betaFeedback

WorksPhysics and Astronomy

Neutron diffraction in MnSb2O6: Magnetic and structural domains in a helicoidal polar magnet with coupled chiralities

Abstract

MnSb2_{2}O6_{6} is based on the structural chiral PP321 space group #150 where the magnetic Mn2+^{2+} moments (S=5/2S=5/2, L≈0L\approx 0) order antiferromagnetically at TN=12T_\mathrm{N}=12 K. Unlike the related iron based langasite (Ba3_3NbFe3_3Si2_2O14_{14}) where the low temperature magnetism is based on a proper helix characterized by a time-even pseudoscalar magnetic' chirality, the Mn$^{2+}$ ions in MnSb$_{2}$O$_{6}$ order with a cycloidal structure at low temperatures, described instead by a time-even vector magnetic' polarity. A tilted cycloidal structure has been found [M. Kinoshita et al. Phys. Rev. Lett. 117, 047201 (2016)] to facilitate ferroelectric switching under an applied magnetic field. In this work, we apply polarized and unpolarized neutron diffraction analyzing the magnetic and nuclear structures in MnSb2_{2}O6_{6} with the aim of understanding this magnetoelectric coupling. We find no evidence for a helicoidal magnetic structure with one of the spin envelope axes tilted away from the cycloidal cc-axis. However, on application of a magnetic field ∥\parallel c⃗\vec{c} the spin rotation plane can be tilted, giving rise to a cycloid-helix admixture that evolves towards a distorted helix (zero cycloidal component) for fields great than ≈\approx 2 T. We propose a mechanism for the previously reported ferroelectric switching based on coupled structural and magnetic chiralities requiring only an imbalance of structural chiral domains.

Introduction

Coupling magnetism and ferroelectricity would allow the possibility for controlling electric polarization with a magnetic field and magnetic moments with an electric field. However, ferroelectricity and magnetism originate from disparate microscopic mechanisms1, and such multiferroic materials are rare. Despite these challenges, complex coupling schemes have been intensively studied and sought after for decades, motivated by the interesting physics and promising multifunctional applications2–5. For example, non-centrosymmetric magnetic ordering can break inversion symmetry and induce an improper electric polarization via the inverse antisymmetric Dzyaloshinskii-Moriya (DM) interaction6,7. This is the case in cycloidal magnets, often stabilized by the competition of exchange interactions, and where the sense of rotation of the spins can be linked to the sign of the electric polarization8–10. Additional interest can be found in materials having a crystallographic chirality that may naturally stabilize a non-centrosymmetric magnetic structure. For example, iron based langasite (Ba3_3NbFe3_3Si2_2O14_{14} [11–15]) crystallizes in the chiral, trigonal space group P321P321, and the structural chirality is coupled to the chirality of its magnetic helix through symmetric Heisenberg exchanges. Recently, a magnetic field induced long-wavelength spin spiral modulation has been discovered in this compound giving rise to an electric polarization.16

MnSb2_2O6_6 hosts magnetic manganese with a valence of Mn2+^{2+} giving a high spin S=5/2S = 5/2 and orbitally quenched L≈0L \approx0 moment.17 Analogous to iron based langasite, magnetic interactions between isolated MnO6_6 octahedra (Figure 1(a)) follow chiral super-super-exchange (SSE) pathways (Mn-O-O-Mn) along the cc-axis (Figure 1(b)-(Figure 1c)). Magnetization measurements find long-range magnetic order below TN≈12T_\mathrm{N} \approx12 K and some evidence for short-range correlations below 200 K has been provided.18,19 Below TNT_\mathrm{N}, Mn magnetic moments rotate within the (acac)-plane. Nearest neighbor moments arranged on triangular motifs in the (abab)-plane are dephased by 120° and follow a cycloidal modulation with propagation vector k=(0,0,0.182)\mathbf{k} = (0, 0, 0.182), as shown in Figure 1(d). The sense of rotation of the spins along the cc-axis and within a basal triangle can be described by so-called vector chiralities, VC\mathbf{V}_\mathrm{C} and VT\mathbf{V}_\mathrm{T}, respectively, which we later show to be related to well-defined, generic ‘magnetic’ parameters ηC\eta_\mathrm{C} and ηT\eta_\mathrm{T} that couple directly to the crystal chirality, σ\sigma. By analogy with various other cycloidal magnets,8,9 MnSb2_2O6_6 can hold an electric polarization.

Nuclear and magnetic structures of chiral MnSb$_2$O$_6$

Figure 1. (a) Nuclear structure of chiral MnSb2_2O6_6. The structural chirality can be defined as the helical winding of the Mn-O-O-Mn super-super-exchange (blue lines) with respect to the cc-axis: it is clockwise for left-handed structure (b) and anticlockwise for right-handed structure (c). Figures made on VESTA.22 (d) Cycloidal magnetic structure. (e) Tilted cycloid model. Figures made on MAG2POL.[23]

Magnetic domains can exist when the symmetry of the paramagnetic phase is lowered by the ordered magnetic structure. These domains are energetically equivalent, and related by symmetry operators which are broken during the phase transition.20 In the case of MnSb2_2O6_6, threefold symmetry is broken by the cycloidal magnetic structure, hence at least three cycloidal domains are expected below TNT_N. Additional magnetic domains related to the signs of ηC\eta_C and ηT\eta_T will also form, as discussed later. These magnetic domains are polar, so could be manipulated by an external electric field.17 Later on, Kinoshita et al. found the cycloids to be tilted away from the cc-axis, with one of the main axes of the spin envelope parallel to [1ˉ10][\bar{1}10],21 as shown in Figure 1(e). The tilt of this alternative ground state magnetic structure was reported to be necessary to explain a macroscopic electric polarization evidenced by measuring pyroelectric current, confirming the multiferroic character of MnSb2_2O6_6.

In this paper, we apply unpolarized and polarized neutron diffraction to show that there is no clear evidence of this tilted model for the magnetic ground state. We do find evidence for a mixture of chiral structural domains

in our single-crystal. Through magnetic diffraction under an applied magnetic field, we show that it is possible to manipulate the magnetic structure with small magnetic fields. Finally we propose an alternative mechanism for the appearance of electric polarization, based on the DM interaction under an external magnetic field and coupled chiralities. This mechanism does not require a tilted cycloid ground state for ferroelectric domain switching in an applied magnetic field.

This paper is based upon five sections including this introduction. After describing the materials preparation and neutron instrumentation used for diffraction studies in § 2, we define twinning afforded by the P321 symmetry and various structural and magnetic chiralities in MnSb2_2O6_6 in Section III. In § 4, we describe the experimental results and finish in § 7 with a phenomenological theory for ferroelectric switching previously observed.

Experimental details

In this section we describe the materials preparation and neutron scattering experiments used to study both powders and single crystals of MnSb2_2O6_6.

Materials preparation

Materials preparation followed the procedure outlined in Ref. 24. Powders of MnSb2_2O6_6 were prepared by mixing stoichiometric amounts of pure MnCO3_3 and Sb2_2O3_3. After mixing through grinding, the powder was pressed into a pellet and heated up to 1000°C with the process repeated with intermediate grinding. It was found that heating the pellet to higher temperatures introduced the impurity Mn2_2Sb2_2O7_7. Single crystals of MnSb2_2O6_6 were prepared using the flux method. Starting ratios for single-crystal growth were (by weight) 73% of flux V2_2O5_5, 20% of polycrystalline MnSb2_2O6_6 and 7% of B2_2O3_3. The powder was ground and pressed into a pellet and flame sealed in a quartz ampoule under vacuum (less than 10−410^{-4} Torr). B2_2O3_3 was used to lower the melting temperature of the V2_2O5_5 flux. Back filling the ampoules with ≈200\approx200 mTorr of Argon gas was found to noticeably improve crystal sizes. Quartz ampoules were then heated to 1000°C at a rate of 60°C/hour and soaked at this temperature for 24 hours. The furnace was then cooled to 700°C at a rate of 2°C/hour and held for 24 hours, before it was switched off and allowed to cool to room temperature. Crystal sizes in the range from a few millimeters to nearly a centimeter were obtained through this procedure.

Neutron diffraction

The nuclear and magnetic structures of MnSb2_2O6_6 were studied on the four-circle diffractometers D9 [25] and D10 [26] (ILL, Grenoble) using a single crystal sample of dimensions ∼3×2×0.2 mm3\sim3 \times2 \times0.2\ \mathrm{mm}^{3} (hexagonal shape). On D9, a monochromatic neutron beam of wavelength λ=0.836 A˚\lambda= 0.836\ \mathrm{\AA} was selected by the (220) reflection of a Cu monochromator in transmission geometry. On D10, a wavelength of λ=2.36 A˚\lambda= 2.36\ \mathrm{\AA} was selected from a vertically focusing pyrolytic graphite monochromator. The same single crystal was previously characterized using the CRYOgenic Polarization Analysis Device (CRYOPAD)[27] on the spin-polarized hot neutron diffractometer D3 [28] (ILL, Grenoble) using a wavelength λ=0.85 A˚\lambda= 0.85\ \mathrm{\AA} selected by the (111) reflection of a Cu2_2MnAl Heusler monochromator. The good quality of the single crystal was confirmed by neutron Laue diffraction. Powder diffraction was performed on the high-intensity two-axis diffractometer D20 [29] (ILL, Grenoble) on ∼17 g\sim17\ \mathrm{g} of powder, using a wavelength λ=2.41 A˚\lambda= 2.41\ \mathrm{\AA} selected by the (002) reflection of a pyrolitic graphite HOPG monochromator in reflection position. Single crystal diffraction under an external magnetic field was performed on the cold triple-axis spectrometer RITA-2 (now replaced by CAMEA, SINQ, Villigen), using a horizontal cryo-magnet MA7 with wavelength λ=4.9 A˚\lambda= 4.9\ \mathrm{\AA} monochromated with a vertically focused pyrolitic graphite PG002 monochromator. The use of a horizontal field was necessary given the need to apply the magnetic field along the cc-axis, parallel to the magnetic propagation vector which is kinematically constrained to be in the horizontal plane.

While conventional powder and single crystal neutron diffraction was used in this work, we relied as well heavily on the use of less standard techniques: Schwinger scattering and spherical neutron polarimetry, to gain extra information into the complex nuclear and magnetic structures of MnSb2_2O6_6. We briefly outline the theory of these techniques here before discussing the structural properties specific to MnSb2_2O6_6.

Schwinger scattering for Structural Handedness

In the reference frame of a moving neutron, the electric field of a non-centrosymmetric crystal creates an effective magnetic field which couples to the neutron spin. This neutron spin-orbit interaction results in a polarization-dependant scattering known as Schwinger scattering[30] which can be used as a probe of the structural handedness of the crystal.[31, 32]

In the local coordinates, where z^∥ki×kf\hat{z} \parallel\mathbf{k}_i \times\mathbf{k}_f is perpendicular to the scattering plane, the asymmetric Schwinger structure factor is given by:[32]

FSO(Q)=iγr02mempFE(Q)cot⁡(θ)σ^⋅z^(1)F_{\mathrm{SO}}(\mathbf{Q}) = i\frac{\gamma r_0}{2}\frac{m_e}{m_p}F_E(\mathbf{Q})\cot(\theta)\hat{\sigma}\cdot\hat{z} \tag*{(1)}

where γ\gamma is the neutron gyromagnetic ratio, r0r_0 is the electron classical radius, θ\theta is the scattering angle, σ^\hat{\sigma} is the neutron spin operator, and FE(Q)F_E(\mathbf{Q}) is the electrostatic unit cell structure factor:

FE(Q)=∑j[Zj−fj(Q)]e−Wj(Q)e−iQ⋅rj(2)F_E(\mathbf{Q}) = \sum_j [Z_j-f_j(\mathbf{Q})]e^{-W_j(\mathbf{Q})}e^{-i\mathbf{Q}\cdot\mathbf{r}_j} \tag*{(2)}

with ZjZ_j, fj(Q)f_j(\mathbf{Q}) and Wj(Q)W_j(\mathbf{Q}), respectively, the atomic number, the X-ray atomic form factor, and the Debye-Waller factor of the jj-th atom of the unit cell. The small ratio between the electron and proton mass me/mpm_e/m_p leads to a weak Schwinger scattering cross-section ∝γr02memp=−1.46×10−4\propto\frac{\gamma r_0}{2}\frac{m_e}{m_p}=-1.46\times10^{-4} in units of 10−12 cm10^{-12}\ \mathrm{cm} (nuclear scattering length).[31] For a nuclear reflection, the contribution from Schwinger scattering adds to the nuclear structure factor FNF_N leading to an intensity:

I±∝∣FN∣2+∣FSO∣2±I(3)I^{\pm} \propto|F_N|^2+|F_{\mathrm{SO}}|^2\pm\mathcal{I} \tag*{(3)}

where I=2pRe⁡(FNFSO∗)\mathcal{I}=2p\operatorname{Re}(F_NF_{\mathrm{SO}}^*) is an interference term and pp is the polarization of the incident beam along ±z^\pm\hat{z}. Measuring both intensities with the incident neutron beam polarized along ±z^\pm\hat{z} allows us to compute the flipping ratio:

R=∣FN∣2+∣FSO∣2+I∣FN∣2+∣FSO∣2−I.(4)R=\frac{|F_N|^2+|F_{\mathrm{SO}}|^2+\mathcal{I}}{|F_N|^2+|F_{\mathrm{SO}}|^2-\mathcal{I}}. \tag*{(4)}

The flipping ratio technique, very well known to the magnetization density community, affords the extraction of the weak Schwinger scattering and to distinguish structural twins in a single crystal discussed below. Indeed, each twin would lead to a different flipping ratio. For example the flipping ratio is inverted for an inversion twin.

Spherical Neutron Polarimetry for Magnetic Handedness

Spherical neutron polarimetry (SNP) is a powerful technique used to determine complex magnetic structures and magnetic chiralities (an example illustrated in Ref. [33]), which plainly demonstrates the benefits of using polarized neutrons.[34, 35] The idea is to measure in three orthogonal directions the final polarization of the neutrons, for incident neutrons polarized along each of the three directions. This allows to measure a 3×33\times3 polarization matrix given by:

Pif=nif−nifˉnif+nifˉ(5)P_{if}=\frac{n_{if}-n_{i\bar{f}}}{n_{if}+n_{i\bar{f}}} \tag*{(5)}

where i,f=x,y,zi,f=x,y,z denotes the polarization direction of the incident and scattered neutrons in the local coordinates where x^\hat{x} is parallel to the scattering vector, z^\hat{z} is perpendicular to the scattering plane and y^\hat{y} completes this right-handed set, nifn_{if} and nˉif\bar{n}_{if} are the number of scattered neutrons with spin parallel and antiparallel to ff-direction. The theoretical cross-sections for polarized neutrons are given by the Blume-Maleev equations.[36, 37] For a purely elastic magnetic reflection and a perfectly polarized neutron beam the polarization matrix PifP_{if} is given by:

(−∣M⊥∣2−Mch∣M⊥∣2+Mch00−Mch∣M⊥∣2∣M⊥y∣2−∣M⊥z∣2∣M⊥∣22Re⁡{M⊥yM⊥z∗}∣M⊥∣2−Mch∣M⊥∣22Re⁡{M⊥zM⊥y∗}∣M⊥∣2∣M⊥z∣2−∣M⊥y∣2∣M⊥∣2)(6)\begin{pmatrix} \frac{-|M_{\perp}|^2-M_{\mathrm{ch}}}{|M_{\perp}|^2+M_{\mathrm{ch}}} & 0 & 0 \\ \frac{-M_{\mathrm{ch}}}{|M_{\perp}|^2} & \frac{|M_{\perp y}|^2-|M_{\perp z}|^2}{|M_{\perp}|^2} & \frac{2\operatorname{Re}\{M_{\perp y}M_{\perp z}^{*}\}}{|M_{\perp}|^2} \\ \frac{-M_{\mathrm{ch}}}{|M_{\perp}|^2} & \frac{2\operatorname{Re}\{M_{\perp z}M_{\perp y}^{*}\}}{|M_{\perp}|^2} & \frac{|M_{\perp z}|^2-|M_{\perp y}|^2}{|M_{\perp}|^2} \tag*{(6)} \end{pmatrix}

While unpolarized single crystal diffraction is only sensitive to the amplitude squared of the magnetic interaction vector ∣M⊥∣2|M_{\perp}|^2, its components are accessible through SNP. Also, Mch=2Im⁡{M⊥yM⊥z∗}M_{\mathrm{ch}}=2\operatorname{Im}\{M_{\perp y}M_{\perp z}^{*}\} gives information on the magnetic chirality.

Theory and Definitions

Given the complexity of the magnetic and nuclear structure in MnSb2_2O6_6, we outline in this section the various definitions for the structural and magnetic chiralities and twins. This is required for presenting powder and single crystal neutron diffraction results discussed below.

Definition of Twins

Twinning occurs when two or more single crystals of the same species are intergrown in different orientations, related by the so-called twin laws.[38, 39] When the twin operation belongs to the point group of the lattice but not to the point group of the crystal, the twinning is called twinning by merohedry. In this case, the crystal lattices of the two twins overlap in both direct and reciprocal space.[40] As all Bravais lattices are centrosymmetric, the non-centrosymmetric basis of MnSb2_2O6_6 (space group P321P321) is expected to form inversion twins. Furthermore, the absence of improper rotations in P321P321 (e.g. mirror plane) implies the inversion twins will have opposite structural chiralities (known as enantiomorphs). It follows that the reciprocal lattice of one twin is the inverse of the other, i.e. (hkl)→(hˉkˉlˉ)(hkl)\rightarrow(\bar{h}\bar{k}\bar{l}). In the case of the P321P321 space group additional merohedral twinning associated with twofold rotation around the cc-axis, i.e. (hkl)→(hˉkˉl)(hkl)\rightarrow(\bar{h}\bar{k}l), is also allowed.[41] We note that these twins related by twofold rotation have the same chirality. Combining the twofold rotation with the inversion twin leads to a fourth twin (hklˉ)(hk\bar{l}). In order to distinguish the structural chirality of these four possible merohedral twins, we will subsequently use the labels L(hkl)L(hkl), L(hˉkˉl)L(\bar{h}\bar{k}l), R(hˉkˉlˉ)R(\bar{h}\bar{k}\bar{l}) and R(hklˉ)R(hk\bar{l}), where L(R) refers to the left(right)-handedness of the crystal structure, defined by the helical

winding of the Mn-O-O-Mn super-super-exchange pathways in Figure 1(b)-(c).

Definition of Structural and Magnetic Chiralities

In crystallography, chirality can be defined as the property of an object “being non-superposable by pure rotation and translation on its image formed by inversion through a point”.[42] On the other hand, the definition of magnetic chirality is not obvious because the time reversal operation (T) has to be considered in addition to parity operation (P). Barron proposed a more general definition: “True chirality is possessed by systems that exist in two distinct enantiomeric states that are interconverted by space inversion but not by time reversal combined with any proper spatial rotation.”[43] In this meaning only helical magnetic structures are truly chiral.[35, 44] However, spin “chirality” is commonly used to refer to the sense of rotation of the spins with respect to a crystallographic reference often taken to be an oriented link between two atomic sites, say rijr_{ij}, and can thus describe the spin configuration of cycloidal structures and triangular networks.[45]

The cross-product of two spins at sites ii and jj defines a vector chirality

Vij=Si×Sj(7)V_{ij}=S_i\times S_j \tag*{(7)}

which is a T-even axial vector (i.e. P-even), changing sign on exchange of indices i↔ji\leftrightarrow j. This chirality vector is well-defined by providing the oriented link between two spins.

For clarification and to understand our diffraction data, we redefine the vectors introduced in Ref. 17 in the context of MnSb2_2O6_6. To do this, we consider an orthonormal basis R=(x^,y^,z^)\mathbf{R}=(\hat{x},\hat{y},\hat{z}) where x^\hat{x} lies along the aa-axis, z^\hat{z} along the cc-axis and y^\hat{y} completes the right-handed basis set of vectors. We define the spin rotation plane using two vectors u^\hat{u} and v^\hat{v}, where we take u^=x^\hat{u}=\hat{x} in the following. In order to account for a tilt of the spin rotation plane we introduce θ\theta as the tilt angle about u^\hat{u} such that v^=[0,−sin⁡θ,cos⁡θ]\hat{v}=[0,-\sin\theta,\cos\theta]. We note that in our analysis, u^\hat{u} could take any direction in the (ab)(ab)-plane, and the definition of the tilt angle θ\theta can be generalized. By definition, any two spins SiS_i and SjS_j, lie within the uvuv-plane, so their cross product must lie along ±n^=u^×v^=[0,−cos⁡θ,−sin⁡θ]\pm\hat{n}=\hat{u}\times\hat{v}=[0,-\cos\theta,-\sin\theta] (Figure 2). Note that when θ=0\theta=0, the spins rotate in a plane containing z^\hat{z} and we obtain a proper cycloid [Figure 1(d)]. When θ=90∘\theta=90^\circ, the spins rotate in a plane perpendicular to z^\hat{z} defining a proper helix, as reported in Ba3_3NbFe3_3Si2_2O14_{14}. Intermediate values of θ\theta give a generic helicoidal structure that can be decomposed into an admixture of helical and cycloidal parts.

Image not extracted

Figure 2. u^\hat{u} and v^\hat{v} are the main axis of the helicoidal spin structure envelope. Any cross product of spins lies along n^\hat{n}. AA and PmP_{\mathrm{m}} lie along u^\hat{u}.

The spin configuration within a basal triangle of Mn2+^{2+} ions is described by the classical vector chirality @references៌មាន

VT=13(S1×S2+S2×S3+S3×S1)V_{\mathrm{T}}=\frac{1}{3}(S_{1}\times S_{2}+S_{2}\times S_{3}+S_{3}\times S_{1}) where the indices are given by right hand rule around the axial vector z^\hat{z} defined as parallel to the positive cc-axis. Similarly, a vector chirality VC=Sα×SβV_{\mathrm{C}}=S_{\alpha}\times S_{\beta} can be introduced to describe the rotation of the spins along the cc-axis, relatively to the polar vector rαβr_{\alpha\beta} where α\alpha and β\beta refer to two neighboring layers along the cc-axis. We can now redefine the axial vector AA and the polar vector PmP_{\mathrm{m}} used to characterize the cycloidal magnetic structure of MnSb2_{2}O6_{6} in Ref. 17 as

A=z^×VT=[ηTcos⁡θ,0,0]Pm=rαβ×VC=[ηCcos⁡θ,0,0](8)\begin{aligned} A&=\hat{z}\times V_{\mathrm{T}}=[\eta_{\mathrm{T}}\cos\theta,0,0]\\ P_{\mathrm{m}}&=r_{\alpha\beta}\times V_{\mathrm{C}}=[\eta_{\mathrm{C}}\cos\theta,0,0] \tag*{(8)} \end{aligned}

where ηT\eta_{\mathrm{T}} and ηC\eta_{\mathrm{C}} are T-even P-even and T-even P-odd parameters associated with the magnetic configuration within the (ab)(ab)-plane triangular motifs and on propagation along the cc-axis, respectively. Importantly, both parameters are conserved upon rotation by θ\theta. We can similarly redefine the triangular chirality ϵT\epsilon_{\mathrm{T}} and spin helicity ϵH\epsilon_{\mathrm{H}} used to characterize the helical magnetic structure of Ba3_{3}NbFe3_{3}Si2_{2}O14_{14} in Ref. 11 as

ϵT=z^⋅VT=−ηTsin⁡θϵH=rαβ⋅VC=−ηCsin⁡θ(9)\begin{aligned} \epsilon_{\mathrm{T}}&=\hat{z}\cdot V_{\mathrm{T}}=-\eta_{\mathrm{T}}\sin\theta\\ \epsilon_{\mathrm{H}}&=r_{\alpha\beta}\cdot V_{\mathrm{C}}=-\eta_{\mathrm{C}}\sin\theta \tag*{(9)} \end{aligned}

These expressions allow us to use ηT\eta_{\mathrm{T}}, ηC\eta_{\mathrm{C}}, and θ\theta to parametrize a generic helicoidal magnetic structure. The vector quantities of Eq. (8) capture the cycloidal component projected into the (ac)(ac)-plane, and the scalar quantities of Eq. (9) capture the helical part projected into the (ab)(ab)-plane. We note that the helical part is odd in θ\theta, while the cycloidal part is even.

Magnetic structure description

Considering the two perpendicular unit vectors u^\hat{u} and v^\hat{v} that define the spin rotation plane, we can describe the magnetic moment for a Mn atom at site j=(1,2,3)j=(1,2,3) on a given triangular motif, in layer α\alpha (along the cc-axis), and with an angle ϕαj\phi_{\alpha j}:

μαj=Mucos⁡ϕαju^+Mvsin⁡ϕαjv^ϕαj=2πηCkzα+ηT(j−1)2π3(10)\begin{aligned} \mu_{\alpha j}&=M_{u}\cos\phi_{\alpha j}\hat{u}+M_{v}\sin\phi_{\alpha j}\hat{v}\\ \phi_{\alpha j}&=2\pi\eta_{\mathrm{C}}k_{z}\alpha+\eta_{\mathrm{T}}(j-1)\frac{2\pi}{3} \tag*{(10)} \end{aligned}

MuM_{u} and MvM_{v} describe the shape of the ellipse (circular for Mu=MvM_{u}=M_{v}), kzk_{z} is the vertical component of the propagation vector k=(0,0,kz)\boldsymbol{k}=(0,0,k_{z}). ηC\eta_{\mathrm{C}} and ηT\eta_{\mathrm{T}} describe the sense of rotation of the spins respectively along the positive cc-axis, and within a Mn2+^{2+} triangle, following the definitions above.

The first magnetic structure proposed in Ref. 17 has u^\hat{u} lying along the crystallographic aa-axis, and v^\hat{v} along the cc-axis. This magnetic structure preserves the twofold symmetry (magnetic space group B21′1^{\prime}). This is not the case in the model proposed in Ref. 21, with u^∥[11ˉ0]\hat{u}\parallel[1\bar{1}0], which lowers the symmetry of the magnetic space group to P11′1^{\prime} owing to the breaking of the twofold symmetry. However, the tilting of v^\hat{v} from the cc-axis reported in Ref. 21, by an angle θ\theta, is also allowed in the B21′1^{\prime} space group as long as the twofold symmetry is preserved. Both models consider the presence of threefold domains, and for each of them, the magnetic moments in Eq. (10) are transformed by rotating u^\hat{u} and v^\hat{v} by 120° around the cc-axis.

Invariant from Heisenberg interactions

If we consider a Heisenberg Hamiltonian with seven SSE pathways, the classical mean-field energy can be derived as a function of the propagation vector kz>0k_{z}>0:

E0(k)=−12(J1+2J2)+J4cos⁡(2πηCkz)+JRcos⁡(2πηCkz+ηT2π3)+JLcos⁡(2πηCkz−ηT2π3)(11)E_{0}(k)=-\frac{1}{2}(J_{1}+2J_{2})+J_{4}\cos(2\pi\eta_{\mathrm{C}}k_{z}) +J_{\mathrm{R}}\cos\left(2\pi\eta_{\mathrm{C}}k_{z}+\eta_{\mathrm{T}}\frac{2\pi}{3}\right) +J_{\mathrm{L}}\cos\left(2\pi\eta_{\mathrm{C}}k_{z}-\eta_{\mathrm{T}}\frac{2\pi}{3}\right) \tag*{(11)}

where JR=J3+2J6J_{\mathrm{R}}=J_{3}+2J_{6} sums the right-handed interactions and JL=J5+2J7J_{\mathrm{L}}=J_{5}+2J_{7} sums the left-handed interactions. Minimizing Eq. (11) with respect to the propagation vector gives for the ground state:

tan⁡(2πηCkz)=ηT3(JR−JL)JR+JL−2J4(12)\tan(2\pi\eta_{\mathrm{C}}k_{z})=\frac{\eta_{\mathrm{T}}\sqrt{3}(J_{\mathrm{R}}-J_{\mathrm{L}})}{J_{\mathrm{R}}+J_{\mathrm{L}}-2J_{4}} \tag*{(12)}

As left-handed and right-handed exchange paths are switched between the enantiomorphs, the quantity JR−JLJ_{\mathrm{R}}-J_{\mathrm{L}} changes sign upon inversion symmetry. Thus taking the DFT values for the exchange constants from Ref. 17, a sign analysis of Eq. (12) gives the invariant:

σηCηT=+1(13)\sigma\eta_{\mathrm{C}}\eta_{\mathrm{T}}=+1 \tag*{(13)}

where σ=+1\sigma=+1 for a left-handed crystal structure (L), and σ=−1\sigma=-1 for a right-handed crystal structure (R). This is similar to iron langasite, where the structural chirality is linked to the pair of magnetic chiralities readily obtained by substituting θ=90∘\theta= 90^\circ into Eq. (9).11

Results and Discussion

Having outlined the experimental neutron diffraction techniques and the definitions relevant for the discussion of MnSb2_2O6_6, we now present the experimental results. We first discuss the nuclear and then the low temperature magnetic structure.

Nuclear structure

Single crystal neutron diffraction

For a given Bragg reflection Q\mathbf{Q}, the inversion twin will scatter with a nuclear structure factor FN(−Q)F_{\mathrm{N}}(-\mathbf{Q}). In absence of resonant scattering, Friedel’s law is valid, and both twins will scatter the same nuclear intensity ∝∣FN(Q)∣2\propto|F_{\mathrm{N}}(\mathbf{Q})|^2. Inversion twins are thus indistinguishable by unpolarized neutrons. On the other hand, twofold twins reveal different nuclear structure factors depending on the (hkl)(hkl) indices so their domain population can be refined using unpolarized neutrons if the appropriate Bragg reflections are measured. We collected intensities from 430 nuclear reflections at 50 K on the four-circle diffractometer D9. Rocking scans show nicely resolved Bragg peaks, with a full width at half-maximum ∼0.4∘\sim0.4^\circ in ω\omega. The data were refined using Fullprof.[46] The parameters scale, extinction, atomic positions, displacements, as well as domain population for twofold twins were refined, showing that our single crystal has no twofold twins as one nuclear intensity domain was refined to a population of 0.991(3). Our refinement results (detailed in Table I) agree with the known crystal structure previously studied by neutron powder diffraction at room temperature.18

As the threefold symmetry from paramagnetic P321P321 space group is broken by the cycloidal structure in the magnetic phase,17 this could relate to a symmetry lowering of the nuclear space group below TNT_{\mathrm{N}}. To investigate the possibility of a structural distortion coinciding with TNT_{\mathrm{N}}, a separate set of 318 Bragg reflections was measured at 2 K (below TN≈12T_{\mathrm{N}} \approx12 K), leading to 75 inequivalent groups of reflections. If the crystal symmetry is reduced, the equivalent reflections in P321P321 should no longer be equivalent within each group of reflections. For example, reflections (h,k,l)(h,k,l), (k,−h−k,l)(k,-h-k,l) and (−h−k,h,l)(-h-k,h,l) are related by threefold symmetry along the cc-axis and are thus equivalent in P321P321. In the case where the threefold symmetry is broken, these three kind of reflections are no more equivalent. In addition, three structural domains rotated by 120∘120^\circ are expected. If these threefold domains are exactly equally-populated, the intensities scattered from each domain will average out, making them impossible to be distinguished from a single threefold symmetric domain. Else, the intensities of reflections within a group of P321P321-equivalent reflections will differ. The internal RR-factor is Rint=4.1%R_{\mathrm{int}} = 4.1\% for the data reduction in P321P321 symmetry, which indicates that the differences of intensities for P321P321-equivalent reflections are not measurable given our setup. In addition, the data was refined including the threefold domains in P1P1 symmetry, but this did not significantly improve the refinement. At the end 845 nuclear reflections were measured at 2 K, and were well refined in P321P321 space group as shown in Figure 3(b), in comparison to the 50 K refinement in Figure 3(a). From this, there is no significant evidence of breaking of P321P321 symmetry below Néel temperature. Detailed refinement results for both temperatures are listed in Table I.

Image not extracted

Figure 3. Observed versus calculated intensities in P321 space group for nuclear reflections measured at (a) 50 K, (b) 2 K.

Schwinger scattering

To characterize the chiral domains, Schwinger scattering was measured on D3 on nine Bragg reflections at T=3T = 3 K on the same single crystal characterized on D9, for which only two out of four possible twins were measured to be present as explained above. Absolute indexation was determined on D9 by comparing the nuclear intensities of Bragg reflections. This was not done on D3 (as only flipping ratios were measured), so the reflections can be indexed with a twofold rotation between D3 and D9 experiments. Thus, either {L(hkl),R(hˉkˉl)}\{L(hkl), R(\bar{h}\bar{k}l)\}, or {L(hˉkˉl),R(hkl)}\{L(\bar{h}\bar{k}l), R(hkl)\} are the twins present (with the indexation from D3 experiment).

The experimental flipping ratios are then fitted to a linear combination of the theoretical ones (calculated with the atomic positions from D9 data refinement at 2 K), as shown in Figure 4. The best fit is obtained considering the twins L(hˉkˉl)L(\bar{h}\bar{k}l) and R(hkl)R(hkl), giving 0.54(2) of left-handed structural domain, and 0.46(2) of right-handed domain. The error bars are quite large in this experiment, but the flipping ratios being close but different than 1 within uncertainties indicate that there is a mixture of chiral inversion twins in the crystal. For an enantiopure, the flipping ratios should be close to one set of predicted flipping ratios, which shows much more pronounced asymmetries as exemplified by the (511) and (153) reflections. The results are thus different from enantiopure Ba3_3NbFe3_3Si2_2O14_{14} single crystals which were previously studied.[32] [11, 13]

Image not extracted

Figure 4. Measured flipping ratios are fitted to a linear combination of the theoretical flipping ratios for two structural twins.

Transmission Polarized Optical Microscopy

Chiral structural domains in a single crystal can also be measured with a polarized optical microscope. Due to the optical activity in chiral compounds, the polarization plane of a linearly polarized light is rotated after traveling through the sample.[47] The sense of rotation depends on the handedness of the considered domains, which can be distinguished by observing the transmitted light through an analyzer.[48, 49]

T=50T = 50 KMeasured, independent, observations with equivalent reflections: 430, 406, 44
Rint=8.78%R_{\mathrm{int}} = 8.78\%RF=4.87%R_{\mathrm{F}} = 4.87\%RBragg=4.69%R_{\mathrm{Bragg}} = 4.69\%χ2=1.31\chi^2 = 1.31
a=b=8.7835(81)a = b = 8.7835(81) Åc=4.7238(58)c = 4.7238(58) Å
AtomsWyckoffxxyyzzBisoB_{\mathrm{iso}} (Å2^2)Occ.
Mn3e3e0.6319(3)0.00000.00000.19(3)1
Sb11a1a0.00000.00000.00000.06(3)1
Sb22d2d0.33330.66670.5059(4)0.04(3)1
Sb33f3f0.3050(3)0.00000.50000.09(2)1
O16g6g0.1046(3)0.8917(3)0.7626(2)0.24(2)1
O26g6g0.4711(2)0.5891(2)0.7286(2)0.19(2)1
O36g6g0.2258(3)0.7804(3)0.2805(2)0.16(2)1
T=2T = 2 KMeasured, independent, observations with equivalent reflections: 845, 529, 423
Rint=4.09%R_{\mathrm{int}} = 4.09\%RF=5.27%R_{\mathrm{F}} = 5.27\%RBragg=5.40%R_{\mathrm{Bragg}} = 5.40\%χ2=1.37\chi^2 = 1.37
a=b=8.7907(19)a = b = 8.7907(19) Åc=4.7176(10)c = 4.7176(10) Å
AtomsWyckoffxxyyzzBisoB_{\mathrm{iso}} (Å2^2)Occ.
Mn3e3e0.6329(3)0.00000.00000.30(3)1
Sb11a1a0.00000.00000.00000.16(3)1
Sb22d2d0.33330.66670.5061(5)0.09(3)1
Sb33f3f0.3050(2)0.00000.50000.09(2)1
O16g6g0.1047(2)0.8920(3)0.7628(2)0.27(1)1
O26g6g0.4710(2)0.5889(2)0.7285(2)0.25(2)1
O36g6g0.2253(3)0.7799(2)0.2804(2)0.23(2)1

Table 1. Structural parameters of MnSb2_2O6_6 single crystal measured on D9, refined with Fullprof[46] within nuclear space group P321 (No. 150)

A different sample of MnSb2_2O6_6, synthesized following the same procedure described in § 2 A, was observed under a transmission polarized optical microscope. The directions of the polarizer and analyzer are shown in blue and red in Figure 5(a)-(Figure 5b), forming an angle θ=90±3∘\theta= 90 \pm3^\circ. These images show several domains with opposite chirality. The contrast between neighboring domains is reverted by rotating the analyzer from θ=93∘\theta= 93^\circ to θ=87∘\theta= 87^\circ because the polarization plane of the transmitted light is rotated in the opposite sense for opposite chirality domains in the sample. Figure 5(c) shows the difference of intensity between Figure 5(a) and Figure 5(b), clearly revealing the chiral areas in the single crystal. Given the same chemical synthesis, our other single crystals, including the one studied under neutron diffraction, are likely to have a similar behavior. They are expected to be a mixture of chiral structural domains, which is consistent with our Schwinger scattering analysis described above.

Image not extracted

Figure 5. Transmission polarized optical microscopy images of a single crystal of MnSb2_2O6_6: for different angles between the polarizer (P) and analyzer (A) in (a) and (b). (c) Images substracted, showing the chiral domains in the sample.

Magneto-structural effects

Neutron powder diffraction was performed on D20 from 2.5 K to 89.5 K. The nuclear structure was refined sequentially as a function of temperature using Fullprof.[46] While no symmetry breaking of the P321 paramagnetic space group was evidenced by our studies, as discussed above, structural changes induced by the phase transition are visible from the powder diffraction data refinement. Figure 6(a) shows the refined volume of the unit cell as a function of temperature. The volume decreases sharply under TN≈12T_\mathrm{N} \approx12 K, demonstrating a deviation from the linear thermal expansion of the unit cell upon magnetic ordering. Actually, this results from the contraction of both aa and cc lattice constants. Similarly, changes in bond distances are caused by magneto-elastic effects, as shown in Figure 6(b) for the distance between Mn atom (in purple) and symmetry equivalent O1 atoms (in red). We note that the unit cell volume shows some anomalies in Figure 6(a) around 3 K and 10 K. We have over-plotted the different diffraction patterns and could

Refinement results from D20

Figure 6. Refinement results from D20. Temperature dependence of: (a) the unit cell volume, (b) the bond length between Mn (in purple) and symmetry equivalent O1 atoms (in red). TN≈12T_{\mathrm{N}} \approx12 K is shown in dashed gray lines.

not observe any shift in the peaks positions. We think that these jumps are numerical artifacts rather than real lattice parameters shifts.

Magnetic structure

Order parameter

Neutron powder diffraction is not sensitive to the direction of the magnetic moments in the (abab)-plane, and neither to the magnetic chiralities. Yet the magnitude of the magnetic moments can be refined from D20 powder diffraction data, as a function of temperature. The cycloid was constrained to be circular (Mu=MvM_u=M_v) and the refined moments are shown in Figure 7. The data in the critical region (88 K <T<12< T < 12 K) are fitted to a power law ∝(T−TN)β\propto(T-T_{\mathrm{N}})^{\beta}, with the critical exponent fixed to β=0.369\beta=0.369 (solid red curve) as expected for the nonfrustrated 3D Heisenberg model,[50] and to β=0.25\beta=0.25 (dashed blue curve) measured for iron langasite13 and XYXY-like stacked-triangular magnets.[51] The critical behavior near TN=11.94(1)T_{\mathrm{N}}=11.94(1) K is in agreement with the 3D Heisenberg model as suggested previously in Ref. 18. Therefore MnSb2_2O6_6 does not have the same universality class as iron langasite and other layered-triangular magnets.

Refined magnetic moments from D20

Figure 7. Refined magnetic moments from D20 as a function of temperature, fitted to a power law ∝(T−TN)β\propto(T-T_{\mathrm{N}})^{\beta} with the critical exponent β\beta fixed for 3D Heisenberg model (solid red curve) and for 2D XYXY model (dashed blue curve).

Unpolarized single crystal diffraction

From the invariant derived in Eq. (13) (σηCηT=1\sigma\eta_{\mathrm{C}}\eta_{\mathrm{T}}=1), a given structural chirality σ\sigma is compatible with two pairs of magnetic configurations (ηC,ηT)(\eta_{\mathrm{C}},\eta_{\mathrm{T}}). We can label the structural and magnetic configurations as σ(ηC,ηT)\sigma(\eta_{\mathrm{C}},\eta_{\mathrm{T}}), which gives four possibilities L(1, 1), L(−1-1, $-1),R(), R(-1,1),R(1,, 1), R(1,-1).L(1,1)andL(). L(1, 1) and L(-1,,-1$) configurations lead to the same magnetic intensities, and R(−1-1, 1), R(1, −1-1) are the respective configurations of their inversion twins, as ηC\eta_{\mathrm{C}} is P-odd and ηT\eta_{\mathrm{T}} P-even from Eq. (8).

Magnetic intensities of inversion twins satisfy Friedel’s law, so the four configurations are undistinguishable by unpolarized neutrons. However, as mentioned above, twofold structural twins can exist in the P321 space group, leading to a different set of nuclear and magnetic intensities (see Table II).

Twinσ=ηCηT\sigma=\eta_{\mathrm{C}}\eta_{\mathrm{T}}∣FN∣2|F_{\mathrm{N}}|^2∣M⊥∣2|M_{\perp}|^2RR
L(hklhkl)+1+1N1N_1M1M_1R1R_1
L(hˉkl\bar{h}kl)+1+1N2N_2M2M_2R2R_2
R(hˉkˉl\bar{h}\bar{k}l)−1-1N1N_1M1M_1R3R_3
R(hklˉhk\bar{l})−1-1N2N_2M2M_2R4R_4

Table II. Summary of the possible twins and their sensitivity to nuclear (∣FN∣2|F_{\mathrm{N}}|^2) and magnetic diffraction (∣M⊥∣2|M_{\perp}|^2), and Schwinger scattering (flipping ratio RR). Different subscripts denote different values. The twins present in our single crystal are highlighted in red.

In previous studies, unpolarized neutron single crystal diffraction data were refined with a mixture of two sets of calculated magnetic intensities, attributed to two chiral structural domains. In light of the present study, one should actually assign these two sets of intensities to at least two twofold domains, with a potential further mixture of chiral domains to which the experiment was not sensitive. In Ref. 17, the single crystal neutron diffraction magnetic refinement shows a 0.8(1):0.2(2) domain fraction of the calculated intensities, which corresponds to a fraction 0.8 of twins {L(hkl),R(hˉklˉ)}\{\mathrm{L}(hkl),\mathrm{R}(\bar{h}k\bar{l})\}, and 0.2 of twins {L(hˉkl),R(hklˉ)}\{\mathrm{L}(\bar{h}kl),\mathrm{R}(hk\bar{l})\}. In absence of a method (Schwinger scattering or anomalous x-ray scattering) sensitive to the inversion twins, one cannot conclude on the population of all four domains. A similar issue arose in Ref. 21, where only one set of magnetic intensities was found and attributed to an enantiopure crystal, but could actually include a mixture of a twin and its chiral inversion twin.

The same single crystal characterized on D3 and D9 was measured on D10. The magnetic structure was refined using Mag2Pol[23] (cross-checked with Fullprof,[46] giving similar results), with 256 magnetic reflections collected at 2 K. The scale and extinction parameters are refined using 145 nuclear reflections (40 inequivalent, giving RF=4.88%R_{\mathrm{F}} = 4.88\%). A single domain in terms of magnetic intensities was found, meaning the absence of twofold structural twins and confirming our results from D9. These intensities are consistent with two twins related by inversion symmetry, shown in red in Table II, which can be distinguished by Schwinger scattering (see § 4 A 2). Extinction parameters can be significantly different for nuclear and magnetic reflections, due to multiple magnetic domains having smaller sizes than the structural domains[52]. This is the case from our refinement, where the extinction parameters refined with the magnetic intensities are found smaller than the one refined with the nuclear intensities. To keep a consistent comparison between the magnetic structure models, the extinction parameters were set to zero for the magnetic refinement described below.

Nameu^\hat{u}MuM_uMvM_vθ\theta (°)p1p_1p2p_2p3p_3RFR_{\mathrm{F}} (%)
Aa^\hat{a}4.5(1)4.7(1)010019.26
Ba^\hat{a}5.7(1)3.7(1)00.400.20(3)0.40(3)15.29
Ca^\hat{a}5.6(3)3.8(3)9(28)0.400.20(5)0.40(3)15.31
D[11ˉ0][1\bar{1}0]5.7(1)3.7(1)00.270.27(3)0.46(3)15.29
E[11ˉ0][1\bar{1}0]5.9(2)3.8(3)15(14)0.280.25(4)0.47(4)15.26

Table 3. Refined parameters obtained for non-tilted and tilted cycloidal models.

The refinement results using different magnetic structure models labeled from A to E are listed in Table III. While including the threefold domains (A→B) with populations p1p_1, p2p_2, and p3p_3 improves the goodness of fit, there is no observable difference between models with the in-plane main axis u^\hat{u} of the cycloid along the aa-axis and along [11ˉ0][1\bar{1}0] (B→D). Similarly, allowing a tilt around the aa-axis (B→C), and around [11ˉ0][1\bar{1}0] (D→E) does not significantly improve the fit. This is because the in-plane direction u^\hat{u} of the spin rotation plane, and the tilt angle θ\theta are correlated with the magnetic domain fractions, which makes no much difference in terms of goodness of fit between models B, C, D and E. Our best fit with the model considered in Ref. 21 is obtained with a tilt angle θ=+15(14)∘\theta= +15(14)^\circ (Figure 8), compared to previously found θ=18(5)∘\theta= 18(5)^\circ. However, two equi-populated tilt domains with θ=±18(5)\theta= \pm18(5) were considered in Ref. 21 while in our refinement, a single tilt domain θ>0\theta> 0 was more consistent. Based on our single crystal diffraction data, we however do not observe a significant improvement in the resulting fit with inclusion of a tilt in the magnetic structure.

Observed versus calculated intensities for magnetic reflections

Figure 8. Observed versus calculated intensities for magnetic reflections measured at 2 K.

Spherical neutron polarimetry

SNP was performed on D3, using the same experimental setup as for the Schwinger experiment with the exception of a 3^3He spin filter necessary for the polarization analysis of the final neutron beam. The full polarization matrices of five magnetic Bragg reflections were measured at T=3T = 3 K. CRYOPAD[27] is used to protect the sample from any external magnetic fields, and to select independently the initial and final polarization directions of the neutrons. In the case of MnSi2_2O6_6, SNP is sensitive to the threefold magnetic domains and the cycloidal parameter ηC\eta_{\mathrm{C}}, while the triangular parameter ηT\eta_{\mathrm{T}} can not be distinguished. The measured polarization matrices were fitted using Mag2Pol[23] to a linear combination of the possible polarization matrices as Pmeas=∑iαiPiP_{\mathrm{meas}} = \sum_i \alpha_i P_i with αi\alpha_i, PiP_i, the population and polarization matrix of the ii-th magnetic domain.

The magnetic moments were first refined in the ac-plane (u^=a^\hat{u} = \hat{a} and v^=c^\hat{v} = \hat{c}). In the absence of a nuclear contribution to the scattered intensity, SNP is not sensitive to the size of the magnetic moments. Therefore, since in this experiment purely magnetic satellites are investigated, only the ratio e=Mv/Mue = M_v/M_u, known as the ellipticity, can be deduced. Considering the model proposed in Ref. 17, threefold and ηC=±1\eta_{\mathrm{C}} = \pm1 domain populations are refined, leading to six polarization matrices to consider. The refinement results for this model are shown in Table IV. The cycloids are found elliptical along the basal direction with e=0.92(1)e = 0.92(1) and χr2=7.14\chi^2_{\mathrm{r}} = 7.14. The population for the third domain with ηC=+1\eta_{\mathrm{C}} = +1 was fixed to 0 in order to avoid fit divergence and unphysical results.

ηC\eta_C113z+3_z^+3z−3_z^-Sum
+1+10.20(1)0.20(1)0.20(1)0.20(1)000.40(2)0.40(2)
−1-10.09(1)0.09(1)0.09(1)0.09(1)0.42(2)0.42(2)0.60(2)0.60(2)
Sum0.29(1)0.29(1)0.28(1)0.28(1)0.42(2)0.42(2)11
χr2\chi_r^27.147.14
ee0.92(1)0.92(1)

Table IV. Refined parameters for the non-tilted cycloid model.

The SNP data were then fitted to the tilted cycloid model proposed in Ref. 21. In this case, the positive and negative tilt of the angle θ\theta have to be taken account because it changes the rotation plane and leads to different polarization matrices. This doubles the number of polarization matrices to include, resulting in 12 domain populations to refine (threefold ×{ηC=±1}×±θ\times\{\eta_C = \pm1\} \times\pm\theta). The vectors u^\hat{u} and v^\hat{v} of each of these 12 magnetic domains are related by symmetry operators and the absolute values of MuM_u are constrained to be the same for each magnetic domain (the same for MvM_v), so that each magnetic domain keeps the same magnetic moment size. This also constrains the absolute value of the tilt angle to be the same for θ>0\theta> 0 and θ<0\theta< 0 domains. The results are shown in Table V. Again, the domains returning unphysical values in a first refinement step were fixed to zero in the following. The positive tilt domains are predominant, with a population of 0.89(4), giving θ=14(7)∘\theta= 14(7)^\circ which is consistent with the best fit from the D10 data. However, this tilted model only slightly improves the goodness of fit to χr2=6.68\chi_r^2 = 6.68.

ηC\eta_Cθ\theta113z+3_z^+3z−3_z^-Sum
−1-1++0.08(1)0.08(1)0.32(3)0.32(3)000.40(3)0.40(3)
+1+1−-0.01(2)0.01(2)0.07(2)0.07(2)0.04(2)0.04(2)0.12(3)0.12(3)
−1-1−-00000000
+1+1++0.14(1)0.14(1)000.35(2)0.35(2)0.49(2)0.49(2)
Sum0.23(2)0.23(2)0.39(4)0.39(4)0.39(2)0.39(2)11
χr2\chi_r^26.686.68
ee0.96(8)0.96(8)
θ\theta14(7)∘14(7)^\circ

Table V. Refined parameters for the tilted cycloid model.

Our diffraction study of the magnetic structure of MnSb2_2O6_6 evidences a mixture of threefold magnetic domains and magnetic polarities. In the absence of a substantial improvement in RR-factors on inclusion of the model with in-plane moments along [11ˉ0][1\bar{1}0], we propose that the model with moments along a^\hat{a} is the ground state because it has a higher symmetry (not breaking twofold symmetry). The tilt is still allowed by symmetry, as pointed out in Section III C. Thus the possibility of a tilted cycloidal structure is not ruled out by symmetry considerations our experiments. In § 7 we discuss the appearance of a macroscopic electric polarization reported in Ref. 21 and propose a different mechanism without invoking the need of a tilted cycloid ground state.

Magnetic field dependence

Before discussing the electric polarization we finally investigate the magnetic field response of the magnetic structure in MnSb2_2O6_6 owing to its importance in any domain switching. Magnetic phase transitions induced by low magnetic fields (below 2 T) were observed previously in MnSb2_2O6_6 bulk magnetization measurements.19,21 This was explained by a very small anisotropy stabilizing the cycloidal magnetic ground state, which can be easily overcome by applying a magnetic field, changing the spin structure to another state. In order to complement these macroscopic measurements, neutron diffraction was performed on RITA-2 using a horizontal magnetic field, on a single crystal of MnSb2_2O6_6, aligned in the (H,0,L)(H,0,L) scattering plane such that the magnetic field could be aligned either along the cc or aa-axes. A single high intensity magnetic peak, Q=(1,0,1)−k\mathbf{Q}=(1,0,1)-\mathbf{k} was scanned over a range of temperatures (between 1.75 and 11.5 K) and magnetic fields (between 0 and 5 T), applied parallel and perpendicular to the cc-axis. Unpolarized neutrons are sensitive to the magnetic moments perpendicular to the scattering vector Q\mathbf{Q}, so a change of the measured intensity can be a direct proof of a change in the magnetic structure.

Figure 9 shows the results for the magnetic field applied along the cc-axis. Figure 9(a)-(Figure 9c) show reciprocal space scans along the LL direction of the Q=(1,0,1)−k\mathbf{Q}=(1,0,1)-\mathbf{k} magnetic peak at T=1.75T=1.75 K. The intensities are fitted to a skewed Gaussian:

Magnetic-field scans and field dependence of the propagation vector and integrated intensities

Figure 9. The magnetic field is applied along the cc-axis. (a)–(c) Scans at T=1.75T = 1.75 K along the (00L)(00L) direction for different values of magnetic field. The mean position of the skewed Gaussian fits are shown in dashed lines and depend on the applied field. (d) Summary of the field dependence of the propagation vector at T=1.75T = 1.75 K. (e) Integrated intensities of the magnetic peak Q=(1,0,1)−kQ = (1, 0, 1) - \mathbf{k} as a function of the magnetic field. The zero-field intensity is subtracted from each respective curve for a clearer comparison of the field-induced intensity increase.

I(L)∝{1+erf⁡[γ(L−L0)σ2]}exp⁡{−(L−L0)22σ2}(14)I(L) \propto\left\{1+\operatorname{erf}\left[\frac{\gamma(L-L_0)}{\sigma\sqrt{2}}\right]\right\}\exp\left\{-\frac{(L-L_0)^2}{2\sigma^2}\right\} \tag*{(14)}

where γ\gamma is the skewness parameter, σ\sigma and L0L_0 are the Gaussian standard deviation and center. The mean values of the skew Gaussian are shown in dashed gray lines and change with the magnetic field. A nuclear reflection (201) was also monitored as a function of the magnetic field and does not present any shift along the LL direction. This means that the shift of the magnetic peak Q=(1,0,1)−k\mathbf{Q}=(1,0,1)-\mathbf{k} is caused by a change of the propagation vector k\mathbf{k} and not of the lattice parameter cc. This is summarized in Figure 9(d) where the propagation vector evolution can clearly be observed until a threshold magnetic field (around 2 T). Magneto-elastic effects can be induced by a change in the magnetic structure as illustrated in the change in bond distances at TNT_N discussed above and shown in Figure 6. A change in the bond distances would result in a change in the strength of the exchange constants, which consequently change the propagation vector in order to minimize the ground state energy, from Eq. (12).

In Figure 9(e), the integrated intensities are displayed as a function of the magnetic field, for different temperatures. The zero-field intensity is subtracted from each respective curve, in order to compare the data on the same scale as the magnetic intensity diminishes when the temperature increases. The integrated intensities increase with the magnetic field until a threshold value (different for each temperature) and then remain constant. For a cycloidal magnetic ground state, when no external field is applied, one main axis of the spin ellipse lies in the (ab)(ab)-plane, and the other one along the cc-axis. Applying a magnetic field H∥cH \parallel c is expected to flop the spin rotation plane from a cycloid to a helix, where the latter is oriented perpendicular to the magnetic field. The gradual increase of the intensity shows that the cycloid plane is continuously tilted from the cc-axis. For T=1.75T = 1.75 K, the observed intensities (with a magnetic field <2< 2 T) of reflection Q=(1,0,1)−kQ = (1, 0, 1) - \mathbf{k} match with calculated intensities for a circular helicoidal magnetic structure (with the main axis u^∥a\hat{u} \parallel a and v^\hat{v} rotated around u^\hat{u} by an angle θ\theta, see Section III B) as shown in Figure 10. The observed intensities were normalized to the intensity at 1.75 K, while the calculated intensities were normalized to the intensity at θ=90∘\theta= 90^\circ. The matching of these normalized intensities indicates that the spin structure goes from a nearly pure cycloid state to a nearly pure helix state which is analogous to the zero field magnetic structure of iron based langasite. At T=1.75T = 1.75 K, the tilt angle of the spin rotation plane seems to increase linearly with the magnetic field, whereas the tilt starts at higher magnetic field for higher temperatures.

Normalized integrated intensity and simulated magnetic intensity as a function of tilt angle

Figure 10. (black points) Normalized integrated intensity of the measured magnetic peak Q=(1,0,1)−kQ = (1, 0, 1) - \mathbf{k} as a function of the magnetic field applied parallel to the cc-axis at T=1.75T = 1.75 K. (red curve) Simulated magnetic intensity as a function of the tilt angle θ\theta of the spin rotation plane from the cc-axis.

The results are different when the magnetic field is rotated by 90° and applied in the abab-plane. In this case, the in-plane main axis of the cycloid will tend to be perpendicular to the magnetic field and the magnetic domains are simply reoriented in the abab-plane. As mentioned above, magnetic diffraction is not very sensitive to the direction of the in-plane main axis, because the intensities of the magnetic peaks do not change significantly between two directions of this axis. This is especially true for the magnetic peak Q=(1,0,1)−kQ = (1, 0, 1) - \mathbf{k}, where the measured intensities are constant as a function of the magnetic field (Figure 11(a)). Contrary to previous thermodynamic magnetization measurements,19 the in-plane reorientation of the spin structure cannot be detected in this experiment. The propagation vector also remains constant, within error, as a function of the magnetic field (Figure 11(b)–(Figure 11e)), indicating the absence of measurable magneto-elastic effects in this case. We note that the difference in L0L_0 values between the two different field directions is an experimental artefact resulting from not being able to refine a zero offset in the scattering angle. This is due to only being able to measure a single Bragg peak owing to kinematic constraints imposed by the horizontal magnetic field geometry.

Magnetic field dependence of the magnetic peak

Figure 11. The magnetic field is applied perpendicular to the cc-axis. (a)–(c) Scans at T=1.75T = 1.75 K along the (00L)(00L) direction for different values of magnetic field. The mean position of the skewed Gaussian fits are shown in dashed lines and remain constant. (d) Summary of the field dependence of the propagation vector at T=1.75T = 1.75 K. (e) Integrated intensities of the magnetic peak Q=(1,0,1)−k\mathbf{Q} = (1, 0, 1) - \mathbf{k} as a function of the magnetic field. The zero-field intensity is subtracted from each respective curve for a clearer comparison of the data.

Theory for an Electric Polarization

In their work, Kinoshita et al. (Ref. 21) have measured the pyroelectric current in a single crystal of MnSb2_2O6_6 along u^∥[11ˉ0]\hat{\mathbf{u}} \parallel[1\bar{1}0] under a magnetic field rotating in the (11ˉ0)(1\bar{1}0) plane. An electric polarization was measured for the magnetic field slightly off the (ab)(ab)-plane and was attributed to the selection of a tilted polar domain. This polarization is reversed when the magnetic field is applied on the other side of the (ab)(ab)-plane, favoring the opposite tilted polar domain. This mechanism relied on the tilted cycloid model considered as the ground state in MnSb2_2O6_6. In this section we discuss a phenomenological theory for the domain switching observed in Ref. 21 under the application of a magnetic field in the absence of a zero-field tilt as discussed in our diffraction results outlined above.

As is the case for many compounds having a cycloidal magnetic structure, MnSb2_2O6_6 is predicted to hold an electric polarization through the inverse DM interaction9 or spin-current induced8 mechanisms which predicts an electric polarization P\mathbf{P} given by:

P∝rij×(Si×Sj)(15)\mathbf{P} \propto\mathbf{r}_{ij} \times(\mathbf{S}_i \times\mathbf{S}_j) \tag*{(15)}

which couples to the magnetic polarity Pm\mathbf{P}_{\mathrm{m}} in the phenomenological free energy through a term ∝λPm⋅P\propto\lambda\mathbf{P}_{\mathrm{m}} \cdot\mathbf{P}. Therefore the electric polarization P\mathbf{P} lies parallel or antiparallel to the magnetic polarity Pm\mathbf{P}_{\mathrm{m}} depending on the sign of the coupling constant λ\lambda.1,7

Using our definitions in Eq. (8) and Eq. (9), we can build trilinear invariants based upon Heisenberg exchange interactions from Eq. (13):

σϵHϵT=σηCηTsin⁡2(θ)\sigma\epsilon_H\epsilon_T = \sigma\eta_C\eta_T \sin^2(\theta)
σPm⋅A=σηCηTcos⁡2(θ)(16)\sigma\mathbf{P}_{\mathrm{m}} \cdot\mathbf{A} = \sigma\eta_C\eta_T \cos^2(\theta) \tag*{(16)}

Again, this shows the equivalence between the scalar and vector coupling schemes from iron langasite and MnSb2_2O6_6, and also the mixture of both with the spin rotation plane tilt angle θ\theta. These invariants imply that the polarization P\mathbf{P}, does not change sign with θ\theta, based on Heisenberg exchanges alone.

However, we can consider a uniform DM interaction with DαβD_{\alpha\beta} parallel to the cc-axis. DαβD_{\alpha\beta} is a T-even axial vector that changes sign on exchange of indices. Its sign will also depend upon the structural chirality σ\sigma, hence we can write Dαβ∝σrαβD_{\alpha\beta} \propto\sigma r_{\alpha\beta} where rαβr_{\alpha\beta} is the bond vector between spin sites α\alpha and β\beta along the cc-axis. Following Eq. (9), the magnetic energy is then given by

EDM=Dαβ⋅(Sα×Sβ)E_{\mathrm{DM}} = D_{\alpha\beta} \cdot(\mathbf{S}_{\alpha} \times\mathbf{S}_{\beta})
∝σrαβ⋅VC\propto\sigma r_{\alpha\beta} \cdot\mathbf{V}_{C}
∝σηCsin⁡θ(17)\propto\sigma\eta_C \sin\theta \tag*{(17)}

Therefore, for a given structural domain with a fixed σ\sigma, when the sign of θ\theta is inverted (through the application of a magnetic field) the uniform DM interaction will favor a change of sign of ηC\eta_C which in turn results in the sign of Pm\mathbf{P}_{\mathrm{m}} being inverted, from Eq. (8). This will change the direction of the electric polarization P\mathbf{P}. The only condition for having a non-zero polarization is an imbalance of structural chiral domains for a given tilt angle θ\theta. This mechanism does not need the magnetic ground state to be tilted. Indeed, the ground state could be a pure cycloid stabilized by Heisenberg exchanges, where the anisotropy overcomes this small DM term. When an external magnetic field is applied slightly out of the (ab)(ab)-plane, this would overcome the anisotropy and tilt the spin rotation plane. In this case the DM term would lift the degeneracy of ±ηC\pm\eta_C domains, and give rise to a non-zero electric polarization for a given structural domain. We note that the DM term is allowed owing to the large distortion of the oxygen octahedra surrounding the Mn2+\mathrm{Mn}^{2+} ions.[53]

From our diffraction data under magnetic field, we know that a small magnetic field (around 2 T) is sufficient to reorient the spin rotation plane perpendicular to the magnetic field, which is consistent with a small single-ion anisotropy in our compound and is consistent with the values used in Ref. 21 in their macroscopic measurement of electric polarization. However, Ref. 21 has considered the tilted cycloid ground state as essential for selecting the polar domains with an external magnetic field applied perpendicularly to the spin rotation plane. This explanation does not work in the case that magnetic domains with polarity ±ηC\pm\eta_C have the exact same populations, because the overall polarization would compensate. As ±ηC\pm\eta_C domains are degenerate from Heisenberg model, our mechanism based on a uniform DM interaction is more general. In particular and in the context of MnSb2O6\mathrm{MnSb}_2\mathrm{O}_6, this mechanism does not depend on a tilted ground state, and requires an imbalance in structural chiral domains and the underlying coupling between magnetic and structural chiralities.

Conclusion

In this study, we have performed a combination of unpolarized and polarized neutron diffraction experiments on MnSb2O6\mathrm{MnSb}_2\mathrm{O}_6. The study of the nuclear structure shows no evidence for the breaking of the paramagnetic crystallographic space group at the magnetic transition. The consideration of structural twins in our work shows that our single crystal is a non-racemic mixture of chiral structural domains. There is no evidence of a helicoidal magnetic ground state, but diffraction under magnetic field shows the possibility to manipulate the spin structure with low magnetic fields. Finally, we propose that a uniform DM interaction, combined with the underlying coupling between structural and magnetic chiralities, is sufficient to explain an electric polarization switching mechanism which was previously measured.

Acknowledgments

We would like to thank H. Lane and R. Ewings for helpful discussions. We are grateful for funding from the Carnegie Trust for the Universities of Scotland, EPSRC, STFC, and the ILL.

References

  1. [23]N. Qureshi, J. Appl. Crystallogr. 52, 175 (2019).
  2. [25]C. Stock, O. R. Fabelo Rosa, N. Qureshi, and M. Songvilay, Institut Laue-Langevin (ILL) (2021), doi: 10.5291/ILL-DATA.5-11-439.DOI
  3. [26]E. Chan, K. Beauvois, N. Qureshi, J. A. Rodriguez Velamazán, M. Songvilay, C. Stock, and A. Stunault, Institut Laue-Langevin (ILL) (2021), doi: 10.5291/ILL-DATA.5-41-1169.DOI
  4. [27]F. Tasset, P. J. Brown, E. Lelievre-Berna, T. Roberts, S. Pujol, J. Allibon, and E. Bourgeat-Lami, Phys. B 267–268, 69 (1999).
  5. [28]C. Stock, L. Chapon, J. Pasztorova, N. Qureshi, M. Songvilay, and A. Stunault, Institut Laue-Langevin (ILL) (2017), doi: 10.5291/ILL-DATA.5-54-237.DOI
  6. [29]E. Chan, N. Qureshi, C. Ritter, and C. Stock, Institut Laue-Langevin (ILL) (2021), doi: 10.5291/ILL-DATA.5-31-2794.DOI
  7. [30]J. Schwinger, Phys. Rev. 73, 407 (1948).
  8. [31]G. P. Felcher and W. Peterson, Acta Crystallogr. A 31, 76 (1975).
  9. [32]N. Qureshi, A. Bombardi, S. Picozzi, P. Barone, E. Lelievre-Berna, X. Xu, C. Stock, D. F. McMorrow, A. Hearmon, F. Fabrizi, P. G. Radaelli, S.-W. Cheong, and L. C. Chapon, Phys. Rev. B 102, 054417 (2020).
  10. [33]N. Giles-Donovan, N. Qureshi, R. D. Johnson, L. Y. Zhang, S.-W. Cheong, S. Cochran, and C. Stock, Phys. Rev. B 102, 024414 (2020).
  11. [34]P. J. Brown, in Neutron Scattering from Magnetic Materials, Chap. 5, edited by T. Chatterji (Elsevier Science, Amsterdam, 2006) pp. 215–244.
  12. [35]V. Simonet, M. Loire, and R. Ballou, Eur. Phys. J.: Spec. Top. 213, 5 (2012).
  13. [36]M. Blume, Phys. Rev. 130, 1670 (1963).
  14. [37]S. V. Maleev, V. G. Baryakhtar, and R. A. Suris, Sov. Phys. Solid State 4, 2533 (1963).
  15. [38]T. Hahn and H. Klapper, in International Tables for Crystallography, edited by A. Authier, 2nd ed. (Wiley, 2013), Vol. D, pp. 413–487.
  16. [39]S. Parsons, Acta Crystallogr. D 59, 1995 (2003).
  17. [40]E. Koch, in International Tables for Crystallography, edited by E. Prince, 1st ed. (Wiley, 2006), Vol. C, pp. 10–14.
  18. [41]N. Chandra, K. R. Acharya, and P. C. E. Moody, Acta Crystallogr. D 55, 1750 (1999).
  19. [42]H. D. Flack, Helv. Chim. Acta 86, 905 (2003).
  20. [43]L. D. Barron, J. Am. Chem. Soc. 108, 5539 (1986).
  21. [44]R. D. Johnson and P. G. Radaelli, Annu. Rev. Mater. Res. 44, 269 (2014).
  22. [45]J. Villain, J. Phys. Condens. Matter 10, 4793 (1977).
  23. [46]J. Rodríguez-Carvajal, Phys. B 192, 55 (1993).
  24. [47]J. Jerphagnon and D. S. Chemla, J. Chem. Phys. 65, 1522 (1976).
  25. [48]X. Wang, F.-T. Huang, J. Yang, Y. S. Oh, and S.-W. Cheong, APL Mater. 3, 076105 (2015).
  26. [49]M. A. Prosnikov, A. N. Smirnov, V. Y. Davydov, Y. Araki, T. Arima, and R. V. Pisarev, Phys. Rev. B 100, 144417 (2019).
  27. [50]M. Capistroni, M. Hasenbusch, A. Pelissetto, P. Rossi, and E. Vicari, Phys. Rev. B 65, 144520 (2002).
  28. [51]H. Kawamura, J. App. Phys. 63, 3086 (1988).
  29. [52]N. Qureshi, M. Zbiri, J. Rodríguez-Carvajal, A. Stunault, E. Ressouche, T. C. Hansen, M. T. Fernández-Díaz, M. R. Johnson, H. Fuess, H. Ehrenberg, Y. Sakurai, M. Itou, B. Gillon, T. Wolf, J. A. Rodríguez-Velamazan, and J. Sánchez-Montero, Phys. Rev. B 79, 094417 (2009).
  30. [53]K. Yosida, Theory of Magnetism (Springer, New York, 1996).DOI

Paper details

vlnc:W_w8rc5phc
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…