betaFeedback

WorksPhysics and Astronomy

Spin wave dispersion of ultra-low damping hematite (α-Fe2O3α\text{-Fe}_2\text{O}_3) at GHz frequencies

Abstract

Low magnetic damping and high group velocity of spin waves (SWs) or magnons are two crucial parameters for functional magnonic devices. Magnonics research on signal processing and wave-based computation at GHz frequencies focussed on the artificial ferrimagnetic garnet Y3_3Fe5_5O12_{12} (YIG) so far. We report on spin-wave spectroscopy studies performed on the natural mineral hematite (α-Fe2O3α\text{-Fe}_2\text{O}_3) which is a canted antiferromagnet. By means of broadband GHz spectroscopy and inelastic light scattering, we determine a damping coefficient of 1.1×10−51.1\times10^{-5} and magnon group velocities of a few 10 km/s, respectively, at room temperature. Covering a large regime of wave vectors up to k≈24 rad/μk\approx 24~{\rm rad}/μm, we find the exchange stiffness length to be relatively short and only about 1 Å. In a small magnetic field of 30 mT, the decay length of SWs is estimated to be 1.1 cm similar to the best YIG. Still, inelastic light scattering provides surprisingly broad and partly asymmetric resonance peaks. Their characteristic shape is induced by the large group velocities, low damping and distribution of incident angles inside the laser beam. Our results promote hematite as an alternative and sustainable basis for magnonic devices with fast speeds and low losses based on a stable natural mineral.

Introduction.— Spin waves (magnons) are collective spin excitations in magnetically ordered materials. They exhibit promising functionalities for information transmission and processing at GHz frequencies [1, 2, 3]. To realize energy efficient magnonic circuits [1, 2, 4, 5, 6] isotropic spin wave (SW) dispersion relations, high group velocities, and low magnetic damping are essential. Until today, the artificial garnet Y3_3Fe5_5O12_{12} (YIG) [7] played a key role for the exploration of magnonics functionalities [8]. Already in 1961, M. Sparks et al. coined the term that YIG was to ferromagnetic resonance research what the fruit fly was to genetics research [9]. This was particularly true for high-quality YIG grown by liquid phase epitaxy on the wafer scale [8, 10]. However, in a ferrimagnetic material like YIG, magnon bands in the regime of small wave vectors, kk, and low GHz frequencies are inherently anisotropic due to the dipolar interaction between spins. To overcome this, a lot of effort has been put into the development of microwave-to-magnon transducers which allow for the excitation of exchange dominated SWs with isotropic properties at high frequencies [11, 12, 13]. The transducers suffer however from typically a narrow bandwidth or require an applied magnetic field in contrast to conventional transmission lines and coplanar waveguides (CPWs).

In antiferromagnetic (AFM) materials, exchange interaction dominates the dispersion relation already at small wave vectors kk. The dipolar interactions are virtually absent due to net zero magnetization. Still, SWs can propagate with high group velocities. Values similar to thick YIG [8, 14] and as high as 30 km/s have been reported [15, 16, 17, 18]. However, the challenge with most AFMs is their net zero magnetization and sub-THz frequencies which make on-chip integration hard due to lack of efficient CPWs and THz sources (THz gap) [19, 20]. Recently, the natural mineral and canted antiferromagnet hematite (α\alpha-Fe2_2O3_3) [21] gained particular attention for magnonics [22, 23] after the observation of long distance spin transport [24, 25] and enhanced spin pumping [26]. It is known that, due to extremely low anisotropy in the basal plane [21, 27] [28], in the canted phase Figure 1a (and (b)) one branch of the magnon modes resides at around 10 GHz at small kk. Depending on the purity of hematite crystals, a damping coefficient as low as 7.8×10−67.8 \times10^{-6} was reported for the magnetic resonance [29]. The hematite’s finite net magnetization and strikingly small damping of below 10−510^{-5} make it hence suitable for magnonic applications. They allow for inductive coupling to CPWs and long-distance SW transport, respectively. However, there is no experiment reporting a measured SW dispersion for kk values accessible by CPWs with integrated microwave-to-magnon transducers [11, 12, 13]. The dispersion measured over a large wave vector regime is of fundamental importance as it allows one to quantify the exchange stiffness length lel_e with large precision. lel_e is the key parameter to estimate the maximum possible spin-wave velocity of hematite in the GHz frequency regime.

Image not extracted

Figure 1. Hexagonal unit cell of the crystal structure of hematite from (a) the side and (b) top view. The cyan spheres and red arrows indicate the Fe atoms and the spins associated with them, respectively (oxygen atoms are not shown). We depict the canted antiferromagnetic state above the Morin temperature for which the sublattice spins lie in the cc-plane along the aa-axis with a small canting. They give rise to sublattice magnetization vectors M1\mathbf{M}_1 and M2\mathbf{M}_2. (c) Sketch of the low frequency quasi-ferromagnetic mode where a small magnetization (green arrow), m\mathbf{m}, precesses elliptically around the applied field (black arrow), H\mathbf{H}. (d) Schematics of the flip-chip VNA measurement. The sample (gray disk) is placed on a CPW. The static magnetic field, H\mathbf{H}, is applied in the aa-plane and with an angle, θH\theta_H, to the normal of the cc-axis of the crystal. The rf magnetic field (orange double-headed arrow), hrf\mathbf{h}_{\rm rf}, of the CPW is parallel to the cc-axis. (e) Sketch of the BLS configuration. The magnetic field, H\mathbf{H}, is applied perpendicular to cc-axis in the aa-plane. The laser light (green) forms a Gaussian beam and is focused on the surface of the sample (gray). The cone angle of the objective lens is θ\theta. The incident laser light with an incidence angle, φ\varphi is scattered by magnons. We measure in back-scattering geometry (dashed green arrow).

Here, we study the magnon band structure of bulk hematite at different wave vectors kk by means of broadband microwave spectroscopy and kk-resolved inelastic Brillouin light scattering (BLS) (Figure 1). Using a CPW in flip-chip configuration we extract a magnetic damping parameter of 1.12×10−51.12 \times10^{-5} which is similar to the best YIG reported in Ref. 30. Still, the measured spectra with BLS show broad linewidths. Our modelling substantiates that the linewidth is explained by the SW dispersion relation, the large SW velocity and the Gaussian profile of the laser used for inelastic light scattering. The data substantiate a high group velocity of 10 km/s for k=2.5k = 2.5 rad/μ\mum which are excited easily by a micron-sized CPW [23, 31]. In an applied field of 90 mT, the velocity increases to 16 km/s near k=5k = 5 rad/μ\mum and levels off to 23.3 km/s for k≥25k \ge25 rad/μ\mum.

The latter value has routinely been realized by transducers. Our findings substantiate hematite as a very promising candidate for a sustainable future of magnonics as its growth avoids the lead-based synthesis route used for high-quality YIG [7, 30].

Properties of hematite.— We first briefly review the relevant magnetic properties of α\alpha-Fe2_2O3_3. Hematite is the stable end product of oxidation of magnetite [32] and known for its great abundance as well as stability in an aqueous environment [33]. It is an insulating antiferromagnet (AFM) with a corundum crystal structure. The arrangement of the magnetic atoms of Fe in the crystal is shown in Figure 1(a) [34]. At room temperature and above the Morin transition temperature of TM=262T_{\rm M} = 262 K the Fe+3^{+3} magnetic moments lie in the cc-plane due to an easy plane anisotropy, HAH_{\rm A}, and stack antiferromagnetically along the cc-axis [Fig. 1(a)] [21] [28]. Within the cc-plane, there is a weak 6-fold anisotropy around the cc-axis, HaH_{\rm a}, which favors the magnetic moments to align with the aa-axes [Fig. 1(b)]. The magnetic moments of the two AFM sublattices are slightly canted away from the aa-axis by the Dzyaloshinskii-Moriya (DM) interaction (Fig. 1(b), resulting in a weak magnetic moment, m\mathbf{m}, perpendicular to both aa- and cc- axes at equilibrium [21] [28]. The magnetization amounts to about 2 kA/m [32]. The magnetization dynamics of hematite in this weak ferromagnetic state offers two modes namely the quasi-ferromagnetic mode (qFM or low frequency mode) and quasi-antiferromagnetic mode (qAFM or high frequency mode) [21, 27] [28].

Here, we explore the qFM mode schematically depicted in Figure 1(c). The canted AFM sublattice magnetization vectors precess elliptically around their equilibrium direction. This results in an elliptic precession of the weak magnetic moment, m\mathbf{m} (green arrow in Figure 1(c)), around the applied field, H\mathbf{H} [21, 27] [28]. The frequency of the qFM mode was derived by Pincus [21, 27] according to

fr=∣γ∣μ02πHsin⁡ξ(Hsin⁡ξ+HD)+2HE(Ha+HME)(1)f_r = \frac{|\gamma|\mu_0}{2\pi}\sqrt{H\sin\xi\left(H\sin\xi+H_D\right)+2H_E\left(H_a+H_{\rm ME}\right)} \tag*{(1)}

where, γ\gamma, μ0\mu_0, HEH_E, HDH_D and HMEH_{\rm ME} is the electron gyromagnetic ratio, vacuum permeability, exchange, DM and spontaneous magnetoelastic effective field, respectively. ξ=π/2−θH\xi= \pi/2-\theta_H is the polar angle between H\mathbf{H} and the cc-axis (zz-direction). We define θH\theta_H in Figure 1(d). Fink [35] derived the dynamic susceptibility χxz(f,fr)\chi_{xz}(f,f_r) for the qFM mode. The real and imaginary parts read

Re⁡[χxz(f,fr)]=(fr2−f2)fr2(fr2−f2)2+Δf2fr2(2)\operatorname{Re}\left[\chi_{xz}(f,f_r)\right] = \frac{\left(f_r^2-f^2\right)f_r^2}{\left(f_r^2-f^2\right)^2+\Delta f^2f_r^2} \tag*{(2)}
Im⁡[χxz(f,fr)]=ffr2Δf(fr2−f2)2+Δf2fr2(3)\operatorname{Im}\left[\chi_{xz}(f,f_r)\right] = \frac{f f_r^2\Delta f}{\left(f_r^2-f^2\right)^2+\Delta f^2f_r^2} \tag*{(3)}

respectively. Here, ff is the frequency of the radiofrequency (rf) magnetic field hrf\mathbf{h}_{\mathrm{rf}} (Figure 1 (d)). The frequency linewidth, Δf\Delta f, is related to the magnetic damping parameter, α\alpha, by

Δf≈2αHE(γ/2π),(4)\Delta f \approx2\alpha H_{\mathrm{E}}(\gamma/2\pi), \tag*{(4)}

for H≪HEH \ll H_{\mathrm{E}}. Unlike ferromagnets and uniaxial antiferromagnets, the resonance line width of a canted antiferromagnet does not depend on frf_{\mathrm{r}} and is governed by the field-independent exchange frequency. Following Turov [15, 16], the SW dispersion of the qFM mode for hematite near k=0k=0 is given by

fm(k)=∣γ∣μ02πH(H+HD)+2HE(Ha+HME+Ak2),(5)f_{\mathrm{m}}(k) = \frac{|\gamma|\mu_{0}}{2\pi} \sqrt{H(H+H_{\mathrm{D}})+2H_{\mathrm{E}}(H_{\mathrm{a}}+H_{\mathrm{ME}}+Ak^{2})}, \tag*{(5)}

where A=HEle2A=H_{\mathrm{E}}l_{\mathrm{e}}^{2} is the dispersion coefficient and lel_{\mathrm{e}} is the effective magnetic lattice parameter or exchange stiffness length. For Eq. (5), we considered the experimental geometry for kk-resolved BLS measurements with an angle ξ=π/2\xi=\pi/2 as described below.

Experimental techniques.— The broadband microwave spectroscopy was conducted at room temperature above TMT_{\mathrm{M}} (Figure 1(d)). The disk-shaped aa-plane α\alpha-Fe2_2O3_3 crystal had a diameter of 2.3 mm and thickness of 0.5 mm. Measurements were done in flip-chip configuration for which the sample was placed on a CPW with signal (ground) line width of 165 μ\mum (295 μ\mum). The aa-axis of the crystal was perpendicular to the disk plane. The cc-axis was in the plane and perpendicular to the CPW axis. Injecting a radio-frequency (rf) current, IrfinI_{\mathrm{rf}}^{\mathrm{in}}, into the CPW by port 1 of a vector network analyzer (VNA) induced the dynamic magnetic field hrf\mathbf{h}_{\mathrm{rf}} (orange double-head arrow). The rf current was collected on the other end of the CPW by port 2 of the VNA (IrfoutI_{\mathrm{rf}}^{\mathrm{out}}). The static magnetic field, H\mathbf{H}, was applied in the aa-plane of the crystal (yzyz-plane in Figure 1(d)). For the angle dependent measurements an external field of 90 mT was applied and the angle, θH\theta_{\mathrm{H}}, was varied in steps of ΔθH=2∘\Delta\theta_{\mathrm{H}}=2^\circ. In case of field sweep measurements, the applied field angle was perpendicular to the cc-axis and in the aa-plane of the crystal (θH=0\theta_{\mathrm{H}}=0 deg). The field amplitude was varied in steps of ΔH=0.5\Delta H=0.5 mT.

Wave vector-resolved BLS measurements were done for θH=0\theta_{\mathrm{H}}=0 deg on a piece of the same crystal in back-scattering geometry (Figure 1(e)) using a green laser with wavelength, λ=532\lambda=532 nm and wave vector k0=2π/λ=11.81k_{0}=2\pi/\lambda=11.81 rad/μ\mum. The external field was applied in the aa-plane and perpendicular to cc-axis. The sample for BLS was irregularly shaped. We ensured that it was tilted with respect to the incident laser beam along the yy-axis in such a way that the laser beam remained in the xzxz-plane formed by the aa- and cc-axis. Since the penetration depth of the green laser in hematite is on the order of 75 nm [36], linear momentum conservation holds only for the in-plane component of the transferred wave vectors. Therefore, we define the transferred momentum from the light to magnons along the cc-axis as kz=2(k0sin⁡φ+kx′cos⁡φ)k_{z}=2(k_{0}\sin\varphi+k'_{x}\cos\varphi), where φ\varphi is the angle between the incident beam and the normal to the plane of the sample (aa-plane) [37]. We

assume a Gaussian beam profile giving rise to a Fourier transform of the beam intensity II as

I(kx′)=ekx′2w02/2(6)I(k'_{x})=e^{k_{x}^{\prime2}w_{0}^{2}/2} \tag*{(6)}

with w0=2k0NAw_{0}=\frac{2}{k_{0}\mathrm{NA}}. NA is the numerical aperture of the lens [38, 39]. The momentum kx′k'_{x} has a projection on zz-direction due to the focusing of the beam.

Broadband microwave spectroscopy data.— Field-dependent VNA spectra are shown in Figure 2(a). We depict the imaginary part of the quantity U(f,H)=iln⁡[S21(f,H)/S21(f,H=0)]U(f,H)=i\ln[S_{21}(f,H)/S_{21}(f,H=0)] in a color-coded plot, where S21S_{21} is the complex scattering parameter measured by the VNA at a given field, HH. We identify two branches which we label f1f_1 and f2f_2 for positive fields. For a detailed analysis, we consider that the parameter UU contains the susceptibility χ\chi of the sample [40, 41] and the electromagnetic response of the rf circuit used in the flip-chip method. To account for the different contributions, we follow Refs. [40, 41] and fit the measured UU with

Image not extracted

Figure 2. (a) Color-coded field dependent Im⁡(U)\operatorname{Im}(U) parameter measured on the sample as indicated in Figure 1(d) with θH=0\theta_{\mathrm{H}}=0 deg. Solid red circles and wine triangles are the frequencies extracted by fitting Eq. (7) on the data. Blue solid line is obtained by fitting Eq. (1) with extracted f1f_{1} values. (b) Imaginary and (c) real part of UexpU_{\mathrm{exp}} (red symbols) and UfitU_{\mathrm{fit}} (black curves) for 70 mT, respectively. (d) Imaginary and (e) real parts of χ1\chi_{1} (red curve), χ2\chi_{2} (blue curve) and their sum (gray curve) for 70 mT, respectively.

Ufit=C[1+χ0+χ(f,f1,Δf1)eiϕ1+χ(f,f2,Δf2)eiϕ2](7)U_{\mathrm{fit}} = C[1+\chi_0+\chi(f,f_1,\Delta f_1)e^{i\phi_1}+\chi(f,f_2,\Delta f_2)e^{i\phi_2}] \tag*{(7)}

as shown in Figure 2(b) and (c) (black lines). CC is a real-numbered scaling parameter, χ0\chi_0 is a complex-numbered offset parameter, and ϕi\phi_i are phase shift adjustments (i=1,2i=1,2). Using Eq. (7), we extract the resonance frequencies and linewidths Δfi\Delta f_i for the two modes labelled by f1f_1 and f2f_2. In Figure 2 (b) and (c), we display the measured imaginary and real parts of UU with red symbols. In Figure 2 (d) and (e), we show the extracted real and imaginary parts together with the total susceptibilities (gray lines) from which the two resonant modes are identified. Their frequencies extracted for different HH are depicted in Figure 2 (a) with solid red circles and magenta triangles. We focus on fields larger than 50 mT to ensure a saturated state.

The blue line in Figure 2(a) results from fitting Eq. (1) to branch f1f_1 with ξ=π/2\xi=\pi/2. From the fit, we obtain μ0HE=1003.61\mu_0H_E=1003.61 T, μ0HD=2.34\mu_0H_D=2.34 T and μ0(Ha+HME)=88.64\mu_0(H_a+H_{\mathrm{ME}})=88.64 μ\muT. Using Eq. (4) and the experimental value of Δf1=0.63\Delta f_1=0.63 GHz for branch f1f_1, we extract a damping parameter of α=1.12×10−5\alpha=1.12\times10^{-5}. This value is similar to the best value reported for YIG in Ref. [30]. The branch f2f_2 will be discussed later.

Angle-dependent VNA spectra are shown in Figure 3. To enhance the signal to noise ratio, we depict

Image not extracted

Figure 3. Color-coded neighbor subtracted angle dependent VNA-FMR spectra measured on the sample as indicated in Figure 1(d) with μ0H=90\mu_0H=90 mT. Orange curve depicts Eq. (1) by extracted material parameters.

Δ∣S12∣=∣S12(H+ΔH)−S12(H)∣\Delta|S_{12}|=|S_{12}(H+\Delta H)-S_{12}(H)|. For such data, a zero-crossing (highlighted by the red curve) represents the resonance frequency. The spectra show a 2-fold symmetry as expected for the cc-axis being in the plane of the applied magnetic fields. Introducing the extracted parameters discussed above, Eq. (1) models well the resonance frequency of branch f1f_1 as a function of angle θH\theta_H (red line). The angular dependency is hence consistent with the effective anisotropy field extracted from the field-dependent data.

BLS data.— The BLS spectra for different values of incident angle, φ\varphi, are shown in Figure 4 (a). Black symbols in Figure 4 (b) depict the frequency position of the maximum BLS peak as a function of wave vector calculated from the incidence angles shown in the legend of Figure 4 (a). The red curve in Figure 4 (b) is obtained by considering first the material parameters obtained from VNA measurements and then fitting Eq. (5) to the black symbols in the same graph. We obtain a dispersion coefficient of μ0A=9.153×10−6\mu_0A=9.153\times10^{-6} T⋅μm2\cdot\mu\mathrm{m}^2 which leads to an exchange stiffness length of le=0.955l_e=0.955 Å. Using Eq. (5) and the obtained parameters we calculate the SW group velocity, vgv_g, for μ0H=90\mu_0H=90 mT [blue line in Fig. 4 (c)]. The velocity vgv_g increases significantly with kk and levels off at 23.3 km/s. Such a high group velocity is the direct result of the strong exchange interaction and at the same time vanishingly small net magnetization. Microstructured CPWs used in magnonics offer spin-wave wave vectors around k=2.5k=2.5 rad/μ\mum [23, 31]. For such a value kk, the qFM spin wave in hematite exhibits a group velocity of vg=10v_g=10 km/s similar to SWs in thick YIG and about a factor of 10 larger compared to ultra-thin YIG [42]. The decay length of the SWs is given by ld=vgτl_d=v_g\tau, where τ=(1/2παfm(k))\tau=(1/2\pi\alpha f_m(k)) is the relaxation time of the SW. For 30 mT applied field and k=2.5k=2.5 rad/μ\mum we calculate vg=13.4v_g=13.4 km/s and τ=840.6\tau=840.6 ns which leads to ld=11.3l_d=11.3 mm, again similar to thick YIG. This is due to low damping and high group velocity of the qFM spin waves in hematite.

Image not extracted

Figure 4. (a) BLS spectra for different incident angles, φ\varphi, measured as indicated in Figure 1(e) with μ0H=90\mu_0 H = 90 mT. (b) Extracted peak maxima frequency (black squares) as a function of corresponding transferred wave vector, kk and fitted dispersion relation (red curve) by Eq. (5). (c) Group velocity (d) partial density of states and obtained from fitted magnon dispersion at μ0H=90\mu_0 H = 90 mT. Inset in (d) depicts pDOS for φ=0\varphi= 0 degree.

Despite the small damping of the hematite sample measured by the VNA, the resonance peaks of the qFM mode in the BLS spectra show a large width of 10 to 20 GHz. Furthermore, the BLS peak taken at nearly normal incidence of the laser beam (e.g. at φ=0\varphi=0 or 5 deg) shows a strong asymmetric shape. As φ\varphi increases, the intensity of the prominent peak reduces and it becomes more and more symmetric. To understand these observations, we calculated the partial density of states (pDOS) by considering the magnon dispersion relation and the Gaussian beam profile according to

pDOS(f,φ)=−1π∫−∞+∞dkx′cos⁡φ Im⁡[I(kx′)f−fm(k)+iΔf].(8)pDOS(f,\varphi) = -\frac{1}{\pi}\int_{-\infty}^{+\infty}dk'_x\cos\varphi\,\operatorname{Im}\left[\frac{I(k'_x)}{f-f_m(k)+i\Delta f}\right]. \tag*{(8)}

Assuming only fully back reflected light we have k=2(k0sin⁡φ+kx′cos⁡φ)k=2(k_0\sin\varphi+k'_x\cos\varphi). Δf\Delta f is the resonance broadening due to the damping given by Eq. (4). The numerical aperture of the objective lens was NA=0.18NA = 0.18. The calculated pDOS for different incident angles is plotted in Figure 4(d). Comparing Figure 4(a) and (Figure 4c), the experimental BLS peaks are broad because they contain a certain frequency regime of the band structure which is determined by the Gaussian wave vector distribution of k=2k0sin⁡φ+Δkk = 2k_0 \sin\varphi+ \Delta k. The central wave vector is kc=2k0sin⁡φk_c = 2k_0 \sin\varphi and the distribution function for Δk=2kx′cos⁡φ\Delta k = 2k'_x \cos\varphi is given by I(kx′)I(k'_x) (Eq. (6)). We attribute the broad BLS peaks hence to the high group velocity of magnons which leads to a peak width proportional to vg×Δkv_g \times\Delta k. The asymmetry of BLS peaks for small φ\varphi can be understood in terms of the Van Hove singularity of the pDOS near k=0k = 0. As φ\varphi increases, the part of the band structure which is relevant for the collected light shifts away from k=0k = 0. Consequently, the peak gets more symmetric with φ\varphi. The peak intensity reduces with φ\varphi due to the factor cos⁡φ\cos\varphi in Eq. (8). We note that Eq. (8) does not include all possible scattering processes.

Still it provides a good qualitative understanding about the contributions giving rise to the characteristics shape and signal strength of BLS peaks as a function of φ\varphi.

Discussion

The branch of mode f2f_2 in Figure 2(a) is higher by about δf=1\delta f = 1 GHz than f1f_1 at the same field HH. A second branch was reported also in Ref. 43. Here the authors studied the qAFM mode at zero field and assumed a distribution of magnetic domains. We applied a large enough magnetic field to avoid domains. A domain formation can not explain our second branch. Another possibility for f2f_2 is a standing wave along the thickness of the sample or a SW excited with a discrete wave vector coming from the CPW. However, for these cases a quantitative estimate based on the magnon dispersion obtained with BLS (Eq. (5)) led to a frequency separation of much smaller than 1 GHz.

The remaining explanation for f2f_2 is a nonuniform magnetoelastic field in the sample induced when fixing the sample on the CPW. We attribute the observed frequency splitting to different strains in different parts of the sample that is either in contact with the CPW conductors or floating on the CPW gaps. A difference of δHME=24 μT\delta H_{\mathrm{ME}} = 24\ \mu\mathrm{T} would account for δf=f2−f1=1\delta f = f_2 - f_1 = 1 GHz. The effect of magnetoelastic interaction by unidirectional compression, p\mathbf{p}, in the basal plane of the crystal, on the qFM mode is given by replacing HMEH_{\mathrm{ME}} with HME′=HME−Rpcos⁡2ψH'_{\mathrm{ME}} = H_{\mathrm{ME}} - R p \cos2\psi [44, 45]. Here, R=287 μT/barR = 287\ \mu\mathrm{T}/\mathrm{bar} [45] is a coefficient determined by the elastic and magnetoelastic parameters of the crystal and ψ=π/2\psi= \pi/2 is the angle between p\mathbf{p} and H\mathbf{H}. Using δHME=Rp\delta H_{\mathrm{ME}} = Rp we obtain p=0.084p = 0.084 bar. This value corresponds to a force of 14.6 mN on the parts of the crystal that are in contact with the CPW conductors. The evaluated force is one order of magnitude smaller than the weight of our sample and indicates the known sensitivity of hematite towards magnetoelastic effects.

From our experiments, we do not determine HaH_a and HMEH_{\mathrm{ME}} separately as they enter Eq. (1) in the same way. To separate the small HaH_a from HMEH_{\mathrm{ME}} an angle dependent VNA measurement with the magnetic field applied in the cc-plane of the crystal would be required. The existing sample was not suitable for that.

Our BLS data were acquired on a seven times larger wave vector regime compared to the data used in Ref. 23 where, the authors extracted an exchange stiffness length lel_e of 1.2 Å. From our extended dataset, we evaluate the value le=0.96l_e = 0.96 Å. The precise determination of lel_e is of key importance as it determines the SW group velocity. Contrary to the ferrimagnetic YIG, dipolar effects are not expected to play an important role in SW dispersion of hematite. Hence, hematite thin films can provide similarly large spin-wave velocities as reported here for the bulk crystal. As a consequence, they potentially outperform YIG thin films concerning speed and decay lengths at wave vectors which are realized by the state-of-the-art transducers. Furthermore, hematite is based on earth abundant elements and as an end product of oxidation of magnetite a stable natural mineral suggesting sustainable synthesis routes.

Conclusion.— We have measured the magnon dispersion relation of hematite for wave vectors kk which are relevant for timely experiments in magnonics. The damping coefficient of the studied natural crystal was 1.1×10−51.1 \times10^{-5} at room temperature. This value is only 40 % larger than the best value reported for pure hematite and is already as good as the best YIG. The estimated spin-wave decay length for k=2.5k = 2.5 rad/μ\mum is larger than 1 cm in a small magnetic field. In optimized thin films, current microwave-to-magnon transducers are expected to achieve larger group velocities in hematite than in YIG. The reported properties suggest that hematite can become the fruit fly of sustainable modern magnonics.

Note added.— While completing the manuscript about our experiments on hematite [22], we became aware of Ref. 23. The authors measured group velocities and the spin-wave dispersion via integrated CPWs for 1 rad/μ\mum ≤k≤\leq k \leq 3.5 rad/μ\mum. Our BLS measurements cover a seven times larger regime of kk values enabling an improved evaluation of the parameter lel_e. This parameter is decisive to estimate the saturation velocity of GHz SWs in hematite.

The scientific colour maps developed by Crameri et al. [46] is used in this study to prevent visual distortion of the data and exclusion of readers with colour-vision deficiencies [47].

Acknowledgement.— The authors thank SNSF for financial support via grant 177550. We acknowledge discussions with A. Mucchietto, M. Mruczkiewicz, S. Nikitov and A. Sadovnikov. The different pieces of the hematite crystal were provided by J.-P. Ansermet and M. Bialek. We thank them for the support and discussions.

References

References

  1. [1]V. V. Kruglyak, S. O. Demokritov, and D. Grundler, J. Phys. D. Appl. Phys. 43, 264001 (2010).
  2. [2]A. Barman, G. Gubbiotti, S. Ladak, A. O. Adeyeye, M. Krawczyk, J. Grafe, C. Adelmann, S. Cotofana, A. Naeemi, V. I. Vasyuchka, B. Hillebrands, S. A. Nikitov, H. Yu, D. Grundler, A. V. Sadovnikov, A. A. Grachev, S. E. Sheshukova, J. Y. Duquesne, M. Marangolo, G. Csaba, W. Porod, V. E. Demidov, S. Urazhdin, S. O. Demokritov, E. Albisetti, D. Petti, R. Bertacco, H. Schultheiss, V. V. Kruglyak, V. D. Poimanov, S. Sahoo, J. Sinha, H. Yang, M. Münzenberg,
  3. [3]K. Baumgaertl and D. Grundler 10.48550/arxiv.2208.10923 (2022).
  4. [4]V. S. Tkachenko, A. N. Kuchko, M. Dvornik, and V. V. Kruglyak, Appl. Phys. Lett. 101, 152402 (2012).
  5. [5]K. Vogt, H. Schultheiss, S. Jain, J. E. Pearson, A. Hoffmann, S. D. Bader, and B. Hillebrands, Appl. Phys. Lett. 101, 024410 (2012).
  6. [6]S. Mieszczak, O. Busel, P. Gruszecki, A. N. Kuchko, J. W. Kłos, and M. Krawczyk, Phys. Rev. Appl. 13, 054038 (2020), arXiv:2001.11356.DOI
  7. [7]D. C. Doughty and E. A. D. White, Acta Crystallogr. 13, 761 (1960).
  8. [8]A. A. Serga, A. V. Chumak, and B. Hillebrands, J. Phys. D. Appl. Phys. 43, 264002 (2010).
  9. [9]M. Sparks, R. Loudon, and C. Kittel, Phys. Rev. 122, 791 (1961).
  10. [10]S. Maendl, I. Stasinopoulos, and D. Grundler, Appl. Phys. Lett. 111, 012403 (2017).
  11. [11]H. Yu, O. D’Allivy Kelly, V. Cros, R. Bernard, P. Bortolotti, A. Anane, F. Brandl, F. Heimbach, and D. Grundler, Nat. Commun. 7, 11255 (2016).
  12. [12]K. Baumgaertl, J. Gräfe, P. Che, A. Mucchietto, J. Förster, N. Träger, M. Bechtel, M. Weigand, G. Schütz, and D. Grundler, Nano Lett. 20, 7281 (2020).
  13. [13]P. Che, K. Baumgaertl, A. Kùkol’ová, C. Dubs, and D. Grundler, Nat. Commun. 11, 1445 (2020).
  14. [14]A. V. Chumak, A. A. Serga, and B. Hillebrands, J. Phys. D. Appl. Phys. 50, 244001 (2017).
  15. [15]E. Turov, J. Exp. Theor. Phys. 9, 890 (1959).
  16. [16]F. Keffer, Spin Waves, edited by H. P. J. Wijn (Springer, 1966) pp. 1–273.DOI
  17. [17]E. J. Samuelsen and G. Shirane, Phys. status solidi 42, 241 (1970).
  18. [18]J. R. Hortensius, D. Afanasiev, M. Matthiessen, R. Leenders, R. Citro, A. V. Kimel, R. V. Mikhaylovskiy, B. A. Ivanov, and A. D. Caviglia, Nat. Phys. 17, 1001 (2021), arXiv:2105.05886.DOI
  19. [19]C. Sirtori, Nature 417, 132 (2002).
  20. [20]I. S. Osborne, Science 320, 220 (2008).
  21. [21]A. H. Morrish, Canted Antiferromagnetism: Hematite (World Scientific, 1995).
  22. [22]M. Hamdi, F. Posva, and D. Grundler, in 67th Annu. Conf. Magn. Magn. Mater. (MMM 2022) (2022) pp. GOE–12.
  23. [23]H. Wang, R. Yuan, Y. Zhou, Y. Zhang, J. Chen, S. Liu, H. Jia, D. Yu, J.-P. Ansermet, C. Song, and H. Yu, (2022), arXiv:2211.10989.DOI
  24. [24]R. Lebrun, A. Ross, S. A. Bender, A. Qaiumzadeh, L. Baldrati, J. Cramer, A. Brataas, R. A. Duine, and M. Kläui, Nature 561, 222 (2018).
  25. [25]R. Lebrun, A. Ross, O. Gomonay, V. Baltz, U. Ebels, A. L. Barra, A. Qaiumzadeh, A. Brataas, J. Sinova, and M. Kläui, Nat. Commun. 11, 6332 (2020).
  26. [26]H. Wang, Y. Xiao, M. Guo, E. Lee-Wong, G. Q. Yan, R. Cheng, and C. R. Du, Phys. Rev. Lett. 127, 117202 (2021).
  27. [27]P. Pincus, Phys. Rev. Lett. 5, 13 (1960). J. O. Artman, J. C. Murphy, and S. Foner, Phys. Rev. 138, A912 (1965).
  28. [29]C. W. Searle and S. T. Wang, J. Appl. Phys. 39, 1025 (1968).
  29. [30]M. Shone, Circuits Systems Signal Process 4, 89 (1985).
  30. [31]S. Watanabe, V. S. Bhat, K. Baumgaertel, M. Hamdi, and D. Grundler, Sci. Adv. 7, eabg3771 (2021).
  31. [32]B. M. Moskowitz, M. Jackson, and V. Chandler, in Treatise Geophys. Resour. Near-Surface Earth, Vol. 11, edited by G. Schubert (Elsevier, 2015) 2nd ed., Chap. 11.05, pp. 139–174.
  32. [33]B. Iandolo, B. Wickman, I. Zorić, and A. Hellman, J. Mater. Chem. A 3, 16896 (2015).
  33. [34]A. H. Hill, F. Jiao, P. G. Bruce, A. Harrison, W. Kock-elmann, and C. Ritter, Chem. Mater. 20, 4891 (2008).
  34. [35]H. J. Fink, Phys. Rev. 133, A1322 (1964).
  35. [36]M. R. Querry, Optical Constants, Tech. Rep. (Missouri University, 1984).
  36. [37]T. Sebastian, K. Schultheiss, B. Obry, B. Hillebrands, and H. Schultheiss, Front. Phys. 3, 35 (2015).
  37. [38]L. Novotny and B. Hecht, Principles of Nano-Optics (Cambridge University Press, 2012) p. 584.
  38. [39]U. Levy, N. Davidson, and Y. Silberberg, Adv. Opt. Photonics 11, 828 (2019).
  39. [40]S. S. Kalarickal, P. Krivosik, M. Wu, C. E. Patton, M. L. Schneider, P. Kabos, T. J. Silva, and J. P. Nibarger, J. Appl. Phys. 99, 093909 (2006).
  40. [41]C. Bilzer, T. Devolder, P. Crozat, C. Chappert, S. Cardoso, and P. P. Freitas, J. Appl. Phys. 101, 074505 (2007).
  41. [42]H. Yu, O. d. Kelly, V. Cros, R. Bernard, P. Bortolotti, A. Anane, F. Brandl, R. Huber, I. Stasinopoulos, and D. Grundler, Sci. Rep. 4, 6848 (2014).
  42. [44]R. Z. Levitin, A. S. Pakhomov, and V. A. Shchurov, J. Exp. Theor. Phys. 29, 669 (1969).
  43. [45]P. P. Maksimenkov and V. I. Ozhogin, J. Exp. Theor. Phys. 38, 324 (1974).
  44. [46]F. Crameri, Zenodo 10.5281/ZENODO.5501399.
  45. [47]F. Crameri, G. E. Shephard, and P. J. Heron, Nat. Commun. 11, 5444 (2020).

Paper details

vlnc:W_y8zthhm3
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 6

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents