MoS2_{2}/Al0.68_{0.68}Sc0.32_{0.32}N negative capacitance field-effect transistors

Abstract

Al0.68_{0.68}Sc0.32_{0.32}N (AlScN) has gained attention for its outstanding ferroelectric properties, including a high coercive field and high remnant polarization. Although AlScN-based ferroelectric field-effect transistors (FETs) for memory applications have been demonstrated, a device for logic applications with minimal hysteresis has not been reported. This study reports on the transport characteristics of a MoS2_{2} negative capacitance FET (NCFET) based on an AlScN ferroelectric material. We experimentally demonstrate the effect of a dielectric layer in the gate stack on the memory window and subthreshold swing (SS) of the NCFET. We show that the hysteresis behavior of transfer characteristics in the NCFET can be minimized with the inclusion of a non-ferroelectric dielectric layer, which fulfills the capacitance-matching condition. Remarkably, we also observe the NC effect in MoS2_{2}/AlScN NCFETs arrays based on large-area monolayer MoS2_{2} synthesized by chemical vapor deposition, showing the SS values smaller than its thermionic limit (~36-60 mV/dec) and minimal variation in threshold voltages (< 20 mV).

Main Text

The advancement of integrated circuit designs has heavily relied on the principles of Dennard scaling to maintain a constant power density as transistor dimensions continue to decrease.[1] However, as transistors reach nanoscale dimensions, reducing the supply voltage (VddV_{\mathrm{dd}}) becomes difficult without increasing leakage current (IoffI_{\mathrm{off}}) and sacrificing on-state current (IonI_{\mathrm{on}}).[1, 2] Given that power density is directly proportional to Vdd2V_{\mathrm{dd}}^{2}, alternative approaches to further scale VddV_{\mathrm{dd}} are imperative to overcome this challenge of power dissipation.[3] A promising solution lies in overcoming the room-temperature (RT) thermionic limit of ~60 mV/dec for subthreshold swing (SS), as achieving a steeper switching behavior allows the transistor to maintain the same IonI_{\mathrm{on}} at lower VddV_{\mathrm{dd}} without an increase in IoffI_{\mathrm{off}}.[2] To overcome the thermionic limit, negative capacitance field-effect transistors (NCFETs) present a novel approach by incorporating a ferroelectric material in the gate stack. According to the Landau-Ginzburg-Devonshire (LGD) theory, ferroelectrics possess a metastable region in their polarization-dependent energy landscape that exhibits NC.[4, 5] By introducing a ferroelectric insulator layer in the gate stack, SS can be reduced to less than 60 mV/dec at RT, as we can have CsCins<0\frac{C_{\mathrm{s}}}{C_{\mathrm{ins}}}<0 in the following expression for SS:

SS=2.3kBTq(∂Vg∂ψs)=2.3kBTq(1+CsCins)(1)SS = \frac{2.3k_{\mathrm{B}}T}{q}\left(\frac{\partial V_{\mathrm{g}}}{\partial\psi_{\mathrm{s}}}\right) = \frac{2.3k_{\mathrm{B}}T}{q}\left(1+\frac{C_{\mathrm{s}}}{C_{\mathrm{ins}}}\right) \tag*{(1)}

, where 2.3kBTq\frac{2.3k_{\mathrm{B}}T}{q} is the thermionic limit at 300 K (~60 mV/dec), and CsC_{\mathrm{s}} and CinsC_{\mathrm{ins}} are the semiconductor and gate insulator capacitance respectively.[6]

However, despite extensive research on ferroelectric materials and theoretical frameworks of the NC effect, achieving reliable hysteresis-free steep switching in NCFETs has been challenging.[4, 5, 7] The main difficulty is stabilizing the NC effect in the NCFET, which requires incorporating a conventional, non-ferroelectric dielectric as an interlayer in series with the ferroelectric material in the gate stack.[7] This creates a stable energy minimum in the NC region while reducing device hysteresis.[7] To eliminate hysteresis, the overall capacitance of the device must be positive, which can be achieved by ensuring that the magnitude of the ferroelectric capacitance (∣CFE∣|C_{\mathrm{FE}}|) remains higher than the combination of all remaining capacitances (CREMC_{\mathrm{REM}}).[7]

Using the LGD theory, one can obtain the following approximation for ∣CFE∣|C_{\mathrm{FE}}| of a ferroelectric material with a certain thickness (tFEt_{\mathrm{FE}}) as follows:[8, 9]

∣CFE∣≈233PrEctFE(2)|C_{\mathrm{FE}}| \approx\frac{2}{3\sqrt{3}}\frac{P_{\mathrm{r}}}{E_{\mathrm{c}}t_{\mathrm{FE}}} \tag*{(2)}

As suggested by Equation (2), it is preferable to use a ferroelectric material with a large remnant polarization (PrP_{\mathrm{r}}) and coercive field (EcE_{\mathrm{c}}) to obtain a high ∣CFE∣|C_{\mathrm{FE}}|.[8, 9] Furthermore, the S-shaped polarization-electric field (PP-EE) characteristics indicate that larger EcE_{\mathrm{c}} values could expand the NC region, which maintains the NC effect over a wide range of gate voltage (VgV_{\mathrm{g}}) sweeps.[8, 10]

Recently discovered wurtzite-structured Al1−xScxN\mathrm{Al}_{1-x}\mathrm{Sc}_{x}\mathrm{N} (AlScN) possesses unique ferroelectric properties,[11, 12, 13] surpassing other thin-film ferroelectrics such as HfxZryO2\mathrm{Hf}_{x}\mathrm{Zr}_{y}\mathrm{O}_{2} and Pb[ZrxTi1−x]O3\mathrm{Pb}[\mathrm{Zr}_{x}\mathrm{Ti}_{1-x}]\mathrm{O}_{3} in PrP_{\mathrm{r}} and EcE_{\mathrm{c}}.[14] AlScN exhibits substantially higher PrP_{\mathrm{r}} ranging from ∼70\sim70 to 110 μC/cm2\mu\mathrm{C}/\mathrm{cm}^{2} and EcE_{\mathrm{c}} between ∼2\sim2 and 9 MV/cm\mathrm{MV}/\mathrm{cm}, both of which can be adjusted by modifying the Sc doping levels.[11, 12] Consequently, AlScN provides a highly tunable platform for ferroelectric NC devices. Additionally, AlScN demonstrates excellent thermal stability of ferroelectric properties, maintaining its ferroelectricity over 1,000 °C.[14] It can also be deposited at low temperatures (< 300-400 °C) compatible with industry-standard Back-End-of-Line processes.[13] However, despite these desirable characteristics, no AlScN-based NCFETs have been reported yet.

Here, we report NCFETs using few-layer and monolayer MoS2\mathrm{MoS}_{2} channels and an Al0.68Sc0.32N\mathrm{Al}_{0.68}\mathrm{Sc}_{0.32}\mathrm{N} ferroelectric material in the gate-dielectric stack. MoS2\mathrm{MoS}_{2} is used for the semiconducting channel due to its near-constant channel capacitance enabling steep switching over large current ranges.[8] We studied the effect of the interlayer on the hysteresis and SS characteristics of AlScN-based NCFETs using various interlayer materials (AlOx\mathrm{AlO}_{x}, HfOx\mathrm{HfO}_{x}, and hexagonal BN (h-BN)) and thicknesses (0.5–2 nm). Notably, we observe HfOx\mathrm{HfO}_{x}/AlScN-based NCFET devices with sub-thermionic SS value (∼30.7\sim30.7 mV/dec) with a reduced shift in threshold voltage (VthV_{\mathrm{th}}).

Figure 1a illustrates the cross-sectional schematic of our fabricated NCFETs (see also Figure S1). The device consists of a semiconducting channel made from mechanically exfoliated few-layer MoS2\mathrm{MoS}_{2}, while a 45-nm-thick Al0.68Sc0.32N\mathrm{Al}_{0.68}\mathrm{Sc}_{0.32}\mathrm{N} layer deposited on Pt(111) functions as the ferroelectric gate insulator. In/Au is selected as S source and drain (S/D) contact electrodes to minimize the possibility of developing a degraded contact interface due to chemical interaction between MoS2_2 and the contact. [15, 16] For the interlayer, HfOx_x and AlOx_x with various thicknesses are deposited, and h-BN is inserted via a wet transfer method (see Supplementary Methods for more details on device fabrication). Figure 1b shows a representative optical micrograph of the fabricated NCFETs with a few-layer MoS2_2 channel (green) and In/Au contacts (gold).

Schematic, optical image, and electrical characterization of a MoS2/AlScN NCFET

Figure 1. (a) Schematic of MoS2_2/AlScN NCFET with a dielectric interlayer. (b) Optical microscope image showing mechanically exfoliated MoS2_2 along with patterned electrodes. (c) Semilogarithmic scale transfer characteristics of devices with only oxide dielectric (i.e., SiO2_2/Si) and only ferroelectric AlScN layer (i.e., AlScN/Pt). Both curves measured at VdsV_{\mathrm{ds}} = 1 V and VgV_{\mathrm{g}} from -12 to 12 V. (d-g) Electrical characterizations of capacitance matched NCFETs with AlScN and 1-nm-thick HfOx_x layer. (d) Semilogarithmic scale transfer characteristic of the NCFET, measured at VdsV_{\mathrm{ds}} of 0.1 V (blue) and 1 V (red) (VdsV_{\mathrm{ds}} step: 50 mV). (e) Corresponding SS vs. IdsI_{\mathrm{ds}} plot under the backward VgV_{\mathrm{g}} sweep, indicating the SSmin⁡\mathrm{SS}_{\min} of ∼\sim63.9 mV/dec. (f) Output characteristic of MoS2_2 NCFET with a VdsV_{\mathrm{ds}} step size of 0.1 V. (g) Corresponding conductance (gdsg_{\mathrm{ds}}) depending on VdsV_{\mathrm{ds}} at the VgV_{\mathrm{g}} of 5 V.

Schematic of MoS₂/AlScN NCFET with a dielectric interlayer

Figure S1. Schematic of MoS2_2/AlScN NCFET with a dielectric interlayer. The contact pads are directly deposited onto the oxide interlayer surface. NCFETs with mechanically exfoliated flakes and CVD-grown MoS2_2 have the same device configuration as depicted. Note that, the device configuration described differs from the one previously reported for the MoS2_2/AlScN FeFET case.[4] In this particular instance, the MoS2_2 layer exists below the contact pad, which is a result of the channel defining process after S/D deposition.

Figure 1c shows transfer characteristics of two different FETs under the VgV_g range from -12 V to 12 V; one with only the AlScN layer (blue) and the other with only a normal dielectric oxide layer (SiO2_2/Si; orange). The AlScN-only FET is referred to as ferroelectric FET (FeFET), commonly used in memory applications due to its ability to provide a large memory window (MW) in the transfer characteristics, which corresponds to a shift in VthV_{\mathrm{th}} (e.g., MW of ~6.0 V in Figure 1c). However, the large MW is undesirable in digital logic devices, and thus we focus on minimizing MW (i.e., VthV_{\mathrm{th}} shift) later in this paper. The FeFET exhibits a counterclockwise hysteresis curve that is indicative of ferroelectric gating, as a non-volatile, reduced channel conductance remains at a high VgV_g regime.[17] On the other hand, the FET with SiO2_2 layer with a thickness of 50 nm (without AlScN) shows a clockwise hysteresis curve, mainly caused by charge traps at the dielectric/MoS2_2 interface.[17]

In Figure 1d, the transfer characteristics of a FET incorporating both AlScN and a 1-nm-thick HfOx_x interlayer are presented. The HfOx_x/AlScN FET demonstrates significantly reduced hysteresis in the switching behavior. The modulation of VthV_{\mathrm{th}} due to sweep direction is only ~0.7 V, which is smaller than that in a normal FeFET without any interlayer (~1.1 V in Figure S2). The smaller VthV_{\mathrm{th}} shift of HfOx_x/AlScN FET can be attributed to the overall device capacitance being more positive and approaching the NCFET capacitance matching condition. The counterclockwise hysteresis curve observed in the HfOx_x/AlScN device further confirms that the dominating switching behavior is attributed to the ferroelectricity of AlScN rather than the effect of interfacial charge traps.

Semilogarithmic scale transfer characteristic of MoS2/AlScN FeFET

Figure S2. Semilogarithmic scale transfer characteristic of MoS2/AlScN\mathrm{MoS}_2/\mathrm{AlScN} FeFET without any interlayers, measured at VdsV_{\mathrm{ds}} of 1 V and VgV_{\mathrm{g}} range of -5 to 5 V.

The MoS2_2/HfOx_x/AlScN NCFET exhibits negative drain-induced barrier lowering (DIBL), since the IdsI_{\mathrm{ds}} values are higher for VgV_g values smaller than VthV_{\mathrm{th}} when measured at drain-source voltage (VdsV_{\mathrm{ds}}) of 0.1 V vs. 1.0 V (Figure 1d). This observation further supports our claim of observation of NC in these devices.[7, 18] In addition, the minimum SS (SSmin⁡_{\min}) achieved during the backward VgV_g sweep (∼\sim63.9 mV/dec) is close to the thermionic limit of ∼\sim60 mV/dec at RT, as illustrated in the SS-IdsI_{\mathrm{ds}} plot in Figure 1e. The significantly lower SSmin⁡\mathrm{SS}_{\min} value compared to the AlScN-only FeFET (∼\sim209 mV/dec) and SiO2_2-only FET (∼\sim1,558 mV/dec) indicates the stacked gate structure with matched capacitance effectively reduces the SS. Note that, the SSmin⁡\mathrm{SS}_{\min} can be even smaller (∼\sim46 mV/dec) when decreasing VdsV_{\mathrm{ds}} step size from 50 mV to 5 mV (Figure S3), which proves the robust NC effect irrespective of sweep speeds.[19] Figure 1f presents the IdsI_{\mathrm{ds}}-VdsV_{\mathrm{ds}} characteristics of the same MoS2_2 NCFET. At high VgV_{\mathrm{g}} bias (5 V), negative differential resistance (NDR) is observed (Figure 1g). The NDR effect is believed to be caused by the negative DIBL effect and/or the self-heating effect resulting from large drain current and voltage in the NCFET[7, 9, 18, 20, 21] providing additional support to our claims of an NCFET effect in these devices.

Transfer characteristic and corresponding SS-$I_{\mathrm{ds}}$ plot of MoS$_2$ NCFET

Figure S3. (a) Transfer characteristic of MoS2_2 NCFET with a small VgV_{\mathrm{g}} step size of 5 mV. The 1.0 nm HfOx_x IL is used for capacitance matching. (b) Corresponding SS-IdsI_{\mathrm{ds}} plot showing the SSmin⁡_{\min} of ∼\sim46 mV/dec.

To comprehensively investigate the impact of dielectric interlayers on the performance of NCFETs, we have fabricated devices with mechanically exfoliated few-layer MoS2_2 channels incorporating various interlayer materials and thicknesses. The corresponding transfer curves are presented in Figure 2a-Figure 2f, allowing for a systematic understanding of how the thickness and type of the interlayer dielectric affect the transport characteristics of NCFETs. All the transfer curves clearly demonstrate the dependence of SS and MW on the type and thickness of the interlayer dielectric. Interestingly, in Figure 2a-Figure 2f, a reduction in MW to values below ∼500 mV is observed, regardless of the interlayer type. Notably, all curves exhibit the counterclockwise hysteric behavior, with an Ion/IoffI_{\mathrm{on}}/I_{\mathrm{off}} greater than ∼10510^{5} indicating that the ferroelectric switching is actively occurring during VgV_{\mathrm{g}} sweep of the device.

Transfer characteristics for mechanically exfoliated MoS$_2$-based NCFETs with interlayers of HfO$_x$, AlO$_x$, and h-BN

Figure 2. Transfer characteristics for mechanically exfoliated MoS2_2-based NCFETs with an interlayer of (a) 0.5 nm thick HfOx_x, (b) 1 nm thick HfOx_x, (c) 1.5 nm thick HfOx_x, (d) 1.0 nm thick AlOx_x, (e) 1.5 nm thick AlOx_x, (f) 1 nm thick hexagonal BN (h-BN). All curves were measured at Vds=1V_{\mathrm{ds}} = 1 V with a step size of 50 mV. The corresponding SS vs. IdsI_{\mathrm{ds}} plots are shown in Figure S4.

We find that interlayers with higher dielectric constants result in steeper SS values at a constant thickness. Due to the high dielectric constant (i.e., kk of ∼16-25) of HfOx_x, it exhibits the lowest SS values, as indicated in Figure 2a-Figure 2c. Interlayers composed of high-kk dielectrics are expected to exhibit a higher capacitance (CILC_{\mathrm{IL}}). It is clear from Equation (1) that to achieve a sub-thermionic SS value, the factor (1+CsCins)=(1+CsCIL−Cs∣CFE∣)\left(1+\frac{C_{\mathrm{s}}}{C_{\mathrm{ins}}}\right)=\left(1+\frac{C_{\mathrm{s}}}{C_{\mathrm{IL}}}-\frac{C_{\mathrm{s}}}{\lvert C_{\mathrm{FE}}\rvert}\right) must be less than 1. Consequently, the SS of NCFET with a ∣CFE∣\lvert C_{\mathrm{FE}}\rvert is expressed as follows:

SS=2.3kBTq(1+CsCIL−Cs∣CFE∣)(3)SS=\frac{2.3k_{\mathrm{B}}T}{q}\left(1+\frac{C_{\mathrm{s}}}{C_{\mathrm{IL}}}-\frac{C_{\mathrm{s}}}{\lvert C_{\mathrm{FE}}\rvert}\right) \tag*{(3)}

Given Equations (2) and (3), to have a SS smaller than 60 meV/dec, the condition of ∣CFE∣<CIL\lvert C_{\mathrm{FE}}\rvert<C_{\mathrm{IL}} must be met, and increasing the CILC_{\mathrm{IL}} assists in maintaining this relationship.[22] To this end, we successfully demonstrate a sub-thermionic SSmin⁡_{\min} value of ∼30.6 mV/dec for the 0.5 nm thick HfOx_x device, as shown in Figure 2a (the corresponding SS vs. IdsI_{\mathrm{ds}} curve is shown in Figure S4.).

SS vs $I_{\mathrm{ds}}$ curves of MoS$_2$ with HfO$_x$ interlayers

Figure S4. SS vs IdsI_{\mathrm{ds}} curves of MoS2_2 with (a) 0.5 and (b) 1.0 nm thickness HfOx_x interlayer. The corresponding transfer curves are presented in Figure 2a, Figure 2b.

Equation (2) also indicates that interlayers with greater thickness can lead to higher SS values due to the inverse relationship between CILC_{\mathrm{IL}} and dielectric thickness. Figure 3a illustrates how the SS extracted from our devices appropriately conforms to the expected trend based on the dielectric constant and thickness of the interlayer. Furthermore, Figure 3b demonstrates an excellent linear fit to a SS vs. 1CIL\frac{1}{C_{\mathrm{IL}}} plot for the devices with the HfOx_x and h-BN interlayers. By extrapolating to the intercept of 1CIL=0\frac{1}{C_{\mathrm{IL}}}=0, where SS=\frac{2.3k_{\mathrm{B}}T}{q}\left(1-\frac{C_{\mathrm{s}}{\lvert C_{\mathrm{FE}}\rvert}\right)}, we can extract a range for ∣CFE∣\lvert C_{\mathrm{FE}}\rvert values by using appropriate values of CsC_{\mathrm{s}}. To this end, we approximate the MoS2_2 channel as a conventional dielectric as its charge screening length (∼\sim7 nm) is larger than the channel thickness of our device.[23] Accounting for the variability in the number of MoS2_2 layers due to exfoliation and utilizing previously reported few-layer dielectric constants for the material,[24] we use CsC_{\mathrm{s}} values range of 2.532.53 to 3.793.79 μF/cm2\mu\mathrm{F}/\mathrm{cm}^{2}. This in turn allows us to extract a range of CFEC_{\mathrm{FE}} values between −2.18-2.18 and −3.26-3.26 μF/cm2\mu\mathrm{F}/\mathrm{cm}^{2}. Note that, the extracted CFEC_{\mathrm{FE}} of our 45-nm-thick AlScN (−2.18-2.18 to −3.26-3.26 μF/cm2\mu\mathrm{F}/\mathrm{cm}^{2}) is lower in magnitude compared to the calculated CFEC_{\mathrm{FE}} of the 20-nm-thick ferroelectric HfxZryO2\mathrm{Hf}_{x}\mathrm{Zr}_{y}\mathrm{O}_{2} (∼−13.1\sim-13.1 μF/cm2\mu\mathrm{F}/\mathrm{cm}^{2});[7] however, the NC value for AlScN/MoS2_2 system will likely be enhanced as the AlScN layer is scaled to lower thickness (tFEt_{\mathrm{FE}}) with an accompanying increase in EcE_{\mathrm{c}} in accordance with Equation (2).

Extracted SSmin values as a function of interlayer type and thickness, and SSmin versus 1/CIL scatter plot

Figure 3. (a) Extracted SSmin⁡SS_{\min} values as a function of interlayer type and thickness. (b) SSmin⁡SS_{\min} vs. 1CIL\frac{1}{C_{\mathrm{IL}}} scatter plot. To account for variability in the dielectric constant of HfOx_x, CILC_{\mathrm{IL}} values are calculated assuming k=16k = 16 and k=25k = 25.

As mechanical exfoliation is unsuitable for large-area applications, we additionally fabricated FeFETs and NCFETs utilizing large-area monolayer MoS2_2 grown through chemical vapor deposition (CVD), as depicted in Figure 4a (and Figure S5). The device configuration is the same as those using mechanically exfoliated flakes to ensure its comparable capacitance network (see Figure S1 and Supplementary Methods). The transfer curves of the MoS2_2/AlScN FeFET devices (without dielectric interlayers) exhibit sub-thermionic SSSS switching behavior (Figure 4b). The minimum observed SSmin⁡SS_{\min} values of the six devices are calculated (Figure 4c) and listed (Figure 4d), and the steepest SSSS is confirmed to be ∼36\sim36 mV/dec. Importantly, all six devices demonstrate steep SSmin⁡SS_{\min} values, which are the same or lower than the thermionic limit (< 60 mV/dec).

Optical microscope image and transfer characteristics of CVD MoS₂ NCFETs

Figure 4. (a) Optical microscope image of CVD MoS₂ NCFET array. (b) Transfer characteristics for various devices without interlayer (Vds=1V_{\mathrm{ds}} = 1 V). The inset shows the zoomed-in curves to highlight their SS values smaller than 60 mV/dec. (c) Corresponding SS-IdsI_{\mathrm{ds}} plot and (d) summary of SS of the devices without interlayer, displaying sub-60 mV/dec SS values. (e) Transfer characteristics for a device with 2 nm AlOx_x interlayer, and its (f) SS values depending on the IdsI_{\mathrm{ds}}. (g) IdsI_{\mathrm{ds}}-VgV_{\mathrm{g}} plot of representative NCFET with 0.9 nm thick HfOx_x interlayer, and (h) its corresponding SS vs. IdsI_{\mathrm{ds}}, demonstrating the SSmin⁡_{\min} of ∼51 mV/dec.

Electrical transport characteristics of MoS2 NCFETs

Figure S5. (a) OM image of a CVD-MoS2_2 NCFET with a HfOx_x 0.9 nm interlayer. (b, c) Transfer curves of the NCFET for a device shown in Figure 4g, Figure 4h in the main text, and (d) its output characteristics. (e-h) Electrical transport of a MoS2_2/HfOx_x/AlScN NCFET different from that introduced in the main text, showing (e) transfer curve, (f) zoomed-in transfer curve to highlight the negative DIBL, (g) output curve and (h) SS-IdsI_{\mathrm{ds}} plot.

On the other hand, CVD-MoS2_2 NCFET with a 2 nm thick interlayer of AlOx_x results in a nearly hysteresis-free transfer curve (Figure 4e) with an SSmin⁡SS_{\min} of ~90 mV/dec (Figure 4f). Additionally, the NCFET exhibits an Ion/IoffI_{\mathrm{on}}/I_{\mathrm{off}} exceeding ~105^{5}, despite the relatively narrow VgV_g sweep range of -3V to 3V, even with a total gate stack thickness of ~47 nm (~2 nm AlOx_x/~45 nm AlScN). Similar to the observations in the mechanically exfoliated samples, thicker dielectric interlayers lead to reduced hysteresis, though maintaining a steep SS below 60 mV/dec becomes challenging. The AlOx_x/AlScN-based NCFET follows a similar trend, necessitating a 2 nm thick dielectric layer to achieve minimal hysteresis (~20 mV).

As an interlayer, HfOx_x can surpass AlOx_x in achieving steeper SS in NCFETs at the same thickness due to higher kk. By utilizing the calculated CFEC_{\mathrm{FE}} from Figure 3, we determine the optimal thickness of the HfOx_x interlayer to be 0.9 nm using the capacitance-matching condition, ensuring minimal hysteresis in the CVD-MoS2_2 NCFET. The representative transfer curve and SS-IdsI_{\mathrm{ds}} plot of NCFET with a 0.9 nm-thick HfOx_x are shown in Figure 4g and Figure 4h, respectively. This specific NCFET exhibits a small MW of ~0.34 V and an SSmin⁡SS_{\min} of ~51 mV/dec. Notably, the extracted SSmin⁡SS_{\min} (~51 mV/dec) is smaller than that with the AlOx_x interlayer (~90 mV/dec in Figure 4e) and the RT-thermionic limit (~60 mV/dec). Moreover, this NCFET exhibits negative DIBL and NDR effects, confirming the occurrence of the NC effect (Figure S5). However, not all NCFETs display sub-thermionic SSmin⁡SS_{\min}; for example, the averaged MW and SSmin⁡SS_{\min} of the NCFETs with a 300-nm-long channel are ~69.7 ±\pm 12.1 mV/dec and ~0.26 ±\pm 0.15 V (average ±\pm standard deviation), possibly due to non-uniformity of channel quality and MoS2_2/AlScN interface (discussed later).

To analyze device-to-device variations and channel length (LL)-dependence on SSmin⁡_{\min}, the transfer characterization of NCFETs with varying LL (300–1,500 nm) is conducted. Figure 5a and Figure 5b display the overlayed transfer curves of 20 devices during the forward and backward sweep of VgV_{\mathrm{g}} respectively. As expected, the IonI_{\mathrm{on}} is highest when the LL is shortest (∼300 nm) (Figure 5c). The best IonI_{\mathrm{on}} approaches ∼9.0 μA/μm at Vds=1V_{\mathrm{ds}} = 1 V (and ∼0.91 μA/μm at Vds=0.1V_{\mathrm{ds}} = 0.1 V). Remarkably, this high IonI_{\mathrm{on}} is comparable to those of previously reported Hfx_xZry_yO2_2-based NCFETs with the mechanical exfoliated MoS2_2[7, 25, 26, 27, 28] and WSe2_2[29, 30] multilayers (∼10−2^{-2}–2 μA/μm at Vds=0.1V_{\mathrm{ds}} = 0.1 V) (Table S1). We also observe that the SSmin⁡_{\min} values increase over LL for our MoS2_2/HfOx_x/AlScN NCFETs (Figure 5d). Interestingly, this is contrary to the behavior for MoS2_2 MOSFETs (e.g., increase or unchanged SSmin⁡_{\min} as LL decreases),[31, 32] indicating that the transport characteristics are largely influenced by the NC effect rather than dielectric capacitances. However, sub-thermionic SSmin⁡_{\min} is only observed in three devices with a short LL of ~300 or ~600 nm (red points below the dashed line in Figure 5d). The CVD-grown large-area MoS2_2 possesses crystalline imperfections such as grain boundaries and sulfur vacancies, which may lead to defect-mediated variations on the channel (e.g., decreased CsC_{\mathrm{s}}, increased interfacial trap density, and field-induced defect migration),[33, 34, 35, 36] thus altering SSmin⁡SS_{\min}. Furthermore, the degradation of SSmin⁡SS_{\min} can be substantial as LL increases due to an increased number of line defects in longer CVD-MoS2_2 channels.[35] This suggests that using a shorter channel and maintaining a higher crystalline quality of 2D channel are key to achieving reproducible high performance in NCFETs.

Transfer curves and boxplot of subthreshold swing for CVD-MoS2/HfOx/AlScN NCFETs

Figure 5. (a, b) The overlayed transfer curves of 20 different CVD-MoS2_2/HfOx_x/AlScN NCFETs with a varying LL (300-1,500 nm) recorded during (a) forward sweep and (b) backward sweep of VgV_{\mathrm{g}} (VdsV_{\mathrm{ds}} = 1 V). (c) Representative transfer characteristics of the NCFETs with different LL, showing the counterclockwise hysteresis behavior. (d) Boxplot of SSmin⁡SS_{\min} depending on the LL, where the statistics show the median (lines in the boxes), standard deviations (error bars), and standard errors (boxes).

ChannelGate dielectric or ferroelectricInterlayerContact metalSSmin⁡SS_{\min} (mV/dec)ΔVth\Delta V_{\mathrm{th}} (mV)LchL_{\mathrm{ch}} (nm)IonI_{\mathrm{on}} (μA·μm) at Vds=0.1V_{\mathrm{ds}} = 0.1 VIon/IoffI_{\mathrm{on}}/I_{\mathrm{off}} ratioRef.
CVD, monolayer MoS2\mathrm{MoS_2}AlScNHfOx\mathrm{HfO_x} 0.9 nmIn/Au513403000.9110610^6This study
Mechanically Exfoliated MoS2\mathrm{MoS_2}CIPSh-BN 7.5 nmCr/Au289857001.96 (at Vds=0.5V_{\mathrm{ds}} = 0.5V)10710^75
Mechanically Exfoliated MoS2\mathrm{MoS_2}HZOAlOx\mathrm{AlO_x} 2 nmTi/Au17.2208325∗1065 * 10^66
Mechanically Exfoliated MoS2\mathrm{MoS_2}HZOAlOx\mathrm{AlO_x} 2 nmAu23772600210810^87
Mechanically Exfoliated WSe2\mathrm{WSe_2}HZOAlOx\mathrm{AlO_x} 4 nmPt18.2205000110610^68
Mechanically Exfoliated MoS2\mathrm{MoS_2}HZOAlOx\mathrm{AlO_x} 2 nmNi5.6122000110710^79
Mechanically Exfoliated MoS2\mathrm{MoS_2}HZOAlOx\mathrm{AlO_x} 6nmCr/Au17.64Negligible30000.810710^710
Mechanically Exfoliated WSe2\mathrm{WSe_2}HZOAlOx\mathrm{AlO_x} 2 nmPt/Au40.2∼200\sim20050010−210^{-2}>105>10^511
Mechanically Exfoliated WSe2\mathrm{WSe_2}HfOx/Ni/AlOx/HZO\mathrm{HfO_x/Ni/AlO_x/HZO} (10/20/3/20 nm)AlOx\mathrm{AlO_x} 2 nmPt/Au14.4∼120\sim120100010−210^{-2}10510^511

Table S1. Benchmarks of NCFETs with 2D semiconductor channels. For NCFETs with 2D channel, the 3D ferroelectric gate of CuInP2S6\mathrm{CuInP_2S_6} (CIPS), and Hf1−xZrxO2\mathrm{Hf_{1-x}Zr_xO_2} (HZO) were used.

In summary, we present the experimental realization of 2D NCFETs utilizing AlScN as the ferroelectric layer and MoS2\mathrm{MoS_2} as the channel. Sub-thermionic SSmin⁡SS_{\min} values as low as ∼\sim30.7 mV/dec, as well as negative DIBL in the transfer characteristics and an NDR effect in output characteristics, were successfully observed, providing clear evidence of the NC effect. By modulating the interlayer dielectric material and its thickness, we are able to reduce hysteresis and MW while simultaneously maintaining a steep SS. Our findings are a first step towards the application of AlScN, a versatile and tunable ferroelectric material, in steep-switching logic devices. Future work on these devices will involve optimizing AlScN composition and thickness together with interlayers for lower operating voltage NCFETs with sub-thermionic SS values for a large swing in current magnitudes.

Supplementary Material

See the supplementary material for Supplementary Methods and Figure S1-Figure 5.

Acknowledgement

D. J. and S.S. acknowledge support from AFOSR GHz-THz program grant number FA9550-23-1-0391. S.S. also acknowledges partial support for this work by Basic Science Research Program through the National Research Foundation of Korea (NRF) funded by the Ministry of Education (Grant No. 2021R1A6A3A14038492).

Author Declarations

Conflict of Interest

The authors declare that they have no conflicts of interest.

Author Contributions

D. J. supervised the study. S.S. and K.-H.K. fabricated the devices. S.S., K.-H.K., and S.C. performed the measurements. Z.H. and G.K. contributed to the discussion. K.Y.M. and H.S.S. grew and provided h-BN layers. R.H.O. contributed to the preparation of AlScN. S.S., K.-H. K. and S. C. wrote the manuscript.

DATA AVAILABILITY

The data that support the findings of this study are available from the corresponding author upon reasonable request.

MoS2_2/Al0.68_{0.68}Sc0.32_{0.32}N negative capacitance field-effect transistors

Seunguk Song; Kwan-Ho Kim; Srikrishna Chakravarthi; Zirun Han; Gwangwoo Kim; Kyung Yeol Ma; Hyeon Suk Shin; Roy H. Olsson III; Deep Jariwala

Supplementary material

  • Supplementary Methods

  • Figures S1-5

  • Supplementary References

Supplementary Methods

Fabrication of interlayer/AlScN/Pt sample

A 45 nm thick layer of Al0.68Sc0.32N\mathrm{Al}_{0.68}\mathrm{Sc}_{0.32}\mathrm{N} was deposited on pre-deposited Pt/SiO2/Si\mathrm{Pt}/\mathrm{SiO}_{2}/\mathrm{Si} using a pulsed-DC reactive sputtering deposition system (Evatec, CLUSTERLINE 200 II pulsed DC PVD).[1, 2] The co-sputtering process involved separate 4-inch Al and Sc targets, operated at 1250 W and 698 W, respectively, at a chuck temperature of 350 °C with 10 sccm of Ar gas flow and 25 sccm of N2\mathrm{N}_{2} gas flow under the constant pressure of ∼1.45×10−3\sim1.45 \times10^{-3} bar. The growth of AlScN was facilitated by the preferentially oriented (111) Pt on SiO2/Si\mathrm{SiO}_{2}/\mathrm{Si} substrates, which promoted highly textured ferroelectricity along the [1] direction. Following the preparation of AlScN/Pt/SiO2/Si\mathrm{AlScN}/\mathrm{Pt}/\mathrm{SiO}_{2}/\mathrm{Si}, oxide interlayers (ILs) were deposited using atomic layer deposition (ALD; Cambridge Nanotech S200 ALD). HfOx\mathrm{HfO}_{x} and AlOx\mathrm{AlO}_{x} ILs were grown using the precursors of [(CH3)2N]4Hf[(\mathrm{CH}_{3})_{2}\mathrm{N}]_{4}\mathrm{Hf} and Al2(CH3)6\mathrm{Al}_{2}(\mathrm{CH}_{3})_{6}, respectively, along with the H2O\mathrm{H}_{2}\mathrm{O} precursor at a temperature of 150 °C. The thickness of the ILs was controlled through the ALD cycles, considering their deposition rate of ∼0.9\sim0.9 Å/cycle for each oxide. The 3nm-thick-h-BN film was used as one of the interlayers in NCFETs, which was grown on a cc-plane sapphire substrate by a low-pressure chemical vapor deposition (CVD) method using ammonia borane powders as the precursor. The previous report[3] contains the specific experimental details for growth and the subsequent polymethyl methacrylate (PMMA)-wet transfer process for h-BN.

Fabrication of mechanically exfoliated MoS2 NCFETs

The align markers were deposited on the IL/AlScN/Pt/SiO2/Si sample using photolithography (SUSS MicroTec MA6 Gen3 Mask Aligner) and e-beam evaporation (Lesker PVD75 E-beam Evaporator) of Ti/Au with a thickness of 10/40 nm. Note that, the heat treatment up to 180 °C for 5 min was performed during the photoresist coating of LOR3A and S1813. Following that, mechanical exfoliation of MoS2 flakes was carried out, and annealing under Ar gas at 180 °C for 1 h was conducted to ensure proper adhesion between MoS2 and the substrate. Subsequently, the source and drain (S/D) contacts of In/Au (10/40 nm) were defined using e-beam lithography (EBL; Elionix ELS-7500EX) and thermal evaporation (Kurt J. Lesker Nano-36). The use of PMMAbased e-beam resist required a thermal budget process at 180 °C for 10 min. To prevent any high-energy process during the metal deposition process, the deposition rate was maintained below 0.03 Å/s. The Pt layer beneath the AlScN\mathrm{AlScN} served as a gate contact, and the gate contact exposure was achieved by wet etching of AlScN\mathrm{AlScN} through immersion in a KOH solution after fabricating the In/MoS2/IL/AlScN/Pt\mathrm{In/MoS_2/IL/AlScN/Pt} heterostructure. No additional heat treatment was conducted after the device fabrication.

Fabrication of CVD-grown MoS2\mathrm{MoS_2} NCFETs

A monolayer MoS2\mathrm{MoS_2} thin film, grown via CVD on a (0001) cc-cut sapphire substrate (purchased from 2D Semiconductors) was used for the NCFETs. The grain size of MoS2\mathrm{MoS_2} was random (∼1\sim1-20 μm\mu\mathrm{m}) and nearly continuous across the 1×1 cm21 \times1\ \mathrm{cm}^{2}. CVD-grown MoS2\mathrm{MoS_2} was transferred onto the oxide/AlScN/Pt/SiO2/Si\mathrm{oxide/AlScN/Pt/SiO_2/Si} sample using a KOH-based wet process. A polymeric supporting layer of PMMA was coated onto the MoS2\mathrm{MoS_2}/sapphire and then floated on a 0.1 M KOH solution to separate the MoS2\mathrm{MoS_2} from the sapphire substrate. The detached PMMA/MoS2\mathrm{MoS_2} free-standing layer was rinsed multiple times in distilled ionized water to prevent any damage to the AlScN\mathrm{AlScN} caused by residues from the KOH-based process. Following the transfer of PMMA/MoS2\mathrm{MoS_2} onto the AlScN\mathrm{AlScN} layer, the PMMA was removed using acetone. Subsequently, the channel-defining process was performed using EBL and a reactive ion etcher (RIE) with oxygen gas (Jupiter II RIE Plasma Etcher). The S/D electrodes were then deposited after the channel definition, utilizing the same method employed for mechanically exfoliated MoS2\mathrm{MoS_2} NCFETs. Etching the MoS2\mathrm{MoS_2} channel before depositing In/Au electrodes results in the same device capacitance network as when using a mechanically exfoliated flake. In this case, the contact pads are in direct contact with the dielectric interlayer surface, without any MoS2\mathrm{MoS_2} underneath (see Figure S1).

Supplementary References

  1. X. Liu, J. Zheng, D. Wang, P. Musavigharavi, E. A. Stach, R. Olsson, III and D. Jariwala, Applied Physics Letters 118 (20) (2021).

  1. X. Liu, D. Wang, K.-H. Kim, K. Katti, J. Zheng, P. Musavigharavi, J. Miao, E. A. Stach, R. H. Olsson, III and D. Jariwala, Nano Letters 21 (9), 3753-3761 (2021).

  1. A. R. Jang, S. Hong, C. Hyun, S. I. Yoon, G. Kim, H. Y. Jeong, T. J. Shin, S. O. Park, K. Wong, S. K. Kwak, N. Park, K. Yu, E. Choi, A. Mishchenko, F. Withers, K. S. Novoselov, H. Lim and H. S. Shin, Nano Letters 16 (5), 3360-3366 (2016).

  1. K.-H. Kim, S. Oh, M. M. A. Fiagbenu, J. Zheng, P. Musavigharavi, P. Kumar, N. Trainor, A. Aljarb, Y. Wan, H. M. Kim, K. Katti, S. Song, G. Kim, Z. Tang, J.-H. Fu, M. Hakami, V. Tung, J. M. Redwing, E. A. Stach, R. H. Olsson and D. Jariwala, Nature Nanotechnology (2023).

  1. X. Wang, P. Yu, Z. Lei, C. Zhu, X. Cao, F. Liu, L. You, Q. Zeng, Y. Deng, C. Zhu, J. Zhou, Q. Fu, J. Wang, Y. Huang and Z. Liu, Nature Communications 10 (1), 3037 (2019).

  1. G. Yang, J. Niu, C. Lu, R. Cao, J. Wang, Y. Zhao, X. Chuai, M. Li, D. Geng, N. Lu, Q. Liu, L. Li and M. Liu, presented at the 2020 IEEE International Electron Devices Meeting (IEDM), 2020 (unpublished).

  1. Z. Yu, H. Wang, W. Li, S. Xu, X. Song, S. Wang, P. Wang, P. Zhou, Y. Shi, Y. Chai and X. Wang, presented at the 2017 IEEE International Electron Devices Meeting (IEDM), 2017 (unpublished).

  1. J. Wang, X. Guo, Z. Yu, Z. Ma, Y. Liu, M. Chan, Y. Zhu, X. Wang and Y. Chai, presented at the 2018 IEEE International Electron Devices Meeting (IEDM), 2018 (unpublished).

  1. M. Si, C.-J. Su, C. Jiang, N. J. Conrad, H. Zhou, K. D. Maize, G. Qiu, C.-T. Wu, A. Shakouri, M. A. Alam and P. D. Ye, Nature Nanotechnology 13 (1), 24-28 (2018).

  1. L. Tu, R. Cao, X. Wang, Y. Chen, S. Wu, F. Wang, Z. Wang, H. Shen, T. Lin, P. Zhou, X. Meng, W. Hu, Q. Liu, J. Wang, M. Liu and J. Chu, Nature Communications 11 (1), 101 (2020).

  1. M. Si, C. Jiang, W. Chung, Y. Du, M. A. Alam and P. D. Ye, Nano Letters 18 (6), 3682-3687 (2018).

References

  1. [1]I. L. Markov, Nature 512 (7513), 147-154 (2014).
  2. [2]H. Amrouch, M. Rapp, S. Salamin and J. Henkel, in A Journey of Embedded and Cyber-Physical Systems: Essays Dedicated to Peter Marwedel on the Occasion of His 70th Birthday, edited by J.-J. Chen (Springer International Publishing, Cham, 2021), pp. 107-123.
  3. [3]S. Kumar, K. S. Singh and K. Nigam, presented at the 2022 8th International Conference on Signal Processing and Communication (ICSC), 2022 (unpublished).
  4. [4]E. Ko, J. Shin and C. Shin, Nano Convergence 5 (1), 2 (2018).
  5. [5]M. Hoffmann, F. P. G. Fengler, M. Herzig, T. Mittmann, B. Max, U. Schroeder, R. Negrea, P. Lucian, S. Slesazeck and T. Mikolajick, Nature 565 (7740), 464-467 (2019).
  6. [6]S. Salahuddin and S. Datta, Nano Letters 8 (2), 405-410 (2008).
  7. [7]M. Si, C.-J. Su, C. Jiang, N. J. Conrad, H. Zhou, K. D. Maize, G. Qiu, C.-T. Wu, A. Shakouri, M. A. Alam and P. D. Ye, Nature Nanotechnology 13 (1), 24-28 (2018).
  8. [8]Malvika, B. Choudhuri and K. Mummaneni, Journal of Electronic Materials 51 (3), 923-937 (2022).
  9. [9]Z. Xie, W. Lü, M. Guo and M. Zhao, Semiconductor Science and Technology 37 (3), 035001 (2022).
  10. [10]H. Agarwal, P. Kushwaha, Y. K. Lin, M. Y. Kao, Y. H. Liao, J. P. Duarte, S. Salahuddin and C. Hu, IEEE Electron Device Letters 39 (8), 1254-1257 (2018).
  11. [11]S. Fichtner, F. Lofink, B. Wagner, G. Schönweger, T. N. Kreutzer, A. Petraru and H. Kohlstedt, presented at the 2020 Joint Conference of the IEEE International Frequency Control Symposium and International Symposium on Applications of Ferroelectrics (IFCS-ISAF), 2020 (unpublished).
  12. [12]S. Fichtner, N. Wolff, F. Lofink, L. Kienle and B. Wagner, Journal of Applied Physics 125 (11) (2019).
  13. [13]K.-H. Kim, S. Oh, M. M. A. Fiagbenu, J. Zheng, P. Musavigharavi, P. Kumar, N. Trainor, A. Aljarb, Y. Wan, H. M. Kim, K. Katti, S. Song, G. Kim, Z. Tang, J.-H. Fu, M. Hakami, V. Tung, J. M. Redwing, E. A. Stach, R. H. Olsson and D. Jariwala, Nature Nanotechnology (2023).
  14. [14]K.-H. Kim, I. Karpov, R. H. Olsson and D. Jariwala, Nature Nanotechnology 18 (5), 422-441 (2023).
  15. [15]Y. Wang, J. C. Kim, R. J. Wu, J. Martinez, X. Song, J. Yang, F. Zhao, A. Mkhoyan, H. Y. Jeong and M. Chhowalla, Nature 568 (7750), 70-74 (2019).
  16. [16]S. Song, A. Yoon, J.-K. Ha, J. Yang, S. Jang, C. Leblanc, J. Wang, Y. Sim, D. Jariwala, S. K. Min, Z. Lee and S.-Y. Kwon, Nature Communications 13 (1), 4916 (2022).
  17. [17]X. Liu, D. Wang, K.-H. Kim, K. Katti, J. Zheng, P. Musavigharavi, J. Miao, E. A. Stach, R. H. Olsson, III and D. Jariwala, Nano Letters 21 (9), 3753-3761 (2021).
  18. [18]M. A. Alam, M. Si and P. D. Ye, Applied Physics Letters 114 (9) (2019).
  19. [19]Y. Wang, X. Bai, J. Chu, H. Wang, G. Rao, X. Pan, X. Du, K. Hu, X. Wang, C. Gong, C. Yin, C. Yang, C. Yan, C. Wu, Y. Shuai, X. Wang, M. Liao and J. Xiong, Advanced Materials 32 (46), 2005353 (2020).
  20. [20]H. Agarwal, P. Kushwaha, J. P. Duarte, Y. K. Lin, A. B. Sachid, M. Y. Kao, H. L. Chang, S. Salahuddin and C. Hu, IEEE Transactions on Electron Devices 65 (5), 2033-2039 (2018).
  21. [21]H. Zhou, D. Kwon, A. B. Sachid, Y. Liao, K. Chatterjee, A. J. Tan, A. K. Yadav, C. Hu and S. Salahuddin, presented at the 2018 IEEE Symposium on VLSI Technology, 2018 (unpublished).
  22. [22]W. Cao and K. Banerjee, Nature Communications 11 (1), 196 (2020).
  23. [23]S. Das and J. Appenzeller, Nano Letters 13 (7), 3396-3402 (2013).
  24. [24]Y. Kang, D. Jeon and T. Kim, The Journal of Physical Chemistry C 125 (6), 3611-3615 (2021).
  25. [25]X. Wang, P. Yu, Z. Lei, C. Zhu, X. Cao, F. Liu, L. You, Q. Zeng, Y. Deng, C. Zhu, J. Zhou, Q. Fu, J. Wang, Y. Huang and Z. Liu, Nature Communications 10 (1), 3037 (2019).
  26. [26]G. Yang, J. Niu, C. Lu, R. Cao, J. Wang, Y. Zhao, X. Chuai, M. Li, D. Geng, N. Lu, Q. Liu, L. Li and M. Liu, presented at the 2020 IEEE International Electron Devices Meeting (IEDM), 2020 (unpublished).
  27. [27]Z. Yu, H. Wang, W. Li, S. Xu, X. Song, S. Wang, P. Wang, P. Zhou, Y. Shi, Y. Chai and X. Wang, presented at the 2017 IEEE International Electron Devices Meeting (IEDM), 2017 (unpublished).
  28. [28]L. Tu, R. Cao, X. Wang, Y. Chen, S. Wu, F. Wang, Z. Wang, H. Shen, T. Lin, P. Zhou, X. Meng, W. Hu, Q. Liu, J. Wang, M. Liu and J. Chu, Nature Communications 11 (1), 101 (2020).
  29. [29]J. Wang, X. Guo, Z. Yu, Z. Ma, Y. Liu, M. Chan, Y. Zhu, X. Wang and Y. Chai, presented at the 2018 IEEE International Electron Devices Meeting (IEDM), 2018 (unpublished).
  30. [30]M. Si, C. Jiang, W. Chung, Y. Du, M. A. Alam and P. D. Ye, Nano Letters 18 (6), 3682-3687 (2018).
  31. [31]L. Xie, M. Liao, S. Wang, H. Yu, L. Du, J. Tang, J. Zhao, J. Zhang, P. Chen, X. Lu, G. Wang, G. Xie, R. Yang, D. Shi and G. Zhang, Advanced Materials 29 (37), 1702522 (2017).
  32. [32]A. Sebastian, R. Pendurthi, T. H. Choudhury, J. M. Redwing and S. Das, Nature Communications 12 (1), 693 (2021).
  33. [33]Y. Zhao, M. Tripathi, K. Černevičs, A. Avsar, H. G. Ji, J. F. Gonzalez Marin, C.-Y. Cheon, Z. Wang, O. V. Yazyev and A. Kis, Nature Communications 14 (1), 44 (2023).
  34. [34]V. K. Sangwan, H.-S. Lee, H. Bergeron, I. Balla, M. E. Beck, K.-S. Chen and M. C. Hersam, Nature 554 (7693), 500-504 (2018).
  35. [35]S. Najmaei, M. Amani, M. L. Chin, Z. Liu, A. G. Birdwell, T. P. O’Regan, P. M. Ajayan, M. Dubey and J. Lou, ACS Nano 8 (8), 7930-7937 (2014).
  36. [36]L. Wang, W. Liao, S. L. Wong, Z. G. Yu, S. Li, Y.-F. Lim, X. Feng, W. C. Tan, X. Huang, L. Chen, L. Liu, J. Chen, X. Gong, C. Zhu, X. Liu, Y.-W. Zhang, D. Chi and K.-W. Ang, Advanced Functional Materials 29 (25), 1901106 (2019).

Paper details

vlnc:W_wdvb4h2d
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents