Ultralow thermal conductivity via weak interactions in PbSe/PbTe monolayer heterostructure for thermoelectric design

Abstract

In this study, we systematically investigate the thermal and electronic transport properties of two-dimensional PbSe/PbTe monolayer heterostructure by combining first-principles calculations, Boltzmann transport theory, and machine learning methods. The heterostructure exhibits a unique honeycomb-like corrugated and asymmetric configuration, which significantly enhances phonon scattering. Moreover, the relatively weak interatomic interactions in PbSe/PbTe lead to the formation of anti-bonding states, resulting in strong anharmonicity and ultimately yielding ultralow lattice thermal conductivity (κL{κ_{\rm L}}). In the four-phonon scattering model, the κL{κ_{\rm L}}~values along the xx and yy directions are as low as 0.37 and 0.31 W/mK, respectively. Contrary to the conventional view that long mean free path acoustic phonons dominate heat transport, we find that optical phonons contribute approximately 59% of the lattice thermal conductivity in this heterostructure. These optical phonons exhibit large Grüneisen parameters, strong anharmonic scattering, and relatively high group velocities, thereby playing a crucial role in the low κL{κ_{\rm L}} regime. Further analysis of thermoelectric performance shows that at a high temperature of 800 K, the heterostructure achieves an exceptional dimensionless figure of merit (ZTZT) of 5.3 along the yy direction, indicating outstanding thermoelectric conversion efficiency. These findings not only provide theoretical insights into the transport mechanisms of PbSe/PbTe monolayer heterostructure but also offer a practical design strategy for developing high-performance two-dimensional layered thermoelectric materials.

Introduction

Driven by the record-high global temperatures and the increased industry consumption, the global energy demand in 2024 rose by 2.2%, according to Global Energy Review 2025 by the International Energy Agency. This growth rate is considerably higher than the average annual increase of 1.3% between 2013 and 2023. The emerging energy crisis has gained global attention and has intensified scientific pursuit of advanced materials capable of providing efficient and sustainable energy solutions. As the energy crisis intensifies, thermoelectric materials are receiving more attention than ever before due to their ability of converting waste heat into clean energy through the direct and reversible conversion between heat and electricity via the Seebeck and Peltier effects [1–4]. The conversion efficiency is typically evaluated using the dimensionless figure of merit:

ZT=S2σTκe+κL(1)ZT = \frac{S^2 \sigma T}{\kappa_e + \kappa_L} \tag*{(1)}

where SS is the Seebeck coefficient, σ\sigma is the electrical conductivity, TT is the absolute temperature, and κe\kappa_e and κL\kappa_L denote the electronic and lattice thermal conductivities, respectively. These parameters are inherently coupled in condensed matter systems, where the Seebeck coefficient SS typically exhibits an inverse relationship with electrical conductivity, and κe\kappa_e is directly proportional to σ\sigma. Such interdependencies pose a significant challenge to optimizing ZTZT, as improving one parameter often compromises another [6] [1, 4, 5]. Several approaches including defect engineering [7, 8, 9, 10], band structure engineering [11, 12], doping strategies [13, 14] [3], and the construction of heterostructures [15, 16] have been proposed to tune the electronic band structure or phonon transport, thereby improving thermoelectric figure of merit.

In the field of thermoelectrics, 2D materials exhibit unique advantages owing to quantum confinement effects and tunable interfacial phonon scattering. Their atomic-scale thickness can significantly suppress phonon transport while maintaining high carrier mobility [17, 18]. Lee et al. demonstrated that in conventional bulk materials, electrical conductivity (σ\sigma) and electronic thermal conductivity (κe\kappa_e) are positively correlated and difficult to decouple. However, in SnS2_2 nanosheets, reducing the thickness significantly lowers the lattice thermal conductivity (κL\kappa_L) while maintaining a moderate σ\sigma, ultimately enhancing thermoelectric efficiency [19]. This observation highlights the unique potential of 2D materials in the synergistic regulation of the power factor and the total thermal conductivity (κL+κe\kappa_L + \kappa_e). In recent years, particular attention has been drawn to two-dimensional (2D) heterostructures with van der Waals (vdW) interactions, as the inherent asymmetry within these systems can enhance the coupling between acoustic and optical phonon modes, thereby strengthening interfacial phonon scattering and resulting in a reduced κL\kappa_L. These systems are typically constructed by stacking different 2D layers vertically through weak vdW forces. Alhemaitijiang Sidis et al. employed interfacial engineering techniques to investigate black phosphorus/arsenic heterostructure devices, focusing on their thermoelectric behavior [20]. Their findings revealed a high figure of merit ZTZT of up to 3.5 at 350 K, highlighting the exceptional thermoelectric performance of such hybrid systems. In another study, Zhou et al. investigated the in-plane thermoelectric properties of vertically stacked black phosphorus (BP) and Ti2_2C, forming van der Waals heterostructures (vdWHs). Remarkably, the ZTZT value of the Ti2_2C/BP vdWHs at room temperature (300 K) exhibited a remarkable improvement by approximately 10310^3 and 10410^4 times compared to pristine Ti2_2C and BP, respectively. This dramatic enhancement is attributed to the strong interlayer coupling, which significantly boosts thermoelectric efficiency and positions these vdWHs as promising candidates for next-generation thermoelectric technologies [21]. Wu et al. also reported significant progress in this field, demonstrating a remarkable improvement in the thermoelectric performance of MoS2_2/h–BN heterostructures compared to their monolayer counterparts. In particular, the thermoelectric power factor of the MoS2_2/h–BN device exhibited an enhancement of two orders of magnitude over that of monolayer MoS2_2, validating the effectiveness of this integration strategy for energy conversion applications [22]. Additionally, research by Tang et al. demonstrated that the RbSe/SnSe heterostructure achieved a ZTZT value of 2.6 at 900 K, representing a remarkable improvement of approximately 100% and 13% over the individual RbSe (ZTZT = 1.3) and SnSe (ZTZT = 2.3) monolayers, respectively. This significant enhancement highlights the strong potential of such heterostructures for high-temperature thermoelectric applications [16].

Recently, the monolayers RbTe and RbSe with same honeycomb-like wrinkled structures have been theoretically reported to show high ZTZT values of 1.55 and 1.33 at 900 K, respectively, based on the three-phonon scattering model [23, 24]. In spite of the high thermoelectric performance of the individual monolayers, the structure and the thermoelectric properties of a heterostructure system consisting of monolayers RbTe and RbSe remain to

Methods

The first-principles calculations based on density functional theory (DFT) were performed by using the VASP code [25, 26], in which the projector augmented wave (PAW) approach were used for the accurate treatment of core valence interactions [27, 28]. The exchange-correlation interactions within the PbSe/PbTe monolayer heterostructure were treated using the Perdew-Burke-Ernzerhof (PBE) functional in the generalized gradient approximation (GGA) [29], A plane-wave kinetic energy cutoff of 500 eV was employed, and the Brillouin zone was sampled with a 12×12×112 \times12 \times1 Monkhorst–Pack k-point grid [30]. To eliminate spurious interactions between periodic images, a vacuum region of 20 Å was inserted along the out-of-plane direction. Convergence thresholds were set to 10−810^{-8} eV for total energy and 0.001 eV/Å for atomic forces. To accurately assess the electronic band structure, the Heyd–Scuseria–Ernzerhof (HSE06) hybrid functional was utilized [31]. Thermal stability of the two-dimensional PbSe/PbTe monolayer heterostructure was verified through ab initio molecular dynamics (AIMD) simulations. Using a 4×4×14 \times4 \times1 supercell, the monolayer heterostructure was simulated at 300 K and 700 K for a total duration of 10 ps with a time step of 1 fs, employing the NVT ensemble. Additionally, crystal orbital Hamilton population (COHP) analysis was carried out using the Local Orbital Basis Suite Towards Electronic-Structure Reconstruction (LOBSTER) code [32]. To account for van der Waals interactions, the VASP calculations were performed with the IVDW = 11 parameter.

MLIP (Machine Learning Interatomic Potential) family offers high precision in modeling atomic interactions and is particularly compatible with the Moment Tensor Potential (MTP) approach. MTP is based on the locality principle, where the total energy of a system with NN atoms is described as a sum over atomic neighborhood contributions:

E=EMTP=∑iV(ui).(2)E = E^{\mathrm{MTP}} = \sum_i V(u_i). \tag*{(2)}

Here, V(ui)V(u_i) represents the energy contribution from the neighborhood of atom ii. Two atoms are considered neighbors if their separation is less than a defined cutoff distance RcutR_{\mathrm{cut}}. In our case, Rcut=5R_{\mathrm{cut}} = 5 Å was used. The neighborhood uiu_i of atom ii includes the positions and types of all its neighbors [33]:

ui=({ri1,Zi,Z1},…,{rij,Zi,Zj},…,{riNneigh,Zi,ZNneigh}),(3)u_i = \left(\{r_{i1}, Z_i, Z_1\}, \ldots, \{r_{ij}, Z_i, Z_j\}, \ldots, \{r_{iN_{\mathrm{neigh}}}, Z_i, Z_{N_{\mathrm{neigh}}}\}\right), \tag*{(3)}

where rijr_{ij}, ziz_i, zjz_j, and NneighN_{\mathrm{neigh}} denote the vector between atoms, the type of the central atom, the type of neighboring atoms, and the count of neighboring atoms, respectively. For a given atomic configuration, its energy contribution is represented as [33]: V(ui)=∑αξαBα(ui)V(u_i) = \sum_\alpha\xi_\alpha B_\alpha(u_i) where BαB_\alpha are the basis functions and ξα\xi_\alpha are tunable parameters within the MLIP. A scalar quantity is then constructed by combining all possible contractions of moment tensor descriptors through these basis functions. A scalar based on basis functions constructed from all possible contractions of moment tensor descriptors is generated as follows [33]:

Mμ,ν(u)=∑j=1Nineighfμ(∣rij∣,zi,zj)(rij)⊗ν.(4)M_{\mu,\nu}(u) = \sum_{j=1}^{N_i^{\mathrm{neigh}}} f_\mu(\lvert r_{ij}\rvert,z_i,z_j)(r_{ij})^{\otimes\nu}. \tag*{(4)}

Here, the radial function fμf_\mu depends on the interatomic distance and atomic types, and is given by [33]:

fμ(∣rij∣,zi,zj)=∑βcμβ(zi,zj)ϕβ(∣rij∣)χ(Rcut−∣rij∣).(5)f_\mu(\lvert r_{ij}\rvert,z_i,z_j) = \sum_\beta c_{\mu\beta}^{(z_i,z_j)}\phi_\beta(\lvert r_{ij}\rvert)\chi(R_{\mathrm{cut}}-\lvert r_{ij}\rvert). \tag*{(5)}

In this formulation, ϕβ\phi_\beta are radial basis functions, χ\chi is a cutoff smoothing function, and cμβc_{\mu\beta} are learnable coefficients.

To construct the MLIP, a MTP framework was adopted, where model fitting was carried out by minimizing a custom-designed loss function [34, 35]:

∑k=1N[we(EkAIMD−EkMTP)+wf∑i∣fk,iAIMD−fk,iMTP∣2+ws∑i,j=13∣σk,ijAIMD−σk,ijMTP∣2]→min⁡.(6)\sum_{k=1}^{N}\left[w_e\left(E_k^{\mathrm{AIMD}}-E_k^{\mathrm{MTP}}\right)+w_f\sum_i\left|f_{k,i}^{\mathrm{AIMD}}-f_{k,i}^{\mathrm{MTP}}\right|^2+w_s\sum_{i,j=1}^{3}\left|\sigma_{k,ij}^{\mathrm{AIMD}}-\sigma_{k,ij}^{\mathrm{MTP}}\right|^2\right]\to\min. \tag*{(6)}

This objective function aims to align MTP predictions with reference data obtained from ab initio molecular dynamics (AIMD), including total energies, atomic forces, and stress tensors. Specifically, EkAIMDE_k^{\mathrm{AIMD}}, fk,iAIMD\mathbf{f}_{k,i}^{\mathrm{AIMD}}, and σk,ijAIMD\sigma_{k,ij}^{\mathrm{AIMD}} represent the AIMD-obtained values, while EkMTPE_k^{\mathrm{MTP}}, fk,iMTP\mathbf{f}_{k,i}^{\mathrm{MTP}}, and σk,ijMTP\sigma_{k,ij}^{\mathrm{MTP}} are their MTP-computed counterparts. The non-negative importance weights of energies, forces, and stresses are represented by the symbols wew_e, wfw_f, and wsw_s, which are set to 1, 0.1, and 0.001, respectively. The dataset used for training was generated from AIMD simulations of a 4×4×14 \times4 \times1 PbSe/PbTe monolayer supercell. These AIMD simulations were performed in the canonical (NVT) ensemble at four temperatures: 50, 300, 500, and 700 K, employing a timestep of 1 fs and a total duration time of 1 ps for each trajectory. Model training was subsequently executed using the MLIP software suite [35]. Phonon calculations were calculated by combining the MTP potentials with the PHONOPY code [36], which enabled computation of phonon dispersion curves and second-order harmonic interatomic force constants (IFCs). For anharmonic interactions, third-order IFCs were obtained using the THIRDORDER.PY utility in conjunction with MTP, taking into account interactions extending to the eighth-nearest neighbors within an enlarged 6×6×16 \times6 \times1 simulation cell. Furthermore, fourth-order IFCs were calculated by interfacing the MTP framework with the FOURTHORDER.PY script [37]. Based on the harmonic and higher-order IFCs, phonon Boltzmann transport equation (BTE) calculations were conducted to determine the lattice thermal conductivity. The ShengBTE and Fourphonon solvers were employed to include three-phonon and four-phonon scattering processes, respectively, utilizing dense qq-point meshes of 60×60×160 \times60 \times1 and 35×35×135 \times35 \times1 to ensure convergence [33, 38]. Supplementary Figure S1 presents the details of the qq-mesh convergence test considering only the three-phonon scattering model, while Supplementary Figure S2 shows the details of the qq-mesh convergence test considering both the three-phonon and four-phonon scattering models. The convergence criterion is set to 0.1 W/mK [39]. As for charge transport, key electronic properties, namely, the Seebeck coefficient (SS), electrical conductivity (σ\sigma), and electronic thermal conductivity (κe\kappa_e), were computed using the BoltzTraP code [40]. The carrier relaxation times were incorporated via deformation potential theory, and the fitting procedure is illustrated in Supplementary Figure 3.

Convergence behavior of lattice thermal conductivity as a function of q-point mesh

Figure S1. Convergence behavior of lattice thermal conductivity in RbSe/RbTe monolayer heterostructure under the three-phonon scattering model, evaluated with varying qq-point meshes.

Convergence behavior of lattice thermal conductivity in RbSe/RbTe monolayer heterostructure under the Four-phonon scattering model

Figure S2. Convergence behavior of lattice thermal conductivity in RbSe/RbTe monolayer heterostructure under the Four-phonon scattering model, evaluated with varying q-point meshes.

Variation of total energy with uniaxial strain for PbSe/PbTe monolayer heterostructure

Supplementary Figure 3. Variation of total energy with uniaxial strain (−1%-1\% to 1%1\%) for PbSe/PbTe monolayer heterostructure calculated using the PBE functional. The left and right panels correspond to strain applied along the (A) xx and (B) yy directions, respectively. Red and yellow lines denote the raw energy data and the fitted curves, respectively, for extracting the deformation potential constants.

Results

Crystal Structure, Chemical Bonding, and Stability

As illustrated in Figure 1A, the monolayer PbSe/PbTe\mathrm{PbSe}/\mathrm{PbTe} monolayer heterostructure exhibits a pronounced wrinkled morphology. The crystal structure consists of two Pb atomic layers sandwiched by alternately arranged Se and Te atoms, and belongs to the P3m1P3m1 (No. 156) space group. According to the structural parameters listed in Table I, the in-plane lattice constant of the heterostructure is 4.30 Å, which lies between those of monolayer PbSe\mathrm{PbSe} (4.091 Å) and PbTe\mathrm{PbTe} (4.364 Å). The atomic size mismatch between Te (atomic radius: 2.07 Å) and Se (1.90 Å) leads to noticeable asymmetry in the bond lengths and bond angles of the Pb–Te and Pb–Se bonds, resulting in local structural distortion at the heterointerface and the formation of a complex wrinkled configuration. This asymmetric wrinkled architecture not only imparts distinctive geometric characteristics to the material, but also enhances interfacial phonon scattering, effectively suppressing the lattice thermal conductivity (κL\kappa_L). To define the transport directions and standardize the simulation domain, a standard unit cell containing eight atoms, as highlighted by the red rectangle in Figure 1A, is chosen for all analyses in this work.

Supercell structure of the PbSe/PbTe monolayer heterostructure

Figure 1. Supercell structure of the PbSe/PbTe\mathrm{PbSe}/\mathrm{PbTe} monolayer heterostructure: (A) Top view and side view; (B) Electron localization function (ELF); (C) -COHP analysis.

Materiala=ba=b (Å)α=β\alpha=\beta (°)γ\gamma (°)dPb−Sed_{\mathrm{Pb-Se}} (Å)dPb−Ted_{\mathrm{Pb-Te}} (Å)θ1\theta_1 (°)θ2\theta_2 (°)HeffH_{\mathrm{eff}} (Å)
PbSe/PbTe4.300901202.8543.00697.7491.326.038

Table I. Lattice constants, lattice angles, bond lengths (dd), bond angles (θ\theta), and effective thickness (HeffH_{\mathrm{eff}}) of the PbSe/PbTe monolayer heterostructure.

Bonding characteristics play a crucial role in determining the performance of thermoelectric materials. To gain deeper insight into the bonding behavior in the PbSe/PbTe monolayer heterostructure and its impact on lattice thermal conductivity (κL\kappa_L), we further computed the electron localization function (ELF), Bader charge and crystal orbital Hamilton population (COHP) [32, 41]. The ELF values provide a measure of electron localization: ELF = 1 corresponds to perfect localization (e.g., lone pair electrons or covalent bonds), ELF = 0.5 represents a free electron gas, and ELF = 0 indicates complete delocalization. As shown in Figure 1B, the ELF values for both Pb–Se and Pb–Te bonds are relatively low, indicating a weak degree of electron localization. This suggests that the bonding nature is not purely covalent but contains weakly ionic characteristics. To further analyze the bonding characteristics, the Bader charges of the atoms were calculated. The Bader (static) charges calculated for Te, Pb, and Se atoms are −0.43 e, 0.44 e/0.63 e, and −0.64 e, respectively. These values are significantly smaller in magnitude compared to their nominal oxidation states: Te and Se typically carry a charge of −2 e, while Pb commonly exhibits 2 e or 4 e oxidation states. Specifically, the charge on Te is −0.43 e, which corresponds to approximately 21.5% of its nominal ionic charge (−2 e), indicating that about 78.5% of the expected ionic charge is not transferred. Similarly, the Bader charge on Se is −0.64 e, representing roughly 32% of the ideal ionic charge, with about 68% of the charge remaining shared or delocalized. For Pb, due to its presence at different atomic positions, the average Bader charge is 0.535 e. These values are significantly lower than the nominal 2 e or 4 e oxidation states, accounting for only about 26.8% of the ideal ionic charge. This indicates that Pb atoms retain the majority of their valence electrons, with Bader charges close to neutrality, reflecting strong electron delocalization. The partial negative charge accumulation on Te and Se, significantly less than full ionic charges, further supports the presence of substantial covalent bonding character. These observations are consistent with the ELF analysis results. Overall, the combination of partial electron transfer and relatively low ELF values suggests that the Pb–Se and Pb–Te bonds are polar covalent, characterized by partial electron sharing alongside minor ionic contributions. Furthermore, COHP projection analysis (Figure 1C) reveals significantly negative -COHP values for Pb–Se and Pb–Te bonds in the energy range of about −2 eV to −3 eV below the Fermi level, indicating the presence of dominant antibonding states. These antibonding states weaken the bond strength and lead to pronounced repulsive interactions. The reduction in bond strength and uneven distribution of bond energies disrupt lattice periodicity and phonon propagation, enhancing phonon scattering and further reducing κL\kappa_L. In summary, the Pb–Se and Pb–Te bonds in the PbSe/PbTe monolayer heterostructure are mainly polar covalent with weak ionic character. Partial charge transfer, low ELF values, and the occupation of antibonding states collectively contribute to weakened bond strength and enhanced lattice anharmonicity, which are key electronic structure origins for achieving low lattice thermal conductivity in this system.

Good stability is essential for thermoelectric materials. Firstly, the elastic constants matrix of the PbSe/PbTe monolayer heterostructure was calculated, as shown in Table II. The PbSe/PbTe monolayer heterostructure satisfies the Born-Huang criteria for mechanical stability, namely: C11>0C_{11} > 0; C66>0C_{66} > 0; C11C22−C122>0C_{11}C_{22} - C_{12}^{2} > 0. Therefore, the PbSe/PbTe monolayer is mechanically stable. Furthermore, the relationship among Young’s modulus (YY), Poisson’s ratio (ν\nu), and elastic constants is given by [42]:

MaterialC11C_{11} (GPa)C12C_{12} (GPa)C22C_{22} (GPa)C66C_{66} (GPa)Y2DY^{2D} (N/m)ν\nuΘ\Theta (K)
PbSe/PbTe9.2082.8499.2023.17461.940.30743.9

Table II. Elastic stiffness matrix (CC), 2D Young’s modulus (Y2DY^{2D}), Poisson’s ratio (ν\nu), and Debye temperature (Θ\Theta) of the PbSe/PbTe monolayer heterostructure.

Y(θ)=C11C22−C122C11sin⁡4θ+Asin⁡2θcos⁡2θ+C22cos⁡4θ(7)Y(\theta) = \frac{C_{11}C_{22} - C_{12}^{2}}{C_{11}\sin^{4}\theta+ A\sin^{2}\theta\cos^{2}\theta+ C_{22}\cos^{4}\theta} \tag*{(7)}
ν(θ)=C12sin⁡4θ−Bsin⁡2θcos⁡2θ+C12cos⁡4θC11sin⁡4θ+Asin⁡2θcos⁡2θ+C22cos⁡4θ(8)\nu(\theta) = \frac{C_{12}\sin^{4}\theta- B\sin^{2}\theta\cos^{2}\theta+ C_{12}\cos^{4}\theta}{C_{11}\sin^{4}\theta+ A\sin^{2}\theta\cos^{2}\theta+ C_{22}\cos^{4}\theta} \tag*{(8)}

where A=(C11C22−C122)/C66−2C12A = (C_{11}C_{22} - C_{12}^{2})/C_{66} - 2C_{12}, B=C11+C22−(C11C22−C122)/C66B = C_{11} + C_{22} - (C_{11}C_{22} - C_{12}^{2})/C_{66}, C66=(C11−C12)/2C_{66} = (C_{11} - C_{12})/2, and θ\theta denotes the polar angle measured from the xx-axis. Based on the polar coordinate representation shown in Figure 2B, the Young’s modulus of the PbSe/PbTe monolayer heterostructure is 61.94 N m−1^{-1}, significantly lower than common 2D materials. such as h-BN (270 N m−1\mathrm{N\,m}^{-1}) and graphene (350 ±\pm 3.15 N m−1\mathrm{N\,m}^{-1}) [43, 44]. The Poisson’s ratio of the PbSe/PbTe heterostructure is 0.307, higher than that of h-BN (0.211) and graphene (0.175) [43, 44]. This indicates that the PbSe/PbTe monolayer exhibits lower stiffness and greater flexibility compared to other common two-dimensional materials. Additionally, the Debye temperature of the PbSe/PbTe monolayer was calculated to be 43.9 K. Compared with the Debye temperatures of black phosphorus (500 K) [45] and h-MoS2_2 (600 K) [46], the lower Debye temperature of PbSe/PbTe suggests a correspondingly low lattice thermal conductivity.

Ab initio molecular dynamics results and mechanical properties of the PbSe/PbTe monolayer heterostructure

Figure 2. (A) Ab initio molecular dynamics (AIMD) results of the 4×4×14 \times4 \times1 supercell of PbSe/PbTe monolayer heterostructure at 300 K and 700 K. (B) Young’s modulus and Poisson’s ratio of the PbSe/PbTe monolayer heterostructure.

To further assess the thermal stability of the PbSe/PbTe monolayer heterostructure, ab initio molecular dynamics (AIMD) simulations were performed in the canonical (NVT) ensemble using a 4 ×\times 4 ×\times 1 supercell at 300 K and 700 K, with a total simulation time of 10 ps and a time step of 1 fs. The results are presented in Figure 2A, indicating that the total energy remained relatively constant throughout the simulations, and the supercell crystal structure exhibited no distortion or disintegration. These findings confirm the structural stability of the PbSe/PbTe monolayer heterostructure at both room temperature (300 K) and elevated temperature (700 K).

Phonon Transport Properties

Based on the machine learning MTP method, we systematically evaluated the phonon dispersion characteristics of the PbSe/PbTe monolayer heterostructure. This method achieves a favorable balance between computational accuracy and efficiency, and its effectiveness in thermoelectric materials research has been extensively validated by numerous studies. Moreover, our previous work has confirmed its applicability to similar systems [47, 48]. Furthermore, as shown in Supplementary Figure S4, the phonon dispersion curves of the PbSe/PbTe monolayer heterostructure unit cell calculated using the finite displacement method and the MTP potential exhibit excellent agreement, which fully validates the reliability of the MTP approach employed in predicting the phonon transport properties of the PbSe/PbTe monolayer heterostructure. Figure 3 shows, the phonon dispersion relations and corresponding phonon density of states (PhDOS) of the PbSe/PbTe monolayer heterostructure along the high-symmetry path Γ\Gamma-M-K-Γ\Gamma. The system comprises three acoustic phonon branches, corresponding to the out-of-plane (ZA), transverse (TA), and longitudinal (LA) vibrational modes, while the remaining nine branches represent optical modes. No imaginary frequencies appear throughout the Brillouin zone, indicating dynamical stability of the structure. Further analysis of the phonon spectrum reveals that the highest phonon frequency of the

Phonon dispersion curves and PhDOS of the PbSe/PbTe monolayer heterostructure

Figure 3. Phonon dispersion curves and PhDOS of the PbSe/PbTe monolayer heterostructure. “Opt” represent the optical phonon modes.

Phonon dispersion curves of PbSe/PbTe monolayer heterostructure

Figure S4. Phonon dispersion curves of PbSe/PbTe monolayer heterostructure calculated using the finite displacement method (red dashed lines) and the machine-learned moment tensor potential (MTP) approach (blue solid lines).

material is 4.72 THz, significantly lower than typical thermoelectric materials such as ZnSe (∼8\sim8 THz) and MoS2 (∼14\sim14 THz) [49, 50]. This low-frequency characteristic typically indicates a reduced lattice thermal conductivity (κL\kappa_{\mathrm{L}}). The acoustic branches are concentrated within the 0∼\sim1.2 THz range, whereas the optical branches mainly lie between 1.2 and 4.7 THz, exhibiting a distinct acoustic–optical phonon gap. Notably, the acoustic modes in the phonon dispersion curves show pronounced flatness, especially the ZA branch, whose dispersion is the flattest, implying an extremely low phonon group velocity. It is well known that lower phonon group velocities suppress lattice thermal conductivity. Therefore, the synergistic effects of frequency range, mode coupling, and phonon transport characteristics in the PbSe/PbTe monolayer heterostructure collectively contribute to the effective reduction of κL\kappa_{\mathrm{L}}.

A peak in the phonon density of states around 1.3 THz is observed, indicating strong acoustic–optical phonon coupling in the PbSe/PbTe monolayer heterostructure. The intense coupling between acoustic and optical modes induces strong phonon scattering, thereby reducing κL\kappa_{\mathrm{L}}. In addition, Pb atoms exhibit dominant vibrational contributions in the low-frequency acoustic region (∼\sim0 to 1.7 THz), and their contributions in the mid- to high-frequency optical region (∼\sim3.2 to 4.8 THz) are also non-negligible. This phenomenon may originate from the complex vibrational coupling induced by weak Pb–Pb bonds between the top and bottom Pb layers, which enhances both phonon–phonon and acoustic–optical phonon scattering mechanisms, further suppressing κL\kappa_{\mathrm{L}}.

Intense atomic thermal vibrations are often closely related to strong anharmonicity in the crystal structure. To further quantify the degree of anharmonicity and characterize atomic vibrations in the PbSe/PbTe monolayer heterostructure, we computed the anisotropic displacement parameters (ADP) of atoms along different crystallographic axes, as shown in Figure 4. It is clearly observed that the ADP along the cc-axis are significantly larger than those along the aa- and bb-axes, indicating more intense thermal vibrations perpendicular to the plane. Specifically, Pb atoms in the top and bottom layers exhibit relatively smaller ADP than Te atoms, which is mainly attributed to their larger atomic mass [51], whereas the higher ADP values of Te atoms can be ascribed to the weaker bonding strength with surrounding atoms. This finding is consistent with the previous conclusions from ELF and –COHP analyses, indicating weak chemical bonding interactions between Pb and Te, which allows freer atomic thermal motion and thereby enhances the structural anharmonicity.

ADP of different atoms along various directions in the PbSe/PbTe monolayer heterostructure

Figure 4. ADP of different atoms along various directions in the PbSe/PbTe monolayer heterostructure.

Overall, the pronounced atomic vibration amplitudes along the cc-axis, the local bonding strength heterogeneity, and the large ADP values in the PbSe/PbTe monolayer heterostructure collectively indicate strong anharmonicity of the system, which effectively enhances phonon scattering and consequently significantly reduces the lattice thermal conductivity (κL\kappa_{\mathrm{L}}).

From the previous analyses, it is evident that the PbSe/PbTe monolayer heterostructure exhibits considerable anharmonicity, and we therefore predict that the PbSe/PbTe monolayer heterostructure will possess a low lattice thermal conductivity (κL\kappa_{\mathrm{L}}). To more accurately evaluate the thermal transport properties of the PbSe/PbTe monolayer heterostructure, we introduced a four-phonon scattering model in addition to the three-phonon scattering processes, thereby enabling a comprehensive assessment of phonon-mediated thermal transport. Based on the phonon Boltzmann transport equation (BTE), the lattice thermal conductivity can be expressed as:

KL,k=1V∑kCkqτkqvkq2(9)K_{\mathrm{L},k} = \frac{1}{V} \sum_{k} C_{kq}\tau_{kq}v_{kq}^{2} \tag*{(9)}

Here, CkqC_{kq}, vkqv_{kq} and τkq\tau_{kq} denote the mode-specific heat capacity, phonon group velocity, and phonon relaxation time of the kk-th phonon branch, respectively. As shown in Figure 5, the temperature dependence of the lattice thermal conductivity (κL\kappa_{\mathrm{L}}) of the monolayer PbSe/PbTe monolayer heterostructure was systematically analyzed under different scattering mechanisms, where the solid lines represent results considering only three-phonon scattering processes, and the dashed lines include the four-phonon scattering mechanism as well. Overall, κL\kappa_{\mathrm{L}} gradually decreases with increasing temperature, which is primarily attributed to the enhanced phonon-phonon scattering strength at elevated temperatures. Due to the pronounced anisotropy of the heterostructure, the lattice thermal conductivity along the yy-direction remains consistently lower than that along the xx-direction, reflecting the directional dependence of its lattice dynamical properties. At 300 K, When the three- and four-phonon scattering processes are considered, the thermal conductivities of the lattice κL\kappa_{\mathrm{L}} along the xx and yy directions are as low as 0.37 W m−1 K−10.37\ \mathrm{W\,m^{-1}\,K^{-1}} and 0.31 W m−1 K−10.31\ \mathrm{W\,m^{-1}\,K^{-1}}, respectively, representing decreases of approximately 29% and 10% compared to 0.52 W m−1 K−10.52\ \mathrm{W\,m^{-1}\,K^{-1}} and 0.44 W m−1 K−10.44\ \mathrm{W\,m^{-1}\,K^{-1}} obtained with only three-phonon scattering. This significant reduction is attributed to the introduction of additional energy dissipation channels by four-phonon scattering processes, which further enhance phonon scattering intensity and effectively suppress the increase in

Temperature dependence of lattice thermal conductivity of the PbSe/PbTe monolayer heterostructure

Figure 5. Temperature dependence of lattice thermal conductivity (κL\kappa_{\mathrm{L}}) of the PbSe/PbTe monolayer heterostructure along the xx and yy directions considering three-phonon and four-phonon scattering mechanisms.

thermal conductivity. To further understand the influence of four-phonon scattering, we fitted the temperature dependence of κL\kappa_{\mathrm{L}} using a power-law relationship (κL∼T−α\kappa_{\mathrm{L}} \sim T^{-\alpha}), as shown in Figure 5. In the three-phonon-only case, the extracted exponents are αx=0.963\alpha_x = 0.963 and αy=0.956\alpha_y = 0.956, which are close to the well-established T−1T^{-1} scaling predicted by the conventional phonon gas model [52]. This agreement indicates that under three-phonon scattering, the system exhibits relatively weak anharmonicity and maintains well-defined phonon quasiparticles. However, upon including four-phonon scattering, the temperature dependence becomes noticeably stronger, with αx=1.153\alpha_x = 1.153 and αy=1.121\alpha_y = 1.121. This enhancement reflects the increased phonon-phonon scattering rates at elevated temperatures due to additional anharmonic channels. While the behavior remains consistent with a phonon-mediated transport picture, the stronger temperature sensitivity highlights the importance of higher-order anharmonic interactions. These results underscore the need to include four-phonon processes for accurate thermal conductivity predictions, especially under high-temperature conditions. Therefore, four-phonon scattering plays a crucial role in the thermal transport behavior of the material studied in this work and must be thoroughly considered when accurately evaluating the κL\kappa_{\mathrm{L}}.

To further elucidate the phonon transport mechanisms in the monolayer PbSe/PbTe monolayer heterostructure, we performed a detailed analysis of the contributions of different acoustic modes (ZA, TA, LA) and optical modes to the total lattice thermal conductivity (κL\kappa_{\mathrm{L}}). As shown in Figure 6, at 300 K, the contributions of each phonon branch to κL\kappa_{\mathrm{L}} were evaluated under both three-phonon scattering only, and the combination of three- and four-phonon scattering models. The results indicate that regardless of the phonon scattering model employed, the contribution of optical branches to the κL\kappa_{\mathrm{L}} consistently exceeds 50%. Generally, acoustic phonon modes are the primary contributors to κL\kappa_{\mathrm{L}} [53], however, it is noteworthy that in the PbSe/PbTe monolayer heterostructure, the optical modes play a dominant role. Specifically, under the four-phonon scattering model, the contribution of optical modes along the yy-direction can reach up to 58%. In the PbSe/PbTe monolayer heterostructure, however, the optical phonons play a dominant role, which can be attributed to several key factors. As shown in Figure 10A, some optical modes exhibit exceptionally high group velocities exceeding 1.5 km s−1^{-1}, even surpassing those of the ZA and TA acoustic modes. This challenges the traditional assumption that optical phonons contribute little due to low group velocity. Additionally, Figure 10B reveals that the Gruneisen parameters of optical phonons are moderate and smoothly distributed, indicating limited anharmonicity and reduced scattering strength. Despite their relatively higher scattering rates (Supplementary Figure 5), the combination of high mode density, large group velocity, and manageable anharmonicity enables optical phonons to become the principal heat carriers in this system.

Contributions of different phonon modes to lattice thermal conductivity in the PbSe/PbTe monolayer heterostructure

Figure 6. Contributions of different phonon modes (ZA, TA, LA, and Optical) to κL\kappa_L of the PbSe/PbTe\mathrm{PbSe}/\mathrm{PbTe} monolayer heterostructure, including four-phonon scattering in both the xx and yy directions. Solid-filled bars represent results obtained using the three-phonon scattering model, while hatched-filled bars denote results considering four-phonon scattering.

Phonon group velocity and Grüneisen parameter as functions of phonon frequency for PbSe/PbTe monolayer heterostructure

Figure 10. (A) Phonon group velocity (vgv_g) and (B) Grüneisen parameter (γ\gamma) as functions of phonon frequency for PbSe/PbTe monolayer heterostructure.

To verify the validity of the phonon quasiparticle picture, we plotted the total phonon scattering rates from 400 K to 800 K under the four-phonon scattering model, and included a reference red line corresponding to the breakdown threshold of the quasiparticle picture, defined as 1/τph=ωph/2π1/\tau_{\mathrm{ph}} = \omega_{\mathrm{ph}}/2\pi. When the total scattering rate exceeds this curve, the phonon lifetime is shorter than its vibrational period, and the quasiparticle description fails [54]. As shown in Supplementary Figure 5, although a few low-frequency modes exceed this threshold at higher temperatures, the majority of phonon modes remain within an acceptable range, confirming the validity of using the Boltzmann transport equation in this study. Next, to gain deeper insight into the low thermal conductivity exhibited by the PbSe/PbTe monolayer heterostructure, we further analyzed its anharmonic phonon-phonon scattering behavior. As shown in Figure 7, the frequency-dependent three-phonon and four-phonon scattering rates of the PbSe/PbTe\mathrm{PbSe}/\mathrm{PbTe} heterostructure at 300 K are presented. Overall, the anharmonic scattering rates of this material span the range from 10−210^{-2} to 10110^{1} ps−1^{-1}. Compared to some reported highly anharmonic thermoelectric materials, the scattering rates are significantly higher than those of materials with relatively low anharmonic scattering levels like GeS [55], KBaBi [56] and Na2TiSb\mathrm{Na_2TiSb} [57] (which typically exhibit rates below 1 ps−1^{-1}), indicating the pronounced anharmonicity of the PbSe/PbTe\mathrm{PbSe}/\mathrm{PbTe} heterostructure.

Frequency-dependent three-phonon and four-phonon scattering rates of PbSe/PbTe monolayer heterostructure

Figure 7. Frequency-dependent three-phonon and four-phonon scattering rates of PbSe/PbTe monolayer heterostructure.

As the frequency increases, both three-phonon and four-phonon scattering rates exhibit a gradually increasing trend, reaching peaks in certain frequency ranges before stabilizing, with two distinct scattering peaks observed near approximately 0.5 THz and 1.5 THz, respectively. Based on phonon density of states analysis, as shown in Figure 3, the scattering peak around 0.5 THz is primarily attributed to the low-frequency vibrational modes of Pb atoms, where strong coupling occurs between the lowest optical branch and acoustic branches, thereby facilitating enhanced phonon-phonon scattering processes. Although the magnitudes of three- and four-phonon scattering rates are comparable, the latter exhibits significant influence across multiple frequency ranges, indicating that four-phonon scattering is also a critical mechanism governing lattice thermal conductivity in the anharmonic thermal transport of the PbSe/PbTe monolayer heterostructure. Figure 8A illustrates the scattering channel behavior under three-phonon scattering mechanisms, distinguishing between absorption processes (λ+λ′→λ′′\lambda+ \lambda' \to\lambda'') and emission processes (λ→λ′+λ′′\lambda\to\lambda' + \lambda''). With increasing frequency, the scattering rate of the emission process significantly increases, whereas that of the absorption process exhibits a decreasing trend. This behavior indicates that the large optical phonon gap effectively suppresses the activation of absorption-type three-phonon scattering channels, thereby revealing the complexity of dynamic equilibrium in phonon interactions and energy transfer [58].

Absorption and emission processes under three-phonon scattering of PbSe/PbTe monolayer heterostructure

Figure 8. Absorption and emission processes under three-phonon scattering of PbSe/PbTe monolayer heterostructure: (A) scattering rates; (B) phase space as a function of frequency.

To further understand the frequency dependence of these scattering channels, the three-phonon scattering phase space was computed and is presented in Figure 8B, separately for absorption and emission processes. It is evident that in the low-frequency range (0 THz to 1 THz), the absorption process possesses a broad scattering phase space, while a relatively large emission phase space exists in the high-frequency range (approximately 4 THz to 4.8 THz). As shown in Figure 3, phonon density of states analysis indicates that the low-frequency region is mainly contributed by acoustic modes of Pb atoms, whereas the high-frequency region is dominated by optical vibrations primarily involving Pb and Se atoms. These results suggest that the optical branches involving Pb and Se atoms provide abundant three-phonon scattering channels at high frequencies, which enhances the density of scattering events and plays a critical role in reducing the thermal conductivity.

To gain deeper insight into four-phonon scattering mechanisms, we further investigated all possible scattering channels in the monolayer PbSe/PbTe heterostructure. As shown in Figure 9, the four-phonon scattering processes in the PbSe/PbTe monolayer heterostructure include both Umklapp and Normal types. These processes can be classified into three main scattering channels: combination (++ process, λ′+λ′′+λ′′′→λ\lambda^{\prime}+\lambda^{\prime\prime}+\lambda^{\prime\prime\prime} \to\lambda), redistribution (+− process, λ+λ′→λ′′+λ′′′\lambda+\lambda^{\prime} \to\lambda^{\prime\prime}+\lambda^{\prime\prime\prime}) and splitting (− process, λ→λ′+λ′′+λ′′′\lambda\to\lambda^{\prime}+\lambda^{\prime\prime}+\lambda^{\prime\prime\prime}), where λ\lambda represents a phonon mode. It can be observed that the Umklapp and Normal processes contribute comparably. Although normal processes do not directly resist heat flow, they influence thermal conductivity via phonon-momentum redistribution. In contrast, Umklapp processes introduce direct thermal resistance and reduce the lattice thermal conductivity. The Umklapp process clearly dominates the four-phonon scattering contribution in the PbSe/PbTe heterostructure. More importantly, among these scattering events, the redistribution process plays the most significant role. This dominant channel contributes substantially to the ultralow lattice thermal conductivity observed in the PbSe/PbTe monolayer heterostructure [59].

Calculated four-phonon scattering rates of PbSe/PbTe heterostructure monolayer as a function of phonon frequency

Figure 9. Calculated four-phonon scattering rates of PbSe/PbTe heterostructure monolayer as a function of phonon frequency, including three scattering channels: combination (++), redistribution (+−), and splitting (−−). "U" denotes Umklapp processes, while "N" refers to the normal processes.

Moreover, in the PbSe/PbTe monolayer heterostructure, the strong four-phonon scattering is intrinsically associated with the presence of an acoustic-optical phonon band gap, as shown in Figure 3. In the vicinity of the pronounced gap between the acoustic and optical branches (1.7 THz to 3.2 THz), the available phase space for three-phonon scattering processes is significantly reduced. As illustrated in Figure 8A and Figure 8B, this leads to a notable suppression of both the three-phonon phase space and the corresponding scattering rates. Specifically, absorption-type three-phonon processes are largely prohibited due to the strict energy conservation constraints imposed by the gap. In contrast, four-phonon processes particularly redistribution and splitting channels remain active near the gap region, as demonstrated in Figure 9. These higher-order interactions are less constrained by energy selection rules and are capable of bridging the phonon band gap, thereby introducing additional anharmonic scattering pathways that are forbidden in the three-phonon regime. This mechanism is further supported by Figure 7, which shows that while the contribution of four-phonon processes is generally lower than that of three-phonon processes in the low-frequency region, a noticeable increase in four-phonon scattering occurs near the gap where three-phonon scattering is substantially weakened. This results in a comparable contribution from both scattering mechanisms in the gap region. These findings highlight the dual role of the phonon band gap: it suppresses conventional three-phonon scattering while simultaneously enhancing the importance of four-phonon interactions. Therefore, the increased activity of four-phonon processes plays a critical role in reducing the lattice thermal conductivity of the PbSe/PbTe monolayer system.

We further calculated the phonon group velocity of the PbSe/PbTe monolayer heterostructure at 300 K based on the standard group velocity expression [60]:

vg=∂ωk(q)∂q(10)v_{\mathrm{g}} = \frac{\partial\omega_k(q)}{\partial q} \tag*{(10)}

where ωk(q)\omega_k(q) and qq denote the phonon frequency and wave vector of the kk-th mode, respectively. The calculated results are illustrated in Figure 10A. It is observed that the group velocity of optical modes is significantly larger than that of the acoustic modes. Among the acoustic branches, the ZA mode exhibits the lowest group velocity, which is consistent with our earlier analysis of the phonon dispersion curves. Interestingly, the group velocity of optical phonons near 0.8 THz is comparable to that of acoustic phonons. This phenomenon can be attributed to the presence of weak interatomic bonding and harmonic mixing between optical and acoustic branches. From the mode-resolved thermal conductivity contribution analysis, it is evident that the lattice thermal conductivity (κL\kappa_{\mathrm{L}}) of the PbSe/PbTe heterostructure monolayer is predominantly determined by the optical phonons. Therefore, the group velocity of optical modes plays a crucial role in shaping κL\kappa_{\mathrm{L}}. Further analysis reveals that the peak group velocity of the PbSe/PbTe monolayer heterostructure reaches only 1.64 km s−1^{-1}, which is significantly lower than that of well-known thermoelectric materials such as PbTe (∼\sim1.80 km s−1^{-1}) and As2_2Ge (∼\sim4.5 km s−1^{-1}) [24, 61]. Such a low group velocity peak is a typical indicator of low lattice thermal conductivity. The Grüneisen parameter (γ\gamma), which quantifies the degree of anharmonicity in a material, can be expressed as [58]:

γk(q)=−V0ωk(q)∂ωk(q)∂V(11)\gamma_k(q)=-\frac{V_0}{\omega_k(q)}\frac{\partial\omega_k(q)}{\partial V} \tag*{(11)}

Here, ωk\omega_k represents the phonon frequency of the kk-th mode at the equilibrium volume V0V_0.

A larger absolute value of the Grüneisen parameter ∣γ∣|\gamma| indicates stronger anharmonicity, which typically correlates with lower lattice thermal conductivity κL\kappa_L. As shown in Figure 10B, the absolute Grüneisen parameter ∣γ∣|\gamma| of the PbSe/PbTe monolayer heterostructure at 300 K exhibits relatively high values for both acoustic and optical phonon modes, with a maximum reaching up to 20. This clearly indicates a strong anharmonic phonon scattering behavior in the structure, which is consistent with the previous analyses. Moreover, materials with such pronounced anharmonicity necessitate the inclusion of four-phonon scattering mechanisms in thermal transport evaluations, as their contributions to phonon-phonon scattering and the suppression of κL\kappa_L become non-negligible.

In addition, we evaluated the specific heat capacity CvC_v, another critical parameter influencing the lattice thermal conductivity κL\kappa_L. As shown in Figure 11A, CvC_v of the PbSe/PbTe monolayer heterostructure increases gradually with temperature and eventually approaches saturation at high temperatures. Notably, the maximum value of CvC_v reaches only 1.01×1061.01 \times10^6 J m−3^{-3} K−1^{-1}, and such a low heat capacity also contributes to the ultralow κL\kappa_L observed in this system. Furthermore, we calculated the phonon mean free path (MFP) of the PbSe/PbTe heterostructure monolayer.

Calculated volumetric heat capacity and lattice thermal conductivity of the PbSe/PbTe heterostructure monolayer

Figure 11. (A) Calculated volumetric heat capacity of PbSe/PbTe heterostructure monolayer as a function of temperature; (B) lattice thermal conductivity at 300 K versus phonon mean free path.

As depicted in Figure 11B, the relationship between κL\kappa_{L} and phonon MFP is illustrated. The critical MFP corresponding to 50% of the total lattice thermal conductivity is highlighted. Typically, nanostructures exhibit phonon MFPs under 100 nm [60], however, the values of MFP along the xx and yy directions for the PbSe/PbTe monolayer heterostructure are as small as 5.41 nm and 3.39 nm, respectively. This indicates that the thermal conductivity in this system is relatively insensitive to dimensional scaling. Therefore, conventional structural engineering strategies such as nanostructuring or polycrystallization may have limited effectiveness in reducing κL\kappa_{L}.

Electronic Transport Properties

We next analyzed the electronic transport properties of the PbSe/PbTe monolayer heterostructure. Initially, the electronic band structure was calculated using the PBE functional. As shown in Table S1 of the Supporting Information, the PbSe/PbTe monolayer heterostructure exhibits a band gap of 0.77 eV, indicating its semiconducting nature. However, it is well known that the PBE functional tends to significantly underestimate band gaps. To obtain more accurate electronic band characteristics, we further performed calculations using the hybrid HSE06 functional. The resulting band structure and density of states (DOS) are presented in Figure 12. The PbSe/PbTe monolayer heterostructure exhibits an indirect band gap, with the band gap value increasing to 1.25 eV, as listed in Table S1. This increase is primarily attributed to the upward shift of the conduction band upon applying the HSE06 method.

Band structures and density of states calculated using HSE and HSE+SOC methods

Figure 12. Band structures and density of states calculated using HSE and HSE+SOC methods.

Moreover, the electronic states near the valence band maximum (VBM) are relatively flat, resulting in a large effective mass that contributes to a high Seebeck coefficient. In contrast, the sharp and highly dispersive nature of the conduction band minimum (CBM) favors high carrier mobility. These intrinsic band characteristics are beneficial for achieving excellent thermoelectric (TE) performance. The projected density of states (PDOS) analysis shows that the CBM is primarily contributed by Pb atoms, while the VBM originates mainly from Se atoms. Additionally, the sharp increase in the DOS near the Fermi level is indicative of a potentially enhanced Seebeck coefficient.

Given the heavy atomic mass of Pb in the PbSe/PbTe heterostructure monolayer, we also considered the influence of spin orbit coupling (SOC). Upon including SOC in HSE06 calculations. we observed an overall downward shift in the band structure shown in Figure 12. However, the bandgap remains at approximately 1.05 eV, showing no significant deviation from the value without SOC. Therefore, SOC effects can be reasonably neglected in subsequent calculations.

Based on the analysis of the band structure, we predict that the PbSe/PbTe monolayer heterostructure possesses promising electronic transport properties. To quantitatively evaluate this, we calculated the Seebeck coefficient (SS) and electrical conductivity (σ\sigma) of the PbSe/PbTe heterojunction in the temperature range of 300 K to 800 K using the semiclassical Boltzmann transport equation as implemented in the BoltzTraP code [40].

In addition, the rigid band approximation (RBA) was employed to simulate the effect of carrier doping on the electronic performance. The RBA assumes that the overall band structure remains unchanged upon doping, while only the position of the Fermi level shifts accordingly to represent different doping concentrations. These electronic transport properties can be expressed as [40]:

σ(T,μ)=e2∫−∞+∞dε[−∂f(T,μ,ε)∂ε]Σ(ε)(12)\sigma(T,\mu) = e^{2}\int_{-\infty}^{+\infty}d\varepsilon\left[-\frac{\partial f(T,\mu,\varepsilon)}{\partial\varepsilon}\right]\Sigma(\varepsilon) \tag*{(12)}
S(T,μ)=eTσ(T,μ)∫−∞+∞dε[−∂f(T,μ,ε)∂ε]Σ(ε)(ε−μ)(13)S(T,\mu) = \frac{e}{T\sigma(T,\mu)}\int_{-\infty}^{+\infty}d\varepsilon\left[-\frac{\partial f(T,\mu,\varepsilon)}{\partial\varepsilon}\right]\Sigma(\varepsilon)(\varepsilon-\mu) \tag*{(13)}

Here, μ\mu represents the chemical potential, ee is the elementary charge of an electron, and ff denotes the Fermi-Dirac distribution function of charge carriers. The function Σ(ε)\Sigma(\varepsilon) refers to the transport distribution function, which is defined as:

Σ(ε)=1ΩNk∑nkτnke∣vnk∣2δ(ε−εnk)(14)\Sigma(\varepsilon)=\frac{1}{\Omega N_k}\sum_{nk}\tau_{nk}^{e}\lvert v_{nk}\rvert^{2}\delta(\varepsilon-\varepsilon_{nk}) \tag*{(14)}

Here, vv represents the electron group velocity. The temperature-dependent relaxation time τ\tau is determined based on the deformation potential theory. Considering the dominant role of acoustic phonon scattering, the 2D carrier mobility μ2D\mu_{\mathrm{2D}} and the electron relaxation time τ\tau can be described by the following equations [62]:

μ2D=2eh3C2D3kBTm∗mi∗mj∗Ei2(15)\mu_{\mathrm{2D}}=\frac{2eh^{3}C^{\mathrm{2D}}}{3k_{\mathrm{B}}Tm^{*}\sqrt{m_{i}^{*}m_{j}^{*}}E_{i}^{2}} \tag*{(15)}
τ=μm∗e(16)\tau=\frac{\mu m^{*}}{e} \tag*{(16)}

Here, C2DC^{\mathrm{2D}} denotes the elastic modulus of the two-dimensional material, defined as:

C2D=[∂2E∂ρ2]/S(17)C^{\mathrm{2D}}=\left[\frac{\partial^{2}E}{\partial\rho^{2}}\right]/S \tag*{(17)}

where ρ\rho is the uniaxial strain applied along the corresponding direction, and SS is the cross-sectional area projected along the zz-axis. The effective mass m∗m^{*} along the transport direction is defined as: The effective mass m∗m^{*} along the transport direction is defined as:

m∗=ℏ2∂2ε/∂k2(18)m^{*} = \frac{\hbar^{2}}{\partial^{2}\varepsilon/\partial k^{2}} \tag*{(18)}

Here, ε\varepsilon denotes the energy of the electronic band, ℏ\hbar is the reduced Planck constant, and kk represents the electron wavevector. The deformation potential constant EE is defined as E=dEe/dρE = dE_{e}/d\rho, where EeE_{e} denotes the energy at the band edge, corresponding to the valence band maximum (VBM) and conduction band minimum (CBM). The elementary charge is denoted as ee, and the geometric mean of the effective masses along the xx- and yy-directions is given as mx∗my∗\sqrt{m_{x}^{*}m_{y}^{*}}. kBk_{B} stands for the Boltzmann constant. It should be noted that in this work, the carrier relaxation time is calculated using the deformation potential (DP) theory, which primarily considers phonon scattering while neglecting other electron scattering mechanisms, such as optical phonon and impurity scattering. While this simplification may lead to a moderate overestimation of the relaxation time, the DP method has been widely adopted in previous studies due to its computational efficiency and physical relevance, especially for two-dimensional (2D) materials. Given the high computational cost of first-principles electron-phonon coupling calculations, the DP approximation offers a practical balance between accuracy and efficiency. Moreover, numerous prior works have successfully employed the DP theory to study charge transport and thermoelectric properties in 2D systems [42, 47, 60]. Therefore despite its limitations, the DP model remains a valuable tool for the preliminary evaluation of carrier mobility and thermoelectric performance in 2D materials [63]. As summarized in Table III, a significant difference in carrier mobility is observed between electrons and holes. This trend is consistent with the band structure analysis, which indicates that the effective mass of holes is larger than that of electrons. Notably, the high electron mobility in the PbSe/PbTe heterostructure monolayer is comparable to that of MoS2. Furthermore, at 300 K, the relaxation time of electrons is noticeably longer than that of holes, leading to superior electronic transport properties under n-type doping. Both the high electron mobility and the relatively long relaxation time are beneficial for enhanced electrical transport performance.

The Seebeck coefficients (SS) of p-type and n-type PbSe/PbTe monolayer heterostructure are shown in Figure 13A and 13B. Clearly, SS increases with rising temperature, and the SS values for n-type doping are significantly lower than those for p-type doping, which is consistent with our previous analysis of the effective masses at the VBM and CBM. At 300 K, the maximum SS values for p-type (n-type) doping along the xx and yy directions reach 1358.6 μ\muV/K (1039.1 μ\muV/K) and 1353.6 μ\muV/K (1013.2 μ\muV/K), respectively.Due to the trade-off relationship between SS, the concentration-dependent behavior of σ\sigma shown in Figure 13C and 13D exhibits a contrasted trend with that of SS. Furthermore, the electrical conductivity of the p-type material is significantly lower than that of the n-type, which aligns with the analysis of carrier concentration. Additionally, σ\sigma increases gradually with temperature.The large SS leads to relatively low σ\sigma in the PbSe/PbTe heterostructure monolayer, with values around 1×1051 \times10^{5} S m−1^{-1} at optimal doping concentrations.

Seebeck coefficient and electrical conductivity versus carrier concentration

Figure 13. Seebeck coefficient (SS) versus carrier concentration of PbSe/PbTe monolayer heterostructure along xx and yy directions in the temperature range 300 K to 800 K: (A) p-type; (B) n-type. Electrical conductivity (σ\sigma) versus carrier concentration: (C) p-type; (D) n-type.

MaterialDirectionCarrier TypeC2DC^{2D} (J/m2^2)EE (eV)m∗m^{*} (m0m_0)μ2D\mu_{2D} (cm2^2/V·s)τ\tau (10−1410^{-14} s)
PbSe/PbTexxn-type34.376.6200.1221126.87.81
xxp-type34.374.1340.627118.874.23
yyn-type37.876.6160.1221243.08.61
yyp-type37.873.3120.531240.957.27

Table 3. Calculated effective masses (m∗m^{*}), 2D elastic modulus (C2DC^{2D}), deformation potential constants (EE), carrier mobilities (μ2D\mu_{2D}), and relaxation times (τ\tau) of the PbSe/PbTe monolayer heterostructure.

Next, the electronic transport performance of the PbSe/PbTe monolayer heterostructure is evaluated using the power factor. As shown in Figure 14A and 14B, the values of power factors under n-type doping are significantly higher than those under p-type doping. Moreover, the power factors along the yy-direction are evidently greater than those along the xx-direction. Specifically, under n-type doping, the power factor in the yy-direction reaches a maximum of 0.035 W m−1^{-1} K−2^{-2}, which is much higher than that of common 2D thermoelectric materials such as ZrSn2_2N4_4 (3.13 mW m−1^{-1} K−2^{-2}) [64] and PbTe (∼\sim5.861 mW m−1^{-1} K−2^{-2}) [65], indicating the superior electronic transport properties of the PbSe/PbTe heterostructure monolayer along the yy-direction.The observed asymmetry in power factor enhancement between n-type and p-type doping can be attributed to their distinct electronic structures, as previously discussed. The VBM exhibits a relatively flat dispersion, resulting in a larger effective mass for holes, which is favorable for achieving a high Seebeck coefficient. In contrast, the CBM is more dispersive and sharper, leading to a smaller effective mass for electrons and, consequently, higher carrier mobility. This fundamental difference in band curvature underlies the disparity in power factor between n-type and p-type doping.Moreover, the transport parameters listed in Table III quantitatively support this interpretation. The effective mass of n-type carriers is only 0.122m00.122m_0 in both directions, significantly lower than that of p-type carriers, which ranges from 0.531m00.531m_0 to 0.627m00.627m_0. As a result, the mobility of n-type carriers reaches 1126.8 cm2 V−1 s−11126.8\ \mathrm{cm^2\,V^{-1}\,s^{-1}} and 1243.0 cm2 V−1 s−11243.0\ \mathrm{cm^2\,V^{-1}\,s^{-1}} along the xx and yy directions, respectively—substantially exceeding the mobilities of p-type carriers (118.87 cm2 V−1 s−1118.87\ \mathrm{cm^2\,V^{-1}\,s^{-1}} and 240.95 cm2 V−1 s−1240.95\ \mathrm{cm^2\,V^{-1}\,s^{-1}}). Additionally, the relaxation time (τ\tau) of n-type carriers is generally longer, further enhancing their transport properties.Although the deformation potential

Power factor and electronic thermal conductivity versus carrier concentration for PbSe/PbTe monolayer heterostructure

Figure 14. Power factor versus carrier concentration of PbSe/PbTe monolayer heterostructure along xx and yy directions in the temperature range 300 k to 800 K: (A) p-type; (B) n-type. Electronic thermal conductivity (κe\kappa_{\mathrm{e}}) versus carrier concentration: (C) p-type; (D) n-type.

constant (EE) of n-type carriers is slightly higher, the advantages in effective mass and relaxation time compensate for this, yielding superior overall mobility. In summary, the lower effective mass, enhanced mobility, and longer relaxation time of n-type carriers collectively account for the more pronounced power factor enhancement observed under n-type doping. The electronic thermal conductivity (κe\kappa_e) is calculated according to the Wiedemann-Franz law [66]:

κe=LσT(19)\kappa_e = L\sigma T \tag*{(19)}

where LL is the Lorenz number, σ\sigma is the electrical conductivity, and TT is the temperature. As an important component of the total thermal conductivity, κe\kappa_e cannot be neglected at high carrier concentrations and may even dominate the heat transport. Figure 14C and Figure 14D show that the variation trend of κe\kappa_e with carrier concentration is consistent with that of σ\sigma, and κe\kappa_e increases with rising temperature. Additionally, the electronic thermal conductivity under n-type doping is significantly higher than that under p-type doping, which may result in lower ZTZT values for p-type materials. However, due to the overall low electrical conductivity of the PbSe/PbTe monolayer heterostructure, its electronic thermal conductivity remains relatively small, below 10 W m−1 K−110\ \mathrm{W}\,\mathrm{m}^{-1}\,\mathrm{K}^{-1}, which helps enhance the thermoelectric performance of the material.

Thermoelectric Figure of Merit

Combining its ultralow lattice thermal conductivity, moderate electronic thermal conductivity, and excellent power factor, we further evaluated the thermoelectric figure of merit ZTZT of the PbSe/PbTe monolayer heterostructure. As shown in Figure 15, the variation of ZTZT with carrier concentration at 300 K, 500 K, and 800 K is presented considering both three-phonon (solid lines) and four-phonon (dashed lines) scattering mechanisms.

Thermoelectric figure of merit of PbSe/PbTe monolayer heterostructure as a function of carrier concentration

Figure 15. Thermoelectric figure of merit (ZTZT) of PbSe/PbTe monolayer heterostructure as a function of carrier concentration along (A) xx and (B) yy directions at 300 K, 500 K, and 800 K. Solid lines represent results with only three-phonon scattering; dashed lines include four-phonon scattering.

The results reveal pronounced anisotropic thermoelectric transport behavior, with the ZTZT values under p-type doping significantly higher than those under n-type doping. This is primarily attributed to the increased electronic thermal conductivity under n-type conditions, which suppresses the enhancement of ZTZT. Moreover, the inclusion of four-phonon scattering mechanisms improves the accuracy of the calculated thermoelectric performance. At 800 K, the maximum ZTZT values along the xx and yy directions under p-type doping reach 4.1 and 5.3, respectively—an increase of approximately 23% compared to the values considering only three-phonon scattering (3.2 and 4.3). For n-type doping, the ZTZT values also increase from 2.5 (xx direction) and 2.9 (yy direction) to 3.1 and 3.7, respectively, further confirming the critical role of four-phonon scattering in accurately evaluating thermoelectric performance.

Notably, the optimal ZTZT value of the PbSe/PbTe monolayer heterostructure is 5.3, occurring at 800 K under p-type doping along the yy-direction, which is significantly higher than the corresponding values for pure monolayer PbTe (1.55) and PbSe (1.3), highlighting the effectiveness of heterostructure design in substantially enhancing thermoelectric performance. Overall, the PbSe/PbTe heterostructure monolayer exhibits outstanding thermoelectric properties at high temperatures, achieving the maximum ZTZT within the carrier concentration range of 101210^{12} cm−2^{-2} to 101310^{13} cm−2^{-2}, demonstrating good experimental feasibility and practical application potential.

Moreover, due to the weak interlayer interactions in the PbSe/PbTe monolayer vdW heterostructure, previous studies have indicated the potential for tuning its electronic structure via cross-plane compressive strain. It has been reported that such strain may modify the band structure and band alignment, thereby influencing carrier effective masses and transport properties [67, 68]. Although this work does not directly investigate the effects of cross-plane compressive strain, based on these studies, we believe this tuning mechanism holds promise for optimizing the electronic performance of PbSe/PbTe heterostructures and warrants further exploration in future research.

Conclusions

Based on first-principles calculations, Boltzmann transport theory, and a four-phonon scattering model assisted by machine-learning interatomic potentials, this work systematically investigates the crystal structural stability, thermal transport, electronic transport, and thermoelectric performance of the two-dimensional PbSe/PbTe monolayer heterostructure. The mechanical, dynamical, and thermodynamical stabilities of the heterostructure are verified through calculations of the elastic modulus, phonon dispersion relations, and ab initio molecular dynamics simulations.

The PbSe/PbTe monolayer heterostructure exhibits an excellent power factor with a peak value reaching 0.035 W m−1 K−20.035\ \mathrm{W\,m^{-1}\,K^{-2}}. In terms of thermal transport, owing to the pronounced anharmonicity of the material (Grüneisen parameter ∣γ∣=20|\gamma| = 20), relatively low phonon group velocities, and volumetric heat capacity, the lattice thermal conductivity at room temperature reduces to ultralow values of 0.37 W m−1 K−10.37\ \mathrm{W\,m^{-1}\,K^{-1}} along the xx-direction and 0.31 W m−1 K−10.31\ \mathrm{W\,m^{-1}\,K^{-1}} along the yy-direction after including four-phonon scattering, representing decreases of approximately 29% and 10%, respectively, compared to considering only three-phonon scattering.

Furthermore, unlike conventional materials where thermal conductivity is mainly dominated by acoustic phonons, optical phonons contribute more than 50% to κ\kappa in this heterostructure, indicating a unique thermal transport mechanism. Regarding thermoelectric performance, due to the combination of a large power factor and ultralow lattice thermal conductivity, the PbSe/PbTe monolayer heterostructure shows significant enhancement in the figure of merit ZTZT under p-type doping. Notably, at 800 K, the maximum ZTZT values reach approximately 4.1 and 5.3 along the xx- and yy-directions, respectively, substantially outperforming those under n-type doping (approximately 3.1 and 3.7).

In summary, this study not only reveals the outstanding thermoelectric performance and underlying microscopic mechanisms of the PbSe/PbTe monolayer heterostructure, highlighting the critical role of higher-order anharmonic scattering in regulating thermal transport, but also provides theoretical guidance and design strategies for enhancing thermoelectric performance via heterostructure engineering.

Declarations

Acknowledgments

None.

Authors’ contributions

R.T. designed this project under the supervision of K.Z. and Y.-W.F.. R.T. performed the calculations. All authors contribute to the interpretations and writing.

Availability of data and materials

The data supporting the findings can be found within the manuscript.

Conflicts of interest

All authors declared that there are no conflicts of interest.

References

Supporting Information

Convergence Test Using ShengBTE

To ensure the accuracy of lattice thermal conductivity calculations, qq-point mesh convergence tests were carried out using ShengBTE and FourPhonon for both three-phonon (Supplementary Figure S1) and four-phonon (Supplementary Figure S2) scattering models. The convergence threshold was defined as a variation of less than 0.1 W/mK.

Variation of CBM/VBM under Strain

As shown in Supplementary Figure 3, the electron and hole carrier mobilities were evaluated using the deformation potential theory, considering the strain-induced shifts in the conduction band minimum (CBM) and valence band maximum (VBM).

Discussion on the Reliability of the MTP Potential

To verify the applicability of the machine-learned interatomic potential (MLIP) used in this study, namely the Moment Tensor Potential (MTP), for the RbSe/RbTe monolayer heterostructure, we present key performance indicators and error statistics from the training process. The MTP model achieved a mean absolute error (MAE) of 0.00040 eV/atom for atomic energies, with a maximum deviation of 0.00192 eV/atom and a root mean square error (RMSE) of 0.00059 eV/atom. For atomic forces, the average error was 0.0154 eV/Å, with an RMSE of 0.0310 eV/Å. The relative error in force fluctuations is only 8.65%, well below the commonly accepted threshold of 15% for reliable atomic simulations, indicating good accuracy and predictive capability.[67]

To further validate the reliability of the MTP potential in describing the phonon transport properties of the PbSe/PbTe monolayer heterostructure, we compared the phonon dispersion curves calculated using MTP with those obtained from density functional theory (DFT). As shown in Supplementary Figure S4, the two sets of results are in excellent agreement, demonstrating that the MTP model accurately captures the lattice dynamics of the heterostructure. This confirms the robustness of MTP in predicting phonon transport properties with high fidelity.[47]

Total phonon scattering rates of each mode as a function of frequency at 300 K under the four-phonon scattering model

Figure S5. Total phonon scattering rates of each mode as a function of frequency at 300 K under the four-phonon scattering model.

Phonon Part

Frequency-dependent total scattering rates of the PbSe/PbTe monolayer heterostructure at temperatures from 400 K to 800 K

Supplementary Figure 6. Frequency-dependent total scattering rates of the PbSe/PbTe monolayer heterostructure calculated under the four-phonon scattering model in the temperature range of 400 K to 800 K. The red line represents ⟨τph−1⟩=ωph/(2π)\langle\tau_{\mathrm{ph}}^{-1} \rangle= \omega_{\mathrm{ph}}/(2\pi).

Band Gap of pbse/pbte Monolayer Heterostructure

As shown in Supplementary Table I, the electronic band structures were computed using both the PBE and HSE06 functionals to accurately determine the band gap.

MaterialBand Gap (eV)
PBEPBE+SOCHSE06HSE06+SOC
PbSe/PbTe0.770.531.251.05

Table I. Band gap values calculated using PBE, PBE+SOC, HSE06, and HSE06+SOC methods for the PbSe/PbTe monolayer heterostructure, with comparison to previously reported results.

Band structures and density of states calculated using PBE methods

Supplementary Figure 7. Band structures and density of states calculated using PBE methods.

References

  1. [6]Y. Xiao, H. Wu, J. Cui, et al., Realizing high performance n-type PbTe by synergistically optimizing effective mass and carrier mobility and suppressing bipolar thermal conductivity, Energy & Environmental Science 11, 2486 (2018).DOI
  2. [7]Y. Zheng, T. J. Slade, L. Hu, et al., Defect engineering in thermoelectric materials: what have we learned?, Chemical Society Reviews 50, 9022 (2021).DOI
  3. [8]C. Wu, X.-L. Shi, L. Wang, et al., Defect engineering advances thermoelectric materials, ACS Nano 18, 31660 (2024).DOI
  4. [9]Y. Zhang, Z. Li, S. Singh, et al., Defect-engineering-stabilized AgSbTe₂ with high thermoelectric performance, Advanced Materials 35, 2208994 (2023).DOI
  5. [10]C.-L. Fu, M. Cheng, N. T. Hung, et al., Al-driven defect engineering for advanced thermoelectric materials, Al-Driven Defect Engineering for Advanced Thermoelectric Materials (2025).
  6. [11]R. Moshwan, X.-L. Shi, W.-D. Liu, et al., Entropy engineering: an innovative strategy for designing high-performance thermoelectric materials and devices, Nano Today 58, 102475 (2024).DOI
  7. [12]H. Wu, X.-L. Shi, M. Li, et al., Sandwich engineering advances ductile thermoelectrics, Advanced Materials, 2503020 (2025).DOI
  8. [13]L. Su, D. Wang, S. Wang, et al., High thermoelectric performance realized through manipulating layered phonon-electron decoupling, Science 375, 1385 (2022).DOI
  9. [14]S.-J. Wang, M. Panhans, I. Lashkov, et al., Highly efficient modulation doping: a path toward superior organic thermoelectric devices, Science Advances 8, eabl9264 (2022).DOI
  10. [15]D. Liu, B. Qin, and L.-D. Zhao, SnSe/SnS: multifunctions beyond thermoelectricity, Materials Lab 1, 220006 (2022).
  11. [16]S. Tang, P. Ai, S. Bai, et al., Weak interatomic interactions induced low lattice thermal conductivity in 2D/2D PbSe/SnSe vdw heterostructure, Materials Today Physics 43, 101398 (2024).DOI
  12. [17]Z. Gao, G. Liu, and J. Ren, High thermoelectric performance in two-dimensional tellurium: an ab initio study, ACS Applied Materials & Interfaces 10, 40702 (2018).DOI
  13. [18]A. Patel, D. Singh, Y. Sonvane, et al., High thermoelectric performance in two-dimensional janus monolayer material WS-X (X = Se and Te), ACS Applied Materials & Interfaces 12, 46212 (2020).DOI
  14. [19]M.-J. Lee, J.-H. Ahn, J. H. Sung, et al., Thermoelectric materials by using two-dimensional materials with negative correlation between electrical and thermal conductivity, Nature Com- munications 7, 12011 (2016).
  15. [20]A. Sidike, B. Zhang, J. Dong, et al., Realization of high thermoelectric performance of black phosphorus/black arsenic hybrid heterojunction nanoscale devices by interface engineering, Physica B: Condensed Matter 673, 415357 (2024).
  16. [21]Y. Zhou and H. Wang, Enhanced in-plane thermoelectric properties achieved through the vertical van der waals stacking of black phosphorus and Ti₂C, International Journal of Heat and Mass Transfer 217, 124670 (2023).DOI
  17. [22]J. Wu, Y. Liu, Y. Liu, et al., Large enhancement of thermoelectric performance in MoS₂/h-BN heterostructure due to vacancy-induced band hybridization, Proceedings of the National Academy of Sciences 117, 13929 (2020).DOI
  18. [23]S. Tang, S. Bai, M. Wu, et al., Honeycomb-like puckered PbSe with wide bandgap as promising thermoelectric material: a first-principles prediction, Materials Today Energy 23, 100914 (2022).DOI
  19. [24]S. Tang, M. Wu, S. Bai, et al., Honeycomb-like puckered PbTe monolayer: a promising n-type thermoelectric material with ultralow lattice thermal conductivity, Journal of Alloys and Compounds 907, 164439 (2022).DOI
  20. [25]G. Kresse and J. Furthmüller, Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set, Phys. Rev. B 54, 11169 (1996).pubmed.ncbi.nlm.nih.gov/9984901
  21. [26]G. Kresse and J. Furthmüller, Efficiency of ab-initio total energy calculations for metals and semiconductors using a plane-wave basis set, Computational Materials Science 6, 15 (1996).DOI
  22. [27]P. E. Blöchl, Projector augmented-wave method, Phys. Rev. B 50, 17953 (1994).pubmed.ncbi.nlm.nih.gov/9976227
  23. [28]G. Kresse and D. Joubert, From ultrasoft pseudopotentials to the projector augmented-wave method, Phys. Rev. B 59, 1758 (1999).DOI
  24. [29]J. P. Perdew, K. Burke, and M. Ernzerhof, Generalized gradient approximation made simple, Physical Review Letters 77, 3865 (1996).pubmed.ncbi.nlm.nih.gov/10062328
  25. [30]H. J. Monkhorst and J. D. Pack, Special points for brillouin-zone integrations, Phys. Rev. B 13, 5188 (1976).DOI
  26. [31]J. Heyd, G. E. Scuseria, and M. Ernzerhof, Hybrid functionals based on a screened coulomb potential, The Journal of Chemical Physics 118, 8207 (2003).DOI
  27. [32]V. L. Deringer, A. L. Tchougréeff, and R. Dronskowski, Crystal orbital hamilton population (COHP) analysis as projected from plane-wave basis sets, Journal of Physical Chemistry A 115, 5461 (2011).DOI
  28. [33]B. Mortazavi, E. V. Podryabinkin, I. S. Novikov, et al., Accelerating first-principles estimation of thermal conductivity by machine-learning interatomic potentials: A MTP/ShengBTE solution, Computer Physics Communications 258, 107583 (2021).
  29. [34]A. V. Shapeev, Moment tensor potentials: A class of systematically improvable interatomic potentials, Multiscale Modeling & Simulation 14, 1153 (2016).DOI
  30. [35]I. S. Novikov, K. Gubaev, E. V. Podryabinkin, and A. V. Shapeev, The mlip package: moment tensor potentials with mpi and active learning, Machine Learning: Science and Technology 2, 025002 (2020).arxiv.org/abs/2007.08555
  31. [36]A. Togo and I. Tanaka, First principles phonon calculations in materials science, Scripta Materialia 108, 1 (2015).arxiv.org/abs/1506.08498
  32. [37]Z. Han, X. Yang, W. Li, T. Feng, and X. Ruan, Fourphonon: An extension module to sheng-bte for computing four-phonon scattering rates and thermal conductivity, Computer Physics Communications 270, 108179 (2022).
  33. [38]W. Li, J. Carrete, N. A. Katcho, and N. Mingo, ShengBTE: A solver of the boltzmann transport equation for phonons, Computer Physics Communications 185, 1747 (2014).DOI
  34. [39]X.-K. Chen, E.-M. Zhang, D. Wu, and K.-Q. Chen, Strain-induced medium-temperature thermoelectric performance of Cu₄TiSe₄: The role of four-phonon scattering, Physical Review Applied 19, 044052 (2023).DOI
  35. [40]G. K. H. Madsen and D. J. Singh, BoltzTraP. a code for calculating band-structure dependent quantities, Computer Physics Communications 175, 67 (2006).DOI
  36. [41]A. Savin, O. Jepsen, J. Flad, O. K. Andersen, H. Preuss, and H. G. von Schnering, Electron localization in solid-state structures of the elements: the diamond structure, Angewandte Chemie International Edition 31, 187 (1992).
  37. [42]Y. Li, J. Li, J. Tian, H. Liu, and J. Shi, A first-principles study of 2D Bi-based BiOClBr, BiOClI, and BiOBrI monolayers with ultralow lattice thermal conductivities for thermoelectric application, ACS Applied Nano Materials 7, 15086 (2024).DOI
  38. [43]A. Lajevardipour, M. Neek-Amal, and F. M. Peeters, Thermomechanical properties of graphene: valence force field model approach, Journal of Physics: Condensed Matter 24, 175303 (2012).DOI
  39. [44]P. Hess, Relationships between the elastic and fracture properties of boronitrene and molybdenum disulfide and those of graphene, Nanotechnology 28, 064002 (2017).DOI
  40. [45]A. Jain and A. J. H. McGaughey, Strongly anisotropic in-plane thermal transport in single-layer black phosphorene, Scientific Reports 5, 8501 (2015).DOI
  41. [46]M. T. Hossain and M. A. Rahman, A first principle study of the structural, electronic, and temperature-dependent thermodynamic properties of graphene/MoS₂ heterostructure, Journal of Molecular Modeling 26, 40 (2020).DOI
  42. [47]J. Lü, F. Xu, Y. Zhou, X. Mo, Y. Ouyang, and X. Tao, Four-phonon enhanced the thermoelectric properties of ScSX (X = Cl, Br, and I) monolayers, ACS Applied Materials & Interfaces 16, 24734 (2024).DOI
  43. [48]F. Xiang, R. Tan, Q. Xie, and K. Zhang, High performance photocatalytic water splitting in two-dimensional BN/Janus SnSSe heterojunctions: ab initio study, Physical Chemistry Chemical Physics 27, 7965 (2025).DOI
  44. [49]J. Ding, C. Liu, L. Xi, J. Xi, and J. Yang, Thermoelectric transport properties in chalcogenides ZnX (X=S, Se): From the role of electron-phonon couplings, Journal of Materiomics 7, 310 (2021).DOI
  45. [50]S. Chaudhuri, A. Bhattacharya, A. K. Das, et al., Understanding the role of four-phonon scattering in the lattice thermal transport of monolayer MoS₂, Physical Review B 109, 235424 (2024).arxiv.org/abs/2312.08219
  46. [51]J. Hu, J. Zhu, X. Dong, et al., Breaking the minimum limit of thermal conductivity of Mg₃Sb₂ thermoelectric mediated by chemical alloying induced lattice instability, Small 19, 2301382 (2023).DOI
  47. [52]Q.-Y. Xie, F. Xiao, K.-W. Zhang, and B.-T. Wang, Anharmonic phonon self-energy and anomalous thermal transport in the quaternary compound BaAg₂SnSe₄, Physical Review B 110, 045203 (2024).DOI
  48. [53]M. Jian, Z. Feng, Y. Xu, et al., Ultralow lattice thermal conductivity induced by anharmonic cation rattling and significant role of intrinsic point defects in TlBiS₂, Physical Review B 107, 245201 (2023).DOI
  49. [54]Y. Xiao, Y. Zhao, J. Ni, S. Meng, and Z. Dai, Phonon hardening and the effect of phonon transport in cubic antiperovskites A₃FB (A = Li, Na; B = Se, Te) induced by quartic anharmonicity, Materials Today Communications 35, 105450 (2023).DOI
  50. [55]H. Minhas, S. Das, and B. Pathak, Importance of four-phonon interactions in lattice thermal conductivity and thermoelectrics: A case study, ACS Applied Energy Materials 6, 7305 (2023).DOI
  51. [56]Z. Feng, Y. Fu, Y. Yan, Y. Zhang, and D. J. Singh, Zintl chemistry leading to ultralow thermal conductivity, semiconducting behavior, and high thermoelectric performance of hexagonal KBaBi, Physical Review B 103, 224101 (2021).DOI
  52. [57]T. Yue, Y. Zhao, J. Ni, S. Meng, and Z. Dai, Strong quartic anharmonicity, ultralow thermal conductivity, high band degeneracy and good thermoelectric performance in Na₂TlSb, npj Computational Materials 9, 17 (2023).DOI
  53. [58]S. Bai, J. Zhang, M. Wu, et al., Theoretical prediction of thermoelectric performance for layered LaAgOX (X = S, Se) materials in consideration of the four-phonon and multiple carrier scattering processes, Small Methods 7, 2201368 (2023).DOI
  54. [59]T. Feng, L. Lindsay, and X. Ruan, Four-phonon scattering significantly reduces intrinsic thermal conductivity of solids, Physical Review B 96, 161201 (2017).DOI
  55. [60]Q.-Y. Xie, J.-J. Ma, Q.-Y. Liu, et al., Low thermal conductivity and high performance anisotropic thermoelectric properties of XSe (X = Cu, Ag, Au) monolayers, Physical Chemistry Chemical Physics 24, 7303 (2022).DOI
  56. [61]Z. Gao, M. Lv, M. Liu, et al., Novel layered As₂Ge with a pentagonal structure for potential thermoelectrics, Journal of Materials Chemistry C 13, 5762 (2025).
  57. [62]R. Peng, Y. Ma, Z. He, et al., Single-layer Ag₂S: a two-dimensional bidirectional auxetic semiconductor, Nano Letters 19, 1227 (2019).DOI
  58. [63]H. Nautiyal and P. Scardi, Thermoelectric properties and thermal transport in two-dimensional GaInSe₃ and GaInTe₃ monolayers: A first-principles study, Journal of Applied Physics 135, 10.1063/5.0207618 (2024).
  59. [64]S. Feng, H. Qi, W. Hu, X. Zu, and H. Xiao, A theoretical prediction of thermoelectrical properties for novel two-dimensional monolayer ZrSn₂N₄, Journal of Materials Chemistry A 12, 13474 (2024).DOI
  60. [65]A. Pandit and B. Hamad, Thermoelectric and lattice dynamics properties of layered MX (M = Sn, Pb; X = S, Te) compounds, Applied Surface Science 538, 147911 (2021).DOI
  61. [66]N. Stojanovic, D. H. S. Maithripala, J. M. Berg, and M. Holtz, Thermal conductivity in metallic nanostructures at high temperature: electrons, phonons, and the wiedemann–franz law, ACS Applied Materials & Interfaces 16, 22715 (2024).
  62. [67]W.-X. Zhou, C.-W. Wu, H.-R. Cao, Y.-J. Zeng, G. Xie, and G. Zhang, Abnormal thermal conductivity increase in β-Ga₂O₃ by an unconventional bonding mechanism using machine-learning potential, Materials Today Physics 52, 101677 (2025).DOI
  63. [68]X.-K. Chen, J. Zhu, M. Qi, P.-Z. Jia, and Z.-X. Xie, Anomalous strain-dependent thermoelectric properties of cubic stuffed-diamond LiCu₃TiQ₄ (Q = S, Se), Physical Review Applied 23, 034085 (2025).DOI

Paper details

vlnc:W_wz9wjjhe
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy