Engineering the spin-orbit torque efficiency and magnetic properties of Tb/Co ferrimagnetic multilayers by stacking order

Abstract

We measured the spin-orbit torques (SOTs), current-induced switching, and domain wall (DW) motion in synthetic ferrimagnets consisting of Co/Tb layers with differing stacking order grown on a Pt underlayer. We find that the SOTs, magnetic anisotropy, compensation temperature and SOT-induced switching are highly sensitive to the stacking order of Co and Tb and to the element in contact with Pt. Our study further shows that Tb is an efficient SOT generator when in contact with Co, such that its position in the stack can be adjusted to generate torques additive to those generated by Pt. With optimal stacking and layer thickness, the dampinglike SOT efficiency reaches up to 0.3, which is more than twice that expected from the Pt/Co bilayer. Moreover, the magnetization can be easily switched by the injection of pulses with current density of about 0.5-2*107A/cm2 despite the extremely high perpendicular magnetic anisotropy barrier (up to 7.8 T). Efficient switching is due to the combination of large SOTs and low saturation magnetization owing to the ferrimagnetic character of the multilayers. We observed current-driven DW motion in the absence of any external field, which is indicative of homochiral Néel-type DWs stabilized by the interfacial Dzyaloshinkii-Moriya interaction. These results show that the stacking order in transition metal/rare-earth synthetic ferrimagnets plays a major role in determining the magnetotransport properties relevant for spintronic applications.

Introduction

Magnetization switching and domain wall (DW) motion driven by spin-orbit torques (SOTs) have attracted extensive research interest due to their potential applications in nonvolatile memory and logic technologies [1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14]. To improve the scalability and thermal stability of devices in these applications, materials with perpendicular magnetic anisotropy (PMA) are often preferred. Ultrathin films of 3d transition metals and alloys (e.g., Co or CoFeB) have been widely investigated for such purposes, where the interfacial spin-orbit coupling gives rise to the PMA [15, 16, 17, 18]. Recently, however, increasing interest has been devoted to ferrimagnetic alloys of rare earth metals and transition metals possessing bulk PMA [19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37]. In these compounds, the rare-earth-metal and transition-metal magnetic sublattices are coupled antiparallel to each other, resulting in a reduced total magnetic moment relative to the individual sublattices [38, 39]. The low magnetization allows for efficient SOT-induced switching, whereas the large PMA increases the thermal stability of the devices. Moreover, the possibility of obtaining angular momentum compensation allows for antiferromagnet-like magnetization dynamics that, e.g., leads to ultrafast switching and DW motion [31, 32, 33]. To date, studies of SOTs and related phenomena have mainly focused on the alloy form of the rare-earth-metal–transition-metal systems [19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33], whereas multilayer structures have been less explored [34, 35, 36, 37]. In such structures, the stacking order and the thickness of each layer offer additional degrees of freedom to tune the SOTs and understand the role of each element in interface-driven phenomena [13].

Theoretical [40] and experimental [34, 37, 41, 42, 43, 44] studies suggest that the rare-earth elements with partially filled ff orbitals are candidates for generating large spin Hall effect, and hence can be used as a source of SOTs. The strong spin-orbit interaction in the rare earth metals combined with the inversion symmetry breaking at their interfaces with transition metals can also produce sizeable Rashba-Edestein effect and Dzyaloshinkii-Moriya interaction (DMI). The latter stabilizes homochiral Néel-type domain walls with efficient and ultrafast current-induced dynamics [9, 10, 11, 45, 46, 47].

Motivated by the above considerations, we investigate the influence of the stacking order and layer thickness on current-induced SOTs, switching, and DW motion in Pt/Co/Tb-based multilayers. Harmonic Hall and magneto-optic Kerr effect measurements reveal strong SOTs in the perpendicularly magnetized Tb/Co multilayers, which lead to efficient current-induced switching and DW motion, comparable to those of TbCo alloys in contact with Pt. Moreover, the SOTs and other magnetic properties, such as the saturation magnetization, magnetic anisotropy, compensation temperature, and the anomalous Hall effect (AHE) are highly sensitive to the stacking order as well as to the element in contact with the Pt underlayer. We find that Tb can be an effective source of SOTs with additive contributions to the ones due to Pt when placed on top of Pt/Co. These results show that the stacking order in rare-earth-metal/transition-metal multilayers offers an additional degree of freedom to tune the efficiency of SOT-controlled switching and DW motion.

Sample preparation and characterization

We grow Pt(4)/Tb(tTbt_{\mathrm{Tb}})/[Co(0.5)/Tb(0.65)/Co(0.5)] and Pt(4)/[Co(0.5)/Tb(0.65)/Co(0.5)]/Tb(tTbt_{\mathrm{Tb}}) multilayers with PMA as well as Pt(5)/Tb(tTbt_{\mathrm{Tb}})/Co(5) and Pt(5)/Co(5)/Tb(tTbt_{\mathrm{Tb}}) trilayers with in-plane anisotropy on thermally oxidized silicon substrates by dc magnetron sputtering (numbers indicate the thickness in nm). For all layers, a Ti capping of 5 nm and a Ta seed layer of 3 nm are used. The base pressure and Ar partial pressure of the deposition chamber are 6×10−86 \times10^{-8} mbar and 4×10−34 \times10^{-3} mbar, respectively. The first two series, schematically illustrated in Figure 1(a), are used for the SOTs, current-induced switching, and DW motion studies, whereas in the last two series only the SOTs are quantified. In the samples with PMA we fix the layers between square brackets and change the Tb thickness (tTbt_{\mathrm{Tb}}) and position relative to them; similarly, in the trilayers with in-plane anisotropy we changed the Tb thickness and position relative to Co. Hall bar devices are fabricated by patterning the substrates using optical lithography before deposition and subsequent lift-off.

Schematic illustration of the Co/Tb/Co multilayers and magnetization measurements

Figure 1. (a) Schematic illustration of the Co/Tb/Co multilayers with different stacking order. (b) Magnetization curves of Pt/Tb(1)/[Co/Tb/Co] and Pt/[Co/Tb/Co]/Tb(1). (c) Saturation magnetization versus Tb thickness.

In Figure 1(b) we show representative magnetization curves measured by a superconducting quantum interference device at room temperature with an out-of-plane field sweep for the two different positions of the Tb(1) layer with respect to the fixed [Co/Tb/Co] trilayer. Both sets of data show clear hysteresis and nearly 100% remanence at zero field, indicative of strong PMA. However, their saturation magnetization (MsM_{\mathrm{s}}) differs significantly even though the amount of Tb and Co is the same in both multilayers. Measurements of all the six samples

with PMA Figure 1(c) show that MsM_{\mathrm{s}} is larger when Co is in direct contact with Pt except for the thickest Tb samples. In both multilayer systems, MsM_{\mathrm{s}} is significantly smaller relative to that expected for Co (>106>10^{6} A/m), as expected due to the antiferromagnetic coupling of Co and Tb. The large difference in MsM_{\mathrm{s}} and its dependence on Tb thickness indicate that the net magnetization is highly sensitive to the stacking order.

Figure 2(a) shows the device layout with the electrical connections and the coordinate system. Figure 2(b) reports the sheet resistance RsR_{\mathrm{s}} measured using a four-point geometry in the structures with PMA. RsR_{\mathrm{s}} is about 20% larger in samples with Pt/Tb interface compared with those with Pt/Co interface. The larger RsR_{\mathrm{s}} and its increase with tTbt_{\mathrm{Tb}} in Pt/Tb(tTbt_{\mathrm{Tb}})/[Co/Tb/Co] might be due to increased interfacial electron scattering and/or intermixing between Tb and Pt in this system. In contrast, in Pt/[Co/Tb/Co]/Tb(tTbt_{\mathrm{Tb}}), RsR_{\mathrm{s}} does not significantly change with the Tb thickness, suggesting that the electric conductivity is predominantly dictated by the Pt and Co layers. The resistivity ρ\rho of all six multilayers with PMA, estimated by considering only the conduction through Pt, Co, and Tb and neglecting the contribution from the buffer and capping layers is reported in Table II along with the other properties measured in this study.

Hall bar device, coordinate system, and magnetic measurements

Figure 2. (a) Schematics of a Hall bar device and coordinate system. The Hall bar channel is 100 μm long and 5 μm wide. (b) Sheet resistance versus thickness of Tb layer in Pt/Tb(tTbt_{\mathrm{Tb}})/[Co/Tb/Co] and Pt/[Co/Tb/Co]/Tb($t_{\mathrm{Tb}}). (c) Hall resistance as a function of out-of-plane magnetic field in samples with different Tb thickness. (d) Coercive field versus temperature in Pt/Tb(1,1.5)/[Co/Tb/Co]. The regions shaded in blue and magenta represent temperature ranges in which the magnetization is strongly polarized (saturated). (e) Magnetization compensation temperature as a function of Tb thickness. The black arrow indicates that TM>370T_{\mathrm{M}} > 370 K, which is the largest temperature reached in our setup; the green solid line indicates room temperature. (f) Anisotropy field at room temperature versus Tb thickness.

In alloys of rare earth metals and transition metals and in multilayers, the magnetotransport properties are dominated by the 3d4s3d4s orbitals of the transition-metal elements near the Fermi level; thus the AHE is mainly driven by the transition-metal sublattice [20, 34, 48]. In Figure 2(c) we report the Hall resistance RHR_{\mathrm{H}} as a function of out-of-plane magnetic field. As evident from the data, the AHE is positive and large in the Pt/[Co/Tb/Co]/Tb series as opposed to the Pt/Tb/[Co/Tb/Co] series, where the AHE is negative and relatively small. This means that ii) at room temperature the total magnetization is dominated by the Co (Tb) sublattice for the layers with Pt/Co (Pt/Tb) interface and that the magnetic compensation temperature TMT_{\mathrm{M}} is below (above) room temperature; iiii) the Pt/Co interface has a significant contribution to the AHE, in agreement with literature data [49]. Our data clearly show that the stacking order plays a crucial role in determining the magnetic compensation point as well as the AHE, in addition to MsM_{\mathrm{s}} and RsR_{\mathrm{s}} discussed earlier. We further study the coercive field (HcH_{\mathrm{c}}) as a function of temperature to characterize TMT_{\mathrm{M}} of all six samples. As the temperature crosses TMT_{\mathrm{M}}, the anomalous Hall resistance RHR_{\mathrm{H}} changes sign; further, HcH_{\mathrm{c}} diverges because a stronger external field is required to reverse the vanishing net magnetization [50], as shown for Pt/Tb(1; 1.5 nm)/[Co/Tb/Co] in Figure 2(d). TMT_{\mathrm{M}} determined from the change of sign of RHR_{\mathrm{H}} is shown in Figure 2(e) for all the six samples. The stacking order gives rise to a substantial difference of more than 100 K in TMT_{\mathrm{M}} between Pt/Tb(tTbt_{\mathrm{Tb}})/[Co/Tb/Co] and Pt/[Co/Tb/Co]/Tb(tTbt_{\mathrm{Tb}}), which is likely related to the larger MsM_{\mathrm{s}} of Pt/[Co/Tb/Co]/Tb(tTbt_{\mathrm{Tb}}).

Finally, we characterize the effective magnetic anisotropy field HanH_{\mathrm{an}} by measuring RHR_{\mathrm{H}} in the samples with PMA as a function of an external magnetic field applied nearly in plane at polar and azimuthal angles θH=88∘\theta_{\mathrm{H}} = 88^\circ and φH=90∘\varphi_{\mathrm{H}} = 90^\circ [see Figure 2(a) for the definition of the angular coordinates]. We use a macrospin approximation to calculate Han=H(sin⁡θHsin⁡θ−cos⁡θHcos⁡θ)H_{\mathrm{an}} = H \left(\frac{\sin\theta_{\mathrm{H}}}{\sin\theta} - \frac{\cos\theta_{\mathrm{H}}}{\cos\theta}\right), where θ=arccos⁡[RAHERAHE]\theta= \arccos\left[\frac{R_{\mathrm{AHE}}}{R_{\mathrm{AHE}}}\right], as reported in Figure 2(f). We find μ0Han=7.8±0.5\mu_0 H_{\mathrm{an}} = 7.8 \pm0.5 T in Pt/Tb(1)/[Co/Tb/Co], which rapidly decreases with

increasing Tb thickness due to the shift of TMT_{\mathrm{M}} to higher temperatures. In the Pt/[Co/Tb/Co]/Tb(1) series, on the other hand, HanH_{\mathrm{an}} is relatively constant, which is consistent with the behavior of TMT_{\mathrm{M}} in these samples. We note that extremely large anisotropy fields in excess of 3 T are measured in all of our samples, with the exception of Pt/Tb(2)/[Co/Tb/Co].

Results and Discussion

SOTs in multilayers with PMA

The SOT-induced effective fields are quantified by performing harmonic Hall effect measurements in the PMA samples [52, 53]. An alternating current with frequency ω/2π=10\omega/2\pi= 10 Hz and amplitude j=0.3j = 0.3–1×1071 \times10^{7} A/cm2^{2} is applied along the xx axis, and the first- and second-harmonic Hall resistances (RH1ωR_{\mathrm{H}}^{1\omega} and RH2ωR_{\mathrm{H}}^{2\omega}) were measured during an in-plane field sweep along the xx and yy axes (HxH_x, HyH_y). The current density is estimated by dividing the current by the total cross section of the Pt, Co, and Tb layers. We neglect the conductivity of the highly resistive Ta buffer and Ti capping layers. In multilayers with inversion symmetry along the zz axis and current injection along xx, the dampinglike and fieldlike SOT effective fields are given by HDL=HDL(y×M)\mathbf{H}_{\mathrm{DL}} = H_{\mathrm{DL}}(\mathbf{y} \times\mathbf{M}) and HFL=HFLy\mathbf{H}_{\mathrm{FL}} = H_{\mathrm{FL}}\mathbf{y}, respectively, where M\mathbf{M} is the unit vector of the magnetization and the current-induced spin accumulation is polarized along y\mathbf{y} [13]. In order to define the sign of the field amplitudes HDL,FLH_{\mathrm{DL,FL}}, we adopt the convention that HDLH_{\mathrm{DL}} (HFLH_{\mathrm{FL}}) is positive (negative) when the field points in the same

direction as in Pt/Co (opposite direction to the Oersted field), where Pt is deposited before Co [52]. Due to the large PMA in our samples, we opt for the small-angle approximation method where the magnetization is slightly tilted away from equilibrium by the applied field. In this regime, the effective fields can be estimated using the following relations [54, 55]:

ΔHx(y)=(∂RH2ω∂Hx(y)/∂2RH1ω∂Hx(y)2),(1)\Delta H_{x(y)} = \left(\frac{\partial R_{\mathrm{H}}^{2\omega}}{\partial H_{x(y)}} \bigg/ \frac{\partial^2 R_{\mathrm{H}}^{1\omega}}{\partial H_{x(y)}^2}\right), \tag*{(1)}
HDL(FL)=−2ΔHx(y)±νΔHy(x)1−4ν2,(2)H_{\mathrm{DL(FL)}} = -2\frac{\Delta H_{x(y)} \pm\nu\Delta H_{y(x)}}{1 - 4\nu^2}, \tag*{(2)}

where ν\nu is the ratio of the planar Hall resistance RPHER_{\mathrm{PHE}} to the anomalous Hall resistance RAHER_{\mathrm{AHE}} and ±\pm corresponds to the measurements taken when the magnetization is pointing along the ±z\pm z direction. To characterize RAHER_{\mathrm{AHE}} and RPHER_{\mathrm{PHE}}, we use the first-harmonic signal given by RHω=RAHEcos⁡θ+RPHEsin⁡2θsin⁡2φR_{\mathrm{H}}^{\omega} = R_{\mathrm{AHE}}\cos\theta+ R_{\mathrm{PHE}}\sin^2\theta\sin2\varphi. Since the magnetization cannot be fully saturated in plane by the available field, we quantify RPHER_{\mathrm{PHE}} by measuring RHωR_{\mathrm{H}}^{\omega} with an external field applied at (θH,φH)=(88∘,45∘)(\theta_{\mathrm{H}}, \varphi_{\mathrm{H}}) = (88^\circ, 45^\circ). We then separate the antisymmetric and symmetric signal contributions (with respect to the field reversal), which originate from the first and second terms in the above equation, respectively. The antisymmetric signal is then plotted as a function of sin⁡2θ\sin^{2}\theta, where θ\theta is estimated using the macrospin approximation as θ=arccos⁡∣RH1ω/RAHE∣\theta= \arccos\left|R_{\mathrm{H}}^{1\omega}/R_{\mathrm{AHE}}\right|. Finally the slope of the linear fit represents RPHER_{\mathrm{PHE}}. The details of this approach can be found in Ref. [52].

Figure 3 shows representative RH1ωR_{\mathrm{H}}^{1\omega} and RH2ωR_{\mathrm{H}}^{2\omega} measurements taken from the Pt/[Co/Tb/Co]/Tb(1.5) and Pt/Tb(1)/[Co/Tb/Co] samples. RH1ωR_{\mathrm{H}}^{1\omega} has a parabolic field dependence due to the coherent rotation of the magnetization. Note that we only plot the data corresponding to the HxH_x sweep since the HyH_y sweep shows an identical behavior. The sign of RHωR_{\mathrm{H}}^{\omega} is opposite in these two samples for a given magnetization orientation due to the opposite AHE [see Figure 2(c)]. RH2ωR_{\mathrm{H}}^{2\omega} varies linearly with both HxH_x and HyH_y as expected from the action of SOTs. We note that the slopes of RH2ωR_{\mathrm{H}}^{2\omega} are opposite in Co-like and Tb-like samples. Considering also the opposite sign of RH1ωR_{\mathrm{H}}^{1\omega} in these two samples we conclude that the SOT effective fields have the same sign in both systems. Thus, the SOTs act on the net magnetization, in agreement with previous works [21, 23]. The SOT effective fields normalized by the current density, χDL(FL)=μ0HDL(FL)/j\chi_{\mathrm{DL(FL)}} = \mu_{0}H_{\mathrm{DL(FL)}}/j, are summarized in Figure 4(a)–Figure 4b as a function of Tb thickness. The values of χDL(FL)\chi_{\mathrm{DL(FL)}} are obtained by performing a linear fit of HDL(FL)H_{\mathrm{DL(FL)}} versus jj for both magnetization orientations (not shown). The fieldlike component includes also

Dampinglike and fieldlike spin-orbit torque effective fields and efficiencies versus Tb thickness

Figure 4. (a) Dampinglike and (b) fieldlike SOT effective field per unit current density χDL,FL\chi_{\mathrm{DL,FL}} versus Tb thickness in Pt/[Co/Tb/Co]/Tb(tTbt_{\mathrm{Tb}}) and (b) Pt/Tb(tTbt_{\mathrm{Tb}})/[Co/Tb/Co]. (c) Dampinglike and (d) fieldlike SOT efficiency ξDL,FL\xi_{\mathrm{DL,FL}} versus Tb thickness. The error bars take into account the errors of the linear and parabolic fits of RHωR_{\mathrm{H}}^{\omega} and RH2ωR_{\mathrm{H}}^{2\omega} respectively, averaged according to Eq. (2) for each current density, propagated in the linear fits of HDL(FL)(j)H_{\mathrm{DL(FL)}}(j) for the +Mz+M_z and −Mz-M_z configurations.

the Oersted field contribution due to the current flowing through Pt, which we estimate as μ0HOe/j=0.3 mT 10−7A−1cm2\mu_{0}H_{\mathrm{Oe}}/j = 0.3\ \mathrm{mT}\ 10^{-7}\mathrm{A}^{-1}\mathrm{cm}^{2} by Ampere’s law [51]. The Oersted field points in the opposite direction to the fieldlike component of the SOT field, and can be neglected due to its small amplitude compared with HFLH_{\mathrm{FL}}. We observe that χDL\chi_{\mathrm{DL}} is very strong in Pt/Tb(1)/[Co/Tb/Co], reaching up to +72 mT 10−7A−1cm2+72\ \mathrm{mT}\ 10^{-7}\mathrm{A}^{-1}\mathrm{cm}^{2} but rapidly decreasing as the Tb thickness is increased. Also χFL\chi_{\mathrm{FL}} reaches remarkable values, about +25 mT 10−7A−1cm2+25\ \mathrm{mT}\ 10^{-7}\mathrm{A}^{-1}\mathrm{cm}^{2} in both Pt/Tb(1)/[Co/Tb/Co] and Pt/[Co/Tb/Co]/Tb(1). To compare the SOTs in different layers on an equal footing we calculate the SOT efficiencies ξDL(FL)=2eℏMstMχDL(FL)\xi_{\mathrm{DL(FL)}} = \frac{2e}{\hbar}M_{\mathrm{s}}t_{\mathrm{M}}\chi_{\mathrm{DL(FL)}} [56], where ee is the electron charge, ℏ\hbar is the reduced Planck’s constant, and tMt_{\mathrm{M}} is the magnetic layer thickness. The SOT efficiencies are plotted in Figure 4(c,–Figure 4d) as a function of Tb thickness. We observe that ξDL\xi_{\mathrm{DL}} and ξFL\xi_{\mathrm{FL}} vary between +0.1+0.1 and +0.3+0.3 and between +0.03+0.03 and +0.2+0.2, respectively. Whereas ξDL\xi_{\mathrm{DL}} and ξFL\xi_{\mathrm{FL}} in Pt/[Co/Tb/Co]/Tb(1) and Pt/Tb(1)/[Co/Tb/Co] are comparable to those measured in Pt/Co bilayers [13, 52], we observe that both efficiencies increase strongly as a function of Tb thickness in Pt/[Co/Tb/Co]/Tb(tTbt_{\mathrm{Tb}}), reaching values that are about two times larger compared with Pt/Co. Moreover, ξFL\xi_{\mathrm{FL}} is significantly larger in Pt/[Co/Tb/Co]/Tb(tTbt_{\mathrm{Tb}}) compared with that in Pt/Tb(tTbt_{\mathrm{Tb}})/[Co/Tb/Co], and has a different thickness dependence in the two series. Similar trends are also observed if we consider the SOT efficiency per unit electric field ξDL(FL)E=ξDL(FL)/ρ\xi_{\mathrm{DL(FL)}}^{E} = \xi_{\mathrm{DL(FL)}}/\rho (see Table II).

First and second harmonic Hall resistance measurements

Figure 3. First and second harmonic of the Hall resistance (RH1ωR_{\mathrm{H}}^{1\omega} and RH2ωR_{\mathrm{H}}^{2\omega}, respectively) versus in-plane longitudinal and transverse magnetic fields (HxH_x and HyH_y) measured using j=0.8×107 A/m2j = 0.8 \times10^{7}\ \mathrm{A/m}^{2} in (a) Pt/[Co/Tb/Co]/Tb(1.5) and (b) Pt/Tb(1)/[Co/Tb/Co].

We note that ξDLj\xi_{\mathrm{DL}}^{j} and ξFLj\xi_{\mathrm{FL}}^{j} are obtained by normalization to the average current density jj flowing in the multilayers, such that even larger efficiencies would be obtained by normalization to the current density flowing in Pt, as often done in the literature. The dependence of ξDL(FL)j\xi_{\mathrm{DL(FL)}}^{j} on the stacking order and Tb thickness can have several origins. First, the structural details of the multilayers and of the interface with Pt generally change with the stacking order, which may ultimately lead to changes of the SOTs. This point is supported by the resistivity measurements, which suggest that Tb deposited on Pt induces intermixing between the two species rather than favoring sharp interfaces. Second, the Tb layer can be a source of dampinglike and fieldlike SOTs in itself, with a contribution opposite to that of Pt. Such a scenario, which agrees with a previous study of Pt/[Co/Ni]/Co/Tb multilayers [37], is consistent with the enhancement of ξDL(FL)j\xi_{\mathrm{DL(FL)}}^{j} when Pt and Tb are placed on opposite sides of the [Co/Tb/Co] trilayer. Third, placing the Tb layer on top of the stack might provide an efficient sink for the spin current generated by Pt and the Pt/Co interface [57]. The monotonic increase of the dampinglike and fieldlike SOTs in this series is consistent with both the second and third explanation taking into account the finite spin diffusion length of Tb.

Overall, even if the exact mechanism giving rise to the enhancement of ξDLj\xi_{\mathrm{DL}}^{j} and ξFLj\xi_{\mathrm{FL}}^{j} cannot be singled out with certainty, our data indicate that Tb and the stacking order of Co/Tb multilayers play a crucial role in determining the strength of the SOTs.

SOTs in Pt/Tb/Co and Pt/Co/Tb trilayers with in-plane magnetic anisotropy

We quantify the dampinglike SOT efficiency in samples with in-plane anisotropy following the method outlined in Ref. [58]. Injection of a relatively small alternating current (ω/2π=10 Hz\omega/2\pi= 10\ \mathrm{Hz}, j=0.3j = 0.3–1×107 A/cm21 \times10^{7}\ \mathrm{A/cm^{2}}) gives rise to periodic oscillations of the magnetization about its equilibrium position. The second-harmonic Hall resistance related to the current-induced fields and the thermoelectric signal due to Joule heating can be written as:

RH2ω=(RAHEHDLHext+I0α∇T)cos⁡φ+2RPHE(2cos⁡3φ−cos⁡φ)HFL+HOeHext+Hdem(3)R_{\mathrm{H}}^{2\omega} = \left(R_{\mathrm{AHE}}\frac{H_{\mathrm{DL}}}{H_{\mathrm{ext}}} + I_0\alpha\nabla T\right)\cos\varphi+ 2R_{\mathrm{PHE}}(2\cos^3\varphi-\cos\varphi)\frac{H_{\mathrm{FL}}+H_{\mathrm{Oe}}}{H_{\mathrm{ext}}+H_{\mathrm{dem}}} \tag*{(3)}

where I0I_0 is the amplitude of the injected current, α\alpha the anomalous Nernst coefficient, ∇T\nabla T the perpendicular thermal gradient and HdemH_{\mathrm{dem}} the demagnetizing field. Figure 5(a) shows a representative angle scan measurement of RH2ωR_{\mathrm{H}}^{2\omega} in Pt/Co/Tb(3) for different external in-plane fields along with the fitting curves (dashed lines) given by Eq. (3). In Figure 5(b) we plot the cos⁡φ\cos\varphi component of RH2ωR_{\mathrm{H}}^{2\omega}, which includes the combined contributions of dampinglike torque and the Nernst (and/or Seebeck) effect. The amplitude of the cos⁡φ\cos\varphi component of RH2ωR_{\mathrm{H}}^{2\omega} decreases on increasing the external field. The latter tends to rigidly align the magnetization along its direction, suppressing the periodic oscillations. This results in a reduction of the SOT and therefore of RH2ωR_{\mathrm{H}}^{2\omega} and its cos⁡φ\cos\varphi component. This field dependence can be exploited to further separate the dampinglike torque and the thermoelectric effects in the cos⁡φ\cos\varphi component of RH2ωR_{\mathrm{H}}^{2\omega}. The anomalous Nernst effect depends only on the magnetization direction and not on the external field amplitude (provided that the magnetization is saturated), whereas the SOT decreases at higher field, as already discussed. Thus, the dampinglike effective field HDLH_{\mathrm{DL}} can be quantified by performing a linear fit of the cos⁡φ\cos\varphi component of RH2ωR_{\mathrm{H}}^{2\omega} versus the inverse of the external field plus the demagnetizing field HdemH_{\mathrm{dem}} [58], as shown in the inset of Figure 5(b). This experiment is repeated for all the samples for several current densities to estimate χDL\chi_{\mathrm{DL}} as the slope of HDLH_{\mathrm{DL}} versus jj, as done for the multilayers with PMA in Sect. III A. The values of χDL\chi_{\mathrm{DL}} are reported in Table I. Compared with the multilayers with PMA, the dampinglike effective field in the samples with in-plane anisotropy is 2 orders of magnitude lower. This is due to the larger magnetization on which the SOT acts, that is dominated by the bulk magnetic moments of the Co layer (the ferromagnetic layer is now thick). The dampinglike SOT efficiency, calculated also here as ξDLj=2eℏMstMχDL\xi_{\mathrm{DL}}^{j} = \frac{2e}{\hbar}M_{\mathrm{s}}t_{\mathrm{M}}\chi_{\mathrm{DL}}, is plotted in Figure 5(c) as a function of tTbt_{\mathrm{Tb}}. Although ξDLj\xi_{\mathrm{DL}}^{j} is significantly lower in these samples

Second-harmonic Hall resistance and dampinglike spin-orbit torque efficiency

Figure 5. (a) In-plane angular dependence of the second-harmonic Hall resistance of Pt/Co/Tb(3) for j=0.8×107 A/cm2j = 0.8 \times10^{7}\,\mathrm{A/cm^{2}}. (b) Dampinglike and thermal contribution to the second-harmonic Hall resistance. Inset: linear fit of the cosine component of the second-harmonic Hall resistance versus the inverse of the external field and the demagnetizing field acting against the current-induced field. (c) Dampinglike SOT efficiency versus Tb thickness. The error bars take into account the uncertainty of the linear fit of HDLH_{\mathrm{DL}} versus jj.

compared with the samples with PMA, it scales in the same way with tTbt_{\mathrm{Tb}}, increasing (decreasing) in the trilayer with Pt/Co (Pt/Tb) interface. The comparison between Pt/Tb/Co and Pt/Co/Tb structures provides further evidence that the SOTs are very sensitive to tTbt_{\mathrm{Tb}} and the stacking order of Co/Tb.

Current-induced magnetization switching

The large SOTs evidenced by the harmonic Hall effect measurements in Sect. III A can be exploited to realize current-induced magnetization switching with enhanced efficiency relative, e.g., to Pt/Co bilayers. In order to study SOT-induced switching in our multilayers with PMA, we injected 10-ms-long current pulses of variable amplitude through the Hall bar devices in the presence of an in-plane bias field HxH_x applied parallel to the current line. This field is required to break the SOT symmetry and uniquely define the switching polarity [1, 13]. Figure 6(a) shows representative AHE hysteresis loops as a function of current measured for Pt/Tb(2)/[Co/Tb/Co] and Pt/[Co/Tb/Co]/Tb(2). In both samples, the net mag-

Threshold current switching measurements and current-density dependence

Figure 6. (a) Change of the anomalous Hall resistance due to SOT-induced switching in Pt/Tb(2)/[Co/Tb/Co] with constant in-plane field μ0Hx=182 mT\mu_0H_x = 182\,\mathrm{mT} and in Pt/[Co/Tb/Co]/Tb(2) with μ0Hx=333 mT\mu_0H_x = 333\,\mathrm{mT}. The Hall resistance is plotted versus the amplitude IpI_p of 10-ms-long current pulses. (b) Threshold current density for switching as function of the in-plane field μ0Hx\mu_0H_x.

TABLE I. Saturation magnetization, demagnetizing field, dampinglike effective field per unit current density and SOT efficiency in trilayers with in-plane anisotropy. Errors are a fraction of the least significant digit.

MsM_{\mathrm{s}} (106 A m−110^{6}\,\mathrm{A\,m^{-1}})μ0Hdem\mu_{0}H_{\mathrm{dem}} (T)χDL\chi_{\mathrm{DL}} (mT 10−7 A−1 cm210^{-7}\,\mathrm{A^{-1}\,cm^{2}})ξDLj\xi_{\mathrm{DL}}^{j}
Pt/Tb(1)/Co1.131.800.190.040
Pt/Tb(3)/Co0.811.590.120.023
Pt/Tb(5)/Co0.481.480.100.014
Pt/Co/Tb(1)1.220.750.270.061
Pt/Co/Tb(3)0.810.720.370.073
Pt/Co/Tb(5)0.680.560.440.091

Table 1.

netization switches from +Mz+M_z to −Mz-M_z when the current is parallel to the in-plane field and from −Mz-M_z to +Mz+M_z when it is antiparallel to it. The loops of Figure 6(a) have opposite polarity because the AHE has opposite sign in these two samples at room temperature [see Fig. 2(c)].

We repeate the measurements summarized in Figure 6(a) for all of the multilayers with PMA and several in-plane magnetic fields to characterize the threshold current density jthj_{\mathrm{th}} required to switch the magnetization. The data are shown in Figure 6(b) as a function of μ0Hx\mu_0 H_x. In the macrospin approximation, the threshold switching current is given by [29, 59]

jth=2eℏμ0MstMξDLj(Hk2−Hx2),(4)j_{\mathrm{th}} = \frac{2e}{\hbar}\frac{\mu_0 M_s t_M}{\xi_{\mathrm{DL}}^j}\left(\frac{H_k}{2} - \frac{H_x}{\sqrt{2}}\right), \tag*{(4)}

where tMt_M is the thickness of the magnetic layer. Although Eq. (4) does not apply to switching by domain nucleation and propagation, which is the preferred mode of magnetization reversal in mesoscopic samples [47], one still expects jthj_{\mathrm{th}} to scale with HkH_k and HxH_x given that these two fields

determine the domain nucleation barrier. Figure 6(b) shows that, despite the very large HkH_k of our multilayers (see Sect. II), we are able to switch all of the samples with current densities below 2.5×107 A/cm22.5 \times10^7\,\mathrm{A/cm^2} and in-plane field Hx≪HkH_x \ll H_k. This is due to the combined effect of strong dampinglike SOTs and low MsM_s owing to the ferrimagnetic character of our multilayers. The strongest dependence of jthj_{\mathrm{th}} on HxH_x is found in the sample with weakest magnetic anisotropy, namely Pt/Tb(2)/[Co/Tb/Co], as expected. The samples with strongest anisotropy, where μ0Hk≥6 T\mu_0H_k \geq6\,\mathrm{T}, present a much weaker dependence of jthj_{\mathrm{th}} on HxH_x, suggesting that the in-plane field is not the main cause of reduction of the domain nucleation barrier in such a case. On the other hand, jthj_{\mathrm{th}} scales with ξDL\xi_{\mathrm{DL}} and MsM_s in samples with comparable anisotropy, such as in the Pt/[Co/Tb/Co]/Tb(tTbt_{\mathrm{Tb}}) series.

To investigate the role of Joule heating in the switching experiments, we measure the Hall effect by injecting different current densities up to j≃2×107 A/cm2j \simeq2 \times10^7\,\mathrm{A/cm^2}. We find that the coercivity decreases by about 30% upon increasing jj from 0.5 to 2×107 A/cm22 \times10^7\,\mathrm{A/cm^2} (not shown). Likewise, we also estimate the anisotropy field μ0Hk\mu_0H_k in all the multilayers and record a drop smaller than 25% from the case of j<1×107 A/cm2j < 1 \times10^7\,\mathrm{A/cm^2} to the case of j=2×107 A/cm2j = 2 \times10^7\,\mathrm{A/cm^2}. Therefore we conclude that the Joule heating does not play a major role in determining jthj_{\mathrm{th}} for j<1×107 A/cm2j < 1 \times10^7\,\mathrm{A/cm^2}, whereas it partially assists the switching at higher current by decreasing the magnetic anisotropy energy barrier and favoring DW depinning. Indeed, jthj_{\mathrm{th}} is determined by the interplay of several factors beyond HkH_k, HxH_x, ξDL\xi_{\mathrm{DL}}, and MsM_s, which include Joule heating as well as ξFL\xi_{\mathrm{FL}}, the DMI and DW pinning properties of the multilayers. Overall, these data show that SOTs can switch ferrimagnetic multilayers with very strong PMA at a current density of the order of 107 A/cm210^7\,\mathrm{A/cm^2}, similarly to what is observed in CoTb alloys [28].

Current-induced domain wall motion

SOTs can efficiently move DWs in suitable devices and heterostructures [31]. Compensated ferrimagnets are particularly interesting for the SOT-induced DW motion because the DWs can be propelled at very high speeds with moderate currents owing to their particular dynamical properties near the magnetic and angular momentum compensation [11, 27, 31, 32, 60, 61, 62]. We investigate the current-induced DW motion in the Pt/[Co/Tb/Co]/Tb(tTbt_{\mathrm{Tb}}) samples. We use a wide-field Kerr microscope configured in the polar geometry to detect the out-of-plane magnetization component in Pt/[Co/Tb/Co]/Tb(tTbt_{\mathrm{Tb}}) racetracks and study the DW response to external fields and currents. The experimental procedure can be briefly described as follows. First, the magnetization is saturated along +z+z or −z-z by applying an out-of-plane magnetic field larger than the coercivity. Next, a domain with the opposite magnetization is nucleated by the Oersted field produced by a short current pulse InucI_{\mathrm{nuc}} injected into an electrically insulated wire crossing the racetrack [Figure 7(a)]. Finally, the DW is displaced by injecting current pulses along the DW track. We perform two types of experiments: i) determination of the critical current for depinning a single DW in the presence or absence of an out-of-plane field (HzH_z); ii) determination of the DW velocity in the absence of any applied field.

Differential Kerr microscopy image, critical current density, and effective fields

Figure 7. (a) Differential Kerr microscopy image showing the nucleation of a magnetic domain (white region) in a Pt/[Co/Tb/Co]/Tb(1) racetrack delimited by the red dotted line. (b) Critical current density required to depin up-down and down-up DWs as a function of applied out-of-plane magnetic field in Pt/[Co/Tb/Co]/Tb(1). (c) Effective out-of-plane magnetic field corresponding to the depinning field ΔHdepin\Delta H_{\mathrm{depin}} (squares) and dampinglike SOT effective field −π/2×HDL-\pi/2 \times H_{\mathrm{DL}} (circles) versus current density for both DWs and magnetic states in Pt/[Co/Tb/Co]/Tb(1).

Figure 7(b) shows the critical current density jdepinj_{\mathrm{depin}} required to depin a DW as function of HzH_z for both the up-down and down-up DWs in Pt/[Co/Tb/Co]/Tb(1). The linear variation of jdepin(Hz)j_{\mathrm{depin}}(H_z) shows that the current induces a dampinglike SOT that acts as an effective magnetic field along ±z\pm z, assisting or hindering HzH_z to depin the DWs [9, 11, 63, 64]. In the one-dimensional DW model, neglecting the spin-transfer and fieldlike torques,

the effective field induced by the current is given by Hzeff=ΔHdepinH_z^{\mathrm{eff}} = \Delta H_{\mathrm{depin}}, where ΔHdepin\Delta H_{\mathrm{depin}} is the change in the DW depinning field under dc current injection. Alternatively, we estimate Hzeff=−π2HDLcos⁡ΨH_z^{\mathrm{eff}} = -\frac{\pi}{2}H_{\mathrm{DL}}\cos\Psi, where HDLH_{\mathrm{DL}} is the dampinglike SOT effective field obtained by the harmonic Hall effect measurements in Sect. III A and Ψ\Psi is the angle between the DW magnetization and the xx axis [65]. Figure 7(c) compares HzeffH_z^{\mathrm{eff}} obtained using ΔHdepin\Delta H_{\mathrm{depin}} and −π2HDL-\frac{\pi}{2}H_{\mathrm{DL}} for different current densities. The two measurements are in excellent agreement, which implies that the DWs are of purely homochiral Néel type (i.e., Ψ=0\Psi= 0 deg). Moreover, the DW motion along the current flow indicates that they have left-handed chirality. This is consistent with the interfacial DMI occurring at the Pt/Co interface with possible additional contributions from the inner interfaces between Co and Tb and the top Tb/Ti interface [66]. Qualitatively the same results are obtained for Pt/[Co/Tb/Co]/Tb(1.5) and Pt/[Co/Tb/Co]/Tb(2), showing that the current-induced DW depinning measurements can be effectively used to identify the DW type and estimate the DL-SOT effective field in this system. Next, we characterize the current-induced DW velocities in Pt/[Co/Tb/Co]/Tb(1, 1.5, 2). To do so, we capture a sequence of Kerr images while injecting a train of current pulses through the track to move a pre-nucleated DW, as shown in Figure 8(a). To estimate the DW velocity (vDWv_{\mathrm{DW}}), we divide the total displacement by the total pulse length.

Series of Kerr differential images and DW velocity as a function of current density

Figure 8. (a) Series of Kerr differential images showing current-driven DW motion in Pt/[Co/Tb/Co]/Tb(2) as hundreds of 20-ns-long current pulses with jp=3.6×107 A/cm2j_{\mathrm{p}} = 3.6 \times10^{7}\,\mathrm{A/cm}^{2} amplitude are injected along the track. (b) DW velocity as a function of current density for different pulse widths τp=15\tau_{\mathrm{p}} = 15–100 ns in Pt/[Co/Tb/Co]/Tb(2). The errors in the DW velocity are due to the arrival time uncertainty, which is larger when a small number of pulses is used.

Figure 8(b) shows the results from Pt/[Co/Tb/Co]/Tb(2), where vDWv_{\mathrm{DW}} is plotted as function of current density jpj_{\mathrm{p}} for different pulse lengths τp\tau_{\mathrm{p}}. The data exhibit several important features. First, the current required to initiate the DW motion, i.e., the onset of the linear regime, is strongly dependent on the pulse width and is lower for longer pulses. This can be understood by the effect of thermal activation on the DW depinning, which is stronger for longer pulses. Second, in the linear regime the slope vDW/jv_{\mathrm{DW}}/j is approximately the same for all pulse widths, suggesting that Joule heating plays a minor role in vDWv_{\mathrm{DW}} unlike in the depinning process. In all of the cases, the depinning current in the Pt/[Co/Tb/Co]/Tb multilayers is comparable to that found in Pt/Co1−x_{1-x}Tbx_x ferrimagnetic alloys [27]. Third, the extrapolation of the linear fits yields velocities in the range of 10–15 m/s for jp=108j_{\mathrm{p}} = 10^8 A/cm2^2. These values are moderate in comparison with those of other ferrimagnetic [27, 31, 67] and synthetic antiferromagnetic [68] systems despite the strong SOTs.

However, we refrain from drawing definitive conclusions on the DW velocity behavior of our films based on the available data because we cannot conclude whether the upturn of the vDWv_{\mathrm{DW}} is due to the onset of a wide creep regime or the flow regime. In the former case, it is not possible to extrapolate the velocities at higher current density.

Finally, we attempt to quantify the effective DMI field HDMIH_{\mathrm{DMI}} in all the samples studied above. To do so, we measure jdepinj_{\mathrm{depin}} as function of applied in-plane field up to Hx=40H_x = 40 mT, the maximum in-plane field available in the Kerr microscope. If HxH_x is applied opposite to HDMIH_{\mathrm{DMI}}, we expect that the DW magnetization rotates first along the yy axis, i.e., the DW becomes Bloch-like for ∣Hx∣≃∣HDMI∣\lvert H_x\rvert\simeq\lvert H_{\mathrm{DMI}}\rvert, and then Néel-like with right-handed chirality for ∣Hx∣>∣HDMI∣\lvert H_x\rvert> \lvert H_{\mathrm{DMI}}\rvert [11]. In the applicable in-plane field range, however, we do not observe any change in the sign of jdepinj_{\mathrm{depin}}, indicating that the chirality is not affected by HxH_x and that ∣HDMI∣>40\lvert H_{\mathrm{DMI}}\rvert> 40 mT. These measurements show that HDMIH_{\mathrm{DMI}} is relatively strong in Pt/[Co/Tb/Co]/Tb.

ρ\rho (μΩ\mu\Omega cm)MsM_{\mathrm{s}} (10510^5 A m−1^{-1})TMT_{\mathrm{M}} (K)RAHER_{\mathrm{AHE}} (mΩ\Omega)RPHER_{\mathrm{PHE}} (mΩ\Omega)μ0Hk\mu_0 H_{\mathrm{k}} (T)χDL\chi_{\mathrm{DL}} (mT 10−710^{-7} A−1^{-1} cm2^2)χFL\chi_{\mathrm{FL}} (mT 10−710^{-7} A−1^{-1} cm2^2)ξDLj\xi_{\mathrm{DL}}^{\mathrm{j}} (10510^5 Ω−1\Omega^{-1} m−1^{-1})ξFLj\xi_{\mathrm{FL}}^{\mathrm{j}} (10510^5 Ω−1\Omega^{-1} m−1^{-1})ξDLE\xi_{\mathrm{DL}}^{\mathrm{E}} (10510^5 Ω−1\Omega^{-1} m−1^{-1})ξFLE\xi_{\mathrm{FL}}^{\mathrm{E}} (10510^5 Ω−1\Omega^{-1} m−1^{-1})
Pt/Tb(1)/[Co/Tb/Co]72.50.24310129187.8+72+23+0.14+0.04+1.92+0.61
Pt/Tb(1.5)/[Co/Tb/Co]80.30.22313154225.2+55+21+0.12+0.04+1.44+0.56
Pt/Tb(2)/[Co/Tb/Co]91.90.50>370120161.1+17+7+0.10+0.04+1.02+0.41
Pt/[Co/Tb/Co]/Tb(1)63.50.74193375893.2+22+20+0.13+0.12+2.09+1.94
Pt/[Co/Tb/Co]/Tb(1.5)67.00.851874251013.5+22+20+0.18+0.17+2.63+2.53
Pt/[Co/Tb/Co]/Tb(2)74.10.53212341622.7+50+35+0.29+0.21+3.93+2.79

Table 2. Summary of the magnetic properties and SOT efficiency of Pt/Tb(tTbt_{\mathrm{Tb}})/[Co/Tb/Co] and Pt/[Co/Tb/Co]/Tb(tTbt_{\mathrm{Tb}}) multilayers with PMA. All values are measured in ambient conditions. Errors are a fraction of the least significant digit, except for TMT_{\mathrm{M}}, whose error is of the order of 1 K.

Conclusions

Our systematic study of synthetic ferrimagnets based on Co/Tb layers shows that the magnetic properties, SOT efficiency, and switching depend strongly on the stacking sequence of Co and Tb in the heterostructures as well as on the thickness of Tb. In Pt/[Co/Tb/Co]/Tb, the dampinglike SOT efficiency reaches up to 0.3, which we attribute to the additive SOT contributions from the bottom Pt and the top Tb layer. Our conclusion is also supported by harmonic Hall measurements performed in the Tb/Co multilayers with in-plane anisotropy. The high value of the SOT efficiency in Pt/[Co/Tb/Co]/Tb is about two and three times larger than that in Pt/Co and Pt/Tb/[Co/Tb/Co], respectively. The PMA in these multilayers is very strong with effective magnetic anisotropy fields estimated between 1 and 8 T. Despite the large PMA, the critical current for magnetization switching is relatively low, of the order of 0.50.5–2.5×1072.5 \times10^7 A/m2^2, depending on the assisting in-plane field. Current-induced DW motion measurements reveal that the DWs are of Néel type with left-handed chirality, stabilized by interfacial DMI similar to Pt/Co bilayers. Our experiments show that synthetic ferrimagnetic heterostructures have comparable or improved PMA, SOT, and DMI relative to ferrimagnetic systems and ferrimagnetic alloys. The stacking order offers an additional degree of freedom to tune and maximize these parameters in spintronic devices.

Acknowledgments

This work was supported by the Swiss National Science Foundation through grants no. 200020_200465 and PZ00P2_179944. The European Metrology Programme for Innovation and Research (EMPIR), under the Grant Agreement 17FUN08 TOPS, is also acknowledged.

References

References

  1. [1]I. M. Miron, K. Garello, G. Gaudin, P.-J. Zermatten, M. V. Costache, S. Auffret, S. Bandiera, B. Rodmacq, A. Schuhl, and P. Gambardella, Perpendicular switching of a single ferromagnetic layer induced by in-plane current injection, Nature 476, 189 (2011).
  2. [2]L. Liu, C.-F. Pai, Y. Li, H. Tseng, D. Ralph, and R. Buhrman, Spin-torque switching with the giant spin hall effect of tantalum, Science 336, 555 (2012).DOI
  3. [3]K. Garello, C. O. Avci, I. M. Miron, M. Baumgartner, A. Ghosh, S. Auffret, O. Boulle, G. Gaudin, and P. Gambardella, Ultrafast magnetization switching by spin-orbit torques, Appl. Phys. Lett. 105, 212402 (2014).
  4. [4]Y.-W. Oh, S.-H. C. Baek, Y. Kim, H. Y. Lee, K.-D. Lee, C.-G. Yang, E.-S. Park, K.-S. Lee, K.-W. Kim, G. Go, et al., Field-free switching of perpendicular magnetization through spin–orbit torque in antiferromagnet/oxide structures, Nat. Nanotech. 11, 878 (2016).DOI
  5. [5]S. Fukami, T. Anekawa, C. Zhang, and H. Ohno, A spin-orbit torque switching scheme with collinear magnetic easy axis and current configuration, Nat. Nanotech. 11, 621 (2016).DOI
  6. [6]C. O. Avci, A. Quindeau, C.-F. Pai, M. Mann, L. Caretta, A. S. Tang, M. C. Onbasli, C. A. Ross, and G. S. Beach, Current-induced switching in a magnetic insulator, Nat. Mater. 16, 309 (2017).
  7. [7]E. Grimaldi, V. Krizakova, G. Sala, F. Yasin, S. Couet, G. S. Kar, K. Garello, and P. Gambardella, Single-shot dynamics of spin–orbit torque and spin transfer torque switching in three-terminal magnetic tunnel junctions, Nat. Nanotech. 15, 111 (2020).DOI
  8. [8]I. M. Miron, T. Moore, H. Szambolics, L. D. Buda-Prejbeanu, S. Auffret, B. Rodmacq, S. Pizzini, J. Vogel, M. Bonfim, A. Schuhl, et al., Fast current-induced domain-wall motion controlled by the rashba effect, Nat. Mater. 10, 419 (2011).DOI
  9. [9]S. Emori, U. Bauer, S.-M. Ahn, E. Martinez, and G. S. Beach, Current-driven dynamics of chiral ferromagnetic domain walls, Nat. Mater. 12, 611 (2013).
  10. [10]K.-S. Ryu, L. Thomas, S.-H. Yang, and S. Parkin, Chiral spin torque at magnetic domain walls, Nat. Nanotech. 8, 527 (2013).DOI
  11. [11]C. O. Avci, E. Rosenberg, L. Caretta, F. Büttner, M. Mann, C. Marcus, D. Bono, C. A. Ross, and G. S. Beach, Interface-driven chiral magnetism and current-driven domain walls in insulating magnetic garnets, Nat. Nanotech. 14, 561 (2019).DOI
  12. [12]Z. Luo, A. Hrabec, T. P. Dao, G. Sala, S. Finizio, J. Feng, S. Mayr, J. Raabe, P. Gambardella, and L. J. Heyderman, Current-driven magnetic domain-wall logic, Nature 579, 214 (2020).
  13. [13]A. Manchon, J. Železný, I. M. Miron, T. Jungwirth, J. Sinova, A. Thiaville, K. Garello, and P. Gambardella, Current-induced spin-orbit torques in ferromagnetic and antiferromagnetic systems, Rev. Mod. Phys. 91, 035004 (2019).
  14. [14]B. Dieny, I. L. Prejbeanu, K. Garello, P. Gambardella, P. Freitas, R. Lehndorff, W. Raberg, U. Ebels, S. O. Demokritov, J. Akerman, et al., Opportunities and challenges for spintronics in the microelectronics industry, Nat. Electron. 3, 446 (2020).
  15. [15]P. Carcia, Perpendicular magnetic anisotropy in pd/co and pt/co thin-film layered structures, J. Appl. Phys. 63, 5066 (1988).
  16. [16]P. Gambardella, S. Rusponi, M. Veronese, S. Dhesi, C. Grazioli, A. Dallmeyer, I. Cabria, R. Zeller, P. Dederichs, K. Kern, et al., Giant magnetic anisotropy of single
  17. [17]S. Ikeda, K. Miura, H. Yamamoto, K. Mizunuma, H. D. Gan, M. Endo, S. Kanai, J. Hayakawa, F. Matsukura, and H. Ohno, A perpendicular-anisotropy CoFeB-MgO magnetic tunnel junction, Nat. Mater. 9, 721 (2010).
  18. [18]B. Dieny and M. Chshiev, Perpendicular magnetic anisotropy at transition metal/oxide interfaces and applications, Rev. Mod. Phys. 89, 025008 (2017).DOI
  19. [19]Z. Zhao, M. Jamali, A. K. Smith, and J.-P. Wang, Spin hall switching of the magnetization in ta/tbfeco structures with bulk perpendicular anisotropy, Appl. Phys. Lett. 106, 132404 (2015).
  20. [20]N. Roschewsky, T. Matsumura, S. Cheema, F. Hellman, T. Kato, S. Iwata, and S. Salahuddin, Spin-orbit torques in ferrimagnetic gdfe co alloys, Appl. Phys. Lett. 109, 112403 (2016).
  21. [21]K. Ueda, M. Mann, C.-F. Pai, A.-J. Tan, and G. S. Beach, Spin-orbit torques in ta/tbxco100-x ferrimagnetic alloy films with bulk perpendicular magnetic anisotropy, Appl. Phys. Lett. 109, 232403 (2016).
  22. [22]K. Ueda, M. Mann, P. W. de Brouwer, D. Bono, and G. S. Beach, Temperature dependence of spin-orbit torques across the magnetic compensation point in a ferrimagnetic tbco alloy film, Phys. Rev. B 96, 064410 (2017).DOI
  23. [23]J. Finley and L. Liu, Spin-orbit-torque efficiency in compensated ferrimagnetic cobalt-terbium alloys, Phys. Rev. Appl. 6, 054001 (2016).arxiv.org/abs/1610.09200
  24. [24]N. Roschewsky, C.-H. Lambert, and S. Salahuddin, Spin-orbit torque switching of ultralarge-thickness ferrimagnetic gdfe co, Phys. Rev. B 96, 064406 (2017).DOI
  25. [25]R. Mishra, J. Yu, X. Qiu, M. Motapothula, T. Venkatesan, and H. Yang, Anomalous current-induced spin torques in ferrimagnets near compensation, Phys. Rev. Lett. 118, 167201 (2017).DOI
  26. [26]W. Seung Ham, S. Kim, D.-H. Kim, K.-J. Kim, T. Okuno, H. Yoshikawa, A. Tsukamoto, T. Moriyama, and T. Ono, Temperature dependence of spin-orbit effective fields in pt/gdfe co bilayers, Appl. Phys. Lett. 110, 242405 (2017).
  27. [27]S. A. Siddiqui, J. Han, J. T. Finley, C. A. Ross, and L. Liu, Current-induced domain wall motion in a compensated ferrimagnet, Phys. Rev. Lett. 121, 057701 (2018).
  28. [28]T. H. Pham, S.-G. Je, P. Vallobra, T. Fache, D. Lacour, G. Malinowski, M.-C. Cyrille, G. Gaudin, O. Boulle, M. Hehn, et al., Thermal contribution to the spin-orbit torque in metallic-ferrimagnetic systems, Phys. Rev. Appl. 9, 064032 (2018).DOI
  29. [29]S.-G. Je, J.-C. Rojas-Sánchez, T. H. Pham, P. Vallobra, G. Malinowski, D. Lacour, T. Fache, M.-C. Cyrille, D.-Y. Kim, S.-B. Choe, et al., Spin-orbit torque-induced switching in ferrimagnetic alloys: Experiments and modeling, Appl. Phys. Lett. 112, 062401 (2018).DOI
  30. [30]Z. Zheng, Y. Zhang, X. Feng, K. Zhang, J. Nan, Z. Zhang, G. Wang, J. Wang, N. Lei, D. Liu, et al., Enhanced spin-orbit torque and multilevel current-induced switching in w/co– tb/pt heterostructure, Phys. Rev. Appl. 12, 044032 (2019).
  31. [31]L. Caretta, M. Mann, F. Büttner, K. Ueda, B. Pfau, C. M. Günther, P. Hessing, A. Churikova, C. Klose, M. Schneider, et al., Fast current-driven domain walls and small skyrmions in a compensated ferrimagnet, Nat. Nanotech. 13, 1154 (2018).DOI
  32. [32]K. Cai, Z. Zhu, J. M. Lee, R. Mishra, L. Ren, S. D. Pollard, P. He, G. Liang, K. L. Teo, and H. Yang, Ultrafast and energy-efficient spin-orbit torque switching in compensated ferrimagnets, Nat. Electron. 3, 37 (2020).
  33. [33]G. Sala, V. Krizakova, E. Grimaldi, C.-H. Lambert, T. Devolder, and P. Gambardella, Real-time hall-effect detection of current-induced magnetization dynamics in ferrimagnets, Nat. Commun. 12, 1 (2021).DOI
  34. [34]K. Ueda, C.-F. Pai, A. J. Tan, M. Mann, and G. S. Beach, Effect of rare earth metal on the spin-orbit torque in magnetic heterostructures, Appl. Phys. Lett. 108, 234205 (2016).
  35. [35]D. Bang, J. Yu, X. Qiu, Y. Wang, H. A. Manchon, and H. Yang, Enhancement of spin hall effect induced torques for current-driven magnetic domain wall motion: Inner interface effect, Phys. Rev. B 93, 174424 (2016).DOI
  36. [36]J. Yu, D. Bang, R. Mishra, R. Ramaswamy, J. H. Oh, H.-J. Park, Y. Jeong, P. Van Thach, D.-K. Lee, G. Go, et al., Long spin coherence length and bulk-like spin-orbit torque in ferrimagnetic multilayers, Nat. Mater. 18, 29 (2019).DOI
  37. [37]Q. Y. Wong, C. Murapaka, W. C. Law, W. L. Gan, G. J. Lim, and W. S. Lew, Enhanced spin-orbit torques in rare-earth pt/[co/ni] 2/co/tb systems, Phys. Rev. Appl. 11, 024057 (2019).
  38. [38]K. Buschow, Intermetallic compounds of rare-earth and 3d transition metals, Rep. Prog. Phys. 40, 1179 (1977).
  39. [39]P. Hansen, C. Clausen, G. Much, M. Rosenkranz, and K. Witter, Magnetic and magneto-optical properties of rare-earth transition-metal alloys containing gd, tb, fe, co, J. Appl. Phys. 66, 756 (1989).DOI
  40. [40]T. Tanaka and H. Kontani, Intrinsic spin and orbital hall effects in heavy-fermion systems, Phys. Rev. B 81, 224401 (2010).
  41. [41]N. Reynolds, P. Jadaun, J. T. Heron, C. L. Jermain, J. Gibbons, R. Collette, R. Buhrman, D. Schlom, and D. Ralph, Spin hall torques generated by rare-earth thin films, Phys. Rev. B 95, 064412 (2017).DOI
  42. [42]Y. C. Wu, K. K. Meng, Q. B. Liu, S. Q. Zheng, J. Miao, X. G. Xu, and Y. Jiang, Spin-orbit torque in antiferromagnetically coupled co and tb multilayers, Phys. Scr. 95, 075802 (2020).
  43. [43]D. Céspedes-Berrocal, H. Damas, S. Petit-Watelot, D. Maccariello, P. Tang, A. Arriola-Córdova, P. Vallobra, Y. Xu, J.-L. Bello, E. Martin, Current-Induced Spin Torques on Single GdFeCo Magnetic Layers, Adv. Mater. 33, 2007047 (2021).
  44. [44]S. Krishnia, E. Haltz, L. Berges, L. Aballe, M. Foerster, L. Bocher, R. Weil, A. Thiaville, J. Sampaio, A. Mougin, Spin-Orbit Coupling in Single-Layer Ferrimagnets: Direct Observation of Spin-Orbit Torques and Chiral Spin Textures, Phys. Rev. Appl. 16, 024040 (2021).DOI
  45. [45]A. Thiaville, S. Rohart, É. Jué, V. Cros, and A. Fert, Dynamics of dzyaloshinskii domain walls in ultrathin magnetic films, Europhys. Lett. 100, 57002 (2012).
  46. [46]E. Martinez, S. Emori, N. Perez, L. Torres, and G. S. Beach, Current-driven dynamics of dzyaloshinskii domain walls in the presence of in-plane fields: Full micromagnetic and one-dimensional analysis, J. Appl. Phys. 115, 213909 (2014).DOI
  47. [47]M. Baumgartner, K. Garello, J. Mendil, C. O. Avci, E. Grimaldi, C. Murer, J. Feng, M. Gabureac, C. Stamm, Y. Acremann, et al., Spatially and time-resolved magnetization dynamics driven by spin-orbit torques, Nat. Nanotech. 12, 980 (2017).
  48. [48]Y. Mimura, N. Imamura, and Y. Kushiro, Hall effect in rare-earth–transition-metal amorphous alloy films, J. Appl. Phys. 47, 3371 (1976).
  49. [49]C. O. Avci, G. S. Beach, and P. Gambardella, Effects of transition metal spacers on spin-orbit torques, spin hall magnetoresistance, and magnetic anisotropy of pt/co bilayers, Phys. Rev. B 100, 235454 (2019).
  50. [50]D. Webb, A. Marshall, Z. Sun, T. Geballe, and R. M. White, Coercivity of a Macroscopic ferrimagnet near a compensation point, IEEE Trans. Magn. 24, 588 (1988).DOI
  51. [51]C. O. Avci, K. Garello, C. Nistor, S. Godey, B. Ballesteros, A. Mugarza, A. Barla, M. Valdivares, E. Pellegrin, A. Ghosh, et al., Fieldlike and antidamping spin-orbit torques in as-grown and annealed ta/cofeb/mgo layers, Phys. Rev. B 89, 214419 (2014).DOI
  52. [52]K. Garello, J. M. Miron, C. O. Avci, F. Freimuth, Y. Mokrousov, S. Blügel, S. Auffret, O. Boulle, G. Gaudin, and P. Gambardella, Symmetry and magnitude of spin-orbit torques in ferromagnetic heterostructures, Nat. Nanotech. 8, 587 (2013).
  53. [53]A. Ghosh, K. Garello, C. O. Avci, M. Gabureac, and P. Gambardella, Interface-enhanced spin-orbit torques and current-induced magnetization switching of pd/co/alo x layers, Phys. Rev. Appl. 7, 014004 (2017).
  54. [54]J. Kim, J. Sinha, M. Hayashi, M. Yamanouchi, S. Fukami, T. Suzuki, S. Mitani, and H. Ohno, Layer thickness dependence of the current-induced effective field vector in ta| cofeb| mgo, Nat. Mater. 12, 240 (2013).
  55. [55]M. Hayashi, J. Kim, M. Yamanouchi, and H. Ohno, Quantitative characterization of the spin-orbit torque using harmonic hall voltage measurements, Phys. Rev. B 89, 144425 (2014).
  56. [56]C.-F. Pai, Y. Ou, L. H. Vilela-Leão, D. Ralph, and R. Buhrman, Dependence of the efficiency of spin hall torque on the transparency of pt/ferromagnetic layer interfaces, Phys. Rev. B 92, 064426 (2015).
  57. [57]X. Qiu, W. Legrand, P. He, Y. Wu, J. Yu, R. Ramaswamy, A. Manchon, and H. Yang, Enhanced spin-orbit torque via modulation of spin current absorption, Phys. Rev. Lett. 117, 217206 (2016).
  58. [58]C. O. Avci K. Garello, M. Gabureac, A. Ghosh, A. Fuhrer, A. F. Santos and P. Gambardella, Interplay of spin-orbit torque and thermoelectric effects in ferromagnet/normal-metal bilayers, Phys. Rev. B 90, 224427 (2014).
  59. [59]K.-S. Lee, S.-W. Lee, B.-C. Min, and K.-J. Lee, Threshold current for switching of a perpendicular magnetic layer induced by spin hall effect, Appl. Phys. Lett. 102, 112410 (2013).
  60. [60]K.-J. Kim, S. K. Kim, Y. Hirata, S.-H. Oh, T. Tono, D.-H. Kim, T. Okuno, W. S. Ham, S. Kim, G. Go, et al., Fast domain wall motion in the vicinity of the angular momentum compensation temperature of ferrimagnets, Nat. Mater. 16, 1187 (2017).
  61. [61]E. Haltz, S. Krishnia, L. Berges, A. Mougin, and J. Sampaiո, Domain wall dynamics in antiferromagnetically coupled double-lattice systems, Phys. Rev. B 103, 014444 (2021).
  62. [62]S. Ghosh, T. Komori, A. Hallal, J. Peña Garcia, T. Gushi, T. Hirose, H. Mitarai, H. Okuno, J. Vogel, M. Chshiev, et al., Current-driven domain wall dynamics in ferrimagnetic nickel-doped mn4n films: Very large domain wall velocities and reversal of motion direction across the magnetic compensation point, Nano Lett. 21, 2580 (2021).
  63. [63]P. Haazen, E. Murè, J. Franken, R. Lavrijsen, H. Swagten, and B. Koopmans, Domain wall depinning governed by the spin hall effect, Nat. Mater. 12, 299 (2013).
  64. [64]S. Emori, E. Martinez, K.-J. Lee, H.-W. Lee, U. Bauer, S.-M. Ahn, P. Agrawal, D. C. Bono, and G. S. Beach, Spin hall torque magnetometry of dzyaloshinskii domain walls, Phys. Rev. B 90, 184427 (2014).
  65. [65]T. Schulz, K. Lee, B. Krüger, R. L. Conte, G. V. Karnad, K. Garcia, L. Vila, B. Ocker, D. Ravelosona, and M. Kläui, Effective field analysis using the full angular spin-orbit torque magnetometry dependence, Phys. Rev. B 95, 224409 (2017).
  66. [66]M. Kuepferling, A. Casiraghi, G. Soares, G. Durin, F. Garcia-Sanchez, L. Chen, C. H. Back, C. H. Marrows, S. Tacchi, and G. Carlotti, Measuring interfacial dzyaloshinskii-moriya interaction in ultra thin films, arXiv preprint arXiv:2009.11830 (2020).arxiv.org/abs/2009.11830
  67. [67]R. Bläsing, T. Ma, S.-H. Yang, C. Garg, F. K. Dejene, A. T. N’Diaye, G. Chen, K. Liu, and S. S. P. Parkin, Exchange coupling torque in ferrimagnetic co/gd bilayer maximized near angular momentum compensation temperature, Nat. Commun. 9, 4984 (2018).
  68. [68]S.-H. Yang, K.-S. Ryu, and S. Parkin, Domain-wall velocities of up to 750 m/s driven by exchange-coupling torque in synthetic antiferromagnets, Nat. Nanotech. 10, 221 (2015).

Paper details

vlnc:W_y4zffwtx
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents