WorksPhysics and Astronomy
Tuneable ion selectivity in vermiculite membranes intercalated with unexchangeable ions
Abstract
Membranes selective to ions of the same charge are increasingly sought for wastewater processing and valuable element recovery. However, while narrow channels are known to be essential, other membrane parameters remain difficult to identify and control. Here we show that Zr, Sn, Ir, and La ions intercalated into vermiculite laminate membranes become effectively unexchangeable, creating stable channels, one to two water layers wide, that exhibit robust and tuneable ion selectivity. Ion permeability in these membranes spans five orders of magnitude, following a trend dictated by the ions' Gibbs free energy of hydration. Unexpectedly, different intercalated ions lead to two distinct monovalent ion selectivity sequences, despite producing channels of identical width. The selectivity instead correlates with the membranes' stiffness and the entropy of hydration of the intercalated ions. These results introduce a new ion selectivity mechanism driven by entropic and mechanical effects, beyond classical size and charge exclusion.
Introduction
Evidence from biological channels[1, 2] and artificial systems[1, 3, 4], such as nanotubes[5, 6, 7], nanochannels[8, 9], and two-dimensional (2D) nanopores[10, 11, 12] has shown that achieving selectivity between ions of the same charge requires membranes with precisely controlled pore size, typically in the subnanometre range[1]. This has attracted attention to laminate membranes made with 2D materials like graphene oxide (GO)[13, 14, 15], MoS[16] or MXenes[17, 18, 19, 20] as systems that could enable such selectivity with scalable technologies. In these membranes, the stacked 2D crystals form narrow channels that can in principle provide such selectivity. However, these membranes swell in water, which increases the interlayer space beyond the hydrated diameters of ions in common salts[13, 14, 15], making them non-selective to these ions[13, 14, 15]. This led to the design of mechanically confined GO membranes[15], and more recently, to cation control of the interlayer spacing in GO and MXenes[19, 20]. In this latter strategy, ions such as Al or K are pre-intercalated into the membranes, and because of their strong binding to the 2D material, prevent the membrane from swelling.
In this context, clays merit attention. This abundant material can be exfoliated into 2D layers, which enables fabricating laminate membranes[21, 22, 23, 24] similar to GO or MXene. The material consists of negatively charged aluminosilicate layers with native cations such as Mg adsorbed in the interlayer spaces that hold the layers together[21, 25, 26]. Crucially, these native ions can be easily substituted for others via ion exchange[27, 28, 29, 30], which enables tuning the interlayer separation[25, 26, 31]. This versatility, however, is also the biggest hinderance to using vermiculite membranes in ion sieving applications. Exposing the membranes to electrolyte solutions exchanges the interlayer ions for those in the solution within hours[28] making their properties unstable and sometimes even leading to complete membrane disintegration. One strategy to tackle this problem is to chemically bond the layers with organic or oxide linkers, which preserves membrane stability and enables ion-selective membranes[32, 33, 34]. In this work, we adopt a different strategy. We show that a group of high valence ions, namely zirconium, iridium, tin and lanthanum intercalated in vermiculite clay laminates, is effectively impossible to exchange at ambient conditions yielding robust and tuneable ion selective membranes.
Results
membrane shows no changes after 180 days of immersion in LiCl. Inset shows that the XRD signal for K-Ver immersed in LiCl is lost within 24 hrs. e, Mass loss of ions in Zr-Ver membranes determined with ICP-OES after exposing the membrane to different chloride electrolytes, acid (HCl, pH=3) and basic (NaOH, pH=12) solution for 24 hrs. Error bars, SD from different measurements.
Membranes with robust ion-exchange resistance. Vermiculite laminate membranes were fabricated from aqueous dispersions prepared from thermally expanded vermiculite crystals via a two-step and ion exchange process, as reported previously[21, 22, 23]. This yielded stable aqueous colloid solutions of high-quality vermiculite nanosheets nm thick and m in lateral size (Figure 1a and Supplementary Figure S1). Membranes with a well-ordered lamellar structure, typically m thick (Figure 1c), were fabricated from the dispersions via vacuum filtration (Figure 1a, Supplementary Figure S1). This as-fabricated vermiculite membrane, saturated with ions (Li-Ver), was then immersed in different electrolyte solutions to exchange the cations for those in the electrolyte. We tested various cations, such as , or , all of which were successfully inserted into the membrane, yielding K-Ver, Na-Ver, etc. However, while this makes vermiculite membranes highly tuneable, it also makes them unstable as ion separation membranes. This can be clearly appreciated for electrolytes, for which the problem is particularly severe. We found that the sharp XRD signal of these membranes (e.g. K-Ver) is lost within hrs of continuous exposure to LiCl electrolyte (Figure 1d inset) and visual examination revealed that these membranes had disintegrated (Supplementary Fig. 2). For other electrolytes (e.g. K-Ver in NaCl), the membranes did not disintegrate in the electrolyte, but their composition changed rapidly. Inductively coupled plasma optical emission spectrometry (ICP-OES) of the membranes revealed that within 24 hrs of exposure to different electrolyte solutions, the mass loss of interlayer ions was ; that is, practically all the initial intercalated ions were exchanged (Figure 1e inset and Supplementary Fig. 3).
Figure 1. Robust ion-exchange resistance of Zr-intercalated vermiculite membranes. a, AFM image of exfoliated vermiculite flakes. Bottom inset, height profile of crystal along section marked by dashed line below. Scale bar, 2 µm. Top inset, aqueous dispersion of the exfoliated crystal. b, Annular dark field scanning transmission electron micrograph of Zr-Ver flake. The crystal consists of aluminosilicate layers with adsorbed Zr ions (marked with yellow arrow). Zr ions display bright contrast due to their relatively heavier atomic number. Yellowed dashed lines mark regions that are not occupied by Zr. Scale bar, 5 Å. c, Cross-sectional SEM image of a typical vermiculite membrane. Scale bar 500 nm. Inset, optical image of typical membrane. d, XRD spectra of Zr-Ver
Figure S1. Sample preparation. a, Schematic illustration of the ion exchange and exfoliation process. b, Vermiculite dispersions show Tyndall effect. c, Optical image of vermiculite flakes dispersed on silicon-dioxide substrate. Typical flake size is about 10 m. Scale bar 10 m. d, TEM images reveal that vermiculite flakes display negligible defects. Scale bar 1 m. e, Optical image of free-standing vermiculite membrane. Scale bar 1 cm. f, Schematic showing that the membranes are soaked in different ion solutions for ion exchange. g, The concentration in a vermiculite laminate membrane as a function of time immersed in 1M ZrCl electrolyte solution. h, Image of Zr-Ver nanosheets on TEM grids. Scale bar 1 m. i, STEM image of Zr-Ver over larger areas. Bright spots, Zr-atoms. Scale bar, 1 nm. j, Electron diffraction taken from the sample. Scale bar, . k, Corresponding EDS spectrum. Cu peaks are from the TEM holder and the supporting grids.
We found that , , and inserted in vermiculite membranes are effectively impossible to remove by immersing the membranes in common electrolytes at ambient conditions and that this makes these membranes robust in ion transport experiments. To fabricate the membranes, the Li-Ver membranes described above were immersed in electrolyte solutions of these ions (e.g. 1.0 M for about 1h) and then rinsed with deionised (DI) water. We then tested the stability of the exchanged membranes by immersing them in various aqueous electrolyte solutions, including LiCl, between 1 to 180 days. XRD characterisation showed that the interlayer separation of the membranes remained stable for as long as we decided to test them, up to 180 days (Figure 1d and Supplementary Fig. 4&5). Additional ICP-OES characterisation revealed only a minor loss of intercalated ions (Figure 1e, Supplementary Fig. 5), which remained stable over the whole testing period. We therefore call these strongly bonded ions ‘unexchangeable ions’, to differentiate them from those that can be readily exchanged (e.g. or , Supplementary Fig. 3). Microscopic insights into the distribution of the unchangeable ions were obtained with aberration-corrected scanning transmission electron microscopy (AC-STEM). This revealed that the ions tended to form domains with quasi-hexagonal symmetry separated by large -free regions (Figure 1b). In fact, only a small fraction of the flake surface is occupied by , leaving extensive areas without coverage (Figure 1b and Supplementary Figure S1). This low coverage is expected, as the valence of each ion balances multiple adsorption sites in vermiculite (each with valence). Selective ion transport. These robust laminates could be used as ion sieving membranes. We measured the permeability of 14 common inorganic cations focusing on Zr-Ver membranes, which is used as a model system. In the experiments, the membrane was used as a separator between two reservoirs, one containing a solution of a common chloride salt and the other filled with deionised (DI) water (Figure 2a inset)[20, 35, 36]. The concentration of ions in this latter reservoir was then measured as a function of time using ICP-OES and atomic absorption spectroscopy (AAS). Figure 2a shows that such concentration increased linearly with time and decreased linearly with membrane thickness, (Supplementary Fig. 6). This allowed extracting the ions’ flux through the membrane, , and the membrane permeability as: , with the difference in electrolyte concentration between feed and permeate chambers. These experiments revealed that the permeability of different monovalent cations extended over an order of magnitude, with Cs the most permeable () and Li the least (); whereas multivalent cations all displayed lower permeability of - . Reference experiments with nitrate salts yielded the same cation selectivity sequence, indicating that the selectivity is intrinsic to the membranes, and not dependent on the specific salt used (Supplementary Fig. 7). We also measured the permeability of the counterions in solutions with various salts, which revealed that all anions permeated through the membrane at a similar rate than their associated cation (Supplementary Fig. 8). This was expected. The unexchangeable Zr ions already maintain the membrane’s electroneutrality and remain adsorbed during permeation experiments. Hence, anions must accompany cation permeation to preserve charge balance. No appreciable osmotic flow was observed during the measurements, and vapour transport measurements revealed low water flux (Supplementary Figure S9), consistent with the narrow channels in the membranes and the small slip length of water in clays[37].
Figure 2. Ion-selective Zr-intercalated vermiculite membranes with controllable 1 or 2 water molecule thick channels. a, Ion permeation vs time data for the Zr-Ver membranes. Inset, schematic of experimental setup. b, Sr permeation vs time for Zr-Ver membrane in SrCl (blue) and CsCl/SrCl (red). Error bars in panels b and d, SD from multiple measurements. Dashed lines, guide to the eye. c, XRD spectra of Zr-Ver membrane after immersion in different electrolytes and
Figure S9. Water vapour transport through vermiculite membranes. Water loss from a sealed container capped with different membranes (colour coded), measured gravimetrically over time. Top inset, water flux extracted from the slopes for each membrane. Bottom inset, schematic of the experimental setup.
water. Most of the electrolytes tested led to interlayer spacing Å (two water layers), except K and Cs, which reduced it to Å (one water layer). d, XRD spectra of membrane after immersion in SrCl (blue curve) and a 50:50 CsCl/SrCl mix (red curve). Cs addition consistently reduces the interlayer spacing to Å across all tested electrolytes. e, Ion flux vs. Gibbs hydration energy for permeating cations (blue). Adding Cs (50:50 electrolyte-CsCl mix) leads to notably sharper ion selectivity (red). Dashed curves, guide to the eye. Right -axis: ion permeability. Grey area: experimental resolution background. Error bars, SD from at least ten different samples. Permeability and interlayer separation data are provided in Supplementary Table 1.
| Membrane | Ion | (mol/cm) | Interlayer spacings (Å) | Average flux (mmol m h) | Permeability (m s) | |
| Without Cs | Zr-Ver | Li | 2.45 | 14.8 | 1.43 | 7.92×10 |
| Na | 4.30 | 14.8 | 1.25 | 6.96×10 | ||
| K | 6.23 | 12.2 | 4.01 | 2.23×10 | ||
| Cs | 10.34 | 12.2 | 11.86 | 6.59×10 | ||
| Mg | \ | 14.0 | 0.96 | 5.34×10 | ||
| Ca | \ | 14.0 | 1.32 | 7.34×10 | ||
| Sr | \ | 14.8 | 0.44 | 2.42×10 | ||
| La | \ | 14.8 | 0.26 | 1.43×10 | ||
| Zr | \ | 14.8 | 0.29 | 1.61×10 | ||
| With Cs | Zr-Ver | Li | \ | 12.8 | 1.99 | 1.11×10 |
| Na | \ | 12.8 | 3.66 | 2.03×10 | ||
| K | \ | 12.8 | 8.53 | 4.74×10 | ||
| Cs | \ | \ | 10.50 | 5.83×10 | ||
| Mg | \ | \ | 0.027 | 1.52×10 | ||
| Ca | \ | \ | 0.051 | 2.83×10 | ||
| Sr | \ | 12.8 | 0.032 | 1.76×10 | ||
| Ce | \ | \ | 0.0005 | 2.78×10 | ||
| Fe | \ | \ | 0.0005 | 2.78×10 | ||
| Al | \ | \ | 0.0005 | 2.78×10 | ||
| La | \ | \ | 0.00037 | 2.04×10 |
Table 1. Ion permeabilities, membrane ion concentrations, and associated interlayer spacings
To understand the membrane’s selectivity, we started by plotting the cation permeability versus their Gibbs energy of hydration[35] (Figure 2e, blue symbols). This revealed that the cations’ permeability was strongly correlated with their Gibbs energy of hydration, with lower hydration energy associated with larger . On the other hand, XRD measurements of the membranes immersed in the different electrolytes (Figure 2c,Figure 2d and Supplementary Fig. 4) revealed that for most electrolytes, the interlayer spacing in Zr-Ver membrane was Å. Given the vermiculite aluminosilicate monolayer thickness ( Å), this accommodates water layers, revealing that the membrane’s interlayer spacing is comparable to or smaller than the hydrated diameters of common cations. The only exceptions to Å were Cs and K electrolytes, which led to even narrower Å, just one water layer thick (XRD measurements in Methods). This well-known phenomenon, so-called ‘collapse’ of the interlayer space, arises because Cs and K are easily dehydrated, and are stabilised as adsorbed inner sphere complexes on the lattice, forming polar bonds with the structural oxygen atoms in the vermiculite layers[31, 38, 39, 40, 41]. During interlayer collapse, the areas of the flake covered with Zr retain a fixed Å interlayer distance. However, since areas without Zr dominate the surface, their collapse governs the overall XRD response. This results in spectra centred at Å, albeit with a broad distribution due to the less uniform interlayer spacing (Figure 2c,Figure 2d and Supplementary Fig. 4).
The collapse of the interlayer space with Cs electrolyte provides a way to study ion diffusion in channels just one water molecule thick, offering further insight into the membranes’ selectivity. To test this, we added 1M of CsCl into all our 1M chloride solutions and measured ion transport as discussed above. XRD characterisation confirmed interlayer spacing of Å, corresponding to a single water layer inside the channels (Figure 2d panel and Supplementary Fig. 4). Figure 2e shows that ion flux in these narrower channels remained correlated with their Gibbs energy of hydration, but with a much sharper dependence. Monovalent ion flux remained similar, but divalent ions now displayed about 100 times smaller than in the absence of Cs and trivalent and tetravalent ions displayed about 1000 times smaller, rendering them effectively impermeable within our measurement’s sensitivity (Figure 2b,Figure 2e). As a result, ion flux now spanned five orders of magnitude. This pronounced selectivity stems from the increased energy cost associated with ion transport through a space confined to a single water layer. Taken together, the selective ion transport phenomena can be understood as arising from the difference in the ions’ Gibbs energy inside and outside the channels (). Weakly hydrated monovalent ions are stabilised by the channel walls and permeate easily even in the narrowest channels. This is particularly evident for Cs, which is more strongly attracted to the channel walls than to water, leading to interlayer collapse and high flux. In contrast, strongly hydrated multivalent ions experience a much larger , interact weakly with the walls, and display low flux.
Tuneable monovalent ion selectivity sequences. We then studied the transport of monovalent ions through membranes intercalated with different unexchangeable ions, namely , , and . As shown in Figure 3a, La-Ver and Zr-Ver membranes followed the same selectivity sequence shown above, , whereas Ir-Ver and Sn-Ver displayed a different sequence: . As a result, for in Ir-Ver and Sn-Ver was about 60 times higher than in Zr-Ver and La-Ver. This behaviour remained stable for as long as we decided to test these membranes, typically hours (Figure 3c, see Supplementary Figure S10 for mixed-salt measurements). To understand this finding, and given that ion permeability depends on both the ions’ equilibrium concentration and diffusion constant within the membrane[42], we measured the composition of the membranes with ICP-OES after the transport measurements (Supplementary Figure S11). This revealed that differences in concentration of the permeating ion in the membranes explained nearly all permeability variations. This was confirmed with electrochemical impedance spectroscopy measurements (Supplementary Figure S12), which showed that the ions’ diffusion constants varied negligibly across different membranes. For example, the concentration of was times higher in Sn-Ver and Ir-Ver than in Zr-Ver and La-Ver, but the diffusion constant changed by less than 20%. To understand why the concentration of the ions changed so strongly across the four different membranes, we first measured the XRD spectra of the membranes immersed in the different electrolytes. Intriguingly, this revealed that the interlayer spacing of the four membranes was the same for a given electrolyte (Figure 3b and Supplementary Fig. 5): Å, for LiCl and NaCl and Å for CsCl and KCl, thus ruling out channel width differences as the cause of these different selectivity sequences.
Figure 3. Monovalent ion selectivity in vermiculite membranes with different intercalated ions. a, Ion permeability through vermiculite membranes intercalated with , , , and (colour-coded), revealing two distinct selectivity sequences. Grey curves, guide to the eye. Inset, statistics of Young’s Moduli of membranes obtained from AFM measurements (same colour code as main panel). Fitted curves to data, guide to the eye. b, XRD spectra of intercalated membranes after 24 hrs in LiCl, all showing an interlayer spacing of Å within experimental scatter. c, permeation vs. time for membranes intercalated with different unexchangeable ions. Error bars, standard deviation (SD) from at least ten samples. Dashed lines, guide to the eye.
Figure S10. Mixed salt transport through vermiculite membranes. a, Ion flux through Zr–Ver membranes for different monovalent ion mixtures (ion pairs shown in blue and green bars). b, Corresponding data for Sn–Ver membranes (ion pairs shown in blue and orange). Error bars in a and b, SD from different membranes. c, XRD patterns of Zr–Ver membranes after exposure to the ion mixtures. d, Equivalent XRD data for Sn–Ver membranes.

Figure S11. Concentration of permeating ion inside membranes intercalated with different unexchangeable ions. Concentration of different ions (colour coded) inside Zr-Ver, La-Ver, Ir-Ver and Sn-Ver membranes after ion transport measurements, as determined by ICP-AES measurements. The concentration obtained from ICP is converted into ion concentration per channel volume (‘Measurement of ion flux’ in Methods). Dashed lines, guide to the eye.

Figure S12. Electrochemical impedance spectroscopy measurements. a, Experimental setup. b, Resistance of typical membrane stack (Zr-Ver) soaked in electrolyte solution (LiCl) as a function of number of stacked membranes. The membrane resistance was extracted from the slope of the linear fit of the resistance vs. the numbers of membranes stacked layer-by-layer. Inset, Nyquist plot of membrane stacks from which resistance in main panel is extracted. c, Diffusion coefficients for different ions in Zr-Ver, Ir-Ver and PES-membrane (bulk) membranes extracted from resistance data.
At first glance, these results seem puzzling, since the selectivity cannot be explained by differences in channel width, nor does it correlate with the charge of the unexchangeable ions.
For example, despite the different charges of and , both Zr-Ver and La-Ver exhibit similar selectivity. To solve this puzzle, we draw insights from biological channels, in which ion selectivity is thought to be primarily determined by three parameters[43]: hydration free energy of the permeating ion, electrostatic interaction between ion and channel and, finally, channel elasticity. Since the first two parameters do not account for our observations, we turned our attention to channel elasticity. This parameter affects ion selectivity in biological porins because it changes the Gibbs energy of ions inside the channel due to thermal fluctuations of channel width[43]. In a first approximation, this elastic component is modelled as , where is the elastic constant as a function of position in the channel, , and is the equilibrium channel width[43]. Similar ionic-mechanical coupling effects have been observed in clays, with time-resolved X-ray scattering revealing that ion exchange is accompanied by dynamic fluctuations of the basal plane spacing[44]. Motivated by this, we measured the Young’s moduli of the membranes, which determines the elasticity of the channels[45]. As shown in Figure 3a (inset) and Supplementary Fig. 13, the moduli of Zr-Ver and La-Ver (0.55 GPa and 0.3 GPa, respectively) were an order of magnitude larger than for Sn-Ver (0.01 GPa) and Ir-Ver (0.03 GPa), suggesting a link between selectivity and membrane stiffness. Hence, understanding why different unexchangeable ions lead to different membrane stiffness should provide insights into the selectivity phenomena.
With this insight, we recall that water exhibits an unusually high resistance to local deformation due to its hydrogen-bond network[46, 47]. This can be quantified by several thermodynamic parameters, such as cohesive energy density, isothermal compressibility, heat capacity density, and dipole orientational correlation[46]. Collectively, these quantities capture the energetic cost of disrupting its structured environment and can be used to define a quantity known as water ‘stiffness’, which is the work required to create a cavity for an additional water molecule[46]. Ions with highly ordered hydration shells – and thus with more negative hydration entropy, – are known to lead to a more ordered water network, thus increasing water’s stiffness[46, 48]. Since confined water in clays is more structured than bulk[49], the influence of solvated ions on its stiffness, and thus the mechanical properties of the membrane, can be expected to be even larger. This is consistent with our observations. Indeed, of the unexchangeable ions tested, (-763 J mol K) and (-454 J mol K) have the most negative [50] and also yield the stiffest membranes. On this basis, we propose that the unexchangeable ions modulate the stiffness of water in the membrane, thereby controlling the channels’ elasticity, and thus modulating ion selectivity, similar to the role of elasticity in biological channels. This explains why displays the largest variations in permeation: having the largest hydrated diameter amongst monovalent ions, it displays the largest changes in .
Discussion
This work investigated vermiculite laminates with immobilised high-valence ions, creating structurally stable membranes with channels either one or two water layers wide. The permeability of different cations spanned orders of magnitude and correlated with their hydration Gibbs energy. Unexpectedly, membranes with different unexchangeable ions showed different monovalent ion selectivity, which could not be explained by channel width, ion charge, or hydration Gibbs energy alone. Mechanical measurements revealed a link between membrane stiffness and the hydration entropy () of the intercalated ions, which in turn reflects the ions’ impact on the structure of confined water within the membrane. This finding mirrors principles observed in biological ion channels, where subtle entropic and mechanical effects – rather than solely size or charge exclusion – govern highly specific ion transport. Our findings establish vermiculite membranes as a versatile and robust model system to explore novel ion selectivity phenomena.
Methods
Materials. Vermiculite clay was sourced from Sigma Aldrich (CAS No 1318-00-9). To characterise its elemental composition, bulk crystals with grain-size of 2-3 mm were initially subjected to thermal expansion and subsequently ground into powders, dried at 80 °C for 24 h and then dissolved using dilute HF. Inductively coupled plasma atomic emission spectroscopy (ICP-AES) was used to determine the elemental composition. The detected interlayer metal cation mass fractions were 3.20% (KO: 3.86%), 14.99% (MgO: 24.98%), 7.77% (AlO: 14.35%), 7.77% (FeO: 11.08%), and 18.95% Si (SiO: 40.60%).
Vermiculite suspension preparation. Vermiculite crystals were exfoliated in a two-step ion exchange process[21, 22, 23], as depicted in Supplementary Figure S1. In the process, 100 mg of vermiculite granules 2-3 mm in size were immersed in 200 mL of saturated NaCl solution (36 wt%) and refluxed for 24 hours. The treated vermiculite flakes were filtered and washed extensively with water and ethanol to remove residual salts. Next, 200 mL of a 2M LiCl solution was used to disperse the sodium-exchanged vermiculite, followed by a 24-hour reflux to facilitate ion exchange. The resultant lithium vermiculite flakes were filtered and subjected to thorough washing with 1 L of hot water and 0.5 L of acetone. Then, the lithium-exchanged vermiculite flakes were dispersed in water and underwent three cycles of centrifugation at 3000 rpm. This dispersion was subsequently sonicated for 20 minutes at 100 W to exfoliate the material into monolayer vermiculite flakes. Further centrifugation at 3000 rpm was employed to eliminate multilayers and bulk residues. The resulting final dispersions exhibit a pronounced Tyndall effect (Fig. Supplementary Figure S1), evidencing high quality dispersions.
To determine the concentration of vermiculite in the suspensions, 1 mL of the suspension was dropped onto an Anodic Aluminium Oxide (AAO) membrane with a diameter of 2.5 cm and dried. After drying, the thin film was peeled off the AAO membrane and weighed to calculate the dispersion concentration. Alternatively, the difference in mass before and after coating the AAO membrane with vermiculite suspension was also used to calibrate the dispersion concentration. Three thin film samples were typically used for concentration calibration.
We characterised the vermiculite flakes using optical microscopy, transmission electron microscopy (TEM) and atomic force microscopy (AFM). For optical microscopy observations, the vermiculite stock solution was diluted to a concentration of mg/mL, and the diluted suspension was dropped onto a silica substrate. The sample was dried at 80°C, followed by heating at 200°C for two hours. We found that most of the flakes had dimensions ranging from 10 to 20 m (Supplementary Figure S1). TEM images revealed that the large vermiculite flakes exhibited no noticeable defects (Supplementary Figure S1).
Membrane preparation. Vermiculite laminate membranes were prepared by vacuum filtration and ion exchange. The dispersion of exfoliated vermiculite nanosheets underwent vacuum filtration using polyether sulfone (PES) membranes (Millipore) or Anodic Aluminium Oxide (AAO) membranes (Whatman) as filters. The polyether sulfone (PES) membranes with pore size of 0.22 m and diameter of 2.5 cm or 4.7 cm were purchased from Millipore. The Anodic Aluminium Oxide (AAO) membranes (pore size of 0.2 m and diameter of 2.5 cm) were purchased from Whatman. Generally, the filtration process to form the vermiculite membrane takes 1–3 days to complete. Once finished, the substrate with the vermiculite membrane is removed from the filtration apparatus and transferred to an oven for drying for 12 hours. The vermiculite membranes can then be easily peeled off the substrate, resulting in intact and complete pristine vermiculite membranes.
The interlayer ions in the resulting membranes are Li due to the exfoliation procedure. To replace them for ‘unexchangeable’ ions, the membranes were immersed in solutions of either 1M of ZrCr, IrCl, SnCl or 0.1 M for IrCl. The concentration of the ion (e.g. Zr) within the membranes was measured by dissolving the membranes in a 2.0 mL solution of 1 wt% dilute HF and then measuring the solution with inductively coupled plasma optical emission spectrometry (ICP-OES). We found that the exchange process equilibrated within 1 hr for 1M solutions and over 24 hrs for 0.1 M solutions. Using this method, vermiculite membranes were immersed in various ion solutions to prepare the various membranes for the study (e.g. K-Ver, Sr-Ver, Ir-Ver, etc). In all cases, including SnCl, the solutions used were well-dispersed and did not display obvious precipitation. TEM characterisation of the resulting membranes revealed that the ions, including Sn, were incorporated as single atoms.
Stability of membranes immersed in electrolyte solutions. We employed three criteria to evaluate the stability of the membranes immersed in electrolyte solutions: the membrane’s visual appearance, the interlayer spacing characterised by XRD and the mass loss of the inserted ion characterised by ICP mass spectrometry.
For optical tests, 1 cm membranes were soaked in both pure water and various salt solutions, such as 1.0 M LiCl. Membranes exchanged with unexchangeable ions (Zr, Ir, Sr and La) exhibited robust mechanical integrity. The membranes remained intact even under vigorous agitation after weeks of immersion in the electrolyte solution. In contrast, membranes intercalated with ions such as K, Ba and Sr (Supplementary Fig. 3) disintegrated after 24 hrs.
To test the compositional stability of the membranes, a 1 cm membrane was cut in six squares, dried at 80°C for 24 hours and weighed with an electronic balance (Mettler Toledo, XPE26; accuracy: 0.001 mg). Each membrane was then soaked in 2 mL of different electrolyte solutions. We tested 1 M LiCl, 1M NaCl, 1M KCl, 1M CsCl, 1M SrCl, 1M MgCl, 1M CaCl, 1 M LaCl, 0.1 M IrCl, as well as acidic (HCl, pH ≈ 3) and basic (NaOH, pH ≈ 12) solutions or pure water for 24 hours. After soaking, the membranes were rinsed with deionised water, degraded with dilute HF, and analysed with ICP-OES to determine the content of the unexchangeable ion in the membrane. The membranes soaked in pure water served as a reference for total unexchangeable ion content in the original membrane. The results for ion mass loss are presented in Figure 1e and Supplementary Fig. 5, revealing mass loss typically below 5% and always below 10%. In contrast, the mass loss in reference membranes exchanged with K, Ba and Sr was nearly 100% after the exposure to the electrolytes for the same period (Supplementary Fig. 3).
The interlayer spacing in the membranes in aqueous environments was characterized via X-ray diffraction (XRD) analysis (Rigaku MiniFlex 600-C with Cu Kα radiation). 1 cm membranes were soaked in 5 mL of the chloride solutions studied in this work (1 M concentration, except for Fe, and Sn, which were 0.1 M) for 24 hours. After soaking, the membranes were thoroughly rinsed with deionised water. The wet membranes were mounted on a silicon wafer for XRD measurements, with excess water removed using filter paper. Scans were performed at 10°/minute with a step size of 0.01°. For membranes soaked in 1 M LiCl for 180 days, the most aggressive test for vermiculite membranes, no significant shift or disappearance of XRD peaks was observed. We also performed this experiment with all the electrolytes used in this study. Supplementary Fig. 4 and 5 show that the XRD was stable for all these electrolytes. It also shows that for most electrolytes the main peak position was at approximately 6.1°. The exception to this were K⁺ and Cs⁺ solutions as well as mixtures of other electrolytes with Cs electrolyte. In this case, the peaks were around 7.2°.
Measurements of ion flux. For permeation measurements, the membranes were affixed over a 0.5 cm diameter hole in a polymethyl methacrylate (PMMA) plate. The plate was then mounted in a polytetrafluoroethylene (PTFE) cell that consisted of two compartments. One compartment (the feed) was filled with 12 mL of salt solution with concentration of 1.0 M for monovalent/divalent cations or 0.1 M for trivalent and tetravalent cations, whereas the other (permeate) contained 12 mL of deionized water. The ion concentration in the permeate solution was monitored periodically using ICP-OES and AAS. Each ion flux experiment was repeated with at least 10 different membranes. The flux, , was calculated using the expression: , where is the ion concentration in the permeate water, the volume of the solution in the permeate (12 mL), the membrane area and the testing time. From the flux, we estimated the permeability for each ion from the equation[42]: , where is the diffusion constant, is the difference in concentration between feed and permeate chambers and is the membrane thickness. The diffusion constant is extracted from the expression: , where is the sorption coefficient, which satisfies , with the average ion concentration in the membrane.
We measured concentration of ions inside the membrane with ICP-OES. We then estimated the ion concentration as a function of channel volume (Supplementary Figure S11). To that end we converted ion content from millimoles per gram of membrane obtained by ICP-OES in C[mmol/g] to millimoles per cubic centimetre of channel volume C[mmol/cm³] using: C[mmol/cm³] = C[mmol/g] × × , where the density of vermiculite is taken as g cm⁻³, the interlayer spacing is obtained from XRD, and the monolayer thickness of vermiculite is approximated as nm.
Electrochemical impedance measurements. Electrochemical impedance measurements of the membranes were performed following the methods reported in ref. 51. Zr-Ver and Ir-Ver membranes were cut into four equal pieces and then stacked on top of each other to form stacks with thickness from 1 to 4 layers of the original membrane. The stacks were soaked with different electrolyte solutions and then clamped in between two stainless steel plates in a custom-made cell (Supplementary Figure S12). Reference experiments were performed using the same methods but using polyethersulfone (PES) membranes instead of vermiculite membranes. Supplementary Figure S12 shows that the resistance scales linearly with thickness for all membranes, which allows extracting the resistance per layer from the slope of this dependence. We then estimated the diffusion coefficient () using the expression: , where is the membrane thickness, is the universal gas constant, is the absolute temperature, is the membrane area, is the charge number of the ions, is Faraday’s constant, and is the ion concentration within the membrane. This analysis yields of about . These values are consistent with the estimated from our flux measurements and the independently measured ion concentrations. Reference experiments with PES membranes yielded about ~100 times larger, consistent with literature values[52].
Osmotic flow measurements. Water vapour flux was quantified gravimetrically using a Zr-Ver membrane under a nitrogen atmosphere in a glove box. Supplementary Figure S9 shows that the water permeation is low, approximately , confirming that osmotic effects are minimal under the experimental conditions.
Mixed salt experiments. We measured ion flux through Zr-Ver and Sn-Ver membranes in equimolar (1 M total) mixtures of two different monovalent salts. For all mixtures containing or , the interlayer spacing collapses (Supplementary Figure S10). Under these conditions, both membranes yield the same selectivity based on Gibbs hydration energy, as expected given that the channels are now one water layer thick. The only mixture that retains the original interlayer spacing in Sn-Ver is the mixture (Supplementary Figure S10,Figure S10). In this case, Sn-Ver exhibits a much larger flux than Zr-Ver, consistent with its permeability in single-salt experiments. However, permeates approximately twice as fast as in Sn-Ver. This represents an intermediate behaviour between the selectivity of Sn-Ver in single-salt experiments, where permeated about six times faster than , and that of Zr-Ver membranes, where permeated roughly ten times faster than . This difference likely arises from competition for adsorption sites between ions within the confined channels. Less strongly hydrated ions may preferentially interact with the channel walls, enhancing their local concentration and flux. Similar competitive adsorption effects are well documented in mineral–water interfaces, where the presence of one ion alters the binding and transport of others[53, 54].
Elastic modulus of vermiculite membranes. Membranes with an area of and in thickness were glued onto silicon wafers using Stycast 1266. The mechanical properties of the membrane were characterised in liquid environment (DI water) using atomic force microscopy (AFM) in mapping mode. The scanning process included 200 scan lines, with 200 data points per line, and a map scan rate of 0.31 Hz. The AFM experiments were conducted using Bruker Instruments (Multi-Mode 8 SPM), equipped with a Bruker's SCM-PIT-V2 probe whose spring constant was calibrated via the thermal noise method. During imaging, a setpoint force of 100 nN was applied, and the Fast Force Mapping mode was used to measure the mechanical properties of the sample. The indentation depth was determined from the difference between the displacement of the sample and the deformation of the AFM probe, which was measured via a detector in the instrument that enables observing the probe’s deformation. These curves were then calibrated to establish the indentation depth's zero point. Supplementary Figure S13 shows the representative force curves for different vermiculite membranes. To extract the modulus from the force curves, we modelled the tip as a sphere in the Hertz model. This yields the relation:

Figure S13. Young’s moduli of vermiculite membranes. a, Experimental setup. b, Optical image of vermiculite membrane on silicon substrate in liquid. c, Force curves from indentation experiments. Each curve was taken at a different point in the sample. Different colours indicate membranes intercalated with different unexchangeable ions. Dark (faded) coloured curves, median (typical) indentation curve for each membrane type.
where is the applied force, is the indentation depth, is the probe radius, and is the effective modulus. The effective modulus accounts for both the sample and probe material properties. However, a posteriori, we find that our membranes, which are rather thick, have moduli of ~0.1 GPa, whereas that of the probe is much stiffer, ~170 GPa. We can therefore neglect the effect of probe on the membranes’ moduli.
The sample’s Young’s modulus is then calculated from the formula , where is the Poisson ratio for vermiculite[55, 56].
Figure Supplementary Fig. 2. Membrane integrity in electrolyte solutions. Optical image of a Li-Ver (a), K-Ver (b) and Zr-Ver (c) membrane in 1M LiCl solution, respectively. The K-Ver and Zr-Ver membranes maintain their integrity over a long period of immersion in 1M LiCl solution, with no significant damage observed macroscopically. All electrolytes tested in this work led to similar results.
Figure Supplementary Fig. 3. Membranes intercalated with common ions are unstable against ion exchange. Ba-Ver (a), Sr-Ver (b) and K-Ver (c) membranes were immersed in 1M LiCl, NaCl, KCl and SrCl electrolyte solutions for 24 hrs, respectively. The mass loss of the original intercalated Ba, Sr and K measured by mass spectrometry.
Figure 4. XRD spectra of Zr-Ver membranes. XRD spectra of Zr-Ver membranes after 24 hr of immersion in 1 M electrolyte solutions. The greyed area shows that the XRD peaks angles fall into two groups.
Figure 5. Vermiculite membranes exchanged with unexchangeable ions are stable against re-exchange. XRD spectra of Sn-Ver (a), Ir-Ver (b), and La-Ver (c) membranes after immersion in 1M chloride salt solutions for 24 hours. d-f, Mass loss of intercalated unexchangeable ions in the membranes in panels a-c.
Figure 6. Ion flux dependence on membrane thickness. Ion flux through Zr-Ver membranes of various thicknesses, . The flux scales linearly with (marked with dashed lines).
Figure 7. Cation flux with nitrate and chloride salts. Ion flux vs. Gibbs hydration energy for permeating cations from nitrate (red) and chloride (grey) salts. Dashed curve, guide to the eye.
Figure 8. Total ion flux through the membranes is electroneutral. a, Flux of chlorine salts with different cations. b, Flux of lithium salts with different anions through Zr-Ver membranes. In all cases, cation and anion transport balance to maintain charge neutrality. Strongly hydrated permeates more slowly than , reducing the accompanying flux. The less strongly hydrated permeates at rates comparable to , with a similar flux.
| Ion | ||||||
| \ | \ | 0.0001 | ||||
| \ | \ | 0.0001 | ||||
| \ | \ | 0.0003 | ||||
| Without | La-Ver | 1.93 | 14.5 | 0.89 | ||
| 8.14 | 14.4 | 5.70 | ||||
| 16.10 | 12.2 | 5.61 | ||||
| 22.78 | 11.9 | 8.40 | ||||
| Without | Ir-Ver | 7.86 | 14.2 | 85.30 | ||
| 8.56 | 14.4 | 14.08 | ||||
| 14.99 | 12.3 | 11.81 | ||||
| 20.04 | 11.9 | 13.27 | ||||
| Without | Sn-Ver | 36.22 | 14.3 | 91.42 | ||
| 50.18 | 14.3 | 12.41 | ||||
| 65.36 | 12.3 | 17.60 | ||||
| 73.10 | 12.0 | 21.84 |
Table 2.
References
- [1]Epsztein, R., DuChanois, R. M., Ritt, C. L., Noy, A. & Elimelech, M. Towards single-species selectivity of membranes with subnanometre pores. Nature Nanotechnology 15, 426-436 (2020). https://doi.org/10.1038/s41565-020-0713-6
- [2]Zhou, Y., Morais-Cabral, J. H., Kaufman, A. & MacKinnon, R. Chemistry of ion coordination and hydration revealed by a K+ channel–Fab complex at 2.0 Å resolution. Nature 414, 43-48 (2001). https://doi.org/10.1038/35102009
- [3]Werber, J. R., Deshmukh, A. & Elimelech, M. The Critical Need for Increased Selectivity, Not Increased Water Permeability, for Desalination Membranes. Environmental Science & Technology Letters 3, 112-120 (2016). https://doi.org/10.1021/acs.estlett.6b00050
- [4]Park, H. B., Kamcev, J., Robeson, L. M., Elimelech, M. & Freeman, B. D. Maximizing the right stuff: The trade-off between membrane permeability and selectivity. Science 356, eaab0530 (2017). https://doi.org/doi:10.1126/science.aab0530
- [5]Tunuguntla, R. H. et al. Enhanced water permeability and tunable ion selectivity in subnanometer carbon nanotube porins. Science 357, 792-796 (2017). https://doi.org/doi:10.1126/science.aan2438
- [6]Choi, W. et al. Diameter-dependent ion transport through the interior of isolated single-walled carbon nanotubes. Nature Communications 4, 2397 (2013). https://doi.org/10.1038/ncomms3397
- [7]Li, Z. et al. Breakdown of the Nernst–Einstein relation in carbon nanotube porins. Nature Nanotechnology 18, 177-183 (2023). https://doi.org/10.1038/s41565-022-01276-0
- [8]Esfandiar, A. et al. Size effect in ion transport through angstrom-scale slits. Science 358, 511-513 (2017). https://doi.org/doi:10.1126/science.aan5275
- [9]Emmerich, T. et al. Enhanced nanofluidic transport in activated carbon nanoconduits. Nature Materials 21, 696-702 (2022). https://doi.org/10.1038/s41563-022-01229-x
- [10]Rollings, R. C., Kuan, A. T. & Golovchenko, J. A. Ion selectivity of graphene nanopores. Nature Communications 7, 11408 (2016). https://doi.org/10.1038/ncomms11408
- [11]Hoenig, E. et al. In situ generation of (sub) nanometer pores in MoS2 membranes for ion-selective transport. Nature Communications 15, 7911 (2024). https://doi.org/10.1038/s41467-024-52109-8
- [12]Jain, T. et al. Heterogeneous sub-continuum ionic transport in statistically isolated graphene nanopores. Nature Nanotechnology 10, 1053-1057 (2015). https://doi.org/10.1038/nnano.2015.222
- [13]Joshi, R. K. et al. Precise and Ultrafast Molecular Sieving Through Graphene Oxide Membranes. Science 343, 752-754 (2014). https://doi.org/doi:10.1126/science.1245711
- [14]Chen, L. et al. Ion sieving in graphene oxide membranes via cationic control of interlayer spacing. Nature 550, 380-383 (2017). https://doi.org/10.1038/nature24044
- [15]Abraham, J. et al. Tunable sieving of ions using graphene oxide membranes. Nature Nanotechnology 12, 546-550 (2017). https://doi.org/10.1038/nnano.2017.21
- [16]Hu, C. Y. et al. pH-dependent water permeability switching and its memory in MoS2 membranes. Nature 616, 719-723 (2023). https://doi.org/10.1038/s41586-023-05849-4
- [17]Ren, C. E. et al. Charge- and Size-Selective Ion Sieving Through Ti3C2Tx MXene Membranes. The Journal of Physical Chemistry Letters 6, 4026-4031 (2015). https://doi.org/10.1021/acs.jpclett.5b01895
- [18]Wang, J. et al. Ion sieving by a two-dimensional Ti3C2Tx alginate lamellar membrane with stable interlayer spacing. Nature Communications 11, 3540 (2020). https://doi.org/10.1038/s41467-020-17373-4
- [19]Zhu, J. et al. Precisely Tunable Ion Sieving with an Al13–Ti3C2Tx Lamellar Membrane by Controlling Interlayer Spacing. ACS Nano 14, 15306-15316 (2020). https://doi.org/10.1021/acsnano.0c05649
- [20]Ding, L. et al. Effective ion sieving with Ti3C2Tx MXene membranes for production of drinking water from seawater. Nature Sustainability 3, 296-302 (2020). https://doi.org/10.1038/s41893-020-0474-0
- [21]Huang, K. et al. Cation-controlled wetting properties of vermiculite membranes and its promise for fouling resistant oil-water separation. Nature Communications 11, 1097 (2020). https://doi.org/ARTN 1097 10.1038/s41467-020-14854-4
- [22]Shao, J.-J., Raidongia, K., Koltonow, A. R. & Huang, J. Self-assembled two-dimensional nanofluidic proton channels with high thermal stability. Nature Communications 6, 7602 (2015). https://doi.org/10.1038/ncomms8602
- [23]Walker, G. F. & Garrett, W. G. Chemical Exfoliation of Vermiculite and the Production of Colloidal Dispersions. Science 156, 385-387 (1967). https://doi.org/doi:10.1126/science.156.3773.385
- [24]Wang, W. et al. 2D Vermiculite Nanolaminated Membranes for Efficient Organic Solvent Nanofiltration. Advanced Functional Materials n/a, 2410635 https://doi.org/10.1002/adfm.202410635
- [25]Nye, P. H. in Advances in Agronomy Vol. 31 (ed N. C. Brady) 225-272 (Academic Press, 1980).
- [26]Madsen, F. T. & Müller-Vonmoos, M. The swelling behaviour of clays. Applied Clay Science 4, 143-156 (1989). https://doi.org/10.1016/0169-1317(89)90005-7
- [27]Lee, S. S., Fenter, P., Nagy, K. L. & Sturchio, N. C. Real-time observation of cation exchange kinetics and dynamics at the muscovite-water interface. Nature Communications 8, 15826 (2017). https://doi.org/10.1038/ncomms15826
- [28]Zou, Y. C. et al. Ion exchange in atomically thin clays and micas. Nat Mater 20, 1677-1682 (2021). https://doi.org/10.1038/s41563-021-01072-6
- [29]Mogg, L. et al. Atomically thin micas as proton-conducting membranes. Nat Nanotechnol 14, 962-966 (2019). https://doi.org/10.1038/s41565-019-0536-5
- [30]Claesson, P. M., Herder, P., Stenius, P., Eriksson, J. C. & Pashley, R. M. An ESCA and AES study of ion-exchange on the basal plane of mica. Journal of Colloid and Interface Science 109, 31-39 (1986). https://doi.org/10.1016/0021-9797(86)90278-X
- [31]Liu, X.-D. & Lu, X.-C. A Thermodynamic Understanding of Clay-Swelling Inhibition by Potassium Ions. Angewandte Chemie International Edition 45, 6300-6303 (2006). https://doi.org/10.1002/anie.200601740
- [32]Liu, Y. et al. Pillared Laminar Vermiculite Membranes with Tunable Monovalent and Multivalent Ion Selectivity. Advanced Materials 37, 2417994 (2025). https://doi.org/10.1002/adma.202417994
- [33]Xia, Z. et al. Tunable Ion Transport with Freestanding Vermiculite Membranes. ACS Nano 16, 18266-18273 (2022). https://doi.org/10.1021/acsnano.2c05954
- [34]Liu, Y. et al. Montmorillonite Membranes with Tunable Ion Transport by Controlling Interlayer Spacing. ACS Applied Materials & Interfaces 15, 57144-57152 (2023). https://doi.org/10.1021/acsami.3c13678
- [35]Wang, Y., Lian, T., Tarakina, N. V., Yuan, J. & Antonietti, M. Lamellar carbon nitride membrane for enhanced ion sieving and water desalination. Nature Communications 13, 7339 (2022). https://doi.org/10.1038/s41467-022-35120-9
- [36]Andreeva, D. V. et al. Two-dimensional adaptive membranes with programmable water and ionic channels. Nature Nanotechnology 16, 174-180 (2021). https://doi.org/10.1038/s41565-020-00795-y
- [37]Zhang, C., Wang, X., Jin, J., Li, L. & Miller, J. D. AFM Slip Length Measurements for Water at Selected Phyllosilicate Surfaces. Colloids and Interfaces 5, 44 (2021).DOI
- [38]N.J. Comans, R., Haller, M. & De Preter, P. Sorption of cesium on illite: Non-equilibrium behaviour and reversibility. Geochimica et Cosmochimica Acta 55, 433-440 (1991). https://doi.org/10.1016/0016-7037(91)90002-M
- [39]de Koning, A. & Comans, R. N. J. Reversibility of radiocaesium sorption on illite2 2Associate editor: D. L. Sparks. Geochimica et Cosmochimica Acta 68, 2815-2823 (2004). https://doi.org/10.1016/j.gca.2003.12.025
- [40]Patra, K. et al. Role of Mg2+ and K+ ions in retention of radio-cesium (137Cs+) in vermiculite clay. Journal of Hazardous Materials Advances 13, 100411 (2024). https://doi.org/10.1016/j.hazadv.2024.100411
- [41]Lee, J., Park, S.-M., Jeon, E.-K. & Baek, K. Selective and irreversible adsorption mechanism of cesium on illite. Applied Geochemistry 85, 188-193 (2017). https://doi.org/10.1016/j.apgeochem.2017.05.019
- [42]Wijmans, J. G. & Baker, R. W. The solution-diffusion model: a review. Journal of Membrane Science 107, 1-21 (1995). https://doi.org/10.1016/0376-7388(95)00102-I
- [43]Laio, A. & Torre, V. Physical Origin of Selectivity in Ionic Channels of Biological Membranes. Biophysical Journal 76, 129-148 (1999). https://doi.org/10.1016/S0006-3495(99)77184-5
- [44]Whittaker, M. L., Lammers, L. N., Carrero, S., Gilbert, B. & Banfield, J. F. Ion exchange selectivity in clay is controlled by nanoscale chemical–mechanical coupling. Proceedings of the National Academy of Sciences 116, 22052-22057 (2019). https://doi.org/doi:10.1073/pnas.1908086116
- [45]Suter, J. L., Coveney, P. V., Greenwell, H. C. & Thyeveitil, M.-A. Large-Scale Molecular Dynamics Study of Montmorillonite Clay: Emergence of Undulatory Fluctuations and Determination of Material Properties. The Journal of Physical Chemistry C 111, 8248-8259 (2007). https://doi.org/10.1021/jp070294b
- [46]Marcus, Y. Effect of Ions on the Structure of Water: Structure Making and Breaking. Chemical Reviews 109, 1346-1370 (2009). https://doi.org/10.1021/cr8003828
- [47]Israelachvili, J. N. in Intermolecular and Surface Forces (Third Edition) (ed Jacob N. Israelachvili) 291-340 (Academic Press, 2011).
- [48]Jenkins, H. D. B. & Marcus, Y. Viscosity B-Coefficients of Ions in Solution. Chemical Reviews 95, 2695-2724 (1995). https://doi.org/10.1021/cr00040a004
- [49]Fukuma, T., Ueda, Y., Yoshioka, S. & Asakawa, H. Atomic-Scale Distribution of Water Molecules at the Mica-Water Interface Visualized by Three-Dimensional Scanning Force Microscopy. Physical Review Letters 104, 016101 (2010). https://doi.org/10.1103/PhysRevLett.104.016101
- [50]Marcus, Y. in Ions in Solution and their Solvation 107-155 (Wiley, 2015).DOI
- [52]Bard, A. J. & Faulkner, L. R. Electrochemical methods : fundamentals and applications / Allen J. Bard, Larry R. Faulkner, Department of Chemistry and Biochemistry, University of Texas at Austin. Second edition. edn, (John Wiley & Sons, Inc., 2001).
- [53]Lee, S. S., Fenter, P., Nagy, K. L. & Sturchio, N. C. Changes in adsorption free energy and speciation during competitive adsorption between monovalent cations at the muscovite (001)-water interface. Geochimica et Cosmochimica Acta 123, 416-426 (2013). https://doi.org/10.1016/j.gca.2013.07.033
- [54]Yang, S. et al. Competitive Adsorption of Metal Ions at Smectite/Water Interfaces: Mechanistic Aspects, and Impacts of Co-Ions, Charge Densities, and Charge Locations. The Journal of Physical Chemistry C 124, 1500-1510 (2020). https://doi.org/10.1021/acs.jpcc.9b10341
- [55]Chen, B. & Evans, J. R. G. Elastic moduli of clay platelets. Scripta Materialia 54, 1581-1585 (2006). https://doi.org/10.1016/j.scriptamat.2006.01.018
- [56]Suk, J. W., Piner, R. D., An, J. & Ruoff, R. S. Evaluation of elastic modulus of ultra-thin vermiculite membranes by contact mode atomic force microscopy imaging. Thin Solid Films 527, 205-209 (2013). https://doi.org/10.1016/j.tsf.2012.12.024