Commissioning of Dedicated Furnace for Nb3Sn Coatings of 2.6 GHz Single Cell Cavities

Abstract

We present the results of commissioning a dedicated furnace for Nb3Sn coatings of 2.6 GHz single cell cavities. Nb3Sn is a desired coating due to its high critical temperature and smaller surface resistance compared to bulk Nb. Usage of Nb3Sn coated cavities will greatly reduce operating costs due to decreased dependance on cryo cooling. Tin is deposited by use of a tin chloride nucleation agent and tin vapor diffusion. Analysis of the resultant coating was performed using SEM/EDS to verify successful formation of Nb3Sn. Witness samples in line of sight of the source were used in order to understand the coating efficacy.

Introduction

Nb3_3Sn-coated cavities achieve accelerating gradients EaccE_{\mathrm{acc}} above 10 MV/m and quality factors in excess of 101010^{10} at 4 K [1, 2, 3, 4, 5]. High quality factors of Nb3_3Sn-coated cavities at 4 K are the enabling technology for compact cryomodules for industrial accelerators [6]. Several projects look to exploit this technology for various industrial applications [7, 8].

Given that the superheating critical field and superconducting transition temperature of Nb3_3Sn is higher than that of niobium, Nb3_3Sn superconducting material has the potential to sustain accelerating gradients twice that of niobium cavities and quality factors close to 5⋅10105 \cdot10^{10}, which will significantly reduce the operating and capital cost of future accelerators. Research and development efforts are ongoing to understand and improve vapor diffusion deposition techniques to realize they potential of Nb3_3Sn material.

Several institutions are pursuing Nb3_3Sn coatings and research is ongoing to understand material limitations and to optimize coating process [9, 10, 11, 12]. Nb3_3Sn coatings at Fermilab are done in the large coating system designed to coat multicell cavities. The coating system is constantly used to coat cavities for various projects. In order to enable Nb3_3Sn coating research on small cavities and samples in parallel with multicell cavity coating, we refurbish and commission for Nb3_3Sn coating an old furnace. Unlike the larger Nb3_3Sn system, which is routinely used for coating of Nb3_3Sn films on single and multi-cell cavities [4], the new system will be used to coat smaller single-cell cavities and for samples studies. This contribution presents the results from the commissioning of the new coating system.

Experimental Setup

For these Nb3_3Sn studies, the old IVI Model 3312-1212-120V furnace was adopted. This is the horizontal front loading furnace that features 12" x 12" x 15" hot zone. The furnace heaters as well as the inner shields are made out of molybdenum. The furnace is controlled by PLC connected to a computer and can reach up to 1200 °C. The furnace is evacuated with an oil-free mechanical pump and a cryopump and can reach down to 10−810^{-8} Torr range cold. The temperature is monitored with four molybdenum-sheathed type C thermocouples.

Experimental setup for Nb3Sn coating

Figure 1. Experimental setup for Nb3_3Sn coating. [a] Assembled experimental setup in the hot zone of the furnace. Note niobium foil covering the assembly and thermocouples at the top. [b,c] Niobium samples (b) and niobium cavity (c) prepared for the coating. Note that the blue color is due to 30 V anodizing. [d] Niobium cavity assembled for the coating inside niobium box on the niobium support fixture.

For Nb3_3Sn coating, a cavity is placed inside a niobium box onto niobium supports, fig. 1. Two samples, one on each end of the cavity, are mounted with niobium wires. One end of the cavity is then assembled with a molybdenum cup, which holds Sn and SnCl2_2. The other end is left open. For the first coating of 2.6 GHz cavity, 2 g of Sn and 0.5 g of SnCl2_2 were used. The assembly is then covered with niobium foil. As part of the preparation for the first Nb3_3Sn coating on SRF cavity, both the cavity and the samples were anodized for 30 V. The coating was done at 1150 °C for 3 hours preceded by the nucleation step at 500 °C. 1.6 g of Sn was consumed in the coating.

Measurements and Results

After the coating, the cavity surface and the samples were visually inspected, Figure 2. The inner surface of the cavity appeared to be well coated with a thick Nb3_3Sn layer. The sample that was placed far from the Sn and SnCl2_2 source appeared uniformly coated. On the sample that was close to the source, some variation in the coating could be visually observed.

Images of the inner surface of the coated cavity and samples

Figure 2. Images of the inner surface of the coated cavity and samples. Coated cavity half cells are shown in the top left and bottom right corners of the cavity. In the top right corner the sample GE048, mounted far from the source, is shown. In the bottom left corner the sample GE025, mounted close to the source, is shown.

Sample analysis

Samples were studied with FEI Helios dual beam system and Oxford EDS. Nearside (GE025) and far side (GE048) samples were compared to understand the quality of the coating, Figure 3. EDS analysis established that atomic percentage of Nb to Sn was in the desired range. Visual comparison of the samples revealed more frequent pits or holes on the surface of the far side sample (GE048). Relative increase in these features was previously linked with Sn deficiency in the coating process [13], which is supported by this data. The dual beam system was used to perform FIB on the sample. FIB crosssections show that the coating was 2–3 μ\mum thick consistent with the visual inspection, Figure 3.

SEM inspection of Nb3Sn-coated samples

Figure 3. SEM inspection of Nb3_3Sn-coated samples. [top] sample mounted close to Sn and SnCl2_2 source. [bottom] sample mounted far from the source. Note more pit-like features in the sample that was far from the source.

Cavity testing

Nb3_3Sn-coated 2.6 GHz cavity was cleaned with HPR and assembled in cleanroom for cryogenic testing in vertical dewar. For the cryogenic test the cavity was instrumented with fluxgates, Cernox temperature sensors, and the magnetic field compensation coil, Figure 5. The test was conducted with the cavity under static vacuum. Because of bi-metallic nature of Nb3_3Sn coating on niobium, the dewar was slowly

Cavity prepared for vertical testing on the vertical test stand

Figure 5. Cavity prepared for vertical testing on the vertical test stand. Note the magnetic field compensation coil, cernox temperature sensors, and the fluxgates.

FIB crosssection of Nb3-coated sample

Figure 4. FIB crosssection of Nb3_3-coated sample. Red dashed lines indicate the thickness of Nb3_3Sn coating.

cooled down with the cavity in the compensated field. The field reading of the fluxgate, which was used for field compensation, read about 0 mG. The other fluxgate reading was close to 8 mG, when the cavity temperature crossed about 18 K. The temperature difference across four temperature sensors was about 100 mK, when the average temperature of the cavity crossed 18 K during cooldown. In Figure 6, cavity test results are shown. At 4.4 K, the cavity exhibit the low field quality factor of about 5⋅10105 \cdot10^{10}. Quality factor degraded to about 5⋅10105 \cdot10^{10} at Eacc=11.5E_{\mathrm{acc}} = 11.5 quench field. At 2.0 K, the cavity exhibit the low field quality factor of above 2⋅10102 \cdot10^{10}. Quality factor degraded to about 8⋅1098 \cdot10^{9} at Eacc=11.8E_{\mathrm{acc}} = 11.8 quench field.

Figure 6. Cavity test results. [filled black squares] quality factor vs field at 4 K. [empty black squares] quality factor vs field at 2 K.

Conclusion

In this contribution we presented the first results of Nb3SnNb_3Sn coating on a 2.6 GHz cavity in the recently refurbished furnace. The coating appearance on the cavity was uniform. However, the detailed analysis of samples coated with the cavity presented evidence of low Sn flux during the coating. In the cryogenic RF test, the cavity showed Q0Q_0 of about 5⋅1095 \cdot10^9 and was limited to about 11.5 MV/m by quench at 4 K. At 2 K, the cavity Q0Q_0 was about 2⋅10102 \cdot10^{10} at low fields and the cavity was limited to about 12 MV/m at 11.8 K. With these promising results, we are continuing Nb3SnNb_3Sn coating optimization using a mock cavity with the goal to control and improve Sn flow.

Acknowledgments

This manuscript has been authored by Fermi Research Alliance, LLC under Contract No. DE-AC02-07CH11359 with the U.S. Department of Energy, Office of Science, Office of High Energy Physics. This material is based upon work supported by the U.S. Department of Energy, Office of Science, Office of Nuclear Physics.

References

  1. [1]S. Posen and M. Liepe, Proc. 16th Int. Conf. RF Supercond., (2013), pp. 666-669
  2. [2]G.V. Eremeev et al., in Proc. 17th Int. Conf. RF Super., (2015), pp. 505-511
  3. [3]S. Posen, M. Liepe, and D. L. Hall, Appl. Phys. Lett. 106, 082601 (2015)
  4. [4]S.Posen and D.L.Hall, Supercond .Sci. Technol. 30033004 (2017)
  5. [5]S.Posen, TTC meeting, Vancouver, Canada(2019)
  6. [6]R. Kephart et al. Proc. 17th Int. Conf. RF Supercond, (2015)
  7. [7]G. Ciovati et al., Phys. Rev. AB 26, 044701 (2023)
  8. [8]R.C. Dhuley et al, Phys. Rev. Accel. Beams 25, 041601 (2022)
  9. [9]C. Dong et al., Phys. C, Volume 600, (2022) 1354107
  10. [10]K. Takahashi et al., Proc. 20th Int. Conf. RF Supercond., (2021), pp. 23 - 26
  11. [11]U. Pudasaini et al., Proc. 20th Int. Conf. RF Supercond., (2021), pp. 516 - 521
  12. [12]R. D. Porter et al., Proc. 20th Int. Conf. RF Supercond., (2021), pp. 6 - 10
  13. [13]U. Pudasaini et al., 2020 Supercond. Sci. Technol. 33 045012

Paper details

vlnc:W_yq3cn2rj
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents