betaFeedback

WorksPhysics and Astronomy

Elastic and structural anisotropy in silica thin films for gravitational-wave detectors

Abstract

The thermal noise of mirror coatings for gravitational-wave detectors critically depends on the elastic properties of the constituent materials. Data analyses and theoretical models typically assume each material is homogeneous and isotropic, but isotropy has never been explicitly verified. Using Brillouin light scattering (BLS), we demonstrate for the first time that ion-beam-sputtered SiO2 – a material still viable for future mirror coatings – exhibits cylindrical elastic symmetry, with in-plane isotropy but a notable 6% compressive anisotropy along the film normal. This anisotropy remains unchanged after the post-deposition heat treatment currently used in ground-based detectors (500 ∘^\circC, 10 h) but is nearly eliminated at 900 ∘^\circC. Infrared reflectivity experiments support these findings by directly revealing heterogeneities in the distribution of bridging and non-bridging oxygen structures along the growth axis. While BLS measures the real part of the elastic constants at GHz frequencies, the data reveal negligible contributions from mechanical relaxations in the kHz-GHz range, making BLS a valid substitute for low-frequency properties obtained from standard anisotropy-insensitive techniques. Our results highlight that restoring isotropy through heat treatment – by softening the material, enabling more than 7% out-of-plane expansion, and smoothing out structural heterogeneities – may play a key role in reducing thermal noise. This proof-of-concept study extends beyond silica, providing critical insights for the design of future coatings.

Introduction

Gravitational wave (GW) detectors are precision instruments designed to measure minute displacements caused by astrophysical signals. The current ground-based detectors are kilometer-scale laser interferometers with Fabry-Pérot cavities, where mirrors are made of high-purity substrates coated with high-reflectivity Bragg reflectors, which consist of multilayer thin-film stacks made of alternating high- and low-refractive-index materials [1, 2, 3]. Surface fluctuations of the mirrors, arising from thermally activated relaxations in the coatings, are a major limitation to detector sensitivity. Therefore, to enhance the astrophysical reach of future detectors, it is crucial to reduce this thermal noise by minimizing elastic energy dissipation in the constituent materials.

The coatings of aLIGO (Advanced Laser Interferometer Gravitational-Wave Observatory) and AdV (Advanced Virgo) detectors, produced by LMA (Laboratoire des Matériaux Avancés) [4] via ion beam sputtering (IBS), consist of alternating layers of amorphous SiO2_2 (low nn) and TiO2_2:Ta2_2O5_5 (high nn) [5]. Several strategies are being explored to reduce coating thermal noise, including variations in deposition conditions [6, 7], use of nanolayering [8], optimization of post-deposition treatments [9, 10, 11], and, importantly, the search for less dissipative high-refractive-index materials to replace TiO2_2:Ta2_2O5_5. Promising candidates include silicon nitrides (SiNx_x) [6, 12] and amorphous oxide mixtures (TiO2_2:GeO2_2 [13] or TiO2_2:SiO2_2 [14]). Meanwhile, SiO2_2 remains the amorphous material with the lowest known room-temperature elastic losses in the acoustic frequency range, and as such, it continues to be the unmatched low-refractive-index candidate for room temperature applications.

The elastic properties of the materials composing the coating are key factors in determining the coating thermal noise. It is important to note that, up to now, all simulations used to derive elastic properties from experimental data [15, 16, 17] and all theoretical models developed to predict the spectral density of thermal noise incorporate varying levels of simplification [13, 18, 19, 20, 21, 22]. Specifically, despite deposition via IBS introduces stress [17], they all rely on the assumption that each individual material can be treated as elastic isotropic and homogeneous. In reality, the hypotheses of isotropy and homogeneity have never been verified, and the measured thermal noise of coatings still exceeds theoretical expectations [15, 16]. This highlights the need for a more detailed and accurate representation of the behavior of ion-beam sputtered materials, going beyond the current literature studies. In this work, we investigate anisotropic signatures in ion-beam sputtered SiO2\mathrm{SiO}_2 thin films produced by LMA, a material still viable for future mirror coatings. Brillouin light scattering (BLS) and infrared (IR) reflectivity experiments are used to probe the elastic properties at the macroscopic scale and examine structural characteristics—such as defects and inhomogeneities—at the atomic scale, while monitoring their sensitivity to thermal exposure. BLS spectroscopy is the most powerful tool for accessing the elastic constants of thin films at GHz frequencies, though it has not been previously applied to characterize materials for GW detectors. Meanwhile, IR spectroscopy remains underexploited in thin film applications. These surface-sensitive techniques, combined with supplementary measurements, demonstrate considerable potential for improved characterization of materials for next-generation high-performance GW mirror coatings.

Materials and Methods

Samples

IBS SiO2\mathrm{SiO}_2 films were deposited on single-side-polished (100)-p-doped Si wafers (∅=3′′\varnothing= 3^{\prime\prime}, thickness =0.5=0.5 mm) at LMA-IP2I (http://lma.in2p3.fr/) using a commercial Veeco Spector system with accelerated Ar+\mathrm{Ar}^{+} ions as sputtering particles. Before deposition, the base pressure in the vacuum chamber was reduced to below 10−510^{-5} mbar. During the coating process, the total pressure was maintained at approximately 10−410^{-4} mbar, with 18 sccm of Ar supplied to the ion source and 15 sccm of O2\mathrm{O}_2 injected inside the vaccum chamber. The energy and current of the sputtering ion beam were set to 1.25 keV and 0.6 A, respectively. SiO2\mathrm{SiO}_2 films were deposited with thicknesses of approximately 720 nm (runs S19175 and S21088) and 2.5 μ\mum (run S21089). Each coated wafer was laser-engraved and cleaved into several 1 cm ×\times 2 cm rectangular pieces, to study both the as-deposited material and the material after heat treatments at various temperatures. All annealing cycles were performed in air, with the temperature ramped up at 100 °C per hour, held at the target value for 10 hours, and then ramped down at 100 °C per hour. The target annealing temperatures included 500 °C and 900 °C.

Characterizations

The mass density (ρ\rho) of the films was determined using x-ray reflectivity (XRR) measurements performed with a Philips MRD diffractometer equipped with a Cu tube operating at 40 kV and 40 mA. The instrument was monochromatized to the Cu K-α\alpha line (λ=1.5406\lambda=1.5406 Å), and the reflected x-rays were detected with a Xe counter detector whose angular acceptance was defined by a Soller slit, a parallel plate collimator, and an additional 0.01 rad slit. Data analysis was carried out with the RE-FLEX software [23], modeling the sample as a silicon substrate with a thin SiO2\mathrm{SiO}_2 layer on top. Figure 10 in Appendix A presents the spectra of the sample S21088 in both the as-deposited state and after annealing at 900 °C. The film density was extracted from the critical angle of the sample, determined by the condition of total external reflection.

Image not extracted

Figure 10. Upper panel: XRR spectra of the sample S21088 as-deposited and annealed at 900 °C (colored lines), together with their best-fit curve (black lines). Bottom panel: Residuals between the experimental data and the fit curve.

The refractive index (nn) and thickness (hh) of the films were determined using spectroscopic ellipsometry (SE) with a J.A. Woollam Co. Variable Angle Spectroscopic Ellipsometer. Data were acquired over the 300–2500 nm spectral range at incidence angles of 60°, 65°, and 70° to optimize the data analysis accuracy [24]. The analysis was performed using the WVASE software, modeling the sample as two distinct layers (substrate and coating) with sharp interfaces and defined dielectric functions [7, 12, 25, 26]. The optical properties of the Si substrate were characterized independently via SE, while the SiO2\mathrm{SiO}_2 coating was modelled both as a isotropic material (see Figure 11 in Appendix A) and as a material uniaxially birefringent along the direction perpendicular to the surface. While the anisotropic model slightly improves agreement in the visible portion of the spectrum, both models accurately reproduce the experimental data for all samples. In Appendix A, Figure 11 shows the measured ellipsometric angles for the as-deposited sample S21088, along with the corresponding fit generated by the isotropic model. In the same Appendix, Figure 12 presents the wavelength-dependent refractive index of the film in its as-deposited state and after annealing at 500 °C and 900 °C. In the thicker sample S21089, interference peaks in the UV region restricted analysis to the 400–2500 nm range, though thickness accuracy (∼0.3%\sim0.3\%) remained uncompromised. However, due to higher depolarization, the refractive index at 532.3 nm—while fully consistent with sample S21088—was estimated with greater uncertainty.

Image not extracted

Figure 11. Spectroscopic ellipsometry (SE). Wavelength dependence of the angles Ψ\Psi and Δ\Delta in the as-deposited sample S21088, at three values of the incidence angle ϑ\vartheta. The fit curve is generated by the isotropic model using a Cauchy function supplemented with a Pole oscillator.

Image not extracted

Figure 12. Wavelength dependence of the refractive index, nn, obtained by reproducing the SE experimental data (Ψ\Psi, Δ\Delta) with the isotropic model, for the sample S21088 in the as-deposited state and after annealing at 500 °C and 900 °C.

The film thickness was additionally measured using scanning electron microscopy (SEM) with a FE-SEM LEO 1525 ZEISS. Samples were mounted vertically on conductive carbon adhesive tape to acquire cross-sectional images of the coating on the substrate (Appendix A, Figure 13). The coating thickness for each sample was estimated with an accuracy of ∼0.3%\sim0.3\%, similar to that of SE, based on the average of 30–40 SEM measurements taken at various points. Elemental composition was confirmed using a Bruker Quantax EDX system.

Image not extracted

Figure 13. SEM images of the sample S21088 in the as-deposited state and after 10-h annealing at 500 °C, 600 °C and 900 °C. The thin layer of SiO2_2 deposited on the thick silicon substrate is visible. Scale bar is 200 nm.

Brillouin light scattering experiments

Brillouin light scattering (BLS) measurements were performed in air at room temperature using a high-resolution, high-contrast Sandercock-type 3+3-pass tandem Fabry–Pérot interferometer. The setup employed a solid-state laser with a wavelength λ=532.3\lambda=532.3 nm (power on the sample: ∼160\sim160 mW). Light was focused and collected in a backscattering geometry using a 50 mm camera objective, with the sample mounted vertically on a goniometer rotatable in the horizontal scattering plane. The incident light was either s-polarized (perpendicular to the plane of incidence) or p-polarized (parallel to the plane of incidence), and the scattered light was analyzed in either s- or p-polarization. A 2 mm-wide vertical slit placed behind the polarization analyzer restricted the angular acceptance of the interferometer around the backscattering direction. The three samples, S21089, S21088, and S19175, were measured in their as-deposited state and after annealing at 500 °C and 900 °C. Polarized (s-s; p-p) and depolarized (s-p) spectra were acquired over a frequency range up to 40 GHz at various angles of incidence (θ\theta=10°, 12°, 20°, 30°, 40°, 45°, 50°, 55°, 60°, 65°, 70°, 75°). At the lowest incidence angle (θ\theta=10°), used to prevent reflected elastic light from entering the spectrometer, the refracted light inside the film propagated at an angle α<7∘\alpha< 7^\circ, as determined by Snell’s law, which is nearly perpendicular to the film surface. Measurements were repeated at two or three different points on each sample, and with the sample plane rotated around the normal axis for additional data. Acquisition times ranged from 2 to 46 hours, depending on the scattering cross-section of the acoustic modes, which varies with sample thickness, annealing state, and scattering configuration. S-s and s-p spectra were recorded at room temperature and θ\theta = 45° on a fused-silica platelet (Suprasil 300, Heraeus), sputter-coated on one side with several hundred nanometers of chromium.

Infrared spectroscopy experiments

Infrared (IR) measurements were performed in both specular reflection (SR) and attenuated total reflection (ATR) modes.

SR-IR spectra were acquired using a Bruker INVENIO-R interferometer equipped with a PIKE Technologies VeeMAX III variable-angle specular reflection accessory. The three samples (S21089, S21088, and S19175) were analyzed in their as-deposited state and after annealing at 500, 600, and 900 °C. Spectra were recorded with unpolarized and p-polarized radiation at incidence angles θ\theta=30°, 40°, 45°, 50°, 55°, 60°, 65°, 70°, 75°, 80°, as well as at a fixed incidence of θ\theta=67° with s-polarized radiation. Polarization was selected using a ZnSe manual polarizer inserted into the dedicated slot of the VeeMAX III accessory. Each spectrum was acquired with a resolution of 4 cm−1^{-1} across the wavevector range 100–9000 cm−1^{-1}, by averaging 60 scans. A gold mirror served as the standard reference for all measurements. Unpolarized and p-polarized spectra, acquired at the same incidence angles as for the IBS films, were recorded at room temperature on a fused-silica sample supplied by Neyco.

ATR-IR spectra were recorded for the same set of samples using the Bruker INVENIO-R system equipped with the ATRMAXII variable-angle ATR accessory and a Ge ATR crystal with a 60° face angle. Measurements were taken at effective incidence angles of θ\theta=50°, 52.5°, 55°, 57.5°, with a resolution of 6 cm−1^{-1}, by averaging 150 scans. A sample press ensured close contact between the sample and the ATR crystal surface. For each acquisition, a background spectrum was collected under identical conditions using the clean Ge ATR crystal.

Background on acoustic and optical modes in thin films

Acoustic modes and selective determination of elastic constants

BLS is the inelastic scattering of photons by thermally-induced acoustic phonons naturally present in a material [27]. This phenomenon arises from the interaction between the electric field of the monochromatic incident light and the periodic modulation of the material’s dielectric constant caused by acoustic waves. The modulation can occur through two primary mechanisms: the photoelastic effect, and surface corrugations (also known as the rippling effect). Whatever the mechanism, from a quantum-mechanical perspective, a Brillouin scattering event is described as a photon-phonon collision in which energy and momentum are conserved, through phonon creation (Stokes process) or phonon annihilation (anti-Stokes process). It follows that in a typical BLS experiment, the probed phonons have wavelengths comparable to that of light, placing their frequencies in the GHz range [28, 29].

The configuration with a transparent amorphous SiO2_2 film deposited on a reflective Si substrate enables two distinct backscattering channels to be accessed within a single BLS experiment. As illustrated in Figure 1, the incident light (wavelength λ\lambda; wavevector ki=2π/λ\mathbf{k}_i = 2\pi/\lambda; angle of incidence θ\theta) passes through the objective lens, refracts at the air-film interface (ki′=nki\mathbf{k}'_i = n\mathbf{k}_i where nn is the refractive index of the film) at an angle α=arcsin⁡(sin⁡θ/n)\alpha= \arcsin(\sin\theta/n), is focused onto the film-substrate interface and then reflected by the substrate. For momentum conservation, only interactions with specific acoustic waves travelling parallel to the surface (surface-like phonons) and within the medium at an angle α\alpha (bulk-like phonons) originate backscattered light (ks′=nks≈ki′\mathbf{k}'_s = n\mathbf{k}_s \approx\mathbf{k}'_i). On one hand, after reflection from the substrate, light is backscattered by acoustic waves having parallel-to-surface wavevector qs=2ki′sin⁡α=2kisin⁡θq_s = 2k'_i\sin\alpha= 2k_i\sin\theta. On the other hand, when the film thickness hh exceeds both the phonon mean-free-path ℓ\ell and the light wavelength λ\lambda, acoustic waves travelling within the medium at an angle α\alpha with a wavevector qb=2nkiq_b = 2nk_i, also contribute to the backscattered light, as they do in an infinite bulk material. The frequency of the scattered light is shifted by ±fBLS\pm f_{BLS} relative to the incident light and, for energy conservation, fBLSf_{BLS} is connected to the phase velocity (vb,sv_{b,s}) of the corresponding acoustic wave as:

Image not extracted

Figure 1. Schematic diagram of the backscattering geometry used for BLS measurements. The wavevectors of incident, refracted, and reflected light are indicated in red, the wavevector of scattered light in green, and the wavevectors of bulk-like and surface-like acoustic waves responsible for backscattered light in blue. All wavevectors lie within the scattering plane. In the experimental setup, the sample is mounted vertically, the scattering plane is horizontal, and s- or p-polarized incoming light is used.

vb=2πfBLSqb=λfBLS2n;vs=2πfBLSqs=λfBLS2sin⁡θ(1)v_b = \frac{2\pi f_{\mathrm{BLS}}}{q_b} = \frac{\lambda f_{\mathrm{BLS}}}{2n}; \quad v_s = \frac{2\pi f_{\mathrm{BLS}}}{q_s} = \frac{\lambda f_{\mathrm{BLS}}}{2\sin\theta} \tag*{(1)}

for bulk and surface modes, respectively. Note that the velocity of surface waves, unlike bulk ones, can be directly determined from fBLSf_{\mathrm{BLS}} without requiring prior knowledge of the material’s refractive index.

By using various angles of incidence for the incoming light and a careful polarization analysis of the incident and scattered light, it is possible to detect and identify several acoustic waves in BLS spectra: the Rayleigh surface wave (RW), the surface-like longitudinal mode (LM), the bulk-like longitudinal mode (LB), all of which contribute to polarized scattering, and the surface-like shear horizontal mode (SHM), which contributes to depolarized scattering. A schematic representation of these modes is provided in Figure 2.

Image not extracted

Figure 2. Schematic view of the four types of acoustic waves detectable in BLS spectra from SiO2 thin films deposited on a reflective substrate. For each acoustic wave, the propagation direction is indicated by a blue vector, and the particle motion is represented by a red symbol. The polarization of the scattered light is indicated below each image.

It has to be noted that, in thin films (h<λ,ℓh < \lambda,\ell) of a homogeneous lossless material supported on a hard substrate, bulk-like phonons propagating perpendicular to the surface (q∥=0q_{\parallel}=0) give rise to standing modes resulting from the constructive interference of waves reflecting back and forth at the film surfaces, having nodes at the interface with the substrate and antinodes at the free surface — as occurs in organ pipes [30]. To satisfy the boundary conditions, the wavevectors along the direction perpendicular to the surface must have discrete values

q⊥=(2m−1)π2h,where m=1,2,3…(2)q_{\perp} = \frac{(2m-1)\pi}{2h}, \quad\text{where } m=1,2,3\ldots \tag*{(2)}

is an integer [30, 31]. The interaction of light at normal incidence with these standing modes produces in the BLS spectrum a series of equally spaced peaks, with a frequency separation Δf=vLB/2h\Delta f = v_{\mathrm{LB}}/2h, where vLBv_{\mathrm{LB}} is the velocity of surface-normal longitudinal bulk-like phonons. The intensity of these peaks is modulated by a sinc⁡2f\operatorname{sinc}^{2}f envelope centered

around the frequency fLBf_{\mathrm{LB}}, corresponding to the single peak produced by longitudinal phonons traveling normal to the surface under bulk conditions [32, 33, 34]. Within this theoretical framework, only when the film thickness increases such that Δf\Delta f becomes smaller than the peaks half-width, the discrete multipeak structure is no longer resolved, and the spectrum merges into a single symmetric peak centered at fLBf_{\mathrm{LB}} [35, 36].

The BLS signal integrates the contributions from the entire illuminated volume, which is defined by the laser spot size of ∼30 μm\sim30\,\mu\mathrm{m} and a lens focal depth of the order of 100 μm100\,\mu\mathrm{m}, significantly larger than the film thickness. Consequently, at the macroscopic length scale probed by BLS, the sample behaves as a homogeneous medium. From an elastic perspective, thin films grown via IBS are reasonably expected to exhibit transverse isotropy, characterized by an extraordinary axis along the growth direction and equivalence among all directions parallel to the surface. Transverse isotropy implies cylindrical symmetry, resulting in five independent elastic constants in the elasticity tensor cijc_{ij}: c11c_{11}, c33c_{33}, c13c_{13}, c44c_{44}, and c66c_{66} (see Appendix, Sec. B1). Importantly, the phase velocity of the detectable acoustic modes generally depends on the elastic constants of both the film and the substrate. Nevertheless, for sufficiently large film thicknesses, the influence of the substrate becomes negligible, and some of the film’s elastic constants can be selectively extracted from the measured acoustic velocities, as in the case of a semi-infinite medium [37]:

vLM=c11ρ;vSHM=c66ρ;vLB(α=0∘)=c33ρ,(3)v_{\mathrm{LM}} = \sqrt{\frac{c_{11}}{\rho}}; \quad v_{\mathrm{SHM}} = \sqrt{\frac{c_{66}}{\rho}}; \quad v_{\mathrm{LB}}(\alpha=0^\circ) = \sqrt{\frac{c_{33}}{\rho}}, \tag*{(3)}

with ρ\rho the material density; the remaining constants can be determined from vRWv_{\mathrm{RW}} and vLB(α≠0∘)v_{\mathrm{LB}}(\alpha\ne0^\circ), which both depend on c11c_{11}, c33c_{33}, c13c_{13}, c44c_{44}, and ρ\rho (see details in the Appendix, Sec. B2 and B3). Numerical simulations show that acoustic-wave propagation in SiO2_2 films on silicon is well approximated by that in a semi-infinite medium — and thus effectively substrate-independent — when the film thickness exceeds the phonon wavelength Λ\Lambda. Remarkably, this also holds for much harder substrates such as sapphire (Figure 14 in Appendix C).

Image not extracted

Figure 14. Numerical simulation of the Rayleigh-wave phase velocity, vRWv_{RW}, for a SiO2_2 thin film deposited on (100)-Si or (0001)-Al2_2O3_3 (C-plane sapphire) substrate, as a function of the ratio h/Λh/\Lambda between film thickness, hh, and phonon wavelength, Λ\Lambda. The simulation is presented for two(three) propagation directions, labeled by the in-plane angle ϕ\phi relative to the x(a1)x(a_1)-axis of silicon(sapphire). It can be seen that the influence of the substrate is negligible when the condition h/Λ≳1h/\Lambda\gtrsim1 is fulfilled.

Notice that elastic moduli are frequency-dependent complex quantities, and, from sound velocities, BLS spectroscopy determines their real part at the single frequency fBLSf_{\mathrm{BLS}}, located in the tens of GHz range. Only in isotropic materials, there are two instead of five independent elastic constants, for example the longitudinal modulus M≡c11=c33M \equiv c_{11} = c_{33} and the shear modulus G≡c66=c44G \equiv c_{66} = c_{44}, whose real parts can be determined by combining the velocity equations (1) with the elasticity relations (2). The isotropic elastic response can alternatively be described using the bulk modulus KK, the Young’s modulus YY, and the Poisson’s ratio ν\nu, which are analytically related to MM and GG as follows:

Y=M−(M−2G)2M−Gν=2G−M2(G−M)K=M−43G(4)Y = M - \frac{(M - 2G)^2}{M - G} \qquad\nu= \frac{2G - M}{2(G - M)} \qquad K = M - \frac{4}{3}G \tag*{(4)}

Another critical property is the internal elastic energy dissipation, characterized by the loss angle Φ=tan⁡−1(Re⁡(Y)/Im⁡(Y))\Phi= \tan^{-1}(\operatorname{Re}(Y)/\operatorname{Im}(Y)), determined by the ratio of the imaginary to the real part of the elastic modulus.

Optical modes and local structure

In both crystalline and amorphous silica, oxygen atoms that link the SiO4\mathrm{SiO}_{4} tetrahedra, which are characteristic of the structure, are referred to as bridging oxygens (BOs). In fused silica, the angle formed by the Si-O-Si bonds, with a BO at the vertex, typically averages around 140° [38, 39, 40]. This angle can vary under conditions of stress or chemical inhomogeneity. The Si-O-Si stretching vibration reflects these variations, as its force constant depends on the arrangement (distance and relative orientation) of the SiO4\mathrm{SiO}_{4} units, thus serving as a probe for the local structure. In SiO2\mathrm{SiO}_{2} films, the long-range Coulomb interactions inherent to this polar material result in anisotropic vibrations: atomic displacements along directions parallel and perpendicular to the surface give rise to two distinct modes, the longitudinal-optic (LO) and the transverse-optic (TO) modes [39, 40, 41]. Additionally, the stretching vibrations of groups containing non-bridging oxygens (NBOs), such as Si-O− and Si-OH, can be detected, providing further insights into the material’s local environment.

The IR signal of the antisymmetric Si-O-Si vibration is particularly intense, but the information obtained from this signal depends on the selection rules for IR absorption, which vary with the polarization and incidence angle of the radiation. For s-polarized radiation, the electric field is always parallel to the sample surface and thus interacts only with vibrations that exhibit a change in dipole moment with a surface-parallel component, such as the TO mode. Conversely, for p-polarized radiation at oblique incidence, the electric field has both parallel and perpendicular components relative to the surface, enabling excitation of both the TO and LO modes, as illustrated in Figure 3.

Image not extracted

Figure 3. Schematic representation of TO and LO modes (red arrows) probed by s- and p-polarized IR radiation. At normal incidence (left panel), IR spectroscopy detects only the transverse (TO) component of the antisymmetric Si-O-Si stretching vibration. At oblique incidence (right panel), both the transverse (TO) and longitudinal (LO) components can be observed.

The spectral signals of the LO and TO modes are observed in the ranges 1200–1250 cm−1^{-1} and 1100–1120 cm−1^{-1}, respectively, while the NBO signal is located in the range 1000–1020 cm−1^{-1}. The configuration with a SiO2\mathrm{SiO}_{2} film deposited on a substrate enables to exploit IR reflectivity to monitor these vibrations while avoiding substrate absorption contributions. This is achieved in either SR or ATR configurations, which utilize the external or internal reflection of the incoming radiation, respectively. The penetration depth of radiation into the film, defined as the distance where the electric field amplitude drops to 1/e1/e of its value at the surface, differs significantly in the two configurations. In SR-IR mode, the penetration depth depends on the wavelength λ\lambda and the incidence angle θ\theta of the incoming radiation, according to [42]:

dpSR(λ,θ)=λ4πk1−sin⁡2θn2+k2(5)d_{p}^{\mathrm{SR}}(\lambda,\theta) = \frac{\lambda}{4\pi k}\sqrt{1 - \frac{\sin^{2}\theta}{n^{2} + k^{2}}} \tag*{(5)}

where n(λ)n(\lambda) and k(λ)k(\lambda) are the real and imaginary parts of the material’s complex refractive index at wavelength λ\lambda. In ATR-IR mode, a crystal (e.g., Ge) is used as internal reflection element due to its high refractive index and superior IR transmission. Here, the incident radiation undergoes total internal reflection within the crystal, and the sample, in close contact with it, absorbs the evanescent wave that propagates outside the crystal at each reflection. This configuration results in reduced radiation penetration into the sample, with a penetration depth given by [38]:

dpATR(λ,θ)=(λ2π[(nATR2sin⁡2θ−n2+(ln⁡10k)2)2+(2nATRln⁡10k)2+(nATR2sin⁡2θ−n2+(ln⁡10k)2)2]−1/2)(6)d_p^{ATR}(\lambda,\theta)=\left(\frac{\lambda}{2\pi}\left[\frac{\sqrt{\left(n_{ATR}^{2}\sin^{2}\theta-n^{2}+(\ln10k)^{2}\right)^{2}+\left(2n_{ATR}\ln10k\right)^{2}}+\left(n_{ATR}^{2}\sin^{2}\theta-n^{2}+(\ln10k)^{2}\right)}{2}\right]^{-1/2}\right) \tag*{(6)}

where nATRn_{ATR} is the refractive index of the ATR crystal. The differing dependencies of dpSRd_p^{SR} and dpATRd_p^{ATR} on θ\theta, nn and kk result in different spectral profiles and sensitivities to vibrational modes between the two techniques [41]. Additionally, in SR-IR spectra, an oscillating background can appear, with period and characteristics dependent on the film thickness, due to interference from light reflections at the air-film and film-substrate interfaces. This interference is absent in ATR-IR spectra, where the reduced penetration depth precludes such effects, making ATR-IR a practical alternative to SR-IR spectroscopy for thin layers, although existing literature on its application in this area is surprisingly limited.

Results and Discussion

Elastic and optical properties

As-deposited material

The Brillouin investigation begins with the ∼2.5 μm\sim2.5\ \mu\mathrm{m}-thick sample S21089 in its as-deposited state. The BLS experiment reveals several peaks, selectively detected in polarized and depolarized spectra, that change differently their frequency position with the incidence angle, as shown in Figure 4(a) and Figure 4(b). Three peaks whose frequencies scale with sin⁡θ\sin\theta, in agreement with Eq. (1), are identified as surface-like acoustic waves: the LM mode (fLMf_{LM}) in s-s spectra, the SHM mode (fSHMf_{SHM}) in s-p spectra, and the Rayleigh wave (fRWf_{RW}) in s-s and p-p spectra. The Rayleigh signal, much weaker than the others, is observed only at a few angles in the s-s configuration, whereas in the p–p configuration it appears more clearly and over a broader angular range (θ≥30∘\theta\ge30^\circ), enabling systematic analysis. For each of these modes, the constant ratio fBLS/sin⁡θf_{BLS}/\sin\theta in Figure 4(b) demonstrates nondispersive propagation and, according to Eq. (1), yields a phase velocity independent of θ\theta (Figure 15 in Appendix C). This behavior is consistent with numerical expectations since all probed phonons satisfy h/Λ≳5h/\Lambda\gtrsim5 — exceeding the h/Λ∼1h/\Lambda\sim1 threshold for substrate-independent acoustic propagation (§ 3 A).

Image not extracted

Figure 4. (a) Polarized (s-s) and depolarized (s-p) BLS spectra of the as-deposited sample S21089 at selected incidence angles θ\theta. The Rayleigh, longitudinal (surface-like and bulk), and shear horizontal peaks are labeled as RW, LM, LB, and SHM, respectively. (b) Lower frame: Brillouin frequency fBLSf_{\mathrm{BLS}} of different surface-like acoustic waves as a function of the incidence angle. Solid spheres are data for the sample S21089, stars are data for the thinner samples S21088 and S19175. Solid lines represent linear fits through the origin. Error bars are smaller than the symbol size. Upper frame: Brillouin frequency fLBf_{\mathrm{LB}} of bulk-like acoustic wave as a function of the incidence angle, from s-s spectra. Black solid spheres are data for the sample S21089, stars are data for the thinner samples S21088 and S19175. The horizontal dotted line highlights the difference between low and high-incidence fLBf_{\mathrm{LB}} values. The red solid line is the numericaly simulated dispersion curve. (c) Enlargement of the BLS spectrum at quasi-normal incidence (θ=10∘\theta=10^\circ) in the LB frequency region, where a sinc2^2 modulation is observed. The central frequency between the zeros of the sinc2^2 function, fLBf_{\mathrm{LB}}, is marked by a vertical red dotted line. The cyan areas in the figure represent deviations from a single-peak structure, as indicated by the black dashed line. (d) BLS spectra acquired at θ=10∘\theta=10^\circ and 65∘65^\circ for the as-deposited thin sample S19175.

Image not extracted

Figure 15. Phase velocity of surface-like acoustic waves —longitudinal mode (vLMv_{LM}), shear horizontal mode (vSHMv_{SHM}), and Rayleigh surface wave (vRWv_{RW}) — as a function of the incidence angle θ\theta, in films of thickness 2.5 μ\mum (S21089) and 720 nm (S21088, S19175) in the as-deposited state. Solid lines are the best-constant fit of the data. All three modes are nondispersive, and the velocities measured in films of different thickness are identical within errors.

In addition, a strong broadened peak around 35 GHz in polarized spectra, nearly fixed with θ\theta, matches the expected behavior of bulk-like modes. Further analysis of this feature suggests a multipeak structure, consistent with predictions for films thin enough to induce transversal phonon confinement and consequent discretization of the surface-normal phonon wavevector (§ 3 A). Indeed, studies [43, 44] report a mean free path ℓ∼6 μm\ell\sim6\ \mu\mathrm{m} for LB phonons in fused silica measured at ambient temperature via BLS. In Figure 4(c), the spectrum is clearly perceived as a triplet, with a central peak significantly more intense than the two lateral contributions, spaced approximately 1 GHz apart. This spacing agrees with the estimate Δf=vLB/2h∼1.2 GHz\Delta f=v_{LB}/2h\sim1.2\ \mathrm{GHz}, using vLB∼6000 m/sv_{LB}\sim6000\ \mathrm{m/s} in fused silica [43]. However, the multipeak structure is blurred due to the peak width being comparable to their separation. Varying the incidence angle further decreases the separation while changing the scattering efficiency of each mode, as evidenced by the differently asymmetric structures observed at higher incidence angles and after annealing at various temperatures (Figure 16 in Appendix C). As explained in § 3 A, fLBf_{LB} corresponds not to the frequency of maximum intensity but to the central frequency between the first zeros of the sinc⁡2\operatorname{sinc}^{2} envelope (see Figure 4(c)).

Image not extracted

Figure 16. BLS spectra in the region of longitudinal bulk-like waves. (Left) Comparison between polarized BLS spectra at θ\theta=10° and 65° of the as-seposited sample S21089. (Right) Comparison between polarized BLS spectra at θ\theta=10° of sample S21089, in the as-deposited state and after annealing at 500 °C and 900 °C. To highlight differences between the spectra, in both cases the comparison is also shown by shifting each spectrum by its frequency of maximum intensity.

The frequencies fLMf_{LM}, fSHMf_{SHM} and fLBf_{LB} allow direct access to three of the five independent elastic constants. By combining Eqs. (1) and (2), fLMf_{LM} and fSHMf_{SHM} are used to calculate c11c_{11} and c66c_{66}, which are independent of θ\theta, while fLB(θ=10∘)≈fLB(α=0∘)f_{LB}(\theta=10^\circ)\approx f_{LB}(\alpha=0^\circ), together with the material refractive index, is used to determine c33c_{33}. For the remaining constants, c13c_{13} and c44c_{44}, they are numerically estimated as those that best reproduce the experimentally measured velocities vRWv_{RW} and vLB(θ)v_{LB}(\theta), according to the procedure detailed in Sec. B3 of the Appendix. This complete characterization, which would be difficult if not impossible with conventional mechanical testing, enables to capture a sizeable elastic anisotropic response of the material. A comparison of c11c_{11} with c33c_{33} — which should be equal in an isotropic medium — reveals c33>c11c_{33}>c_{11}, meaning that the compressibility along the growth axis is lower than in directions parallel to the surface. The anisotropy ratio c33/c11c_{33}/c_{11} is 1.062±0.0041.062\pm0.004, providing the first direct evidence of a (6.2±0.4)%(6.2\pm0.4)\% compressive anisotropy in the as-deposited material. By contrast, c44c_{44} and c66c_{66} are identical within errors, revealing the absence of shear anisotropy (c66/c44=1.01±0.02c_{66}/c_{44}=1.01\pm0.02). Therefore, although the film is stiffer in compression along the growth direction, it exhibits similar resistance to shearing out of plane and in plane. Finally, c13c_{13} is higher than c12=c11−2c66c_{12}=c_{11}-2c_{66} by (10±1)%(10\pm1)\%, still in contrast with the isotropic case (Table III in Appendix F).

n532n_{532}nBLSn_{\mathrm{BLS}}ρ\rho (g/cm3^3)c11c_{11} (GPa)c33c_{33} (GPa)c66c_{66} (GPa)c44c_{44} (GPa)c13c_{13} (GPa)c12c_{12} (GPa)
as-deposited1.494 ± 0.0031.523 ± 0.0032.39 ± 0.0188.1 ± 0.293.6 ± 0.332.0 ± 0.131.8 ± 0.426.8 ± 0.824.1 ± 0.3
10h@500 °C1.475 ± 0.0031.509 ± 0.0032.28 ± 0.0182.8 ± 0.288.5 ± 0.330.9 ± 0.130.6 ± 0.624.9 ± 1.121.0 ± 0.3
10h@900 °C1.467 ± 0.0031.479 ± 0.0032.22 ± 0.0176.7 ± 0.278.9 ± 0.330.6 ± 0.130.4 ± 0.417.6 ± 0.715.5 ± 0.3

Table III. Elastic and optical properties of sample S21089. Refractive index at λ=532.3\lambda=532.3 nm, n532n_{532}, obtained from the SE isotropic model. BLS-apparent refractive index nBLS≡(fLB/fLM)sin⁡θn_{\mathrm{BLS}} \equiv(f_{\mathrm{LB}}/f_{\mathrm{LM}})\sin\theta. Mass density ρ\rho, determined by XRR. Elastic constants cijc_{ij}, obtained by BLS. The values of nBLSn_{\mathrm{BLS}}, c11c_{11}, c33c_{33}, and c66c_{66} are reported as average ±SD of several independent measurements; the values of c44c_{44} and c13c_{13} are obtained as best-fit results of a numerical simulation model; c12c_{12} is calculated as c11−2c66c_{11}-2c_{66}, for symmetry constraint. The values of n532n_{532} refer to the sample S21088, since they are identical to those of sample S21089 but affected by lower uncertainty.

A behavior consistent with transverse isotropy, where all directions parallel to the surface are equivalent, is confirmed by rotating the sample around its normal axis and observing that the velocity vLMv_{LM} of longitudinal waves remains invariant across different in-plane directions. Additionally, the velocity vLBv_{LB} of longitudinal bulk-like waves propagating at different angles within the film, rather than being independent of θ\theta as in the isotropic

case, exhibits a slight but significant variation with θ\theta (as shown in Figure 17 in the Appendix C), resulting 1% lower at higher incidence (6190±106190 \pm10 m/s for θ=75∘\theta= 75^\circ) compared to quasi-normal incidence (6260±106260 \pm10 m/s). The dependence of vLBv_{\mathrm{LB}} on θ\theta directly reflects that of the frequency fLBf_{\mathrm{LB}}, shown in the upper panel of Figure 4(b).

Image not extracted

Figure 17. Phase velocity vLBv_{LB} of the longitudinal bulk-like wave, as a function of the incidence angle θ\theta, in the 2.5 μ\mum-thick film in different states. Solid lines are numerical simulation curves calculated from the measured values of c11c_{11}, c33c_{33}, ρ\rho and the best-fit values of c44c_{44}, c13c_{13}.

The velocity vLBv_{\mathrm{LB}}, at any incidence, is calculated here from s-s spectra using n532n_{532}, the refractive index at the BLS wavelength obtained from the isotropic SE model. This warrants particular attention, because transverse elastic isotropy may be accompanied by uniaxial birefringence, with the film’s growth direction acting as the optic axis. In our experimental geometry (see Figure 1), s-polarized incoming light is always polarized perpendicular to the optic axis and is thus governed by the ordinary refractive index non_{\mathrm{o}}, which may differ from n532n_{532} in case of birefringence. However, we find that n532n_{532}, within the uncertainty, matches non_{\mathrm{o}} at the same wavelength, as obtained by reproducing the SE data with the anisotropic model (§ 2 B), which indicates that the approximation n532≈non_{532} \approx n_{\mathrm{o}} used to calculate vLBv_{\mathrm{LB}} is very accurate. It has to be noted that the anisotropic model describes the SE data with a difference between nen_{\mathrm{e}} and non_{\mathrm{o}} of 0.001–0.002 in all samples investigated, suggesting that a small birefringence, if any, is beyond the experimental sensitivity.

Comparing BLS and SE measurements further highlights the anisotropy of the material in terms of acoustic wave propagation. According to Eq. (1), the velocity ratio vLB/vLMv_{\mathrm{LB}}/v_{\mathrm{LM}} is provided at any incidence angle by the expression (fLB/fLM)sin⁡θ/n532≡nBLS/n532(f_{\mathrm{LB}}/f_{\mathrm{LM}})\sin\theta/n_{532} \equiv n_{\mathrm{BLS}}/n_{532}, where nBLSn_{\mathrm{BLS}} denotes the quantity (fLB/fLM)sin⁡θ(f_{\mathrm{LB}}/f_{\mathrm{LM}})\sin\theta. This was evaluated for twelve spectra at θ≥30∘\theta\ge30^\circ in the as-deposited film. While largely independent of θ\theta in the measured range, the velocity ratio is found to be 1.019±0.0041.019 \pm0.004, reflecting anisotropic acoustic wave propagation within the material. It should be noted that nBLSn_{\mathrm{BLS}} cannot be calculated at quasi-normal incidence, where vLBv_{\mathrm{LB}} is higher than the values measured at θ≥30∘\theta\ge30^\circ. This accounts for the 2% difference from n532n_{532}, instead of the 3% expected from the elasticity ratio c33/c11=vLB2/vLM2c_{33}/c_{11} = v_{\mathrm{LB}}^2/v_{\mathrm{LM}}^2, where vLBv_{\mathrm{LB}} is measured at θ=10∘\theta= 10^\circ. Also, it is interesting to note that, if the film were isotropic in both elastic and optical properties, nBLSn_{\mathrm{BLS}} would coincide with the refractive index of the material at the BLS wavelength, n532n_{532}.

In conclusion, as a remarkable first achievement, we provide evidence that the elastic properties of the as-deposited sample S21089 differ substantially from those expected in an isotropic material. The possibility that the observed anisotropy is a measurement artifact is ruled out by results obtained from a reference isotropic sample (details are provided in Appendix § 2.4).

For the thinner samples S21088 and S19175, BLS spectra allow the determination of the frequencies fLMf_{\mathrm{LM}}, fSHMf_{\mathrm{SHM}}, and fRWf_{\mathrm{RW}} of surface-like acoustic modes at θ≥45∘\theta\ge45^\circ (stars in Figure 4(b)), which — as expected for h/Λ>1.9h/\Lambda> 1.9 — are nondispersive and yield the same phase velocities

as measured in sample S21089 (Figure 15 in Appendix C). The determination of fLBf_{\mathrm{LB}} at different incidence angles is subject to larger uncertainty due to the phonon discretization effect arising from the reduced sample thickness. Nevertheless, albeit with reduced precision, all elastic constants and the quantity nBLSn_{\mathrm{BLS}} can still be extracted by applying the same procedure used for sample S21089. As shown in Figure 4(d), the multipeak structure in the thinner samples is particularly pronounced at quasi-normal incidence, and the information provided will be further discussed in § 5 C.

Post-deposition annealing effects

BLS spectra of samples annealed at 500 °C and 900 °C are qualitatively similar to those in the as-deposited state and allow for the calculation of the same quantities described in the previous section. An example is shown in the spectra of sample S21089 (Figure 18 in Appendix C). The derived elastic constants c11c_{11}, c33c_{33}, c66c_{66}, c44c_{44}, and c13c_{13}, along with the density and refractive index used in the calculations, are listed in Table III in the Appendix § 17. Figure 5(a)–(Figure 5c) display the refractive index, sound velocities, and elastic moduli of all investigated samples as a function of annealing temperature. The density is used as the x-axis in Figure 5(d). All the mentioned quantities can be measured in films with thickness of ∼720\sim720 nm (S21088, S19175) and ∼2.5 μm\sim2.5\ \mu\mathrm{m} (S21089) and are identical within error, which demonstrates that macroscopic properties can be reliably probed regardless of film thickness, consistently with numerical expectations.

Image not extracted

Figure 5. (a) Dependence on the annealing temperature of the refractive index n532n_{532} obtained from the SE isotropic model and the BLS-apparent refractive index nBLSn_{\mathrm{BLS}}. (b) Dependence of the sound velocities vLMv_{\mathrm{LM}}, vSHMv_{\mathrm{SHM}}, vRWv_{\mathrm{RW}}, and vLBv_{\mathrm{LB}} on the annealing temperature, with vLBv_{\mathrm{LB}} measured at quasi-normal incidence. (c) Dependence on the annealing temperature of the elastic constants c11c_{11}, c33c_{33}, c66c_{66}, and c44c_{44}. (d) Dependence of the quantity (n5322−1)/(n5322+2)(n_{532}^{2}-1)/(n_{532}^{2}+2) on the film density ρ\rho, and best fit with the Lorentz-Lorenz equation (solid line). The legend is the same for all the panels. Dashed lines are just a visual guide.

Image not extracted

Figure 18. BLS spectra vs. annealing. Polarized (s-s) and depolarized (s-p) BLS spectra of sample S21089, as-deposited and annealed at 500 °C and 900 °C, collected at a fixed incidence angle of θ\theta=70° (only the Stokes side is shown for clarity). Arrows indicate the variation in the frequency of longitudinal (LB, LM) and shear (SHM) acoustic waves and the frequency invariance of the Rayleigh wave (RW).

We now examine the effects of post-deposition heat treatment in detail. Figure 5(a) and Figure 5(c) show that both the optical and elastic properties of IBS SiO2_2 films are highly sensitive to annealing, with higher temperatures resulting in lower refractive index and stiffness coefficients (Table III in Appendix § 17). From an elasticity perspective, annealing induces a general softening of the material: the decreases in c33c_{33} and c44c_{44} — both reflecting out-of-plane properties — indicate that the film becomes easier to compress and shear along the direction perpendicular to the surface, while the decreases in c11c_{11} and c66c_{66} — both reflecting in-plane properties — indicate diminished resistance to in-plane compressional and shear deformation. Figure 5(d) reveals that variations in refractive index correlate strongly with density changes, consistent with the Lorentz–Lorenz relation (n5322−1)/(n5322+2)=ρ(NAαe)/(3Me)(n_{532}^2 - 1)/(n_{532}^2 + 2) = \rho(N_{\mathrm{A}}\alpha_{\mathrm{e}})/(3M_{\mathrm{e}}), where NAN_{\mathrm{A}} is Avogadro’s number, MeM_{\mathrm{e}} the effective molecular weight, and αe\alpha_{\mathrm{e}} the effective polarizability of the material’s structural units. Quantitatively, after annealing at 900 °C, n532n_{532} drops by 2%, and the density decreases by 7%. While density reduction after 10–hour annealing at 500 °C has been reported for materials like SiO2_2, Ta2_2O5_5, and TiO2_2:Ta2_2O5_5 [9, 45], this study shows that for SiO2_2, the effect persists even at much higher temperatures.

Annealing reduces the elastic moduli to varying de-

grees [Fig. 5(c)], and it is instructive to separate the purely acoustic and density-related contributions to these reductions. Heat treatment simultaneously affects sound velocity and atomic concentration, two factors that can have compensating effects on elasticity [see Eq. (2)]. The data in Figure 5(b) show that the sound velocities of longitudinal and horizontal shear modes are affected in opposite ways, with longitudinal waves becoming slower and shear waves faster as the annealing temperature increases. The slowdown of longitudinal acoustic waves after annealing at 900 °C is considerably larger than that produced by annealing at 500 °C (see also Figure 17 in Appendix C). By contrast, the Rayleigh-wave velocity, which mainly involves particle motion localized near the film surface, is largely insensitive not only to film thickness but also to heat treatment, as shown in Figure 19 in the Appendix C. The density reduction decreases both c11c_{11} and c33c_{33} by up to 13–16% at 900 °C and dominates the concurrent 4% decrease of c44c_{44}. By compensating the increase in vSHMv_{\mathrm{SHM}}, it also leads to a net 4% reduction in c66c_{66}. As a result, compressional softening in both in-plane and out-of-plane directions is markedly more pronounced than shear softening, while the material preserves its shear isotropy.

Image not extracted

Figure 19. Phase velocity vRWv_{RW} of the Rayleigh surface wave, as a function of the incidence angle θ\theta, in films of thickness 2.5 μ\mum (S21089) and 720 nm (S21088, S19175) in different states. The solid line is the best-constant fit of all data, with the 95% confidence band highlighted.

An important point is how anisotropy is affected by the post-deposition treatment. Although all measured quantities decrease as the annealing temperature increases, we find that the differences nBLS−n532n_{\mathrm{BLS}}-n_{532} and c33−c11c_{33}-c_{11} [Figs. 5(a) and 5(c)] surprisingly remain unchanged within the experimental error after annealing at 500 °C. Instead, both differences are reduced by approximately a factor of 2.5 after annealing at 900 °C. Therefore, as a second remarkable finding, we demonstrate that the heat treatment so far adopted for mirrors in GW detectors (10 hours at 500 °C), although beneficial for reducing coating thermal noise, is unable to alter the compressive anisotropy that silica acquires during deposition. Notably, the reduced anisotropy observed after annealing at 900 °C correlates well with a higher degree of structural relaxation, as reported in IR [46] and Raman [9] studies. This suggests that recovering isotropy is correlated to mechanical loss reduction.

Comparison with low-frequency elastic properties

As anticipated, BLS spectroscopy probes the elastic constants of SiO2_2 at frequencies of tens of GHz, which is far above the frequency range between about 10 Hz and a few hundred Hz where mirror coatings represent a limiting noise source for GW detectors. However, a recent study [15] reported the elastic characterization of the same material — produced by LMA under identical conditions — in the much lower frequency range of 1–30 kHz, which is more directly relevant for the detection of GW signals. Data are only available for the as-deposited material and after annealing at 500 °C [15], obtained using a Gentle Nodal Suspension (GeNS) system.

We now compare the results of the two techniques. First, one has to consider that GeNS measurements yield the real part of the Young’s modulus and Poisson’s ratio under the assumption of isotropic medium. A direct comparison with the present BLS results, which reveal elastic anisotropy, is therefore not straightforward. However, an approximate comparison can be made using the estimated values of YY and ν\nu that would reasonably be obtained by neglecting the anisotropy described in the previous section. To this end, we calculate YY and ν\nu according to Eq. (3), replacing MM with the average of the longitudinal moduli c11c_{11} and c33c_{33}, and GG with the average of the shear moduli c44c_{44} and c66c_{66}. The results are reported in Table I. Notably, as the annealing temperature increases, the BLS-estimated values of YY and ν\nu confirm material’s softening.

Although a comparison up to 900 °C is not available, some observations deserve attention. As a first remark, the value of the Young’s modulus in the as-deposited materials is the same at GHz and kHz frequencies, meaning that the contribution of relaxation processes in the intermediate frequency range is negligible within the experimental sensitivity. The implication would be that the more accurate high-frequency value provided by BLS can be used in place of the low-frequency value provided by GeNS. Apparently, the same is not true in the materials annealed at 500 °C. This discrepancy may find an explanation in the density used in the two studies. The values for the as-deposited materials (2.39 ± 0.01 and 2.38 ± 0.01 g/cm3^3, respectively, in Ref. [15] and in this work), despite determined by different methods coincide within the uncertainty. By contrast, those for the materials annealed at 500 °C (2.28±0.01 and 2.36±0.03 g/cm3^3, respectively) differ significantly. Notably, thanks to their smaller uncertainties, the BLS data clearly resolve the dependence of YY on annealing temperature — a trend that in the GeNS results is entirely masked by experimental uncertainty — and reveal that, as the treatment temperature increases, YY approaches the value of fused silica, measured in the present work and consistent with textbooks [47] and technical datasheets [48, 49, 50]. While we are unable to provide an explanation of the higher density reported in Ref. [15] for the film annealed at 500 °C, we note that if the density measured in the present study were used, then the best-value of Young’s modulus determined by GeNS would be in perfect agreement with the BLS estimate. These considerations suggest that contributions from mechanical relaxations in the GHz to kHz range are within the experimental uncertainty.

The experimental evidence is supported by theoretical expectation. The well-known model of thermally activated relaxations in amorphous solids by Gilroy and Phillips [51] predicts a loss angle with a power-law frequency dependence, ϕ=ϕ0⋅(f/f0)α\phi=\phi_0\cdot(f/f_0)^\alpha, valid for 2πf≪1/τ02\pi f\ll1/\tau_0, where τ0≈10−13\tau_0\approx10^{-13} s is a characteristic time, f0f_0 is a reference frequency, and ϕ0=ϕ(f0)\phi_0=\phi(f_0) and α\alpha are constants. From Eqs. (13) and (14) of ref. [51], one derives the real part of the Young’s modulus YY, relative to Y0=Y(f0)Y_0=Y(f_0),

as Y/Y0=[(2πfτ0)α−1]⋅(2ϕ0)/[πα(2πτ0f0)α]Y/Y_0 = [(2\pi f\tau_0)^\alpha- 1] \cdot(2\phi_0)/[\pi\alpha(2\pi\tau_0 f_0)^\alpha]. Using this expression, the relative difference of the modulus at frequencies f1f_1 and f2f_2 is given by:

Y(f2)−Y(f1)Y0=2ϕ0πα[(f2f0)α−(f1f0)α](7)\frac{Y(f_2)-Y(f_1)}{Y_0} = \frac{2\phi_0}{\pi\alpha}\left[\left(\frac{f_2}{f_0}\right)^\alpha-\left(\frac{f_1}{f_0}\right)^\alpha\right] \tag*{(7)}

Reasonable parameters for a silica film are f0=10f_0 = 10 kHz, ϕ0=10−4\phi_0 = 10^{-4}, and α≃0.1\alpha\simeq0.1 [15]. With these values, the relative difference between f1=1f_1 = 1 kHz and f2=30f_2 = 30 GHz is approximately 0.2%, corresponding to about 0.2 GPa for a modulus of around 80 GPa. The result is that the Young’s modulus measured with GeNS and BLS is expected to differ by an amount well within the experimental uncertainty. Therefore, the value provided by BLS can be used to constraint the analysis of GeNS measurements, and to reduce the effect of criticalities such as the influence by sample geometry and boundary conditions, the need of a model to simulate the experimental data, and prior knowledge of the substrate properties (limitations to which Brillouin spectroscopy is immune) [15, 16, 52]. More importantly, BLS is capable of detecting anisotropy effects —that correlate to the presence of residual dissipative mechanisms— to which the GeNS analysis remains insensitive.

Finally, a remark on the Poisson’s ratio is in order. All studies of silica for GW detectors assume isotropy in this parameter. However, unlike the Young’s modulus, the Poisson’s ratio estimated from BLS under the isotropic approximation is nearly twice the value previously reported from GeNS measurements [15] up to 500 °C of annealing temperature, and markedly reduces when the material is annealed well above 500 °C. This result is unexpected, and indicates a resistance to lateral deformation under axial stretching that is substantially lower than that adopted in earlier modeling and data analysis [15, 16, 17]. Prompted by the marked discrepancy identified in the present work, the GeNS measurements originally reported in Ref. [15] were carefully reanalyzed by Granata and Cagnoli, who are the holders of the original GeNS data and coauthors of both Ref. [15] and the present manuscript. The reanalysis revealed that the discrepancy originates from a transcription error in the numerical simulation code used to extract the elastic parameters in Ref. [15]. The discrepancy is therefore neither attributable to a frequency-dependent Poisson’s ratio nor to geometric or boundary-condition artifacts of the GeNS technique. The corrected GeNS values are reported in Table I, together with the originally published estimates and the BLS results. The corrected values are fully consistent, within uncertainties, with the BLS estimates, similarly to what is observed for the Young’s modulus. Owing to their significantly smaller uncertainties (by about one order of magnitude), the BLS data clearly resolve the dependence on annealing temperature —a trend that is only barely visible in the best-fit GeNS values and entirely masked by their experimental uncertainty— revealing that both YY and ν\nu of IBS silica approach the values of fused silica as the annealing temperature increases [47, 48, 49, 50].

YY (GPa)ν\nu
BLS(a)^{(a)}GeNS(b)^{(b)}GeNS(c)^{(c)}BLS(a)^{(a)}GeNS(b)^{(b)}GeNS(c)^{(c)}
as-deposited78.5±0.478.5 \pm0.478±178 \pm179±179 \pm10.229±0.0040.229 \pm0.0040.14±0.010.14 \pm0.010.23±0.050.23 \pm0.05
10h@500 °C75.0±0.575.0 \pm0.578±178 \pm178±278 \pm20.220±0.0050.220 \pm0.0050.11±0.010.11 \pm0.010.20±0.050.20 \pm0.05
10h@900 °C71.8±0.371.8 \pm0.30.178±0.0040.178 \pm0.004
fused SiO2_2≈72−73(d)\approx72 - 73^{(d)}≈0.17(d)\approx0.17^{(d)}

Table I. Real part of the Young’s modulus YY and Poisson’s ratio ν\nu of IBS SiO2_2 films, estimated under the assumption of isotropic material from BLS and GeNS. The values for fused silica at room temperature are also reported for comparison.

This downshift toward fused-silica-like properties, that emerges clearly from the BLS characterization, reasonably extends to the elastic dissipation behavior and has potential implications for the level of thermal noise in the material. In the absence of an analytic expression for the thermal noise in anisotropic media, an approximate estimate of its relative variation as a function of the annealing temperature is performed for sample S21088 by considering its isotropic-analogous properties. For these calculations, we use the elastic parameters reported in Table I, the layer thickness derived in § 5 C, and the loss angle ϕ\phi given in the Appendix § 16. Different analytic models [13, 18, 19, 20, 21], in their commonly used approximate expressions Eqs. (12) and (13) in the Appendix, indicate that the amplitude spectral density of thermal noise in the silica monolayer is reduced by about 60% relative to the as-deposited state (corresponding to a factor of 2.5) after annealing at 500 °C, and by a further 60% relative to the 500 °C sample after annealing at 900 °C. The results are confirmed for substrates other than silicon, such as fused silica and sapphire. These findings suggest that suppression of residual anisotropy —which concomitantly lowers both the real part of the elastic constants and their associated loss factors— can reduce, albeit to different extents, the thermal-noise contribution of individual materials within high-reflectivity multilayer coatings. At present, extending such thermal treatments to full high-reflectivity stacks is constrained by the thermal stability of the high-index material currently employed, which limits the accessible annealing temperatures. More refined estimates, both for monolayers and heterostructures, require models that allow for anisotropic tensors with independent loss factors for different elastic moduli. In this respect, numerical modeling—although demanding—appears to be the only rigorous approach.

Local structure

Structure on planes parallel to the surface

In the SR-IR spectra of samples S21089 and S21088 at different annealing temperatures [Figure 6(a)] the TO component of the antisymmetric Si-O-Si stretching vibration stands out at ∼1100–1120 cm−1^{-1} as the most intense signal, superimposed on an oscillating background. As recalled in § 3 B, this mode serves as a probe of the structure on surface-parallel planes, and acquisition at fixed incidence of θ=30∘\theta=30^\circ ensures that the structure is probed in the two samples of different thicknesses up to an equal depth from the surface. According to the central force network model [38, 39] the frequency position ωTO\omega_{TO} of the TO mode depends on θ∥\theta_{\parallel}, the mean Si-O-Si bonding angle on planes parallel to the surface. Figure 6(b) indicates a blue shift of about 20 cm−1^{-1} in ωTO\omega_{TO}, corresponding to an increase of about 5∘5^\circ in θ∥\theta_{\parallel} on increasing the annealing temperature up to 900 °C. ωTO\omega_{TO} could be determined with an uncertainty of about 2% because of the intense oscillating background present in the spectra. The result, confirmed in sample S19175, suggests that the structural properties and the changes induced by the post-deposition treatment are largely independent of the film thickness. It is interesting to note that the values of ωTO\omega_{TO} and θ∥\theta_{\parallel} on increasing the annealing temperature align fairly well with the values of fused silica measured in the present work and consistent with literature data [42, 46].

Image not extracted

Figure 6. (a) SR-IR spectra of the samples S21089 and S21088 as-deposited and annealed at different temperatures, acquired at incidence angle θ=30∘\theta=30^\circ in the wavenumber region of 6000–800 cm−1^{-1}, together with their enlargement in the absorption peaks region of 1400–900 cm−1^{-1}. (b) Frequency position of the TO mode, ωTO\omega_{\mathrm{TO}} (upper panel), and mean Si-O-Si bonding angle on the planes parallel to the surface, θ∥\theta_{\parallel} (lower panel), as a function of the annealing temperature. The values of fused silica are reported for comparison with crosses (black: this work; orange: Ref. [42]; cyan: Ref. [46]).

Structure in direction perpendicular to the surface

The polarization of IR radiation significantly influences the spectra in the region 1400–900 cm−1^{-1}. At fixed incidence, p-polarized radiation markedly enhances the relative intensity of the TO and LO bands compared to s-polarized radiation, while having a negligible effect on their frequencies (Figure 20 in Appendix C). In contrast, varying the angle of incidence leaves ωTO\omega_{TO} unchanged but causes a significant shift in the LO mode [Figure 7(a)] [53]. Different incidence angles result in different values of penetration depth, depending also on nn and kk [Eq. (5)]. Optical quantities in the absorption region were obtained from Kramers-Krönig (KK) transformation of SR-IR spectra of SiO2_2 films on SiO2_2 substrates, with perfectly flat background, deposited by LMA under identical conditions. The values of nn and kk obtained this way for the untreated and annealed material can be found in Table IV in Appendix § 17. They exhibit a strong frequency dispersion, and a good agreement with the value of nn measured by SE at higher frequency. Notice that this behavior reflects into a great frequency dependence of dpSRd_p^{SR}. As shown in Tab. II for the as-deposited material, at 1000–1100 cm−1^{-1}, characteristic range of the TO band, dpSRd_p^{SR} is approximately independent of θ\theta from 30° to 80°. Conversely, there is a significant dependence on θ\theta at 1200–1250 cm−1^{-1}, characteristic range of the LO band. The values of dpSRd_p^{SR} indicate that, by changing the radiation incidence, the LO band is capable of probing layers of film material with varying thicknesses from the surface.

Image not extracted

Figure 7. (a) SR-IR spectra of the as-deposited sample S21089, measured at different incidence angles θ\theta using p-polarized radiation. (b) Peak position of the LO mode, ωLO\omega_{\mathrm{LO}}, as a function of the radiation penetration depth, dpSRd_p^{\mathrm{SR}}, in the sample S21089 and (c) the samples S21088 and S19175.

Image not extracted

Figure 20. Longitudinal (LO) and transverse (TO) optical modes. Specular reflection infrared (SR-IR) spectra of sample S21089 in the as-deposited state, acquired at a fixed incidence angle of θ=67∘\theta= 67^\circ with different IR radiation polarizations. This angle was selected to reduce overlap with interference fringes and to amplify the intensity of the LO band.

by IR ±0.03
n1000 cm−1n_{1000\ \mathrm{cm}^{-1}}k1000 cm−1k_{1000\ \mathrm{cm}^{-1}}n1100 cm−1n_{1100\ \mathrm{cm}^{-1}}k1100 cm−1k_{1100\ \mathrm{cm}^{-1}}n1200 cm−1n_{1200\ \mathrm{cm}^{-1}}k1200 cm−1k_{1200\ \mathrm{cm}^{-1}}n1250 cm−1n_{1250\ \mathrm{cm}^{-1}}k1250 cm−1k_{1250\ \mathrm{cm}^{-1}}
as deposited3.301.020.541.990.480.780.360.43
10h@500°C3.330.640.442.250.440.810.320.43
10h@900°C2.860.400.452.320.370.790.280.40
by SE ±0.005by IR ±0.03
n4000 cm−1n_{4000\ \mathrm{cm}^{-1}}n4000 cm−1n_{4000\ \mathrm{cm}^{-1}}k4000 cm−1k_{4000\ \mathrm{cm}^{-1}}
as deposited1.4641.430.08
10h@500°C1.4451.450.05
10h@900°C1.4371.440.03

Table IV. Real (nn) and imaginary part (kk) of the complex refractive index obtained from the Kramers-Krönig (KK) transformation of SR-IR spectra of SiO2_2 films on SiO2_2 substrate. The upper part of the table reports the values at selected wavevectors in the range 1000–1250 cm−1^{-1}. The lower part of the table compares the value of nn estimated by the KK transformation at 4000 cm−1^{-1} with that measured by SE for sample S21088.

The frequency position ωLO\omega_{LO} of the LO mode is associated with θ⊥\theta_{\perp}, the average angle between tetrahedral silicate units along the direction perpendicular to the surface [42]. ωLO\omega_{LO} for the sample S21089 is reported in Figure 7(b) as a function of dpSRd_p^{SR}, in the range of θ\theta from 40° to 75°. Its value decreases over the penetration range of 70–600 nm, more markedly from 70 to 150 nm, suggesting that the film exhibits a structural gradient along the surface-normal direction, likely driven by a variation in the distribution of angles at bridging oxygens along the growth axis, formed during the deposition process. The data indicate that this gradient is particularly pronounced in the as-deposited film, and progressively reduces on increasing the annealing temperature up to 900°C, tending to the case of fused silica where the gradient is absent. Similar behavior is found in thinner films (samples S21088 and S19175) where reliable values of ωLO\omega_{LO} are only obtained in the limited range 65∘<θ<80∘65^\circ<\theta<80^\circ [Figure 7(c)]. Nonetheless, it is evident a decrease in the 70–150 nm penetration range, less pronounced with increasing the annealing temperature: ∼15 cm−1^{-1} in the untreated material, and ∼5 cm−1^{-1} after annealing at 900°C. Therefore, in all samples, within the first hundred nanometers from the surface the distribution of Si-O-Si angles is consistent with the picture of a material grown with compressive stress and a lower surface density. The post-deposition heat treatment reduces the heterogeneity in the growth direction by increasing the average Si-O-Si bonding angle, thus leading to an average density decrease.

Chemical defects

The reduced penetration depth of the IR radiation in ATR configuration accounts for the absence of interference fringes in the spectra, shown in Figure 8(a). In the absorption peaks region they exhibit a maximum intensity at frequencies where the stretching mode of NBO-containing groups resonates (∼1000 cm−1^{-1}). Thus, ATR-IR spectra enable a convenient evaluation of NBO-related chemical defects in the silica structure. These defects are here attributed to the presence of Si-O−^- groups inside the material rather than to the presence of Si-OH groups from moisture capture, since no OH-stretching signal around 3600 cm−1^{-1} is detected.

Image not extracted

Figure 8. (a) ATR-IR spectra of the sample S21089, as-deposited and annealed at different temperatures, acquired in the range 3800–700 cm−1^{-1}. (b) ATR-IR profile in the as-deposited material fitted by four Gaussian components. (c) Relative area of the NBO band as a function of the radiation penetration depth, dpATRd_p^{\mathrm{ATR}}, in the samples as-deposited (upper panel) and annealed at 900 °C (lower panel).

Wavenumber (cm−1^{-1})dpSRd_p^{\mathrm{SR}} (nm), θ=30∘\theta=30^\circdpSRd_p^{\mathrm{SR}} (nm), θ=40∘\theta=40^\circdpSRd_p^{\mathrm{SR}} (nm), θ=50∘\theta=50^\circdpSRd_p^{\mathrm{SR}} (nm), θ=55∘\theta=55^\circdpSRd_p^{\mathrm{SR}} (nm), θ=60∘\theta=60^\circdpSRd_p^{\mathrm{SR}} (nm), θ=65∘\theta=65^\circdpSRd_p^{\mathrm{SR}} (nm), θ=70∘\theta=70^\circdpSRd_p^{\mathrm{SR}} (nm), θ=75∘\theta=75^\circdpSRd_p^{\mathrm{SR}} (nm), θ=80∘\theta=80^\circ
1000714712706704700613606568541
1100356352344340334333330327321
12006646044563642471881657473
12506765722451381161111067575

Table 2. Penetration depth dpSRd_p^{\mathrm{SR}} of the IR radiation of different wavenumber in SR-IR configuration, inside the as-deposited material. Estimated uncertainty is 10%.

A quantitative estimate of the NBO structures is obtained by fitting the ATR-IR profile in the range 1310–750 cm−1^{-1} with four Gaussian components, reproducing the LO, TO, and NBO bands, plus the symmetric stretching mode of the Si-O-Si unit [Fig. 8(b)]. The relative area of the NBO component in the as-deposited material and that annealed at 900 °C is reported as a function of dpATRd_p^{\mathrm{ATR}} in Figure 8(c). Along with a significant reduction in NBO structures after annealing, the data show a slight increase in these defects at smaller radiation penetration depths, suggesting that a higher concentration of NBOs is localized near the surface. This indicates that an additional source of inhomogeneity may be related to the material’s ability to capture cations, likely Ar+^+ involved in the deposition process. These cations are intuitively expected to induce the formation of Si-O−^- groups, particularly near the surface. Therefore, anisotropy is also associated to the presence of chemical defects that persist in the film even after high temperature treatment.

Film thickness

In thin films such as sample S21088, both BLS and SR-IR spectra exhibit features resulting from wave interference, useful for determining the film thickness. In SR-IR spectra the interfering waves are IR electromagnetic radiation, whereas in BLS spectra they are acoustic waves. Despite the differing nature of these waves, the dependence of the interference phenomenon on hh can be exploited as explained hereafter.

On one hand, the interference pattern in SR-IR spectra arises from the difference in optical distance traveled by light of each wavelength λ\lambda reflected at the two film interfaces. Taking into account the dependence on λ\lambda of the material’s refractive index, the film thickness can be determined from regions of the spectrum where individual interference fringes can be resolved, according to

hIR=N2[n(λ1)/λ1−n(λ2)/λ2],h_{\mathrm{IR}} = \frac{N}{2[n(\lambda_1)/\lambda_1-n(\lambda_2)/\lambda_2]},

where NN is the number of fringes observed from wavelength λ1\lambda_1 to λ2>λ1\lambda_2 > \lambda_1, and n(λ1,2)n(\lambda_{1,2}) is the refractive index at these wavelengths [54]. For sample S21088, hIRh_{\mathrm{IR}} is calculated from Figure 6(a) with λ1=1667\lambda_1=1667 nm and λ2=2500\lambda_2=2500 nm by using n(λ)n(\lambda) measured by SE (Figure 12 in Appendix A). On the other hand, the multiple peaks in BLS spectra at quasi-normal incidence (Figure 9(a)) arise from the scattering of light by discrete acoustic modes normal to the film surface, that exist as standing waves because they satisfy the condition for constructive interference of propagating acoustic waves reflected at the two film interfaces. The film thickness can be determined from the frequency separation Δf\Delta f of these peaks, according to

Image not extracted

Figure 9. (a) Polarized BLS spectra at quasi-normal incidence of the sample S21088, as-deposited and annealed at 500 °C and 900 °C. The frequency separation Δf\Delta f of the discrete peaks in the as-deposited film are shown on the right. Solid lines are a fit with Gaussian functions of equal width. (b) Thickness hh of the sample S21088 as a function of the annealing temperature, estimated by different techniques as indicated in the legend. Dotted lines are a guide for the eyes.

hBLS=vLB2Δf.h_{\mathrm{BLS} } = \frac{v_{\mathrm{LB}}}{2\Delta f}.

Δf\Delta f is obtained by a simple data analysis, as illustrated in Figure 9(a). The velocity vLBv_{\mathrm{LB}} of longitudinal acoustic waves traveling in the surface-normal direction is taken from sample S21089, as it has been demonstrated that the acoustic properties of the material are independent of film thickness.

In Figure 9(b), hIRh_{\mathrm{IR}} and hBLSh_{\mathrm{BLS}} are reported as a function of the annealing temperature, and compared with the values provided with nanometer-level accuracy by SEM and SE. An excellent agreement of hIRh_{\mathrm{IR}} is observed at all temperatures. The data, while confirming the previously established result [15] that annealing at 500 °C causes a thickness increase, reveal that the effect becomes nearly three times larger at 900 °C (+7.4 % relative to the as-deposited film) and correlates with a decrease in material’s density. Notably, assuming that the mass and surface area remain unchanged upon annealing, this thickening fully accounts for the observed density reduction. Unexpectedly, the agreement of hBLSh_{\mathrm{BLS}} is limited to the highest temperature. Specifically, in the untreated material and that annealed at 500 °C, hBLSh_{\mathrm{BLS}} underestimates hh by ~5–6%, while the disagreement vanishes in the material annealed at 900 °C, where elastic anisotropy is drastically reduced. The result is confirmed in sample S19175 (Figure 21 in Appendix C), ruling out any measurement artifact. It should be noted that only optical properties of the material are required to calculate hIRh_{\mathrm{IR}}. Conversely, the calculation of hBLSh_{\mathrm{BLS}} relies on acoustic parameters (vLBv_{\mathrm{LB}}, Δf\Delta f), which are linked through a simplified model assuming a homogeneous film where specific boundary conditions at the interfaces must be fulfilled by acoustic waves (§ 3 A). One plausible reason for the observed mismatch between hBLSh_{\mathrm{BLS}} and the actual film thickness in both the as-deposited and 500 °C-annealed samples is the simplicity of the adopted model, which does not account for the structural heterogeneity along the surface-normal direction revealed by the IR analysis. The discrepancy can therefore be interpreted not merely as a limitation of the model, but as a signature of inhomogeneity, directly linked to elastic anisotropy in our samples. Consistently, it disappears in the 900 °C-annealed sample, where both the structural gradient and elastic anisotropy are strongly suppressed.

Image not extracted

Figure 21. Variation of film thickness, hh, with annealing temperature for sample S19175, as determined by SE and BLS spectroscopy.

Conclusions

The elastic and structural properties of IBS thin films have so far been assumed isotropic without direct verification, despite their central role in governing coating thermal noise in GW detectors. Any unaccounted anisotropy in these properties may contribute to the persistent gap between predicted and measured noise [15, 16] and limit future sensitivity improvements. Silica remains a cornerstone material for mirror coatings, making its study per se crucial and, at the same time, a gateway to uncovering a fundamental and previously overlooked link between elastic and structural anisotropy and mechanical dissipation. Establishing this link can feed new predictive models, with direct impact on both coating design and processing strategies.

Addressing this issue requires an experimental approach that goes beyond current characterization practices. This study combines macroscopic information from BLS measurements with structural insight from IR spectroscopy. BLS provides a complete characterization of the elastic response — difficult, if not impossible, to achieve with conventional mechanical testing — revealing that ion-beam sputtered SiO2_2 exhibits cylindrical symmetry and a sizeable out-of-plane compressive anisotropy (+6%) in the as-deposited state. At the atomic scale, IR reflectivity measurements, including depth profiling of bridging and non-bridging oxygens, confirm in-plane structural isotropy while uncovering a gradient along the growth axis, consistent with compressive stress and lower surface density. Annealing leads to a softening of all elastic constants. Critically, however, the anisotropy remains unchanged after the post-deposition heat treatment currently used in ground-based detectors (10 hours at 500 °C), and is almost completely removed only after annealing at the highest temperature tested (900 °C). The structural gradient — not directly resolvable by BLS — is likewise strongly reduced at high temperature, consistent with the trend toward restoring macroscopic isotropy revealed by BLS, and with both the elastic response and the structural profile converging toward those of fused

silica. Beyond their independent diagnostic power, both BLS and IR yield sub-micrometric thickness estimates that can be benchmarked against SEM and SE. IR, SE and SEM consistently show that annealing drives a directional recovery, with pronounced film expansion (> 7%) exclusively along the growth axis, while the in-plane dimensions remain essentially unchanged. By contrast, the BLS-based thickness agrees with IR, SE, and SEM estimates only at the highest annealing temperature, where elastic isotropy is nearly restored. The discrepancy at lower temperatures thus emerges as a direct marker of structural inhomogeneity, which correlates with elastic anisotropy and vanishes as the material approaches isotropic behavior.

In addition, our study has direct implications for how the elastic properties of mirror-coating materials are determined. BLS probes the real part of the elastic constants at GHz frequencies, clearly resolving their dependence on annealing temperature. By contrast, the standard technique in the field, GeNS, operates at kHz frequencies — closer to the GW-relevant band — but with lower accuracy and no sensitivity to elastic anisotropy. The comparison shows that relaxation processes between kHz and GHz contribute negligibly to the isotropic-effective Young’s modulus, validating the high-frequency BLS values as reliable proxies for the low-frequency response. Crucially, this study enables a robust reassessment of the widely used GeNS Poisson’s ratio values for silica, removing a systematic bias in current inputs to coating-thermal-noise estimates. Using the more realistic values determined here will directly improve future simulations.

Our study challenges the long-standing assumption of elastic and structural isotropy in amorphous materials for GW mirror coatings, providing quantitative evidence of anisotropy in ion-beam sputtered SiO2_2 and linking it to mechanical dissipation. A coherent physical picture emerges in which the downshift toward fused-silica-like isotropic properties translates, within isotropic-equivalent modeling, into a substantial reduction of thermal noise, by about a factor of 2.5. Crucially, our results indicate that restoring isotropy — and thus reducing thermal noise — requires annealing temperatures significantly above the current standard.

The implications extend well beyond silica, offering a concrete pathway to unlock sensitivity gains in future GW detectors. Low-loss materials are essential not only for upgrading current facilities but also for designing next-generation detectors, including the Einstein Telescope [55], where mirror coatings may depart from the conventional high/low-index doublet paradigm and may involve other materials than currently used. In this broader context, anisotropy-aware characterization is indispensable for assessing candidate materials, guiding the evolution of deposition and post-processing strategies, and refining coating design. Achieving quantitatively reliable thermal-noise predictions will also require sustained efforts toward numerical modeling frameworks capable of incorporating transverse isotropy tensors with independent loss factors and, when relevant, thickness variations induced by anisotropy suppression.

Beyond gravitational-wave detection, the thin-film characterization approach presented in this work may prove valuable in fields such as information and communication technologies and optoelectronics, where precise control of elastic and structural properties is likewise critical.

Acknowledgments

G. Cagnoli, M. G., and D. H. gratefully acknowledge the support of the French Agence Nationale de la Recherche (ANR) through grant n. ANR-18-CE08-0023 to the ViSIONs project. G. Carlotti, S. Corezzi, and P. S., acknowledge support from the European Union - NextGenerationEU, Mission 4, Component 2, under the Italian Ministry of University and Research (MUR) National Innovation Ecosystem Grant ECS00000041 - VITALITY - CUP J97G22000170005. G. Carlotti acknowledges support from Fondazione Cassa di Risparmio Terni e Narni (Project n. FCTR24UNIPG).

Author Contributions

S. Corezzi and P. S. conceived and supervised the work. D. H. and M. G. provided the samples. B. B., S. Corezzi, and G. Carlotti designed and performed the BLS study. B. B. and P. S. designed and performed the IR study. M. M. and S. Colace performed and analyzed the SE measurements. G. F. performed and analyzed the XRR measurements. A. D. M. performed and analyzed the SEM measurements. M. B. and M. C. provided resources. B. B. and S. Corezzi wrote the manuscript draft. B. B., S. Corezzi, and P. S. wrote the paper with contributions from G. Carlotti, G. Cagnoli, M. M., M. G., and L. S.. All authors read and reviewed the data and manuscript.

Characterization data

This appendix collects characterization data for sample S21088, including measurements obtained by XRR (Figure 10), SE (Figure 11 and Figure 12), and SEM (Figure 13). Detailed descriptions of the experimental methods and discussion of the results are reported in § 2 B of the main text.

Elasticity in a transversely isotropic semi-infinite medium

Elasticity tensor

The elastic behavior of a transversely isotropic medium (cylindrical symmetry; space group: D∞hD_{\infty h}) is described by five independent elastic constants. With axis x3x_3 perpendicular to the film surface, and axes x1x_1 and x2x_2 in plane, these constants are c11c_{11}, c33c_{33}, c44c_{44}, c66c_{66}, c13c_{13}. The fourth-order elasticity tensor cijklc_{ijkl}, symmetric under index exchange i↔ji \leftrightarrow j, k↔lk \leftrightarrow l, and (ij)↔(kl)(ij) \leftrightarrow(kl), can be represented in the compact Voigt notation as a symmetric (6 x 6) matrix given by:

cij=(c11c12c13000c12c11c13000c13c13c33000000c44000000c44000000c66)(8)c_{ij} = \begin{pmatrix} c_{11} & c_{12} & c_{13} & 0 & 0 & 0 \\ c_{12} & c_{11} & c_{13} & 0 & 0 & 0 \\ c_{13} & c_{13} & c_{33} & 0 & 0 & 0 \\ 0 & 0 & 0 & c_{44} & 0 & 0 \\ 0 & 0 & 0 & 0 & c_{44} & 0 \\ 0 & 0 & 0 & 0 & 0 & c_{66} \end{pmatrix} \tag*{(8)}

with the symmetry constraint c12=c11−2c66c_{12}=c_{11}-2c_{66}. Physical meaning: the coefficients c11c_{11} and c33c_{33} (longitudinal stiffness in the isotropic plane and along the symmetry axis) describe the resistance to horizontal and vertical compression; c44c_{44} and c66c_{66} (vertical and horizontal shear modulus) describe the resistance to shearing along planes containing the symmetry axis and along the isotropic plane; c13c_{13} (coupling constant between axial and in-plane strains) describes how vertical compression induces lateral deformation and vice versa; c12c_{12} (coupling constant between deformations in the isotropic plane) is not independent, and can be computed from c11c_{11} and c66c_{66}.

Relation to bulk and surface wave velocities

(i) The phase velocities vv of bulk acoustic waves propagating in an arbitrary direction within a transversely isotropic half-space is governed by the Christoffel equation

det⁡[Γik−ρv2δik]=0(9)\det\left[\Gamma_{ik}-\rho v^2\delta_{ik}\right]=0 \tag*{(9)}

where Γik(n)=cijklnjnl\Gamma_{ik}(\mathbf{n})=c_{ijkl}n_jn_l is the Christoffel matrix build with the elastic constants in Eq. (8), n=(n1,n2,n3)\mathbf{n}=(n_1,n_2,n_3) the unit propagation vector, and ρ\rho the mass density. By solving Eq. (9) yields three bulk wave modes, i.e. longitudinal, shear vertical, and shear horizontal (SH), whose velocities depend on the propagation angle (α\alpha) relative to the symmetry axis. Special cases of propagation include those in Eq. (2) of the main text, namely:

along symmetry axis (x3x_3) →vLB(α=0∘)=c33ρ\rightarrow v_{LB}(\alpha=0^\circ)=\sqrt{\frac{c_{33}}{\rho}}

in isotropic plane (e.g., x1x_1) →vLM=c11ρ\rightarrow v_{LM}=\sqrt{\frac{c_{11}}{\rho}};

vSHM=c66ρ.(10)v_{SHM}=\sqrt{\frac{c_{66}}{\rho}}. \tag*{(10)}

Although the constants c44c_{44} and c13c_{13} do not appear in the above special cases, according to Eq. (9) the velocity of longitudinal bulk waves for oblique directions, vLB(α≠0∘)v_{LB}(\alpha\ne0^\circ), depends explicitly on c11c_{11}, c33c_{33}, c13c_{13}, c44c_{44}, and ρ\rho. (ii) The phase velocity vRv_R of the Rayleigh-wave, propagating along a surface direction (e.g., x1x_1), follows from solutions to the Christoffel equation that are exponentially decaying with depth (x3→∞x_3\rightarrow\infty), and by imposing the traction-free boundary condition at the surface. This leads to a secular equation depending on c11c_{11}, c33c_{33}, c13c_{13}, c44c_{44}, and ρ\rho, whose smallest positive root (less than the slowest bulk shear velocity) defines the Rayleigh-wave velocity vRv_R. The analytic relation between vRWv_{RW} and elastic constants, derived by Dobrzynski and Maradudin [56], is the following:

c33(vRW2−c44ρ)(vRW2−c11ρ+c132c33ρ)2=c44vRW4(vRW2−c11ρ).(11)c_{33}\left(v_{RW}^{2}-\frac{c_{44}}{\rho}\right)\left(v_{RW}^{2}-\frac{c_{11}}{\rho}+\frac{c_{13}^{2}}{c_{33}\rho}\right)^{2}=c_{44}v_{RW}^{4}\left(v_{RW}^{2}-\frac{c_{11}}{\rho}\right). \tag*{(11)}

Procedure for complete determination of elastic moduli

According to Eqs. (10), with the material density known, the elastic constants c11c_{11} and c66c_{66} are directly determined by measuring the velocities vLMv_{LM} and vSHMv_{SHM} of longitudinal and shear-horizontal waves propagating parallel to the surface, while c33c_{33} is determined by measuring the velocity vLB(α=0∘)v_{LB}(\alpha=0^\circ) of longitudinal waves propagating along the normal-to-surface direction. The remaining independent constants, c13c_{13} and c44c_{44}, can be evaluated from the Rayleigh surface-wave velocity vRWv_{RW} and the longitudinal bulk waves velocity vLB(α≠0∘)v_{LB}(\alpha\ne0^\circ) for different oblique directions. In fact, both vRWv_{RW} and vLBv_{LB} for each propagation angle depend on c11c_{11}, c33c_{33}, c13c_{13}, c44c_{44}, and ρ\rho. Thus, once c11c_{11}, c33c_{33} and ρ\rho are measured directly, only c13c_{13} and c44c_{44} remain unknown. Their values can be obtained by jointly fitting the theoretical predictions of the Christoffel [Eq. (9)] and Maradudin [Eq. (11)] equations to the experimental wave velocities. This procedure uniquely determines the elastic constants c44c_{44} and c13c_{13}, leading to complete determination of the material’s elastic behavior.

Additional BLS and IR data

This appendix collects additional BLS (Figure 16 and Figure 17) and SR-IR spectra (Figure 20), along with data on acoustic velocities obtained from numerical simulations (Figure 14) and BLS experiments (Figure 15, Figure 17, and Figure 19), and data of film thickness (Figure 21) derived from BLS measurements. The figures included here complement the results presented in the main text, providing a more complete representation of the experimental data, and illustrating trends and features discussed in § 5 of the article.

BLS results for D 263® M cover glass

The borosilicate cover glass D 263® M by SCHOTT (https://www.schott.com/en-gr/products), 145 ±\pm 15 μ\mum-thick, served as a reference isotropic material. A reflective substrate was created by sputter-coating several hundred nanometers of chromium onto one side, replicating the scattering geometry in Figure 1 of the manuscript. BLS spectra were collected using the same setup and measurement conditions as those used for the IBS SiO2_2 films produced by LMA. Polarized (s-s) and depolarized (s-p) spectra were acquired at incidence angles θ=10∘\theta= 10^\circ, 65∘65^\circ, 70∘70^\circ, 75∘75^\circ (Figure 22). Consistent with thick films of glassy materials, the high-frequency spectrum is unimodal and well-fitted by a Lorentzian line shape.

Image not extracted

Figure 22. Polarized (s-s) and depolarized (s-p) BLS spectra of D 263® M cover glass at varying incidence angles. Arrows indicate that the frequencies fLMf_{LM} and fSHMf_{SHM} of LM and SHM acoustic waves increase with incidence angle, whereas the frequency fLBf_{LB} of LB acoustic wave remains unchanged.

As expected for elastically and optically isotropic materials, the calculated quantity nBLS=(fLB/fLM)sin⁡θ=1.528±0.003n_{BLS} = (f_{LB}/f_{LM})\sin\theta= 1.528 \pm0.003 is found to be independent of θ\theta and agrees, within the experimental error, with the refractive index at the BLS wavelength, n532=1.5265±0.0015n_{532} = 1.5265 \pm0.0015, derived from the certified value of standard refractive index at 546.1 nm, ne=1.5255±0.0015n_e = 1.5255 \pm0.0015.

Additionally, the Poisson’s ratio ν\nu is determined from BLS frequencies using the relation:

ν=2G−M2(G−M)=2fSHM2−fLM22(fSHM2−fLM2).\nu= \frac{2G-M}{2(G-M)} = \frac{2f_{SHM}^{2}-f_{LM}^{2}}{2(f_{SHM}^{2}-f_{LM}^{2})}.

The calculated value, 0.220 ±\pm 0.005, is in excellent agreement with the reported value of 0.21.

Thermal noise estimate

We report here commonly used analytic models of coating thermal noise, explicitly assuming isotropic materials. For each model, we first present the general expression for a multilayer stack, followed by the simplified form for a single layer. All expressions are given in terms of the amplitude spectral density of thermal noise, defined as

x(f)=Sx(f),x(f) = \sqrt{S_x(f)},

where Sx(f)S_x(f) is the power spectral density of thermal fluctuations of the coating surface.

(i) According to Hong et al. [18], assuming equal mechanical losses for bulk and shear motions, the amplitude spectral density for a multilayer stack is:

x(f)=2kBTπ2fw21−νS−2νS2YS∑jbjhjΦjx(f) = \sqrt{\frac{2 k_B T}{\pi^2 f w^2}\frac{1-\nu_S-2\nu_S^2}{Y_S}\sum_j b_j h_j \Phi_j}

where kBk_B is the Boltzmann constant, TT the mirror temperature, ff the frequency, ww the radius of the laser beam on the coating, YSY_S and νS\nu_S the Young’s modulus and Poisson’s ratio of the substrate, and hjh_j and Φj\Phi_j are the thickness and loss angle of each layer forming the coating. bjb_j is a weighting factor whose expression, after the correction to Yam et al. [19] reported by Tait et al. [20], is given by:

bj=(1−2νj)(1+νj)(1−2νS)(1+νS)11−νj[(1−nj∂θc∂θj)2YSYj+(1−νS−2νS2)2(1+νj)2(1−2νj)YjYS]b_j = \frac{(1-2\nu_j)(1+\nu_j)}{(1-2\nu_S)(1+\nu_S)}\frac{1}{1-\nu_j}\left[\left(1-n_j\frac{\partial\theta_c}{\partial\theta_j}\right)^2\frac{Y_S}{Y_j}+\frac{(1-\nu_S-2\nu_S^2)^2}{(1+\nu_j)^2(1-2\nu_j)}\frac{Y_j}{Y_S}\right]

where νj\nu_j and νS\nu_S are the Poisson’s ratios of each coating layer and the substrate. njn_j is the refractive index of the jjth layer and ∂θc∂θj\frac{\partial\theta_c}{\partial\theta_j} describes the field penetration in each layer. Ignoring the field penetration (∂θc∂θj→0\frac{\partial\theta_c}{\partial\theta_j}\to0), for a monolayer, the amplitude spectral density simplifies to:

x(f)=2kBTπ2fw21−νS−2νS2YShΦ(1−2ν)(1+ν)(1−2νS)(1+νS)11−νYSY+(1−νS−2νS2)2Y(1+ν)2(1−2ν)YS(12)x(f) = \sqrt{\frac{2 k_B T}{\pi^2 f w^2}\frac{1-\nu_S-2\nu_S^2}{Y_S}h\Phi\frac{(1-2\nu)(1+\nu)}{(1-2\nu_S)(1+\nu_S)}\frac{1}{1-\nu}}\sqrt{\frac{Y_S}{Y}+\frac{(1-\nu_S-2\nu_S^2)^2Y}{(1+\nu)^2(1-2\nu)Y_S}} \tag*{(12)}

(ii) According to the approach of Fejer [21], then used in Vajente et al. [13], the amplitude spectral density of thermal noise, in the limit of equal bulk and shear loss angles, is given by:

x(f)=2kBThπ2fw2[⟨Y1−ν2Φ⟩(1+νS)2(1−2νS)2YS2+⟨(1+ν)(1−2ν)(1−ν)YΦ⟩]x(f) = \sqrt{\frac{2 k_B T h}{\pi^2 f w^2}\left[\left\langle\frac{Y}{1-\nu^2}\Phi\right\rangle\frac{(1+\nu_S)^2(1-2\nu_S)^2}{Y_S^2}+\left\langle\frac{(1+\nu)(1-2\nu)}{(1-\nu)Y}\Phi\right\rangle\right]}

where hh is the total thickness of the coating, while the angular bracket expression ⟨x⟩\langle x\rangle indicates the effective medium average of the material property xx through the multilayer stack, weighted by the physical thickness of the layers. For a monolayer, this reduces to:

x(f)=2kBTπ2fw2hΦ[Y1−ν2(1+νS)2(1−2νS)2YS2+(1+ν)(1−2ν)(1−ν)Y](13)x(f) = \sqrt{\frac{2 k_B T}{\pi^2 f w^2}h\Phi\left[\frac{Y}{1-\nu^2}\frac{(1+\nu_S)^2(1-2\nu_S)^2}{Y_S^2}+\frac{(1+\nu)(1-2\nu)}{(1-\nu)Y}\right]} \tag*{(13)}

The relative variation upon annealing of the amplitude spectral density of thermal noise in the range 1–10 kHz for sample S21088 was calculated using both Eq. (12) and Eq. (13), by adopting the following parameter sets (νS\nu_S, YSY_S) for the substrate: (0.28, 130 GPa) for Si(100), (0.17, 73.2 GPa) for fused silica, (0.29, 400 GPa) for sapphire, and by using the following parameters for the film material:

hh (nm)Φ\Phi (rad)ν\nuYY (GPa)
as-deposited7204.5⋅10−44.5 \cdot10^{-4} [a]0.22978.5
10h@500 °C7377⋅10−57 \cdot10^{-5} [a]0.22075.0
10h@900 °C7731⋅10−51 \cdot10^{-5} [b]0.17871.8

Table 1.

Additional Tables

This appendix reports additional tabulated data supporting the results discussed in the article. Table III summarizes the elastic and optical properties of sample S21089, including some of the parameters presented in Figure 5(a), Figure 5(c), and Figure 5(d), along with additional values not shown in graphical form in the main text. Table IV collects optical properties in the infrared spectral region, which are discussed in § 5 B 2 of the main text.

References

  1. [1]The LIGO Scientific Collaboration et al., Advanced LIGO, Classical and Quantum Gravity 32, 074001 (2015).
  2. [2]F. Acernese et al., Advanced Virgo: a second-generation interferometric gravitational wave detector, Classical and Quantum Gravity 32, 024001 (2015).
  3. [3]T. Akutsu et al., Overview of KAGRA: Detector design and construction history, Progress of Theoretical and Experimental Physics 2021, 05A101 (2020).arxiv.org/abs/2005.05574
  4. [4]Laboratoire des matériaux avancés; https://lma.in2p3.fr.
  5. [5]L. Pinard, C. Michel, B. Sassolas, L. Balzarini, J. Degallaix, V. Dolique, R. Flaminio, D. Forest, M. Granata, B. Lagrange, N. Straniero, J. Teillon, and G. Cagnoli, Mirrors used in the ligo interferometers for first detection of gravitational waves, Appl. Opt. 56, C11 (2017).DOI
  6. [6]M. Granata, A. Amato, G. Cagnoli, M. Coulon, J. Degallaix, D. Forest, L. Mereni, C. Michel, L. Pinard, B. Sassolas, and J. Teillon, Progress in the measurement and reduction of thermal noise in optical coatings for gravitational-wave detectors, Appl. Opt. 59, A229 (2020).DOI
  7. [7]O. Durante, M. Magnozzi, V. Fiumara, J. Neilson, M. Canepa, G. Avallone, F. Bobba, G. Carapella, F. Chiadini, R. De Salvo, R. De Simone, C. Di Giorgio, R. Fittipaldi, A. Micco, I. M. Pinto, A. Vecchione, V. Pierro, and V. Granata, Toward the optimization of SiO₂ and TiO₂-based metamaterials: Morphological, structural, and optical characterization, Optical Materials 157, 116038 (2024).DOI
  8. [8]L. Yang, M. Fazio, G. Vajente, A. Ananyeva, G. Billingsley, A. Markosyan, R. Bassiri, M. M. Fejer, and C. S. Menoni, Structural evolution that affects the room-temperature internal friction of binary oxide: Implications for ultrastable optical cavities, ACS Applied Nano Materials 3, 12308 (2020).DOI
  9. [9]M. Granata, E. Coillet, V. Martinez, V. Dolique, A. Amato, M. Canepa, J. Margueritat, C. Martinet, A. Mermet, C. Michel, L. Pinard, B. Sassolas, and G. Cagnoli, Correlated evolution of structure and mechanical loss of a sputtered silica film, Phys. Rev. Mater. 2, 053607 (2018).DOI
  10. [10]A. Amato, S. Terreni, M. Granata, C. Michel, L. Pinard, G. Gemme, M. Canepa, and G. Cagnoli, Effect of heating treatment and mixture on optical properties of coating materials used in gravitational-wave detectors, Journal of Vacuum Science & Technology B 37, 062913 (2019).DOI
  11. [11]S. Colace, S. Samandari, M. Granata, A. Amato, M. Caminale, C. Michel, G. Gemme, L. Pinard, M. Canepa, and M. Magnozzi, Monitoring the evolution of optical coatings during thermal annealing with real-time, in-situ spectroscopic ellipsometry, Classical and Quantum Gravity 41, 175016 (2024).DOI
  12. [12]A. Amato, M. Bazzan, G. Cagnoli, M. Canepa, M. Coulon, J. Degallaix, N. Demos, A. Di Michele, M. Evans, F. Fabrizi, G. Favaro, D. Forest, S. Gras, D. Hofman, A. Lemaître, G. Maggioni, M. Magnozzi, V. Martinez, L. Mereni, C. Michel, V. Milotti, M. Montani, A. Paolone, A. Pereira, F. Piergiovanni, V. Pierro, L. Pinard, I. M. Pinto, E. Placidi, S. Samandari, B. Sassolas, N. Shcheblanov, J. Teillon, I. Vickridge, and M. Granata, Development of ion-beam sputtered silicon nitride thin films for low-noise mirror coatings ofDOI
  13. [13]G. Vajente, L. Yang, A. Davenport, M. Fazio, A. Ananyeva, L. Zhang, G. Billingsley, K. Prasai, A. Markosyan, R. Bassiri, M. M. Fejer, M. Chicoine, F. m. c. Schiettekatte, and C. S. Menoni, Low mechanical loss TiO₂:GeO₂ coatings for reduced thermal noise in gravitational wave interferometers, Phys. Rev. Lett. 127, 071101 (2021).
  14. [14]G. I. McGhee, V. Spagnuolo, N. Demos, S. C. Tait, P. G. Murray, M. Chicoine, P. Dabadie, S. Gras, J. Hough, G. A. Iandolo, R. Johnston, V. Martinez, O. Patane, S. Rowan, F. m. c. Schiettekate, J. R. Smith, L. Terkowski, L. Zhang, M. Evans, I. W. Martin, and J. Steinlechner, Titania mixed with silica: A low thermal-noise coating material for gravitational-wave detectors, Phys. Rev. Lett. 131, 171401 (2023).DOI
  15. [15]M. Granata, A. Amato, L. Balzarini, M. Canepa, J. Degallaix, D. Forest, V. Dolique, L. Mereni, C. Michel, L. Pinard, B. Sassolas, J. Teillon, and G. Cagnoli, Amorphous optical coatings of present gravitational-wave interferometers*, Classical and Quantum Gravity 37, 095004 (2020).DOI
  16. [16]M. Granata, E. Saracco, N. Morgado, A. Cajgfinger, G. Cagnoli, J. Degallaix, V. Dolique, D. Forest, J. Franc, C. Michel, L. Pinard, and R. Flaminio, Mechanical loss in state-of-the-art amorphous optical coatings, Phys. Rev. D 93, 012007 (2016).DOI
  17. [17]C. Malhaire, M. Granata, D. Hofman, A. Amato, V. Martinez, G. Cagnoli, A. Lemaitre, and N. Shcheblanov, Determination of stress in thin films using micro-machined buckled membranes, Journal of Vacuum Science & Technology A 41, 043401 (2023).DOI
  18. [18]T. Hong, H. Yang, E. K. Gustafson, R. X. Adhikari, and Y. Chen, Brownian thermal noise in multilayer coated mirrors, Phys. Rev. D 87, 082001 (2013).
  19. [19]W. Yam, S. Gras, and M. Evans, Multimaterial coatings with reduced thermal noise, Phys. Rev. D 91, 042002 (2015).
  20. [20]S. C. Tait, J. Steinlechner, M. M. Kinley-Hanlon, P. G. Murray, J. Hough, G. McGhee, F. Pein, S. Rowan, R. Schnabel, C. Smith, L. Terkowski, and I. W. Martin, Demonstration of the multimaterial coating concept to reduce thermal noise in gravitational-wave detectors, Phys. Rev. Lett. 125, 011102 (2020).DOI
  21. [21]M. M. Fejer, Effective medium description of multilayer coatings, LIGO Document T2100186 (2021), https://dcc.ligo.org/LIGO-T2100186/public.
  22. [22]G. Lovelace, N. Demos, and H. Khan, Numerically modeling brownian thermal noise in amorphous and crystalline thin coatings, Classical and Quantum Gravity 35, 025017 (2017).DOI
  23. [23]G. Vignaud and A. Gibaud, REFLEX: a program for the analysis of specular X-ray and neutron reflectivity data, Journal of Applied Crystallography 52, 201 (2019).DOI
  24. [24]J. A. Woollam, B. D. Johns, C. M. Herzinger, J. N. Hilfiker, R. A. Synowicki, and C. L. Bungay, Overview of variable-angle spectroscopic ellipsometry (VASE): I. Basic theory and typical applications, in Optical Metrology: A Critical Review, Vol. 10294, edited by G. A. Al-Jumaily, International Society for Optics and Photonics (SPIE, 1999) p. 1029402.DOI
  25. [25]M. Magnozzi, S. Terreni, L. Anghinolfi, S. Uttiya, M. Carnasciali, G. Gemme, M. Neri, M. Principe, I. Pinto, L.-C. Kuo, S. Chao, and M. Canepa, Optical properties of amorphous SiO2-TiO2 multi-nanolayered coatings for 1064-nm mirror technology, Opt. Mater. 75, 94 (2018).DOI
  26. [26]A. Amato, M. Magnozzi, N. Shcheblanov, A. Lemaître, G. Cagnoli, M. Granata, C. Michel, G. Gemme, L. Pinard, and M. Canepa, Enhancing Titania-Tantala Amorphous Materials as High-Index Layers in Bragg Reflectors of Gravitational-Wave Detectors, ACS Applied Optical Materials 1, 395 (2023).DOI
  27. [27]L. Brillouin, Léon, Diffusion de la lumière et des rayons x par un corps transparent homogène - influence de l’agitation thermique, Ann. Phys. 9, 88 (1922).DOI
  28. [28]M. Merklein, I. V. Kabakova, A. Zarifi, and B. J. Eggleton, 100 years of Brillouin scattering: Historical and future perspectives, Applied Physics Reviews 9, 041306 (2022).DOI
  29. [29]S. Kojima, 100th Anniversary of Brillouin scattering: Impact on materials science, Materials 15, 3518 (2022).DOI
  30. [30]X. Zhang, R. Sooryakumar, A. G. Every, and M. H. Manghnani, Observation of organ-pipe acoustic excitations in supported thin films, Phys. Rev. B 64, 081402 (2001).DOI
  31. [31]X. Zhang, R. Sooryakumar, and K. Bussmann, Confinement and transverse standing acoustic resonances in free-standing membranes, Phys. Rev. B 68, 115430 (2003).
  32. [32]J. R. Sandercock, Structure in the Brillouin spectra of thin films, Phys. Rev. Lett. 29, 1735 (1972).
  33. [33]J. R. Sandercock, Light Scattering in Solids III: Recent Results, edited by M. Cardona and G. Güntherodt (Springer Berlin Heidelberg, Berlin, Heidelberg, 1982) pp. 173–206.
  34. [34]N. Gomopoulos, W. Cheng, M. Efremov, P. F. Nealey, and G. Fytas, Out-of-Plane Longitudinal Elastic Modulus of Supported Polymer Thin Films, Macromolecules 42, 7164 (2009).DOI
  35. [35]O. El Abouti, J. Cuffe, E. H. El Boudouti, C. M. Sotomayor Torres, E. Chavez-Angel, B. Djafari-Rouhani, and F. Alzina, Comparison of brillouin light scattering and density of states in a supported layer: Analytical and experimental study, Crystals 12, 10.3390/cryst12091212 (2022).
  36. [36]A. Passeri, A. Di Michele, I. Neri, F. Cottone, D. Fioretto, M. Mattarelli, and S. Caponi, Size and environment: The effect of phonon localization on micro-brillouin imaging, Biomaterials Advances 147, 213341 (2023).DOI
  37. [37]G. Carlotti, Elastic characterization of transparent and opaque films, multilayers and acoustic resonators by surface Brillouin scattering: A review, Applied Sciences 8, 124 (2018).DOI
  38. [38]H. Hosono, Fourier transform infrared attenuated total reflection spectra of ion-implanted silica glasses, Journal of Applied Physics 69, 8079 (1991).
  39. [39]T. de los Arcos, H. Müller, F. Wang, V. R. Damerla, C. Hoppe, C. Weinberger, M. Tiemann, and G. Grundmeier, Review of infrared spectroscopy techniques for the determination of internal structure in thin SiO2 films, Vibrational Spectroscopy 114, 103256 (2021).
  40. [40]I. Efthimiopoulos, D. Palles, S. Richter, U. Hoppe, D. Möncke, L. Wondraczek, S. Nolte, and E. I. Kamitsos, Femtosecond laser-induced transformations in ultra-low expansion glass: Microstructure and local density variations by vibrational spectroscopy, Journal of Applied Physics 123, 233105 (2018).DOI
  41. [41]S. Amma, J. Luo, C. G. Pantano, and S. H. Kim, Specular reflectance (SR) and attenuated total reflectance (ATR) infrared (IR) spectroscopy of transparent flat glass surfaces: A case study for soda lime float glass, Journal of Non-Crystalline Solids 428, 189 (2015).DOI
  42. [42]C. Z. Tan, Determination of surface structure and the depth profile of silica glass by infrared spectroscopy, Optics and Precision Engineering 13, 413 (2005).
  43. [43]R. Vacher, J. Pelous, and E. Courtens, Mean free path of high-frequency acoustic excitations in glasses with application to vitreous silica, Phys. Rev. B 56, R481 (1997).
  44. [44]G. Baldi, V. Giordano, G. Monaco, and B. Ruta, High frequency acoustic attenuation of vitreous silica: New insight from inelastic x-ray scattering, Journal of Non-Crystalline Solids 357, 538 (2011).
  45. [45]A. Paolone, E. Placidi, E. Stellino, M. G. Betti, E. Majorana, C. Mariani, A. Nucara, O. Palumbo, P. Postorino, M. Sbroscia, F. Trequattrini, M. Granata, D. Hofman, C. Michel, L. Pinard, A. Lemaitre, N. Shcheblanov, G. Cagnoli, and F. Ricci, Argon and other defects in amorphous SiO2 coatings for gravitational-wave detectors, Coatings 12, 1001 (2022).
  46. [46]T. Hirose, K. Saito, and A. J. Ikushima, Structural relaxation in sputter-deposited silica glass, Journal of Non-Crystalline Solids 352, 2198 (2006).
  47. [47]B. A. Auld, Acoustic fields and waves in solids, edited by John Wiley & Sons (Elsevier, 1973).
  48. [48]Heraeus Quarzglas GmbH & Co. KG, Fused Quartz & Fused Silica for Optical Applications, https://www.heraeus-convatics.com, accessed March 2026.
  49. [49]Crystran Ltd., Optical Materials, Fused Silica Glass, https://www.crystran.com/optical-materials/fused-silica-sio2/, accessed March 2026.
  50. [50]Corning Inc., HPFS®Fused Silica Industrial Grade: Technical data sheet, https://www.corning.com, accessed March 2026.
  51. [51]K. S. Gilroy and W. A. Phillips, An asymmetric double-well potential model for structural relaxation processes in amorphous materials, Philosophical Magazine B 43, 735 (1981).
  52. [52]E. Cesarini, M. Lorenzini, E. Campagna, F. Martelli, F. Piergiovanni, F. Vetrano, G. Losurdo, and G. Cagnoli, A ’gentle’ nodal suspension for measurements of the acoustic attenuation in materials, Review of Scientific Instruments 80, 053904 (2009).
  53. [53]T. B. Wang, Z. G. Liu, and C. Z. Tan, Relationship between the frequency of the main LO mode of silica glass and angle of incidence, The Journal of Chemical Physics 119, 505 (2003).
  54. [54]P. D. T. Huibers and D. O. Shah, Multispectral Determination of Soap Film Thickness, Langmuir 13, 5995 (1997).
  55. [55]Einstein Telescope Italy, https://www.einstein-telescope.it/en/home-en/, accessed March 2026.
  56. [56]L. Dobrzynski and A. A. Maradudin, Surface contribution to the low-temperature specific heat of a hexagonal crystal, Phys. Rev. B 14, 2200 (1976).

Paper details

vlnc:W_wv85a6h2
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 2

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…