betaFeedback

WorksPhysics and Astronomy

Boron-related defects in n-type 4H-SiC Schottky barrier diodes

Abstract

We report on boron-related defects in the low-doped n-type (nitrogen-doped) 4H-SiC semitransparent Schottky barrier diodes (SBDs) studied by minority carrier transient spectroscopy (MCTS). An unknown concentration of boron was introduced during chemical vapor deposition (CVD) crystal growth. Boron incorporation was found to lead to the appearance of at least two boron-related deep-level defects, namely, shallow (B) and deep boron (D-center), with concentrations as high as 2 x 1015 cm-3. Even though the boron concentration exceeded the nitrogen doping concentration by almost an order of magnitude, the steady-state electrical characteristics of the n-type 4H-SiC SBDs did not deteriorate.

The earliest experimental studies of boron-related deep-level defects in SiC using deep-level transient spectroscopy (DLTS) date back to the 1980s. The pioneering work was made by Anikin et al.^{1} on boron-doped 6H6H-SiC p+np^+n diodes. They not only reported the peak labeled as the D-center but also indicated that the D-center consists of two overlapping peaks with activation energies for hole emission of Ev+0.63E_\mathrm{v} + 0.63 eV and Ev+0.73E_\mathrm{v} + 0.73 eV. This result was recently confirmed experimentally using the Laplace minority carrier transient spectroscopy (Laplace-MCTS). [2] Capan et al.^{2} provided direct evidence that the D-center consists of two components (i.e. emission lines), and labeled these as D1 and D2, respectively. The estimated activation energies for hole emission are Ev+0.49E_\mathrm{v} + 0.49 eV and Ev+0.57E_\mathrm{v} + 0.57 eV. They are assigned to the deep boron (isolated boron sitting at the C site) (-h and -k site, respectively). The intensity ratio D1:D2 is approximately 1:1, indicating that the BC_\mathrm{C}(h) and BC_\mathrm{C}(k) sites are equally occupied.

Suttrop et al.^{3} have made significant progress in understanding boron-related defects, as it became evident that boron introduces two electrically active deep-level defects into SiC material. In their study, they used 6H6H-SiC grown by a liquid phase epitaxy (LPE) process. Boron was introduced either by ion implantation or during the LPE process from a B-doped silicon melt, and this time two electrically active deep-level defects were detected. The shallow boron at Ev+0.30E_\mathrm{v} + 0.30 eV, and, already known, deep boron (D-center) at Ev+0.58E_\mathrm{v} + 0.58 eV.

Together with aluminum, boron is the most common p-type dopant in SiC. However, unintentional incorporation of boron can occur during crystal growth. This incorporation has been previously reported and explained by the presence of boron in the graphite susceptor used for CVD growth. [4, 5, 6] The concentration of unintentionally incorporated boron can reach more than 101310^{13} cm−3\mathrm{cm}^{-3} yielding the appearance of boron-related deep levels in the lower part of the bandgap. [2, 6] This problem was studied by Storasta et al. [7] They applied MCTS to check the influence of unintentional boron incorporation during growth in low-doped n-type 4H4H-SiC\mathrm{SiC}. The SiC material was grown by hot-wall chemical vapor deposition (CVD). Their results also confirmed previous findings that boron introduces two deep levels, shallow (B) and deep boron (D-center) with activation energies of Ev+0.27E_{\mathrm{v}} + 0.27 and Ev+0.67E_{\mathrm{v}} + 0.67 eV, respectively. Moreover, they concluded that residual boron strongly affects the properties of SiC material grown by the CVD method. Boron-related defects act as hole traps, have large capture-cross sections, and significantly reduce the minority carrier lifetime.

In this work, we have performed electrical characterization employing temperature-dependent current-voltage (II-VV), capacitance-voltage (CC-VV), DLTS, and MCTS measurements to verify the effect of unintentionally incorporated boron on the steady-state electrical performance of n-type 4H4H-SiC\mathrm{SiC} semitransparent Schottky barrier diodes. One of the main goals of this work is to show how MCTS can be utilized in the study of boron-related deep-level defects in n-type 4H4H-SiC\mathrm{SiC} materials.

Schottky barrier diodes (SBDs) were fabricated on nitrogen-doped (∼3×1014\sim3 \times10^{14} cm−3\mathrm{cm}^{-3}) 4H4H-SiC\mathrm{SiC} epitaxial layers with a thickness of approximately 25 μ\mum. The n-type epi-layer was grown on an 8° off-cut silicon face of a 350 μ\mum thick 4H-SiC (0001) wafer without a buffer layer by CVD. [8] Semitransparent SBDs for MCTS measurements were formed by the evaporation of a thin film of nickel (15 nm) through a metal mask with openings of 2 mm ×\times 2 mm. For wire bonding, a thick nickel film (100 nm) was stacked on one corner of the Ni thin film. The same semitransparent diodes were used for all experimental techniques. No high-temperature annealing was performed before electrical characterization.

The quality of the fabricated semitransparent SBDs was evaluated by temperature-dependent II-VV and CC-VV measurements using a Keithley 4200 SCS (Keithley Instruments, Cleveland, OH, USA). Electrically active defects were characterized by DLTS (electron traps) and MCTS (hole traps). DLTS measurements were performed in the temperature range of 100 to 450 K. The temperature ramp rate was 2 K/min. Capacitance transients were measured using a Boonton (Boonton Electronics, Parsippany, NJ, USA) 7200 capacitance meter using a 30 mV, 1 MHz sinusoidal signal. Voltage settings were reverse bias voltage, VR=−10V_{\mathrm{R}} = -10 V, pulse bias, VP=−0.1V_{\mathrm{P}} = -0.1 V. The pulse duration, tPt_{\mathrm{P}}, was 10 ms. MCTS measurements were carried out using an experimental setup consisting of a Boonton 7200 capacitance meter and NI PCI-6251 DAQ. For optical excitation, a 365 nm LED (Thorlabs M365D2 LED) with a Thorlabs LDC205C LED driver was used. For the depth-profiling measurements, the reverse bias voltage was varied from -10 V to -1 V.

The steady-state electrical properties of the fabricated n-type 4H4H-SiC\mathrm{SiC} SBDs were checked by temperature-dependent II-VV and CC-VV measurements. Figure 1a and Figure 1b show respectively the II-VV and CC-VV characteristics at temperatures from 100 K to 450 K. The ideality factor at 300 K was extracted to a value of ∼\sim1.01. The forward II-VV characteristics at temperatures below 200 K revealed two distinct regions separated by a kink that is attributed to the presence of a Schottky barrier inhomogeneity affected either by surface defects or doping inhomogeneities.[9, 10, 11] At higher temperatures, only the dominant Schottky barrier determined the saturation current, which remained below 50 pA even for a reverse bias voltage of 100 V and at the operating temperature of 450 K. The low leakage current of 4H-SiC SBD indicates the absence of generation-recombination mechanisms, even for a fully depleted epitaxial layer, that could otherwise degrade the electrical performance. Apart from the effect of temperature on series resistance, the CC-VV characteristics measured at 1 MHz and temperatures from 100 K to 450 K show no impact of additional charge carriers on the capacitance.

I-V and C-V characteristics for as-grown n-type 4H-SiC SBD

Figure 1. (a) II-VV and (b) CC-VV characteristics for as-grown n-type 4H-SiC SBD measured at temperatures from 100 K to 450 K.

Figure 2 shows the DLTS spectrum for the as-grown n-type 4H4H-SiC SBD. Only one, slightly asymmetric, peak with a temperature maximum of around 310 K is observed. The peak, labeled as Z1/2Z_{1/2}, was previously assigned to a transition between the double negative and neutral charge states of carbon vacancy VCV_\mathrm{C} (=/0).[12] Additionally, this asymmetric DLTS peak was resolved into two components, Z1Z_1(=/0) and Z2Z_2(=/0), using the high-resolution Laplace DLTS measurements, which were assigned to carbon vacancies residing on two different lattice sites with local cubic (-k) and hexagonal (-h) symmetry, respectively.[13, 14] Carbon vacancy is often labeled as a “lifetime killer” due to its detrimental effect on carrier lifetime[15] and it is one of the most studied and dominant defects in 4H4H-SiC material. The activation energy for electron emission was estimated from the Arrhenius plot as EcE_\mathrm{c} - 0.65 eV. We also estimated the Z1/2Z_{1/2} concentration to be 3×1012 cm−33 \times10^{12}\ \mathrm{cm}^{-3}. The obtained value is compatible with all previously published results for the low-doped n-type 4H4H-SiC SBDs.[13, 14, 16, 17]

DLTS spectrum for as-grown n-type 4H-SiC SBD

Figure 2. DLTS spectrum for as-grown n-type 4H-SiC SBD. Measurement settings were VRV_{\mathrm{R}} = -10 V, VPV_{\mathrm{P}} = -0.1 V, and tPt_{\mathrm{P}} = 10 ms.

Since the unknown boron concentration was incorporated into the SiC material during CVD growth, there was a need for an experimental technique that will enable us to study the lower part of the bandgap, i.e., to study the minority carrier traps. It is worth noting that minority carrier traps are studied to a smaller extent compared to majority carrier traps in SiC, even though they could play an even more notable role as “lifetime-killers” than the widely known Vc.[7, 18]

In this work, we carried out MCTS measurements to investigate the presence of boron in n-type 4H4H-SiC material. Figure 3 shows the MCTS spectrum for as-grown material. The boron concentration was high enough to introduce two known boron-related deep-level defects, labeled as the B and D-center. Together with the B and D-center, two smaller peaks, labeled X and Y, are observed in the MCTS spectrum. The activation energy for hole emission for these defects could not be accurately calculated, but comparison shows that the X resembles the defect recently reported by Fur et al.¹⁹. They estimated the activation energy for X as EV+0.195E_\mathrm{V} + 0.195 eV. For Y, the activation energy as well as the origin are still unclear. Further studies are needed to find out if X and Y are boron-related defects or not.

MCTS spectrum showing X, B, Y, and D-center peaks

Figure 3.

Image not extracted

Figure 3 (PDF p. 5). MCTS spectrum for as-grown n-type 4H4H-SiCSiC SBD. Measurement settings were VR=−10V_{\mathrm{R}} = -10 V, and the optical pulse width 10 ms.

From the Arrhenius plots, the activation energies for hole emissions for B and D-center are estimated as EV+0.21E_{\mathrm{V}} + 0.21 and EV+0.60E_{\mathrm{V}} + 0.60 eV, respectively. They are well-known defects and have already been assigned to shallow boron (substitutional boron at the silicon site, BSi\mathrm{B}_{\mathrm{Si}}) and deep boron (substitutional boron at the carbon site, BC\mathrm{B}_{\mathrm{C}}). [2, 7, 18, 20]

The intensity of the B peak is striking (Figure 3), and it is evident that the shallow boron concentration (B) is not only significantly higher compared to deep boron (D-center), but to Z1/2Z_{1/2} (Figure 2) as well. Since shallow boron occupies Si-sites, and deep boron occupies C-sites in the 4H4H-SiCSiC materials, our results show that SiC grew under C-rich growth conditions since many empty Si-sites were available for boron. [21]

We conducted depth profiling measurements using the CC-VV and MCTS to acquire additional information on boron incorporation and distribution. Figure 4 shows concentration profiles as a function of depth for B and D-center, as well as the free carrier concentration profile.

Depth profiles for B and D-center in n-type 4H-SiC SBD

Figure 4. Depth profiles for B and D-center in n-type 4H4H-SiCSiC SBD measured by MCTS. The free carrier concentration (nitrogen doping) profile was estimated from CC-VV measurements at room temperature (RT).

The concentration of both, B and D-center is increasing towards the surface. Moreover, the concentration of shallow boron, B, is more than an order of magnitude higher than the concentration of deep boron, D-center. This is consonant with the previously mentioned C-rich CVD growth conditions where boron easily finds empty Si-sites near the surface.

Yang et al.[6] studied the correlation between the introduced boron concentration and the concentration of the D-center using MCTS and secondary-ion mass spectrometry (SIMS) measurements. They found that the ratio between the D-center and the boron concentration is 0.02. If we take this ratio and the estimated concentration of the D-center from Figure 4 as 4.5 ×1013 cm−3\times10^{13}\ \mathrm{cm}^{-3}, we obtain 2.25×1015 cm−32.25 \times10^{15}\ \mathrm{cm}^{-3} as the boron concentration in the SiC material. This is almost an order of magnitude higher than the nitrogen doping concentration (Figure 4), and an order of magnitude higher than the concentration of unintentionally introduced boron during CVD growth, as previously assumed. [2, 4, 6] It is noteworthy that such a high boron concentration did not affect the steady-state electrical properties of the n-type 4H4H-SiC SBDs, as we show in Figure 1.

Another interesting feature is boron diffusion in SiC, which is extremely important from a technological aspect. Most of the available studies agree that the fast diffusion of shallow baron (BSi_{\mathrm{Si}}) is explained by two mechanisms, the interstitial-mediated and the kick-out mechanisms[22]:

BSi↔Bi+VSiBSi+Sii↔Bi\mathrm{B}_{\mathrm{Si}} \leftrightarrow\mathrm{B}_{\mathrm{i}} + \mathrm{V}_{\mathrm{Si}} \\ \mathrm{B}_{\mathrm{Si}} + \mathrm{Si}_{\mathrm{i}} \leftrightarrow\mathrm{B}_{\mathrm{i}}

where BSi_{\mathrm{Si}}, Bi_{\mathrm{i}}, VSi_{\mathrm{Si}}, and Sii_{\mathrm{i}} denote substitutional boron at the Si-site, interstitial boron, silicon vacancy, and silicon interstitial, respectively.

Regarding the deep boron (BC_{\mathrm{C}}), Bockstedte et al.[23] described the preferential formation of deep boron in diffusion tails and suggested that the appearance of deep boron is more favorable compared to shallow boron under nonequilibrium conditions.

From Figure 4, we can also see a slight difference in the slope of measured depth profiles. While the concentration of D-center is more uniformly distributed over the measured volume (4×1013 cm−3<[D]<5×1013 cm−34 \times10^{13}\ \mathrm{cm}^{-3} < [\mathrm{D}] < 5 \times10^{13}\ \mathrm{cm}^{-3}), the concentration of B changes more rapidly (1.2×1015 cm−3<[B]<6×1014 cm−31.2 \times10^{15}\ \mathrm{cm}^{-3} < [\mathrm{B}] < 6 \times10^{14}\ \mathrm{cm}^{-3}). The examined volume is rather limited, and the changes in concentrations are not too significant, therefore we cannot draw definite conclusions. For accurate and complete diffusion analysis, high-temperature (17001700 - 2100 ∘C2100\ ^\circ\mathrm{C}) annealing and SIMS measurements are a prerequisite. However, the observed dependencies in the depth profiles could be tentatively explained by different diffusion mechanisms for shallow boron (BSi_{\mathrm{Si}}) and deep boron (BC_{\mathrm{C}}), as described above.

MCTS measurements provided direct evidence that unintentional boron incorporation during CVD growth has resulted in the appearance of at least two boron-related deep-level defects, shallow boron (B) and deep boron (D-center). These defects have already been assigned to substitutional boron occupying the Si-site (BSi_{\mathrm{Si}}, shallow boron), and the C-site (BC_{\mathrm{C}}, deep boron). The estimated boron concentration (∼2×1015 cm−3\sim2 \times10^{15}\ \mathrm{cm}^{-3}) has exceeded the nitrogen doping concentration (∼3×1014 cm−3\sim3 \times10^{14}\ \mathrm{cm}^{-3}), however, the steady-state electrical performance of the n-type 4H4H-SiC SBDs has been preserved.

Acknowledgement

This work was supported by the North Atlantic Treaty Organization Science for Peace and Security Program through Project No. G5674.

References

  1. [2]2) I. Capan, T. Brodar, Y. Yamazaki, Y. Oki, T. Ohshima, Y. Chiba, Y. Hijikata, L. Snoj, and V. Radulović, Nucl. Instrum. Methods Phys. Res. Sect. B Beam Interact. Mater. Atoms. 478, 224 (2020).
  2. [4]4) F. C. Beyer, C. G Hemmingsson, S. Leone, Y-C. Lin, A. Gällström, A. Henry,E. Janzén, J. Appl. Phys. 110, 123701 (2011).
  3. [5]5) J. Zhang, L. Storasta, J. P. Bergman, N.T. Son, E. Janzén, J Appl Phys 93, 4708 (2003).
  4. [6]6) A. Yang, K. Murata, T. Miyazawa, T. Tawara, and H. Tsuchida, J. Appl. Phys. 126, 055103 (2019).
  5. [7]7) L.Storasta, J.P. Bergman, C.Hallin, and E.Janzen, Mat. Sci. Forum 389-393, 549 (2002).
  6. [8]8) M. Ito, L. Storasta, H. Tsuchida, (2008) Appl. Phys. Express 1, 015001 (2008).
  7. [9]9) V.E. Gora, F.D. Auret, H.T. Danga, S.M. Tunhuyma, C. Nyamhere, E. Igumbor, A. Chawanda, Materials Science and Engineering: B. 247, 114370 (2019).
  8. [10]10) S.K. Mourya, G. Malik, Alisha, B. Kumar, R. Chandra, Materials Science in Semiconductor Processing. 149,106855 (2022).
  9. [11]11) H. J. Im, Y. Ding, J.P. Pelz, W.J. Choyke, Phys. Rev. B. 64, 075310 (2001).
  10. [12]12) N.T. Son, X.T. Trinh, L.S. Løvlie, B.G. Svensson, K. Kawahara, J. Suda, T. Kimoto, T. Umeda, J. Isoya, T. Makino, T. Ohshima, and E. Janzén, Phys. Rev. Lett. 109, 187603 (2012).
  11. [13]13) I. Capan, T. Brodar, Z. Pastuović, R. Siegele, T. Ohshima, S.I. Sato, T. Makino, L. Snoj, V. Radulović, J. Coutinho, V.J.B. Torres, and K. Demmouche, J. Appl. Phys. 123, 161597 (2018).
  12. [14]14) I. Capan, T. Brodar, J. Coutinho, T. Ohshima, V.P. Markevich, and A.R. Peaker, J. Appl. Phys. 124, 245701 (2018).
  13. [15]15) T. Kimoto, K. Danno, J. Suda, Phys. Stat. Sol. (b). 245,1327 (2008).
  14. [16]16) I. Capan, T. Brodar, R. Bernat, Ž. Pastuović, T. Makino, T. Ohshima, J. D. Gouveia, J. Coutinho, J. Appl. Phys. 130, 125703 (2021).
  15. [17]17) T. Knežević, T. Brodar, V. Radulović, L. Snoj, T. Makino, and I. Capan, Appl. Phys. Express 15,101002 (2022).
  16. [18]18) V. J. B. Torres, I. Capan, and J. Coutinho, Phys. Rev. B 106, 224112 (2022).
  17. [20]20) M. Bockstedte, A. Mattausch, O.Pankratov, Mat. Sci. Forum 353–356, 447 (2001).
  18. [21]21) P. Deák, B. Aradi, A. Gali, U. Gerstmann, Phys. Status. Solidi. Basic Res. 235, 139 (2003).
  19. [22]22) K. Ruschenschmidt, H. Bracht, M. Laube, N.A. Stolwijk, G. Pensl, Physica B 308–310, 734 (2001).
  20. [23]23) M. Bockstedte, A. Mattausch, O.Pankratov, Phys. Rev. B 70, 115203 (2004).

Paper details

vlnc:W_yhj53kyy
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 1

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents