betaFeedback

WorksPhysics and Astronomy

Superconductivity and normal-state properties of kagome metal RbV3Sb5 single crystals

Abstract

We report the discovery of superconductivity and detailed normal-state physical properties of RbV3Sb5 single crystals with V kagome lattice. RbV3Sb5 single crystals show a superconducting transition at Tc ~ 0.92 K. Meanwhile, resistivity, magnetization and heat capacity measurements indicate that it exhibits anomalies of properties at T* ~ 102 - 103 K, possibly related to the formation of charge ordering state. When T is lower than T*, the Hall coefficient RH undergoes a drastic change and sign reversal from negative to positive, which can be partially explained by the enhanced mobility of hole-type carriers. In addition, the results of quantum oscillations show that there are some very small Fermi surfaces with low effective mass, consistent with the existence of multiple highly dispersive Dirac band near the Fermi energy level.

Two-dimensional (2D) kagome lattice composed of corner-sharing triangles and hexagons is one of the most studied systems in the last decades due to its unique structural feature. On the one hand, if only the spin degree of freedom is considered, insulating magnetic kagome materials can host some exotic magnetism ground states, like quantum spin liquid state, because of the nature of strongly geometrical frustration for kagome lattice [1, 2, 3, 4]. On the other hand, when the charge degree of freedom becomes dominant (partial filling), the band topology starts to manifest its features in kagome metals, such as nontrivial Dirac points and flat band in the band structure [5, 6, 7]. More interestingly, when both of spin and charge degrees of freedom exist, many of exotic phenomena appear in the correlated magnetic kagome metals. For example, in ferromagnetic Fe₃Sn₂ and TbMn₆Sn₆ kagome metals, due to the spin orbital coupling and broken of time reversal symmetry, the Chern gap can be opened at the Dirac point, leading to large anomalous Hall effect (AHE), topological edge state and large magnetic-field tunability [8, 9, 10]. Moreover, antiferromagnetic Mn₃Sn and ferromagnetic Co₃Sn₂S₂ kagome metals exhibit large intrinsic AHE, which is related to the existence of Weyl node points in these materials [11, 12, 13].

Besides the intensively studied magnetic kagome metals, other correlation effects and ordering states in partially filled kagome lattice have also induced great interests. Theoretical studies suggest that the doped kagome lattice could lead to unconventional superconductivity [1, 14, 15, 16, 17]. Especially, when the kagome lattice is filled near van Hove filling, the Fermi surface (FS) is perfectly nested and has saddle points on the MM point of Brillouin zone (BZ) [16]. Depends on the variations of on-site Hubbard interaction UU and Coulomb interaction on nearest-neighbor bonds VV, the system can develop different ground states, including unconventional superconductivity, ferromagnetism, charge bond order and charge

density wave (CDW) order and so on [16, 17]. However, the realizations of superconducting and charge ordering states are still scarce in kagome metals.

In very recent, a novel family of kagome metals AV₃Sb₅ (A = K, Rb and Cs) was discovered [18]. Among them, KV₃Sb₅ and CsV₃Sb₅ exhibit superconductivity with transition temperature TcT_c = 0.93 and 2.5 K, respectively [19, 20]. The proximity-induced spin-triplet superconductivity was also observed in Nb/KV₃Sb₅ devices [21]. More importantly, theoretical calculations and angle-resolved photoemission spectroscopy (ARPES) demonstrate that there are several Dirac nodal points near the Fermi energy level (EFE_F) with a non-zero Z2Z_2 topological invariant in KV₃Sb₅ and CsV₃Sb₅ [18, 19, 20, 22]. Moreover, AV₃Sb₅ exhibits transport and magnetic anomalies at T∗∼80T^* \sim80 K - 110 K [18, 19, 20]. The X-ray diffraction (XRD) and scanning tunnelling microscopy (STM) measurements on KV₃Sb₅ and CsV₃Sb₅ indicate that there is a 2×22 \times2 superlattice emerging below T∗T^*, i.e., the formation of charge order (CDW-like state) [19, 23]. Furthermore, the STM spectra show that this charge order has a chiral anisotropy, which can be tuned by magnetic field and may lead to the anomalous Hall effect (AHE) at low temperature even KV₃Sb₅ does not exhibit magnetic order or local moments [22, 23, 24].

Motivated by these studies, in this work, we carried out a comprehensive study on physical properties of RbV₃Sb₅ single crystals. We find that RbV₃Sb₅ shows a superconducting transition at Tc∼0.92T_c \sim0.92 K, which co-exist with the anomalies of properties at T∗∼102T^* \sim102 - 103 K. This could be related to the emergence of charge ordering state. Below T∗T^*, the transport properties change significantly, possibly rooting in the dramatic changes of electronic structure due to the formation of charge order. Furthermore, the analysis of low-temperature quantum oscillations indicates that there are small Fermi surfaces (FSs) with low effective mass in RbV₃Sb₅, revealing the existence of highly dispersive bands near the Fermi energy level EFE_F.

Single crystals of RbV₃Sb₅ were grown from Rb ingot (purity 99.75%), V powder (purity 99.9%) and Sb grains (purity 99.999%) using the self-flux method [19]. The eutectic mixture of RbSb and Rb3_3Sb7_7 is mixed with VSb2_2 to form a composition with 50 at.% Rbx_xSby_y and 50 at.% VSb2_2 approximately. The mixture was put into an alumina crucible and sealed in a quartz ampoule under partial argon atmosphere. The sealed quartz ampoule was heated to 1273 K for 12 h and soaked there for 24 h. Then it was cooled down to 1173 K at 50 K/h and further to 923 K at a slowly rate. Finally, the ampoule was taken out from the furnace and decanted with a centrifuge to separate RbV3_3Sb5_5 single crystals from the flux. Except sealing and heat treatment procedures, all of other preparation processes were carried out in an argon-filled glove box in order to prevent the reaction of Rb with air and water. The obtained crystals have a typical size of 2 × 2 × 0.02 mm3^3. RbV3_3Sb5_5 single crystals are stable in the air. XRD pattern was collected using a Bruker D8 X-ray diffractometer with Cu Kα_\alpha radiation (λ=0.15418\lambda= 0.15418 nm) at room temperature. The elemental analysis was performed using the energy-dispersive X-ray spectroscopy (EDX). Electrical transport and heat capacity measurements were carried out in a Quantum Design physical property measurement system (PPMS-14T). The longitudinal and Hall electrical resistivity were measured using a five-probe method and the current flows in the abab plane of the crystal. The Hall resistivity was obtained from the difference in the transverse resistivity measured at the positive and negative fields in order to remove the longitudinal resistivity contribution due to the voltage probe misalignment, i.e., ρyx(μ0H)=[ρyx(+μ0H)−ρyx(−μ0H)]/2\rho_{yx}(\mu_0 H) = [\rho_{yx}(+\mu_0 H) - \rho_{yx}(-\mu_0 H)]/2. The c-axial resistivity was measured by attaching current and voltage wires on the opposite sides of the plate-like crystal. Magnetization measurements were performed in a Quantum Design magnetic property measurement system (MPMS3).

As shown in the left panel of Figure 1(a), RbV3_3Sb5_5 has a layered structure with hexagonal symmetry (space group P6/mmmP6/mmm, No. 191). It consists of Rb layer and V-Sb slab stacking along cc axis alternatively, isostructural to KV3_3Sb5_5 and CsV3_3Sb5_5 [18]. The key structural ingredient of this material is two-dimensional (2D) kagome layer formed by the V atoms in the V-Sb slab (right panel of Figure 1(a)). There are two kinds of Sb sites and the Sb atoms at Sb1 site occupy at the centers of V hexagons when another Sb atoms at Sb2 site locate below and above the centers of V triangles, forming graphene-like hexagon layers. The XRD pattern of a RbV3_3Sb5_5 single crystal (Figure 1(b)) reveals that the crystal surface is parallel to the (00ll)-plane. The estimated cc-axial lattice constant is about 9.114 Å, close to previously reported values [18]. The thin-plate-like crystals (inset of Figure 1(b)) are also consistent with the layered structure of RbV3_3Sb5_5. The measurement of EDX by examination of multiple points on the crystals gives the atomic ratio of Rb : V : Sb = 0.90(6) : 3 : 5.07(4) when setting the content of V as 3. The composition of Rb is slightly less than 1, indicating that there may be small amount of Rb

Image not extracted

Figure 1. (a) Crystal structure of RbV3_3Sb5_5. The big green, small red, medium blue and cyan balls represent Rb, V, Sb1 and Sb2 sites, respectively. (b) XRD pattern of a RbV3_3Sb5_5 single crystal. Inset: photo of typical RbV3_3Sb5_5 single crystals on a 1 mm grid paper.

deficiencies in the present RbV3_3Sb5_5 crystals. Figure 2(a) exhibits the temperature dependence of in-plane resistivity ρab(T)\rho_{ab}(T) and c-axial resistivity ρc(T)\rho_c(T) of RbV3_3Sb5_5 single crystal from 2 K to 300 K. The zero-field ρab(T)\rho_{ab}(T) exhibits a metallic behavior in the measured temperature range and the residual resistivity ratio (RRR), defined as ρab(300 K)/ρab(2 K)\rho_{ab}(300\ \mathrm{K})/\rho_{ab}(2\ \mathrm{K}), is about 44, indicating the high quality of crystals. At T∗∼103T^* \sim103 K, the ρab(T)\rho_{ab}(T) shows an inflection point and it is related to the onset of charge ordering transition [19, 23]. It should be noted that the T∗T^* is higher than those in KV3_3Sb5_5 and CsV3_3Sb5_5 [19, 20], implying that the relationship between T∗T^* and the lattice parameters (or ionic radius of alkali metal) is not monotonic. At μ0H=14\mu_0 H = 14 T, ρab(T)\rho_{ab}(T) is insensitive to magnetic field when T>T∗T > T^* but the significant magnetoresistance (MR) appears gradually below T∗T^*. On the other hand, the ρc(T)\rho_c(T) has a much larger absolute value than the ρab(T)\rho_{ab}(T). The ratio of ρc/ρab\rho_c/\rho_{ab} is about 7 at 300 K and increases to about 33 when temperature is down to 2 K, manifesting a significant 2D nature of RbV3_3Sb5_5. However this anisotropy is smaller than that in CsV3_3Sb5_5, which could be partially ascribed to the smaller interlayer spacing between two V-Sb slabs [19]. More importantly, in contrast to ρab(T)\rho_{ab}(T), the ρc(T)\rho_c(T) shows a remarkable upturn starting from T∗T^* with a maximum at about 97 K and this behavior is distinctly different from that in CsV3_3Sb5_5 [19]. It suggests that the QCDW in RbV3_3Sb5_5 might have a c-axial component, leading to the significantly gapped FS along the kzk_z direction. Similar behavior has also been observed in PdTeI with CDW vector qCDW=(0,0,0.396)q_{\mathrm{CDW}}=(0,0,0.396) [25] and GdSi with spin density wave (SDW) vector qSDW=(0,0.483,0.092)q_{\mathrm{SDW}}=(0,0.483,0.092) [26]. Figure 2(b) exhibits the ρab(T)\rho_{ab}(T) as a function of temperature below 1.3 K. It can be seen that there is a sharp resistivity drop appearing in the ρab(T)\rho_{ab}(T) curve at zero field and it corresponds to the superconducting transition. The onset superconducting transition temperature Tc,onsetT_{\mathrm{c,onset}} determined from the cross point of the two lines extrapolated from the high-temperature normal state and the low-temperature superconducting state is 0.92 K with the transition width ΔTc=0.17\Delta T_{\mathrm{c}}=0.17 K. This TcT_{\mathrm{c}} is lower than that of CsV3_3Sb5_5 (Tc∼2.5T_{\mathrm{c}}\sim2.5 K) but very close to that of KV3_3Sb5_5 (Tc∼0.93T_{\mathrm{c}}\sim0.93 K) [19, 20].

Image not extracted

Figure 2. (a) Temperature dependence of ρab(T)\rho_{ab}(T) and ρc(T)\rho_c(T) at zero field and 14 T between 2 K and 300 K. (b) Temperature dependence of zero-field ρab(T)\rho_{ab}(T) below 1.3 K. (c) Temperature dependence of M(T)M(T) at μ0H=1\mu_0H=1 T for H∥cH \parallel c with ZFC and FC modes. (d) Temperature dependence of Cp(T)C_p(T) at zero field between 2 K and 117 K. Inset: Cp/TC_p/T vs. T2T^2 at low temperature region. The red solid line represents the linear fit using the formula Cp/T=γ+βT2C_p/T=\gamma+\beta T^2.

The charge ordering transition also has a remarkable influence on the magnetic property of RbV3_3Sb5_5. As shown in Figure 2(c), the magnetization M(T)M(T) curve exhibits a relatively weak temperature dependence with a small absolute value above T∗T^*, reflecting the Pauli paramagnetism of RbV3_3Sb5_5. In contrast, when T<T∗T<T^*, there is a sharp drop in the M(T)M(T) curve because of the decreased carrier density originating from the partially gapped FS by the charge ordering transition. In addition, the nearly overlapped zero-field-cooling (ZFC) and field-cooling (FC) M(T)M(T) curves also suggest that this anomaly should be due to certain density wave transition not an antiferromagnetic one. Figure 2(d) shows the temperature dependence of heat capacity Cp(T)C_p(T) of RbV3_3Sb5_5 single crystals measured between T=2T=2 and 117 K at zero field. It can be seen that there is a jump at ∼102\sim102 K, in agreement with the T∗T^* obtained from resistivity and magnetization measurements. The jump in Cp(T)C_p(T) curve of RbV3_3Sb5_5 is similar to those of KV3_3Sb5_5 and CsV3_3Sb5_5 [18, 19, 20], suggesting the same origin of this anomaly of heat capacity from the charge ordering transition.

The electronic specific heat coefficient γ\gamma and phonon specific heat coefficient β\beta can be obtained from the linear fit of low-temperature heat capacity using the formula Cp/T=γ+βT2C_p/T=\gamma+\beta T^2 (inset of Figure 2(d)). The fitted γ\gamma and β\beta is 17(1) mJ mol−1^{-1} K−2^{-2} and 3.63(2) mJ mol−1^{-1} K−4^{-4}, respectively. The latter one gives the Debye temperature ΘD=168.9(3)\Theta_D=168.9(3) K using the formula ΘD=(12π4NR/5β)1/3\Theta_D=(12\pi^4NR/5\beta)^{1/3}, where NN is the number of atoms per formula unit and RR is the gas constant. The electron-phonon coupling λe−ph\lambda_{e-ph} can be estimated with the values of ΘD\Theta_D and TcT_c using McMillan’s formula [27],

λe−ph=1.04+μ∗ln⁡(ΘD/1.45Tc)(1−0.62μ∗)ln⁡(ΘD/1.45Tc)−1.04(1)\lambda_{e-ph}=\frac{1.04+\mu^*\ln(\Theta_D/1.45T_c)}{(1-0.62\mu^*)\ln(\Theta_D/1.45T_c)-1.04} \tag*{(1)}

where μ∗\mu^* is the repulsive screened Coulomb potential and is usually between 0.1 and 0.15. Assuming μ∗=0.13\mu^*=0.13, the calculated λe−ph\lambda_{e-ph} is about 0.489, implying that RbV3_3Sb5_5 is a weakly coupled BCS superconductor [28].

The MR =[(ρab(μ0H)−ρab(0))/ρab(0)]=[(\rho_{ab}(\mu_0H)-\rho_{ab}(0))/\rho_{ab}(0)] of RbV3_3Sb5_5 is negligible above T∗T^* and increases gradually below T∗T^* (Figure 3(a)), consistent with the ρab(T)\rho_{ab}(T) data (Figure 2(a)). At low temperature, the MR does not saturate up to 14 T and the Shubnikov-de Haas (SdH) quantum oscillations (QOs) can be clearly observed at low-temperature and high-field region (inset of Figure 3(a)). The MR at 2 K can be fitted using the formula MR=A(μ0H)α\mathrm{MR}=A(\mu_0H)^\alpha with α=1.001(5)\alpha=1.001(5) (inset of Figure 3(a)), such linear behavior of MR extends to T∗T^*, especially at μ0H>3\mu_0H>3 T. Figure 3(b) shows the field dependence of Hall resistivity ρyx(T,μ0H)\rho_{yx}(T,\mu_0H) at several typical temperatures. At high temperature, the values of ρyx(T,μ0H)\rho_{yx}(T,\mu_0H) are negative with nearly linear dependence on field. When decreasing temperature below 50 K, the ρyx(T,μ0H)\rho_{yx}(T,\mu_{0}H) becomes positive but the linear field dependence is almost unchanged at high-field region. Similar to the MR curves, the SdH QOs appear at low temperatures. The Hall coefficient RHR_{\mathrm{H}} obtained from the linear fits of ρyx(T,μ0H)\rho_{yx}(T,\mu_{0}H) curves are shown in Figure 3(c). The strong temperature dependence of RHR_{\mathrm{H}} implies that RbV3_3Sb5_5 is a multi-band metal, consistent with theoretical calculations and ARPES measurements of KV3_3Sb5_5 and CsV3_3Sb5_5 [18, 19, 22]. At high temperature, the negative RHR_{\mathrm{H}} suggests that the electron-type carriers are dominant, which could originate from the electron pockets around Γ\Gamma and KK points of BZ [18, 19, 22]. The most remarkable feature is that the weakly temperature dependent RHR_{\mathrm{H}} starts to decrease rapidly below T∗T^{*} and changes its sign to positive at about 40 K. Such behavior is very similar to the typical CDW materials NbSe2_2 and TaSe2_2 [29], and SDW system GdSi [26]. Both theory and STM results indicate that the qCDWq_{\mathrm{CDW}} connects the MM point when the Fermi level is close to the van Hove filling as in the case of AV3_3Sb5_5 [16, 17, 18, 19, 23]. Moreover, there are a band with van Hove singularity and a pair of Dirac-cone like bands near the MM point [23], which can form hole pockets especially when the EFE_{\mathrm{F}} shifts downward slightly due to the slight Rb deficiency [18, 19]. Therefore, the charge order may lead to the gap opening of hole bands not electron ones. It seems very peculiar that the ρab(T)\rho_{ab}(T) becomes smaller with positive RHR_{\mathrm{H}} in the charge ordering state even though the portions of hole-type FSs are gapped. Here, we explain this phenomenon in the framework of two-band model. According to the two band model at low-field region [30],

Image not extracted

Figure 3. (a) and (b) Field dependence of MR and ρyx(T,μ0H)\rho_{yx}(T,\mu_0H) at various temperatures up to 9 T. Inset of (a) shows the field dependence of MR at 2 K with the field up to 14 T. The red line represents the fit using the formula MR=A(μ0H)α\mathrm{MR}=A(\mu_0H)^\alpha. (c) Temperature dependence of ρH(T)\rho_H(T) obtained from the linear fits of ρyx(T,μ0H)\rho_{yx}(T,\mu_0H) curves. (d) Temperature dependence of ρH/ρab(0)\rho_H/\rho_{ab}(0). Inset: the enlarged part of ρH/ρab(0)\rho_H/\rho_{ab}(0) near T∗T^* and the vertical red line represents the temperature of T∗T^*.

RH=ρyxμ0H=nhμh2−neμe2e(nhμh+neμe)2(2)R_{\mathrm{H}}=\frac{\rho_{yx}}{\mu_{0}H}=\frac{n_{\mathrm{h}}\mu_{\mathrm{h}}^{2}-n_{\mathrm{e}}\mu_{\mathrm{e}}^{2}}{e(n_{\mathrm{h}}\mu_{\mathrm{h}}+n_{\mathrm{e}}\mu_{\mathrm{e}})^{2}} \tag*{(2)}

where μe,h\mu_{\mathrm{e,h}} and ne,hn_{\mathrm{e,h}} are the mobilities and densities of electron- and hole-type carriers, respectively. Because of zero-field ρab(0)=1/σab(0)=1/(nheμh+neeμe)\rho_{ab}(0)=1/\sigma_{ab}(0)=1/(n_{\mathrm{h}}e\mu_{\mathrm{h}}+n_{\mathrm{e}}e\mu_{\mathrm{e}}), it has,

RH/ρab(0)=nhμh2−neμe2nhμh+neμe(3)R_{\mathrm{H}}/\rho_{ab}(0)=\frac{n_{\mathrm{h}}\mu_{\mathrm{h}}^{2}-n_{\mathrm{e}}\mu_{\mathrm{e}}^{2}}{n_{\mathrm{h}}\mu_{\mathrm{h}}+n_{\mathrm{e}}\mu_{\mathrm{e}}} \tag*{(3)}

The derived RH/ρab(0)R_{\mathrm{H}}/\rho_{ab}(0) with the dimension of mobility is shown in Figure 3(d). According to eq. (3), if the neμe2n_{\mathrm{e}}\mu_{\mathrm{e}}^{2} is much larger than the nhμh2n_{\mathrm{h}}\mu_{\mathrm{h}}^{2} which should be the case above T∗T^{*}, the RH/ρab(0)R_{\mathrm{H}}/\rho_{ab}(0) is negative and the 1/∣RH∣1/\lvert R_{\mathrm{H}}\rvert will be close to nen_{\mathrm{e}}, which is about 1.6×1022 cm−31.6\times10^{22}\ \mathrm{cm}^{-3} at 300 K. On the other hand, when the TT is just below T∗T^{*}, the μh\mu_{\mathrm{h}} may still not increase remarkably and the nhn_{\mathrm{h}} decreases continuously because the FS reconstruction has not finished yet, manifesting from the drops of M(T)M(T) curves shown in Figure 2(c). This would result in an even negative value of RH/ρab(0)R_{\mathrm{H}}/\rho_{ab}(0), which can be clearly seen in the inset of Figure 3(d). In contrast, when the TT is far below T∗T^{*} (<70<70 K), the nhn_{\mathrm{h}} becomes insensitive to temperature and the μh\mu_{\mathrm{h}} may be much larger than the μe\mu_{\mathrm{e}} because both of electron and hole mobilities have the temperature dependence BT−nBT^{-n} with different BB and nn values. It will lead to a sign reversal of RH/ρab(0)R_{\mathrm{H}}/\rho_{ab}(0) to positive even the nhn_{\mathrm{h}} is smaller than the value above T∗T^{*}. This also explains the even smaller ρab(T)\rho_{ab}(T) below T∗T^{*}. Since the strongly CDW-like coupled portions of FSs near MM point may play a negative role in conductivity above T∗T^{*}, the carrier scattering around this area can be effectively reduced when entering charge ordering state, and thus the μh\mu_{\mathrm{h}} can enhance significantly [31]. Similar discussion about the sign change of RHR_{\mathrm{H}} has been developed by Ong for 2D multi-band system and applied to Sr2_2RuO4_4 and CDW material 2H-NbSe2_2 [32, 33, 34].

Analysis of SdH QOs provides insight on the features of FSs and carriers further. After subtracting the slowly changed part of ρab(μ0H)\rho_{ab}(\mu_{0}H) (≡⟨ρab⟩\equiv\langle\rho_{ab}\rangle), the oscillation parts of resistivity Δρab=ρab−⟨ρab⟩\Delta\rho_{ab}=\rho_{ab}-\langle\rho_{ab}\rangle as a function of 1/(μ0H)1/(\mu_{0}H) for H∥cH\mathbin{\|}c at several representative temperatures are shown in Figure 4(a). The amplitudes of QOs decrease with increasing temperature or decreasing field, but still observable at 30 K. The fast Fourier transform (FFT) spectra of the QOs reveal two principal frequencies Fα=33.5F_{\alpha} = 33.5 T and Fβ=117.2F_{\beta} = 117.2 T (Figure 4(b)). Both of them are slightly smaller than those in KV3_3Sb5_5 [22], indicating RbV3_3Sb5_5 has smaller extremal orbits of FSs than KV3_3Sb5_5. According to the Onsager relation F=(ℏ/2πe)AFF = (\hbar/2\pi e)A_F where AFA_F is the area of extremal orbit of FS, the determined AFA_F is 0.0032 and 0.011 Å−2^{-2} for α\alpha and β\beta extremal orbits, respectively. These AFA_Fs are very small, taking only about 0.0934 % and 0.321 % of the whole area of BZ in the kx−kyk_x-k_y plane when taking the lattice parameter a=5.4715a = 5.4715 Å [18]. The effective mass m∗m^* can be extracted from the temperature dependence of the amplitude of FFT peak using the Lifshitz-Kosevich (LK) formula,

Image not extracted

Figure 4. (a) SdH QOs Δρab=ρab−⟨ρab⟩\Delta\rho_{ab}=\rho_{ab}-\langle\rho_{ab}\rangle as a function of 1/(μ0H)1/(\mu_{0}H) at various temperatures. (b) FFT spectra of the QOs between 4 T and 14 T at various temperatures. (c) The temperature dependence of FFT amplitude of FαF_{\alpha} frequency. The solid line is the fit using the LK formula to extract the effective mass.

Δρab∝Xsinh⁡X(4)\Delta\rho_{ab} \propto\frac{X}{\sinh X} \tag*{(4)}

where X=2π2kBT/ℏωc=14.69m∗/μ0HavgX = 2\pi^2 k_B T/\hbar\omega_c = 14.69m^*/\mu_0H_{\mathrm{avg}} with ℏωc\hbar\omega_c being the cyclotron frequency and μ0Havg\mu_0H_{\mathrm{avg}} (= 9 T) being the average value of the field window used for the FFT of QOs [35, 36]. As shown in Figure 4(c), the temperature dependence of FFT amplitude of FαF_{\alpha} can be fitted very well using eq. (4) and the obtained m∗m^* is 0.091(2) mem_e, where mem_e is the bare electron mass. This value is even smaller than that in KV3_3Sb5_5 (0.125 mem_e for the α\alpha orbit) [22]. The small extremal cross sections of FSs accompanying with such light m∗m^* could be related to the highly dispersive bands near either MM point or along the Γ−K\Gamma-K path of BZ [18, 19, 22, 23].

In summary, we carried out the detailed study on physical properties of RbV3_3Sb5_5 single crystals grown by the self-flux method. RbV3_3Sb5_5 single crystals exhibit a superconducting transition at Tc,onset=0.92T_{c,\mathrm{onset}} = 0.92 K with a weakly coupling strength, accompanying with anomalies of properties at T∗∼102T^* \sim102 - 103 K. The high-temperature anomaly could be related to the formation of charge ordering state and it results in the sign change of RHR_H, which can be partially ascribed to the enhancement of mobility for hole-type carriers due to the reduced carrier scattering by the gapping of strongly CDW-like coupled portions of FSs. Furthermore, there are some very small FSs with rather low m∗m^*, indicating the existence of highly dispersive bands near EFE_F in RbV3_3Sb5_5. Moreover, due to the similar electronic structure of RbV3_3Sb5_5 to KV3_3Sb5_5 and CsV3_3Sb5_5 [18], RbV3_3Sb5_5 should also be a candidate of Z2_2 topological metal. Therefore, the V-based kagome metals AV3_3Sb5_5 provide a unique platform to explore the interplay between nontrivial band topology, electronic correlation and possible unconventional superconductivity.

This work was supported by National Natural Science Foundation of China (Grant No. 11822412 and 11774423), Ministry of Science and Technology of China (Grant No. 2018YFE0202600 and 2016YFA0300504), Beijing Natural Science Foundation (Grant No. Z200005), and Fundamental Research Funds for the Central Universities and Research Funds of Renmin University of China (RUC) (Grant No. 18XNL G14 and 19XNLG17).

References

  1. [1]L. Balents, Nature 464, 199-208 (2010).
  2. [2]M. P. Shores, E. A. Nytko, B. M. Bartlett, and D. G. Nocera, J. Am. Chem. Soc. 127, 13462-13463 (2005).
  3. [3]T.-H. Han, J. S. Helton, S. Chu, D. G. Nocera, J. A. Rodriguez-Rivera, C. Broholm, and Y. S. Lee, Nature 492, 406-410 (2012).
  4. [4]M. Fu, T. Imai, T.-H. Han, and Y. S. Lee, Science 350, 655-658 (2015).
  5. [5]M. Kang, L. Ye, S. Fang, J.-S. You, A. Levitan, M. Han, J. I. Facio, C. Jozwiak, A. Bostwick, E. Rotenberg, M. K. Chan, R. D. McDonald, D. Graf, K. Kaznatcheev, E. Vescovo, D. C. Bell, E. Kaxiras, J. van den Brink, M. Richter, M. P. Ghimire, J. G. Checkelsky, and R. Comin,, Nat. Mater. 19, 163-169 (2020).
  6. [6]Z. Liu, M. Li, Q. Wang, G. Wang, C. Wen, K. Jiang, X. Lu, S. Yan, Y. Huang, D. Shen, J.-X. Yin, Z. Wang, Z. Yin, H. Lei, and S. Wang, Nat. Commun. 11, 4002 (2020).
  7. [7]M. Kang, S. Fang, L. Ye, H. C. Po, J. Denlinger, C. Jozwiak, A. Bostwick, E. Rotenberg, E. Kaxiras, J. G. Checkelsky, and R. Comin, Nat. Commun. 11, 4004 (2020).
  8. [8]L. Ye, M. Kang, J. Liu, F. von Cube, C. R. Wicker, T. Suzuki, C. Jozwiak, A. Bostwick, E. Rotenberg, D. C. Bell, L. Fu, R. Comin, and J. G. Checkelsky, Nature 555, 638-642 (2018).
  9. [9]J.-X. Yin, W. Ma, T. A. Cochran, X. Xu, S. S. Zhang, H.-J. Tien, N. Shumiya, G. Cheng, K. Jiang, B. Lian, Z. Song,G. Chang, J. I. Belopolsky, D. Multer, M. Litskevich, Z.-J. Cheng, X. P. Yang, B. Swidler, H. Zhou, H. Lin, T. Neupert, Z. Wang, N. Yao, T.-R. Chang, S. Jia, and M. Z. Hasan, Nature 583, 533-536 (2020).
  10. [10]J.-X. Yin, S. S. Zhang, H. Li, K. Jiang, G. Chang, B. Zhang, B. Lian, C. Xiang, I. Belopololskip, H. Zheng, T. A. Cochran, S.-Y. Xu, G. Bian, K. Liu, T.-R. Chang, H. Lin, Z.-Y. Lu, Z. Wang, S. Jia, W. Wang, and M. Z. Hasan, Nature 562, 91-95 (2018).
  11. [11]K. Kuroda, T. Tomita, M.-T. Suzuki, C. Bareille, A. A. Nugroho, P. Goswami, M. Ochi, M. Ikhlas, M. Nakayama, S. Akebi, R. Noguchi, R. Ishii, N. Inami, K. Ono, H. Kumigashira, A. Varykhalov, T. Muro, T. Kotetsune, R. Arita, S. Shin, T. Kondo, and S. Nakatsuji, Nat. Mater. 16, 1090-1095 (2017).
  12. [12]E. Liu, Y. Sun, N. Kumar, L. Muechler, A. Sun, L. Jiao, S.-Y. Yang, D. Liu, A. Liang, Q. Xu, J. Kroder, V. Süß, H. Borrmann, C. Shekhar, Z. Wang, C. Xi, W. Wang, W. Schnelle, S. Wirth, Y. Chen, S. T. B. Goennenwein, and C. Felser, Nat. Phys. 14, 1125-1131 (2018).
  13. [13]Q. Wang, Y. Xu, R. Lou, Z. Liu, M. Li, Y. Huang, D. Shen, H. Weng, S. Wang, and H. Lei, Nat. Commun. 9, 3681 (2018).
  14. [14]P. W. Anderson, Mater. Res. Bull. 8, 153-160 (1973).
  15. [15]W.-H. Ko, P. A. Lee, and X.-G. Wen, Phys. Rev. B 79, 214502 (2009).
  16. [16]W.-S. Wang, Z.-Z. Li, Y.-Y. Xiang, and Q.-H. Wang, Phys. Rev. B 87, 115135 (2013).
  17. [17]M. L. Kiesel, C. Platt, and R. Thomale, Phys. Rev. Lett. 110, 126405 (2013).
  18. [18]B. R. Ortiz, L. C. Gomes, J. R. Morey, M. Winiarski, M. Bordelon, J. S. Mangum, I. W. H. Oswald, J. A. Rodriguez-Rivera, J. R. Neilson, S. D. Wilson, E. Ertekin, T. M. McQueen, and E. S. Toberer, Phys. Rev. Mater. 3, 094407 (2019).
  19. [19]B. R. Ortiz, S. M. L. Teicher, Y. Hu, J. L. Zuo, P. M. Sarte, E. C. Schueller, A. M. M. Abeykoon, M. J. Krogstad, S. Rosenkranz, R. Osborn, R. Seshadri, L. Balents, J. He, and S. D. Wilson, Phys. Rev. Lett. 125, 247002 (2020).
  20. [20]B. R. Ortiz, P. M. Sarte, E. Kenney, M. J. Graf, S. M. L. Teicher, R. Seshadri, and S. D. Wilson, arXiv: 2012.09097 (2020).DOI
  21. [21]Y. Wang, S.-Y. Yang, P. K. Sivakumar, B. R. Ortiz, S. M. L. Teicher, H. Wu, A. K. Srivastava, C. Garg, D. Liu, S. S. P. Parkin, E. S. Toberer, T. McQueen, S. D. Wilson, and M. N. Ali, arXiv: 2012.05898 (2020).arxiv.org/abs/2012.05898
  22. [22]S.-Y. Yang, Y. Wang, B. R. Ortiz, D. Liu, J. Gayles, E. Derunova, R. Gonzalez-Hernandez, L. Šmejkal, Y. Chen, S. S. P. Parkin, S. D. Wilson, E. S. Toberer, T. McQueen, and M. N. Ali, Sci. Adv. 6, eab6003 (2020).
  23. [23]Y.-X. Jiang, J.-X. Yin, M. M. Denner, N. Shumiya, B. R. Ortiz, J. He, X. Liu, S. S. Zhang, G. Chang, I. Belopolski, Q. Zhang, M. S. Hossain, T. A. Cochran, D. Multer, M. Litskevich, Z.-J. Cheng, X. P. Yang, Z. Guguchia, G. Xu, Z. Wang, T. Neupert, S. D. Wilson, and M. Z. Hasan, arXiv: 2012.15709 (2020).DOI
  24. [24]E. M. Kenney, B. R. Ortiz, C. Wang, S. D. Wilson, and M. J. Graf, arXiv: 2012.04737 (2020).DOI
  25. [25]H. C. Lei, K. Liu, J.-i. Yamaura, S. Maki, Y. Murakami, Z.-Y. Lu, and H. Hosono, Phys. Rev. B 93, 121101(R) (2016).
  26. [26]Y. Feng, J. Wang, D. M. Silevitch, B. Mihaila, J. W. Kim, J.-Q. Yan, R. K. Schulze, N. Woo, A. Palmer, Y. Ren, J. van Wezel, P. B. Littlewood, and T. F. Rosenbaum, Proc. Natl. Acad. Sci. 110, 3287-3292 (2013).
  27. [27]W. L. McMillan, Phys. Rev. 167, 331-344 (1968).
  28. [28]P. B. Allen and R. C. Dynes, Phys. Rev. B 12, 905-922 (1975).
  29. [29]M. Naito and S. Tanaka, J. Phys. Soc. Jpn. 51, 219-227 (1982).
  30. [30]J. M. Ziman, Electrons and Phonons, Clarendon Press, Oxford, England (1960).
  31. [31]T. Valla, A. V. Fedorov, P. D. Johnson, P.-A. Glans, C. McGuinness, K. E. Smith, E. Y. Andrei, and H. Berger, Phys. Rev. Lett. 92, 086104 (2004).
  32. [32]N. P. Ong, Phys. Rev. B 43, 193-201 (1991).
  33. [33]A. P. Mackenzie, N. E. Hussey, A. J. Diver, S. R. Julian, Y. Maeno, S. Nishizaki, and T. Fujita, Phys. Rev. B 54, 7425-7429 (1996).
  34. [34]L. Li, J. Shen, Z. Xu, and H. Wang, Int. J. Mod. Phys. B 19, 275-279 (2005).
  35. [35]D. Shoenberg, Magnetic Oscillations in Metals, Cambridge University Press, Cambridge, England (1984).DOI
  36. [36]D. Rhodes, S. Das, Q. R. Zhang, B. Zeng, N. R. Pradhan, N. Kikugawa, E. Manousakis, and L. Balicas, Phys. Rev. B 92, 125152 (2015).

Paper details

vlnc:W_wn4eezpk
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents