Abstract

Silver bismuth diselenide (AgBiSe2) has much attention as an efficient thermoelectric material due to its low thermal conductivity. However, AgBiSe2 exhibits multiple crystal structural transitions with temperature, and high thermoelectric performance was realized only in high-temperature cubic phase. We previously reported the stabilization of cubic phase in AgBiSe2-2xSxTex with x = 0.6-0.8 at room temperature by high-entropy-alloy (HEA) approach. The cubic HE-type AgBiSe0.8S0.6Te0.6 achieved a high ZT value of 0.8 at 748 K. In this paper, we succeeded in stabilizing the cubic phase in AgBiSe2-2xSxTex with x = 0-0.6 by ice-quenching method, and investigated the HE effect on the thermoelectric properties. Cubic AgBiSe2-2xSxTex exhibited n-type conductivity from 300 K to 10 K. We found that electronic conductivity was largely increased around room temperature with increasing the amount of S and Te, although carrier concentration showed almost the same values. The S and Te substitutions induced the variation of band structure, resulting in the carrier mobility enhancement. Furthermore, thermal conducutivity showed reduction tendency with increasing the amount of S and Te due to enhancement of phonon scattering. Simultaneous electronic conductivity increase and thermal conductivity reduction resulted in the systematic improvement of the ZT values for HE-type cubic AgBiSe2-2xSxTex.

*Corresponding author: Aichi Yamashita

E-mail: [email protected]

Introduction

The thermoelectric generators can play an important role in a sustainable energy solution since they can directly convert heat into electricity. Thermoelectric energy conversion efficiency is defined as figure of merit ZTZT; ZT=S2T/ρκtotZT = S^{2}T/\rho\kappa_{\mathrm{tot}}, where SS is Seebeck coefficient, TT is absolute temperature, ρ\rho is electrical resistivity, and κtot\kappa_{\mathrm{tot}} is total thermal conductivity, respectively. The κtot\kappa_{\mathrm{tot}} is the summation of lattice (κlat\kappa_{\mathrm{lat}}) and electronic (κele\kappa_{\mathrm{ele}}) contributions. The term of S2/ρS^{2}/\rho, called as power factor (PF), can be maximized by carier concentration and band tuning. Therefore, high-performance thermoelectric materials require high PF and low κtot\kappa_{\mathrm{tot}}, as shown in the formula of ZTZT.[1]

Recently, silver bismuth diselenide (AgBiSe2_{2}) has attracted much interest as a high-performance thermoelectric material due to its intrinsically low κtot<1\kappa_{\mathrm{tot}} < 1 Wm−1^{-1}K−1^{-1} at room temperature.[2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13] Both n-type and p-type thermoelectric properties of AgBiSe2_{2} were reported. The difference in polarity of AgBiSe2_{2} is due to the defect of Se.[8] Nb-doped[3] and Cl-doped[4] AgBiSe2_{2} bulks achieved high ZTZT of 1 and 0.9, respectively. The remarkable characteristic of AgBiSe2_{2} is structural phase transitions with temperature, as shown in Figure 1. It crystallizes in a hexagonal P3ˉm1P\bar{3}m1 (#164) space group at room temperature, a rhombohedral R3ˉmR\bar{3}m (#166) space group around 490 K, and a cubic Fm3ˉmFm\bar{3}m (#225) space group above 590 K. However, this complicated crystal structural transition would be a drawback for module application due to the difference in crystal structure between low-temperature and high-temperature sides. This transition issue was solved by our previous work using the concept of high-entropy-alloys (HEAs).[13] HEAs are typically defined as — (a) alloys containing five or more elements with a concentration between 5 and 35%, (b) 1.5RR or more mixing entropy ΔSmix\Delta S_{\mathrm{mix}}, calculated by ΔSmix=−R∑iciln⁡ci\Delta S_{\mathrm{mix}} = -R\sum_i c_i\ln c_i, where cic_i and RR are the compositional ratio and the gas constant, respectively.[14, 15] HEAs introduce a new path of developing advanced materials with unique properties such as severe lattice-distortion effect, fatigue strength, and sluggish diffusion effect. The HEAs have been developed for “metal alloys”; on the other hand, many high-entropy-type (HE-type) compounds, for which the HEAs concept is extended, have been reported recently. For instance, new HE-type layered compounds and NaCl-type metal chalcogenides as superconductors and thermoelectric materials have been reported.[13, 16, 17, 18, 19, 20, 21, 22, 23, 24] Focused on thermoelectric materials, HE-type compounds are expected to — (a) the stabilization of solid solution phases by decreasing Gibbs free energy with an increase in the entropy, (b) the reduction of the κlat\kappa_{\mathrm{lat}} by enhancing lattice disorder.[25] Recently we have reported new HE-type AgBiSe2−2xSxTex\mathrm{AgBiSe}_{2-2x}\mathrm{S}_{x}\mathrm{Te}_{x} with ultra-low κlat\kappa_{\mathrm{lat}} and maximum ZTZT value of 0.9 without optimizing carrier concentration.26 The cubic phase was successfully stabilized at room temperature with above x=0.6x = 0.6. According to the analysis of κlat\kappa_{\mathrm{lat}} in the hexagonal phase, the point defects scattering (PDS) model estimated with the contribution of mass and strain contrast indicates the lattice disorder and/or strain by S and Te substitution fostered the phonon scattering and contributed to the decrease of κlat\kappa_{\mathrm{lat}}. However, the S and Te substitution effects on the thermoelectric properties including the mechanism of the decrease of κlat\kappa_{\mathrm{lat}} in the cubic phase could not be discussed in whole xx amount due to the appearance of the impurity phase at high temperature and incompletely stabilized cubic phase between x=0x = 0–0.50.5 at room temperature. In the present work, we successfully stabilized the cubic phase of HE-type AgBiSe2−2xSxTex\mathrm{AgBiSe}_{2-2x}\mathrm{S}_{x}\mathrm{Te}_{x} with x=0x = 0–0.60.6 by conducting the ice-quenching at the enough high temperature for single phase of cubic structure,26 and investigated the S and Te substitution effects on the thermoelectric properties below room temperature.

Temperature dependence of crystal structure change in AgBiSe2

Figure 1. Temperature dependence of crystal structure change in AgBiSe2_2.

Experimental

Polycrystalline samples of AgBiSe2−2x_{2-2x}Sx_xTex_x with x=0x = 0, 0.2, 0.4, 0.6 were prepared by melting method using elemental grains of Ag (99.99%, Kojundo Kagaku), Bi (99.999%, Kojundo Kagaku), Se (99.999%, Kojundo Kagaku), S (99.9999%, Kojundo Kagaku), and Te (99.999%, Kojundo Kagaku).

The stoichiometric ratio of grains was annealed in an evacuated quartz tube at 1,000°C for 15 h, and then the obtained powders were pelletized and heated at 500°C for 20 h. Hot-press treatment was performed in order to densify the obtained compounds using graphite dies at 500°C for 30 min under a uniaxial pressure of 60 MPa. Samples in the form of rectangular solids (typically a 1.5-mm-width, 2.5-mm-depth, 80-mm-hight) were cut from the cylinders using a diamond saw for electrical and thermal transport property measurements. The samples were placed in the evacuated quartz tube and heated at 450°C, which all samples become cubic phase, for 5 h. Then ice-quench treatment was performed to obtain the single phase of cubic structure. Relative density of all samples was beyond 90%, and there was no large difference in the relative density between the as-annealed and ice-quenched samples.

The actual composition was analyzed by energy-dispersive X-ray spectroscopy (EDX) on a TM-3030 (Hitachi Hightech) equipped with an EDX-SwiftED analyzer (Oxford). The phase purity and crystal structure were examined by powder X-ray diffraction (XRD), using Miniflex-600 (RIGAKU) with CuKα_\alpha radiation in Bragg-Brentano θ\theta-2θ\theta method with a high-resolution semiconductor detector/tex-Ultra at room temperature. The crystal structure parameters were refined using the Rietveld method using a RIETAN-FP software,[27] and crystal structures were visualized using VESTA software.[28]

Temperature dependence of electrical resistivity (ρ\rho), Seebeck coefficient (SS), and total thermal conductivity (κtot\kappa_{\mathrm{tot}}) were measured on the samples of AgBiSe2−2x_{2-2x}Sx_xTex_x with x=0x = 0, 0.2, 0.4, 0.6 from room temperature down to 10 K. The ρ\rho was measured using the four-probe method with the electrical resistivity measurement option of Magnetic Property Measurement System (MPMS3, Quantum Design). A Thermal Transport Option (TTO) of Physical Property Measurement System (PPMS, Quantum Design) was used for the κtot\kappa_{\mathrm{tot}} and the SS measurements with the two-probe method. The Hall resistivity was measured with PPMS under magnetic field up to 5 T to examine the Hall coefficient RHR_{\mathrm{H}}.

Sound velocity measurement was performed using 1077DATA (KARL DEUTSCH) for longitudinal vlongv_{\mathrm{long}} and transverse sound velocity vtransv_{\mathrm{trans}}. The Grüneisen parameter γ\gamma, Poisson ratio νP\nu_{\mathrm{P}}, and mean sound velocity vmeanv_{\mathrm{mean}} were calculated by following equations.[29]

γ=32(1+νP2−3νP)\gamma= \frac{3}{2}\left(\frac{1+\nu_{\mathrm{P}}}{2-3\nu_{\mathrm{P}}}\right)
νP=(1−2(vtransvlong)2)/(2−2(vtransvlong)2)\nu_{\mathrm{P}} = \left(1-2\left(\frac{v_{\mathrm{trans}}}{v_{\mathrm{long}}}\right)^2\right)\mathbin{/}\left(2-2\left(\frac{v_{\mathrm{trans}}}{v_{\mathrm{long}}}\right)^2\right)

The Debye temperature ΘD\Theta_{\mathrm{D}} can be written using vmeanv_{\mathrm{mean}}, Dirac’s constant ℏ\hbar, Boltzmann constant kBk_{\mathrm{B}}, and volume per atom Ω\Omega.[30, 31]

ΘD=ℏkB(6π2Ω)1/3⋅vmean\Theta_{\mathrm{D}} = \frac{\hbar}{k_{\mathrm{B}}}\left(\frac{6\pi^2}{\Omega}\right)^{1/3}\cdot v_{\mathrm{mean}}
vmean3=3vlong−3+2vtrans−3v_{\mathrm{mean}}^3 = \frac{3}{v_{\mathrm{long}}^{-3}+2v_{\mathrm{trans}}^{-3}}

Point defect scattering model for alloy phase can assess the lattice thermal conductivity κlat\kappa_{\mathrm{lat}} using following equations.[5, 6, 32, 33, 34, 35]

κlat,alloyκlat,pure=arctan⁡(u)u\frac{\kappa_{\mathrm{lat,alloy}}}{\kappa_{\mathrm{lat,pure}}} = \frac{\arctan(u)}{u}

The κlat,alloy\kappa_{\mathrm{lat,alloy}} is the lattice thermal conductivity of a disordered alloy, and the κlat,pure\kappa_{\mathrm{lat,pure}} is the lattice thermal conductivity of a pure crystal without disorder. The disorder scaling factor uu can be written using the ΘD\Theta_{\mathrm{D}}, the Ω\Omega, the vmeanv_{\mathrm{mean}}, and the scattering parameter Γ\Gamma.

u2=πΘDΩ2ℏvmeanκlat,pureΓu^2 = \frac{\pi\Theta_{\mathrm{D}}\Omega}{2\hbar v_{\mathrm{mean}}}\kappa_{\mathrm{lat,pure}}\Gamma

The Γ\Gamma is the summation of mass contribution ΓM\Gamma_{\mathrm{M}} and strain contribution ΓS\Gamma_{\mathrm{S}}.

ΓM=∑i=1nci(M‾iM‾)2∑kfik(1−MikM‾i)2(∑i=1nci)\Gamma_{\mathrm{M}} = \frac{\sum_{i=1}^{n}c_i\left(\frac{\overline{M}_i}{\overline{M}}\right)^2\sum_k f_i^k\left(1-\frac{M_i^k}{\overline{M}_i}\right)^2}{\left(\sum_{i=1}^{n}c_i\right)}
ΓS=∑i=1nciεi(M‾iM‾)2∑kfik(1−rikr‾i)2(∑i=1nci)\Gamma_{\mathrm{S}} = \frac{\sum_{i=1}^{n} c_i \varepsilon_i \left(\frac{\overline{M}_i}{\overline{M}}\right)^2 \sum_k f_i^k \left(1-\frac{r_i^k}{\overline{r}_i}\right)^2}{\left(\sum_{i=1}^{n} c_i\right)}

M‾\overline{M} is the average mass of compound, cic_i is relative degeneracies of ith sublattice M‾i\overline{M}_i and r‾i\overline{r}_i are average mass and average atomic radius of ith sublattice, fikf_i^k is fractional occupation of kth atom of the ith sublattice, MikM_i^k and rikr_i^k are mass and atomic radius of kth atom of the ith, respectively. εi\varepsilon_i is the elastic parameter and regarded as a phenomenological adjustable parameter.[35]

Results and discussion

Structural characterization

Figure 2 shows the room-temperature powder XRD patterns for AgBiSe2−2xSxTex\mathrm{AgBiSe}_{2-2x}\mathrm{S}_{x}\mathrm{Te}_{x} with x=0.0x = 0.0–0.60.6 before and after quenching. All diffraction peaks for quenched samples were indexed by the rock-salt type structure (space group: Fm3‾mFm\overline{3}m, #225) which is well known as the typical high-temperature phase of AgBiSe2\mathrm{AgBiSe}_{2}[2, 3, 4, 5, 6, 8, 9, 10, 11, 12, 13], indicating the successful stabilization of cubic phase without impurities at room temperature. The diffraction peaks for x=0.0x = 0.0–0.40.4 before quenching showed the hexagonal structure. While the diffraction peaks for x=0.6x = 0.6 before quenching was attributed to the rock-salt type structure, the peaks become sharper after quenching, indicating the crystallinity is much improved in the quenched sample. To assess the sample homogeneity, SEM imaging and EDX mapping were performed. No secondary phase was found in the SEM images (Figure S1), and also EDX mapping (Figure S2) revealed that there was no compositional inhomogeneity in all samples. An actual chemical composition, mixing entropy (ΔSmix\Delta S_{\mathrm{mix}}), lattice constant, and volume of the unit cell are summarized in Table 1. The actual chemical composition was estimated using the EDX, and the estimated values were almost same as the nominal compositions, even though tiny deficiencies of chalcogenides were found. The ΔSmix\Delta S_{\mathrm{mix}} was estimated by the following equations.[16] The value of ΔSmix\Delta S_{\mathrm{mix}} at ith crystallographically independent (CI) site is given by

X-ray diffraction patterns of quenched AgBiSe$_{2-2x}$S$_x$Te$_x$ samples

Figure 2. X-ray diffraction (XRD) patterns of quenched AgBiSe2−2x_{2-2x}Sx_xTex_x samples at room temperature. XRD patterns of before quenching samples were also plotted below those of each quenched samples as a comparison.

xxnominalactualΔSmix/R\Delta S_{\mathrm{mix}}/Raa (Å)VV (Å3^3)Δ\Delta (meV)
0.0AgBiSe2_2Ag1.02_{1.02}Bi1.04_{1.04}Se1.94_{1.94}0.6935.8269197.8462.2
0.2AgBiSe1.6_{1.6}S0.2_{0.2}Te0.2_{0.2}Ag1.04_{1.04}Bi1.02_{1.02}Se1.58_{1.58}S0.15_{0.15}Te0.21_{0.21}1.4035.8459199.7855.9
0.4AgBiSe1.2_{1.2}S0.4_{0.4}Te0.4_{0.4}Ag1.04_{1.04}Bi1.03_{1.03}Se1.17_{1.17}S0.36_{0.36}Te0.40_{0.40}1.6595.8692202.1851.3
0.6AgBiSe0.8_{0.8}S0.6_{0.6}Te0.6_{0.6}Ag1.02_{1.02}Bi1.03_{1.03}Se0.80_{0.80}S0.57_{0.57}Te0.57_{0.57}1.7645.8834203.6547.6

Table 1. Chemical composition, mixing entropy, lattice constant, volume, and activation energy of electrical resistivity for quenched AgBiSe2−2x_{2-2x}Sx_xTex_x samples.

SEM images for quenched AgBiSe$_{2-2x}$S$_x$Te$_x$ samples

Figure S1. SEM images for quenched AgBiSe2−2x_{2-2x}Sx_xTex_x samples.

EDX mapping for quenched AgBiSe2−2xSxTex samples

Figure S2. EDX mapping for quenched AgBiSe2−2x_{2-2x}Sx_xTex_x samples.

ΔSmixi=−R∑j=1Nxjln⁡xj\Delta S_{\mathrm{mix}}^{i} = -R \sum_{j=1}^{N} x_j \ln x_j

where RR, NN, and xjx_j are the gas constant, the number of the component at the ith CI site, and the atomic fraction of the component, respectively. This formula is utilized to calculate the total mixing entropy of the unit cell.

ΔSmix(total)=∑i=1nΔSmixi\Delta S_{\mathrm{mix}}(\mathrm{total}) = \sum_{i=1}^{n} \Delta S_{\mathrm{mix}}^{i}

where nn is the number of the CI sites in the unit cell. According to the value ΔSmix\Delta S_{\mathrm{mix}} in Table 1, the samples of x=0.4x = 0.4 and 0.60.6 can be considered as HE-type compounds. Rietveld refinement was performed to estimate the lattice constant and the volume of unit cell. The results of Rietveld refinement are shown in Figure S3. The lattice constant systematically increased with xx, and the behavior corresponds to the increase in average ionic radius of chalcogenide sites with equimolar ratio of S (0.184 nm, coordination number of 6) and Te (0.221 nm, coordination number of 6).

The result of Rietveld refinement for quenched AgBiSe$_{2-2x}$S$_x$Te$_x$ samples

Figure S3. The result of Rietveld refinement for quenched AgBiSe2−2x_{2-2x}Sx_xTex_x samples.

Electrical transport properties

The ρ\rho of quenched AgBiSe2−2xSxTex\mathrm{AgBiSe}_{2-2x}\mathrm{S}_{x}\mathrm{Te}_{x} samples is shown in Figure 3. The magnitude of ρ\rho at room temperature ranged from 52 to 442 mΩ\Omegacm. Systematic decrease in ρ\rho was observed with increasing xx. The temperature dependence of ρ\rho showed different behavior from both the typical semiconductors and the previously reported hexagonal structure of AgBiSe2\mathrm{AgBiSe}_{2}[3]. It can be divided into following three regimes (i–iii) similar to the (Bi,Sb)2(Te,Se)3(\mathrm{Bi}, \mathrm{Sb})_{2}(\mathrm{Te}, \mathrm{Se})_{3}[36, 37].

Temperature dependence of electrical resistivity for quenched AgBiSe$_{2-2x}$S$_x$Te$_x$ samples

Figure 3. Temperature (TT) dependence of electrical resistivity (ρ\rho) for quenched AgBiSe2−2x_{2-2x}Sx_xTex_x samples. Red, green and blue regions are activated regime, variable-range hopping (VRH) regime and saturation regime, respectively. (b) and (c) are the Arrhenius plot [log⁡10ρ\log_{10} \rho vs 1000/T1000/T] and the 3D- VRH plot [log⁡10ρ\log_{10} \rho vs 1000/T1/41000/T^{1/4}] of electrical resistivity data, respectively. Solid line and Dashed line represent linear fittings of the activation and VRH behaviors, respectively.

(i) Activated regime. In the temperature range from around 100 K to 300 K, the ρ\rho can be fitted with the Arrhenius law,

ρ∼exp⁡(Δ/kBT)\rho\sim\exp(\Delta/k_{\mathrm{B}}T)

where Δ\Delta is the activation energy, kBk_{\mathrm{B}} is the Boltzmann constant. Figure 3(b) shows the Arrhenius plot of the data with linear fittings (solid line) to estimate Δ\Delta. In Table 1, Δ\Delta has a negative correlation with xx (Figure S4), indicating that the energy gap between the conduction band and donor level probably becomes narrower because quenched AgBiSe2−2xSxTex\mathrm{AgBiSe}_{2-2x}\mathrm{S}_{x}\mathrm{Te}_{x} samples show n-type conductivity by Hall measurement.

Activation energy of electrical resistivity for quenched AgBiSe$_{2-2x}$S$_x$Te$_x$ samples

Figure S4. Activation energy (Δ\Delta) of electrical resistivity for quenched AgBiSe2−2x_{2-2x}Sx_xTex_x samples.

(ii) Variable-range hopping (VRH) regime. In the temperature range from ~80 K to ~100 K, the ρ\rho can be described by Mott’s 3D-VRH behavior,[38]

ρ∼exp⁡[(T0/T)1/4]\rho\sim\exp\left[(T_{0}/T)^{1/4}\right]

where T0T_{0} is a constant that depends on the density of state at the Fermi level EFE_{\mathrm{F}}. The linear fittings (dashed line) of VRH behavior are shown in Figure 3(c). This hopping conduction occurs due to localized states in a narrow band near the EFE_{\mathrm{F}}. The temperature range in which VRH behavior appear overlapped with the activated temperature range. The distinction between the two transport mechanisms depend on the level of disorder in the sample as discussed in the previous paper.[37]

(iii) Saturation regime. Below the VRH temperature range, the ρ\rho tended to saturate, rather than to diverge as expected for intrinsic semiconductors. This saturation behavior implies that some extended states and two or more transport channels exist at EFE_{\mathrm{F}} in the zero-temperature limit, moreover chemical potential is pinned to these states.[37] Antisites between Ag, Bi cation and S, Se, Te anion are assumed as the factor of the existing these states. In Bi2Se3\mathrm{Bi}_{2}\mathrm{Se}_{3}, the antisites create some shallow donor or acceptor levels;[39, 40, 41] hence, antisite should be the reason for this saturation behavior. To reveal the origin of this phenomenon, further information from the experiments, which can observe electronic defect states, such as scanning tunnel microscopy (STM) or current imaging tunneling spectroscopy (CITS).[39] Figure 4(a) shows the temperature dependence of Hall carrier concentration nHn_{\mathrm{H}}. The nHn_{\mathrm{H}} showed almost the same values, indicating that the ρ\rho behavior around room temperature can be described as Hall mobility contribution. In quenched AgBiSe2\mathrm{AgBiSe}_{2}, nHn_{\mathrm{H}} gradually decreases with decreasing temperature and saturates below around 75 K, indicating Hall carrier concentration is almost constant in the saturation regime. The temperature dependence of nHn_{\mathrm{H}} for other samples exhibited the same behavior, although it was not able to be measured below 50 K because of difficulty in the measurement of reliable Hall voltage. Temperature dependence of Hall mobility μH\mu_{\mathrm{H}} is shown in Figure 4(b). The μH\mu_{\mathrm{H}} of almost all samples showed a reduction tendency with decreasing temperature. In VRH conduction, its constituent states are far away from each other, and their spatial distribution can be considered uncorrelated.[38] Hence, this μH\mu_{\mathrm{H}} behavior should be the effect of hopping conduction or some transport channels. This kind of behavior was observed in Ni-doped CoSb3\mathrm{CoSb}_{3} which has VRH conduction in low temperature.[42]

Temperature dependence of Hall carrier concentration and Hall mobility for quenched AgBiSe2−2xSxTex samples

Figure 4. Temperature (TT) dependence of (a) Hall carrier concentration (nHn_{\mathrm{H}}), and (b) Hall mobility (μH\mu_{\mathrm{H}}) for quenched AgBiSe2−2x_{2-2x}Sx_xTex_x samples.

Figure 5(a) shows the temperature dependence of SS. Around room temperature, the absolute value of SS systematically decreases with increasing the amount of xx. The absolute values of SS slightly decreased when temperature is reduced to ∼200\sim200 K, and slightly increased until the range of 50–100 K.

Temperature dependence of Seebeck coefficient and Pisarenko plots

Figure 5. Temperature (TT) dependence of (a) Seebeck coefficient (SS). (b) Pisarenko plots for absolute SS (∣S∣|S|) vs Hall carrier concentration (nHn_{\mathrm{H}}) at 275 K.

Finally, they dramatically decreased and became close to zero. The temperature region of SS behavior corresponds to that of VRH or ρ\rho saturation, and it implies the localized states or pinned extended states.

This SS behavior is similar to Ni-doped CoSb3_3 behavior,[42] where the SS vanishing is explained by the effect of the impurity band from Ni. The SS behavior around room temperature corresponds to the behavior of the ρ\rho. However, nHn_H contribution is less discussed above. The Pisarenko plot at 275 K is shown in Figure 5(b). They did not follow the SPB model trend, indicating that the reason for decreasing the absolute value of SS should be band flattening or multi-band effect.[43, 44] This result indicates increasing μH\mu_H with increasing xx is due to the modification of band structure by S and Te substitutions.

Thermal transport properties

The κtot\kappa_{\mathrm{tot}}, κlat\kappa_{\mathrm{lat}}, and κele\kappa_{\mathrm{ele}} are shown in Figure 6(a), (Figure 6b), and Fig. S5, respectively. The κele\kappa_{\mathrm{ele}} is directly estimated using Wiedemann-Franz law: κele=LT/ρ\kappa_{\mathrm{ele}} = LT/\rho, where LL is Lorenz number which is expressed by L=1.5+exp⁡(−∣S∣/116)L = 1.5 + \exp(-|S|/116) (where LL is in 10−8^{-8} and SS in μ\muV/K).[45] The κlat\kappa_{\mathrm{lat}} is obtained by subtracting κele\kappa_{\mathrm{ele}} from κtot\kappa_{\mathrm{tot}}. The κtot\kappa_{\mathrm{tot}} for x=0x = 0 shows weak temperature dependence up to ∼\sim100 K, and largely decreased below ∼\sim100 K. Finally, κtot\kappa_{\mathrm{tot}} suddenly increased around 20 K. Around the room temperature and 20 K regions, measurement was not stable and they have large error bar as shown in Figure S6. The ρ\rho and SS showed unexpected behavior possibly due to some extended states near EFE_F; therefore, κtot\kappa_{\mathrm{tot}} should be also affected by the forementioned matter in the case of ∼\sim20 K region. Other samples show similar behavior and κlat\kappa_{\mathrm{lat}} almost the same, indicating that the contribution of the κtot\kappa_{\mathrm{tot}} is dominant by κlat\kappa_{\mathrm{lat}}. The κlat\kappa_{\mathrm{lat}} is expressed as 1/3CvlCv l, where CC is lattice specific heat, vv is sound velocity, and ll is the mean free path of phonons. According to the equation, increase in the CC raises the κlat\kappa_{\mathrm{lat}} until around one-third of Debye temperature, and κlat\kappa_{\mathrm{lat}} almost saturates above that temperature. In general, κlat\kappa_{\mathrm{lat}} has a peak around that temperature due to the decreasing ll which is caused by phonon-phonon Umklapp scattering.[46] However, the quenched AgBiSe2−2x_{2-2x}Sx_xTex_x samples did not show the peak possibly due to the shortening of ll against the temperature by severe phonon scattering systems.47 The κlat\kappa_{\mathrm{lat}} around room temperature almost systematically decreases with increasing xx. Here, point defect scattering (PDS) model fitting was performed to assess the magnitude of the substitution effect for κlat\kappa_{\mathrm{lat}}, and the result at 275 K is shown in Figure 6(c). This model can evaluate the κlat\kappa_{\mathrm{lat}} of the contribution of mass and strain contrast. The κlat\kappa_{\mathrm{lat}} and mean sound velocity vmeanv_{\mathrm{mean}} of the pristine sample is required for this model. The κlat\kappa_{\mathrm{lat}} of 0.90 W/mK and the vmeanv_{\mathrm{mean}} of 1636.2 ms−1^{-1}, obtained from a longitudinal sound velocity of 2888.9 ms−1^{-1} and transversal sound velocity of 1459.4 ms−1^{-1}, were utilized to perform the PDS model. The ε\varepsilon of 5 gives good fitting for the trend of quenched AgBiSe2−2x_{2-2x}Sx_xTex_x. No deviation between the mass contribution and mass and strain contribution in Figure 6(c) suggests that the mass contribution dominates in this cubic system. The ε\varepsilon of the hexagonal AgBiSe2−2x_{2-2x}Sx_xTex_x is 32.5, and it shows that the contribution fraction of mass and strain is largely different. This difference should be due to the difference in anharmonicity. The Grü̈neisen parameter of the hexagonal AgBiSe2_2 was estimated as 1.68[13], while that of the cubic AgBiSe2_2 was 1.97, indicating the high anharmonicity nature of the cubic structure of AgBiSe2_2 system. Moreover, the atomic bond length of the cubic phase is more fluctuated than that of the hexagonal phase for AgBiSe2_2.[7] Hence, the pristine cubic sample already has a large strain indicating that the contribution of substitution of S and Te for strain should be small.

Temperature dependence of thermal conductivity and PDS model fitting

Figure 6. Temperature dependence of (a) total thermal conductivity (κtot\kappa_{\mathrm{tot}}) and (b) lattice thermal conductivity (κlat\kappa_{\mathrm{lat}}) for quenched AgBiSe2−2x_{2-2x}Sx_xTex_x samples. (c) PDS model fitting to κlat\kappa_{\mathrm{lat}} (color plots) at 275 K. The Dashed line shows mass contribution, and the solid line shows mass and strain contributions.

Temperature dependence of total thermal conductivity with error bars for quenched AgBiSe$_{2-2x}$S$_x$Te$_x$ samples

Figure S6. Temperature dependence (TT) of total thermal conductivity (κtot\kappa_{\mathrm{tot}}) with error bar for quenched AgBiSe2−2x_{2-2x}Sx_xTex_x samples.

The power factor PF of quenched AgBiSe2−2x_{2-2x}Sx_xTex_x is shown in Figure 7(a). The PF for x=0x = 0 was 0.54 μWcm−1^{-1}K−2^{-2} at room temperature and decreased with the temperature. The maximum PF among the obtained samples were 1.27 μWcm−1^{-1}K−2^{-2} for x=0.6x = 0.6 at room temperature. Although PF for x=0.4x = 0.4 and 0.6 showed almost the same values of PF, it tended to increase with increase in the xx amount.

Temperature dependence of PF and ZT for quenched AgBiSe$_{2-2x}$S$_x$Te$_x$ samples

Figure 7. Temperature dependence of (a) PF and (b) ZTZT of quenched AgBiSe2−2x_{2-2x}Sx_xTex_x samples.

Figure 7(b) shows the ZTZT of quenched AgBiSe2−2x_{2-2x}Sx_xTex_x. The ZTZT values systematically increased with xx amount, indicating that the simultaneous substitution of Se site by S and Te improved the ZTZT values due to the improvement of both electrical and thermal properties. The maximum ZTZT reached 0.05 with x=0.6x = 0.6 at room temperature.

Conclusion

In summary, we successfully stabilize the high-temperature cubic phase in AgBiSe2−2x_{2-2x}Sx_xTex_x with x=0x = 0–0.6 at room temperature by ice-quench technique and investigated the HE effects on the thermoelectric properties of the cubic phase. Around room temperature, systematic change of electrical transport properties was observed and it was discussed using SPB model. In consequence, it was explained by the variation of band structure. In lower temperature regions, the ρ\rho showed 3D-VRH and saturated behavior possibly due to some localized states or extended states near EFE_{\mathrm{F}}. Moreover, the vanishment of SS around 50 K also could be caused by the same mechanism. The existence of some transport channels is consistent with the result of the Pisarenko plot, suggesting that the simultaneous substitution of S and Te for Se site should affect band structure. The temperature dependence of κlat\kappa_{\mathrm{lat}} without a peak around 50 K indicates the shortening of ll for AgBiSe2−2x_{2-2x}Sx_xTex_x, possibly due to the severe phonon scattering. Finally, the ZTZT value of 0.05 was achieved for the x=0.6x = 0.6 sample at room temperature. Our work offered an approach to investigate the thermoelectric properties of cubic structure of AgBiSe2−2x_{2-2x}Sx_xTex_x and we succeeded in enhancing the thermoelectric properties around room temperature.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

The authors thank Hiroto Arima for his supports in experiments. This work was partially performed with Collaborative Research Project of Laboratory for Materials and Structures, Institute of Innovative Research, Tokyo Institute of Technology. A. Y. was partly supported by a Grant-in-Aid for Scientific Research (KAKENHI) (No. 22K14480), and the Asahi Glass Foundation. Y. M. was partly supported by a Grant-in-Aid for Scientific Research (KAKENHI) (No. 21H00151), JST-ERATO (No. JPMJER2201), and the Tokyo Metropolitan Government Advanced Research (No. H31-1).

Figure

Supporting Information

Temperature dependence of electronic thermal conductivity for quenched AgBiSe$_{2-2x}$S$_x$Te$_x$ samples

Figure S5. Temperature (TT) dependence of electronic thermal conductivity (κele\kappa_{\mathrm{ele}}) for quenched AgBiSe2−2x_{2-2x}Sx_xTex_x samples.

References

  1. [1]1 G. J. Snyder and E. S. Toberer, Nat. Mater., 2008, 7, 105–114.
  2. [2]C. Xiao, X. Qin, J. Zhang, R. An, J. Xu, K. Li, B. Cao, J. Yang, B. Ye and Y. Xie, J. Am. Chem. Soc., 2012, 134, 18460–18466.
  3. [3]L. Pan, D. Bérardan and N. Dragoë, J. Am. Chem. Soc., 2013, 135, 4914–4917.
  4. [4]S. N. Guin, V. Srihari and K. Biswas, J. Mater. Chem. A, 2014, 3, 648–655.
  5. [5]F. Böcher, S. P. Culver, J. Peilstöcker, K. S. Weldert and W. G. Zeier, Dalton Trans., 2017, 46, 3906–3914.
  6. [6]Y. Goto, A. Nishida, H. Nishiate, M. Murata, C. H. Lee, A. Miura, C. Moriyoshi, Y. Kuroiwa and Y. Mizuguchi, Dalton Trans., 2018, 47, 2575–2580.
  7. [7]T. Bernges, J. Peilstöcker, M. Dutta, S. Ohno, S. P. Culver, K. Biswas and W. G. Zeier, Inorg. Chem., 2019, 58, 9236–9245.
  8. [8]S. Li, Z. Feng, Z. Tang, F. Zhang, F. Cao, X. Liu, D. J. Singh, J. Mao, Z. Ren and Q. Zhang, Chem. Mater., 2020, 32, 3528–3536.
  9. [9]T. Zhao, H. Zhu, B. Zhang, S. Zheng, N. Li, G. Wang, G. Wang, X. Lu and X. Zhou, Acta Mater., 2021, 220, 117291.
  10. [10]H. Zhu, T. Zhao, B. Zhang, Z. An, S. Mao, G. Wang, X. Han, X. Lu, J. Zhang and X. Zhou, Adv. Energy Mater., 2021, 11, 2003304.
  11. [11]Z. Guo, Y.-K. Zhu, M. Liu, X. Dong, B. Sun, F. Guo, Q. Zhang, J. Li, W. Gao, Y. Fu, W. Cai, J. Sui and Z. Liu, Mater. Today Phys., 2023, 38, 101238.
  12. [12]L. Zhang, W. Shen, Z. Zhang, C. Fang, Q. Wang, B. Wan, L. Chen, Y. Zhang and X. Jia, J. Materiomics, 2024, 10, 70–77.
  13. [13]A. Seshita, A. Yamashita, T. Fujita, T. Katase, A. Miura, Y. Nakahira, C. Moriyoshi, Y. Kuroiwa and Y. Mizuguchi, 2024.
  14. [14]J.-W. Yeh, S.-K. Chen, S.-J. Lin, J.-Y. Gan, T.-S. Chin, T.-T. Shun, C.-H. Tsau and S.-Y. Chang, Adv. Eng. Mater., 2004, 6, 299–303.
  15. [15]J.-W. Yeh, JOM, 2013, 65, 1759–1771.
  16. [16]A. Yamashita, Y. Goto, A. Miura, C. Moriyoshi, Y. Kuroiwa and Y. Mizuguchi, Mater. Res. Lett., 2021, 9, 366–372.
  17. [17]R. Sogabe, Y. Goto and Y. Mizuguchi, Appl. Phys. Express, 2018, 11, 053102.
  18. [18]R. Sogabe, Y. Goto, T. Abe, C. Moriyoshi, Y. Kuroiwa, A. Miura, K. Tadanaga and Y. Mizuguchi, Solid State Commun., 2019, 295, 43–49.
  19. [19]Y. Mizuguchi, J. Phys. Soc. Jpn., 2019, 88, 124708.
  20. [20]M. R. Kasem, K. Hoshi, R. Jha, M. Katsuno, A. Yamashita, Y. Goto, T. D. Matsuda, Y. Aoki and Y. Mizuguchi, Appl. Phys. Express, 2020, 13, 033001.
  21. [21]Y. Shukunami, A. Yamashita, Y. Goto and Y. Mizuguchi, Phys. C Supercond. Its Appl., 2020, 572, 1353623.
  22. [22]A. Yamashita, R. Jha, Y. Goto, T. D. Matsuda, Y. Aoki and Y. Mizuguchi, Dalton Trans., 2020, 49, 9118–9122.
  23. [23]Y. Mizuguchi, Md. R. Kasem and T. D. Matsuda, Mater. Res. Lett., 2021, 9, 141–147.
  24. [24]Md. R. Kasem, A. Yamashita, Y. Goto, T. D. Matsuda and Y. Mizuguchi, J. Mater. Sci., 2021, 56, 9499–9505.
  25. [25]B. Jiang, Y. Yu, J. Cui, X. Liu, L. Xie, J. Liao, Q. Zhang, Y. Huang, S. Ning, B. Jia, B. Zhu, S. Bai, L. Chen, S. J. Pennycook and J. He, Science, 2021, 371, 830–834.
  26. [27]K. Momma and F. Izumi, J. Appl. Crystallogr., 2011, 44, 1272–1276.
  27. [28]D. S. Sanditov and V. N. Belomestnykh, Tech. Phys., 2011, 56, 1619–1623.
  28. [29]O. L. Anderson, J. Phys. Chem. Solids, 1963, 24, 909–917.
  29. [30]A. Zevalkink, E. S. Toberer, W. G. Zeier, E. Flage-Larsen and G. J. Snyder, Energy Environ. Sci., 2011, 4, 510–518.
  30. [31]J. Yang, G. P. Meisner and L. Chen, Appl. Phys. Lett., 2004, 85, 1140–1142.
  31. [32]P. G. Klemens, Proc. Phys. Soc. Sect. A, 1955, 68, 1113.
  32. [33]J. Callaway and H. C. von Baeyer, Phys. Rev., 1960, 120, 1149–1154.
  33. [34]B. Abeles, Phys. Rev., 1963, 131, 1906–1911.
  34. [35]Z. Ren, A. A. Taskin, S. Sasaki, K. Segawa and Y. Ando, Phys. Rev. B, 2010, 82, 241306.
  35. [36]Z. Ren, A. A. Taskin, S. Sasaki, K. Segawa and Y. Ando, Phys. Rev. B, 2011, 84, 165311.
  36. [37]B. I. Shklovskii and A. L. Efros, Springer Berlin Heidelberg, Berlin, Heidelberg, 1984, vol. 45.
  37. [38]S. Urazhdin, D. Bilc, S. H. Tessmer, S. D. Mahanti, T. Kyratsi and M. G. Kanatzidis, Phys. Rev. B, 2002, 66, 161306.
  38. [39]G. Wang, X.-G. Zhu, Y.-Y. Sun, Y.-Y. Li, T. Zhang, J. Wen, X. Chen, K. He, L.-L. Wang, X.-C. Ma, J.-F. Jia, S. B. Zhang and Q.-K. Xue, Adv. Mater., 2011, 23, 2929–2932.
  39. [40]M. Lee, S. W. Cho, Y. Yi and S. Lee, J. Alloys Compd., 2019, 800, 81–87.
  40. [41]J. S. Dyck, W. Chen, J. Yang, G. P. Meisner and C. Uher, Phys. Rev. B, 2002, 65, 115204.
  41. [42]A. F. May and G. J. Snyder, 2012, 1–18.
  42. [43]Y. Luo, S. Hao, S. Cai, T. J. Slade, Z. Z. Luo, V. P. David, C. Wolverton, Q. Yan and M. G. Kanatzidis, J. Am. Chem. Soc., 2020, 142, 15187–15198.
  43. [44]H.-S. Kim, Z. M. Gibbs, Y. Tang, H. Wang and G. J. Snyder, APL Mater., 2015, 3, 041506.
  44. [45]A. Yamashita, K. Kihou, H. Kunioka, H. Nishiate, A. Yamamoto, Y. Goto, Y. Mizuguchi, T. Iida, Y. Takano and C.-H. Lee, J. Solid State Chem., 2020, 291, 121588.
  45. [46]J. Zhang, X. Y. Qin, H. X. Xin, D. Li and C. J. Song, J. Electron. Mater., 2011, 40, 980–986.

Paper details

vlnc:W_x2t7a66a
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents