Structural Polymorphism Kinetics Promoted by Charged Oxygen Vacancies in HfO2_2

Abstract

Defects such as oxygen vacancy are widely considered to be critical for the performance of HfO2-based devices, and yet atomistic mechanisms underlying various exotic effects such as wake-up and fluid imprint remain elusive. Here, guided by a lattice-mode-matching criterion, we systematically study the phase transitions between different polymorphs of hafnia under the influences of neutral and positively charged oxygen vacancies by mapping out the minimum energy pathways using a first-principles-based variable-cell nudged elastic band technique. We find that the positively charged oxygen vacancy can substantially promote the transition of various nonpolar phases to the polar phase kinetically, enabled by a transient high-energy tetragonal phase and extreme charge-carrier-inert ferroelectricity of the polar Pca21Pca2_1 phase. The intricate coupling between structural polymorphism kinetics and the charge state of the oxygen vacancy has important implications for the origin of ferroelectricity in HfO2_2-based thin films as well as wake-up, fluid imprint, and inertial switching.

Ferroelectric memory has long been considered as a competitive non-volatile information storage technology because of various merits such as fast switching rate, low power consumption, and high endurance [1, 2, 3]. Conventional perovskite ferroelectrics are not compatible with the modern complementary metal oxide semiconductor (CMOS) technology, severely limiting the scalability [4]. The discovery of ferroelectricity in silicon-doped thin films of hafnium oxide in 2011 [5] quickly made HfO2_2 a leading candidate material for incorporating ferroelectric functionalities into integrated circuits. Thanks to its robust electric dipoles at the nanoscale [6], simple composition, and the CMOS compatibility, HfO2_2-based ferroelectrics have already been implemented in several memory devices [7, 8].

The commercialization of ferroelectric HfO2_2-based devices is mainly hindered by the device reliability issues associated with the profound wake-up effect, strong imprint, and limited endurance [9, 10]. For example, the imprint effect, manifested as the shift of a hysteresis loop along the voltage axis with time, will destabilize one of the polarization states and cause retention loss [11]. It is widely accepted that the polar orthorhombic (PO) Pca21Pca2_1 phase of HfO2_2 is responsible for the ferroelectricity [12, 13, 14, 15, 16], despite being higher in energy than the nonpolar monoclinic (M) P21/cP2_1/c phase. The stabilization of the PO phase in thin films has been attributed to the concerted effects of extrinsic factors such as surface/interface effects of grains [12, 16, 17, 18, 19, 20], clamping stress [21, 22] [23], defects [24–30], and electric fields [22]. The as-prepared HfO2_2-based thin film often contains high volume factions of nonpolar M phase and tetragonal (T) P42/nmcP4_2/nmc phase [26, 31, 32]. The models explaining the performance instability during electrical cycling can be categorized into two groups: (i) defects and their evolution; (2) electric field-induced structural polymorphism that may originate from defects [33]. In this work, we discover an intricate coupling between structural polymorphism kinetics and the charge state of the oxygen vacancy in HfO2_2 that has important implications for the origin of ferroelectricity and several device reliability issues.

We start by emphasizing two unique features of the ferroelectric PO phase of HfO2_2. First, the X2−X_2^- lattice mode characterized by antiparallel xx-displacements of neighboring oxygen atoms (Figure 1a) plays an important role in structural polymorphism of HfO2_2. Though phase transitions between different polymorphs of HfO2_2 have been investigated with density functional theory (DFT) calculations previously [23], the importance of the X2−X_2^- mode matching was not appreciated. There exist multiple pathways connecting two phases depending on the choice of atom-to-atom mapping. We find that an atomic mapping that conserves the sign of the X2−\mathrm{X}_{2}^{-} mode gives a lower enthalpy barrier than a mapping that reverses the X2−\mathrm{X}_{2}^{-} mode. As shown in Figure 1a, the X2−\mathrm{X}_{2}^{-}-sign-conserving pathway of T→\toPO has an enthalpy barrier of 2.5 meV per formula unit (f.u.), much lower than the pathway with the X2−\mathrm{X}_{2}^{-} mode reversed (47.5 meV/f.u.). Recent DFT studies also found that the polarization switching in PO that reverses the X2−\mathrm{X}_{2}^{-} mode needs to overcome a large barrier [34]. The small enthalpy barrier of T→\toPO already hints at the importance of nonopolar-polar structural polymorphism in HfO2_2-based devices.

Schematic illustration of the X₂⁻ mode and polar atomic displacement

Figure 1. (a) Schematic illustration of X2−X_{2}^{-} mode in the tetragonal phase of HfO2_2. The tetragonal unit cell has the long axis along xx. The closer and further Hf atoms are colored in dark and light grey; outward and inward displaced oxygen atoms are colored in blue and red, respectively. The generic phase space coordinate is denoted as λ\lambda. (b) Polar atomic displacement (dzd_z) as a function of charge-carrier concentration for the PO phase of HfO2_2 and tetragonal BaTiO3_3. The insets illustrate the definitions of dzd_z in HfO2_2 and BaTiO3_3.

Another intriguing feature is the extreme charge-carrier-inert ferroelectricity of the PO phase. We compute the polar atomic displacements in ferroelectric tetragonal BaTiO3_3 and the PO phase of HfO2_2 as a function of charge-carrier concentration obtained via the background-charge method [35]. Both hole doping and electron doping quickly suppress the polar displacements in tetragonal BaTiO3_3 [36]. In contrast, the local atomic displacements of polar oxygen atoms in PO are insensitive to charge-carrier doping (Figure 1b). Such feature, likely resulting from the improper nature of ferroelectric HfO2_2 [37], suggests that the PO phase can support a substantial amount of charged defects while maintaining the polar structure. Since the charge injection to and entrapment from defects occur frequently during the electrical cycling, understanding the impacts of charged defects on polymorphism kinetics is expectedly important.

Here, we focus on neutral oxygen vacancy (VO0\mathrm{V}_{\mathrm{O}}^{0}) and doubly positively charged oxygen vacancy (VO2+\mathrm{V}_{\mathrm{O}}^{2+}), as they are known prominent defects in HfO2_2-based thin films [33, 38], particularly at the electrode/HfO2_2 interface [39–41]. Different from several previous DFT studies on oxygen-deficient HfO2_2 where the assumed vacancy concentration reaches a rather high level (up to 12.5 f.u.% [42]), we focus on a relatively low vacancy concentration (3.125 f.u.%). DFT calculations are performed using Vienna Ab initio Simulation Package (VASP) with Perdew-Burke-Ernzerhof (PBE) density functional [43]. Structural parameters of unit cells of hafnia polymorphs are optimized using a plane-wave cutoff of 600 eV, a 4×4×44 \times4 \times4 Monkhorst-Pack kk-point grid for Brillouin zone sampling, an energy convergence threshold of 10−610^{-6} eV, and a force convergence threshold of 10−310^{-3} eV/Å. All possible configurations of a 48-atom supercell with an oxygen vacancy concentration of 3.125 f.u.% are explored to identify the lowest-energy configuration. The minimum energy pathway (MEP) connecting two polymorphs is identified with the variable-cell nudged elastic band (VCNEB) technique implemented in the USPEX code [44–46]. The main difference between conventional NEB and VCNEB is that VCNEB allows lattice constants to change during solid-solid transformations, thus capable of quantifying the intrinsic transition barrier between two phases possessing different lattice constants. It is noted that lattice constants and phase transition barriers predicted with PBE are comparable with values computed with SCAN [47]. More computational details are reported in Supplementary Material (SM)[48] that includes Refs. [11] [23, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68].

We first examine the intrinsic transition barriers in the absence of defects between different phases of HfO2\mathrm{HfO_2} including an “antiferroelectric-like” orthorhombic (AO) PbcaPbca phase and another polar orthorhombic Pmn21Pmn2_1 phase that may form in (111)-oriented Hf0.5Zr0.5O2\mathrm{Hf_{0.5}Zr_{0.5}O_2} thin films [69, 70]. All pathways conserve the sign of the X2−\mathrm{X_2^-} mode (Figure S1 in SM[48]). Taking the lowest-energy M phase as the reference, the energy of T, AO, PO, and Pmn21Pmn2_1 phase is 166, 73, 84, and 143 meV/f.u., respectively. The transitions of T→\toM, T→\toPO, and T→\to Pmn21Pmn2_1 are all kinetically fast with negligible enthalpy barriers (<5< 5 meV/f.u., 2a), indicating the precursor role of the high-temperature T phase [23]. The transition of T→\toAO needs to overcome a large kinetic barrier despite AO being the second most favored phase thermodynamically. The transitions from the polar Pmn21Pmn2_1 phase to M and Pca21Pca2_1 only needs to overcome a small barrier of 28 and 37 meV/f.u., respectively. We suggest that although the emergence of the Pmn21Pmn2_1 phase from the T phase is effortless kinetically, it may quickly evolve to other phases such that its transient presence during crystallization is probably undetectable in experiments.

Transition pathways between polymorphs of HfO2

Figure S1. Transition pathways that conserve the sign of the X2−X^{-}_{2} model. The blue and red colors indicate the oxygen atoms that are outward and inward displaced, respectively.

Phase transitions of Pca21Pca2_1 to other nonpolar phases are all hindered by large barriers. Overall, the formation of the M phase is the most favored process both kinetically and thermodynamically in the absence of extrinsic effects. This explains why the most stable M phase dominates in bulk synthesis. We discover that M→\toPO involves another lattice mode, X5y\mathrm{X_5^y}. It is impossible for the transition pathway to conserve both X5y\mathrm{X_5^y} and X2−\mathrm{X_2^-}, thus making M→\toPO a high-barrier (169 meV/f.u.) process that can not be activated by an electric field alone (see § 3.C in SM[48]). This is inconsistent with experimental observations that a substantial amount of M phase is transformed to the PO phase in the woken-up thin films of HfO2\mathrm{HfO_2} [15] [50, 64]. As we will discuss in below, the presence of charged oxygen vacancies resolves this puzzle.

The oxygen vacancy has long been postulated to be important for the stabilization of the PO phase. Experimentally, a low oxygen content during the deposition favors the formation of T and PO phases whereas a high oxygen content tends to stabilize the M phase [71, 72]. However, DFT calculations suggested that even at a high VO0V_{\mathrm O}^{0} concentration of ≈12.5\approx12.5 f.u.%, the M phase remains much more stable thermodynamically than the PO phase [73]. Rushchanskii et al. proposed that configurations with two-dimensional extended oxygen vacancies tend to transform into the PO phase [42], but the VO0V_{\mathrm O}^{0} concentration in their model reached 12.5 f.u.%, much higher than typical experimental values of 2–3 f.u.% [30, 72]. We further investigate the effects of VO0V_{\mathrm O}^{0} on polymorphism kinetics at a concentration of 3.125 f.u.%. Compared with intrinsic defect-free cases, the presence of VO0V_{\mathrm O}^{0} has little impact on the relative stability, nor does it substantially affect the kinetics of phase transitions (Figure 2b). We conclude that at experimentally relevant concentrations, VO0V_{\mathrm O}^{0} alone cannot explain the strong impacts of O2_2 partial pressures on the ferroelectric properties of HfO2_2-based thin films.

Minimum energy pathways connecting different polymorphs of HfO₂

Figure 2. (a) Minimum energy pathways connecting different polymorphs of HfO₂ obtained with VCNEB. (b) Comparison of transition pathways between M, T, and PO phases at the pristine state (solid lines) and those in the presence of V⁰ₒ at a concentration of 3.125 % (dashed lines). The energy of the M phase is chosen as the energy zero point.

Recently, He et al. reported that the presence of VO2+V_{\mathrm O}^{2+} beyond some critical concentration will make PO more stable than M [67]. At a low VO2+V_{\mathrm O}^{2+} concentration of 3.125 f.u.% studied here, we carefully examine the energetics of different configurations containing VO2+V_{\mathrm O}^{2+} and find that M remains to be most stable thermodynamically (See Table S2 in SM[48]). Interestingly, the relative stability between two representative configurations of the T phase, denoted as Ta_a and Tc_c (Figure 3a), depends sensitively on the charge state of oxygen vacancy. Specifically, Ta_a and Tc_c has the vacancy pair aligned along the long axis aa and the short axis cc, respectively. Such local oxygen vacancy ordering is almost inevitable statistically even at a low vacancy concentration (see § 3.E and experimental evidences in Sec. III of SM[48]). The energies of VO0V_{\mathrm O}^{0}@Ta_a and VO0V_{\mathrm O}^{0}@Tc_c are comparable when the oxygen vacancy is charge neutral, but VO2+V_{\mathrm O}^{2+}@Tc_c becomes rather unstable relative to VO2+V_{\mathrm O}^{2+}@Ta_a after the electron entrapment of VO0→VO2+V_{\mathrm O}^{0} \rightarrow V_{\mathrm O}^{2+}. The strong impact of VO2+V_{\mathrm O}^{2+} on the relative stability is confirmed with both 96-atom and 768-atom supercells (Table S3). We perform a series of calculations to identify and separate the contributions to the change in the relative stability (see § 10 of SM[48]). As shown in Figure 3b, the electronic screening already makes VO2+V_{\mathrm O}^{2+}@Ta_a containing VO2+V_{\mathrm O}^{2+} more stable than VO2+V_{\mathrm O}^{2+}@Tc_c by 0.55 eV. We compute the displacements of all Wannier centers (WCs, roughly viewed as the positions of electrons, Figure S8) after VO0→VO2+V_{\mathrm O}^{0} \rightarrow V_{\mathrm O}^{2+}. The displacements of some WCs in Ta_a are much larger than those in Tc_c, indicating a more substantial electronic charge density redistribution in TaT_a. The most displaced WC in VO2+@TaV_{\mathrm{O}}^{2+}@T_a is of Hf-5p5p character (Figure S9). After incorporating the effects of ionic screening and lattice relaxation, VO2+@TaV_{\mathrm{O}}^{2+}@T_a containing VO2+V_{\mathrm{O}}^{2+} remains more stable than VO2+@TcV_{\mathrm{O}}^{2+}@T_c by 0.53 eV.

Schematics, displacement histograms, transition pathways, and phase transition network

Figure 3. (a) Schematics of two different configurations of T phase containing a pair of VO2+\mathrm{V}_{\mathrm{O}}^{2+}. (b) Histograms of displacements of Wannier centers in Ta\mathrm{T}_{a} and Tc\mathrm{T}_{c} right after the electron entrapment of VO0→VO2+\mathrm{V}_{\mathrm{O}}^{0} \rightarrow\mathrm{V}_{\mathrm{O}}^{2+}. The inset shows different contributions to the change in the relative stability between Ta\mathrm{T}_{a} and Tc\mathrm{T}_{c}. Only the energies of configurations containing the same type of oxygen vacancy are comparable. (c) Transition pathways in the presence of VO2+\mathrm{V}_{\mathrm{O}}^{2+} at a concentration of 3.125%. (d) Phase transition network involving multiple polymorphs of HfO2\mathrm{HfO}_{2} containing VO2+\mathrm{V}_{\mathrm{O}}^{2+}. The color of the arrow scales with the magnitude of the transition barrier (see values in Table S5).

ConfigurationEE
VO0V_{\mathrm{O}}^{0}VO2+V_{\mathrm{O}}^{2+}
TTaT_{\mathrm{a}}152.432.1
TTcT_{\mathrm{c}}151.148.8
Pca21Pca2_{1}POa\mathrm{PO}_{\mathrm{a}}-390.642
Pca21Pca2_{1}POb\mathrm{PO}_{\mathrm{b}}-389.848.3
Pca21Pca2_{1}POc\mathrm{PO}_{\mathrm{c}}-388.835.2
Pca21Pca2_{1}POa\mathrm{PO}_{\mathrm{a}}-472.651.4
Pca21Pca2_{1}POb\mathrm{PO}_{\mathrm{b}}-472.743.8
Pca21Pca2_{1}POc\mathrm{PO}_{\mathrm{c}}-475.157.5
Pmn21Pmn2_{1}POa′\mathrm{PO}'_{\mathrm{a}}-3137.131.6
Pmn21Pmn2_{1}POc′\mathrm{PO}'_{\mathrm{c}}-3138.744.4
Pmn21Pmn2_{1}POa′\mathrm{PO}'_{\mathrm{a}}-4136.431.4
Pmn21Pmn2_{1}POc′\mathrm{PO}'_{\mathrm{c}}-4136.343.3
MMa\mathrm{M}_{\mathrm{a}}-38.60
MMb\mathrm{M}_{\mathrm{b}}-37.72.2
MMc\mathrm{M}_{\mathrm{c}}-38.44.3
MMa\mathrm{M}_{\mathrm{a}}-40.950.8
MMb\mathrm{M}_{\mathrm{b}}-4048.6
MMc\mathrm{M}_{\mathrm{c}}-404.1

Table S2. Energy of oxygen-deficient HfO2\mathrm{HfO}_{2} containing VO0\mathrm{V}_{\mathrm{O}}^{0} and VO2+\mathrm{V}_{\mathrm{O}}^{2+} in meV per formula unit (meV/f.u.) relative to the lowest-energy configuration. Ma\mathrm{M}_{\mathrm{a}}-4 (Mb\mathrm{M}_{\mathrm{b}}-4) is the Mh\mathrm{M}_{h} configuration; POa\mathrm{PO}_{\mathrm{a}}-4 (POc\mathrm{PO}_{\mathrm{c}}-4) is the POh\mathrm{PO}_{h} configuration discussed in the main text and Figure 3d.

SupercellCharge StateEE
Ta\mathrm{T}_{a}Tc\mathrm{T}_{c}Tc\mathrm{T}_{c}-Ta\mathrm{T}_{a}
2×2×22 \times2 \times2VO0V_{\mathrm{O}}^{0}-949.282-949.334-0.0519
VO2+V_{\mathrm{O}}^{2+}-975.887-975.3690.518
4×4×44 \times4 \times4VO0V_{\mathrm{O}}^{0}-7749.796-7749.809-0.0135
VO2+V_{\mathrm{O}}^{2+}-7777.126-7776.6210.505

Table S3. Energies of supercells containing oxygen vacancy pair in the T phase. Energy in eV.

Wannier centers in Ta and Tc structures

Figure S8. Wannier centers represented as gray balls in TaT_a and TcT_c containing VO0\mathrm{V}_{\mathrm{O}}^{0} and VO2+\mathrm{V}_{\mathrm{O}}^{2+}, respectively.

Electronic band structure and projected density of states of V$_{\mathrm{O}}^{2+}$@T$_a$

Figure S9. Electronic band structure of VO2+@Ta\mathrm{V}_{\mathrm{O}}^{2+}@\mathrm{T}_{a} with contributions from the most displaced Wannier center colored according to the colorbar. To improve the clarity, only weights larger than 0.1 are shown. The right panel shows the projected density of states (PDOS).

The MEPs connecting VO2+@TaV_{\mathrm{O}}^{2+}@T_a (VO2+@TcV_{\mathrm{O}}^{2+}@T_c) to the most stable configurations of M and PO phases containing VO2+V_{\mathrm{O}}^{2+} are shown in Figure 3c. We find that VO2+@Tc→VO2+@POV_{\mathrm{O}}^{2+}@T_c \rightarrow V_{\mathrm{O}}^{2+}@\mathrm{PO} with a barrier of 24 meV/f.u. is kinetically favored over VO2+@Tc→VO2+@MV_{\mathrm{O}}^{2+}@T_c \rightarrow V_{\mathrm{O}}^{2+}@\mathrm{M} with a barrier of 54 meV/f.u., while M and PO remain well separated by a large barrier. Therefore, VO2+V_{\mathrm{O}}^{2+} promotes Tc→POT_c \rightarrow\mathrm{PO} but suppresses Tc→MT_c \rightarrow\mathrm{M}. As TaT_a is more difficult to undergo phase transitions (Figure 3c), it also explains why as-prepared thin films of HfO2\mathrm{HfO_2} often exhibit a high volume fraction of nonpolar T phase.

The VO2+V_{\mathrm{O}}^{2+}-promoted nonpolar-polar structural polymorphism, Tc→POT_c \rightarrow\mathrm{PO}, likely plays an important role for the emergence of ferroelectricity. A capping electrode was often required to induce the ferroelectricity in Si-doped HfO2\mathrm{HfO_2} thin films [74, 75]. This could be due to the easy formation of VO2+V_{\mathrm{O}}^{2+} at the metal/HfO2\mathrm{HfO_2} interface as the two electrons of VO0V_{\mathrm{O}}^{0} may fall to the metal Fermi level [39]. Since raising the temperature effectively increases the charge-carrier concentration, we propose that during the high-temperature annealing treatment of thin films, the formation of VO2+V_{\mathrm{O}}^{2+} at the metal/HfO2\mathrm{HfO_2} interface is facilitated such that the occurrence of Tc→POT_c \rightarrow\mathrm{PO} becomes substantial. Recent observations that the light ion bombardment can greatly enhance the ferroelectricity in HfO2\mathrm{HfO_2}-based thin films [62] corroborates the VO2+V_{\mathrm{O}}^{2+}-promoted formation of polar HfO2\mathrm{HfO_2}. The difficulty to obtain the PO phase of HfO2\mathrm{HfO_2} through bulk synthesis may be attributed to the high formation energy of oxygen vacancy in bulk HfO2\mathrm{HfO_2} (6.38 eV) [76]. Moreover, the necessity of VO2+V_{\mathrm{O}}^{2+} for Tc→POT_c \rightarrow\mathrm{PO} is consistent with a large body of experimental data that nearly all cation dopants inducing ferroelectricity in HfO2\mathrm{HfO_2}-based thin films are of pp-type because the substitution of Hf4+\mathrm{Hf}^{4+} with acceptor dopants such as Y3+\mathrm{Y}^{3+} naturally promotes the formation of VO2+V_{\mathrm{O}}^{2+} to maintain charge neutrality. The latest verification of intrinsic ferroelectricity in Y-doped HfO2\mathrm{HfO_2} thin films with a large remnant polarization of 64 μC/cm2\mu\mathrm{C}/\mathrm{cm}^{2} [77] serves as another example supporting our hypothesis. For the same reason, the emergence of ferroelectricity in N-doped HfO2\mathrm{HfO_2} [29] could be arising from VO2+V_{\mathrm{O}}^{2+} that compensates NO−N_{\mathrm{O}}^{-} [78].

The finding that VO2+V_{\mathrm{O}}^{2+} can strongly modulate the relative configurational stability is not unique to the T phase. We discover an oxygen-deficient configuration of M (denoted as Mh\mathrm{M_h}) which is stable with VO0V_{\mathrm{O}}^{0} but becomes highly unstable upon the charge entrapment from VO0V_{\mathrm O}^{0}. It is kinetically feasible for VO2+V_{\mathrm O}^{2+}@Mh_{\mathrm h} to transform to VO2+V_{\mathrm O}^{2+}@Tc_{\mathrm c}/Ta_{\mathrm a} and VO2+V_{\mathrm O}^{2+}@PO (<29< 29 meV/f.u.), highlighting that VO2+V_{\mathrm O}^{2+} can enable a previously forbidden transition of M→\rightarrowPO. We also identify a configuration of PO, denoted as POh_{\mathrm h}, which is destabilized by VO2+V_{\mathrm O}^{2+} and easily transforms to nonpolar T and M phases. Contributions to the destabilization effect of VO2+V_{\mathrm O}^{2+} are separated and quantified for Mh_{\mathrm h} and POh_{\mathrm h}, revealing a subtle competition between the electronic/ionic screening and lattice relaxation (see Sec. IV of SM[48]). The phase transition network involving multiple polymorphs containing VO2+V_{\mathrm O}^{2+} (Figure 3d) reveals that VO2+V_{\mathrm O}^{2+} can enable facile transitions among nopolar M and T phases and the polar PO phase, the kinetic barriers of which are lower than the polarization switching barrier of the PO phase (≈55\approx55 meV/f.u.). We suggest that the charge state of VOV_{\mathrm O} is another tuning knob to modulate the stabilities among competing phases in addition to epitaxial strain and electric boundary condition in modern thin-film technology [79].

The intricate coupling between VO2+V_{\mathrm O}^{2+} and structural polymorphism kinetics could contribute to performance instability issues including wake-up and imprint. In a pristine HfO2_2-based capacitor at room temperatures, VO0V_{\mathrm O}^{0} is the dominant type of oxygen vacancy, as supported by recent DFT calculations [80] and experiments [40]. Therefore, VO0V_{\mathrm O}^{0} may distribute at the metal-ferroelectric interface in the matrix of M, T, and PO phases (Figure 4a). Upon the application of a voltage, electrons of VO0V_{\mathrm O}^{0} tend to detrap to the adjacent electrode (top electrode in Figure 4b), leading to the formation of VO2+V_{\mathrm O}^{2+} and the activation of Mh→_{\mathrm h}\rightarrowPO and Tc→_{\mathrm c}\rightarrowPO (Figure 4c). The diffusion of VO2+V_{\mathrm O}^{2+}, recently observed in experiments [68], further helps the nonpolar-polar phase transitions in regions away from the electrode. Similar processes will occur near another electrode after reversing the bias. The overall result is a reduction of M and T and an increase of PO after field cycling, leading to the wake-up effect [64].

Schematics of wake-up and inertial switching enabled by V_O^{2+}-promoted nonpolar-polar structural polymorphisms

Figure 4. Schematics of wake-up and inertial switching enabled by VO2+V_{\mathrm{O}}^{2+}-promoted nonpolar-polar structural polymorphisms. Oxygen vacancies in the right schematics are not shown in (c) and (d) for clarity.

Finally, Mh→_{\mathrm h}\rightarrowPO and Tc→_{\mathrm c}\rightarrowPO to some extent explains “fluid imprint” in ferroelectric La-doped HfO2_2 capacitors where the imprint is easily changeable and has a strong dependence on the switching prehistory [11]. As illustrated in Figure 4d, after the application of a preset pulse that polarize an woken-up capacitor (that still has residual nonpolar phases), the electron entrapment occurs more easily near the negative bound charge side. The presence of VO2+V_{\mathrm O}^{2+} creates a local electric field that aligns with the bulk polarization, a probable source of imprint field (EiE_{\mathrm i}). Even in the absence of additional bias, the VO2+V_{\mathrm O}^{2+}-promoted nonpolar-polar phase transitions, due to their low kinetic barriers (<29< 29 meV/f.u.), could still occur driven by EiE_i, leading to continued polarization switching toward the same direction as the previously applied field, a feature of “inertial switching” [11]. The fluid imprint is associated with an evolving microstructure with a changing volume fraction of the PO phase.

In summary, the robust ferroelectricity of the Pca21Pca2_1 phase against charge doping highlights the necessity of understanding the effects of charged defects on the ferroelectric properties of HfO2_2-based devices. Our DFT calculations suggest that the positively charged oxygen vacancy can drastically modulate the relative configurational stability of the same phase. The VO2+V_\mathrm{O}^{2+}-promoted nonpolar-polar structural polymorphism is probably an overlooked yet important mechanism for the emergence of polar Pca21Pca2_1 phase in HfO2_2-based thin films, offering a new perspective to experimentally observed electrode and doping effects. Generic mechanisms based on the coupling between VO2+V_\mathrm{O}^{2+} and structural polymorphism kinetics are proposed to explain performance instability issues. To fully understand the wake-up and imprint effects, continued experimental and theoretical efforts are needed. Future studies focusing on the coupling between structural polymorphism kinetics and other extrinsic effects such as strain and direct experimental characterizations of these mechanisms are important for comprehending this complicated ferroelectric compound.

Acknowledgments

L.M. and S.L. acknowledge the supports from National Key R&D Program of China (2021YFA1202100), National Natural Science Foundation of China (12074319), and Westlake Education Foundation. The computational resource is provided by Westlake HPC Center. We thank Dr. Yichun Zhou and Jiangheng Yang for useful discussions inspired by which we discovered the importance of the X2−X_2^- mode for phase transitions.

Supplemental Material: Structural Polymorphism Kinetics Promoted by Charged Oxygen Vacancies in HfO2_2

Li-Yang Ma; Shi Liu

HAFNIA POLYMORPHS IN THE PRESENCE OF OXYGEN VACANCIES

Hafnia Polymorphs

The most stable phase of HfO2\mathrm{HfO_2} in bulk at ambient conditions is the monoclinic (M) P21/c\mathrm{P2_1/c} phase. With increasing temperature, the tetragonal (T) P42/nmc\mathrm{P4_2/nmc} phase and the cubic Fm3ˉm\mathrm{Fm\bar{3}m} phase will appear sequentially. At a higher pressure (>10>10 GPa), HfO2\mathrm{HfO_2} transforms to the “antiferroelectric-like” orthorhombic (AO) Pbca\mathrm{Pbca} phase. All these phases are centrosymmetric. The non-centrosymmetric orthorhombic phase of HfO2\mathrm{HfO_2} may adopt two polar space groups, Pca21\mathrm{Pca2_1} and Pnm21\mathrm{Pnm2_1} (denoted as PO and PO′). The Pca21\mathrm{Pca2_1} phase has the polarization aligned along [100][100] while the Pnm21\mathrm{Pnm2_1} phase has the polarization pointing along [110][110]. The optimized lattice constants and relative energies are reported in Table S1.

aabbccEE
T5.2255.0745.074166.3
Pca21\mathrm{Pca2_1}5.2665.0465.07784.3
Pmn21\mathrm{Pmn2_1}5.1835.1175.117142.9
AO10.4695.0735.07472.9
M5.3265.1375.1880

Table S1. Lattice parameters in Å and relative energies in meV per unit cell (meV/f.u.) in reference to the M phase.

Intrinsic phase transition conserving the sign of X2−X^{-}_{2}

In FIG. S1, we illustrate the phase transition pathways between different polymorphs of HfO2_2. The sign of the X2−X^{-}_{2} mode is maintained during the phase transition. The blue and red colors indicate the oxygen atoms that are outward and inward displaced, respectively. Each path is constructed by at least 20 images. When the root-mean-square forces are lower than 0.03 eV/A˚\mathrm{eV}/\mathring{\mathrm{A}} on images, VCNEB calculations are considered converged.

X2−X_{2}^{-} and X5yX_{5}^{y} modes during the transition of M→\toPO

As shown in Figure S2, the X2−X_{2}^{-} lattice mode is characterized by antiparallel xx-displacements of neighboring oxygen atoms in the yzyz plane. We explained in the main text that a transition pathway that conserves the sign of the X2−X_{2}^{-} mode has a lower enthalpy barrier than a pathway that reverses the X2−X_{2}^{-} mode. Interestingly, the transition of M→\toPO involves another lattice mode, X5yX_{5}^{y}, that is characterized by antiparallel xx-displacements of Hf atoms and yy-displacements of oxygen atoms (Figure S2). We find that it is impossible to conserve both X2−X_{2}^{-} and X5yX_{5}^{y} modes during the transition of M→\toPO, as sketched in Figure S2. The pathway that conserves the displacement pattern of the X5yX_{5}^{y} mode fails to match the X2−X_{2}^{-} mode; another pathway conserves the X2−X_{2}^{-} mode but mismatches the X5yX_{5}^{y} mode. Consequently, both pathways possess large kinetic barriers of 169 and 196 meV/f.u., respectively.

Schematic illustrations of the $X^{-}_{2}$ and $X^{y}_{5}$ modes and transition pathways

Figure S2. (a) Schematic illustration of the X2−X^{-}_{2} mode in the tetragonal phase of HfO2_{2}. The tetragonal unit cell has the long axis along xx. The closer and further Hf atoms are colored in dark and light grey; outward and inward displaced oxygen atoms are colored in blue and red, respectively. (b) Schematic illustration of the X5yX^{y}_{5} mode. Viewing along the xx-direction, the hafnium atoms along zz alternately displace inward and outward. (c) Two possible transition pathways of M→\rightarrowPO. One pathway conserves the displacement pattern of the X5yX^{y}_{5} mode but cannot match the X2−X^{-}_{2} mode; another pathway conserves the X2−X^{-}_{2} mode but mismatches the X5yX^{y}_{5} mode. Both pathways need to overcome large kinetic barriers (>160>160 meV/f.u.).

Modeling oxygen-deficient HfO2_2

We remove one oxygen atom from a 2×2×12 \times2 \times1 supercell containing 32 oxygen atoms to model defective HfO2−x_{2-x} with a vacancy concentration of 3.125 f.u.%. For a given phase, there exists multiple oxygen-deficient configurations. The configuration is labeled by two indexes, the oxygen coordination number and the vacancy ordering direction. Take the Pca21Pca2_1 phase (a>c>ba > c > b) as an example. There are six unique configurations for a 2×2×12 \times2 \times1 supercell containing one oxygen vacancy: POa\mathrm{PO}_{a}-3, POb\mathrm{PO}_{b}-3, and POc\mathrm{PO}_{c}-3 that has a threefold-coordinated oxygen removed, and POa\mathrm{PO}_{a}-4, POb\mathrm{PO}_{b}-4, and POc\mathrm{PO}_{c}-4 that has a fourfold-coordinated oxygen removed. The lattice constants and atomic positions are fully optimized. The relative energies of all configurations are reported in Table S2. All files of optimized structures are uploaded to https://github.com/sliutheorygroup/supplementary-material/tree/main/L23.

Schematics of POa-3 and POb-4

Figure S3. Schematics of POa\mathrm{PO}_{a}-3 and POb\mathrm{PO}_{b}-4.

Oxygen vacancy pair in the T phase

We investigated the impact of oxygen vacancy pair on the relative stability between Ta\mathrm{T}_{a} and Tc\mathrm{T}_{c} using supercells of different sizes. The lattice constants are fixed to the ground-state values of the defect-free T phase. The atomic positions are fully relaxed. The structures are shown in Figure S4. As reported in Table S3, once the charge state of the oxygen vacancy becomes +2+2, the Tc\mathrm{T}_{c} phase becomes highly unstable.

Schematics of $T_a$ and $T_c$ modeled with $2 \times 2 \times 2$ and $4 \times 4 \times 4$ supercells

Figure S4. Schematics of TaT_a and TcT_c modeled with a 2×2×22 \times2 \times2 supercell (top) and a 4×4×44 \times4 \times4 supercell (bottom).

We note that the key structural feature of Ta\mathrm{T}_{a} (Tc\mathrm{T}_{c}) is the presence of oxygen vacancies in neighboring unit cells. Statistically, such oxygen vacancy pair is almost inevitable even at a relatively low vacancy concentration (i.e. 3.125% studied in this work). We performed a simple statistical test where a 18×18×1818 \times18 \times18 T-phase supercell has oxygen vacancies randomly distributed. The distributions of oxygen vacancies from multiple tests are illustrated in Figure S5. It is evident that many oxygen vacancy pairs adopt Ta/Tc\mathrm{T}_{a}/\mathrm{T}_{c} ordering locally even at a low concentration of 2.0%.

Oxygen-vacancy distributions in an 18 × 18 × 18 supercell at vacancy concentrations of 3.125% and 2.0%, shown in Tests 1, 2, and 3, with unit cells containing 1 V$_{\mathrm{O}}$ and 2 V$_{\mathrm{O}}$'s, and labels $T_a$ and $T_c$

Figure S5. Oxygen-vacancy distributions in a 18 × 18 × 18 supercell at a vacancy concentration of 3.125% and 2% from three statistical tests. Only one layer of the supercell is shown for a test. The presence of Ta/TcT_a/T_c is inevitable even at a relatively low vacancy concentration.

Structural Polymorphisms in the Presence of Oxygen Vacancies

We explored all possible transition pathways that conserve the sign of the X2−\mathrm{X}_{2}^{-} mode connecting low-energy oxygen-deficient configurations in the presence of VO0\mathrm{V}_{\mathrm{O}}^{0} and VO2+\mathrm{V}_{\mathrm{O}}^{2+}, respectively. The results are reported in Table S4 and Table S5. All converged transition pathways can be found in https://github.com/sliutheorygroup/supplementary-material/tree/main/L23.

Phase transitionVO0\mathrm{V}_{\mathrm{O}}^{0}
forwardreverse
T→PO\mathrm{T}\to\mathrm{PO}Ta→POa−4\mathrm{T}_{a}\to\mathrm{PO}_{a-4}4.484.2
Tc→POc−4\mathrm{T}_{c}\to\mathrm{PO}_{c-4}5.982
T→M\mathrm{T}\to\mathrm{M}Ta→Ma−4\mathrm{T}_{a}\to\mathrm{M}_{a-4}2.7154.4
Tc→Mc−4\mathrm{T}_{c}\to\mathrm{M}_{c-4}5.9157.1
M→PO\mathrm{M}\to\mathrm{PO}Mb−4→POb−4\mathrm{M}_{b-4}\to\mathrm{PO}_{b-4}183.9111

Table S4. Phase transition barriers in the presence of VO0\mathrm{V}_{\mathrm{O}}^{0} in meV per formula unit (meV/f.u.).

Phase transitionVO2+V_{\mathrm{O}}^{2+}
forwardreverse
fate of TTa→Ma\mathrm{T}_{a}\rightarrow\mathrm{M}_{a}-348.381.6
fate of TTa→POc\mathrm{T}_{a}\rightarrow\mathrm{PO}_{c}-350.248.6
fate of TTc→POc\mathrm{T}_{c}\rightarrow\mathrm{PO}_{c}-32439.2
fate of TTc→POb\mathrm{T}_{c}\rightarrow\mathrm{PO}_{b}-418.425.4
fate of TTc→Mc\mathrm{T}_{c}\rightarrow\mathrm{M}_{c}-453.9100
fate of POPOc\mathrm{PO}_{c}-3→Mc\rightarrow\mathrm{M}_{c}-356.787.5
fate of POh\mathrm{PO}_{h}POa\mathrm{PO}_{a}-4→Ta\rightarrow\mathrm{T}_{a}23.140.7
fate of POh\mathrm{PO}_{h}POa\mathrm{PO}_{a}-4→Tc\rightarrow\mathrm{T}_{c}25.125.8
fate of POh\mathrm{PO}_{h}POa\mathrm{PO}_{a}-4→Mb\rightarrow\mathrm{M}_{b}-335.984.9
fate of POh\mathrm{PO}_{h}POa\mathrm{PO}_{a}-4→POc\rightarrow\mathrm{PO}_{c}-374.190.1
fate of POh\mathrm{PO}_{h}POc\mathrm{PO}_{c}-4→POc\rightarrow\mathrm{PO}_{c}-3 (via VO2+V_{\mathrm{O}}^{2+} diffusion)16.138.1
fate of Mh\mathrm{M}_{h}Ma\mathrm{M}_{a}-4→Ta\rightarrow\mathrm{T}_{a}31.147.9
fate of Mh\mathrm{M}_{h}Ma\mathrm{M}_{a}-4→Tc\rightarrow\mathrm{T}_{c}26.726.8
fate of Mh\mathrm{M}_{h}Mb\mathrm{M}_{b}-4→POb\rightarrow\mathrm{PO}_{b}-492.197.4
fate of Mh\mathrm{M}_{h}Mb\mathrm{M}_{b}-4→POc\rightarrow\mathrm{PO}_{c}-329.342.8
fate of Mh\mathrm{M}_{h}Ma\mathrm{M}_{a}-4→Ma\rightarrow\mathrm{M}_{a}-3 (via VO2+V_{\mathrm{O}}^{2+} diffusion)81.3131.4

Table S5. Phase transition barriers in the presence of VO2+V_{\mathrm{O}}^{2+} in meV per formula unit (meV/f.u.). Ma\mathrm{M}_{a}-4 (Mb\mathrm{M}_{b}-4) is the Mh\mathrm{M}_{h} configuration; POa\mathrm{PO}_{a}-4 (POc\mathrm{PO}_{c}-4) is the POh\mathrm{PO}_{h} configuration discussed in the main text. The values colored in blue are used to plot Fig. 3d.

Experiment-Theory Comparison

Even before the discovery of ferroelectricity in HfO2\mathrm{HfO}_{2}-based thin films, nonpolar HfO2−x\mathrm{HfO}_{2-x} has already been actively studied as a promising resistive switching (RS) material for non-volatile resistive random access memory (ReRAM) [1, 2, 3, 4, 5, 6].

The RS mechanism in binary-oxide-based ReRAM has been the subject of numerous of studies [3, 7, 8, 9]. The current consensus is that the ON-OFF resistive switching is governed by the reversible formation and disruption of conducting filaments of chainlike oxygen vacancies, as illustrated in Figure S6. In particular, Kwon et al. used high-resolution transmission electron microscopy to probe directly the nanofilaments in a Pt/TiO2_2/Pt system during RS and confirmed that the switching occurs by the formation and disruption of TinO2n−1\mathrm{Ti}_{n}\mathrm{O}_{2n-1}, a phase with ordered oxygen vacancies [[10]]. These previous studies of the RS mechanism in binary oxides could be viewed as “direct” evidences supporting our proposed TaT_{\mathrm{a}} and TcT_{\mathrm{c}} ordering in HfO2\mathrm{HfO}_{2}.

Experimental evidences supporting various $V_{\mathrm{O}}^{2+}$-dependent mechanisms proposed in this work

Figure S6. Experimental evidences supporting various VO2+V_{\mathrm{O}}^{2+}-dependent mechanisms proposed in this work[10, 11, 12, 13, 14, 15].

Third, as summarized in Figure S6, our proposed generic mechanisms based on the coupling between VO2+V_{\mathrm{O}}^{2+} and structural polymorphism kinetics can well explain a broad range of experimental observations relevant to the origin of ferroelectricity in HfO2\mathrm{HfO}_{2}-based thin films as well as interfacial phase transitions at the metal/HfO2\mathrm{HfO}_{2} interface, wake-up, fluid imprint, and inertial switching. For example, the proposed VO2+V_{\mathrm{O}}^{2+}-promoted nonpolar-polar structural polymorphism explains a very recent observation that the light ion bombardment greatly enhanced the ferroelectricity in HfO2\mathrm{HfO}_{2}-based ferroelectric thin films [11]. These experimental observations in HfO2\mathrm{HfO}_{2}-based thin films could also be viewed as “indirect evidences”.

Destabilization Effects Arising from the Electron Entrapment

A series of calculations are carried out to fully disentangle the destabilization effects arising from the electron entrapment of VO0→VO2+V_{\mathrm{O}}^{0} \to V_{\mathrm{O}}^{2+}. We perform three successive calculations in order to identify and separate the contributions to the change in the relative configurational stability. The first calculation is simply a self-consistent field calculation (i. e., single-point energy calculation) without structural relaxations upon the electron entrapment of VO0→VO2+V_{\mathrm{O}}^{0} \to V_{\mathrm{O}}^{2+}. The change in the relative stability can thus be attributed to the difference in electronic screening. In the second calculation, we relax internal atomic positions with lattice constants fixed. The change in the relative stability is due to varying degrees of ionic screening. Finally, we perform a full structural optimization by relaxing both internal coordinates and lattice parameters, and name this contribution to the stability change as “lattice relaxation”.

The naming scheme used to distinguish different oxygen-deficient configurations is detailed in § 3.D. The configuration is labeled by two indexes, the oxygen coordination number and the vacancy ordering direction. For example, Ma_{a}-3 denotes a configuration of M phase that has threefold-coordinated oxygen atoms removed, resulting in an oxygen vacancy pair aligned along the aa axis.

As shown in Figure S7, in the presence of VO0V_{\mathrm{O}}^{0}, Ma_{a}-4 and Ma_{a}-3 are close in energy with Ma_{a}-4 being slightly more stable. We note that Ma_{a}-4, Mb_{b}-4, and Mc_{c}-4 are close in energy, while Ma_{a}-3, Mb_{b}-3, and Mc_{c}-3 have comparable energies (see values in Table S2 in SM). After the electron entrapment from VO0V_{\mathrm{O}}^{0}, the electronic screening in Ma_{a}-3 is stronger such that Ma_{a}-3 becomes more stable than Ma_{a}-4 (denoted as Mh_{h} with VO2+V_{\mathrm{O}}^{2+} in Figure 3d of the main text) by ≈1.0\approx1.0 eV. The ionic relaxation further stabilize Ma_{a}-3 more than Ma_{a}-4. Eventually, Ma_{a}-4 (Mh_{h}) is higher in energy than the most stable configuration of Ma_{a}-3 by 1.62 eV in the presence of VO2+V_{\mathrm{O}}^{2+}.

Different contributions to the change in the relative stability upon electron entrapment for the M and PO phases

Figure S7. Different contributions to the change in the relative stability upon the electron entrapment of VO0→VO2+V_{\mathrm{O}}^{0} \to V_{\mathrm{O}}^{2+} in (a) M phase and (b) PO phase.

The situation is more complicated for the polar orthorhombic (PO) phase (Figure S7). The lowest-energy configuration with VO0V_{\mathrm{O}}^{0} is POa_{a}-4 while POa_{a}-3 is higher in energy by 0.57 eV; POa_{a}-4 and POc_{c}-4 are close in energy, and POa_{a}-3 and POc_{c}-3 have comparable stability. Right after the electron entrapment of VO0→VO2+V_{\mathrm{O}}^{0} \to V_{\mathrm{O}}^{2+}, the electronic screening in POc_{c}-3 is the strongest, whereas POc_{c}-4 (denoted as POh_{h} with VO2+V_{\mathrm{O}}^{2+} in Figure 3d of the main text) becomes unstable and has an energy higher by ≈1.0\approx1.0 eV, comparable with the energy difference between Ma\mathrm{M}_{\mathrm{a}}-4 and Ma\mathrm{M}_{\mathrm{a}}-3 containing VO2+\mathrm{V}_{\mathrm{O}}^{2+} when only the electronic screening is accounted for.

We find that both the ionic screening and lattice relaxation will reduce the energy difference between POc\mathrm{PO}_{\mathrm{c}}-4 and POc\mathrm{PO}_{\mathrm{c}}-3 to ≈0.7\approx0.7 eV. Therefore, because of the different degrees of ionic screening and lattice relaxation, the destabilization effect of the charged vacancy in the M phase is much more substantial than that in the PO phase.

We projected the band structures onto the Wannier function (WF) corresponding to the most displaced WC after the electron entrapment of VO0→VO2+\mathrm{V}_{\mathrm{O}}^{0} \rightarrow\mathrm{V}_{\mathrm{O}}^{2+} in Ta\mathrm{Ta} (Figure S9, left panel). It turns out the most displaced WC is of Hf-5p5p character based on the computed projected density of states (PDOS, Figure S9, right panel). The inset also compares the change in the position of the most displaced WC (represented as a green ball) before and after the electron entrapment. These results reveal an interesting effect of Hf semicore 5p5p electrons on the electronic screening. We note that despite the nearly identical ionic radii of Zr4+\mathrm{Zr}^{4+} and Hf4+\mathrm{Hf}^{4+}, many experiments highlighted the drastic differences between ZrO2\mathrm{ZrO}_{2} and HfO2\mathrm{HfO}_{2} concerning the easiness of stabilizing the PO phase in HfO2\mathrm{HfO}_{2} but not in ZrO2\mathrm{ZrO}_{2} [16]. Our finding actually hints at the importance of semicore 5p5p electrons of Hf. With that said, to fully resolve this puzzle demands further investigations beyond the scope of current work.

Oxygen Vacancy Migration

As shown in Figure S10, the migration barrier of VO0V_{\mathrm{O}}^{0} hopping to the nearest-neighbor site (≈2.1\approx2.1 eV) is much higher than that of VO2+V_{\mathrm{O}}^{2+} (≈0.4\approx0.4 eV), consistent with previous DFT investigations [17]. This also indicates the reversible oxygen migration in hafnia-based ferroelectric thin films recently observed by the scanning transmission electron microscopy [18] is due to VO2+V_{\mathrm{O}}^{2+}, corroborating our proposed VO2+V_{\mathrm{O}}^{2+}-related mechanisms.

Possible oxygen vacancy migration pathways and minimum energy pathways

Figure S10. (a) Possible oxygen vacancy migration pathways (A and B) that transform Ta\mathrm{T}_a to Tc\mathrm{T}_c. Minimum energy pathways obtained with NEB for (b) single VO0/VO2+\mathrm{V}_{\mathrm{O}}^{0}/\mathrm{V}_{\mathrm{O}}^{2+} hopping to nearest-neighbor sites, (c) VO0\mathrm{V}_{\mathrm{O}}^{0} migration from Ta\mathrm{T}_a to Tc\mathrm{T}_c, and (d) VO2+\mathrm{V}_{\mathrm{O}}^{2+} migration from Ta\mathrm{T}_a to Tc\mathrm{T}_c.

We investigated two possible oxygen-vacancy migration pathways that transform TaT_{\mathrm{a}} to TcT_{\mathrm{c}} (denoted as A and B in Figure S10), and the corresponding minimum energy pathways (MEPs) determined with DFT-based NEB are reported in Figure S10-Figure S10. It is clear that VO2+V_{\mathrm{O}}^{2+} is more mobile than VO0V_{\mathrm{O}}^{0}. A full transformation from TcT_{\mathrm{c}} to TaT_{\mathrm{a}} requires successive oxygen-vacancy hopping, a multistep process that has to overcome multiple barriers. For this reason, we suggest the transition between TaT_{\mathrm{a}} and TcT_{\mathrm{c}} via the VO0/VO2+V_{\mathrm{O}}^{0}/V_{\mathrm{O}}^{2+} diffusion is not likely a major process at room temperatures.

Influence of metal electrodes

We performed additional model calculations to understand the effect of interfacial oxygen vacancies on the structural transition in a T-phase thin film sandwiched by Cu electrodes. The Cu electrode is chosen for its small lattice mismatch (<1.73%<1.73\%) with the T-phase of HfO2_2. As shown in Figure S11, we first optimized the capacitor-like structure without oxygen vacancy. Then we introduced the VO2+V_{\mathrm O}^{2+} pair by removing oxygen atoms close to the interface to create VO2+@TcV_{\mathrm O}^{2+}@T_{\mathrm c} and VO2+@TaV_{\mathrm O}^{2+}@T_{\mathrm a}, and the atomic positions of HfO2_2 were then fully relaxed. Despite the simplicity of our model, we observed a spontaneous transformation of VO2+@Tc→VO2+@POV_{\mathrm O}^{2+}@T_{\mathrm c} \to V_{\mathrm O}^{2+}@\mathrm{PO} with an out-of-plane polarization while VO2+@TaV_{\mathrm O}^{2+}@T_{\mathrm a} is much more stable. All files of optimized structures are uploaded to https://github.com/sliutheorygroup/supplementary-material/tree/main/L23. These additional calculations further corroborate our main conclusion that charged oxygen vacancies close to the metallic electrodes could induce structural polymorphism. Additionally, we report the energy difference between VO2+@TaV_{\mathrm O}^{2+}@T_{\mathrm a} and VO2+@TcV_{\mathrm O}^{2+}@T_{\mathrm c} between the metallic electrodes and the energy difference in bulk in Table S6, showing that the energy difference is reduced between metallic electrodes compared to that in bulk.

EE
VO2+@TaV_{\mathrm O}^{2+}@T_{\mathrm a}VO2+@TcV_{\mathrm O}^{2+}@T_{\mathrm c}VO2+@Tc−VO2+@TaV_{\mathrm O}^{2+}@T_{\mathrm c}-V_{\mathrm O}^{2+}@T_{\mathrm a}
bulk975.887−975.3690.518
between electrodes−1363.1506−1362.81640.334

Table S6. Comparison of energy difference between VO2+@TaV_{\mathrm O}^{2+}@T_{\mathrm a} and VO2+@TcV_{\mathrm O}^{2+}@T_{\mathrm c} between metallic electrodes and in bulk. Energy in eV.

Effects of interfacial oxygen vacancies on the structural transition in a T-phase thin film sandwiched by Cu electrodes. Panel (a): fully optimized Cu/HfO₂/Cu without oxygen vacancy; create interfacial vacancy pair by removing oxygen atoms; fully optimized Cu/HfO₂−x/Cu with oxygen vacancy pair. Panel (b): corresponding configurations with vacancy pair aligned along c.

Figure S11. Effects of interfacial oxygen vacancies on the structural transition in a T-phase thin film sandwiched by Cu electrodes. (a) VO2+V_{\mathrm{O}}^{2+} pair aligned along aa representing VO2+@TaV_{\mathrm{O}}^{2+}@T_a. (b) VO2+V_{\mathrm{O}}^{2+} pair aligned along cc representing VO2+@TcV_{\mathrm{O}}^{2+}@T_c. Some unit cells transform to the PO phase spontaneously after the structural relaxation.

Results Obtained Using SCAN

It is indeed the case that PBE often strongly overestimates the structural distortions for perovskite ferroelectrics. Specifically, PBE substantially overestimates the tetragonality (ξ=c/a\xi= c/a) of PbTiO3_3, predicting a value of 1.20 that is much larger than the experimental value of 1.06. However, many previous DFT investigations (including our work) have shown that PBE can accurately predict the lattice constants of different polymorphs of HfO2_2. We performed a benchmark study using different exchange-correlation (XC) functionals including the more advanced functional such as SCAN. As reported in Table S7, the lattice constants predicted with PBE are comparable with SCAN results and agree with experimental values very well (error < 0.8%).

Phaseaabbcc
TPBE(our work) 5.225 [0.48%]5.074 [0.28%]5.074 [0.28%]
TSCAN 5.179 [0.40%]5.015 [0.89%]5.015 [0.89%]
TLDA 5.08 [2.3%]5.00 [1.19%]5.00 [1.19%]
TExp. 5.205.065.06
POPBE(our work) 5.266 [0.69%]5.046 [0.72%]5.077 [0.34%]
POSCAN 5.208 [0.42%]4.979 [0.62%]5.017 [0.85%]
POLDA 5.18 [0.96%]4.98 [0.60%]5.00 [1.19%]
POExp. 5.2294.9945.059
MPBE(our work) 5.326 [0.19%]5.137 [0.25%]5.188 [0.1%]
MSCAN 5.264 [0.98%]5.000 [2.9%]5.134 [0.95%]
MLDA 5.22 [1.81%]5.05 [1.94%]5.14 [0.83%]
MExp. 5.3165.1505.183

Table S7. Lattice parameters in Å for different phases of HfO2_2 computed with different types of XC functionals. Error relative to the experimental value[19, 20, 21] reported in the square bracket. LDA results taken from [22].

Moreover, as presented in Table S8, PBE and SCAN predict nearly identical energy difference between Ta_a and Tc_c containing oxygen vacancy pair of different charge states: Ta_a and Tc_c containing charge neutral oxygen vacancies, denoted as VO0_{\mathrm{O}}^{0}@Ta_a and VO0_{\mathrm{O}}^{0}@Tc_c, have comparable stability (energy difference within 0.05 eV); Ta_a and Tc_c containing charged oxygen vacancies, denoted as VO2+_{\mathrm{O}}^{2+}@Ta_a and VO2+_{\mathrm{O}}^{2+}@Tc_c, have drastically different stabilities with VO2+_{\mathrm{O}}^{2+}@Ta_a being much lower in energy than VO2+_{\mathrm{O}}^{2+}@Tc_c by at least 0.5 eV.

Charge stateEE
TaT_{\mathrm{a}}TcT_{\mathrm{c}}Tc−TaT_{\mathrm{c}}-T_{\mathrm{a}}
PBEVO0V_{\mathrm{O}}^{0}−949.282−949.334−0.0519
PBEVO2+V_{\mathrm{O}}^{2+}−975.887−975.3690.518
SCANVO0V_{\mathrm{O}}^{0}−2748.1654−2748.1964−0.031
SCANVO2+V_{\mathrm{O}}^{2+}−2376.2376−2775.63910.598

Table S8. Energies of 2×2×2 supercells containing oxygen vacancy pair in the T phase. Energy in eV.

Finally, we also identified the minimum energy pathways (MEPs) for several representative phase transitions using SCAN with the values of energy barriers reported in Table S9. Figure. Figure S12 compares the MEPs determined with PBE and SCAN. It is evident that PBE and SCAN predict the same energetic ordering for M, PO, and T phases and similar magnitudes of energy barriers for phase transitions. In particular, the suppression of Tc→M_c \to\mathrm{M} in the presence of VO2+_{\mathrm{O}}^{2+} is more pronounced in SCAN. These additional calculations demonstrate that the key mechanisms proposed in this work are quite robust.

Phase transitionΔE\Delta E
PBESCAN
VO0\mathrm{V}_{\mathrm{O}}^{0}Tc→Mc-4T_{\mathrm{c}}\to M_{\mathrm{c}\text{-}4}5.97.9
Tc→POc-3T_{\mathrm{c}}\to\mathrm{PO}_{\mathrm{c}\text{-}3}5.96.4
VO2+\mathrm{V}_{\mathrm{O}}^{2+}Tc→Mc-4T_{\mathrm{c}}\to M_{\mathrm{c}\text{-}4}53.961.8
Tc→POc-3T_{\mathrm{c}}\to\mathrm{PO}_{\mathrm{c}\text{-}3}2424.9

Table S9. Phase transition barriers (ΔE\Delta E) in meV per formula unit (meV/f.u.).

Comparison of minimum energy pathways for phase transitions between M, T, and PO phases in the presence of neutral and doubly charged oxygen vacancies

Figure S12. Comparison of minimum energy pathways identified with PBE and SCAN for phase transitions between M, T, and PO phases in the presence of (a) VO0\mathrm{V}_{\mathrm{O}}^{0} and (b) VO2+\mathrm{V}_{\mathrm{O}}^{2+} at a concentration of 3.125 %. The energy of the M phase is chosen as the zero energy point.

References

  1. [1]R.-C. Fang, Q.-Q. Sun, P. Zhou, W. Yang, P.-F. Wang, and D. W. Zhang, High-performance bilayer flexible resistive random access memory based on low-temperature thermal atomic layer deposition, Nanoscale Res Lett 8, 92 (2013).DOI
  2. [2]C. Quinteros, R. Zazpe, F. G. Marlasca, F. Golmar, F. Casanova, P. Stoliar, L. Hueso, and P. Levy, HfO₂ based memory devices with rectifying capabilities, Journal of Applied Physics 115, 024501 (2014).DOI
  3. [3]D. Duncan, B. Magyarı-Kope, and Y. Nishi, Filament-induced anisotropic oxygen vacancy diffusion and charge trapping effects in hafnium oxide RRAM, IEEE Electron Device Lett. 37, 400 (2016).DOI
  4. [4]Y. Hou, U. Celano, L. Goux, L. Liu, A. Fantini, R. Degraeve, A. Youssef, Z. Xu, Y. Cheng, J. Kang, M. Jurczak, and W. Vandervorst, Sub-10 nm low current resistive switching behavior in hafnium oxide stack, Appl. Phys. Lett. 108, 123106 (2016).DOI
  5. [5]A. K. Singh, S. Blonkowski, and M. Kogelschatz, Resistive switching study in HfO₂ based resistive memories by conductive atomic force microscopy in vacuum, Journal of Applied Physics 124, 014501 (2018).DOI
  6. [6]V. Antad, P. A. Shaikh, A. Biswas, S. S. Rajput, S. Deo, M. V. Shelke, S. Patil, and S. Ogale, Resistive switching in HfO₂−x/La₀.₆₇Sr₀.₃₃MnO₃ heterostructures: An intriguing case of low h-field susceptibility of an e-field controlled active interface, ACS Appl. Mater. Interfaces 13, 54133 (2021).
  7. [7]S. Clima, Y. Y. Chen, R. Degraeve, M. Mees, K. Sankaran, B. Govoreanu, M. Jurczak, S. D. Gendt, and G. Pourtois, First-principles simulation of oxygen diffusion in HfOₓ: Role in the resistive switching mechanism, Appl. Phys. Lett. 100, 133102 (2012).DOI
  8. [8]K. Kamiya, M. Y. Yang, T. Nagata, S.-G. Park, B. Magyari-Köpe, T. Chikyow, K. Yamada, M. Niwa, Y. Nishi, and K. Shiraishi, Generalized mechanism of the resistance switching in binary-oxide-based resistive random-access memories, Phys. Rev. B 87, 155201 (2013).DOI
  9. [9]S. Dirkmann, J. Kaiser, C. Wenger, and T. Mussenbrock, Filament growth and resistive switching in hafnium oxide memristive devices, ACS Appl. Mater. Interfaces 10, 14857 (2018).DOI
  10. [10]D.-H. Kwon, K. M. Kim, J. H. Jang, J. M. Jeon, M. H. Lee, G. H. Kim, X.-S. Li, G.-S. Park, B. Lee, S. Han, M. Kim, and C. S. Hwang, Atomic structure of conducting nanofilaments in TiO₂ resistive switching memory, Nature Nanotech 5, 148 (2010).
  11. [11]S. Kang, W.-S. Jang, A. N. Morozovska, O. Kwon, Y. Jin, Y.-H. Kim, H. Bae, C. Wang, S.-H. Yang, A. Belianinov, et al., Highly enhanced ferroelectricity in HfO₂-based ferroelectric thin film by light ion bombardment, Science 376, 731 (2022).DOI
  12. [12]R. Zhang, H. Huang, Q. Xia, C. Ye, X. Wei, J. Wang, L. Zhang, and L. Q. Zhu, Role of oxygen vacancies at the TiO₂ / HfO₂ interface in flexible oxide-based resistive switching memory, Adv. Electron. Mater. 5, 1800833 (2019).
  13. [13]E. D. Grimley, T. Schenk, X. Sang, M. Pešić, U. Schroeder, T. Mikolajick, and J. M. LeBeau, Structural changes underlying field-cycling phenomena in ferroelectric HfO₂ thin films, Adv. Electron. Mater. 2, 1600173 (2016).DOI
  14. [14]T. Mittmann, M. Materano, S.-C. Chang, I. Karpov, T. Mikolajick, and U. Schroeder, Impact of oxygen vacancy content in ferroelectric HZO films on the device performance, in 2020 IEEE International Electron Devices Meeting (IEDM) (IEEE, 2020) p. 18.4.1.DOI
  15. [15]P. Buragohain, A. Erickson, P. Kariuki, T. Mittmann, C. Richter, P. D. Lomenzo, H. Lu, T. Schenk, T. Mikolajick, U. Schroeder, and A. Gruverman, Fluid imprint and inertial switching in ferroelectric La:HfO₂ capacitors, ACS Appl. Mater. Interfaces 11, 35115 (2019).DOI
  16. [16]Z. Fan, J. Deng, J. Wang, Z. Liu, P. Yang, J. Xiao, X. Yan, Z. Dong, J. Wang, and J. Chen, Ferroelectricity emerging in strained (111)-textured ZrO₂ thin films, Applied Physics Letters 108, 012906 (2016).DOI
  17. [17]R. He, H. Wu, S. Liu, H. Liu, and Z. Zhong, Ferroelectric structural transition in hafnium oxide induced by charged oxygen vacancies, Phys. Rev. B 104, L180102 (2021).DOI
  18. [18]P. Nukala, M. Ahmadi, Y. Wei, S. de Graaf, E. Stylianidis, T. Chakrabortty, S. Matzen, H. W. Zandbergen, A. Björling, D. Mannix, D. Carbone, B. Kooi, and B. Noheda, Reversible oxygen migration and phase transitions in hafnia-based ferroelectric devices, Science 372, 630 (2021).DOI
  19. [19]I. MacLaren, T. Ras, M. MacKenzie, A. J. Craven, D. W. McComb, and S. D. Gendt, Texture, twinning, and metastable “tetragonal” phase in ultrathin films of HfO₂ on a si substrate, J. Electrochem. Soc. 156, G103 (2009).DOI
  20. [20]M. Hoffmann, U. Schroeder, T. Schenk, T. Shimizu, H. Funakubo, O. Sakata, D. Pohl, M. Drescher, C. Adelmann, R. Materlik, A. Kersch, and T. Mikolajick, Stabilizing the ferroelectric phase in doped hafnium oxide, J. Appl. Phys. 118, 072006 (2015).DOI
  21. [21]J. Wu, Impact of oxygen vacancies on monoclinic hafnium oxide and band alignment with semiconductors, Mater. Today Commun. 25, 101482 (2020).DOI
  22. [22]S. Liu and B. M. Hanrahan, Effects of growth orientations and epitaxial strains on phase stability of HfO₂ thin films, Phys. Rev. Mater. 3, 054404 (2019).DOI

Paper details

vlnc:W_ynz2w7p6
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents