Tilted pp-wave magnet candidate CeNiAsO

Abstract

The unexpectedly small ordered moments of CeNiAsO, a candidate for correlated pp-wave magnet, have posed a serious challenge to the precise determination of its magnetic structure, hindering the understanding of its fundamental properties. By leveraging the high sensitivity to local internal fields, our 75^{75}As nuclear quadrupole / magnetic resonance experiments reveal a commensurate antiferromagnetic order with a small out-of-plane moment mz≈0.05m_z\approx0.05 μBμ_{\mathrm{B}}. This tilted magnetic configuration not only rotates the spin polarization axis away from the crystallographic c\mathbf{c}-axis, but also enhances the non-relativistic spin splitting. We refer to this rare paradigm as a \textit{tilted pp-wave magnet}.

Recently, altermagnetism has attracted widespread attention as a novel magnetic classification beyond conventional ferromagnetism and antiferromagnetism. Remarkably, altermagnetic materials exhibit spin-split electronic bands without showing net moment or stray field in real space [1], holding great promise for spintronic applications. Typical examples include MnTe [11], CrSb [14], and RuO2_2 [3] that possess dd- or gg-wave symmetry. In contrast to these even-parity magnetisms in which the moments are collinearly ordered, an alternate branch – odd-parity, pp-wave magnetism – often occurs in non-collinear orders, preserving the combined time-reversal and translation operation (Tτ)(T\tau) symmetry [18]. Such anisotropic nodal spin splitting potentially gives rise to even richer properties and application prospects, e.g. Majorana fermions via proximity coupling to superconductors [19], as well as the highly efficient spin-charge conversion in the absence of spin-orbit coupling – namely, the non-relativistic Edelstein effect [24].

Among the handful of proposed candidates for pp-wave magnet [28, 29] [18, 27], the heavy-fermion compound CeNiAsO is special in that the strong electronic correlation effect arising from the fluctuating Ce-4f4f electrons likely endow it with higher tunability and better functionality. CeNiAsO crystallizes in the tetragonal ZrCuSiAs-type structure with the space group P4/nmmP4/nmm (No. 129), iso-structural to the well-known 1111 iron-based superconductors [30]. The cerium moments in this compound undergo two sequential antiferromagnetic (AFM) transitions at TN1∼9T_{N1} \sim9 K and TN2∼7T_{N2} \sim7 K, respectively [31].

Unconventional heavy-fermion quantum criticality and strange-metal-like behavior were attained by either pressure tuning or As-for-P doping [32]. Neutron scattering and muon spin rotation studies suggested that its ground-state magnetic structure for below TN2T_{N2} is a commensurate AFM (CAFM) order with propagation vector q=(0.5,0,0)\mathbf{q}=(0.5, 0, 0) and [±1/2][\pm1/2] Kramers doublet character [33]. This proposed magnetic structure is characterized by a coplanar, non-collinear arrangement of moments, preserving both TτT\tau and C2zsTC_{2z}^{s}T symmetries, with the spin polarization oriented perpendicular to the moment plane (Sz∥c\mathbf{S}_z \parallel\mathbf{c}). These features prompted the suggestion of candidate pp-wave magnet [29] [18, 24, 34].

However, many aspects of this compound remain puzzling. First of all, the ordered moment (∼0.37 μB\sim0.37~\mu_{\mathrm{B}}/Ce [33]) is far less than the expected value for [±1/2][\pm1/2] doublet and than that in the structural analog CeFeAsO (0.83 μB0.83~\mu_{\mathrm{B}}/Ce) [35]. Second, this magnetic order is highly resistant to external field – the cc-axis magnetization reaches only 0.17 μB0.17~\mu_{\mathrm{B}}/Ce up to 58 T (see Figure S1 in Supplemental Material (SM) [36]). Although Kondo hybridization might plausibly explain the reduction of Ce moments, this is ruled out by the high magnetic entropy gain (>0.7Rln⁡2>0.7R\ln2) at TN1T_{N1} [31] and the recent angular resolved photoemission spectroscopy (ARPES) experiments [37, 38], which all confirm that Ce-4f4f is highly localized. Last but not least, the mysteriously small magnetic moment also imposes exceptional difficulty to definitively resolve mzm_z, the out-of-plane component of the Ce moments [33, 39]. Whether the moments are strictly coplanar, and how the zz-canted components are arranged, directly dictate the preservation or breakdown of the C2zTC_{2z}T symmetry. This epitomizes a broader, unresolved issue in the field of altermagnetism: how does this canting universally impact the stability of symmetry-enforced spin-splitting? Accurately resolving the magnetic structure of CeNiAsO, therefore, provides an essential benchmark for disentangling these competing effects and lays a robust foundation for understanding the underlying physical properties [37, 38, 40, 41].

Figure S1. Sample characterization of CeNiAsO. (a) Temperature dependence of magnetic susceptibility, χ(T)\chi(T). (b) Electrical resistivity as a function of TT, ρ(T)\rho(T). Two AFM transitions are seen in both polycrystalline and single-crystalline samples. (c) Isothermal field dependent magnetization, M(H)M(H), measured at 1.6 K. The magnetizations under pulsed field are calibrated by the low-field results measured with SQUID. For both H∥c\mathbf{H} \parallel c and H⊥c\mathbf{H} \perp c, M(H)M(H) curves are linear with field up to 58 T. In particular, McM_c reaches only 0.17 μB\mu_{\mathrm{B}} at 58 T.

Here, by virtue of the high-sensitivity to local internal field, we exploit 75^{75}As nuclear quadrupole resonance (NQR) and nuclear magnetic resonance (NMR) to reinvestigation into the magnetic order of CeNiAsO. Our analysis reveals that the ground state of CeNiAsO is a tilted coplanar CAFM order with a small cc-canting moment mz≈0.05 μBm_z \approx0.05\,\mu_{\mathrm{B}}. This magnetic canting establishes a new spin plane and reconstructs the spin-group symmetry, resulting in a reorientation of the spin polarization axis n^\hat{n} deviating from the crystallographic cc axis (Figure 1). The anomalous Hall effect (AHE) is forbidden at zero field by the preserved TτT\tau symmetry, but emerges under a high magnetic field when this symmetry is broken, revealing the intimate connection between magnetic-symmetry reconstruction and the pp-wave spin-splitting behavior, which is further supported by first-principles calculations.

Figure 1. (a) Crystalline / magnetic structure of CeNiAsO, and local environment of As. The red arrows denote the proposed commensurate AFM structure of Ce ions with q=(0.5,0,0)\mathbf{q} = (0.5, 0, 0) for T<TN2T < T_{\mathrm{N2}}, while the blue arrows indicate the internal field at the As sites. (b) Top-view and side-view of the magnetic structure; the canted component mz∼0.05 μBm_z \sim0.05\,\mu_{\mathrm{B}}. TτT\tau symmetry is preserved in this magnetic structure. (c) Tilted spin polarization axis n^≈(0,0.231,0.973)\hat{n} \approx(0, 0.231, 0.973).

75^{75}As (nuclear spin 75I=3/2^{75}I = 3/2, gyromagnetic ratio 75γn=7.2919^{75}\gamma_n = 7.2919 MHz/T, and quadrupole moment 75Q=0.29^{75}Q = 0.29 barns) NQR and NMR (external field μ0H=10\mu_0H = 10 T) measurements were conducted on high-quality CeNiAsO samples. High-field Hall effect and magnetization measurements were made at Hefei (steady) and Wuhan (pulsed) high magnetic field laboratories, respectively. DFT +U+ U calculations [42] with constrained moment directions [43] were performed using Vienna ab initio simulation package (VASP) [44] with Perdew-Burke-Ernzerhof type generalized gradient approximation [45] and projected augmented-wave [46] pseudo-potentials.

The anomalous Hall conductivity was then evaluated via Wannier functions [47]. See SM for details [36].

The raw data of 75^{75}As NQR spectra of CeNiAsO at low temperature are displayed in Figure S2 [36]. For 75I=3/2^{75}I = 3/2, only one resonance peak is expected in the NQR spectra in the paramagnetic regime, which is indeed the case at 10 K. νQ=8.007\nu_Q = 8.007 MHz is obtained by Gaussian fitting, close to but slightly larger than that from NMR experiments at 10 T (Figure S3). Below TN1T_{\mathrm{N1}}, for instance 8 K and 7.5 K, the peak broadens significantly due to the continuous distribution of the internal field in the incommensurate AFM (ICAFM) order. Upon further cooling to below TN2T_{\mathrm{N2}}, the NQR peak clearly splits into two peaks (Figure 2(a)), manifesting the development of CAFM order [33, 39].

Comparison of experimental and calculated $^{75}$As NQR spectra, $^{75}$As NMR spectra, and contour plot of fitting parameters

Figure 2. (a) Comparison of the experimental (left) and calculated (right) 75^{75}As NQR spectra determines the angle between Bint\mathbf{B}_{\mathrm{int}} and the EFG principle axis, θint≈44∘\theta_{\mathrm{int}} \approx44^\circ, and Bint≈0.213B_{\mathrm{int}} \approx0.213 T. The colormap represents the normalized transition probability. (b) 75^{75}As NMR spectra of single crystalline CeNiAsO for H⊥c\mathbf{H} \perp c (top) and H∥c\mathbf{H} \parallel c (bottom). Note that νzz′\nu_{zz'} differs slightly from νzz\nu_{zz} (or νQ\nu_Q) due to the small misalignment of cc axis with respect to H\mathbf{H}. The vertical lines in these panels signify the simulated NMR frequencies. (c) The contour plot of log⁡10Rp\log_{10} R_p gives the optimal parameters for the refinement, θm=8.2∘\theta_m = 8.2^\circ, and ϕm=37.5∘\phi_m = 37.5^\circ.

${}^{75}\mathrm{As}$ NQR and NMR spectra of CeNiAsO

Figure S2. (a) 75As{}^{75}\mathrm{As} NQR spectra of CeNiAsO for T≤10T \le10 K. The black solid lines are the Gaussian fittings. (b-c) 75As{}^{75}\mathrm{As} NMR spectra of CeNiAsO measured at external field μ0H≈10\mu_0H \approx10 T, and H∥c\mathbf{H} \parallel c. The gray circles are reproduced from our previous aligned-powder results [39], while the red and blue circles stand for the new results obtained from single crystals at 10 K and 2 K, respectively. The asterisk in panel (b) indicates a small amount of nonaligned powders. (d-e), ibid, but for H⊥c\mathbf{H} \perp c. At 10 K in the paramagnetic phase, the resonance peaks are narrow; for TN2<T<TN1T_{\mathrm{N2}} < T < T_{\mathrm{N1}} in the incommensurate AFM phase, broad resonance peaks are observed due to the continuous distribution of internal field; for T<TN2T < T_{\mathrm{N2}} in the commensurate AFM phase, well split resonance peaks are seen.

${}^{75}\mathrm{As}$ NMR spectra of single crystalline CeNiAsO

Figure S3. (a-b) 75As{}^{75}\mathrm{As} NMR spectra of single crystalline CeNiAsO for H∥c\mathbf{H} \parallel c and H⊥c\mathbf{H} \perp c, respectively. The external field μ0H=10\mu_0H = 10 T. Note that νzz′\nu_{zz'} differs slightly from νzz\nu_{zz} (or νQ\nu_Q) due to the small misalignment of cc axis with respect to H\mathbf{H}.

Such an evolution of magnetic order in CeNiAsO is also evidenced by 75^{75}As NMR experiments. In Figure S2-Figure S2) [36], we reproduce our previous aligned-powder NMR spectra in gray [39], and show the recent single crystalline NMR results in red (10 K) and blue (2 K). On the whole, the single crystal results well resemble those from aligned powders. At 10 K in the paramagnetic phase, three distinct peaks are discernible for both H∥c\mathbf{H} \parallel c and H⊥c\mathbf{H} \perp c, arising from the central (−12↔12)(-\frac{1}{2} \leftrightarrow\frac{1}{2}) and satellite (±12↔±32)(\pm\frac{1}{2} \leftrightarrow\pm\frac{3}{2}) transitions of the 75I=3/2^{75}I = 3/2 nucleus. Further cooled down to below TN2T_{\mathrm{N2}}, each peak splits (seeing also Figure 2(b)), which is better seen in the single crystal data, characteristic of CAFM order.

We now analyze these NQR and NMR results in depth aiming to obtain the magnetic structure of the CAFM phase. For more details, we refer the readers to SM [36]. First of all, it is necessary to figure out the internal field (Bint\mathbf{B}_{\mathrm{int}}) with respect to the electric field gradient (EFG), and this can be obtained by a combination of numerical simulation and fitting to the experimental spectra. To account for both NQR and NMR results, we write the total Hamiltonian as

Htot=HZ+Hint+HQ,(1)\mathcal{H}_{\mathrm{tot}} = \mathcal{H}_{Z} + \mathcal{H}_{\mathrm{int}} + \mathcal{H}_{Q}, \tag*{(1)}

where HZ\mathcal{H}_{Z} is the Zeeman term caused by the external field; Hint\mathcal{H}_{\mathrm{int}} is the (Zeeman) term induced by internal field; and HQ\mathcal{H}_{Q} is the nuclear quadrupole interaction with EFG [48], taking the form

HQ=eQVzz4I(2I−1)[3I^z2−I^2+η(I^x2−I^y2)],(2)\mathcal{H}_{Q} = \frac{eQV_{zz}}{4I(2I-1)}[3\hat{I}_{z}^{2} - \hat{I}^{2} + \eta(\hat{I}_{x}^{2} - \hat{I}_{y}^{2})], \tag*{(2)}

in which I^=(I^x,I^y,I^z)\hat{\mathbf{I}} = (\hat{I}_{x}, \hat{I}_{y}, \hat{I}_{z}) is nuclear spin operator, and η=(Vxx−Vyy)/Vzz\eta= (V_{xx} - V_{yy})/V_{zz} is the asymmetry parameter with VxxV_{xx}, VyyV_{yy} and VzzV_{zz} being the components of the EFG tensor. First, to simulate the zero-field NQR results, we ignore HZ\mathcal{H}_Z in Eq. (1), and calculate the resonance frequencies as functions of BintB_{\mathrm{int}} with varying polar angle θint\theta_{\mathrm{int}}. The representative results are provided in Figure S5 [36]. We find the results that best fit our NQR spectra are Bint=0.213B_{\mathrm{int}} = 0.213 T with θint=44∘\theta_{\mathrm{int}} = 44^\circ, as shown in Figure 2(a).

75As NQR frequency as a function of B_int

Figure S5. 75^{75}As NQR frequency as a function of BintB_{\mathrm{int}}. The orientation of Bint\mathbf{B}_{\mathrm{int}} is characterized by θint\theta_{\mathrm{int}} with respect to the principle axis of EFG. (a) θint=0\theta_{\mathrm{int}} = 0. (b) θint=45∘\theta_{\mathrm{int}} = 45^\circ. (c) θint=90∘\theta_{\mathrm{int}} = 90^\circ. The colormap represents the normalized transition probability.

Second, the azimuthal angle ϕint\phi_{\mathrm{int}} of the Bint\mathbf{B}_{\mathrm{int}} can also be determined by calculating the central peak splitting (Δf\Delta f) of the 75^{75}As NMR spectra, as shown in Figure S4 and Figure S6 [36]. We find ϕint=26.5∘\phi_{\mathrm{int}} = 26.5^\circ uniquely fits the experimental satisfactorily. Hence, the internal field at the As site can be fully determined, as is shown by the blue arrows in Figure 1(a).

NMR spectra of $^{75}$As central transition in aligned-powder CeNiAsO under different magnetic fields at 2 K

Figure S4. NMR spectra of 75^{75}As central transition in aligned-powder CeNiAsO under different magnetic fields at 2 K. The reference frequency f0=75γnμ0Hf_0 = {}^{75}\gamma_n\mu_0H. (a) H⊥c\mathbf{H} \perp c. (b) H∥c\mathbf{H} \parallel c. Below ∼13\sim13 T, the peak splitting Δf\Delta f in both field directions remains essentially unchanged with field; above ∼13\sim13 T, Δf\Delta f decreases substantially, suggesting that the magnetic moments start to be reoriented.

Calculated $^{75}$As NMR central peak splitting as a function of azimuthal angle

Figure S6. The calculated 75^{75}As NMR central peak splitting (Δf\Delta f) as a function of the azimuthal angle of Bint\mathbf{B}_{\mathrm{int}} with respect to a axis. Within the range of [0,180∘][0,180^\circ], Δf\Delta f for H∥c\mathbf{H} \parallel c increases monotonically with ϕint\phi_{\mathrm{int}}, while the results for H⊥c\mathbf{H} \perp c minimizes at ϕint=90∘\phi_{\mathrm{int}}=90^\circ. It is found that only ϕint≈26.5∘\phi_{\mathrm{int}}\approx26.5^\circ can simultaneously fit both experimental results satisfactorily well.

In Ce-based heavy-fermion compounds, the internal field is mainly governed by the transferred hyperfine interaction with Ce-4f4f spins that relies on orbital overlap [49, 50]. Note that Ni is non-magnetic in CeNiAsO and thus has little contribution to spin susceptibility [51, 52] [31]. In this context, each As has four nearest-neighbor Ce spins [labeled as Ce1-4 in Figure 1(a)]. In addition, the two next-nearest-neighbor Ce5 and Ce6 – which sit right above and below As – should also be taken into account due to their considerable hybridization with As-4pz4p_z orbitals [39]. Therefore, we have

Bint=∑i=16Ai⋅mi,(3)\mathbf{B}_{\mathrm{int}} = \sum_{i=1}^{6} \mathbf{A}_i \cdot\mathbf{m}_i, \tag*{(3)}

where Ai\mathbf{A}_i is the ii-th hyperfine tensor, and mi\mathbf{m}_i is the ordered magnetic moment of the ii-th Ce ion. The detailed forms of Ai\mathbf{A}_i tensors are described in SM [36]. To obtain the magnetic structure, we combine the internal field information obtained above and use the magnetic moment m≈0.37 μB\mathbf{m} \approx0.37\ \mu_{\mathrm{B}} from previous neutron scattering studies [33]. For different orientations of ordered moments characterized by a combination of polar angle (θm\theta_m) and az-

imuthal angle (ϕm\phi_m), hyperfine coupling constant Ahf,abcalA_{\mathrm{hf},ab}^{\mathrm{cal}} can be computed and compared with the experimental Ahf,abexp=−0.42A_{\mathrm{hf},ab}^{\mathrm{exp}} = -0.42 T/μB\mu_{\mathrm{B}} [39]. The goodness of the fitting is evaluated by

Rp(θm,ϕm)=(Ahf,abcal−Ahf,abexp)2.(4)R_p(\theta_m, \phi_m) = \left(A_{\mathrm{hf},ab}^{\mathrm{cal}} - A_{\mathrm{hf},ab}^{\mathrm{exp}}\right)^2. \tag*{(4)}

The optimal parameters θm=8.2∘\theta_m = 8.2^\circ and ϕm=37.5∘\phi_m = 37.5^\circ are obtained where log⁡10Rp\log_{10} R_p minimizes, as is shown in Figure 2(c). Note that the derived ϕm\phi_m is very close to 36∘36^\circ, the value reported by the previous neutron scattering study [33]. The little θm\theta_m yields a small mz≈0.05 μBm_z \approx0.05\ \mu_{\mathrm{B}}, which is also within the uncertainty of the neutron scattering experiment (∼0.06 μB\sim0.06\ \mu_{\mathrm{B}}) [33]. The as-proposed canted CAFM order is depicted in Figure 1, and a comparison of measured and simulated NMR spectra is provided in Figure 2(b). The sign of mzm_z alternates along the aa axis in this magnetic structure; we hereafter denote it as CAFMz_z for brevity.

Due to the emergence of a finite mzm_z component, the C2zsTC_{2z}^{s}\mathcal{T} symmetry is violated, and the spin polarization is no longer constrained along the crystallographic cc-axis. Instead, the canted magnetic moments define a new spin plane with a normal vector n^≈(0, 0.231, 0.973)\hat{\mathbf{n}} \approx(0,\ 0.231,\ 0.973) [36]. Consequently, the spin-group symmetry is reconstructed into a combined operation of T\mathcal{T} and a twofold spin rotation about n^\hat{\mathbf{n}}, namely C2nsTC_{2\mathbf{n}}^{s}\mathcal{T}. Under this symmetry, together with the preserved T\mathcal{T} symmetry, the spin polarization axis of the electronic bands is rotated from the crystallographic cc-axis to the magnetic axis n^\hat{\mathbf{n}}, resulting in a reorientation of the altermagnetic spin polarization. To see this clearly, we performed first-principles calculations using the DFT+UU method. Relative large U=5U = 5 eV and J=2J = 2 eV were employed to account for the localized Ce-4f4f electron here [37, 38]. Figure 3(a) shows the band structure along the Γ\Gamma-XX path. Despite the tilted CAFMz_z structure, the non-relativistic odd-parity spin-split bands remain robustly preserved. Remarkably, by calculating the spin band splitting ΔS\Delta_S as a function of the canting angle θm\theta_m, we uncover a non-monotonic dependence as shown in Figure 3(b), i.e., ΔS\Delta_S initially increases with θm\theta_m, reaching a maximum near 32∘32^\circ where its value is enhanced by 23% as compared with that in the non-canted case, and then decreases continuously and diminishes at θm=90∘\theta_m = 90^\circ. Our results demonstrate that magnetic tilting provides a new route to actively reorient the spin polarization axis and to further promote the non-relativistic Edelstein effect in altermagnetic materials, beyond the conventional picture that the spin texture is constrained by the crystallographic symmetry.

Spin-dependent band structures, spin band splitting, and anomalous Hall conductivity for CeNiAsO

Figure 3. (a) Spin dependent band structure of CeNiAsO for CAFMz_z, θm=8∘\theta_m = 8^\circ. (b) Spin band splitting ΔS\Delta_S as a function of θm\theta_m in CAFMz_z. (c) Spin dependent band structure for canted FMz_z, θm=8∘\theta_m = 8^\circ; this configuration is to simulate the oriented magnetic state under high field H∥c\mathbf{H} \parallel\mathbf{c}. (d) Calculated anomalous Hall conductivity σxyA\sigma_{xy}^{A} for CAFMz_z and FMz_z configurations with θm=8∘\theta_m = 8^\circ.

Another hallmark for pp-wave magnet is the absence of zero-field AHE, prohibited by the Tτ\mathcal{T}\tau symmetry that enforces Ω(k)=−Ω(−k)\Omega(\mathbf{k}) = -\Omega(-\mathbf{k}), leading to a vanishing Berry curvature (Ω\Omega) integral over the Brillouin zone. This is indeed the case in the CAFMz_z configuration of CeNiAsO, seeing Figure 3(d). Nonetheless, the AHE can be expected to emerge when the magnetic moments are reoriented by an external field, provided that the Tτ\mathcal{T}\tau symmetry is broken. To see this, we also simulate a FMz_z configuration wherein the magnetic moments have a partially polarized component along c\mathbf{c} [Figure 3(c)]; a significant σxyA\sigma_{xy}^{A} is anticipated in this configuration, cf Figure 3(d).

The experimental observation of this evolution, however, faces formidable challenges, primarily due to the good metallicity and the exceptionally hard magnetization of CeNiAsO (Figure S1 [36]). To overcome these dif-

ficulties, we performed high-precision high-field Hall effect measurements with H∥c\mathbf{H} \parallel\mathbf{c}, as shown in Figure 4 and Figure S8 [36]. At 2 K, the Hall resistivity ρyx\rho_{yx} consists of two parts: an ordinary contribution ρyxO\rho_{yx}^{O}, and a loop-structured AHE ρyxA\rho_{yx}^{A}. The ordinary part can be well fitted to ρyxO(H)=RHH+R2H2\rho_{yx}^{O}(H) = R_HH + R_2H^2; the H2H^2 term is expected to become important in the high-field regime where the condition ωcτtr≪1\omega_c\tau_{\mathrm{tr}} \ll1 no longer holds (ωc\omega_c is cyclotron frequency; τtr\tau_{\mathrm{tr}} is scattering time) [53, 54]. The obtained small Hall coefficient RH=2.9(1)×10−10R_H = 2.9(1) \times10^{-10} m3^3/C reaffirms the good metallicity [32]. The AHE component is extracted and displayed in Figure 4(b) for temperatures in different magnetic phases. Remarkably, such AHE appears only in the CAFMz_z phase, and disappears immediately when TT surpasses TN2T_{N2}. Moreover, by checking the field dependent 75^{75}As NMR spectra [Figure S4] [36], one finds that the central peak splitting Δf\Delta f only slightly decreases for fields below 12 T, but starts to drop rapidly when field exceeds 13 T, cf Figure 4(c); this onset field agrees well with the field region where the first AHE loop is observed (black vertical dashed line). Such a substantial reduction of Δf\Delta f is a signature of the reorientation of Ce moments under high field [seeing the red dashed line in Figure 4(c)]. We conjecture that once field is large enough to generate a net mzm_z (viz FMz_z state), the Tτ\mathcal{T}\tau symmetry is broken, and this can lead to the appearance of AHE. Due to the small magnetic moment and the extremely-hard magnetization process Figure S1 [36], such a field-induced reorientation is expected to be slow or quasi-continuous, for which magnetization measurements under pulsed high field may not be capable of resolving this feature. We should also admit that the underlying mechanism for the two separate AHE loops at low temperature remains unclear to us. To further clarify this issue, additional NMR experiments with much higher field will be necessary. We leave this open question for future investigation.

Figure 4. (a) Hall resistivity as a function of field at 2 K. The open symbols represent the smoothed curve, serving as guides to the eye. (b) AHE at various temperatures (raw data in Figure S8 [36]). The curves are vertically shifted for clarity. The colors of the background manifest distinct magnetic phases: white - paramagnetic; magenta - ICAFМ [33]; cyan - CAFM. (c) 75^{75}As NMR central peak splitting Δf\Delta f measured under varying field. The red dashed line is a theoretical prediction assuming that the Ce moments do not reorient with applied field. The insets depict the conjectured magnetic structures in the field regions below and above ∼13\sim13 T, wherein the Tτ\mathcal{T}\tau symmetry is preserved and violated, respectively.

Field dependence of Hall resistivity in CeNiAsO single crystal at selected low temperatures

Figure S8. Field dependence of Hall resistivity ρyx\rho_{yx} in CeNiAsO single crystal at selected low temperatures. The open symbols are smoothed curves, serving as guides to the eye. (a) T=2T = 2 K. (b) T=3T = 3 K. (c) T=4T = 4 K. (d) T=5T = 5 K. (e) T=6T = 6 K. (f) T=7T = 7 K. (g) T=8T = 8 K. (h) T=10T = 10 K.

In conclusion, we successfully revised the magnetic structure of CeNiAsO utilizing a combination of 75^{75}As NQR and NMR measurements. The results reveal a tilted-coplanar commensurate AFM order, featuring a small out-of-plane moment mz≈0.05 μBm_z \approx0.05\,\mu_{\mathrm{B}} that readily breaks the C2zsTC_{2z}^{s}T symmetry while preserves the TτT\tau symmetry, thereby giving rise to potential tilted pp-wave magnetism, which is further supported by DFT+UU calculations and the avoided AHE at zero field. Our work prompts a renewed examination of the peculiar pp-wave magnetism and the underlying physical properties of this heavy-fermion altermagnet. In addition, the method we established in this work should also be applicable to determining the magnetic structure in other small-ordered-moment systems, particularly under the extreme conditions (e.g. high pressure or strong magnetic field) where conventional neutron techniques may prove inadequate.

**Acknowledgments—**The authors acknowledge Joe D. Thompson and Wu Xie for helpful discussions. This work is supported by National Key R&D Program of China (2023YFA1609600, 2022YFA1602602, 2023YFA1406101), National Natural Science Foundation of China (U23A20580 and 52588101), and Beijing National Laboratory for Condensed Matter Physics (2024BNLCMPKF004). We thank the HM of the Steady High Magnetic Field Facility, CAS (https://cstr.cn/31125.02.SHMFF.HM) for the assistance on the experiment. We also thank the Magnetic Property Station of Wuhan National High Magnetic Field Center (https://whmfc.hust.edu.cn/yhfw/cljs.htm).

**Data availability—**All data that support the findings of this study are available from the corresponding authors upon request.

Supplemental Material: Tilted pp-wave magnet candidate CeNiAsO

Zhuo Wang; Zheng Liu; Shuo Zou; Hua-Xun Li; Jin-Xin Hu; Zhuolun Qiu; Ze Wang; Jiamin Gong; Lucheng Wei; Kangjian Luo; Hai Zeng; Meng Zhang; Chao Dong; Chuanyin Xi; Junfeng Wang; Jiakun Fang; Xiaotao Han; Guang-Han Cao; Liang Li; Yongkang Luo

In this Supplemental Material (SM), we provide additional results that further support the discussion and conclusion in the main text, including experimental and calculation methods, sample characterization, magnetization under pulsed high field, Hall effect, the raw 75As^{75}\mathrm{As} NQR and NMR data, and the details of internal field calculation.

Methods {#sec:SM I}

High-purity polycrystalline CeNiAsO was grown by solid-state reaction [31, 32]. CeNiAsO single crystals were grown by the NaAs-flux method as described elsewhere [40]. The quality of these samples were characterized by magnetic susceptibility and resistivity measurements (Figure S1). 75As{}^{75}\mathrm{As} (nuclear spin 75I=3/2{}^{75}I = 3/2, gyromagnetic ratio 75γn=7.2919 MHz/T{}^{75}\gamma_n = 7.2919\ \mathrm{MHz/T}, and quadrupole moment 75Q=0.29{}^{75}Q = 0.29 barns) NQR and NMR spectra were acquired by a stepped frequency-sweep method using a Redstone spectrometer (Tecmag) and a high-homogeneity superconducting magnet (Oxford Instruments). Approximately 500 mg of powder sample was used for the zero-field NQR measurements. For NMR experiments, 19 pieces of CeNiAsO single crystals with a total mass ∼2\sim2 mg were accumulated and properly aligned in the sample coil; the measurements were made under μ0H≈10\mu_0H \approx10 T, the precise value of which was determined by the in-situ 63Cu{}^{63}\mathrm{Cu} shift of the sample coil. High-field Hall effect and magnetization measurements were conducted at Hefei (steady) and Wuhan (pulsed) high magnetic field laboratories, respectively. High-precision Hall signal was measured by a low-noise lock-in amplifier SR865A equipped with an SR554A pre-amplifier.

Our first-principles calculations were performed by using the projected augmented-wave method [46] as implemented in the Vienna ab initio simulation package (VASP) [44]. The generalized gradient approximation of the Perdew-Burke-Ernzerhof type was used to describe the exchange-correlation interaction [45]. All the atoms were allowed to relax until the Hellmann-Feynman force on each atom is smaller than 0.02 eV/A˚\mathring{\mathrm{A}}. The Γ\Gamma-centered Monkhorst-Pack grid of 4×8×44 \times8 \times4 was used during the calculation. The plane-wave energy cutoff was set to 460 eV. The DFT +U+U method [42] with U=5.0U = 5.0 eV and J=2.0J = 2.0 eV was used to account for the on-site Coulomb interaction of the Ce-4ff electrons. The directions of the magnetic moments were constrained by adding a penalty functional to the total energy [43]. The Wigner-Seitz radii were chosen as 1.98 A˚\mathring{\mathrm{A}}, 1.21 A˚\mathring{\mathrm{A}}, 1.09 A˚\mathring{\mathrm{A}}, and 0.24 A˚\mathring{\mathrm{A}} for Ce, Ni, As, and O atoms, respectively. After obtaining the self-consistent electronic structure, maximally localized Wannier functions were constructed using the Wannier90 package [47]. The anomalous Hall conductivity was subsequently calculated in the Wannier representation. A 120×120×120120 \times120 \times120 kk-point mesh was adopted to evaluate the anomalous Hall conductivity of canted AFM and canted FM CeNiAsO.

Sample characterization {#sec:SM II}

SM III. Raw data of 75As{}^{75}\mathrm{As} NQR and NMR

SM IV. Determination of the internal field

To incorporate both NMR and NQR results, we write the total Hamiltonian as

Htot=HZ+Hint+HQ,(5)\mathcal{H}_{\mathrm{tot}}=\mathcal{H}_{Z}+\mathcal{H}_{\mathrm{int}}+\mathcal{H}_{Q}, \tag*{(5)}

where HZ\mathcal{H}_{Z} is the Zeeman term caused by the external field; Hint\mathcal{H}_{\mathrm{int}} is the (Zeeman) term induced by the internal field (Bint\mathbf{B}_{\mathrm{int}}); and HQ\mathcal{H}_{Q} is the nuclear quadrupole interaction with the electric field gradient (EFG), taking the form

HQ=eQVzz4I(2I−1)[3I^z2−I^2+η(I^x2−I^y2)],(6)\mathcal{H}_{Q}=\frac{eQV_{zz}}{4I(2I-1)}\left[3\hat{I}_{z}^{2}-\hat{I}^{2}+\eta\left(\hat{I}_{x}^{2}-\hat{I}_{y}^{2}\right)\right], \tag*{(6)}

in which I^=(I^x,I^y,I^z)\hat{\mathbf{I}}=(\hat{I}_{x},\hat{I}_{y},\hat{I}_{z}) is nuclear spin operator, QQ is nuclear quadrupole moment, and η≡(Vxx−Vyy)/Vzz\eta\equiv(V_{xx}-V_{yy})/V_{zz} is the asymmetry parameter with VxxV_{xx}, VyyV_{yy} and VzzV_{zz} being the components of the EFG tensor.

According to the NMR experiments, we estimate that the amplitude of Bint\mathbf{B}_{\mathrm{int}} is in the order of 0.1 T, in which case for the NQR measurements (HZ=0\mathcal{H}_{Z}=0) the Hint\mathcal{H}_{\mathrm{int}} can not be treated as a perturbation to HQ\mathcal{H}_{Q}, or vise versa. A rigorous numerical calculation, therefore, is needed. Since the principal axes of these three terms are generally different, we diagonalize the total Hamiltonian via a unitary transformation

H=U†HtotU,(7)\mathcal{H}=\mathbf{U}^{\dagger}\mathcal{H}_{\mathrm{tot}}\mathbf{U}, \tag*{(7)}

where U\mathbf{U} is the eigenvector matrix. The diagonal elements of the Hamiltonian represent the splitting of energy levels. Transitions only occur between specific energy levels, and their probabilities can be computed from

P=U†I^+U,(8)\mathcal{P}=\mathbf{U}^{\dagger}\hat{I}_{+}\mathbf{U}, \tag*{(8)}

where I^+=I^x+iI^y\hat{I}_{+}=\hat{I}_{x}+i\hat{I}_{y}. For 75^{75}As with I=3/2I=3/2,

I^+=(0300002000030000).(9)\hat{I}_{+}= \begin{pmatrix} 0 & \sqrt{3} & 0 & 0 \\ 0 & 0 & 2 & 0 \\ 0 & 0 & 0 & \sqrt{3} \\ 0 & 0 & 0 & 0 \end{pmatrix}. \tag*{(9)}

First, we can compute the 75^{75}As NQR frequency as a function of Bint\mathbf{B}_{\mathrm{int}} with specific Bint\mathbf{B}_{\mathrm{int}} orientations θint\theta_{\mathrm{int}} with respect to the principle axis of EFG. In Figure S5, we show the representative results for θint=0\theta_{\mathrm{int}} = 0, 4545 and 90∘90^\circ, and the colormap indicates the normalized transition probabilities. For EFG principle axis parallel to the internal field (θint=0∘\theta_{\mathrm{int}} = 0^\circ), the energy level splitting and the resonance frequencies are linear with field. On the contrary, for EFG principle axis perpendicular to the internal field (θint=90∘\theta_{\mathrm{int}} = 90^\circ), these dependencies are nonlinear. As field increases, transitions between adjacent energy levels gradually become stronger, while transitions across energy levels weaken rapidly and finally disappear. For θint=45∘\theta_{\mathrm{int}} = 45^\circ, the situation is more complex: transitions between non-adjacent levels occur with significant probability, leading to multiple sub-branches of resonance frequency. The calculated results are then compared with the experiments, and we find that the best fitting parameters are θint≈44∘\theta_{\mathrm{int}} \approx44^\circ and Bint=0.213B_{\mathrm{int}} = 0.213 T, seeing Figure 2(a).

Next, the NMR frequencies (in the presence of external field μ0H=10\mu_{0}H = 10 T) can also be simulated and compared with the experimental, seeing Figure 2(b) and Figure S3. At 10 K, given that the satellite-peak frequencies in single-crystal and polycrystalline NMR are essentially consistent for H⊥c\mathbf{H} \perp c, whereas the quadrupole splitting frequency measured in single-crystal NMR along H∥c\mathbf{H} \parallel c is relatively smaller than that in the polycrystalline case [cf Figure S2], we infer a slight misalignment of the external magnetic field away from the cc-axis. Fitting results indicate an angular deviation of approximately 5.5∘5.5^\circ. Another salient feature is that, from 10 K to 2 K, the quadrupole splitting measured for H⊥c\mathbf{H} \perp c (i.e. νyy\nu_{yy}) increases much faster than that for H∥c\mathbf{H} \parallel c (i.e. νzz′\nu_{zz'}), seeing Figure S3. This suggests the emergence of in-plane anisotropy due to magnetic ordering with q=(0.5,0,0)\mathbf{q} = (0.5, 0, 0), and yields a finite asymmetry parameter η≈0.0102\eta\approx0.0102. To better reconcile the NMR and NQR data, we attempted to fit all resonance peaks using a single νQ\nu_{Q} value; however, this turns out to be not very successful. Hence, we propose that under a strong magnetic field of 10 T, subtle modifications of the electric field gradient may occur, leading to distinct νQ\nu_{Q} values between NMR and NQR measurements. The simulated central peak splitting (Δf\Delta f) for both H∥c\mathbf{H} \parallel c and H⊥c\mathbf{H} \perp c are monotonic with the azimuthal angle of internal field ϕint\phi_{\mathrm{int}} in the range of [0,90∘][0, 90^\circ], and this gives rise to ϕint=26.5∘\phi_{\mathrm{int}} = 26.5^\circ uniquely, seeing Figure S6.

Calculations of hyperfine coupling tensors {#sec:SM V}

There are six cerium neighbors surrounding the As, as shown in Figure S7. Among them, Ce1-4 are nearest neighbors, and Ce5-6 are next-nearest neighbors. In the lattice-coordinate system, the hyperfine coupling tensor of the nearest neighboring Ce1 atom writes as

Figure S7. Local environment of As in CeNiAsO. Only Ce and As atoms are shown for clarity. There are six cerium neighbors surrounding the As, denoted as Ce1-6. The transferred hyperfine coupling relies on Ce-As orbital hybridization. (a) The principle axes of the transferred hyperfine tensors AiA_i of the As sites from the nearest-neighbor Ce (Take Ce1 as an example). (b) The principle axes of the transferred hyperfine tensors AiA_i of the As sites from the next-nearest neighbor Ce (as exemplified by Ce5).

A1=(AaaAabAacAbaAbbAbcAcaAcbAcc)(10)A_1=\begin{pmatrix} A_{aa} & A_{ab} & A_{ac} \\ A_{ba} & A_{bb} & A_{bc} \\ A_{ca} & A_{cb} & A_{cc} \end{pmatrix} \tag*{(10)}

By symmetry, the tensors for the other three nearest-neighbor sites (Ce2-4) are

A2=(Aaa−Aab−Aac−AbaAbbAbc−AcaAcbAcc),A3=(AaaAab−AacAbaAbb−Abc−Aca−AcbAcc),A4=(Aaa−AabAac−AbaAbb−AbcAca−AcbAcc).(11)\mathbf{A}_2=\begin{pmatrix} A_{aa} & -A_{ab} & -A_{ac} \\ -A_{ba} & A_{bb} & A_{bc} \\ -A_{ca} & A_{cb} & A_{cc} \end{pmatrix},\quad \mathbf{A}_3=\begin{pmatrix} A_{aa} & A_{ab} & -A_{ac} \\ A_{ba} & A_{bb} & -A_{bc} \\ -A_{ca} & -A_{cb} & A_{cc} \end{pmatrix},\quad \mathbf{A}_4=\begin{pmatrix} A_{aa} & -A_{ab} & A_{ac} \\ -A_{ba} & A_{bb} & -A_{bc} \\ A_{ca} & -A_{cb} & A_{cc} \end{pmatrix}. \tag*{(11)}

For the next-nearest neighbors (Ce5-6), the hyperfine coupling tensors are

A5=(BaaBabBacBbaBbbBbcBcaBcbBcc),A6=(BaaBab−BacBbaBbb−Bbc−Bca−BcbBcc).(12)\mathbf{A}_5=\begin{pmatrix} B_{aa} & B_{ab} & B_{ac} \\ B_{ba} & B_{bb} & B_{bc} \\ B_{ca} & B_{cb} & B_{cc} \end{pmatrix},\quad \mathbf{A}_6=\begin{pmatrix} B_{aa} & B_{ab} & -B_{ac} \\ B_{ba} & B_{bb} & -B_{bc} \\ -B_{ca} & -B_{cb} & B_{cc} \end{pmatrix}. \tag*{(12)}

According to the previous neutron-scattering results [33], in the commensurate AFM phase with q=(0.5,0,0)\mathbf{q}=(0.5,0,0), the moments m1=−m2=−m3=m4\mathbf{m}_1=-\mathbf{m}_2=-\mathbf{m}_3=\mathbf{m}_4; m5x=m1xm_{5x}=m_{1x}, and m5y=−m1ym_{5y}=-m_{1y}. Putting these together, the internal field at As site can be obtained,

Bint=(4Aacmz+2Baamx−2Babmy, 2Bbamx−2Bbbmy, 4Acamx±2Bccmz),(13)\mathbf{B}_{\mathrm{int}}=(4A_{ac}m_z+2B_{aa}m_x-2B_{ab}m_y,\ 2B_{ba}m_x-2B_{bb}m_y,\ 4A_{ca}m_x\pm2B_{cc}m_z), \tag*{(13)}

where “+/−” denotes that the upper and lower Ce layers in a single CeO slab have the same/opposite mzm_z components, viz m1z=±m5zm_{1z}=\pm m_{5z}.

In the bond coordinate (cf Figure S7), the tensors A~i\tilde{\mathbf{A}}_i are diagonal, e.g.

A~1=(A⊥1000A⊥2000A∥),A~5=(B⊥1000B⊥2000B∥),(14)\tilde{\mathbf{A}}_1=\begin{pmatrix} A_{\perp1} & 0 & 0 \\ 0 & A_{\perp2} & 0 \\ 0 & 0 & A_{\parallel} \end{pmatrix},\quad \tilde{\mathbf{A}}_5=\begin{pmatrix} B_{\perp1} & 0 & 0 \\ 0 & B_{\perp2} & 0 \\ 0 & 0 & B_{\parallel} \end{pmatrix}, \tag*{(14)}

where the elements A∥A_{\parallel} and B∥B_{\parallel} mean the hyperfine coupling along the Ce-As bonding, while A⊥1A_{\perp1}, A⊥2A_{\perp2}, B⊥1B_{\perp1} and B⊥2B_{\perp2} are the components for perpendicular to the bonds. Ai\mathbf{A}_i and A~i\tilde{\mathbf{A}}_i are connected and converted through coordinate transformation,

Ai=R−1A~iR,(15)\mathbf{A}_i=\mathbf{R}^{-1}\tilde{\mathbf{A}}_i\mathbf{R}, \tag*{(15)}

where R\mathbf{R} is the coordinate transformation matrix. In particular, for Ce5 and Ce6, the two coordinates are equivalent, therefore,

A5=A~5=(B⊥1000B⊥2000B∥).(16)\mathbf{A}_5=\tilde{\mathbf{A}}_5=\begin{pmatrix} B_{\perp1} & 0 & 0 \\ 0 & B_{\perp2} & 0 \\ 0 & 0 & B_{\parallel} \end{pmatrix}. \tag*{(16)}

For A1\mathbf{A}_1, it can be obtained via rotating A~1\tilde{\mathbf{A}}_1 by approximately −60∘-60^\circ about the (−1 1 0)(-1\ 1\ 0) direction, i.e.,

A1=(9A⊥116+A⊥216+3A∥83A⊥116+3A⊥216−3A∥836A⊥116−6A⊥216−6A∥83A⊥116+3A⊥216−3A∥8A⊥116+9A⊥216+3A∥86A⊥116−36A⊥216+6A∥836A⊥116−6A⊥216−6A∥86A⊥116−36A⊥216+6A∥83A⊥18+3A⊥28+A∥4).(17)\mathbf{A}_1= \begin{pmatrix} \frac{9A_{\perp1}}{16}+\frac{A_{\perp2}}{16}+\frac{3A_{\parallel}}{8} & \frac{3A_{\perp1}}{16}+\frac{3A_{\perp2}}{16}-\frac{3A_{\parallel}}{8} & \frac{3\sqrt{6}A_{\perp1}}{16}-\frac{\sqrt{6}A_{\perp2}}{16}-\frac{\sqrt{6}A_{\parallel}}{8} \\ \frac{3A_{\perp1}}{16}+\frac{3A_{\perp2}}{16}-\frac{3A_{\parallel}}{8} & \frac{A_{\perp1}}{16}+\frac{9A_{\perp2}}{16}+\frac{3A_{\parallel}}{8} & \frac{\sqrt{6}A_{\perp1}}{16}-\frac{3\sqrt{6}A_{\perp2}}{16}+\frac{\sqrt{6}A_{\parallel}}{8} \\ \frac{3\sqrt{6}A_{\perp1}}{16}-\frac{\sqrt{6}A_{\perp2}}{16}-\frac{\sqrt{6}A_{\parallel}}{8} & \frac{\sqrt{6}A_{\perp1}}{16}-\frac{3\sqrt{6}A_{\perp2}}{16}+\frac{\sqrt{6}A_{\parallel}}{8} & \frac{3A_{\perp1}}{8}+\frac{3A_{\perp2}}{8}+\frac{A_{\parallel}}{4} \end{pmatrix}. \tag*{(17)}

Considering the tetragonal symmetry, Aaa=AbbA_{aa}=A_{bb}, Baa=BbbB_{aa}=B_{bb}. Therefore, A⊥1=A⊥2=A⊥A_{\perp1}=A_{\perp2}=A_{\perp}, and B⊥1=B⊥2=B⊥B_{\perp1}=B_{\perp2}=B_{\perp}. Eq. (16)-(17) can thus be further simplified.

Refinement of the magnetic structure {#sec:SM VI}

In order to obtain the possible magnetic structure, we need to find out the orientations of each Ce moment - a configuration that can simultaneously satisfy all the existing NMR and NQR results. Here we have to make a few appropriate assumptions. First of all, we assume that the magnetic structure (and also the Bint\mathbf{B}_{\mathrm{int}}) of CeNiAsO is robust to external field up to 10 T, which seems to reasonable because the field dependent magnetization curve M(H)M(H) remains linear and is far away from saturation even for field as high as 58 T, seeing Figure S1. Additional evidence for this can be provided by the field dependent NMR shown in Figure S4, from which we notice that the peak splitting Δf\Delta f does not change much below ∼13\sim13 T.

The Knight shift KK along the principal axis can be expressed in terms of AiA_i and the magnetic susceptibility χ(T)\chi(T),

Kα(T)≈(4Aαα+2Bαα)χ(T),(18)K_{\alpha}(T) \approx(4A_{\alpha\alpha}+2B_{\alpha\alpha})\chi(T), \tag*{(18)}

where α=a,b,c\alpha= a, b, c. Eq. (18) omitted on-site hyperfine interaction to the conduction electron spin, whose effect is much weaker than the localized 4f4f electrons. From the previous NMR experiments, the parameters Ahf,cexp=0.86(2)A_{\mathrm{hf},c}^{\mathrm{exp}} = 0.86(2) T/μB\mu_{\mathrm{B}} and Ahf,abexp=−0.42(9)A_{\mathrm{hf},ab}^{\mathrm{exp}} = -0.42(9) T/μB\mu_{\mathrm{B}} were obtained through Clogston-Jaccarino plot KK vs χ\chi [39]. Neutron scattering gives the magnitude of ordered moment m=0.37(5)m = 0.37(5) μB\mu_{\mathrm{B}} [33], and

mx2+my2+mz2=m2.(19)m_x^2+m_y^2+m_z^2=m^2. \tag*{(19)}

According to the NQR analysis shown in Figure 2(a), we already get Bint=0.213B_{\mathrm{int}} = 0.213 T, polar angle θint=44∘\theta_{\mathrm{int}} = 44^\circ, and azimuthal angle ϕint=26.5∘\phi_{\mathrm{int}} = 26.5^\circ. Therefore,

Bint,x2+Bint,y2+Bint,z2=Bint2,(20)B_{\mathrm{int},x}^2+B_{\mathrm{int},y}^2+B_{\mathrm{int},z}^2=B_{\mathrm{int}}^2, \tag*{(20)}
Bint,x2+Bint,y2=Bint,z2tan⁡2θint,(21)B_{\mathrm{int},x}^2+B_{\mathrm{int},y}^2=B_{\mathrm{int},z}^2\tan^2\theta_{\mathrm{int}}, \tag*{(21)}

and

Bint,y2/Bint,x2=tan⁡2ϕint.(22)B_{\mathrm{int},y}^2/B_{\mathrm{int},x}^2=\tan^2\phi_{\mathrm{int}}. \tag*{(22)}

By solving Eq. (13) and (S13-S18) simultaneously, we can obtain possible hyperfine coupling tensors for different magnetic moment directions characterized by θm\theta_m and ϕm\phi_m. The out-of-plane hyperfine coupling constant Ahf,cA_{\mathrm{hf},c} is imposed as a constraint, whereas the in-plane constant Ahf,abA_{\mathrm{hf},ab} serves as a validation criterion. The theoretical value Ahf,abcalA_{\mathrm{hf},ab}^{\mathrm{cal}} can be calculated from the obtained hyperfine coupling tensor via Eq. (18) and then compared with the experimental Ahf,abexpA_{\mathrm{hf},ab}^{\mathrm{exp}}. The goodness of the fitting is evaluated by log⁡10Rp\log_{10}R_p, where

Rp(θm,ϕm)=(Ahf,abcal−Ahf,abexp)2=[4Aaa(θm,ϕm)+2Baa(θm,ϕm)−Ahf,abexp]2.(23)\begin{aligned} R_p(\theta_m,\phi_m) &= \left(A_{\mathrm{hf},ab}^{\mathrm{cal}}-A_{\mathrm{hf},ab}^{\mathrm{exp}}\right)^2\\ &= \left[4A_{aa}(\theta_m,\phi_m)+2B_{aa}(\theta_m,\phi_m)-A_{\mathrm{hf},ab}^{\mathrm{exp}}\right]^2. \tag*{(23)} \end{aligned}

The optimal parameters (θm,ϕm)(\theta_m,\phi_m) should lead to the minimal log⁡10Rp\log_{10}R_p, as is shown in Figure 2(c).

Raw data of Hall effect {#sec:SM VII}

In Figure S8 we present the raw data of Hall effect of CeNiAsO single crystal for H∥cH \parallel c. Due to the good metallicity of CeNiAsO, the Hall signal is very small. The raw data were smoothed and fitted with great care. At low temperatures well below TN2T_{\mathrm{N2}}, two distinct hysteresis loops are clearly observed in the Hall resistivity ρyx\rho_{yx} upon sweeping the magnetic field upward and downward [Figure S8-Figure S8)]. When approaching TN2T_{\mathrm{N2}}, these anomalies are strongly suppressed, evolving into a weak single-loop response at 5-6 K [Figure S8-Figure S8)]. Such anomalous Hall effect (AHE) dies away for temperature above TN2T_{\mathrm{N2}} [Figure S8], in both of the incommensurate AFM [Figure S8] and paramagnetic [Figure S8] regimes. The systematic temperature evolution indicates that the anomalous Hall response is closely associated with the commensurate AFM phase that is deemed as a pp-wave magnetic state [29] [18, 24, 34].

To extract the AHE component, we express the total Hall resistivity as follows,

ρyx(H)=ρyxO+ρyxA,(24)\rho_{yx}(H) = \rho_{yx}^{\mathrm{O}} + \rho_{yx}^{\mathrm{A}}, \tag*{(24)}

where ρyxO\rho_{yx}^{\mathrm{O}} and ρyxA\rho_{yx}^{\mathrm{A}} are the ordinary and anomalous Hall resistivities, respectively. In the high-field limit where the condition ωcτtr≪1\omega_{\mathrm{c}}\tau_{\mathrm{tr}} \ll1 no-longer holds (ωc\omega_{\mathrm{c}} is cyclotron frequency; τtr\tau_{\mathrm{tr}} is scattering time), ρyxO(H)\rho_{yx}^{\mathrm{O}}(H) becomes superlinear and can be fitted to a superposition of linear (HH) and quadratic (H2H^2) terms [53, 54]. After subtracting the background contribution of ρyxO\rho_{yx}^{\mathrm{O}}, the anomalous contribution ρyxA\rho_{yx}^{\mathrm{A}} can be obtained, as shown in Figure 4(b).

The direction of the spin polarization axis

Tilted coplanar CAFM_z order of CeNiAsO

Figure S9. Tilted coplanar CAFMz_z order of CeNiAsO.

To determine whether the magnetic moments form a non-coplanar spin configuration, we analyze the geometrical relation among the 4 kinds of magnetic moments in the CAFMz_z order of CeNiAsO:

m1=(mx, my, −mz),m2=(−mx, −my, mz),m5=(mx, −my, mz),m7=(−mx, my, −mz),(25)\begin{aligned} \mathbf{m}_1 &= (m_x,\,m_y,\,-m_z),\\ \mathbf{m}_2 &= (-m_x,\,-m_y,\,m_z),\\ \mathbf{m}_5 &= (m_x,\,-m_y,\,m_z),\\ \mathbf{m}_7 &= (-m_x,\,m_y,\,-m_z), \tag*{(25)} \end{aligned}

with mx=∣m∣cos⁡θmcos⁡ϕmm_x = \lvert m\rvert\cos\theta_m \cos\phi_m, my=∣m∣cos⁡θmsin⁡ϕmm_y = \lvert m\rvert\cos\theta_m \sin\phi_m, and mz=∣m∣sin⁡θmm_z = \lvert m\rvert\sin\theta_m. Note that θm\theta_m is with respect to the ab plane. The normal vector (n\mathbf{n}) of the plane spanned by m1\mathbf{m}_1, m2\mathbf{m}_2, and m5\mathbf{m}_5 can be obtained from their cross product:

n=m2×m5=(0, −2mxmz, −2mxmy).(26)\mathbf{n} = \mathbf{m}_2 \times\mathbf{m}_5 = (0,\,-2m_xm_z,\,-2m_xm_y). \tag*{(26)}

The remaining magnetic moment satisfies

n⋅m7=(0, −2mxmz, −2mxmy)⋅(−mx, my, −mz)=0,(27)\mathbf{n} \cdot\mathbf{m}_7 = (0,\,-2m_xm_z,\,-2m_xm_y) \cdot(-m_x,\,m_y,\,-m_z) = 0, \tag*{(27)}

demonstrating that all four magnetic moments lie within the same plane. Therefore, this magnetic configuration is coplanar. The normal direction of the magnetic plane is given by

n^=n∣n∣=(0, mz, my)mz2+my2≈(0, 0.231, 0.973).(28)\hat{\mathbf{n}} = \frac{\mathbf{n}}{\lvert\mathbf{n}\rvert} = \frac{(0,\,m_z,\,m_y)}{\sqrt{m_z^2 + m_y^2}} \approx(0,\,0.231,\,0.973). \tag*{(28)}

This magnetic canting establishes a new spin plane, whose normal direction is rotated from the crystallographic c axis to n^\hat{\mathbf{n}}.

References

  1. [1][1–11]
  2. [3][3–8]
  3. [11][11–13]
  4. [14][14–17]
  5. [19][19–23]
  6. [24][24–26]
  7. [28]Yamada, R., Birch, M. T., Baral, P. R., Okumura, S., Nakano, R., Gao, S., Ezawa, M., Nomoto, J., Masell, J., Ishihara, Y., Kolincio, K. K., Belopolski, I., Sagayama, H., Nakao, H., Ohishi, T., Kiyanagi, R., Nakajima, Y., Tokura, T.-. h ., Arima, Y., … Hirschberger, M. (2025). A metallic p-wave magnet with commensurate spin helix. Nature, 646, 837.
  8. [29]M. Zhao, W.-W. Yang, X. Guo, H.-G. Luo, and Y. Zhong, Altermagnetism in heavy-fermion systems: Mean-field study on the Kondo lattice, Phys. Rev. B 111, 085145 (2025).DOI
  9. [49]N. J. Curro, Hyperfine interactions in the heavy fermion CeMIn₅ systems, New J. Phys. 8, 173 (2006).DOI
  10. [50]N. J. Curro, B.-L. Young, J. Schmalian, and D. Pines, Scaling in the emergent behavior of heavy-electron materials, Phys. Rev. B 70, 235117 (2004).DOI
  11. [51]G. Xu, W. Ming, Y. Yao, X. Dai, S.-C. Zhang, and Z. Fang, Doping-dependent phase diagram of LaOMAs (M=V–Cu) and electron-type superconductivity near ferromagnetic instability, EPL 82, 67002 (2008).DOI
  12. [52]F. Ronning, E. Bauer, T. Park, N. Kurita, T. Klimczuk, R. Movshovich, A. Sefat, D. Mandrus, and J. Thompson, Ni₂X₂ (X=pnictide, chalcogenide, or B) based superconductors, Physica C 469, 396 (2009).DOI
  13. [53]S. Nair, S. Wirth, M. Nicklas, J. L. Sarrao, J. D. Thompson, Z. Fisk, and F. Steglich, Precursor State to Unconventional Superconductivity in CeIrIn₅, Phys. Rev. Lett. 100, 137003 (2008).pubmed.ncbi.nlm.nih.gov/18517989
  14. [54]X. He, Y. Li, Y. Ge, H. Zeng, S.-J. Song, J. Liu, S. Zou, Z. Wang, Y. Li, W. Ding, J. Dai, G.-H. Cao, X.-X. Zhang, T. Zhai, G. Xu, and Y. Luo, Rich unconventional Hall effects in a single quasi-kagome Kondo Weyl semimetal candidate Ce₃TiSb₅, Commun. Mater. 6, 206 (2025).DOI

Paper details

vlnc:W_vs48ps47
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents