betaFeedback

WorksPhysics and Astronomy

Terahertz Time-Domain Spectroscopy as a Universal Defect Fingerprinting Tool for Organic Halide Perovskite Solar Cells

Abstract

Organic-inorganic hybrid perovskites (OHPs) deliver certified single-junction power conversion efficiencies (PCEs) exceeding 26% and perovskite-silicon tandem values surpassing 34%, yet a substantial gap with the Shockley-Queisser (S-Q) limit persists-primarily due to grain-boundary (GB) defects that drive non-radiative recombination, ion migration, and degradation. Rational passivation demands a non-contact tool capable of identifying and quantifying specific defect species in device-relevant thin films, a capability absent from conventional probes. This short review demonstrates that terahertz time-domain spectroscopy (THz-TDS, 0.3-3.0 THz) fulfills this role. Across four OHP compositions fabricated by sequential vacuum evaporation (SVE)-MAPbI3, MAPbBr3, FAPbI3, and CsPbI3-the THz spectral window captures both intrinsic phonon modes and GB-localized molecular defect vibrations, enabling species-specific, quantitative characterization at room temperature. Notably, the oscillator strength of the SVE-specific 1.58 THz absorption in MAPbI3 scales linearly with XPS-quantified CH3NH2 defect concentration, establishing THz-TDS as a direct, non-destructive defect meter. Building on these findings, we propose a three-pillar framework for THz-guided defect engineering: (I) quantitative defect measurement via oscillator-strength analysis, (II) material-specific fingerprint identification from a systematically constructed THz library, and (III) fingerprint-guided defect elimination with real-time feedback-together defining a closed-loop quality-control cycle that connects spectroscopic diagnosis to passivation strategy and, ultimately, to enhanced solar-cell efficiency.

Introduction

Organic halide perovskites (OHPs) of the ABX₃ crystal family (A=CH3NH3+\mathrm{A} = \mathrm{CH_3NH_3^+} [MA], CH(NH2)2+\mathrm{CH(NH_2)_2^+} [FA], Cs+\mathrm{Cs^+}; B=Pb2+\mathrm{B} = \mathrm{Pb^{2+}}; X=I−\mathrm{X} = \mathrm{I^-}, Br−\mathrm{Br^-}) have emerged as one of the most disruptive developments in photovoltaics over the past decade [1]. From a PCE of 3.8% in 2009, certified single-junction OHP solar cells now exceed 26.7% [2], approaching silicon in single-junction configuration and surpassing it in tandem. Longi Green Energy reported a perovskite–silicon two-terminal tandem efficiency of 34.85% in 2025, as certified by NREL [3], exceeding the Shockley–Queisser limit for single-junction devices and underscoring the transformative commercial potential of OHP technology. These advances rest on the exceptional intrinsic properties of OHPs: tunable bandgaps of 1.1–3.0 eV by halide substitution, absorption coefficients exceeding 10410^{4} cm−1^{-1}, long carrier diffusion lengths (>1> 1 μ\mum in thin films, >175> 175 μ\mum in single crystals), and scalable deposition by solution and vacuum methods [4, 5].

Despite these achievements, the gap between laboratory-record efficiencies and the Shockley–Queisser theoretical limit (∼30.5%\sim30.5\% for the ∼1.55\sim1.55 eV bandgap of MAPbI3_{3}; the absolute S–Q maximum of ∼33.7%\sim33.7\% occurs near 1.341.34 eV) remains substantial, and long-term operational stability under heat, humidity, and illumination continues to impede commercialization. Both shortcomings converge on a single root cause: defects—particularly those at grain boundaries (GBs) in polycrystalline thin films. GB defects in OHP act as deep-level non-radiative recombination centers, reducing open-circuit voltage (Voc^{\mathrm{oc}}) and fill factor (FF) below their radiative limits [6]. Ion migration through GB defect pathways drives phase segregation, halide redistribution, and irreversible degradation under operating conditions [7, 8]. Consequently, GB defect passivation has emerged as the central engineering challenge for achieving simultaneously high efficiency and stability in OHP photovoltaics. Recent strategies—including ammonium-salt treatments, sulfonium-based passivators, and ultra-thin polymer interlayers—have extended device lifetimes to over 4,500 hours under continuous illumination [9, 10].

Maximizing the impact of defect passivation strategies critically depends on the ability to identify, classify, and quantify the specific defect species present in each OHP composition and fabrication method. Yet, this remains a formidable analytical challenge. Conventional structural probes—X-ray diffraction (XRD) and scanning electron microscopy (SEM)—reveal grain morphology and crystallographic phase but are insensitive to the molecular-level chemical states of GB defects. Photoluminescence (PL) spectroscopy provides defect-density information through non-radiative recombination rates but convolutes multiple recombination pathways and cannot distinguish specific defect chemical species. X-ray photoelectron spectroscopy (XPS) directly identifies defect chemical states with high sensitivity but is surface-limited (∼10\sim10 nm probing depth), requires high-vacuum sample transfer, and cannot be applied non-destructively to device-integrated films [12]. Impedance spectroscopy accesses trap densities through device-level measurements but requires electrical contacts and cannot resolve individual defect species [13]. Consequently, comprehensive, non-contact, direct characterization of molecular defect species in OHP GB regions—the very defects that limit efficiency—remains an unmet need.

Terahertz time-domain spectroscopy (THz-TDS) operates in the 0.10.1–3.03.0 THz range (0.40.4–12.412.4 meV), a spectral window that directly overlaps with: (i) low-energy phonon vibration modes of OHP lattices (Pb–X cage vibrations, organic cation librations), (ii) molecular vibrations of defect species at grain boundaries, and (iii) intraband free-carrier dynamics. As a contact-free, non-destructive probe operating at room temperature under ambient conditions, THz-TDS is uniquely suited for direct, species-specific defect characterization. Early optical pump–terahertz probe (OPTP) studies by Poncea et al. [14] confirmed ultrafast, balanced free carriers in MAPbI3_{3} with a sum mobility (μe+μh≈25\mu_{\mathrm{e}} + \mu_{\mathrm{h}} \approx25 cm2^{2} V−1^{-1}s−1^{-1}), establishing THz-TDS as a benchmark for OHP carrier quality. Subsequent work revealed phase-dependent phonon mode transformations [11], optical phonon–carrier coupling [15], and electron–phonon interactions [16] using THz spectroscopy. Near-field THz nanoimaging recently demonstrated GB-resolved trap mapping with sub-20 nm spatial resolution [17]. Together, these studies establish THz-TDS as a powerful—yet underexploited—tool for OHP defect diagnostics.

In this short review, we present a comprehensive account of THz defect fingerprints in OHP thin films fabricated by sequential vacuum evaporation (SVE)—a scalable, substrate-universal vacuum deposition method. By systematically mapping THz fingerprints across four OHP compositions—MAPbI3_{3}, MAPbBr3_{3}, FAPbI3_{3}, and CsPbI3_3—we construct a material-specific THz defect library and show how it enables a three-pillar engineering cycle that closes the loop between defect identification and elimination, positioning THz-TDS as an indispensable quality-control tool for OHP manufacturing.

Defects in OHP Thin Films: Classification, Origin, and Impact

Defects in polycrystalline OHP thin films originate from multiple sources and manifest in distinct chemical and structural forms. Point defects—including halide vacancies (VIV_{\mathrm{I}}, VBrV_{\mathrm{Br}}), B-site vacancies (VPbV_{\mathrm{Pb}}), A-site vacancies (VMAV_{\mathrm{MA}}), interstitials (IiI_{\mathrm{i}}, Pbi\mathrm{Pb}_{\mathrm{i}}), and antisites—form within grains with formation energies governed by chemical potential [18, 19]. Among these, iodine interstitials and MA-on-Pb antisites create deep trap levels (>0.5>0.5 eV from band edges) that dominate non-radiative recombination in MAPbI3_3. Grain boundaries concentrate these point defects due to under-coordinated Pb2+^{2+} and X−^{-} sites at the lattice termination, making GBs the primary recombination-active regions in polycrystalline films [20].

The fabrication method profoundly determines GB defect chemistry. Solution-processed OHP films form GBs during solvent evaporation with residual solvent molecules and incomplete crystallization creating point-defect clusters. Vacuum-deposited films formed by SVE (sequential deposition of MAI and PbI2_2 in separate steps) create smaller, denser grain structures with higher GB area density. Critically, incomplete perovskite reaction under vacuum conditions at GBs leaves residual CH3_3NH2_2 molecular entities incorporated into the Pb–I bonding network at the GB interface—a process-specific molecular defect class absent in solution-processed films [21].

Beyond chemical point defects, structural discontinuities at phase boundaries introduce lattice strain-mediated defect states. In mixed-phase FAPbI3_3, the photoinactive δ-phase and photoactive α-phase coexist during thermal processing, creating δ/α interface regions with structurally frustrated Pb–I bonding configurations [22]. Halide compositional non-uniformity at GBs in FAPb(Br,I)3_3 leads to I-rich and Br-rich domain segregation under operating conditions [23, 24]. Characterizing these diverse defect classes across multiple OHP compositions requires a probe with molecular vibrational specificity, which conventional electrical and optical methods cannot provide.

THz-TDS Methodology and the Lorentz Harmonic Oscillator Analysis

THz-TDS measurements were performed in transmission geometry using a photoconductive antenna-based system. THz pulses were generated and detected by ZnTe(110) electro-optic crystals driven by an 800 nm femtosecond laser (35 fs pulse duration, 80 MHz repetition rate). The spectral range covered 0.2–2.5 THz with dynamic range >40>40 dB, enclosed in a dry N2_2-purged chamber to suppress atmospheric water-vapor absorption lines. OHP thin films were deposited on Al2_2O3_3 or sapphire substrates and measured at room temperature without contacts or encapsulation.

The complex optical conductivity σ~(ω)\tilde{\sigma}(\omega) was extracted from the measured complex transmission T~(ω)=T~sam(ω)/T~sub(ω)\tilde{T}(\omega) = \tilde{T}_{\mathrm{sam}}(\omega)/\tilde{T}_{\mathrm{sub}}(\omega) using the thin-film approximation [25]:

σ~(ω)=[nsub+1Z0⋅d]⋅[1−T~sam(ω)T~sub(ω)]\tilde{\sigma}(\omega) = \left[\frac{n_{\mathrm{sub}}+1}{Z_0 \cdot d}\right]\cdot\left[1-\frac{\tilde{T}_{\mathrm{sam}}(\omega)}{\tilde{T}_{\mathrm{sub}}(\omega)}\right]

where nsubn_{\mathrm{sub}} is the substrate refractive index, Z0=377 ΩZ_0 = 377\ \Omega the free-space impedance, and dd the film thickness [26].

To decompose carrier transport and phonon/defect resonances, a multi-oscillator Lorentz harmonic oscillator (LHO) model was fitted [21, 27]:

σ~(ω)=ε0⋅∑j[Ωj2γjiωωj2−ω2+iγjω]\tilde{\sigma}(\omega) = \varepsilon_0 \cdot\sum_j \left[ \frac{\Omega_j^2 \gamma_j i\omega}{\omega_j^2 - \omega^2 + i\gamma_j\omega} \right]

where ωj\omega_j, Ωj\Omega_j, and γj\gamma_j are respectively the resonance frequency, oscillator strength, and scattering rate of the jj-th mode. Defect modes are distinguished from intrinsic phonon modes by: (i) sensitivity to post-annealing treatment, (ii) correlation with XPS-quantified chemical defect concentration, and (iii) absence in solution-processed reference films.

THz Defect Fingerprint Library Across OHP Compositions

MAPbI₃: The 1.58 THz Fingerprint of CH₃NH₂ Grain-Boundary Defects

The most definitive example of a process-specific THz defect fingerprint was established in 2019 by Maeng et al. [21], who showed that SVE-fabricated MAPbI₃ thin films exhibit a strong, narrow absorption at 1.58 THz with an absorption coefficient exceeding 11,000 cm−1^{-1}—approximately two orders of magnitude above the background phonon level. Figure 1 compares the THz transmission spectra of MAPbI₃ fabricated by SVE, two-step solution, anti-solvent, and the MASnI₃. Only the SVE sample shows the 1.58 THz absorption, accounting for ~50 % suppression of THz transmission at that frequency. LHO fitting resolves three oscillators at 0.95, 1.58, and 1.87 THz, where the 0.95 and 1.87 THz modes are present in all samples as intrinsic lattice phonons, while the 1.58 THz oscillator is exclusive to SVE fabrication.

THz characterization of MAPbI₃ thin films by different fabrication methods

Figure 1. THz characterization of MAPbI3\mathrm{MAPbI_3} thin films by different fabrication methods. (a) THz waveforms and (b) transmission spectra: the SVE film uniquely shows ∼50\sim50 % suppression at 1.58 THz. (c) Absorption coefficient spectra (>11,000 cm−1>11{,}000\ \mathrm{cm}^{-1} at 1.58 THz for SVE). (d) THz absorbance decomposed into three Lorentz oscillators at 0.95, 1.58, and 1.87 THz. Reproduced from Maeng et al., Sci. Rep. 2019, 9, 5811 [21].

DFT phonon calculations on tetragonal CH3NH3PbI3\mathrm{CH_3NH_3PbI_3} reproduce the 0.95 and 1.87 THz intrinsic modes but not the 1.58 THz peak, directly pointing to a defect-related origin. XPS characterization confirms higher CH3NH2\mathrm{CH_3NH_2} molecular density at grain boundaries in SVE films: C and N 1s core-level spectra show elevated intensities at 287.0 eV and 402.7 eV (CH3NH2+\mathrm{CH_3NH_2^+} binding energies), absent in anti-solvent films. SEM reveals smaller grains and higher GB density in SVE films (RMS roughness 18.8 nm vs. 8.4 nm). (Figure 2) The 1.58 THz mode is thus assigned to vibration of the Pb−I\mathrm{Pb-I} bond structurally deformed by the co-incorporated CH3NH2\mathrm{CH_3NH_2} molecular defect at GB sites [11, 15].

XPS and surface morphology evidence for CH₃NH₂ grain-boundary defects

Figure 2. XPS and surface morphology evidence for CH3NH2\mathrm{CH_3NH_2} grain-boundary defects. (a,b) SEM images: SVE (RMS = 18.8 nm) vs. anti-solvent film (RMS = 8.4 nm). (c,d) C and N 1s1s XPS spectra confirming elevated CH3NH2+\mathrm{CH_3NH_2^+} intensities at 287.0 eV and 402.7 eV in SVE films. Reproduced from Maeng et al., Sci. Rep. 2019, 9, 5811 [21].

Quantitative Correlation: THz Oscillator Strength as a Direct Defect Density Meter

Maeng et al. [27] [27] established the quantitative value of the 1.58 THz fingerprint by systematically varying CH3NH2\mathrm{CH_3NH_2} defect density in MAPbI3\mathrm{MAPbI_3} through post-annealing under N2\mathrm{N_2} atmosphere and correlating results with XPS-derived defect concentrations. Four MAPbI3\mathrm{MAPbI_3} samples (A–D) were prepared at different annealing conditions: no anneal (A), 110 °C/45 min (B, optimal), 150 °C/10 min (C), and 150 °C/30 min (D, over-annealed).

Figure 3 shows the curve-fitting results of C 1s1s core-level spectra and extracted CH3NH2\mathrm{CH_3NH_2} relative intensity across samples A–D. The CH3NH2\mathrm{CH_3NH_2} defect concentration follows a non-monotonic trend: high in sample A (~18%), nearly eliminated in sample B (~1%), then recovered in C and D (~15%) as over-annealing decomposes the perovskite.

Quantitative defect fingerprinting in MAPbI$_3$

Figure 3. Quantitative defect fingerprinting in MAPbI3_3. (a) the curve fittings of C 1s core-level spectra for samples A–D. (b) Relative CH3_3NH2_2 peak intensity (%) vs. annealing condition: non-monotonic behavior linearly correlated with THz oscillator strength at 1.6 THz. Reproduced from Maeng et al., Nanomaterials 2020, 10, 721 [27].

LHO fitting yields oscillator strengths at 0.97, 1.62, and 2.01 THz. Only the 1.62 THz oscillator strength reproduces the same non-monotonic pattern—in direct, linear proportion to XPS-quantified CH3NH2\mathrm{CH_3NH_2} defect concentration. The 0.97 and 2.01 THz modes remain constant, confirming their intrinsic phonon origin.

This linear THz oscillator strength–defect concentration relationship establishes THz-TDS as a quantitative, contact-free defect meter that bypasses the surface-depth limitation of XPS and the species-averaging limitation of PL [12]. Eliminating this defect (Sample B, Ω\Omega(1.6 THz) ≈\approx 0) directly correlates with recovery of full OHP crystal structure and optimal device performance. This constitutes Pillar I of the three-pillar framework.

MAPbBr3_3: Defect-Immune Intrinsic Phonon Fingerprints

Maeng et al. (2020) [25] demonstrated that SVE-fabricated MAPbBr3_3 shows three sharp, stable phonon absorptions at 0.8, 1.4, and 2.0 THz completely insensitive to grain-boundary CH3_3NH2_2 defect chemistry. Despite XPS confirming substantial CH3_3NH2_2 reduction upon post-annealing, the THz phonon modes remain unchanged in frequency, oscillator strength, and linewidth (Figure 4). This contrast with MAPbI3_3 is mechanistically explained by the stronger Pb–Br bond, which resists structural deformation upon CH3_3NH2_2 incorporation and thus does not produce a defect-induced vibration shift.

Defect-immune THz phonon fingerprints of SVE-fabricated MAPbBr₃

Figure 4. Defect-immune THz phonon fingerprints of SVE-fabricated MAPbBr₃. (a) CC 1s core-level spectra before/after 150 °C annealing: CH₃NH₂ molecular defect (287.0 eV) substantially eliminated. (b) THz absorption spectra: three phonon modes at 0.8, 1.4, and 2.0 THz unchanged by defect chemistry modification. Reproduced from Maeng et al., NPG Asia Mater. 2020, 12, 53 [25].

First-principles phonon calculations using the temperature-dependent effective potential (TDEP) method on cubic MAPbBr₃ at 300 K (Figure 5) [25] assign the three modes as: 0.8 THz—transverse libration of the MA cation; 1.4 THz—longitudinal optical vibration of the Pb–Br framework; 2.0 THz—self-vibration of the Br sublattice. This DFT-level assignment provides a rigorous quantum-mechanical basis for the THz fingerprint assignments.

First-principles phonon calculations and phonon-mode visualizations

Figure 5.

Figure 5. TDEP-DFT phonon analysis of MAPbBr3\mathrm{MAPbBr}_{3}. (a) Phonon dispersion at 300 K with three IR-active branches. (b) Simulated IR absorption vs. experimental THz conductivity. (c–e) Phonon eigenvectors at 0.8, 1.4, and 2.0 THz. Reproduced from Maeng et al., NPG Asia Mater. 2020, 12, 53 [25].

MAPbBr3\mathrm{MAPbBr}_{3} thus represents the 'clean phonon' regime in the OHP THz fingerprint library: when the THz spectrum matches the DFT-predicted intrinsic phonon structure without additional oscillators, the grain boundaries harbor no THz-active molecular defect modes—a spectroscopic certificate of GB vibrational integrity. This does not exclude the possible presence of THz-silent defect states detectable only by complementary techniques.

FAPbI₃: Phase-Boundary Phonon Fingerprints

Phase control is a central challenge for FA-based perovskites: the photoactive α\alpha-FAPbI3_3 (black cubic phase) is thermodynamically metastable at room temperature and reverts to the photoinactive δ\delta-phase (yellow hexagonal phase) unless stabilized. THz-TDS provides a direct, non-destructive window into phase-boundary formation that complements XRD, offering sensitivity to the interfacial bonding state rather than the bulk crystal structure.

Maeng et al. (2021) [22] demonstrated that δ/α\delta/\alpha-mixed-phase FAPbI3_3 single-crystal surface regions, formed by controlled annealing at 140°C for 30 min, exhibit two unique THz absorption peaks at 2.0 and 2.2 THz absent from both pure δ\delta- and α\alpha-phases (Figure 6). The pure α\alpha-phase (180°C) shows a single phonon mode at ~1.45 THz. Phase assignments were confirmed by Pb 4f4f and I 4d4d core-level spectra, which show no new chemical states at the mixed-phase boundary.

Phase-sensitive THz fingerprints in FAPbI₃

Figure 6. Phase-sensitive THz fingerprints in FAPbI3_3. (a–c) Surface morphology: δ\delta-phase (as-deposited), δ/α\delta/\alpha-mixed (140°C/30 min), α\alpha-phase (180°C/30 min). (d) THz real conductivity: mixed phase uniquely shows 2.0 and 2.2 THz modes. (e,f) Pb 4f4f and I 4d4d XPS confirming phase identity. Reproduced from Maeng et al., NPG Asia Mater. 2021, 13, 75 [22].

Molecular dynamics (MD) simulations—employed here instead of static DFT to capture the thermal disorder inherent to the δ/α\delta/\alpha mixed-phase interface at finite temperature—confirm that the 2.0 and 2.2 THz modes originate from compressed Pb–I bond lengths at the structurally frustrated δ/α\delta/\alpha interface layer. These interfacial phonon modes are: (i) upshifted from the bulk α\alpha-phase 1.45 THz mode by bond compression, (ii) invisible to XRD, and (iii) uniquely correlated with the presence of a seamless phase boundary. They constitute a THz fingerprint of phase-boundary structural integrity.

In mixed-halide FAPb(BrxI1−x)3\mathrm{FAPb(Br}_{x}\mathrm{I}_{1-x}\mathrm{)}_{3}, the THz fingerprint is tunable by composition [23]. I-rich formulations (x≤0.3x \le0.3) show strong absorption at ∼1.6\sim1.6 THz from I-rich GB domains, while Br-rich compositions (x≥0.5x \ge0.5) transition toward three-phonon behavior (Figure 7). This composition–THz fingerprint map directly guides halide optimization for minimizing I-related GB defect density in FA-based tandem cells [24].

Composition-dependent THz conductivity spectra and phonon fingerprints for mixed-halide FAPb(BrₓI₁₋ₓ)₃ thin films

Figure 7. Composition-dependent THz fingerprints in FAPb(BrxI1−x)3\mathrm{FAPb(Br}_{x}\mathrm{I}_{1-x}\mathrm{)}_{3} thin films by SVE. THz conductivity spectra across the composition series: I-rich compositions show large ∼1.6\sim1.6 THz GB absorption; Br-rich compositions converge on three intrinsic phonon modes. Reproduced from Maeng et al., Appl. Phys. Express 2021, 14, 121002 [23].

γ-CsPbI₃: Grain-Size-Independent Phonon Fingerprints Confirming Defect-Free GBs

The all-inorganic γ\gamma-CsPbI3_3 (orthorhombic, black phase) is thermally stable compared to organic-cation analogs. The absence of CH3_3NH2_2 decomposition products at grain boundaries provides a direct test of whether the 1.58 THz defect fingerprint in SVE-fabricated films is uniquely tied to organic MA cation chemistry.

Maeng et al. [28] [28] fabricated γ\gamma-CsPbI3_3 films by SVE with three grain sizes (A: 300 nm, B: 350 nm, C: 460 nm) and measured THz conductivity (Figure 8). All three samples show three clean phonon absorption peaks at 0.9, 1.5, and 1.8 THz with no additional absorption. Both resonance frequencies and oscillator strengths are entirely grain-size-independent. DFT phonon calculations assign the three modes as: 0.9 THz (Cs rattling mode), 1.5 THz (Pb–I–Pb bending), and 1.8 THz (Pb–I stretching).

Grain-size-independent THz phonon fingerprints in $\gamma$-CsPbI$_3$ thin films

Figure 8. Grain-size-independent THz phonon fingerprints in γ\gamma-CsPbI3_3 thin films. (a) Real conductivity for samples A (300 nm), B (350 nm), C (460 nm): identical three-phonon spectra. (b) LHO resonance frequencies and oscillator strengths vs. grain size: no dependence observed. (c–e) Individual LHO component fits for A, B, C. Reproduced from Maeng et al., Mater. Today Phys. 2023, 30, 100960 [28].

The complete absence of grain-size-dependent THz absorption in γ\gamma-CsPbI3_3 confirms: (i) SVE does not introduce molecular defects at CsPbI3_3 grain boundaries; and (ii) the THz fingerprint is a reliable, grain-size-independent indicator of GB chemical integrity. The stark contrast between the defect-active 1.58 THz mode in MAPbI3_3 and the defect-free three-phonon spectrum of γ\gamma-CsPbI3_3 provides compelling evidence that the 1.58 THz fingerprint is a molecular-chemistry-specific signal, not a structural grain-boundary artifact.

The Three-Pillar THz Defect Engineering Framework

The THz fingerprint library presented above directly enables a three-pillar engineering framework that links spectroscopic defect identification to process optimization and device performance enhancement. Figure 9 illustrates the interconnected cycle: Pillar I provides quantitative measurement capability, Pillar II supplies compositional context, and Pillar III closes the engineering loop through targeted defect elimination.

Schematic of the three-pillar THz defect engineering framework

Figure 9. Schematic of the three-pillar THz defect engineering framework. Three interconnected pillars—(I) quantitative defect measurement, (II) universal fingerprint library, and (III) fingerprint-guided defect elimination—operate in a continuous cycle around the central THz-TDS engine, converting raw spectral data into actionable process feedback for OHP solar cell manufacturing.

Pillar I—Quantitative Defect Measurement

The linear correlation between Ω(1.6 THz)\Omega(1.6\ \mathrm{THz}) and XPS-quantified CH₃NH₂ concentration [27] transforms THz oscillator strength into a non-contact defect concentration meter. The measurement uncertainty, estimated from repeated LHO fits on identically prepared films, is <5% for films >100 nm [27]; spectral isolation of the 1.6 THz mode from the 0.97 and 2.0 THz phonons enables unambiguous LHO decomposition; and room-temperature ambient measurement eliminates the vacuum-sample-transfer requirement of XPS. This enables: (i) substrate-by-substrate, process-step-resolved defect quantification; (ii) inline monitoring of post-annealing conditions without device fabrication; and (iii) tracking of defect density evolution across roll-to-roll SVE production sequences.

Pillar II—Universal THz Fingerprint Library

The four OHP systems reviewed define a material-specific THz fingerprint library (Table 1) spanning defect-active, defect-immune, phase-sensitive, and composition-tunable regimes. This library enables unambiguous spectroscopic discrimination of: (i) fabrication method (SVE vs. solution-processed, through presence/absence of 1.58 THz mode); (ii) OHP composition (distinct phonon frequencies for MA, FA, Cs); (iii) crystallographic phase (δ\delta vs. α\alpha vs. δ/α\delta/\alpha-mixed through 1.45 vs. 2.0/2.2 THz modes); and (iv) halide composition (THz oscillator strength map for FAPb(Br,I)3_3 series). No single conventional technique provides this combination of information non-destructively from a single measurement.

OHP SystemTHz Modes (THz)Defect SensitivityPhysical AssignmentRef.
MAPbI₃ (SVE)0.95/1.58*/1.87Strongly defect-active (1.58 THz)*CH₃NH₂ mol. defect at GB; others = bulk phonons[21, 27]
MAPbBr₃ (SVE)0.8/1.4/2.0Defect-immuneAll intrinsic phonons (TDEP-DFT verified)[25]
δ/α-FAPbI₃1.45/2.0*/2.2*Phase-boundary sensitive*Interfacial phonons at seamless δ/α boundary[22]
FAPb(BrₓI₁₋ₓ)₃Composition-dep.Halide-composition-tunableI-rich: GB absorption; Br-rich: intrinsic phonons[23]
γ-CsPbI₃ (SVE)0.9/1.5/1.8Grain-size independentBulk phonons; defect-free GB confirmed[28]

Table 1. THz defect fingerprint library for SVE-fabricated OHP thin films. Asterisk (*) denotes defect- or phase-boundary-specific modes.

Pillar III—Fingerprint-Guided Defect Elimination

The THz fingerprint provides immediate, quantitative feedback for elimination strategies. Thermal post-annealing at 110°C for 45 min in N2_2 reduces Ω\Omega(1.6 THz) from ~0.37 to near zero in MAPbI3_3 [27]. Electric-bias treatment (15 V) of MAPbBr3_3 single-crystal surfaces eliminates 55% of CH3_3NH2_2 through field-driven ionic migration [29]. Ultra-thin P3HT (7 nm) HTL deposition creates a chemically clean interface and provides 2-week air stability protection [30]. Advanced sequential ligand strategies such as the two-step dedicated-ligand approach by Choy et al. [31]—applying DFABr for grain boundaries and 4APPBr2_2 for grain surfaces—have demonstrated >93% PCE retention after 3,000 hours under high humidity; THz defect fingerprinting before and after such treatments directly quantifies elimination efficacy, providing a spectroscopic certificate of passivation.

PillarCore CapabilityKey EvidenceApplication
ITHz oscillator strength Ω\Omega(1.6 THz) as contact-free defect meter (<5% uncertainty)Linear Ω\Omega–[CH3_3NH2_2] correlation in MAPbI3_3 (samples A–D) [27]Substrate-by-substrate process monitoring; inline SVE QC without device fabrication
IIMaterial-specific THz fingerprint database spanning 4 OHP systemsDefect-active (MAPbI3_3), immune (MAPbBr3_3), phase-sensitive (FAPbI3_3), tunable (FAPb(Br,I)3_3), inorganic-clean (γ\gamma-CsPbI3_3) [21, 22, 23, 24, 25, 26, 27, 28]Non-contact discrimination of composition, phase, and halide ratio in a single scan
IIITHz fingerprint as real-time feedback loop for defect eliminationN2_2 anneal (110°C/45 min): Ω\Omega→0 [27]; E-bias: 55% CH3_3NH2_2 eliminated [29]; P3HT HTL: 2-week stability [30]Iterative passivation optimization without full device fabrication

Table 2. The three-pillar THz defect engineering framework: capabilities, evidence base, and application scope.

Discussion

The THz defect fingerprint approach occupies a unique position in the OHP characterization landscape. Early OPTP-THz studies focused on carrier mobility and dynamics [14], establishing THz-TDS as a benchmark for transport quality but not defect identity. Temperature-dependent Time-Resolved Terahertz Spectroscopy (TRTS) by Milot et al. [32] demonstrated how charge-carrier recombination and mobility in MAPbI3\mathrm{MAPbI}_{3} evolve across phase transitions. Transmission THz-TDS studies by La-o-vorakiat et al. [11] and Sendner et al. [15] mapped intrinsic phonon modes and their coupling to carrier transport. Near-field THz nanoimaging by Kim et al. [17] spatially resolved GB trap filling with <20<20 nm resolution—a nanoscale complement to the far-field oscillator strength approach. Hempel et al. [33] demonstrated that THz and microwave transient measurements alone can quantitatively predict PCE of perovskite solar cells, bridging the gap between non-contact spectroscopy and device-level benchmarking.

Table 3 compares THz-TDS against principal competing characterization techniques. Compared to PL: THz oscillator strength is immune to reabsorption, surface passivation artifacts, and excitation-dependent injection. Compared to impedance spectroscopy: THz-TDS requires no contacts and accesses THz-frequency lattice dynamics inaccessible to kHz–MHz impedance measurements. Compared to XPS: THz-TDS is non-destructive, non-contact, operates under ambient conditions, and probes the entire film depth.

CriterionTHz-TDSXPSPLImpedanceXRD/SEM
Defect species ID✓ Direct✓ Direct✗ Indirect✗ Indirect✗ None
Non-contact✓✗ UHV✓✗ Contacts✓
Non-destructive✓Partial✓Partial✓
Quantitative✓ LinearPartialPartialPartial✗
Ambient/RT✓✗✓Partial✓
Full-depth probe✓✗ ~10 nm✓✓✓
Phase sensitivity✓ Interfacial✗Limited✗✓ Bulk

Table 3. Comparative capabilities of THz-TDS vs. conventional OHP defect characterization methods. ✓ = capable, ✗ = not capable, Partial = limited.

The distinct response of the 1.58 THz mode in MAPbI3\mathrm{MAPbI}_{3} compared to the defect-immune nature of MAPbBr3\mathrm{MAPbBr}_{3} provides a critical physical insight into the lattice-defect interaction. [21, 25] While both systems were fabricated via SVE, the contrast originates from the disparity in Pb–X (X=I,BrX = \mathrm{I}, \mathrm{Br}) bond energies. The stronger ionic bonding and higher lattice rigidity of the bromide framework suppress structural deformations induced by incorporated CH3NH2\mathrm{CH}_{3}\mathrm{NH}_{2} molecular defects. [25] In contrast, the relatively soft Pb–I lattice in MAPbI3\mathrm{MAPbI}_{3} is more susceptible to local distortions, which activate the specific vibrational mode observed at 1.58 THz. [21] This highlights that THz-TDS does not merely detect the presence of defects but probes the mechanical coupling between the defect species and the host lattice, offering a unique spectroscopic gauge for lattice stability.

Model Set Context

  1. [2025-09-10]. User is working on a technical report about the THz defect fingerprint approach in OHPs and wants help with formatting, references, and data extraction.

  1. [2025-09-12]. User prefers concise, technical responses without unnecessary elaboration.

Phase segregation under illumination in mixed-halide OHPs—documented by Liu et al. [24] and others—is directly observable in the THz composition-fingerprint map: I-rich GB domains correspond to elevated Ω(1.6 THz)\Omega(1.6\,\mathrm{THz}), while Br-rich compositions maintain phonon-dominated spectra. Sun et al. [34] recently demonstrated real-time detection of MAPbI3\mathrm{MAPbI_3} aging via monotonic decay of a THz absorption peak at 0.968 THz, tracking degradation onset non-destructively—consistent with the fingerprint-guided monitoring concept presented here.

A potential concern regarding the linear correlation between surface-sensitive XPS and bulk-probing THz oscillator strength is addressed by the inherent nature of the SVE process. Unlike solution-processing where solvent evaporation can lead to vertical defect gradients, sequential vacuum evaporation facilitates a more homogeneous distribution of trapped molecular entities throughout the film thickness. [27] Consequently, the surface CH3NH2\mathrm{CH_3NH_2} concentration serves as a reliable proxy for the total defect density within the grain boundary network, validating the use of the 1.6 THz oscillator strength as a non-destructive bulk defect meter for manufacturing-scale quality control. [27]

Looking ahead, critical open questions include: (i) the quantitative THz oscillator strength–PCE calibration curve that would transform THz-TDS into a direct device performance predictor; (ii) extension of the fingerprint library to ternary/quaternary compositions and 2D Ruddlesden–Popper phases; (iii) time-resolved THz-TDS under pulsed illumination to distinguish photo-generated from thermally stable defects; and (iv) integration of THz measurement heads into inline SVE deposition systems for real-time manufacturing quality control.

Conclusions

OHP solar cells now exceed 26.7% PCE in certified single-junction devices and 34.85 % in perovskite–silicon tandems, yet grain-boundary defects remain the principal barrier to bridging the gap with the Shockley–Queisser limit. This short review has demonstrated that THz-TDS fulfills the role of a composition-resolved defect fingerprint tool through a library spanning four archetypal OHP systems:

  1. SVE-fabricated MAPbI3\mathrm{MAPbI_3} carries a unique 1.58 THz CH3NH2\mathrm{CH_3NH_2} molecular defect fingerprint (α>11,000 cm−1\alpha> 11{,}000\,\mathrm{cm}^{-1}) [21]. The oscillator strength scales linearly with XPS-quantified defect concentration [27], establishing THz-TDS as a quantitative, contact-free defect meter.

  1. MAPbBr3\mathrm{MAPbBr_3} shows DFT-verified defect-immune THz phonon modes at 0.8, 1.4, and 2.0 THz, defining the 'clean grain boundary' spectroscopic benchmark for bromide-based compositions [25].

  1. δ/α\delta/\alpha-mixed FAPbI3\mathrm{FAPbI_3} displays interfacial phonon modes at 2.0 and 2.2 THz from seamless phase boundaries—invisible to XRD but accessible by THz—enabling non-contact phase-boundary quality assessment [22].

  1. FAPb(Br,I)3\mathrm{FAPb(Br,I)_3} provides a composition-tunable THz map from defect-active (I-rich, ∼\sim1.6 THz) to defect-immune (Br-rich, phonon-dominated), directly guiding halide ratio optimization [23].

  1. γ\gamma-CsPbI3\mathrm{CsPbI_3} shows grain-size-independent bulk phonon modes at 0.9, 1.5, and 1.8 THz, confirming defect-free grain boundaries in all-inorganic perovskite absent of organic cation chemistry [28].

Looking forward, the establishment of a direct 'THz Fingerprint–to–PCE' calibration curve will be the final step in transitioning THz-TDS from a laboratory diagnostic tool to a predictive manufacturing engine. [33] By integrating THz measurement heads directly into inline SVE deposition systems, real-time feedback loops can be realized to optimize passivation strategies without the need for full device fabrication. This shift toward spectroscopy-guided manufacturing offers a scalable and cost-effective pathway to close the remaining efficiency gap with the Shockley–Queisser limit, ensuring both the high performance and long-term reliability required for the commercialization of perovskite photovoltaics.

Author Contributions: Conceptualization, I.M. and M.-C.J.; Writing—Original Draft Preparation, I.M. and Y.M.L.; Writing—Review & Editing, S.J.O. and M.-C.J.; Supervision, I.M. and M.-C.J. All authors have read and agreed to the published version of the manuscript.

Funding: This work was supported by

Institutional Review Board Statement: Not applicable.

Informed Consent Statement: Not applicable.

Data Availability Statement: The raw data supporting the conclusions of this article will be made available by the authors on request.

Conflicts of Interest: The authors declare no conflicts of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript; or in the decision to publish the results.

References

  1. [1]Stoumpos, C.C.; Malliakas, C.D.; Kanatzidis, M.G. Semiconducting tin and lead iodide perovskites with organic cations: Phase transitions, high mobilities, and near-infrared photoluminescent properties. Inorg. Chem. 2013, 52, 9019–9038. https://doi.org/10.1021/ic401371n
  2. [2]NREL Best Research-Cell Efficiency Chart. National Renewable Energy Laboratory (NREL), 2025. Available online: https://www.nrel.gov/pv/cell-efficiency.html (accessed on 1 March 2025).DOI
  3. [3]Longi Green Energy Technology Co., Ltd. Perovskite/Silicon Tandem Solar Cell Efficiency 34.85%, Certified by NREL, 2025.
  4. [4]Park, N.-G.; Asghar, M.I. Achievements, challenges, and future prospects for industrialization of perovskite solar cells. Light Sci. Appl. 2024, 13, 163. https://doi.org/10.1038/s41377-024-01501-6
  5. [5]Herz, L.M. Charge-carrier dynamics in organic–inorganic metal halide perovskites. Annu. Rev. Phys. Chem. 2016, 67, 65–89. https://doi.org/10.1146/annurev-physchem-040215-112222
  6. [6]Ball, J.M.; Petrozza, A. Defects in perovskite-halides and their effects in solar cells. Nat. Energy 2016, 1, 16149. https://doi.org/10.1038/nenergy.2016.149
  7. [7]Lin, Y.; Bai, Y.; Fang, Y.; Wang, Q.; Deng, Y.; Huang, J. Suppressed ion migration in low-dimensional perovskites. ACS Energy Lett. 2017, 2, 1571–1577. https://doi.org/10.1021/acsenergylett.7b00442
  8. [8]Futscher, M.H.; Lee, J.M.; McGovern, L.; Muscarella, L.A.; Wang, T.; Haider, M.I.; Fakharuddin, A.; Schmidt-Mende, L.; Ehrler, B. Quantification of ion migration in CH₃NH₃PbI₃ perovskite solar cells by transient capacitance measurements. Mater. Horiz. 2019, 6, 1497–1503. https://doi.org/10.1039/C9MH00445A
  9. [9]Jeong, M.; Choi, I.W.; Go, E.M.; Cho, Y.; Kim, M.; Lee, B.; Jeong, S.; Jo, Y.; Choi, H.W.; Lee, J.; et al. Stable perovskite solar cells with efficiency exceeding 24.8% and 0.3-V voltage loss. Science 2020, 369, 1615–1620. https://doi.org/10.1126/science.abb7167
  10. [10]Zhang, S.; Ye, F.; Wang, X.; Chen, R.; Zhang, H.; Zhan, L.; Jiang, X.; Li, Y.; Ji, X.; Liu, S.; et al. Minimizing buried interfacial defects for efficient inverted perovskite solar cells. Science 2023, 380, 404–409. https://doi.org/10.1126/science.abq4573
  11. [11]La-o-vorakiat, C.; Xia, H.; Kadro, J.; Salim, T.; Zhao, D.; Ahmed, T.; Lam, Y.M.; Zhu, J.-X.; Marcus, R.A.; Michel-Beyerle, M.-E.; et al. Phonon mode transformation across the orthorhombic–tetragonal phase transition in CH₃NH₃PbI₃ by terahertz time-domain spectroscopy. J. Phys. Chem. Lett. 2016, 7, 1–6. https://doi.org/10.1021/acs.jpclett.5b02523
  12. [12]Siekmann, J.; Ravishankar, S.; Kirchhartz, T. Apparent defect densities in halide perovskite thin films and single crystals. ACS Energy Lett. 2021, 6, 3244–3251. https://doi.org/10.1021/acsenergylett.1c01449
  13. [13]Srivastava, S.; Ranjan, S.; Yadav, L.; Sharma, T.; Choudhary, S.; Agarwal, D.; Singh, A.; Satapathi, S.; Gupta, R.K.; Garg, A.; et al. Advanced spectroscopic techniques for characterizing defects in perovskite solar cells. Commun. Mater. 2023, 4, 52. https://doi.org/10.1038/s43246-023-00378-5
  14. [14]Ponseca, C.S.; Savenije, T.J.; Abdulkarim, M.; Trinh, M.T.; Salim, T.; Lam, Y.M.; Sundström, V.; Yartsev, A. Organometal halide perovskite solar cell materials rationalized: Ultrafast charge generation, high and microsecond-long balanced mobilities. J. Am. Chem. Soc. 2014, 136, 5189–5192. https://doi.org/10.1021/ja412583t
  15. [15]Sendner, M.; Nayak, P.K.; Egger, D.A.; Beck, S.; Müller, C.; Löhrer, B.; Kronik, L.; Snaith, H.J.; Bunz, U.H.F.; Pucci, A. Optical phonons in methylammonium lead halide perovskites and implications for charge transport. Mater. Horizons 2016, 3, 613–620. https://doi.org/10.1039/C6MH00275G
  16. [16]Wright, A.D.; Verdi, C.; Milot, R.L.; Eperon, G.E.; Pérez-Osorio, M.A.; Snaith, H.J.; Giustino, F.; Johnston, M.B.; Herz, L.M. Electron–phonon coupling in hybrid lead halide perovskites. Nat. Commun. 2016, 7, 11755. https://doi.org/10.1038/ncomms11755
  17. [17]Kim, H.; Hunger, J.; Canovès-Valiente, E.; Bonn, M.; Turchinovich, D. Terahertz nanoimaging of perovskite solar cell materials. ACS Photonics 2022, 9, 3550–3556. https://doi.org/10.1021/acsphotonics.2c00864
  18. [18]Meggiolaro, D.; Motti, S.G.; Mosconi, E.; Barker, A.J.; Ball, J.M.; Perini, C.A.R.; Deschler, F.; Petrozza, A.; De Angelis, F. Iodine chemistry determines the defect tolerance of lead-halide perovskites. Energy Environ. Sci. 2018, 11, 702–713. https://doi.org/10.1039/C8EE00124C
  19. [19]Yin, W.-J.; Shi, T.; Yan, Y. Unusual defect physics in CH₃NH₃PbI₃ perovskite solar cell absorber. Appl. Phys. Lett. 2014, 104, 063903. https://doi.org/10.1063/1.4864778
  20. [20]Yun, J.S.; Ho-Baillie, A.; Huang, S.; Woo, S.H.; Heo, Y.; Seidel, J.; Huang, F.; Cheng, Y.-B.; Green, M.A. Benefit of grain boundaries in organic–inorganic halide planar perovskite solar cells. J. Phys. Chem. Lett. 2015, 6, 875–880. https://doi.org/10.1021/acs.jpclett.5b00182
  21. [21]Maeng, I.; Cheon, W.; Lee, J.; Shin, J.; Noh, C.; Park, S.; Oh, S.J.; Kang, M.; Jung, M.-C. Significant terahertz absorption of methylammonium lead iodide perovskite originating from the grain boundary. Sci. Rep. 2019, 9, 5811. https://doi.org/10.1038/s41598-019-42226-w
  22. [22]Maeng, I.; Lee, J.; Shin, J.; Jung, M.-C. Unusual terahertz-wave absorptions in δ/α-mixed-phase FAPbI₃ single crystals from interfacial phonon vibration modes. NPG Asia Mater. 2021, 13, 75. https://doi.org/10.1038/s41427-021-00345-x
  23. [23]Maeng, I.; Lee, J.; Jung, M.-C. Halogen-composition-dependent terahertz phonon modes of FAPb(Br₁−xIₓ)₃ hybrid perovskite thin films by sequential vacuum evaporation. Appl. Phys. Express 2021, 14, 121002. https://doi.org/10.35848/1882-0786/ac3472
  24. [24]Liu, Y.; Lorenz, M.; Merdasa, A.; Petrov, A.I.; Ostrovt­sov, S.; Scheblykin, I.G.; Meerholz, K.; Herz, L.M. Phase segregation in mixed-halide perovskites affects charge-carrier dynamics while preserving mobility. Nat. Commun. 2021, 12, 6249. https://doi.org/10.1038/s41467-021-26461-w
  25. [25]Maeng, I.; Lee, J.; Shin, J.; Cheon, W.; Noh, C.; Park, S.; Jung, M.-C. Stable three-phonon modes of methylammonium lead bromide thin film verified by terahertz time-domain spectroscopy and density functional theory. NPG Asia Mater. 2020, 12, 53. https://doi.org/10.1038/s41427-020-0235-6
  26. [26]Nienhuys, H.-K.; Sundström, V. Influence of plasmons on terahertz conductivity measurements. Appl. Phys. Lett. 2005, 87, 012101. https://doi.org/10.1063/1.1984080
  27. [27]Maeng, I.; Lee, J.; Shin, J.; Cheon, W.; Jung, M.-C. Strong linear correlation between CH₃NH₂ molecular defect and THz oscillator strength in methylammonium lead iodide perovskite thin films. Nanomaterials 2020, 10, 721. https://doi.org/10.3390/nano10040721
  28. [28]Maeng, I.; Lee, J.; Jung, M.-C. Grain-boundary-independent terahertz phonon modes in γ-CsPbI₃ inorganic perovskite thin films. Mater. Today Phys. 2023, 30, 100960. https://doi.org/10.1016/j.mtphys.2022.100960
  29. [29]Lee, J.; Maeng, I.; Jung, M.-C. Electric-field-induced reduction of CH₃NH₂ molecular defect state in MAPbBr₃ single crystal surface. Appl. Surf. Sci. 2021, 542, 148536. https://doi.org/10.1016/j.apsusc.2020.148536
  30. [30]Jung, M.-C.; Lee, J.; Maeng, I.; Cheon, W.; Noh, C.; Park, S. Clean interface between poly-3-hexylthiophene hole transport layer and MAPbI₃ perovskite. Sci. Rep. 2019, 9, 10835. https://doi.org/10.1038/s41598-019-47342-5
  31. [31]Choy, W.C.H.; et al. Sequential organic ligand modifications to dedicatedly restructure grain boundary and surface of perovskites. Nat. Commun. 2025, 16, 11502. https://doi.org/10.1038/s41467-025-56811-3
  32. [32]Milot, R.L.; Eperon, G.E.; Snaith, H.J.; Johnston, M.B.; Herz, L.M. Temperature-dependent charge-carrier dynamics in CH₃NH₃PbI₃ perovskite thin films. Adv. Funct. Mater. 2015, 25, 6218–6227. https://doi.org/10.1002/adfm.201502340
  33. [33]Hempel, H.; Savenjie, T.J.; Stolterfoht, M.; Unold, T.; Sievers, V.; Kaufmann, C.A.; Vargas-Castrillon, A.; Merdasa, A.; Saidaminov, M.I.; et al. Predicting solar cell performance from terahertz and microwave spectroscopy. Adv. Energy Mater. 2022, 12, 2102776. https://doi.org/10.1002/aenm.202102776
  34. [34]Sun, Y.; Zhao, F.; Chen, M.; Li, Y.; Ma, Z.; Liang, W.; Li, H.; Zhang, J.; Zhu, J. Real-time detection of aging status of methylammonium lead iodide perovskite thin films by using terahertz time-domain spectroscopy. Front. Optoelectron. 2024, 17, 19. https://doi.org/10.1007/s12200-024-00117-x

Paper details

vlnc:W_xwvraery
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…