Temperature-dependent Structural Evolution of Ruddlesden-Popper Bilayer Nickelate La3_3Ni2_2O7_7

Abstract

A recent J.Am.Chem.Soc.J. Am. Chem. Soc. Article (DOI: 10.1021/jacs.3c13094) details a pressure-temperature (PP-TT) phase diagram for the Ruddlesden-Popper bilayer nickelate La3_3Ni2_2O7_7 (LNO-2222) using synchrotron X-ray diffraction. This study identifies a phase transition from AmamAmam (#63) to FmmmFmmm (#69) within the temperature range of 104 K to 120 K under initial pressure and attributes the I4/I\rm{4/}mmmmmm (#139) space group to the structure responsible for the superconductivity of LNO-2222. Herein, we examine the temperature-dependent structural evolution of LNO-2222 single crystals at ambient pressure. Contrary to symmetry increase and the established AmamAmam-FmmmFmmm phase boundary, we observe an enhancement in the CmcmCmcm reflections as temperature decreases. This work not only establishes a benchmark method for single crystal structure studies of LNO-2222 using laboratory X-rays, but also enhances the understanding of the complex crystallographic behavior of this system, contributing insights to further experimental and theoretical explorations.

Nickelates have emerged as promising candidates for high-temperature superconductivity, drawing parallel with the cuprates first discovered in the 1980s,[1] due to their analogous crystal and electronic structures.[2] Notably, superconductivity was previously identified in epitaxial thin films of reduced square-planar phases,[3, 4, 5, 6, 7, 8, 9] characterized by an ultra-low valence state of Ni1+\mathrm{Ni}^{1+}, isostructural to Cu2+\mathrm{Cu}^{2+}. Continuing this trajectory, a significant breakthrough was reported last year with the observation of superconductivity signatures in Ruddlesden–Popper bilayer nickelate La3Ni2O7\mathrm{La}_{3}\mathrm{Ni}_{2}\mathrm{O}_{7} (LNO-2222), which exhibited a TCT_{\mathrm{C}} up to 80 K within a pressure range of 14.0 GPa to 43.5 GPa.[10] This discovery was also marked by a structural transition from the ambient pressure Amam (#63) to the high-pressure Fmmm (#69) above 15.0 GPa, aligning with the onset of superconductivity. Further advancements have been achieved through in situ low-temperature high-pressure synchrotron X-ray diffraction (XRD), which has effectively mapped the pressure-temperature (PP-TT) structure phase diagram of LNO-2222, clarifying the phase boundaries among the Amam, Fmmm, and I4/mmm (#139) space group.[11]

Initially, this study caught our attention, because a phase transition from Amam to Fmmm was observed within the temperature range of 104 K to 120 K under initial pressure conditions.[11] However, this symmetry increase contradicts our previous observations in high-quality Sr-doped LNO-2222 single crystals synthesized under high pressure.[12] The absence of detailed crystal structure data targeting the Amam to Fmmm transition in the study prompted further investigation into the temperature effects on this specific symmetry change. Meanwhile, the structure determination in the referenced study[11] was conducted using powder XRD refinements, achieving a resolution limit of approximately 1.14 Å. While it is recognized that obtaining higher resolution and enhanced data quality under high pressure presents significant challenges, in the case of LNO-2222, precise determination of lattice centering and space groups critically depends on the observation of some weak peaks. Therefore, a more dedicated focus on studying the crystal structure, particularly through the use of single crystals, is essential for comprehensively resolving the complexities of this material.

On the other hand, increasing efforts have been directed toward theoretical investigations of the mechanism behind high-TCT_{\mathrm{C}} superconductivity in LNO-2222. The accuracy of these theoretical models might be compromised without precisely determined crystal structures. Notably, conflicting suggestions regarding the size of A-site cations and their role in stabilizing the superconducting phase at ambient pressure have been reported.[13, 14]

We conducted temperature-dependent single crystal XRD experiments on LNO-2222, spanning a temperature range from 80 K to 400 K at ambient pressure. Our results indicate that with decreasing temperature, the tilt of octahedra in LNO-2222 is enhanced, and the Cmcm space group becomes increasingly favorable. This work aims to establish a benchmark method for single crystal structure studies of LNO-2222 using laboratory X-rays. Further investigations exploring the crystal structure and structure-property relationship in LNO-2222 will likely require much more high-quality data, utilizing advanced techniques such as synchrotron X-rays and neutrons.

Procedures of our single crystal XRD experiments and data analysis of LNO-2222 are detailed in Scheme 1. The crystals of LNO-2222 used in this study were selected from the same batch as previously reported[15] and grown using the floating zone method under 100% O2_2 at a pressure of 14–15 bar at the University of Tennessee. A single crystal with dimensions of 0.069×0.045×0.014 mm30.069 \times0.045 \times0.014\ \mathrm{mm}^{3} was picked up, mounted on a nylon loop with paratone oil, and measured using an XtalLAB Synergy, Dualflex, Hypix single crystal X-ray diffractometer equipped with an Oxford Cryosystems 800 low-temperature device. Prior to initiating temperature-varied data collection, the quality of the crystal was examined at room temperature, confirming its bilayer stacking. The temperature protocol commenced with cooling the sample to 80(2) K, followed by sequential heating to 400(2) K in increments of 40 K. A 10-minute stabilization period was allowed between each temperature scan, with continuous monitoring and adjustment of crystal centering as needed throughout the process. Data acquisition was performed using ω\omega scans with Mo Kα_{\alpha} radiation (λ=0.71073\lambda= 0.71073 Å, micro-focus sealed X-ray tube, 50 kV, 1 mA). The measurement strategy, including the total number of runs and images, was determined using the strategy calculation feature in CrysAlisPro software (version 1.171.43.104a, Rigaku OD, 2023), which was established at 80(2) K and consistently applied across all temperature steps. Data reduction induced correction for Lorentz polarization. Numerical absorption correction based on Gaussian integration over a multifaceted crystal model. Empirical absorption correction was applied using spherical harmonics implemented in SCALE3 ABSPACK scaling algorithm. Structure solution and refinement were conducted using the Bruker SHELXTL Software Package.[16, 17]

Procedure of single crystal XRD experiments and data analysis of LNO-2222

Figure 1. Procedure of our single crystal XRD experiments and data analysis of LNO-2222.

The initial determination of the crystal structure of LNO-2222, classified in the F\mathit{F}-centered orthorhombic Fmmm\mathit{Fmmm} space group, was performed using powder XRD and Rietveld refinement on polycrystalline samples.[18] Recognizing the substantial uncertainty in determining oxygen coordinates, neutron powder diffraction (NPD) was subsequently employed.[19, 20] The results indicated that the Fmmm\mathit{Fmmm} space group was inappropriate, as it failed to account for extra weak peaks, suggesting a lower symmetry. Consequently, a C\mathit{C}-centered orthorhombic lattice in the space group Cmcm\mathit{Cmcm} was proposed.[19] Challenges related to the lattice centering, the impact of oxygen vacancies, and the coexistence of Ruddlesden–Popper bilayer and trilayer phases highlight the complexities in structure determination, underscoring the necessity for pure LNO-2222 single crystals. Recent advances in the high-pressure floating zone method, which allows for a 100% O2\mathrm{O}_{2} atmosphere with controllable gas pressure, have facilitated the growth of high-purity Ruddlesden–Popper nickelate single crystals, enabling precise structure determination using laboratory Xrays.[15, 21, 22] Furthermore, a previously unrecognized phase of La3Ni2O7\mathrm{La}_3\mathrm{Ni}_2\mathrm{O}_7 with distinct layer stacking, LNO-1313, was first reported by Chen et al.^{22} in the growth of LNO-2222, and supported by later studies.[15, 23]

In the referenced low-temperature high-pressure study,[11] multiple instances of twins and severe texture development were reported during pressure increase across multiple runs, yet these claims lacked experimental evidence. If the sample quality was thoroughly examined prior to pressurization, it would be essential to document at which pressure and temperature conditions these multiple twins (or texture development) occurred in LNO-2222, their intrinsic nature, and their impacts on the results of structure determination. The results from powder XRD refinement results remain ambiguous, with “atomic positions optimized theoretically” mentioned but without additional details provided.

The presence of oxygen vacancies significantly influences the determination of crystal structure, often leading to a symmetry increase. For example, polycrystalline samples of La3Ni2O6.92\mathrm{La}_3\mathrm{Ni}_2\mathrm{O}_{6.92}-2222 and La3Ni2O6.94\mathrm{La}_3\mathrm{Ni}_2\mathrm{O}_{6.94}-2222 were determined to be Fmmm\mathit{Fmmm} by powder XRD,[18, 24] while La3Ni2O6\mathrm{La}_3\mathrm{Ni}_2\mathrm{O}_6-2222 and La3Ni2O6.35\mathrm{La}_3\mathrm{Ni}_2\mathrm{O}_{6.35}-2222 was identified as I4/mmm\mathit{I4/mmm} by NPD.[25, 26]

Concerning the tuning of LNO-2222 crystal structures through A-site doping, there are claims that using smaller atoms might induce a chemical precompression effect.[11] One argument presented is the comparison of the A/B atomic size ratio between tetragonal Sr3Ti2O7\mathrm{Sr}_3\mathrm{Ti}_2\mathrm{O}_7 and LNO-2222. However, the lack of a referenced source for atomic size data undermines the credibility of this comparison. Whether using atomic size or ionic size is more appropriate remains unclear. According to the authors’ logic, a rough calculation reveal that Sr2+/Ti4+=132/74.5=1.772\mathrm{Sr}^{2+}/\mathrm{Ti}^{4+} = 132/74.5 = 1.772, while La3+/(0.5∗(Ni2++Ni3+))=117.2/(0.5∗(83+70))=1.532\mathrm{La}^{3+}/(0.5*(\mathrm{Ni}^{2+}+\mathrm{Ni}^{3+})) = 117.2/(0.5*(83+70)) = 1.532.[27] Even considering Ni2+/3+\mathrm{Ni}^{2+/3+} as Ni3+\mathrm{Ni}^{3+} exclusively, the upper boundary for La3+/Ni2+/3+\mathrm{La}^{3+}/\mathrm{Ni}^{2+/3+} would be 117.2/70=1.674117.2/70 = 1.674, still smaller than the Sr2+/Ti4+\mathrm{Sr}^{2+}/\mathrm{Ti}^{4+} ratio, suggesting an opposite conclusion. Furthermore, in the case of La2−2xSr1+2xMn2O7\mathrm{La}_{2-2x}\mathrm{Sr}_{1+2x}\mathrm{Mn}_2\mathrm{O}_7, detailed crystallographic and magnetic phase diagram provided by temperature-dependent neutron powder diffraction shows a tetragonal-to-orthorhombic phase transition, peaking at x=0.80x = 0.80.[28] However, these findings were never related to the size of A-site in the original report. The persistence of the tetragonal I4/mmm\mathit{I4/mmm} structure to 35 GPa in LaSr2Mn2O7\mathrm{LaSr}_2\mathrm{Mn}_2\mathrm{O}_7[29] (x=1.00x = 1.00) contradicts the claims, as the size of Sr2+\mathrm{Sr}^{2+} is larger than La3+\mathrm{La}^{3+}.

Our previous report[12] included a temperature-dependent crystal structure study of high-quality Sr-doped LNO-2222 single crystals (formula La2.80(1)Sr0.20(1)Ni2O6.95(1)\mathrm{La}_{2.80(1)}\mathrm{Sr}_{0.20(1)}\mathrm{Ni}_{2}\mathrm{O}_{6.95(1)}, denoted as Sr-LNO-2222), obtained via high-pressure synthesis. A comparison of the out-of-plane Ni–O–Ni bond angles between undoped LNO-2222 and Sr-LNO-2222 reveals that Sr-LNO-2222 exhibits fewer octahedral tilts, which supports the hypothesis that the incorporation of larger A-site atoms contributes to a potential rise in symmetry.

Figure 1 illustrates the crystal structure of LNO-2222 in the space groups CmcmCmcm, FmmmFmmm, and I4/mmmI4/mmm, providing a detailed view of their structural variations. Central to this discussion are the group-subgroup relationships that explain how LNO-2222 crystallizes in these specific space groups. In the CmcmCmcm space group, the structure can be interpreted as I4/mmmI4/mmm with two octahedral tilts about the [011][011] and [011ˉ][01\bar{1}] axes. These tilts are highlighted in Figure 1d with orange and red arrows indicating different directions of octahedral tilts, while an asterisk marks the consistent octahedral across different views. Transitioning to the FmmmFmmm space group, the octahedral tilts are absent, resulting in a structure that might otherwise resemble the I4/mmmI4/mmm symmetry. However, as shown in Figure 1e, lattice distortions along the aa and bb axes prevent this. Furthermore, it is worth mentioning that the I4/mmmI4/mmm structure does not display a perfect square lattice. This difference is primarily due to a slight displacement of oxygen along the cc-axis, as represented in Figure 1f, which disrupts the planarity between the oxygen and nickel atoms, inducing nonlinear “in-plane” Ni–O–Ni bond angles.

Crystal structure of LNO-2222

Figure 1 (PDF p. 7). Crystal structure of LNO-2222. (a–c) Layer stacking views in the space group Cmcm, Fmmm, and I4/mmm, respectively. Green, grey, and red represent La, Ni, and O atoms. In the Cmcm space group, crystallographically unique atoms are labeled. (d) Two octahedral tilts about the [11] and [0-11] axes in the Cmcm space group. (e) Lattice distortion along the aa and bb axes in the Fmmm space group. (f) Oxygen displacements along the cc axis in the I4/mmm space group, leading to nonlinear “in-plane” Ni–O–Ni bond angles.

The crystallographic data and structure refinements for LNO-2222 at 80 K and 280 K are summarized in Table 1–Table 3. Our refinements revealed no instances of oxygen vacancies. A slight lattice expansion was observed at 280 K when compared to the structure at 80 K as expected for thermal expansion. Our experimental reciprocal lattice planes, (0kl)(0kl), (h1l)(h1l), and (hk0)(hk0) at temperatures of 80 K, 280 K, and 400 K, are presented in Figure 2. To enable a clearer visual comparison, the Cmcm unit cell was transformed into a symmetry-equivalent Amam setting, with the cc axis oriented perpendicular to the perovskite layers. Laue symmetry mmm was applied in the regeneration of these (hkl)(hkl) planes. The reflection conditions for the Amam space group are defined as k+l=2nk+l=2n for all reflections, and h=2nh=2n specifically for reflections on the (h0l)(h0l) plane. For the FF-centering lattice, the reflection conditions stipulate that hh, kk, ll must all be either even or odd (‘unmixed’). In our analysis, additional reflections that characterize the Amam space group and signify violations for the Fmmm space group were observed and labeled on each reciprocal lattice plane. These reflections progressively become weaker as temperatures increased. Further details on the crystallographic data, structure refinements, and reciprocal lattice planes at other temperatures studied are available in Figure S1, Figure S2, and Table S1–Table S14.

Chemical formulaLa3Ni2O7\mathrm{La}_{3}\mathrm{Ni}_{2}\mathrm{O}_{7}-2222La3Ni2O7\mathrm{La}_{3}\mathrm{Ni}_{2}\mathrm{O}_{7}-2222
Temperature80(2) K280(2) K
Formula weight646.15 g/mol646.15 g/mol
Space groupCmcmCmcm
Unit cell dimensionsa=20.4840(6)a = 20.4840(6) Å; b=5.44800(16)b = 5.44800(16) Å; c=5.37711(17)c = 5.37711(17) Åa=20.5290(6)a = 20.5290(6) Å; b=5.44684(18)b = 5.44684(18) Å; c=5.38990(18)c = 5.38990(18) Å
Volume600.07(3) Å3^{3}602.69(3) Å3^{3}
ZZ44
Density (calculated)7.152 g/cm3^{3}7.121 g/cm3^{3}
Absorption coefficient27.042 mm−1^{-1}26.924 mm−1^{-1}
F(000)F(000)11321132
θ\theta range3.87 to 40.76°3.87 to 40.71°
Reflections collected1864518646
Independent reflections1054 [Rint=0.0682R_{\mathrm{int}} = 0.0682]1056 [Rint=0.0663R_{\mathrm{int}} = 0.0663]
Refinement methodFull-matrix least-squares on F2F^{2}Full-matrix least-squares on F2F^{2}
Data / restraints / parameters1054 / 0 / 371056 / 0 / 37
Final RR indicesR1 (I>2σ(I))=0.0280R_{1}\ (I>2\sigma(I)) = 0.0280; wR2 (I>2σ(I))=0.0695wR_{2}\ (I>2\sigma(I)) = 0.0695; R1 (all)=0.0341R_{1}\ (\mathrm{all}) = 0.0341; wR2 (all)=0.0720wR_{2}\ (\mathrm{all}) = 0.0720R1 (I>2σ(I))=0.0265R_{1}\ (I>2\sigma(I)) = 0.0265; wR2 (I>2σ(I))=0.0670wR_{2}\ (I>2\sigma(I)) = 0.0670; R1 (all)=0.0358R_{1}\ (\mathrm{all}) = 0.0358; wR2 (all)=0.0711wR_{2}\ (\mathrm{all}) = 0.0711
Largest diff. peak and hole+5.390 e/Å−3^{-3} and −1.962 e/Å−3^{-3}+6.066 e/Å−3^{-3} and −1.831 e/Å−3^{-3}
R.M.S. deviation from mean0.461 e/Å−3^{-3}0.439 e/Å−3^{-3}
Goodness-of-fit on F2F^{2}1.1841.109

Table 1. Crystal data and structure refinement of LNO-2222 at 80 K and 280 K.

Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
La1_14c4c00.75058(4)1/410.00729(7)
La2_28g8g0.32019(2)0.25789(3)1/410.00634(7)
Ni8g8g0.09589(3)0.25242(7)1/410.00472(9)
O1_18e8e0.39534(16)0010.0115(5)
O2_28e8e0.08932(15)0010.0109(5)
O3_38g8g0.20441(16)0.2173(6)1/410.0129(5)
O4_44c4c00.2909(8)1/410.0117(7)

Table 3. Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^2) of LNO-2222 at 280 K. UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.

Reciprocal lattice planes of LNO-2222

Figure 2. Reciprocal lattice planes of LNO-2222. (a–c) (0kl)(0kl), (h1l)(h1l) and (hk0)(hk0) planes at 80 K. (d–f) (0kl)(0kl), (h1l)(h1l) and (hk0)(hk0) planes at 280 K. (g–i) (0kl)(0kl), (h1l)(h1l) and (hk0)(hk0) planes at 400 K. The CmcmCmcm unit cell has been transformed into the AmamAmam setting to enhance visual clarity. Laue symmetry mmmmmm has been applied in the regeneration of these (hkl)(hkl) planes.

Reciprocal lattice planes of LNO-2222

Figure S1. (a–c) (0kl)(0kl), (h1l)(h1l) and (hk0)(hk0) planes at 120 K. (d–f) (0kl)(0kl), (h1l)(h1l) and (hk0)(hk0) planes at 160 K. (g–i) (0kl)(0kl), (h1l)(h1l) and (hk0)(hk0) planes at 200 K. The CmcmCmcm unit cell has been transformed into the AmamAmam setting to enhance visual clarity. Laue symmetry mmmmmm has been applied in the regeneration of these (hkl)(hkl) planes.

Reciprocal lattice planes of LNO-2222 at 240 K, 320 K, and 360 K

Figure S2. Reciprocal lattice planes of LNO-2222. (a–c) (0kl)(0kl), (h1l)(h1l) and (hk0)(hk0) planes at 240 K. (d–f) (0kl)(0kl), (h1l)(h1l) and (hk0)(hk0) planes at 320 K. (g–i) (0kl)(0kl), (h1l)(h1l) and (hk0)(hk0) planes at 360 K. The CmcmCmcm unit cell has been transformed to the AmamAmam setting to enhance visual clarity. Laue symmetry mmmmmm has been applied in the regeneration of these (hkl)(hkl) planes.

Chemical formulaLa3Ni2O7\mathrm{La}_3\mathrm{Ni}_2\mathrm{O}_7-2222
Temperature120(2) K
Formula weight646.15 g/mol
Space groupCmcmCmcm
Unit cell dimensionsa=20.4948(6)a = 20.4948(6) Å
b=5.44843(15)b = 5.44843(15) Å
c=5.37889(16)c = 5.37889(16) Å
Volume600.63(3) Å3^3
ZZ4
Density (calculated)7.146 g/cm3^3
Absorption coefficient27.017 mm−1^{-1}
F(000)F(000)1132
θ\theta range3.87 to 40.71°
Reflections collected18774
Independent reflections1053 [Rint=0.0635R_{\mathrm{int}} = 0.0635]
Refinement methodFull-matrix least-squares on F2F^2
Data / restraints / parameters1053 / 0 / 37
Final RR indicesR1R_1 (I>2σ(I)I>2\sigma(I)) = 0.0275; wR2wR_2 (I>2σ(I)I>2\sigma(I)) = 0.0683
R1R_1 (all) = 0.0335; wR2wR_2 (all) = 0.0710
Largest diff. peak and hole+6.281 e/Å−3^{-3} and −1.674 e/Å−3^{-3}
R.M.S. deviation from mean0.462 e/Å−3^{-3}
Goodness-of-fit on F2F^21.165

Table S1. Crystal data and structure refinement of LNO-2222 at 120 K.

Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
La1_14c00.75044(4)1/410.00969(7)
La2_28g0.32020(2)0.25748(3)1/410.00819(7)
Ni8g0.09586(3)0.25234(6)1/410.00592(9)
O1_18e0.39570(15)0010.0150(5)
O2_28e0.09007(14)0010.0137(5)
O3_38g0.20438(14)0.2191(5)1/410.0152(5)
O4_44c00.2892(7)1/410.0141(6)

Table S14. Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^{2}) of LNO-2222 at 400 K. UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.

Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
La1_14c4c00.75089(5)1/410.00354(7)
La2_28g8g0.32024(2)0.25870(3)1/410.00340(7)
Ni8g8g0.09589(3)0.25256(8)1/410.00287(10)
O1_18e8e0.39468(16)0010.0062(5)
O2_28e8e0.08878(15)0010.0063(5)
O3_38g8g0.20448(16)0.2140(6)1/410.0080(5)
O4_44c4c00.2944(9)1/410.0066(6)

Table 2. Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^2) of LNO-2222 at 80 K. UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.

Figure 3a and 3b display the temperature-dependent evolution of the lattice parameters, aa, bb, cc, and the unit cell volume of LNO-2222. These parameters follow the expected thermal expansion behavior as temperature increases. Notably, the evolution of the lattice parameter bb is non-monotonic, exhibiting a distinct anomaly at 120 K. One possible explanation is structure modulations, potentially through charge ordering or the formation of density waves. Figure 3c and 3d provide more structure details about the in-plane and out-of-plane Ni–O–Ni bond angles. As temperature decreases, these bond angles increasingly deviate from 180 degrees, indicative of enhanced octahedral tilts. Such behavior points to potential signs of symmetry lowering. Outlined within Scheme 1 is the methodology for analyzing experimental reflection data. We identify and focus on specific reflections characteristic of CC-centering and violate FF-centering norms, which are expected to be weak, as well as reflections common to both CC- and FF-centering. Due to data redundancy, the same reflections are observed multiple times during data collection. We also merge reflections equivalent under Laue symmetry to streamline the analysis. Moreover, we define the average intensity ratio of specific reflections from these two classes, for example, 041 and 002 here, as a metric to evaluate potential changes in symmetry. The unbiased selection of reflections has been validated by incorporating an additional CC-centering characteristic reflection, 330, which is among the most intense. The results are presented in Figure S3, demonstrating the consistency and reliability of our methodology. Our comprehensive analysis confirms that at low temperatures, down to 80 K, the CmcmCmcm space group becomes increasingly favorable, aligning with the observed changes in the out-of-plane Ni–O4–Ni bond angle as detailed in Figure 3c. This correlation emphasizes the structural dynamics of LNO-2222 under varying thermal conditions.

Figure 3. Temperature-dependent structure evolution of LNO-2222. (a) Lattice parameters bb and cc. (b) Lattice parameter aa and unit cell volume. (c) Out-of-plane Ni–O4–Ni bond angle and the observed intensity ratio of the 041 and 002 reflections, normalized to 80 K. (d) In-plane Ni–O1–Ni and Ni–O2–Ni bond angles. Lines serve as guides to the eye, and error bars are indicated by color filling.

Validation of unbiased reflection selections

Figure S3. Validation of unbiased reflection selections. (a) Temperature-dependent evolution of out-of-plane Ni–O4–Ni bond angle and the observed intensity ratio of the 330 and 002 reflections, normalized at 80 K. (b) Structure phase diagram of LNO-2222. The dashed line indicates the phase boundary between the Cmcm and Fmmm space groups.

Given the observed enhancement of Cmcm reflections at low temperatures, considering external pressure as a tuning parameter offers a new perspective on the structure behavior of LNO-2222. We can extrapolate its temperature behavior at ambient pressure to at least slightly higher pressures, under the assumption that the Cmcm-Fmmm transition at low temperatures and high pressures is gradual rather than abrupt. This assumption is reasonable, as no formation or breaking of chemical bonds is involved. In terms of crystal structure dynamics, for the transition to occur, the out-of-plane Ni–O–Ni bond angle must approach exactly 180 degrees. Based on this requirement, we hypothesize that, compared to room temperature, a higher pressure would be necessary to induce this transition at lower temperatures. Figure 4 presents our structure phase diagram of LNO-2222, where the CmcmCmcm-FmmmFmmm phase boundary is indicated by a dashed line. This boundary is notably inconsistent with the reported one.[11] Additionally, it is plausible that sufficiently high temperatures could also facilitate this phase transition, although such conditions may extend beyond the scope of our current discussion.

Structure phase diagram of LNO-2222

Figure 4. Structure phase diagram of LNO-2222. The dashed line indicates the phase boundary between the CmcmCmcm and FmmmFmmm space groups. The phase diagram extrapolates the ambient pressure behavior of LNO-2222 to a little higher pressure (less than 0.2 GPa). Further experiments under high pressure are necessary for confirmation.

The evaluation of the FmmmFmmm-I4/mmmI4/mmm phase boundary, as reported in the referenced study,[11] presents distinct challenges due to inconsistencies in unit cell selection, necessitating the use of 2\sqrt{2} super reciprocal vectors in the hkhk plane for accurate analysis. Furthermore, the detection of very weak difference reflections, which appear on half-integral reciprocal lattice planes when using original sub cell axes, requires specialized efforts. These reflections are critical for confirming the phase transition but may not be readily observable under high-pressure conditions due to the inherent experimental challenges. Further detailed experiments involving (low-temperature) high-pressure single crystal XRD will be essential to fully elucidate the complex crystallographic behavior of LNO-2222.

In conclusion, we present our investigation into the temperature-dependent structural evolution of LNO-2222 single crystals at ambient pressure. Our results highlight the enhancement of CmcmCmcm reflections as temperature decreases. Additionally, we have developed our structure phase diagram for LNO-2222 that differs from the reported, particularly concerning the CmcmCmcm-FmmmFmmm phase boundary. This study not only provides a benchmark method for conducting single crystal structure analysis of LNO-2222 using laboratory X-rays but also delivers high-quality crystallographic data across various temperatures. More importantly, our work enhances the understanding of the complex crystallographic behavior of this system, laying a solid foundation for further experimental and theoretical investigations.

Supporting Information

Reciprocal lattice planes of LNO-2222 at temperatures of 120 K, 160 K, 200 K, 240 K, 320 K, and 360 K; Validation of unbiased reflection selections; Crystal data and structure refinement, atomic coordinates, and equivalent isotropic atomic displacement parameters of LNO-2222 at temperatures of 120 K, 160 K, 200 K, 240 K, 320 K, 360 K, and 400 K.

Acknowledgments

The work at Michigan State University was supported by U.S. DOE-BES under Contract DE-SC0023648. The work at the University of Tennessee (crystal growth) was supported by the Air Force Office of Scientific Research under Grant No. FA9550-23-1-0502. H.W. appreciate helpful discussions with Dr. Xinglong Chen (Argonne National Laboratory).

For Table of Contents Only

Phase diagram of LNO-2222

Figure 5 (PDF p. 18).

Temperature-dependent Structural Evolution of Ruddlesden–Popper Bilayer Nickelate La3Ni2O7\mathrm{La}_3\mathrm{Ni}_2\mathrm{O}_7

Haozhe Wang; Haidong Zhou; Weiwei Xie

Supporting Information

Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
La1_14c00.75081(5)1/410.00438(7)
La2_28g0.32024(2)0.25860(3)1/410.00406(7)
Ni8g0.09591(3)0.25254(7)1/410.00329(10)
O1_18e0.39473(16)0010.0075(5)
O2_28e0.08887(15)0010.0072(5)
O3_38g0.20437(16)0.2143(6)1/410.0081(5)
O4_44c00.2929(9)1/410.0085(7)

Table S2. Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^2) of LNO-2222 at 120 K. UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.

Chemical formulaLa₃Ni₂O₇-2222
Temperature160(2) K
Formula weight646.15 g/mol
Space groupCmcmCmcm
Unit cell dimensionsa=20.4939(6)a = 20.4939(6) Å
b=5.44613(17)b = 5.44613(17) Å
c=5.38089(18)c = 5.38089(18) Å
Volume600.57(3) Å3^{3}
ZZ4
Density (calculated)7.146 g/cm3^{3}
Absorption coefficient27.019 mm−1^{-1}
F(000)F(000)1132
θ\theta range3.87 to 40.70°
Reflections collected18729
Independent reflections1053 [Rint=0.0709R_{\mathrm{int}} = 0.0709]
Refinement methodFull-matrix least-squares on F2F^{2}
Data / restraints / parameters1053 / 0 / 37
Final RR indicesR1R_{1} (I>2σ(I)I>2\sigma(I)) = 0.0286; wR2wR_{2} (I>2σ(I)I>2\sigma(I)) = 0.0684
R1R_{1} (all) = 0.0368; wR2wR_{2} (all) = 0.0716
Largest diff. peak and hole+5.998 e/Å−3^{-3} and −2.019 e/Å−3^{-3}
R.M.S. deviation from mean0.468 e/Å−3^{-3}
Goodness-of-fit on F2F^{2}1.104

Table S3. Crystal data and structure refinement of LNO-2222 at 160 K.

Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
La₁4c4c00.75085(5)1/410.00498(7)
La₂8g8g0.32023(2)0.25840(3)1/410.00453(7)
Ni8g8g0.09591(3)0.25242(8)1/410.00363(10)
O₁8e8e0.39481(17)0010.0083(5)
O₂8e8e0.08915(16)0010.0076(5)
O₃8g8g0.20437(17)0.2152(6)1/410.0091(5)
O₄4c4c00.2942(9)1/410.0082(7)

Table S4. Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^{2}) of LNO-2222 at 160 K. UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.

Chemical formulaLa3Ni2O7\mathrm{La}_3\mathrm{Ni}_2\mathrm{O}_7-2222
Temperature200(2) K
Formula weight646.15 g/mol
Space groupCmcmCmcm
Unit cell dimensionsa=20.5017(7)a = 20.5017(7) Å
b=5.44564(18)b = 5.44564(18) Å
c=5.38391(19)c = 5.38391(19) Å
Volume601.08(3) Å3^3
ZZ4
Density (calculated)7.140 g/cm3^3
Absorption coefficient26.996 mm−1^{-1}
FF(000)1132
θ\theta range3.87 to 40.75°
Reflections collected18613
Independent reflections1057 [Rint=0.0741R_{\mathrm{int}} = 0.0741]
Refinement methodFull-matrix least-squares on F2F^2
Data / restraints / parameters1057 / 0 / 37
Final RR indicesR1R_1 (I>2σ(I)I>2\sigma(I)) = 0.0289; wR2wR_2 (I>2σ(I)I>2\sigma(I)) = 0.0697
R1R_1 (all) = 0.0384; wR2wR_2 (all) = 0.0739
Largest diff. peak and hole+6.311 e/Å−3^{-3} and −2.267 e/Å−3^{-3}
R.M.S. deviation from mean0.488 e/Å−3^{-3}
Goodness-of-fit on F2F^21.103

Table S5. Crystal data and structure refinement of LNO-2222 at 200 K.

Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
La1_14c4c00.75074(5)1/410.00575(8)
La2_28g8g0.32021(2)0.25822(3)1/410.00517(7)
Ni8g8g0.09589(3)0.25243(8)1/410.00393(10)
O1_18e8e0.39482(18)0010.0089(6)
O2_28e8e0.08923(17)0010.0093(6)
O3_38g8g0.20430(17)0.2155(6)1/410.0099(6)
O4_44c4c00.2926(9)1/410.0089(7)

Table S6. Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^2) of LNO-2222 at 200 K. UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.

Chemical formulaLa3Ni2O7-2222\mathrm{La}_3\mathrm{Ni}_2\mathrm{O}_7\text{-2222}
Temperature240(2) K
Formula weight646.15 g/mol
Space groupCmcm\mathit{Cmcm}
Unit cell dimensionsa=20.5189(6)a = 20.5189(6) \AA
b=5.44597(17)b = 5.44597(17) \AA
c=5.38630(18)c = 5.38630(18) \AA
Volume601.89(3) \AA3^3
ZZ4
Density (calculated)7.131 g/cm3^3
Absorption coefficient26.960 mm−1^{-1}
F(000)F(000)1132
θ\theta range3.87 to 40.73°
Reflections collected18656
Independent reflections1055 [Rint=0.0649R_{\mathrm{int}} = 0.0649]
Refinement methodFull-matrix least-squares on F2F^2
Data / restraints / parameters1055 / 0 / 37
Final RR indicesR1R_1 (I>2σ(I)I>2\sigma(I)) = 0.0271; wR2wR_2 (I>2σ(I)I>2\sigma(I)) = 0.0672
R1R_1 (all) = 0.0360; wR2wR_2 (all) = 0.0711
Largest diff. peak and hole+6.097 e/\AA−3^{-3} and −2.068 e/\AA−3^{-3}
R.M.S. deviation from mean0.442 e/\AA−3^{-3}
Goodness-of-fit on F2F^21.126

Table S7. Crystal data and structure refinement of LNO-2222 at 240 K.

Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
La1_14c4c00.75067(5)1/410.00656(7)
La2_28g8g0.32020(2)0.25804(3)1/410.00581(7)
Ni8g8g0.09591(3)0.25247(7)1/410.00435(9)
O1_18e8e0.39502(16)0010.0100(5)
O2_28e8e0.08934(15)0010.0095(5)
O3_38g8g0.20454(15)0.2156(6)1/410.0111(5)
O4_44c4c00.2922(8)1/410.0110(7)

Table S8. Atomic coordinates and equivalent isotropic atomic displacement parameters (\AA2^2) of LNO-2222 at 240 K. UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.

Chemical formulaLa3Ni2O7\mathrm{La}_3\mathrm{Ni}_2\mathrm{O}_7-2222
Temperature320(2) K
Formula weight646.15 g/mol
Space groupCmcmCmcm
Unit cell dimensionsa=20.5374(7)a = 20.5374(7) Å
b=5.44684(18)b = 5.44684(18) Å
c=5.39285(19)c = 5.39285(19) Å
Volume603.27(4) Å3^3
ZZ4
Density (calculated)7.114 g/cm3^3
Absorption coefficient26.899 mm−1^{-1}
FF(000)1132
θ\theta range3.87 to 40.83°
Reflections collected18690
Independent reflections1060 [Rint=0.0591R_{\mathrm{int}} = 0.0591]
Refinement methodFull-matrix least-squares on F2F^2
Data / restraints / parameters1060 / 0 / 37
Final RR indicesR1R_1 (I>2σ(I)I>2\sigma(I)) = 0.0258; wR2wR_2 (I>2σ(I)I>2\sigma(I)) = 0.0640
R1R_1 (all) = 0.0348; wR2wR_2 (all) = 0.0677
Largest diff. peak and hole+6.146 e/Å−3^{-3} and −1.499 e/Å−3^{-3}
R.M.S. deviation from mean0.433 e/Å−3^{-3}
Goodness-of-fit on F2F^21.114

Table S9. Crystal data and structure refinement of LNO-2222 at 320 K.

Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
La1_14c4c00.75055(4)1/410.00810(7)
La2_28g8g0.32020(2)0.25766(3)1/410.00700(6)
Ni8g8g0.09589(3)0.25237(6)1/410.00515(9)
O1_18e8e0.39545(15)0010.0129(5)
O2_28e8e0.08962(14)0010.0121(5)
O3_38g8g0.20435(15)0.2179(5)1/410.0137(5)
O4_44c4c00.2898(7)1/410.0126(6)

Table S10. Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^2) of LNO-2222 at 320 K. UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.

Chemical formulaLa3Ni2O7\mathrm{La}_3\mathrm{Ni}_2\mathrm{O}_7-2222
Temperature360(2) K
Formula weight646.15 g/mol
Space groupCmcm\mathit{Cmcm}
Unit cell dimensionsa=20.5497(6)a = 20.5497(6) Å
b=5.44845(18)b = 5.44845(18) Å
c=5.39774(18)c = 5.39774(18) Å
Volume604.35(3) Å3^3
ZZ4
Density (calculated)7.102 g/cm3^3
Absorption coefficient26.850 mm−1^{-1}
F(000)F(000)1132
θ\theta range3.87 to 40.91°
Reflections collected18283
Independent reflections1062 [Rint=0.0566R_{\mathrm{int}} = 0.0566]
Refinement methodFull-matrix least-squares on F2F^2
Data / restraints / parameters1062 / 0 / 37
Final RR indicesR1R_1 (I>2σ(I)I>2\sigma(I)) = 0.0258; wR2wR_2 (I>2σ(I)I>2\sigma(I)) = 0.0654
R1R_1 (all) = 0.0333; wR2wR_2 (all) = 0.0686
Largest diff. peak and hole+6.010 e/Å−3^{-3} and −1.941 e/Å−3^{-3}
R.M.S. deviation from mean0.409 e/Å−3^{-3}
Goodness-of-fit on F2F^21.079

Table S11. Crystal data and structure refinement of LNO-2222 at 360 K.

Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
La1_14c4c00.75044(4)1/410.00881(7)
La2_28g8g0.32020(2)0.25748(3)1/410.00760(6)
Ni8g8g0.09586(3)0.25234(6)1/410.00549(9)
O1_18e8e0.39570(15)0010.0137(5)
O2_28e8e0.08994(14)0010.0127(5)
O3_38g8g0.20439(14)0.2190(5)1/410.0143(5)
O4_44c4c00.2887(8)1/410.0138(6)

Table S12. Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^2) of LNO-2222 at 360 K. UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.

Chemical formulaLa3Ni2O7\mathrm{La}_{3}\mathrm{Ni}_{2}\mathrm{O}_{7}-2222
Temperature400(2) K
Formula weight646.15 g/mol
Space groupCmcm\mathit{Cmcm}
Unit cell dimensionsa=20.5679(7)a = 20.5679(7) Å
b=5.45019(19)b = 5.45019(19) Å
c=5.4028(2)c = 5.4028(2) Å
Volume605.65(4) Å3^{3}
ZZ4
Density (calculated)7.086 g/cm3^{3}
Absorption coefficient26.793 mm−1^{-1}
FF(000)1132
θ\theta range3.87 to 40.87°
Reflections collected18515
Independent reflections1062 [Rint=0.0566R_{\mathrm{int}} = 0.0566]
Refinement methodFull-matrix least-squares on F2F^{2}
Data / restraints / parameters1062 / 0 / 37
Final RR indicesR1R_{1} (I>2σ(I)I>2\sigma(I)) = 0.0266; wR2wR_{2} (I>2σ(I)I>2\sigma(I)) = 0.0678
R1R_{1} (all) = 0.0352; wR2wR_{2} (all) = 0.0715
Largest diff. peak and hole+6.303 e/Å−3^{-3} and −1.854 e/Å−3^{-3}
R.M.S. deviation from mean0.427 e/Å−3^{-3}
Goodness-of-fit on F2F^{2}1.133

Table S13. Crystal data and structure refinement of LNO-2222 at 400 K.

References

  1. [1]Bednorz, J. G.; Müller, K. A., Possible highTc superconductivity in the Ba–La–Cu–O system. Z. Phys. B: Condens. Matter 1986, 64 (2), 189-193.
  2. [2]Anisimov, V. I.; Bukhvalov, D.; Rice, T. M., Electronic structure of possible nickelate analogs to the cuprates. Phys. Rev. B 1999, 59 (12), 7901-7906.DOI
  3. [3]Li, D.; Lee, K.; Wang, B. Y.; Osada, M.; Crossley, S.; Lee, H. R.; Cui, Y.; Hikita, Y.; Hwang, H. Y., Superconductivity in an infinite-layer nickelate. Nature 2019, 572 (7771), 624-627.DOI
  4. [4]Osada, M.; Wang, B. Y.; Goodge, B. H.; Lee, K.; Yoon, H.; Sakuma, K.; Li, D.; Miura, M.; Kourkoutis, L. F.; Hwang, H. Y., A Superconducting Praseodymium Nickelate with Infinite Layer Structure. Nano Lett. 2020, 20 (8), 5735-5740.DOI
  5. [5]Wang, N. N.; Yang, M. W.; Yang, Z.; Chen, K. Y.; Zhang, H.; Zhang, Q. H.; Zhu, Z. H.; Uwatoko, Y.; Gu, L.; Dong, X. L.; Sun, J. P.; Jin, K. J.; Cheng, J. G., Pressure-induced monotonic enhancement of T_c to over 30 K in superconducting Pr₀.₈₂Sr₀.₁₈NiO₂ thin films. Nat. Commun. 2022, 13 (1), 4367.
  6. [6]Osada, M.; Wang, B. Y.; Goodge, B. H.; Harvey, S. P.; Lee, K.; Li, D.; Kourkoutis, L. F.; Hwang, H. Y., Nickelate Superconductivity without Rare-Earth Magnetism: (La,Sr)NiO₂. Adv. Mater. 2021, 33 (45), 2104083.DOI
  7. [7]Zeng, S.; Li, C.; Chow, L. E.; Cao, Y.; Zhang, Z.; Tang, C. S.; Yin, X.; Lim, Z. S.; Hu, J.; Yang, P.; Ariando, A., Superconductivity in infinite-layer nickelate La₁₋ₓCaₓNiO₂ thin films. Sci. Adv. 2022, 8 (7), eabl9927.DOI
  8. [8]Pan, G. A.; Ferenc Segedin, D.; LaBollita, H.; Song, Q.; Nica, E. M.; Goodge, B. H.; Pierce, A. T.; Doyle, S.; Novakov, S.; Córdova Carrizales, D.; N’Diaye, A. T.; Shafer, P.; Paik, H.; Heron, J. T.; Mason, J. A.; Yacoby, A.; Kourkoutis, L. F.; Erten, O.; Brooks, C. M.; Botana, A. S.; Mundy, J. A., Superconductivity in a quintuple-layer square-planar nickelate. Nat. Mater. 2022, 21 (2), 160-164.DOI
  9. [9]Ferenc Segedin, D.; Goodge, B. H.; Pan, G. A.; Song, Q.; LaBollita, H.; Jung, M.-C.; El-Sherif, H.; Doyle, S.; Turkiewicz, A.; Taylor, N. K.; Mason, J. A.; N’Diaye, A. T.; Paik, H.; El Baggari, I.; Botana, A. S.; Kourkoutis, L. F.; Brooks, C. M.; Mundy, J. A., Limits to the strain engineering of layered square-planar nickelate thin films. Nat. Commun. 2023, 14 (1), 1468.DOI
  10. [10]Sun, H.; Huo, M.; Hu, X.; Li, J.; Liu, Z.; Han, Y.; Tang, L.; Mao, Z.; Yang, P.; Wang, B.; Cheng, J.; Yao, D.-X.; Zhang, G.-M.; Wang, M., Signatures of superconductivity near 80 K in a nickelate under high pressure. Nature 2023, 621 (7979), 493-498.DOI
  11. [11]Wang, L.; Li, Y.; Xie, S.-Y.; Liu, F.; Sun, H.; Huang, C.; Gao, Y.; Nakagawa, T.; Fu, B.; Dong, B.; Cao, Z.; Yu, R.; Kawaguchi, S. I.; Kadobayashi, H.; Wang, M.; Jin, C.; Mao, H.-K.; Liu, H., Structure Responsible for the Superconducting State in La₃Ni₂O₇ at High-Pressure and Low-Temperature Conditions. J. Am. Chem. Soc. 2024, 146 (11), 7506-7514.DOI
  12. [12]Xu, M.; Huyan, S.; Wang, H.; Bud'ko, S. L.; Chen, X.; Ke, X.; Mitchell, J. F.; Canfield, P. C.; Li, J.; Xie, W., Pressure-Dependent “Insulator–Metal–Insulator” Behavior in Sr-Doped La₃Ni₂O₇. Adv. Electron. Mater. 2024, 2400078.arxiv.org/abs/2312.14251
  13. [13]13.Geisler, B.; Hamlin, J. J.; Stewart, G. R.; Hennig, R. G.; Hirschfeld, P. J., Structural transitions, octahedral rotations, and electronic properties of A₃Ni₂O₇ rare-earth nickelates under high pressure. npj Quantum Mater. 2024, 9 (1), 38.DOI
  14. [14]Rhodes, L. C.; Wahl, P., Structural routes to stabilize superconducting La₃Ni₂O₇ at ambient pressure. Phys. Rev. Mater. 2024, 8 (4), 044801.DOI
  15. [15]Wang, H.; Chen, L.; Rutherford, A.; Zhou, H.; Xie, W., Long-Range Structural Order in a Hidden Phase of Ruddlesden–Popper Bilayer Nickelate La₃Ni₂O₇. Inorg. Chem. 2024, 63 (11), 5020-5026.DOI
  16. [16]Sheldrick, G., SHELXT - Integrated space-group and crystal-structure determination. Acta Cryst. A 2015, 71 (1), 3-8.DOI
  17. [17]Sheldrick, G., Crystal structure refinement with SHELXL. Acta Cryst. C 2015, 71 (1), 3-8.DOI
  18. [18]Zhang, Z.; Greenblatt, M.; Goodenough, J. B., Synthesis, Structure, and Properties of the Layered Perovskite La₃Ni₂O₇−δ. J. Solid State Chem. 1994, 108 (2), 402-409.DOI
  19. [19]Ling, C. D.; Argyriou, D. N.; Wu, G.; Neumeier, J. J., Neutron Diffraction Study of La₃Ni₂O₇: Structural Relationships Among n = 1, 2, and 3 Phases Laₙ₊₁NiₙO₃ₙ₊₁. J. Solid State Chem. 2000, 152 (2), 517-525.DOI
  20. [20]Voronin, V. I.; Berger, I. F.; Cherepanov, V. A.; Gavrilova, L. Y.; Petrov, A. N.; Ancharov, A. I.; Tolochko, B. P.; Nikitenko, S. G., Neutron diffraction, synchrotron radiation and EXAFS spectroscopy study of crystal structure peculiarities of the lanthanum nickelates Laₙ₊₁NiₙOᵧ (n = 1, 2, 3). Nucl. Instrum. Methods Phys. Res. A 2001, 470 (1), 202-209.DOI
  21. [21]Zhang, J.; Zheng, H.; Chen, Y.-S.; Ren, Y.; Yonemura, M.; Huq, A.; Mitchell, J. F., High oxygen pressure floating zone growth and crystal structure of the metallic nickelates R₄Ni₃O₁₀ (R = La, Pr). Phys. Rev. Mater. 2020, 4 (8), 083402.DOI
  22. [22]Chen, X.; Zhang, J.; Thind, A. S.; Sharma, S.; LaBollita, H.; Peterson, G.; Zheng, H.; Phelan, D. P.; Botana, A. S.; Klie, R. F.; Mitchell, J. F., Polymorphism in the Ruddlesden–Popper Nickelate La₃Ni₂O₇: Discovery of a Hidden Phase with Distinctive Layer Stacking. J. Am. Chem. Soc. 2024, 146 (6), 3640-3645.DOI
  23. [23]23.Puphal, P.; Reiss, P.; Enderlein, N.; Wu, Y.-M.; Khaliullin, G.; Sundaramurthy, V.; Priessnitz, T.; Knauft, M.; Richter, L.; Isobe, M.; van Aken, P. A.; Takagi, H.; Keimer, B.; Eren Suyolcu, Y.; Wehinger, B.; Hansmann, P.; Hepting, M., Unconventional crystal structure of the high-pressure superconductor La₃Ni₂O₇. 2023, arXiv:2312.07341.
  24. [24]Park, J.-C.; Kim, D.-K.; Byeon, S.-H.; Kim, D., XANES study on Ruddlesden-Popper phase, Laₙ₊₁NiₙO₃ₙ₊₁ (n = 1, 2, and ∞). J. Synchrotron Rad. 2001, 8 (2), 704-706.pubmed.ncbi.nlm.nih.gov/11512902
  25. [25]Poltavets, V. V.; Lokshin, K. A.; Dikmen, S.; Croft, M.; Egami, T.; Greenblatt, M., La₃Ni₂O₆: A New Double T-type Nickelate with Infinite Ni¹⁺/²⁺O₂ Layers. J. Am. Chem. Soc. 2006, 128 (28), 9050-9051.
  26. [26]Poltavets, V. V.; Lokshin, K. A.; Egami, T.; Greenblatt, M., The oxygen deficient Ruddlesden–Popper La₃Ni₂O₇−δ (δ = 0.65) phase: Structure and properties. Mater. Res. Bull. 2006, 41 (5), 955-960.DOI
  27. [27]Shannon, R., Revised effective ionic radii and systematic studies of interatomic distances in halides and chalcogenides. Acta Cryst. A 1976, 32 (5), 751-767.DOI
  28. [28]Ling, C. D.; Millburn, J. E.; Mitchell, J. F.; Argyrıou, D. N.; Linton, J.; Bordallo, H. N., Interplay of spin and orbital ordering in the layered colossal magnetoresistance manganite La₂₋₂ₓSr₁₊₂ₓMn₂O₇ (0.5 ≤ x ≤ 1.0). Phys. Rev. B 2000, 62 (22), 15096-15111.DOI
  29. [29]Kumar, R. S.; Prabhakaran, D.; Boothroyd, A.; Nicol, M. F.; Cornelius, A., High-pressure structure of LaSr₂Mn₂O₇ bilayer manganite. J. Phys. Chem. Solids 2006, 67 (9), 2046-2050.DOI

Paper details

vlnc:W_wb82qm9s
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents