 heterostructure

Figure 3. Field-free switching of TaIrTe4/Fe3GaTe2\mathrm{TaIrTe}_{4}/\mathrm{Fe}_{3}\mathrm{GaTe}_{2} heterostructure. a) Deterministic switching can(cannot) be achieved when current is imposed along the a(b)-axis. b) Repeatable switching using ±3.4 mA\pm3.4\,\mathrm{mA} current, applied along a-axis. c) Switching loops at different temperature. d) Temperature dependence of the critical switching current. The decrease on the switching current density as temperature rises suggests the assistance from thermal effect in the switching process. e) Switching loops at different magnetic field when I∥aI \parallel a-axis. BaB_a represents that the magnetic field is along the a-axis. The arrows on the switching curve indicate the switching polarity. f) Variation of the switching ratio, ΔRxy(B)/ΔRxy(0)\Delta R_{xy}(B)/\Delta R_{xy}(0), with the external magnetic field BB. Here, ΔRxy(B)\Delta R_{xy}(B) represents the Hall resistance change in the switching from large negative to large positive current under the in-plane magnetic field BB. The polarity-changed magnetic field is 252mT, which is record-high at room temperature.

To show the robustness of switching against the external magnetic field, we also do the switching measurement under an in-plane magnetic field. For magnetization switching induced purely by the in-plane polarized spin current, the switching polarity depends on the direction of the in-plane magnetic field and the switching-polarity-changed critical field BcriticalB_{\mathrm{critical}} is 0. On the other hand, in the presence of the out-of-plane polarized spin current, BcriticalB_{\mathrm{critical}} shifts from 0 since the switching by the out-of-plane polarized spin current doesn’t change its polarity under the magnetic field. As shown in Figure 3e, the switching behavior distinguishes under negative and positive magnetic fields. The switching amplitude becomes zero at 252mT and the polarity changes if the magnetic field further increases. By contrast, the polarity doesn’t change under the negative magnetic field. We define the switching ratio, ΔRxy(B)/ΔRxy(0)\Delta R_{xy}(B)/\Delta R_{xy}(0), where ΔRxy(B)\Delta R_{xy}(B) represents the Hall resistance change in the switching from large negative to large positive current under the in-plane magnetic field BB. The switching ratio changes its sign when the switching polarity changes. The switching ratio as a function of the external magnetic field is plotted in Figure 3f. It is worth noticing that the critical field in TaIrTe4/Fe3GaTe2\mathrm{TaIrTe}_{4}/\mathrm{Fe}_{3}\mathrm{GaTe}_{2} is more than one order larger than TaIrTe4/CoFeB\mathrm{TaIrTe}_{4}/\mathrm{CoFeB}[33, 34].

To explore the origin of the robustness, we perform the numerical macrospin simulation based on Landau-Lifshitz-Gilbert (LLG) equation. We take the thermal effect into consideration by adding the thermal effective field (see Method)[42]. The damping-like SOT term in LLG equation is proportional to (m×σ)×m(\boldsymbol{m} \times\boldsymbol{\sigma}) \times\boldsymbol{m}, where m\boldsymbol{m} and σ\boldsymbol{\sigma} is the unit vector of magnetization and spin polarization, respectively. Here we only include the anti-damping term as the results capture the essential physics as we show below. In heavy metal or topological insulator/ferromagnet heterostructure, σ\boldsymbol{\sigma} is taken as in-plane direction. In the TaIrTe4/Fe3GaTe2\mathrm{TaIrTe}_{4}/\mathrm{Fe}_{3}\mathrm{GaTe}_{2}, σ\boldsymbol{\sigma} tilts to the out-of-plane direction with a spin canting angle ψ\psi. First, we simulate the relation between the spin canting angle and the switching ratio (Figure 4a). For every ψ\psi and external magnetic field, 800 times switching simulations for a certain current are done, and the final magnetization M is taken as the average value of these simulations. By sweeping the current, a switching loop is calculated, so the switching ratio can be obtained. For ψ=0∘\psi= 0^\circ, the critical magnetic field BcriticalB_{\mathrm{critical}} is 0 since the switching polarity changes at Bx=0B_x = 0. The zero-switching ratio at Bx=0B_x = 0 means that field-free deterministic switching cannot be achieved without the unconventional SOT. As ψ\psi increases, the critical field gets larger and the switching current JcJ_c decreases (Figure 4b). The numerical simulation results suggest that the higher switching efficiency and larger polarity-change critical field in TaIrTe4/Fe3GaTe2\mathrm{TaIrTe}_{4}/\mathrm{Fe}_{3}\mathrm{GaTe}_{2}, compared to TaIrTe4/CoFeB\mathrm{TaIrTe}_{4}/\mathrm{CoFeB}, can be attributed to larger unconventional SOT that exerted on Fe3GaTe2\mathrm{Fe}_{3}\mathrm{GaTe}_{2}. The experimental switching efficiency and the critical magnetic field are summarized in Figure 4c. We see that our device achieves the record-high robustness against the in-plane field disturbance while maintaining a high energy efficiency.

Numerical simulations and benchmark for switching efficiency and critical magnetic field

Figure 4. Numerical simulations and the benchmark for the switching efficiency and critical magnetic field. a) The switching ratio changes with the external magnetic field for various spin canting angles. The upper left part shows the definition of xx, yy and zz-axis. The spin canting angle is defined as the angle between the spin polarization and sample plane. Four insets show simulated current-induced switching loops for different spin canting angles. b) The relation of switching critical current and critical magnetic field of switching polarity reversal with the spin canting angle in the simulation results. c) The benchmark of experimental critical magnetic field and switching efficiency. Benchmark data are from [28, 33, 34, 38, 40, 51, 52, 54, 55]. The error bar is the standard derivation of seven repeated measurements.

Discussion and conclusion

We show the field-free switching in the all-vdW heterostructure TaIrTe4/Fe3GaTe2\mathrm{TaIrTe}_{4}/\mathrm{Fe}_{3}\mathrm{GaTe}_{2} at and above room temperature with high switching efficiency. The strengths of unconventional SOT and switching-polarity-change magnetic field are further determined. The high experimental critical magnetic field and switching efficiency can be attributed to the large unconventional SOT, according to our numerical simulation results. Notice that the critical magnetic field and unconventional SOT effective field efficiency are both one order larger than the heterostructure consisting of TaIrTe4\mathrm{TaIrTe}_{4} and a non-vdW ferromagnet CoFeB\mathrm{CoFeB}[33, 34]. Here we propose several possible reasons for this. First, compared to the magnetron sputtering method, the dry-transfer method keeps the surface of TaIrTe4\mathrm{TaIrTe}_{4} high-quality$[43]. As the space group of bulk TaIrTe4\mathrm{TaIrTe}_{4} is Pmn21Pmn2_1, which forbids the generation of out-of-plane polarized spin current$[44, 45], the out-of-plane polarized spin current is mainly generated near the surface of TaIrTe4\mathrm{TaIrTe}_{4}. As a result, the unconventional spin conversion highly depends on the surface quality. The dry-transfer method will not do damage to the surface of materials, which may lead to a large unconventional spin generation. Second, the interfacial magnetic spin Hall effect has been discovered in the MoTe2/Fe3GeTe2\mathrm{MoTe}_{2}/\mathrm{Fe}_{3}\mathrm{GeTe}_{2}[46], where the misalignment between the mirror planes of MoTe2\mathrm{MoTe}_{2} and Fe3GeTe2\mathrm{Fe}_{3}\mathrm{GeTe}_{2} breaks the interfacial symmetry and leads to the generation of T-odd spin current. Since MoTe2\mathrm{MoTe}_{2} has the similar crystal structure to TaIrTe4\mathrm{TaIrTe}_{4}, and Fe3GaTe2\mathrm{Fe}_{3}\mathrm{Ga}\mathrm{Te}_{2} is the counterpart of Fe3GeTe2\mathrm{Fe}_{3}\mathrm{GeTe}_{2}, the similar spin-generation mechanism should also exist in TaIrTe4/Fe3GaTe2\mathrm{TaIrTe}_{4}/\mathrm{Fe}_{3}\mathrm{GaTe}_{2}. Third, the strength of spin torque exerted on the ferromagnet layer is not only determined by the spin source material but also dependent on the electronic band structure of the ferromagnet[47, 48]. Since the few-layer Fe3GaTe2\mathrm{Fe}_{3}\mathrm{GaTe}_{2} is a highly anisotropic material compared to CoFeB, the response to the spin current in Fe3GaTe2\mathrm{Fe}_{3}\mathrm{GaTe}_{2} and CoFeB may be different. Finally, the atomically flat interface may also enlarge the spin transparency. These possible reasons are beyond the scope of our experiment, and further theory and experiment investigations remain to be explored.

In summary, we show a highly efficient field-free switching in all-vdW TaIrTe4/Fe3GaTe2\mathrm{TaIrTe}_{4}/\mathrm{Fe}_{3}\mathrm{GaTe}_{2}. The unconventional SOT and polarity-change critical magnetic field are found to be quite high, compared to TaIrTe4\mathrm{TaIrTe}_{4}/CoFeB. The efficient and robust magnetization switching show the advantage of using all-vdW heterostructure as the next generation spintronics device, and many possibilities like gate-controlled spin generation in all-vdW heterostructures are waiting to be explored. For the industrial application, with the success of growing wafer-scale vdW ferromagnets with controlled thickness[49, 50, 15], integrating them into spintronics device for industrial application should also attract more attention.

Figures and captions

Methods

Crystal Growth: The growth method of TaIrTe4TaIrTe_4 has been described in the previous published procedures[34]. Fe3GaTe2Fe_3GaTe_2 crystals were from two source. One was purchased from Nanjing MKNANO Tech. Co., Ltd. The other was grown via a self-flux method. Fe, Ga, and Te were used in a molar ratio of 1:1:2, with high-purity Fe powder (99.99%), Ga lumps (99.9999%), and Te powder (99.999%), placed in a vacuum quartz tube and sealed. The mixture was first heated to 1000°C within 6 hours and maintained at 1000°C for 24 hours. Then, it was cooled down to 880°C within 1 hour, followed by a week-long cooling to 780°C, and maintained at 780°C for 2 days. After reaching room temperature, the sample was crushed, and Fe3GaTe2Fe_3GaTe_2 single crystals were separated using a magnet.

Device Fabrication: Bulk TaIrTe4TaIrTe_4 and Fe3GaTe2Fe_3GaTe_2 were mechanically exfoliated on Si/SiO2(285nm) on the N2_2-filled glovebox. The flakes with appropriate thickness were then optically selected. A PDMS/PC stamp was used to pick up hBN, Fe3GaTe2Fe_3GaTe_2 and TaIrTe4TaIrTe_4 in sequence. To prepare the electrodes, the electron beam lithography was used to define the inner pattern with PMMA. The magnetron sputtering was then carried out to grow 6nm platinum as the electrode. After that, the second electron beam lithography combined with electron beam deposition were used to make the outer pattern Ti(5nm)/Au(50nm).

Transport Measurement: The room-temperature transport measurement is conducted in a custom-built measurement stage and the temperature-varied measurement is done in the Cryogen Free Measurement System (CFMS). The Keithley 2440 and the Kepco current source are used to offer the current for magnet in the custom-built measurement stage. The Keithley 6221 current source and the Keithley 2182 nanovoltmeter are used to measure the loop-shift curve and magnetization switching.

Numerical Simulation: The numerical macrospin simulation is carried out based on the LLG equation combined with the thermal field as

dmdt=−γm×Bk+αm×dmdt+γBSOT[(m×σ)×m]+Bthermal\frac{d\mathbf{m}}{dt}=-\gamma\mathbf{m}\times\mathbf{B}_k+\alpha\mathbf{m}\times\frac{d\mathbf{m}}{dt}+\gamma B_{\mathrm{SOT}}\left[(\mathbf{m}\times\boldsymbol{\sigma})\times\mathbf{m}\right]+\mathbf{B}_{\mathrm{thermal}}

γ\gamma is the gyromagnetic ratio, α\alpha is the Gilbert damping constant, m\mathbf{m} and σ\boldsymbol{\sigma} is the unit vector of magnetization and spin polarization, Bk\mathbf{B}_k is the magnetic anisotropy field, BSOTB_{\mathrm{SOT}} is the magnitude of damping-like SOT field, Bthermal\mathbf{B}_{\mathrm{thermal}} is the thermal field. Here, Bk=(2Ku/Ms)mzz^\mathbf{B}_k=(2K_u/M_s)m_z\hat{z}, σ=(0,cos⁡ψ,−sin⁡ψ)\boldsymbol{\sigma}=(0,\cos\psi,-\sin\psi) (ψ\psi is the spin canting angle), BSOT=ℏθJ/2etFMMsB_{\mathrm{SOT}}=\hbar\theta J/2et_{\mathrm{FM}}M_s (θ\theta is the spin hall angle, JJ is the electric current density, tFMt_{\mathrm{FM}} is the thickness of the ferromagnetic layer, MsM_s is the saturation magnetization), Bthermal=g2kBTα/MsγVΔt\mathbf{B}_{\mathrm{thermal}}=\mathbf{g}\sqrt{2k_BT\alpha/M_s\gamma V\Delta t} (TT is temperature, VV is the volume of the ferromagnetic layer, Δt\Delta t is the time-step of the magnetization evolution, gg is the unit vector consist of three independent Gaussian random variables). We set this parameter as: Ms=2.2×105M_s=2.2\times10^5 A/m, Ku=1×105K_u=1\times10^5 J/m3^3, α=0.2\alpha=0.2, θ=0.2\theta=0.2, tFM=3t_{\mathrm{FM}}=3 nm, T=300T=300 K, V=9×10−19V=9\times10^{-19} m3^3. The simulation time-step is 1 ps. We simulate the magnetization switching 800 times for every current to get 800 final states and the magnetization is taken as the average value of these final states to generate a switching loop. This averaging is simulating the multi-domain effect in the micrometer-size TaIrTe4TaIrTe_4/CoFeB devices.

Acknowledgement

The authors thank Zhencun Pan, Zhiming Liao, Xingkai Cheng, Junwei Liu, Chen Liu, Xixiang Zhang, Yi Wan, Lain-Jong Li for inspiring discussions. The authors at HKUST acknowledge funding support from NSFC/RGC Joint Research Scheme (No. N_HKUST620/21), National Key R&D Program of China (Grants No.2021YFA1401500), Research Grant Council—Early Career Scheme (Grant No. 26200520), General Research Fund (Grant No. 16303521), and the State Key Laboratory of Advanced Displays and Optoelectronics Technologies. The authors at IOP, CAS are supported by the National Natural Science Foundation of China (Grant No. 52161160334). K.W. and T.T. acknowledge support from the JSPS KAKENHI (Grant Numbers 21H05233 and 23H02052) and World Premier International Research Center Initiative (WPI), MEXT, Japan.

Conflicts of interest

The authors declare that they have no conflict of interest.

Author Contributions

Y. Z. fabricated the devices, performed the measurement and analyzed the data with assistance from X. R. and R. L. X. R. and Y. Z. performed the Raman spectroscopy measurement. Z. C. performed the numerical simulation. X. W. helped to fabricate the platinum electrode. G. L., G. Y., J. P. and Y. S offered the TaIrTe4 crystal and W. W. grew the Fe3GaTe2 crystal. K. W., T. T. offer the high-quality hBN. Q. S. conceived and supervised the project. Y. Z. wrote the manuscript, and all authors discussed the content of the manuscript.

Data Availability Statement

The data that support the findings of this study are available from the corresponding author upon reasonable request.

References

  1. [1]Huang, B. et al. Layer-dependent ferromagnetism in a van der Waals crystal down to the monolayer limit. Nature 546, 270–273 (2017).DOI
  2. [2]Gong, C. et al. Discovery of intrinsic ferromagnetism in two-dimensional van der Waals crystals. Nature 546, 265–269 (2017).
  3. [3]Deng, Y. et al. Gate-tunable room-temperature ferromagnetism in two-dimensional Fe3GeTe2. Nature 563, 94–99 (2018).DOI
  4. [4]Huang, B. et al. Electrical control of 2D magnetism in bilayer CrI3. Nat. Nanotechnol. 13, 544–548 (2018).DOI
  5. [5]Jiang, S., Li, L., Wang, Z., Mak, K. F. & Shan, J. Controlling magnetism in 2D CrI3 by electrostatic doping. Nat. Nanotechnol. 13, 549–553 (2018).DOI
  6. [6]Tang, M. et al. Continuous manipulation of magnetic anisotropy in a van der Waals ferromagnet via electrical gating. Nat. Electron. 6, 28–36 (2022).DOI
  7. [7]Wang, Z.-A. et al. Selectively controlled ferromagnets by electric fields in van der Waals ferromagnetic heterojunctions. Nano Lett. 23, 710–717 (2023).DOI
  8. [8]Zhang, K. et al. Gigantic Current Control of Coercive Field and Magnetic Memory Based on Nanometer-Thin Ferromagnetic van der Waals Fe3GeTe2. Adv. Mater. 33, 4 (2021).DOI
  9. [9]Liu, L., Lee, O. J., Gudmundsen, T. J., Ralph, D. C. & Buhrman, R. A. Current-induced switching of perpendicularly magnetized magnetic layers using spin torque from the spin hall effect. Phys. Rev. Lett. 109, 096602 (2012).pubmed.ncbi.nlm.nih.gov/23002867
  10. [10]Liu, L. et al. Spin-torque switching with the giant spin hall effect of tantalum. Science. 336, 6081 (2012).DOI
  11. [11]Sierra, J. F., Fabian, J., Kawakami, R. K., Roche, S. & Valenzuela, S. O. Van der Waals heterostructures for spintronics and opto-spintronics. Nat. Nanotechnol. 16, 856–868 (2021).DOI
  12. [12]Gong, C. & Zhang, X. Two-dimensional magnetic crystals and emergent heterostructure devices. Science. 363, 6428 (2019).DOI
  13. [13]Liu, Y. & Shao, Q. Two-Dimensional Materials for Energy-Efficient Spin-Orbit Torque Devices. ACS Nano 14, 9389–9407 (2020).DOI
  14. [14]Yang, H. et al. Two-dimensional materials prospects for non-volatile spintronic memories. Nature 606, 663–673 (2022).DOI
  15. [15]Wang, H. et al. Room temperature energy-efficient spin-orbit torque switching in two-dimensional van der Waals Fe3GeTe2 induced by topological insulators. Nat. Commun. 14, 5173 (2023).DOI
  16. [16]Zhang, G. et al. Above-room-temperature strong intrinsic ferromagnetism in 2D van der Waals Fe3GaTe2 with large perpendicular magnetic anisotropy. Nat. Commun. 13, 5067 (2022).DOI
  17. [17]Wang, M., Lei, B. & Chen, X. Hard ferromagnetism in van der Waals Fe3GaTe2 nanoflake down to monolayer. npj 2D Mater Appl 8, 22 (2024).DOI
  18. [18]Li, P. et al. Spin-momentum locking and spin-orbit torques in magnetic nano-heterojunctions composed of Weyl semimetal WTe2. Nat. Commun. 9, 3990 (2018).DOI
  19. [19]Song, P. et al. Coexistence of large conventional and planar spin Hall effect with long spin diffusion length in a low-symmetry semimetal at room temperature. Nat. Mater. 19, 292-298 (2020).DOI
  20. [20]Shao, Q. et al. Roadmap of Spin-Orbit Torques. IEEE Trans. Magn. 57, 7 (2021).
  21. [21]Shao, Q. et al. Strong Rashba-Edelstein Effect-Induced Spin-Orbit Torques in Monolayer Transition Metal Dichalcogenide/Ferromagnet Bilayers. Nano Lett. 16, 7514–7520 (2016).pubmed.ncbi.nlm.nih.gov/27960524
  22. [22]MacNeill, D. et al. Control of spin-orbit torques through crystal symmetry in WTe2/ferromagnet bilayers. Nat. Phys. 13, 300–305 (2017).
  23. [23]Zhao, B. et al. Unconventional Charge–Spin Conversion in Weyl-Semimetal WTe2. Adv. Mater. 32, 38 (2020).DOI
  24. [24]Wang, X. et al. Room temperature field-free switching of CoFeB/MgO heterostructure based on large-scale few-layer WTe2. Cell Reports Phys. Sci. 4, 7 (2023).DOI
  25. [25]De Sousa, D. J. P., Haney, P. M., Wang, J. P. & Low, T. Field-Free-Switching State Diagram of Perpendicular Magnetization Subjected to Conventional and Unconventional Spin-Orbit Torques. Phys. Rev. Appl. 18, 054020 (2022).arxiv.org/abs/2210.16344
  26. [26]Zhang, T., Wan, C. & Han, X. Threshold current of field-free perpendicular magnetization switching using anomalous spin-orbit torque. Phys. Rev. B 108, 014432 (2023).DOI
  27. [27]Yun, C. et al. Efficient current-induced spin torques and field-free magnetization switching in a room-temperature van der Waals magnet. Sci. Adv. 9, 49 (2023).DOI
  28. [28]Li, W. et al. Room-Temperature van der Waals Ferromagnet Switching by Spin-Orbit Torques. Adv. Mater. 35, 51 (2023).DOI
  29. [29]Kajale, S. N., Nguyen, T., Hung, N. T., Li, M. & Sarkar, D. Field-free deterministic switching of all–van der Waals spin-orbit torque system above room temperature. Sci. Adv 10, 11 (2024).DOI
  30. [30]Kajale, S.N., Nguyen, T., Chao, C.A. et al. Current-induced switching of a van der Waals ferromagnet at room temperature. Nat Commun 15, 1485 (2024).DOI
  31. [31]Koepernik, K. et al. TaIrTe4: A ternary type-II Weyl semimetal. Phys. Rev. B 93, 201101 (2016).
  32. [32]Haubold, E. et al. Experimental realization of type-II Weyl state in noncentrosymmetric TaIrTe4. Phys. Rev. B 95, 241108 (2017).
  33. [33]Liu, Y. et al. Field-free switching of perpendicular magnetization at room temperature using out-of-plane spins from TaIrTe4. Nat. Electron. 6, 732–738 (2023).DOI
  34. [34]Zhang, Y. et al. Room temperature field-free switching of perpendicular magnetization through spin-orbit torque originating from low-symmetry type II Weyl semimetal. Sci. Adv. 9, 44 (2023).DOI
  35. [35]Kao, J. H. et al. Deterministic switching of a perpendicularly polarized magnet using unconventional spin-orbit torques in WTe2. Nat. Mater. 21, 1029–1034 (2022).DOI
  36. [36]Ye, X. G. et al. Orbit-Transfer Torque Driven Field-Free Switching of Perpendicular Magnetization. Chinese Phys. Lett. 39, 037303 (2022).DOI
  37. [37]Pan, Z. C. et al. Room-temperature orbit-transfer torque enabling van der Waals magnetoresistive memories. Sci. Bull. 68, 2743–2749 (2023).DOI
  38. [38]Hu, S. et al. Efficient perpendicular magnetization switching by a magnetic spin Hall effect in a noncollinear antiferromagnet. Nat. Commun. 13, 4447 (2022).DOI
  39. [40]Alghamdi, M. et al. Highly Efficient Spin-Orbit Torque and Switching of Layered Ferromagnet Fe3GeTe2. Nano Lett. 19, 4400–4405 (2019).DOI
  40. [41]Shao, Q. et al. Role of dimensional crossover on spin-orbit torque efficiency in magnetic insulator thin films. Nat. Commun. 9, 3612 (2018).
  41. [42]Borjas, L. et al. Thermal Fluctuations of a Single-Domain Particle. Phys. Rev. 130, 1677 (1963).
  42. [43]Dean, C. R. et al. Boron nitride substrates for high-quality graphene electronics. Nat. Nanotechnol. 5, 722–726 (2010).DOI
  43. [44]Seemann, M., Ködderitzsch, D., Wimmer, S. & Ebert, H. Symmetry-imposed shape of linear response tensors. Phys. Rev. B - Condens. Matter Mater. Phys. 92, 155138 (2015).DOI
  44. [45]Železný, J. et al. Spin-orbit torques in locally and globally noncentrosymmetric crystals: Antiferromagnets and ferromagnets. Phys. Rev. B 95, 014403 (2017).DOI
  45. [46]Dai, Y. et al. Interfacial magnetic spin Hall effect in van der Waals Fe3GeTe2/MoTe2 heterostructure. Nat. Commun. 15, 1129 (2024).DOI
  46. [47]Kurebayashi, H., Garcia, J. H., Khan, S., Sinova, J. & Roche, S. Magnetism, symmetry and spin transport in van der Waals layered systems. Nat. Rev. Phys. 4, 150–166 (2022).arxiv.org/abs/2107.03763
  47. [48]Manchon, A. et al. Current-induced spin-orbit torques in ferromagnetic and antiferromagnetic systems. Rev. Mod. Phys. 91, 035004 (2019).DOI
  48. [49]Wu, P. et al. Interfacial engineering of ferromagnetism in wafer-scale van der Waals Fe4GeTe2 far above room temperature. Nat. Commun. 14, 2483 (2023).DOI
  49. [50]Liu, S. et al. Wafer-scale two-dimensional ferromagnetic Fe3GeTe2 thin films grown by molecular beam epitaxy. npj 2D Mater. Appl. 1, 30 (2017).DOI
  50. [51]Wang, F. et al. Field-free switching of perpendicular magnetization by two-dimensional PtTe2/WTe2 van der Waals heterostructures with high spin Hall conductivity. Nat. Mater. 23, 769-774 (2024).DOI
  51. [52]Wei, L. et al. Field-free spin-orbit torque-induced switching of perpendicular magnetization at room temperature in WTe2/ferromagnet heterostructures. Appl. Phys. Lett. 123, 252404 (2023).arxiv.org/abs/2212.14281
  52. [54]Lau, Y. C., Betto, D., Rode, K., Coey, J. M. D. & Stamenov, P. Spin-orbit torque switching without an external field using interlayer exchange coupling. Nat. Nanotechnol. 11, 758–762 (2016).DOI
  53. [55]Razavi, A. et al. Deterministic spin-orbit torque switching by a light-metal insertion. Nano Lett. 20, 3703–3709 (2020).DOI
  54. [56]Bainsla, L., Zhao, B., Behera, N. et al. Large out-of-plane spin–orbit torque in topological Weyl semimetal TaIrTe4. Nat Commun. 15, 4649 (2024).

Paper details

vlnc:W_vhex6jur
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents