Coupling between colossal charge density wave ordering and magnetism in Ho2Ir3Si5

Abstract

Ho2Ir3Si5 belongs to the family of three-dimensional (3D) R2Ir3Si5 (R = Lu, Er and Ho) compounds that exhibit a colossal first-order charge density wave (CDW) transition where there is a strong orthorhombic-to-triclinic distortion of the lattice accompanied by superlattice reflections. The analysis by single-crystal X-ray diffraction (SXRD) has revealed that the Ir-Ir zigzag chains along c are responsible for the CDW in all three compounds. The replacement of the rare earth element from non-magnetic Lu to magnetic Er or Ho lowers TCDW, where TCDWLu = 200 K, TCDWEr = 150 K and TCDWHo = 90 K. Out of the three compounds, Ho2Ir3Si5 is the only system where second-order superlattice reflections could be observed, indicative of an anharmonic shape of the modulation wave. The CDW transition is observed as anomalies in the temperature dependencies of the specific heat, electrical conductivity and magnetic susceptibility, which includes a large hysteresis of 90 to 130 K for all measured properties, thus corroborating the SXRD measurements. Similar to previously reported Er2Ir3Si5, there appears to be a coupling between CDW and magnetism such that the Ho3+ magnetic moments are influenced by the CDW transition, even in the paramagnetic state. Moreover, earlier investigations on polycrystalline material revealed antiferromagnetic (AFM) ordering at TN = 5.1 K, whereas AFM order is suppressed and only the CDW is present in our highly ordered single-crystal. First-principles calculations predict Ho2Ir3Si5 to be a metal with coexisting electron and hole pockets at the Fermi level. The Ho and Ir atoms have spherically symmetric metallic-type charge density distributions that are prone to CDW distortion. Phonon calculations affirm that the Ir atoms are primarily responsible for the CDW distortion, which is in agreement with the experiment.

Introduction

Structural phase transitions, such as the development of charge density waves (CDWs), have attracted continued interest from condensed-matter physicists and chemists. Originally, the manifestation of a CDW was proposed to originate in Fermi surface nesting (FSN), as it is present in quasi-one-dimensional metals (1D).[1] More recently, alternative mechanisms were proposed that explain, for example, the formation of CDWs by qq-dependent electron-phonon coupling (EPC) in three-dimensional (3D) CDW compounds. Examples of 3D metals with CDWs include α\alpha-Uranium,[2] CuV2S4\mathrm{CuV}_{2}\mathrm{S}_{4}[3, 4, 5, 6], La3Co4Sn13\mathrm{La}_{3}\mathrm{Co}_{4}\mathrm{Sn}_{13}7–9, RTe3\mathrm{RTe}_{3} (R=La,Sm,Gd,Tb,Dy,Ho,Er,TmR = \mathrm{La}, \mathrm{Sm}, \mathrm{Gd}, \mathrm{Tb}, \mathrm{Dy}, \mathrm{Ho}, \mathrm{Er}, \mathrm{Tm}10–12), RTe2\mathrm{RTe}_{2} (R=La,CeR = \mathrm{La}, \mathrm{Ce}[14] [13]), R5Ir4Si10\mathrm{R}_{5}\mathrm{Ir}_{4}\mathrm{Si}_{10} (R=Dy,Ho,Er,Yb,LuR = \mathrm{Dy}, \mathrm{Ho}, \mathrm{Er}, \mathrm{Yb}, \mathrm{Lu}[15]), Sm2Ru3Ge5\mathrm{Sm}_{2}\mathrm{Ru}_{3}\mathrm{Ge}_{5}[16], EuAl4\mathrm{EuAl}_{4}[17, 18, 19, 20, 21] and CuIr2−xCrxTe4\mathrm{CuIr}_{2-x}\mathrm{Cr}_{x}\mathrm{Te}_{4}[22]. In several of these compounds a coexistence and competition exists between the CDW and antiferromagnetic (AFM) order or superconductivity (SC).

In the family of compounds RNiC2\mathrm{RNiC}_{2} (R=Ce,Pr,Nd,Sm,Gd,Tb,Dy,Ho,Er,TmR = \mathrm{Ce}, \mathrm{Pr}, \mathrm{Nd}, \mathrm{Sm}, \mathrm{Gd}, \mathrm{Tb}, \mathrm{Dy}, \mathrm{Ho}, \mathrm{Er}, \mathrm{Tm}[23, 24, 25, 26, 27, 28, 29]) the CDW competes with AFM. In the case of SmNiC2\mathrm{SmNiC}_{2} ferromagnetic (FM) order completely destroys the CDW.[24, 25] On the other hand, Kolincio et al.29 have established the coexistence of a CDW and field-induced FM order in TmNiC2\mathrm{TmNiC}_{2}, suggesting strong coupling of the rare-earth spins to the CDW in these rare-earth materials. However, the magnetic susceptibility of the paramagnetic regime does not exhibit anomalies at the CDW transitions.

Er2Ir3Si5\mathrm{Er}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5} differs from most magnetic CDW compounds, in that the magnetic susceptibility of the paramagnetic state exhibits an anomaly at the CDW transition.[30] Presently, we report a similar effect for Ho2Ir3Si5\mathrm{Ho}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5}. On the other hand, the CDW of non-magnetic Lu2Ir3Si5\mathrm{Lu}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5} coexists with SC at low temperatures.[31]

Investigations of the CDW in Lu2Ir3Si5\mathrm{Lu}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5} has been extensively done.[32, 33, 34, 35] Studies by transmission electron microscopy (TEM) reported the modulation wave vector as q=σ(1ˉ21)\mathbf{q} = \sigma(\bar{1}21) with σ=0.23\sigma= 0.23–0.250.25 around 200 K.[35] Recently, the modulated crystal structure of Lu2Ir3Si5\mathrm{Lu}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5} was reported as similar to that of Er2Ir3Si5\mathrm{Er}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5}.[36] In both systems it was elucidated that the CDW resides on the zigzag chains of Ir atoms along cc. Although the rare earth element is not directly involved in the stabilization of the CDW, we have earlier proposed that it would indirectly influence the CDW through its size (atomic radius). Er has a larger atomic radius than to Lu has (2.26 vs 2.17 Å), [37] while the transition occurs 50 K lower in Er2_2Ir3_3Si5_5 than in Lu2_2Ir3_3Si5_5. Here, we find that there is no such simple relationship between atomic radius and TCDWT_{CDW}. The atomic radii of Ho and Er are equal, but TCDW=90T_{CDW} = 90 K of Ho2_2Ir3_3Si5_5 is much lower than TCDW=150T_{CDW} = 150 K of Er2_2Ir3_3Si5_5.

From SXRD we found that Ho2_2Ir3_3Si5_5 undergoes a large distortion of the lattice where the symmetry is lowered from orthorhombic (IbamIbam) to triclinic (I1ˉI\bar{1}) below the transition temperature TCDWT_{CDW}. Simultaneously, superlattice reflections appear at incommensurate positions, with values of q=[0.2494(2),0.4978(2),0.2488(2)]\mathbf{q} = [0.2494(2), 0.4978(2), 0.2488(2)] at 70 K. The CDW is supported by zigzag chains of Ir atoms in all three compounds R2_2Ir3_3Si5_5. Ho2_2Ir3_3Si5_5 differs from Lu2_2Ir3_3Si5_5 and Er2_2Ir3_3Si5_5 by the presence of second-order superlattice reflections in its SXRD, indicative of anharmonic contributions to the displacive modulation wave.

We present for Ho2_2Ir3_3Si5_5 the temperature dependencies of the electrical resistivity ρ(T)\rho(T), the specific heat Cp(T)C_p(T) and the magnetic susceptibility χ(T)\chi(T). They show anomalies in agreement with a first-order CDW transition with a hysteresis of about 40 K. Due to the strain imposed by the transition onto the crystal, it cracks which can be seen clearly from the resistivity measurements. Such cracking of crystals has also been observed in other CDW compounds, like BaFe2_2Al9_9. [38] From the magnetic susceptibility we observed that there is an influence of the CDW on the effective magnetic moment of Ho3+^{3+}, which is similar to what was reported in Er2_2Ir3_3Si5_5. [30] Such an effect of the CDW on the rare earth spin in the paramagnetic state is not commonly seen in rare earth compounds. Earlier studies have shown that the disorder in the polycrystalline material allows long-range AFM order to develop at low temperatures. [32, 33] However, in the present high-quality single crystal, long-range AFM order is absent and only the CDW is observed. Here, we elucidate the differences and similarities in the incommensurate structure of Ho2_2Ir3_3Si5_5 by comparing with Lu2_2Ir3_3Si5_5 and Er2_2Ir3_3Si5_5. Furthermore, we explore the coupling of the CDW and magnetism of Ho3+^{3+} spins and absence of long-range AFM order.

Experimental and computational details

Crystal growth and characterization

A single crystal of Ho2Ir3Si5\mathrm{Ho}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5} has been grown by the Czochralski method in a tetra-arc furnace as shown in Figure 1. We have chosen the Czochralski over flux growth or any other technique because the individual elements have high melting points. Furthermore, iridium metal does not dissolve in most of the typical fluxes. To start with, high purity individual elements of Ho : Ir : Si (99.99% for Ho and Ir, and 99.999% for Si) were taken in the stoichiometric ratio 2 : 3 : 5, amounting to about 8 to 9 g, and melted repeatedly to ensure its homogeneity. Next, a seed crystal was cut from this polycrystalline ingot for the purpose of crystal growth. The polycrystalline seed was gently inserted into the molten solution and initially pulled at a rapid speed of about 80 mm/h. The temperature of the melt was adjusted such that a necking is formed and then we employed a pulling speed of about 10 mm/h throughout the growth process. About 50 mm long ingot was pulled. Energy-dispersive X-ray spectroscopy (EDX) was used to verify the chemical composition.

Image not extracted

Figure 1. Crystal growth in a tetra arc furnace by the Czochralski method. A bar was obtained of about 50 mm length and 15 mm in diameter.

Single-crystal X-ray diffraction (SXRD): data collection and data processing.

Small pieces of single-crystalline Ho2Ir3Si5\mathrm{Ho}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5} were obtained by crushing a large single crystal, from which crystal A of dimensions 0.15×0.07×0.1 mm30.15 \times0.07 \times0.1\ \mathrm{mm}^{3} was selected for a single-crystal X-ray diffraction (SXRD) experiment at beamline P24 of PETRA-III Extension at DESY in Hamburg, Germany. SXRD was measured at station EH2 of beamline P24, employing radiation of a wavelength of λP24=0.50000 A˚\lambda_{\mathrm{P24}} = 0.50000\ \mathrm{\mathring{A}}. For further details regarding data collection refer to the supporting information. 40

The EVAL15 software suite 41 was used for processing the SXRD data. SADABS 42 was used for scaling and absorption correction, with Laue symmetry mmmmmm for the data in the periodic phase and 1‾\overline{1} for the CDW phase. As the crystal structure in the CDW phase is incommensurately modulated we had to use the superspace approach 39,43,44 to index and integrate the data. Section S2 in the supporting information 40 provides further details. The resulting reflection file was imported into JANA2006. 45,46 Table 1 gives the crystallographic information at 200 K (periodic phase) and at 70 K (incommensurate phase). The crystallographic data at other temperatures and details regarding SXRD data processing are given in the Supporting Information. 40

20070
Temperature (K)20070
Crystal systemOrthorhombicTriclinic
Space/Superspace groupIbamIbamI1ˉ(σ1 σ2 σ3)0I\bar{1}(\sigma_{1}\ \sigma_{2}\ \sigma_{3})_{0}
Space/Superspace group No.39397272 2.1.1.12.1.1.1
aa (Å)9.9023(4)9.8356(5)
bb (Å)11.3747(3)11.4902(4)
cc (Å)5.7745(3)5.7304(3)
α\alpha (deg)9089.983(3)
β\beta (deg)9091.772(2)
γ\gamma (deg)9089.975(1)
Volume (Å3^{3})650.42(5)647.32(5)
Wave vector q\mathbf{q}-(0.2494(2), 0.4978(2), 0.2488(2))
ZZ44
Wavelength (Å)0.500000.50000
Detector distance (mm)110110
2θ2\theta-offset (deg)00
χ\chi-offset (deg)-60-60
Rotation per image (deg)11
(sin⁡(θ)/λ)max⁡(\sin(\theta)/\lambda)_{\max} (Å−1^{-1})0.6835890.684039
Absorption, μ\mu (mm−1^{-1})34.82334.990
Tmin⁡T_{\min}, Tmax⁡T_{\max}0.0220, 0.05010.0230, 0.0501
Criterion of observabilityI>1.5σ(I)I > 1.5\sigma(I)I>1.5σ(I)I > 1.5\sigma(I)
Number of (m=0m = 0) reflections
measured37652706
unique (obs/all)451/4701298/1474
Number of (m=1m = 1) reflections
measured-12770
unique (obs/all)-2779/6454
Number of (m=2m = 2) reflections
measured-12725
unique (obs/all)-714/3263
RintR_{\mathrm{int}} (m=0m = 0) (obs/all)0.0487/0.04870.0287/0.0288
RintR_{\mathrm{int}} (m=1m = 1) (obs/all)-0.0828/0.1051
RintR_{\mathrm{int}} (m=2m = 2) (obs/all)-0.0967/0.1833
No. of parameters31147
RFR_{\mathrm{F}} (m=0m = 0) (obs)0.02960.0578
RFR_{\mathrm{F}} (m=1m = 1) (obs)-0.0798
RFR_{\mathrm{F}} (m=2m = 2) (obs)-0.2148
wRFwR_{\mathrm{F}} (m=0m = 0) (all)0.03800.0717
wRFwR_{\mathrm{F}} (m=1m = 1) (all)-0.0973
wRFwR_{\mathrm{F}} (m=2m = 2) (all)-0.3748
wRFwR_{\mathrm{F}} all (all)0.03800.0879
GoF (obs/all)1.83/1.331.69/1.23
Δρmin⁡\Delta\rho_{\min}, Δρmax⁡\Delta\rho_{\max} (e Å−3^{-3})-3.00, 2.94-14.56, 14.53

Table 1. Crystallographic data of crystal A of Ho2_2Ir3_3Si5_5 at 200 K (periodic phase) and 70 K (CDW phase).

Physical properties

A commercial superconducting quantum interference device (SQUID) magnetometer (MPMS5, Quantum Design, USA) was used to measure dc magnetic susceptibility in a field of 100 mT as a function of temperature from 2 to 300 K. The electrical resistivity between 1.8 and 300

K was measured by the standard dc four probe technique on a commercial physical property measurement system (PPMS, Quantum Design, USA). The specific heat data were measured both on PPMS as well as using a commercial differential scanning calorimeter (DSC) setup.

Density functional theory calculations

Density functional theory (DFT) based calculations were performed using the projector augmented wave (PAW) 47 method as implemented in the Vienna ab initio simulation package (VASP). 48 Exchange-correlation effects were included using the Perdew-Burke-Ernzerhof (PBE) 49 version of the generalized gradient approximation. A 8 × 10 × 12 Γ\Gamma-centered kk-mesh was used for the Brillouin zone (BZ) sampling with an energy cut-off of 380 eV for the plane-wave basis set. Spin-orbit coupling (SOC) effects were taken into account self-consistently to consider the relativistic effects. We employed Ho3+^{3+} potential by considering the remaining 4f4f electrons as core electrons. Experimental lattice parameters were used, while the internal atomic positions were relaxed until the residual forces on each atom were less than 0.0001 eV/Å. The VESTA 50 program was used to visualize the charge density distributions. The phonon spectrum was obtained using a 2 × 2 × 2 supercell following the frozen phonon method as implemented in the phonopy 51 package.

Results and discussion

Analysis of the CDW structure

Unlike Er2_2Ir3_3Si5_5, [30] the manifestation of the CDW appears to be sluggish in Ho2_2Ir3_3Si5_5. The crystal was initially cooled from room temperature down to 70 K, where it remained in the orthorhombic phase, despite TCDWT_{CDW} being about 90 K according to the physical property measurements.

It is possible that the crystal was cooled too rapidly, thereby not allowing it to settle in the CDW phase, and resulting in an undercooled state. Upon further lowering of the temperature to 20 K, we observed the coexistence of orthorhombic and CDW phases, indicative of a first-order transition (Figure 2 and Figure 3). The CDW phase is characterized by superlattice reflections at positions q=[0.2496(3),0.4987(3),0.2493(3)]\mathbf{q} = [0.2496(3), 0.4987(3), 0.2493(3)], accompanied by a large monoclinic distortion of the lattice (β=91.784(3)\beta= 91.784(3) deg), similar to R2Ir3Si5\mathrm{R}_2\mathrm{Ir}_3\mathrm{Si}_5 (R=Lu,ErR = \mathrm{Lu}, \mathrm{Er}) (details are given in the Supporting Information)40.

Image not extracted

Figure 2. (a), (b), (c) The h0lh0l plane, and (d), (e), (f) the hkhhkh plane reconstructed from measured SXRD data. (a), (d) are for SXRD on the periodic phase at 200 K. (b), (e) show the intermediate phase (undercooled state), where threefold splitting of the reflections can be observed at 20 K, indicating coexistence of CDW and periodic phases. (c), (f) are for SXRD on the CDW phase at 50 K, showing groups of two instead of groups of three split reflections. The degree of splitting increases with the value of hh. Panels (e) and (f) show satellite reflections of order m=2m = 2.

Image not extracted

Figure 3. Temperature dependence of (a) the lattice parameters aa, bb and cc relative to their values at T=200T = 200 K: a(200)=9.9023(4)a(200) = 9.9023(4), b(200)=11.3747(3)b(200) = 11.3747(3) and c(200)=5.7745(3)c(200) = 5.7745(3) Å; (b) the lattice parameters α\alpha, β\beta and γ\gamma; (c) the volume of the unit cell; and (d) components of the modulation wave vector q\mathbf{q}. Orange and blue symbols refer to data obtained during heating and cooling of the crystal, respectively. The undercooled state at 20 K has coexisting CDW and periodic phases.

The severity of the distortions induces a colossal strain in the crystal, causing the diffraction spots in SXRD to become broad and elongated [Figure 2(b) and Figure 2(c)], resulting in many partially overlapped reflections which cannot be used for structural analysis. Sometimes the strain is too much for the crystal to handle, such that it physically shatters, rendering it unusable for further investigations. Such destructive behaviour of the CDW has also been reported for BaFe2Al9\mathrm{BaFe}_2\mathrm{Al}_9.[38]

Another important difference to Lu2Ir3Si5\mathrm{Lu}_2\mathrm{Ir}_3\mathrm{Si}_5 and Er2Ir3Si5\mathrm{Er}_2\mathrm{Ir}_3\mathrm{Si}_5 is that we observe in SXRD on Ho2Ir3Si5\mathrm{Ho}_2\mathrm{Ir}_3\mathrm{Si}_5 second-order superlattice reflections (m=2m = 2) in addition to first-order superlattice reflections (m=1m = 1) [Figure 2(e) and Figure 2(f)]. The orthorhombic phase disappears after the crystal is heated to 50 K, and only the CDW phase remains at temperatures 50–130 K (Figure 2(c) and Figure 3). Further heating to 150 and 200 K causes the crystal to enter the orthorhombic phase and the CDW phase disappears [Figure 2(a)]. Similar to Lu2Ir3Si5\mathrm{Lu}_2\mathrm{Ir}_3\mathrm{Si}_5 and Er2Ir3Si5\mathrm{Er}_2\mathrm{Ir}_3\mathrm{Si}_5, there is a lowering of the point symmetry from orthorhombic to triclinic which causes the crystal to be twinned with four orientations.52

Figure 3 shows the temperature dependence of the lattice parameters. One can observe the clear distortion of the lattice upon entering the CDW state, including an expansion of bb and contractions of aa and cc. Furthermore, the change in lattice type at TCDWT_{\mathrm{CDW}} appears discontinuous, in agreement with the first-order character of the phase transition. Barring 20 K and 130 K as 20 K is an undercooled mixed state and 130 K is on the onset of TCDWT_{\mathrm{CDW}} warming and therefore unreliable, it can be inferred from Figure 3(d) that the modulation wave vector q\mathbf{q} decreases with temperature.

The presence of second-order satellite reflections required refinement of the crystal struc-

ture with higher order harmonics for the modulation functions. Table 2 provides a comparison of the models to see which provides the best fit to the SXRD data in the CDW phase.

ModelsABC
No. of parameters147177177
RFR_F (m=0m = 0) (obs)0.05780.05770.0535
RFR_F (m=1m = 1) (obs)0.07980.07960.0672
RFR_F (m=2m = 2) (obs)0.21480.21190.0894
wRFwR_F (m=0m = 0) (all)0.07170.07170.0695
wRFwR_F (m=1m = 1) (all)0.09730.09720.0869
wRFwR_F (m=2m = 2) (all)0.37480.37210.1319
wRFwR_F all (all)0.08790.08770.0738
GoF (obs/all)1.69/1.231.69/1.231.52/1.03
Δρmin⁡,Δρmax⁡\Delta\rho_{\min}, \Delta\rho_{\max} (e Å−3^{-3})-14.56, 14.53-14.52, 14.69-8.73, 6.14

Table 2. Quality of the fit to the SXRD data at 70 K for three structure models for the CDW phase. See text for models A, B and C. The number of unique reflections is 1298/1474 for obs/all main reflections (m=0m = 0), 2779/6454 for obs/all m=1m = 1 satellites, and 714/3263 for obs/all m=2m = 2 satellites. Criterion of observability is I>1.5σ(I)I > 1.5\sigma(I).

Model A

Here, up to second-order harmonics have been applied to holmium and iridium atoms, whereas silicon atoms have only first-order harmonics (Eq. S6 in 40). This resulted in fewer parameters and minimal changes to the results as compared to models B and C (Table 2). This model has been selected to describe the crystal structure in the CDW phase.

Model B

In this model up to second-order displacement modulation parameters have been applied to all atoms and then refined. The refinement resulted in a fit to the SXRD data that is almost identical to that of Model A. However, the second-order modulation amplitudes of the silicon atoms appear to have large standard uncertainties (s.u.’s). This is probably due to the poor scattering power of silicon as compared to holmium or iridium. Together, these features imply that the additional 30 parameters in model B do not lead to a significant improvement, and model B is not selected.

Model C

Model C builds upon model A and model B in order to try solve the issue with the high value of RFR_F for the second-order satellites. Up to third-order harmonics are used for the modulation functions of the holmium and iridium atoms, while employing only first-order harmonics for silicon atoms, as higher-order harmonics have been discarded for Si on the basis of models A and B. As a rule of thumb the highest harmonics in the modulation wave should not exceed the highest order of observed satellite reflections, the latter which is two in the present SXRD experiment. At first glance from Table 2 we see a huge improvement of the fit to the second-order satellites upon introduction of third-order harmonics. However, all these parameters have a s.u. that is larger than the refined value itself. The latter indicate that the system would have third-order satellite reflections with intensities larger than its first- and second-order satellites. As we did not observe third-order satellites, the refined values of the third-order harmonics appear to be unreliable, and model A is chosen in favor of model C.

Location of the CDW

Table S8 in the Supporting Information 40 shows the atomic coordinates at 200 K and 70 K (warming). The six crystallographically independent atoms, Ho1, Ir1, Ir2, Si1, Si2, and Si3, of the Ibam structure at 200 K split into the Ho1a, Ho1b, Ir1a, Ir1b, Ir2, Si1, Si2a, Si2b, Si3a, Si3b atoms of the triclinic structure at 70 K. Figure 4 shows the crystal structure projected onto the a-c plane at 200 K and 70 K (average structure at 70 K). Figure 4(b) appears skew compared to Figure 4(a) due to β>90\beta> 90 deg in the CDW phase. As the modulation wave vector is close to (1/4,1/2,1/4)(1/4, 1/2, 1/4), Figure 4(c) shows a 4×2×44 \times2 \times4 superstructure approximation, where one can see zigzag chains of Ir1a-Ir1b along c. Tables S9 and S10 in the Supporting Information40 show the refined modulation amplitudes.

Image not extracted

Figure 4. Projection onto the (a,c)(a,c)-plane of the crystal structures of Ho2_2Ir3_3Si5_5 for (a) 200 K and (b,c) 70 K. Panel (c) shows the 4×2×44 \times2 \times4 superstructure approximation. Large purple spheres correspond to Ho atoms; green spheres of intermediate size correspond to Ir atoms; small yellow spheres are Si atoms. Dashed lines give the distances in the basic structure, with values of 3.390 (3) and 3.728 (3) Å.

Analysis of the modulation amplitudes and distances revealed that Ho2_2Ir3_3Si5_5 follows a similar pattern as R2R_2Ir3_3Si5_5 (Lu, Er), [30, 36] such that the CDW resides on zigzag chains of Ir1a–Ir1b atoms, as they have the shortest metal-metal distances and exhibit the largest modulation of these distances (Figure 5). The lattice distortion results in alternating short and long Ir1a–Ir1b distances, where the shorter distance is the most affected by the modulation. The formation of dimers on the Ir1a–Ir1b zigzag chains along cc is responsible for the formation of the CDW.

Image not extracted

Figure 5. tt-Plot of the interatomic distances between atoms Ir1a and Ir1b (x,y,zx,y,z) and between Ir1a and Ir1b at (x,y,z−1x,y,z-1) for the crystal in the CDW phase at T=70T=70 K.

Table 3 provides a comparison of essential structural parameters between the three compounds R2R_2Ir3_3Si5_5. Our earlier proposal, that TCDWT_{\mathrm{CDW}} would be inversely proportional to the atomic radius of the rare earth element, is not confirmed by Ho2_2Ir3_3Si5_5. The atomic radius of Ho is comparable to that of Er, however TCDWT_{\mathrm{CDW}} of Ho2_2Ir3_3Si5_5 is much lower than that of Er2_2Ir3_3Si5_5. The variation of distances Ir1a–Ir1b is more or less similar in all three compounds.

CompoundLu2_2Ir3_3Si5_5Er2_2Ir3_3Si5_5Ho2_2Ir3_3Si5_5
Atomic radius of RR (Å)37{}^{37}2.172.262.26
TCDWT_{\mathrm{CDW}} (K)202–231150–16690–130
TT (K)607570
aa (Å)9.8182(3)9.8494(3)9.8356(5)
bb (Å)11.4093(3)11.4863(3)11.4902(4)
cc (Å)5.6835(2)5.7268(2)5.7304(3)
α\alpha (deg)90.001(2)90.079(1)89.983(3)
β\beta (deg)91.945(2)91.695(2)91.772(2)
γ\gamma (deg)90.018(2)90.051(1)89.975(1)
VV (Å3^{3})636.34(3)647.60(5)647.32(5)
qxq_x0.2499(3)0.2495(2)0.2494(2)
qyq_y0.4843(4)0.4973(1)0.4978(2)
qzq_z0.2386(2)0.2483(1)0.2488(2)
Distance Ir1a–Ir1ba{}^{a}
max (Å)3.801(1)3.818(2)3.801(3)
min (Å)3.711(1)3.714(2)3.719(3)
avg (Å)3.755(1)3.764(2)3.763(3)
Distance Ir1a–Ir1bb{}^{b}
max (Å)3.761(1)3.782(2)3.728(3)
min (Å)3.002(1)3.008(2)3.053(3)
avg (Å)3.385(1)3.398(2)3.390(3)

Table 3. Crystal data of the CDW phases of Lu2_2Ir3_3Si5_5, [31, 36] Er2_2Ir3_3Si5_5[30] and Ho2_2Ir3_3Si5_5 (present results). a{}^{a}Symmetry code for Ir1b (xx, yy, zz); given are the maximum (max), minimum (min) and average (avg) distances. b{}^{b}Symmetry code for Ir1b (xx, yy, z−1z - 1).

Electronic structure and phonons

The band structure of Ho2_2Ir3_3Si5_5 is shown in Figure 6(a) for several high-symmetry directions in the primitive BZ given in Figure 6(b). It is metallic such that both electron and hole pockets exist at the Fermi level. To resolve the contributions of electronic states near the Fermi energy, we show the atomic orbital projected density of states (PDOS) in Figure 6(c). The Ir states are dominant near EFE_F, whereas the Ho and Si states have lower weight than those of Ir atoms. To understand the charge density distributions of these atoms, we have shown the charge density on two different planes in the primitive unit cell, which contain Ho and Ir atoms, respectively [Figs. 6(d) and 6(e)]. The spherical charge distribution of these atoms is reminiscent of the metallic type ionic environment and suggests that these atoms are more likely to undergo CDW modulations to find a low energy state.53

Image not extracted

Figure 6. (a) Bulk electronic band structure of the orthorhombic phase of Ho2_2Ir3_3Si5_5 along various high-symmetry directions in the primitive Brillouin zone. (b) Brillouin zone with high-symmetry points. (c) Total (highlighted grey color) and orbital projected density of states (green, red, and blue lines). (d) and (e) Electronic charge density distributions on planes containing Ho and Ir atoms, respectively. (f) Phonon band structure of the orthorhombic phase, as calculated with smearing parameter σ=0.05\sigma= 0.05 eV. (g) Phonon density of states. The imaginary frequencies are represented by negative values and are mainly associated with Ir atoms. (h) Expanded view of the phonon band structure along the VV–RR–YY directions. The absence of imaginary frequencies for smearing parameter σ=0.5\sigma= 0.5 eV indicates the stability of the orthorhombic structure towards higher temperatures.

Figure 6(f) shows the phonon spectrum along various high-symmetry directions in the BZ. The system is dynamically unstable with Kohn-type54 soft modes at ZZ, RR and in be-

tween YY and UU points. The phonon PDOS Figure 6(g) shows that Ho and Ir atoms contribute to the low-frequency phonon modes, whereas high-frequency phonon modes are dominated by Si atoms. The imaginary frequencies are inherent to the Ir atoms, confirming that the CDW is associated mainly with the Ir atoms. The lowest value of negative frequency is found near the reciprocal point (0.25,0.50,0.25)(0.25, 0.50, 0.25), which is consistent with the incommensurate wave vector q\mathbf{q} found in the SXRD experiment. Figure 6(h) demonstrates the evolution of the soft phonon mode as a function of the smearing parameter σ\sigma, which represents the electronic temperature in our calculations. The soft phonon mode disappears upon increasing the smearing parameter σ\sigma from 0.05 eV to 0.5 eV. This particular dependence of the phonon frequencies on the smearing parameter (electronic temperature) indicates that the orthorhombic structure is stable only at higher temperatures as seen in our experiments.

Electrical resistivity

From Figure 7 we infer that, upon cooling the crystal, there is a sharp upward turn of the electrical resistivity at 90 K, which signifies the opening of a gap in the electronic density of states over a major fraction of the Fermi surface, in agreement with the formation of a charge density wave (CDW) at this temperature. The metallic nature of the crystal after the CDW transition indicates a partial opening of the gap at the Fermi surface. Upon heating, ρ(T)\rho(T) shows a sharp anomaly at 130 K, thereby establishing a huge hysteresis of 90–130 K. This large hysteresis and the sharpness of the transition signify that it is a first-order transition much like the one seen in R2Ir3Si5\mathrm{R}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5} (R=Lu,ErR = \mathrm{Lu}, \mathrm{Er}).[30, 31] Such a large hysteresis is uncommon for CDW transitions. Especially for incommensurate CDWs the transition usually is of second order, e.g. as found in the canonical CDW system NbSe3\mathrm{NbSe}_{3}.55

Image not extracted

Figure 7. Temperature dependence of the electrical resistivity ρ(T)\rho(T) of Ho2_2Ir3_3Si5_5. The pink and green regions indicate the periodic and CDW phases, respectively. A large hysteresis of 40 K is clearly seen. The crystal shattered on heating to above 130 K.

All measurements were made using virgin samples. After cooling and then heating through the phase transition, micro-cracks develop due to the strain induced by the transition. This feature is visible in the electrical resistivity through a lower resistivity of virgin samples than of samples that have gone through a cooling/heating cycle (Figure 7). Similar behavior has been observed for ceramic material of R2Ir3Si5\mathrm{R}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5} (R=Lu,ErR = \mathrm{Lu}, \mathrm{Er}).[32, 33] It was explained by variations of pinning of the CDW in those systems. However, it is possible that the large lattice distortions accompanying the CDW transition could be responsible for the formation of micro-cracks. This leads to a reduction of sizes of mosaic blocks, and an increase in texture, which, in turn, would cause an increase of the electrical resistance at each thermal cycle. The presence of micro-cracks is supported by the observation that the transition temperatures and hysteresis are the same in each thermal cycle. On the other hand, the increase of pinning centers would lead to a lowering of the CDW transition temperature, which is not observed here. Just as in the case of R2Ir3Si5\mathrm{R}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5} (R=Lu,ErR = \mathrm{Lu}, \mathrm{Er}),[30, 36] we observe that the electrical resistivity exhibits a T2T^{2} dependence below T=50T = 50 K, which is up to much higher temperatures than ∼10\sim10 K for a Fermi liquid, implying dominant contributions from short-range magnetic fluctuations of Ho spins in the absence of long-range magnetic ordering.

Magnetic susceptibility

The temperature-dependent magnetic susceptibility, χ(T)\chi(T), of Ho2Ir3Si5\mathrm{Ho}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5} was measured on a single crystal from the same rod as used for the other bulk measurements. Measurements were performed with a commercial superconducting quantum interference device (SQUID) magnetometer (MPMS 7, Quantum Design, USA) employing a magnetic field of 0.1 T along cc, during cooling and heating between 2 and 300 K (Figure 8). The most interesting feature

Image not extracted

Figure 8. Temperature dependence of the inverse magnetic susceptibility (1/χ(T)1/\chi(T)) of Ho2_2Ir3_3Si5_5. The upper inset shows an expanded view of 1/χ(T)1/\chi(T) versus temperature. The lower inset shows an expanded view χ(T)\chi(T) versus temperature.

of the temperature-dependent magnetic susceptibility is the noticeable increase of χ(T)\chi(T) at 90(1) K upon cooling through the CDW transition. The observed effect cannot be explained by a change of Pauli susceptibility at the transition, since the estimated magnitude of the Pauli susceptibility is at least two orders of magnitude smaller than the observed change in the susceptibility. Furthermore, one would expect a smaller Pauli susceptibility in the CDW phase, whereas we observe an increase of the susceptibility when cooling through the transition. The same transition is found at 130(1) K upon heating. The observed hysteresis is in good agreement with the hysteresis in the electrical resistivity and DSC measurements. A Curie-Weiss fit to the data at 140–300 K results in a Curie constant of C=31.78(1)C = 31.78(1) emu/mol K and an antiferromagnetic Weiss temperature of θ=−2.6(1)\theta= -2.6(1) K. A Curie-Weiss fit to the low-temperature paramagnetic regime 40–90 K results in C=32.4(1)C = 32.4(1) emu/mol K and θ=−6.3(1)\theta= -6.3(1) K. The different Curie constants correspond to different effective magnetic moments on Ho3+^{3+} of 11.27 μB\mu_B and 11.38 μB\mu_B, respectively. These values are slightly higher than the free ion magnetic moment of Ho3+^{3+} ions.

So we see that Ho2_2Ir3_3Si5_5 joins our earlier studied Er2_2Ir3_3Si5_5 [30] as yet another exceptional case in showing an effect of the CDW transition on the magnetic susceptibility. Usually, compounds containing magnetic rare-earth elements do not show any anomaly in the paramagnetic susceptibility at the high-temperature CDW transitions. This is true for many of the magnetic CDW compounds which are mentioned in the introduction. For example, the paramagnetic susceptibility of Ho5_5Ir4_4Si10_{10} does not show any anomalies at its CDW transition.56,57 The coexistence of antiferromagnetic order (TN=2T_{\mathrm{N}} = 2 K) and CDW in Ho5_5Ir4_4Si10_{10} might be related to the presence of weakly coupled 4f4f electrons of Ho3+^{3+} ions,[15] while for Ho2_2Ir3_3Si5_5 the reduced magnitude of the magnetic moments and strong coupling suggest influence of the 4f4f electrons in the CDW transition and vice versa. It is not clear, whether the small but distinct change of Ho3+^{3+} moment (11.27 μB\mu_{\mathrm{B}} vs 11.38 μB\mu_{\mathrm{B}}) across the CDW transition in a single crystal of Ho2_2Ir3_3Si5_5 could be responsible for the absence of magnetic ordering of Ho3+^{3+} moments in the crystal down to 2 K.

Specific heat

The specific heat (Cp(T)C_p(T)) of Ho2_2Ir3_3Si5_5 was measured by the thermal relaxation method, using a physical property measuring system (PPMS, Quantum Design, USA). Data obtained during heating of a single crystal of 10.5 mg from 2 to 250 K exhibit a sharp peak at the temperature of the CDW transition at 131.1 (1) K (Figure 9). We are unable to find a peak in Cp(T)C_p(T) while cooling the crystal. Similar behavior was noted earlier for a crystal of Lu2_2Ir3_3Si5_5. [31] This feature could be the result of the specific method of measurement employed in the PPMS instrument. In a second experiment, differential scanning calorimetry (DSC) was measured from 80 to 150 K on the same single crystal of Ho2_2Ir3_3Si5_5 (Figure 10). The DSC data show clear peaks at different temperatures in the heating and cooling runs, that appear at similar temperatures as are found for the electrical resistivity and magnetic susceptibility, and thus confirm the first-order character of the phase transition. The peaks appear of similar width as for Lu2_2Ir3_3Si5_5, [31] while the DSC peaks are much sharper for Er2_2Ir3_3Si5_5. [30] Since other features, like Cp(T)C_p(T) and ρ(T)\rho(T), exhibit very sharp anomalies at the CDW transition, the broadened features in the DSC signal might be related to the rate of change of temperature in this experiment in conjunction with the sluggish character of the transition.

Temperature dependence of the specific heat

Figure 9. Temperature dependence of the specific heat CpC_p from 2 to 250 K using PPMS. The inset provides an enlarged view of the CDW transition where ΔCp=60.5(1)\Delta C_p = 60.5(1) J/(mol K).

Temperature dependence of the excess specific heat $\Delta C_p$

Figure 10. Temperature dependence of the excess specific heat ΔCp\Delta C_p, obtained by subtracting a smooth baseline from the DSC signal. Blue and red circles refer to cooling and warming data. Clear peaks are observed in both cooling and warming with a hysteresis of about 40 K.

The lattice contribution to the specific heat was determined from a fit to the data far away from the transition. Subtraction of the lattice contribution resulted in ΔCp(T)\Delta C_p(T) (inset in Fig. 9). A similar value was obtained from the DSC measurement (Figure 10). The change of entropy at the transition ΔS\Delta S has been determined by integration of ΔCp(T)T\frac{\Delta C_p(T)}{T} over temperature. The values of ΔCp=60.5(1)\Delta C_p = 60.5(1) J/(mol K) and ΔS=0.6\Delta S = 0.6 J/mol are comparable to transition entropies for R5Ir4Si10R_5\mathrm{Ir}_4\mathrm{Si}_{10} and R2Ir3Si5R_2\mathrm{Ir}_3\mathrm{Si}_5. [15, 31] However, they are much larger than obtained for conventional CDW systems, such as K0.3MoO3\mathrm{K}_{0.3}\mathrm{MoO}_3 (ΔCp(max)=8\Delta C_p(\mathrm{max}) = 8 J/(mol K); ΔS=0.18R\Delta S = 0.18R)53 and NbSe3\mathrm{NbSe}_3 (ΔCp(max)=9\Delta C_p(\mathrm{max}) = 9 J/(mol K); ΔS=0.08R\Delta S = 0.08R).55 The specific heat anomaly indicates a much sharper transition for single crystals of Ho2Ir3Si5\mathrm{Ho}_2\mathrm{Ir}_3\mathrm{Si}_5 than for conventional CDW systems, which is in agreement with the first-order character of the transition as deduced from resistivity and magnetic susceptibility data.

Conclusions

We have established an incommensurately modulated crystal structure of the CDW phase of Ho2Ir3Si5\mathrm{Ho}_2\mathrm{Ir}_3\mathrm{Si}_5. The incommensurate modulation is accompanied by a strong lattice distortion, both of which are important for the modulation of interatomic distances on zigzag chains of iridium atoms along cc. This is in accordance with the CDW being supported by these zigzag chains. Similar to the case of Er2Ir3Si5\mathrm{Er}_2\mathrm{Ir}_3\mathrm{Si}_5, the rare earth atoms are not directly involved in the CDW formation. The occurrence of a large lattice distortion accounts for the sluggish character and large hysteresis of the transition, as they are apparent in the temperature dependencies of the electrical resistivity, magnetic susceptibility and specific heat. Another unique feature of the compounds R2Ir3Si5R_2\mathrm{Ir}_3\mathrm{Si}_5 (R=LuR = \mathrm{Lu}, Er\mathrm{Er} and Ho\mathrm{Ho}) is the extreme sensitivity of the phase transitions to crystalline order. The present single crystals of high perfection undergo a CDW transition, while magnetic order is suppressed down to at least 1.5 K. It is worthwhile to point out that the previous experiments on polycrystalline material did not observe the CDW transition, while magnetic order appeared below TN=5.1T_N = 5.1 K.[32, 33] The present results on Ho2Ir3Si5\mathrm{Ho}_2\mathrm{Ir}_3\mathrm{Si}_5 do not confirm the idea that TCDWT_{CDW} would scale with the atomic radius of the rare earth element. While the size of Ho is equal to that of Er, TCDWT_{CDW} is much lower for Ho2Ir3Si5\mathrm{Ho}_2\mathrm{Ir}_3\mathrm{Si}_5 than for Er2Ir3Si5\mathrm{Er}_2\mathrm{Ir}_3\mathrm{Si}_5. This absence of a correlation in the series R2Ir3Si5R_2\mathrm{Ir}_3\mathrm{Si}_5 is in contrast to the series of isostructural rare-earth compounds R5Ir4Si10\mathrm{R}_{5}\mathrm{Ir}_{4}\mathrm{Si}_{10}[15], where TCDWT_{\mathrm{CDW}} increases with increasing size of the rare earth element RR.

The SXRD data have revealed that the structure of Ho2Ir3Si5\mathrm{Ho}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5} is different from that of Lu2Ir3Si5\mathrm{Lu}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5} and Er2Ir3Si5\mathrm{Er}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5}. Although the symmetries are the same for all three compounds, the presence of second-order superlattice reflections in the CDW phase of Ho2Ir3Si5\mathrm{Ho}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5} has added more complexity to it, requiring modulation functions with up to second-order harmonics (model A in Section ).

From physical property measurements, a huge hysteresis is found of about 40 K, with the transition proceeding at 90 K (cooling) and 130 K (warming). The transition implies severe structural distortions, such that sometimes the crystal shatters. This is visible in the electrical resistivity, which is higher after cycling though the transition than before (Figure 7). The effective magnetic moment of Ho is found to change at the CDW transition, from 11.38 μB\mu_{\mathrm{B}} to 11.27 μB\mu_{\mathrm{B}} (Figure 8). This kind of coupling between CDW and magnetism is rare. It has only been observed in isostructural Er2Ir3Si5\mathrm{Er}_{2}\mathrm{Ir}_{3}\mathrm{Si}_{5}. This feature can probably be attributed to the participation of 4f4f orbitals of Ho or Er in states near the Fermi level that are involved in CDW ordering. The fact the effective moment of the rare earth is influenced by the CDW transition suggests a competition between CDW and magnetic order, with both interactions presumedly employing the same part of the Fermi surface. In order to clearly understand the mechanism for this unusual nature one would probably need microscopic probes of magnetism, such as elastic and inelastic neutron scattering.

Acknowledgement

We acknowledge DESY (Hamburg, Germany), a member of the Helmholtz Association HGF, for the provision of experimental facilities. Parts of this research were carried out at PETRA III, using beamline P24. J.-K. Bao acknowledges financial support from the Alexander-von-Humboldt foundation. The work at TIFR Mumbai was supported by the Department of Atomic Energy of the Government of India under Project No. 12-R&D-TFR-5.10-0100. This research has been funded by the Deutsche Forschungsgemeinschaft (DFG; German Research Foundation)–406658237.

Supporting Information Available

Details of the SXRD data collection, data processing and structural analysis. This material is available free of charge via the Internet at http://pubs.acs.org.

Graphical TOC Entry

Figure 11 (PDF p. 33).

References

  1. [1]Grüner, G. Charge Density Waves in Solids; Addison-Wesley: Reading, Massachusetts, 1994.
  2. [2]Marmeggi, J. C.; Delapalme, A.; Lander, G. H.; Vettier, C.; Lehner, N. Atomic displacements in the incommensurable charge-density wave in alpha-uranium. Sol. Stat. Commun. 1982, 43, 577–581.DOI
  3. [3]Fleming, R. M.; DiSalvo, F. J.; Cava, R. J.; Waszczak, J. V. Observation of Charge-Density waves in the cubic spinel structure CuV₂S₄. Phys. Rev. B 1981, 24, 2850–2853.DOI
  4. [4]Kawaguchi, S.; Kubota, Y.; Tsuji, N.; Kim, J.; Kato, K.; Takata, M.; Ishibashi, H. Structural Analysis of Spinel Compound CuV₂S₄ with Incommensurate Charge-Density Wave. J. Phys. Conf. Ser. 2012, 391, 012095.DOI
  5. [5]Okada, H.; Koyama, K.; Watanabe, K. Two-Step Structural Modulations and Fermi Liquid State in Spinel Compound CuV₂S₄. J. Phys. Soc. Jpn 2004, 73, 3227–3230.DOI
  6. [6]Ramakrishnan, S.; Schönleber, A.; Hübschle, C. B.; Eisele, C.; Schaller, A. M.; Rekis, T.; Bui, N. H. A.; Feulner, F.; van Smaalen, S.; Bag, B.; Ramakrishnan, S.;
  7. [14]Shim, J. H.; Kang, J.-S.; Min, B. I. Electronic Structures of RTe₂ (R = La, Ce): A Clue to the Pressure-Induced Superconductivity in CeTe₁.₈₂. Phys. Rev. Lett. 2004, 93, 156406.pubmed.ncbi.nlm.nih.gov/15524914
  8. [15]Ramakrishnan, S.; van Smaalen, S. Unusual ground states in R₅T₄X₁₀ (R = rare earth; T = Rh, Ir; and X = Si, Ge, Sn): a review. Rep. Prog. Phys. 2017, 80, 116501.DOI
  9. [16]Kuo, C. N.; Hsu, C. J.; Tseng, C. W.; Chen, W. T.; Lin, S. Y.; Liu, W. Z.; Kuo, Y. K.; Lue, C. S. Charge density wave like behavior with magnetic ordering in orthorhombic Sm₂Ru₃Ge₅. Phys. Rev. B 2020, 101, 155140.DOI
  10. [17]Nakamura, A.; Uejo, T.; Honda, F.; Takeuchi, T.; Harima, H.; Yamamoto, E.; Haga, Y.; Matsubayashi, K.; Uwatoko, Y.; Hedo, M.; Nakama, T.; Onuki, Y. Transport and Magnetic Properties of EuAl₄ and EuGa₄. J. Phys. Soc. Jpn 2015, 84, 124711.
  11. [18]Shimomura, S.; Murao, H.; Tsutsui, S.; Nakao, H.; Nakamura, A.; Hedo, M.; Nakama, T.; Onuki, Y. Lattice Modulation and Structural Phase Transition in the Antiferromagnet EuAl₄. J. Phys. Soc. Jpn 2019, 88, 014602.
  12. [19]Kaneko, K.; Kawasaki, T.; Nakamura, A.; Munakata, K.; Nakao, A.; Hanashima, T.; Kiyanagi, R.; Ohhara, T.; Hedo, M.; Nakama, T.; Onuki, Y. Charge-Density-Wave Order and Multiple Magnetic Transitions in Divalent Europium Compound EuAl₄. J. Phys. Soc. Jpn 2021, 90, 064704.DOI
  13. [20]Ramakrishnan, S. et al. Orthorhombic charge density wave on the tetragonal lattice of EuAl₄. IUCrJ 2022, 9, 378–385.DOI
  14. [21]Meier, W. R.; Torres, J. R.; Hermann, R. P.; Zhao, J.; Lavina, B.; Sales, B. C.; May, A. F. Thermodynamic insights into the intricate magnetic phase diagram of EuAl₄. Phys. Rev. B 2022, 106, 094421.DOI
  15. [22]Zeng, L.; Hu, X.; Wang, N.; Sun, J.; Yang, P.; Boubêche, M.; Luo, S.; He, Y.; Cheng, J.; Yao, D.-X.; Luo, H. Interplay between Charge-Density-Wave, Superconductivity, and Ferromagnetism in CuIr₂₋ₓCrₓTe₄ Chalcogenides. J. Phys. Chem. Lett. 2022, 13, 2442–2451.arxiv.org/abs/2203.04599
  16. [23]Roman, M.; Strychalska-Nowak, J.; Klimczuk, T.; Kolincio, K. K. Extended phase diagram of RNiC₂ family: Linear scaling of the Peierls temperature. Phys. Rev. B 2018, 97, 041103(R).DOI
  17. [24]Shimomura, S.; Hayashi, C.; Asaka, G.; Wakabayashi, N.; Mizumaki, M.; Onodera, H. Charge-Density-Wave Destruction and Ferromagnetic Order in SmNiC₂. Phys. Rev. Lett. 2009, 102, 076404.pubmed.ncbi.nlm.nih.gov/19257698
  18. [25]Wölfel, A.; Li, L.; Shimomura, S.; Onodera, H.; van Smaalen, S. Commensurate charge-density wave with frustrated interchain coupling in SmNiC₂. Phys. Rev. B 2010, 82, 054120.DOI
  19. [26]Shimomura, S.; Hayashi, C.; Hanasaki, N.; Ohnuma, K.; Kobayashi, Y.; Nakao, H.; Mizumaki, M.; Onodera, H. Multiple charge density wave transitions in the antiferromagnets RNiC₂ (R = Gd, Tb). Phys. Rev. B 2016, 93, 165108.
  20. [27]Kolincio, K. K.; Roman, M.; Winiarski, M. J.; Strychalska-Nowak, J.; Klimczuk, T. Magnetism and charge density waves in RNiC₂ (R = Ce, Pr, Nd). Phys. Rev. B 2017, 95, 235156.DOI
  21. [28]Maeda, H.; Kondo, R.; Nogami, Y. Multiple charge density waves compete in ternary rare-earth nickel carbides, RNiC₂ (R: Y, Dy, Ho, and Er). Phys. Rev. B 2019, 100, 104107.DOI
  22. [29]Kolincio, K. K.; Roman, M.; Klimczuk, T. Enhanced Mobility and Large Linear Non-saturating Magnetoresistance in the Magnetically Ordered States of TmNiC₂. Phys. Rev. Lett. 2020, 125, 176601.DOI
  23. [30]Ramakrishnan, S.; Schönleber, A.; Rekis, T.; van Well, N.; Noohinejad, L.; van Smaalen, S.; Tolkiehn, M.; Paulmann, C.; Bag, B.; Thamizhavel, A.; Pal, D.; Ramakrishnan, S. Unusual charge density wave transition and absence of magnetic ordering in Er₂Ir₃Si₅. Phys. Rev. B 2020, 101, 060101(R).DOI
  24. [31]Sangeetha, N. S.; Thamizhavel, A.; Tomy, C. V.; Basu, S.; Awasthi, A. M.; Rajak, P.; Bhattacharyya, S.; Ramakrishnan, S.; Pal, D. Multiple charge density wave transitions in single-crystalline Lu₂Ir₃Si₅. Phys. Rev. B 2015, 91, 205131.DOI
  25. [32]Singh, Y.; Pal, D.; Ramakrishnan, S. Low-temperature studies of the magnetic and superconducting properties of the R₂Ir₃Si₅ (R = Y, La, Ce–Nd, Gd–Tm) system. Phys. Rev. B 2004, 70, 064403.DOI
  26. [33]Singh, Y.; Pal, D.; Ramakrishnan, S.; Awasthi, A. M.; Malik, S. K. Phase transitions in Lu₂Ir₃Si₅. Phys. Rev. B 2005, 71, 045109.DOI
  27. [34]Kuo, Y. K.; Sivakumar, K. M.; Su, T. H.; Lue, C. S. Phase transitions in Lu₂Ir₃Si₅: An experimental investigation by transport measurements. Phys. Rev. B 2006, 74, 045115.DOI
  28. [35]Lee, M. H.; Chen, C. H.; Chu, M.-W.; Lue, C. S.; Kuo, Y. K. Electronically phase-separated charge-density waves in Lu₂Ir₃Si₅. Phys. Rev. B 2011, 83, 155121.
  29. [36]Ramakrishnan, S.; Schönleber, A.; Bao, J.-K.; Rekis, T.; Kotla, S. R.; Schaller, A. M.; van Smaalen, S.; Noohinejad, L.; Tolkiehn, M.; Paulmann, C.; Sangeetha, N. S.; Pal, D.; Thamizhavel, A.; Ramakrishnan, S. Modulated crystal structure of the atypical charge density wave state of single-crystal Lu₂Ir₃Si₅. Phys. Rev. B 2021, 104, 054116.DOI
  30. [37]Clementi, E.; Raimondi, D. L.; Reinhardt, W. P. Atomic Screening Constants from SCF Functions. II. Atoms with 37 to 86 Electrons. J. Chem. Phys. 1967, 47, 1300.DOI
  31. [38]Meier, W. R.; Chakoumakos, B. C.; Okamoto, S.; McGuire, M. A.; Hermann, R. P.;

Paper details

vlnc:W_xud282jk
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy