betaFeedback

WorksPhysics and Astronomy

Room temperature ferroic orders in Zr and (Zr, Ni) doped SrTiO3_3

Abstract

We synthesized strontium titanate SrTiO3_3 (STO), Zr doped Sr1-xZrxTiO3\text{Sr}_\text{1-x}\text{Zr}_\text{x}\text{Ti}\text{O}_3 and (Zr, Ni) co-doped Sr1-xZrxTi1-yNiyO3\text{Sr}_\text{1-x}\text{Zr}_\text{x}\text{Ti}_\text{1-y}\text{Ni}_\text{y}\text{O}_3 samples using solid state reaction technique to report their structural, electrical and magnetic properties. The cubic PmPm-3m3m phase of the synthesized samples has been confirmed using Rietveld analysis of the powder X-ray diffraction pattern. The grain size of the synthesized materials was reduced significantly due to Zr doping as well as (Zr, Ni) co-doping in STO. The chemical species of the samples were identified using energy-dispersive X-ray spectroscopy. We observed forbidden first order Raman scattering at 148, 547 and 797 cm−1^{-1} which may indicate nominal loss of inversion symmetry in cubic STO. The absence of absorption at 500 cm−1^{-1} and within 600-700 cm−1^{-1} band in Fourier Transform Infrared spectra corroborates Zr and Ni as substitutional dopants in our samples. Due to 4% Zr doping in Sr0.96Zr0.04TiO3\text{Sr}_\text{0.96}\text{Zr}_\text{0.04}\text{Ti}\text{O}_3 sample dielectric constant, remnant electric polarization, remnant magnetization and coercivity were increased. Notably, in the case of 4% Zr and 10% Ni co-doping we have observed clearly the existence of both FE and FM hysteresis loops in Sr0.96Zr0.04Ti0.90Ni0.10O3\text{Sr}_{0.96}\text{Zr}_{0.04}\text{Ti}_{0.90}\text{Ni}_{0.10}\text{O}_3 sample. In this co-doped sample, the remnant magnetization and coercivity were increased by ∼\sim1 and ∼\sim2 orders of magnitude respectively as compared to those of undoped STO. The coexistence of FE and FM orders in (Zr, Ni) co-doped STO might have the potential for interesting multiferroic applications.

Introduction

Strontium titanate SrTiO3 (STO) is perhaps one of the most prominent prototypical ABO3 perovskite oxide materials having potentials in diverse fields of applications such as high-k dielectrics [1], substrate materials [2], tunable microwave devices [3, 4], non-volatile memory applications [5], O2 and H2S sensing [6, 7] and photocatalytic water splitting [8], to name just a few. At room temperature, STO exists in cubic structure with space group Pm-3m where the Sr2+ occupies A site which is surrounded by four TiO6 octahedra and Ti4+ occupies B site which is located at the octahedral void formed by six O2− ions situated at the faces of the cube [9]. Pure stoichiometric STO is a band-insulator whose quantum paraelectric behaviour excludes the emergence of the ferroic phases such as ferroelectric (FE) and ferromagnetic (FM) orders [10, 11, 12, 13, 14]. Over the years numerous attempts have been made to induce FE and FM orders in STO by means of cation doping for achieving multiferroic behaviour. The FM ordering is induced in STO by doping transition metals (Mn, Fe, Co, Cd) and rare-earth elements (Yb, Mn) [15, 16, 17, 18, 19, 20]. The FE behavior has been observed at room temperature in Pr doped STO [21] whereas Mn doping introduced FE relaxor type behaviour at low temperature [14, 22, 23, 24, 25]. Moreover, (Nd, Dy) and (La, Mn) co-doped STO showed promising results for multiferroic applications [14, 21, 22, 23, 24, 25].

Here we doped STO with two different transition metal elements which are Zr and Ni. In the stable Zr4+ oxidation state, the empty 4d orbital has the possibility of inducing the ferroelectric order in STO and thereby may enhance dielectric properties in Zr doped STO [10, 26, 27]. The rationale behind co-doping of Zr4+ and Ni2+ is that the magnetic moments of the unpaired electrons in the partially filled 3d orbitals in Ni2+ oxidation state might have the potential to tune the magnetic properties of STO. We assume substitutional doping following the general rule where ions with smaller radius Ni2+ (ro = 0.69 Å) tend to substitute Ti4+ in B site and ions with larger radius Zr4+ (ro = 0.80 Å) prefer to go in A site occupied by Sr2+ [28]. The objective of this investigation is to synthesize a number of Zr and Ni co-doped STO materials and extensively characterize their structural, electrical and magnetic properties [29, 30, 31, 32]. To this aim, undoped STO, Zr-doped Sr1-xZrxTiO3 and (Zr, Ni) co-doped Sr1-xZrxTi1-yNiyO3 samples were synthesized using solid state reaction technique. Based on the findings from the pertinent materials characterization techniques, we report a particular composition of this (Zr, Ni) co-doped samples with improved multiferroic properties which might have potential for multifunctional applications [30].

METHODOLOGY

Sample Preparation

A number of samples for undoped SrTiO3_3, Zr-doped SrTiO3_3 and (Zr, Ni) co-doped SrTiO3_3 have been synthesized using the standard solid state reaction method [33, 34]. For the starting materials, proper combinations of analytical grade SrCO3_3 (98% pure), TiO2_2 (99.9% pure), ZrO2_2 (99.9% pure) and NiO (99.9% pure) were used with desired stoichiometric ratio. For the Zr-doped samples, x=0.02x = 0.02, 0.04, 0.06 were prepared with the chemical formula Sr1−x_{1-x}Zrx_xTiO3_3. In case of (Zr, Ni) co-doped samples with chemical formula Sr1−x_{1-x}Zrx_xTi1−y_{1-y}Niy_yO3_3, a series of combinations with y=0.05y = 0.05, 0.10, 0.15 and 0.20 for fixed x=0.04x = 0.04 have been synthesized. The powder mixtures were hand milled for 6 hours using mortar and pestle to produce a homogeneous solid mixture with fine constituent particles in proximity with each other. Several droplets of polyvinyl alcohol were mixed with the samples in a steel die to facilitate binding before being subjected to uniaxial force of 20 kN in a hydraulic press to form circular disk-shaped pellets. These pellets were calcined at 800°C for 4 hours to promote reaction among the mixture constituents. The pre-sintered disk-shaped pellets were smashed into fine powders by hand milling in a ceramic mortar and pestle for 3 hours to expedite solid state reactions probabilities in the subsequent sintering of the samples. The crystallization temperatures of the udoped, Zr doped and (Zr, Ni) co-doped samples were measured to be ∼1080°, ∼1085° and ∼942°C respectively using a differential scanning calorimeter. The pre-sintered powder materials were pressed into circular disk shaped pellets and toroid rings by using a hydraulic press and sintered at 1250°C for 4 hours.

Characterization Techniques

To estimate the crystallization temperature of our synthesized samples, the differential scanning calorimetry was performed using a NETZSCH STA 449 F3 Jupiter simultaneous thermal analyzer. The high temperature sintering of the samples was done in a Nabertherm Muffle Furnace LT 5/14. The X-ray Diffraction (XRD) patterns for the synthesized samples were obtained from 10° to 80° at 35 kV accelerating voltage with an emission current of 20 mA using a Rigaku SmartLab SE multipurpose XRD system with Cu Kα radiation (λ=0.15418\lambda= 0.15418 nm). The surface morphology and chemical species identification were performed with Scanning Electron Microscopy (SEM) and Energy-dispersive X-ray spectroscopy (EDX) respectively using a AVO 18 Research Scanning Electron Microscope from ZEISS. The room temperature Raman scattering spectroscopy was performed with a Confocal Raman Microscope MonoVista CRS+ using a 532.090 nm laser. To characterize the chemical bond vibrations inside our samples, we used the KBr pellet technique in Fourier Transform Infrared (FTIR) PerkinElmer Spectrum spectrometer. The dielectric constant and resistivity of the samples were measured from complex impedance spectroscopy performed by Wayne Kerr 6500B Impedance Analyzer. For the electric hysteresis measurements, the electric polarization PP vs. electric field EE loops were recorded using a Precision Multiferroic II Ferroelectric Test System from Marine India. The magnetization MM vs. magnetic field HH hysteresis loops of the samples were obtained using a vibrating sample magnetometer VSM from Quantum Design PPMS DynaCool.

Results and Discussion

X-ray Diffraction Analysis

We have investigated the crystallographic structure, phase and purity of the synthesized samples using the XRD patterns, see Figure 1. The pure STO exhibit cubic PmPm-3m3m phase (space group no. 221) according to the standard JCPDS data (01-084-0443) [17, 35]. The phase purity and crystalline nature of the samples were evident from the sharp and intense diffraction peaks. In case of Zr doped Sr1−x_{1-x}Zrx_xTiO3_3 samples, extraneous peaks started to appear for x=0.06x = 0.06 indicating the presence of additional phases on top of the cubic phase. Hence, to avoid the influence of these secondary phases in (Zr, Ni) co-doped samples, we fixed Zr concentration xx to be at 0.04 as Sr0.96_{0.96}Zr0.04_{0.04}Ti1−y_{1-y}Niy_yO3_3. For y≥0.10y \geq0.10, the small extraneous peaks at 37.18°, 43.20°, 62.75° and 75.25° were observed due excess NiO [36]. The lattice parameters were extracted by Rietveld refinement of the XRD profile using FullProf software. We estimated bulk density, X-ray density, porosity, crystallite size and full-width-half-maximum using standard techniques [37], see Table I. The bulk density remained unchanged for undoped and doped STO. For Zr doped and (Zr, Ni) co-doped samples, an increasing trend in the X-ray-density was observed with Zr and Ni concentrations. These increments may have originated from the change in molecular weights due to the incorporation of the Zr and Ni dopants in the sample. A nominal variation in porosity has been observed across the synthesized samples. As for the crystallite size, monotonic decrements have been detected with increasing Zr concentration in STO. The change in the full-width-at-half-maximum (FWHM) for (Zr, Ni) co-doped samples indicates slight distortion and disorder due to size differences of dopants and interstitial dopants respectively [38]. From the peak shift analysis (as shown in Figure S1 of the Supplementary Information), it is evident that the peak shift between pure STO and Sr0.96_{0.96}Zr0.04_{0.04}TiO3_3 is very nominal almost conforming with pure cubic phase. We superimposed the Rietveld refined pattern on experimentally measured XRD data for three selected samples; SrTiO3_3, Sr0.96_{0.96}Zr0.04_{0.04}TiO3_3 (due to superior dielectric properties in Section III E) and Sr0.96_{0.96}Zr0.04_{0.04}Ti0.90_{0.90}Ni0.10_{0.10}O3_3 (manifested superior magnetic properties as shall be seen later in § 1.2 H) in Figure 2. The goodness of fitting parameter χ2\chi^2 for the three samples were found to be 3.784, 3.590 and 3.806 which indicate simulated patterns are in good agreement with experimental observations conforming cubic structure. The auxiliary crystallographic parameters such as atomic positions in Wyckoff coordinates, relevant bond lengths and bond angles have also been extracted from the refinement (see Table S1 in the Supplementary Information).

Figure 1. X-ray diffraction patterns of Sr1−x_{1-x}Zrx_xTi1−y_{1-y}Niy_yO3_3 for (x, y) = (0.00, 0.00), (0.02, 0.00), (0.04, 0.00), (0.06, 0.00), (0.04, 0.05), (0.04, 0.10), (0.04, 0.15) and (0.04, 0.20). The unknown impurity phase is marked with black diamonds in case of (x, y) = (0.06, 0.00).

Figure 2. Simulated Rietveld least square minimized XRD patterns superimposed on experimentally observed data of Sr1−xZrxTi1−yNiyO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} for (x,y)=(0.00,0.00)(x,y)=(0.00,0.00), (0.04,0.00)(0.04,0.00) and (0.04,0.10)(0.04,0.10). The red solid circles are the experimental data points (YobsY_{\mathrm{obs}}), the dark solid line represents calculated refined pattern YcalY_{\mathrm{cal}}, the bottom blue curve YdiffY_{\mathrm{diff}} shows difference between the experimental YobsY_{\mathrm{obs}} and calculated YcalY_{\mathrm{cal}} values and pink vertical lines mark the positions of Bragg peaks for cubic SrTiO3\mathrm{SrTiO}_{3} with Pm3ˉmPm\bar{3}m space group. The green vertical lines represent NiO phase.

XRD peak evolution of the (110) plane

Figure S1. The evolution of XRD intensity peak of Sr1−xZrxTi1−yNiyO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} for (x,y)=(0.00,0.00)(x,y) = (0.00, 0.00), (0.02,0.00)(0.02, 0.00), (0.04,0.00)(0.04, 0.00), (0.06,0.00)(0.06, 0.00), (0.04,0.05)(0.04, 0.05), (0.04,0.10)(0.04, 0.10), (0.04,0.15)(0.04, 0.15) and (0.04,0.20)(0.04, 0.20).

Rietveld refined analysis for Wyckoff position, bond lengths and bond angles
SrTiO3\mathrm{SrTiO}_{3}Sr0.96Zr0.04TiO3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{TiO}_{3}Sr0.96Zr0.04Ti0.90Ni0.10O3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{Ti}_{0.90}\mathrm{Ni}_{0.10}\mathrm{O}_{3}
atomsitexwx_\mathrm{w}ywy_\mathrm{w}zwz_\mathrm{w}atomsitexwx_\mathrm{w}ywy_\mathrm{w}zwz_\mathrm{w}atomsite
Sr1a000Sr1a0.00.00.0Sr1a
Ti1b0.50.50.5Ti1b0.50.50.5Ti1b
O3c0.00.50.5O3c0.00.50.5O3c
Zr1a0.00.00.0Zr1a
Ni1b
Bond length (A˚\mathrm{\AA})Bond length (A˚\mathrm{\AA})Bond length (A˚\mathrm{\AA})
Ti-O1.953 (3)Ti-O1.955 (5)Ti/Ni-O1.957 (6)
Sr-O2.762 (4)Sr/Zr-O2.762 (4)Sr/Zr-O2.768 (8)
Bond angle (∘^\circ)Bond angle (∘^\circ)Bond angle (∘^\circ)
⟨Sr−O−Sr⟩\langle\mathrm{Sr-O-Sr}\rangle90, 180⟨Sr/Zr−O−Sr/Zr⟩\langle\mathrm{Sr/Zr-O-Sr/Zr}\rangle90, 180⟨Sr/Zr−O−Sr/Zr⟩\langle\mathrm{Sr/Zr-O-Sr/Zr}\rangle90, 180
⟨Sr−O−Ti⟩\langle\mathrm{Sr-O-Ti}\rangle90⟨Sr/Zr−O−Ti⟩\langle\mathrm{Sr/Zr-O-Ti}\rangle90⟨Sr/Zr−O−Ti/Ni⟩\langle\mathrm{Sr/Zr-O-Ti/Ni}\rangle90
RpR_\mathrm{p}5.755RpR_\mathrm{p}5.334RpR_\mathrm{p}5.462
RwpR_\mathrm{wp}7.580RwpR_\mathrm{wp}7.169RwpR_\mathrm{wp}7.32
RexpR_\mathrm{exp}2.023RexpR_\mathrm{exp}1.997RexpR_\mathrm{exp}1.923
χ2\chi^23.748χ2\chi^23.590χ2\chi^23.806

Table S1. Atomic coordinates xwx_\mathrm{w}, ywy_\mathrm{w}, zwz_\mathrm{w} in Wyckoff notation, bond lengths and bond angles obtained from Rietveld refinement of XRD patterns of SrTiO3\mathrm{SrTiO}_{3}, Sr0.96Zr0.04TiO3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{TiO}_{3} and Sr0.96Zr0.04Ti0.90Ni0.10O3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{Ti}_{0.90}\mathrm{Ni}_{0.10}\mathrm{O}_{3}.

CompositionLattice ParametersBulk DensityX-ray densityPorosityCrystallite SizeFWHM
xya(Å)b(Å)c(Å)c/aα(°)β(°)γ(°)(gcm−3^{-3})(gcm−3^{-3})(%)(nm)(110)(°)
0.000.003.9083.9083.9081.09090903.995.10221.71080.073
0.020.003.9033.9033.9031.09090903.995.12722.1880.086
0.040.003.8993.8993.8991.09090903.995.14522.4570.135
0.060.003.9083.9083.9081.09090903.995.10921.8550.137
0.040.053.9053.9053.9051.09090903.995.13322.21000.085
0.040.103.8883.8883.8881.09090903.995.21823.5360.193
0.040.153.8973.8973.8971.09090903.995.16922.8360.202
0.040.203.8943.8943.8941.09090903.995.19523.1490.148

Table 1. Lattice parameters a, b, c, α, β and γ extracted from Rietveld refinement of XRD patterns of Sr1−x_{1-x}Zrx_xTi1−y_{1-y}Niy_yO3_3 for (x, y) = (0.00 ,0.00), (0.02, 0.00), (0.04, 0.00), (0.06, 0.00), (0.04, 0.05), (0.04, 0.10), (0.04, 0.15) and (0.04, 0.20). The bulk density, X-ray density, porosity, crytallite size were derived from standard formulas. The values for FWHM were for the most intense XRD peak corresponding to (110) plane.

Morphological and EDX Analysis

To understand the effect of doping on the microstructure and to perform chemical species identification of our samples, SEM micrographs and EDX spectra of the three selected samples SrTiO3_3, Sr0.96_{0.96}Zr0.04_{0.04}TiO3_3 and Sr0.96_{0.96}Zr0.04_{0.04}Ti0.90_{0.90}Ni0.10_{0.10}O3_3 have been obtained. The average grain size was estimated to be 2 μ\mum in case of undoped SrTiO3_3, see SEM micrograph in Figure 3(a). The estimated average grain size is comparable with the previous studies on STO in Refs. [28, 39]. The detection of Sr, Ti and O peaks in the corresponding EDX spectra for undoped STO excludes the presence of unwanted chemical species in the sample (see Figure S2 in the Supplementary Information). The average grain size was reduced to 0.343 μ\mum for Sr0.96_{0.96}Zr0.04_{0.04}TiO3_3 sample as showed in Figure 3(b). This shrinkage of the gain size can be due to the presence of Zr or Ti at the grain boundaries [28]. In addition, Zr substitution prompted grain irregularity and inhomogeneity. The presence of Zr peak in addition with Sr, Ti and O peaks in the corresponding EDX spectra for Sr0.96_{0.96}Zr0.04_{0.04}TiO3_3 corroborates its incorporation as a dopant in the sample (see Figure S2 in the Supplementary Information). For (Zr, Ni) co-doped Sr0.96_{0.96}Zr0.04_{0.04}Ti0.90_{0.90}Ni0.10_{0.10}O3_3 sample, the estimated grain size was found to be 0.341 μ\mum according to the SEM micrograph in Figure 3(c). The corresponding EDX spectra containing Zr and Ni peaks elucidates the co-doping of the STO (see Figure S2 in the Supplementary Information). Moreover the atomic weights (%) of

SEM micrographs of SrTiO3, Zr-doped SrTiO3, and Zr, Ni-doped SrTiO3

Figure 3. SEM micrographs (a) SrTiO3\mathrm{SrTiO}_{3}, (b) Sr0.96Zr0.04TiO3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{TiO}_{3} and (c) Sr0.96Zr0.04Ti0.90Ni0.10O3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{Ti}_{0.90}\mathrm{Ni}_{0.10}\mathrm{O}_{3} samples.

EDX spectra of (a) SrTiO3, (b) Sr0.96Zr0.04TiO3 and (c) Sr0.96Zr0.04Ti0.90Ni0.10O3

Figure S2. EDX spectra of (a) SrTiO3\mathrm{SrTiO}_{3}, (b) Sr0.96Zr0.04TiO3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{TiO}_{3} and (c) Sr0.96Zr0.04Ti0.90Ni0.10O3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{Ti}_{0.90}\mathrm{Ni}_{0.10}\mathrm{O}_{3}.

chemical species in all aforementioned samples were compared with the corresponding theoretical values in Table S2 of the Supplementary Information.

ElementEDX Atomic (%)Theoretical Atomic (%)
SrTiO3\mathrm{SrTiO_3}Sr15.5420
Ti19.9820
O64.5760
Sr0.96Zr0.04TiO3\mathrm{Sr_{0.96}Zr_{0.04}TiO_3}Sr16.1219.2
Ti23.9620
O59.2560
Zr0.670.8
Sr0.96Zr0.04Ti0.90Ni0.10O3\mathrm{Sr_{0.96}Zr_{0.04}Ti_{0.90}Ni_{0.10}O_3}Sr16.5819.2
Ti20.8218
O57.3660
Zr0.540.8
Ni4.72

Table S2. Chemical species identification and concentration analysis using EDX of SrTiO3\mathrm{SrTiO_3}, Sr0.96Zr0.04TiO3\mathrm{Sr_{0.96}Zr_{0.04}TiO_3} and Sr0.96Zr0.04Ti0.90Ni0.10O3\mathrm{Sr_{0.96}Zr_{0.04}Ti_{0.90}Ni_{0.10}O_3} samples.

Raman Analysis

We performed room temperature Raman scattering spectroscopy to characterize the vibrational phonon in terms of transverse acoustic (TA), longitudinal acoustic (LA), transverse optical (TO) and longitudinal optical (LO) modes of our samples. For a three dimensional (d=3d=3) unit cell with cubic symmetry, the STO contains n=5n=5 atoms (one Sr, one Ti and three O) that generates 3n=153n=15 vibrational phonon modes; out of which the 3 low frequency acoustic modes (F1uF_{1u}) are degenerate, 3 degenerate optical modes (F1uF_{1u}) are Raman and infrared

(IR) inactive and the rest of 9 optical modes (F2uF_{2u}) are IR-active [40, 41, 42, 43, 44]. As cubic symmetry forbids first order Raman scattering, the Raman modes in cubic STO originate from second order scattering processes [40]. The two photon momentum conservation processes made the second order Raman scattering peaks to appear broad and continuous, see Figure 4. The broad intensity peaks of the Raman scattered radiation appeared in 250-500 cm−1^{-1} and 600-800 cm−1^{-1} wave number ranges. These Raman peaks were identified with corresponding vibrational phonon modes of the samples according to Refs. [42, 43] in Table S3 of the Supplementary Information. The 2TA mode appeared around 208 cm−1208\ \mathrm{cm}^{-1}, whereas the combined acoustic and optical modes such as TO1+LA\mathrm{TO_1+LA}, LO1+TA\mathrm{LO_1+TA} and LA+LO3\mathrm{LA+LO_3} contributed at 275275, 383383 and 702 cm−1702\ \mathrm{cm}^{-1} respectively. The modes corresponding to two optical phonons such as TO1+TO4\mathrm{TO_1+TO_4} (641 cm−1641\ \mathrm{cm}^{-1}) and LO3+TO2\mathrm{LO_3+TO_2} (762 cm−1762\ \mathrm{cm}^{-1}) were there for both Zr and (Zr, Ni) co-doped STO. The presence of peaks at 148 cm−1148\ \mathrm{cm}^{-1} (TO1), 547 cm−1547\ \mathrm{cm}^{-1} (TO4) and 797 cm−1797\ \mathrm{cm}^{-1} (LO4) for undoped STO can be attributed to forbidden first order Raman scattering. This may indicate a nominal loss of inversion symmetry due to surface frozen dipoles and oxygen vacancies [45, 46]. In case of doped samples, this nominal symmetry breaking can happen due to incorporation of dopants in the host STO [18].

Figure 4. Raman spectra of (a) SrTiO3\mathrm{SrTiO_3}, (b) Sr0.96Zr0.04TiO3\mathrm{Sr_{0.96}Zr_{0.04}TiO_3} and (c) Sr0.96Zr0.04Ti0.90Ni0.10O3\mathrm{Sr_{0.96}Zr_{0.04}Ti_{0.90}Ni_{0.10}O_3} samples.

Fourier Transform Infrared Spectroscopy

We also measured FTIR spectra for the undoped STO, 4% Zr doped Sr0.96Zr0.04TiO3\mathrm{Sr_{0.96}Zr_{0.04}TiO_3} and (4% Zr, 10% Ni) co-doped Sr0.96Zr0.04Ti0.90Ni0.10O3\mathrm{Sr_{0.96}Zr_{0.04}Ti_{0.90}Ni_{0.10}O_3} samples at room temperature from 350350 to 4000 cm−14000\ \mathrm{cm}^{-1} and displayed in Figure 5. The measured FTIR absorption peaks were identified to corresponding chemical bond vibrations following Refs. [47, 48, 49, 50] in Table S4 of the Supplementary Information. The absorption peaks at 1652 cm−11652\ \mathrm{cm}^{-1} and 3465 cm−13465\ \mathrm{cm}^{-1} can be designated to hydroxyl –OH stretching vibration, see Figure 5 (a)&(b). The stemming of H2O\mathrm{H_2O} or -OH in our sample may imply adsorption of water molecules from air surrounding the sample. The FTIR peaks at 14621462, 14601460 and 1485 cm−11485\ \mathrm{cm}^{-1} for the three samples hinted deformed -OH in C-OH bond [47]. The trace of C may have its origin in SrCO3\mathrm{SrCO_3} even after the calcination process. The FTIR bands in 300300-600 cm−1600\ \mathrm{cm}^{-1} represent characteristic IR absorptions due to Ti-O in STO. The peaks around ∼366 cm−1\sim366\ \mathrm{cm}^{-1} for different samples can appear from TiO2\mathrm{TiO_2} bending vibrations. Moreover the one near ∼598 cm−1\sim598\ \mathrm{cm}^{-1} can be ascribed to TiO6\mathrm{TiO_6} stretching vibration connected to Sr. We have not observed any sharp absorption peak at 500 cm−1500\ \mathrm{cm}^{-1} in Sr0.96Zr0.04TiO3\mathrm{Sr_{0.96}Zr_{0.04}TiO_3} which corresponds to Zr-O stretching vibrations in ZrO2\mathrm{ZrO_2}, see Figure 5(b). This corroborates the fact that Zr4+\mathrm{Zr^{4+}} ions have been incorporated in STO lattice. But Zr4+\mathrm{Zr^{4+}} ions, as it replaces Sr2+\mathrm{Sr^{2+}}, shorten different Ti-O bond lengths to different degrees; effectively generate several very closely spaced IR absorption peaks. The combined effect the Sr–Ti–O absorption peak at 594 cm−1^{-1}. In case of (Zr, Ni) co-doped sample, as Ni2+^{2+} ions replace the Ti4+^{4+}, they affect Ti-O bonds and shift the Sr–Ti–O absorption peak to 536 cm−1^{-1} in Figure 5(c).

Figure 5. FTIR spectra of (a) SrTiO3\mathrm{SrTiO_3}, (b) Sr0.96Zr0.04TiO3\mathrm{Sr_{0.96}Zr_{0.04}TiO_3} and (c) Sr0.96Zr0.04Ti0.90Ni0.10O3\mathrm{Sr_{0.96}Zr_{0.04}Ti_{0.90}Ni_{0.10}O_3} samples.

Peak AssignmentSrTiO3_3 (cm−1^{-1})Sr0.96_{0.96}Zr0.04_{0.04}TiO3_3 (cm−1^{-1})Sr0.96_{0.96}Zr0.04_{0.04}Ti0.90_{0.90}Ni0.10_{0.10}O3_3 (cm−1^{-1})
TiO2_2366366370
TiO6_6598594536
C-OH146214601485
-OH16531652-
-OH34653465-

Table S4. Experimentally observed FTIR absorption peak assignment to different chemical bond vibrational modes of SrTiO3_3, Sr0.96_{0.96}Zr0.04_{0.04}TiO3_3 and Sr0.96_{0.96}Zr0.04_{0.04}Ti0.90_{0.90}Ni0.10_{0.10}O3_3.

Dielectric Measurements

The circular disk-shaped pellets were used to form parallel plate capacitors with a geometric capacitance C0C_{0} giving rise to a frequency ff and complex dielectric constant ϵ=ϵreal+iϵimag\epsilon= \epsilon_{\mathrm{real}} + i\epsilon_{\mathrm{imag}} (i=−1i = \sqrt{-1}) dependent impedance Z(f)=1/i2πfC0ϵZ(f) = 1/i2\pi fC_{0}\epsilon which was measured with the impedance analyzer [51, 52]. The real part ϵreal\epsilon_{\mathrm{real}} of the complex dielectric constant was plotted for Sr1−xZrxTi1−yNiyO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} samples as a function of excitation frequency ff in Figure 6(a). The ϵreal\epsilon_{\mathrm{real}} gradually decreases with increasing ff for undoped, Zr doped and (Zr, Ni) co-doped STO samples. This indicates electric dipoles inside the material struggle to synchronize and fall out of steps with high frequency electric field. The dielectric behaviour is controlled by different constituents polarizations arising from interfacial charge, space charge, oriental dipolar, ionic and electronic contributions [53]. Owing to the fact that the ϵreal\epsilon_{\mathrm{real}} decays rapidly beyond 1 kHz, we attribute this to interfacial and space charge polarization effects [35, 54, 55]. This polarization may arise due to charges trapped at the interface between the sample and the electrodes, space charges at the grain boundaries, interstitial and voids. These trapped charges are sluggish in responding to the applied field in the high frequency regime beyond 1 kHz and usually modelled within the general framework of Maxwell-Wagner relaxation processes occurring inside the sample [56]. For the

Figure 6. (a) The real ϵreal\epsilon_{\mathrm{real}} vs frequency ff and (b) the imaginary part ϵimag\epsilon_{\mathrm{imag}} vs frequency ff of the complex dielectric constant ϵ=ϵreal+iϵimag\epsilon= \epsilon_{\mathrm{real}} + i\epsilon_{\mathrm{imag}} of Sr1−xZrxTi1−yNiyO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} for (x,y)=(0.00,0.00)(x,y)=(0.00, 0.00), (0.02,0.00)(0.02, 0.00), (0.04,0.00)(0.04, 0.00), (0.06,0.00)(0.06, 0.00), (0.04,0.05)(0.04, 0.05), (0.04,0.10)(0.04, 0.10), (0.04,0.15)(0.04, 0.15) and (0.04,0.20)(0.04, 0.20).

dielectric loss analysis, the imaginary part ϵimag\epsilon_{\mathrm{imag}} of the complex ϵ\epsilon was plotted as a function of frequency ff in Figure 6(b). This ϵimag\epsilon_{\mathrm{imag}} quantifies the energy dissipation of the electric dipoles due to random collisions or phase lag during their orientation change in response to the oscillating field. The frequency response of ϵimag\epsilon_{\mathrm{imag}} has similar trend as compared to ϵreal\epsilon_{\mathrm{real}}, i.e. it diminishes with increasing ff for undoped, Zr doped and (Zr, Ni) co-doped samples. This is expected as higher losses occur at low frequencies due to interfacial and space charge polarizations.

The effect of doping on εreal\varepsilon_{\mathrm{real}} was analyzed in Figure 7 for a fixed frequency of 1 kHz. For Zr doped Sr1−xZrxTiO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{TiO}_{3} samples, the εreal\varepsilon_{\mathrm{real}} increases monotonically with increasing composition x=0.02x=0.02, 0.04 and 0.06. This enhancement of dielectric constant can be attributed to more space charge accumulation due to higher oxidation state of Zr4+\mathrm{Zr}^{4+} as compared to Sr2+\mathrm{Sr}^{2+} in A site of STO. But in case of Sr0.96Zr0.04Ti1−yNiyO3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} samples, εreal\varepsilon_{\mathrm{real}} decreases steadily with increasing Ni concentrations as shown in the inset of Figure 7. This εreal\varepsilon_{\mathrm{real}} reduction may imply depletion of space charges as Ni2+\mathrm{Ni}^{2+} substitutes Ti4+\mathrm{Ti}^{4+} ion at the B-site of STO. Moreover, the substitutional Ni2+\mathrm{Ni}^{2+} can restrain the rattling of Ti4+\mathrm{Ti}^{4+} ions in TiO6\mathrm{TiO}_{6} octahedra causing the reduction of dielectric constant [28, 57, 58].

Figure 7. The ϵreal\epsilon_{\mathrm{real}} of Sr1−xZrxTiO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{TiO}_{3} sample for x=0.00x = 0.00, 0.02, 0.04 and 0.06. Inset: The ϵreal\epsilon_{\mathrm{real}} of Sr0.96Zr0.04Ti1−yNiyO3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} sample for y=0.05y = 0.05, 0.10, 0.15 and 0.20. All estimations were done at f=1f = 1 kHz.

Resistivity Measurements

The frequency dependant ac resistivity ρ\rho of the samples was measured from the complex impedance Z=Zreal+iZimagZ=Z_{\mathrm{real}}+iZ_{\mathrm{imag}} by using the relation ρ=AsZreal/ds\rho=A_{\mathrm{s}}Z_{\mathrm{real}}/d_{\mathrm{s}}, where AsA_{\mathrm{s}} and dsd_{\mathrm{s}} represent area and thickness of the circular disc shape pellets respectively [59]. The resistivity ρ\rho decays with ff in Figure 8. This indicates enhanced mobile charge hopping in the grain boundaries and sample-electrode interfaces [35, 60]. The interfacial charges can produce a thin conductive layer at the sample surface effectively reducing the resistivity at high frequencies. Moreover the carrier transport in high frequency is dominated by bulk of the grains whereas grain boundary dictates the low frequency transport [61]. The carrier activation energy at the grain boundaries may fall at high frequencies resulting in enhanced charge conduction [62]. To analyze the effect of doping, we plot ρ\rho for undoped, Zr doped Sr1−xZrxTiO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{TiO}_{3} and (Zr, Ni) co-doped Sr0.96Zr0.04Ti1−yNiyO3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} samples at a fixed ff of 1 kHz in Figure 9. The insulating characteristics of undoped STO is well captured in its high resistivity value. As we dope STO with Zr, the resistivity ρ\rho of the Sr1−xZrxTiO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{TiO}_{3} samples decreases with increasing concentrations x=0.02x=0.02, 0.04. This can be attributed to the fact that Zr4+\mathrm{Zr}^{4+} acts as an n-type dopant for Sr2+\mathrm{Sr}^{2+} and raises the conductivity of the samples. The Ni, as a second dopant in Sr0.96Zr0.04Ti1−yNiyO3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} samples, seems to gradually increase the ρ\rho for y=0.10y=0.10, 0.15, and 0.20 as shown in the inset of Figure 9. A number of reasons can be ascribed to this conductivity depletion. The Ni2+\mathrm{Ni}^{2+} ion can act as an acceptor dopant for Ti4+\mathrm{Ti}^{4+}. This suppresses the n-type conductivity between the grain bulks as acceptor dopants can act as a non-conductive layer for mobile charge carriers across the grain boundaries [63, 64]. Moreover, any oxygen vacancies induced by Ni2+\mathrm{Ni}^{2+} can act as a charge trapping center reducing the carrier mobility.

Figure 8. The resistivity ρ\rho of Sr1−xZrxTi1−yNiyO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} as a function of frequency ff for (x,y)=(0.00,0.00)(x,y)=(0.00, 0.00), (0.02,0.00)(0.02, 0.00), (0.04,0.00)(0.04, 0.00), (0.06,0.00)(0.06, 0.00), (0.04,0.05)(0.04, 0.05), (0.04,0.10)(0.04, 0.10), (0.04,0.15)(0.04, 0.15) and (0.04,0.20)(0.04, 0.20).

Resistivity at fixed frequency as a function of Zr concentration

Figure 9. The resistivity ρ\rho at a fixed frequency f=1f=1 kHz of Sr1−xZrxTiO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{TiO}_{3} samples for x=0.00x=0.00, 0.02, 0.04 and 0.06. Inset: The ρ\rho of Sr0.96Zr0.04Ti1−yNiyO3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} samples for y=0.05y=0.05, 0.10, 0.15 and 0.20.

Electric Hysteresis Measurements

The room temperature electric polarization (PP) vs electric field (EE) hysteresis PP-EE loops were measured with external triangular ac field excitation up to ±3\pm3 kVcm−1^{-1} at 50 Hz for undoped, Zr doped and (Zr, Ni) co-doped samples. The standard PP-EE loop parameters such as coercive electric field EcE_{\mathrm{c}}, remnant polarization PrP_{\mathrm{r}}, maximum polarization PmaxP_{\mathrm{max}} and leakage current IdI_{\mathrm{d}} at PmaxP_{\mathrm{max}} were extracted and displayed in Table 2. The undoped STO exhibits a small PP-EE hysteresis loop where the PP is almost linear with EE and does not reach any saturation, see Figure 10(a). At E=3 kVcm−1E = 3\ \mathrm{kVcm}^{-1} the sample showed a Pmax⁡=0.103 μCcm−2P_{\max} = 0.103\ \mu\mathrm{Ccm}^{-2}, a tiny Pr=0.017 μCcm−2P_{\mathrm{r}} = 0.017\ \mu\mathrm{Ccm}^{-2} and Ec=0.154 kVcm−1E_{\mathrm{c}} = 0.154\ \mathrm{kVcm}^{-1}. The incorporation of Zr seems to enhance FE behaviour in STO. For Zr doped Sr1−xZrxTiO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{TiO}_{3} samples, the PrP_{\mathrm{r}} and EcE_{\mathrm{c}} values monotonically increase with the Zr concentration, see Table II. For (Zr, Ni) co-doped Sr0.96Zr0.04Ti1−yNiyO3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} sample with a composition of y=0.05y=0.05, the Ni dopants diminish the ferroelectric characteristics by narrowing down the PP-EE loop (Ec=0.791 kVcm−1E_{\mathrm{c}} =0.791\ \mathrm{kVcm}^{-1}, Pr=0.039 μCcm−2P_{\mathrm{r}} =0.039\ \mu\mathrm{Ccm}^{-2} and Pmax⁡=0.112 μCcm−2P_{\max} =0.112\ \mu\mathrm{Ccm}^{-2}) as compared to Sr0.96Zr0.04TiO3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{TiO}_{3} (Ec=1.216 kVcm−1E_{\mathrm{c}} =1.216\ \mathrm{kVcm}^{-1}, Pr=0.083 μCcm−2P_{\mathrm{r}} =0.083\ \mu\mathrm{Ccm}^{-2} and Pmax⁡=0.162 μCcm−2P_{\max} =0.162\ \mu\mathrm{Ccm}^{-2}), see Figure 10(b). The FE hysteresis existed for all (Zr, Ni) co-doped samples even for higher Ni concentrations; for example in case of Sr0.96Zr0.04Ti0.90Ni0.10O3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{Ti}_{0.90}\mathrm{Ni}_{0.10}\mathrm{O}_{3} sample Ec=1.420 kVcm−1E_{\mathrm{c}} =1.420\ \mathrm{kVcm}^{-1}, Pr=0.079 μCcm−2P_{\mathrm{r}} =0.079\ \mu\mathrm{Ccm}^{-2} and Pmax⁡=0.125 μCcm−2P_{\max} =0.125\ \mu\mathrm{Ccm}^{-2}. For higher doping concentration in Zr and (Zr, Ni) co-doped samples, the area of the PE loop was enlarged which indicates increased dielectric losses were present inside the sample. This is consistent with the increased leakage current in the samples as displayed in Table II. The origin of the leakage current can be due to carriers originated from the oxygen vacancies [65]. The dominance of the leakage current prevented complete saturation in polarization to occur in our samples [66].

Figure 10. PP-EE hysteresis loops of (a) Sr1−xZrxTiO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{TiO}_{3} for x=0.0,0.02,0.04x = 0.0, 0.02, 0.04 and 0.060.06, (b) Sr0.96Zr0.04Ti1−yNiyO3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} with y=0.00,0.05,0.10,0.15y = 0.00, 0.05, 0.10, 0.15 and 0.200.20.

xxyyEcE_{\mathrm{c}} (kVcm−1^{-1})PrP_{\mathrm{r}} (μ\muCcm−2^{-2})Pmax⁡P_{\max} (μ\muCcm−2^{-2})IdI_{\mathrm{d}} (μ\muAcm−2^{-2})
0.000.000.3120.0110.1030.073
0.020.000.7680.0320.1060.076
0.040.001.2160.0830.1620.085
0.060.001.4580.1530.2600.108
0.040.050.7910.0390.1120.077
0.040.101.4200.0790.1250.083
0.040.151.9830.2470.3440.136
0.040.201.6320.1520.2400.149

Table 2. The coercive field (EcE_{\mathrm{c}}), the remnant polarization (PrP_{\mathrm{r}}), the maximum polarization (Pmax⁡P_{\max}) and leakage current IdI_{\mathrm{d}} at Pmax⁡P_{\max} of Sr1−xZrxTi1−yNiyO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} for different values of xx and yy.

Magnetization Measurements

We have recorded magnetization (MM) vs. magnetic field (HH) hysteresis loops of the as-prepared samples using a vibrating sample magnetometer applying a maximum magnetic field of ±20 kOe\pm20\ \mathrm{kOe} and displayed in Figure 11. The inset of Figure 11 shows an enlarged view of the hysteresis loop for the 4 % Zr and 10 % Ni co-doped Sr0.96Zr0.04Ti0.90Ni0.10O3\mathrm{Sr}_{0.96}\mathrm{Zr}_{0.04}\mathrm{Ti}_{0.90}\mathrm{Ni}_{0.10}\mathrm{O}_{3} sample. We extracted different MM-HH loop parameters such as remnant magnetization

Figure 11. Magnetic hysteresis loop of Sr1−x_{1-x}Zrx_xTi1−y_{1-y}Niy_yO3_3 samples using vibrating sample magnetometer for (x,y)=(0.00,0.00),(0.04,0.00),(0.04,0.05),(0.04,0.10),(0.04,0.15),(0.04,0.20)(x, y) = (0.00, 0.00), (0.04, 0.00), (0.04, 0.05), (0.04, 0.10), (0.04, 0.15), (0.04, 0.20). Inset: The enlarged view of the hysteresis loop for 4% Zr and 10% Ni co-doped sample.

tion (MrM_{\mathrm{r}}), the coercive field (HcH_{\mathrm{c}}) and the saturation magnetization (MsM_{\mathrm{s}}); and the values were inserted in Table III. The HcH_{\mathrm{c}} was quantified following the formula Hc=(Hc1−Hc2)/2H_{\mathrm{c}} = (H_{\mathrm{c1}} - H_{\mathrm{c2})/2} where Hc1H_{\mathrm{c1}} and Hc2H_{\mathrm{c2}} are the left and right coercive fields respectively [67].

xxyyMr×10−3M_{\mathrm{r}} \times10^{-3} (emug−1^{-1})HcH_{\mathrm{c}} (Oe)MsM_{\mathrm{s}} (emug−1^{-1})
0.000.003542.80
0.040.0064920.50
0.040.05114601.30
0.040.103223751.27
0.040.152463711.00
0.040.203653080.50

Table 3. The remnant magnetization (MrM_{\mathrm{r}}), the coercive field (HcH_{\mathrm{c}}) and the saturation magnetization (MsM_{\mathrm{s}}) of Sr1−xZrxTi1−yNiyO3\mathrm{Sr}_{1-x}\mathrm{Zr}_{x}\mathrm{Ti}_{1-y}\mathrm{Ni}_{y}\mathrm{O}_{3} for different values of xx and yy.

The saturated hysteresis loop with a saturation magnetization MsM_{\mathrm{s}} of 2.80 emug−1^{-1} and coercive field of 4 Oe revealed soft FM nature of the as-synthesized STO sample. The origin of FM behaviour can be attributed to the presence oxygen vacancies VO2−V_{\mathrm{O}}^{2-} induced as a result of charge imbalance due to loss of Sr2+^{2+} at high sintering temperature [68, 69, 70, 71, 72, 73]. Moreover the variable oxidation state of Ti (Ti4+⇔^{4+} \Leftrightarrow Ti3+^{3+}) in STO can also facilitate oxygen vacancy to maintain charge equilibrium. The reduction in MsM_s to 0.50 emug−1^{-1} in case of 4% Zr doped Sr0.96_{0.96}Zr0.04_{0.04}TiO3_3 sample can be ascribed to diamagnetic Zr4+^{4+} ion with its empty 4d orbitals [74]. In addition, the presence of Zr4+^{4+} in the grain boundaries may reduce the defects at the grain surfaces that can cause suppression in MsM_s [70]. Moreover we observed increments in MrM_r and HcH_c as compared to those of undoped STO which indicates reduction in softness of FM order due to Zr doping. The incorporation of Ni dopants notably increased HcH_c and MrM_r in (Zr, Ni) co-doped STO. In particular, for 4% Zr and 10% Ni co-doped sample, the values of HcH_c, MrM_r and MsM_s are mentionable. For a further increment of the amount of Ni to 15% and 20%, HcH_c and MrM_r do not change significantly, however, MsM_s reduced notably. Due to Zr and Ni co-doping in STO, the coercivity enhancement was very high compared to that of undoped STO which might have originated form the inflated exchange coupling between Ni2+^{2+} ions mediated by trapped electron in the oxygen vacancy [75, 76]. Note also the variation in HcH_c with doping concentration is not surprising as it depends on large number of factors defining the microstructure of the sample such as grain homogeneity, grain size distribution and domain wall pinning [77]. For the case of remnant magnetization MrM_r, we observed an order of magnitude enhancement in Sr0.96_{0.96}Zr0.04_{0.04}Ti0.90_{0.90}Ni0.10_{0.10}O3_3 sample (322 ×\times 10−3^{-3} emug−1^{-1}) as compared to that of undoped STO (35 ×\times 10−3^{-3} emug−1^{-1}). Overall the presence of hysteresis loop and the remnant magnetization corroborates long range FM order in our (Zr, Ni) co-doped samples.

Conclusion

Undoped, Zr doped and (Zr, Ni) co-doped SrTiO3_3 samples were synthesized with varying degrees of doping concentrations and were characterized comprehensively using the appropriate techniques. We confirmed the cubic phase up to 4% Zr doping in STO from Rietveld analysis of the powder X-ray diffraction pattern. The substitution of 4% Zr instead of Sr in STO improved the morphological, electrical and magnetic properties. Therefore, Zr and Ni co-doped samples were prepared for this fixed % of Zr to improve further the electrical and magnetic properties of STO. Interestingly, 4% Zr and 10% Ni co-doped Sr0.96_{0.96}Zr0.04_{0.04}Ti0.90_{0.90}Ni0.10_{0.10}O3_3 sample demonstrated ∼\sim1 and ∼\sim2 orders of magnitude enhancement in remnant magnetization and coercivity respectively at room temperature. Along with a clear ferroelectric hysteresis loop we observed also a ferromagnetic hysteresis loop for this co-doped sample. We may anticipate that simultaneous existence of ferromagnetic and ferroelectric phases in this as-synthesized (Zr, Ni) co-doped Sr0.96_{0.96}Zr0.04_{0.04}Ti0.90_{0.90}Ni0.10_{0.10}O3_3 sample may open up the potentials as a multiferroic material for use in multifunctional applications.

Acknowledgments

We gratefully acknowledge the support from Dr. Ishtiaque M. Syed for providing access to high temperature sintering facility in Semiconductor Technology Research Center, University of Dhaka.

Author contributions

S.A. and A. K. M. S. H. F. contributed equally. Competing interests: The authors declare no competing interests.

References

Supplementary information for “Room temperature ferroic orders in Zr and (Zr, Ni) doped SrTiO3”

Shahran Ahmed; A. K. M. Sarwar Hossain Faysal; M. N. I. Khan; M. A. Basith; Muhammad Shahriar Bashar; H. N. Das; Tarique Hasan; Imtiaz Ahmed

XRD PEAK EVOLUTION

The highest intensity peak (110) shifts as Zr and Ni dopants are introduced in the sample, see Figure S1. These shifts can be attributed to strains induced in the STO cubic structure due to the incorporation of Zr and Ni. Peak shift towards lower diffraction angle usually results from tensile strain due to dopant ions with smaller radii Zr4+\mathrm{Zr}^{4+} (ro=0.80r_o = 0.80 Å) replacing the Sr2+\mathrm{Sr}^{2+} (ro=1.26r_o = 1.26 Å) in A-site; or Ni2+\mathrm{Ni}^{2+} (ro=0.69r_o = 0.69 Å) replacing Ti+4\mathrm{Ti}^{+4} (ro=0.74r_o = 0.74 Å) in B-site. Peak shift towards higher angle results from compressive strain; for example the bigger Zr4+\mathrm{Zr}^{4+} (ro=0.80r_o = 0.80 Å) ion replacing smaller Ti+4\mathrm{Ti}^{+4} (ro=0.74r_o = 0.74 Å). At low Zr concentration such as x=0.02x=0.02, the XRD peak shifted to higher angle indicating the presence of a compressive strain as some of the Zr4+\mathrm{Zr}^{4+} ions may have substituted the Ti+4\mathrm{Ti}^{+4}. But as the Zr concentration was increased to 4% and 6%, the peak moved to lower diffraction angle as more Zr4+\mathrm{Zr}^{4+} ions started to substitute Sr2+\mathrm{Sr}^{2+}. It is evident the peak shift between pure STO and Sr0.96Ni0.04TiO3\mathrm{Sr}_{0.96}\mathrm{Ni}_{0.04}\mathrm{TiO}_{3} is very nominal almost conforming with pure cubic phase. The changes in the full-width-at-half-maximum (FWHM) for (Zr, Ni) co-doped samples indicates slight distortion and disorder due to size differences of substituted dopants and possible interstitial dopants respectively.

RIETVELD REFINEMENT

EDX Peak Analysis

To perform chemical species identification of our samples Energy-dispersive X-ray spectroscopy (EDX) spectra for SrTiO3\mathrm{SrTiO_3}, Sr0.96Zr0.04TiO3\mathrm{Sr_{0.96}Zr_{0.04}TiO_3} and Sr0.96Zr0.04Ti0.90Ni0.10O3\mathrm{Sr_{0.96}Zr_{0.04}Ti_{0.90}Ni_{0.10}O_3} samples have been obtained as shown in Figure S2. The atomic weights (%) of chemical species obtained from EDX measurements were compared with corresponding theoretical values for all aforementioned samples, see Table S2.

Raman Peak Assignment

The Raman peaks for SrTiO3\mathrm{SrTiO_3}, Sr0.96Zr0.04TiO3\mathrm{Sr_{0.96}Zr_{0.04}TiO_3} and Sr0.96Zr0.04Ti0.9Ni0.1O3\mathrm{Sr_{0.96}Zr_{0.04}Ti_{0.9}Ni_{0.1}O_3} samples were identified with their transverse acoustic (TA), longitudinal acoustic (LA), transverse optical (TO) and longitudinal optical (LO) vibrational phonon modes in Table S3.

Peak Assgn.SrTiO3_3 (cm−1^{-1})Sr0.96_{0.96}Zr0.04_{0.04}TiO3_3 (cm−1^{-1})Sr0.96_{0.96}Zr0.04_{0.04}Ti0.90_{0.90}Ni0.10_{0.10}O3_3 (cm−1^{-1})
TO1_1148160145
2TA208201202
TO1_1+LA275285274
LO1_1+TA, 2TO2_2383377374
TO4_4547--
TO1_1+TO4_4-641-
LA+LO3_3702701689
LO3_3+TO2_2--762
LO4_4797800-

Table S3. Experimentally observed Raman peak assignments to different phonon vibrational modes of SrTiO3_3, Sr0.96_{0.96}Zr0.04_{0.04}TiO3_3 and Sr0.96_{0.96}Zr0.04_{0.04}Ti0.90_{0.90}Ni0.10_{0.10}O3_3.

Fourier Transform Infrared Spectroscopy (FTIR)

The FTIR absorption peaks for SrTiO3_3, Sr0.96_{0.96}Zr0.04_{0.04}TiO3_3 and Sr0.96_{0.96}Zr0.04_{0.04}Ti0.90_{0.90}Ni0.10_{0.10}O3_3 were identified with their chemical bonds vibrations inside the samples in Table S4.

References

  1. [1]J. Robertson, Journal of Vacuum Science & Technology B: Microelectronics and Nanometer Structures Processing, Measurement, and Phenomena 18, 1785 (2000).
  2. [2]D. V. Christensen, F. Trier, W. Niu, Y. Gan, Y. Zhang, T. S. Jespersen, Y. Chen, and N. Pryds, Adv. Mater. Interfaces 6, 1900772 (2019).
  3. [3]A. Eriksson, A. Deleoniv, and S. Gevorgian, Journal of Applied Physics 93, 2848 (2003).
  4. [4]D. Fuchs, C. W. Schneider, R. Schneider, and H. Rietschel, Journal of Applied Physics 85, 7362 (1999).
  5. [5]K. Szot, W. Speier, G. Bihlmayer, and R. Waser, Nature Materials 5, 312 (2006).
  6. [6]Y. Hu, O. K. Tan, J. S. Pan, and X. Yao, The Journal of Physical Chemistry B 108, 12114 (2004).
  7. [7]D. D. Kajale, G. E. Patil, V. B. Gaikwad, S. D. Shinde, D. N. Chavan, N. K. Pawar, S. R. Shirsath, and G. H. Jain, International Journal on Smart Sensing & Intelligent Systems 5 (2012).
  8. [8]Y. Sakata, Y. Miyoshi, T. Maeda, K. Ishikiriyama, Y. Yamazaki, H. Imamura, Y. Ham, T. Hisatomi, J. Kubota, A. Yamakata, et al., Applied Catalysis A: General 521, 227 (2016).
  9. [9]C. Li, K. C. K. Soh, and P. Wu, Journal of Alloys and Compounds 372, 40 (2004).
  10. [10]N. A. Spaldin and R. Ramesh, Nature materials 18, 203 (2019).
  11. [11]S. Kustov, I. Liubimova, and E. K. H. Salje, Physical Review Letters 124, 016801 (2020).
  12. [12]K. A. Müller and H. Burkard, Physical Review B 19, 3593 (1979).
  13. [13]J. Haeni, P. Irvin, W. Chang, R. Uecker, P. Reiche, Y. Li, S. Choudhury, W. Tian, M. Hawley, B. Craigo, et al., Nature 430, 758 (2004).
  14. [14]D. Choudhury, S. Mukherjee, P. Mandal, A. Sundaresan, U. Waghmare, S. Bhattacharjee, R. Mathieu, P. Lazor, O. Eriksson, B. Sanyal, et al., Physical Review B 84, 125124 (2011).
  15. [15]D. Yao, X. Zhou, and S. Ge, Applied Surface Science 257, 9233 (2011).
  16. [16]A. J. Ahmed, S. M. K. Nazrul Islam, R. Hossain, J. Kim, M. Kim, M. Billah, M. S. A. Hossain, Y. Yamauchi, and X. Wang, Royal Society Open Science 6, 190870 (2019).
  17. [17]E. Padmini and K. Ramachandran, Solid State Communications 302, 113716 (2019).
  18. [18]M. Muralidharan, V. Anbarasu, A. E. Perumal, and K. Sivakumar, Journal of Materials Science: Materials in Electronics 25, 4078 (2014).
  19. [19]D. Norton, N. Theodoropoulou, A. Hebard, J. Budai, I. Boatner, S. Pearton, and R. Wilson, Electrochemical and Solid State Letters 6, G19 (2002).
  20. [20]J. Lee, Z. Khim, Y. Park, D. Norton, N. Theodoropoulou, A. Hebard, J. Budai, L. Boatner, S. Pearton, and R. Wilson, Solid-State Electronics 47, 2225 (2003).
  21. [21]A. Durán, E. Martínez, J. Díaz, and J. Siqueiros, Journal of Applied Physics 97, 104109 (2005).
  22. [22]A. Tkach, P. M. Vilarinho, and A. L. Kholkin, Acta Materialia 53, 5061 (2005).
  23. [23]D. Choudhury, B. Pal, A. Sharma, S. Bhat, and D. D. Sarma, Scientific Reports 3, 1433 (2013).
  24. [24]C. Azzoni, M. Mozzati, A. Paleari, V. Massarotti, M. Bini, and D. Capsoni, Solid State Communications
  25. [25]M. Savinov, V. Trepakov, P. Syrnikov, V. Železný, J. Pokorný, A. Dejneka, L. Jastrabik, and P. Galinetto, Journal of Physics: Condensed Matter 20, 095221 (2008).
  26. [26]H. S. Bhatti, S. T. Hussain, F. A. Khan, and S. Hussain, Applied Surface Science 367, 291 (2016).
  27. [27]K. C. Pitike, W. D. Parker, L. Louis, and S. M. Nakhmanson, Physical Review B 91, 035112 (2015).
  28. [28]W. Bian, X. Lu, Y. Li, C. Min, H. Zhu, Z. Fu, and Q. Zhang, Journal of Materials Science: Materials in Electronics 29, 2743 (2018).
  29. [29]B. Ahmmad, M. Z. Islam, A. Billah, and M. A. Basith, Journal of Physics D: Applied Physics 49, 095001 (2016).
  30. [30]M. A. Basith, A. Billah, M. A. Jalil, N. Yesmin, M. A. Sakib, E. K. Ashik, S. M. E. H. Yousuf, S. S. Chowdhury, M. S. Hossain, S. H. Firoz, and B. Ahmmad, Journal of Alloys and Compounds 694, 792 (2017).
  31. [31]B. Soni, S. Makkar, and S. Biswas, Materials Characterization 174, 110990 (2021).
  32. [32]W. Zhou, H. Deng, N. Ding, L. Yu, F. Yue, P. Yang, and J. Chu, Materials Characterization 107, 1 (2015).
  33. [33]I. N, Esha, K. N. Munny, M. N. I. Khan, and K. H. Maria, AIP Advances 10, 125026 (2020).
  34. [34]M. A. Basith, O. Kurni, M. S. Alam, B. L. Sinha, and B. Ahmmad, Journal of Applied Physics 115, 024102 (2014).
  35. [35]G. Saravanan, K. Ramachandran, J. Gajendiran, and E. Padmini, Chemical Physics Letters , 137314 (2020).
  36. [36]H. Qiao, Z. Wei, H. Yang, L. Zhu, and X. Yan, Journal of Nanomaterials 2009 (2009).
  37. [37]B. D. Cullity, Elements of X-ray Diffraction (Addison-Wesley Publishing, 1956).
  38. [38]V.-L. Merupo, S. Velumani, K. Ordon, N. Errien, J. Szade, and A.-H. Kassiba, CrystEngComm 17, 3366 (2015).
  39. [39]S. K. Rout, S. Panigrahi, and J. Bera, Bulletin of Materials Science 28, 275 (2005).
  40. [40]P. S. Narayanan and K. Vedam, Zeitschrift für Physik 163, 158 (1961).
  41. [41]W. G. Nilssen and J. G. Skinner, The Journal of Chemical Physics 48, 2240 (1968).
  42. [42]R. F. Schaufele and M. J. Weber, The Journal of Chemical Physics 46, 2859 (1967).
  43. [43]C. H. Perry, J. H. Fertel, and T. F. McNelly, The Journal of Chemical Physics 47, 1619 (1967).
  44. [44]A. A. Sirenko, I. A. Akimov, J. R. Fox, A. M. Clark, H.-C. Li, W. Si, and X. X. Xi, Physical review letters 82, 4500 (1999).
  45. [45]F. A. Rabuffetti, H.-S. Kim, J. A. Enterkin, Y. Wang, C. H. Lanier, L. D. Marks, K. R. Poeppelmeier, and P. C. Stair, Chemistry of Materials 20, 5628 (2008).
  46. [46]D. A. Tenne, I. E. Gonenli, A. Soukiassian, D. G. Schlom, S. M. Nakhmanson, K. M. Rabe, and X. X. Xi, Physical Review B 76, 024303 (2007).
  47. [47]T. Xian, H. Yang, L. Di, J. Ma, H. Zhang, and J. Dai, Nanoscale Research Letters 9, 1 (2014).
  48. [48]C. Srilakshmi, R. Saraf, and C. Shivakumara, ACS Omega 3, 10503 (2018).
  49. [49]S. K. Patil, N. Shah, F. D. Blum, and M. N. Rahaman, Journal of Materials Research 20, 3312 (2005).
  50. [50]T. Xie, Y. Wang, C. Liu, and L. Xu, Materials 11, 646 (2018).
  51. [51]P. Ganguly, A. Jha, and K. Deori, Solid State Communications 146, 472 (2008).
  52. [52]Priyanka and A. Jha, Bulletin of Materials Science 36, 135 (2013).
  53. [53]S. O. Kasap, Principles of Electronic Materials and Devices (Tata McGraw-Hill, 2006).
  54. [54]A. Hossain, I. N. Esha, I. B. Elius, M. N. I. Khan, and K. H. Maria, Journal of Materials Science: Materials in Electronics , 1 (2020).
  55. [55]M. Muralidharan, V. Anbarasu, A. E. Perumal, and K. Sivakumar, Journal of Materials Science: Materials in Electronics 26, 6352 (2015).
  56. [56]J. Qi, M. Cao, Y. Chen, Y. Fang, W. Pan, H. Hao, Z. Yao, Z. Yu, and H. Liu, Journal of Alloys and Compounds 762, 950 (2018).
  57. [57]M. S. Fu, X. Q. Liu, and X. M. Chen, Journal of the European Ceramic Society 28, 585 (2008).
  58. [58]E. R. Kipkoech, F. Azough, and R. Freer, Journal of Applied Physics 97, 064103 (2005).
  59. [59]A. Dutta, T. P. Sinha, and S. Shannigrahi, Physical Review B 76, 155113 (2007).
  60. [60]H. Trabelsi, M. Bejar, E. Dhahri, M. Sajieddine, K. Khi- rouni, P. Reprezas, B. M. G. Melo, M. A. Valente, and M. P. F. Graça, Journal of Alloys and Compounds 723, 894 (2017).
  61. [61]M. Smari, H. Rahmouni, N. Elghoul, I. Walha, E. Dhahri, and K. Khirouni, RSC Advances 5, 2177 (2014).
  62. [62]J. R. Jurado, M. T. Colomer, and J. R. Frade, Journal of the American Ceramic Society 83, 2715 (2000).
  63. [63]M. Vollman and R. Waser, Journal of the American Ceramic Society 77, 235 (1994).
  64. [64]M. Vollmann, R. Hagenbeck, and R. Waser, Journal of the American Ceramic Society 80, 2301 (1997).
  65. [65]T. Shibata, S. Chattopadhyay, B. Lin, and V. R. Palkar, in AIP Conference Proceedings, Vol. 882 (American Institute of Physics, 2007) pp. 780–782.
  66. [66]S. S. Chowdhury, A. H. M. Kamal, R. Hossain, M. Hasan, M. F. Islam, B. Ahmmad, and M. A. Basith, Ceramics International 43, 9191 (2017).
  67. [67]M. A. Basith, F. A. Khan, B. Ahmmad, S. Kubota, F. Hirose, D.-T. Ngo, Q.-H. Tran, and K. Mølhave, Journal of Applied Physics 118, 023901 (2015).
  68. [68]W. Xu, J. Yang, W. Bai, K. Tang, Y. Zhang, and X. Tang, Journal of Applied Physics 114, 154106 (2013).
  69. [69]K. C. Verma, R. K. Kotnala, N. Thakur, V. S. Rangra, and N. S. Negi, Journal of Applied Physics 104, 093908 (2008).
  70. [70]Z. Zhang, J. Hu, Z. Xu, H. Qin, L. Sun, F. Gao, Y. Zhang, and M. Jiang, Solid State Sciences 13, 1391 (2011).
  71. [71]D. A. Crandles, B. DesRoches, and F. S. Razavi, Journal of Applied Physics 108, 053908 (2010).
  72. [72]K. Potzger, J. Osten, A. A. Levin, Shalimov, G. Talut, H. Reuther, S. Arpaci, D. Bürger, H. Schmidt, T. Nestler, et al., Journal of Magnetism and Magnetic materials 323, 1551 (2011).
  73. [73]S. Middey, C. Meneghini, and S. Ray, Applied Physics Letters 101, 042406 (2012).
  74. [74]S. H. Blundell, Magnetism in Condensed Matter, 1st ed. (Oxford. Univ. Press Inc., 2001).
  75. [75]Z. Ren, G. Xu, X. Wei, Y. Liu, X. Hou, P. Du, W. Weng, G. Shen, and G. Han, Applied Physics Letters 91, 063106 (2007).
  76. [76]S. Lei, L. Liu, C. Wang, X. Shen, D. Guo, C. Wang, S. Zeng, B. Cheng, Y. Xiao, and L. Zhou, CrystEng-Comm 16, 1322 (2014).
  77. [77]B. Ahmmad, K. Kanomata, K. Koike, S. Kubota, H. Kato, F. Hirose, A. Billah, M. A. Jalil, and M. A. Basith, Journal of Physics D: Applied Physics 49, 2650003 (2016).

Paper details

vlnc:W_y3mea8ar
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 7

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents