betaFeedback

WorksPhysics and Astronomy

Elastic polymer networks of exceptional strength by deconcentrating tension

Abstract

The strength of a polymer network is orders of magnitude below that of a polymer chain, because the network concentrates high tension in a small fraction of polymer strands. Here we show that the strength of a network can be greatly amplified by recruiting a larger fraction of strands to bear high tension. We develop approaches to fabricate hydrogels of exceptional strength while maintaining low hysteresis. The strength of the hydrogel increases from ~0.05 MPa for a regular network, to ~1 MPa for a highly entangled network, and further to ~10 MPa for a prestretched interpenetrating network. Similar amplifications of strength are achieved for elastomers. Furthermore, experimental data suggest a scaling relation between strength and strand length. This work provides design principles for creating elastic and strong polymer networks.

Introduction

A single polymer chain can be pulled, by various techniques, to record force as a function of displacement [1]. The chain coils entropically before being pulled. As the displacement increases, the force rises gently when the chain uncoils, and steeply when the chain nearly straightens (Figure 1A). The chain ruptures by breaking a covalent bond. The strength of a polymer network, however, is orders of magnitude below that of a polymer chain [2, 3, 4, 5, 6]. A molecular origin of this large reduction in strength is identified in recent computational simulations [7, 8, 9]. When stretched, a polymer network distributes tension nonuniformly: sparse high-tension paths form and break in succession. Each high-tension path is a sequence of strands (Figure 1B). The strands off the path remain coiled and carry low tension.

Rupture of a polymer chain and a polymer network

Figure 1. Rupture of a polymer chain and a polymer network. (A) Force-displacement curve of a polymer chain. (B) In a polymer network of dense crosslinks, strands are short, and a high-tension path is a sequence of strands. (C) A crosslink connects four strands, only two of which bear high tension, and the other two do not.

We attribute the concentration of tension to crosslinks. In a polymer network, each crosslink connects four strands by covalent bonds. The noncovalent interactions between strands are much weaker than the covalent bonds, so that high tension can transmit along an entire strand. The strand, however, does not transmit its high tension to all the strands connected to the crosslink. Of the four strands connected by the crosslink, only two bear high tension, and the other two do not (Figure 1C). It is the crosslinks that concentrate tension.

Here we fabricate polymer networks to achieve high strength by deconcentrating tension. In a polymer network of sparse crosslinks, strands are long and entangled. We hypothesize that such a network forms high-tension cylinders (Figure 2A). Each high-tension cylinder consists of a volume of long and entangled strands. The diameter of the cylinder in the undeformed state scales with the end-to-end distance of a strand between nearby crosslinks. Because the noncovalent interactions between strands are much weaker than covalent bonds, entanglements readily slip and do not retard the transmission of high tension along the strand. When an entanglement in the cylinder engages four segments, all of them bear high tension (Figure 2B). Crosslinks concentrate tension and set the diameter of a high-tension cylinder. By contrast, entanglements do not retard the transmission of high tension along each strand, and enable the transmission of high tension from one strand to another within each cylinder. Longer strands promote more uniform tension, engage a larger fraction of strands to bear high tension, and elevate the stress carried by surrounding strands. Our experiments with both gels and elastomers confirm that networks of long strands have high strength. The experimental data also suggest a scaling relation between strength and strand length. Guided by the scaling relation we prepare prestretched interpenetrating networks and demonstrate that they amplify strength further.

Schematic of a high-tension cylinder and an entanglement

Figure 2. High-tension cylinder. (A) In a polymer network of sparse crosslinks, strands are long and entangled, and a high-tension cylinder is a volume of strands. (B) In the cylinder, an entanglement engages four segments, all of which bear high tension.

Results

As illustrations, we demonstrate the strength of hydrogels synthesized under three conditions (Figure 3A). The strength of the hydrogel increases from ∼0.05\sim0.05 MPa for a regular network, to ∼1\sim1 MPa for a highly entangled network, and further to ∼10\sim10 MPa for a prestretched interpenetrating network. The hydrogel of a prestretched interpenetrating network can support a weight two orders of magnitude greater than that supported by a regular hydrogel (Figure 3, B and C; Movies S1 and S2). The influence of network topology on strength will be discussed in detail in the following sections.

Stress-stretch curves and photographs of regular, highly entangled, and prestretched interpenetrating hydrogels

Figure 3. Polyacrylamide hydrogels prepared under three conditions. (A) Stress-stretch curves. (B) A regular hydrogel, and (C) a prestretched interpenetrating hydrogel hanging a weight, respectively.

We test the hypothesis using polyacrylamide (PAAm) hydrogels, prepared by free radical polymerization using precursors composed of four components: monomer, crosslinker, water, and photoinitiator. Let CC be the crosslinker-to-monomer molar ratio, and WW be the water-to-monomer molar ratio. The photoinitiator-to-crosslinker molar ratio is fixed at 0.4, and the reaction is conducted under an ultraviolet light of low intensity. These conditions ensure that the fraction of dangling ends in the network is negligible, and the network is properly formed [10, 11, 12, 13]. We choose PAAm hydrogels as the model system for two reasons. First, in a fully swollen hydrogel, the polymer chains are screened by water molecules, so that the noncovalent interactions between strands are weak, and their effect on strength is negligible compared to network topology. Second, the densities of crosslinks and entanglements can be independently varied in wide ranges, by changing CC and WW, respectively. In applications, hydrogels are commonly used in contact with water. Thus, the as-prepared hydrogels are submerged in pure water to swell to equilibrium. The fully swollen hydrogels are then used to measure various properties.

The three hydrogels shown in Figure 3 are prepared as follows. First, we follow the common practice to synthesize hydrogels using precursors with high values of W=24W = 24 and C=10−3C = 10^{-3}. The resulting polymer network is densely crosslinked and sparsely entangled. Such materials are referred to as regular hydrogels. Second, we synthesize hydrogels using precursors with low values of W=2W = 2 and C=10−4.5C = 10^{-4.5}. The resulting polymer network is sparsely crosslinked and densely entangled [10]. Third, to further enhance strength, we prepare a hydrogel of a prestretched interpenetrating network.

The effect of crosslinks on strength is studied by preparing PAAm networks using precursors of a fixed W=8W = 8 and various CC. As noted before, each hydrogel is submerged in pure water and swells to equilibrium before the measurement of various properties. The polymer content ϕ\phi is defined as the volume of dry polymer divided by the volume of the fully swollen hydrogel. As expected, the polymer content ϕ\phi increases with CC (Figure 4A). Swelling is constrained mostly by entanglements at low CC, and mostly by crosslinks at high CC [10].

Hydrogels prepared using precursors of various crosslinker-to-monomer molar ratios

Figure 4. Hydrogels prepared using precursors of various crosslinker-to-monomer molar ratios, CC, and a fixed water-to-monomer molar ratio, W=8W = 8. The as-prepared networks are submerged in pure water to swell to equilibrium before properties are measured as a function of CC. (A) Polymer content ϕ\phi. (B) Stress-stretch curves. (C) Nominal strength sfs_f. (D) Stretchability λf\lambda_f. (E) Effective strength Σf\Sigma_f.

Stress–stretch curves are measured for samples of various CC (Figure 4B). The nominal stress ss is defined as the applied force divided by the cross-sectional area of the undeformed sample. The stretch λ\lambda is defined as the length of the deformed sample divided by the length of the undeformed sample. The nominal stress and the stretch at rupture define the nominal strength sfs_f and stretchability λf\lambda_f (Figure 4C and D)

The nominal strength sfs_f is a non-monotonic function of CC, reaching a maximum at C∼10−0.45C \sim10^{-0.45} and a minimum at C∼10−2.5C \sim10^{-2.5} (Figure 4C). When C<10−4.5C < 10^{-4.5}, the network is poorly formed, and the strength drops. When C>10−2.5C > 10^{-2.5}, the strength rises again, but scatters widely. These densely crosslinked networks are brittle, so that their strengths are sensitive to flaws. In the rest of this paper, we focus on the intermediate range of CC, so that the network is well formed, and the strength is flaw-insensitive.

To compare the strength of the polymer network of various stretchability and polymer content, we define the effective stress Σ\Sigma as follows. When stretched, a sample changes its volume negligibly, and is taken to be incompressible. The true stress σ\sigma is defined as the applied force divided by the cross-sectional area of the deformed sample. The incompressibility relates the true stress to the nominal stress as σ=sλ\sigma= s\lambda. In a hydrogel, water molecules do not bear load, so that the effective stress carried by the polymer network itself is the true stress divided by the polymer content, Σ=sλ/ϕ\Sigma= s\lambda/\phi. In an elastomer without solvent, the polymer content is ϕ=100%\phi= 100\%, and the effective stress coincides with the true stress. In a hydrogel, the polymer content ϕ\phi is lower than 100%, and the effective stress exceeds the true stress. The effective strength, Σf=sfλf/ϕ\Sigma_f = s_f \lambda_f / \phi, is computed using the measured nominal strength, stretchability, and polymer content.

The effective strength, Σf\Sigma_f, varies with the crosslinker-to-monomer molar ratio, CC (Figure 4E). At a low C=10−4.5C = 10^{-4.5}, both the nominal strength and the stretchability are large, so that the effective strength is high, Σf∼100\Sigma_f \sim100 MPa. At a high C=10−2.5C = 10^{-2.5}, both the nominal strength and the stretchability are small, so that the effective strength is low, Σf∼3\Sigma_f \sim3 MPa. As noted before, when CC is too low (C<10−4.5C < 10^{-4.5}), hydrogels have poorly formed polymer networks and show low strength. When CC is too high (C>10−2.5C > 10^{-2.5}), hydrogels are brittle, and the strengths are sensitive to flaws and scatter significantly. Once the data in these two extreme regimes are excluded, the effective strength scales with the crosslinker-to-monomer molar ratio as Σf∼C−1\Sigma_f \sim C^{-1}. This scaling indicates that sparse crosslinks enable a larger fraction of strands to approach high tension.

Next, the effect of entanglements on strength is studied by preparing PAAm networks using precursors of various WW and a fixed C=10−3.5C = 10^{-3.5}. When the precursor has a high water-to-monomer molar ratio, W=24W = 24, the resulting polymer chains are dilute and sparsely entangled (Figure 5A). When the precursor has a low water-to-monomer molar ratio, W=2W = 2, the resulting polymer chains are concentrated and densely entangled (Figure 5B). In either case, once the polymer chains are crosslinked into a network, the number of entanglements is invariant when the network is submerged in pure water to swell.

Hydrogel structure and mechanical properties for varying water-to-monomer molar ratios

Figure 5. Hydrogels prepared with varying water-to-monomer molar ratios, WW, at a fixed crosslinker-to-monomer molar ratio, C=10−3.5C = 10^{-3.5}. (A) The hydrogel prepared at a high WW is sparsely entangled. (B) The hydrogel prepared at a low WW is highly entangled. (C) Polymer content ϕ\phi. (D) Nominal strength sfs_f. (E) Stretchability λf\lambda_f. (F) Effective strength Σf\Sigma_f.

Stress–stretch curves are measured for samples of various WW (Fig. S1). As WW increases, the polymer content decreases (Figure 5C), the nominal strength decreases (Figure 5D), and the stretchability increases (Figure 5E). Notably, the effective strength is less sensitive to WW, varying by less than a factor of two (Figure 5F). Our experimental results support the molecular picture: crosslinks concentrate tension, while entanglements do not. Because noncovalent interactions between strands are much weaker than the covalent bonds along strands, entanglements slip readily under load. That is, an entanglement acts like a pulley, and does not hinder the transmission of high tension along a strand. This “pully effect” between entangled strands is analogous to that in a network containing molecular slide rings [14, 15].

We further examine the effect of crosslinks and entanglements on strength by measuring the properties of PAAm hydrogels prepared with various CC and WW. These hydrogels exhibit substantial variations in polymer content (Figure 6A), nominal strength (Figure 6B), and stretchability (Figure 6C). By comparison, the effective strength collapses onto a scaling relation of Σf∼C−1\Sigma_f \sim C^{-1} and shows weak dependence on WW (Figure 6D).

Four panels showing polymer content, nominal strength, stretchability, and effective strength of hydrogels prepared using precursors of various $C$ and $W$

Figure 6. Hydrogels prepared using precursors of various CC and WW. The hydrogels are then submerged in pure water to swell to equilibrium, before properties are measured. (A) Polymer content ϕ\phi. (B) Nominal strength sfs_f. (C) Stretchability λf\lambda_f. (D) Effective strength Σf\Sigma_f.

The effective strength Σf\Sigma_f quantifies the capability of the network to recruit strands to bear high tension, and the nominal strength sfs_f quantifies the force that can be sustained by a material. The former aids in molecular understanding, and the latter is important in applications. By definition, the two measures of strength are related by sf=ϕΣf/λfs_f = \phi\Sigma_f/\lambda_f. The sparse crosslinks set a high effective strength Σf\Sigma_f, whereas the entanglements constrain swelling, which leads to a high polymer content ϕ\phi, and limits the stretch, which leads to a low stretchability λf\lambda_f. The combination of high Σf\Sigma_f, high ϕ\phi, and low λf\lambda_f leads to a high nominal strength. Among all hydrogels prepared with various CC and WW, the highest nominal strength achieved is sf∼1s_f \sim1 MPa (Figure 6B). This high nominal strength is attained by a sample prepared with a precursor with an unusually low value of CC, which leads to sparse crosslinks, and an unusually low value of WW, which leads to dense entanglements. By comparison, commonly reported nominal strength for PAAm hydrogels is on the order of 0.05 MPa [2, 16, 17].

The above understanding suggests that nominal strength can be amplified by maintaining a high effective strength while increasing polymer content and reducing stretchability. Following this idea, we prepare an interpenetrating network in which strands are long, entangled, and prestretched (Figure 7A). The long and entangled strands deconcentrate high tension, while the prestretch shifts strand configurations closer to full extension prior to external loading.

Hydrogels of prestretched interpenetrating networks

Figure 7. Hydrogels of prestretched interpenetrating networks. (A) An as-prepared single-network (SN) hydrogel is fully swollen in a precursor, and then biaxially prestretched, followed by photopolymerization of the second network to form a prestretched double-network (PDN) hydrogel. The process is repeated to form a prestretched triple-network (PTN) hydrogel. All networks are synthesized with the same precursor (W=3W = 3 and C=5×10−5C = 5 \times10^{-5}). The resulting hydrogels are fully swollen in water before the test. (B) Polymer content. (C) stress-stretch curves. (D) Effective strength.

We start with an as-prepared single-network (SN) hydrogel of sparse crosslinks and dense entanglements, and then submerge it in the same precursor to swell to equilibrium. The precursor-swollen SN hydrogel is then compressed in the thickness direction into a state of in-plane biaxial prestretch. In the deformed state, upon exposure to ultraviolet light, the precursor polymerizes into a second network, which interpenetrates with the first network. The second network partially locks the deformation of the first network, leading to a prestretched double-network (PDN) hydrogel. The process can repeat itself multiple times. For example, repeating this process twice produces a prestretched triple-network (PTN) hydrogel.

All SN, PDN, PTN hydrogels are submerged in pure water to swell to equilibrium. The fully swollen hydrogels are then used to measure polymer contents (Figure 7B) and stress-stretch curves (Figure 7C), as well as to calculate the effective strength (Figure 7D). A PTN hydrogel exhibits an exceptional nominal strength of ∼10\sim10 MPa, a high polymer content of ∼25%\sim25\%, and a moderate stretchability of ∼2.8\sim2.8. By contrast, SN hydrogel has a strength of ∼0.8\sim0.8 MPa, a moderate polymer content of ∼13%\sim13\%, and a high stretchability of ∼6\sim6.

The high nominal stress is contributed by the two processes during the preparation of interpenetrating networks, namely swelling and mechanical prestretch. First, each round of precursor swelling leads to an isotropic prestretch of the pre-existing polymer network. Second, the mechanical prestretch further straightens the pre-existing network strands. The prestretch effect limits the stretchability (Fig. S2). The reduced stretchability does not result from the brittleness or premature fracture. Rather, it is because more strands in the network reach their full extension at a smaller stretch. This interpretation is supported by the pronounced strain-stiffening of the PTN hydrogel before rupture, consistent with the single-chain mechanics that the chain stiffens as it approaches its full extension.

Moreover, the effective strength of the PTN is about 115 MPa, ~2.6 times that of SN about 45 MPa, and still falls in the scaling plane of the effective strength range at C=5×10−5C = 5 \times10^{-5} (Fig. S3). The enhancement in effective strength of PTN compared to the SN likely results from more efficient stress deconcentration across neighboring strands by interpenetrating structure, enabling more strands to bear high tension.

The high effective strength set by sparse crosslinks, together with the high polymer content and limited stretchability set by entanglements and the prestretch, lead to the high nominal strength of PTN hydrogel. To the best of our knowledge, the strength of PTN hydrogel is the highest among the polyacrylamide hydrogels.

In addition to the high strength, the PTN hydrogel remains highly elastic, with a low hysteresis of 8.4% (Fig. S4). Here, hysteresis is defined by the ratio of two areas: the area enclosed by the loading-unloading curves, and the area underneath the loading curve, measured up to the stretch of two. The low hysteresis results from two aspects. First, the noncovalent interactions between strands are weak. Second, strands are long and remain intact at a moderate stretch. In the plane of hysteresis and nominal strength, the PTN hydrogel shows both high strength and low hysteresis, outperforming existing PAAm-based hydrogels (Figure 8). Also note that high nominal strength has been achieved by some polymer networks with significant noncovalent interactions between strands. Examples include natural rubber and PEG hydrogels that undergo strain induced crystallization, PVA hydrogels and polyurethane that contain hard domains, and glassy gels strengthened by solvent-mediated noncovalent crosslinking [18, 19, 20, 21, 22, 23]. These noncovalent interactions usually increase hysteresis. And how noncovalent interactions enhance strength requires further study.

Comparison of various polyacrylamide-based hydrogels on the plane of nominal strength and hysteresis

Figure 8. Comparison of various polyacrylamide-based hydrogels on the plane of nominal strength and hysteresis. [2, 10, 24, 25, 26, 27, 28].

To demonstrate the generality of our design principles, we prepare a model elastomer, poly(ethyl acrylate) (PEA), by free radical polymerization using precursors composed of three components: monomer, crosslinker, and photoinitiator. Because no extra solvents are used, the entanglement density is invariant. The nominal stress–stretch curves are measured for PEA with different crosslinker-to-monomer molar ratios CC (Figure 9A). The nominal strength increases from ~1 MPa for a highly crosslinked network, to ~4 MPa for a sparse crosslinked network (Figure 9B). The effective strength also roughly follows the Σf∼C−1\Sigma_f \sim C^{-1} scaling relation (Figure 9C). We further amplify the nominal strength of the sparsely crosslinked network by making a prestretched double-network (PDN) PEA (Figure 9D). As the ratio of mechanical prestretch increases, more strands approach their full extension prior to external loading, so that the nominal strength further enhances to ~25 MP (Figure 9E). In addition to this exceptional strength, the PDN network maintains a low hysteresis of ~5% (Figure 9F).

Mechanical properties of elastomers

Figure 9. Mechanical properties of elastomers. (A) Stress–stretch curves of single-network (SN) poly(ethyl acrylate) (PEA) elastomers prepared with varying CC. (B) Nominal strength sfs_f as a function of CC for SN elastomers. (C) Effective strength of SN. The effective strength of SN elastomers as a function of CC is fitted to the Σf∼C−1\Sigma_f \sim C^{-1} scaling. (D) Stress–stretch curves of double-network (DN) elastomers prepared with different prestretch ratios λpre\lambda_{\mathrm{pre}}. (E) Nominal strength sfs_f as a function of λpre\lambda_{\mathrm{pre}} for DN elastomers. (F) The loading-unloading curve of the DN elastomer prepared with λpre=2\lambda_{\mathrm{pre}}=2. The elastomer has a low hysteresis of 4.3% for loading up to λ=2\lambda=2 and 6.2% for λ=3\lambda=3.

Discussion

In summary, we have shown that the strength of a network can be greatly amplified by recruiting a larger fraction of strands to bear high tension. We fabricate hydrogels of exceptional strength by several approaches, including forming polymer networks with long and entangled strands, interpenetrating networks, and prestretched networks. The strength is ∼\sim0.05 MPa for a regular network, ∼\sim1 MPa for a highly entangled network, and ∼\sim10 MPa for a prestretched interpenetrating network. Similar amplifications of strength are achieved for elastomers. Furthermore, experimental data suggest a scaling relation between strength and strand length. This work provides design principles for creating elastic and strong polymer networks.

Our experimental data indicate an approximate scaling of Σf∼C−1\Sigma_f \sim C^{-1}. Several observations provide some understanding. As noted before, in a polymer network of sparse crosslinks, strands form high-tension cylinders (Figure 2A). Each high-tension cylinder consists of a volume of long and entangled strands. Crosslinks concentrate tension and set the diameter of a high-tension cylinder. In the undeformed state, the diameter of such a cylinder scales with the end-to-end distance of a strand between nearby crosslinks, which follows C−0.5C^{-0.5} for the random walk model. Therefore, the cross-sectional area of the high-tension cylinder in the undeformed state scales as C−1C^{-1}. Because the noncovalent interactions between strands are much weaker than covalent bonds, entanglements readily slip and do not retard the transmission of high tension along the strand. When an entanglement in the cylinder engages four segments, all of them bear high tension (Figure 2B). These considerations are consistent with the experimental findings that high effective strength is achieved at a low crosslink density, and is not sensitive to either entanglement density or prestretch.

Polymer networks of sparse crosslinks, the highest effective strength achieved is Σf∼100\Sigma_f \sim100 MPa, which is, however, still much smaller than the strength of covalent bonds of ∼10\sim10 GPa. This large reduction in strength indicates that within the polymer network the high-tension cylinders are sparse. About 1% of strands achieve the covalent bond strength, while the strands off high-tension cylinders carry much lower tension. How to recruit more strands to bear high tension remains an open question and may require new network architectures.

Materials and Methods

Preparation of single-network (SN) PAAm hydrogel

Acrylamide (AAm, A8887), N,N′-methylenebisacrylamide (MBAA, M7279), and 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone (Irgacure 2959, 410896) were used as the monomer, crosslinker, and photoinitiator, respectively. All chemicals were purchased from Sigma-Aldrich and used as received. Deionized water was used as the solvent and obtained from Poland Spring. The monomer, crosslinker, and initiator solutions were mixed with water in a conical tube to obtain precursors with different water-to-monomer (WW), crosslinker-to-monomer (CC), and initiator-to-monomer (II) molar ratios. The initiator-to-crosslinker molar ratio is fixed at I/C=0.4I/C = 0.4. A mold was prepared by pressing a silicone spacer (thickness 0.8 mm) onto a glass plate. The precursor solution was poured into the mold and covered with a second glass plate. The two plates were clamped together using binder clips. The assembled mold was placed inside a nitrogen-filled plastic bag and irradiated for 3 hours using a UV lamp (365 nm, ∼5\sim5 mW cm−2^{-2}). After curing, the hydrogel sample was submerged in water for at least 24 hours to swell to equilibrium.

Preparation of double-network (DN) PAAm hydrogel

The first network was prepared from a precursor solution with a water-to-monomer molar ratio W=3W = 3 and a crosslinker-to-monomer molar ratio C=5×10−5C = 5 \times10^{-5}. The resulting SN hydrogel was then soaked in the same precursor for 24 hours to fully swell. The swollen hydrogel was placed between two glass plates, with the edges sealed using parafilm. The plates were compressed using eight C-shaped clamps (McMaster-Carr, 5133A13) to achieve various prestretch λpre\lambda_{\mathrm{pre}}. The PDN hydrogel in Figure 7 is synthesized with λpre=2\lambda_{\mathrm{pre}} = 2. The assembled mold was placed in a nitrogen-filled plastic bag and irradiated for 3 hours using a UV lamp (365 nm, ∼5\sim5 mW cm−2^{-2}). After curing, the DN hydrogel was submerged in water for at least 24 hours to swell to equilibrium.

Preparation of triple-network (TN) PAAm hydrogel

The TN hydrogel was prepared by soaking a DN hydrogel in a precursor solution with W=3W = 3 and C=5×10−5C = 5 \times10^{-5}, followed by photopolymerization. TN-free hydrogels were obtained without applying any prestretch during the polymerization of both the second and third network. To prepare PTN hydrogels, a DN hydrogel (synthesized with λpre=2\lambda_{\mathrm{pre}} = 2) was soaked in the same precursor solution and prestretched to λpre=1.5\lambda_{\mathrm{pre}} = 1.5 during the polymerization of the third network.

Preparation of single-network (SN) PEA

Ethyl acrylate (EA), tricyclo[5.2.1.02,6^{2,6}]decanedimethanol diacrylate (TDDA), and 2-hydroxy-2-methylpropiophenone (Irgacure 1173) were used as the monomer, crosslinker, and photoinitiator, respectively. All reagents were purchased from Sigma-Aldrich and used as received. Solutions of the initiator and crosslinker were mixed with the monomer in a conical tube. The initiator-to-crosslinker molar ratio was fixed at 0.4, while the crosslinker-to-monomer molar ratio CC was varied. A mold was prepared by pressing a silicone spacer (thickness 0.8 mm) onto a glass plate. The precursor solution was poured into the mold and covered with a second glass plate. The two plates were clamped together using binder clips. The assembled mold was placed inside a nitrogen-filled plastic bag and irradiated overnight using a UV lamp (365 nm, ∼5\sim5 mW cm−2^{-2}). After curing, the sample was removed from the mold and left in a fume hood for 24 hours to allow evaporation of residual monomers.

Preparation of double-network (DN) PEA

The SN network was prepared from a precursor solution with a crosslinker-to-monomer molar ratio C=10−4C=10^{-4}. The elastomer was then soaked in a second precursor solution of the same composition for 24 hours to allow full swelling. The swollen elastomer was placed between two glass plates, and the edges were sealed using parafilm. The plates were compressed using eight C-shaped clamps to achieve various prestretch λpre\lambda_{\mathrm{pre}}. The assembled mold was enclosed in a nitrogen-filled plastic bag and irradiated for 12 hours using a UV lamp (365 nm, ∼5\sim5 mW cm−2^{-2}).

Tensile tests

Samples were cut into a dumbbell shape using a die cutter (Ace Steel Rule Dies, ISO 527-2-5B). All mechanical tests were conducted with Instron 5966 universal testing machine equipped with a 100 N load cell. The gauge length and width of the sample were 20 mm and 2 mm, respectively. All tensile tests were performed at a constant stretch rate of 0.05 s−1^{-1}. A humidifier was used to provide vapor to hydrogel samples during the tensile tests to prevent water loss.

Polymer content measurement

The polymer content ϕ\phi was calculated as the volume of dry polymer divided by the volume of the fully swollen hydrogel. ϕ\phi was calculated as ϕ=1/[(m/mdry−1)(ρA/ρW)+1]\phi= 1/[(m/m_{\mathrm{dry}}-1)(\rho_A/\rho_W)+1], where mm is the mass of the fully swollen hydrogel, mdrym_{\mathrm{dry}} is the dry mass, ρA=1.13\rho_A=1.13 g/cm3^3 is the density of acrylamide, and ρW=1\rho_W=1 g/cm3^3 is the density of water.

Acknowledgments

Funding: This work was supported by the National Science Foundation under MRSEC (DMR-2011754).

Author contributions: Y.Z. conceived of the project. Y.Z., C.L., Z.C., and Z.S. designed the study and interpreted the results. Y.Z. conducted the experiments. Y.Z., C.L., Z.C., X.B., and Z.S. wrote the manuscript. Z.S. supervised the research. All authors discussed the result and commented on the manuscript.

Competing interests: The authors declare that they have no competing interests.

References

  1. [1]W. Zhang, S. Zou, C. Wang, X. Zhang, Single polymer chain elongation of poly (N-isopropylacrylamide) and poly (acrylamide) by atomic force microscopy. The Journal of Physical Chemistry B 104, 10258-10264 (2000).DOI
  2. [2]C. Yang, T. Yin, Z. Suo, Polyacrylamide hydrogels. I. Network imperfection. Journal of the Mechanics and Physics of Solids 131, 43-55 (2019).
  3. [3]G. J. Lake, A. G. Thomas, The strength of highly elastic materials. Proceedings of the Royal Society of London. Series A. Mathematical and Physical Sciences 300, 108-119 (1967).DOI
  4. [4]M. Tao, S. Lavoie, Z. Suo, M. K. Cameron, The effect of scatter of polymer chain length on strength. Extreme Mechanics Letters 61, 102024 (2023).arxiv.org/abs/2304.12815
  5. [5]T. Sakai, T. Matsunaga, Y. Yamamoto, C. Ito, R. Yoshida, S. Suzuki, N. Sasaki, M. Shibayama, U.-i. Chung, Design and fabrication of a high-strength hydrogel with ideally homogeneous network structure from tetrahedron-like macromonomers. Macromolecules 41, 5379-5384 (2008).DOI
  6. [6]X. Zhao, Designing toughness and strength for soft materials. Proceedings of the National Academy of Sciences 114, 8138-8140 (2017).DOI
  7. [7]J. Li, K. Zhang, F. Tian, X. Lei, X. Shi, J. Wang, Inherent tensile strength and stretchability of unentangled elastomers. Macromolecules 58, 11445-11464 (2025).DOI
  8. [8]Z. Yu, N. E. Jackson, Shortest paths govern bond rupture in thermoset networks. Macromolecules 58, 1728-1736 (2025).DOI
  9. [9]S. Mohanty, J. Blanchet, Z. Suo, W. Cai, Why is the strength of a polymer network so low? arXiv preprint arXiv:2502.11339, (2025).arxiv.org/abs/2502.11339
  10. [10]J. Kim, G. Zhang, M. Shi, Z. Suo, Fracture, fatigue, and friction of polymers in which entanglements greatly outnumber cross-links. Science 374, 212-216 (2021).DOI
  11. [11]X. Bao, G. Nian, Y. Kutsovsky, J. Kim, Q. Jiao, Z. Suo, Low-intensity mixing process of high molecular weight polymer chains leads to elastomers of long network strands and high fatigue threshold. Soft Matter 19, 5956-5966 (2023).DOI
  12. [12]Z. Chen, Z. Suo, Thermodynamic and Molecular Origins of Crack Resistance in Polymer Networks. Chemical Reviews 126, 606-670 (2025).DOI
  13. [13]P. J. Flory, Principles of polymer chemistry (Cornell university press, 1953).
  14. [14]S. Granick, M. Rubinstein, A multitude of macromolecules. Nature Materials 3, 586-587 (2004).pubmed.ncbi.nlm.nih.gov/15343287
  15. [15]Y. Okumura, K. Ito, The polyrotaxane gel: a topological gel by figure-of-eight cross-links. Advanced materials 13, 485-487 (2001).doi.org/10.1002/1521-4095(200104)13:7<485::aid-adma485>3.0.co;2-t
  16. [16]Y. Wang, G. Nian, J. Kim, Z. Suo, Polyacrylamide hydrogels. VI. Synthesis-property relation. Journal of the Mechanics and Physics of Solids 170, 105099 (2023).DOI
  17. [17]X. Li, J. P. Gong, Design principles for strong and tough hydrogels. Nature Reviews Materials 9, 380-398 (2024).DOI
  18. [18]G. Nian, Z. Chen, X. Bao, M. W. M. Tan, Y. Kutsovsky, Z. Suo, Natural rubber with high resistance to crack growth. Nature Sustainability 8, 692-701 (2025).DOI
  19. [19]C. Liu, N. Morimoto, L. Jiang, S. Kawahara, T. Naromi, H. Yokoyama, K. Mayumi, K. Ito, Tough hydrogels with rapid self-reinforcement. Science 372, 1078-1081 (2021).DOI
  20. [20]M. Hua, S. Wu, Y. Ma, Y. Zhao, Z. Chen, I. Frenkel, J. Strzalka, H. Zhou, X. Zhu, X. He, Strong tough hydrogels via the synergy of freeze-casting and salting out. Nature 590, 594-599 (2021).DOI
  21. [21]Y. Eom, S.-M. Kim, M. Lee, H. Jeon, J. Park, E. S. Lee, S. Y. Hwang, J. Park, D. X. Oh, Mechano-responsive hydrogen-bonding array of thermoplastic polyurethane elastomer captures both strength and self-healing. Nature communications 12, 621 (2021).DOI
  22. [22]S. Lin, J. Liu, X. Liu, X. Zhao, Muscle-like fatigue-resistant hydrogels by mechanical training. Proceedings of the National Academy of Sciences 116, 10244-10249 (2019).DOI
  23. [23]M. Wang, X. Xiao, S. Siddika, M. Shamsi, E. Frey, W. Qian, W. Bai, B. T. O’Connor, M. D. Dickey, Glassy gels toughened by solvent. Nature 631, 313-318 (2024).DOI
  24. [24]R. Zhu, D. Zhu, Z. Zheng, X. Wang, Tough double network hydrogels with rapid self-reinforcement and low hysteresis based on highly entangled networks. Nature Communications 15, 1344 (2024).DOI
  25. [25]H. Savolainen, N. Hosseiniyan, M. Piedrahita-Bello, O. Ikkala, Bioinspired nondissipative mechanical energy storage and release in hydrogels via hierarchical sequentially swollen stretched chains. Nature Communications 16, 4544 (2025).DOI
  26. [26]C. H. Yang, M. X. Wang, H. Haider, J. H. Yang, J.-Y. Sun, Y. M. Chen, J. Zhou, Z. Suo, Strengthening alginate/polyacrylamide hydrogels using various multivalent cations. ACS applied materials & interfaces 5, 10418-10422 (2013).DOI
  27. [27]J. P. Gong, Y. Katsuyama, T. Kurokawa, Y. Osada, Double-network hydrogels with extremely high mechanical strength. Advanced materials 15, 1155-1158 (2003).DOI
  28. [28]W. Zhang, X. Liu, J. Wang, J. Tang, J. Hu, T. Lu, Z. Suo, Fatigue of double-network hydrogels. Engineering Fracture Mechanics 187, 74-93 (2018).DOI

Paper details

vlnc:W_vksgucvd
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents