betaFeedback

WorksPhysics and Astronomy

How to Report and Benchmark Emerging Field-Effect Transistors

Abstract

Emerging low-dimensional nanomaterials have been studied for decades in device applications as field-effect transistors (FETs). However, properly reporting and comparing device performance has been challenging due to the involvement and interlinking of multiple device parameters. More importantly, the interdisciplinarity of this research community results in a lack of consistent reporting and benchmarking guidelines. Here we report a consensus among the authors regarding guidelines for reporting and benchmarking important FET parameters and performance metrics. We provide an example of this reporting and benchmarking process for a two-dimensional (2D) semiconductor FET. Our consensus will help promote an improved approach for assessing device performance in emerging FETs, thus aiding the field to progress more consistently and meaningfully.

Research into field-effect transistors (FETs) based on emerging nanomaterials, including carbon nanotubes[1, 2], graphene[3], phosphorene[4], silicene[5], tellurene[6], transition metal dichalcogenides[7, 8, 9], organic semiconductors[10, 11] and ultrathin metal oxides[12], is thriving. Such studies allow the fundamental properties of the materials to be explored, and may lead to the development of various commercial applications; however, effectively and uniformly assessing the performance of emergent FETs is difficult due to the dependence of performance metrics on unique aspects of the device structure (Figure 1a)[13].

Basic device structure and electrical characteristics

Figure 1. Basic device structure and electrical characteristics. a, Diagram of a typical nanomaterial-based n-type FET highlighting the structure parameters and electric fields. b, Subthreshold and c, transfer (IDI_{\mathrm{D}}-VGSV_{\mathrm{GS}}) curves of an n-type FET under different VDSV_{\mathrm{DS}} voltages. Representative curves are shown for single-sweep in (b), but forward- and backward-sweeps of VGSV_{\mathrm{GS}} should be collected to determine hysteresis, as shown in (c). The gate leakage current is also shown in (b). d, Output (IDI_{\mathrm{D}}-VDSV_{\mathrm{DS}}) curves of the device with three main operation regimes labelled.[14] VGSV_{\mathrm{GS}} is swept from low to high in steps of ΔVGS\Delta V_{\mathrm{GS}}. vsatv_{\mathrm{sat}} is the saturation velocity of carriers in the channel material. IsatI_{\mathrm{sat}} scales as VOV2V_{\mathrm{OV}}^2 in the classical pinch-off regime, but only linearly with VOVV_{\mathrm{OV}} when the velocity saturates. Self-heating could render this increase even sub-linear.[14, 15] Note, VDDV_{\mathrm{DD}} is the supply voltage for the transistor (i.e., the target maximum voltage of operation for both VDSV_{\mathrm{DS}} and VGSV_{\mathrm{GS}}).

Structural parameters that influence device performance include channel (LchL_{\mathrm{ch}}) and contact lengths (LcL_{\mathrm{c}}), gate insulator thickness (tinst_{\mathrm{ins}}) and permittivity (ϵins\epsilon_{\mathrm{ins}}), contact metal types, the thickness of channel material (tcht_{\mathrm{ch}}), and gating scheme (e.g., top, bottom, gate-all-around, multi-channel). Performance metrics include on-current (IonI_{\mathrm{on}}), off-current (IoffI_{\mathrm{off}}), Ion/IoffI_{\mathrm{on}}/I_{\mathrm{off}} ratio, contact resistance (RcR_{\mathrm{c}}), transconductance (gmg_{\mathrm{m}}), subthreshold swing (SSSS), channel mobilities, and drain-induced barrier lowering (DIBL). While different studies reported in the literature often include some of these benchmarking figures, they struggle to capture the myriad variables, making comparisons inaccurate or even biased at times. In addition, the emerging device community consists of researchers from disparate disciplines — including electrical engineering, chemistry, materials science, and physics — which also makes consistent reporting and benchmarking challenging. In this Perspective, we examine the challenges involved in assessing the operation and performance of FETs based on emerging materials, and provide guidelines on how to report and benchmark the devices.

A full list of affiliations appears at the end of the paper.

Field-effect transistor structure and key parameters

In a FET, the structural parameters determine the electric fields and the eventual device performance (Figure 1a). Subthreshold, transfer, and output characteristics in Figure 1b-Figure 1d are the most common II-VV (current-voltage) curves to capture the device performance. Plotting the log of the drain current (IDI_{\mathrm{D}}) as a function of gate-source voltage (VGSV_{\mathrm{GS}}) highlights the subthreshold (i.e., off-state) device behaviour. In contrast, transfer characteristics plot IDI_{\mathrm{D}} vs. VGSV_{\mathrm{GS}} on a linear scale and emphasize the device behaviour after VGSV_{\mathrm{GS}} exceeds the threshold voltage (VTV_{\mathrm{T}}), where the device is in the on-state. Ideally, the gate leakage current (IGI_{\mathrm{G}}) vs. VGSV_{\mathrm{GS}} should be plotted on the subthreshold plot as well.

The IDI_{\mathrm{D}}-VGSV_{\mathrm{GS}} sweeps in Figure 1b-Figure 1c should be conducted at both “small” and “high” drain-source voltage (VDSV_{\mathrm{DS}}) values to characterize the device operation in both linear and saturation regimes. We note that the “small” VDSV_{\mathrm{DS}} value should be sufficiently small to ensure linear regime operation, but greater than ∼2kBT\sim2k_{\mathrm{B}}T (where kBk_{\mathrm{B}} is the Boltzmann constant and TT is the absolute temperature, i.e., ∼50\sim50 mV at room temperature) to ensure that the subthreshold behaviour, and here in particular DIBL (∂VT/∂VDS\partial V_{\mathrm{T}}/\partial V_{\mathrm{DS}}), is not misinterpreted due to thermal injection of carriers from the drain. These curves enable easy extraction of DIBL to demonstrate how VDSV_{\mathrm{DS}} impacts VTV_{\mathrm{T}}. The transfer characteristics should be acquired with forward and backward sweeps, checking for the presence of any hysteresis due to charge trapping[16]. When comparing hysteresis from different devices, the precise measurement conditions such as sweep rates, hold times, and maximum bias voltages should be listed as these parameters influence hysteresis. If hysteresis exists, it should be accounted for in the analysis of VTV_{\mathrm{T}} uncertainty and other device parameters that depend on VTV_{\mathrm{T}}.

In the output characteristics (Figure 1d), three main operation regimes are highlighted. The linear regime is characterized by the linear increase of IDI_{\mathrm{D}} with both VDSV_{\mathrm{DS}} and VGSV_{\mathrm{GS}}. After VDSV_{\mathrm{DS}} surpasses the overdrive voltage (VOV=VGS−VTV_{\mathrm{OV}} = V_{\mathrm{GS}} - V_{\mathrm{T}}, for n-channel FETs), IDI_{\mathrm{D}} starts to saturate to IsatI_{\mathrm{sat}}, which could (based on the classical FET model[17]) increase quadratically with VOVV_{\mathrm{OV}} in the pinch-off regime and linearly with VOVV_{\mathrm{OV}} in the velocity saturation regime[14]. Note, the linear regime may present as nonlinear (often exponential) in the event of poor carrier injection at the contacts, such as from large Schottky barriers.

Multiple performance parameters can be extracted from the II-VV curves in Figure 1b-Figure 1d. The most important performance metrics are the currents, which must be reported normalized by the channel width, WchW_{\mathrm{ch}} (e.g., units of μA/μm\mu\mathrm{A}/\mu\mathrm{m}). For 1D or quasi-1D devices, it is common to first report the current per CNT/nanowire/nanosheet stack. Then the current can be normalized to μA/μm\mu\mathrm{A}/\mu\mathrm{m} by considering the expected channel density and pitch of the channel material (e.g., 10 μA\mu\mathrm{A}/CNT with 50 CNTs/μm\mu\mathrm{m}, giving 500 μA/μm\mu\mathrm{A}/\mu\mathrm{m}) since the aerial footprint of the device is a critical aspect of performance. When extracting IonI_{\mathrm{on}} and IoffI_{\mathrm{off}} from these II-VV curves, in a simplified scenario, IoffI_{\mathrm{off}} is the IDI_{\mathrm{D}} measured at VGS=0V_{\mathrm{GS}} = 0 and VDS=VDDV_{\mathrm{DS}} = V_{\mathrm{DD}}, whereas IonI_{\mathrm{on}} is the IDI_{\mathrm{D}} measured at VGS=VDS=VDDV_{\mathrm{GS}} = V_{\mathrm{DS}} = V_{\mathrm{DD}}. Here, VDDV_{\mathrm{DD}} is the voltage that would be supplied to operate the transistors. (For mainstream silicon technology, VDDV_{\mathrm{DD}} has dropped to 1 V near 2010 and to 0.7 V in recent years[18].) For modern technologies, the exact value of VDDV_{\mathrm{DD}} depends on the application. For example, if the emergent transistor is used as an access transistor in a dynamic random-access memory (DRAM), then its VDDV_{\mathrm{DD}} will be a small value to ensure linear regime operation in the on-state. Reported emergent devices often do not have threshold voltages tuned such that VGS=0V_{\mathrm{GS}} = 0 is a sensible off-state; additionally, there is often not a well-defined VDDV_{\mathrm{DD}} value due to the wide variety of device structural parameters. We hence suggest extracting the maximum and minimum IDI_{\mathrm{D}} (ImaxI_{\mathrm{max}} and IminI_{\mathrm{min}}) from a typical subthreshold curve and reporting the Imax⁡/Imin⁡I_{\max}/I_{\min} ratios when VDSV_{\mathrm{DS}} is biased in both linear and saturation regimes. A more detailed description on reporting and benchmarking Imax⁡/Imin⁡I_{\max}/I_{\min} is in Note S1.

When reporting the IsatI_{\mathrm{sat}} of a device, it is necessary to note the carrier density nn, at which the IsatI_{\mathrm{sat}} is extracted. Ideally, the Hall effect is used to measure the carrier density for the channel material, but for most researchers in the FET community, more accessible approaches are needed that do not require specially designed test structures. In the linear regime, the average carrier density can be estimated as n≈Cins(VOV−VDS/2)/qn \approx C_{\mathrm{ins}}(V_{\mathrm{OV}}-V_{\mathrm{DS}}/2)/q, where CinsC_{\mathrm{ins}} is the gate insulator capacitance and qq is the elementary charge; however, in the saturation regime, the depletion region in the channel complicates the estimation. The carrier density near the source side is the same for both the linear and saturation regimes. For convenience and simplicity, we recommend clearly labelling the carrier density near the source as nSn_{\mathrm{S}} (=CinsVOV/q=C_{\mathrm{ins}}V_{\mathrm{OV}}/q) and using this value for both operation regimes. To determine VOVV_{\mathrm{OV}}, VTV_{\mathrm{T}} is usually estimated using extrapolation in the linear portion of the transfer curve, as listed in Table 1. Other methods, such as constant current[19], Y-function methods[20, 21] and four-probe measurements[22], can be used to cross-check the linear extraction of VTV_{\mathrm{T}} and reduce the variation when estimating nSn_{\mathrm{S}}. More discussion regarding VTV_{\mathrm{T}} extraction is given in Note S2.

In addition to IDI_{\mathrm{D}}, RcR_{\mathrm{c}} is also essential to represent device performance. The transfer length method (TLM) is the most commonly used approach for extracting RcR_{\mathrm{c}}, along with the sheet resistance, RshR_{\mathrm{sh}}, of the channel (in units of Ω\Omega/square)[23]. The TLM approach requires a series of FETs with different channel lengths and consistent contact and gating configurations. It entails plotting the total resistance of each device versus LchL_{\mathrm{ch}} at a given nSn_{\mathrm{S}}, allowing RcR_{\mathrm{c}} to be extracted as the extrapolated y-axis intercept from a linear fit to the data points. Typically, the VDSV_{\mathrm{DS}} for calculating the total resistance is the “small” VDSV_{\mathrm{DS}} used in Figure 1b to ensure linear regime operation. The channel lengths in the TLM should range from “short” (where the total resistance is dominated by RcR_{\mathrm{c}}) to “long” (dominated by channel resistance, Rch=Rtot−2RcR_{\mathrm{ch}} = R_{\mathrm{tot}} - 2R_{\mathrm{c}} or RshLchR_{\mathrm{sh}}L_{\mathrm{ch}}) where the actual “short” and “long” channel lengths will depend on the relationship between the channel resistance and the contact resistance. A more detailed discussion on extracting RcR_{\mathrm{c}} and other considerations using TLM data is in Note S3.

Another frequently reported parameter is the carrier mobility of the channel material. Among various forms of mobility, the field-effect mobility μFE=Lchgm/(WchCinsVDS)\mu_{\mathrm{FE}} = L_{\mathrm{ch}}g_{\mathrm{m}}/(W_{\mathrm{ch}}C_{\mathrm{ins}}V_{\mathrm{DS}}) is often used. However, μFE\mu_{\mathrm{FE}} can be underestimated[21, 24] or overestimated[22, 25, 26] relative to the drift mobility of the channel material depending on the details of VDSV_{\mathrm{DS}}, VGSV_{\mathrm{GS}}, RcR_{\mathrm{c}}, LchL_{\mathrm{ch}}, and gate capacitance. In particular, gated contact effects can significantly affect mobility extraction. Although different approaches[21, 23] have been proposed to make μFE\mu_{\mathrm{FE}} less dependent on various factors, such as RcR_{\mathrm{c}} and LchL_{\mathrm{ch}}, none of them is sufficiently general enough to be widely adopted. Conductivity mobility (μcon\mu_{\mathrm{con}}) has the advantage of strictly reflecting the channel material properties and the quality of the channel-dielectric interface[23] [27]. In a FET, μcon\mu_{\mathrm{con}}[23] can be estimated from the sheet resistance of the semiconductor channel and the carrier density nSn_{\mathrm{S}} (see Table 1); thus, it does not involve the contact resistance or the device structure. High mobility is often a goal for research FETs; when such reports are made, it is critical to clearly state how the values are determined, and ideally multiple approaches (such as μFE\mu_{\mathrm{FE}} and four-probe measurements[22]) are taken to cross-validate the claims. It is worth noting that the usefulness of channel mobility as an indicator of performance in aggressively scaled FETs is debatable as devices with channel lengths < 30 nm are going to be strongly limited by contact resistance (including carrier injection efficiency) with minimal dependence on transport in the channel28,29.

The most representative FET parameters are listed in Table 1 as a suggested reporting checklist. Additional parameters are briefly discussed in Note S4.

NameCharacteristicsAdditional details
Structural parametersContact length, LcL_{\mathrm{c}}<br>Channel length, LchL_{\mathrm{ch}}<br>Channel width, WchW_{\mathrm{ch}}<br>Insulator thickness, tinst_{\mathrm{ins}}<br>Channel thickness, tcht_{\mathrm{ch}}Specify contact and gating geometry/materials; include high-resolution electron microscopy evidence when reporting sub-20 nm dimensions (especially for LcL_{\mathrm{c}} and LchL_{\mathrm{ch}})
Insulator capacitance, CinsC_{\mathrm{ins}}Capacitance-voltage or Capacitance-frequencyMeasured CinsC_{\mathrm{ins}} is more accurate than estimating ϵins\epsilon_{\mathrm{ins}} especially when a high-kk insulator is used
Threshold voltage, VTV_{\mathrm{T}}, and hysteresis, ΔVT\Delta V_{\mathrm{T}}Extrapolation in the linear portion of the transfer curve[19]• IDI_{\mathrm{D}}-VGSV_{\mathrm{GS}} should have forward and backward sweeps<br>• Consider VTV_{\mathrm{T}} uncertainty due to hysteresis (charge trapping), the dependence of VDSV_{\mathrm{DS}} and II-VV sweeps (Note S2)
Drain current in saturation regime, IsatI_{\mathrm{sat}}IDI_{\mathrm{D}}-VDSV_{\mathrm{DS}} (saturation regime)• Sweep IDI_{\mathrm{D}}-VDSV_{\mathrm{DS}} to saturation regime<br>• Specify carrier density where IsatI_{\mathrm{sat}} is extracted<br>• Normalized by channel width
Contact resistance, RcR_{\mathrm{c}}TLM[23] (Note S3)• Linear regime (small VDSV_{\mathrm{DS}})<br>• Specify carrier density nSn_{\mathrm{S}} or plot RcR_{\mathrm{c}} vs. nSn_{\mathrm{S}}<br>• TLM should have at least four channels and include at least one each of contact and channel resistance dominated devices
Conductivity mobility, μcon\mu_{\mathrm{con}}1qnSRsh\frac{1}{q n_{\mathrm{S}} R_{\mathrm{sh}}}• RshR_{\mathrm{sh}} is extracted from the slope of TLM plots or from four-probe measurements[22]. Unit: Ω\Omega/square<br>• Carrier density near the source: nS≈CinsVov/qn_{\mathrm{S}} \approx C_{\mathrm{ins}} V_{\mathrm{ov}}/q<br>• Mobility from Rsh=(qnSμ)−1R_{\mathrm{sh}} = (q n_{\mathrm{S}} \mu)^{-1}<br>• Plot mobility vs nSn_{\mathrm{S}} to show field dependence

Table 1. Checklist of suggested device parameters to report

Transconductance, gmg_{\mathrm{m}}Transfer or output curves gm=∂ID∂VGSg_{\mathrm{m}}=\frac{\partial I_{\mathrm{D}}}{\partial V_{\mathrm{GS}}} at certain VDSV_{\mathrm{DS}}Specify gmg_{\mathrm{m}} (linear) or gmg_{\mathrm{m}} (saturation)
Subthreshold Swing, SSSSSubthreshold curves (inverse slope in mV/decade below VTV_{\mathrm{T}})• SSSS depends on CinsC_{\mathrm{ins}} and interface trap capacitance CitC_{\mathrm{it}}<br>• Plot SSSS vs. log⁡10(ID)\log_{10}(I_{\mathrm{D}})
Ion/IoffI_{\mathrm{on}}/I_{\mathrm{off}}Subthreshold curves at saturation regime, VDS=VDSV_{\mathrm{DS}}=V_{\mathrm{DS}} (sat)• Report Imax/IminI_{\mathrm{max}}/I_{\mathrm{min}} as an alternative along with nSn_{\mathrm{S}} range<br>• Plot IGI_{\mathrm{G}} vs VGSV_{\mathrm{GS}} to show leakage current
DIBLΔVT/ΔVDS\Delta V_{\mathrm{T}}/\Delta V_{\mathrm{DS}} from transfer curvesKey for short-channel devices

Table 1 (PDF p. 6).

Beyond the parameters in Table 1, showing statistics and variation is strongly encouraged to obtain comprehensive coverage of the device performance. The variation can be shown as error bars, box plots, coefficient of variation, or cumulative distribution function (see Note S5 for demonstration).

Due to many nonidealities associated with emerging materials or unconventional device geometries, it is almost unavoidable that there could be considerable uncertainties in many extracted parameters, including RcR_{\mathrm{c}}, nSn_{\mathrm{S}}, and mobilities. These parameters are often interdependent. Reducing device variation is a major research theme for the eventual application of emergent FETs. Whatever measurements and specific analysis approaches are taken to determine these parameters, the details should be clearly and explicitly reported, and our recommended approaches are demonstrated herein.

Once an emerging FET has been systematically parameterized, benchmarking tables and plots are extremely useful for comparing devices from different reports. Because the electric fields are the driving forces within FETs, benchmarking performance metrics based on electric fields is natural. However, special care is needed in considering electric fields in devices, because they are spatially non-uniform and depend on many other factors, such as fringing fields and quantum capacitance CqC_{\mathrm{q}}. Thus, the electric fields in nanoscale FETs are more complicated than the simple definition of an applied voltage divided by a physically defined length. For example, it is a reasonable assumption that the channel electric field in the channel, EchE_{\mathrm{ch}} increases linearly from source to drain in the linear region of operation, but EchE_{\mathrm{ch}} peaks sharply at the drain end of the channel in classical pinch-off (saturation)30. To account for this, the average EchE_{\mathrm{ch}} can be approximated as (VDS−2IlinRc)/Lch(V_{\mathrm{DS}}-2I_{\mathrm{lin}}R_{\mathrm{c}})/L_{\mathrm{ch}} in the linear regime, accounting for voltage dropped at the contacts.

The vertical electric field at the source end, EgateE_{\mathrm{gate}}, can be estimated as VOV/tinsV_{\mathrm{OV}}/t_{\mathrm{ins}} if a planar gate is used. In turn, EgateE_{\mathrm{gate}} and the gate insulator permittivity determine the carrier density in the channel. Yet, both EgateE_{\mathrm{gate}} and the gate insulator permittivity are rather challenging to measure accurately. One more word of caution is justified: because many low-dimensional materials exhibit a low density of states, CinsC_{\mathrm{ins}} needs to be replaced by CinsCq/(Cins+Cq)C_{\mathrm{ins}}C_{\mathrm{q}}/(C_{\mathrm{ins}}+C_{\mathrm{q}}) where quantum capacitance (CqC_{\mathrm{q}}) can be approximated as q2DOSq^{2}\mathrm{DOS} (density of states)31,32. Only for Cins≪CqC_{\mathrm{ins}}\ll C_{\mathrm{q}} this expression becomes equivalent to CinsC_{\mathrm{ins}}. Because multiple parameters in Table 1 depend on nSn_{\mathrm{S}}, benchmarking these versus nSn_{\mathrm{S}} is recommended to evaluate devices from different studies. A suggested list of benchmarking plots to evaluate device parameters and performance metrics is given in Table 2.

ParameterBenchmarking PlotNotes
Imin⁡I_{\min} and Imax⁡I_{\max}Imin⁡I_{\min} vs. Imax⁡I_{\max}• Specify LchL_{\mathrm{ch}} or Lch/EOTL_{\mathrm{ch}}/\mathrm{EOT}<br>• Ideally specify the carrier density at which Imax⁡I_{\max} is extracted (Note S1)
IsatI_{\mathrm{sat}}IsatI_{\mathrm{sat}} vs. nSn_{\mathrm{S}}Label LchL_{\mathrm{ch}} and tcht_{\mathrm{ch}} to imply channel resistance
IDI_{\mathrm{D}}IDI_{\mathrm{D}} vs. LchL_{\mathrm{ch}}At certain VDSV_{\mathrm{DS}} and nSn_{\mathrm{S}} (e.g., VDS=1V_{\mathrm{DS}} = 1 V and nS=1013 cm−2n_{\mathrm{S}} = 10^{13}\ \mathrm{cm}^{-2})
RcR_{\mathrm{c}}RcR_{\mathrm{c}} vs. nSn_{\mathrm{S}}• Or benchmark RcR_{\mathrm{c}} vs. tcht_{\mathrm{ch}} at certain nSn_{\mathrm{S}}<br>• Specify if semiconductor in contact regions is gated or not
μcon\mu_{\mathrm{con}}μcon\mu_{\mathrm{con}} vs. tcht_{\mathrm{ch}}For the same material, a thicker channel could have higher mobility due to less surface scattering
gmg_{\mathrm{m}}gmg_{\mathrm{m}} vs. nS/Lchn_{\mathrm{S}}/L_{\mathrm{ch}}• Since gm=WLμCinsVovg_{\mathrm{m}} = \frac{W}{L}\mu C_{\mathrm{ins}}V_{\mathrm{ov}}, gm∝CinsVov/Lchg_{\mathrm{m}} \propto C_{\mathrm{ins}}V_{\mathrm{ov}}/L_{\mathrm{ch}}<br>• nS≈CinsVOV/qn_{\mathrm{S}} \approx C_{\mathrm{ins}}V_{\mathrm{OV}}/q near the source end, so gm∝nS/Lchg_{\mathrm{m}} \propto n_{\mathrm{S}}/L_{\mathrm{ch}}
SSSSSSSS vs. CinsC_{\mathrm{ins}}• Larger CinsC_{\mathrm{ins}} can yield smaller SSSS<br>• Identify Schottky barrier branch and thermal branch<br>• Or plot SSSS vs. LchL_{\mathrm{ch}} to show short-channel robustness<br>• Or plot SSSS vs. log⁡10(ID)\log_{10}(I_{\mathrm{D}})

Table 2. Suggested benchmarking plots for evaluating device performance compared with other FETs

Drain current is the key output of a FET and is also frequently benchmarked and compared. However, many comparisons are oversimplified and not fairly conducted as the drain current depends on many parameters. As mentioned in Table 2, we recommend benchmarking IDI_{\mathrm{D}} vs. LchL_{\mathrm{ch}} at certain VDSV_{\mathrm{DS}} and nSn_{\mathrm{S}} values, enabling fair comparison between devices having different channel lengths. On the other hand, if a record IsatI_{\mathrm{sat}} is claimed, we recommend benchmarking the maximum IsatI_{\mathrm{sat}} vs. nSn_{\mathrm{S}} because it is a much closer indicator for the eventual drive current and ultimately sets the operating delay of a circuit stage (delay τ∝CVDD/Isat\tau\propto CV_{\mathrm{DD}}/I_{\mathrm{sat}}). As mentioned previously, assuming limited short-channel effects, IsatI_{\mathrm{sat}} mainly depends on nSn_{\mathrm{S}} and not on EchE_{\mathrm{ch}}. Usually, one performance metric depends on multiple parameters; hence, key parameters should be annotated on the benchmarking plot (see Table 2).

Reporting and benchmarking example

To demonstrate reporting and benchmarking based on the principles proposed above, MoS2_2 is chosen as the example emerging channel material because it is among the most studied semiconducting nanomaterials in recent years and represents a family of 2D materials that holds promise for future transistor applications. Figure 2a shows an example transistor based on monolayer (1L) MoS2_2 grown by chemical vapor deposition (CVD). The device is top-contacted and back-gated, which is the most common and convenient FET structure used to explore emergent channel materials. The approach is as follows:

Example of reporting device performance for monolayer Au-contacted MoS2 FETs

Figure 2. Example of reporting device performance for monolayer Au-contacted MoS2_2 FETs. a, Device schematic and the basic structural parameters of the MoS2_2 FET. An SEM image of a TLM structure with false-colored MoS2_2 area (scale bar, 1 µm) and a cross-section TEM image of the AlOx_x (scale bar, 10 nm). b, Subthreshold (IDI_\mathrm{D}–VGSV_\mathrm{GS}) curve of the device with ImaxI_\mathrm{max} and IminI_\mathrm{min} labelled. The IGI_\mathrm{G} is the gate leakage current at VDSV_\mathrm{DS} = 4 V. The curve for VDSV_\mathrm{DS} = 1 V is intentionally not shown so the plot is less crowded. c, Transfer (IDI_\mathrm{D}–VGSV_\mathrm{GS}) curves of the device showing larger hysteresis with larger VDSV_\mathrm{DS}. d, Output (IDI_\mathrm{D}–VDSV_\mathrm{DS}) curves of the device. VGSV_\mathrm{GS} changes in steps of 1 V. e, SS vs. IDI_\mathrm{D} for both forwards and backwards VGSV_\mathrm{GS} sweeps in (b). f, Extraction of RcR_\mathrm{c} from the TLM structure in (a). The RtotR_\mathrm{tot} is extracted at VDSV_\mathrm{DS} = 100 mV. g, Contact resistance vs. nSn_\mathrm{S} showing the contact gating effect that is a result of the device operating as a Schottky barrier transistor with the gate modulating the semiconductor in the source/drain contact regions33. h, Extracted sheet resistance (left axis) and conductivity mobility (right axis) versus nSn_\mathrm{S}. In g and h, error bars reflect 90% confidence interval from a least-squares fit of the TLM.

Step 1. The structural parameters of the device are determined and labelled (Figure 2a). In this example, the gate insulator is AlOx\mathrm{AlO}_{x}, which is grown by atomic layer deposition (ALD) with the oxide capacitance (Cins≈280C_{\mathrm{ins}} \approx280 nF/cm2^{2}) evaluated from a capacitance-voltage measurement of a large-area test capacitor. The thickness of the oxide (tins≈20t_{\mathrm{ins}} \approx20 nm) is further confirmed by cross-sectional transmission electron microscope (TEM) imaging. From the thickness and capacitance, the dielectric constant of the oxide is estimated to be εins≈6\varepsilon_{\mathrm{ins}} \approx6. Other dimensions such as LchL_{\mathrm{ch}}, WchW_{\mathrm{ch}}, and LcL_{\mathrm{c}} are confirmed by scanning electron microscopy (SEM) after electrical characterization.

Step 2. IDI_{\mathrm{D}}-VGSV_{\mathrm{GS}} and IDI_{\mathrm{D}}-VDSV_{\mathrm{DS}} characterization are performed, making sure that VDSV_{\mathrm{DS}} and VGSV_{\mathrm{GS}} are swept high enough for the device to reach saturation, and the VGSV_{\mathrm{GS}} sweep range is sufficient to observe IminI_{\mathrm{min}} in both the linear (low VDSV_{\mathrm{DS}}) and saturation (high VDSV_{\mathrm{DS}}) operation regions. Imax/IminI_{\mathrm{max}}/I_{\mathrm{min}} of ∼4×107\sim4 \times10^{7} at VDS=4V_{\mathrm{DS}} = 4 V can be extracted from the subthreshold curve in Figure 2b. ImaxI_{\mathrm{max}} is extracted at nS≈1.4×1013n_{\mathrm{S}} \approx1.4 \times10^{13} cm−2^{-2}. IminI_{\mathrm{min}} is extracted under subthreshold conditions, where VGS<VTV_{\mathrm{GS}} < V_{\mathrm{T}}, yielding a negative VOVV_{\mathrm{OV}} and nS≈0n_{\mathrm{S}} \approx0. The larger hysteresis for VDS=4V_{\mathrm{DS}} = 4 V in Figure 2b,Figure 2c highlights the impact of the larger source-drain field on the interface charges in the channel. Due to hot-carrier stress from the high VDSV_{\mathrm{DS}} (explained later), VTV_{\mathrm{T}} increases for high VDSV_{\mathrm{DS}}, resulting in an extracted DIBL of −274-274 to −436-436 mV/V considering the effect of hysteresis. Also, from the transfer curves in Figure 2c, the maximum gm(sat)g_{\mathrm{m}}(\mathrm{sat}) and gm(lin)g_{\mathrm{m}}(\mathrm{lin}) are estimated to be ∼59\sim59 μ\muS/μ\mum and ∼1.7\sim1.7 μ\muS/μ\mum, respectively. In Figure 2d, approximate current saturation is observed with IsatI_{\mathrm{sat}} around 325 μ\muA/μ\mum obtained at nS≈1.3×1013n_{\mathrm{S}} \approx1.3 \times10^{13} cm−2^{-2} at VDS=4V_{\mathrm{DS}} = 4 V. The blue and red shows linear and saturation regions, approximately. The IDI_{\mathrm{D}}-VDSV_{\mathrm{DS}} spacing is sub-linear at the highest VGSV_{\mathrm{GS}}, which is a sign of possible self-heating.

Figures 2a-d are used for primary characterization of one device, and more derived plots are shown in Figure 2e-Figure 2h, providing a more complete picture of the device characteristics. The device spread and parameter variations based on ten similar TLM structures are shown in Figure S5. The full range of SSSS vs. IDI_\mathrm{D} is plotted in Figure 2d, with a minimum SSSS of 280 mV/dec extracted in the subthreshold regime. Additionally, because VTV_\mathrm{T} depends on VDSV_\mathrm{DS}, it is key to extract VTV_\mathrm{T} at the associated VDSV_\mathrm{DS} (as noted in Table 1). RcR_\mathrm{c}, RshR_\mathrm{sh}, and subsequently μcon\mu_\mathrm{con} are extracted by using a TLM structure as shown in Figure 2f-Figure 2h. The RcR_\mathrm{c} is estimated to be around 2.1 kΩ⋅µm, which is comparable to the RchR_\mathrm{ch} of 2.8 kΩ⋅µm for the device with channel length of 280 nm. The relation between nSn_\mathrm{S} and extracted RcR_\mathrm{c} is plotted in Figure 2g to show the effect of the overall back gate on the contact resistance (i.e., contact gating33–35). Figure 2h shows μcon\mu_{\mathrm{con}} decreases from 59 to 40 cm2V−1s−1\mathrm{cm}^{2}\mathrm{V}^{-1}\mathrm{s}^{-1} with increasing nSn_{\mathrm{S}}, likely due to the increased electron scattering with the oxide surface roughness.

Seven-panel plots demonstrating device spread and parameter variations

Figure S5. Demonstration of device spread and parameter variations based on ten TLM structures. a, Example transfer curves (IDI_\mathrm{D}–VGSV_\mathrm{GS}) for the TLM structure in Figure 2. b, Measured subthreshold curves (IDI_\mathrm{D}–VGSV_\mathrm{GS}) of ten devices with LchL_\mathrm{ch} of 280 nm of 280 nm. c, Cumulative distribution function (CDF) of the hysteresis voltage for the ten devices with LchL_\mathrm{ch} of 280 nm. Boxplots of (d) VTV_\mathrm{T}, (e) IDI_\mathrm{D} at VDSV_\mathrm{DS} = 1 V and nSn_\mathrm{S} = 1.3×10131.3 \times10^{13} cm−2^{-2}, (f) the minimal SS extracted near IDI_\mathrm{D} = 10 nA, and (g) ten TLM plots with the median RcR_\mathrm{c} value of 3 kΩ⋅μ\Omega\cdot\mum.

Step 3: As a simplified example, we benchmark key device performance parameters in Figure 3 with a limited number of reports included. Currently, most papers do not report IDI_{\mathrm{D}}-VGSV_{\mathrm{GS}} at VDSV_{\mathrm{DS}} (sat) or close to VDDV_{\mathrm{DD}} as recommended above. Hence, plotting Imin⁡I_{\min} vs. Imax⁡I_{\max} at certain VDSV_{\mathrm{DS}} (e.g., VDS=1V_{\mathrm{DS}} = 1 V) while annotating LchL_{\mathrm{ch}} is an acceptable approach (Figure 3a). The upper limit of the carrier density is set at nS=1013 cm−2n_{\mathrm{S}} = 10^{13}\ \mathrm{cm}^{-2}, ensuring a fair comparison of Imax⁡I_{\max}. The Imax⁡/Imin⁡I_{\max}/I_{\min} ratio annotated on the right axis is also shown in the dashed lines in Figure 3a. Due to a better electrostatic control from the gate, devices with a larger Lch/EOTL_{\mathrm{ch}}/\mathrm{EOT} ratio tend to yield a higher Imax⁡/Imin⁡I_{\max}/I_{\min} (where EOT is the equivalent oxide thickness). Other parameters also play a role such as the leakage currents through the gate insulator or from source to drain. Large channel width can also produce a more accurate width-normalized Imin⁡I_{\min}, especially when Imin⁡I_{\min} is below the instrument noise floor. For example, Illarionov 36 demonstrated a relatively high Imax⁡/Imin⁡I_{\max}/I_{\min} ratio in devices with a 20 μ\mum channel width. Further study is still needed to investigate how to achieve high Imax⁡I_{\max} and small Imin⁡I_{\min} in aggressively scaled devices (small LchL_{\mathrm{ch}}, LcL_{\mathrm{c}}, and EOT).

Example benchmarking device performance of monolayer MoS$_2$ FETs, with four panels benchmarking $I_{\min}$ versus $I_{\max}$, $I_{\mathrm{sat}}$ versus $n_{\mathrm{S}}$, $I_{\mathrm{D}}$ versus $L_{\mathrm{ch}}$, and $R_{\mathrm{c}}$ versus $n_{\mathrm{S}}$.

Figure 3. Example Benchmarking device performance of monolayer MoS2_2 FETs. a, Benchmarking Imin⁡I_{\min} vs. Imax⁡I_{\max}. The Imax⁡I_{\max} is extracted at nS=1013 cm−2n_{\mathrm{S}} = 10^{13}\ \mathrm{cm}^{-2}. For simplicity, the Imin⁡I_{\min} of the data points are extracted at their respective smallest current. More rigorous benchmarking of Imin⁡I_{\min} vs Imax⁡I_{\max} is in Note S1. b, Benchmarking IsatI_{\mathrm{sat}} versus nSn_{\mathrm{S}}, where the channel length in nm is labelled next to the contact metals used in the devices. IsatI_{\mathrm{sat}} are extracted at different VDSV_{\mathrm{DS}} (listed in Table 3). These devices do not have the same VDS(sat)V_{\mathrm{DS}(\mathrm{sat})} as devices with different channel lengths and saturate at different VDSV_{\mathrm{DS}}. The IRDS HP is shown in a range of nSn_{\mathrm{S}} to represent uncertainties of the carrier density in future generation technologies. c, Benchmarking IDI_{\mathrm{D}} versus LchL_{\mathrm{ch}} at VDS=1 VV_{\mathrm{DS}} = 1\ \mathrm{V} and nS=1013 cm−2n_{\mathrm{S}} = 10^{13}\ \mathrm{cm}^{-2}. Ref. 41 uses top-gate, while other reports use back-gate. d, Benchmarking RcR_{\mathrm{c}} versus nSn_{\mathrm{S}} in a few representative reports. The shaded regions represent uncertainties reported in the respective studies (Ag[14] uses 95% confidence interval, while In/Au42, Sn/Au42, and Au use standard error from the linear regression of TLM). The RcR_{\mathrm{c}} vs. nSn_{\mathrm{S}} of Sb43 is obtained from Y-function method. The filled and open symbol show that the shortest channel device in the TLM structure is 2Rc2R_{\mathrm{c}} and RchR_{\mathrm{ch}} dominated, respectively. If RchR_{\mathrm{ch}} dominates or the RcR_{\mathrm{c}} is over an order of magnitude smaller than the RtotR_{\mathrm{tot}} for the smallest device in TLM, the extracted RcR_{\mathrm{c}} is of questionable validity; i.e., solid symbol data is more reliable per Note S3. Different colors are assigned to different reported devices. The purple Au data denote devices in Figure 2. Most of the data are extracted from published reports: Ag[14], AlOx_x doped/Au[15], In/Au42, Sn/Au42, Sb43, In44 and Sn45. In a and c, reference numbers are added for Au-contacted devices to better differentiate their performance. A few studies are plotted as dotted lines to highlight the trends and to improve the clarity of the plots.

As mentioned previously, a high drain current in the saturation regime is a key performance metric. In Figure 3b, IsatI_{\mathrm{sat}} is plotted versus nSn_{\mathrm{S}} from representative studies of FETs based on MoS2_2 as the channel material. We note that the IsatI_{\mathrm{sat}} is extracted at different VDSV_{\mathrm{DS}} because different devices have different channel lengths, as annotated in Figure 3b. We caution against plotting Isat/LchI_{\mathrm{sat}}/L_{\mathrm{ch}} vs. nSn_{\mathrm{S}} because it implies that LchL_{\mathrm{ch}} is the main limiting factor for IsatI_{\mathrm{sat}}, which is not necessarily true, especially for scaled devices where contact resistance typically dominates IsatI_{\mathrm{sat}} performance. Importantly, it is clear that IsatI_{\mathrm{sat}} needs to be further improved to meet the high-performance target of the most recent technology guidelines (at VDD≈0.65V_{\mathrm{DD}} \approx0.65 V near 2030)37. Many reports already used high nSn_{\mathrm{S}} but fell short on IsatI_{\mathrm{sat}} even with channel lengths down to ∼10\sim10 nm38, being strongly limited by their contacts.

Recently, semimetal contacts such as bismuth have been shown to produce high-quality contacts39. It is nevertheless noteworthy that the two Bi-1L MoS2_2 devices have a wide range of IsatI_{\mathrm{sat}} performance, encompassing all the other devices in Figure 3b, yet the channel length difference between the two devices is only 115 nm. Interestingly, one of the Bi-contacted devices (Lch=150L_{\mathrm{ch}} = 150 nm) actually underperforms other Au-contacted devices with longer channel lengths. Hence, although some approaches show potential to achieve the International Roadmap for Devices and Systems (IRDS) high-performance goal of IsatI_{\mathrm{sat}} for the post-2030 era37, further investigation is still needed to reliably and reproducibly realize high IsatI_{\mathrm{sat}} from a monolayer channel. In next-generation FETs, IsatI_{\mathrm{sat}} could also be increased by shifting to nanosheet device designs, which stack multiple channels vertically to improve current density in the same device footprint40.

In some reports, a proper saturation current is not given. Also, since different devices use different channel lengths, IsatI_{\mathrm{sat}} is often extracted at different VDSV_{\mathrm{DS}}. To highlight the impact of channel length, we recommend benchmarking IDI_{\mathrm{D}} vs. LchL_{\mathrm{ch}} at VDS=1V_{\mathrm{DS}} = 1 V and nS=1013n_{\mathrm{S}} = 10^{13} cm−2^{-2}. This plot enables a direct comparison of devices with similar LchL_{\mathrm{ch}}. In Figure 3c, with channel length decreasing from 200 nm to 38 nm, both Bi39 and Sn45 contacted devices yield relatively large increases in drain current. We note that the Bi-contacted devices are based on different MoS2_2 films. The different quality of the MoS2_2 may partially contribute to the large increase of IDI_{\mathrm{D}} with a relatively small change in LchL_{\mathrm{ch}}. Nevertheless, Figure 3c,Figure 3d present the potential of atomic thin materials for producing high drain current, especially for scaled devices.

In Figure 3d, RcR_{\mathrm{c}} is plotted against nSn_{\mathrm{S}} considering most devices have gated contacts (i.e., the back-gate modulates the channel and contacts33–35). While some reported RcR_{\mathrm{c}} values reach below 500 Ω·µm, their TLM extractions are all based on channel resistance-dominated devices, which can lead to questionable validity in their claimed RcR_{\mathrm{c}} (an artificially small or even a negative RcR_{\mathrm{c}} can be extracted, see Note S3 for details). We advocate that if a record RcR_{\mathrm{c}} is claimed from TLM, RshR_{\mathrm{sh}} should be cross-examined by using other methods such as four-probe measurements, which can provide a relatively accurate estimation of RshR_{\mathrm{sh}} vs. nSn_{\mathrm{S}} (Note S3). With RshR_{\mathrm{sh}} vs. nSn_{\mathrm{S}} from four-probe measurements, RcR_{\mathrm{c}} vs. nSn_{\mathrm{S}} can be derived by deducting the Rch=RshLchR_{\mathrm{ch}} = R_{\mathrm{sh}}L_{\mathrm{ch}} from RtotR_{\mathrm{tot}} to confirm the TLM extracted value. Showing extraction of RcR_{\mathrm{c}} from many TLM structures can also increase confidence in the data by providing an average value of the RcR_{\mathrm{c}} rather than just the minimal value from a single TLM46,47. Furthermore, RcR_{\mathrm{c}} is heavily impacted by contact gating, as evident from the similar trends of RcR_{\mathrm{c}} vs. nSn_{\mathrm{S}} observed in different studies; therefore, further research is needed to obtain a small RcR_{\mathrm{c}} without gating the contacts.

Looking forward, many opportunities remain to develop transistors that simultaneously have small contact resistance, high IsatI_{\mathrm{sat}}, large Imax/IminI_{\mathrm{max}}/I_{\mathrm{min}} ratio, and minimal short-channel effects by using emergent nanomaterials. To achieve this technological goal, interface engineering at the contacts and gate dielectric needs to be further investigated48–50, along with progress in material synthesis51 and integration52. Moreover, it is important to focus on channel thicknesses below ∼3\sim3 nm, where low-dimensional nanomaterials can excel compared to Si, which suffers from poor carrier transport properties and a widened band gap in this thickness regime53.

In addition to the example benchmarking plots in Figure 3, other benchmarks can also be used to compare different devices. For example, as included in Table 2, plotting Imax/IminI_{\mathrm{max}}/I_{\mathrm{min}} vs. tcht_{\mathrm{ch}} or Imax/IminI_{\mathrm{max}}/I_{\mathrm{min}} vs. Lch/EOTL_{\mathrm{ch}}/\mathrm{EOT} to compare the off-state device performance. Plotting SSSS vs. CinsC_{\mathrm{ins}} or SSSS vs. log⁡10(ID)\log_{10}(I_{\mathrm{D}})54 can be used to evaluate subthreshold behaviour and trends across different devices. Finally, to show the quality of the channel materials, the channel sheet resistance or conductivity mobility can be plotted vs. carrier densities, as in Figure 2h. Representative reports with relatively large IsatI_{\mathrm{sat}} are listed in Table S1, including results for FETs with both monolayer and multilayer MoS2_2 channels (example benchmarking plots in Note S6). In the literature, notable benchmarking examples can be found in Refs.39,55 that highlight different channel materials, and in Ref.56 that focuses on device performance in integrated circuits (speed, gain, density, power consumption, and fan-out capabilities, etc.).

ContactsRef.tcht_{\mathrm{ch}} (nm)LchL_{\mathrm{ch}} (nm)nsn_{\mathrm{s}} (101310^{13} cm−2^{-2})RcR_{\mathrm{c}} (kΩ⋅μ\Omega\cdot\mum)VDSV_{\mathrm{DS}} (V)IsatI_{\mathrm{sat}} (μ\muA/μ\mum)
Ag[18]1L721.441.31.8320
Aua1L2801.324325
Au[21]1L202.8N/A2350
Bi[3]1L1503.40.122380
Ni+Cl doping[1]41002.160.51.6460
Au[21]6102.19N/A2470
Sn[22]1L3510.841.5615
Transferred Ag[16]4~201601.58N/A3660
AlOx_x+Au[17]1L38020.485700
Ni/Gr[2]10L802.580.542830
Ni[23]TG4.210002.43N/A3290
Au[24]TG1L10∼7\sim71.72425
Cr[25]TG∼\sim4L4002.443.34526

Table S1. Representative reporting on studies of MoS2\mathrm{MoS}_2 FETs with IsatI_{\mathrm{sat}}.

Conclusions

Our guidelines should help put key performance metrics in a proper context and enable researchers to effectively report and benchmark emergent transistors based on various emergent nanomaterials. While each of the listed metrics is significant, it is not necessary — nor always possible — to extract and present all of them. As such, it is essential to completely describe the device geometry, to collect and report appropriate current-voltage characteristics, and to describe in detail the procedures followed in the experiments. The approaches used to analyze data and extract benchmarking metrics should also be described in detail. Depending on the context and need, we recommend three sets of parameters to report and benchmark. The first includes maximum saturation current, on/off-current ratio, transconductance, and subthreshold swing. These values can be directly obtained from the measured II-VV characteristics that cover both linear and saturation regimes. These values are mainly determined by the intrinsic material properties, gate stack configuration, and contact quality. The second includes the derived parameters such as mobilities and contact resistance, where uncertainty and statistical spread on these derived parameters should be shown. The third set of parameters are those specific to certain transistor demonstrations based on the target application57,58. For example, DIBL is essential when reporting and evaluating ultra-scaled FETs. It is important — whenever possible — to benchmark against other novel materials and also state-of-the-art in mature technology39,55. By using these guidelines, it should be possible to comprehensively and consistently reveal, highlight, discuss, compare, and evaluate device performance, thus helping to identify advances and opportunities in the search for improved transistors.

1Nanoscale Device Characterization Division, National Institute of Standards and Technology, Gaithersburg, MD 20899, USA. 2Department of Electrical and Computer Engineering, Purdue University, West Lafayette, IN 47907, USA. 3Department of Chemistry and Biochemistry, University of California, Los Angeles, Los Angeles, CA 90095, USA. 4Theiss Research, La Jolla, CA 92037, USA. 5School of Integrated Circuits, Peking University, Beijing 100871, China. 6Electrical and Computer Engineering, New York University, Brooklyn, NY 11201, USA. 7Center for Quantum Phenomena, Physics Department, New York University, New York, NY 10003, USA. 8IMEC, Leuven, Belgium. 9RWTH Aachen University, Chair of Electronic Devices, Otto-Blumenthal-Str. 2, Aachen 52074, Germany. 10AMO GmbH, Advanced Microelectronic Center Aachen, Otto-Blumenthal-Str. 25, Aachen, 52074 Germany. 11Key Laboratory for the Physics and Chemistry of Nanodevices and Center for Carbon-based Electronics, Department of Electronics, Peking University, Beijing, China. 12Department of Electrical and Computer Engineering, University of Minnesota, Minneapolis, MN 55455 USA. 13Department of Electrical Engineering, Stanford University, Stanford, CA 94305, USA. 14Department of Electrical and Computer Engineering, Duke University, Durham, NC 27708, USA. 15Department of Chemistry, Duke University, Durham, NC 27708, USA. ‡: corresponding authors.

Acknowledgements

We acknowledge Dr. Huairuo Zhang and Dr. Albert Davydov from the National Institute of Standards and Technology for their help on the TEM images of the oxide in Figure 2. We acknowledge Dr. Guoqing Li and Prof. Linyou Cao from North Carolina State University for providing the CVD MoS₂ film. This work is supported by NEWLIMITS, a center in nCORE, a Semiconductor Research Corporation (SRC) program sponsored by NIST through award number 70NANB17H041. A.D.F acknowledges the support from the National Science Foundation under Grant ECCS 1915814. M.C.L. acknowledges funding from the European Union's Horizon 2020 research and innovation program under grant agreements 881603 (Graphene Flagship), 952792 (2D-EPL) and 829035 (QUEFORMAL), as well as the Deutsche Forschungsgemeinschaft (DFG, German Research Foundation) through the grants LE 2440/7-1 and LE 2440/8-1. Furthermore, support by the Bundesministerium für Bildung und Forschung (BMBF, German Ministry of Education and Research) through the grants 03XP0210 (GIMMIK) and 03ZU1106 (NeuroSys) is acknowledged. L.-M.P. acknowledges the National Science Foundation of China under the grant 61888102. S.J.K. acknowledges support from the NSF through award no. DMR-1921629. Fabrication and measurements were partially performed at the NIST Center for Nanoscale Science and Technology and at Duke Shared Manufacturing and Instrument Facility (SMIF).

Author contributions

All authors contributed to the preparation of the manuscript.

Notes

The authors declare no competing financial interest.

Certain commercial equipment, instruments, or materials are identified in this paper to specify the experimental procedure adequately. Such identifications are not intended to imply recommendation or endorsement by the National Institute of Standards and Technology (NIST), nor it is intended to imply that the materials or equipment identified are necessarily the best available for the purpose.

Corresponding authors

Zhihui Cheng, [email protected]

Aaron D. Franklin, [email protected]

Curt A. Richter, [email protected]

Data availability

The data used in the paper are available from the corresponding authors upon reasonable request.

Supplementary Information for How to Report and Benchmark Emerging Field-Effect Transistors

Zhihui Cheng; Chin-Sheng Pang; Peiqi Wang; Son T. Le; Yanqing Wu; Davood Shahrjerdi; Iuliana Radu; Max C. Lemme; Lian-Mao Peng; Xiangfeng Duan; Zhihong Chen; Joerg Appenzeller; Steven J. Koester; Eric Pop; Aaron D. Franklin; Curt A. Richter

†: corresponding authors.

Note S1: Rigorously reporting and benchmarking Imax⁡/Imin⁡I_{\max}/I_{\min}

Note S2: Different methods to extract threshold voltage VTV_{\mathrm{T}} and its uncertainties

Note S3: Extracting RcR_{\mathrm{c}} from TLM

Note S4: Additional Parameters

Note S5: Demonstration of device spread and parameter variations

Note S6: Benchmarking devices with different channel thicknesses

Rigorously reporting and benchmarking Imax⁡/Imin⁡I_{\max}/I_{\min}

The Imax⁡/Imin⁡I_{\max}/I_{\min} ratio is the most-used figure of merit for evaluating off-state performance of a transistor and it depends on multiple factors. First, Imax⁡/Imin⁡I_{\max}/I_{\min} is impacted by material properties such as material quality, bandgaps, and doping conditions. Secondly, the specific device structure and geometry, including the channel length and gate capacitance, also affect the achievable Imax⁡/Imin⁡I_{\max}/I_{\min}. Thirdly, the same device operating at different operation regimes might also have different Imax⁡/Imin⁡I_{\max}/I_{\min}. Combined with the absence of a well-defined VDDV_{\mathrm{DD}}, these factors make rigorous reporting and benchmarking guidelines strongly desired for Imax⁡/Imin⁡I_{\max}/I_{\min}. Rigorously reporting Imax⁡/Imin⁡I_{\max}/I_{\min} involves clearly identifying the VDSV_{\mathrm{DS}} and VGSV_{\mathrm{GS}} values at which the Imax⁡I_{\max} and Imin⁡I_{\min} are extracted. This practice will help fairly benchmark Imax⁡/Imin⁡I_{\max}/I_{\min} between different devices.

Similar to Figure 3a, Fig. S1a represents benchmarking Imax⁡/Imin⁡I_{\max}/I_{\min} at VDS=1V_{\mathrm{DS}} = 1 V, which is a commonly used bias condition when obtaining subthreshold curves. Under VDS=1V_{\mathrm{DS}} = 1 V, short-channel devices (e.g., Device A) may operate at the saturation regime, whereas long-channel devices (e.g., Device B) at the linear regime. While using the same VDS=1V_{\mathrm{DS}} = 1 V is a convenient and simple method, the Imax⁡/Imin⁡I_{\max}/I_{\min} likely represent different operation regimes for the two example devices. For a more precise comparison, instead of extracting the Imax⁡I_{\max} and Imin⁡I_{\min} at the same VDSV_{\mathrm{DS}} value for the different devices, it is possible to ensure they are extracted in the same regime (linear or saturation) by using the drain-source electric field instead of VDSV_{\mathrm{DS}}; e.g., EDS=0.1E_{\mathrm{DS}} = 0.1 V/μ\mum for the linear regime. This improved comparison is demonstrated in Fig. S1b, where the carrier density at which the Imax⁡I_{\max} is extracted is also labeled.

Rigorously benchmarking Imax/Imin

Figure S1. Rigorously benchmarking Imax⁡/Imin⁡I_{\max}/I_{\min}. a, Benchmarking Imax⁡/Imin⁡I_{\max}/I_{\min} at VDS=1V_{\mathrm{DS}} = 1 V, similar to Figure 3a. Devices A and B are not actual experimental data and are used to demonstrate benchmarking devices with different channel lengths. The carrier densities at which the Imax⁡I_{\max} and Imin⁡I_{\min} are extracted are also labeled. b, Benchmarking Imax⁡/Imin⁡I_{\max}/I_{\min} at the same operation regime, which is the linear regime with drain-to-source field EDS=0.1E_{\mathrm{DS}} = 0.1 V/μ\mum used as an example. Note, the diagonal dashed lines indicate certain values of Imax⁡/Imin⁡I_{\max}/I_{\min}.

Additional factors can impact Imax⁡/Imin⁡I_{\max}/I_{\min} ratio. When benchmarking devices with the same channel material but with different channel thicknesses, plotting Imax⁡/Imin⁡I_{\max}/I_{\min} vs. tcht_{\mathrm{ch}} is suggested. It is noteworthy that Imax⁡/Imin⁡I_{\max}/I_{\min} also depends on channel length and the equivalent oxide thickness (EOT) of the gate insulator. When the devices to be benchmarked have the same channel thickness, then benchmarking Imax⁡/Imin⁡I_{\max}/I_{\min} vs. Lch/EOTL_{\mathrm{ch}}/\mathrm{EOT} should be considered. In addition, Imin⁡I_{\min} can be limited by the measurement instrumentation, especially in materials with larger band gap such as monolayer TMDs. Additional factors impacting Imax⁡/Imin⁡I_{\max}/I_{\min} include contact resistance (which limits Imax⁡I_{\max}), leakage currents (which dominate Imin⁡I_{\min}) and parasitic capacitances (which affect electrostatic control of the gate), etc.

Different methods to extract threshold voltage VTV_{\mathrm{T}} and its uncertainties

Different methods to extract VTV_{\mathrm{T}}

A standard method to extract the VTV_{\mathrm{T}} is not yet available. Refs. 4–7 have investigated and compared different VTV_{\mathrm{T}} extraction methods. Specifically, in Ref. 4, the authors investigated eleven approaches to extract the VTV_{\mathrm{T}} and found that similar VTV_{\mathrm{T}} values in the linear regime can be extracted. In Refs. 5,6, the authors proposed the Y-function method to eliminate the RcR_{\mathrm{c}} effect when evaluating mobility values. In their studies, the VTV_{\mathrm{T}} is extracted from the ID/gm0.5I_{\mathrm{D}}/g_{\mathrm{m}}^{0.5} curve.

Uncertainty of VTV_{\mathrm{T}} induced by I-V sweeps

The threshold voltage VTV_{\mathrm{T}} uncertainties can propagate to the estimation of carrier density. Figure S2 shows an example of VTV_{\mathrm{T}} shift due to different sweeps (IDI_{\mathrm{D}}-VGSV_{\mathrm{GS}} vs. IDI_{\mathrm{D}}-VDSV_{\mathrm{DS}}) on the same device illustrated in Figure 2c.

Comparison of transfer curves from $I_{\mathrm{D}}$-$V_{\mathrm{GS}}$ and $I_{\mathrm{D}}$-$V_{\mathrm{DS}}$ sweeps

Figure S2. Comparison of transfer curves at VDS=4V_{\mathrm{DS}} = 4 V from IDI_{\mathrm{D}}-VGSV_{\mathrm{GS}} sweep (red) and extraction from IDI_{\mathrm{D}}-VDSV_{\mathrm{DS}} sweeps (black) based on data in Figure 2b,Figure 2d of the main text. The direction of the sweeps is the same (backward). A VTV_{\mathrm{T}} shift of ~0.6 V is observed comparing the IDI_{\mathrm{D}}-VGSV_{\mathrm{GS}} and IDI_{\mathrm{D}}-VDSV_{\mathrm{DS}} sweeps. We presume this shift arises from hot-carrier stress during the IDI_{\mathrm{D}}-VDSV_{\mathrm{DS}} sweeping at high VDSV_{\mathrm{DS}} and VGSV_{\mathrm{GS}}. Due to high electric fields, energetic electrons become trapped in the gate oxide as fixed charges[8], increasing the VTV_{\mathrm{T}}. This phenomenon highlights the dependence of VTV_{\mathrm{T}} on IDI_{\mathrm{D}}-VDSV_{\mathrm{DS}} sweeping.

Note S3: Extracting RcR_\mathrm{c} from TLM

Extracting RcR_\mathrm{c} from TLM data can lead to significant uncertainties. As a reminder, TLM data is a plot of the total resistance (RtotR_\mathrm{tot}) from a set of devices having all things consistent with their structure and materials except their channel length. TLM data is plotted as RtotR_\mathrm{tot} vs LchL_\mathrm{ch}, where the Rtot=Rch+2Rc=RshLch+2RcR_\mathrm{tot}=R_\mathrm{ch}+2R_\mathrm{c}=R_\mathrm{sh}L_\mathrm{ch}+2R_\mathrm{c}, which means when the channel length is zero (y-axis intercept) Rtot=2RcR_\mathrm{tot}=2R_\mathrm{c}. A reliable RcR_\mathrm{c} must be derived from TLM data that includes devices in the short-channel limit, where RcR_\mathrm{c} dominates the total resistance or at least is comparable to the RchR_\mathrm{ch}. Ideally, the sheet resistance and its variation need to be sufficiently small; otherwise, a small variation in RshR_\mathrm{sh} could lead to substantial errors in RcR_\mathrm{c}. Three examples of TLM data are presented in Figure S3, all claiming an RcR_\mathrm{c} of 500 Ω·µm, based on the intercepts to the RtotR_\mathrm{tot} axis. However, due to the larger RshR_\mathrm{sh}, the uncertainty of RcR_\mathrm{c} in TLM A is significantly larger than TLM B (e.g., a small change in RshR_\mathrm{sh} for TLM A would result in a large change in the extracted RcR_\mathrm{c}). In TLM A, the shortest channel device has an RtotR_\mathrm{tot} of 10 kΩ·µm, which is much larger than the claimed RcR_\mathrm{c} of 500 Ω·µm, whereas in TLM B, the RtotR_\mathrm{tot} is 2 kΩ·µm and the claimed RcR_\mathrm{c} is 500 Ω·µm. As noted above, with a slight variation in the RshR_\mathrm{sh} in TLM A, the RcR_\mathrm{c} might be extracted as a very small (and often untrue) value or even a negative value.

Demonstration of TLM data sets and four-probe measurements

Figure S3. a, Demonstration of TLM data sets with all RchR_\mathrm{ch}-dominant devices (TLM A, leading to unreliable RcR_\mathrm{c} extraction), all RcR_\mathrm{c}-dominant devices (TLM C, leading to unreliable RshR_\mathrm{sh} extraction), and an appropriate balance of devices (TLM B). b, Example diagram of four-probe measurements to extract RshR_\mathrm{sh}, with a back-gate as a demonstration. The channel resistance RchR_\mathrm{ch} between probe 2 and 3 is R14,23=V23/I14R_{14,23}=V_{23}/I_{14}, where I14I_{14} is the current flowing from probe 1 to 4 and V23V_{23} is the voltage between probe 2 and 3. Rsh=R14,23(W/L)R_\mathrm{sh}=R_{14,23}(W/L). RshR_\mathrm{sh} can be obtained while VGSV_\mathrm{GS} is swept, yielding RshR_\mathrm{sh} vs. VGSV_\mathrm{GS} or carrier density, which can be used to cross-examine the RshR_\mathrm{sh} extracted from TLM.

Hence, it is critical to have both of the following in a TLM: 1) devices with channel length small enough to ensure 2Rc2R_\mathrm{c} dominates RtotR_\mathrm{tot} and 2) a sufficient number of longer channel length devices to ensure a reliable RshR_\mathrm{sh} extraction based on a linear fit. Another possible scenario to avoid is illustrated with TLM C, which represents a TLM data set where all of the devices are 2Rc2R_\mathrm{c} dominated thus leading to an inaccurate estimation of RshR_\mathrm{sh}. This comparison further highlights the need for proper TLM data; as a summary, a valid TLM data set should have at least four channels and include at least one each of contact and channel resistance-dominated devices.

Since there can be considerable variation in the quality of emerging semiconducting materials, even on the same chip (e.g., variation in crystal quality in MoS2_2), this can translate to a sizeable variation in RshR_{\mathrm{sh}} from one device to another. Note, a perfect TLM is based on the assumption that RshR_{\mathrm{sh}} is the same for all devices being tested, so any disruption to this assumption translates to inaccuracy in the extraction of RcR_{\mathrm{c}}. Hence, it is highly recommended to fabricate several TLM device sets and plot the full distribution of resultant TLM data (multiple data points for each channel length). This provides evidence for how dependable the extraction is; a good example of this is in Ref. 9 and Figure S5 below.

Another critical aspect of proper TLM data sets is the need for reporting the uncertainties of RshR_{\mathrm{sh}} and RcR_{\mathrm{c}} in standard error or confidence interval from a least-squares fit of the TLM curve; an example of this can be seen in Figure 2h and Ref. 10. Lastly, if a record parameter is claimed based on TLM, four-probe measurements[7, 11] should ideally be used as a complementary method to cross-check the results. Traditionally, four-probe measurements are used to characterize the resistivity of “bulk” doped films and a gate bias is not involved. However, to estimate the RshR_{\mathrm{sh}} for emergent semiconducting materials, it is necessary to sweep the gate bias so that RshR_{\mathrm{sh}} vs. gate voltage (carrier density, nSn_{\mathrm{S}}) can be obtained. An example of the four-probe measurement is given in Figure S3. It is key to have probe 2 and 3 placed to the side of the channel so that the voltage probes (2 and 3) do not obstruct the current flow from probe 1 to 4. After obtaining RshR_{\mathrm{sh}} vs. nSn_{\mathrm{S}}, RcR_{\mathrm{c}} vs. nSn_{\mathrm{S}} can be derived by subtracting RshR_{\mathrm{sh}} from RtotR_{\mathrm{tot}}.

A final caution regarding the use of TLM data is regarding the transfer length (LTL_{\mathrm{T}}), which is the length of the contact over which the majority of carrier injection occurs between the metal and semiconductor. Traditionally, LTL_{\mathrm{T}} was also extracted from TLM data as the intercept of the linear fit with the LchL_{\mathrm{ch}} (x-axis). However, extracting LTL_{\mathrm{T}} in this manner assumes that the sheet resistance of the semiconductor in the metal-contacted region is the same as for the semiconductor in the channel region. For emergent semiconducting materials, particularly low-dimensional materials like CNTs or 2D TMDs, this is not a valid assumption as transport through the materials happens predominantly (if not entirely) on the surface and is strongly dependent on the materials interfacing with the semiconductor. Because LTL_{\mathrm{T}} has significant implications for the scalability of the contact length in emergent FETs, it must not be improperly extracted and reported from simple TLM data sets. This is commented on further in the next section (Note S4).

Additional Parameters

In the main text, we covered the most representative parameters for reporting and benchmarking emergent FETs. Here we describe some additional parameters used in specific studies.

_Normalization of IDI_{\mathrm{D}} for 1D devices:_ For 1D or close to 1D devices, to compare IDI_{\mathrm{D}}, it is sometimes necessary to convert the IDI_{\mathrm{D}} per CNT/nanowire/nanosheet stack to IDI_{\mathrm{D}} per µm. If the 1D channel materials are aligned CNTs or nanowires (Figure S4), the normalization of currents depends on the density of the 1D channel or the number of 1D channels in 1 µm. If the CNTs or nanowire are a dense network, treating the channel similar to a 2D material is more appropriate. For gate-all-around nanosheet devices (Figure S4), it is common to report IDI_{\mathrm{D}} per nanosheet stack. If reporting the IDI_{\mathrm{D}} per channel footprint, then the current per nanosheet stack should be divided by the nanosheet width (WNSW_{\mathrm{NS}}). A more detailed reporting of IDI_{\mathrm{D}} per channel width would require the calculation total channel width of the nanosheets in the stack, which is close to WNS×TNS×W_{\mathrm{NS}} \times T_{\mathrm{NS}} \times number of nanosheets in the stack. The normalized drain currents per channel width is IDI_{\mathrm{D}} per stack divided by the total channel width of the stack. Ultimately, what matters is both an indication of what is achieved on a per nanomaterial/structure basis (e.g., per CNT or per nanosheet stack) as well as what is achieved on a per aerial footprint width basis (i.e., µA per WchW_{\mathrm{ch}}).

Normalization of currents for transistors based on 1D or close to 1D channel materials

Figure S4. Normalization of currents for transistors based on 1D or close to 1D channel materials. a, top-down view of transistors based on CNTs or nanowires in the form of aligned channels and a dense network. b, side-view and top-down (aerial) view of gate-all-around nanosheet transistors.

Schottky barrier height: For Schottky contacts between metal and semiconductors, the Schottky barrier height determines the efficiency of carrier transport in the contacts. Hence, properly extracting the barrier height is key for comparing different contact engineering approaches. Examples of Schottky barrier extraction can be found in Ref. [3, 12, 13, 14], with some variances in the equations and approaches used.

Transfer length (LTL_{\mathrm{T}}): Because charge carriers tend to crowd near the contact edge when transported between the metal contacts and the channel material, only a certain portion of the contacts actively participate in the carrier transport process. The transfer length denotes the distance over which most of the current transfers in the contact. Traditionally, LTL_{\mathrm{T}} can be estimated as ρcρsh\sqrt{\frac{\rho_{\mathrm{c}}}{\rho_{\mathrm{sh}}}} from the transfer length method plot, where the ρc\rho_{\mathrm{c}} is the specific contact resistivity (unit: Ω⋅cm2\Omega\cdot\mathrm{cm}^{2}) and ρsh\rho_{\mathrm{sh}} is the sheet resistance underneath the contact (unit: Ω\Omega/square) – this is discussed in some detail in Note S3 above. However, this estimation is not reliable for emergent transistors due to: 1) many of the emergent transistors use ultra-thin, low-dimensional nanomaterials, which can alter the current crowding behavior; 2) lots of research-grade emergent transistors have gated contacts, which complicates the estimation of the sheet resistance underneath the contact; and 3) the difference in the interface between the metal-semiconductor and gate insulator semiconductor leads to further differences in sheet resistance of the semiconductor in these regions. Hence, accurately determining LTL_{\mathrm{T}} will depend on physically scaled contacts to observe the contact scaling behavior.

Interface trap density (DitD_{\mathrm{it}}): This parameter is essential for studying and evaluating novel gate dielectrics. Different methods for determining DitD_{\mathrm{it}} can be found in Ref. [12].

High-frequency response of the gate insulator capacitance: Although most of the parameters covered in the main text are low-frequency parameters, for devices to be eventually used in high-frequency and high-performance applications, it is necessary to properly evaluate the high-frequency response of the gate insulator capacitance and the current-voltage characteristics[15].

Note S5: Demonstration of device spread and parameter variations

As indicated in the main text, we recommend showing device spread and parameter variations to demonstrate the full picture of the reported devices. In Figure S5, based on ten TLM structures similar to the one used in Figure 2, we demonstrate the spread of device characteristics and parameter variations using a cumulative distribution function plot and boxplots.

Benchmarking devices with different channel thicknesses

Example benchmarking device performance of MoS2 FETs with different channel thicknesses, with panels a and b showing benchmarking plots

Figure S6. Example benchmarking device performance of MoS2\mathrm{MoS}_2 FETs with different channel thicknesses. a, Benchmarking IsatI_{\mathrm{sat}} versus nSn_{\mathrm{S}}, where the channel length in nm is labeled next to the metal contacts used in the devices. b, Benchmarking RcR_{\mathrm{c}} versus nSn_{\mathrm{S}} in a few representative reports, where the channel thickness is labeled for the multilayer channels. “a” stands for the example device in Figure 2. A few studies are plotted as dotted lines to keep the plots from cluttering and also highlight the trends. Different colors are assigned to different reported devices. Most of the data are extracted from the following published reports: transferred Ag[16], AlOx_x doped+Au[17], Ag[18], In[19], Ni[20], Cl doping[1], Ni/Gr[2], and Bi[3].

Representative reports with relatively large IsatI_{\mathrm{sat}} are listed in Table S1, with both monolayer and multilayer MoS2\mathrm{MoS}_2 channels included.

The Table lists IsatI_{\mathrm{sat}} in ascending order but not including the last three rows because they are top-gated. All other FETs were back-gated. μFE\mu_{\mathrm{FE}} is not benchmarked as several of the studies listed have overestimated values. More studies that may not have IsatI_{\mathrm{sat}} reported can be accessed at Ref. 26.

References

  1. [1]Yang, L. et al. High-Performance MoS₂ Field-Effect Transistors Enabled by Chloride Doping : Record Low Contact Resistance (0.5 κ·μm) and Record High Drain Current (460 μA/μm). in VLSI Technology (2014).
  2. [2]Liu, Y. et al. Pushing the Performance Limit of Sub-100 nm Molybdenum Disulfide Transistors. Nano Lett 16, 6337–6342 (2016).pubmed.ncbi.nlm.nih.gov/27579678
  3. [3]Shen, P.-C. et al. Ultralow contact resistance between semimetal and monolayer semiconductors. Nature 593, 211–217 (2021).DOI
  4. [4]Ortiz-Conde, A. et al. A review of recent MOSFET threshold voltage extraction methods. Microelectron. Reliab. 42, 583–596 (2002).
  5. [5]Ghibaudo, G. New method for the extraction of MOSFET parameters. Electron. Lett. 24, 543–545 (1988).DOI
  6. [6]Chang, H. Y., Zhu, W. & Akinwande, D. On the mobility and contact resistance evaluation for transistors based on MoS₂ or two-dimensional semiconducting atomic crystals. Appl. Phys. Lett. 104, 113504 (2014).DOI
  7. [7]Pang, C. et al. Mobility Extraction in 2D Transition Metal Dichalcogenide Devices—Avoiding Contact Resistance Implicated Overestimation. Small 17, 2100940 (2021).DOI
  8. [8]Streetman, B. G. & Banerjee, S. K. Solid State Electronic Devices, 6th Edition. (Pearson, 2006).
  9. [9]Kumar, A. et al. Sub-200 Ω·μm Alloyed Contacts to Synthetic Monolayer MoS₂. in IEEE International Electron Devices Meeting (IEDM) 154–157 (2021).DOI
  10. [10]Smithe, K. K. H., English, C. D., Suryavanshi, S. V. & Pop, E. Intrinsic electrical transport and performance projections of synthetic monolayer MoS₂ devices. 2D Mater. 4, (2016).DOI
  11. [11]Guros, N. B. et al. Reproducible Performance Improvements to Monolayer MoS₂ Transistors through Exposed Material Forming Gas Annealing. ACS Appl. Mater. Interfaces 11, 16683–16692 (2019).DOI
  12. [12]Schroder, D. K. Semiconductor Material and Device Characterization, 3rd Edition. (Wiley-IEEE Press, 2015).
  13. [13]Das, S., Chen, H. Y., Penumatcha, A. V & Appenzeller, J. High performance multilayer MoS₂ transistors with scandium contacts. Nano Lett 13, 100–105 (2013).DOI
  14. [14]Cheng, Z. et al. Immunity to Contact Scaling in MoS₂ Transistors Using in Situ Edge Contacts. Nano Lett. 19, 5077–5085 (2019).DOI
  15. [15]Bethge, O. et al. Process temperature dependent high frequency capacitance-voltage response of ZrO2/GeO2/germanium capacitors. Appl. Phys. Lett. 96, 052902 (2010).DOI
  16. [16]Liu, Y. et al. Approaching the Schottky-Mott limit in van der Waals metal-semiconductor junctions. Nature (2018) doi:10.1038/s41586-018-0129-8.DOI
  17. [17]McClellan, C. J., Yalon, E., Smithe, K. K. H., Suryavanshi, S. V. & Pop, E. High Current Density in Monolayer MoS₂ Doped by AlOx. ACS Nano 15, 1587–1596 (2021).DOI
  18. [18]Smithe, K. K. H., English, C. D., Suryavanshi, S. V. & Pop, E. High-Field Transport and Velocity Saturation in Synthetic Monolayer MoS₂. Nano Lett. 18, 4516–4522 (2018).DOI
  19. [19]Wang, Y. et al. Van der Waals contacts between three-dimensional metals and two-dimensional semiconductors. Nature 568, 70–74 (2019).DOI
  20. [20]Smets, Q. et al. Ultra-scaled MOCVD MoS₂ MOSFETs with 42nm contact pitch and 250μA/μm drain current. in Technical Digest - International Electron Devices Meeting, IEDM (2019). doi:10.1109/IEDM.2019.8993650.DOI
  21. [21]Patel, K. A., Grady, R. W., Smithe, K. K. H., Pop, E. & Sordan, R. Ultra-scaled MoS₂ transistors and circuits fabricated without nanolithography. 2D Mater. 7, 015018 (2020).DOI
  22. [22]Chou, A. S. et al. High On-State Current in Chemical Vapor Deposited Monolayer MoS₂ nFETs with Sn Ohmic Contacts. IEEE Electron Device Lett. 42, 272–275 (2021).DOI
  23. [23]Li, X. et al. Effect of Dielectric Interface on the Performance of MoS₂ Transistors. ACS Appl Mater Interfaces 9, 44602–44608 (2017).DOI
  24. [24]English, C. D., Smithe, K. K. H., Xu, R. L. & Pop, E. Approaching ballistic transport in monolayer MoS₂ transistors with self-aligned 10 nm top gates. Tech. Dig. - Int. Electron Devices Meet (IEDM) 5.6.1-5.6.4 (2017) doi:10.1109/IEDM.2016.7838355.
  25. [25]Zou, X. et al. Interface engineering for high-performance top-gated MoS₂ field-effect transistors. Adv. Mater. 26, 6255–6261 (2014).
  26. [26]McClellan, C. J. et al. 2D Device Trends. http://2d.stanford.edu.

Paper details

vlnc:W_xs4xgf8k
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents