betaFeedback

WorksPhysics and Astronomy

Graphical Direct-Writing of Macroscale Domain Structures with Nanoscale Spatial Resolution in Non-Polar-Cut Lithium Niobate on Insulators

Abstract

We reported on a graphical domain engineering technique with the capability to fabricate macroscale domain structures with nanoscale spatial resolution in non-polar-cut lithium niobate thin film on insulators through the biased probe tip of scanning atomic force microscopy. It was found that the domain writing process is asymmetric with respect to the spontaneous polarization Ps even though the tip-induced poling field is mirror-symmetric. Various domain structures, with a dimension larger than millimeters while consisting of nanoscale domain elements and with arbitrary domain-wall inclination angle with respect to Ps, were designed graphically and then written directly into non-polar-cut lithium niobate crystals. As a proof of principle demonstration, periodically poled x-cut lithium niobate thin film on insulators with a period of 600 nm, a depth of 460 nm and a length of ~1 mm was fabricated. This technique could be useful for device applications in integrated optics and opto-electronics and domain-wall nanoelectronics based on lithium niobate on insulator.

Introduction

Lithium niobate (LN) crystal is of excellent electro-optic, pyroelectric, piezoelectric, acousto-optic and nonlinear optical properties, especially with the mature of the fabrication technique of lithium niobate on insulators (LNOI) [2, 3, 4, 5] [1], providing a golden material platform for various ferroelectric, opto-electronic and nonlinear optical applications such as ferroelectric and holographic memories [6, 7, 8], electro-optic modulator [9, 10, 11], optical waveguide and integrated optics [4, 12], and nonlinear optical frequency conversion [13, 14, 15, 16, 17], to just mention a few. The ferroelectric LN crystal is of 180∘180^{\circ} domain structure, and its ferroelectric domain can be inverted and designed to improve the device performance, for example, the nonlinear optical frequency conversion efficiency can be improved through periodically poled LN (PPLN) based on quasi-phase-matching technique [18, 19]. Various domain poling techniques were developed, including the traditional electric field poling technique [20, 21], the light-assisted domain inversion technique [22], the direct laser pulse and electron beam irradiation techniques [23, 24, 25, 26], and the tip-field-induced domain inversion technique via scanning probe microscope [27, 28, 29, 30, 31, 32, 33]. Currently, PPLN with a domain period in micrometers can be easily fabricated in both z-cut and non-polar-cut (x-cut or y-cut) LN crystals. Nanoscale domain structures were also reported in z-cut bulk LN or LNOI, while most of them in bulk LN are surface structures with their size limited by the lateral domain expansion effect during the domain growth [29, 34]. Therefore, up to now, it is still a challenging task to produce PPLN with a sub-micron period in non-polar-cut LN crystals, which is usually required to achieve the parametric interaction of counter-propagating light beams based on quasi-phase-matching technique and to use the largest nonlinear coefficient d33d_{33} of LN crystal with improved nonlinear optical frequency conversion efficiency [35, 36]. Tremendous efforts have been put and several groups have tried to fabricate PPLN with sub-micron periodicity in non-polar-cut LN by employing the in-plane electric field poling technique with a finger poling electrode configuration, however, the quality of the sub-micron PPLN still cannot meet the requirement of practical applications such as nonlinear frequency conversion [15, 37, 38, 39, 40].

More recently, the domain wall of LN was found to be conductive, which makes it also possible for applications in nanoelectronics [41, 42]. The domain-wall conductivity in LN is proportional to 2Pssin⁡θ2P_s\sin\theta, where PsP_s is the spontaneous polarization of LN and θ\theta is the inclination angle of the domain wall with respect to PsP_s [43]. Unfortunately, the domain-wall inclination angle θ\theta was found to be almost impossible to control precisely and was small and less than ∼5∘\sim5^{\circ} in z-cut LN crystals, which puts a serious limitation on the optimization of domain-wall conductivity in LN [44, 45, 46, 47]. Therefore, it is desired to develop a method to fabricate domain walls with large inclination angle θ\theta in a precisely controllable way.

In this paper, we reported on the successful fabrication of high quality PPLN with a sub-micron periodicity and a longitudinal length longer than millimeters in non-polar-cut LNOI by scanning the biased probe tip of atomic force microscope (AFM). Domain structures with arbitrary shape and domain-wall inclination angle, and with the size ranging from tens of nanometers to millimeters or longer, are predicable in a graphical way and can then be written directly into non-polar-cut LNOI through the biased AFM tip. This technique is useful in the precise design of domain structures in LNOI for practical applications in nanoelectronics, integrated optics, nonlinear optical frequency conversion and parametric interaction of counter-propagating beams with high efficiency.

Experimental Results

Figure 1a shows the schematic diagram to fabricate the domain structures in non-polar-cut LNOI with a positively biased AFM tip. In the experiments, we used a x-cut LNOI sample consisting of a 600-nm Mg-doped (5.0 mol.%) x-cut LN thin film, a 2-µm silica and a 500-µm LN substrate bonded to each other in sequence. The spontaneous polarization PsP_s of the x-cut LN thin film was in the surface plane of the x-cut LN and was set to be along the z-axis of the experimental coordinate system, as shown in Figure 1a. The AFM tip with a radius of 30 nm was in contact with the top surface of the x-cut LN thin film, and was loaded with a positive voltage and scanned in the direction parallel to the spontaneous polarization PsP_s of the x-cut LN according to a predesigned graphical map, for example, as that shown in Figure 1b, where the AFM tip was positively biased when scanning in the green regions, while the AFM tip was grounded when scanning in the blue regions. Typical domain stripes were fabricated in x-cut LNOI according to the graphical map shown in Figure 1b, in which the AFM tip voltage was 150 V when scanning in the green regions with a scanning speed of 80 μ\mum/s. The domain stripes were characterized by using piezoresponse force microscopy (PFM, MFP-3D Infinity, Asylum Research, Goleta, CA, USA), and the PFM amplitude and phase images are shown in Figure 1c and Figure 1d, respectively. Figure 1e is the phase distribution profile along the red solid line in Figure 1d. One sees

Image not extracted

Figure 1. (a) Schematic diagram to fabricate domain structures in x-cut LNOI by scanning the positively biased AFM tip along the spontaneous polarization PsP_s, the grey arrows indicate the scanning direction of the AFM tip. (b) The graphical map used to produce domain stripes, where a positive voltage is applied on the scanning AFM tip in the green regions while no voltage is applied on the AFM tip in the blue regions. (c) The PFM amplitude image of the fabricated domain stripes. (d) The PFM phase image of the fabricated domain stripes. (e) The phase distribution profile of the fabricated domain stripes along the red solid line in (d). (f) The PFM phase image of the x-cut LNOI surface when the positively biased AFM tip scanned anti-parallel to the spontaneous polarization PsP_s based on the designed voltage map shown in (b).

that the graphical map in Figure 1b is exactly mapped into the domain stripes in x-cut LNOI. However, we found that the domain stripes could not be written into the x-cut LNOI when the AFM tip was scanning in the direction anti-parallel to the spontaneous polarization PsP_s, and only the small area just in front of the scanning tip at the scanning tail terminal was found to be inverted, as shown in Figure 1f.

Surprisingly, the domain stripes can be written into the x-cut LNOI when the AFM tip was scanning in the direction anti-parallel to the spontaneous polarization PsP_s but applied with a negative voltage, as shown in Figure 2a. The predesigned graphical map is shown in Figure 2b, in which the AFM tip was applied with a negative voltage when scanning in the orange regions, while it was grounded when scanning in the blue regions. Figure 2c and Figure 2d show the PFM amplitude and phase images of the fabricated domain stripes when the AFM tip was applied with a negative voltage of −150 V and scanning with a speed of 80 μ\mum/s according to the graphical map in Figure 2b. The PFM phase distribution profile of the domain stripes along the red solid line in Figure 2d is shown in Figure 2e. Again, one sees that the graphical map in Figure 2b is exactly mapped into the domain stripes in x-cut LNOI. Note that, in contrast to the case with a positively biased AFM tip, in this case the domain stripes could not be written into the x-cut LNOI when the negatively biased AFM tip was scanning in the direction parallel to the spontaneous polarization PsP_s, and only a small part of the domain stripes were written into the x-cut LNOI at the areas just in front of the scanning AFM tip at the scanning tail terminal, as shown in Figure 2f.

Image not extracted

Figure 2. (a) Schematic diagram to fabricate domain structures in x-cut LNOI by scanning the negatively biased AFM tip anti-parallel to the spontaneous polarization PsP_s, the grey arrows indicate the scanning direction of the AFM tip. (b) The graphical map used to produce domain stripes, where a negative voltage is applied on the scanning AFM tip in the orange regions while no voltage is applied on the AFM tip in the blue regions. (c) The PFM amplitude image of the fabricated domain stripes. (d) The PFM phase image of the fabricated domain stripes. (e) The phase distribution profile of the fabricated domain stripes along the red solid line in (d). (f) The PFM phase image of the x-cut LNOI surface when the negatively biased AFM tip scanned parallel to the spontaneous polarization PsP_s based on the designed graphical voltage map shown in (b).

To measure the depth of the inverted domain stripes, one first fabricated the domain stripes by scanning the negatively biased AFM tip in the direction anti-parallel to the spontaneous polarization PsP_s with a −150-150-V voltage and a scanning speed of 8080 μ\mum/s. Then we digged a rectangular groove with a depth of 600 nm across the domain stripes by employing focused ion beam (FIB) etching, so that the +Z-surface and -Z-surface of the domain stripes were exposed to air. The sample was then immersed in the HF acid with a concentration of 42% for 3 hours, and the -Z-surface of the domain stripes was etched much faster than the +Z-surface because of the selective etching property of the LN crystals. The PFM phase image and the AFM height map of the etched domain structures are shown in Figure 3a and Figure 3b. Figure 3c shows the magnified AFM height map around the -Z-surface of the central domain stripe in Figure 3b, and the height profile of the domain structure along the white line in Figure 3c, which is across the etched -Z-surface of the central domain stripe, is shown in Figure 3d, from which the depth of the inverted domain stripe was measured to be ∼460\sim460 nm.

Figure 3. (a) The PFM phase image of the domain stripes fabricated in the x-cut LNOI with a rectangular groove digged by using FIB after a 3-hour HF-acid etching. The red and white arrows represent the polarization direction of the respective domain stripes. (b) The AFM height map of the grooved domain stripes after a 3-hour HF-acid etching, the red and blue vertical lines indicate the location of the +Z- and -Z-surface of the domain stripes, respectively. (c) The magnified AFM height map of the -Z-surface of the central domain stripe in (b). (d) The height profile across the etched -Z-surface of the domain stripe along the white line in (c), the depth of the inverted domain stripe was measured to be 460 nm.

Discussions

One notes that the domain structures can be directly written into the x-cut LNOI when the positively biased AFM tip scans in the direction parallel to PsP_s, or the negatively biased AFM tip scans in the direction anti-parallel to PsP_s, but not the vice versa. The reason is that the lateral in-plane component of the electric field generated by the biased AFM tip is of opposite direction on the two lobe-sides of the AFM tip. Figure 4 shows the numerically simulated distribution of the lateral in-plane parallel component of the electric field generated by the biased AFM tip, in which the lateral in-plane parallel electric field component EzE_z is the electric field component parallel to PsP_s in the x-z or y-z planes. In the simulation, the relative dielectric constant of LN was ϵ11=44\epsilon_{11}=44 and ϵ33=29\epsilon_{33}=29, respectively. The radius of the AFM tip was set to be 30 nm, and the tip was in direct contact with the top surface of the x-cut LNOI. The biased voltage was 150 V for Figure 4a and Figure 4c, and was −150-150 V for Figure 4b and Figure 4d, respectively. The red thin curves in Figure 4 show the location where EzE_z is equal to 4.5 kV/mm, i.e., the contour curves of the coercive field of Mg-doped LN [20]. One sees that the electric field component EzE_z is strong enough to invert the domain polarization around the biased AFM tip, and the depth of the inverted domain can be deeper than 300 nm determined by the contour curves of the coercive field. The experimentally measured depth of the domain stripes is slightly larger than the simulated one determined by the contour curves of the coercive field, this is due to the fact that the domain could grow even when the external electric field is lower than the coercive field, as also observed and confirmed by other groups in LN crystals [32, 33].

Image not extracted

Figure 4. (a) and (c), The spatial distribution of EzE_z in the xx-zz and yy-zz planes, respectively, produced by the positively biased AFM tip with a 150-V voltage. (b) and (d), The spatial distribution of EzE_z in the xx-zz and yy-zz planes, respectively, generated by the negatively biased AFM tip with a −150-V voltage. The red arrows represent the tip-induced electric field component EzE_z. The red solid thin curves in all figures are the contour curves of the coercive field with a value of 4.5 kV/mm for Mg-doped LN crystals.

The mirror-symmetric distribution of EzE_z induced by the biased AFM tip would result in the asymmetric behaviour of the domain inversion induced by the biased AFM tip. This is shown in two aspects. First, the domain structure induced by a stationary biased AFM tip is asymmetric. Second, the domain structure formed by the scanning biased AFM tip is asymmetric, and is dependent on the scanning direction with respect to the spontaneous polarization PsP_s. This could be further confirmed experimentally by the following experiments. For example, one wrote a domain structure in the x-cut LNOI with the biased AFM tip at point A, and then lifted the AFM tip and moved the AFM tip to the next point B, where one wrote another domain structure with the biased AFM tip. In this way, one wrote 5 domain structures in sequence with the biased AFM tip with different neighbouring interval distance of 3 μ\mum and 1 μ\mum, respectively, as shown in Figure 5. One notes that a wedge-like domain structure was formed no matter the AFM tip was positively or negatively biased with a voltage magnitude larger than 65 V, and only the area on one side of the biased AFM tip with its domain polarization anti-parallel to EzE_z was inverted, while the area on the opposite side of the biased AFM tip with its polarization parallel to EzE_z was kept to be unchanged, as shown in Figure 5bFigure 1 and Figure 5eFigure 1. Similar tip-induced wedge-like domain structures were also observed by other groups in non-polar-cut LN crystals [32, 33]. Interestingly, the wedge-like domain structures are also dependent on the neighbouring interval distance and the scanning direction of the biased AFM tip. For example, the wedge-like domain structures are well isolated from each other when the neighbouring interval distance is large enough, irrespective of the polarity and the scanning direction of the biased AFM tip. On the other hand, when the neighbouring interval distance is small enough, it is possible that the wedge-like domain structure written by the biased AFM tip could be partially or totally erased by the subsequently followed domain writing process, as shown in Figure 5bFigure 2, Figure 5bFigure 4, Figure 5eFigure 2 and Figure 5eFigure 4. This is because the formerly inverted domain polarization was switched back by the electric field induced by the subsequent neighbouring biased AFM tip, for example when the tip was moved from point B to point A in Figure 5c or from point A to point B in Figure 5f, due to the fact that the directions of the tip-induced electric field component EzE_z on the two sides of the biased AFM tip are exactly opposite with respect to each other along the zz-axis, as shown in Figure 4. However, the wedge-like domain stripes written by the biased AFM tip in sequence can also be connected one after another and form a long continue domain stripe, as shown in Figure 5bFigure 3 and Figure 5eFigure 3, when the positively biased AFM tip scanning in the direction parallel to PsP_s (see Figure 5a) or the negatively biased AFM tip scanning in the direction anti-parallel to PsP_s (see Figure 5d) with a small enough neighbouring interval distance. In this way, domain stripes as those shown in Figure 1d and Figure 2d can be directly written via the

Image not extracted

Figure 5. (a) and (c). Schematic diagrams to write the domain structures with a positively biased AFM tip scanning in different directions with respect to PsP_s. (b) The PFM amplitude images of the domain structures written with a 150-V biased AFM tip, wherein, (b1) and (b3) represent the cases that the tip scanned in the direction parallel to PsP_s but with different neighbouring interval distance of 3 μm and 1 μm, respectively. (b2) and (b4) show the cases with the tip scanning in the direction anti-parallel to PsP_s but with different neighbouring interval distance of 3 μm and 1 μm, respectively. (d) and (f). Schematic diagrams to write domain structures with a negatively biased AFM tip scanning in different directions with respect to PsP_s. (e) The PFM amplitude images of the domain structures generated with a −150-V biased AFM tip, wherein, (e1) and (e3) represent the cases that the tip scanned in the direction anti-parallel to PsP_s but with different neighbouring interval distance of 3 μm and 1 μm, respectively. (e2) and (e4) show the cases with the tip scanning in the direction parallel to PsP_s but with different neighbouring interval distance of 3 μm and 1 μm, respectively.

biased AFM tip.

With this graphical direct-writing technique, it is capable to design graphically the domain structures and then map onto the non-polar-cut LNOI via the biased AFM tip. Figure 6 shows various domain structures fabricated through this graphical direct-writing technique via the biased AFM tip in a 600-nm thick x-cut LNOI, including PPLNs with domain period in sub-micron and micron scale (Figure 6a and Figure 6b), domain stripes with arbitrary domain-wall inclination angle θ\theta (Figure 6c), head-to-head and tail-to-tail domain walls with an inclination angle θ=90∘\theta= 90^\circ (Figure 6d), and so on. The width of the domain stripes can be down to tens of nanometers (∼70\sim70 nm in our experiments). Figure 6e shows a PPLN with a domain grating period of 600 nm, a domain depth of ∼$460nmandatotallongitudinallengthof\sim\$460 nm and a total longitudinal length of\sim11 mm. Note that the scanning area of the AFM probe tip was limited within a scope of 90 × 90 μm². To fabricate domain structures long enough in the longitudinal dimension, we employed an overlay technique by dividing the whole area into separate divisions, each division with an area reachable by the AFM tip, and then mapping the domain structure into each division in sequence, as shown in Figure 6e and Figure 7. Figure 6f shows the magnified image of the nano-domain gratings in the red box of Figure 6e, which covers around two divisions, showing the good homogeneity of the fabricated sub-micron PPLN. Such non-polar-cut sub-micron PPLNs are essential for parametric interaction of counter-propagating light beams and nonlinear conversion generation of ultraviolet light with the feasibility to use the largest nonlinear coefficient d33d_{33} based on quasi-phase-matching technique. In addition, the capability to fabricate domain walls with arbitrary domain-wall inclination angle in a controllable and designable way also paves the way for applications in domain-wall nanoelectronics based on LNOI [42].

Image not extracted

Figure 6. Various domain structures fabricated in a 600-nm thick Mg-doped (5.0 mol.%) x-cut LNOI via a −150-150-V biased AFM tip with a speed of 80 μ\mum/s scanning in the direction anti-parallel to the spontaneous polarization Ps\mathbf{P}_{s}. (a) The PFM phase image of PPLN with a grating period of 600 nm. (b) The PFM image of PPLN with a grating period of 15 μ\mum. (c) The PFM image of domain stripes arranged on a circle with arbitrary domain-wall inclination angle θ\theta. (d) The PFM image of domain structures with head-to-head and tail-to-tail domain walls of a domain-wall inclination angle θ=90∘\theta= 90^\circ. (e) The scanning electron microscope (SEM) image of PPLN (in the white rectangular box) with a domain period of 600 nm and a longitudinal length of ∼1\sim1 mm. (f) The magnified SEM image of nano-domain gratings of PPLN in the red rectangular box in (e).

Image not extracted

Figure 7. The overlay scheme to fabricate macroscale domain structures with a nanoscale spatial resolution via a biased AFM tip of atomic force microscopy.

Conclusion

In summary, we demonstrated a graphical direct-writing technique of domain structures in non-polar-cut LNOI with a biased AFM tip. We showed the asymmetric behaviour of this domain direct-writing technique, in which the domain can be directly written into the non-polar-cut LNOI when scanning the positively biased AFM tip in the direction parallel to Ps\mathbf{P}_{s} or scanning the negatively biased AFM tip in the direction anti-parallel to Ps\mathbf{P}_{s}, but not the vice versa. The tip voltage can be as low as 65 V. The depth of the inverted domain increases with the increase of the biased voltage, and it reaches ∼460\sim460 nm with a biased voltage of 150 V and a scanning speed of 80 μ\mum/s. Various domain structures, with the size ranging from nanoscale to millimeter-scale and with precisely controllable domain-wall inclination angle, were designed graphically and then mapped precisely into the non-polar-cut LNOI. As a proof of principle demonstration, PPLN with a domain period of 600 nm, a domain depth of 460 nm and a longitudinal length of ∼1\sim1 mm was fabricated in a x-cut Mg-doped (5.0 mol%) LNOI, which shows the possibility to use the largest nonlinear coefficient d33d_{33} in the nonlinear frequency conversion and parametric interaction of counter-propagating light beams based on quasi-phase-matching technique. In addition, domain structures with head-to-head and tail-to-tail domain walls were also fabricated in the same LNOI sample. The capability to fabricate various domain structures with a nanoscale spatial resolution in a designable and controllable way makes this technique useful for device applications in integrated optics and opto-electronics and domain-wall nanoelectronics.

acknowledgement

The authors thank Dr. Xiaojie Wang, Mr. Sanbing Li, Ms Yuchen Zhang and Ms Meili Li from Nankai University for their helpful discussions, and Mr. Wei Wu for the help on the preparation of the FIB-etched samples. This work is supported by the National Key Research and Development Program of China (2019YFA0705000), the National Natural Science Foundation of China (NSFC) (Grant Nos. 12134007, 11774182, 11734009), and the 111 project (B07013).

References

  1. [2]A. Boes, B. Corcoran, L. Chang, J. Bowers, and A. Mitchell, Status and potential of lithium niobate on insulator (LNOI) for photonic integrated circuits, Laser Photonics Rev. 12, 1700256 (2018).DOI
  2. [3]A. Honardoust, K. Abdelmalek, and S. Fathpour, Rejuvenating a versatile photonic material: Thin-film lithium niobate, Laser Photonics Rev. 14, 2000088 (2020).
  3. [4]D. Zhu, L. Shao, M. Yu, R. Cheng, B. Desiatov, C. J. Xin, Y. Hu, J. Holzgrafe, S. Ghosh, A. Shams-Ansari, E. Puma, N. Sinclair, C. Reimer, M. Zhang, and M. Loncar, Integrated photonics on thin-film lithium niobate, Adv. Opt. Photonics 13, 242 (2021).DOI
  4. [5]Y. Jia, L. Wang, and F. Chen, Ion-cut lithium niobate on insulator technology: Recent advances and perspectives, Appl. Phys. Rev. 8, 011307 (2021).DOI
  5. [6]L. Hesselink, S. S. Orlov, A. Liu, A. Akella, D. Lande, and R. R. Reughegar, Photorefractive materials for non-volatile volume holographic data storage, Science 282, 1089 (1998).
  6. [7]A. Q. Jiang, W. P. Geng, P. Lv, J. W. Hong, J. Jiang, C. Wang, X. J. Chai, J. W. Lian, Y. Zhang, R. Huang, D. W. Zhang, J. F. Scott, and C. S. Hwang, Ferroelectric domain wall memory with embedded selector realized in LiNbO₃ single crystals integrated on Si wafers, Nat. Mater. 19, 1188 (2020).DOI
  7. [8]X. Chai, J. Jiang, Q. Zhang, X. Hou, F. Meng, J. Wang, L. Gu, D. W. Zhang, and A. Q. Jiang, Nonvolatile ferroelectric field-effect transistors, Nat. Commun. 11, 2811 (2020).DOI
  8. [9]C. Wang, M. Zhang, X. Chen, M. Bertrand, A. Shams-Ansari, S. Chandrasekhar, P. Winzer, and M. Loncar, Integrated lithium niobate electro-optic modulators operating at cmos-compatible voltages, Nature 562, 101 (2018).DOI
  9. [10]M. He, M. Xu, Y. Ren, J. R. Jian, Y. Xu, S. Gao, S. Sun, X. Wen, L. Zhou, L. Liu, C. Guo, H. Chen, S. Yu, L. Liu, and X. Cai, High-performance hybrid silicon and lithium niobate mach-zehnder modulators for 100 Gbit/s and beyond, Nat. Photon. 13, 359 (2019).DOI
  10. [11]M. Li, J. Ling, Y. He, U. A. Javid, S. Xue, and Q. Lin, Lithium niobate photonic-crystal electro-optic modulator, Nat. Commun. 11, 4123 (2020).
  11. [12]R. Wu, M. Wang, J. Xu, J. Qi, W. Chu, Z. Fang, J. Zhang, J. Zhou, L. Qiao, Z. Chai, J. Lin, and Y. Cheng, Long low-loss-lithium niobate on insulator waveguides with sub-nanometer surface roughness, Nanomaterials (Basel) 8, 910 (2018).DOI
  12. [13]M. Zhang, B. Buscaino, C. Wang, A. Shams-Ansari, C. Reimer, R. Zhu, J. M. Kahn, and M. Loncar, Broadband electro-optic frequency comb generation in a lithium niobate microring resonator, Nature 568, 373 (2019).DOI
  13. [14]J.-Y. Chen, Z.-H. Ma, Y. M. Sua, Z. Li, C. Tang, and Y.-P. Huang, Ultra-efficient frequency conversion in quasi-phase-matched lithium niobate microrings, Optica 6, 1244 (2019).
  14. [15]J. Zhao, C. Ma, M. Rusing, and S. Mookherjea, High quality entangled photon pair generation in periodically poled thin-film lithium niobate waveguides, Phys. Rev. Lett. 124, 163603 (2020).DOI
  15. [16]S. Yuan, Y. Wu, Z. Dang, C. Zeng, X. Qi, G. Guo, X. Ren, and J. Xia, Strongly enhanced second harmonic generation in a thin film lithium niobate heterostructure cavity, Phys. Rev. Lett. 127, 153901 (2021).DOI
  16. [17]Q. Luo, C. Yang, R. Zhang, Z. Hao, D. Zheng, H. Liu, X. Yu, F. Gao, F. Bo, Y. Kong, G. Zhang, and J. Xu, On-chip erbium-doped lithium niobate microring lasers, Opt. Lett. 46, 3275 (2021).
  17. [18]Z. Hao, L. Zhang, A. Gao, W. Mao, X. Lyu, X. Gao, F. Bo, F. Gao, G. Zhang, and J. Xu, Periodically poled lithium niobate whispering gallery mode microcavities on a chip, Sci. China-Phys. Mech. Astron. 61, 114211 (2018).DOI
  18. [19]S. Zhu, Y. Zhu, and N. Ming, Quasi-phase-matched third-harmonic generation in a quasi-periodic optical superlattice, Science 278, 843 (1997).DOI
  19. [20]A. Kuroda, S. Kurimura, and Y. Uesu, Domain inversion in ferroelectric MgO:LiNbO₃ by applying electric fields, Appl. Phys. Lett. 69, 1565 (1996).DOI
  20. [21]K. Mizuuchi, A. Morikawa, T. Sugita, and K. Yamamoto, Electric-field poling in Mg-doped LiNbO₃, J. Appl. Phys. 96, 6585 (2004).DOI
  21. [22]C. L. Sones, M. C. Wengler, C. E. Valdivia, S. Mailis, R. W. Eason, and K. Buse, Light-induced order-of-magnitude decrease in the electric field for domain nucleation in MgO-doped lithium niobate crystals, Appl. Phys. Lett. 86, 212901 (2005).DOI
  22. [23]M. Fujimura, T. Sohmura, and T. Suhara, Fabrication of domain-inverted gratings in MgO:LiNbO₃ by applying voltage under ultraviolet irradiation through photomask at room temperature, Electron. Lett. 39, 719 (2003).DOI
  23. [24]A. C. Muir, C. L. Sones, S. Mailis, R. Eason, T. Jungk, A. Hoffmann, and E. Soergel, Direct-writing of inverted domains in lithium niobate using a continuous wave ultra-violet laser, Opt. Express 16, 2336 (2008).pubmed.ncbi.nlm.nih.gov/18542312
  24. [25]V. Y. Shur, D. S. Chezganov, M. M. Smirnov, D. O. Alikin, M. M. Neradovskiy, and D. K. Kuznetsov, Domain switching by electron beam irradiation of z⁺-polar surface in Mg-doped lithium niobate, Appl. Phys. Lett. 105, 052908 (2014).DOI
  25. [26]L. S. Koshkinach and T. R. Volk, Domain inversion in LiNbO₃ and Zn-doped LiNbO₃ crystals by the electron-beam irradiation of the nonpolar y-surface, Appl. Phys. B 110, 367 (2012).
  26. [27]O. Kolosov, A. Gruverman, J. Hatano, K. Takahashi, and H. Tokumoto, Nanoscale visualization and control of ferroelectric domains by atomic force microscopy, Phys. Rev. Lett. 74, 4309 (1995).pubmed.ncbi.nlm.nih.gov/10058468
  27. [28]M. Abplanalp, J. Fousek, and P. Gunter, Higher order ferroic switching induced by scanning force microscopy, Phys. Rev. Lett. 86, 5799 (2001).pubmed.ncbi.nlm.nih.gov/11415361
  28. [29]G. Rosenman, P. Urenski, A. Agronin, Y. Rosenwaks, and M. Molotskii, Submicron ferroelectric domain structures tailored by high-voltage scanning probe microscopy, Appl. Phys. Lett. 82, 103 (2003).DOI
  29. [30]N. A. Pertsev and A. L. Kholkin, Subsurface nanodomains with in-plane polarization in uniaxial ferroelectrics via scanning force microscopy, Phys. Rev. B 88, 174109 (2013).DOI
  30. [31]R. V. Gaitanudinov, T. R. Volk, and H. H. Zhang, Domain formation and polarization reversal under atomic force microscopy-tip voltages in ion-sliced LiNbO₃ films on SiO₂/LiNbO₃ substrates, Appl. Phys. Lett. 107, 162903 (2015).
  31. [32]D. O. Alikin, A. V. Levlev, A. P. Turygin, A. I. Lobov, S. V. Kalinin, and V. Y. Shur, Tip-induced domain growth on the non-polar cuts of lithium niobate single-crystals, Appl. Phys. Lett. 106, 182902 (2015).
  32. [33]A. Leylev, D. Alikin, A. Morozovska, O. V. Varenyk, E. Eliseev, A. Kholkin, V. Shur, and S. Kalinin, Symmetry breaking and electrical frustration during tip-induced polarization switching in the nonpolar cut of lithium niobate single crystals, ACS NANO 9 1, 769 (2015).
  33. [34]A. Boes, V. Sivan, G. Ren, D. Yudistira, S. Mailis, E. Soergel, and A. Mitchell, Precise, reproducible nano-domain engineering in lithium niobate crystals, Appl. Phys. Lett. 107, 022901 (2015).DOI
  34. [35]S. E. Harris, Proposed backward wave oscillation in the infrared, Appl. Phys. Lett. 9, 114 (1966).DOI
  35. [36]C. Canalias and V. Pasiskivicius, Mirrorless optical parametric oscillator, Nat. Photon. 1, 459 (2007).DOI
  36. [37]L. Gui, H. Hu, M. García-Granda, and W. J. Q. e Sohler, Local periodic poling of ridges and ridge waveguides on x- and y-cut LiNbO3 and its application for second harmonic generation, Opt. Express 17, 3923 (2009).pubmed.ncbi.nlm.nih.gov/19259233
  37. [38]P. Mackwitz, M. Rüsing, G. Berth, A. Widhalm, K. Müller, and A. Zrenner, Periodic domain inversion in x-cut single-crystal lithium niobate thin film, Appl. Phys. Lett. 108, 152902 (2016).DOI
  38. [39]B. J. Stanicki, M. Younesi, F. J. F. Löchner, H. Thakur, W.-K. Chang, R. Geiss, F. Setzpfandt, Y.-H. Chen, and T. Pertsch, Surface domain engineering in lithium niobate, OSA Continuum 3, 345 (2020).DOI
  39. [40]J. Zhao, M. Rüsing, M. Rooper, L. M. Eng, and S. Mookherjea, Poling thin-film x-cut lithium niobate for quasi-phase matching with sub-micrometer periodicity, J. Appl. Phys. 127, 193104 (2020).DOI
  40. [41]M. Schröder, A. Haußmann, A. Thiessen, E. Soergel, T. Woike, and L. M. Eng, Conducting domain walls in lithium niobate single crystals, Adv. Funct. Mater. 22, 3936 (2012).DOI
  41. [42]G. Catalan, J. Seidel, R. Ramesh, and J. F. Scott, Domain wall nanoelectronics, Rev. Mod. Phys. 84, 119 (2012).DOI
  42. [43]E. A. Eliseev, A. N. Morozovska, G. S. Svechnikov, V. Gopalan, and V. Y. Shur, Static conductivity of charged domain walls in uniaxial ferroelectric semiconductors, Phys. Rev. B 83, 235313 (2011).DOI
  43. [44]C. S. Werner, S. J. Herr, K. Buse, B. Sturman, E. Soergel, C. Razzaghi, and I. Breuning, Large and accessible conductivity of charged domain walls in lithium niobate, Sci. Rep. 7, 9862 (2017).DOI
  44. [45]B. Kirbus, C. Godau, L. Wehmeier, H. Beccard, E. Beyreuther, A. Haußmann, and L. M. Eng, Real-time 3D imaging of nanoscale ferroelectric domain wall dynamics in lithium niobate single crystals under electric stimuli: Implications for domain-wall-based nanoelectronic devices, ACS Appl. Nano Mater. 2, 5787 (2019).DOI
  45. [46]C. Godau, T. Kampfe, A. Thiessen, L. M. Eng, and A. Haußmann, Enhancing the domain wall conductivity in lithium niobate single crystals, ACS Nano 11, 4816 (2017).DOI
  46. [47]A. A. Esin, A. R. Akhmatkhanov, and V. Y. Shur, Tilt control of the charged domain walls in lithium niobate, Appl. Phys. Lett. 114, 092901 (2019).DOI

Paper details

vlnc:W_ymcfxv24
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 9

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents