betaFeedback

WorksPhysics and Astronomy

Efficient photoreforming of plastic waste using a high-entropy oxide catalyst

Abstract

Simultaneous catalytic hydrogen (H2) production and plastic waste degradation under light, known as photoreforming, is a novel approach to green fuel production and efficient waste management. Here, we use a high-entropy oxide (HEO), a new family of catalysts with five or more principal cations in their structure, for plastic degradation and simultaneous H2 production. The HEO shows higher activity than that of P25 TiO2, a benchmark photocatalyst, for the degradation of polyethylene terephthalate (PET) plastics in water. Several valuable products are produced by photoreforming of PET bottles and microplastics including H2, terephthalate, ethylene glycol and formic acid. The high activity is attributed to the diverse existence of several cations in the HEO lattice, lattice defects, and appropriate charge carrier lifetime. These findings suggest that HEOs possess high potential as new catalysts for concurrent plastic waste conversion and clean H2 production.

*Corresponding author (E-mail: [email protected]; Tel: +80-92-802-6744)

Introduction

Plastics have become an indispensable part of modern society for a vast range of applications including the food industry, agriculture, and medical systems [1]. The widespread use of plastics is due to numerous advantages such as low density, versatility, and resistance to corrosion and fracture. However, a significant environmental challenge arises from plastic waste, with over 80% of plastic packages ending up in landfills or polluting the environment [2]. In addition to environmental problems, they can also cause a huge loss of valuable resources. Small pieces of plastic that are less than 5 mm in size are usually referred to as microplastics. Microplastics have become pervasive and abundant in various environments such as drinking water, oceans, terrestrial lands, and the atmosphere. Nowadays, microplastics are recognized as emergent environmental hazards and have drawn a lot of community attention due to their severe toxicity to ecosystems and human beings. It is extremely challenging to gather and reuse microplastics because of their small size and dilution in the environment. The most prevalent polyester plastic and a significant contributor to plastic waste is polyethylene terephthalate (PET), which is basically recyclable. However, although around 30 million tons of PET are globally produced, only 9% of PET is practically recycled [3]. Current waste management systems are unable to efficiently and affordably treat a variety of plastic waste including PET microplastics, and thus, new technologies are urgently needed to convert microplastic waste into useful products. Photocatalysis is a technology that has been recently developed for microplastic treatment to produce valuable organic chemicals and fuels [4, 5].

In addition to environmental pollution by microplastics, the world is also facing an energy crisis and CO2\mathrm{CO}_2 emissions by fossil fuels. It is important to develop sustainable fuels and novel technologies to effectively tackle this energy crisis. Hydrogen (H2\mathrm{H}_2), characterized by its eco-friendly nature, presents itself as an ideal clean energy carrier [6, 7]. H2\mathrm{H}_2 is primarily produced through energy-intensive and unclean processes. For instance, the steam-methane reforming method, which is used worldwide, necessitates the use of high-temperature (973-1273 K) and high-pressure (3-25 bar) [7]. Moreover, a significant amount of CO2\mathrm{CO}_2 is emitted into the atmosphere during steam reforming. Photocatalytic H2\mathrm{H}_2 production from water has emerged as an effective and clean alternative to produce H2\mathrm{H}_2 at ambient temperature and pressure utilizing solar energy as a power source. In this process, photoexcited electrons of the catalyst contribute to H2\mathrm{H}_2 production and corresponding holes contribute to O2\mathrm{O}_2 production. However, limited catalysts can produce both H2\mathrm{H}_2 and O2\mathrm{O}_2, and thus, most of the H2\mathrm{H}_2 production systems need a sacrificial agent for holes such as alcohol. Researchers have developed an ambient-temperature catalytic process for H2\mathrm{H}_2 production and simultaneous plastic degradation that not only does not need any extra sacrificial agent but also converts plastic waste to useful organic chemicals. The process, which is known as photoreforming and shown schematically in Figure 1a [4, 5], comprises four essential elements of catalyst, substrate (plastics), water, and light. Under light irradiation, electrons in the valence band (VB) of the catalyst are excited to the conduction band (CB). The excited electrons reduce H+\mathrm{H}^{+} of water to form H2\mathrm{H}_2, while the holes left in VB together with hydroxyl radicals oxidize plastics to other organic products [5, 8, 9, 10].

Schematics of photoreforming process, illustration of HPT method, and illustration of this study’s steps of synthesis process

Figure 1. (a) Schematics of photoreforming process, (b) illustration of HPT method, and (c) illustration of this study’s steps of synthesis process.

A catalyst for simultaneous H2\mathrm{H}_{2} production and plastic degradation should have several features such as a suitable bandgap to absorb light photons and produce electrons and holes, an appropriate band structure for water reduction and plastic degradation, an appropriate lifetime of electrons and holes, and a stable chemical structure under alkaline conditions. Currently, several groups of catalysts, including sulfides [5, 11, 12, 13, 14], nitrides [15, 16, 17, 18], phosphides [19, 20], metal oxides [21, 22], and bimetallic metal-organic frameworks (MOFs) [23] are used for this process. While phosphides and sulfides demonstrate the best activity for photoreforming, they usually have low stability compared to oxides [13, 14, 15, 16]. Despite the development of such catalysts, particularly in recent years, there is still high demand to explore new families of materials that are highly stable and active for converting plastic waste and producing H2\mathrm{H}_{2}. One possible candidate for this application is high-entropy ceramics which have recently gained attention due to their remarkable stability and promising functional properties including catalytic activity [24, 25, 26, 27]. High-entropy ceramics are typically defined as multi-component materials with at least five principal cations and a configurational entropy higher than 1.5R1.5R (RR: the gas constant) [28, 29, 30]. The high stability of these materials is due to high configurational entropy and accordingly low Gibbs energy, while their unique functional properties are due to their strained lattice, heterogenous valence electron distribution, and cocktail effect [28, 29, 30]. The most popular high-entropy ceramics are high-entropy oxides (HEOs), which have been employed in numerous applications such as Li-ion batteries [31, 32], Li-S batteries [33], Zn-air batteries [34], dielectric components [35], magnetic components [36], thermal barrier coating [37], and catalysts [38, 39, 40, 41]. Despite the high potential of HEOs for catalysis, there have been no reports to date to employ them for photoreforming for simultaneous H2\mathrm{H}_{2} production and plastic degradation.

In this study, TiZrHfTaNbO11\mathrm{TiZrHfTaNbO}_{11}, an HEO catalyst, is synthesized and its catalytic activity for simultaneous H2\mathrm{H}_{2} production and PET plastic degradation is investigated. This HEO is selected because five transition elements of titanium, zirconium, niobium, hafnium, and tantalum have the d0d^{0} electronic configuration which is suitable for photocatalysis and their mixture can thus show catalytic properties under light [39]. This first application of HEOs for photoreforming and simultaneous H2\mathrm{H}_{2} production and plastic conversion reveals that TiZrHfTaNbO11\mathrm{TiZrHfTaNbO}_{11} exhibits superior activity compared to the benchmark photocatalyst P25 TiO2\mathrm{TiO}_{2}, introducing HEOs as a new family of catalysts for photoreforming.

Materials and methods

The HEO was synthesized by a three-step synthesis method of arc-melting, high-pressure torsion (HPT) severe plastic deformation processing, and high-temperature oxidation, and examined by various characterization methods, as illustrated below.

Reagents

Pure metals of Ti (99.9%, Furuuchi Chemical, Japan), Zr (99.7%, Furuuchi Chemical, Japan), Hf (99.7%, Sigma-Aldrich, USA), Nb (99.9%, Kojundo Chemical, Japan), and Ta (99.9%, Furuuchi Chemical, Japan) were used without any further purification. Pure PET micropowder with particle sizes smaller than 300 μm\mu\mathrm{m} was purchased from GoodFellow, England, and a PET plastic water bottle with a thickness of 160 μm\mu\mathrm{m} was purchased from a local market, dried, and cut into pieces with a diameter of 6 mm. NaOH was purchased from Fujifilm, Japan, and a solution of 40% NaOD in D2O\mathrm{D}_{2}\mathrm{O} (99 at% of D) was obtained from Sigma-Aldrich, USA. Coumarin as a hydroxyl radical trapper was prepared from Tokyo Chemical Industry Co., LTD, Japan. Isopropanol was purchased from Sigma-Aldrich, USA.

Synthesis of catalyst

The HEO oxide was synthesized in three steps including arc-melting, HPT processing, and oxidation. The illustration of the HPT method is shown in Figure 1b [42, 43], and the sample synthesis procedure is shown in Figure 1c. Initially, high-purity Ti, Zr, Hf, Nb, and Ta pieces, possessing equal atomic fractions, were arc-melted using a non-consumable tungsten electrode and a water-cooled copper crucible in a high-purity Ar atmosphere to achieve an ingot of high-entropy alloy (HEA) TiZrHfTaNb with 10 g mass. To ensure a homogeneous chemical composition, the resulting HEA ingot was accurately rotated and re-melted seven times. For further enhancement of the homogeneity, the HEA was subjected to HPT. For HPT processing, the HEA ingot was first cut into disc-shaped samples with 10 mm in diameter and 0.8 mm in thickness using an electric-discharge wire cutting. The HPT process was conducted for 10 turns under a pressure of 6 GPa at ambient temperature with a rotation speed of 1 rpm. In the third step, the HPT-processed discs were exposed to air oxidation at 1373 K for 48 h, which resulted in a 22.5% increase in the sample mass, which reasonably corresponds to a composition of TiZrHfTaNbO11\mathrm{O}_{11}.

Catalyst characterization

The crystal structure of as-prepared HEO was measured by X-ray diffraction (XRD) using a Cu Kα\alpha source. Raman spectra were also recorded with a 325 nm laser as an excitation source. The microstructure and distribution of elements at the micrometer level were examined by scanning electron microscopy (SEM) equipped with energy-dispersive X-ray spectroscopy (EDS). The samples for SEM were dispersed onto the carbon tape and analyzed under 15 kV. The microstructure and the distribution of elements at the nanometer levels were examined by transmission electron microscopy (TEM) and scanning-transmission electron microscopy (STEM) equipped with an EDS detector. For TEM and STEM, the samples were crushed in ethanol and dispersed on copper grids covered with a carbon film. TEM and STEM were conducted in the bright-field (BF) mode, the dark-field (DF) mode, selected area electron diffraction (SAED), and high-resolution (HR) imaging combined with fast Fourier transform (FFT). The specific surface area of catalysts was estimated by N2\mathrm{N}_{2} adsorption and the Brunauer-Emmett-Teller (BET) approach which was 0.7 m2^{2}/g.

Optical properties were first examined by ultraviolet-visible (UV-Vis) diffuse reflectance spectroscopy. Bandgap was calculated by considering the light absorbance using the Kubelka-Munk analysis. To examine the electron-hole recombination, steady-state photoluminescence (PL) was conducted using a 325 nm laser source. The lifetime of excited electrons was examined by a time-resolved photoluminescence decay (PL decay) with a 285 nm laser source. To evaluate the mobility of photoexcited electrons, photocurrent was examined. For photocurrent measurement, fluorine-doped tin oxide glass was coated with a mixture of catalyst and ethanol. Then, to enhance the binding between the catalyst particles and glass substrate, the coated glass was baked in a muffle furnace at 473 K for 1 h. The potentiostatic amperometry mode of photocurrent measurement was performed in Na2SO4\mathrm{Na}_2\mathrm{SO}_4 (0.1 M) electrolyte using the glass as a working electrode, Pt wire as the counter electrode, and Ag/AgCl as a reference electrode. To investigate the generation of oxygen vacancies, electron paramagnetic resonance (EPR) analysis was performed at room temperature using a 9.4688 GHz microwave source.

Catalytic experiments

50 mg of PET and 50 mg of the HEO were dispersed in 3 mL of 10 M NaOH mixed with 250 μ\muL of 0.01 M Pt(NH3)4(NO3)2\mathrm{Pt}(\mathrm{NH}_3)_4(\mathrm{NO}_3)_2 (to deposit 1 wt% of Pt as a co-catalyst) in a quartz photoreactor tube with a volume of 30 mL. The alkaline NaOH is used to hydrolyze PET to terephthalate and ethylene glycol during photoreforming. A concentration of 10 M of NaOH was selected based on the literature and optimization by the authors [4, 11]. The mixture was capped with a rubber septum, air-evacuated by Ar injection for 30 min, and ultrasonicated for 5 min. The samples were then irradiated by a 300 W Xe light. The distance between the light source and the sample was 10 cm and the intensity of the light source at this distance was 18 kW/m2^{2}. The temperature of the photoreactor was kept at 298 K by using a water bath, while stirred with a rate of 800 rpm. H2_{2} generation was quantified by gas chromatography using a thermal conductivity detector with Ar being the carrier gas. For comparison purposes, P25 TiO2_{2} as a reference catalyst was also examined under similar reaction conditions.

Post-catalysis characterizations

The stability of the catalyst after the catalytic test was examined by conducting XRD and Raman analyses and comparing the results with the initial HEO. The reusability of the HEO was assessed through three consecutive photocatalytic cycles. After each cycle, the HEO was collected, thoroughly rinsed with deionized water until the pH was neutral, dried at 333 K, and then reused in the photoreforming process.

For the evaluation of the plastic degradation products and radicals, the liquid phase was examined by nuclear magnetic resonance (NMR) and fluorescence spectroscopy. The concentration of hydroxyl (∙OH\bullet\mathrm{OH}) radical in the liquid phase after the catalytic process was measured by adding 0.4 mg of coumarin in the form of 1 mM solution. Since coumarin reacts with ∙OH\bullet\mathrm{OH} and produces 7-hydroxycoumarin, a spectrofluorometer with an excitation wavelength of 332 nm was employed to record the fluorescence signal of the generated 7-hydroxycoumarin at 450 nm as an indicator of the ∙OH\bullet\mathrm{OH} concentration. The quenching experiment with isopropanol (0.02 mmol/L) was conducted to investigate the role of ∙OH\bullet\mathrm{OH} in the photoreforming reactions. 1^{1}H NMR spectra were collected by a Bruker spectrometer using 10 M NaOD in D2_{2}O to identify the degradation products of PET plastic during catalytic degradation. The noesygppr1d process program was used for the 1^{1}H NMR analysis with water suppression. Maleic acid with a concentration of 50 mg mL−1^{-1} in D2_{2}O was utilized for quantitative analysis. The quantity of oxidized products (mproductm_{\mathrm{product}}) after the photoreforming reaction was calculated by Eq. (1).

mproduct=IproductImaleic acid×Nmaleic acidNproduct×MproductMmaleic acid×mmaleic acid(1)m_{\mathrm{product}} = \frac{I_{\mathrm{product}}}{I_{\mathrm{maleic\ acid}}} \times\frac{N_{\mathrm{maleic\ acid}}}{N_{\mathrm{product}}} \times\frac{M_{\mathrm{product}}}{M_{\mathrm{maleic\ acid}}} \times m_{\mathrm{maleic\ acid}} \tag*{(1)}

with mm, II, NN and MM are the mass, integral of the NMR peak, number of protons corresponding to the peak and molar mass, respectively.

The plastic pieces were also examined by different methods. An analytical balance was used to measure the degraded plastic mass during catalysis. Remained plastic pieces were sputter-coated with a thin layer of gold and analyzed by SEM. Attenuated total reflectance-Fourier transform infrared spectroscopy (ATR-FTIR) within the range of 600-4000 cm−1^{-1} was utilized to analyze the possible changes in the structure of plastic during catalytic degradation.

Results

Catalyst characterization

Crystal structure evolution during each synthesis step was examined by XRD profiles, as shown in Figure 2a. The ingot after arc melting possesses a body-centered cubic (BCC) phase with a space group of Im3‾mIm\overline{3}m (229) and a lattice parameter of a=3.41±0.21a = 3.41 \pm0.21 Å. This is consistent with previous reports on similar HEA [44, 45]. The same BCC phase of HEA is obtained after the second synthesizing step of HPT, but the main difference is the significant peak broadening due to the crystallite size reduction and defect generation, as reported in a wide range of HPT-processed materials [42, 43]. Oxidized samples contain two phases with monoclinic and orthorhombic structures with almost equal mass fractions. The monoclinic phase has a A2/mA2/m space group with the cell parameters of a=11.87±0.07a = 11.87 \pm0.07 Å, b=3.82±0.15b = 3.82 \pm0.15 Å, c=20.55±2.05c = 20.55 \pm2.05 Å, α=γ=90∘\alpha= \gamma= 90^\circ, and β=119.93∘±4.80∘\beta= 119.93^\circ\pm4.80^\circ [46]. The orthorhombic phase has an Ima2Ima2 space group with the cell parameters of a=45.97±1.84a = 45.97 \pm1.84 Å, b=4.62±0.23b = 4.62 \pm0.23 Å, c=5.12±0.26c = 5.12 \pm0.26 Å, and α=β=γ=90∘\alpha= \beta= \gamma= 90^\circ [47]. Raman spectra taken from different positions of HEO confirm similar spectra, as shown in Figure 2b, but peak intensities follow two distinguishable patterns which should be due to the presence of dual phases.

Dual-phase structure of high-entropy oxide examined by XRD and Raman spectroscopy

Figure 2. Dual-phase structure of high-entropy oxide examined by (a) XRD and (b) Raman spectroscopy taken at four different positions.

The microstructure of the HEO sample, examined by SEM micrographs at different magnifications is shown in Figure 3. SEM measurement indicates that the average particle size is 1.9 μm, while the examination of microstructure in a higher magnification indicates that there are numerous crystals in particles with an average size of 310 nm. These rather large particle sizes are due to the synthesis method which uses high pressure and high temperature, leading to the consolidation of HEOs [30].

Morphology of high-entropy oxide examined by SEM at different magnifications

Figure 3. Morphology of high-entropy oxide examined by SEM at different magnifications.

High-entropy materials usually possess a uniform distribution of elements [30, 31, 32, 33, 34, 35, 36, 37]. To confirm the uniformity of elements in the HEO, SEM-EDS, and STEM-EDS were performed, as shown in Figure 4. Despite the dual-phase feature of the HEO, the distribution of five elements is reasonably homogeneous. SEM-EDS analysis also suggests that the general composition of the HEO should be TiZrHfTaNbO11\mathrm{TiZrHfTaNbO}_{11} which is consistent with the mass analysis before and after arc melting as well as with mass analysis before and after oxidation. Moreover, the valence of cations in this system suggests a composition of TiZrHfTaNbO11\mathrm{TiZrHfTaNbO}_{11} which is consistent with SEM-EDS and mass analyses [38].

Uniform distribution of elements in high-entropy oxide

Figure 4. Uniform distribution of elements in high-entropy oxide. (a) SEM-EDS and (b) STEM-EDS analyses.

Nanostructural examinations are shown in Figure 5 using TEM in (a) BF, (b) SAED, and (c-f) HR modes. The BF image and ring pattern of SAED verify the presence of numerous nanocrystals with random crystallographic orientations. The lattice image in Figure 5c exhibits significant lattice distortion with numerous dislocation defects within the crystal structure. The presence of dislocations can be considered a positive feature in this work because previous studies indicated that dislocations could amplify light absorption and improve catalytic activity [48]. The lattice images in Figure 5d-Figure 5f support the co-existence of monoclinic and orthorhombic phases and a significant proportion of interphase boundaries. The interphases can serve as charge heterojunctions to facilitate the separation and mobility of charge carriers to increase catalytic activity [49]. Here, it should be noted that EPR spectroscopy did not provide a clear piece of evidence for oxygen vacancies in this HEO, although vacancies are generally expected to exist in high-entropy materials [28, 29, 30].

TEM images showing formation of dual-phase high-entropy oxide

Figure 5. Formation of dual-phase high-entropy oxide with high density of dislocations and interfaces. TEM (a) BF image, (b) SAED pattern, and (c-f) HR images at different magnifications.

Figure 6a presents the UV-Vis spectrum of HEO with an obvious absorbance edge at 430 nm and some light absorbance in the visible light region. For comparison, the UV-Vis spectrum of P25 TiO2\mathrm{TiO}_{2}, as a benchmark catalyst, is included in Figure 6a. The absorbance edge of HEO, which is similar to P25, is related to the bandgap of the material, while the defects might be considered as the reason for the higher visible light absorbance of HEO compared to P25. Based on the Kubelka-Munk analysis, the bandgap is estimated at 3.2 eV, as shown in Figure 6b. This is reasonably similar to the TiO2\mathrm{TiO}_{2} bandgap and narrower than that of other binary oxides in the Ti-Zr-Hf-Nb-Ta-O system which were reported from 3.2 eV to 5.7 eV [50].

Light absorbance of high-entropy oxide in both UV and visible light regions

Figure 6. Light absorbance of high-entropy oxide in both UV and visible light regions. (a) UV-Vis light absorbance spectrum of high-entropy oxide compared to P25 TiO2\mathrm{TiO}_2, and (b) Kubelka-Munk plot for bandgap calculation (α\alpha: light absorption, h: Planck’s constant, ν\nu: light frequency).

Charge-carrier dynamics and oxygen vacancies were examined by various techniques including steady-state PL, time-resolved PL decay, and photocurrent, as shown in Figure 7. The steady-state PL spectra show a PL peak of HEO at 552 nm, which should be due to radiative recombination of electrons and holes on defects. The PL peak intensity of the HEO is comparatively low compared to the PL peak intensity of P25 (Figure 7a). This suggests that the current HEO can serve as a good catalyst with low electron-hole recombination. PL decay spectrum in Figure 7b follows an exponential equation [51].

Reasonable charge carrier dynamics of high-entropy oxide

Figure 7. Reasonable charge carrier dynamics of high-entropy oxide. (a) Steady-state PL emission of HEO and P25, (b) time-resolved PL decay of HEO, (c) photocurrent generation of HEO, and (d) photocurrent generation of P25.

I(t)=A1exp⁡(−tτ1)+A2exp⁡(−tτ2)(2)I(t) = A_1 \exp\left(-\frac{t}{\tau_1}\right) + A_2 \exp\left(-\frac{t}{\tau_2}\right) \tag*{(2)}

In this equation, I(t)I(t) represents the PL decay intensity at time tt, A1A_1 and A2A_2 are the amplitudes of the first and second exponential functions, respectively, and τ1\tau_1 and τ2\tau_2 correspond to the fast and slow decay time. The analysis of the PL decay yields values of A1=42.3A_1 = 42.3, A2=57.7A_2 = 57.7, τ1=1.5\tau_1 = 1.5 ns, and τ2=10.4\tau_2 = 10.4 ns. Subsequently, the average electron lifetime of the HEO, τave\tau_{ave} was calculated as 9.5 ns based on the following equation [51].

τave=A1τ12+A2τ22A1τ1+A2τ2(3)\tau_{\mathrm{ave}}=\frac{A_{1}\tau_{1}^{2}+A_{2}\tau_{2}^{2}}{A_{1}\tau_{1}+A_{2}\tau_{2}} \tag*{(3)}

This lifetime is considered rather long for photocatalysts. For example, the previously reported lifetime values of the most common TiO2_{2} catalysts are 0.93 ns for anatase [52], 0.03 ns for rutile [53], and 1.55 ns [54] or 2.41 ns [55] for P25. The longer charge carrier lifetime of the current HEO indicates its high potential for superior photoreforming. Photocurrent measurements in Figure 7c confirm that the HEO successfully generates photo-induced electrons. For comparison, Figure 7d shows the photocurrent generation of P25. Here, it should be noted that P25 has nanopowders that make a large interface area with FTO glass for electron transfer, while the HEO has micropowders with a small interface area with FTO. Therefore, a direct comparison of photocurrent intensities does not provide much information about the behavior of the two materials. However, the differences in the shape of photocurrent spectra give important information. For P25, spike peaks are visible at the start of illumination followed by a significant decrease in photocurrent, indicating that the generation of electrons and holes is followed by quick recombination. For the HEO, the spike peaks are absent except for the first illumination cycle, suggesting a better electron-hole separation than P25.

Photoreforming of PET microplastics

The catalytic activity of HEO in comparison with P25 for H2H_2 production from PET microplastic photoreforming under light with and without platinum co-catalyst is presented in Figure 8. No H2H_2 is detected for blank tests without a catalyst addition and with irradiation (red curve) or with catalyst addition under the dark conditions (data at time zero). The amount of produced H2H_2 increases as the photo-exposure time increases, indicating a direct correlation between photo-exposure time and H2H_2 production yield. During the first 30 min, there is a higher rate of H2H_2 production, but the rate of H2H_2 production subsequently reduces and follows a linear curve. The faster rate at the first 30 min can be attributed to the abundance of initial active sites on both catalysts and PET plastic surfaces [4, 5]. Figure 8a shows that the addition of platinum co-catalyst enhances the H2H_2 production in both P25 and HEO systems which signifies the important role of co-catalyst in providing active sites for the photoreforming process. Since the comparisons in Figure 8a can be influenced by a large difference between the surface area of the two catalysts (HEO and P25), additional comparisons were made by TiO2\mathrm{TiO}_2 polymorphs (rutile, anatase and brookite) and ZnO which are well-known photocatalysts for hydrogen production. To bring the surface area of these TiO2\mathrm{TiO}_2- and ZnO-based catalysts closer to the HEO, HPT processing was applied to them, as attempted in a few earlier studies [56, 57, 58, 59]. Although HPT processing can significantly enhance the photocatalytic activity by the introduction of oxygen vacancies and phase transformations (e.g. anatase to columbite in TiO2\mathrm{TiO}_2 [56, 57] and wurtzite to rocksalt in ZnO [59]), it is still interesting to compare such catalysts with the HEO for photoreforming. As shown in Figure 8b, anatase-columbite TiO2\mathrm{TiO}_2 processed by HPT for 3 turns (surface area: 0.7 m2/g0.7\ \mathrm{m}^2/\mathrm{g} [57]) and black brookite TiO2\mathrm{TiO}_2 processed by HPT at 473 K for 1 turn (surface are: 0.2 m2/g0.2\ \mathrm{m}^2/\mathrm{g} [58]) exhibits a better activity than HEO perhaps due to easy charge separation, slow decay and moderate electron trap energy in black brookite [60], and high water adsorption energy and better surface activity for proton formation in columbite [61]. However, the activity of the HEO (surface area: 0.7 m2/g0.7\ \mathrm{m}^2/\mathrm{g}) is better than rutile TiO2\mathrm{TiO}_2 synthesized by HPT for 3 turns followed by annealing at 1073 K and ZnO processed by HPT for 4 turns (surface area: 1.3 m2/g1.3\ \mathrm{m}^2/\mathrm{g} [59]).

High activity of high-entropy oxide for hydrogen production from photoreforming of PET microplastics

Figure 8. High activity of high-entropy oxide for hydrogen production from photoreforming of PET microplastics. (a) H2H_2 production versus irradiation time for high-entropy oxide and P25 TiO2TiO_2 catalysts with and without co-catalyst including blank test. (b) H2H_2 production versus irradiation time for high-entropy oxide with co-catalyst addition compared with rutile TiO2TiO_2 synthesized by HPT for 3 turns followed by annealing at 1073, anatase-columbite TiO2TiO_2 processed by HPT for 3 turns, black brookite TiO2TiO_2 processed by HPT at 473 K for 1 turn and ZnO processed by HPT for 4 turns.

In the photoreforming process, not only green H2H_2 is generated from water through the reduction half-reaction but also other useful products are produced through plastic oxidation. To identify the organic oxidation products from PET, 1H^1H NMR analysis was performed in 10 M NaOD in D2OD_2O with the same sample concentration as that of the catalytic test. The 1H^1H NMR spectra are shown in Figure 9 and the quantitative data are presented in Table 1, indicating PET is degraded into different products after 4 h of light irradiation. It can be observed that PET undergoes hydrolysis to ethylene glycol and terephthalate. Terephthalate is quite stable and is recovered to produce PET plastic again, while ethylene glycol is subsequently photo-converted into formic acid. The PET plastic degradation pathway is illustrated in Figure 10. Comparable oxidation products of PET have been documented in several previous studies [4, 62, 63]; however, variations in the degradation products have been also observed, likely due to differences in experimental conditions such as the choice of catalyst, alkaline concentration, irradiation duration, pre-treatment method or the quantity of plastic used. For example, in a previous study, after 8 days of photoreforming, carbonized polymer dots/g-C3N4\mathrm{C}_{3}\mathrm{N}_{4} converts PET to 110 µmol glycolaldehyde, 383 µmol glycolic acid, 139 µmol formic acid, 128 µmol ethanol, 43 µmol acetaldehyde, and 554 µmol acetic acid [16]. In another study, carbon nitride - carbon nanotubes - NiMo hybrid converted PET to glyoxal and glycolic acid [3], while MoS2/CdxZn1−xS\mathrm{MoS}_{2}/\mathrm{Cd}_{x}\mathrm{Zn}_{1-x}\mathrm{S} led to the formation of formic acid, glycolic acid and methylglyoxal from PET [64].

Formation of various valuable chemicals from photoreforming of PET microplastics using high-entropy oxide

Figure 9. Formation of various valuable chemicals from photoreforming of PET microplastics using high-entropy oxide. 1H^{1}\mathrm{H} NMR spectra of PET after 4 h light irradiation in the presence of high-entropy oxide using 10 M NaOD in D2O\mathrm{D}_{2}\mathrm{O} and maleic acid as internal standard.

ProductsAmount (mmol)Amount (mmol/m2^{2})
H2_20.0421.20
Terephthalate0.0060.17
Ethylene glycol0.0501.43
Formic acid0.0190.54

Table 1. Quantitative PET photoreforming products after 4 h light irradiation in the presence of high-entropy oxide, 10 M NaOD in D2_2O and maleic acid.

Figure 10. Degradation pathways of PET microplastics using high-entropy oxide.

Quantitative data gathered for hydrogen production and plastic degradation can be used to estimate the degradation rate, charge balance and carbon balance. During 4 h of experiments using a solution of 10 M NaOH, the hydrolysis process produces 0.17 mmol m−2^{-2} terephthalate and 1.43 mmol m−2^{-2} ethylene glycol. Subsequently, 16% of ethylene glycol is oxidized to produce 0.54 mmol m−2^{-2} formic acid. The electrons utilized in hydrogen generation (2 electrons per H2\mathrm{H}_{2}) after 4 h of photoreforming are estimated at approximately 2.4 mmol m−2^{-2}, closely matching the hole transfer number (4.3 mmol m−2^{-2}) calculated from the oxidation of ethylene glycol to formic acid (8 holes per HCOOH), resulting in a charge balance of 55%. The carbon balance achieved by comparing the mass of the initial plastic and the mass of degradation products is at least 32%, possibly underestimated due to the remaining undegraded plastics as well as due to not detecting certain oxidized products by NMR. It should be noted that the hydrolysis products were too small to be detected by NMR when NaOH concentration was low and pH was below 14. Even using a 5 M NaOH solution did not lead to measurable hydrolysis products within the detection limes of NMR. These results indicate that a highly alkaline solution is essential for the photoreforming of PET, which is somehow a negative aspect of this process. Future studies should incorporate more sensitive analyses, such as high-performance liquid chromatography (HPLC), to detect a wider range of products.

In the photoreforming process, the generated reactive radicals, particularly ∙OH\bullet\mathrm{OH} radicals, contribute to the oxidation transformations and control the catalyst activities [4, 5]. Therefore, it is important to assess the generation of radicals during the process. The quantification of ∙OH\bullet\mathrm{OH} radical generation was conducted by employing coumarin as a probe radical trap reagent, and examination of the formation of coumarin-OH adduct (7-hydroxycoumarin) by fluorescence spectroscopy [64]. Figure 11a presents a comparison of the production of 7-hydroxycoumarin resulting from the use of the HEO compared with P25 TiO2_2. The data reveal a notably higher production of 7-hydroxycoumarin from the HEO, signifying that it exhibits a superior rate of ∙OH\bullet\mathrm{OH} radical formation, even in comparison with the benchmark catalyst P25 TiO2_2. To further investigate the role of ∙OH\bullet\mathrm{OH} radicals on the photoreforming process, the quenching experiment for ∙OH\bullet\mathrm{OH} radical scavenger was conducted. As shown in Figure 11b, the addition of isopropanol leads to a decrease in H2H_2 production from PET plastic photoreforming. Therefore, ∙OH\bullet\mathrm{OH} radical is one of the important factors in the photoreforming process.

High •OH radical formation from photoreforming using high-entropy oxide

Figure 11. High •OH radical formation from photoreforming using high-entropy oxide. (a) Fluorescent light intensity corresponding to reaction of •OH radicals and coumarin and formation of 7-hydroxycoumarin using high-entropy oxide and P25 TiO2_2 catalysts after 20 min light irradiation and (b) hydrogen production versus irradiation time during photoreforming process with and without addition of isopropanol (•OH radical scavenger) for Pt/TiZrHfNbTaO11_{11}.

Photoreforming of PET plastic bottle

In this study, the photoreforming of a PET bottle was also examined. Since commercial plastic bottles often contain additional fillers, antioxidants, or linkers, their degradation behavior can be different from pure PET micropowders. Figure 12 shows catalytic H2_2 production versus light irradiation time for the photoreforming of PET bottle and micropowders. After 4 h of irradiation, photoreforming of PET bottle produces 343 μ\mumol m−2^{-2} of H2_2, while the generated H2_2 amount is as high as 1276 μ\mumol m−2^{-2} for photoreforming of PET micropowders. A four-time higher activity of PET micropowder compared to the PET bottle can be due to its higher purity as well as larger surface area. Photoreforming of the PET bottle even with a lower rate compared to pure microplastics is still of significance because plastic bottles are responsible for a large environmental contamination [1, 2]. Here, it should be noted that although plastic waste cannot enhance the light absorbance by the catalyst for photoreforming, the charge carrier transition from catalyst to plastic can positively enhance the lifetime of charge carriers [65].

Hydrogen production versus irradiation time for PET plastic bottle and PET microplastic

Figure 12. Slower photoreforming rate of PET plastic bottle compared to micropvders using high-entropy oxide. Hydrogen production versus irradiation time for PET bottle and microplastics using high-entropy oxide and P25 TiO2_2 catalysts.

Figure 13 shows the change in (a) light transmission, (b) mass loss, and (c, d) surface morphology of PET plastic, examined by SEM, before and after the photoreforming process. The mass loss was calculated as

Loss of transparency and mass of PET plastics during photoreforming using high-entropy oxide catalyst

Figure 13. Loss of transparency and mass of PET plastics during photoreforming using high-entropy oxide catalyst. (a) UV-Vis transmission spectra of PET plastic bottle before and after photoreforming for 0.5 and 2 h, (b) mass loss of PET plastic bottle versus irradiation time, and (c, d) surface morphology of PET plastic bottle examined by SEM (c) before and (d) after photoreforming for 12 h.

Mass loss (%)=m0−mtm0×100(4)\text{Mass loss (\%)} = \frac{m_0-m_t}{m_0} \times100 \tag*{(4)}

where, m0m_0 and mtm_t represent the initial and final masses of PET pieces after photodegradation. The light transmittance of PET plastic slightly decreases over time, as shown in Figure 13a. In other words, the surface of the initial PET sample is clean, and its light transmittance is high; however, as the degradation progresses, it becomes slightly opaque due to the development of surface roughness and micro-holes. The mass loss, shown in Figure 13b versus irradiation time, indicates a significant increase in plastic mass with irradiation time. After 16 h of irradiation, 100% of the plastic pieces are estimated to be photodegraded. Figure 13c presents the spotlessness of the initial PET surface; however, an increase in surface roughness and formation of deep cavities and holes are observed after irradiation (Figure 13d). This indicates that PET erosion occurs as a result of the photodegradation process which leads to transparency and mass losses as already shown in Figure 13a and Figure 13b. The observation of the photoreactor during irradiation also confirmed the gradual degradation of plastics and loss of transparency due to the formation of terephthalate monomers over time. These results indicate that photoreforming and mass loss of PET bottles proceed within a rather long time, but such a reaction can be accelerated by the mechanical treatment of bottles to form fine powders [1, 2].

ATR-FTIR spectroscopy was utilized to investigate the deterioration of PET pieces through oxidative degradation by the catalytic process. ATR-FTIR spectra were compared before and after the process for 12 h and shown in Figure 14. As illustrated in Figure 14a for the initial PET plastic bottle, the main identified peaks are C-H bending ethyl (731 cm−1731\ \mathrm{cm}^{-1}), C-O ester (10501050-1100 cm−11100\ \mathrm{cm}^{-1}), C-C phenyl ring (1408 cm−11408\ \mathrm{cm}^{-1}), C=O ester (1725 cm−11725\ \mathrm{cm}^{-1}), H-C=O group (2907 cm−12907\ \mathrm{cm}^{-1}), and C-H ethyl (2970 cm−12970\ \mathrm{cm}^{-1}) stretching vibration modes [66]. A comparison between the ATR-FTIR spectra before and after photoreforming, as shown in Figure 14b, indicates several points. (i) Peak intensities mostly reduce with photoreforming due to the photodegradation-induced elimination of ketones and aromatic characters in PET. (ii) The peak shift at vibration mode of 845 cm−1845\ \mathrm{cm}^{-1} affirms the deterioration of aromatic rings [66]. (iii) The peak shift at the vibration mode of 1725 cm−11725\ \mathrm{cm}^{-1}, which corresponds to the C=O stretching mode, indicates the formation of a terminal carboxylic acid group in the molecule. (vi) Several characteristic vibration modes at 12451245, 11251125, 13401340, 975975, and 845 cm−1^{-1}, corresponding to carbonyl, benzene, ether, and methylene groups, exhibit peak shifts due to the trans conformer. (v) IR bands at 1370 and 1040 cm−1^{-1}, which are attributed to the ethylene glycol unit vibrations, shift due to the gauche conformer. (vi) The IR band at 975 cm−1^{-1}, resulting from the asymmetric stretching of the trans-oxy-ethylene (O-CH2_2) group, shifts due to morphological changes [65]. To quantify ATR-FTIR data, the carbonyl index (CICI) and vinyl index (VIVI) were determined as follows [8].

ATR-FTIR spectra of PET bottle before and after photoreforming

Figure 14. Reduction of the intensity of ATR-FTIR peaks and their shift after photoreforming of PET bottle using high-entropy oxide. ATR-FTIR spectra for (a) initial PET bottle and (b) PET bottle before and after catalysis.

CI=A1740−A18350.08×t(5)CI = \frac{A_{1740} - A_{1835}}{0.08 \times t} \tag*{(5)}
VI=A909A2020(6)VI = \frac{A_{909}}{A_{2020}} \tag*{(6)}

where A1740A_{1740} and A1835A_{1835} represent the absorption intensities of the stretching vibration of the carbonyl group at 1740 cm−1^{-1} and 1835 cm−1^{-1}, respectively, tt is the sample thickness (0.16 mm), A909A_{909} and A2020A_{2020} denote the absorption intensities at 909 cm−1^{-1} and 2020 cm−1^{-1}, respectively. The calculated CICI for the initial PET bottle and after 12-hour photodegradation are 7.36 and 3.95 as shown in Table 2.

A1740A_{1740}A1835A_{1835}CICIA909A_{909}A2020A_{2020}VIVI
Initial-1.906-2.0007.36-1.968-2.0020.98
12 h photoreforming-1.947-1.9973.95-1.971-1.9970.99

Table 2. Decrease in the carbonyl index (CICI) and a minor increase in the vinyl index (VIVI) after photodegradation of PET bottle using high-entropy oxide catalyst. ATR-FTIR absorbance intensities at wavenumbers of 1740, 1853, 909, and 2020 cm−1^{-1} together with CICI and VIVI values before and after photodegradation for 12 h.

Concurrently, the VIVI exhibits a minor change from 0.98 to 0.99 after 12 hours of light irradiation. These variations in CICI and VIVI are indicative of the photodegradation process occurring in PET plastic under light exposure [8].

Catalyst stability and reusability

Characterization of the HEO catalyst after H2_2 generation and PET degradation was performed by XRD and Raman spectroscopy, as shown in Figure 15a and 15b, respectively. Data show that the crystal structure of the oxide is stable under light irradiation and high alkaline conditions during the catalytic test. Both monoclinic and orthorhombic phases remain unchanged after catalytic reactions. The stability of current HEO is consistent with previous studies which reported the remarkable stability of HEOs for numerous applications including Li-ion batteries [31, 32], Li-S batteries [33], Zn-air batteries [34], dielectric components [35], magnetic components [36], thermal barrier coating [37], and catalysts [38, 39, 40, 41]. The reusability of the HEO catalyst in three repeated cycles is presented in Figure 15c. The HEO catalyst exhibits good reusability because there is no significant decrease in hydrogen production between the three cycles. The high stability and reusability of HEOs are attributed to their high entropy, leading to a low Gibbs energy that promotes enduring performance through various environmental conditions and operational demands [28, 29, 30].

Stability and reusability of high-entropy oxide for photoreforming and simultaneous hydrogen production and PET plastic degradation

Figure 15. Stability and reusability of high-entropy oxide for photoreforming and simultaneous hydrogen production and PET plastic degradation. (a) XRD and (b) Raman spectra before and after catalytic test, and (c) H2\mathrm{H}_2 production versus irradiation time for high-entropy oxide for three repeated tests.

Discussion

This study reports the first application of HEOs for simultaneous H2_2 production and plastic degradation from the photoreforming process. H2_2 production was observed from both PET microplastics and a real PET bottle using a HEO. H2_2 production was confirmed by gas chromatography and plastic degradation is assessed during the photoreforming process by different methods. Firstly, degradation was confirmed by the decrease in mass and light transmittance, and the change in plastic surface morphology. Secondly, FTIR analysis indicated the deterioration of PET plastic and a decrease in the carbonyl index. Finally, the successful oxidation of PET plastic was verified by NMR measurement, indicating that PET is photodegraded to terephthalate, ethylene glycol, and formic acid. Three main questions need to be discussed here: (i) a comparison of the photoreforming performance of this HEO with the benchmark catalyst of P25 TiO2_2 and other available catalysts from the literature, (ii) reasons for the superior catalytic activity of the HEO, and (iii) underlying mechanism for simultaneous H2_2 production and PET degradation.

Regarding the first question, a comparison of the PET photoreforming performance of various catalysts is presented in Table 3. The catalytic activity of the HEO for H2_2 production significantly surpasses that of the P25 TiO2_2 benchmark catalyst (Figure 8). The H2_2 production yield after 4 h of light irradiation is 319 and 32 μ\mumol m−2^{-2} h−1^{-1} for the HEO and P25 TiO2_2, respectively. Although it is hard to compare the results reported in different publications due to the experimental differences in reactor, light source, catalyst concentration, etc., Table 3 suggests that the current HEO has one of the highest reported activities for photoreforming [3, 14, 17, 18, 67, 68, 69, 70]. The H2_2 production rate of the HEO is higher than many of the published results and comparable with highly active phosphides and sulfides. However, phosphides and sulfides are not as stable as oxides, particularly HEOs which are known for their high stability [28, 29, 30]. Besides the performance of the HEO for H2_2 production, the second aspect that should be compared is plastic photo-oxidation. The degradation of different plastics using different catalysts is shown by the mass loss in Table 4. It can be concluded that this HEO is an active catalyst for plastic degradation compared to the data reported in the literature [71, 72, 73, 74, 75, 76, 77, 78, 79].

CatalystProduced H2\mathrm{H}_2 (μmol m−2 h−1\mu\mathrm{mol}\ \mathrm{m}^{-2}\ \mathrm{h}^{-1})Ref.
High-entropy oxide319This study
P25 TiO2\mathrm{TiO}_232This study
CN-CNTs-NiMo0.77[3]
CdS16.23[13]
Defect-rich NiPS3\mathrm{NiPS}_3540.78
CdS/d-NiPS3\mathrm{NiPS}_3926.48
CPDs-CN20.76[16]
Pt/g-C3N4\mathrm{C}_3\mathrm{N}_4102[18]
MXene/ZnxC1−xS\mathrm{Zn}_x\mathrm{C}_{1-x}\mathrm{S}123[67]
O-CuIn5S8\mathrm{CuIn}_5\mathrm{S}_8 nanosheet27.39[68]
CN0.14\mathrm{CN}_{0.14} porous microtube0.42[69]
RP@CoxPy/Cd0.5Zn0.5S\mathrm{RP}@\mathrm{Co}_x\mathrm{P}_y/\mathrm{Cd}_{0.5}\mathrm{Zn}_{0.5}\mathrm{S}59.27[70]

Table 3. Hydrogen production on high-entropy oxide from photoreforming of PET plastic, compared with P25 benchmark catalyst and reported data in the literature for various catalysts.

Type of plasticCatalystLight sourceIrradiation time (h)Mass loss (%)Ref.
PETHigh-entropy oxideUV16100This study
PE filmTiO2_2-MWCNTsUV18035[71]
HDPE microbeadsC, N-TiO2_2Visible5077.17[72]
LDPEFe-ZnOSunlight12040[73]
PP-LDPENiAl2_2O4_4Visible510[74]
PE filmTiO2_2Solar30042[75]
PAN nanofibersTiO2_2/gCNSimulated sunlight6063.2[76]
sunlight9099
PVC filmTiO2_2/nanographiteUV3017.24[77]
PS and PETiO2_2UV2499.99[78]
HDPEPorous N-TiO2_2Visible186.4[79]

Table 4. Photoreforming efficiency of different catalyst for degradation of various plastics, including polyethylene terephthalate (PET), polyethylene (PE), high-density polyethylene (HDPE), low-density polyethylene (LDPE), polyethylene plastic-low density polyethylene (PP-LDPE), polyacrylonitrile (PAN), polyvinyl chloride (PVC), and polystyrene (PS).

Regarding the second question, different aspects can be responsible for the high photocatalytic activity of the HEO: the presence of multiple cations in the catalyst leading to hybridized orbitals with higher activity for photocatalytic reactions [25, 80], the coexistence of two phases preventing charge carrier recombination at interfaces (as heterojunctions) and boosting photocatalytic activity [40, 48], the presence of lattice effects acting as activation sites of the catalyst [41, 49], the high visible light absorbance (Figure 6), the prolonged lifetime of charge carriers due to the defective nature of high-entropy materials (Figure 7), and the lattice straining effect caused by the coexistence of five cations [28, 29, 30]. All these aspects contribute to the enhanced photocatalytic activity of HEOs as a new family of catalysts for photoreforming.

Regarding the third question, the mechanism of simultaneous catalytic H2_2 production and plastic conversion is similar to the conventional photocatalytic H2_2 evolution process with organic sacrificial agents such as methanol. In this process, PET plastic serves as a hole sacrificial agent, it is oxidized by the photogenerated holes, while the photoexcited electrons reduce water to produce H2\mathrm{H}_2 [11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22]. When exposed to light irradiation, the high-entropy catalyst becomes photoexcited and its electrons migrate from the valence band to the conduction band. Under anaerobic conditions, these electrons actively participate in reducing H+\mathrm{H}^{+} of water to form H2\mathrm{H}_2. Simultaneously, holes remain in the valence band of catalysts or generate reactive ∙OH\bullet\mathrm{OH} radicals from OH−\mathrm{OH}^{-} of water. These holes and radicals oxidize PET plastic into organic chemicals with smaller molecules. The reaction can be summarized as follows [11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22].

HEO+hν→h(VB)++e(CB)−(7)\mathrm{HEO} + h\nu\to h^{+}_{(\mathrm{VB})} + e^{-}_{(\mathrm{CB})} \tag*{(7)}
2H++2e−→H2(8)2\mathrm{H}^{+} + 2e^{-} \to\mathrm{H}_{2} \tag*{(8)}
h(VB)++OH−→∙OH(9)h^{+}_{(\mathrm{VB})} + \mathrm{OH}^{-} \to\bullet\mathrm{OH} \tag*{(9)}
h(VB)+/∙OH+PET→Organic Products(10)h^{+}_{(\mathrm{VB})} / \bullet\mathrm{OH} + \mathrm{PET} \to\text{Organic Products} \tag*{(10)}

In summary, in photoreforming, not only plastic wastes are used as a sacrificial agent (instead of valuable chemicals like methanol), but also they are converted to value-added materials like hydrogen, terephthalate, ethylene glycol and formic acid. Therefore, the process has the potential to address two main issues of plastic waste management and clean H2\mathrm{H}_2 fuel production [5, 11, 12, 13, 14]. While this study proves the high photoreforming performance of HEO micropowders synthesized by the assistance of severe plastic deformation [81], future experimental and theoretical studies and in situ observation are essential to synthesize nanopowders of these materials, to clarify their high catalytic activity and to understand the contribution of individual elements to their performance.

Conclusions

A high-entropy catalyst is synthesized by a three-step procedure of arc-melting, high-pressure torsion processing, and oxidation, and used for simultaneous H2_2 production and PET plastic conversion through the photoreforming process. The synthesized high-entropy oxide showed better catalytic performance for H2_2 generation and plastic degradation compared to the benchmark catalyst P25 TiO2_2. In addition to green H2_2, other valuable chemicals including terephthalate, ethylene glycol, and formic acid were also produced through the photoreforming using the high-entropy catalyst. This study introduces HEOs as a new family of catalysts for photoreforming which have a higher stability and comparable activity to highly active sulfides and phosphides.

Acknowledgments

This study is supported partly by Mitsui Chemicals, Inc., Japan, partly through Grants-in-Aid from the Japan Society for the Promotion of Science (JP22K18737), and partly by the ASPIRE project of the Japan Science and Technology Agency (JST) (JPMJAP2332).

References

  1. [1]F. Zhang, M. Zeng, R.D. Yappert, J. Sun, Y.H. Lee, A.M. LaPointe, B. Peters, M.M. Abu-Omar, S.L. Scott, Polyethylene upcycling to long-chain alkylaromatics by tandem hydrogenolysis/aromatization, Science 370 (2020) 437-441.DOI
  2. [2]R. Geyer, J.R. Jambeck, K.L. Law, Production, use, and fate of all plastics ever made, Sci. Adv. 3 (2017) 1700782.DOI
  3. [3]X. Gong, F. Tong, F. Ma, Y. Zhang, P. Zhou, Z. Wang, Y. Liu, P. Wang, H. Cheng, Y. Dai, Z. Zheng, Photoreforming of plastic waste poly (ethylene terephthalate) via in-situ derived CN-CNTs-NiMo hybrids, Appl. Catal. B 307 (2022) 121143.DOI
  4. [4]T. Uekert, H. Kasap, F. Reisner, Photoreforming of nonrecyclable plastic waste over a carbon nitride/nickel phosphide catalyst, J. Am. Chem. Soc. 141(2019) 15201-15210.DOI
  5. [5]M. Du, Y. Zhang, S. Kang, X. Guo, Y. Ma, M. Xing, Y. Zhu, Y. Chai, B. Qiu, Trash to treasure: photoreforming of plastic waste into commodity chemicals and hydrogen over MoS₂-tipped CdS nanorods, ACS Catal. 12 (2022) 12823-12832.DOI
  6. [6]X. Jiang, H. Gong, Q. Liu, M. Song, C. Huang, In situ construction of NiSe/Mn₀.₅Cd₀.₅S composites for enhanced photocatalytic hydrogen production under visible light, Appl. Catal. B 268 (2020) 118439.DOI
  7. [7]E.T. Edirisooriya, P.S. Senanayake, H.B. Wang, M.R. Talipov, P. Xu, H. Wang, Photoreforming and degradation of waste plastics under UV and visible light for H₂ production using nanocomposite photocatalysts, J. Environ. Chem. Eng. 11 (2023) 109580.DOI
  8. [8]T. Kawai, T. Sakata, Photocatalytic hydrogen production from water by the decomposition of poly-vinylchloride, protein, algae, dead insects, and excrement, Chem. Lett. 10 (1981) 81-84.DOI
  9. [9]V. Preethi, S. Kanmani, Photocatalytic hydrogen production, Mater. Sci. Semicond. Process. 16 (2013) 561-575.DOI
  10. [10]B. Xia, Y. Zhang, B. Shi, J. Ran, K. Davey, S.Z. Qiao, Photocatalysts for hydrogen evolution coupled with production of value-added chemicals, Small Methods 4 (2020) 2000063.DOI
  11. [11]T. Uekert, M.F. Kuehnel, D.W. Wakerley, E. Reisner, Plastic waste as a feedstock for solar-driven H₂ generation, Energy Environ. Sci. 11 (2018) 2853-2857.
  12. [12]H. Nagakawa, M. Nagata, Photoreforming of organic waste into hydrogen using a thermally radiative CdOₓ/CdS/SiC photocatalyst, ACS Appl. Mater. Interfaces 13 (2021) 47511-47519.DOI
  13. [13]S. Zhang, H. Li, L. Wang, J. Liu, G. Liang, K. Davey, J. Ran, S.Z. Qiao, Boosted photoreforming of plastic waste via defect-rich NiPS₃ nanosheets, J. Am. Chem. Soc. 145 (2023), 6410-6419.DOI
  14. [14]C. Zhu, J. Wang, J. Lv, Y. Zhu, Q. Huang, C. Sun, Solar-driven reforming of waste polyester plastics into hydrogen over CdS/NiS catalyst, Int. J. Hydrogen Energy 51 (2024) 91-103.DOI
  15. [15]J.Q. Yan, D.W. Sun, J.H. Huang, Synergistic poly(lactic acid) photoreforming and H₂ generation over ternary NiₓCo₁₋ₓP/reduced graphene oxide/g-C₃N₄ composite, Chemosphere 286 (2022) 131905.DOI
  16. [16]M. Han, S. Zhu, C. Xia, B. Yang, Photocatalytic upcycling of poly(ethylene terephthalate) plastic to high-value chemicals, Appl. Catal. B 316 (2022) 120764.
  17. [17]Y.H. Lai, P.W. Yeh, M.J. Jhong, P.C. Chuang, Solar-driven hydrogen evolution in alkaline seawater over earth-abundant g-C₃N₄/CuFeO₂ heterojunction photocatalyst using microplastic as a feedstock, Chem. Eng. J. 475 (2023) 146413.DOI
  18. [18]T.K.A. Nguyen, T.P. Tran, X.M.C. Ta, T.N. Truong, J. Leverett, R. Daiyan, R. Amal, A. Tricoli, Understanding structure-activity relationship in Pt-loaded g-C₃N₄ for efficient solar-photoreforming of polyethylene terephthalate plastic and hydrogen production, Small Methods 8 (2023) 2300427.
  19. [19]G. Peng, X. Qi, Q. Qu, X. Shao, L. Song, P. Du, J. Xiong, Photocatalytic degradation of PET microfibers and hydrogen evolution by Ni₅P₄/TiO₂/C NFs, Catal. Sci. Technol. 13 (2023) 5868-5879.
  20. [20]Q. Wenbin, X. Qi, G. Peng, M. Wang, L. Song, P. Du, J. Xiong, An efficient and recyclable Ni₂P-Co₂P/ZrO₂/C nanofiber photocatalyst for the conversion of plastic waste into H₂ and valuable chemicals, J. Mater. Chem. C 11 (2023) 14359-14370.
  21. [21]D. Jiang, H. Yuan, Z. Liu, Y. Chen, Y. Li, X. Zhang, G. Xue, H. Liu, X. Liu, L. Zhao, W. Zhou, Defect-anchored single-atom-layer Pt clusters on TiO₂-x/Ti for efficient hydrogen evolution via photothermal reforming plastics, Appl. Catal. B 339 (2023) 123081.DOI
  22. [22]J. Yuting, H. Zhang, L. Hong, J. Shao, B. Zhang, J. Yu, S. Chu, An integrated plasma-photocatalytic system for upcycling of polyolefin plastics, Chem. Sus. Chem. 16 (2023) e202300106.DOI
  23. [23]J. Qin, Y. Dou, F. Wu, Y. Yao, H.R. Andersen, C. Hélix-Nielsen, S.Y. Lim, W. Zhang, In-situ formation of Ag₂O in metal-organic framework for light-driven upcycling of microplastics coupled with hydrogen production, Appl. Catal. B 319 (2022) 121940.DOI
  24. [24]M.S. Lal, R. Sundara, High entropy oxides - a cost-effective catalyst for the growth of high yield carbon nanotubes and their energy applications, ACS Appl. Mater. Interfaces 11 (2019) 30846-30857.DOI
  25. [25]S.H. Albedwawi, A. AlJaberi, G.N. Haidemenopoulos, K. Polychronopoulou, High entropy oxides-exploring a paradigm of promising catalysts: a review, Mater. Des. 202 (2021) 109534.DOI
  26. [26]S. Akrami, P. Edalati, Y. Shundo, M. Watanabe, T. Ishihara, M. Fuji, K. Edalati, Significant CO₂ photoreduction on a high-entropy oxynitride, Chem. Eng. J. 449 (2022) 137800.DOI
  27. [27]P. Edalati, X.F. Shen, M. Watanabe, T. Ishihara, M. Arita, M. Fuji, K. Edalati, High-entropy oxynitride as low-bandgap and stable photocatalyst for hydrogen production, J. Mater. Chem. A 9 (2021) 15076-15086.DOI
  28. [28]A.J. Wright, Q. Wang, C Huang, A. Nieto, R. Chen, J. Luo, From high-entropy ceramics to compositionally-complex ceramics: a case study of fluorite oxides, J. Eur. Ceram. Soc. 40 (2020) 2120-2129.arxiv.org/abs/1912.11742
  29. [29]C. Oses, C. Toher, S. Curtarolo, High-entropy ceramics, Nat. Rev. Mater. 5 (2020) 295-309.DOI
  30. [30]S. Akrami, P. Edalai, M. Fuji, K. Edalati, High-entropy ceramics: review of principles, production and applications, Mater. Sci. Eng. R 146 (2021) 100644.DOI
  31. [31]A. Sarkar, L. Velasco, D.I. Wang, Q. Wang, G. Talasila, L. de Biasi, C. Kübel, T. Brezesinski, S.S. Bhattacharya, H. Hahn, B. Breitung, High entropy oxides for reversible energy storage, Nat. Commun. 9 (2018) 3400.DOI
  32. [32]T.X. Nguyen, J. Patra, J.K. Chang, J.M. Ting, High entropy spinel oxide nanoparticles for superior lithiation–delithiation performance, J. Mater. Chem. 8 (2020) 18963-18973.DOI
  33. [33]Y. Zheng, Y. Yi, M. Fan, H. Liu, X. Li, R. Zhang, M. Li, Z.A. Qiao, A high-entropy metal oxide as chemical anchor of polysulfide for lithium-sulfur batteries, Energy Storage Mater. 23 (2019) 678-683.DOI
  34. [34]G. Fang, J. Gao, J. Lv, H. Jia, H. Li, W. Liu, G. Xie, Z. Chen, Y. Huang, Q. Yuan, X. Liu, Multi-component nanoporous alloy/(oxy) hydroxide for bifunctional oxygen electrocatalysis and rechargeable Zn-air batteries, Appl. Catal. B 268 (2020) 118431.
  35. [35]S. Zhou, Y. Pu, Q. Zhang, R. Shi, X. Guo, W. Wang, J. Ji, T. Wei, T. Ouyang, Microstructure and dielectric properties of high entropy Ba (Zr₀.₂Ti₀.₂Sn₀.₂Hf₀.₂Me₀.₂)O₃ perovskite oxides, Ceram. Int. 46 (2020) 7430-7437.DOI
  36. [36]R. Witte, A. Sarkar, R. Kruk, B. Eggert, R.A. Brand, H. Wende, H. Hahn, High-entropy oxides: An emerging prospect for magnetic rare-earth transition metal perovskites, Phys. Rev. Mater. 3 (2019) 034406.DOI
  37. [37]A.J. Wright, C. Huang, M.J. Walock, A. Ghoshal, M. Murugan, J. Luo, Sand corrosion, thermal expansion, and ablation of medium-and high-entropy compositionally complex fluorite oxides, J. Am. Ceram. Soc. 104 (2021) 448-462.
  38. [38]H. Chen, W. Lin, Z. Zhang, K. Jie, D.R. Mullins, X. Sang, S.Z. Yang, C.J. Jafta, C.A. Bridges, X. Hu, R.R. Unocic, Mechanochemical synthesis of high entropy oxide materials under ambient conditions: dispersion of catalysts via entropy maximization, ACS Mater. Lett. 1 (2019) 83-88.DOI
  39. [39]P. Edalati, Q. Wang, H. Razavi-Khosroshahi, M. Fuji, T. Ishihara, K. Edalati, Photocatalytic hydrogen evolution on a high-entropy oxide, J. Mater. Chem. A 8 (2020) 3814-3821.DOI
  40. [40]P. Edalati, Y. Itagoe, H. Ishihara, T. Ishihara, H. Emami, M. Arita, M. Fuji, K. Edalati, Visible-light photocatalytic oxygen production on a high-entropy oxide with multiple-heterojunction introduction, J. Photochem. Photobio. A 433 (2022) 114167.DOI
  41. [41]S. Akrami, Y. Murakami, M. Watanabe, T. Ishihara, M. Arita, M. Fuji, K. Edalati, Defective high-entropy oxide photocatalyst with high activity for CO₂ conversion, Appl. Catal. B 303 (2022) 120896.DOI
  42. [42]K. Edalati, Z. Horita, A review on high-pressure torsion (HPT) from 1935 to 1988, J. Mater. Sci. Eng. A 652 (2016) 325-352.DOI
  43. [43]K. Edalati, A. Bachmaier, V.A. Beloshenko, Y. Beygelzimer, V.D. Blank, W.J. Botta, K. Bryła, J. Čížek, S. Divinski, N.A. Enikeev, Y. Estrin, G. Faraji, R.B. Figueiredo, M. Fuji, T. Furuta, T. Grosdidier, J. Gubicza, A. Hohenwarter, Z. Horita, J. Huot, Y. Ikoma, M. Janeček, M. Kawasaki, P. Král, S. Kuramoto, T.G. Langdon, D.R. Leiva, V.I. Levitas, A. Mazilkin, M. Mito, H. Miyamoto, T. Nishizaki, R. Pippan, V.V. Popov, E.N. Popova, G. Purcek, O. Renk, Á. Révész, X. Sauvage, V. Sklenicka, W. Skrotzki, B.B. Straumal, S. Suwas, L.S. Toth, N. Tsuji, R.Z. Valiev, G. Wilde, M.J. Zehetbauer, X. Zhu, Nanomaterials by severe plastic deformation: review of historical developments and recent advances, Mater. Res. Lett. 10 (2022) 163-256.DOI
  44. [44]J.P. Couzinié, L. Lilensten, Y. Champion, G. Dirras, L. Perrière, I. Guillot, On the room temperature deformation mechanisms of a TiZrHfNbTa refractory high-entropy alloy, Mater. Sci. Eng. A 645 (2015) 255-263.DOI
  45. [45]O.N. Senkov, J.M. Scott, S.V. Senkova, D.B. Miracle, C.F. Woodward, Microstructure and room temperature properties of a high-entropy TaNbHfZrTi alloy, J. Alloys Compd. 509 (2011) 6043-6048.DOI
  46. [46]A.D. Wadsley, Mixed oxides of titanium and niobium. I., Acta Cryst. 14 (1961) 660-664.
  47. [47]J. Galy, R.S. Roth, The crystal structure of Nb₂Zr₆O₁₇, J. Solid State Chem. 7 (1973) 277-285.DOI
  48. [48]K. Li, B. Peng, T. Peng, Recent advances in heterogeneous photocatalytic CO₂ conversion to solar fuels, ACS Catal. 6 (2016) 7485-7527.DOI
  49. [49]L. Ran, J. Hou, S. Cao, Z. Li, Y. Zhang, Y. Wu, B. Zhang, P. Zhai, L. Sun, Defect engineering of photocatalysts for solar energy conversion, Solar Rrl. 4 (2020) 1900487.
  50. [50]M.R. Hoffmann, S.T. Martin, W. Choi, D.W. Bahnemann, Environmental applications of semiconductor photocatalysis, Chem. Rev. 95 (1995) 69-96.DOI
  51. [51]Z. Zhang, K. Liu, Z. Feng, Y. Bao, B. Dong, Hierarchical sheet-on-sheet ZnIn₂S₄/g-C₃N₄ heterostructure with highly efficient photocatalytic H₂ production based on photoinduced interfacial charge transfer, Sci. Rep. 6 (2016) 19221.DOI
  52. [52]M.C. Wu, C.H. Chen, W.K. Huang, K.C. Hsiao, T.H. Lin, S.H. Chan, P.Y. Wu, C.F. Lu, Y.H. Chang, T.F. Lin, K.H. Hsu, Improved solar-driven photocatalytic performance of highly crystalline hydrogenated TiO₂ nanofibers with core-shell structure, Sci. Rep. 7 (2017) 40896.DOI
  53. [53]K. Fujihara, S. Izumi, T. Ohno, M. Matsumura, Time-resolved photoluminescence of particulate TiO₂ photocatalysts suspended in aqueous solutions, J. Photochem. Photobiol. A 132 (2000) 99-104.
  54. [54]W. Zhao, J. Liu, X. Wang, Y. Huang, H. Zhou, J. Yu, J. Liu, B. Hao, X. Wang, Y. Li, A novel high efficiency polar photocatalyst, Zn (IO₃)₂: synthesis, crystal structure and photocatalytic activity, New J. Chem. 45 (2021) 7844-7849.DOI
  55. [55]C.B. Hiragond, S. Biswas, N.S. Powar, J. Lee, E. Gong, H. Kim, H.S. Kim, J.W. Jung, C.H. Cho, B.M. Wong, S.I. In, Surface-modified Ag@ Ru-P25 for photocatalytic CO₂ conversion with high selectivity over CH₄ formation at the solid–gas interface, Carbon Energy 6 (2024) e386.
  56. [56]K. Edalati, Q. Wang, H. Eguchi, H. Razavi-Khosroshahi, H. Emami, M. Yamauchi, M., Fuji, Z. Horita, Impact of TiO₂-II phase stabilized in anatase matrix by high-pressure torsion on electrocatalytic hydrogen production. Mat. Res. Lett. 2019 (7) 334-339
  57. [57]T.T. Nguyen, K. Edalati, Impact of high-pressure columbite phase of titanium dioxide (TiO₂) on catalytic photoconversion of plastic waste and simultaneous hydrogen (H₂) production, J. Alloys Compd. 1008 (2024) 176722.DOI
  58. [58]M. Katai, P. Edalati, J. Hidalgo-Jimenez, Y. Shundo, T. Akbay, T. Ishihara, M. Arita, M. Fuji, K. Edalati, Black brookite rich in oxygen vacancies as an active photocatalyst for CO₂ conversion: experiments and first-principles calculations, J. Photochem. Photobio. A 449 (2024) 115409.
  59. [59]Y. Shundo, T.T. Nguyen, S. Akrami, P. Edalati, Y. Itagoe, T. Ishihara, M. Arita, Q. Guo, M. Fuji, K. Edalati, Oxygen vacancy-rich high-pressure rocksalt phase of zinc oxide for enhanced photocatalytic hydrogen evolution, J. Colloid Interface Sci. 666 (2024) 22-34.DOI
  60. [60]T.T. Nguyen, K. Edalati, Brookite TiO₂ as an active photocatalyst for photoconversion of plastic wastes to acetic acid and simultaneous hydrogen production: comparison with anatase and rutile, Chemosphere 355 (2024) 141785.DOI
  61. [61]J. Hidalgo-Jiménez, T. Akbay, T. Ishihara, K. Edalati, Understanding high photocatalytic activity of the TiO₂ high-pressure columbite phase by experiments and first-principles calculations, J. Mater. Chem. A 11 (2023) 23523-23535.
  62. [62]S. Chu, B. Zhang, X. Zhao, H.S. Soo, F. Wang, R. Xiao, H. Zhang, Photocatalytic conversion of plastic waste: from photodegradation to photosynthesis, Adv. Energy Mater. 12 (2022) 2200435.DOI
  63. [63]Y. Li, S. Wan, C. Lin, Y. Gao, Y. Lu, L. Wang, K. Zhang, Engineering of 2D/2D MoS₂/CdxZn₁−xS photocatalyst for solar H₂ evolution coupled with degradation of plastic in alkaline solution, Solar Rrl. 5 (2021) 2000427.
  64. [64]K.I. Ishibashi, A. Fujishima, T. Watanabe, K. Hashimoto, Detection of active oxidative species in TiO₂ photocatalysis using the fluorescence technique, Electrochem. Commun. 2 (2000) 207-210.DOI
  65. [65]T.T. Nguyen, K. Edalati, Impact of high-pressure torsion on hydrogen production from photodegradation of polypropylene plastic wastes, Int. J. Hydrog. Energy 81 (2024) 411-417.DOI
  66. [66]A.A. El-Saftawy, A. Elfalaky, M.S. Ragheb, S.G. Zakhary, Electron beam induced surface modifications of PET film, Radiat. Phys. Chem. 102 (2014) 96-102.
  67. [67]B. Cao, S. Wan, Y. Wang, H. Guo, M. Ou, Q. Zhong, Highly-efficient visible-light-driven photocatalytic H₂ evolution integrated with microplastic degradation over MXene/ZnxCd₁−xS photocatalyst, J. Colloid Interface Sci. 605 (2022) 311-319.DOI
  68. [68]M. Du, M. Xing, W. Yuan, L. Zhang, T. Sun, T. Sheng, C. Zhou, Q. Qiu, Upgrading polyethylene terephthalate plastic into commodity chemicals paired with hydrogen evolution over a partially oxidized CuIn₅S₈ nanosheet photocatalyst, Green Chem. 25 (2023) 9818-9825.DOI
  69. [69]S. Guo, Y. Huang, D. Li, Z. Xie, Y. Jia, X. Wu, D. Xu, W. Shi, Visible-light-driven photoreforming of poly (ethylene terephthalate) plastics via carbon nitride porous microtubes, Chem. Commun. 59 (2023) 7791-7794.DOI
  70. [70]R. Li, F. Wang, F. Lv, P. Wang, X. Guo, J. Feng, D. Li, Y. Chen, Simultaneous hydrogen production and conversion of plastic wastes into valued chemicals over a Z-scheme photocatalyst, Int. J. Hydrogen Energy 51 (2024) 406-414.DOI
  71. [71]Y. An, J. Hou, Z. Liu, B. Peng, Enhanced solid-phase photocatalytic degradation of polyethylene by TiO₂–MWCNTs nanocomposites, Mater. Chem. Phys. 148 (2014) 387-394.DOI
  72. [72]M.C. Ariza-Tarazona, J.F. Villarreal-Chiu, J.M. Hernández-López, J.R. De la Rosa, V. Barbieri, C. Siligardi, E.I. Cedillo-González, Microplastic pollution reduction by a carbon and nitrogen-doped TiO₂: Effect of pH and temperature in the photocatalytic degradation process, J. Hazard. Mater. 395 (2020) 122632.
  73. [73]S.M. Lam, J.C. Sin, H. Zeng, H. Lin, H. Li, Y.Y. Chai, M.K. Choong, A.R. Mohamed, Green synthesis of Fe-ZnO nanoparticles with improved sunlight photocatalytic performance for polyethylene film deterioration and bacterial inactivation, Mater. Sci. Semicond. Process. 123 (2021) 105574.DOI
  74. [74]C. Venkataramana, S.M. Botsa, P. Shyamala, R. Muralikrishna, R., Photocatalytic degradation of polyethylene plastics by NiAl₂O₄ spinels-synthesis and characterization, Chemosphere 265 (2021) 129021.DOI
  75. [75]X. u Zhao, Z. Li, Y. Chen, L. Shi, Y. Zhu, Solid-phase photocatalytic degradation of polyethylene plastic under UV and solar light irradiation, J. Mol. Catal. A. Chem. 268 (2007) 101-106.DOI
  76. [76]Y. Zhong, H. Chen, X. Chen, B. Zhang, W. Chen, W. Lu, Abiotic degradation behavior of polyacrylonitrile-based material filled with a composite of TiO₂ and g-C₃N₄ under solar illumination, Chemosphere 299 (2022) 134375.DOI
  77. [77]Y. Zhang, T. Sun, D. Zhang, Z. Shi, X. Zhang, C. Li, L. Wang, J. Song, Q. Lin, Enhanced photodegradability of PVC plastics film by codoping nano-graphite and TiO₂, Polym. Degrad. Stab. 181 (2020) 109332.DOI
  78. [78]I. Nabi, K. Li, H. Cheng, T. Wang, Y. Liu, S. Ajmal, Y. Yang, Y. Feng, L. Zhang, Complete photocatalytic mineralization of microplastic on TiO₂ nanoparticle film, Iscience 23 (2020) 101326.DOI
  79. [79]M.C. Ariza-Tarazona, J.F. Villarreal-Chiu, V. Barbieri, C. Siligardi, E.I. Cedillo-González, New strategy for microplastic degradation: Green photocatalysis using a protein-based porous N-TiO₂ semiconductor. Ceram. Int. 45 (2019) 9618-9624.
  80. [80]J. Hidalgo-Jiménez, T. Akbay, T. Ishihara, K. Edalati, Investigation of a high-entropy oxide photocatalyst for hydrogen generation by first-principles calculations coupled with experiments: significance of electronegativity, Scr. Mater. 250 (2024) 116205.
  81. [81]K. Edalati, A.Q. Ahmed, S. Akrami, K. Ameyama, V. Aptukov, R.N. Asfandiyarov, M. Ashida, V. Astanin, A. Bachmaier, V. Beloshenko, E.V. Bobruk, K. Bryla, J.M. Cabrera, A.P. Carvalho, N.Q. Chinh, I.C. Choi, R. Chulist, J.M. Cubero-Sesin, G. Davdian, M. Demirtas, S. Divinski, K. Durst, J. Dvorak, P. Edalati, S. Emura, N.A. Enikeev, G. Faraji, R.B. Figueiredo, R. Floriano, M. Fouladvind, D. Fruchart, M. Fuji, H. Fujiwara, M. Gajdics, D. Gheorghe, Ł. Gondek, J.E. González-Hernández, A. Gornakova, T. Grosdidier, J. Gubicza, D. Gunderov, L. He, O.F. Higuera, S. Hirosawa, A. Hohenwarter, Z. Horita, J. Horky, Y. Huang, J. Huot, Y. Ikoma, T. Ishihara, Y. Ivanisenko, J.I. Jang, A.M. Jorge Jr. M. Kawabata-Ota, M. Kawasaki, T. Khelfa, J. Kobayashi, L. Kommel, A. Korneva, P. Kral, N. Kudriashova, S. Kuramoto, T.G. Langdon, D.H. Lee, V.I. Levitas, C. Li, H.W. Li, Y. Li, Z. Li, H.J. Lin, K.D. Liss, Y. Liu, D.M. Marulanda Cardona, K. Matsuda, A. Mazilkin, Y. Mine, H. Miyamoto, S.C. Moon, T. Müller, J.A. Muñoz, M.Y. Murashkin, M. Naeem, M. Novelli, D. Olasz, R. Pippan, V.V. Popov, E.N. Popova, G. Purcek, P. de Rango, O. Renk, D. Retrain, Á. Révész, V. Roche, P. Rodriguez-Calvillo, L. Romero-Resendiz, X. Sauvage, T. Sawaguchi, H. Sena, H. Shahmir, X. Shi, V. Sklenicka, W. Skrotzki, N. Skryabina, F. Staab, B. Straumal, Z. Sun, M. Szczerba, Y. Takizawa, Y. Tang, R.Z. Valiev, A. Vozniak, A. Voznyak, B. Wang, J.T. Wang, G. Wilde, F. Zhang, M. Zhang, P. Zhang, J. Zhou, X. Zhu, Y.T. Zhu, Severe plastic deformation for producing superfunctional ultrafine-grained and heterostructured materials: an interdisciplinary review, J. Alloys Compd. 1002 (2024) 174667.

Paper details

vlnc:W_x7c8nyw6
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents