betaFeedback

WorksPhysics and Astronomy

Magnon-phonon coupling of synthetic antiferromagnets in a surface acoustic wave cavity resonator

Abstract

We use a surface acoustic wave (SAW) cavity resonator to study the coupling of acoustic magnons in a synthetic antiferromagnet (SAF) and the phonons carried by SAWs. The SAF is composed of a CoFeB/Ru/CoFeB trilayer and the scattering matrix of the SAW resonator is studied to assess the coupling. We find that the spectral linewidth of the SAW resonator is modulated when the frequency of the excited magnons approaches the SAW resonance frequency. Moreover, the linewidth modulation varies with the magnitude and orientation of the external magnetic field. Such change in the spectral linewidth can be well reproduced using macrospin-like model calculations. From the model analyses, we estimate the magnon-phonon coupling strength to be ∼\sim15.6 MHz at a SAW resonance frequency of 1.8 GHz: the corresponding magnomechanical cooperativity is ∼\sim0.66. As the spectral shape hardly changes in a CoFeB single layer reference sample under the same experimental condition, these results show that SAF provides an ideal platform to study magnon-phonon coupling in a SAW cavity resonator.

The interaction between phonons and magnons in magnetic systems is increasingly attracting interest not only for advancing understanding on the coupling mechanism[1, 2, 3, 4, 5] but also for developing viable quantum technologies[6, 7, 8]. Recent studies have shown that the cooperativity of the magnon-phonon coupled systems, a figure of merit that defines the degree of coupling, can be significantly larger than 1, achieving the necessary condition for the strong coupling[6, 8, 9]. As the magnetostrictive interaction of the magnets is primarily responsible for the magnon-phonon coupling, systems with mechanical degrees of freedom are employed to facilitate the coupling.

Surface acoustic waves (SAWs) are acoustic phonons that propagate on the surface of piezoelectric substrate. SAWs can be excited simply by applying a microwave electric field to an interdigital transducer (IDT) patterned on the substrate. The simple device structure is attracting interest as it allows fabrication of on-chip phononic devices[10]. Moreover, SAWs can propagate distances that exceed a millimeter[11], exemplifying their exceptionally high coherence and small decay rate. SAWs typically generate strains of the order of 10−610^{-6} and can reach 10−410^{-4} under appropriate conditions[11]. Importantly, one can form a SAW cavity resonator by confining the waves in a region surrounded by Bragg reflectors, which are made of metallic electrodes[12, 13, 14, 15]. The quality factor of such SAW cavity resonator can exceed 10410^4 at room temperature[15].

Coherent excitation of magnons using SAWs in a ferromagnetic thin film has been reported since the pioneering work from Weiler et al. [1, 2, 7, 16, 17]. The resonance frequency to excite SAWs, defined by the period of the wires that comprise the IDT, is typically of the order of 1 GHz. In contrast, the frequency of magnons in ferromagnetic thin films is in the range of a few GHz. Previous studies have thus used materials with low magnetization, typically Ni, so that the resonance frequencies of the SAW and magnons match, a requirement for strong coupling. However, even for Ni, the magnon resonance frequency is rather high such that the coupling can be studied only under a small magnetic field, which often causes multi-domain formation that impedes coherent excitation of magnons. (Note that the quality factor of the SAW cavity resonator tends to decrease as the frequency increases[18].)

To overcome this problem, one may use synthetic antiferromagnets (SAF) composed of two antiferromagnetically coupled ferromagnetic layers that are separated by a non-magnetic spacer layer[19]. The frequency to excite magnons in a SAF is typically smaller than that of its single layer counterpart (see Figure 1(b))[20, 21], which in turn requires larger magnetic field to meet the condition of simultaneously exciting magnons and SAW. Thus SAF will enable exploration of materials with large saturation magnetization, some of which possess small magnetic damping, and allow better control of the magnon-phonon coupling that would have been otherwise difficult in a single layer film.

Schematic illustration of the study and device structure

Figure 1. (a) Schematic illustration of the study. A synthetic antiferromagnet (SAF) is placed on the delay line of the SAW cavity resonator that is composed of the interdigital transducers and Bragg reflectors. SAW phonons in the cavity interact with acoustic magnons of the SAF. Phonon-magnon coupling is obtained by measuring the change in the SAW transmission spectra when the magnetic field magnitude and angle are varied. (b) Calculated magnon resonance frequency plotted as a function of in-plane magnetic field for a single layer film and a SAF. The horizontal dashed line represents the SAW resonance frequency used in the experiments. (c) Illustration of the device geometry. The design of the SAW cavity resonator is as follows: L=692 μmL = 692\ \mu\mathrm{m}, d1=618 μmd_1 = 618\ \mu\mathrm{m}, d2=37 μmd_2 = 37\ \mu\mathrm{m}, d3=2 μmd_3 = 2\ \mu\mathrm{m}, d4=800 μmd_4 = 800\ \mu\mathrm{m}, p=1 μmp = 1\ \mu\mathrm{m}, w=100 μmw = 100\ \mu\mathrm{m}, l=600 μml = 600\ \mu\mathrm{m}, and l′=695 μml' = 695\ \mu\mathrm{m}. The xx-axis is parallel to SAW delay line and the film normal points along the zz-axis. The relative angle between the xx-axis and the external field is defined as φH\varphi_H. (d) An exemplary transmission spectrum of the SAW cavity resonator. The red arrow indicates the spectrum for which the results on the magnetic field dependence are presented in Figure 2 and Figure 3. (d) Quality factor of the SAW transmission peaks as a function of the SAW resonance frequency ωa/2π\omega_a/2\pi.

Here we study the magnon-phonon coupling in a SAF composed of a CoFeB/Ru/CoFeB trilayer[22, 23, 24] and a CoFeB single layer film, where the latter serves as a reference. We use a SAW cavity resonator to assess the coupling constant by extending the evaluation method previously developed[17]. We find that the spectral linewidth of the resonator is significantly modified only when acoustic magnons of SAF is excited; little change is found for the single layer film. The coupling constant, determined from the difference in the spectral linewidth with and without the magnon excitation, is ∼15.6 MHz. As the change in the resonator spectra can be accounted for quantitatively using model calculations, these results show that SAF can be used as a platform to study the coupling of magnons and phonons for on-chip cavity magnomechanics.

Concept of this study and a schematic illustration of the device structure (SAW cavity with a trilayer SAF) are shown in Figure 1(a). A pair of IDTs and Bragg reflectors composed of Ti(5)/Au(30) are fabricated on a piezoelectric Y+128°-cut LiNbO3_3 substrate using a standard liftoff process that involves electron-beam lithography and vapor deposition. The numbers in the parentheses show the layer thickness in nanometers. Both widths and intervals of the wires in the IDTs and the Bragg reflectors are set to 500 nm. A second liftoff process is employed to form a multilayer structure made of Ta(3)/Ru(3)/CoFeB(5)/Ru(tRut_{\mathrm{Ru}})/CoFeB(5)/Ru(3) with tRu=0.53t_{\mathrm{Ru}} = 0.53 nm on the delay line (i.e. the path between the two IDTs) of the SAW cavity. A single magnetic layer film made of 10 nm thick CoFeB (tRu=0t_{\mathrm{Ru}} = 0 nm in the film stacking) is made for comparison. RF magnetron sputtering is used to deposit the film and photolithography is used to pattern the device. Details of the device structure are described in Figure 1(c).

The IDTs are connected to a vector network analyzer (VNA), which is used to carry out scattering matrix measurements of the device. SijS_{ij} with i≠ji \ne j (i=ji = j) represents the signal transmission (reflection) amplitude from port jj to port ii of the VNA (i,j=1,2i,j = 1,2). An in-plane external magnetic field is applied during the scattering matrix measurements to change the magnetization direction of the CoFeB layer. The relative angle between the magnetic field and the xx-axis (parallel to the SAW propagation direction) is defined as φH\varphi_H, as shown in the Figure 1(c). All measurements are performed at room temperature.

Figure 1(d) shows an exemplary ∣S21∣\lvert S_{21}\rvert spectrum obtained from the scattering matrix measurements. We find multiple peaks within the frequency range of 1.8 to 1.85 GHz. Due to the SAW confinement within the cavity, the fundamental mode is split into the eigenmodes of the cavity. Using multi-peak fitting, we determine the acoustic resonance frequency ωa/2π\omega_a/2\pi, the acoustic damping κa/2π\kappa_a/2\pi (half width of half value) and the amplitude AaA_a of each peak. The following formula is used to fit the data:

∣S21∣2=∑aAa1+(ω−ωa2κa)2+const.,(1)\lvert S_{21}\rvert^2 = \sum_a \frac{A_a}{1+\left(\frac{\omega-\omega_a}{2\kappa_a}\right)^2} + \mathrm{const.}, \tag*{(1)}

where aa runs over all the peaks observed in the ∣S21∣\lvert S_{21}\rvert spectrum. We define the quality factor of each peak as Q=ωa2κaQ = \frac{\omega_a}{2\kappa_a}. As shown in Figure 1(e), the quality factor of all peaks are larger than 10310^3. Such large quality factor ensures that the SAWs are effectively enclosed inside the cavity.

We next show the change in the shape of the ∣S21∣\lvert S_{21}\rvert spectrum under application of external magnetic field for the single CoFeB layer film and the SAF. Figure 2(a) shows a contour plot of ∣S21∣2\lvert S_{21}\rvert^2 plotted as a function of the external magnetic field HextH_{\mathrm{ext}} and the SAW excitation frequency for the single CoFeB layer film. The magnetic field is applied along φH=0∘\varphi_H = 0^\circ. Here we show a contour plot of one of the multiple peaks found in the ∣S21∣2|S_{21}|^2 spectrum. The color contrast represents the SAW transmission amplitude. Near μ0Hext=0\mu_0H_{\mathrm{ext}} = 0, small changes in the color contrast are found. To show this more explicitly, line profiles of the spectrum along fixed HextH_{\mathrm{ext}} (μ0Hext=−3.4\mu_0H_{\mathrm{ext}} = -3.4 mT, 48.8 mT) are presented in Figure 2(b). As evident, the peak amplitude is slightly reduced when μ0Hext=−3.4\mu_0H_{\mathrm{ext}} = -3.4 mT compared to that of μ0Hext=48.8\mu_0H_{\mathrm{ext}} = 48.8 mT.

Contour plots and frequency dependence of $|S_{21}|^2$ for CoFeB single layer film and SAF

Figure 2. (a,c) Contour plot of ∣S21∣2|S_{21}|^2 as a function of the frequency and magnetic field measured for the CoFeB single layer film with φH=0∘\varphi_H = 0^\circ (a) and the SAF with φH=60∘\varphi_H = 60^\circ (c). (b,d) The frequency dependence of ∣S21∣2|S_{21}|^2 obtained under constant μ0Hext\mu_0H_{\mathrm{ext}} for CoFeB single layer film (b) and SAF (d).

We have varied the magnetic field angle φH\varphi_H and obtained similar contour plots as shown in Figure 2(a). For the CoFeB single layer film, we found notable change in ∣S21∣2|S_{21}|^2 only when φH=0∘\varphi_H = 0^\circ and 180∘180^\circ, and the changes are small. In contrast, significant variation in ∣S21∣2|S_{21}|^2 with HextH_{\mathrm{ext}} were found for the SAF film. The largest change was observed when the field angle was set to φH=60∘\varphi_H = 60^\circ: the results are presented in Figure 2(c). Line profiles along fixed HextH_{\mathrm{ext}} are shown in Figure 2(d). Here we show plots along μ0Hext=16.7\mu_0H_{\mathrm{ext}} = 16.7 mT and −41.6-41.6 mT. Comparing the two plots, one finds not only the peak amplitude drops but also the peak frequency shifts and the linewidth broadens when μ0Hext=16.7\mu_0H_{\mathrm{ext}} = 16.7 mT compared to those of μ0Hext=−41.6\mu_0H_{\mathrm{ext}} = -41.6 mT. Hereafter, we focus on the results of the SAF and discuss the results on the CoFeB single layer film later.

Figure 3(a) shows the HextH_{\mathrm{ext}} dependence of AaA_a, ωa/2π\omega_a/2\pi and κa/2π\kappa_a/2\pi extracted from fitting the experimental results of the SAF (Figure 2(c)) with Eq. (1). As evident, AaA_a takes a minimum at μ0Hext=16.7\mu_0H_{\mathrm{ext}} = 16.7 mT, suggesting that a fraction of the SAW power is absorbed. ωa/2π\omega_a/2\pi shows a significant change around μ0Hext=16.7\mu_0H_{\mathrm{ext}} = 16.7 mT while

κa/2π\kappa_a/2\pi takes a maximum. Numerical calculations are performed to quantitatively account for these results. The Landau–Lifshitz–Gilbert (LLG) equation and the elastic wave equation[2, 17, 25] are used to study the change in AaA_a, ωa\omega_a and κa\kappa_a with HextH_{\mathrm{ext}}: see the Supplementary materials for the details. Material parameters for the system are obtained from the experiments and the literature. The calculation results are summarized in Figure 3(b). Overall, we find the model calculations can account for the experimental results well. From the calculations, we find that μ0Hext=16.7\mu_0H_{\mathrm{ext}} = 16.7 mT is the resonance field, denoted as HresH_{\mathrm{res}} hereafter, of the acoustic magnons in the SAF under an excitation frequency of 1.828 GHz and a field angle of φH=60∘\varphi_H = 60^\circ. (The resonance frequency of the optical magnons at the same field is ∼10.5\sim10.5 GHz.) At this condition, the amplitude of the excited magnons becomes large such that they counteract on the SAW via the magnetostrictive coupling, causing the change in the SAW resonance frequency and linewidth around HresH_{\mathrm{res}}. Such back action are often observed in coupled oscillator systems[17, 25, 26]. For large ∣Hext∣|H_{\mathrm{ext}}|, the acoustic magnons are not excited (off-resonance condition) and thus the SAW transmission properties hardly change.

Experimental and calculated field dependence of SAW transmission parameters

Figure 3. The HextH_{\mathrm{ext}} dependence of the ∣S21∣2|S_{21}|^2 transmission amplitude AaA_a (upper), the peak frequency ωa/2π\omega_a/2\pi (center) and the linewidth κa/2π\kappa_a/2\pi when the magnetic field is applied along φH=60∘\varphi_H = 60^\circ. (a) experimental results, (b) calculations.

We estimate the strength of the magnon-phonon coupling using the change in κa\kappa_a with HextH_{\mathrm{ext}}. The coupled equations of motion of magnetization and the longitudinal stress associated with the SAW are linearized and Fourier transformed, from which we obtain the longitudinal stress amplitude Exx\mathcal{E}_{xx}:

Exx≈F0−2ωa0(ω−ωa0−Re⁡[χam]2ωa0)+i2ω(κa0+Im⁡[χam]2ω)(2)\mathcal{E}_{xx} \approx\frac{\mathcal{F}_0}{-2\omega_a^0\left(\omega-\omega_a^0-\frac{\operatorname{Re}[\chi_{\mathrm{am}}]}{2\omega_a^0}\right)+i2\omega\left(\kappa_a^0+\frac{\operatorname{Im}[\chi_{\mathrm{am}}]}{2\omega}\right)} \tag*{(2)}

where F0\mathcal{F}_0 is the excitation amplitude of the SAW, ω\omega and ωa0\omega_a^0 are the SAW excitation and resonance angular frequency, κa0\kappa_a^0 is the SAW decay rate. Note that ωa0\omega_a^0 and κa0\kappa_a^0 represent quantities without the influence of magnon-phonon coupling. χam\chi_{\mathrm{am}} is defined as

χam≡i2ωa0gi(ω−ωm)+κm,(3)\chi_{\mathrm{am}} \equiv\frac{i2\omega_a^0 g}{i(\omega-\omega_m)+\kappa_m}, \tag*{(3)}

where gg is the magnon-phonon coupling constant, ωm\omega_m and κm\kappa_m are the resonance angular frequency and damping constant of the magnetization. (2) shows that Exx\mathcal{E}_{xx} takes the form of a Lorentzian, consistent with the observed spectra shown in Figure 2(b,Figure 2d) and Eq. (1). The peak position and the linewidth of the Lorentzian in Eq. (2), defined as ωa\omega_a and κa\kappa_a, respectively, are modified under the influence of magnon-phonon coupling. ωa\omega_a and κa\kappa_a read

ωa=ωa0+Re⁡[χam]2ω≈ωa0+g(ωa0−ωm)(ωa0−ωm)2+κm2,κa=κa0+Im⁡[χam]2ω≈κa0+gκm(ωa0−ωm)2+κm2.(4)\begin{aligned} \omega_a &= \omega_a^0+\frac{\operatorname{Re}[\chi_{\mathrm{am}}]}{2\omega}\approx\omega_a^0+\frac{g(\omega_a^0-\omega_m)}{(\omega_a^0-\omega_m)^2+\kappa_m^2},\\ \kappa_a &= \kappa_a^0+\frac{\operatorname{Im}[\chi_{\mathrm{am}}]}{2\omega}\approx\kappa_a^0+\frac{g\kappa_m}{(\omega_a^0-\omega_m)^2+\kappa_m^2}. \tag*{(4)} \end{aligned}

where we have substituted ω≈ωa0\omega\approx\omega_a^0 after the nearly equal symbol, the condition set in experiments. We note that Eq. (4) is consistent with the results shown in Figure 3. That is, ωa\omega_a and κa\kappa_a are, respectively, antisymmetric and symmetric functions of HextH_{\mathrm{ext}} with respect to HresH_{\mathrm{res}}. This can be understood if one replaces ωm\omega_m and ωa0\omega_a^0 with HextH_{\mathrm{ext}} and HresH_{\mathrm{res}} in Eq. (4), which is justified since ωm\omega_m scales with HextH_{\mathrm{ext}} (see e.g. Figure 1(b)).

To determine gg, we study the difference in the linewidth κa\kappa_a when the magnon frequency ωm/(2π)\omega_m/(2\pi), defined by HextH_{\mathrm{ext}}, is either set close to the SAW resonance frequency ωa/(2π)\omega_a/(2\pi) or set far from it. The linewidth of the former is defined as κares\kappa_a^{\mathrm{res}} while that for the latter is equal to κa0\kappa_a^0. From the magnetic field dependence of κa\kappa_a shown in Figure 3, we extract κares\kappa_a^{\mathrm{res}} and κa0\kappa_a^0. The latter is obtained by taking the average κa\kappa_a at large HextH_{\mathrm{ext}} where the magnon-phonon coupling is suppressed. We determine κares\kappa_a^{\mathrm{res}} and κa0\kappa_a^0 for all the peaks associated with the cavity eigenmodes shown in Figure 1(c). Values of κares\kappa_a^{\mathrm{res}} are plotted against κa0\kappa_a^0 in Figure 4(a) with the blue circles. As evident, κares\kappa_a^{\mathrm{res}} linearly scales with κa0\kappa_a^0.

Dependence of resonance linewidth and cooperativity on acoustic linewidth and magnetic-field angle

Figure 4. (a) The κares\kappa_a^{\mathrm{res}} dependence on κa0\kappa_a^0 in the SAF when φH=60∘\varphi_H=60^\circ. The blue circles and the black solid line show experimental results and linear fit to the data, respectively. The intercept of the linear line is equal to cooperativity parameter CC. The slope of the linear line is fixed to 1. (b) The φH\varphi_H dependence of CC for the SAF.

To account for these results, we substitute the relation ∣ωa0−ωm∣≪κm\lvert\omega_a^0-\omega_m\rvert\ll\kappa_m, which applies to the system under investigation, into the second line of Eq. (4) to obtain

κares≈κa0(1+C),(5)\kappa_a^{\mathrm{res}}\approx\kappa_a^0(1+C), \tag*{(5)}

where CC is the cooperativity defined as

C≡g2κa0κm.(6)C\equiv\frac{g^2}{\kappa_a^0\kappa_m}. \tag*{(6)}

(5) shows the linear relation of κares\kappa_a^{\mathrm{res}} with κa0\kappa_a^0, consistent with the experiments. We fit a linear function to the data presented in Figure 4(a) with the slope fixed to 1. According to Eqs. (5) and (6), the yy-axis intercept of the linear fit gives g2/κmg^2/\kappa_m, from which we find g2/(2πκm)g^2/(2\pi\kappa_m)

=0.375±0.006=0.375\pm0.006 MHz. With κa0/(2π)=0.570\kappa_a^0/(2\pi)=0.570 MHz (the average value obtained from all experiments), we obtain C=0.66C=0.66 from Eq. (6).

The magnetic field orientation dependence of the cooperativity CC is shown in Figure 4(b). CC takes a maximum at φH=60∘\varphi_H=60^\circ and 120∘120^\circ. Note that the magneto-elastic coupling is the largest when the relative angle between the magnetization and the strain (here it is parallel to the SAW propagation, i.e. along the xx-axis) is 45∘45^\circ and 135∘135^\circ. The results shown in Figure 4(b) thus suggest that a non-zero magnetic anisotropy is present and influences the angular dependence of CC. To confirm this, the field angle dependence of the cooperativity is numerically calculated assuming an uniaxial magnetic anisotropy along the yy-axis. The results are shown by the red solid line in Figure 4(b). The calculations are in good agreement with the experimental results. The uniaxial magnetic anisotropy field of CoFeB is largely caused by the shape anisotropy: see Figure 1(c).

Finally, we determine the magnon-phonon coupling constant gg using the maximum CC found in Figure 4(a), which we denote as Cmax⁡C_{\max}. In order to estimate gg using Eq. (6), one must find the value of κm\kappa_m. We use the relation κm≈2παγMs\kappa_m\approx2\pi\alpha\gamma M_s [25] to obtain κm/2π=651\kappa_m/2\pi=651 MHz from the material parameters used in fitting the data presented in Figure 3 and Figure 4. Substituting κm\kappa_m, κa0\kappa_a^0 and Cmax⁡(=0.66)C_{\max}(=0.66) into Eq. (6), we obtain g/2π∼15.6g/2\pi\sim15.6 MHz. This is similar to the value of gg reported previously for a Ni single layer film (g/(2π)∼9.9g/(2\pi)\sim9.9 MHz), despite the difference in the product of the magneto-elastic coupling constant bb and saturation magnetization MsM_s that defines the magnitude of gg. Using reported material parameters, the calculated value of MsbM_sb is larger for Ni than CoFeB, which cannot account for the values of gg found in the experiments.

Here we discuss the difference in the coupling constant gg for a single layer film and a SAF. In Figure 1(b), we show the calculated magnon resonance frequency as a function of an in-plane external magnetic field for a CoFeB single layer film and the CoFeB/Ru/CoFeB SAF. Details of the calculations are presented in the supplementary material. The horizontal dashed line shows the SAW resonance frequency. For the single layer film, the magnetic field at which the magnon and the SAW resonance frequencies match is close to zero. Under such condition, multidomain formation and magnetization switching of domains can occur and impede coherent magnon excitation. This is corroborated by the fact that little change is found in the SAW resonance frequency and linewidth in the CoFeB single layer film (Figure 2(a,Figure 2b)). As we do not observe any signal that can be attributed to magnon excitation when the external field is oriented along φH∼45±90n\varphi_H \sim45 \pm90n deg (nn: integer) where the magneto-elastic coupling is the strongest, we infer that the SAW cannot efficiently excite magnons under the experimental condition for the CoFeB single layer film.

In contrast, the resonance frequency of acoustic magnons of SAF is reduced compared to the single layer film: see Figure 1(b). As a consequence, the magnetic field at which the acoustic magnon and SAW resonance frequencies coincide becomes sufficiently large such that multidomain formation and domain switching are suppressed. The fact that the magnetic field dependence of the spectral parameters (Figure 3) and the field angle dependence of the cooperativity (Figure 4(b)) can be well reproduced using model calculations[25] demonstrate that SAF provides an ideal platform to study magnon-phonon coupling.

In summary, we have studied the magnon-phonon coupling in a CoFeB/Ru/CoFeB tri-layer SAF and a CoFeB single layer film using a surface acoustic wave cavity resonator. The cavity resonator exhibits a quality factor that exceeds ∼103\sim10^3, providing strong confinement of the SAWs. The SAW transmission spectra are measured under application of an in-plane magnetic field. For the SAF, the SAW spectrum of the cavity eigenmodes exhibits reduction in amplitude as well as frequency shift and linewidth broadening at the resonance field of the acoustic magnons. Interestingly, such changes in the SAW spectra are hardly found for a CoFeB single layer film. We infer the difference is due to the difference in the magnon resonance field. The resonance field is close to zero for the single layer film, where multidomain structures can form to impede excitation of coherent magnons. In contrast, the resonance field for the SAF is sufficiently large to allow efficient coupling of SAW and the acoustic magnons. From the change in the linewidth of the SAW transmission peak, we estimate the coupling constant gg of the acoustic magnons and the SAW phonons to be ∼15.6\sim15.6 MHz. The corresponding magnonomechanical cooperativity parameter CC is ∼0.66\sim0.66. These results thus show that SAF can be used as an effective media for magnon-phonon coupling and provide a playground for on-chip cavity magnomechanics.

Acknowledgements

We are grateful to R. Hisatomi, T. Taniguchi, S. Nakatsuji, H. Yamaguchi and H. Okamoto for fruitful discussion. This work was partly supported by JSPS KAKENHI (Grant Number 20J20952, 20J21915, 23KJ1419, 23H05463) from JSPS, JSR Fellowship from the University of Tokyo, MEXT Initiative to Establish Next-generation Novel Integrated Circuits Centers (X-NICS).

References

  1. [1]M. Weiler, L. Dreher, C. Heeg, H. Huebl, R. Gross, M. S. Brandt, and S. T. B. Goennenwein, Elastically driven ferromagnetic resonance in nickel thin films, Phys. Rev. Lett. 106, 117601 (2011).
  2. [2]L. Dreher, M. Weiler, M. Pernpeintner, H. Huebl, R. Gross, M. S. Brandt, and S. T. B. Goennenwein, Surface acoustic wave driven ferromagnetic resonance in nickel thin films: Theory and experiment, Phys. Rev. B 86, 134415 (2012).DOI
  3. [3]L. Thevenard, C. Gourdain, J. Y. Prieur, H. J. von Bardeleben, S. Vincent, L. Becerra, L. Largeau, and J. Y. Duquesne, Surface-acoustic-wave-driven ferromagnetic resonance in (ga,mn)(as,p) epilayers, Phys. Rev. B 90, 094401 (2014).DOI
  4. [4]P. G. Gowtham, T. Moriyama, D. C. Ralph, and R. A. Buhrman, Traveling surface spin-wave resonance spectroscopy using surface acoustic waves, J. Appl. Phys. 118, 233910 (2015).DOI
  5. [5]K. An, A. N. Litvinenko, R. Kohno, A. A. Fuad, V. V. Naletov, L. Vila, U. Ebels, G. de Loubens, H. Hurdequint, N. Beaulieu, J. Youssef, N. Vukadinovic, G. E. W. Bauer, A. N. Slavin, V. S. Tiberkevich, and O. Klein, Coherent long-range transfer of angular momentum between magnon kittel modes by phonons, Phys. Rev. B 101, 060407 (2020).DOI
  6. [6]C. Berk, M. Jaris, W. G. Yang, S. Dhuey, S. Cabrini, and H. Schmidt, Strongly coupled magnon-phonon dynamics in a single nanomagnet, Nat. Commun. 10, 2652 (2019).DOI
  7. [7]Y. Li, C. B. Zhao, W. Zhang, A. Hoffmann, and V. Novosad, Advances in coherent coupling between magnons and acoustic phonons, APL Mater. 9, 066902 (2021).DOI
  8. [8]T. Hioki, Y. Hashimoto, and E. Saitoh, Coherent oscillation between phonons and magnons, Comm. Phys. 5, 115 (2022).DOI
  9. [9]X. F. Zhang, C. L. Zou, L. Jiang, and H. X. Tang, Cavity magnomechanics, Sci. Adv. 2, e1501286 (2016).DOI
  10. [10]P. Delsing, A. N. Cleland, M. J. A. Schuetz, J. Knoerzer, G. Giedke, J. I. Cirac, K. Srinivasan, M. Wu, K. C. Balram, C. Bauerle, T. Meunier, C. J. B. Ford, P. V. Santos, E. Cerda-Mendez, H. Wang, H. J. Krenner, E. D. S. Nysten, M. Weiss, G. R. Nash, L. Thevenard, C. Gourdain, P. Rovillain, M. Marangolo, J.-Y. Duquesne, G. Fischerauer, W. Ruile, A. Reiner, B. Paschke, D. Denysenkov, D. Volkmer, A. Wixforth, H. Bruus, M. Wiklund, J. Reboud, J. M. Cooper, Y. Fu, M. S. Brugger, F. Rehfeldt, and C. Westerhausen, The 2019 surface acoustic waves roadmap, J. Phys. D-Appl. Phys. 52, 353001 (2019).
  11. [11]B. Casals, N. Statuto, M. Foerster, A. Hernandez-Minguez, R. Cichelero, P. Manshausen, A. Mandziak, L. Aballe, J. M. Hernandez, and F. Macia, Generation and imaging of magnetoacoustic waves over millimeter distances, Phys. Rev. Lett. 124, 137202 (2020).DOI
  12. [12]D. T. Bell and R. C. M. Li, Surface-acoustic-wave resonators, Proc. IEEE 64, 711 (1976).DOI
  13. [13]R. Manenti, M. J. Peter, A. Nersisyan, E. B. Magnusson, A. Patterson, and P. J. Leek, Surface acoustic wave resonators in the quantum regime, Phys. Rev. B 93, 041411(r) (2016).DOI
  14. [14]A. N. Bolgar, J. I. Zotova, D. D. Kirichenko, I. S. Besedin, A. V. Semenov, R. S. Shaikhidarov, and O. V. Astafiev, Quantum regime of a two-dimensional phonon cavity, Phys. Rev. Lett. 120, 223603 (2018).DOI
  15. [15]L. B. Shao, S. Maity, L. Zheng, L. Wu, A. Shams-Ansari, Y. I. Sohn, E. Pumar, M. N. Gadalla, M. A. Zhang, C. Wang, E. Hu, K. J. Lai, and M. Loncar, Phononic band structure engineering for high-q gigahertz surface acoustic wave resonators on lithium niobate, Phys. Rev. Appl. 12, 014022 (2019).DOI
  16. [16]R. Sasaki, Y. Nii, and Y. Onose, Magnetization control by angular momentum transfer from surface acoustic wave to ferromagnetic spin moments, Nat. Commun. 12, 2599 (2021).DOI
  17. [17]D. Hatanaka, M. Asano, H. Okamoto, Y. Kunihashi, H. Sanada, and H. Yamaguchi, On-chip coherent transduction between magnons and acoustic phonons in cavity magnonmechanics, Phys. Rev. Appl. 17, 034024 (2022).DOI
  18. [18]A. H. Safavi-Naeini, D. V. Thourhout, R. Baets, and R. V. Laer, Controlling phonons and photons at the wavelength scale: integrated photonics meets integrated phononics, Optica 6, 213 (2019).
  19. [19]S. S. P. Parkin, N. More, and K. P. Roche, Oscillations in exchange coupling and magnetoresistance in metallic superlattice structures - co/ru, co/cr, and fe/cr, Phys. Rev. Lett. 64, 2304 (1990).pubmed.ncbi.nlm.nih.gov/10041640
  20. [20]A. Kamimaki, S. Iihama, K. Z. Suzuki, N. Yoshinaga, and S. Mizukami, Parametric amplification of magnons in synthetic antiferromagnets, Phys. Rev. Appl. 13, 044036 (2020).DOI
  21. [21]Y. Shiota, T. Taniguchi, M. Ishibashi, T. Moriyama, and T. Ono, Tunable magnon-magnon coupling mediated by dynamic dipolar interaction in synthetic antiferromagnets, Phys. Rev. Lett. 125, 017203 (2020).DOI
  22. [22]M. Ishibashi, Y. Shiota, T. Li, S. Funada, T. Moriyama, and T. Ono, Switchable giant nonreciprocal frequency shift of propagating spin waves in synthetic antiferromagnets, Science Advances 6, eaez6931 (2020).DOI
  23. [23]H. Matsumoto, T. Kawada, M. Ishibashi, M. Kawaguchi, and M. Hayashi, Large surface acoustic wave nonreciprocity in synthetic antiferromagnets, Appl. Phys. Express 15, 063003 (2022).DOI
  24. [24]M. Kuss, M. Hassan, Y. Kunz, A. Hoerner, M. Weiler, and M. Albrecht, Nonreciprocal magnetoacoustic waves in synthetic antiferromagnets with dzyaloshinskii-moriya interaction, Phys. Rev. B 107, 024424 (2023).DOI
  25. [25]M. Asano, H. Matsumoto, M. Hayashi, and D. Hatanaka, Cavity magnomechanical coupling with coupled magnon modes in a synthetic antiferromagnet, Phys. Rev. B 108, 064415 (2023).DOI
  26. [26]C. A. Potts, E. Varga, V. Bittencourt, S. V. Kuminsk y, and J. P. Davis, Dynamical backaction magnomechanics, Phys. Rev. X 11, 031053 (2021).

Paper details

vlnc:W_xehtn2gc
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents